Soft magnetic alloy material and inductor using the same
A Fe-Co-P soft magnetic alloy with controlled nanocrystal sizes addresses the challenges of maintaining high saturation magnetization and uniform crystal growth, enhancing electromagnetic properties in inductors and other magnetic products.
Patent Information
- Application Number
- JP2024063341
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-18
- Filing Date
- 2024-04-10
- Publication Date
- 2024-10-30
AI Technical Summary
Existing Fe-based soft magnetic materials face challenges in maintaining high saturation magnetization characteristics and uniform nanocrystal growth due to excessive content of elements like Nb, which impairs electromagnetic properties.
A soft magnetic alloy material composed of Fe, Co, and P, with specific atomic percentage ranges and controlled nanocrystal sizes, is developed to improve amorphousness and electromagnetic characteristics.
The alloy maintains high saturation magnetization and improves electromagnetic properties by controlling nanocrystal growth and enhancing amorphousness, achieving superior performance in inductors and other magnetic products.
Smart Images

Figure 2024154386000005 
Figure 2024154386000006 
Figure 2024154386000007
Abstract
Description
[Technical field]
[0001] The present invention relates to a soft magnetic alloy material and an inductor using the same. [Background technology]
[0002] Recently, with the miniaturization and high integration of electronic elements, power supply voltages have been decreasing, and as a result, the current value has been increasing to transmit the same amount of power. Therefore, metal inductors that maintain their inductor performance even at high currents have been used, and recently, materials that have high current characteristics among metals, in other words, materials with high saturation magnetization (Ms) values, are being used in order to use higher currents.
[0003] In existing Fe-based soft magnetic materials, the electromagnetic properties have been improved by increasing the content of elements such as Nb and controlling the size of nanocrystals in the material. However, when the content of elements such as Nb is increased, the content of metals such as Fe is reduced, making it difficult to improve the Ms value.
[0004] Also, if the content of metals such as Fe is too high, the Ms value can be increased, but there is a problem that nanocrystals grow locally during heat treatment, which causes uneven crystal growth and impairs the electromagnetic properties of the soft magnetic material. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2018-206836 A Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention has been made in view of the problems of the above-mentioned prior art, and an object of the present invention is to provide a soft magnetic alloy material that can improve the amorphous ratio of the initial alloy and maintain high saturation magnetization characteristics while improving electromagnetic characteristics. Another object of the present invention is to provide an inductor using the above soft magnetic alloy material.
[0007] However, the problems to be solved by the present invention are not limited to the above-mentioned problems, and can be variously extended within the scope of the technical idea included in the present invention.
Means for Solving the Problems
[0008] The soft magnetic alloy material according to one aspect of the present invention made to achieve the above object contains nanocrystals and amorphous, contains Fe (iron), Co (cobalt), and P (phosphorus), and is represented by the following compositional formula 1. When the average Co content in the amorphous is Co(a) (at%) and the average Co content in the nanocrystals is Co(c) (at%), Co(c) - Co(a) > 0. Compositional formula 1 Fe a Co b P c M d In the compositional formula 1, a, b, c, and d respectively represent the atomic percentage contents (at%) of the corresponding elements, 0 < a ≦ 90, 0 < b ≦ 20, 0 < c ≦ 10, 0 < d ≦ 20, a + b + c + d = 100, and M includes Si, B, Cu, Cr, C, Ni, Al, Mn, Ag, Zn, Sn, As, Sb, Bi, N, O, S, or a combination thereof.
[0009] When the average P content in the amorphous is P(a) (at%) and the average P content in the nanocrystals is P(c) (at%), P(a) - P(c) > 0 may be satisfied. In the above, 0.4 ≦ Co(c) - Co(a) ≦ 1.5 may be satisfied. In the above, 0.5 ≦ P(a) - P(c) ≦ 2.5 may be satisfied. In the above, 2 ≦ b ≦ 16 may be satisfied. In the above, 1 ≦ c ≦ 6 may be satisfied. The M does not contain Nb. The average crystal size of the nanocrystals may be 20 nm or less.
[0010] A soft magnetic alloy material according to one aspect of the present invention made to achieve the above object includes nanocrystals and amorphous, contains Fe (iron), Co (cobalt), and P (phosphorus), is represented by the following Composition Formula 1, and when the average P content in the amorphous is P(a) (at%) and the average P content in the nanocrystals is P(c) (at%), P(a) - P(c) > 0. Composition Formula 1 Fe a Co b P c M d In the Composition Formula 1, a, b, c, and d represent the atomic percentage contents (at%) of the corresponding elements, 0 < a ≦ 90, 0 < b ≦ 20, 0 < c ≦ 10, 0 < d ≦ 20, a + b + c + d = 100, and the M includes Si, B, Cu, Cr, C, Ni, Al, Mn, Ag, Zn, Sn, As, Sb, Bi, N, O, S, or a combination thereof.
[0011] When the average Co content in the amorphous is Co(a) (at%) and the average Co content in the nanocrystals is Co(c) (at%), Co(c) - Co(a) > 0 may be satisfied. In the above, 0.5 ≦ P(a) - P(c) ≦ 2.5 may be satisfied. In the above, 0.4 ≦ Co(c) - Co(a) ≦ 1.5 may be satisfied. In the above, 2 ≦ b ≦ 16 may be satisfied. In the above, 1 ≦ c ≦ 6 may be satisfied. The M does not contain Nb. The average crystal size of the nanocrystals may be 20 nm or less.
[0012] A method for manufacturing a soft magnetic alloy material according to an aspect of the present invention made to achieve the above object includes: (1) a step of mixing raw materials; (2) a step of melting the mixed raw materials; (3) a step of rapidly cooling the melted raw materials to produce an amorphous soft magnetic alloy; and (4) a step of heat-treating the amorphous soft magnetic alloy. The amorphous ratio of the amorphous soft magnetic alloy may be 95% or more.
[0013] An inductor according to an aspect of the present invention made to achieve the above object includes a body including a magnetic material including a soft magnetic alloy material, a coil disposed in the body, and an external electrode disposed on an outer surface of the body. The soft magnetic alloy material includes nanocrystals and amorphous, includes Fe (iron), Co (cobalt), and P (phosphorus), is represented by the following Composition Formula 1. When the average Co content in the amorphous is Co(a) (at%) and the average Co content in the nanocrystals is Co(c) (at%), Co(c) - Co(a) > 0, or when the average P content in the amorphous is P(a) (at%) and the average P content in the nanocrystals is P(c) (at%), P(a) - P(c) > 0. Composition Formula 1 Fe a Co b P c M d In the Composition Formula 1, a, b, c, and d respectively indicate the atomic percentage contents (at%) of the corresponding elements, 0 < a ≤ 90, 0 < b ≤ 20, 0 < c ≤ 10, 0 < d ≤ 20, a + b + c + d = 100, and M includes Si, B, Cu, Cr, C, Ni, Al, Mn, Ag, Zn, Sn, As, Sb, Bi, N, O, S, or a combination thereof.
