Multilayer coating film and coated article, as well as method for producing coated article

The multilayer coating film, composed of a scaly glitter pigment, colored pigment, and matting agent, addresses the need for high chroma and soft brilliance, offering a luxurious and diverse design.

JP2024154077AActive Publication Date: 2024-10-30NIPPON PAINT AUTOMOTIVE COATINGS

Patent Information

Application Number
JP2023067692
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-18
Publication Date
2024-10-30
Estimated Expiration
2043-04-18

AI Technical Summary

Technical Problem

Existing multilayer coatings lack the ability to provide high chroma in the highlight region while offering a soft brilliance and diverse design options to meet the evolving consumer preferences for originality and luxury appearance.

Method used

A multilayer coating film comprising a first coating film with a scaly glitter pigment, a second coating film with a colored pigment, and a clear coating film containing a matting agent, optimized for spectral reflectance and specular gloss to achieve high chroma and soft brilliance.

Benefits of technology

The coating film achieves high chroma in the highlight region with a feeling of soft brilliance, providing a new design that is both vivid and luxurious.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024154077000001
    Figure 2024154077000001
Patent Text Reader

Abstract

To provide a multilayer coated film having high chroma in a highlight area, and sensible of soft bright feeling, and a coated article provided with the multilayer coated film, as well as a method for producing the same.SOLUTION: A multilayer coated film comprising a first coating film, a second coating film, and a clear coating film in this order, wherein the first coated film includes a scaly photoluminescent pigment, the second coated film includes a colored pigment, and the clear coated film includes a matting agent, and chroma C*15 in a L*C*h color system based on the spectral reflectance of the reflected light which has received an incident light entering at an angle of 45 degrees with respect to the surface of the multilayer coated film, at an angle of 15 degrees with respect to the specular reflective light is 83 or more, and the 60 degree specular gloss of the multilayer coated film is 55 or more and 90 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a multi-layer coating and a coated article, as well as a method for producing a coated article. [Background technology]

[0002] Automobiles are usually provided with a multi-layer coating film. Conventionally, a high-class feel is required for the exterior of an automobile, and a multi-layer coating film with a strong metallic tone and high flip-flop property is often formed. For example, Patent Document 1 discloses a multi-layer coating film with a metallic texture that varies depending on the viewing angle and a remarkable flip-flop property. Patent Document 2 discloses a multi-layer coating film with a glittering sense of brilliance due to multi-directional reflection. Patent Document 3 discloses a multi-layer coating film with high gloss in highlights and high brightness overall from highlights to shades. On the other hand, Patent Document 4 discloses a multi-layer coating film with a soft texture. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 08-238451 [Patent Document 2] JP 2002-275421 A [Patent Document 3] International Publication No. 2017 / 135426 [Patent Document 4] International Publication No. 2013 / 154168 Summary of the Invention [Problem to be solved by the invention]

[0004] In recent years, due to diversification of consumer tastes and pursuit of originality, the designs required for multilayer coating films have become more diverse. The present invention aims to provide a multilayer coating film with a design different from those in Patent Documents 1 to 4, which has high saturation in the highlight area and gives a soft glittering feeling. [Means for solving the problem]

[0005] In order to solve the above problems, the present invention provides the following aspects. [1] A multi-layer coating film having a first coating film, a second coating film, and a clear coating film in this order, The first coating film contains a scale-like luster pigment, the second coating film comprises a color pigment; The clear coating film contains a matting agent, The L based on the spectral reflectance of the reflected light received at an angle of 15 degrees to the specular reflected light, which is incident on the surface of the multi-layer coating film at an angle of 45 degrees. * C * Saturation C in the h color system * 15 is 83 or more, The multi-layer coating film has a 60 degree specular gloss of 55 or more and 90 or less. [2] The multi-layer coating film according to [1] above, wherein the average light transmittance of the second coating film at a wavelength of 400 to 700 nm is 25% or more and 45% or less. [3] The multi-layer coating film according to the above [1] or [2], wherein the content of the matting agent in the clear coating film is 0.5 parts by mass or more and 6 parts by mass or less per 100 parts by mass of resin solids. [4] The spectral reflectance of light reflected from the surface of the first coating film at an angle of 15 degrees relative to the incident light incident at an angle of 45 degrees is At a wavelength of 400 to 580 nm, the optical transmittance is 25% or more and 215% or less, and The multi-layer coating film of [1] or [2] above, which has a transmittance of 95% or more and 220% or less at a wavelength of 650 to 700 nm. [5] The multi-layer coating film according to [1] or [2] above, wherein the first coating film further contains a coloring pigment. [6] The light transmittance of the second coating film is At a wavelength of 400 to 580 nm, the optical transparency is 2% or more and 40% or less, and The multi-layer coating film of [1] or [2] above, having a transmittance of 85% or more and 100% or less at a wavelength of 650 to 700 nm. [7] A coated object and A coated article having the multilayer coating film of [1] or [2] above provided on the substrate. [8] The method comprises sequentially coating a first coating composition, a second coating composition and a clear coating composition on an object to be coated to form a multi-layer coating film; The first coating composition contains a scale-like luster pigment, The second coating composition comprises a color pigment; The clear coating composition contains a matting agent, The L based on the spectral reflectance of the reflected light received at an angle of 15 degrees to the specular reflected light, which is incident on the surface of the multi-layer coating film at an angle of 45 degrees. * C * Saturation C in the h color system * 15 is 83 or more, The method for producing a coated article, wherein the multi-layer coating film has a 60 degree specular gloss of 55 or more and 90 or less. Effect of the Invention

[0006] According to the present invention, there are provided a multi-layer coating film that has high saturation in the highlight area and gives a soft glittering feel, a coated article having this multi-layer coating film, and a method for producing the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] [Multi-layer coating] The multilayer coating film of the present disclosure comprises, in this order, a first coating film containing a scaly luster pigment, a second coating film containing a coloring pigment, and a clear coating film containing a matting agent.

[0008] The L is based on the spectral reflectance of the reflected light received at an angle of 15 degrees to the specular reflected light of the incident light incident at an angle of 45 degrees to the surface of the multi-layer coating (the surface of the clear coating). * C * Saturation C in the h color system *15 is greater than or equal to 83, which indicates that vivid colors are observed in the highlight areas.

[0009] The 60-degree specular gloss of the multi-layer coating is 55 or more and 90 or less. This indicates that the reflection is not excessively strong (for example, it is a soft reflection, as if through a thin veil). The fact that the above-mentioned 60-degree specular gloss is obtained even though the first coating containing the scaly luster pigment is covered by the second coating indicates that the second coating has a certain degree of light transmittance.

[0010] In this way, by combining a first coating film containing a scaly luster pigment with a second coating film containing a coloring pigment but having light transmission, a high chroma color in the highlight region is achieved. In addition, by providing a clear coating film containing a matting agent so as to cover the second coating film, the multilayer coating film of the present disclosure can express a new design that is different from so-called pastel, matte, or metallic tones, and has high chroma in the highlight region while having a soft brilliance.

[0011] The highlight region is defined as the range of 25 degrees or less with respect to the specular light incident at an angle of 45 degrees. In this disclosure, the highlight region is defined as the saturation at an angle of 15 degrees with respect to the specular light, which can also be called the super highlight region.

[0012] (Saturation C * 15 ) Saturation C * 15 is 83 or more. Saturation C * 15 If the chroma is less than 83, the color will be less vivid and the desired design will not be obtained. * 15 may be 84 or more, and may be 85 or more. * 15 may be 120 or less, and may be 115 or less.

[0013] Saturation C *15 is based on the spectral reflectance of the reflected light received at an angle of 15 degrees to the specular reflected light, which is incident on the surface of the multi-layer coating at an angle of 45 degrees. * C * It is the saturation in the h color system. * C * In the h color system, chroma C * As the value increases, the vividness of the measured substance increases, and as the value decreases, the dullness increases.

[0014] L * C * The h color system is CIEL * a * bColor system (CIE1976L * a * b * It is calculated based on the CIE1976L color space. * a * b * The color space can be calculated according to JIS Z 8781-4. * a * The b color system has been defined by the International Commission on Illumination and is described in Section 4.2 of CIE Publication 15.2 (1986).

[0015] Saturation C * 15 can be obtained using a spectrophotometer (for example, BYK-mac i manufactured by BYK Gardner).

[0016] (60 degree specular gloss) The 60-degree specular gloss of the multi-layer coating film is 55 or more and 90 or less. If the 60-degree specular gloss is less than 55, the reflection is too small and the coating film becomes cloudy, resulting in a design with a so-called matte feel. If the 60-degree specular gloss is more than 90, the reflection is too strong and a soft brilliance cannot be obtained. The 60-degree specular gloss may be 60 or more, or may be 65 or more. The 60-degree specular gloss may be 88 or less, or may be 85 or less.

