Manufacturing method for thin film transistor, sputtering target, and sintered body
By integrating In, Zn, and Al into the oxide semiconductor layer and forming an oxide gas barrier layer, the method addresses hydrogen-induced instability in thin film transistors, enhancing operational stability and carrier mobility.
Patent Information
- Application Number
- JP2024016439
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-18
- Filing Date
- 2024-02-06
- Publication Date
- 2024-10-30
AI Technical Summary
Thin film transistors with oxide semiconductor layers are prone to operational instability due to hydrogen diffusion from protective layers containing SiN, which affects carrier mobility and threshold voltage stability.
Incorporating In, Zn, and Al into the oxide semiconductor layer and forming an oxide gas barrier layer with these elements to suppress hydrogen diffusion and desorption, thereby enhancing operational stability.
The method improves the operational stability and carrier mobility of thin film transistors by effectively preventing hydrogen infiltration, resulting in improved electrical characteristics and optical stress resistance.
Smart Images

Figure 2024154366000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for producing a thin-film transistor, a sputtering target, and a sintered body. [Background technology]
[0002] Thin film transistors (TFTs) are becoming more and more popular as active elements used in flat panel displays such as organic electroluminescence (EL) displays. Well-known types of thin film transistors include top-gate (staggered) and bottom-gate (inverted staggered) types.
[0003] Such thin film transistors are required to have operational stability. Thin film transistors that have improved operational stability by increasing carrier mobility and light stress resistance are known (JP 2020-194945 A). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2020-194945 A Summary of the Invention [Problem to be solved by the invention]
[0005] The thin film transistor of Patent Document 1 has an oxide semiconductor layer containing In, Zn, and Fe, thereby improving the operational stability. SiN is often used as the protective layer of a thin film transistor. The protective layer containing SiN has a high hydrogen content, and hydrogen may be desorbed from the protective layer and diffused due to the thermal history during the manufacturing process. If this hydrogen penetrates into the oxide semiconductor layer of the thin film transistor, it may deteriorate the characteristics of the thin film transistor, such as the Vth shift. Such deterioration of characteristics has a large effect on thin film transistors having an oxide semiconductor layer with high carrier mobility, and tends to make the operation unstable. There is a demand for reducing the effect of hydrogen and improving the operational stability of thin film transistors having an oxide semiconductor layer.
[0006] The present disclosure has been made in consideration of the above circumstances, and aims to provide a method for manufacturing a thin-film transistor capable of improving operational stability, and a sputtering target for forming an oxide semiconductor layer and an oxide gas barrier layer of a thin-film transistor having high operational stability. [Means for solving the problem]
[0007] A method for manufacturing a thin film transistor according to one embodiment of the present disclosure is a method for manufacturing a thin film transistor having at least an oxide semiconductor layer, a protective layer, a gate insulating layer, a gate electrode, a source electrode, and a drain electrode on a substrate, the method including the steps of forming the oxide semiconductor layer containing In, Zn, and Al as metal elements on the substrate, and forming the protective layer containing SiN on the oxide semiconductor layer.
[0008] A method for manufacturing a thin film transistor according to another embodiment of the present disclosure is a method for manufacturing a thin film transistor having at least an oxide semiconductor layer, an oxide gas barrier layer, a protective layer, a gate insulating layer, a gate electrode, a source electrode, and a drain electrode on a substrate, the method including the steps of forming the oxide semiconductor layer on the substrate, forming the oxide gas barrier layer containing In, Zn, and Al as metal elements on the oxide semiconductor layer, and forming the protective layer containing SiN on the oxide gas barrier layer.
[0009] A sputtering target according to yet another embodiment of the present disclosure is a sputtering target for forming at least one of an oxide semiconductor layer and an oxide gas barrier layer used in a thin film transistor, which contains In, Zn and Al as metal elements, and the contents of the In, Zn and Al relative to the total of all metal elements contained are In: 40 atomic % or more and 75 atomic % or less, Zn: 15 atomic % or more and 45 atomic % or less, and Al: 0.5 atomic % or more and 20 atomic % or less. Effect of the Invention
[0010] The method for producing a thin film transistor according to one aspect of the present disclosure can improve the operational stability of the thin film transistor. The sputtering target according to another aspect of the present disclosure can form an oxide semiconductor layer and an oxide gas barrier layer of a thin film transistor having high operational stability. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a schematic cross-sectional view showing a top-gate thin film transistor according to an embodiment of the present disclosure. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing a top-gate type thin film transistor different from that in FIG. [Diagram 3] FIG. 3 is a schematic cross-sectional view showing a top-gate type thin film transistor different from those in FIGS. [Figure 4]FIG. 4 is a graph showing the measurement results of the Id-Vg characteristics of a thin-film transistor of Sample 15 having a channel length of 10 μm and including an oxide semiconductor layer containing In and Zn. [Diagram 5] FIG. 5 is a graph showing the measurement results of the Id-Vg characteristics of a thin film transistor of Sample 16 having a channel length of 10 μm and including an oxide semiconductor layer containing In, Zn and Al. [Figure 6] FIG. 6 is a graph showing the results of measuring the Id-Vg characteristics of a thin-film transistor of sample 15 having a channel length of 10 μm and an oxide semiconductor layer containing In and Zn, and comparing the light stress resistance in a gate negative bias and light irradiation (Negative Bias Temperature Illumination Stress: NBTIS) test. [Figure 7] FIG. 7 is a graph showing a comparison result of light stress resistance by an NBTIS test, in which Id-Vg characteristics of a thin-film transistor of Sample 16 having a channel length of 10 μm and an oxide semiconductor layer containing In, Zn, and Al are measured. [Figure 8] FIG. 8 is a graph showing the measurement results of Id-Vg characteristics of thin film transistors in which the channel length of an oxide semiconductor layer containing In and Zn is changed. [Figure 9] FIG. 9 is a graph showing the measurement results of Id-Vg characteristics of thin film transistors in which the channel length of an oxide semiconductor layer containing In, Zn, and Al is changed. [Figure 10] FIG. 10 is a graph showing the measurement results of the Id-Vg characteristics of a thin-film transistor of Sample 27 having a channel length of 10 μm and including an oxide semiconductor layer containing In, Zn, and Al. [Figure 11] FIG. 11 is a graph showing the measurement results of Id-Vg characteristics of thin film transistors in which the channel length of an oxide semiconductor layer containing In, Zn, and Al is changed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] [Description of the embodiments of the present disclosure] First, the embodiments of the present disclosure will be listed and described.