[0014] The coil includes a support member, an upper coil and a lower coil respectively disposed on the upper and lower surfaces of the support member, and the upper coil and the lower coil can be electrically connected through a via penetrating the support member. The body includes a molded portion, a cover portion arranged on one side of the molded portion, and a core protruding from one side of the molded portion, the coil being arranged between the one side of the molded portion and the cover portion, and the core may pass through the coil. The body may include a plurality of magnetic sheets containing the magnetic material. Effect of the Invention
[0015] The soft magnetic alloy material according to the present invention has the effect of improving the amorphous ratio of the initial alloy and improving the electromagnetic properties while maintaining high saturation magnetization characteristics.
[0016] However, the various and beneficial advantages and effects of the present invention are not limited to the above, and will be more easily understood in the course of describing specific embodiments of the present invention. [Brief description of the drawings]
[0017] [Figure 1] 1 shows a TEM photograph and a graph showing a line profile of a soft magnetic alloy material according to an embodiment of the present invention, which is subjected to spot quantitative analysis by TEM analysis. [Diagram 2] 1 shows a TEM photograph and a graph showing a line profile of a soft magnetic alloy material according to an embodiment of the present invention, which is subjected to spot quantitative analysis by TEM analysis. [Diagram 3] 2 is a graph showing the amorphous rate of an amorphous soft magnetic alloy depending on the Co metal content (at %). [Figure 4] 2 is a graph showing the amorphous rate of an amorphous soft magnetic alloy depending on the Co metal content (at %). [Diagram 5] 2 is a graph showing the amorphous rate of an amorphous soft magnetic alloy depending on the Co metal content (at %). [Figure 6] 2 is a graph showing the amorphous rate of an amorphous soft magnetic alloy depending on the Co metal content (at %). [Figure 7] FIG. 2 is a transparent perspective view of an inductor according to an embodiment. [Figure 8]8 is a cross-sectional view showing a schematic cross section taken along the line II' of FIG. 7. [Figure 9] FIG. 9 is an enlarged view of region A in FIG. 8. [Figure 10] FIG. 13 is a transparent perspective view of an inductor according to another embodiment. [Figure 11] 11 is a cross-sectional view showing a schematic cross section taken along the line II-II' of FIG. 10. FIG. [Figure 12] FIG. 13 is a transparent perspective view of an inductor according to another embodiment. [Figure 13] 13 is a cross-sectional view showing a schematic cross section taken along the line III-III' in FIG. 12. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, the present invention will be described in detail with reference to the drawings so that a person having ordinary skill in the art to which the present invention pertains can easily carry out the present invention. In the drawings, parts unnecessary for the explanation are omitted in order to clearly explain the present invention, and the same or similar components are given the same reference numerals throughout the specification. In addition, the drawings are merely for the purpose of making it easy to understand the embodiments disclosed in the present specification, and the technical ideas disclosed in the specification are not limited by the drawings, and all modifications, equivalents, or alternatives included within the ideas and technical scope of the present invention are included. In addition, some components are exaggerated, omitted, or shown roughly in the drawings, and the size of each component does not completely reflect the actual size.
[0019] Throughout the specification, when a part is described as "comprising" a certain element, this means that it further includes other elements, not excluding other elements, unless specifically stated to the contrary.
[0020] Throughout the specification, the term "stacking direction" refers to the direction in which the components are stacked one on top of the other, which is the "thickness direction" perpendicular to the broad surface (principal surface) of the sheet-like component, and corresponds to the T-axis direction in the drawings. And the term "lateral" refers to the direction extending parallel to the broad surface (principal surface) from the periphery of the sheet-like component, which is the "planar direction", and corresponds to the L-axis direction in the drawings. And the W-axis direction in the drawings is the "width direction."
[0021] Hereinafter, various embodiments and modifications will be described in detail with reference to the drawings.
[0022] [Soft magnetic alloy material]
[0023] The soft magnetic alloy material according to one embodiment includes nanocrystalline and amorphous phases, and includes Fe (iron), Co (cobalt), and P (phosphorus).
[0024] The soft magnetic alloy material according to one embodiment is represented by the following composition formula 1.
[0025] [Composition formula 1] Fe a Co b P c M d In the composition formula 1, a, b, c, and d each represent the atomic percentage content (at%) of the corresponding element, and <a≦90、0<b≦20、0<c≦10、0<d≦20、a+b+c+d=100である。 M includes Si, B, Cu, Cr, C, Ni, Al, Mn, Ag, Zn, Sn, As, Sb, Bi, N, O, S, or combinations thereof.
[0026] In one embodiment, M includes B, P, Cu, or a combination thereof.
[0027] In one embodiment, M does not include Nb.
[0028] In the composition formula 1, a represents the atomic percentage content of Fe (iron) metal, and it is preferable that 70≦a≦80. If a is less than 70, the saturation magnetization value is low and the high current characteristics may be poor, and if a exceeds 80, there is a problem that it is difficult to improve the amorphous nature of the initial alloy before heat treatment, that is, the amorphous soft magnetic alloy.
[0029] In the composition formula 1, b represents the atomic percentage content of Co (cobalt) metal, and it is preferable that 2≦b≦16. When this range is satisfied, the amorphousness of the amorphous soft magnetic alloy can be effectively improved.
[0030] In the composition formula 1, c represents the atomic percentage content of P (phosphorus) element, and it is preferable that 1≦c≦6.
[0031] The soft magnetic alloy material contains P element in the above content range instead of Nb element, so that the size of nanocrystals can be adjusted to realize a material with excellent electromagnetic properties.
[0032] In the composition formula 1, it is preferable that 5≦b+c≦20.
[0033] In the composition formula 1, it is preferable that 10≦d≦15.
[0034] As a specific example, the composition formula 1 is Fe 75.2 Co8Si2B 12 P2Cu 0.8 , Fe 75.2 Co8Si2B 11 P3Cu 0.8 , Fe 75.2 Co8Si2B 10 P4Cu 0.8 , Fe 75.2 Co8Si1B 10 P5Cu 0.8 , Fe 75.2 Co8Si1B 10 P6Cu 0.8 may be also possible.
[0035] In one embodiment of the soft magnetic alloy material, when the average Co content in the amorphous portion is Co(a) (at%) and the average Co content in the nanocrystals is Co(c) (at%), Co(c)-Co(a)>0; or when the average P content in the amorphous portion is P(a) (at%) and the average P content in the nanocrystals is P(c) (at%), P(a)-P(c)>0.
