Tire
The tire's cap tread composition with silica and a specific Sc/Tt ratio addresses the challenge of balancing fuel efficiency, wear resistance, and ice/snow performance by improving silica dispersion and reinforcing properties.
Patent Information
- Application Number
- JP2023063715
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-10
- Publication Date
- 2024-10-23
AI Technical Summary
Existing tires face challenges in achieving a well-balanced improvement in fuel efficiency, wear resistance, and performance on ice and snow, as these performances are often contradictory.
A tire design with a cap tread composed of a rubber composition containing silica, a resin with modifying groups, and a specific silica-to-tread thickness ratio (Sc/Tt) of 5.0 or more, enhancing silica dispersion and reinforcing properties.
The design improves overall performance by reducing stress concentration, increasing silica contact with the road surface, and enhancing abrasion resistance and ice/snow performance.
Smart Images

Figure 2024150342000003 
Figure 2024150342000004 
Figure 2024150342000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a tire. [Background technology]
[0002] Tires such as winter tires (e.g., studless tires) and all-season tires are required to have various performance characteristics, such as low fuel consumption, wear resistance, performance on snow and ice, etc. However, since these are generally contradictory performance characteristics, it is desirable to improve these performance characteristics in a well-balanced manner (see Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2013-249423 A Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present invention is to provide a tire that can solve the above problems and improve the overall performance of fuel economy, wear resistance, and performance on snow and ice. [Means for solving the problem]
[0005] The present invention provides a tire having a cap tread formed of a rubber composition including a rubber component, a filler including silica, and a resin, the resin contains a modified resin having a modifying group containing at least one atom selected from the group consisting of a nitrogen atom, an oxygen atom, a fluorine atom, and a chlorine atom, The tire has a ratio (Sc / Tt) of the content Sc (parts by mass) of the silica per 100 parts by mass of the rubber component to a tread thickness Tt (mm) of 5.0 or more. Effect of the Invention
[0006] The present invention relates to a tire having a cap tread formed from a rubber composition containing a rubber component, a filler containing silica, and a resin, wherein the resin contains a modified resin having a modifying group containing at least one atom selected from the group consisting of nitrogen atoms, oxygen atoms, fluorine atoms, and chlorine atoms, and the ratio (Sc / Tt) of the silica content Sc (parts by mass) per 100 parts by mass of the rubber component to the tread thickness Tt (mm) is 5.0 or more, thereby enabling improvement in overall performance in terms of fuel economy, wear resistance, and performance on ice and snow. [Brief description of the drawings]
[0007] [Figure 1] 1 is a cross-sectional view showing a portion of a pneumatic tire. [Diagram 2] 2 is an enlarged cross-sectional view showing the vicinity of the tread 4 of the tire 2 of FIG. 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The tire of the present invention has a cap tread formed from a rubber composition containing a rubber component, a filler containing silica, and a resin, the resin containing a modified resin having a modifying group containing at least one atom selected from the group consisting of nitrogen atoms, oxygen atoms, fluorine atoms, and chlorine atoms, and the relationship of Sc / T being 5.0 or more is satisfied.
[0009] The reason why the above-mentioned effect is obtained is not entirely clear, but it is presumed to be due to the following mechanism. Silica is a polar substance that has a strong tendency to self-aggregate and is difficult to disperse in diene rubber. However, by compounding a modified resin having a modifying group containing at least one atom selected from the group consisting of nitrogen atoms, oxygen atoms, fluorine atoms, and chlorine atoms, the modified resin is adsorbed onto the silica surface, improving the affinity for the rubber component, and it is believed that the dispersibility of the silica is improved. Furthermore, by blending a relatively large amount of silica relative to the thickness of the tread so that the ratio (Sc / T) of the silica content Sc to the tread thickness T is 5.0 or more, the proportion of silica that can come into contact with the road surface is increased and high reinforcement is ensured. Since high reinforcement is ensured, high abrasion resistance and hardness at low temperatures are ensured. Therefore, by satisfying the above relationship, stress concentration within the rubber is less likely to occur, the tread rubber is sufficiently reinforced, and the proportion of silica that can come into contact with the road surface is increased, thereby improving abrasion resistance and performance on ice and snow while maintaining low rolling resistance.It is therefore presumed that this will result in improved overall fuel efficiency, abrasion resistance, and performance on ice and snow.
[0010] In this way, the present invention solves the problem (objective) of improving the overall performance of fuel economy, wear resistance, and performance on snow and ice by configuring a tire that has a cap tread formed from a rubber composition containing a rubber component, a filler containing silica, and the resin, and that satisfies Sc / T of 5.0 or more. In other words, the parameter Sc / T of 5.0 or more does not define the problem (objective), and the problem of the present application is to improve the overall performance of fuel economy, wear resistance, and performance on snow and ice, and a configuration that satisfies the above parameter is used as a means to achieve this.
[0011] The tire of the present invention includes a cap tread. In this specification, the cap tread refers to the part of the tread that is disposed on the outermost side in the tire radial direction and comes into contact with the road surface. That is, when the tread has a single-layer structure, the single layer corresponds to the cap tread, when the tread has a two-layer structure of a surface layer (cap part) and an intermediate layer (base part), the surface layer corresponds to the cap tread, and when the tread has a structure of three or more layers, the outermost layer that comes into contact with the road surface corresponds to the cap tread.
[0012] The cap tread is formed from a rubber composition for cap treads. First, the rubber composition for cap tread will be described below.
[0013] The rubber component contained in the rubber composition for cap tread is a component that contributes to crosslinking, and generally corresponds to a polymer component that is not extracted with acetone and is a polymer having a weight average molecular weight (Mw) of 10,000 or more. The rubber component is in a solid state at room temperature (25°C).
[0014] The weight average molecular weight of the rubber component is preferably 50,000 or more, more preferably 150,000 or more, and even more preferably 200,000 or more, and is preferably 2,000,000 or less, more preferably 1,500,000 or less, and even more preferably 1,000,000 or less. Within the above ranges, the effect tends to be better obtained.
[0015] In this specification, the weight average molecular weight (Mw) can be determined by converting it into standard polystyrene based on the measured value obtained by gel permeation chromatography (GPC) (GPC-8000 series manufactured by Tosoh Corporation, detector: differential refractometer, column: TSKGEL SUPERMULTIPORE HZ-M manufactured by Tosoh Corporation).
[0016] As the rubber component usable in the rubber composition for cap tread, for example, diene rubber can be used. Examples of diene rubber include isoprene rubber, butadiene rubber (BR), styrene butadiene rubber (SBR), styrene isoprene butadiene rubber (SIBR), ethylene propylene diene rubber (EPDM), chloroprene rubber (CR), and acrylonitrile butadiene rubber (NBR). Examples also include butyl rubber and fluororubber. These may be used alone or in combination of two or more. Among them, isoprene rubber, BR, and SBR are preferred from the viewpoint of obtaining a better effect. In addition, these rubber components may be modified or hydrogenated as described below, and extended rubber extended by oil, resin, liquid rubber component, etc. may be used.
[0017] The diene rubber may be a non-modified diene rubber or a modified diene rubber. The modified diene rubber may be any diene rubber having a functional group that interacts with a filler such as silica. Examples of the modified diene rubber include terminal-modified diene rubber (terminal-modified diene rubber having the functional group at the terminal) in which at least one terminal of the diene rubber has been modified with a compound (modifier) having the functional group, main-chain modified diene rubber having the functional group in the main chain, main-chain terminal-modified diene rubber having the functional group in the main chain and at least one terminal (for example, main-chain terminal-modified diene rubber having the functional group in the main chain and at least one terminal modified with the modifier), and terminal-modified diene rubber modified (coupled) with a polyfunctional compound having two or more epoxy groups in the molecule and having a hydroxyl group or epoxy group introduced therein.
[0018] Examples of the functional group include an amino group, an amide group, a silyl group, an alkoxysilyl group, an isocyanate group, an imino group, an imidazole group, a urea group, an ether group, a carbonyl group, an oxycarbonyl group, a mercapto group, a sulfide group, a disulfide group, a sulfonyl group, a sulfinyl group, a thiocarbonyl group, an ammonium group, an imide group, a hydrazo group, an azo group, a diazo group, a carboxyl group, a nitrile group, a pyridyl group, an alkoxy group, a hydroxyl group, an oxy group, and an epoxy group. These functional groups may have a substituent. Among them, an amino group (preferably an amino group in which a hydrogen atom of an amino group is substituted with an alkyl group having 1 to 6 carbon atoms), an alkoxy group (preferably an alkoxy group having 1 to 6 carbon atoms), and an alkoxysilyl group (preferably an alkoxysilyl group having 1 to 6 carbon atoms) are preferred.
[0019] Examples of isoprene-based rubber include natural rubber (NR), isoprene rubber (IR), modified NR, modified NR, and modified IR. Examples of NR include SIR20, RSS♯3, TSR20, and other rubber industry-standard rubbers. Examples of IR include IR2200 and other rubber industry-standard rubbers. Examples of modified NR include deproteinized natural rubber (DPNR), high-purity natural rubber (UPNR), and other rubbers. Examples of modified NR include epoxidized natural rubber (ENR), hydrogenated natural rubber (HNR), and grafted natural rubber. Examples of modified IR include epoxidized isoprene rubber, hydrogenated isoprene rubber, and grafted isoprene rubber. These may be used alone or in combination of two or more.
[0020] When the rubber composition for cap tread contains isoprene-based rubber, the content of isoprene-based rubber in 100% by mass of rubber component is preferably 9% by mass or more, more preferably 15% by mass or more, even more preferably 16% by mass or more, particularly preferably 20% by mass or more, and is preferably 45% by mass or less, more preferably 35% by mass or less, and even more preferably 30% by mass or less. When it is within the above range, the effect tends to be better obtained. In addition, it is possible to increase the sustainable material ratio.
[0021] The mechanism by which greater effects are obtained when the isoprene-based rubber is contained within the above range, particularly 15 to 45% by mass, is not clear, but is presumed to be as follows. By blending a specified amount of isoprene-based rubber, it is possible to control the incompatible phase structure, suppress the uneven distribution of silica, and improve the viscoelastic balance, which is thought to particularly improve fuel efficiency and performance on ice and snow.
[0022] The BR is not particularly limited, and for example, high cis BR with a high cis content, BR containing syndiotactic polybutadiene crystals, BR synthesized using a rare earth catalyst (rare earth BR), etc. can be used. These may be used alone or in combination of two or more. In particular, the BR preferably contains high cis BR with a cis content of 90% by mass or more. The cis content is more preferably 95% by mass or more. The cis content can be measured by infrared absorption spectroscopy.
[0023] In addition, either unmodified or modified BR can be used as the BR. Modified BR includes modified BR into which functional groups similar to those of modified diene rubbers have been introduced. In addition, hydrogenated butadiene polymer (hydrogenated BR) can also be used as the BR.
[0024] When the rubber composition for cap tread contains BR, the content of BR in 100% by mass of the rubber component is preferably 10% by mass or more, more preferably 20% by mass or more, even more preferably 25% by mass or more, particularly preferably 30% by mass or more, and is preferably 80% by mass or less, more preferably 50% by mass or less, and even more preferably 35% by mass or less. When it is within the above range, the effect tends to be better obtained.
[0025] The SBR is not particularly limited, and for example, emulsion polymerized styrene butadiene rubber (E-SBR), solution polymerized styrene butadiene rubber (S-SBR), etc. can be used, but from the viewpoint of obtaining better effects, solution polymerized styrene butadiene rubber is preferred. These may be used alone or in combination of two or more kinds.