[0017] The 60-degree specular gloss is measured using a gloss meter (for example, trade name: AG-4446, manufactured by BYK Gardner) in accordance with JIS Z 8741, Specular Gloss-Measuring Method.

[0018] Saturation C * 15 The specular gloss at 60 degrees and 60 degrees are measured for the multi-layer coating film. The multi-layer coating film to be measured is prepared as follows. First, a cationic electrocoating paint and an undercoat paint are applied to a steel plate, and each is heated and cured to obtain a coating material. The first coating composition described below is spray-applied to the coating material so that the dry coating thickness is 3 μm or more and 15 μm or less (typically 10 μm), then the second coating composition is spray-applied wet-on-wet so that the dry film thickness is 3 μm or more and 15 μm or less (typically 10 μm), and then the clear coating composition is spray-applied wet-on-wet so that the dry film thickness is 10 μm or more and 80 μm or less (typically 35 μm). Finally, these uncured three-layer coating films are heat-cured at 140° C. for 20 minutes. The multi-layer coating film refers to a laminate of the cured coating film of the first coating composition, the cured coating film of the second coating composition, and the cured coating film of the clear coating composition applied to the coating material.

[0019] (First coating) The first coating film contains a scaly luster pigment. This provides light reflectivity to the multi-layer coating film. The first coating film is typically a cured product of a first coating composition containing a scaly luster pigment and a coating film-forming resin.

[0020] The thickness of the first coating film may be, for example, 3 μm or more and 15 μm or less. The thickness of the first coating film may be 7 μm or more. The thickness of the first coating film may be 14 μm or less, or may be 13 μm or less.

[0021] Incident light I1 incident at an angle of 45 degrees on the surface of the first coating 45 The reflected light R1 is received at an angle of 15 degrees to the regular reflected light. 15The spectral reflectance of the first coating film may be 25% or more and 220% or less at a wavelength of 400 to 700 nm. This allows the first coating film to exhibit good reflectivity in the visible light region and the highlight region, and the multi-layer coating film can exhibit a more vivid color regardless of the hue of the color pigment of the second coating film.

[0022] If the color pigment of the second coating is red, the reflected light R1 15 The spectral reflectance of may be 25% or more and 215% or less at wavelengths of 400 to 580 nm, and 95% or more and 220% or less at wavelengths of 650 to 700 nm, which allows the multilayer coating film to exhibit a more vivid red color in the highlight region.

[0023] When the color pigment of the second coating is red, reflected light R1 at wavelengths of 400 to 580 nm 15 The spectral reflectance of the reflected light R1 at a wavelength of 650 to 700 nm may be 200% or less, 170% or less, or 150% or less. 15 The spectral reflectance may be 110% or more, 120% or more, or 125% or more.

[0024] Reflected light R1 15 The spectral reflectance is measured for the first coating film alone, not for the multi-layer coating film. The first coating film alone to be measured is obtained by spraying the first coating composition onto a steel plate coated with a cationic electrocoating paint and an undercoat paint, which are then heat-cured, so that the dry coating thickness is 3 μm to 15 μm (typically 10 μm), and then heat-curing at 140° C. for 20 minutes. The first coating film alone to be measured refers to the cured coating film of the first coating composition applied to the substrate.

[0025] The spectral reflectance of the first coating film alone is measured using a spectrophotometer (for example, BYK-mac i manufactured by BYK Gardner) in the range of 400 to 700 nm in wavelength scan mode at a sampling interval of 10 nm.

[0026] Reflected light R1 15 The spectral reflectance of is not an average value. For example, the reflected light R1 15 The spectral reflectance of the reflected light R1 at a wavelength of 400 to 700 nm is 25% or more and 220% or less. 15 This means that the minimum and maximum values ​​of the spectral reflectance are in the range of 25% or more and 220% or less.

[0027] Reflected light R1 15 The spectral reflectance can be adjusted, for example, by the type and mass proportion of the scaly luster pigment contained in the first coating film, the presence or absence of a coloring pigment, the type and mass proportion of the coloring pigment, and the thickness of the first coating film.

[0028] (First paint composition) The first coating composition contains a scaly luster pigment and a film-forming resin. The first coating composition may be water-based or solvent-based. The water-based first coating composition may contain water as the main solvent, and optionally a water-soluble or water-miscible organic solvent. The solvent-based first coating composition may contain, for example, an ester solvent, an ether solvent, an alcohol solvent, a ketone solvent, an aliphatic hydrocarbon solvent, or an aromatic solvent as the main solvent. The first coating composition may be diluted with a solvent suitable for coating before use. The first coating composition may be water-based. The main solvent accounts for 50% by mass or more of the total solvent.

[0029] The first coating composition is prepared by kneading and dispersing the scaly luster pigment, the film-forming resin, the curing agent, etc., using a disperser, homogenizer, kneader, etc. A pigment paste may be prepared in advance using a pigment such as the scaly luster pigment and a pigment dispersant, and this may then be mixed with the film-forming resin, etc.

[0030] <Scaly luster pigment> Examples of the scaly luster pigment include mica pigments such as interference mica, white mica, and colored mica; graphite pigments; glass flake pigments; and metal pigments such as aluminum, copper, zinc, iron, nickel, tin, aluminum oxide, chromium oxide, and alloys containing these. These may be used alone or in combination of two or more. The scaly luster pigment may be colored or uncolored. The scaly luster pigment may be an aluminum pigment.

[0031] The term "scaly pigment" refers to a shape in which the aspect ratio (average major axis of the pigment / average thickness of the pigment) exceeds 1.0. The aspect ratio of the scaly pigment is, for example, 20 or more and 300 or less. The aspect ratio of the scaly pigment may be 30 or more. The aspect ratio of the scaly pigment may be 200 or less.

[0032] The average particle size of the scaly luster pigment may be 4 μm or more, or 5 μm or more.The average particle size of the scaly luster pigment may be 12 μm or less, or 10 μm or less.

[0033] The average particle size of the scaly pigment is the average value of the long diameter. The average particle size is obtained by observing the scaly pigment with a shape analysis laser microscope (e.g., VK-X 250 manufactured by Keyence Corporation) and averaging the long diameter (maximum length) of 100 arbitrarily selected scaly pigment particles.

[0034] The average thickness of the scaly luster pigment is, for example, 0.01 μm or more and 0.1 μm or less. The average thickness of the scaly luster pigment may be 0.04 μm or more. The average thickness of the scaly luster pigment may be 0.08 μm or less.

[0035] The average thickness of the scaly pigments is obtained by observing the cross section of a coating film containing the scaly pigments using a transmission electron microscope (TEM) and averaging the thicknesses of 100 arbitrarily selected scaly pigments.

[0036] The scaly bright pigment may or may not be surface-treated. Examples of compounds used for the surface treatment include metal oxide compounds, phosphorus compounds, amine compounds, and silane compounds.

[0037] The content of the scaly luster pigment in the first coating film, that is, the mass ratio of the scaly luster pigment to the total mass of the resin solid content and the scaly luster pigment contained in the first coating composition (PPWC 1g ) is, for example, 2% by mass or more and 20% by mass or less. This makes it easier to achieve a desired sense of brilliance.

[0038] PWC 1g may be 3 mass% or more, or 5 mass% or more. 1g may be 15% by mass or less, or may be 10% by mass or less. The solid content of the resin refers to the solid content of all resin components such as the coating film-forming resin and the hardener, which will be described later.

[0039] Other pigments The first coating composition (first coating film) may further contain a pigment other than the scaly luster pigment. Examples of other pigments include color pigments, extender pigments, anti-rust pigments, and luster pigments other than scaly. In particular, the first coating film may contain a color pigment. The color pigments contained in the first coating film and the second coating film may be the same or different. When the color pigments contained in the first coating film and the second coating film are the same, the multi-layer coating film looks more vivid.

[0040] The color pigment may be inorganic or organic. The color pigment may be chromatic or achromatic. Examples of organic color pigments include azo chelate pigments, insoluble azo pigments, condensed azo pigments, diketopyrrolopyrrole pigments, phthalocyanine pigments, indigo pigments, perinone pigments, perylene pigments, dioxane pigments, quinacridone pigments, isoindolinone pigments, and metal complex pigments. Examples of inorganic color pigments include yellow lead, yellow iron oxide, red iron oxide, carbon black, and titanium dioxide. These may be used alone or in combination of two or more.

[0041] Examples of the extender pigment include calcium carbonate, barium sulfate, clay, and talc. These may be used alone or in combination of two or more.