[0013] As described above, hydrogen (H2) desorbed from the protective layer containing SiN and diffused into the oxide semiconductor layer, or this hydrogen becomes moisture (H2O) and penetrates into the oxide semiconductor layer, which may deteriorate the characteristics of the thin film transistor, such as the Vth shift. The inventors of the present invention have conducted extensive research and found that the intrusion of H2 and H2O into the oxide semiconductor layer can be suppressed by including indium (In), zinc (Zn) and aluminum (Al) in the oxide semiconductor layer, or that the intrusion of H2 and H2O into the oxide semiconductor layer can be suppressed by providing the thin film transistor with an oxide gas barrier layer containing In, Zn and Al. At the same time, they found that the above-mentioned Al can suppress the desorption of Zn, which may be desorbed from the layer due to aging or the like.
[0014] (1) A method for manufacturing a thin film transistor according to one embodiment of the present disclosure is a method for manufacturing a thin film transistor having at least an oxide semiconductor layer, a protective layer, a gate insulating layer, a gate electrode, a source electrode and a drain electrode on a substrate, the method including the steps of forming the oxide semiconductor layer containing In, Zn and Al as metal elements on the substrate, and forming the protective layer containing SiN on the oxide semiconductor layer.
[0015] In the method for manufacturing a thin-film transistor, an oxide semiconductor layer containing In, Zn, and Al is formed on a substrate, so that it is possible to suppress the intrusion of H and HO that have diffused into the oxide semiconductor layer, thereby improving the operational stability of the obtained thin-film transistor.
[0016] (2) A method for manufacturing a thin film transistor according to another embodiment of the present disclosure is a method for manufacturing a thin film transistor having at least an oxide semiconductor layer, an oxide gas barrier layer, a protective layer, a gate insulating layer, a gate electrode, a source electrode, and a drain electrode on a substrate, the method including the steps of: forming the oxide semiconductor layer on the substrate; forming the oxide gas barrier layer containing In, Zn, and Al as metal elements on the oxide semiconductor layer; and forming the protective layer containing SiN on the oxide gas barrier layer.
[0017] In the method for manufacturing a thin-film transistor, an oxide gas barrier layer containing In, Zn, and Al is formed on an oxide semiconductor layer, so that it is possible to suppress the intrusion of H and HO that have diffused into the oxide semiconductor layer, and it is possible to improve the operational stability of the obtained thin-film transistor.
[0018] (3) In the above (2), the oxide semiconductor layer may contain In, Zn, and Al as metal elements, which can further suppress the diffusion of H2 and H2O into the oxide semiconductor layer.
[0019] (4) In the above (1), (2) and (3), the content of the metal elements may be In: 40 atomic % to 75 atomic %; Zn: 15 atomic % to 45 atomic %; and Al: 0.5 atomic % to 20 atomic %. In this way, the content of the In, Zn and Al in the metal elements is within the above ranges, which effectively suppresses the intrusion of H2 and H2O into the oxide semiconductor layer and promotes optimization of the carrier mobility and threshold voltage of the thin film transistor.
[0020] (5) In the above (1), (2), and (3), the oxide semiconductor layer and the oxide gas barrier layer may be amorphous layers, which can improve the effect of suppressing the diffusion of H2 and H2O.
[0021] (6) In the above (1) to (5), the oxide semiconductor layer and the oxide gas barrier layer may be formed as a barrier layer against at least one of H2 and H2O. That is, the oxide semiconductor layer itself may be formed as a layer that also serves as a gas barrier layer that suppresses the intrusion of at least one of H2 and H2O.
[0022] (7) In the above (1) to (6), the Al in the oxide semiconductor layer and the oxide gas barrier layer may suppress desorption of the Zn, that is, the Al may be contained as a metal element that suppresses desorption of Zn.
[0023] A sputtering target according to yet another embodiment of the present disclosure is a sputtering target for forming at least one of an oxide semiconductor layer and an oxide gas barrier layer used in a thin film transistor, which contains In, Zn and Al as metal elements, and the contents of the In, Zn and Al relative to the total of all metal elements contained are In: 40 atomic % or more and 75 atomic % or less, Zn: 15 atomic % or more and 45 atomic % or less, and Al: 0.5 atomic % or more and 20 atomic % or less.
[0024] The sputtering target can form an oxide semiconductor layer and an oxide gas barrier layer that can suppress the diffusion of H 2 and H 2 O into the oxide semiconductor layer.
[0025] A sintered body according to yet another embodiment of the present disclosure is a sintered body for forming the above-mentioned sputtering target.
[0026] That is, the sputtering target may be formed of a sintered body.
[0027] [Details of the embodiment of the present disclosure] Hereinafter, the embodiments of the present disclosure will be described in detail with reference to the drawings as appropriate. Note that, for the numerical values described in this specification, only one of the upper limit value and the lower limit value described can be adopted, or the upper limit value and the lower limit value can be arbitrarily combined. In this specification, all numerical ranges from the upper limit value to the lower limit value that can be combined are described as suitable ranges.
