Water-based coating composition
An aqueous coating composition with SiC and epoxy resin particles addresses the need for corrosion-resistant and thermally conductive films for power semiconductors, offering improved immersion cooling and environmental advantages.
Patent Information
- Application Number
- JP2023064040
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-11
- Publication Date
- 2024-10-24
AI Technical Summary
Existing coating compositions for power semiconductors do not provide sufficient corrosion resistance and thermal conductivity for liquid immersion cooling, and there is a need for a water-based paint that addresses these issues.
Aqueous coating composition containing silicon carbide (SiC) particles and epoxy resin particles dispersed in an aqueous medium, with specific proportions and particle sizes, optionally including organic titanate, to form a coating film with excellent corrosion resistance and thermal conductivity.
The coating film exhibits superior corrosion resistance and thermal conductivity, suitable for immersion cooling of power semiconductors, and can be used at lower temperatures, providing environmental benefits over solvent-based paints.
Smart Images

Figure 2024150965000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a water-based paint capable of forming a coating film having excellent corrosion resistance and thermal conductivity, and to a coating film and an article obtained by using the same. In particular, it relates to an aqueous coating composition in which silicon carbide (SiC) particles and epoxy resin particles are dispersed in an aqueous medium. [Background technology]
[0002] Power semiconductors that control electric power have been attracting attention in recent years, particularly for use in electric vehicles (EVs) and plug-in hybrid vehicles (PHEVs). However, because power semiconductors use large currents and high voltages and generate a lot of heat, it is important to efficiently dissipate heat during use.
[0003] Until now, the mainstream methods of dissipating heat when using power semiconductors have been air cooling or liquid cooling via heat sinks such as heat sinks or heat dissipation fins. However, in order to simplify the heat dissipation mechanism and achieve excellent heat dissipation performance, attention has been focused on liquid immersion cooling, which is advantageous in terms of space and involves cooling power semiconductor devices by directly immersing them in a circulating liquid medium.
[0004] However, if the power semiconductor device is directly immersed in the liquid medium, a problem occurs in that the metal parts of the power semiconductor device corrode.
[0005] Therefore, there is a need for a paint that can form a coating film with excellent corrosion resistance and thermal conductivity that can be suitably used for immersion cooling of power semiconductors.
[0006] For example, Patent Document 1 discloses a coating composition capable of forming a coating film with high heat dissipation effect for use on metal plates used as heat sinks. This heat dissipation coating composition contains a binder resin and a filler of an orthorhombic silicate mineral, and is said to have a high heat dissipation effect by controlling the average particle size of the filler.
[0007] Also, a technology is known in which particles having a particle size of 10 μm or more are added to the paint to form large unevenness on the coating film surface with large height differences, resulting in a coating film with high efficiency in heat dissipation by radiation and convection (Patent Document 2). On the other hand, since the heat dissipation effect depends on the thickness of the coating film, it has been proposed to increase the heat energy transport effect by making the film thinner, and to mix a specific acrylic resin or the like to not only improve the heat dissipation properties of the coating film, but also ensure adhesion to the substrate and mechanical strength (Patent Document 3).
[0008] Furthermore, a heat dissipation material for semiconductor elements has also been proposed, which contains a specific epoxy resin and a curing agent, a thermally conductive filler, and an organic titanate (Patent Document 4).
[0009] Although the above-mentioned prior art documents disclose coating compositions (materials) with high heat dissipation properties, none of them take into consideration immersion cooling, and the corrosion resistance is insufficient. In addition, in recent years, from the standpoint of environmental protection and the cost of recovering volatile solvents, there is a demand for water-based coatings using water as a medium rather than solvent-based coatings using organic solvents as a medium. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] JP 2013-100454 A [Patent Document 2] International Publication No. WO2009 / 142036 [Patent Document 3] JP 2013-209645 A [Patent Document 4] JP 2000-183252 A Summary of the Invention [Problem to be solved by the invention]
[0011] An object of the present invention is to provide a water-based paint capable of forming a coating film having excellent corrosion resistance and thermal conductivity suitable for immersion cooling of power semiconductors, and to provide a coating film and an article. [Means for solving the problem]
[0012] As a result of extensive research aimed at solving the above problems, the inventors discovered that a coating film having excellent corrosion resistance and thermal conductivity can be formed by dispersing silicon carbide (SiC) particles and epoxy resin particles in an aqueous medium, and thus completed the present invention.