[0042] The content of the color pigment in the first coating film, that is, the mass ratio of the color pigment to the total mass of the resin solid content and the color pigment contained in the first coating composition (PWC 1c ) is, for example, 0.05% by mass or more and 35% by mass or less. 1c may be 5% by mass or more, or 7% by mass or more. 1c may be 20% by mass or less, or 15% by mass or less.

[0043] 《Coating film forming resin》 Examples of the film-forming resin include acrylic resin, acrylic silicone resin, polyester resin, polyurethane resin, epoxy resin, fluororesin, and silicone resin. These may be used alone or in combination of two or more. Among them, acrylic resin is preferable.

[0044] In the water-based first coating composition, these resins may be contained as an emulsion, may be contained as a dispersion, or may be contained in a state dissolved in a solvent.

[0045] For example, the acrylic resin emulsion can be prepared by emulsion polymerization of α,β-ethylenically unsaturated monomers. Examples of the α,β-ethylenically unsaturated monomers include (meth)acrylic acid esters, α,β-ethylenically unsaturated monomers having an acid group, and α,β-ethylenically unsaturated monomers having a hydroxyl group. The monomers can be used alone or in combination of two or more.

[0046] Examples of (meth)acrylic acid esters include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, phenyl (meth)acrylate, isobornyl (meth)acrylate, cyclohexyl (meth)acrylate, t-butylcyclohexyl (meth)acrylate, dicyclopentadienyl (meth)acrylate, and dihydrodicyclopentadienyl (meth)acrylate. (Meth)acrylic acid esters refer to acrylic acid esters and methacrylic acid esters.

[0047] Examples of α,β-ethylenically unsaturated monomers having an acid group include acrylic acid, methacrylic acid, crotonic acid, 2-acryloyloxyethyl phthalic acid, 2-acryloyloxyethyl succinic acid, ω-carboxy-polycaprolactone mono(meth)acrylate, isocrotonic acid, α-hydro-ω-((1-oxo-2-propenyl)oxy)poly(oxy(1-oxo-1,6-hexanediyl)), maleic acid, fumaric acid, itaconic acid, 3-vinylsalicylic acid, 3-vinylacetylsalicylic acid, 2-acrylamido-2-methylpropanesulfonic acid, p-hydroxystyrene, and 2,4-dihydroxy-4′-vinylbenzophenone.

[0048] Examples of the α,β-ethylenically unsaturated monomer having a hydroxyl group include hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, allyl alcohol, methallyl alcohol, and adducts of these with ε-caprolactone.

[0049] Other α,β-ethylenically unsaturated monomers may be used in combination. Examples of other α,β-ethylenically unsaturated monomers include polymerizable amide compounds, polymerizable aromatic compounds, polymerizable nitriles, polymerizable alkylene oxide compounds, polyfunctional vinyl compounds, polymerizable amine compounds, α-olefins, dienes, polymerizable carbonyl compounds, polymerizable alkoxysilyl compounds, and other polymerizable compounds.

[0050] The method of emulsion polymerization is not particularly limited. For example, an emulsifier is dissolved in an aqueous medium containing water or, if necessary, an organic solvent such as alcohol, ether (e.g., dipropylene glycol methyl ether, propylene glycol methyl ether, etc.), and an α,β-ethylenically unsaturated monomer and a polymerization initiator are dropped under heating and stirring. The α,β-ethylenically unsaturated monomer may be emulsified in advance by an emulsifier.

[0051] The polymerization initiator and emulsifier may be those commonly used by those skilled in the art. If necessary, the molecular weight may be adjusted using a chain transfer agent such as mercaptan (e.g., lauryl mercaptan) and α-methylstyrene dimer. The reaction temperature, reaction time, etc. may be appropriately selected within the range commonly used by those skilled in the art. The obtained acrylic resin emulsion is neutralized with a base as necessary.

[0052] The acrylic resin (acrylic resin emulsion) obtained by emulsion polymerization may have a number average molecular weight of 3,000 or more. The acrylic resin may have a hydroxyl value (solid content hydroxyl value) of 20 mgKOH / g or more and 180 mgKOH / g or less. The acrylic resin may have an acid value (solid content acid value) of 1 mgKOH / g or more and 80 mgKOH / g or less.

[0053] The number average molecular weight is determined by the GPC method using polystyrene as the standard. The acid value and hydroxyl value of the film-forming resin are calculated from the monomer composition used in the preparation, based on the JIS regulations.

[0054] The acrylic resin dispersion can be prepared, for example, by solution polymerizing the above-mentioned α,β-ethylenically unsaturated monomer and dispersing the resultant with a basic compound.

[0055] The water-soluble acrylic resin can be prepared, for example, by solution polymerizing the above-mentioned α,β-ethylenically unsaturated monomer and then making it water-soluble using a basic compound.

[0056] The acrylic resin to be blended in the solvent-based first coating composition can be prepared, for example, by solution polymerization of an α,β-ethylenically unsaturated monomer. The number average molecular weight of the acrylic resin is, for example, 1,000 or more and 20,000 or less. The acid value (solid acid value) of the acrylic resin may be 1 mgKOH / g or more and 80 mgKOH / g or less. The hydroxyl value (solid hydroxyl value) of the acrylic resin may be 101 mgKOH / g or more and 200 mgKOH / g or less.

[0057] Hardener The first coating composition may include a curing agent that reacts with the film-forming resin to form the first coating therewith.

[0058] Examples of the curing agent include melamine resin, blocked isocyanate compound, epoxy compound, aziridine compound, carbodiimide compound, oxazoline compound, and metal ion. These may be used alone or in combination of two or more. Among them, at least one of melamine resin and blocked isocyanate compound may be used.

[0059] The melamine resin may be water-soluble or water-insoluble. The melamine resin includes a structure in which hydrogen atoms or substituents (alkyl ether groups, methylol groups, etc.) are bonded to the periphery of a melamine nucleus (triazine nucleus) via three nitrogen atoms. The melamine resin is generally composed of a polynuclear body in which a plurality of melamine nuclei are bonded to each other. The melamine resin may be a mononuclear body consisting of one melamine nucleus.

[0060] Commercially available melamine resins may be used. Examples of commercially available melamine resins include the Cymel series (trade name) manufactured by Allnex, specifically Cymel 202, Cymel 204, Cymel 211, Cymel 232, Cymel 235, Cymel 236, Cymel 238, Cymel 250, Cymel 251, Cymel 254, Cymel 266, Cymel 267, Cymel 272, Cymel 285, Cymel 301, Cymel 303, Cymel 325, Cymel 327, Cymel 350, Cymel 370, Cymel 701, Cymel 703, and Cymel 1141; and the U-Ban (trade name) series manufactured by Mitsui Chemicals. These may be used alone or in combination of two or more.

[0061] The blocked isocyanate compound can be prepared by adding a blocking agent having an active hydrogen to a polyisocyanate such as trimethylene diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, isophorone diisocyanate, or the like.

[0062] The content of the curing agent may be 10% by mass or more and 80% by mass or less of the resin solid content contained in the first coating composition. The content of the curing agent may be 15% by mass or more. The content of the curing agent may be 60% by mass or less.

[0063] 《Organic compounds containing phosphate groups》 The first coating composition may further contain a phosphoric acid group-containing organic compound, which facilitates improving the dispersibility of the scaly bright pigment.

[0064] The content of the phosphoric acid group-containing compound may be 0.1% by mass or more and 15% by mass or less of the total solid content of the first coating composition. The content of the phosphoric acid group-containing compound may be 1% by mass or more. The content of the phosphoric acid group-containing compound may be 12% by mass or less.

[0065] The phosphate group-containing compound is not particularly limited as long as it has a phosphate group (-P(=O)(OR)2 (each R is independently hydrogen or a hydrocarbon group)). The phosphate group-containing compound is, for example, at least one of an alkyl phosphate ester having an alkyl group having 4 to 30 carbon atoms and a phosphate group-containing polymer having a phosphate group value of 5 mgKOH / g or more and 300 mgKOH / g or less.

[0066] <Alkyl phosphate ester> The alkyl phosphate ester has an alkyl group having 4 to 30 carbon atoms. Examples of the alkyl phosphate ester include monoalkyl phosphate ester, dialkyl phosphate ester, and mixtures thereof. In the dialkyl phosphate ester, the two alkyl groups may be the same or different. The dialkyl phosphate ester preferably has the same two alkyl groups.

