Laminate and method for manufacturing the same
The laminate structure with a primer, plating base, and metal plating layers on a support addresses the challenge of achieving smoothness and adhesion in printed wiring boards, enhancing adhesion and high-frequency transmission, suitable for electronic components.
Patent Information
- Application Number
- JP2023069237
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-20
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional printed wiring boards face challenges in achieving both smoothness and adhesion between copper wiring and interlayer resin while maintaining high-frequency transmission characteristics, limiting miniaturization and performance in high-speed electronic circuits.
A laminate structure is developed with a primer layer, a plating base layer, a metal plating layer, and an adhesive layer, which are sequentially formed on a support, ensuring a smooth surface and strong adhesion without roughening the copper wiring, thereby enhancing adhesion and high-frequency transmission.
The laminate structure achieves excellent adhesion between copper wiring and interlayer resin, reducing conductor loss and improving high-frequency transmission characteristics, suitable for various electronic components and devices.
Smart Images

Figure 2024154967000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a printed wiring board, a high-frequency transmission printed wiring board, a rigid printed wiring board, a package substrate, an interposer, an antenna, a semiconductor chip, and the like. [Background technology]
[0002] The miniaturization and high speed of electronic devices has led to demands for higher density and higher performance of printed wiring boards, and to meet these demands, copper wiring with a smooth surface is in demand. Among these, attention has been focused on small electronic circuit boards with fine circuits and high-speed electronic circuit boards with excellent high-frequency transmission properties, which can be produced by processing the copper wiring of wiring boards without roughening treatment.
[0003] Conventional wiring boards are generally subjected to a roughening treatment of the wiring surface, which is called blackening treatment. This blackening treatment is responsible for the adhesion between the copper circuit formed on the inner layer circuit board and the exterior circuit board or the interlayer resin such as prepreg or bonding sheet for laminating the copper foil in multilayer printed wiring boards for small applications and high-speed transmission applications. However, roughening the wiring surface causes deterioration of high-frequency transmission characteristics due to a decrease in conductor loss of the wiring, and makes it difficult to form fine circuits with high accuracy.
[0004] Currently, efforts are being made to achieve both smoothness and adhesion of the wiring by using a low-roughness treatment that finely etches the wiring surface. However, because this is a trade-off, there are limits to the speed and fineness that will be required in the future for electronic circuit boards.
[0005] Therefore, instead of the conventional physical adhesion method that uses the anchor effect created by roughening treatment, a technology has been developed that uses a chemical adhesion method to bond the smooth wiring surface to an interlayer resin such as a prepreg or bonding sheet, without performing a roughening treatment on the wiring.
[0006] Patent Document 1 describes an invention relating to a metal surface treatment liquid composition and a surface treatment method that can maintain adhesion between metal and insulating materials such as resin without roughening the metal used in wiring.
[0007] Patent Document 2 describes an invention relating to a copper surface treatment liquid composition and a surface treatment method that can improve the adhesive strength between copper and resin by forming a resin adhesive layer made of an alloy of copper, tin, and a third metal on the copper surface of a wiring without roughening the wiring surface.
[0008] Patent Document 3 describes an invention relating to a composition and a method for forming an adhesive layer that forms two layers, an elastomer layer and a molecular adhesion layer, without roughening the wiring surface, thereby not only maintaining adhesion between metal and insulating materials such as resin, but also alleviating stress concentration, improving reliability, and improving heat resistance, which are issues that arise when manufacturing laminates.
[0009] The above-mentioned technique for bonding a smooth wiring surface with an interlayer resin such as a prepreg or a bonding sheet is capable of bonding the wiring surface with a prepreg or a bonding sheet, but it is difficult to bond a smooth substrate with an interlayer resin such as a prepreg or a bonding sheet. In addition, since only the copper wiring surface is treated, it has the disadvantage that it is not compatible with the process for bonding the interface between the substrate and the wiring smoothly.
[0010] Therefore, there has been a demand for a structure and a manufacturing method for a printed wiring board having a multi-layer structure in which the surfaces of the substrate and copper wiring are formed smooth and have excellent adhesion and high-frequency transmission properties. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] JP 2015-92020 A [Patent Document 2] JP 2012-94918 A [Patent Document 3] WO2009 / 154083 publication Summary of the Invention [Problem to be solved by the invention]
[0012] The problem that the present invention aims to solve is to provide a metal circuit board that has excellent transmission characteristics and is highly reliable by forming a thin adhesive layer on the surface of a smooth substrate and smooth copper wiring, thereby achieving high adhesion with the interlayer resin of a multilayer wiring board. [Means for solving the problem]
[0013] As a result of intensive research to solve the above-mentioned problems, the inventors discovered that the above-mentioned problems can be solved by a laminate in which a primer, a plating underlayer, and a metal plating layer are sequentially formed on the surface of a substrate, and an adhesive layer is provided on the wiring surface of the laminate having copper wiring formed thereon, thereby completing the present invention.
[0014] That is, the present invention provides a laminate characterized by having a support (A) on which a primer layer (B) containing an organic resin component, a plating underlayer (C), a metal plating layer (D), and an adhesive layer (E) are sequentially laminated, and a printed wiring board, a package substrate, and an interposer using the same.