[0036] In one embodiment, the soft magnetic alloy material may be Co(c)-Co(a)>0 and P(a)-P(c)>0.
[0037] Co(a) means the average content (at%) of Co element with respect to all atoms constituting the amorphous portion of the soft magnetic alloy material, and Co(c) means the average content (at%) of Co element with respect to all atoms constituting the nanocrystalline portion of the soft magnetic alloy material.
[0038] P(a) means the average content (at%) of P element with respect to all atoms constituting the amorphous portion of the soft magnetic alloy material, and P(c) means the average content (at%) of P element with respect to all atoms constituting the nanocrystalline portion of the soft magnetic alloy material.
[0039] 1 and 2 are line profile diagrams showing quantitative spot analysis by TEM analysis of a soft magnetic alloy material according to an embodiment. For reference, the boundary between the amorphous portion and the nanocrystalline portion is defined by dividing the light and dark areas by a method such as binarizing the transmission electron microscope (TEM) image. In Figs. 1 and 2, the relatively bright areas correspond to nanocrystalline phase, and the relatively dark areas correspond to the amorphous phase.
[0040] Referring to FIGS. 1 and 2, Co(a) and Co(c), or P(a) and P(c), are measured by line analysis using an Energy Disperse X-Ray Spectrometer (EDS) installed in a Transmission Electron Microscope (TEM).
[0041] Specifically, using the surface of any one nanocrystalline particle as a reference, a line profile was quantitatively analyzed over a 20 nm area inside the nanocrystalline particle and a 200 nm area outside the particle, and the maximum value inside the nanocrystalline particle was compared with the maximum value in the amorphous portion.
[0042] In order to measure the average, the above-described analysis is repeated for 5 or more points, and the average value is calculated.
[0043] 1 and 2, it can be seen that the soft magnetic alloy material according to one embodiment contains Co metal, and contains P element having a relatively small atomic weight instead of Nb element, so that P is more abundant in the amorphous phase than in the nanocrystals, and Co is more abundant in the nanocrystals than in the amorphous phase.
[0044] In one embodiment, 0.4≦Co(c)−Co(a)≦1.5 is preferable. If the Co(c)−Co(a) value is less than 0.4, it is difficult to improve the amorphous nature of the initial amorphous soft magnetic alloy before heat treatment, and if the Co(c)−Co(a) value is more than 1.5, there is a problem that the nanocrystals grow non-uniformly during the heat treatment of the nanocrystals.
[0045] In one embodiment, 0.5≦P(a)-P(c)≦2.5 is preferable. If the P(a)-P(c) value is less than 0.5, it may be difficult to control the size of the nanocrystals, resulting in poor electromagnetic properties, and if the P(a)-P(c) value is more than 2.5, the nanocrystal fraction is low, resulting in problems in achieving Ms.
[0046] The nanocrystals of the soft magnetic alloy material may be amorphous grains.
[0047] In one embodiment, the average crystal size of the nanocrystals of the soft magnetic alloy material is 20 nm or less. When a crystalline phase containing Fe is formed by including Co metal, the soft magnetic alloy material can delay the growth of the crystalline phase, thereby significantly improving the amorphousness of the amorphous soft magnetic alloy, which is the initial alloy before heat treatment.
[0048] As an example, the average crystal size of nanocrystals can be calculated using the Scherrer equation using the full width at half maximum (FWHM) of the main peak in the XRD graph.
[0049] As an example, the average size of the nanocrystals may be determined by measuring the maximum long axis of at least 100 nanocrystals in a scanning electron microscope (SEM) image of a cross section of a soft magnetic alloy material, creating a size distribution curve, and calculating D50 to determine the average size.
[0050] The soft magnetic alloy material described above can significantly improve the amorphousness of the amorphous soft magnetic alloy, which is the initial alloy before heat treatment, by delaying the growth of the crystalline phase containing Fe, including Co metal, when the crystalline phase is formed.
[0051] In addition, the soft magnetic alloy material does not contain Nb element, but instead contains P element, which has a relatively smaller atomic weight than Nb, and after heat treatment, the P element exists more in amorphous form than in nanocrystals. As a result, the P element acts as an inhibitor that prevents the growth of nanocrystals, thereby adjusting the size of the nanocrystals to a certain size or less, thereby improving electromagnetic properties such as magnetic permeability and core loss.
[0052] [Method of manufacturing soft magnetic alloy material]
[0053] A method for manufacturing a soft magnetic alloy material according to one embodiment includes the steps of: (1) mixing raw materials; (2) melting the mixed raw materials; (3) rapidly cooling the molten raw materials to produce an amorphous soft magnetic alloy; and (4) heat treating the amorphous soft magnetic alloy.
[0054] Step (1) is a step of preparing, weighing, and mixing raw materials. The raw materials may be metals or alloys. The raw materials are weighed so as to finally obtain a soft magnetic alloy material having a desired composition. As an example, the raw materials can be mixed using an arc melting method, but the method is not limited thereto.
[0055] In step (2), the mixed raw materials are melted to obtain a molten metal. The melting temperature is determined taking into consideration the melting points of the metals, and is, for example, 1300°C or higher or 1450°C or higher.
[0056] In step (3), the molten raw material is quenched to produce an amorphous soft magnetic alloy. For example, the quenching is performed using a water atomization method or a gas atomization method.
[0057] The amorphous soft magnetic alloy is in a state where the raw materials of the alloy are weighed, mixed, melted, and quenched. The amorphous soft magnetic alloy may have nanocrystals formed in part.
[0058] Step (4) is a step of producing a soft magnetic alloy material containing nanocrystals and amorphous by heat-treating the amorphous soft magnetic alloy, for example, at a temperature of 350 to 500° C. for 10 to 60 minutes.
[0059] In one embodiment, the amorphous soft magnetic alloy may have an amorphous ratio of 95% or more as calculated by the following Equation 1:
[0060] [Formula 1] Amorphous ratio (%) = [Ia / (Ic+Ia)] x 100
[0061] In the above formula 1, Ic is the sum of integral values of scattering intensity of crystalline peaks in the X-ray diffraction analysis spectrum of the amorphous soft magnetic alloy, and Ia is the sum of integral values of scattering intensity of amorphous halo in the X-ray diffraction analysis spectrum of the amorphous soft magnetic alloy.
[0062] The amorphous rate of an amorphous soft magnetic alloy is calculated based on a graph obtained by X-ray diffraction spectroscopy. From the X-ray diffraction analysis spectrum, the relationship between the wavelength λ and incident angle θ of the incident X-rays and the lattice spacing d is 2d·sinθ=nλ, which is called the Bragg equation. With this, the lattice spacing d can be calculated when the incident angle is determined.