[0067] Examples of the alkyl group having 4 to 30 carbon atoms include a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, a undecyl group, a dodecyl group, a tridecyl group, a tetradecyl group, a pentadecyl group, a hexadecyl group, a heptadecyl group, an octadecyl group, a nonadecyl group, an eicosyl group, a docosyl group, a tetracosyl group, a hexacosyl group, and an octacosyl group. The alkyl group may be linear or branched.

[0068] Examples of alkyl phosphate esters include butyl acid phosphate (a mixture of monobutyl phosphate ester and dibutyl phosphate ester), 2-ethylhexyl acid phosphate (a mixture of mono-2-ethylhexyl phosphate ester and di-2-ethylhexyl phosphate ester), isodecyl acid phosphate (a mixture of monoisodecyl phosphate ester and diisodecyl phosphate ester), dilauryl acid phosphate, lauryl acid phosphate (a mixture of monolauryl phosphate ester and dilauryl phosphate ester), tridecyl acid phosphate (monotridecyl phosphate), Examples of suitable phosphates include monostearyl acid phosphate, distearyl acid phosphate, stearyl acid phosphate (a mixture of monostearyl phosphate and distearyl phosphate), isostearyl acid phosphate (a mixture of monoisostearyl phosphate and diisostearyl phosphate), oleyl acid phosphate (a mixture of monooleyl phosphate and dioleyl phosphate), and behenyl acid phosphate (a mixture of monobehenyl phosphate and dibehenyl phosphate).

[0069] Phosphate-containing polymer The phosphate group-containing polymer has a phosphate value of 5 mgKOH / g or more and 300 mgKOH / g or less. The phosphate value of the phosphate group-containing polymer may be 10 mgKOH / g or more, or 50 mgKOH / g or more. The phosphate value of the phosphate group-containing polymer may be 250 mgKOH / g or less, or 150 mgKOH / g or less.

[0070] The phosphate value is the number of milligrams of potassium hydroxide (KOH) required for neutralization, calculated based on the blend amount of a phosphate group-containing component such as a phosphate ester used in the preparation of a phosphate group-containing polymer.

[0071] The number average molecular weight of the phosphate group-containing polymer is, for example, 1,000 or more and 50,000 or less. The number average molecular weight of the phosphate group-containing polymer may be 3,000 or more, or 5,000 or more. The number average molecular weight of the phosphate group-containing polymer may be 30,000 or less, or 20,000 or less.

[0072] Examples of the phosphate group-containing polymer include acrylic resins, polyester resins, polyether resins, and epoxy resins having a phosphate group value of 5 mgKOH / g or more and 300 mgKOH / g or less. These may be used alone or in combination of two or more. Among them, phosphate group-containing acrylic resins may be used. The phosphate group-containing acrylic resins may be obtained, for example, by polymerizing a phosphate group-containing α,β-ethylenically unsaturated monomer, or by copolymerizing this monomer with another α,β-ethylenically unsaturated monomer that does not contain a phosphate group.

[0073] Additives The first coating composition may contain additives commonly used by those skilled in the art, such as a surface conditioner, a viscosity control agent, a thickener, an antioxidant, an ultraviolet inhibitor, and an antifoaming agent.

[0074] (Second coating) The second coating film contains a color pigment, which imparts a desired hue to the multi-layer coating film. The second coating film is typically a cured product of a second coating composition containing a color pigment and a coating film-forming resin.

[0075] The thickness of the second coating film may be, for example, 3 μm or more and 15 μm or less. The thickness of the second coating film may be 7 μm or more. The thickness of the second coating film may be 14 μm or less, or may be 13 μm or less.

[0076] The light transmittance of the second coating film may affect the saturation of the multi-layer coating film. The average light transmittance of the second coating film at a wavelength of 400 to 700 nm may be 25% or more and 45% or less. When the average light transmittance of the second coating film in the visible light range is 25% or more, the color expressed by the multi-layer coating film becomes more vivid. When the average light transmittance of the second coating film in the visible light range is 45% or less, the color expressed by the multi-layer coating film becomes deeper. The above average light transmittance may be 30% or more, or may be 35% or more. The above average light transmittance may be 44% or less, or may be 43% or less.

[0077] The average light transmittance is measured not for the multi-layer coating film but for the single second coating film. The single second coating film to be measured is obtained by spraying the second coating composition onto a polypropylene plate so that the dry film thickness is 3 μm or more and 15 μm or less (typically 10 μm), heat curing at 140° C. for 20 minutes, and then peeling the coating film off from the polypropylene plate. The single second coating film to be measured refers to the cured product of the film-like second coating composition.

[0078] The light transmittance of the second coating film alone is measured using a spectrophotometer (e.g., Hitachi, product name: U-4100) in the range of 400 to 700 nm under the conditions of wavelength scan mode, scan speed of 300 nm / min, and sampling interval of 0.5 nm. The arithmetic mean value of the obtained light transmittances every 10 nm is defined as the average light transmittance.

[0079] When the color pigment of the second coating film is red, the light transmittance of the second coating film may be 2% or more and 40% or less at a wavelength of 400 to 580 nm, and 85% or more and 100% or less at a wavelength of 650 to 700 nm. This allows the multi-layer coating film to exhibit a more vivid red color. Such light transmittance is not an average value. For example, a light transmittance of 2% or more and 40% or less at a wavelength of 400 to 580 nm means that the minimum and maximum values ​​of the light transmittance in the wavelength range are included in the range of 2% or more and 40% or less.

[0080] The light transmittance of the second coating film can be adjusted, for example, by the type and mass proportion of the color pigment contained in the second coating film, the presence or absence of a luster pigment, and the thickness of the second coating film.

[0081] (Second paint composition) The second coating composition includes a color pigment and a film-forming resin. The second coating composition may be water-based or solvent-based. The second coating composition may be water-based. The solvent contained in the second coating composition and the preparation method thereof are the same as those of the first coating composition.

[0082] Color pigments The second coating composition (second coating film) contains a color pigment. Examples of the color pigment include the same ones that can be contained in the first coating composition. The color pigment may be used alone or in combination of two or more kinds.

[0083] The content of the color pigment in the second coating film, that is, the mass ratio of the color pigment to the total mass of the resin solid content and the color pigment contained in the second coating composition (PWC 2c ) is, for example, 0.05% by mass or more and 35% by mass or less. 2c may be 1 mass% or more, or 2 mass% or more. 2c may be 20% by mass or less, or 10% by mass or less.

[0084] Other pigments The second coating film may further contain a pigment other than the color pigment. Examples of the other pigments include a luster pigment, an extender pigment, and an anti-rust pigment. In particular, the second coating film may contain a luster pigment. The luster pigments contained in the first coating film and the second coating film may be the same or different.

[0085] The content of the luster pigment in the second coating film, that is, the mass ratio of the luster pigment to the total mass of the resin solid content and the luster pigment contained in the second coating composition (PWC 2g ) is, for example, 0.05% by mass or more and 30% by mass or less. 2gmay be 0.1 mass% or more, or 0.2 mass% or more. 2g may be 10% by mass or less, or 5% by mass or less.

[0086] 《Coating film forming resin》 The film-forming resin may be the same as that contained in the first coating composition. The film-forming resins contained in the first and second coating compositions may be the same or different. In addition, the second coating composition may contain the same components as the first coating composition.

[0087] (Clear coating) The clear coating film contains a matting agent, which softens the glossiness of the multi-layer coating film. The clear coating film is typically a cured product of a clear coating composition that contains a matting agent and a clear coating material.

[0088] The thickness of the clear coating film may be, for example, 10 μm or more and 80 μm or less. The thickness of the clear coating film may be 20 μm or more. The thickness of the clear coating film may be 50 μm or less.

[0089] (Clear paint composition) The clear coating composition includes a matting agent and a clear coating. The clear coating composition may be solvent-based, water-based, or powder-type. The clear coating composition may be solvent-based.

[0090] Matting agent The matting agent creates minute irregularities on the surface of the clear coating, causing light diffusion. This reduces the particle size of the scaly photoluminescent pigment, especially that contained in the first coating, and softens the glittering effect.

[0091] The matting agent is, for example, fine particles of an inorganic or organic substance. As the matting agent, a conventionally known agent for paints can be used.

[0092] Examples of inorganic fine particles include silica particles, aluminum oxide particles, titanium dioxide particles, zirconium dioxide particles, zircon particles, tin oxide particles, and magnesium oxide particles. These may be used alone or in combination of two or more. Among them, silica particles may be used from the viewpoint of matting ability and storage stability. The shape of the silica particles is not particularly limited, and may be spherical, hollow, porous, rod-like, plate-like, fibrous, or amorphous.