[0013] That is, the above problems can be solved by the present invention described below. (1) An aqueous coating composition in which silicon carbide (SiC) particles and epoxy resin particles are dispersed in an aqueous medium, and the proportion of silicon carbide (SiC) in the components excluding the aqueous medium is 40 to 65 mass %. (2) The aqueous coating composition according to (1), wherein the silicon carbide (SiC) particles have an average particle size within the range of 0.3 to 5.0 μm. (3) The aqueous coating composition according to (1) or (2), further comprising an organic titanate. (4) The aqueous coating composition according to any one of (1) to (3), wherein the epoxy resin is a linear high molecular weight epoxy compound. (5) A coating film obtained by coating the aqueous coating composition according to any one of (1) to (4). (6) An article having the coating film described in (5). (7) An electronic component including the article described in (6). Effect of the Invention
[0014] According to the present invention, it is possible to provide an aqueous coating composition capable of forming a coating film having excellent corrosion resistance and thermal conductivity suitable for immersion cooling of power semiconductors, a coating film obtained by applying the aqueous coating composition, an article having the coating film, and an electronic component including the article.
[0015] In addition, since the aqueous coating composition of the present invention can form a film at temperatures below 200°C, it can be used for power semiconductor devices that contain materials such as resin molds and solder that cannot withstand high temperatures of 200°C or higher.
[0016] Furthermore, since the composition of the present invention uses an aqueous medium, it is more environmentally friendly than solvent-based paints that use organic solvents as a medium. [Brief description of the drawings]
[0017] [Figure 1] The thermal conductivity measuring device is shown. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The present invention will be described in detail below. 1.Paint composition The aqueous coating composition of the present invention contains epoxy resin particles, silicon carbide (SiC) particles, and an organic titanate.
[0019] <Epoxy resin particles> The "epoxy resin" used in the present invention is a compound having two or more epoxy groups in the molecule, and is a thermosetting resin that can be crosslinked by a curing agent having any of the following structures: amino group, thiol group, hydroxyl group, phenol group, imidazole group, dicyandiamide, acid anhydride, and hydrazide. Alternatively, the epoxy resin is polymerized in a linear chain to a high molecular weight. The epoxy resin may be a thermoplastic phenoxy resin obtained by ring-opening the epoxy groups at both ends of the molecule after the epoxy resin is heated to a high molecular weight as described above. Furthermore, the epoxy resin may be a modified epoxy resin such as a copolymer or terpolymer in which one molecule is composed of two or more kinds of repeating units by polymerizing other monomers from the epoxy groups at both ends of the molecule of the epoxy resin having a high molecular weight as described above. Epoxy resins suitable for use in corrosion-resistant coating applications include mainly epoxy resins made of the polymerization of bisphenol A and epichlorohydrin, with linear high-molecular-weight epoxy compounds with a molecular weight of 10,000 or more being particularly preferred. Due to their high molecular weight, heating is required to form a film after application, but a coating film with excellent corrosion resistance can be formed without using a curing agent. On the other hand, heat curing with a curing agent is required to form a film from a relatively low molecular weight epoxy resin, and the curing agent component in the coating film may contribute to a decrease in corrosion resistance. Water-soluble epoxy resins are not preferred because they reduce the water resistance of the coating film. However, modified epoxy resins obtained by polymerizing a second component with high water affinity from the terminal of an epoxy resin do not require a surfactant to disperse the resin particles, so the surfactant components remaining in the coating film can be reduced, and the corrosion resistance of the coating film is improved, making them suitable for use. The amount of the second component is preferably adjusted to a level that does not deteriorate the corrosion resistance of the coating film.
[0020] The epoxy resin particles of the present invention may be prepared by dispersing a powder of the particles in an aqueous medium. From the viewpoint of productivity, however, it is preferable to use a previously prepared aqueous dispersion of the epoxy resin particles.
[0021] The average particle size of the epoxy resin particles is preferably 0.05 to 0.5 μm.
[0022] The shape of the epoxy resin particles is not particularly limited, but from the viewpoint of dispersion stability, a spherical shape is preferred.