[0028] [First embodiment] FIG. 1 shows a top-gate type thin-film transistor 10 (hereinafter, also simply referred to as "thin-film transistor 10") as an example of a thin-film transistor obtained by the manufacturing method of the thin-film transistor (hereinafter, also simply referred to as "the manufacturing method"). The thin-film transistor 10 has an oxide semiconductor layer 12, a protective layer 13, a gate insulating layer 14, a gate electrode 15, a source electrode 16, and a drain electrode 17 on a substrate 11. The protective layer 13 of the thin-film transistor 10 in FIG. 1 includes a first protective layer 131 containing silicon oxide (SiOx) and a second protective layer 132 containing silicon nitride (SiN) and laminated on the first protective layer 131. The gate insulating layer 14 and the gate electrode 15 are disposed in the protective layer 13 (first protective layer 131). The gate insulating layer 14 is laminated on the oxide semiconductor layer 12, and the gate electrode 15 is laminated on the gate insulating layer 14. The source electrode 16 and the drain electrode 17 are disposed so that parts of them contact the conductive S / D region of the oxide semiconductor layer 12. The region of the oxide semiconductor layer 12 where the gate insulating layer 14 is laminated is a channel region that is not made into a conductor.
[0029] The thin film transistor 10 is obtained by the manufacturing method including a step of forming an oxide semiconductor layer 12 containing In, Zn, and Al as metal elements on a substrate 11, and a step of forming a protective layer 13 containing SiN on the oxide semiconductor layer 12. Between these two steps, the manufacturing method includes a step of forming a gate insulating layer 14 on the oxide semiconductor layer 12, and a step of forming a gate electrode 15 on the gate insulating layer 14. The manufacturing method also includes a step of forming a source electrode 16 and a drain electrode 17 after the step of forming the protective layer 13.
[0030] [Step of forming oxide semiconductor layer] In the step of forming the oxide semiconductor layer 12, the oxide semiconductor layer 12 containing In, Zn, and Al as metal elements is formed on the substrate 11.
[0031] (substrate) The substrate 11 is not particularly limited, and examples thereof include a glass substrate, a silicon substrate, etc. Examples of glass used for the glass substrate include non-alkali glass, high strain point glass, soda lime glass, etc. In addition, the substrate 11 may be a metal substrate such as a stainless steel sheet, or a resin substrate such as a polyethylene terephthalate (PET) film.
[0032] From the viewpoint of workability, the average thickness of the substrate 11 is preferably 0.001 mm or more and 10 mm or less. The size and shape of the substrate 11 can be set according to the size of the display, etc.
[0033] (Oxide semiconductor layer) The oxide semiconductor layer 12 contains In, Zn, and Al as metal elements. By containing these metal elements, the oxide semiconductor layer 12 can suppress the intrusion of H2 diffused from the second protective layer 132 containing SiN, which will be described later, into the inside. In addition, it can suppress the intrusion of the diffused H2 into the inside as H2O by combining with oxygen. That is, the oxide semiconductor layer 12 functions as a barrier layer against H2 and H2O gases.
[0034] <in> In is an element that suppresses the intrusion of H2 and H2O into the oxide semiconductor layer 12 and also contributes to improving the conductivity (electrical conductivity). The greater the In content, the more the conductivity of the oxide semiconductor layer 12 is improved, and the more the carrier density and carrier mobility are improved.
[0035] The lower limit of the In content relative to the total of the above metal elements is preferably 40 atomic %. The upper limit of the above content is preferably 75 atomic %, and more preferably 65 atomic %. By setting the In content within the above range, it is possible to improve the reliability of the effect of suppressing the intrusion of H2 and H2O into the oxide semiconductor layer 12, and to ensure sufficient carrier mobility, etc.
[0036] <zn> Zn is an element that inhibits the intrusion of H 2 and H 2 O into the oxide semiconductor layer 12 and also affects the processing characteristics of the oxide semiconductor layer 12.
[0037] The lower limit of the Zn content relative to the total of the above metal elements is preferably 15 atomic %, and more preferably 25 atomic %. The upper limit of the above content is preferably 45 atomic %, and more preferably 35 atomic %. By setting the Zn content within the above range, the reliability of the effect of suppressing the intrusion of H2 and H2O into the oxide semiconductor layer 12 can be improved, and the processability and uniformity of the oxide semiconductor layer 12 can be easily ensured.
[0038] <al> Al is an element that suppresses the intrusion of H2 and H2O into the oxide semiconductor layer 12 and also suppresses the desorption of Zn from the oxide semiconductor layer 12. Specifically, Zn may be desorbed from the oxide semiconductor layer 12 due to aging or the like. By including Al, the desorption of Zn can be suppressed. Furthermore, by including Al in the oxide semiconductor layer 12, the light stress resistance of the thin film transistor 10 can be improved.
[0039] The lower limit of the Al content relative to the total of the metal elements is preferably 0.5 atomic %, and more preferably 1.5 atomic %. The upper limit of the Al content is preferably 20 atomic %, and more preferably 10 atomic %. By setting the Al content within the above range, it is possible to improve the reliability of the effect of suppressing the intrusion of H2 and H2O into the oxide semiconductor layer 12 and to improve the reliability of the effect of suppressing the Zn desorption.
[0040] The reason why Al can suppress the desorption of Zn is thought to be as follows. It is known that Zn in the oxide layer is released after the H2 and H2O contained in the oxide layer are released. When Al is added to the oxide layer, in addition to the function of suppressing the penetration of H2 and H2O into the oxide layer (gas barrier function), the oxide layer also acquires the function of suppressing the release of H2 and H2O in the oxide layer. For this reason, it is thought that adding Al to the oxide layer can suppress the desorption of Zn in the oxide layer.