[0026] The styrene content of SBR is preferably 5% by mass or more, more preferably 20% by mass or more, and even more preferably 25% by mass or more. The styrene content is preferably 60% by mass or less, more preferably 40% by mass or less, and even more preferably 35% by mass or less. When it is within the above range, the effect tends to be better obtained. In this specification, the styrene content is 1 It can be measured by H-NMR measurement.
[0027] The vinyl bond content of SBR is preferably 3% by mass or more, more preferably 5% by mass or more, and even more preferably 7% by mass or more. When the vinyl bond content is within the above range, preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less, the effect tends to be better. In this specification, the vinyl bond amount (1,2-bonded butadiene unit amount) can be measured by infrared absorption spectroscopy.
[0028] The glass transition temperature (Tg) of SBR is preferably −25° C. or lower, more preferably −30° C. or lower, even more preferably −40° C. or lower, and particularly preferably −50° C. or lower. The lower limit of the glass transition temperature is preferably −78° C. or higher, more preferably −75° C. or higher, even more preferably −72° C. or higher, and particularly preferably −70° C. or higher. In this specification, the glass transition temperature is a value measured by differential scanning calorimetry (DSC) at a temperature rise rate of 10° C. / min according to JIS K7121.
[0029] The mechanism by which greater effectiveness is achieved when SBR with a Tg of -25°C or lower is included is not clear, but it is presumed that combining such SBR with a resin having the modifying group enhances the effect of dispersing silica, resulting in improved overall fuel efficiency, abrasion resistance, and performance on snow and ice.
[0030] Both unmodified and modified SBR can be used. Modified SBR includes modified SBR with the same functional groups as modified diene rubber. Hydrogenated styrene-butadiene copolymer (hydrogenated SBR) can also be used as SBR.
[0031] When the rubber composition for cap tread contains SBR, the content of SBR in 100% by mass of the rubber component is preferably 10% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, particularly preferably 50% by mass or more, and is preferably 90% by mass or less, more preferably 80% by mass or less, and even more preferably 70% by mass or less. When it is within the above range, the effect tends to be better obtained.
[0032] The rubber composition for the cap tread contains silica as a filler. Examples of silica that can be used include dry process silica (anhydrous silica) and wet process silica (hydrated silica). Among them, wet process silica is preferred because it has a large number of silanol groups. Commercially available products include products from Evonik Degussa, Rhodia, Tosoh Silica, Solvay Japan, and Tokuyama. These may be used alone or in combination of two or more. In addition to these silicas, silica made from biomass materials such as rice husks may be used. The rice husk silica may be obtained by heat treating rice husks, or may be obtained by treating rice husks with an acid and then heat treating them, reacting the heat-treated crude rice husk silica with alcohol to convert it into water glass, and then obtaining silica particles in the same manner as ordinary wet silica.
[0033] The nitrogen adsorption specific surface area (N2SA) of the silica is preferably 50 m 2 / g or more, more preferably 100m 2 / g or more, more preferably 150m 2 The upper limit of the N2SA of silica is not particularly limited, but is preferably 350 m 2 / g or less, more preferably 300m 2 / g or less, more preferably 250m 2 Within the above range, there is a tendency for the effect to be better obtained. The N2SA of silica is a value measured by the BET method in accordance with ASTM D3037-93.
[0034] The average primary particle size of silica is preferably 24 nm or less, more preferably 17 nm or less, even more preferably 16 nm or less, and particularly preferably 15 nm or less. Also, it is preferably 6 nm or more, more preferably 9 nm or more, and even more preferably 12 nm or more. When it is within the above range, curing tends to be obtained better.
[0035] The above-mentioned "average primary particle size of silica" is a value calculated by taking an arithmetic average of particle sizes of 400 particles photographed with a transmission or scanning electron microscope, taking the diameter of the sphere as the particle size if the particle shape is approximately spherical, taking the minor axis as the particle size if the particle shape is needle-like or rod-like, and taking the average of the minor axis and the diameter as the particle size if the particle shape is irregular.
[0036] In the rubber composition for cap tread, the content of silica is preferably 30 parts by mass or more, more preferably 58 parts by mass or more, even more preferably 75 parts by mass or more, and is preferably 200 parts by mass or less, more preferably 150 parts by mass or less, even more preferably 120 parts by mass or less. When it is within the above range, the effect tends to be better obtained.
[0037] The rubber composition for a cap tread preferably further contains a silane coupling agent. The silane coupling agent is not particularly limited, and those known in the rubber field can be used. For example, bis(3-triethoxysilylpropyl)tetrasulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(4-triethoxysilylbutyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, bis(2-trimethoxysilylethyl)tetrasulfide, bis(2-triethoxysilylethyl)trisulfide, bis(4-trimethoxysilylbutyl)trisulfide, bis(3-triethoxysilylpropyl)disulfide, bis(2-triethoxysilylethyl)disulfide, bis(4-triethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide, bis(2-trimethoxysilylethyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide, bis(2-trimethoxysilylethyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, 3-trimethoxysilylpropyl-N, Examples of such silylsilanes include sulfide-based silylsilanes such as N-dimethylthiocarbamoyl tetrasulfide, 2-triethoxysilylethyl-N,N-dimethylthiocarbamoyl tetrasulfide, and 3-triethoxysilylpropyl methacrylate monosulfide; mercapto-based silylsilanes such as 3-mercaptopropyltrimethoxysilane, 2-mercaptoethyltriethoxysilane, and Momentive's NXT and NXT-Z; vinyl-based silylsilanes such as vinyltriethoxysilane and vinyltrimethoxysilane; amino-based silylsilanes such as 3-aminopropyltriethoxysilane and 3-aminopropyltrimethoxysilane; glycidoxy-based silylsilanes such as γ-glycidoxypropyltriethoxysilane and γ-glycidoxypropyltrimethoxysilane; nitro-based silylsilanes such as 3-nitropropyltrimethoxysilane and 3-nitropropyltriethoxysilane; and chloro-based silylsilanes such as 3-chloropropyltrimethoxysilane and 3-chloropropyltriethoxysilane. Commercially available products include those manufactured by Evonik Degussa, Momentive, Shin-Etsu Silicones, Tokyo Chemical Industry, Azumax, and Dow Corning Toray Co., Ltd. These may be used alone or in combination of two or more.
[0038] In the rubber composition for cap tread, the content of the silane coupling agent is preferably 0.1 parts by mass or more, more preferably 3 parts by mass or more, even more preferably 5 parts by mass or more, and particularly preferably 7 parts by mass or more, based on 100 parts by mass of silica. The upper limit of the content is preferably 50 parts by mass or less, more preferably 20 parts by mass or less, even more preferably 15 parts by mass or less, and particularly preferably 10 parts by mass or less. Within the above range, the effect tends to be better obtained.
[0039] The rubber composition for a cap tread may contain a filler other than silica. Fillers other than silica are not particularly limited, and materials known in the rubber field can be used, such as inorganic fillers such as carbon black, calcium carbonate, talc, alumina, clay, aluminum hydroxide, aluminum oxide, mica, biochar, poorly dispersible fillers, etc. Among these, carbon-derived fillers (carbon-containing fillers) such as carbon black are preferred.
[0040] In the rubber composition for cap treads, the content of the filler (total amount of fillers such as silica, carbon black, etc.) is preferably 30 parts by mass or more, more preferably 50 parts by mass or more, even more preferably 70 parts by mass or more, particularly preferably 90 parts by mass or more, and is preferably 250 parts by mass or less, more preferably 200 parts by mass or less, and even more preferably 150 parts by mass or less, based on 100 parts by mass of the rubber component. When the content is within the above range, the effect tends to be better obtained.
[0041] Carbon black usable in the rubber composition for cap tread is not particularly limited, but may be N134, N110, N220, N234, N219, N339, N330, N326, N351, N550, N762, etc. Commercially available products include those from Asahi Carbon Co., Ltd., Cabot Japan Co., Ltd., Tokai Carbon Co., Ltd., Mitsubishi Chemical Co., Ltd., Lion Co., Ltd., Shin-Nichika Carbon Co., Ltd., Columbia Carbon Co., Ltd., etc. These may be used alone or in combination of two or more. In addition to conventional carbon black made from mineral oils, etc., carbon black made from biomass materials such as lignin may be used. Recycled carbon black obtained by decomposing rubber products containing carbon black such as tires, plastic products, etc. may be appropriately substituted for the above carbon black in an equal amount.
[0042] The nitrogen adsorption specific surface area (N2SA) of carbon black is 30m 2 / g or more is preferable, and 50m 2 / g or more is more preferable, and 70m 2 / g or more is more preferable. 2 / g or less is preferable, and 150m 2 / g or less is more preferable, and 130m 2 / g or less is more preferable, and 120m 2 Within the above range, there is a tendency that the effect is more favorable.
[0043] When the rubber composition for cap tread contains carbon black, the content of carbon black is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 15 parts by mass or more, and is preferably 80 parts by mass or less, more preferably 50 parts by mass or less, and even more preferably 35 parts by mass or less. When the content is within the above range, the effect tends to be better.
[0044] Examples of the poorly dispersible filler include microfibrillated vegetable fibers, short fiber cellulose, gel compounds, etc. Among these, microfibrillated vegetable fibers are preferred.
[0045] The microfibrillated plant fiber is preferably cellulose microfibril, since it has good reinforcing properties. The cellulose microfibril is not particularly limited as long as it is derived from a natural product, and examples thereof include those derived from resource biomass such as fruits, grains, and root vegetables, wood, bamboo, hemp, jute, and kenaf, and pulp, paper, cloth, agricultural waste, waste biomass such as food waste and sewage sludge obtained from these as raw materials, unused biomass such as rice straw, wheat straw, and thinned wood, as well as cellulose produced by sea squirts, acetic acid bacteria, etc. These microfibrillated plant fibers may be used alone or in combination of two or more.
[0046] In this specification, cellulose microfibrils typically refer to cellulose fibers having an average fiber diameter of 10 μm or less, more typically cellulose fibers having a microstructure formed by the aggregation of cellulose molecules and an average fiber diameter of 500 nm or less. Typical cellulose microfibrils are formed, for example, as an aggregate of cellulose fibers having the above-mentioned average fiber diameter.
[0047] When the rubber composition for cap tread contains a poorly dispersible filler, the content of the poorly dispersible filler is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, even more preferably 20 parts by mass or less, and particularly preferably 10 parts by mass or less. Within the above range, the effect tends to be better obtained.
[0048] The rubber composition for the cap tread desirably contains a plasticizer. In this specification, the plasticizer is a material that imparts plasticity to the rubber component, and may be liquid or solid at room temperature (25° C.) These may be used alone or in combination of two or more kinds.
[0049] When the rubber composition for cap tread contains a plasticizer, the content of the plasticizer (total amount of plasticizers such as liquid plasticizers and solid plasticizers) is preferably 10 parts by mass or more, more preferably 25 parts by mass or more, even more preferably 30 parts by mass or more, particularly preferably 35 parts by mass or more, and is preferably 100 parts by mass or less, more preferably 60 parts by mass or less, and even more preferably 50 parts by mass or less, per 100 parts by mass of the rubber component. When the content is within the above range, the effect tends to be better obtained. In addition, when the above-mentioned extension rubber is used, the amount of the extension component used in the extension rubber is included in the content of the plasticizer.