[0023] Specific examples of epoxy resin particles include EPICLON (registered trademark) H-502-42W, EPICLON H-504-42W, EPICLON H-505-42W, EPICLON EXA-8843, EPICLON EM-N01-56W (2K epoxy), EPICLON EM-102-60W (2K epoxy) (all manufactured by DIC Corporation), jER (registered trademark) series W2801, W2821R70, W3435R67, W8735R70, W1155R55 (all 2K epoxy, manufactured by Mitsubishi Chemical Corporation), and ADEKA RESIN (registered trademark) EM series. Examples of epoxy resins include EM-0427WC, EM-0425C, EM-101-50, EM-051R, EM-0517, EM-058 (all 2K epoxy resins, manufactured by ADEKA Corporation), EM-0464, EM-0180, EM-0434AN (all 1K epoxy resins, manufactured by ADEKA Corporation).
[0024] <Silicon carbide particles> The silicon carbide (SiC) particles of the present invention are spherical or anisotropic silicon carbide particles, and have an average particle size preferably in the range of 0.3 to 5.0 μm, more preferably 0.5 to 3.0 μm, and a maximum particle size (Dmax) preferably less than 15 μm, more preferably less than 10 μm. If the particle size of the silicon carbide particles is too large, liquids may easily permeate through the surface of the coating film, which may result in a decrease in corrosion resistance, whereas if the particle size of the silicon carbide particles is too small, the particles are difficult to disperse in the paint, which may result in defects in the coating film or a decrease in thermal conductivity.
[0025] In the present invention, the average particle size is determined as the particle size (d50) at an integrated value of 50% (volume basis). The maximum particle size is the maximum particle size on a volume basis. As a measurement method, various known methods such as a laser diffraction method, a centrifugal sedimentation method, and an electrical resistance method can be used.
[0026] In the present invention, the proportion of silicon carbide (SiC) is preferably 40 to 65 mass %. If the proportion of silicon carbide is high, the coating film becomes more susceptible to peeling, and if it is 70 mass % or more, problems arise in terms of corrosion resistance.
[0027] The silicon carbide particles are preferably anisotropic particles with an aspect ratio of 0.5 to 0.9. The aspect ratio is expressed as a ratio of the major axis of the particle in a triaxial system to the major axis of the particle. where a is the minor axis diameter and b is the minor axis diameter, and a is the value expressed as b / a.
[0028] As the silicon carbide particles, for example, GC series manufactured by Fujimi Incorporated or C series manufactured by Fujimi Incorporated can be used.
[0029] <Other fillers> The aqueous coating composition of the present invention may contain fillers other than silicon carbide, provided that the fillers do not impair the performance (corrosion resistance, thermal conductivity) of the resulting coating film. Various organic and inorganic fillers can be selected as the other fillers in the present invention depending on the desired properties. Examples of organic materials include engineering plastics and general-purpose plastics such as polyphenylene sulfide, polyether ether ketone, polyether sulfone, polyphenyl sulfone, polyamide, polyimide, phenolic resin, fluororesin, urea resin, urethane resin, melamine resin, polyester resin, polyether resin, acrylic resin, acrylic silicone resin, silicone resin, and silicone polyester resin. Examples of inorganic materials include metals, metal oxides (aluminum oxide, zinc oxide, tin oxide, titanium oxide, etc.), glass, ceramics, silicon oxide, calcium fluoride, carbon black, graphite, mica, and barium sulfate. The filler used in the aqueous coating composition of the present invention may be in a variety of shapes, including particulate, fibrous, and flake-like shapes.
[0030] In the aqueous coating composition of the present invention, the average particle size of the filler can be appropriately selected depending on the substance, shape and desired properties.
[0031] <Organic titanate> The coating composition and the coating film using the coating composition in the present invention preferably contain an organic titanate. The organic titanate is considered to function as an improvement in the dispersibility of silicon carbide particles and as a crosslinking agent for epoxy resins. The organic titanate is not particularly limited as long as it is soluble in water and stable in water to a certain extent in order to ensure the stability of the coating composition until painting, but is preferably an alkoxytitanium, titanium acylate, or titanium chelate having a structure containing a Ti-O-C bond formed by Ti(IV) or Ti(III) and a compound having an alcoholic hydroxyl group, a phenolic hydroxyl group, or a carboxyl group. Among them, titanium aminoethylaminoethanolate or a compound similar thereto is preferred. Those having one hydrolyzable group (an alkoxy group with a low carbon number (specifically, an isopropoxy group, an ethoxy group, etc.)) in the molecule are preferably used because they are considered to be able to suppress the adverse effects caused by the release of the hydrolyzable group.