[0093] Commercially available silica particles include, for example, the Sylysia series (Sylysia 350, Sylysia 430, Sylysia 435, Sylysia 436, Sylysia 450, etc.) manufactured by Fuji Silysia Co., Ltd., the Sylohobic series (Sylohobic 100, Sylohobic 200, Sylohobic 702, Sylohobic 100, 4004, etc.), the Sylosphere series (Sylosphere 1504, Sylosphere 1510, etc.) manufactured by Grace Japan Co., Ltd., the SYLOID series (Syloid W300, Syloid W500, etc.) manufactured by Evonik Degussa Japan Co., Ltd., and the ACEMATT series (ACEMATT HK460, ACEMATT K400, ACEMATT OK412, ACEMATT OK520, ACEMATT TS100, ACEMATT 3200, ACEMATT 3300, ACEMATT 3600, etc.), NIPGEL series (NIPGEL AZ-200, etc.), NIPSIL series (NIPSIL E-200A, NIPSIL SS-50B, NIPSIL SS-178B, etc.) manufactured by Nippon Silica Industry Co., Ltd., Mizukasil series (Mizukasil P-73, P-526, etc.) manufactured by Mizusawa Chemicals Co., Ltd., Carplex series (Carplex CS-8, etc.) manufactured by Shionogi & Co., Ltd., AEROSIL series (AEROSIL 200, AEROSIL R805, AEROSIL R972, etc.) manufactured by Nippon Aerosil Co., Ltd., and Radiolite series (Radiolite 100, Radiolite 200, Radiolite 500, Radiolite 500R, Radiolite 500RS, etc.) manufactured by Showa Chemical Industry Co., Ltd.

[0094] The inorganic fine particles may be surface-treated with an organic compound and / or an inorganic compound. In particular, from the viewpoint of storage stability, the inorganic fine particles may be surface-treated with an organic compound. Examples of the treatment with an organic compound include a polyethylene wax treatment and a silane compound treatment. In particular, a polyethylene wax treatment is preferred.

[0095] Examples of organic fine particles (hereinafter sometimes referred to as resin beads) include PMMA (polymethyl methacrylate) resin beads, MMA-EGDM (ethylene glycol dimethacrylate) copolymer resin beads, nylon resin beads, and polytetrafluoroethylene resin beads.

[0096] Commercially available resin beads include, for example, "Techpolymer Series (product name)" manufactured by Sekisui Plastics Co., Ltd. and "Dyneon Series (product name)" manufactured by Sumitomo 3M Limited.

[0097] The average particle size of the matting agent may be 1 μm or more, 2 μm or more, or 3 μm or more from the viewpoint of matting ability, storage stability, etc. From the same viewpoint, the average particle size of the matting agent may be 10 μm or less, 9 μm or less, or 8 μm or less.

[0098] The average particle size of the matting agent is the 50% average particle size (D50) in the volumetric particle size distribution measured using a laser diffraction / scattering particle size distribution measuring device. D50 is measured after adding the matting agent to a mixed solvent of acetone and isopropyl alcohol, dispersing it with ultrasonic waves for 1 minute, and adjusting the concentration to a specified transmittance range.

[0099] The oil absorption of the matting agent may be 100 mL / 100 g or more from the viewpoint of matting ability, etc. From the same viewpoint, the oil absorption of the matting agent may be 400 mL / 100 g or less, 380 mL / 100 g or less, or 360 mL / 100 g or less. The oil absorption is measured in accordance with JIS K 5101-13-2:2004.

[0100] Matting agent content (PWC m ) may be 0.5 parts by mass or more and 6 parts by mass or less based on 100 parts by mass of the resin solid content of the clear coating composition. m By having the content of PWC be 0.5 parts by mass or more, the glittering effect tends to be soft. m By making the content of PWC 6 parts by mass or less, the sense of cloudiness is suppressed, and sufficient saturation and a sense of depth of color can be easily expressed. m may be 0.8 parts by mass or more, 1.0 parts by mass or more, or 1.2 parts by mass or more. m may be 5.5 parts by mass or less, or 5.0 parts by mass or less.

[0101] Clear paint The clear coating may be, for example, an acid epoxy curing type containing a polyepoxide and a polycarboxylic acid, or a urethane curing type containing a hydroxyl group-containing resin and a polyisocyanate curing agent. The urethane curing type clear coating may be a two-component type.

[0102] The acid-epoxy curing type clear coating material contains, for example, an acid anhydride group-containing acrylic resin (a), a carboxyl group-containing polyester resin (b), and an acrylic resin (c) having a hydroxyl group and an epoxy group. From the viewpoint of storage stability, the acid anhydride group of the acid anhydride group-containing acrylic resin (a) may be half-esterified with a low molecular weight alcohol or the like. The carboxyl group-containing polyester resin (b) may further have a hydroxyl group.

[0103] The above resins (a) to (c) are blended, for example, so that the molar ratio of the carboxyl groups contained in the acrylic resin (a) and the polyester resin (b) to the epoxy groups contained in the acrylic resin (c) is 1 / 1.4 to 1 / 0.6 (preferably 1 / 1.2 to 1 / 0.8), and the molar ratio of the carboxyl groups derived from the acid anhydride groups contained in the acrylic resin (a) to the hydroxyl groups contained in the polyester resin (b) and the acrylic resin (c) is 1 / 2.0 to 1 / 0.5 (preferably 1 / 1.5 to 1 / 0.7).

[0104] The urethane curing clear coating contains, for example, a hydroxyl group-containing resin and a polyisocyanate curing agent. Examples of the polyisocyanate curing agent include aliphatic isocyanates such as trimethylene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate (HDI), and trimethylhexamethylene diisocyanate; aliphatic cyclic isocyanates such as 1,3-cyclopentane diisocyanate, 1,4-cyclohexane diisocyanate, and 1,2-cyclohexane diisocyanate; aromatic isocyanates such as xylylene diisocyanate (XDI), 2,4-tolylene diisocyanate (TDI), and 2,6-tolylene diisocyanate; alicyclic isocyanates such as isophorone diisocyanate (IPDI), and norbornane diisocyanate methyl; and polymers and mixtures thereof such as biuret and nurate forms.

[0105] The hydroxyl value of the hydroxyl-containing resin is, for example, 20 mgKOH / g or more and 200 mgKOH / g or less. The hydroxyl value may be 30 mgKOH / g or more. The hydroxyl value may be 180 mgKOH / g or less. The weight average molecular weight of the hydroxyl-containing resin is, for example, 1000 or more and 20000 or less. The weight average molecular weight may be 2000 or more. The weight average molecular weight may be 15000 or less. The acid value of the hydroxyl-containing resin is, for example, 2 mgKOH / g or more and 30 mgKOH / g or less. The acid value may be 3 mgKOH / g or more. The acid value may be 25 mgKOH / g or less.

[0106] The hydroxyl-containing resin and the polyisocyanate curing agent are mixed so that the equivalent ratio (NCO / OH) between the isocyanate group (NCO) and the hydroxyl group (OH) is 0.5 or more and 1.7 or less. The equivalent ratio may be 0.7 or more. The equivalent ratio may be 1.5 or less.

[0107] Alternatively, an acrylic melamine curing type clear paint may be used.

[0108] [Painted items] The coated article according to the present disclosure comprises a substrate and the above-mentioned multi-layer coating film provided on the substrate. In the coated article, the clear coating film is disposed on the outside. The coated article comprising the above-mentioned multi-layer coating film has a unique design in which the highlight area has high saturation and a soft glittering feel.

[0109] (subject to be coated) Examples of the material of the object to be coated include metal, plastic, and foam. In particular, the object may be a metal (particularly a casting), and may be a metal that can be electrocoated. Examples of such metals include iron, copper, aluminum, tin, zinc, and alloys containing these metals.

[0110] The shape of the substrate is not particularly limited, and may be flat or three-dimensional. Specific examples of the substrate include automobile bodies and parts thereof, such as passenger cars, trucks, motorcycles, and buses.

[0111] The metal substrate may be subjected to a chemical conversion treatment using a phosphoric acid-based chemical conversion treatment agent, a zirconium-based chemical conversion treatment agent, or the like, and may be subjected to an electrodeposition coating. The electrodeposition coating composition may be of the cationic type or the anionic type. The cationic electrodeposition coating composition can form a coating film having excellent corrosion resistance.

[0112] The metal substrate may have an electrodeposition coating and an intermediate coating applied thereon. The intermediate coating is usually applied for the purpose of improving the adhesion and durability of the multi-layer coating. The intermediate coating composition may contain, for example, a film-forming resin, a hardener, a color pigment, and an extender pigment. The film-forming resin and hardener may be the same as those contained in the first coating composition.