[0050] When the rubber composition for cap tread contains a liquid plasticizer, the content of the liquid plasticizer is preferably 5 parts by mass or more, more preferably 20 parts by mass or more, and even more preferably 25 parts by mass or more, and is preferably 80 parts by mass or less, more preferably 60 parts by mass or less, and even more preferably 45 parts by mass or less, based on 100 parts by mass of the rubber component. When the content is within the above range, the effect tends to be better obtained.
[0051] When the rubber composition for cap tread contains a solid plasticizer, the content of the solid plasticizer is preferably 3 parts by mass or more, more preferably 5 parts by mass or more, and even more preferably 27 parts by mass or more, and is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, even more preferably 20 parts by mass or less, and particularly preferably 12 parts by mass or less, based on 100 parts by mass of the rubber component. When the content is within the above range, the effect tends to be better obtained.
[0052] The plasticizer usable in the rubber composition for cap tread is not particularly limited, and examples thereof include oil, liquid polymer, resin, etc. These may be used alone or in combination of two or more kinds.
[0053] Examples of the oil include process oil, vegetable oil, and mixtures thereof. Examples of the process oil include paraffin-based process oil, aroma-based process oil, naphthene-based process oil, and the like, such as MES (Mild Extract Solvated), DAE (Distillate Aromatic Extract), TDAE (treated Distillate Aromatic Extract), TRAE (treated Residual Aromatic Extract), and RAE (residual aromatic extract). Examples of the vegetable oil include castor oil, cottonseed oil, linseed oil, rapeseed oil, soybean oil, palm oil, coconut oil, peanut oil, rosin, pine oil, pine tar, tall oil, corn oil, rice oil, safflower oil, sesame oil, olive oil, sunflower oil, palm kernel oil, camellia oil, jojoba oil, macadamia nut oil, and tung oil. As commercially available products, products from Idemitsu Kosan Co., Ltd., Sankyo Yuka Kogyo Co., Ltd., Japan Energy Co., Ltd., Orisoi Co., Ltd., H&R Co., Ltd., Toyokuni Oil Mills Co., Ltd., Showa Shell Sekiyu K.K., Fuji Kosan Co., Ltd., Nisshin Oillio Group Co., Ltd., etc. can be used. Among them, process oils (paraffin-based process oils, aromatic process oils, naphthenic process oils, etc.) and vegetable oils are preferred. From the viewpoint of life cycle assessment, the above-mentioned oils may be lubricating oils used in rubber mixers and engines, or oils refined from waste edible oils used in restaurants.
[0054] When the rubber composition for cap tread contains oil, the content of the oil is preferably 5 parts by mass or more, more preferably 20 parts by mass or more, and even more preferably 25 parts by mass or more, and is preferably 80 parts by mass or less, more preferably 60 parts by mass or less, and even more preferably 45 parts by mass or less, based on 100 parts by mass of the rubber component. When the content is within the above range, the effect tends to be better obtained.
[0055] Examples of liquid polymers include liquid diene polymers and liquid farnesene polymers that are in a liquid state at room temperature (25°C). Examples of liquid diene polymers include liquid styrene butadiene copolymers (liquid SBR), liquid butadiene polymers (liquid BR), liquid isoprene polymers (liquid IR), liquid styrene isoprene copolymers (liquid SIR), liquid styrene butadiene styrene block copolymers (liquid SBS block polymers), and liquid styrene isoprene styrene block copolymers (liquid SIS block polymers), which are in a liquid state at 25°C. The ends or main chains of these may be modified with polar groups. Hydrogenated products of these polymers may also be used.
[0056] The rubber composition for the cap tread contains a resin. The above resin may be either solid or liquid at room temperature (25° C.).
[0057] The rubber composition for cap tread contains, as the resin, a modified resin having a modifying group containing at least one atom selected from the group consisting of a nitrogen atom, an oxygen atom, a fluorine atom and a chlorine atom.
[0058] In the rubber composition for cap tread, the content of the modified resin is preferably 3 parts by mass or more, more preferably 5 parts by mass or more, and even more preferably 27 parts by mass or more, and is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, even more preferably 20 parts by mass or less, and particularly preferably 12 parts by mass or less, based on 100 parts by mass of the rubber component. When the content is within the above range, the effect tends to be better obtained.
[0059] The resin constituting the skeleton of the modified resin is not particularly limited, and any known resin can be used. The resin constituting the skeleton is preferably a hydrocarbon resin. As the hydrocarbon resin, a resin containing a hydrocarbon chain can be used, and for example, a thermoplastic resin such as an aromatic vinyl polymer, a coumarone-indene resin, a coumarone resin, an indene resin, a C5 resin, a C5-C9 resin, a C9 resin, a terpene resin, a terpene-aromatic compound resin, a rosin resin, a dicyclopentadiene resin, or an alkylphenol resin can be preferably used. Among them, an aromatic vinyl polymer is preferable.
[0060] The aromatic vinyl polymer is a polymer containing an aromatic vinyl monomer as a constituent unit. For example, it can be a resin obtained by polymerizing α-methylstyrene and / or styrene, and specifically, it can be a homopolymer of styrene (styrene resin), a homopolymer of α-methylstyrene (α-methylstyrene resin), a copolymer of α-methylstyrene and styrene, a copolymer of styrene and another monomer, etc.
[0061] Coumarone-indene resin is a resin containing coumarone and indene as the main monomer components that make up the resin skeleton (main chain). Other monomer components contained in the skeleton besides coumarone and indene include styrene, α-methylstyrene, methylindene, vinyltoluene, etc.
[0062] The coumarone resin is a resin that contains coumarone as the main monomer component that constitutes the skeleton (main chain) of the resin.
[0063] An indene resin is a resin that contains indene as a main monomer component that constitutes the skeleton (main chain) of the resin.
[0064] Examples of C5 resins include C5 synthetic petroleum resins, such as aliphatic petroleum resins obtained by polymerizing a C5 fraction obtained by thermal cracking of naphtha in the petrochemical industry using a Friedel-Crafts catalyst such as AlCl3 or BF3. C5 fractions usually include olefinic hydrocarbons such as 1-pentene, 2-pentene, 2-methyl-1-butene, 2-methyl-2-butene, and 3-methyl-1-butene; diolefinic hydrocarbons such as 2-methyl-1,3-butadiene, 1,2-pentadiene, 1,3-pentadiene, and 3-methyl-1,2-butadiene; and the like. Commercially available C5 resins can be used, such as T-REZ RA100 (manufactured by Tonen Chemical Industry Co.), Escorez 1000 series (manufactured by ExxonMobil Chemical Corporation), and Quinton 100 series A100, B170, M100, and R100 (manufactured by Zeon Corporation).
[0065] Examples of C5-C9 resins include C5-C9 synthetic petroleum resins, such as solid polymers obtained by polymerizing petroleum-derived C5 fractions and C9 fractions using Friedel-Crafts catalysts such as AlCl3 and BF3. Specific examples include copolymers mainly composed of styrene, vinyltoluene, α-methylstyrene, indene, etc. Commercially available C5-C9 resins include T-REZ RD104 (manufactured by Tonen Chemical Industry Co., Ltd.), ECR213 (manufactured by ExxonMobil Chemical Co., Ltd.), and Quinton G100B (manufactured by Zeon Corporation).
[0066] C9 resins are by-produced C9 fractions produced by thermal decomposition of naphtha in the petrochemical industry together with basic petrochemical raw materials such as ethylene and propylene, and include resins polymerized from aromatics having a carbon number of 9, with vinyltoluene, alkylstyrene, and indene as the main monomer. Specific examples of C9 fractions include vinyltoluene, α-methylstyrene, β-methylstyrene, γ-methylstyrene, o-methylstyrene, p-methylstyrene, and indene. C9 resins include C8 fractions such as styrene, C9 fractions, and C8 fractions such as styrene, C9 fractions, and C9 fractions. 10The fractions methylindene, 1,3-dimethylstyrene, and even naphthalene, vinylnaphthalene, vinylanthracene, p-tert-butylstyrene are used as raw materials, and these C8-C 10 The fractions and the like can be copolymerized as a mixture with, for example, a Friedel-Crafts catalyst to obtain the C9 resin. Commercially available C9 resins can be used, and examples of C9 petroleum resins include Nippon Oil Neopolymer L-90, Nippon Oil Neopolymer 120, Nippon Oil Neopolymer 130, and Nippon Oil Neopolymer 140 (manufactured by JX Nippon Oil & Energy Corporation).
[0067] Terpene resins include turpentine oil obtained at the same time as rosin is obtained from pine trees, or solid resins obtained by blending polymerizable components separated from this and polymerizing them using a Friedel-Crafts catalyst. Specific examples include β-pinene resin and α-pinene resin. Commercially available terpene resins include the YS Resin series (manufactured by Yasuhara Chemical Co., Ltd.) and the Picolite series A115, S115, etc. (manufactured by Hercules Co., Ltd.).
[0068] A representative example of the terpene-aromatic compound resin is terpene-phenol resin. The terpene-phenol resin can be obtained by reacting terpenes with various phenols using a Friedel-Crafts catalyst, or by further condensing with formalin. There is no particular limitation on the terpene as the raw material, and monoterpene hydrocarbons such as α-pinene and limonene are preferred, and those containing α-pinene are more preferred. Commercially available terpene-aromatic compound resins can be used, and examples of such resins include YS Polystar U series, YS Polystar T series, YS Polystar S series, YS Polystar G series, YS Polystar N series, YS Polystar K series, and YS Polystar TH series (manufactured by Yasuhara Chemical Co., Ltd.), Tamanol 803L, and Tamanol 901 (manufactured by Arakawa Chemical Industries Co., Ltd.).
[0069] Rosin resins are the residues remaining after collecting balsams such as pine resin (pine tar), which is the sap of plants of the Pinaceae family, and distilling turpentine essential oil. Examples of rosin resins include natural resins mainly composed of rosin acid (abietic acid, palustric acid, isopimaric acid, etc.), and modified resins and hydrogenated resins obtained by modifying, hydrogenating, etc., of these. Specific examples include natural resin rosin, polymerized rosin and partially hydrogenated rosin thereof; glycerin ester rosin, partially hydrogenated rosin, fully hydrogenated rosin and polymerized rosin thereof; pentaerythritol ester rosin, partially hydrogenated rosin and polymerized rosin thereof; and the like. Examples of natural resin rosins include gum rosin, tall oil rosin, wood rosin, etc., contained in raw rosin and tall oil. Rosin-based resins can be commercially available products, such as Polypale and Pentalin C (manufactured by Eastman Chemical Co.), Lime Resin No. 1, Pencel A and Pencel AD (manufactured by Arakawa Chemical Industries Co., Ltd.), Neotoll 105 (manufactured by Harima Chemical Co., Ltd.), SN Tack 754 (manufactured by San Nopco Co., Ltd.), and Hi-Rosin S (manufactured by Taisha Matsu Oil Co., Ltd.).
[0070] Examples of dicyclopentadiene resins include resins obtained by polymerizing dicyclopentadiene using Friedel-Crafts catalysts such as AlCl3 and BF3. Commercially available dicyclopentadiene resins include Marcaretz M-890A (manufactured by Maruzen Petrochemical Co., Ltd.), Quinton 1920, and Quinton 1105 (manufactured by Zeon Corporation).