[0041] In the oxide semiconductor layer 12, elements other than those mentioned above are O (oxygen) and inevitable impurities. The inevitable impurities may be contained due to raw materials, materials, manufacturing equipment, and the like. Examples of the inevitable impurities include Pb, Si, Fe, Ni, Ti, Mg, Cr, and Zr. The content of the inevitable impurities in the oxide semiconductor layer 12 is preferably 1 mass % or less for each element, and more preferably 500 mass ppm or less. In this configuration, the content of the In, Zn, and Al in the oxide semiconductor layer 12 can also be considered as a proportion of all elements except O.
[0042] The average thickness of the oxide semiconductor layer 12 can be determined based on the condition that the drain current can be turned off when the oxide semiconductor layer 12 is used as a switching element. The lower limit of the average thickness of the oxide semiconductor layer 12 is preferably 10 nm, more preferably 15 nm. Meanwhile, the upper limit of the average thickness is preferably 60 nm, more preferably 50 nm. In this specification, the "average thickness" refers to the average value of thicknesses at any five points.
[0043] The oxide semiconductor layer 12 is preferably an amorphous layer. Alternatively, it is preferable that at least a part of the oxide semiconductor layer 12 is formed as an amorphous layer. That is, it is preferable that the oxide forming the oxide semiconductor layer 12 is amorphous or at least a part of the oxide is amorphous. Even if the oxide semiconductor layer 12 has such a configuration, it can sufficiently increase the carrier mobility compared to general-purpose amorphous silicon. Furthermore, by having such a configuration, it is possible to easily and reliably increase the optical band gap.
[0044] In general, the denser the oxide layer, the better the gas barrier function. The denser the oxide layer, the more amorphous it is, rather than polycrystalline with many grain boundaries. In oxide has a gas barrier function, but tends to crystallize the oxide layer. On the other hand, the addition of Zn can promote the amorphization of the oxide layer. Al tends to crystallize the part by reacting with H2O to become Al oxide, but Al can promote the amorphization of the oxide layer. For this reason, it is considered that the oxide layer containing In, Zn, and Al promotes the amorphization and exhibits a suitable gas barrier function against H2 and H2O.
[0045] The oxide semiconductor layer 12 can be made into an amorphous layer by controlling the gas pressure to be in the range of 1 mTorr to 5 mTorr, and by subjecting the oxide semiconductor layer 12 to a surface treatment using plasma or a reducing gas after the oxide semiconductor layer 12 is formed.
[0046] The upper limit of the sheet resistance of the oxide semiconductor layer 12 (sheet resistance of the S / D region after surface treatment) is preferably 1.0 kΩ / □, and more preferably 0.5 kΩ / □. When the sheet resistance of the oxide semiconductor layer 12 after surface treatment is equal to or less than the upper limit, the S / D region can be easily and reliably made conductive. The sheet resistance can be a value measured by a four-probe resistance meter.
[0047] The oxide semiconductor layer 12 is formed by a sputtering method using a sputtering target. After the oxide semiconductor layer 12 is formed, it is patterned by photolithography or the like. In addition, immediately after this patterning, it is preferable to perform a heat treatment (pre-annealing treatment) to improve the film quality.
[0048] <Sputtering target> The oxide semiconductor layer 12 can be formed by a sputtering target containing In, Zn, and Al as metal elements, with the contents of In, Zn, and Al relative to the total of all contained metal elements being In: 40 atomic % to 75 atomic %, Zn: 15 atomic % to 45 atomic %, and Al: 0.5 atomic % to 20 atomic %. Elements in the sputtering target other than the above are unavoidable impurities. The contents of each element in the sputtering target can be the same as the ranges described for the oxide semiconductor layer 12.
[0049] The sputtering target material formed in the above sputtering target can be used to form the oxide semiconductor layer 12, and can also be used to form an oxide gas barrier layer described later. The sputtering target material contains the same metal elements as the above sputtering target, and the content of the metal elements is also approximately the same, so that the sputtering target material can have a gas barrier function against H2 and H2O.
[0050] <Sintered body> The sputtering target is formed of a sintered body.
[0051] [Step of forming gate insulating layer] In the step of forming the gate insulating layer 14, the gate insulating layer 14 is formed on the oxide semiconductor layer 12. The gate insulating layer 14 is formed on the oxide semiconductor layer 12 after the pre-annealing treatment.
[0052] Examples of the gate insulating layer 14 include a silicon oxide layer, a silicon nitride layer, a silicon oxynitride layer, and a metal oxide layer such as Al2O3 or Y2O3. The gate insulating layer 14 can be formed by using a CVD method, a PECVD method, or the like. The gate insulating layer 14 may be a single layer or a multilayer body of two or more layers. When the gate insulating layer 14 is a multilayer body of two or more layers, it is preferable that the first layer and the second and subsequent layers have different components.
[0053] The lower limit of the average thickness of the gate insulating layer 14 is preferably 50 nm, more preferably 100 nm. On the other hand, the upper limit of the average thickness of the gate insulating layer 14 is preferably 300 nm, more preferably 250 nm. If the average thickness is less than the lower limit, the withstand voltage of the gate insulating layer 14 may be insufficient. Conversely, if the average thickness exceeds the upper limit, the capacitance of the capacitor formed between the gate electrode 15 and the oxide semiconductor layer 12 may be insufficient, and the drain current may be insufficient. Note that, when the gate insulating layer 14 is a multilayer structure, the "average thickness of the gate insulating layer" refers to the average thickness of the entire gate insulating layer.