[0015] Specifically, the present invention relates to 1. A laminate comprising a primer layer (B), a patterned plating base layer (C), and a metal plating layer (D) laminated in that order on at least one surface of a support (A), and an adhesive layer (E) having a thickness of 0.001 to 1 μm laminated only on the surfaces of the plating base layer (C) and the metal plating layer (D). 2. A laminate comprising a primer layer (B), a patterned plating base layer (C), and a metal plating layer (D) laminated in that order on at least one surface of a support (A), and further an adhesive layer (E) having a thickness of 0.001 to 1 μm laminated on the surfaces of the primer layer (B), the patterned plating base layer (C), and the metal plating layer (D). 3. The laminate according to 1 or 2, further comprising an interlayer resin layer (F) on the primer layer (B) and / or the adhesive layer (E) or on the adhesive layer (E). 4. The laminate according to any one of 1 to 3, wherein the surface roughness (maximum height Sz) of the support (A) as measured by a laser microscope is 0.001 to 50 μm. 5. The laminate according to any one of 1 to 4, wherein the surface roughness (maximum height Sz) of the primer layer (B) measured with a laser microscope is 0.001 to 30 μm. 6. The laminate according to any one of 1 to 5, wherein the surface roughness (maximum height Sz) of the plating underlayer (C) measured with a laser microscope is 0.001 to 30 μm. 7. The laminate according to any one of 1 to 6, wherein the surface roughness (maximum height Sz) of the metal plating layer (D) measured with a laser microscope is 0.001 to 20 μm. 8. The laminate according to any one of 1 to 7, wherein the adhesive layer (E) has a surface roughness (maximum height Sz) of 0.001 to 20 μm as measured by a laser microscope. 9. A laminate according to any one of 1 to 8, characterized in that the primer layer (B) is selected from at least a urethane resin, an acrylic resin, a core-shell type composite resin having a urethane resin as the shell and an acrylic resin as the core, an epoxy resin, a phenoxy resin, an imide resin, an amide resin, a melamine resin, a phenolic resin, a urea-formaldehyde resin, a blocked isocyanate obtained by reacting a blocking agent such as phenol with a polyisocyanate, polyvinyl alcohol, and polyvinylpyrrolidone. 10. The laminate according to any one of 1 to 9, wherein the primer layer (B) is one or more layers. 11. The laminate according to any one of 1 to 10, wherein the patterned plating underlayer (C) is one or more layers. 12. The adhesive layer (E) is at least one of a mercaptosilane compound, a vinylsilane compound, a vinylphenylsilane compound, an epoxysilane compound, an acryloxysilane compound, a methacryloxysilane compound, an aminosilane compound, a ureidosilane compound, a chloropropylsilane compound, a sulfidosilane compound, an isocyanatesilane compound, a triazolesilane compound, a thiadiazolesilane compound, an isocyanatopropylsilane compound, a styrylsilane compound, a carboxysilane compound, an alkoxysilane compound, a triazinesilane compound, an imidazolesilane compound, an azolesilane compound, a pyrrolesilane compound, a pyrazolesilane compound, a tetrazolesilane compound, an indolesilane compound, an isoindolesilane compound, an indazole ... 12. The laminate according to any one of 1 to 11, characterized in that the resin is selected from one or more of a silane compound, a benzimidazole silane compound, a benzotriazole silane compound, a triazine thiol compound, a triazine azide compound, a triazine amino compound, a triazine isoyanate compound, a triazine urethane compound, a triazine ester compound, a triazine silane compound, a urethane resin, an acrylic resin, a core-shell type composite resin having a urethane resin as the shell and an acrylic resin as the core, an epoxy resin, a phenoxy resin, an imide resin, an amide resin, a melamine resin, a phenolic resin, a urea-formaldehyde resin, a blocked isocyanate polyvinyl alcohol obtained by reacting a blocking agent such as phenol with a polyisocyanate, and polyvinylpyrrolidone. 13. A laminate according to any one of 1 to 12, characterized in that the adhesive layer (E) is selected from one or more of copper, tin, silver, bismuth, nickel, palladium, platinum, cobalt, titanium, molybdenum, chromium, manganese, ruthenium, indium, zinc, tungsten, aluminum, and zirconium. 14. Step 1 of forming the primer layer (B) on at least one surface of the support (A); Step 2 of forming the plating underlayer (C) on the surface of the primer layer (B); Step 3 of forming a metal plating layer (D) on the surface of the plating underlayer (C); Step 4 of forming an adhesive layer (E) on the surface of the metal plating layer (D). 14. The method for producing a laminate according to any one of 1, 2, and 4 to 13, comprising the steps of: 15. Step 1 of producing a transfer laminate in which a plating underlayer (C) and a primer layer (B) are successively formed on a temporary support (G); A step 2 of laminating the surface of the transfer laminate on which the primer layer (B) is formed to at least one surface of the support (A); A step 3 of peeling off the temporary support (G) of the transfer laminate attached to the support (A) and forming the primer layer (B) and the plating underlayer (C) on at least one surface of the support (A); Step 4 of forming a metal plating layer (D) on the surface of the plating underlayer (C); Step 5 of forming an adhesive layer (E) on the surface of the metal plating layer (D). 14. The method for producing a laminate according to any one of 1, 2, and 4 to 13, comprising the steps of: 16. Step 1 of forming the primer layer (B) on at least one surface of the support (A); Step 2 of forming the plating underlayer (C) on the surface of the primer layer (B); Step 3 of forming a metal plating layer (D) on the surface of the plating underlayer (C); Step 4 of forming an adhesive layer (E) on the surface of the metal plating layer (D); Step 5 further comprises forming an interlayer resin layer (F) on the primer layer (B) and the adhesive layer (E) or on the adhesive layer (E); 14. The method for producing a laminate according to any one of 3 to 13, comprising the steps of: 17. Step 1 of producing a transfer laminate in which a plating underlayer (C) and a primer layer (B) are successively formed on a temporary support (G); A step 2 of laminating the surface of the transfer laminate on which the primer layer (B) is formed to at least one surface of the support (A); A step 3 of peeling off the temporary support (G) of the transfer laminate attached to the support (A) and forming the primer layer (B) and the plating underlayer (C) on at least one surface of the support (A); Step 4 of forming a metal plating layer (D) on the surface of the plating underlayer (C); Step 5 of forming an adhesive layer (E) on the surface of the metal plating layer (D); Further, a step 6 of forming an interlayer resin layer (F) on the primer layer (B) and the adhesive layer (E) or on the adhesive layer (E); 14. The method for producing a laminate according to any one of 3 to 13, comprising the steps of: 18. A printed wiring board, a package substrate, an interposer, a wiring substrate for LED electrodes, or a photonics-electronics hybrid device, comprising the laminate according to any one of 1 to 13. Effect of the Invention