[0071] Examples of the alkylphenol resin include those obtained by condensation reaction of alkylphenol and formaldehyde under a catalyst. Commercially available alkylphenol resins include Tackirol 201 (alkylphenol formaldehyde resin, manufactured by Taoka Chemical Industry Co., Ltd.), Tackirol 250-I (brominated alkylphenol formaldehyde resin, manufactured by Taoka Chemical Industry Co., Ltd.), Tackirol 250-III (brominated alkylphenol formaldehyde resin, manufactured by Taoka Chemical Industry Co., Ltd.), Hitanol 1502P (alkylphenol formaldehyde resin, manufactured by Hitachi Chemical Co., Ltd.), R7521P, SP1068, R7510PJ, R7572P and R7578P (manufactured by SI GROUP INC.).
[0072] The softening point of the resin constituting the skeleton of the modified resin is preferably 60° C. or higher, more preferably 70° C. or higher, and even more preferably 80° C. or higher, when the resin is in a solid state at room temperature (25° C.). The upper limit is preferably 160° C. or lower, more preferably 130° C. or lower, and even more preferably 115° C. or lower. By keeping the softening point within the above range, the effect tends to be better obtained. Furthermore, when the resin constituting the skeleton of the modified resin is in a liquid state at room temperature (25°C), the softening point is preferably 25°C or lower, more preferably 15°C or lower, and even more preferably 0°C or lower. The softening point of the resin is the temperature at which the ball drops when the softening point specified in JIS K6220-1:2001 is measured using a ring and ball softening point tester. The softening point of a resin is usually 50°C ± 5°C higher than the glass transition temperature of the resin.
[0073] In the modified resin, the modifying group containing at least one atom selected from the group consisting of nitrogen atom, oxygen atom, fluorine atom and chlorine atom is not particularly limited as long as it is a group containing at least one atom of nitrogen atom, oxygen atom, fluorine atom and chlorine atom. Among them, a group containing at least one atom of nitrogen atom and oxygen atom is preferable.
[0074] Specific examples of the modified group include a group represented by SiOR (R is a hydrogen atom or a hydrocarbon group), an amino group, an amide group, a silyl group, an alkoxysilyl group, an isocyanate group, an imino group, an imidazole group, a urea group, an ether group, a carbonyl group, an oxycarbonyl group, a mercapto group, a sulfonyl group, a sulfinyl group, a thiocarbonyl group, an ammonium group, an imide group, a hydrazo group, an azo group, a diazo group, a carboxyl group, a nitrile group, a pyridyl group, an alkoxy group, a hydroxyl group, an oxy group, and an epoxy group. The functional group may have a substituent. The functional group may be one type or two or more types.
[0075] Among these, the modifying group is preferably a group represented by SiOR (R is a hydrogen atom or a hydrocarbon group), which may have a substituent, an alkoxysilyl group, an amino group, a hydroxyl group, an epoxy group, or a carboxyl group.
[0076] The group represented by SiOR includes SiOH and SiOR (R is a hydrocarbon group). The hydrocarbon group of R preferably has 1 to 12 carbon atoms, more preferably 1 to 6 carbon atoms, and even more preferably 1 to 4 carbon atoms. The hydrocarbon group may be linear, branched, or cyclic. Examples of the hydrocarbon group of R include alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, iso-butyl, sec-butyl, tert-butyl, pentyl, and hexyl groups.
[0077] The alkoxysilyl group is -Si(OR 1 ) k (R 2 ) 3-k A group represented by R 1 ~R 2 represents hydrogen or a hydrocarbon group and may be the same or different. k represents an integer of 1, 2 or 3. 1 ~R 2 The number of carbon atoms in the hydrocarbon group is preferably 1 to 12, more preferably 1 to 8, and still more preferably 1 to 4. Specific examples of the unsubstituted or substituted alkoxysilyl group include monoalkoxysilyl groups (monomethoxysilyl group, monoethoxysilyl group, monopropoxysilyl group, monobutoxysilyl group, etc.), dialkoxysilyl groups (dimethoxysilyl group, diethoxysilyl group, dipropoxysilyl group, dibutoxysilyl group, etc.), trialkoxysilyl groups (trimethoxysilyl group, triethoxysilyl group, tripropoxysilyl group, tributoxysilyl group, etc.), methyldimethoxysilyl group, methyldiethoxysilyl group, dimethylethoxysilyl group, aminoalkoxysilyl group, etc.
[0078] The amino group includes primary amino groups (-NH2), secondary amino groups (-NHR 11 ), tertiary amino group (-NR 12 R 13), where R 11 ~R 13 R is any organic group, which may be linked to form a ring. As described above, the amino group may have a substituent. 11 ~R 13 The number of carbon atoms is preferably 1 to 12, more preferably 1 to 6, and further preferably 1 to 4. Specific examples of the unsubstituted or substituted amino group include mono-C groups such as a primary amino group (-NH2), an amino group, and an alkylamino group (a methylamino group, an ethylamino group, a propylamino group, an isopropylamino group, and a butylamino group). 1-4 alkylamino group), dialkylamino group (dimethylamino group, diethylamino group, dipropylamino group, diisopropylamino group, dibutylamino group, methylethylamino group, etc.) 1-4 alkylamino group), alkoxycarbonylamino group (e.g., methoxycarbonylamino group, isoproxycarbonylamino group, tert-butoxycarbonylamino group, etc. 1-6 alkoxycarbonylamino groups, and the like.
[0079] For the introduction of the modifying group, any compound capable of introducing the modifying group can be used, and examples thereof include compounds represented by the following formula.
[0080] [ka] (In the formula, R 1 , R 2 and R 3 R may be the same or different and represents an alkyl group, an alkoxy group, a silyloxy group, an acetal group, a carboxyl group (-COOH), a mercapto group (-SH), or a derivative thereof. 4 and R 5 R may be the same or different and represents a hydrogen atom or an alkyl group. 4 and R 5 may be bonded to form a ring structure together with the nitrogen atom, and n represents an integer.
[0081] R 1 , R 2 and R 3R is preferably an alkoxy group (preferably an alkoxy group having 1 to 8 carbon atoms, more preferably an alkoxy group having 1 to 4 carbon atoms). 4 and R 5 is preferably an alkyl group (preferably an alkyl group having 1 to 3 carbon atoms). n is preferably 1 to 5, more preferably 2 to 4, and further preferably 3. In addition, R 4 and R 5 When the nitrogen atom and the nitrogen atom are bonded to each other to form a ring structure, the ring is preferably a 4- to 8-membered ring. The alkoxy group also includes a cycloalkoxy group (such as a cyclohexyloxy group) and an aryloxy group (such as a phenoxy group and a benzyloxy group).
[0082] Specific examples of the compound represented by the formula include 2-dimethylaminoethyl trimethoxysilane, 3-dimethylaminopropyl trimethoxysilane, 2-dimethylaminoethyl triethoxysilane, 3-dimethylaminopropyl triethoxysilane, 2-diethylaminoethyl trimethoxysilane, 3-diethylaminopropyl trimethoxysilane, 2-diethylaminoethyl triethoxysilane, 3-diethylaminopropyl triethoxysilane, etc. Among them, 3-dimethylaminopropyl trimethoxysilane, 3-dimethylaminopropyl triethoxysilane, and 3-diethylaminopropyl trimethoxysilane are preferred. These may be used alone or in combination of two or more.
[0083] Other compounds into which the modifying group can be introduced include the following compounds. Ethylenically unsaturated silane compounds such as vinyltrimethoxysilane, vinyltriethoxysilane, allyltrimethoxysilane, allyltriethoxysilane, dimethoxymethylvinylsilane, diethoxymethylvinylsilane, p-styryltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, and 3-acryloxypropyltrimethoxysilane;
[0084] Polyglycidyl ethers of polyhydric alcohols such as ethylene glycol diglycidyl ether, glycerin triglycidyl ether, trimethylolethane triglycidyl ether, and trimethylolpropane triglycidyl ether; polyglycidyl ethers of aromatic compounds having two or more phenol groups such as diglycidylated bisphenol A; polyepoxy compounds such as 1,4-diglycidylbenzene, 1,3,5-triglycidylbenzene, and polyepoxidized liquid polybutadiene; 4,4'-diglycidyl -diphenylmethylamine, 4,4'-diglycidyl-dibenzylmethylamine, and other epoxy group-containing tertiary amines; diglycidylamino compounds such as diglycidylaniline, N,N'-diglycidyl-4-glycidyloxyaniline, diglycidylorthotoluidine, tetraglycidylmetaxylenediamine, tetraglycidylaminodiphenylmethane, tetraglycidyl-p-phenylenediamine, diglycidylaminomethylcyclohexane, and tetraglycidyl-1,3-bisaminomethylcyclohexane;
[0085] Amino group-containing acid chlorides such as bis-(1-methylpropyl)carbamic acid chloride, 4-morpholinecarbonyl chloride, 1-pyrrolidinecarbonyl chloride, N,N-dimethylcarbamic acid chloride, and N,N-diethylcarbamic acid chloride; epoxy group-containing silane compounds such as 1,3-bis-(glycidyloxypropyl)-tetramethyldisiloxane and (3-glycidyloxypropyl)-pentamethyldisiloxane;
[0086] Sulfide group-containing silane compounds such as (trimethylsilyl)[3-(trimethoxysilyl)propyl]sulfide, (trimethylsilyl)[3-(triethoxysilyl)propyl]sulfide, (trimethylsilyl)[3-(tripropoxysilyl)propyl]sulfide, (trimethylsilyl)[3-(tributoxysilyl)propyl]sulfide, (trimethylsilyl)[3-(methyldimethoxysilyl)propyl]sulfide, (trimethylsilyl)[3-(methyldiethoxysilyl)propyl]sulfide, (trimethylsilyl)[3-(methyldipropoxysilyl)propyl]sulfide, and (trimethylsilyl)[3-(methyldibutoxysilyl)propyl]sulfide;
[0087] N-substituted aziridine compounds such as ethyleneimine and propyleneimine; alkoxysilanes such as methyltriethoxysilane; (thio)benzophenone compounds having amino groups and / or substituted amino groups such as 4-N,N-dimethylaminobenzophenone, 4-N,N-di-t-butylaminobenzophenone, 4-N,N-diphenylaminobenzophenone, 4,4'-bis(dimethylamino)benzophenone, 4,4'-bis(diethylamino)benzophenone, 4,4'-bis(diphenylamino)benzophenone, and N,N,N',N'-bis-(tetraethylamino)benzophenone; 4-N,N-dimethylaminobenzaldehyde, 4-N,N-diphenylaminobenzaldehyde, 4- benzaldehyde compounds having an amino group and / or a substituted amino group, such as N,N-divinylaminobenzaldehyde; N-substituted pyrrolidones, such as N-methyl-2-pyrrolidone, N-vinyl-2-pyrrolidone, N-phenyl-2-pyrrolidone, Nt-butyl-2-pyrrolidone, and N-methyl-5-methyl-2-pyrrolidone; N-substituted piperidones, such as N-methyl-2-piperidone, N-vinyl-2-piperidone, and N-phenyl-2-piperidone; N-substituted lactams, such as N-methyl-ε-caprolactam, N-phenyl-ε-caprolactam, N-methyl-ω-laurylolactam, N-vinyl-ω-laurylolactam, N-methyl-β-propiolactam, and N-phenyl-β-propiolactam;
[0088] N,N-Bis-(2,3-epoxypropoxy)-aniline, 4,4-methylene-bis-(N,N-glycidylaniline), tris-(2,3-epoxypropyl)-1,3,5-triazine-2,4,6-triones, N,N-diethylacetamide, N-methylmaleimide, N,N-diethylurea, 1,3-dimethylethyleneurea, 1,3-divinylethyleneurea, 1,3-diethyl-2-imidazolidinone, 1-methyl-3-ethyl-2-imidazolidinone, 4-N,N-dimethylaminoacetophene, 4-N,N-diethylaminoacetophenone, 1,3-bis(diphenylamino)-2-propanone, 1,7-bis(methylethylamino)-4-heptanone;
[0089] Ethylenediamine, 1,3-propanediamine, 1,4-butanediamine, 1,2-cyclohexanediamine, N-methylethylenediamine, N-methylpropanediamine, N,N-dimethylethylenediamine, N,N-dimethylpropanediamine, N-acetylethylenediamine, isophoronediamine;
[0090] 4-N,N-dimethylaminoethylstyrene, 3-N,N-dimethylaminoethylstyrene, 4-N,N-diethylaminoethylstyrene, 3-N,N-diethylaminoethylstyrene, 4-N,N-di-n-propylaminoethylstyrene, 3-N,N-di-n-propylaminoethylstyrene, 4-N,N-di-n-butylaminoethylstyrene, 3-N,N-di-n-butylaminoethylstyrene, 4-N,N-diallylaminoethylstyrene, 3-N,N-diallylaminoethylstyrene, 4-N,N-bis(trimethylsilyl)aminoethylstyrene, 3-N,N-bis(trimethylsilyl)aminoethylstyrene, 4-N,N-bis(tert-butyldimethylsilyl)aminoethylstyrene, 3-N,N-bis(tert-butyldimethylsilyl)aminoethylstyrene, 4-aziridinylethylstyrene, 3-aziridinylethylstyrene, 4-pyrrolidinylethylstyrene, 3-pyrrolidinylethylstyrene, 4-piperidinylethylstyrene, 3-piperidinylethylstyrene, 4-hexamethyleneiminoethylstyrene, 3-hexamethyleneiminoethylstyrene;
[0091] The modified resin having the functional group can be produced by a known method. Specifically, examples of the method for imparting the modifying group to a resin constituting the skeleton include, but are not limited to, a method in which a monomer having the modifying group is copolymerized during polymerization of the resin to introduce the modifying group into the terminal and / or main chain, and a method in which a compound having the modifying group is added to a resin after polymerization or a commercially available resin to introduce the modifying group.