[0032] <Other ingredients (additives)> The aqueous coating composition of the present invention may contain various additives used in ordinary coatings depending on the desired properties such as dispersibility, electrical conductivity, foam prevention, and wear resistance, for example, surfactants (for example, polyoxyethylene alkyl ether and polyoxyethylene alkyl phenyl ether-based nonionic surfactants such as LEOCOL manufactured by Lion Corporation, TRITON and TERGITOL series manufactured by Dow Chemical Company, and Emulgen manufactured by Kao Corporation; sulfosuccinates, sodium alkyl ether sulfonates, and mono-long-chain alkyl sulfate-based anionic surfactants such as REPARL manufactured by Lion Corporation, EMAL and PEREX manufactured by Kao Corporation; polycarboxylic acids such as RHEOR manufactured by Lion Corporation and OROTAN manufactured by Dow Chemical Company; Salts, acrylate-based polymer surfactants, Momentive's L-77, AirProduct's Surfynol series (Surfynol SE-F, Surfynol 420, Surfynol 440, Surfynol 465, Surfynol 485, etc.), film-forming agents (for example, polymer film-forming agents such as polyamide, polyamideimide, acrylic, acetate, higher alcohols, ethers, polymer surfactants with film-forming effects), thickeners (water-soluble celluloses, solvent-dispersed thickeners, sodium alginate, casein, sodium caseinate, xanthan gum, cellulose nanofiber, polyacrylic acid, acrylic esters), and the like can also be added.
[0033] <Aqueous medium> The aqueous coating composition of the present invention is mainly made of water. However, although it is not preferable from the environmental and cost perspectives, a polar solvent compatible with water can be added or an organic solvent incompatible with water can be dispersed in order to adjust the rheological properties such as the liquid viscosity of the aqueous coating composition or to improve the dispersibility of silicon carbide (SiC) particles, organic titanates, and other fillers. In addition, by adding a polar solvent, the epoxy resin before curing is dissolved, the epoxy resin becomes more uniform during the drying process after coating, the coating film becomes dense, and the epoxy resin easily penetrates into the concaves of the unevenness of the substrate, thereby improving the adhesive strength with the substrate. Examples of polar solvents include alcohols, N-methyl-2-pyrrolidone (NMP), N-ethylmorpholine, N-formylmorpholine, N-acetylmorpholine, N,N'-dimethylethyleneurea, N,N-dimethylacetamide or N,N-dimethylformamide, and γ-butyrolactone.
[0034] 2. Coating The "coating film" of the present invention is a coating film formed by applying the aqueous coating composition of the present invention. The aqueous coating composition of the present invention exhibits excellent performance in terms of thermal conductivity and corrosion resistance. The "coating film" of the present invention includes one-coat coating, a coating film in which the aqueous coating composition of the present invention is used as a primer layer that adheres to a substrate, and multiple layers are applied and laminated thereon, and the like. The "coating film" of the present invention can be formed by various existing coating methods, for example, spray coating, dip coating, spin coating, and other commonly used methods. In order to melt and flow the coating film and obtain a uniform coating film, it is preferable to heat the coating film after coating to a temperature above the melting point of the resin.
[0035] In order to efficiently remove heat in immersion cooling, the thermal conductivity is preferably 0.3 W / m·K or more, more preferably 0.4 W / m·K or more, and particularly preferably 0.5 W / m·K or more.
[0036] 3.Painted items The "coated article" of the present invention is an article having a coating film formed by coating the aqueous paint composition of the present invention. The "coated article" of the present invention includes automobile parts such as power semiconductors, and also heat exchangers and the like not limited to automobile applications. EXAMPLES
[0037] The preparation and performance evaluation of the aqueous coating composition of the present invention will be explained below with reference to examples, but the present invention is not limited to these examples in any way.