[0016] The laminate of the present invention has the characteristics of excellent adhesion between the copper wiring and the interlayer resin while maintaining a smooth wiring shape, reducing conductor loss due to the wiring shape, and having excellent high-frequency transmission characteristics, compared to the conventional method of bonding the copper wiring and the interlayer resin by roughening treatment. Therefore, the laminate of the present invention can be suitably used as electronic parts such as printed wiring boards, rigid printed wiring boards, flexible printed wiring boards, package substrates, metal substrates, metal meshes for touch panels, organic solar cells, organic EL elements, wiring substrates for LED electrodes, organic transistors, RFIDs such as non-contact IC cards, electromagnetic wave shields, LED lighting substrates, digital signage, photoelectric convergence devices, and interposers. [Brief description of the drawings]
[0017] [Figure 1] 1 is a cross-sectional view of a laminate of the present invention in which a primer layer, a plating underlayer, and a metal plating layer are successively formed on one side of a support, followed by patterning, and then an adhesive layer is formed on the wiring surface. [Diagram 2] FIG. 2 is a cross-sectional view of a laminate of the present invention in which a primer layer, a plating underlayer, and a metal plating layer are successively formed on both sides of a support, followed by patterning, and then an adhesive layer is formed on the wiring surface. [Diagram 3]FIG. 2 is a cross-sectional view of a laminate of the present invention in which a primer layer, a plating underlayer, and a metal plating layer are successively formed on one side of a support, followed by patterning, and then an adhesive layer is formed on the wiring surface and the substrate surface. [Figure 4] FIG. 2 is a cross-sectional view of a laminate of the present invention in which a primer layer, a plating underlayer, and a metal plating layer are successively formed on both sides of a support, followed by patterning, and then an adhesive layer is formed on the wiring surface and the substrate surface. [Diagram 5] This is a cross-sectional view of a laminate of the present invention in which a primer layer, a plating underlayer, and a metal plating layer are formed in sequence on one side of a support, patterned, an adhesive layer is formed on the wiring surface, and then an interlayer resin layer is formed. [Figure 6] This is a cross-sectional view of a laminate of the present invention in which a primer layer, a plating underlayer, and a metal plating layer are formed in sequence on both sides of a support, patterned, an adhesive layer is formed on the wiring surface, and then an interlayer resin layer is formed. [Figure 7] This is a cross-sectional view of a laminate of the present invention in which a primer layer, a plating underlayer, and a metal plating layer are formed in sequence on one side of a support, patterned, and then an adhesive layer is formed on the wiring surface and the base material surface, and then an interlayer resin layer is formed. [Figure 8] This is a cross-sectional view of a laminate of the present invention in which a primer layer, a plating underlayer, and a metal plating layer are formed in sequence on both sides of a support, patterned, and then an adhesive layer is formed on the wiring surface and the base material surface, and then an interlayer resin layer is formed. [Figure 9] This is a cross-sectional view of a laminate of the present invention, in which a primer layer, a plating underlayer, and a metal plating layer are formed in sequence on one side of a support, and then patterned, and an adhesive layer is formed on the wiring surface, and then an interlayer resin layer and a metal layer are formed. [Figure 10] FIG. 1 is a cross-sectional view of a laminate of the present invention, in which a primer layer, a plating underlayer, and a metal plating layer are successively formed on one side of a support, followed by patterning, and then an adhesive layer is formed on the wiring surface and the substrate surface, followed by forming an interlayer resin layer and a metal layer. [Figure 11] This is a cross-sectional view of a laminate of the present invention, in which a primer layer, a plating underlayer, and a metal plating layer are formed in sequence on both sides of a support, patterned, an adhesive layer is formed on the wiring surface, and then laminated via an interlayer resin layer. [Figure 12] This is a cross-sectional view of a laminate of the present invention in which a primer layer, a plating underlayer, and a metal plating layer are formed in that order on both sides of a support, patterned, and then an adhesive layer is formed on the wiring surface and the base material surface, and then laminated via an interlayer resin layer. [Figure 13] This is a cross-sectional view of a laminate of the present invention in which a primer layer, a plating underlayer, and a metal plating layer are sequentially formed on one side of a support, patterned, a thick adhesive layer is formed on the wiring surface and the substrate surface, and then an interlayer resin layer is formed. [Figure 14] FIG. 1 is a cross-sectional view of a conventional laminate in which a primer layer, a plating underlayer, and a metal plating layer are successively formed on one side of a support, followed by patterning and then forming an interlayer resin layer. [Figure 15] FIG. 1 is a cross-sectional view of a conventional laminate in which a metal layer is formed on one side of a support, patterned, and then an interlayer resin layer is formed. [Figure 16] FIG. 1 is a cross-sectional view of a conventional laminate in which a metal layer is formed on one side of a support, patterned, an adhesive layer is formed on the wiring surface, and then an interlayer resin layer is formed. [Figure 17] FIG. 1 is a cross-sectional view of a conventional laminate in which a plating underlayer and a metal plating layer are successively formed on one side of a support, followed by patterning, and then an adhesive layer is formed on the wiring surface, followed by forming an interlayer resin layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The laminate of the present invention is characterized by having, on at least one surface of a support (A), a primer layer (B), a plating underlayer (C), a metal plating layer (D), and an adhesive layer (E), and a manufacturing method thereof.
[0019] The laminate of the present invention may be a laminate in which a primer layer (B) and the like are sequentially laminated on one side of a support (A), or a laminate in which a primer layer (B) and the like are sequentially laminated on both sides of the support (A).
