Manufacturing method of lithium sulfide
The described method addresses the inefficiencies and instability in lithium sulfide production by using a controlled heat treatment with sulfur gas and lithium salts, achieving high-quality lithium sulfide with minimal impurities and by-products.
Patent Information
- Application Number
- JP2024040042
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-11
- Filing Date
- 2024-03-14
- Publication Date
- 2024-10-24
AI Technical Summary
Existing methods for producing lithium sulfide face issues such as high manufacturing costs, complex processes, low efficiency, and instability in product quality due to unreacted raw materials and by-products, particularly when using organic solvents or toxic gases, and require multiple reaction cycles or handling of reactive metals.
A method involving a heat treatment step where sulfur gas is passed through a reaction vessel containing a lithium salt, with controlled heating conditions and gas pressures to directly react and produce lithium sulfide, minimizing unreacted materials and by-products.
This method enables efficient production of high-quality lithium sulfide by directly reacting sulfur gas with lithium salts, suppressing residual raw materials and by-products, and ensuring stable product quality.
Smart Images

Figure 2024151307000002 
Figure 2024151307000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing lithium sulfide suitable for use as a sulfide-based solid electrolyte in an all-solid-state battery, for example. [Background technology]
[0002] Lithium-ion batteries are widely used as power sources in vehicles such as EVs (electric vehicles) and HEVs (hybrid electric vehicles), as well as electronic devices such as mobile phones and laptops. Conventional lithium-ion batteries use an organic electrolyte solution in which lithium salts such as lithium hexafluorophosphate (LiPF6) are dissolved in an organic solvent.
[0003] Such organic electrolytes are flammable and may be damaged by excessive heating or impact. In addition, in lithium-ion batteries that use metallic lithium in the negative electrode, dendrite-like metallic lithium grows on the surface of the negative electrode during charging, which may cause an internal short circuit between the electrodes and lead to malfunctions.
[0004] In order to improve the safety and durability of conventional lithium-ion batteries using such organic electrolytes, all-solid-state lithium-ion batteries using sulfide-based solid electrolytes have been proposed. Examples of sulfide-based solid electrolytes currently proposed include Li2S-P2S5, Li2S-P2S3, Li2S-SiS2, Li2S-Ga2S2, and Li2S-GeS2. In all of these sulfide-based solid electrolytes, high-purity lithium sulfide (Li2S) is used as a constituent material.
[0005] As a method for producing high-purity lithium sulfide, for example, Patent Document 1 discloses a method in which lithium hydroxide is reacted with hydrogen sulfide in an aprotic organic solvent to generate lithium hydrosulfide, and lithium sulfide is obtained from the lithium hydrosulfide.
[0006] Furthermore, Patent Document 2 discloses a method for obtaining lithium sulfide by repeating a reaction cycle in which lithium metal is reacted with sulfur gas or hydrogen sulfide to generate lithium sulfide on the surface of the lithium metal, the unreacted lithium metal is melted, and diffused and penetrated into the lithium sulfide that has already been generated, and then the unreacted lithium metal is reacted again with sulfur gas or hydrogen sulfide.
[0007] Patent Document 3 proposes a method for producing lithium sulfide by reacting lithium carbonate with hydrogen sulfide.
[0008] Patent Document 4 also discloses a method for producing lithium sulfide by mixing lithium sulfate and a carbon material and heating the mixture. This method also discloses that both the lithium sulfate and the carbon material are made into fine particles to increase the reaction area and reduce the amount of unreacted raw materials.
[0009] Furthermore, Patent Document 5 discloses a method for obtaining lithium sulfide by thermally reducing lithium sulfate with a carbon material in a vacuum atmosphere. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] JP 2006-151725 A [Patent Document 2] Japanese Patent Application Publication No. 09-110404 [Patent Document 3] JP 2012-221819 A [Patent Document 4] JP 2013-227180 A [Patent Document 5] Patent Publication No. 2021-147251 Summary of the Invention [Problem to be solved by the invention]
[0011] However, the invention disclosed in Patent Document 1 requires the use of an aprotic organic solvent, and the organic solvent used must be treated separately, which leads to problems such as a complicated production process and high production costs. In addition, there is a risk that a part of the aprotic organic solvent may remain in the produced lithium sulfide.
[0012] In the invention disclosed in Patent Document 2, it is necessary to repeatedly react metallic lithium with sulfur gas or hydrogen sulfide multiple times, which results in a long production time and low production efficiency. In addition, metallic lithium is highly reactive and is prone to generating an oxide film on its surface, so it is necessary to handle it in an inert gas atmosphere, making it difficult to handle the raw material. In addition, if the reaction cycle is insufficient, there is a risk that unreacted substances will remain in the lithium sulfide produced.