[0113] [Manufacturing method of coated articles] A method for producing a coated article according to the present disclosure comprises sequentially coating a substrate with a first coating composition, a second coating composition, and a clear coating composition to form a multilayer coating film.

[0114] In one embodiment, the coated article is produced by sequentially coating a first coating composition and a second coating composition on a substrate, curing the coating, and then coating and curing a clear coating composition. After coating the first coating composition, preheating may be performed before coating the second coating composition.

[0115] In another embodiment, the coated article is produced by successively applying the first coating composition, the second coating composition, and the clear coating composition wet-on-wet to the substrate, and then curing these coating compositions at once. Preheating may be performed after applying the first coating composition and before applying the second coating composition, and after applying the second coating composition and before applying the clear coating composition.

[0116] Examples of the coating method include air spray coating, airless spray coating, electrostatic spray coating, multi-stage coating (preferably two-stage coating) using air electrostatic spray coating, and coating that combines air electrostatic spray coating with a rotary atomizer-type electrostatic coater.

[0117] Curing of each coating composition is carried out, for example, under conditions of a heating temperature of 80° C. to 180° C. (preferably 100° C. to 160° C.) and a heating time of 5 minutes to 60 minutes (preferably 10 minutes to 30 minutes). EXAMPLES

[0118] The present invention will be described in more detail with reference to the following examples, but the present invention is not limited thereto. In the examples, "parts" and "%" are by weight unless otherwise specified.

[0119] The number average molecular weight was measured using a GPC apparatus (trade name: "HLC8220GPC") (manufactured by Tosoh Corporation) and four columns (trade names: "Shodex F-606M" and "Shodex KF-603") (both manufactured by Showa Denko K.K.), under the following conditions: mobile phase: tetrahydrofuran, measurement temperature: 40°C, flow rate: 0.6 cc / min, and detector: RI.

[0120] The phosphate value is the amount of potassium hydroxide (KOH) required for neutralization, calculated based on the amount of phosphate-containing components such as phosphate esters used in the preparation of the phosphate-containing polymer. The acid value and hydroxyl value were calculated from the monomer composition used in the preparation, based on the JIS regulations.

[0121] [Production Example 1] Production of acrylic resin emulsion 633 parts of deionized water was added to the reaction vessel, and the temperature was raised to 80°C while mixing and stirring in a nitrogen stream. Separately, 75.65 parts of styrene (ST), 178.96 parts of methyl methacrylate (MMA), 75.94 parts of n-butyl acrylate (BA), 64.45 parts of 2-ethylhexyl acrylate (2-EHA), and 105.0 parts of hydroxyethyl methacrylate (HEMA) were mixed to prepare a first-stage monomer mixture. Next, this monomer mixture was mixed with 25.0 parts of Aqualon HS-10 (polyoxyethylene alkylpropenyl phenyl ether sulfate, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), 25.0 parts of Adeka Reasoap NE-20 (α-[1-[(allyloxy)methyl]-2-(nonylphenoxy)ethyl]-ω-hydroxyoxyethylene, manufactured by Asahi Denka Co., Ltd.), and 400 parts of deionized water to prepare a monomer emulsion. Separately, an initiator solution consisting of 1.2 parts of ammonium persulfate and 500 parts of deionized water was prepared. The monomer emulsion and the initiator solution were dropped into the reaction vessel in parallel over 1.5 hours. After the dropwise addition was completed, the mixture was aged at the same temperature for 1 hour.

[0122] Further, 53.65 parts of styrene (ST), 178.96 parts of methyl methacrylate (MMA), 75.94 parts of n-butyl acrylate (BA), 64.45 parts of 2-ethylhexyl acrylate (2-EHA), 105.0 parts of hydroxyethyl methacrylate (HEMA), and 22 parts of acrylic acid were mixed to prepare a second-stage monomer mixture. Next, this monomer mixture was mixed with 10 parts of Aqualon HS-10 and 250 parts of deionized water to prepare a monomer emulsion. Separately, an initiator solution consisting of 3.0 parts of ammonium persulfate and 500 parts of deionized water was prepared. The monomer emulsion and the initiator solution were dropped in parallel into the above reaction vessel over 1.5 hours. After the dropwise addition was completed, the mixture was aged at the same temperature for 2 hours.

[0123] The reaction product was then cooled to 40°C and filtered through a 400 mesh filter. Finally, 100 parts of deionized water and 1.6 parts of dimethylaminoethanol were added to the reaction product to adjust the pH to 6.5. In this way, an acrylic resin emulsion was obtained with an average particle size of 150 nm, a solid content concentration of 35%, a solid content acid value of 20 mgKOH / g, and a hydroxyl value of 100 mgKOH / g.

[0124] [Production Example 2] Production of phosphoric acid group-containing polymer A 1-liter reaction vessel equipped with a stirrer, a temperature regulator, and a cooling tube was charged with 40 parts of ethoxypropanol. Separately, 20 parts of Hosmer PP (acid phosphooxyhexa(oxypropylene)monomethacrylate manufactured by Unichemical Co., Ltd.) were dissolved in 20 parts of ethoxypropanol to prepare a solution. 40 parts of this solution, 4 parts of styrene, 35.96 parts of n-butyl acrylate, 18.45 parts of ethylhexyl methacrylate, 13.92 parts of 2-hydroxyethyl methacrylate, 7.67 parts of methacrylic acid, and 1.7 parts of azobisisobutyronitrile were mixed to prepare a monomer solution. 121.7 parts of the monomer solution were dropped into the reaction vessel at 120° C. over 3 hours. The mixture was further stirred for 1 hour to obtain a phosphate group-containing polymer. The phosphate group-containing polymer thus obtained had an acid value of 105 mgKOH / g, a phosphate value of 55 mgKOH / g, a hydroxyl value of 60 mgKOH / g, a number average molecular weight of 6,000 and a solids concentration of 63%.

[0125] [Production Example 3] Production of water-soluble acrylic resin 23.89 parts of tripropylene glycol methyl ether and 16.11 parts of propylene glycol methyl ether were added to the reaction vessel, and the mixture was heated to 105°C while being mixed and stirred in a nitrogen stream. Next, a monomer mixture containing 13.1 parts of methyl methacrylate, 68.4 parts of ethyl acrylate, 11.6 parts of 2-hydroxyethyl methacrylate, and 6.9 parts of methacrylic acid was prepared, and an initiator solution consisting of 100 parts of the monomer mixture, 10.0 parts of tripropylene glycol methyl ether, and 1 part of tertiary butyl peroxy 2-ethylhexanoate was dropped into the reaction vessel in parallel over a period of 3 hours. After the dropwise addition, the mixture was aged at the same temperature for 0.5 hours.

[0126] Further, an initiator solution consisting of 5.0 parts of tripropylene glycol methyl ether and 0.3 parts of tertiary butyl peroxy 2-ethylhexanoate was added dropwise to the reaction vessel over 0.5 hours. After the completion of the addition, the mixture was aged at the same temperature for 2 hours.

[0127] After 16.1 parts of the solvent was distilled off at 110°C under reduced pressure (70 torr) using a solvent remover, 204 parts of deionized water and 7.1 parts of dimethylaminoethanol were added to obtain a water-soluble acrylic resin solution. The solid content of the obtained water-soluble acrylic resin solution was 30%, with a solid content acid value of 40 mgKOH / g, a hydroxyl value of 50 mgKOH / g, and a viscosity of 140 poise (E-type viscometer 1 rpm / 25°C).

[0128] [Example 1] (1) Preparation of the first coating composition (1-1) Preparation of color pigment dispersion 38.9 parts of the water-soluble acrylic resin solution of Production Example 3, 11.7 parts of a color pigment (perylene red, trade name: PALIOGEN RED L-3875, manufactured by BASF), 14.0 parts of a pigment dispersant (trade name: DISPEX ULTRA PA 4550AN), 34.9 parts of ion-exchanged water, and 0.5 parts of an antifoaming agent (trade name: BYK-011) were mixed with a stirrer. Then, the mixture was dispersed using a disperser filled with 0.05 mm zirconia beads at a volumetric filling rate of 70%, to obtain a color pigment dispersion.