[0020] The laminate of the present invention is a laminate characterized by having, on at least one surface of a support (A), a primer layer (B), a plating underlayer (C), a metal plating layer (D), and a thin adhesive layer (E), and a manufacturing method thereof.
[0021] The laminate of the present invention is a laminate characterized by having, on at least one surface of a support (A), a primer layer (B), a plating underlayer (C), a metal plating layer (D), a thin adhesive layer (E), and an interlayer resin layer (F), and a manufacturing method thereof.
[0022] The laminate of the present invention is a laminate characterized by having, on at least one surface of a support (A), a primer layer (B), a plating underlayer (C), a metal plating layer (D), a thin adhesive layer (E), and an interlayer resin layer (F), and a metal layer or a wiring board on top of the primer layer (B), a plating underlayer (C), a metal plating layer (D), a thin adhesive layer (E), and an interlayer resin layer (F), and a manufacturing method thereof.
[0023] Examples of materials for the support (A) include polyimide resins, modified polyimide resins (MPI), polyamideimide resins, polyamide resins, polyethylene terephthalate resins, polybutylene terephthalate resins, polyethylene naphthalate resins, polycarbonate resins, acrylonitrile-butadiene-styrene (ABS) resins, polyarylate resins, polyacetal resins, acrylic resins such as poly(methyl meth)acrylate, polyvinylidene fluoride resins, polytetrafluoroethylene resins, polyvinyl chloride resins, polyvinylidene chloride resins, vinyl chloride resins graft-copolymerized with acrylic resins, polyvinyl alcohol resins, polyethylene resins, polypropylene resins, and urethane resins. Examples of suitable materials include cycloolefin resin, polystyrene, liquid crystal polymer (LCP), polyether ether ketone (PEEK) resin, polyphenylene sulfide (PPS), polyphenylene sulfone (PPSU), polyphenylene ether (PPE), bismaleimide-triazine resin (BT resin), fluororesin composite polyimide resin (film with a fluororesin layer formed on the surface of a polyimide resin), thermoplastic polyimide resin composite polyimide resin (film with a thermoplastic polyimide resin layer formed on the surface of a polyimide resin), cellulose nanofiber, silicon, silicon carbide, gallium nitride, sapphire, ceramics, glass, diamond-like carbon (DLC), and alumina.
[0024] In addition, a resin substrate containing a thermosetting resin and an inorganic filler can be suitably used as the support (A). Examples of the thermosetting resin include epoxy resin, phenol resin, unsaturated imide resin, cyanate resin, isocyanate resin, benzoxazine resin, oxetane resin, amino resin, unsaturated polyester resin, allyl resin, dicyclopentadiene resin, silicone resin, triazine resin, melamine resin, liquid crystal polymer (LCP), polyether ether ketone (PEEK) resin, polyphenylene sulfide (PPS), polyphenylene sulfone (PPSU), polyphenylene ether (PPE), etc. On the other hand, examples of the inorganic filler include silica, alumina, talc, mica, aluminum hydroxide, magnesium hydroxide, calcium carbonate, aluminum borate, borosilicate glass, etc. These thermosetting resins and inorganic fillers can be used alone or in combination of two or more.
[0025] The inorganic filler may be in the form of powder, flakes, fibers, or the like.
[0026] The support (A) may be in the form of a planar flexible material, a rigid material, or a rigid-flexible material. More specifically, the insulating substrate (A) may be a commercially available material formed into a film, sheet, or plate shape, or may be a material formed into a planar shape from a solution, melt, or dispersion of the above-mentioned resin. The support (A) may be a substrate in which the above-mentioned resin material is formed on a conductive material such as a metal, or a substrate in which the above-mentioned resin material is laminated on a printed wiring board on which a circuit pattern is formed.
[0027] In the case of flexible wiring boards, polyimide resin, modified polyimide resin (MPI), polytetrafluoroethylene resin, cycloolefin resin, polystyrene, liquid crystal polymer (LCP), polyphenylene sulfide (PPS), fluororesin composite polyimide resin (film with a fluororesin layer formed on the surface of polyimide resin, multilayer film with polyimide resin and fluororesin laminated alternately), thermoplastic polyimide resin composite polyimide resin (film with a thermoplastic polyimide resin layer formed on the surface of polyimide resin), etc. can be used.
[0028] When the support (A) is in the form of a film or sheet, the thickness is not particularly limited, but taking into consideration flexibility and bendability, the thickness is usually about 1 to 5,000 μm, more preferably 1 to 500 μm, and even more preferably 1 to 200 μm.
[0029] In the case of rigid wiring boards, composite substrates of glass fiber and epoxy resin (glass epoxy resin, FR-4, FR-5), composite substrate of paper and epoxy resin (FR-3), composite substrate of glass nonwoven fabric and epoxy resin (CEM-3), composite substrate of paper, glass nonwoven fabric and epoxy resin (CEM-1), composite substrate of paper and phenolic resin (paper phenolic resin, FR-1, FR-2), composite substrate of glass fiber and PPE resin (e.g. Panasonic's Megtron 6, Megtron 7, Megtron 8), composite substrate of glass fiber and maleimide resin, bismaleimide triazine resin (BT resin), composite substrate of ceramic and fluororesin (e.g. Examples of materials that can be used include: RO3003 manufactured by Rogers, composite substrates of silica and epoxy resin (for example, build-up film manufactured by Ajinomoto Co.), polyimide, liquid crystal polymer, polyether ether ketone, polyphenylene sulfide, polystyrene, polycarbonate, polyester resin, polypropylene, polyethylene, acrylic resin, urethane resin, cycloolefin polymer, silicon, silicon carbide, gallium nitride, gallium oxide, sapphire, ceramics, alumina ceramic, alumina, glass, diamond-like carbon, aluminum, stainless steel, copper, silver, gold, iron, nickel, etc.