[0063] However, in amorphous materials, random arrangements rather than regular atomic arrangements appear, so multiple X-ray diffraction patterns do not appear at specific wavelengths, and a wide halo pattern appears in the diffraction angle range of 15° to 35°. If there are no peaks at specific angles in the diffraction angle range of 10° to 60° and a diffuse halo pattern appears, the material can be determined to be 100% amorphous. However, the surface of the amorphous soft magnetic alloy exposed to the X-rays must not contain any contaminants other than organic matter. Only results measured under conditions without factors that affect the diffraction pattern are highly reliable.
[0064] If crystals exist in an amorphous soft magnetic alloy, one or more crystalline peaks will exist within the range of the measured diffraction angle. The presence of a peak means that, on an X-ray diffraction diagram in which the maximum intensity in the range of diffraction angles 2θ=5° to 50° in an XRD pattern graph is taken as the total area on the vertical axis, the peak can be recognized at least with the naked eye, or the waveform processor can recognize the peak as clearly distinguished from background noise.
[0065] At this time, if the amorphous ratio is low, the halo region will be reduced, and there will be no halo region in materials with an amorphous ratio of 0%. When crystalline and amorphous materials are mixed, the amorphous ratio can be calculated by calculating the relative ratio of the area of the crystalline peak and the area of the halo region in a graph consisting of the intensity and diffraction angle range.
[0066] 3 to 6 are graphs showing the amorphous ratio of an amorphous soft magnetic alloy depending on the content (at%) of Co metal. Referring to Fig. 3 to Fig. 6, when the above-described Co metal is contained in a soft magnetic alloy material within a specific numerical range, the amorphous ratio of the amorphous soft magnetic alloy becomes 95% or more, and high amorphousness can be realized. The amorphous soft magnetic alloy that has achieved high amorphousness has the advantage that it has low magnetic loss when it is later heat-treated and used in magnetic products such as inductors.
[0067] [Inductor]
[0068] An example of an inductor 100 including a magnetic material containing the soft magnetic alloy material described above will be described below. Types of inductors can include thin film inductors, laminated inductors, wire-wound inductors, and wound inductors. In the following, a thin film inductor will be described first.
[0069] Fig. 7 is a schematic view of a see-through perspective view of a thin film inductor according to an embodiment, and Fig. 8 is a schematic view of a cut surface along the II' direction of Fig. 7, which is a schematic view of a cross section of the inductor shown in Fig. 7. A thin film inductor 100 according to an embodiment includes a body 110 including a magnetic substance including a soft magnetic alloy material, a coil 130 disposed within the body 110, and external electrodes 161, 162 disposed on an external surface of the body 110.
[0070] The body 110 forms the outer appearance of the thin film inductor 100 .
[0071] The body 110 may be a hexahedron having an upper surface and a lower surface facing in the stacking direction of the coils, a side surface facing laterally, and a front surface facing in the width direction, and when mounted on a printed circuit board, the lower surface (the other surface) of the body may be a mounting surface. The corners where the surfaces meet may be rounded by grinding or the like.
[0072] The body 110 is formed by forming the coil 130, laminating sheets containing a magnetic material on the upper and lower parts of the coil 130, and then compressing and curing the laminate.
[0073] The body 110 includes a magnetic material, which includes a soft magnetic alloy material according to one embodiment.
[0074] FIG. 9 is an enlarged view of region A in FIG.
[0075] 9, the magnetic material includes magnetic particles including a resin 20 and coarse magnetic particles 11 or fine magnetic particles 12 dispersed in the resin. As an example, the coarse magnetic particles 11 and the fine magnetic particles 12 may be mixed and dispersed at a certain ratio in the resin 20 as a matrix.
[0076] The coarse magnetic particles 11 have an average particle size of 10 μm to 30 μm, and the fine magnetic particles 12 have an average particle size of 1 μm to 10 μm.
[0077] The diameter of the magnetic particles present in the body 110 can be measured on a cross section of the body 110. Specifically, a plurality of regions (e.g., 10 regions) equally spaced in the T-axis direction on a LT-direction cross section passing through the center of the body 110 are photographed with a scanning electron microscope, and the diameter of the magnetic particles can be obtained using an image analysis program. In this case, the diameter of the magnetic particles is measured excluding the outer peripheral region of the body 110, since the magnetic particles may be deformed or destroyed during a compression process or the like. For example, a region corresponding to a length within 5% or 10% of the surface of the body 110 can be excluded.
[0078] The magnetic particles can be any type used in the industry without any restrictions. As an example, the magnetic particles can be made of ferrite or metal-based soft magnetic material.
[0079] The ferrite may include known ferrites such as Mn-Zn ferrite, Ni-Zn ferrite, Ni-Zn-Cu ferrite, Mn-Mg ferrite, Ba ferrite, or Li ferrite.
[0080] The metallic soft magnetic material may be an alloy containing one or more selected from the group consisting of Fe, Si, Cr, Al, and Ni, and includes, for example, Fe-Si-B-Cr amorphous metal particles, but is not limited to this.
[0081] In one embodiment, the magnetic particles comprise a soft magnetic alloy material, and in one example, the coarse magnetic particles are a soft magnetic alloy material.
[0082] The resin is an insulating resin, and includes, but is not limited to, an epoxy resin, a polyimide resin, a liquid crystal polymer, or a combination thereof.
[0083] The soft magnetic alloy materials include nanocrystalline and amorphous, and contain Fe (iron), Co (cobalt), and P (phosphorus).
[0084] The soft magnetic alloy material is represented by the following composition formula 1.
[0085] [Composition formula 1] Fe a Co b P c M d In the composition formula 1, a, b, c, and d each represent the atomic percentage content (at%) of the corresponding element, and <a≦90、0<b≦20、0<c≦10、0<d≦20、a+b+c+d=100であり、 M includes Si, B, Cu, Cr, C, Ni, Al, Mn, Ag, Zn, Sn, As, Sb, Bi, N, O, S, or combinations thereof.
[0086] In one embodiment, M includes B, P, Cu, or a combination thereof, and M does not include Nb.
[0087] In composition formula 1, a represents the atomic percentage content of Fe (iron) metal, and it is preferable that 70≦a≦80.
[0088] In the composition formula 1, b represents the atomic percentage content of Co (cobalt) metal, and it is preferable that 2≦b≦16.
[0089] In the composition formula 1, c represents the atomic percentage content of P (phosphorus) element, and it is preferable that 1≦c≦6.
[0090] By including P element in the above content range instead of Nb element in the soft magnetic alloy material, the size of nanocrystals can be adjusted to realize an inductor with excellent electromagnetic properties.