[0013] The invention disclosed in Patent Document 3 requires the use of toxic hydrogen sulfide gas, and has problems such as high equipment costs due to the need to maintain the airtightness of the reaction apparatus, treat unreacted hydrogen sulfide gas, etc. In addition, when the reaction is insufficient, there is a risk that unreacted substances remain in the produced lithium sulfide.
[0014] Here, in Patent Documents 4 and 5, there is no need to use an organic solvent or hydrogen sulfide, and handling and management are relatively easy.
[0015] However, in the invention disclosed in Patent Document 4, in order to obtain a granular mixture, it is necessary to carry out processes such as pulverization, mixing, and extrusion granulation, which causes a loss of raw materials and reduces the yield. In addition, due to the multiple processes, there is a risk of variation in the mixture ratio of lithium sulfate and carbon material in the mixture. Furthermore, when water is added in the mixing process, a part of the water-soluble lithium sulfate dissolves, which may cause composition variation in the granular mixture. For this reason, there is a problem that the quality of the produced lithium sulfide is not stable.
[0016] In addition, in the invention disclosed in Patent Document 5, since granulation is not performed, it is possible to suppress loss of raw materials and composition variation. However, there is a possibility that problems such as the residue of unreacted raw materials and the generation of by-products due to poor contact between lithium sulfate and a carbon material may occur.
[0017] The present invention has been made in consideration of the above-mentioned circumstances, and has an object to provide a method for producing lithium sulfide that can discharge excess sulfur gas as waste gas, thereby suppressing the residue of unreacted raw materials and the occurrence of by-products, and thus enabling stable production of high-quality lithium sulfide. [Means for solving the problem]
[0018] In order to solve the above problems, a method for producing lithium sulfide according to a first aspect of the present invention is characterized by including a heat treatment step of circulating sulfur gas through a reaction vessel containing a lithium salt, heating the reaction vessel, and generating lithium sulfide.
[0019] The method for producing lithium sulfide according to the first aspect of the present invention includes a heat treatment step of generating lithium sulfide by circulating sulfur gas through a reaction vessel containing a lithium salt and heating the vessel. This makes it possible to efficiently produce lithium sulfide by directly reacting the lithium salt with the sulfur gas, and to suppress the remaining of unreacted raw materials and the generation of by-products. The sulfur gas (elementary sulfur gas) may be mixed with an inert gas in any ratio and then circulated in the reaction vessel.
[0020] A method for producing lithium sulfide according to a second aspect of the present invention is characterized in that, in the method for producing lithium sulfide according to the first aspect of the present invention, the heating conditions in the heat treatment step are such that the heating temperature is within the range of 500° C. or more and 938° C. or less.
[0021] According to the method for producing lithium sulfide of the second aspect of the present invention, the heating temperature in the heat treatment step is set within the range of 500° C. or higher and 938° C. or lower. This makes it possible to sufficiently promote the reaction between the lithium salt and the sulfur gas, and efficiently produce high-quality lithium sulfide with fewer unreacted raw materials and by-products.
[0022] A method for producing lithium sulfide according to a third aspect of the present invention is characterized in that, in the method for producing lithium sulfide according to the first or second aspect of the present invention, the lithium salt is one or more selected from the group consisting of lithium sulfate, lithium carbonate, lithium hydroxide, and lithium oxide.
[0023] According to the method for producing lithium sulfide of the third aspect of the present invention, the lithium salt is one or more selected from lithium sulfate, lithium carbonate, lithium hydroxide, and lithium oxide. Therefore, lithium sulfide can be reliably produced by reacting these lithium salts with sulfur gas.
[0024] The lithium sulfide producing method of the fourth aspect of the present invention is a lithium sulfide producing method of any one of the first to third aspects of the present invention, further comprising the step of: S It is characterized in that the pressure is 1 Pa or more.
[0025] According to the method for producing lithium sulfide of the fourth aspect of the present invention, the sulfur partial pressure P S Since the pressure is set to 1 Pa or more, the reaction between the lithium salt and the sulfur gas proceeds reliably, and lithium sulfide can be produced efficiently. In addition, it is possible to suppress the lithium raw material from remaining and being mixed as an impurity into the produced lithium sulfide, and it is possible to produce high-quality lithium sulfide with fewer impurities.