[0092] Specifically, the following methods can be mentioned, but the method is not limited to these. (1) The compound having the modifying group has an unsaturated bond and is added to the resin ionically and / or radically. (2) A radical generator such as a peroxide compound is allowed to react with the compound having the modifying group to add it to the resin. (3) The resin has a functional group such as a carboxyl group or a hydroxyl group, and is further reacted with a compound having the modifying group to introduce the desired modifying group into the resin. (4) When polymerizing the resin, a monomer having the modifying group is copolymerized.
[0093] Examples of plasticizers that can be used include products from Maruzen Petrochemical Co., Ltd., Sumitomo Bakelite Co., Ltd., Yasuhara Chemical Co., Ltd., Tosoh Corporation, Rutgers Chemicals, BASF, Arizona Chemical Company, Nitto Chemical Co., Ltd., Nippon Shokubai Co., Ltd., ENEOS Corporation, Arakawa Chemical Industries, Ltd., and Taoka Chemical Co., Ltd.
[0094] From the viewpoints of crack resistance, ozone resistance, and the like, the rubber composition for cap tread preferably contains an antioxidant.
[0095] The antiaging agent is not particularly limited, and examples thereof include naphthylamine-based antiaging agents such as phenyl-α-naphthylamine; diphenylamine-based antiaging agents such as octylated diphenylamine and 4,4'-bis(α,α'-dimethylbenzyl)diphenylamine; N-isopropyl-N'-phenyl-p-phenylenediamine, N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, N,N'-di-2-naphthyl-p-phenylenediamine, Examples of the antioxidant include p-phenylenediamine antioxidants such as amines; quinoline antioxidants such as polymerized 2,2,4-trimethyl-1,2-dihydroquinoline; monophenol antioxidants such as 2,6-di-t-butyl-4-methylphenol and styrenated phenol; and bis, tris, and polyphenol antioxidants such as tetrakis-[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane. Among these, p-phenylenediamine antioxidants and quinoline antioxidants are preferred, and N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine and polymerized 2,2,4-trimethyl-1,2-dihydroquinoline are more preferred. Commercially available products include, for example, products from Seiko Chemical Co., Ltd., Sumitomo Chemical Co., Ltd., Ouchi Shinko Chemical Co., Ltd., and Flexis Co., Ltd.
[0096] In the rubber composition for cap tread, the content of the antioxidant is preferably 0.2 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 2.0 parts by mass or more, based on 100 parts by mass of the rubber component. The content is preferably 7.0 parts by mass or less, and more preferably 4.0 parts by mass or less.
[0097] The rubber composition for the cap tread preferably contains stearic acid. In the rubber composition for cap tread, the content of stearic acid is preferably 0.5 to 10 parts by mass, and more preferably 0.5 to 4 parts by mass, based on 100 parts by mass of the rubber component.
[0098] As the stearic acid, any conventionally known product can be used, for example, products available from NOF Corp., Kao Corp., Fujifilm Wako Pure Chemical Industries, Ltd., Chiba Fatty Acid Co., Ltd., and the like.
[0099] The rubber composition for a cap tread preferably contains zinc oxide. In the rubber composition for cap tread, the content of zinc oxide is preferably 0.5 to 10 parts by mass, and more preferably 1 to 3 parts by mass, based on 100 parts by mass of the rubber component.
[0100] As the zinc oxide, any known zinc oxide can be used, for example, products available from Mitsui Mining & Smelting Co., Ltd., Toho Zinc Co., Ltd., Hakusui Tech Co., Ltd., Seido Chemical Industry Co., Ltd., Sakai Chemical Industry Co., Ltd., etc.
[0101] The rubber composition for the cap tread may contain wax. In the rubber composition for cap tread, the content of the wax is preferably 0.5 to 10 parts by mass, and more preferably 1 to 5 parts by mass, based on 100 parts by mass of the rubber component.
[0102] The wax is not particularly limited, and examples thereof include petroleum waxes, natural waxes, etc. Also, synthetic waxes obtained by refining or chemically treating multiple waxes can be used. These waxes may be used alone or in combination of two or more kinds.
[0103] Examples of petroleum waxes include paraffin wax and microcrystalline wax. Examples of natural waxes are not particularly limited as long as they are derived from resources other than petroleum, and include, for example, vegetable waxes such as candelilla wax, carnauba wax, Japan wax, rice wax, and jojoba wax; animal waxes such as beeswax, lanolin, and spermaceti; mineral waxes such as ozokerite, ceresin, and petrolactam; and refined products thereof. Examples of commercially available products include products from Ouchi Shinko Chemical Industry Co., Ltd., Nippon Seiro Co., Ltd., and Seiko Chemical Co., Ltd.
[0104] It is preferable to compound sulfur into the rubber composition for cap tread in order to form an appropriate amount of crosslinked chains in the polymer chains and to impart good performance.
[0105] In the rubber composition for cap tread, the content of sulfur is preferably 0.1 parts by mass or more, more preferably 1.0 parts by mass or more, and even more preferably 1.7 parts by mass or more, based on 100 parts by mass of the rubber component. The content is preferably 5.0 parts by mass or less, more preferably 3.0 parts by mass or less, and even more preferably 2.0 parts by mass or less.
[0106] Examples of sulfur include powdered sulfur, precipitated sulfur, colloidal sulfur, insoluble sulfur, highly dispersible sulfur, soluble sulfur, etc., which are commonly used in the rubber industry. Commercially available products include those from Tsurumi Chemical Industry Co., Ltd., Karuizawa Sulfur Co., Ltd., Shikoku Chemical Industry Co., Ltd., Flexis Corporation, Nippon Kanzuri Kogyo Co., Ltd., Hosoi Chemical Industry Co., Ltd., etc. These may be used alone or in combination of two or more kinds.
[0107] The rubber composition for a cap tread preferably contains a vulcanization accelerator. In the rubber composition for cap tread, the content of the vulcanization accelerator is not particularly limited and may be freely determined according to the desired vulcanization speed and crosslink density, but it is preferably 0.5 parts by mass or more, more preferably 2.0 parts by mass or more, and even more preferably 2.7 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit is preferably 8.0 parts by mass or less, more preferably 6.0 parts by mass or less, and even more preferably 5.0 parts by mass or less.
[0108] The type of vulcanization accelerator is not particularly limited, and commonly used ones can be used. Examples of the vulcanization accelerator include thiazole-based vulcanization accelerators such as 2-mercaptobenzothiazole, di-2-benzothiazolyl disulfide, and N-cyclohexyl-2-benzothiazyl sulfenamide; thiuram-based vulcanization accelerators such as tetramethylthiuram disulfide (TMTD), tetrabenzylthiuram disulfide (TBzTD), and tetrakis(2-ethylhexyl)thiuram disulfide (TOT-N); sulfenamide-based vulcanization accelerators such as N-cyclohexyl-2-benzothiazole sulfenamide, Nt-butyl-2-benzothiazolyl sulfenamide, N-oxyethylene-2-benzothiazole sulfenamide, and N,N'-diisopropyl-2-benzothiazole sulfenamide; and guanidine-based vulcanization accelerators such as diphenylguanidine, di-orthotolyl guanidine, and orthotolyl biguanidine. These may be used alone or in combination of two or more. Among them, sulfenamide-based, guanidine-based and benzothiazole-based vulcanization accelerators are preferred.
[0109] In addition to the above-mentioned components, the rubber composition for cap tread may contain compounding agents generally used in the tire industry, such as materials such as a mold release agent, as appropriate.
[0110] The rubber composition for cap treads can be produced by a known method, for example, by kneading the above-mentioned components using a rubber kneading device such as an open roll or a Banbury mixer, and then vulcanizing the mixture.
[0111] As for the kneading conditions, in the base kneading step in which additives other than the vulcanizing agent and the vulcanization accelerator are kneaded, the kneading temperature is usually 50 to 200°C, preferably 80 to 190°C, and the kneading time is usually 30 seconds to 30 minutes, preferably 1 minute to 30 minutes. In the finish kneading step in which the vulcanizing agent and the vulcanization accelerator are kneaded, the kneading temperature is usually 100°C or lower, preferably room temperature to 80°C. Furthermore, the composition kneaded with the vulcanizing agent and the vulcanization accelerator is usually subjected to a vulcanization treatment such as press vulcanization. The vulcanization temperature is usually 120 to 200°C, preferably 140 to 180°C.
[0112] In the rubber composition for cap treads, the ratio (St / Ic) of the total styrene amount St (mass%) in 100% by mass of the rubber component to the isoprene-based rubber content Ic (mass%) in 100% by mass of the rubber component is desirably 2.0 or less. St / Ic is preferably 1.0 or less, more preferably 0.9 or less, and even more preferably 0.8 or less. The lower limit of St / Ic is not particularly limited, but is preferably 0.2 or more, more preferably 0.5 or more, and even more preferably 0.7 or more. Within the above range, the effect tends to be better.