[0030] Examples of the support (A) include synthetic fibers such as polyester fibers, polyamide fibers, and polyaramid fibers; inorganic fibers such as carbon fibers; and natural fibers such as cellulose nanofibers.
[0031] The surface of the support (A) is preferably smooth in a printed wiring board that requires high-frequency transmission. In the fifth generation mobile communication system (5G) and millimeter wave communication, the frequency of the alternating current is increasing for high-speed communication, and the higher the frequency, the more the skin effect occurs in which the current flows on the surface layer of the copper wiring. If the unevenness of the outermost surface layer of the copper wiring through which the current flows is large, it becomes a resistance and the transmission loss increases. Therefore, the surface of the support (A) is preferably smooth, and the surface roughness (maximum height Sz) measured with a laser microscope is preferably in the range of 0.001 to 50 μm, preferably in the range of 0.01 to 20 μm, and more preferably in the range of 0.05 to 10 μm. The surface roughness (maximum height Sz) is measured by the evaluation method described in ISO 25178 and represents the distance from the highest point to the lowest point on the surface.
[0032] The method for smoothing the support (A) includes a method for physically smoothing the surface of the support (A) and a method for smoothing the surface by chemical treatment. Examples of the physical smoothing method include calendaring, cutting, grinding, abrasive polishing, electric discharge machining, laser machining, and water jet machining, which smooth the surface by passing the support (A) between two smooth rolls. Examples of the chemical smoothing method include electrolytic polishing and etching polishing.
[0033] In addition, when the support (A) is an uncured or semi-cured thermosetting resin or a thermoplastic resin, a smooth metal foil such as a copper foil or an aluminum foil, or a heat-resistant film such as a smooth polyimide film or a fluororesin film can be used as a smoothing treatment substrate, and the smooth surface can be attached to the surface of the support (A) by thermocompression bonding, and then peeled off to transfer the smooth surface to the surface of the support (A). In particular, when the support (A) is a substrate for a rigid substrate containing a thermosetting resin such as an epoxy resin or a polyphenylene ether resin, glass fiber, or an inorganic filler, the smooth surface of the copper foil can be thermocompressed to the substrate using a press or the like, and then the copper foil can be removed by etching the copper foil with copper chloride or iron chloride to smooth the substrate surface. The surface roughness of the smoothing treatment substrate affects the surface roughness of the support (A) that is ultimately to be smoothed. Therefore, the surface roughness of the smoothing-treated substrate is preferably smooth, and the surface roughness (maximum height Sz) measured by a laser microscope is preferably in the range of 0.001 to 50 μm, more preferably in the range of 0.01 to 20 μm, and more preferably in the range of 0.05 to 10 μm. The surface roughness (maximum height Sz) is measured by the evaluation method described in ISO 25178, and represents the distance from the highest point to the lowest point on the surface.
[0034] In addition, since this can improve the adhesion between the support (A) and the primer layer (B) described below, the surface of the support (A) may be subjected to a surface treatment such as forming fine irregularities, cleaning off dirt adhering to the surface, or introducing functional groups such as hydroxyl groups, carbonyl groups, carboxyl groups, etc. Specifically, the surface may be subjected to a plasma discharge treatment such as corona discharge treatment, a dry treatment such as ultraviolet treatment, or a wet treatment using water, an aqueous solution of an acid or alkali, or an organic solvent, etc.
[0035] The primer layer (B) not only adheres to the plating underlayer (C) described later, but also adheres to the interlayer resin layer (F) described later. By forming the interlayer resin layer (F) by thermocompression bonding, the unreacted functional groups of the primer and the interlayer resin layer (F) react with each other, improving adhesion.
[0036] The primer layer (B) can be formed by applying a resin solution to a part or the whole of the surface of the support (A) and removing the solvent, such as the aqueous medium or the organic solvent, contained in the resin solution.
[0037] Examples of the method for applying the primer layer (B) to the surface of the support (A) include a gravure method, a coating method, a screen method, a roller method, a rotary method, and a spray method.
[0038] The surface of the primer layer (B) is preferably surface-treated by, for example, a plasma discharge treatment method such as a corona discharge treatment method, a dry treatment method such as an ultraviolet treatment method, or a wet treatment method using water, an acidic or alkaline chemical solution, an organic solvent, or the like, for the purpose of further improving adhesion to the plating underlayer (C) described below.
[0039] After the primer layer (B) is applied to the surface of the support (A), the solvent contained in the coating layer is generally removed by, for example, drying the coating layer using a dryer to volatilize the solvent. The drying temperature may be set within a range that allows the solvent to volatilize and does not cause adverse effects such as thermal deformation on the support (A).
[0040] The thickness of the primer layer (B) varies depending on the application of the laminate of the present invention, but is preferably in a range that further improves the adhesion between the support (A) and the plating underlayer (C) described below, and the thickness of the primer layer (B) is preferably in the range of 0.01 μm to 100 μm, preferably in the range of 0.05 μm to 50 μm, more preferably in the range of 0.1 μm to 30 μm, and even more preferably in the range of 0.2 μm to 5 μm.
[0041] As described above, the surface of the primer layer (B) is preferably smooth. Therefore, the surface roughness (maximum height Sz) measured by a laser microscope is preferably in the range of 0.001 to 30 μm, more preferably in the range of 0.01 to 20 μm, and more preferably in the range of 0.05 to 10 μm. The surface roughness (maximum height Sz) is measured by the evaluation method described in ISO 25178, and represents the distance from the highest point to the lowest point on the surface.
[0042] As the resin composition (b) for the primer layer used in forming the primer layer (B), those containing various resins and a solvent can be used.