[0054] [Step of forming gate electrode] In the step of forming the gate electrode 15, the gate electrode 15 is formed on the gate insulating layer 14. After the gate electrode 15 is formed, the gate insulating layer 14 and the gate electrode 15 are patterned by photolithography or the like.
[0055] (gate electrode) The gate electrode 15 is conductive. The gate electrode 15 is formed, for example, after forming the gate insulating layer 14 and then subjecting the oxide semiconductor layer 12 to a heat treatment (annealing treatment). The gate electrode 15 is not particularly limited, but may be made of a metal having low electrical resistivity, such as Al or Cu, or an alloy of a high-melting-point metal having high heat resistance, such as Mo, Cr, or Ti.
[0056] The lower limit of the average thickness of the gate electrode 15 is preferably 50 nm, and more preferably 80 nm. By setting the average thickness to be equal to or greater than the lower limit, it is possible to suppress an increase in the resistance of the gate electrode 15 and to suppress an increase in power consumption in the gate electrode 15. On the other hand, the upper limit of the average thickness of the gate electrode 15 is preferably 500 nm, and more preferably 400 nm, from the viewpoint of processability and the like.
[0057] [Step of forming protective layer] In the step of forming the protective layer 13, the protective layer 13 containing SiN is formed on the oxide semiconductor layer 12. This step in the present embodiment includes a procedure of forming a first protective layer 131 containing SiOx on the oxide semiconductor layer 12 so as to cover the gate insulating layer 14 and the gate electrode 15, and a procedure of forming a second protective layer 132 containing SiN on the first protective layer 131.
[0058] The first protective layer 131 is formed after patterning the gate insulating layer 14 and the gate electrode 15, and after performing a surface treatment on the oxide semiconductor layer 12. The surface treatment of the oxide semiconductor layer 12 is performed to make the S / D region conductive, and can be performed by, for example, ion implantation, element diffusion, reduction with a reducing gas, plasma treatment, or the like.
[0059] The first protective layer 131 and the second protective layer 132 can be formed by using a CVD method, a PECVD method, etc. After the film formation, contact holes for disposing the source electrode 16 and the drain electrode 17 are formed by photolithography or the like.
[0060] The first protective layer 131 includes SiOx, and the second protective layer 132 includes SiN. That is, the first protective layer 131 is a silicon oxide layer, and the second protective layer 132 is a silicon nitride layer.
[0061] By providing the protective layer 13, it is possible to reduce the influence of the external environment on the oxide semiconductor layer 12, the gate electrode 15, and the like. The second protective layer 132 containing SiN is suitable for reducing the influence of H2O and the like. On the other hand, the second protective layer 132 containing SiN contains a large amount of H2, and may release the H2 due to the thermal history in the manufacturing process. If the released H2 penetrates into the oxide semiconductor layer 12, the electrical characteristics of the thin film transistor 10 may deteriorate. The first protective layer 131 containing SiOx can suppress the penetration of H2, and therefore, by disposing the first protective layer 131 between the oxide semiconductor layer 12 and the second protective layer 132, it is possible to suppress the H2 released from the second protective layer 132 from directly penetrating into the oxide semiconductor layer 12. The thin film transistor 10 further includes the oxide semiconductor layer 12 having a gas barrier function, and therefore can further suppress the penetration of H2 into the oxide semiconductor layer 12.
[0062] [Step of forming electrodes] In the step of forming the electrodes, the source electrode 16 and the drain electrode 17 are formed. Specifically, the source electrode 16 and the drain electrode 17 are formed in the contact holes so that a portion of each of the source electrode 16 and the drain electrode 17 is in contact with the S / D region of the oxide semiconductor layer 12. After being formed, the source electrode 16 and the drain electrode 17 are patterned by photolithography or the like.
[0063] The source electrode 16 and the drain electrode 17 are conductive. The source electrode 16 and the drain electrode 17 are not particularly limited, but may be made of a metal having low electrical resistivity, such as Al or Cu, a high melting point metal having high heat resistance, such as Mo, Cr or Ti, or an alloy of these.
[0064] The source electrode 16 and the drain electrode 17 cover a part of the protective layer 13 and fill the contact holes. By providing them in this manner, the source electrode 16 and the drain electrode 17 are electrically connected to the oxide semiconductor layer 12 at both ends of the channel region of the thin film transistor 10.
[0065] The lower limit of the average thickness of the source electrode 16 and the drain electrode 17 is preferably 100 nm, more preferably 150 nm. By setting the average thickness to be equal to or greater than the lower limit, it is possible to suppress an increase in the resistance of the source electrode 16 and the drain electrode 17, and to suppress an increase in power consumption. The upper limit of the average thickness of the source electrode 16 and the drain electrode 17 is desirably larger than the total thickness of the gate insulating layer 14 and the gate electrode 15, and is preferably 1000 μm, more preferably 800 μm, for example.
[0066] <Advantages> This manufacturing method includes a step of forming an oxide semiconductor layer 12 containing In, Zn, and Al as metal elements on a substrate 11, and a step of forming a protective layer 13 containing SiN on the oxide semiconductor layer 12, so that H2 diffused from the protective layer 13 due to the thermal history in the manufacturing process can be prevented from penetrating into the oxide semiconductor layer 12. Therefore, the obtained thin film transistor 10 has high carrier mobility and excellent operational stability.
[0067] The sputtering target is suitable for producing the oxide semiconductor layer 12.
[0068] [Second embodiment] Hereinafter, another embodiment of the method for manufacturing a thin film transistor will be described, in which the same components as those in the first embodiment are denoted by the same reference numerals and will not be described.