[0038] The following reagents were used in the present examples and comparative examples. Epoxy Resin DIC Corporation EPICLON H-502-42W (aqueous dispersion of modified polymeric epoxy resin particles), solid content 39.2% by mass Silicon carbide (SiC) Manufactured by Fujimi Incorporated GC#3000, average particle size (D50) 4μm, maximum particle size 13μm GC#6000, average particle size (D50) 2μm, maximum particle size 8μm GC#8000, average particle size (D50) 1.2μm, maximum particle size 6μm GC#10000, average particle size (D50) 0.5μm, maximum particle size 2μm alumina Spherical alumina DAM-03 manufactured by Denka Co., Ltd., average particle size 4.5 μm Spherical alumina DAW-01 manufactured by Denka Co., Ltd., average particle size 1.8 μm Denka Company, Ltd. Spherical alumina ASFP-40, average particle size 0.3 μm Showa Denko Co., Ltd. Spherical alumina Alna Beads (registered trademark) CB-P02, average particle size 2.9 μm Boron Nitride Showa Denko Co., Ltd., flake boron nitride UHP-S2, average particle size 0.7μm Organic Titanate Matsumoto Fine Chemical Co., Ltd. Orgatics TC-510
[0039] Example 1 (organotitanate-free composition) 17.8g of pure water was placed in a 150mL stainless steel container at room temperature, and 0.5g of surfynol SE-F was slowly dropped in as a wetting agent while stirring at 140 rpm using a stirrer (manufactured by YAMATO SCIENTIFIC CO.LTD.). 16.0g of filler (silicon carbide (SiC) GC#8000) was added and dispersed by ultrasonic waves for 5 minutes. Next, 61.2g of epoxy resin particle aqueous dispersion (EPICLON H-502-42W) was added and stirred for 5 minutes. 1.5g of surfynol SE-F was slowly dropped in as an additional wetting agent, and then 3.0g of ethylene glycol was dropped in as a film-forming material and stirred for 10 minutes to obtain an aqueous coating composition.
[0040] Example 9 (Composition containing organic titanate) 34.7g of pure water was placed in a 150mL stainless steel container at room temperature, and 0.5g of surfynol SE-F was slowly dropped in as a wetting agent while stirring at 140 rpm using a stirrer (manufactured by YAMATOSCIENTIFIC CO.LTD.). 24.0g of filler (silicon carbide (SiC) GC#10000) was added and dispersed by ultrasonic waves for 5 minutes. Then, 5.7g of an organic titanium compound (Orgatics TC-510) was dropped in while stirring, and stirred for 10 minutes. Next, 30.6g of an aqueous dispersion of epoxy resin particles (EPICLON H-502-42W) was added and stirred for 5 minutes. 1.5g of surfynol SE-F was slowly dropped in as an additional wetting agent, and 3.0g of ethylene glycol was dropped in as a film-forming material and stirred for 10 minutes to obtain an aqueous coating composition.
[0041] Examples 2 to 8, 10, and 11 The amount of each component was adjusted to obtain the paint composition (mass%) shown in Table 1 below, and an aqueous paint composition was obtained in the same manner as in Examples 1 or 9 (for example, in Example 10, 35.7 g of the epoxy resin particle aqueous dispersion was used instead of 30.6 g, and 2.9 g of organic titanate (Orgatix TC-510) was used instead of 5.7 g, compared to Example 9).
[0042] Comparative Examples 1 to 9 Coating compositions were obtained in the same manner as in Example 1, adjusting the amounts of each component so as to obtain the coating compositions (mass %) shown in Comparative Examples 1 to 9 in Table 1 below. Incidentally, alumina (73.1 mass%) and boron nitride (42.7 mass%) have almost the same volume percentage as silicon carbide (60 mass%).
[0043] The coating films used for performance evaluation were prepared according to the following procedure. <Creating test pieces for evaluating corrosion resistance> A 70 mm x 50 mm copper plate (oxygen-free copper C1020-1 / 2H, thickness 1 mm) was used as the substrate. It was wiped and degreased with isopropyl alcohol, and the coating composition of each Example and Comparative Example was spray-coated (0.1 to 0.3 g of coating composition) using a spray gun (W-101-101G, manufactured by Anest Iwata Corporation). The plate was then baked at 120°C for 10 minutes and then at 140°C (test condition 1) or 180°C (test condition 2) for 15 minutes to form an evaluation test piece with a film thickness of approximately 10 μm.
[0044] An evaluation test piece was similarly prepared using an aluminum alloy plate (ADC12, thickness 2 mm) instead of the copper plate.
[0045] (Corrosion resistance evaluation method) The obtained evaluation test pieces (copper plate substrate and aluminum alloy plate substrate) were immersed in boiling 5% saline solution for 8 hours, after which the salt water adhering to the surface was washed off with pure water and the moisture was wiped off with tissue. After immersion, the test pieces were visually inspected for the presence or absence of blisters and exposed substrate. Furthermore, the corrosion resistance of the coating film was evaluated (cross-cut test) according to the JIS K5600-5-6 cross-cut method. For the cross-cutting, a commercially available cutter was used to make a grid pattern so that 100 1 mm pieces were cut, and Scotch (registered trademark) Filament Tape 898 (manufactured by 3M) was attached and peeled off 10 times. The number of squares that did not peel off after 10 tape peeling attempts was counted and evaluated. The number of squares that did not peel off after the tape peeling process is shown in Table 1.