[0043] Examples of the resin (b) include urethane resin, acrylic resin, core-shell type composite resin having urethane resin as the shell and acrylic resin as the core, epoxy resin, phenoxy resin, imide resin, amide resin, melamine resin, phenol resin, urea formaldehyde resin, blocked isocyanate polyvinyl alcohol obtained by reacting polyisocyanate with a blocking agent such as phenol, polyvinylpyrrolidone, etc. Note that the core-shell type composite resin having urethane resin as the shell and acrylic resin as the core can be obtained, for example, by polymerizing acrylic monomers in the presence of urethane resin. These resins can be used alone or in combination of two or more kinds.
[0044] The aminotriazine modified novolac resin is a novolac resin in which an aminotriazine ring structure and a phenol structure are bonded via a methylene group. The aminotriazine modified novolac resin can be obtained, for example, by co-condensing an aminotriazine compound such as melamine, benzoguanamine, or acetoguanamine with a phenol compound such as phenol, cresol, butylphenol, bisphenol A, phenylphenol, naphthol, or resorcin and formaldehyde in the presence of a weak alkaline catalyst such as an alkylamine or without a catalyst at about neutral, or by reacting an alkyl ether of an aminotriazine compound such as methyl etherified melamine with the phenol compound.
[0045] The aminotriazine-modified novolak resin is preferably one that does not substantially have a methylol group. The aminotriazine-modified novolak resin may contain a molecule in which only the aminotriazine structure is methylene-bonded, a molecule in which only the phenol structure is methylene-bonded, or the like, which is generated as a by-product during the production of the aminotriazine-modified novolak resin. Furthermore, the aminotriazine-modified novolak resin may contain a small amount of unreacted raw materials.
[0046] Examples of the phenol structure include a phenol residue, a cresol residue, a butylphenol residue, a bisphenol A residue, a phenylphenol residue, a naphthol residue, and a resorcinol residue. The term "residue" used herein means a structure in which at least one hydrogen atom bonded to a carbon atom of an aromatic ring has been removed. For example, in the case of phenol, it means a hydroxyphenyl group.
[0047] Examples of the triazine structure include structures derived from aminotriazine compounds such as melamine, benzoguanamine, and acetoguanamine.
[0048] The phenol structure and the triazine structure can be used alone or in combination of two or more. In addition, the phenol structure is preferably a phenol residue, and the triazine structure is preferably a structure derived from melamine, because these structures can further improve adhesion.
[0049] The hydroxyl value of the aminotriazine modified novolak resin is preferably in the range of 50 to 200 mgKOH / g, more preferably in the range of 80 to 180 mgKOH / g, and even more preferably in the range of 100 to 150 mgKOH / g, since this can further improve adhesion.
[0050] The aminotriazine-modified novolak resins can be used alone or in combination of two or more kinds.
[0051] When an aminotriazine-modified novolak resin is used as the compound having an aminotriazine ring, it is preferable to use an epoxy resin in combination.
[0052] Examples of the epoxy resin include bisphenol A type epoxy resin, bisphenol F type epoxy resin, biphenyl type epoxy resin, cresol novolac type epoxy resin, phenol novolac type epoxy resin, bisphenol A novolac type epoxy resin, alcohol ether type epoxy resin, tetrabromobisphenol A type epoxy resin, naphthalene type epoxy resin, phosphorus-containing epoxy compound having a structure derived from 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide derivative, epoxy resin having a structure derived from dicyclopentadiene derivative, epoxidized oil such as epoxidized soybean oil, etc. These epoxy resins can be used alone or in combination of two or more.
[0053] Among the epoxy resins, bisphenol A type epoxy resins, bisphenol F type epoxy resins, biphenyl type epoxy resins, cresol novolac type epoxy resins, phenol novolac type epoxy resins, and bisphenol A novolac type epoxy resins are preferred because they can further improve adhesion, and bisphenol A type epoxy resins are particularly preferred. The epoxy group of the epoxy resin reacts with a basic nitrogen atom-containing group contained in the plating underlayer (C) described below to form a covalent bond, thereby improving the adhesion at the interface between the plating underlayer (C) described below and the primer layer (B).
[0054] The epoxy equivalent of the epoxy resin is preferably in the range of 100 to 300 g / equivalent, more preferably in the range of 120 to 250 g / equivalent, and even more preferably in the range of 150 to 200 g / equivalent, because this can further improve adhesion.
[0055] When the primer layer (B) is a layer containing an aminotriazine-modified novolac resin and an epoxy resin, the molar ratio [(x) / (y)] of the phenolic hydroxyl group in the aminotriazine-modified novolac resin to the epoxy group in the epoxy resin is preferably in the range of 0.1 to 5, more preferably in the range of 0.2 to 3, and even more preferably in the range of 0.3 to 2, in order to further improve adhesion.
[0056] In order to promote the reaction between the aminotriazine-modified novolac resin and the epoxy resin, a curing accelerator may be used in combination. Examples of the curing accelerator include amine compounds having a primary, secondary, or tertiary amino group. In addition, any of aliphatic, alicyclic, and aromatic amine compounds can be used as the amine compound. In addition, mercaptans, acid anhydrides, boron acid fluorides, boric acid esters, organic acid hydrazides, Lewis acids, organometallic compounds, onium salts, and cationic compounds can also be used as the curing accelerator.
[0057] It is also preferable to use one containing a phenoxy resin. The primer layer (B) has a function of improving adhesion to the support (A) and the plating underlayer (C). In the present invention, it is preferable to use a phenoxy resin having a weight average molecular weight in the range of 10,000 to 100,000. By using a high molecular weight phenoxy resin for the primer layer (B), it is possible to improve the elongation of the polymer and further improve adhesion.