[0113] The mechanism by which a greater effect is obtained when St / Ic is adjusted to the above range, particularly to 1.0 or less, is not clear, but is presumed to be as follows. By blending isoprene-based rubber with a diene-based rubber, it is possible to control the structure of the incompatible phase, thereby enhancing the reinforcing properties with the filler, which is thought to lead to improved abrasion resistance in particular.
[0114] The rubber composition for cap tread has a total styrene content St (mass%) in 100% by mass of the rubber component of preferably 10.0% by mass or more, more preferably 11.0% by mass or more, even more preferably 12.0% by mass or more, and particularly preferably 12.5% by mass or more. The upper limit of the total styrene content is preferably 18.1% by mass or less, more preferably 16.2% by mass or less, even more preferably 15.0% by mass or less, and particularly preferably 13.9% by mass or less. Within the above range, the effect tends to be better obtained.
[0115] The mechanism by which a greater effect is obtained when the total styrene amount St is adjusted to the above range, particularly to 15.0 mass % or less, is not clear, but is presumed to be as follows. By keeping the total styrene amount at a certain value or less, it is possible to improve the incompatibility of diene rubber and suppress heat build-up in the rubber composition, which is believed to lead in particular to improved fuel economy.
[0116] Here, the total styrene content in 100% by mass of the rubber component is the total content of styrene parts contained in the entire rubber component (unit: mass%), and can be calculated by Σ (content of each rubber component × styrene content in each rubber component / 100). For example, in a case where 100% by mass of the rubber component contains 85% by mass of SBR with a styrene content of 40% by mass, 5% by mass of SBR with a styrene content of 25% by mass, and 10% by mass of BR with a styrene content of 0% by mass, the total styrene content in the rubber component is 35.25% by mass (=85×40 / 100+5×25 / 100+10×0 / 100).
[0117] The ratio (Sc / AE) of the silica content Sc (parts by mass) per 100 parts by mass of the rubber component of the rubber composition for cap tread to the acetone extract amount AE (% by mass) of the rubber composition for cap tread is preferably 1.5 or more, more preferably 1.7 or more, even more preferably 1.9 or more, and particularly preferably 2.5 or more. The upper limit of Sc / AE is not particularly limited, but is preferably 6.0 or less, more preferably 5.0 or less, and even more preferably 4.0 or less. Within the above range, the effect tends to be better obtained.
[0118] The mechanism by which better effects are obtained when Sc / AE is adjusted to the above range, particularly to 1.9 or more, is not clear, but is presumed to be as follows. By keeping the ratio of the silica content to the acetone extractable amount at or below a certain level, the dispersibility of silica in the rubber composition can be improved and uneven distribution of silica can be suppressed, and the formation of agglomerates that serve as the starting point for fracture can be prevented, which is thought to lead to improved abrasion resistance in particular.
[0119] The rubber composition for cap tread has an acetone extract amount AE (mass%) of preferably 12.0 or more, more preferably 14.0 or more, and even more preferably 15.0 or more. The upper limit of AE is not particularly limited, but is preferably 38.5 or less, more preferably 34.5 or less, even more preferably 32.5 or less, and particularly preferably 28.0 or less. Within the above range, the effect tends to be better obtained.
[0120] The mechanism by which a greater effect is obtained when the acetone extractable amount AE is adjusted to the above range, particularly to 32.5 mass % or less, is not clear, but is presumed to be as follows. By keeping the amount of acetone extraction below a certain level, it is possible to suppress the seepage of plasticizer and ensure the hardness of the cap portion, which is thought to lead to improved abrasion resistance in particular. Another possible mechanism is that by blending a certain amount or less of a resin or other component, the silica becomes more soluble in the polymer, making it possible to fix the uneven distribution of silica, which is thought to lead to improved abrasion resistance.
[0121] In the present invention, the acetone extractable amount AE is measured for a vulcanized rubber composition (sample) by a method for measuring an acetone extractable amount in accordance with JIS K 6229:2015 (unit: mass % in the vulcanized rubber composition (sample)).
[0122] The acetone extractable amount (AE) can be adjusted by any method known to those skilled in the art. For example, the AE tends to increase when the amount of a plasticizer such as oil in the rubber composition increases.
[0123] Examples of tires to which the present invention can be applied include pneumatic tires and non-pneumatic tires, among which pneumatic tires are preferred. In particular, the present invention can be suitably used as summer tires (summer tires), winter tires (studless tires, snow tires, studded tires, etc.), and all-season tires. The tires can be used as passenger car tires, large passenger car tires, large SUV tires, heavy load tires such as trucks and buses, light truck tires, two-wheeled vehicle tires, and racing tires (high performance tires). In particular, the present invention can be suitably used as all-season tires. It is preferable that: An all-season tire is a tire that can be used in all seasons, including spring, summer, autumn, and winter, and can be used on any road surface, including dry road surfaces, wet road surfaces, icy road surfaces, and snowy road surfaces. The road surface temperature can be, for example, from -20°C to 100°C.
[0124] The tire can be manufactured by a conventional method. For example, each component such as a cap tread is prepared in an unvulcanized state by a known method, and each component is molded by a conventional method on a tire building machine to form an unvulcanized tire. The unvulcanized tire is heated and pressurized in the vulcanizer to obtain a tire.
[0125] The tire includes a cap tread formed from the rubber composition for cap tread, and the ratio (Sc / Tt) of the silica content Sc (parts by mass) per 100 parts by mass of the rubber component in the rubber composition for cap tread to the tread thickness Tt (mm) satisfies 5.0 or more. Sc / Tt is preferably 6.0 or more, more preferably 7.3 or more, and even more preferably 7.8 or more. The upper limit of Sc / Tt is not particularly limited, but is preferably 13.0 or less, more preferably 10.7 or less, even more preferably 10.0 or less, and particularly preferably 9.4 or less. Within the above range, the effect tends to be better obtained.
[0126] The tread thickness Tt is preferably 5.0 mm or more, more preferably 7.0 mm or more, even more preferably 8.0 mm or more, and is preferably 12.0 mm or less, more preferably 11.0 mm or less, even more preferably 10.0 mm or less. Within the above ranges, the effect tends to be better obtained.
[0127] In the tire, the product (St×Tt) of the total styrene amount St (mass %) in 100% by mass of the rubber component of the rubber composition for cap tread and the tread thickness Tt (mm) is desirably 145 or less. St × Tt is preferably 120 or less, more preferably 113 or less, even more preferably 108 or less, and particularly preferably 102 or less. There is no particular restriction on the lower limit of St × Tt, but it is preferably 75 or more, more preferably 85 or more, and even more preferably 89 or more. Within the above range, the effect tends to be better obtained.
[0128] The mechanism by which a greater effect is obtained when St×Tt is adjusted to the above range, particularly to 120 or less, is not clear, but is presumed to be as follows. By lowering the total styrene content in 100% by mass of the rubber component and reducing the tread thickness, it is possible to improve the compatibility of diene rubber, as well as reduce the heat generated by the movement of polymer chains and inhibit the accumulation of the generated heat, which is believed to lead to improved fuel efficiency in particular.
[0129] In the tire, the product (AE×Tt) of the acetone extractable amount AE (mass %) in 100 mass % of the rubber component of the rubber composition for cap tread and the tread thickness Tt (mm) is desirably 300 or less. AE×Tt is preferably 276 or less, more preferably 260 or less, even more preferably 244 or less, and particularly preferably 224 or less. There is no particular restriction on the lower limit of AE×Tt, but it is preferably 80 or more, more preferably 100 or more, and even more preferably 105 or more. Within the above range, the effect tends to be better obtained.
[0130] The mechanism by which a greater effect is obtained when AE×Tt is adjusted to the above range, particularly to 300 or less, is not clear, but is presumed to be as follows. The thicker the tread, the greater the centrifugal force acting on the cap section. Therefore, by keeping the product of the amount of acetone extracted and the tread thickness below a certain level, it is believed that the outflow of acetone extractables from the cap section can be suppressed, which will lead to improved abrasion resistance in particular. In addition, as a mechanism other than the above, it is believed that adding a certain amount of resin or other components improves the dispersibility of silica, leading to improved wear resistance. Furthermore, it is believed that reducing the tread thickness can also suppress the deterioration of low heat generation.
[0131] In this specification, "tread thickness (Tt)" means the thickness of the tread on the tire equatorial plane in the tire radial cross section. The tread thickness on the tire equatorial plane is a value measured from the outermost surface of the tread on the tire equatorial plane along the tire equatorial plane. And, Tt is the straight-line distance from the tread surface to the interface of the reinforcing layer containing other fiber materials such as the belt layer and the carcass layer on the tire radial outermost surface side in the tire radial cross section of the tire, and in the case where the tread has grooves on the equatorial plane, it is the straight-line distance from the intersection of the straight line connecting the ends of the grooves on the outermost surface side in the tire radial direction and the tire equatorial plane.
[0132] In the tire, the groove depth D of the circumferential groove formed in the tread is preferably 15 mm or less, more preferably 10 mm or less, and even more preferably 8 mm or less. The lower limit of D is preferably 2 mm or more, more preferably 3 mm or more, and even more preferably 5 mm or more. Within the above range, the effect tends to be better obtained.
[0133] In the tire, the product (Sc×D) of the silica content Sc (parts by mass) per 100 parts by mass of the rubber component of the rubber composition for cap tread and the groove depth D (mm) of the circumferential groove formed in the tread is preferably 400 or more, more preferably 450 or more, even more preferably 500 or more, and particularly preferably 525 or more. The upper limit of Sc×D is not particularly limited, but is preferably 3000 or less, more preferably 1500 or less, even more preferably 960 or less, and particularly preferably 700 or less. Within the above range, the effect tends to be better obtained.
[0134] The mechanism by which a greater effect is obtained when Sc×D is adjusted to the above range, particularly to 450 or more, is not clear, but is presumed to be as follows. By setting the product of the silica content and the circumferential groove depth formed in the tread to a certain level or less, the large amount of silica suppresses the movement of the polymer and reduces the movement of the rubber at the contact area with the road surface, thereby reducing heat generation in the cap portion and improving fuel efficiency in particular.
[0135] In this specification, the groove depth D of the circumferential groove means the distance measured along the normal to the extension of the surface forming the contact surface of the outermost tread surface, from the extension of the surface forming the contact surface to the deepest groove bottom, and refers to the maximum distance among the groove depths of the circumferential grooves provided.
[0136] In this specification, unless otherwise specified, the dimensions of each part of the tire are values measured under normal conditions. In this specification, the term "normal condition" refers to a condition in which the tire is mounted on a normal rim (not shown), inflated to normal internal pressure, and no load is applied.
[0137] When it is not possible to measure with the tire mounted on a regular rim, the dimensions and angles of each part in the meridian section of the tire are measured by cutting the tire along a plane including the axis of rotation, and the distance between the left and right beads in the cross section is measured so that it corresponds to the distance between the beads of the tire mounted on a regular rim.
[0138] "Genuine rim" refers to the rim that is specified for each tire by the standard system that includes the standard on which the tire is based, for example, "Standard rim" in the applicable size listed in the "JATMA YEAR BOOK" for JATMA (Japan Automobile Tire Manufacturers Association), "Measuring Rim" in the "STANDARDS MANUAL" for ETRTO (The European Tire and Rim Technical Organisation), and "Design Rim" in the "YEAR BOOK" for TRA (The Tire and Rim Association, Inc.). Refer to JATMA, ETRTO, and TRA in that order, and follow the standard if there is an applicable size at the time of reference. In the case of a tire not specified in the standard, it refers to the rim that can be assembled to the rim and can hold internal pressure, that is, the rim with the smallest rim diameter and the next narrowest rim width among the rims that do not leak air from between the rim and tire.