[0069] 2 shows a top-gate type thin-film transistor 20 (hereinafter, also simply referred to as "thin-film transistor 20") obtained by the thin-film transistor manufacturing method (hereinafter, also simply referred to as "the manufacturing method"). The thin-film transistor 20 has an oxide semiconductor layer 22, an oxide gas barrier layer 27, a protective layer 13, a gate insulating layer 14, a gate electrode 15, a source electrode 16, and a drain electrode 17 on a substrate 11. The protective layer 13 includes a first protective layer 131 containing SiOx, and a second protective layer 132 laminated on the first protective layer 131 and containing SiN.
[0070] The thin film transistor 20 includes a step of forming an oxide semiconductor layer 22 on a substrate 11, a step of forming an oxide gas barrier layer 27 containing In, Zn, and Al as metal elements on the oxide semiconductor layer 22, and a step of forming a protective layer 13 containing SiN on the oxide gas barrier layer 27. The manufacturing method includes a step of forming a gate insulating layer 14 on the oxide semiconductor layer 22 and a step of forming a gate electrode 15 on the gate insulating layer 14 between the step of forming the oxide semiconductor layer and the step of forming the oxide gas barrier layer. The manufacturing method also includes a step of forming a source electrode 16 and a drain electrode 17 after the step of forming the protective layer 13.
[0071] [Step of forming oxide semiconductor layer] In the step of forming an oxide semiconductor layer, an oxide semiconductor layer 22 is formed on a substrate 11. The metal elements contained in this oxide semiconductor layer 22 are not particularly limited, and the oxide semiconductor layer 22 may not contain any one or all of In, Zn, and Al.
[0072] Next, the gate insulating layer 14 and the gate electrode 15 are formed on the oxide semiconductor layer 22 .
[0073] [Step of forming oxide gas barrier layer] In the step of forming the oxide gas barrier layer, the oxide gas barrier layer 27 containing In, Zn and Al as metal elements is formed on the oxide semiconductor layer 22. Specifically, the oxide gas barrier layer 27 is formed so as to cover the gate insulating layer 14 and the gate electrode 15 formed on the oxide semiconductor 22.
[0074] The oxide gas barrier layer 27 contains In, Zn, and Al as metal elements. The content of each of the In, Zn, and Al relative to the total of these metal elements can be the same as that of the oxide semiconductor layer 12 described in the first embodiment. The oxide gas barrier layer 27 is preferably an amorphous layer. Alternatively, it is preferable that at least a part of the oxide gas barrier layer 27 is formed as an amorphous layer. The oxide gas barrier layer 27 functions as a barrier layer for H2 and H2O gases. The Al suppresses the Zn from being desorbed from the oxide gas barrier layer 27.
[0075] [Step of forming protective layer] In the step of forming the protective layer 13, the protective layer 13 containing SiN is formed on the oxide gas barrier layer 27. This step in the present embodiment includes a procedure of forming a first protective layer 131 containing SiOx on the oxide gas barrier layer 27, and a procedure of forming a second protective layer 132 containing SiN on the first protective layer 131.
[0076] After the protective layer 13 is formed, contact holes are formed, and a source electrode 16 and a drain electrode 17 are formed in the contact holes.
[0077] <Advantages> The manufacturing method includes a step of forming an oxide semiconductor layer 22 on a substrate 11, a step of forming an oxide gas barrier layer 27 containing In, Zn, and Al as metal elements on the oxide semiconductor layer 22, and a step of forming a protective layer 13 containing SiN on the oxide gas barrier layer 27. That is, the manufacturing method can obtain a thin film transistor 20 in which the oxide gas barrier layer 27 containing In, Zn, and Al is formed between the oxide semiconductor layer 22 and the protective layer 13 containing SiN. Therefore, it is possible to suppress the intrusion of H2 diffused from the protective layer 13 due to the thermal history in the manufacturing process into the oxide semiconductor layer 22.
[0078] [Other embodiments] The above-mentioned embodiment does not limit the configuration of the present invention. Therefore, the above-mentioned embodiment may omit, replace or add components of each part of the above-mentioned embodiment based on the description in this specification and common general technical knowledge, and it should be understood that all of these are within the scope of the present invention.
[0079] The oxide semiconductor layer of the thin film transistor (second embodiment) having an oxide gas barrier layer may contain In, Zn, and Al. When the oxide semiconductor layer 12 containing In, Zn, and Al is used, as shown in FIG. 3, the oxide gas barrier layer 27 of the thin film transistor 30 may be disposed in the protective layer 13 (between the first protective layer 131 and the second protective layer 132).
[0080] The specific configuration of the thin film transistor is not limited to the configurations shown in Figures 1, 2, and 3. For example, the protective layer may be only a protective layer containing SiN. The thin film transistor may be a bottom gate type.
[0081] In the thin film transistor, another layer such as a buffer layer may be provided between the substrate and the oxide semiconductor layer to improve adhesion or as a buffer material. EXAMPLES
[0082] The present invention will be described in detail below based on examples. However, the present invention should not be construed as being limited to the descriptions of these examples.
[0083] Samples 1 to 14 were prepared to evaluate the gas barrier resistance of oxide layers containing In, Zn, and Al against H2 and HO. For each sample, a second protective layer (containing SiN) with a thickness of 150 nm was formed on a silicon substrate with a thickness of 525 μm, a first protective layer (containing SiO) with a thickness of 200 nm was formed on this second protective layer, and an oxide layer with a different content of In, Zn, and Al was formed on this first protective layer.