[0046] (Thermal conductivity evaluation method) The thermal conductivity of the aqueous coating composition was measured by the following method.
[0047] <Creating test pieces for measuring thermal conductivity> A 20mm x 20mm copper plate (oxygen-free copper C1020-1 / 2H, 1mm thick) was used as the substrate, wiped and degreased with isopropyl alcohol, and the coating composition of each Example and Comparative Example was drop-cast with a dropper and baked at 120°C for 10 minutes, then at 140°C (test condition 1) or 180°C (test condition 2) for 15 minutes to obtain a test piece for measuring thermal conductivity with a film thickness of about 50 to 80μm. The film thickness of the obtained test piece was measured using an eddy current film thickness meter (manufactured by Fisher Instruments, ISOSCOPE).
[0048] <Measurement of thermal conductivity> The thermal conductivity (W / m K) of the coating was measured by the method (temperature gradient method) described in JIS H7903 using a thermal conductivity measuring device (Rhesca Corporation, TCM1000) in the following procedure. First, since it is necessary to attach the test piece to the thermal conductivity measuring device for accurate measurement, silicone grease (Shin-Etsu Chemical Co., Ltd., heat dissipation oil compound G-747, thermal conductivity 0.9 W / m K) was applied to both sides of the test piece while measuring the weight so that the thickness was 15 μm on each side. Next, the test piece with silicone grease applied was set in the thermal conductivity measuring device and the measurement was performed (see Figure 1, in which the hole indicates the thermometer insertion port). The thermal resistance value obtained by the measurement and the thermal conductivity of the coating film to be obtained are expressed by the following formula. [Thermal resistance value obtained by measurement] = 2 × (thickness of silicone grease / thickness of silicone grease) Thermal conductivity) + (thickness of copper base material / thermal conductivity of copper base material) + (thickness of coating film / thermal conductivity of coating film) Here, the thermal resistance value on the left side is obtained by the above measurement, and on the right side, the values other than the thermal conductivity of the coating film to be calculated are known, so the thermal conductivity of the coating film can be calculated. The calculated thermal conductivity of the coating film is shown in Table 1.
[0049] [Table 1]
[0050] It was confirmed that the aqueous coating composition of the present invention exhibits excellent corrosion resistance and thermal conductivity. In Examples 1 to 11, the aqueous coating composition of the present invention has good corrosion resistance and thermal conductivity. was shown.
[0051] Furthermore, the coating composition of Comparative Example 2 demonstrated that as the proportion of silicon carbide in the composition components increases, thermal conductivity increases but problems arise in corrosion resistance.
[0052] The aqueous coating composition of the present invention can form a coating film having both good corrosion resistance and good thermal conductivity, and can therefore be used as an excellent aqueous coating material. [Explanation of symbols]
[0053] 1 Heating section 2 Cooling section 3. Coating 4 Copper base material 5 Silicone grease
Claims
1. The aqueous coating composition comprises silicon carbide (SiC) particles and epoxy resin particles dispersed in an aqueous medium, and the proportion of silicon carbide (SiC) in the components excluding the aqueous medium is 40 to 65 mass %.
2. 2. The aqueous coating composition according to claim 1, wherein the silicon carbide (SiC) particles have an average particle size within the range of 0.3 to 5.0 μm.
3. 3. The aqueous coating composition according to claim 1, further comprising an organic titanate.
4. 4. The aqueous coating composition according to claim 3, wherein the epoxy resin is a linear high molecular weight epoxy compound.
5. A coating film obtained by coating the aqueous coating composition according to claim 4.
6. An article having the coating of claim 5.
7. An electronic component comprising the article of claim 6.
Citation Information
Patent Citations
Heat transfer property compound
JP2000183252A
Heat-radiating coating composition and heat-radiating member using the same
JP2013100454A
Heat-dissipating coating material composition, heat-dissipating coating film and coated article
JP2013209645A
Heat radiating cured coating film, coating composition, process for producing heat radiating cured coating film and electronic device having heat radiating cured coating film
WO2009142036A1