[0026] The lithium sulfide producing method of the fifth aspect of the present invention is the lithium sulfide producing method of any one of the first to fourth aspects of the present invention, further comprising the step of: O is 1×10 3It is characterized by being less than Pa.
[0027] According to the method for producing lithium sulfide of the fifth aspect of the present invention, the oxygen partial pressure P O is 1×10 3 Since the pressure is set to 0.1 Pa or less, it is possible to suppress the generation of lithium compounds other than lithium sulfide due to the reaction between the lithium salt and oxygen, and it is possible to produce high-quality lithium sulfide with fewer impurities. In addition, it is possible to suppress the consumption of lithium salt by oxygen gas, and it is possible to efficiently produce lithium sulfide.
[0028] A method for producing lithium sulfide according to a sixth aspect of the present invention is characterized in that, in the method for producing lithium sulfide according to any one of the first to fifth aspects of the present invention, a lithium salt other than lithium carbonate is used as the lithium salt.
[0029] According to the method for producing lithium sulfide of the sixth aspect of the present invention, since a lithium salt other than lithium carbonate is used as the lithium salt, it is possible to suppress the generation of carbon dioxide gas during the reaction. Effect of the Invention
[0030] According to the present invention, since excess sulfur gas can be discharged as a waste gas, it is possible to suppress the remaining of unreacted raw materials and the occurrence of by-products, and it is possible to provide a method for producing lithium sulfide that can stably produce high-quality lithium sulfide. [Brief description of the drawings]
[0031] [Figure 1] 1 shows the results of powder X-ray diffraction measurement of lithium sulfide produced in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0032] Hereinafter, embodiments of the present invention will be described with reference to the accompanying drawings. Note that the following embodiments are specifically described to provide a better understanding of the gist of the invention, and do not limit the present invention unless otherwise specified.
[0033] The method for producing lithium sulfide according to the present embodiment is for producing lithium sulfide (Li2S), which is a constituent material of a sulfide solid electrolyte used as a solid electrolyte constituting an all-solid-state battery, for example. The sulfide solid electrolyte material has high ionic conductivity, is non-flammable, and is highly safe, making it suitable as a material for on-board batteries for electric vehicles (EVs) and hybrid electric vehicles (HEVs).
[0034] The method for producing lithium sulfide according to the present embodiment includes a heat treatment step in which sulfur gas (elemental sulfur gas) is circulated in a reaction vessel containing a lithium salt and heated to a high temperature to cause a reaction between the lithium salt and the sulfur gas to produce lithium sulfide.
[0035] In addition, it is preferable to use a method in which sulfur gas (elementary sulfur gas) is generated by a sulfur vapor generator disposed outside the reaction vessel, and the sulfur gas generated by the sulfur vapor generator is supplied into the reaction vessel together with a carrier gas consisting of an inert gas such as Ar gas. The concentration of sulfur gas supplied to the reaction vessel can be adjusted by the amount of sulfur gas generated by the sulfur vapor generator and the flow rate of the carrier gas. Here, there is no particular restriction on the mixing ratio of the inert gas and the sulfur gas (elementary sulfur gas), and they can be mixed at any ratio.
[0036] The lithium salt used as the raw material is preferably one or more selected from the group consisting of lithium sulfate, lithium carbonate, lithium hydroxide, and lithium oxide. Reacting these lithium salts with sulfur gas ensures the production of lithium sulfide. In order to suppress the generation of carbon dioxide gas (CO2 gas) during the reaction, it is preferable to use a lithium salt other than lithium carbonate.
[0037] In this embodiment, the heating conditions in the heat treatment step are preferably an atmosphere with a dew point of -60°C or less, a heating temperature in the range of 500°C to 938°C, and a holding time at the heating temperature in the range of 5 minutes to 420 minutes.
[0038] When the atmosphere has a dew point of −60° C. or lower, the moisture content in the atmosphere is sufficiently low, making it possible to suppress deterioration of the product, lithium sulfide.
[0039] Furthermore, when the heating temperature is 500°C or higher, the reaction rate between the lithium salt and sulfur gas is ensured, and lithium sulfide can be produced efficiently. On the other hand, when the heating temperature is 938°C or lower, the reaction occurs below the melting point of lithium sulfide, and lithium sulfide can be produced with a high yield. The heating temperature is more preferably 600° C. or higher, and more preferably 750° C. or lower.
[0040] When the holding time at the heating temperature is 5 minutes or more, the lithium salt and the sulfur gas can be sufficiently reacted with each other, and the remaining unreacted substances and the occurrence of by-products can be further suppressed. On the other hand, when the holding time at the heating temperature is 300 minutes or less, lithium sulfide can be produced more efficiently. The holding time at the heating temperature is more preferably 60 minutes or more, and more preferably 300 minutes or less.