[0091] The soft magnetic alloy material included in the inductor satisfies Co(c)-Co(a)>0 when the average Co content in the amorphous is Co(a)(at%) and the average Co content in the nanocrystal is Co(c)(at%), or satisfies P(a)-P(c)>0 when the average P content in the amorphous is P(a)(at%) and the average P content in the nanocrystal is P(c)(at%). In one embodiment, it is preferable that Co(c)-Co(a)>0 and P(a)-P(c)>0.
[0092] The method for measuring Co(a), Co(c), P(a), and P(c) in inductor 100 is as follows.
[0093] In a cross-sectional sample (hereinafter referred to as the "cross-sectional sample") cut from the center of the W-axis direction of the inductor body 110 in the L-axis direction and the T-axis direction, the soft magnetic alloy material dispersed in the resin is subjected to line analysis using an EDS (Energy Disperse X-Ray Spectrometer) installed in a transmission electron microscope (TEM).
[0094] A cross-sectional sample of the inductor body 110 is prepared, for example, by immersing the inductor 100 in an epoxy mixture and hardening it, then polishing the sides of the inductor body 110 in the L-axis and T-axis directions to the 1 / 2 point in the W-axis direction, fixing it, and maintaining it in a chamber with a vacuum atmosphere.
[0095] Specifically, the surface of any one nanocrystalline particle contained in the soft magnetic alloy material is used as a reference, and the maximum value inside the nanocrystalline particle is compared with the maximum value in the amorphous part in a line profile obtained by spot quantitative analysis of 20 nm inside the nanocrystalline particle and 200 nm outside the nanocrystalline particle. In addition, to measure the average, the above-described analysis is repeated for 5 points or more, and the average value is calculated.
[0096] The average crystal size of the nanocrystals contained in the soft magnetic alloy material is preferably 20 nm or less.
[0097] As an example, the average crystal size of nanocrystals is calculated using the Scherrer equation using the full width at half maximum (FWHM) of the main peak in the XRD graph.
[0098] Specifically, the average crystal size of the nanocrystals is calculated using the half-width after obtaining an XRD graph of the soft magnetic alloy material from a cross-sectional sample of the inductor body 110. The XRD graph of the soft magnetic alloy material can be obtained through a sample obtained by crushing and classifying the cross-sectional sample of the body to about 20 μm or more.
[0099] As an example, the average crystal size of the nanocrystals can be measured in the soft magnetic alloy material corresponding to the coarse magnetic particles having a particle size of 10 μm to 30 μm in a scanning electron microscope (SEM) or transmission electron microscope (TEM) image of a cross-sectional sample of the body. Specifically, in the image of the cross-sectional sample, the center point in the L-axis direction is set as a reference point, and the sizes of the nanocrystals generated inside the coarse magnetic particles observed in a plurality of regions (e.g., 10 regions) at a predetermined interval in the T-axis direction are measured, and the average value can be calculated. The intervals between the plurality of regions can be adjusted according to the scale of the scanning electron microscope (SEM) or transmission electron microscope (TEM) image, and may be equal intervals. In this case, the plurality of regions must be located within the body, and if all 10 points are not located within the body, the position of the reference point is changed or the intervals between the 10 points are adjusted.
[0100] The soft magnetic alloy material is the same as that described above, so the remaining description will be omitted.
[0101] In one embodiment, an insulating film (not shown) is additionally disposed on the surface of the soft magnetic alloy material in order to impart insulating properties and ensure inductance.
[0102] The insulating film may be arranged in one or more layers, up to three layers. As an example, the insulating film may be an organic film including epoxy resin, polyimide resin, liquid crystal polymer, or a combination thereof, or may be an inorganic film including silicon oxide (SiO), silica (SiO2), alumina (Al2O3), or may be a metal oxide film such as FeO (iron oxide) or CrO (chromium oxide). When the insulating film is a metal oxide film, the metal oxide film may include, but is not limited to, a metal element included in the soft magnetic alloy material.
[0103] The thickness of the insulating film is preferably 1 to 20% of the grain size of the soft magnetic alloy material.
[0104] If the thickness of the insulating film exceeds 20% of the grain size of the soft magnetic alloy material, the magnetic permeability and magnetic susceptibility will decrease, so it is preferable to make the thickness as thin as possible.
[0105] The coil 130 is disposed within the body 110 and serves to develop the characteristics of an inductor. For example, when the inductor 100 is used as a power inductor, the coil serves to stabilize the power supply of an electronic device by storing an electric field as a magnetic field and maintaining an output voltage. The coil may be any of a wire-wound type formed by a wire winding method, a thin-film type formed by a thin-film method, and a laminated type formed by a lamination method, and a thin-film type coil will be described below as an example.
[0106] The coil 130 includes an upper coil 131 and a lower coil 132 that are respectively disposed on the upper and lower surfaces of the support member 120. The upper coil 131 and the lower coil 132 are coil layers that are disposed facing each other with the support member 120 as the reference.
[0107] The upper coil 131 and the lower coil 132 are formed as a plated layer on the support member 120 by a plating process or a photolithography method.
[0108] The coil 130 is formed from a material having excellent electrical conductivity, for example, one metal selected from gold (Au), silver (Ag), platinum (Pt), copper (Cu), nickel (Ni), palladium (Pd), aluminum (Al), titanium (Ti), etc., or an alloy of these metals, but any ordinary conductive material can be used without restriction.
[0109] The material and type of the support member 120 are not particularly limited as long as it can support the upper coil 131 and the lower coil 132. For example, the support member 120 may be a copper clad laminate (CCL), a polypropylene glycol (PPG) substrate, a ferrite substrate, or a metal-based soft magnetic substrate. The support member 120 may also be an insulating substrate made of insulating resin. As the insulating resin, a thermosetting resin such as an epoxy resin, a thermoplastic resin such as a polyimide, or a resin impregnated with a reinforcing material such as glass fiber or an inorganic filler, for example, a prepreg, ABF (Ajinomoto Build-up Film), FR-4, BT (Bismaleimide Triazine) resin, PID (Photo Imagable Dielectric) resin, etc., may be used. From the viewpoint of maintaining rigidity, an insulating substrate containing glass fiber and epoxy resin may be used, but is not limited thereto.
[0110] Holes are formed through the center of the support member 120 from the upper and lower surfaces, and the holes are filled with a magnetic material to form the core portion 150. By forming the core portion filled with a magnetic material, inductance can be improved.
[0111] The upper coil 131 and the lower coil 132 stacked on both sides of the support member 120 are electrically connected to each other through vias 140 that penetrate the support member 120 .
[0112] The via 140 is formed by forming a through hole using a mechanical drill or a laser drill, and then filling the inside of the through hole with a conductive material by plating.