[0139] "Regular internal pressure" refers to the air pressure specified for each tire by each standard in the standard system including the standard on which the tire is based. For JATMA, it refers to the "Maximum Air Pressure", for ETRTO, it refers to the "INFLATION PRESSURE", and for TRA, it refers to the maximum value listed in the table "TIRE LOAD LIMITS AT VARIOUS COLD INFLATION PRESSURES". As with "regular rims", it refers to JATMA, ETRTO, TRA in that order and follows those standards. For tires not specified in the standard, it refers to the regular internal pressure (250kPa or more) of another tire size (specified in the standard) that is specified with the regular rim as the standard rim. Note that if multiple regular internal pressures of 250kPa or more are specified, it refers to the smallest value among them.
[0140] In this specification, the term "normal load" refers to the load that is determined for each tire by each standard in the standard system including the standard on which the tire is based, and is the maximum load capacity in the case of JATMA, the "LOAD CAPACITY" in the case of ETRTO, and the maximum value listed in the table "TIRE LOAD LIMITS AT VARIOUS COLD INFLATION PRESSURES" in the case of TRA. As in the case of the "normal rim" and "normal internal pressure" mentioned above, JATMA, ETRTO, and TRA are referred to in that order and their standards are followed. In the case of a tire not determined by a standard, the normal load W is calculated as follows: L Request. V = {(Dt / 2) 2 -(Dt / 2-Ht) 2}×π×Wt W L =0.000011×V+175 W L :Normal load (kg) V: Virtual volume of the tire (mm 3 ) Dt: Tire outer diameter (mm) Ht: Section height of the tire (mm) Wt: tire section width (mm)
[0141] The "section width Wt (mm)" of a tire is the maximum width between the outer surfaces of the sidewalls when the tire is in its normal condition, excluding any patterns or lettering on the sidewalls.
[0142] The "outer diameter Dt (mm)" of a tire refers to the outer diameter of the tire under normal conditions.
[0143] The "section height Ht (mm)" of a tire refers to the radial height of the tire at its radial cross section, and corresponds to half the difference between the tire's outer diameter Dt and the rim diameter R, where R is the tire's rim diameter (mm). In other words, the section height Ht can be calculated by (Dt-R) / 2.
[0144] In addition, in this specification, the "aspect ratio" of a tire is the ratio of the tire's section height Ht (mm) to the tire's section width Wt (mm) expressed as a percentage, and can be calculated by Ht / Wt×100.
[0145] An example of a tire according to the present invention will be described below with reference to the drawings, but the present invention is not limited to this embodiment.
[0146] 1, the up-down direction is the radial direction of the tire 2, the left-right direction is the axial direction of the tire 2, and the direction perpendicular to the paper surface is the circumferential direction of the tire 2. The tire 2 is symmetrical. The tread 4 includes a cap layer 30 (cap tread) and a base layer 28 (base tread).
[0147] Although FIG. 1 shows an example of a two-layer tread 4 made up of a cap layer 30 and a base layer 28, a single-layer tread or a tread having a structure of three or more layers may also be used.
[0148] In the tire 2, each sidewall 6 extends radially inward from an end of the tread 4. A radially outer portion of the sidewall 6 is joined to the tread 4. A radially inner portion of the sidewall 6 is joined to a clinch 10 (clinch apex). The sidewall 6 can prevent damage to the carcass 14. In addition, when joining the sidewall 6 to the end of the tread 4, the radially outer end of the sidewall 6 may be joined in a manner that covers the radially outer side of the tread 4.
[0149] In the tire 2 of FIG. 1, the cap layer 30 is formed from the rubber composition for cap tread.
[0150] 1 is located between the tread 4 and the sidewall 6. The wing 8 is joined to the tread 4 and the sidewall 6, respectively.
[0151] Each clinch 10 is located approximately radially inward of the sidewall 6. Each clinch 10 is located axially outward of the beads 12 and the carcass 14.
[0152] Each bead 12 is located axially inward of the clinch 10. The bead 12 includes a core 32 and an apex 34 extending radially outward from the core 32. The core 32 is preferably ring-shaped and includes a wound non-stretchable wire. The apex 34 tapers radially outward.
[0153] The carcass 14 includes a carcass ply 36. In the tire 2, the carcass 14 is made up of one carcass ply 36, but may be made up of two or more carcass plies.
[0154] In the tire 2, the carcass ply 36 is laid between the beads 12 on both sides and extends along the tread 4 and the sidewall 6. The carcass ply 36 is folded back from the inside to the outside in the axial direction around each of the cores 32. By this folding back, the carcass ply 36 is formed with a main portion 36a and a pair of folded back portions 36b. That is, the carcass ply 36 includes the main portion 36a and a pair of folded back portions 36b.
[0155] Although not shown, the carcass ply 36 is preferably made of a number of parallel cords and a topping rubber. The absolute value of the angle that each cord makes with respect to the equator plane is preferably 75° to 90°. In other words, it is preferable that the carcass 14 has a radial structure.
[0156] The belt layer 16 in FIG. 1 is located radially inward of the tread 4. The belt layer 16 is laminated with the carcass 14. The belt layer 16 reinforces the carcass 14. The belt layer 16 is composed of an inner layer 38 and an outer layer 40. As is clear from FIG. 1, it is desirable that the width of the inner layer 38 is slightly larger than the width of the outer layer 40 in the axial direction. In this tire 2, the axial width of the belt layer 16 is preferably 0.6 times or more and 0.9 times or less of the cross-sectional width of the tire 2.
[0157] Although not shown, each of the inner layer 38 and the outer layer 40 is preferably made of a number of cords arranged in parallel and a topping rubber. In other words, the belt layer 16 includes a number of cords arranged in parallel. Each cord is inclined with respect to the equatorial plane. The general absolute value of the inclination angle is 10° or more and 35° or less. The inclination direction of the cords of the inner layer 38 with respect to the equatorial plane is opposite to the inclination direction of the cords of the outer layer 40 with respect to the equatorial plane.
[0158] The band 18 in Fig. 1 is located radially outside the belt layer 16. In the axial direction, the band 18 has a width equal to the width of the belt layer 16. The band 18 may also have a width greater than the width of the belt layer 16.
[0159] Although not shown, the band 18 is preferably made of a cord and a topping rubber. The cord is wound in a spiral shape. This band 18 has a so-called jointless structure. The cord extends substantially in the circumferential direction. The angle of the cord with respect to the circumferential direction is preferably 5° or less, and more preferably 2° or less. Since the belt layer 16 is restrained by the cord, lifting of the belt layer 16 is suppressed.
[0160] 1 constitute a reinforcing layer. The reinforcing layer may be constituted by the belt layer 16 alone.
[0161] FIG. 2 is an enlarged view of the vicinity of the tread 4 in FIG. The tire in Fig. 2 is a tire 2 having a groove 26 on the tire equatorial plane (CL). In this case, the tread thickness (Tt) is the thickness on the tire equatorial plane in a plane formed by a straight line connecting the ends of the grooves 26 on the tire radial outermost surface side in a radial cross section of the tire, and is a value measured along a normal to the tread surface 24 on the tire equatorial plane, and specifically, it refers to the linear distance in the tire radial direction from the straight line connecting the ends of the grooves 26 on the tire equatorial plane to the interface of the band 18 on the tire outermost surface side.
[0162] The inner liner 20 is located inside the carcass 14. The inner liner 20 is bonded to the inner surface of the carcass 14. A typical base rubber of the inner liner 20 is butyl rubber or halogenated butyl rubber. The inner liner 20 holds the internal pressure of the tire 2.
[0163] Each chafer 22 is located adjacent to a bead 12. In this embodiment, the chafer 22 is preferably made of fabric with rubber impregnated into the fabric. The chafer 22 may be integral with the clinch 10.
[0164] In the tire 2, the tread 4 has a main groove 42 as the groove 26. As shown in FIG. 1, a plurality of main grooves 42, specifically three main grooves 42, are formed in the tread 4. These main grooves 42 are arranged at intervals in the axial direction. The three main grooves 42 are formed in the tread 4, thereby forming four ribs 44 extending in the circumferential direction. In other words, the spaces between the ribs 44 constitute the main grooves 42.
[0165] Each of the main grooves 42 extends in the circumferential direction. The main grooves 42 are continuous in the circumferential direction without interruption. The main grooves 42 facilitate the drainage of water present between the road surface and the tire 2, for example, in rainy weather. Therefore, even if the road surface is wet, the tire 2 can make sufficient contact with the road surface.
[0166] 2D indicates the depth of the main groove 42 formed in the circumferential direction of the tread 4. As shown in FIG.
[0167] And for the tires 2 in FIGS. 1 and 2, the ratio (Sc / Tt) of the content Sc (parts by mass) of silica to 100 parts by mass of the rubber component in the cap layer 30 to the tread thickness Tt (mm) is 5.0 or more. Also, the tread thickness Tt, St×T, AE×Tt, the groove depth D of the circumferential groove formed in the tread, and Sc×D are preferably in the aforementioned ranges.
Examples
[0168] A tread formed from a rubber composition for a cap tread based on the various compounding materials shown below and a tire (size 195 / 65R15) composed of other rubber members were examined, and the examination results are shown in Table 1. Note that examples (Examples) considered preferable for implementation are shown, but the scope of the present invention is not limited to the examples.
[0169] SBR1 and a modified resin are produced by the following method.
[0170] <Production of SBR1> 600 mL of hexane, 75 g of 1,3-butadiene, 25 g of styrene, and 60 mL of tetrahydrofuran are charged into a nitrogen-substituted autoclave reactor and stirred at 40°C. After scavenging treatment by adding 0.5 mL of a 0.1 mol / L n-butyllithium / hexane solution each time, 4 mL of a 0.1 mol / L n-butyllithium / hexane solution is added, the stirring speed is set to 130 rpm, and the jacket temperature is set to 80°C and stirred. After confirming the formation of a polymer with Mw of 1,000,000 by GPC, the polymerization solution is poured into 4 L of ethanol, and the precipitate is recovered. After the obtained precipitate is dried by blowing, it is dried under reduced pressure at 80°C / 10 Pa or less until the loss on drying becomes 0.1% to obtain SBR1.
[0171] <Production of Modified Resin 1> Aluminum chloride and toluene are added to a glass flask purged with an inert gas, and styrene and α-methylstyrene are added dropwise. After that, an isoprene / toluene solution to which allyltriethoxysilane has been added by the slurry method is added dropwise to the reaction liquid, and water is added to the reaction liquid to stop the reaction. After repeating the process of removing the water layer by liquid separation, the organic layer obtained by liquid separation is dried with air to volatilize the toluene, and then dried under reduced pressure to obtain a modified styrene α-methylstyrene resin (modified resin 1).
[0172] <Production of Modified Resin 2> Aluminum chloride and toluene are added to a glass flask purged with an inert gas, and styrene and α-methylstyrene are added dropwise. After that, an isoprene / toluene solution to which 3-aminopropyltriethoxysilane has been added by the slurry method is added dropwise to the reaction liquid, and water is added to the reaction liquid to stop the reaction. After repeating the process of removing the water layer by liquid separation, the organic layer obtained by liquid separation is dried with air to volatilize the toluene, and then dried under reduced pressure to obtain a modified styrene α-methylstyrene resin (modified resin 2).