[0041] In the method for producing lithium sulfide according to this embodiment, the sulfur partial pressure P S is preferably 1×Pa or more. Sulfur partial pressure P in the reaction vessel during the heat treatment process SWhen the pressure is 1 Pa or more, there is a sufficient amount of sulfur gas in the reaction vessel, and the reaction between the lithium salt and the sulfur gas is promoted, so that lithium sulfide can be efficiently produced. In addition, it is possible to suppress the lithium raw material from remaining and being mixed as an impurity into the produced lithium sulfide. In addition, the sulfur partial pressure P S is 1 x 10 2 It is more preferable that the sulfur partial pressure P S There is no upper limit to the 4 It is preferable that the pressure is 0.1 Pa or less.
[0042] In the method for producing lithium sulfide according to this embodiment, the oxygen partial pressure P O is 1×10 3 It is preferable that the pressure is 0.1 Pa or less. The oxygen partial pressure P in the reaction vessel during the heat treatment process O is 1×10 3 When the pressure is 0.01 Pa or less, the content of oxygen gas in the reaction vessel is small, and it is possible to suppress the generation of lithium compounds other than lithium sulfide (e.g., lithium oxide, lithium sulfate, etc.) by the reaction between the lithium salt and the oxygen gas. Therefore, lithium sulfide with few impurities can be produced, and the consumption of lithium salt can be suppressed, so that lithium sulfide can be produced efficiently. In addition, the oxygen partial pressure P O is 1 x 10 2 It is more preferable that the oxygen partial pressure P O There is no particular lower limit, but in practice it is 1×10 -5 Pa or more.
[0043] In the present embodiment, the reaction vessel is not particularly limited. For example, the reaction vessel may be a rotary kiln, and sulfur gas may be circulated through the reaction vessel. A lithium salt may be introduced into the furnace of the rotary kiln, which is maintained at a predetermined temperature, to cause a reaction between the lithium salt and the sulfur gas to produce lithium sulfide. In this embodiment, when a rotary kiln is used as the reaction vessel, the rotation speed of the kiln may be set to 0.1 rpm or more and 20 rpm or less.
[0044] Specifically, lithium salt is placed in a hopper at the top of a rotary kiln, sulfur gas is circulated through the rotary kiln together with an inert gas, and the inside of the rotary kiln is heated to a predetermined heating temperature. The lithium salt in the hopper is supplied to the rotary kiln at a constant rate using a screw feeder, thereby causing a continuous reaction between the lithium salt and the sulfur gas to produce lithium sulfide.
[0045] Through the above-mentioned steps, lithium sulfide is produced with reduced contamination by unreacted raw materials and by-products.
[0046] The method for producing lithium sulfide of the present embodiment configured as described above includes a heat treatment step of circulating sulfur gas through a reaction vessel containing a lithium salt, heating the vessel, and producing lithium sulfide. This makes it possible to efficiently produce lithium sulfide by directly reacting the lithium salt with the sulfur gas, and to suppress the remaining of unreacted raw materials and the production of by-products.
[0047] In the present embodiment, when the heating conditions in the heat treatment step are an atmosphere with a dew point of −60° C. or lower and a heating temperature within a range of 500° C. or higher and 938° C. or lower, the reaction between the lithium salt and the sulfur gas can be sufficiently promoted, and high-quality lithium sulfide with few unreacted raw materials and by-products can be efficiently produced.
[0048] In the present embodiment, when the lithium salt is one or more selected from lithium sulfate, lithium carbonate, lithium hydroxide, and lithium oxide, it is possible to reliably produce lithium sulfide by reacting these lithium salts with sulfur gas.
[0049] In this embodiment, when a lithium salt other than lithium carbonate is used as the lithium salt, it is possible to suppress the generation of carbon dioxide gas in the heat treatment step.
[0050] In this embodiment, the sulfur partial pressure P in the reaction vessel in the heat treatment process S is 1×10 -5 When the pressure is equal to or higher than Pa, the reaction between the lithium salt and the sulfur gas proceeds reliably, and lithium sulfide can be produced efficiently. In addition, it is possible to suppress the lithium raw material remaining and unreacted lithium raw material from being mixed as an impurity into the produced lithium sulfide, making it possible to produce high-quality lithium sulfide with fewer impurities.