[0113] The shape and material of the via 140 are not particularly limited as long as it can electrically connect the upper coil 131 on the upper side and the lower coil 132 on the lower side, which are respectively arranged on both sides of the support member 120. Here, the upper side and the lower side are determined based on the stacking direction of the coil patterns in the drawings.
[0114] The vias 140 include a conductive material such as copper (Cu), aluminum (Al), silver (Ag), tin (Sn), gold (Au), nickel (Ni), lead (Pd), or alloys thereof.
[0115] The upper and lower coils 131 , 132 are covered with an insulating layer 133 so as not to come into direct contact with the magnetic material that makes up the body 110 .
[0116] The insulating layer 133 serves to protect the upper and lower coils 131,132.
[0117] The material of the insulating layer 133 may be any material containing an insulating substance, and may include, for example, insulating substances used in ordinary insulating coatings, such as epoxy resin, polyimide resin, liquid crystal crystalline polymer resin, etc., and known photosensitive insulating (Photo Imageable Dielectric: PID) resins may also be used, but are not limited to these.
[0118] The insulating layer 133 is formed by a method such as, but not limited to, vapor phase deposition, and may be formed by laminating insulating films on both sides of the support member.
[0119] The inductor 100 according to the embodiment includes external electrodes 161 and 162 electrically connected to the upper and lower coils 131 and 132 and disposed on the outer surface of the body 110 .
[0120] The external electrodes 161 and 162 are electrically connected to lead terminals of the upper and lower coils 131 and 132 exposed on both sides of the body 110, respectively.
[0121] When the inductor 100 is mounted in an electronic device, the external electrodes 161 and 162 serve to electrically connect the coil 130 in the inductor to the electronic device.
[0122] The external electrodes 161 and 162 include multiple electrode layers.
[0123] The multiple electrode layers are formed using a conductive paste containing a conductive metal or a conductive resin.
[0124] The conductive resin layer includes a conductive metal for ensuring electrical conductivity and a resin for shock absorption. The resin is not particularly limited as long as it has bonding and shock absorption properties and can be mixed with the conductive metal powder to form a paste, and can include, for example, a phenol resin, an acrylic resin, a silicone resin, an epoxy resin, or a polyimide resin.
[0125] The conductive metal may include, for example, copper (Cu), tin (Sn), nickel (Ni), silver (Ag), palladium (Pd), gold (Au), platinum (Pt), tungsten (W), titanium (Ti), alloys thereof, or combinations thereof.
[0126] The external electrodes 161 and 162 include a plurality of plating layers formed by plating a conductive metal.
[0127] As an example, the plating layer may include any one or more selected from the group consisting of nickel (Ni), copper (Cu), tin (Sn), or a combination thereof. For example, a nickel (Ni) layer and a tin (Sn) layer may be formed in sequence, or a copper (Cu) layer, a nickel (Ni) layer, and a tin (Sn) layer may be formed in sequence.
[0128] The wire-wound inductor 200 and the multilayer inductor 300 will be described in more detail below. Only the configurations of the wire-wound inductor 200 and the multilayer inductor 300 that differ from the thin-film inductor 100 will be described below. The explanation for the thin-film inductor 100 can be applied to the remaining configurations as is.
[0129] FIG. 10 is a schematic diagram showing a see-through perspective view of a wound inductor according to another embodiment, and FIG. 11 is a schematic diagram showing a cross-section in the II-II' direction of FIG. 10, and is a schematic diagram showing a cross-sectional view of the inductor shown in FIG. 10.
[0130] The wire-wound inductor 200 according to one embodiment includes a body 210 including a magnetic material that includes a soft magnetic alloy material, a coil 230 disposed within the body 210 , and external electrodes 261 , 262 disposed on an external surface of the body 210 .
[0131] In one embodiment, the body 210 includes a molded portion 211, a cover portion 212 disposed on one side of the molded portion 211, and a core 250 protruding from one side of the molded portion 211, the coil 230 being disposed between the one side of the molded portion 211 and the cover portion 212, and the core 250 passing through the coil 230.
[0132] The body 210 of the wire-wound inductor 200 includes a molded part 211, a cover part 212 disposed on one surface of the molded part 211, and further includes a core 250 disposed to protrude from one surface of the molded part 211. In this case, the coil 230 is disposed on one surface of the molded part 211, and has a shape in which the coil 230 surrounds the core 250.
[0133] The body 210 includes a magnetic material, and the magnetic material includes a soft magnetic alloy material according to an embodiment. That is, at least one of the molded part 211, the cover part 212, and the core 250 includes a magnetic material including a soft magnetic alloy material. As an example, the molded part 211 is formed by filling a mold with a magnetic material. As another example, the molded part 211 is formed by filling a mold with a composite material including a magnetic material and a resin. A process of applying high temperature and high pressure to the magnetic material or composite material in the mold is additionally performed, but is not limited thereto. The molded part 211 and the core part 250 are integrally formed by the above-mentioned mold, and no boundary is formed between them. The cover part 212 is formed by placing a magnetic composite sheet in which a magnetic material is dispersed in a resin on the molded part 211 and the coil 230, and then applying heat and pressure.
[0134] In the wire-wound inductor 200 , the lead-out portion (not shown) passes through the molded portion 211 and can be connected to the external electrodes 261 , 262 .
[0135] The description of the magnetic material and the soft magnetic alloy material in the body 210 can be applied to the thin film inductor 100 according to an embodiment.
[0136] In the wire-wound inductor 200, the surface of the coil 230 is covered with an insulating layer 231, which serves to provide insulation between the magnetic material of the body 210 and the coil 230. The same description of the insulating layer 133 described above can be applied to the insulating layer 231.
[0137] The wire-wound inductor 200 differs from the thin-film inductor 100 in the configuration of the coil 230 and the presence or absence of a support member.
[0138] The coil 230 is a wound type coil and does not include a support member. The coil 230 is a wound coil formed by winding a metal wire such as a copper wire (Cu-wire) including a metal wire and an insulating layer 231 that covers the surface of the metal wire. The metal wire may be, but is not limited to, a rectangular wire.
[0139] Although coil 230 is shown in FIG. 10 with alpha (α) configuration windings, this is by way of example only and coil 230 may also be edge-wise wound.
[0140] FIG. 12 is a schematic diagram showing a see-through perspective view of a layered inductor according to another embodiment, and FIG. 13 is a schematic diagram showing a cross-section in the III-III' direction of FIG. 12, and is a schematic diagram showing a cross-sectional view of the inductor shown in FIG. 12.
[0141] A stacked inductor 300 according to one embodiment includes a body 310 including a magnetic material including a soft magnetic alloy material, a coil 330 disposed within the body 310, and external electrodes 361, 362 disposed on an external surface of the body 310, where the body 310 includes a plurality of magnetic sheets including the magnetic material.