[0084] The deposition conditions and thickness (film thickness) of the oxide layer of each sample are shown below. (1) Samples 1 to 12 Film formation method: DC (direct current) sputtering method Equipment: ULVAC CS200 Film forming temperature: room temperature Gas pressure: 1mTorr Carrier gas: Ar Oxygen partial pressure: 100 x O2 / (Ar+O2) = 4% by volume Deposition power density: 2.55W / cm 2 Film thickness: 15 nm (2) Sample 13 and Sample 14 Film formation method: DC (direct current) sputtering method Equipment: ULVAC CS200 Film forming temperature: room temperature Gas pressure: 1mTorr Carrier gas: Ar Oxygen partial pressure (first partial pressure): 100 × O2 / (Ar+O2) = 0% by volume Oxygen partial pressure (second partial pressure): 100 × O2 / (Ar+O2) = 4% by volume Deposition power density: 2.55W / cm 2 Film thickness: 10 nm was formed at the first partial pressure, and then 15 nm was formed at the second partial pressure (total 25 nm).
[0085] The gas barrier resistance of each sample was judged from the amount of H2 and H2O measured by TDS (Thermal Desorption Spectrometry) analysis.
[0086] The gas barrier resistance was evaluated by TDS analysis as follows. (1)H2: The sample was judged as A, B or C depending on whether the ion current [A] was exceeded within the temperature range of 300°C to 450°C. "A" indicates good H2 gas barrier resistance, "C" indicates poor H2 gas barrier resistance, and "B" indicates an intermediate evaluation between A and C. 1E -9 [A]Super:C 5E -10 [A]Super:B 5E -10 [A] Below: A (2)H2O: Based on the relationship between the temperature range and ion current [A] below, the product was judged as A, B or C. "A" indicates good gas barrier resistance to HO, "C" indicates poor gas barrier resistance to HO, and "B" indicates an intermediate evaluation between A and C. 1E -9 [A] Temperature exceeds 300℃ or more and less than 350℃: C 1E -9 [A] Temperatures exceeding 350℃ or more and less than 400℃: B 1E -9 [A] Temperatures exceeding 400℃ or more and less than 450℃: A
[0087] After the TDS analysis, the resistance value of the oxide layer of each sample was measured. Resistance values less than 100 Ωcm were rated "A," and resistance values of 100 Ωcm or more were rated "B." Oxide layers rated "B" are considered difficult to use as semiconductor layers.
[0088] The measurements were carried out as follows. (1) Measurement of ion current Analytical equipment: TDS1200II (manufactured by Electronic Science Co., Ltd.) Temperature conditions: Set temperature USC temperature RT-500℃ (60℃ / min) Sample stage: Quartz stage ·Quadrupole Mass Spectrometer Ionization method: Electron ionization Measurement mode: SIM mode (selective mass number measurement mode) (2) Resistance measurement -Analyzer: MCP-HT450 (manufactured by Nitto Seiko Analytech Co., Ltd.) Measurement method: constant voltage application, leakage current measurement method
[0089] The contents and measurement results of In, Zn, and Al for each sample are shown in Table 1. In Table 1, the numerical values are the contents of In, Zn, and Al, and "-" indicates that they are not contained.
[0090] [Table 1]
[0091] From Table 1, it can be seen that Samples 8, 9, 10 and 14 all received high ratings.
[0092] Next, a thin film transistor (sample 15) having an oxide semiconductor layer containing 65 atomic % In, 35 atomic % Zn, and 0 atomic % Al, a thin film transistor (sample 16) having an oxide semiconductor layer containing 65 atomic % In, 28 atomic % Zn, and 7 atomic % Al, and a thin film transistor (sample 27) having an oxide semiconductor layer containing 64 atomic % In, 35 atomic % Zn, and 0.7 atomic % Al were fabricated. The Id-Vg characteristics of samples 15, 16, and 27, and the light stress resistance of samples 15 and 16 were compared. The results are shown in Figs. 4 to 11.
[0093] The Id-Vg characteristics (drain current (Id) - gate voltage (Vg) characteristics) of Sample 15, Sample 16, and Sample 27 were compared with a channel length of 10 μm. The Id-Vg characteristics were measured three times for each sample. The results for Sample 15 are shown in Figure 4, those for Sample 16 in Figure 5, and those for Sample 27 in Figure 10.
[0094] Comparing Figures 4, 5, and 10, in the vicinity of Vg0 [V], the slope decreases (approaching parallel to the vertical axis) in the order of Figure 4 (sample 15), Figure 10 (sample 27), and Figure 5 (sample 16). From this, it is believed that the inclusion of Al and increasing the Al content can improve the transfer characteristics (Id-Vg characteristics).
[0095] Next, the light stress resistance of Sample 15 and Sample 16 were compared. To evaluate the light stress resistance, a stress application test (NBTIS test) was conducted for each sample (thin film transistor: TFT) in which a negative bias was continuously applied to the gate electrode while irradiating the sample with light (white light), simulating the environment (stress) when an actual liquid crystal panel is driven, and the change in threshold voltage (Vth) before and after the stress application (threshold voltage shift amount: ΔVth) was used as an index of light stress resistance in the TFT characteristics. Light stress resistance is one of the important characteristics in driving a liquid crystal display. The NBTIS test was conducted under the following conditions. Gate voltage: -20V Source-drain voltage: 10V Substrate temperature: 60℃ Stress application time: 2 hours Light intensity during light stress: 25000nit Light source during light stress: White LED (Light Emitting Diode)
[0096] The ΔVth of sample 15 was 3.0 [V], and the ΔVth of sample 16 was 1.8 [V]. The results of the light stress resistance of sample 15 are shown in FIG. 6, and the results of the light stress resistance of sample 16 are shown in FIG. 7. Comparing FIG. 6 and FIG. 7, in the vicinity of Vg0 [V], the variation in the horizontal axis direction of sample 15 is relatively large, and the inclination (tilt angle) with respect to the vertical axis is relatively large. In sample 16, the variation in the horizontal axis direction is relatively small, and the inclination with respect to the vertical axis is relatively small. This shows that the inclusion of Al improves the light stress resistance. The numbers on the left in the graphs (FIG. 6 and FIG. 7) indicate the application time of the light stress. 0 sec is the start of the application of the light stress, and measurements were taken after 30 sec of application, then 100 sec, and then 300 sec, 1000 sec, 3600 sec, and 7200 sec, respectively.