[0051] In this embodiment, the oxygen partial pressure P O is 1×10 -2 When the pressure is equal to or less than Pa, it is possible to suppress the reaction of the lithium salt with oxygen to produce lithium compounds other than lithium sulfide, and it is possible to produce high-quality lithium sulfide with fewer impurities. In addition, it is possible to suppress the consumption of lithium salt by oxygen gas, and it is possible to efficiently produce lithium sulfide.
[0052] In the present embodiment, when the reaction vessel is a rotary kiln, by continuously supplying a lithium salt to the rotary kiln through which sulfur gas is circulated, the lithium salt and the sulfur gas can be continuously reacted with each other, and lithium sulfide can be produced more efficiently.
[0053] Although one embodiment of the present invention has been described above, the present invention is not limited to this embodiment, and can be modified as appropriate without departing from the technical concept of the invention. EXAMPLES
[0054] A confirmation experiment conducted to confirm the effectiveness of the present invention will be described.
[0055] (Examples 1 to 12) The thoroughly dried lithium salt powder (average particle size 25 μm) was weighed out to the weight shown in Table 1, placed in an alumina boat, and then charged into a tubular furnace and heated in the atmosphere and at the heating temperature shown in Table 1. The sulfur generation tank containing sulfur was heated to 400°C to generate sulfur gas, and the Ar gas circulated through the sulfur generation device was then introduced into the tubular furnace to cause the sulfur gas to flow through the tubular furnace. Table 1 shows the amount of sulfur gas generated, the amount of gas (mixture of sulfur gas and Ar) introduced into the tubular furnace, and the sulfur partial pressure and oxygen partial pressure in the tubular furnace. Lithium sulfide was produced by reacting lithium salt with sulfur gas in a tubular furnace.
[0056] (Comparative Example) The thoroughly dried lithium salt powder (average particle size 25 μm) was weighed out to the weight shown in Table 1, placed on an alumina board, and charged into a tubular furnace and heated to the heating temperature shown in Table 1. In this comparative example, no sulfur gas was introduced, and only Ar gas was circulated in the tubular furnace. The sulfur partial pressure and oxygen partial pressure in the tubular furnace are shown in Table 1.
[0057] The samples obtained as described above were evaluated for the presence or absence of unreacted substances and by-products as follows. The obtained sample was pulverized in an agate mortar, and powder X-ray diffraction measurements were performed using this powder sample to evaluate the presence or absence of unreacted substances and by-products as the "impurity intensity ratio." An example of the powder X-ray diffraction measurement results is shown in Figure 1. The impurity intensity ratio was calculated by dividing the strongest peak intensity of each impurity excluding the background by the strongest peak intensity of lithium sulfide located at 27.04°.
[0058] [Table 1]
[0059] In the comparative example, lithium sulfate was confirmed. It is presumed that because sulfur gas was not introduced into the furnace, lithium sulfate remained unreacted. In contrast, in the examples, as shown in FIG. 1, no unreacted residues or by-products other than lithium sulfide were observed.
[0060] As described above, according to the present invention, it has been confirmed that it is possible to provide a method for producing lithium sulfide that can stably produce high-quality lithium sulfide because excess sulfur gas can be discharged as waste gas and therefore the presence of unreacted raw materials and by-products can be suppressed.
Claims
1. 1. A method for producing lithium sulfide, comprising: a heat treatment step of circulating sulfur gas through a reaction vessel containing a lithium salt, thereby generating lithium sulfide.
2. 2. The method for producing lithium sulfide according to claim 1, wherein the heating condition in the heat treatment step is a heating temperature in the range of 500° C. or more and 938° C. or less.
3. 3. The method for producing lithium sulfide according to claim 1, wherein the lithium salt is one or more selected from the group consisting of lithium sulfate, lithium carbonate, lithium hydroxide, and lithium oxide.
4. The sulfur partial pressure P in the reaction vessel in the heat treatment step S The method for producing lithium sulfide according to claim 1 or 2, characterized in that the pressure is 1 Pa or more.
5. The oxygen partial pressure P O is 1 x 10 3 The method for producing lithium sulfide according to claim 1 or 2, characterized in that the pressure is 0.01 Pa or less.
6. The method for producing lithium sulfide according to claim 1 or 2, characterized in that the lithium salt used is other than lithium carbonate.
Citation Information
Patent Citations
Production of lithium sulfide
JP1997110404A
Lithium sulfide particle powder, production method therefor and inorganic solid electrolyte
JP2006151725A
Method for manufacturing lithium sulfide for solid electrolyte material of lithium ion battery
JP2012221819A
Method for producing lithium sulfide
JP2013227180A
Method for producing lithium sulfide
JP2021147251A