[0142] The description of the magnetic material and soft magnetic alloy material in the body 310 can be applied to the thin film inductor 100 according to an embodiment.
[0143] As an example, the body 310 is formed by stacking a plurality of magnetic sheets containing a magnetic material in the thickness direction and then sintering the same, and the shape, dimensions, and number of stacked magnetic sheets of the body 310 are not limited to those shown in one embodiment.
[0144] Conductive patterns for forming coils 330 are formed on one surface of the magnetic sheets, and conductive vias for electrically connecting the conductive patterns positioned above and below are formed through the magnetic sheets in the thickness direction.
[0145] Therefore, one end of the conductor pattern formed on each magnetic sheet is electrically connected to each other through the conductive via formed on the adjacent magnetic sheet to form the coil 330.
[0146] The surface of the coil 330 is covered with an insulating layer 331, and the insulating layer 331 functions to provide insulation between the magnetic material of the body 310 and the coil 330. The same description of the insulating layer 133 described above can be applied to the insulating layer 331.
[0147] Both ends of the coil 330 are led out through the body 310 and can be electrically connected to a pair of external electrodes 361 and 362 formed on the body 310 by contacting them, respectively.
[0148] In particular, both ends of the coil 330 are led out through both ends of the body 310, and a pair of external electrodes 361, 362 are formed on both ends of the body 310 through which the coil 330 is led out.
[0149] The conductor pattern can be formed by thick-film printing, coating, vapor deposition, sputtering, or the like of a conductive paste for forming a conductor pattern on a green sheet for forming a magnetic sheet, but is not limited to this.
[0150] The conductive vias can be formed by forming through holes in the thickness direction of each sheet and then filling the through holes with a conductive paste or the like, but are not limited to this.
[0151] The conductive metal contained in the conductive paste for forming the conductor pattern may be one of silver (Ag), palladium (Pd), platinum (Pt), nickel (Ni) and copper (Cu), or an alloy thereof, but the present invention is not limited to this.
[0152] Due to its excellent properties, soft magnetic alloy materials can maintain high saturation magnetization while improving electromagnetic properties by being included in the body of a thin film, wound, or multilayer inductor as described above.
[0153] In addition to the inductors described above, the soft magnetic alloy materials can be used in magnetic products such as transformers, motors, or motor stators.
[0154] Specific examples of the present invention are presented below. However, the examples described below are merely for the purpose of specifically illustrating or explaining the present invention, and should not be construed as limiting the scope of the present invention.
[0155] (Production example: Production of amorphous soft magnetic alloy)
[0156] (Production Example 1) Composition formula Fe 75.2 Co8Si2B 12 P2Cu 0.8 The Fe, Co, Si, B, P, and Cu raw materials are weighed and mixed to produce a master alloy using an arc melting method, so that an amorphous soft magnetic alloy represented by the formula (1) is produced. The produced master alloy is melted and then rapidly cooled in a rapid cooling facility to produce a ribbon-shaped amorphous soft magnetic alloy with a thickness of 20 μm.
[0157] (Production Examples 2 to 5, and Comparative Production Examples 1 to 10) An amorphous soft magnetic alloy was prepared in the same manner as in Preparation Example 1, except that the composition formula was as shown in Table 2 below.
[0158] (Example: Manufacturing of soft magnetic alloy material) The amorphous soft magnetic alloys of Production Examples 1 to 5 and Comparative Production Examples 1 to 10 are heat-treated (400°C, 40 minutes) to produce the soft magnetic alloy materials of Examples 1 to 5 and Comparative Examples 1 to 10. The composition formula of the soft magnetic alloy materials produced in the Examples is the same as the composition formula of the amorphous soft magnetic alloys produced in the Production Examples.
[0159] (Experimental Example 1: Before heat treatment - Amorphous ratio analysis) For the amorphous soft magnetic alloys of Manufacturing Examples 1 to 5 and Comparative Manufacturing Examples 1 to 10, data fitting was performed after XRD analysis, and the amorphous rate (%) was calculated based on the area ratio of the amorphous and crystalline regions using Equation 1 described above, and is shown in Table 3.
[0160] Referring to Table 3, it can be seen that the amorphous ratios of Preparation Examples 1 to 5 are 95% or more, and therefore the amorphous characteristics are improved.
[0161] In contrast, the amorphous ratios of Comparative Production Examples 1 to 10, which do not contain Co metal, are less than 95%, and it can be seen that the amorphous characteristics are significantly reduced.
[0162] (Experimental Example 2: Analysis of the difference in Co and P content between the amorphous phase and the crystalline phase after heat treatment) Quantitative spot analysis was performed at six points for each of the soft magnetic alloy materials of Examples 1 to 5 by TEM analysis, and the average content was calculated. At this time, the Co content (Co(a), Co(c)) (unit: at%) in the amorphous phase and the crystalline phase is shown in Table 1 below. The P content (P(a), P(c)) (unit: at%) in the amorphous phase and the crystalline phase is shown in Table 2 below.
[0163] Referring to Table 1 below, it can be seen that the average Co atom content in the nanocrystals (Co(c)) is higher than the average Co atom content in the amorphous state (Co(a)). This shows that the inclusion of Co metal can delay the growth of the crystalline phase containing Fe when it is formed.
[0164] Referring to Table 2 below, it can be seen that the average P atomic content in the amorphous phase (P(a)) is higher than the average P atomic content in the nanocrystals (P(c)). This shows that the P element, which has a smaller atomic weight than the Nb element, remains in the amorphous phase and plays a role in suppressing the growth of nanocrystals in the soft magnetic alloy material.
[0165] [Table 1]
[0166] [Table 2]
[0167] (Experimental Example 3: After heat treatment - crystal size analysis) The average crystal size of the nanocrystals in the soft magnetic alloy materials of Examples 1 to 5 and Comparative Examples 1 to 10 was calculated using the Scherrer equation expressed by the following Equation 2, which uses the full width at half maximum (FWHM) of the main peak in the XRD graph. The results are shown in Table 3.
[0168]
number
[0169] In Equation 2, D is the average crystal size, λ is the wavelength of the XRD target, β is the full width at half maximum (FWHM), and θ is the half value of the XRD graph peak 2θ.
[0170] Referring to Table 3, it can be seen that in Examples 1 to 5, the average crystal size of the nanocrystals is 20 nm or less.
[0171] In contrast, in Comparative Examples 6 to 10, which do not contain the P element, it can be confirmed that the average crystal size of the nanocrystals exceeds 20 nm.
[0172] (Experimental Example 4: Evaluation of electromagnetic characteristics) The magnetic permeability at a frequency of 1 kHz and the core loss in a magnetic field of 0.2 T and 100 kHz of the soft magnetic alloy materials of Examples 1 to 5 and Comparative Examples 1 to 10 were measured and are shown in Table 3 below.