[0129] (1-2) Preparation of first coating composition 122.1 parts of the acrylic resin emulsion of Production Example 1, 2.0 parts of dimethylaminoethanol, 28.4 parts of melamine resin (trade name: Cymel 370N, mixed alkylated melamine resin, manufactured by Allnex, solid content 90%), 109.3 parts of the above color pigment dispersion, 18.9 parts of aluminum paste (trade name: WL-Z440, crushed type scaly aluminum pigment, average particle size 14 μm, manufactured by Toyo Aluminum Co., Ltd., active ingredient 66%) per 100 parts of resin solid content, 5 parts of the phosphate group-containing polymer of Production Example 2, 0.4 parts of lauryl acid phosphate, 50 parts of butyl cellosolve, 5.5 parts (3 parts in terms of solid content) of a surfactant (trade name: Noigen EA-207D, manufactured by Daiichi Kogyo Seiyaku Co., Ltd., number average molecular weight 4200, solid content 55%), and 3 parts of linoleic acid (manufactured by Kishida Chemical Co., Ltd.) were uniformly dispersed. Dimethylaminoethanol was added to this dispersion so that the pH was adjusted to 8.1, and the dispersion was diluted with deionized water to obtain a water-based first coating composition with a resin solids concentration of 33%.

[0130] (2) Preparation of second coating composition (2-1) Preparation of color pigment dispersion 38.9 parts of the water-soluble acrylic resin solution of Production Example 3, 11.7 parts of a color pigment (perylene red, trade name: PALIOGEN RED L-3875, manufactured by BASF), 14.0 parts of a pigment dispersant (trade name: DISPEX ULTRA PA 4550AN), 34.9 parts of ion-exchanged water, and 0.5 parts of an antifoaming agent (trade name: BYK-011) were mixed with a stirrer. Then, the mixture was dispersed using a disperser filled with 0.05 mm zirconia beads at a volumetric filling rate of 70%, to obtain a color pigment dispersion.

[0131] (2-2) Preparation of second coating composition 143.3 parts of the acrylic resin emulsion of Production Example 1, 1.4 parts of dimethylaminoethanol, 28.4 parts of melamine resin (product name: Cymel 370N), 34.8 parts of the above color pigment dispersion, 50 parts of butyl cellosolve, 5.5 parts of surfactant (product name: Noigen EA-207D) (3 parts in terms of solid content), and 3 parts of linoleic acid (Kishida Chemical Co., Ltd.) were uniformly dispersed. Dimethylaminoethanol was added to this dispersion to adjust the pH to 8.1, and the mixture was diluted with deionized water to prepare an aqueous second coating composition with a resin solid content concentration of 15%.

[0132] (3) Preparation of clear coating composition A clear coating composition was prepared by adding 1.6 parts of a matting agent (silica, polyethylene wax-treated silica, product name: ACEMATT OK520, Evonik Degussa Japan, D50: 6.5 μm, oil absorption 300 mL / 100 g) to 100 parts of resin solids of an acid epoxy curing clear coating (product name: Macflow-O-1810 Clear, manufactured by Nippon Paint Automotive Coatings) and mixing with a stirrer.

[0133] (4) Formation of multi-layer coating A zinc phosphate-treated dull steel plate with a thickness of 0.8 mm, length of 30 cm, and width of 40 cm was electrocoated with a cationic electrodeposition coating composition "Power Top U-50)" (manufactured by Nippon Paint Automotive Coatings) to a dry film thickness of 20 μm, and baked at 160°C for 30 minutes. The resulting coated plate was air-sprayed with an intermediate coating composition "OP-30P Middle Gray" (manufactured by Nippon Paint Automotive Coatings, polyester-melamine paint, pre-diluted for 25 seconds (measured at 20°C using a No. 4 Ford cup)) using an air spray gun W-101-132G manufactured by Anest Iwata to a dry film thickness of 35 μm, and heated at 140°C for 30 minutes. In this way, a coated object having an electrodeposition coating film and an intermediate coating film was obtained.

[0134] The first coating composition was air-spray-coated on the substrate at room temperature of 23°C and humidity of 68% to a dry film thickness of 10 μm. After setting for 4 minutes, the substrate was preheated at 80°C for 5 minutes. The second coating composition was then air-spray-coated wet-on-wet at room temperature of 23°C and humidity of 68% to a dry film thickness of 10 μm. After setting for 4 minutes, the substrate was preheated at 80°C for 5 minutes. The coated plate was allowed to cool to room temperature, and the clear coating composition was air-spray-coated to a dry film thickness of 35 μm, and the substrate was set for 7 minutes. Finally, the coated plate was heated in a dryer at 140°C for 30 minutes to obtain a coated article having a multi-layer coating film.

[0135] [Example 2] A clear coating composition was prepared in the same manner as in Example 1, except that the amount of silica, which is a matting agent, was changed to 3.2 parts. A multi-layer coating film and a coated article were obtained in the same manner as in Example 1, except that this clear coating composition was used.

[0136] [Example 3] Except for changing the amount of silica, which is a matting agent, to 4.8 parts, a clear coating composition was prepared in the same manner as in Example 1. Except for using this clear coating composition, a multi-layer coating film and a coated article were obtained in the same manner as in Example 1.

[0137] [Example 4] In the preparation of the second coating composition, 0.4 parts of a colored pearl pigment (Xirallic NXT M260-30 SW Leonis Gold: manufactured by MERCK) was further mixed in, except that the second coating composition was prepared in the same manner as in Example 1. A multi-layer coating film and a coated article were obtained in the same manner as in Example 1, except that this second coating composition was used.

[0138] [Example 5] In the preparation of the first coating composition, except that the color pigment dispersion was not mixed, the first coating composition was prepared in the same manner as in Example 1. Except that this first coating composition was used, a multi-layer coating film and a coated article were obtained in the same manner as in Example 1.

[0139] [Example 6] A clear coating composition was prepared by mixing 100 parts of resin solids of a urethane curing clear coating (trade name: PU Excel O-2100, manufactured by Nippon Paint Automotive Coatings Co., Ltd., two-component type) with 3.2 parts of a matting agent (trade name: ACEMATT OK520). A multilayer coating film and a coated article were obtained in the same manner as in Example 1, except that this clear coating composition was used.

[0140] [Comparative Example 1] A multi-layer coating film and a coated article were obtained in the same manner as in Example 1, except that no matting agent was added and Macflow-O-1810 Clear was used as it was as the clear coating composition.

[0141] [Comparative Example 2] A clear coating composition was prepared in the same manner as in Example 1, except that the amount of silica, which is a matting agent, was changed to 6.4 parts. A multi-layer coating film and a coated article were obtained in the same manner as in Example 1, except that this clear coating composition was used.

[0142] [Comparative Example 3] A second coating composition was prepared in the same manner as in Example 1 using a mixture of 7.0 parts of a color pigment (trade name: PALIOGEN RED L-3875), 8.4 parts of a pigment dispersant (trade name: DISPEX ULTRA PA 4550AN), 20.9 parts of ion-exchanged water, and 0.3 parts of an antifoaming agent (trade name: BYK-011) as a color pigment dispersion. A multilayer coating film and a coated article were obtained in the same manner as in Example 1, except that this second coating composition was used.

[0143] [Comparative Example 4] As the color pigment dispersion, a mixture of 37.4 parts of color pigment (trade name: PALIOGEN RED L-3875), 44.8 parts of pigment dispersant (trade name: DISPEX ULTRA PA 4550AN), 111.7 parts of ion-exchanged water, and 1.6 parts of defoamer (trade name: BYK-011) was used to prepare a second coating composition in the same manner as in Example 1. A multilayer coating film and a coated article were obtained in the same manner as in Example 1, except that this second coating composition was used.

[0144] [Comparative Example 5] A multi-layer coating film and a coated article were obtained in the same manner as in Example 1, except that the first coating composition was not applied.

[0145] [Comparative Example 6] (1) Preparation of coating composition (1-1) Preparation of color pigment dispersion 38.9 parts of the water-soluble acrylic resin solution of Production Example 3, 21.1 parts of a color pigment (trade name: PALIOGEN RED L-3875), 25.2 parts of a pigment dispersant (trade name: DISPEX ULTRA PA 4550AN), 62.8 parts of ion-exchanged water, and 0.9 parts of an antifoaming agent (trade name: BYK-011) were mixed with a stirrer. Then, the mixture was dispersed using a disperser filled with 0.05 mm zirconia beads at a volumetric filling rate of 70%, to obtain a color pigment dispersion.

[0146] (1-2) Preparation of coating composition 143.3 parts of the acrylic resin emulsion of Production Example 1, 1.4 parts of dimethylaminoethanol, 28.4 parts of melamine resin (trade name: Cymel 370N), 1.6 parts of pearl pigment (trade name: XIRALLIC F60-51WNT RADIANT RED, manufactured by MERCK), 34.8 parts of the above colored pigment dispersion, 3.9 parts of colored aluminum pigment (trade name: F120-58CWT wahiba orange, manufactured by MERCK) per 100 parts of resin solids, 5 parts of the phosphoric acid group-containing polymer of Production Example 2, 0.4 parts of lauryl acid phosphate, 50 parts of butyl cellosolve, 5.5 parts of surfactant (trade name: Noigen EA-207D) (3 parts in terms of solids), and 3 parts of linoleic acid (manufactured by Kishida Chemical Co., Ltd.) were uniformly dispersed. Dimethylaminoethanol was added to this dispersion to make the pH 8.1, and the dispersion was diluted with deionized water to obtain a coating composition with a resin solids concentration of 33%.