[0058] Phenoxy resin is a polyhydroxy polyether obtained by reacting a divalent phenol compound with epichlorohydrin, or by reacting a divalent epoxy compound with a divalent phenol compound. Examples of divalent phenol compounds include bisphenols. Examples of phenoxy resins include phenoxy resins having a bisphenol A structure (skeleton), phenoxy resins having a bisphenol F structure, phenoxy resins having a bisphenol S structure, phenoxy resins having a bisphenol M structure, phenoxy resins having a bisphenol P structure, and phenoxy resins having a bisphenol Z structure. Other examples include phenoxy resins having a skeleton structure such as a novolac structure, anthracene structure, fluorene structure, dicyclopentadiene structure, norbornene structure, naphthalene structure, biphenyl structure, and adamantane structure. These phenoxy resins may be used alone or in combination of two or more. Among these, those having a bisphenol structure are preferred, and bisphenol A skeleton, bisphenol F skeleton, and bisphenol S skeleton are more preferred. The terminal of the phenoxy resin may be any functional group such as a phenolic hydroxyl group or an epoxy group.
[0059] In the present invention, the weight average molecular weight of the phenoxy resin used is preferably in the range of 10,000 to 100,000. When the molecular weight is 10,000 or more, the plating adhesion after a long-term heat resistance test is high, and when the molecular weight is 100,000 or less, the solubility in organic solvents is improved, and the viscosity of the coating liquid when forming the primer layer (B) becomes appropriate, so that handling becomes good. The preferred weight average molecular weight of the phenoxy resin is 20,000 to 80,000, more preferably 22,000 to 50,000. The weight average molecular weight of the phenoxy resin can be adjusted by the molar ratio of the epoxy resin and the phenolic resin and the reaction time in the above reaction. In the present specification, the weight average molecular weight is a value measured by gel permeation chromatography (GPC) described later and converted into standard polystyrene. For the GPC measurement, a high-speed GPC device (HLC-8420GPC, manufactured by Tosoh Corporation) was used as the measurement device, and TSKgel G5000HxL / G4000HxL / G3000HxL / G2000HxL (manufactured by Tosoh Corporation) were used as the columns connected in series, and tetrahydrofuran was used as the eluent, and the measurement was performed using an RI detector. In addition, although a phenoxy resin generally means a high molecular weight epoxy resin, in this specification, the term "epoxy resin" means one having a weight average molecular weight of less than 10,000, and is to be distinguished from the above-mentioned phenoxy resin.
[0060] As the phenoxy resin, commercially available ones may be used. For example, 1256, 4250 (all of which are phenoxy resins containing a bisphenol A skeleton), 4275 (a mixed type of bisA / bisF), YL6794, YL7213, YL7290, YL7482, YL7553, YX8100 (phenoxy resin containing a bisphenol S skeleton), X6954 (phenoxy resin containing a bisphenol acetophenone skeleton, YX7200), all manufactured by Mitsubishi Chemical Corporation, may be used. (phenoxy resin containing a cyclohexane skeleton), YP-70 (bisphenol F type phenoxy resin), ZX356-2 (phenoxy resin containing bisphenol A and bisphenol F skeletons), YPB-40PXM40 (bromine-containing phenoxy resin), ERF-001M30 (phosphorus-containing phenoxy resin), FX-280, FX-293, FX-310 (phenoxy resin containing a fluorene skeleton), and PKHA, PKHB, PKHB+, PKHC, PKHH, PKHJ, PKFE, and the like manufactured by Gabriel Phenoxies.
[0061] In the present invention, the primer layer (B) preferably contains an epoxy resin in combination with the phenoxy resin. By using the phenoxy resin in combination with the epoxy resin, the adhesion to the metal plating layer (D) described below is further improved under normal conditions and after a long-term heat resistance test.
[0062] Examples of epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, biphenyl type epoxy resins, cresol novolac type epoxy resins, phenol novolac type epoxy resins, bisphenol A novolac type epoxy resins, alcohol ether type epoxy resins, tetrabromobisphenol A type epoxy resins, naphthalene type epoxy resins, phosphorus-containing epoxy compounds having a structure derived from 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide derivatives, epoxy resins having a structure derived from dicyclopentadiene derivatives, epoxidized oils and fats such as epoxidized soybean oil, etc. These epoxy resins may be used alone or in combination of two or more.
[0063] As the epoxy resin to be used in combination with the phenoxy resin, aromatic epoxy resins such as bisphenol A type epoxy resins, bisphenol F type epoxy resins, biphenyl type epoxy resins, cresol novolac type epoxy resins, phenol novolac type epoxy resins, bisphenol A novolac type epoxy resins and naphthalene type epoxy resins are preferred, as they can further improve the adhesion of the metal plating layer (D) described below, and furthermore, liquid epoxy resins are preferred, with bisphenol A type epoxy resins being particularly preferred.
[0064] The epoxy equivalent of the epoxy resin is preferably 100 to 5,000 g / equivalent, more preferably 120 to 2,000 g / equivalent, and even more preferably 120 to 250 g / equivalent, in that this allows for further improved adhesion.
[0065] When the primer layer (B) further contains an epoxy resin in addition to the phenoxy resin, the blending ratio of the phenoxy resin to the epoxy resin is preferably 90:10 to 10:90, and more preferably 85:15 to 15:80, on a mass basis.
[0066] The primer layer (B) is preferably made of a thermoplastic resin having excellent heat resistance that can conform to the metal plating layer (D) described below when the metal plating layer (D) is deformed under load such as heat. Examples of the preferred resins that can be used include phenoxy resin, urethane resin, acrylic resin, core-shell type composite resin having urethane resin as the shell and acrylic resin as the core, polyimide resin, polyphenylene ether resin, aromatic polyamide resin, polycarbonate resin, polyacetal resin, polybutylene terephthalate resin, polyphenylene sulfide resin, polysulfone resin, polyetherimide resin, polyethersulfone resin, polyamideimide resin, polyetheretherketone resin, and polytetrafluoroethylene resin.