[0173] Referring to Table 3, it can be seen that Examples 1 to 5 have excellent electromagnetic properties, with a magnetic permeability of 5300 or more and a core loss of 1700 mW / cc or less.
[0174] In contrast, in Comparative Examples 6 to 10 which do not contain the P element, the magnetic permeability is less than 5300, the core loss is more than 1700 mW / cc, and it can be confirmed that the electromagnetic properties are significantly deteriorated.
[0175] [Table 3]
[0176] In Table 3, the amorphous ratio (%) corresponds to the value measured in Production Examples 1 to 5 and Comparative Production Examples 1 to 10, which are amorphous soft magnetic alloys before the soft magnetic alloy material is sintered.
[0177] Although the preferred embodiment of the present invention has been described above, the present invention is not limited thereto, and various modifications can be made within the scope of the detailed description and drawings of the invention, which of course also fall within the scope of the present invention. [Explanation of symbols]
[0178] 11: Coarse magnetic particles 12: Fine magnetic particles 20: Resin 100, 200, 300: Inductor 110, 210, 310: Body 120: Support member 130, 230, 330: Coil 131: Upper coil 132: Lower coil 133, 231, 331: Insulating layer 140:Beer 150, 250: Core 161, 162, 261, 262, 361, 362: External electrode 211:Mold section 212: Cover part
Claims
1. It includes nanocrystalline and amorphous, and includes Fe (iron), Co (cobalt), and P (phosphorus); Represented by the following composition formula 1: When the average Co content in the amorphous phase is Co(a) (at%) and the average Co content in the nanocrystals is Co(c) (at%), the soft magnetic alloy material is characterized in that Co(c)-Co(a)>0. Composition formula 1 Fe a Co b P c M d In the composition formula 1, a, b, c, and d each represent the atomic percentage content (at %) of the corresponding element, where 0<a≦90, 0<b≦20, 0<c≦10, 0<d≦20, and a+b+c+d=100. The M includes Si, B, Cu, Cr, C, Ni, Al, Mn, Ag, Zn, Sn, As, Sb, Bi, N, O, S, or a combination thereof.
2. The soft magnetic alloy material according to claim 1, characterized in that, when the average P content in the amorphous phase is P(a) (at%) and the average P content in the nanocrystals is P(c) (at%), P(a)-P(c)>0.
3. 2. The soft magnetic alloy material according to claim 1, wherein 0.4≦Co(c)−Co(a)≦1.
5.
4. 3. The soft magnetic alloy material according to claim 2, wherein 0.5≦P(a)−P(c)≦2.
5.
5. 2. The soft magnetic alloy material according to claim 1, wherein b satisfies 2≦b≦16.
6. 2. The soft magnetic alloy material according to claim 1, wherein 1≦c≦6.
7. 2. The soft magnetic alloy material according to claim 1, wherein said M does not contain Nb.
8. 2. The soft magnetic alloy material according to claim 1, wherein the nanocrystals have an average crystal size of 20 nm or less.
9. It includes nanocrystalline and amorphous, and includes Fe (iron), Co (cobalt), and P (phosphorus); Represented by the following composition formula 1: When the average P content in the amorphous phase is P(a) (at%) and the average P content in the nanocrystals is P(c) (at%), a soft magnetic alloy material characterized in that P(a)-P(c)>0. Composition formula 1 Fe a Co b P c M d In the composition formula 1, a, b, c, and d each represent the atomic percentage content (at %) of the corresponding element, where 0<a≦90, 0<b≦20, 0<c≦10, 0<d≦20, and a+b+c+d=100. The M includes Si, B, Cu, Cr, C, Ni, Al, Mn, Ag, Zn, Sn, As, Sb, Bi, N, O, S, or a combination thereof.
10. The soft magnetic alloy material according to claim 9, characterized in that, when the average Co content in the amorphous phase is Co(a) (at%) and the average Co content in the nanocrystal is Co(c) (at%), Co(c)-Co(a)>0.
11. 10. The soft magnetic alloy material according to claim 9, wherein 0.5≦P(a)−P(c)≦2.
5.
12. 11. The soft magnetic alloy material according to claim 10, wherein 0.4≦Co(c)−Co(a)≦1.
5.
13. 10. The soft magnetic alloy material according to claim 9, wherein 2≦b≦16.
14. 10. The soft magnetic alloy material according to claim 9, wherein 1≦c≦6.
15. The soft magnetic alloy material according to claim 9 , wherein the M does not contain Nb.
16. 10. The soft magnetic alloy material according to claim 9, wherein the nanocrystals have an average crystal size of 20 nm or less.
17. (1) mixing raw materials; (2) melting the mixed raw materials; (3) rapidly cooling the molten raw material to produce an amorphous soft magnetic alloy; (4) A method for producing a soft magnetic alloy material, comprising the steps of: heat treating the amorphous soft magnetic alloy.
18. 18. The method for producing a soft magnetic alloy material according to claim 17, wherein the amorphous soft magnetic alloy has an amorphous rate of 95% or more.
19. a body including a magnetic substance including a soft magnetic alloy material; A coil disposed within the body; an external electrode disposed on an external surface of the body; The soft magnetic alloy material includes nanocrystalline and amorphous, and includes Fe (iron), Co (cobalt), and P (phosphorus); Represented by the following composition formula 1: When the average Co content in the amorphous phase is Co(a) (at %) and the average Co content in the nanocrystal is Co(c) (at %), Co(c)-Co(a)>0; An inductor characterized in that, when the average P content in the amorphous material is P(a) (at %) and the average P content in the nanocrystals is P(c) (at %), P(a)-P(c)>0. Composition formula 1 Fe a Co b P c M d In the composition formula 1, a, b, c, and d each represent the atomic percentage content (at %) of the corresponding element, where 0<a≦90, 0<b≦20, 0<c≦10, 0<d≦20, and a+b+c+d=100. The M includes Si, B, Cu, Cr, C, Ni, Al, Mn, Ag, Zn, Sn, As, Sb, Bi, N, O, S, or a combination thereof.
20. The coil includes a support member and an upper coil and a lower coil disposed on an upper surface and a lower surface, respectively, of the support member; The inductor of claim 19 , wherein the upper coil and the lower coil are electrically connected to each other through a via that penetrates the support member.
21. the body includes a molded portion, a cover portion disposed on one surface of the molded portion, and a core protruding from the one surface of the molded portion; The inductor according to claim 19 , wherein the coil is disposed between one surface of the molded portion and the cover portion, and the core passes through the coil.
22. The inductor of claim 19 , wherein the body includes a plurality of magnetic sheets containing the magnetic material.
Citation Information
Patent Citations
Laminated inductor
JP2018206836A