[0173] Various chemicals used in the examples and comparative examples will be collectively described below. NR:TSR20 SBR1: S-SBR produced by the above method (Tg: -50°C, styrene content: 25% by mass, vinyl content: 25% by mass, Mw: 1 million, non-oil extended) SBR2: Tufuden 3830 manufactured by Asahi Kasei Corporation (Tg: -30°C, styrene content: 35% by mass, vinyl content: 30% by mass, Mw: 420,000, contains 37.5 parts by mass of oil per 100 parts by mass of rubber solids) SBR3: N9541 manufactured by ZS Elastomers Co., Ltd. (Tg: -23°C (above -25°C), styrene content: 46% by mass, contains 37.5 parts by mass of oil per 100 parts by mass of rubber solids) BR: Buna CB24 manufactured by LANXESS (BR synthesized using a Nd-based catalyst, cis content: 96% by mass, vinyl content: 0.7% by mass) Carbon black: N134 (N2SA:148m) manufactured by Cabot Japan Co., Ltd. 2 / g) Silica 1: ZEOSIL 195GR (N2SA: 180m) manufactured by Solvay Japan Co., Ltd. 2 / g, average primary particle size: 18nm) Silica 2: ULTRASIL 9100GR (N2SA: 230m) manufactured by Evonik Degussa 2 / g, average primary particle diameter: 15nm) Silane coupling agent: Si266 (bis(3-triethoxysilylpropyl) disulfide) manufactured by Evonik Degussa Resin: SYLVARES SA85 manufactured by Arizona Chemical Company (α-methylstyrene resin (copolymer of α-methylstyrene and styrene), softening point: 85°C) Modified resin 1: Modified α-methylstyrene resin 1 produced by the above method Modified resin 2: Modified α-methylstyrene resin 2 produced by the above method Oil: H&R VIVATEC 500 (aromatic process oil) Zinc oxide: Zinc oxide No. 1 manufactured by Mitsui Mining & Smelting Co., Ltd. Anti-aging agent: Nocrac 6C (N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Processing aid: ULTRA-FLOW 440 (zinc fatty acid) from Performance Additives Stearic acid: NOF Corporation's "Tsubaki" stearic acid Wax: Ozoace 0355 manufactured by Nippon Seiro Co., Ltd. Sulfur: Powdered sulfur manufactured by Tsurumi Chemical Industry Co., Ltd. Vulcanization accelerator 1: Noccelaer D (diphenyl guanidine) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Vulcanization accelerator 2: Noccela NS (N-tert-butyl-2-benzothiazolyl sulfenamide) manufactured by Ouchi Shinko Chemical Industry Co., Ltd.
[0174] <Production of test tires> According to the formulation in Table 1, materials other than sulfur and vulcanization accelerator are kneaded to obtain a kneaded mixture. To the kneaded mixture, sulfur and a vulcanization accelerator are added according to the formulation in Table 1, and the mixture is kneaded at 70° C. for 8 minutes to obtain an unvulcanized rubber composition. The unvulcanized rubber composition is extruded into a cap layer shape, and is laminated together with other tire components on a tire building machine to form an unvulcanized tire. The unvulcanized tire is press-vulcanized at 170° C. for 20 minutes to obtain a test tire (size 195 / 65R15, specifications: Table 1) shown in FIGS. 1 and 2.
[0175] The results are shown in Table 1, which are calculated based on the following evaluation method assuming a test tire obtained from a composition whose formulation is changed according to Table 1. The reference comparative examples are as follows. Table 1: Comparative Example 2
[0176] <Acetone extractables (AE)> A 300 mg rubber test piece is taken from the cap tread of the test tire. The amount of acetone extractable material (mass%) contained in the rubber test piece is measured using the acetone extractable amount measurement method in accordance with JIS K 6229:2015. Amount of acetone extractables (mass%) = (mass of sample before extraction - mass of sample after extraction) / mass of sample before extraction × 100
[0177] <Fuel-efficient> Using a rolling resistance tester, the rolling resistance of each test tire was measured when it was run at a speed of 80 km / h, and the rolling resistance was expressed as an index with the reference comparative example being set at 100. The higher the index, the lower the rolling resistance and the better the fuel economy.
[0178] <Grip performance on icy and snowy roads> The test tires are mounted on a domestically manufactured FF vehicle and the vehicle is driven on an ice-covered test course. The reciprocal of the braking distance is expressed as an index, with the standard comparison example being set at 100. The higher the index, the shorter the braking distance and the better the performance on snow and ice. (Grip performance index on snowy and icy roads) = (braking distance of standard comparative example) / (braking distance of each test tire) x 100
[0179] <Wear resistance> The test tires were fitted to a domestically produced FF vehicle, and the tire tread depth was measured after 8,000 km of driving. The distance traveled when the tire groove depth was reduced by 1 mm was calculated and indexed using the following formula. The higher the index, the better the wear resistance. (Wear resistance index) = (travel distance when the tread depth of each test tire is reduced by 1 mm) / (travel distance when the tread depth of the reference comparative tire is reduced by 1 mm) × 100
[0180] <Overall performance> The overall performance of fuel economy, wear resistance, and performance on snow and ice is evaluated based on the sum of the three indices obtained from the evaluation of fuel economy, grip performance on snow and ice, and wear resistance. The higher the value, the better the overall performance.
[0181] [Table 1]
[0182] The present invention (1) is a tire having a cap tread formed of a rubber composition including a rubber component, a filler including silica, and a resin, the resin contains a modified resin having a modifying group containing at least one atom selected from the group consisting of a nitrogen atom, an oxygen atom, a fluorine atom, and a chlorine atom, The tire has a ratio (Sc / Tt) of the content Sc (parts by mass) of the silica per 100 parts by mass of the rubber component to a tread thickness Tt (mm) of 5.0 or more.
[0183] The present invention (2) is characterized in that the content Ic (mass%) of the isoprene-based rubber in 100 mass% of the rubber component is 15 to 45 mass%, The tire according to the present invention (1), wherein the ratio (St / Ic) of the total styrene amount St (mass%) in 100% by mass of the rubber component to the isoprene-based rubber content Ic (mass%) in 100% by mass of the rubber component is 1.0 or less.
[0184] The present invention (3) is the tire according to the present invention (1) or (2), wherein the rubber component contains a styrene-butadiene rubber having a glass transition temperature (Tg) of −25° C. or lower.
[0185] The present invention (4) is a tire in any combination with any of the present inventions (1) to (3) in which the Sc / Tt is 7.8 or more.
[0186] The present invention (5) is a tire in any combination with any of the present inventions (1) to (4), in which the total styrene amount St (mass %) in 100 mass % of the rubber component is 15.0 mass % or less.
[0187] The present invention (6) is a tire in any combination with any of the present inventions (1) to (5), wherein the acetone extractable amount AE (mass %) of the rubber composition is 32.5 mass % or less.
[0188] The present invention (7) is a tire in any combination with any of the present inventions (1) to (6), in which the ratio (Sc / AE) of the content Sc (parts by mass) of the silica relative to 100 parts by mass of the rubber component to the amount of acetone extraction AE (% by mass) of the rubber composition is 1.9 or more.
[0189] The present invention (8) is a tire in any combination with any of the present inventions (1) to (7), in which the product (St×Tt) of the total styrene content St (mass%) in 100% by mass of the rubber component and the tread thickness Tt (mm) is 120 or less.
[0190] The present invention (9) is a tire in any combination with any of the present inventions (1) to (8), in which the product (AE×Tt) of the acetone extractable amount AE (mass%) of the rubber composition and the tread thickness Tt (mm) is 300 or less.
[0191] The present invention (10) is a tire in any combination with any of the present inventions (1) to (9), in which the product (Sc×D) of the content Sc (parts by mass) of the silica per 100 parts by mass of the rubber component and the groove depth D (mm) of the circumferential groove formed in the tread is 450 or more.
[0192] The present invention (11) is a tire in any combination with any of the present inventions (1) to (10), wherein the silica contains silica having an average primary particle diameter of 16 nm or less.
[0193] The present invention (12) is a tire in any combination with any of the present inventions (1) to (11), wherein the resin is a modified resin having a modifying group containing at least one atom selected from the group consisting of a nitrogen atom and an oxygen atom. [Explanation of symbols]
[0194] 2. Pneumatic tires 4 Tread section 6 Sidewall 8 Wing 10 Clinch (Clinch Apex) 12 Beads 14 Carcass 16 Belt Layer 18 Bands 20 Inner Liner 22 Chafer 24 Tread surface 26 Groove 28 Base layer (base tread) 30 Cap Layer 32 cores 34 Apex 36 Carcass ply 36a Main part 36b Folded part 38 Inner layer 40 outer layer 42 Main groove 44 Ribs CL Equatorial plane of tire 2 Tt Tread thickness D: Depth of the circumferential main groove formed in the tread
Claims
1. A tire having a cap tread formed of a rubber composition including a rubber component, a filler including silica, and a resin, the resin contains a modified resin having a modifying group containing at least one atom selected from the group consisting of a nitrogen atom, an oxygen atom, a fluorine atom, and a chlorine atom, The tire has a ratio (Sc / Tt) of a content Sc (parts by mass) of the silica per 100 parts by mass of the rubber component to a tread thickness Tt (mm) of 5.0 or more.
2. The content Ic (mass%) of the isoprene-based rubber in 100% by mass of the rubber component is 15 to 45% by mass, 2. The tire according to claim 1, wherein a ratio (St / Ic) of a total styrene amount St (mass%) in 100% by mass of the rubber component to a content Ic (mass%) of an isoprene-based rubber in 100% by mass of the rubber component is 1.0 or less.
3. The tire according to claim 1, wherein the rubber component contains a styrene-butadiene rubber having a glass transition temperature (Tg) of -25°C or lower.
4. 2. The tire according to claim 1, wherein the Sc / Tt is 7.8 or more.
5. The tire according to claim 1, wherein a total styrene amount St (mass %) in 100 mass % of the rubber component is 15.0 mass % or less.
6. The tire according to claim 1, wherein the rubber composition has an acetone extractable amount AE (mass %) of 32.5 mass % or less.
7. 2. The tire according to claim 1, wherein a ratio (Sc / AE) of a content Sc (parts by mass) of the silica relative to 100 parts by mass of the rubber component to an acetone extractable amount AE (% by mass) of the rubber composition is 1.9 or more.
8. The tire according to claim 1, wherein a product (St x Tt) of a total styrene amount St (mass %) in 100 mass % of the rubber component and a tread thickness Tt (mm) is 120 or less.
9. The tire according to claim 1, wherein a product (AE x Tt) of an acetone extractable amount AE (mass%) of the rubber composition and a tread thickness Tt (mm) is 300 or less.
10. 2. The tire according to claim 1, wherein a product (Sc×D) of a content Sc (parts by mass) of the silica per 100 parts by mass of the rubber component and a groove depth D (mm) of a circumferential groove formed in the tread is 450 or more.
11. The tire according to claim 1 , wherein the silica contains silica with an average primary particle size of 16 nm or less.
12. 2. The tire according to claim 1, wherein the resin is a modified resin having a modifying group containing at least one atom selected from the group consisting of a nitrogen atom and an oxygen atom.
Citation Information
Patent Citations
Rubber composition for studless tire and the studless tire made using the same
JP2013249423A