[0097] Samples with different channel lengths (length of channel region) were prepared for a thin film transistor having an oxide semiconductor layer containing In: 65 atomic %, Zn: 35 atomic %, and Al: 0 atomic %, a thin film transistor having an oxide semiconductor layer containing In: 65 atomic %, Zn: 28 atomic %, and Al: 7 atomic %, and a thin film transistor having an oxide semiconductor layer containing In: 64 atomic %, Zn: 35 atomic %, and Al: 0.7 atomic %, and the channel length dependency was compared. The metal elements contained and the channel length of each sample number are shown in Table 2. Note that the above-mentioned sample 15 and sample 19 in Table 2 are the same sample, the above-mentioned sample 16 and sample 24 in Table 2 are the same sample, and the above-mentioned sample 27 and sample 30 in Table 2 are the same sample.
[0098] [Table 2]
[0099] The transmission characteristics were measured and compared for Samples 17 to 26, and Samples 28 to 32. The results for Samples 17 to 21 are shown in FIG. 8, the results for Samples 22 to 26 in FIG. 9, and the results for Samples 28 to 32 in FIG.
[0100] 8, 9, and 11, in the samples with a channel length of 8 μm or more, the slope decreases (approaching parallel to the vertical axis) in the order of FIG. 8, FIG. 11, and FIG. 9 near Vg0 [V]. This suggests that the inclusion of Al and the increase in the Al content can improve the transfer characteristics (Id-Vg characteristics). In addition, when comparing Sample 17, Sample 22, and Sample 28 with a channel length of 5 μm, a large shift (deviation) occurs in the horizontal axis direction near Vg0 [V] in Sample 17, whereas the shift is small in Samples 22 and 28. This suggests that the inclusion of Al in the oxide semiconductor layer can reduce the size of thin film transistors. [Industrial Applicability]
[0101] As described above, the method for manufacturing a thin film transistor according to one embodiment of the present disclosure can provide a thin film transistor that has high operational stability and is suitable for use in organic EL displays and the like. [Explanation of symbols]
[0102] 10,20,30 Thin-film transistor 11 Substrate 12,22 Oxide semiconductor layer 13 Protective layer 131 1st protective layer 132 Second protective layer 14 Gate insulating layer 15 Gate electrode 16 Source electrode 17 Drain electrode 27 Oxide gas barrier layer< / al> < / zn> < / in>
Claims
1. A method for manufacturing a thin film transistor having at least an oxide semiconductor layer, a protective layer, a gate insulating layer, a gate electrode, a source electrode, and a drain electrode on a substrate, comprising the steps of: forming the oxide semiconductor layer containing In, Zn and Al as metal elements on the substrate; forming the protective layer containing SiN on the oxide semiconductor layer; A method for manufacturing a thin film transistor comprising:
2. A method for manufacturing a thin film transistor having at least an oxide semiconductor layer, an oxide gas barrier layer, a protective layer, a gate insulating layer, a gate electrode, a source electrode, and a drain electrode on a substrate, comprising the steps of: forming the oxide semiconductor layer on the substrate; forming an oxide gas barrier layer containing In, Zn and Al as metal elements on the oxide semiconductor layer; forming the protective layer containing SiN on the oxide gas barrier layer; A method for manufacturing a thin film transistor comprising:
3. The method for producing a thin film transistor according to claim 2 , wherein the oxide semiconductor layer contains In, Zn and Al as metal elements.
4. The content of the above metal elements relative to the total is In: 40 atomic % or more and 75 atomic % or less, Zn: 15 atomic % or more and 45 atomic % or less, and Al: 0.5 atomic% or more and 20 atomic% or less 4. The method for producing a thin film transistor according to claim 1, 2 or 3, wherein
5. The method for producing a thin film transistor according to claim 1 , wherein the oxide semiconductor layer is an amorphous layer.
6. The method for producing a thin film transistor according to claim 3 , wherein at least one of the oxide semiconductor layer and the oxide gas barrier layer is an amorphous layer.
7. The oxide semiconductor layer is treated with H 2 and H 2 4. The method for producing a thin film transistor according to claim 1, wherein the barrier layer is formed against at least one of oxygen and oxygen.
8. The oxide gas barrier layer is 2 and H 2 4. The method for producing a thin film transistor according to claim 2, wherein the barrier layer is formed against at least one of oxygen and oxygen.
9. A sputtering target for forming at least one of an oxide semiconductor layer and an oxide gas barrier layer used in a thin film transistor, comprising: Contains In, Zn and Al as metal elements; The content of the In, the Zn and the Al relative to the total of all the metal elements contained is In: 40 atomic % or more and 75 atomic % or less, Zn: 15 atomic % or more and 45 atomic % or less, and Al: 0.5 atomic% or more and 20 atomic% or less A sputtering target comprising:
10. A sintered body for forming the sputtering target according to claim 9.
Citation Information
Patent Citations
Electronic display
JP2009021554A
Thin film field effect transistor and display using the same
JP2009212497A
Semiconductor device and touch panel
JP2016201539A
Oxide semiconductor thin film for display, thin film transistor for display, and sputtering target
JP2020194945A
Semiconductor device
WO2020178654A1