[0147] (2) Formation of multi-layer coating The above coating composition was air-spray coated on the substrate obtained in the same manner as in Example 1 at room temperature of 23°C and humidity of 68% so that the dry film thickness was 4 μm. After setting for 4 minutes, the coating was preheated at 80°C for 5 minutes. The coated plate was then allowed to cool to room temperature, and Macflow-O-1810 Clear was air-spray coated as a clear coating composition so that the dry film thickness was 35 μm, and the coating was allowed to set for 7 minutes. Finally, the coated plate was heated in a dryer at 140°C for 30 minutes to obtain a multi-layer coating film and a coated article.

[0148] [evaluation] The following evaluations were carried out using the multi-layer coating film, the single first coating film, or the single second coating film obtained in the Examples and Comparative Examples. The evaluation results are shown in the following table.

[0149] (Preparation of a single first coating film) The above first coating composition was spray-coated on a substrate obtained in the same manner as in Example 1 so that the dry coating film had a thickness of 10 μm, and the substrate was cured by heating at 140° C. for 20 minutes. This resulted in a cured coating film (single first coating film) of the first coating composition applied to the substrate.

[0150] (Preparation of a separate second coating) The above second coating composition was spray-coated on a polypropylene plate so that the dry film thickness was 10 μm, and then heat-cured for 20 minutes at 140° C. The coating was then peeled off from the polypropylene plate to obtain a film-like second coating (single second coating).

[0151] (1) Spectral reflectance The spectral reflectance was measured using a spectrophotometer (BYK-mac i, manufactured by BYK Gardner) in the range of 400 to 700 nm in wavelength scan mode at a sampling interval of 10 nm.

[0152] (2) Saturation Measured using a spectrophotometer (BYK Gardner, BYK-mac i)

[0153] (3) Light transmittance The light transmittance was measured using a spectrophotometer (Hitachi, product name: U-4100) in the range of 400 to 700 nm under the conditions of wavelength scan mode, scan speed of 300 nm / min, and sampling interval of 0.5 nm. The average light transmittance was obtained by averaging the light transmittance every 10 nm.

[0154] (4) 60 degree specular gloss The 60-degree specular gloss was measured using a gloss meter (BYK Gardner, AG-4446) in accordance with JIS Z 8741, Specular Gloss Measurement Method.

[0155] (5) Vividness of color The multi-layer coating film was viewed from an incident angle of 45° and a receiving angle of about 15° and evaluated according to the following criteria.

[0156] Evaluation criteria A: A vivid and deep red color. B: A little less vivid, but has a deep red color. C: A dull red color is felt

[0157] (6) Brilliant feeling The multi-layer coating film was viewed from an incident angle of 45° and a receiving angle of about 15° and evaluated according to the following criteria.

[0158] Evaluation criteria A: A soft, veiled glow. B: Slightly inferior to A, but has a soft glow. C: A feeling of cloudiness or strong brilliance is felt

[0159] [Table 1]

[0160] The present disclosure includes the following aspects. [1] A multi-layer coating film having a first coating film, a second coating film, and a clear coating film in this order, The first coating film contains a scale-like luster pigment, the second coating film comprises a color pigment; The clear coating film contains a matting agent, The L based on the spectral reflectance of the reflected light received at an angle of 15 degrees to the specular reflected light, which is incident on the surface of the multi-layer coating film at an angle of 45 degrees. * C * Saturation C in the h color system * 15 is 83 or more, The multi-layer coating film has a 60 degree specular gloss of 55 or more and 90 or less. [2] The multi-layer coating film according to [1] above, wherein the average light transmittance of the second coating film at a wavelength of 400 to 700 nm is 25% or more and 45% or less. [3] The multi-layer coating film according to the above [1] or [2], wherein the content of the matting agent in the clear coating film is 0.5 parts by mass or more and 6 parts by mass or less per 100 parts by mass of resin solids. [4] The spectral reflectance of light reflected from the surface of the first coating film at an angle of 15 degrees relative to the incident light incident at an angle of 45 degrees is At a wavelength of 400 to 580 nm, the optical transmittance is 25% or more and 215% or less, and The multilayer coating film of any one of the above [1] to [3], which has a transmittance of 95% or more and 220% or less at a wavelength of 650 to 700 nm. [5] The multilayer coating film according to any one of the above [1] to [4], wherein the first coating film further contains a color pigment. [6] The light transmittance of the second coating film is At a wavelength of 400 to 580 nm, the optical transparency is 2% or more and 40% or less, and The multilayer coating film of any one of the above [1] to [5], which has a transmittance of 85% or more and 100% or less at a wavelength of 650 to 700 nm. [7] A coated object and A coated article comprising the multilayer coating film of any one of the above [1] to [6] provided on the substrate. [8] The method comprises sequentially coating a first coating composition, a second coating composition and a clear coating composition on an object to be coated to form a multi-layer coating film; The first coating composition contains a scale-like luster pigment, The second coating composition comprises a color pigment; The clear coating film contains a matting agent, The L based on the spectral reflectance of the reflected light received at an angle of 15 degrees to the specular reflected light, which is incident on the surface of the multi-layer coating film at an angle of 45 degrees. * C * Saturation C in the h color system * 15 is 83 or more, The method for producing a coated article, wherein the multi-layer coating film has a 60 degree specular gloss of 55 or more and 90 or less. [Industrial Applicability]

[0161] The multilayer coating film of the present disclosure has high saturation in the highlight region and a soft sense of brilliance, making it possible to impart new designs to a variety of substrates.

Claims

1. A multi-layer coating film having a first coating film, a second coating film, and a clear coating film in this order, The first coating film contains a scale-like luster pigment, The second coating film includes a color pigment, The clear coating film contains a matting agent, The incident light incident on the surface of the multi-layer coating film at an angle of 45 degrees is reflected at an angle of 15 degrees relative to the regular reflection light. * C * Saturation C in the h color system * 15 is 83 or more, The multilayer coating film has a 60 degree specular gloss of 55 or more and 90 or less.

2. The multilayer coating film according to claim 1, wherein the average light transmittance of the second coating film at a wavelength of 400 to 700 nm is 25% or more and 45% or less.

3. 3. The multi-layer coating film according to claim 1, wherein the content of the matting agent in the clear coating film is 0.5 parts by mass or more and 6 parts by mass or less per 100 parts by mass of resin solids.

4. The spectral reflectance of light reflected from the surface of the first coating film at an angle of 15 degrees relative to the specular reflection of incident light incident at an angle of 45 degrees to the surface of the first coating film is At a wavelength of 400 to 580 nm, the reflection coefficient is 25% or more and 215% or less, and The multilayer coating film according to claim 1 or 2, which has a transmittance of 95% or more and 220% or less at a wavelength of 650 to 700 nm.

5. The multi-layer coating film according to claim 1 or 2, wherein the first coating film further comprises a color pigment.

6. The light transmittance of the second coating film is At a wavelength of 400 to 580 nm, the reflection ratio is 2% or more and 40% or less, and The multilayer coating film according to claim 1 or 2, which has a transmittance of 85% or more and 100% or less at a wavelength of 650 to 700 nm.

7. A coated object and A coated article comprising the multi-layer coating film according to claim 1 or 2 provided on the substrate.

8. The method comprises sequentially coating a first coating composition, a second coating composition and a clear coating composition on an object to be coated to form a multi-layer coating film; The first coating composition contains a scale-like luster pigment, The second coating composition comprises a color pigment; The clear coating composition contains a matting agent, The incident light incident on the surface of the multi-layer coating film at an angle of 45 degrees is reflected at an angle of 15 degrees relative to the regular reflection light. * C * Saturation C in the h color system * 15 is 83 or more, The method for producing a coated article, wherein the multilayer coating film has a 60 degree specular gloss of 55 or more and 90 or less.

Citation Information

Patent Citations

  • Colored and clear coated metal board

    JP2005087954A

  • Method for forming luster multi-layer coating and coated article

    JP2006289247A

  • Coating composition and method for forming coating film

    JP2012041508A

  • Coating composition and coated film forming method

    JP2016089003A

  • Method for forming multilayer coating film

    WO2018074376A1

Cited By

  • Multilayer coating film

    JP2026092509A

  • Multi-layer coating

    JP7808170B1