[0067] The primer layer (B) may be one layer or may be two or more layers. When two or more primer layers (B) are formed, for example, the layer close to the plating base layer (C) described later improves adhesion with the plating base layer (C) described later, while the primer layer (B) close to the support (A) can improve adhesion with the support (A). In addition, the first primer layer (B) close to the plating base layer (C) described later becomes a layer close to the plating base layer (C) described later and the metal plating layer (D) described later, and becomes a part close to the copper wiring when a conductive pattern is formed, so that a resin composition of the primer layer (B) can be selected and formed for the purpose of improving insulation reliability.
[0068] In addition, since the paint for the primer layer (B) is applied to the surface of the support (A), it is preferable to mix an organic solvent to obtain a viscosity that is easy to apply. Examples of the organic solvent include ethyl acetate, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, isopropyl alcohol, diacetone alcohol, ethylene glycol, and toluene. These solvents can be used alone or in combination of two or more.
[0069] Furthermore, known additives such as film-forming assistants, leveling agents, thickeners, water repellents, antifoaming agents, and antioxidants may be appropriately added to the coating material for the primer layer (B) as required.
[0070] Examples of the method for applying the paint for the primer layer (B) include a gravure method, a coating method, a screen method, a roller method, a rotary method, a spray method, a capillary method, and a doctor roll method.
[0071] A typical method for removing the organic solvent contained in the coating layer after the coating material of the primer layer (B) is formed on the surface of the support (A) is, for example, drying using a dryer to volatilize the organic solvent.
[0072] The drying temperature for the primer layer (B) is preferably in the range of 50°C to 400°C, more preferably in the range of 80°C to 340°C, preferably in the range of 120°C to 280°C, and further preferably in the range of 150°C to 200°C.
[0073] The plating underlayer (C) is formed on the primer layer (B), and the metal constituting the plating underlayer (C) includes transition metals or their compounds, among which ionic transition metals are preferred. Examples of the ionic transition metals include copper, silver, gold, nickel, palladium, platinum, cobalt, and the like. Among these ionic transition metals, copper, silver, and gold are preferred because they have low electrical resistance and can provide a conductive pattern that is resistant to corrosion. The plating underlayer (C) is preferably porous, and in this case, has voids in the layer.
[0074] The method for producing the laminate of the present invention includes a method in which the primer layer (B) is formed on the support (A), then a fluid containing nano-sized metal nanoparticles (c) is applied, and the organic solvent contained in the fluid is removed by drying to form the plating underlayer (C), and then a metal plating layer (D) is formed by electrolytic or electroless plating. When forming the plating underlayer (C), a fluid containing the metal nanoparticles (c) is applied on the primer layer (B), dried to form the plating underlayer (C'), and then fired to remove the organic compound containing the dispersant present in the plating underlayer (C') to form voids and make the plating underlayer (C) porous, which is preferable because it improves adhesion with the metal plating layer (D) described below.
[0075] The shape of the metal nanoparticles (c) used to form the plating underlayer (C) is preferably particulate or fibrous. The size of the metal nanoparticles (c) is nano-sized. Specifically, when the shape of the metal nanoparticles (c) is particulate, a fine mesh-like conductive pattern can be formed, and the resistance value can be further reduced, so that the average particle size is preferably in the range of 1 to 100 nm, more preferably in the range of 1 to 50 nm. The "average particle size" is a volume average value measured by diluting the conductive material with a good dispersion solvent and measuring it by a dynamic light scattering method. For this measurement, "Nanotrac UPA-150" manufactured by Microtrac can be used.
[0076] On the other hand, when the metal nanoparticles (c) are fibrous, a fine mesh-like conductive pattern can be formed and the resistance value can be further reduced, so the fiber diameter is preferably in the range of 5 to 100 nm, more preferably in the range of 5 to 50 nm, and the fiber length is preferably in the range of 0.1 to 100 μm, more preferably in the range of 0.1 to 30 μm.
[0077] The content of the metal nanoparticles (c) in the fluid is preferably in the range of 1 to 90 mass %, more preferably in the range of 1 to 60 mass %, and further preferably in the range of 1 to 10 mass %.
[0078] The components to be blended into the fluid include dispersants and solvents for dispersing the metal nanoparticles (c) in the solvent, and, if necessary, surfactants, leveling agents, viscosity adjusters, film-forming aids, antifoaming agents, preservatives, etc., which will be described later.
[0079] In order to disperse the metal nanoparticles (c) in the solvent, it is preferable to use a low molecular weight or high molecular weight dispersant. Examples of the dispersant include dodecanethiol, 1-octanethiol, triphenylphosphine, dodecylamine, polyethylene glycol, polyvinylpyrrolidone, polyethyleneimine, polyvinylpyrrolidone; fatty acids such as myristic acid, octanoic acid, and stearic acid; polycyclic hydrocarbon compounds having a carboxyl group such as cholic acid, glycillic acid, and abintin acid. Among these, polymer dispersants are preferred because the adhesion between the plating underlayer (C) and the metal plating layer (D) described below can be improved by making the plating underlayer (C) porous. Examples of the polymer dispersant include polyalkyleneimines such as polyethyleneimine and polypropyleneimine, compounds in which polyoxyalkylene is added to the polyalkyleneimine, urethane resins, acrylic resins, and compounds containing a phosphoric acid group in the urethane resins or acrylic resins.
[0080] As described above, by using a polymer dispersant as the dispersant, the dispersant in the plating underlayer (C) can be removed to make it porous, and the void size can be increased to form voids of nano to submicron order sizes, compared to using a low molecular weight dispersant. This makes it easier for the metal constituting the metal plating layer (D) described later to fill these voids, and the filled metal acts as an anchor, greatly improving the adhesion between the plating underlayer (C) and the metal plating layer (D) described later.
[0081] The amount of the dispersant required to disperse the metal nanoparticles (c) is preferably 0.01 to 50 parts by mass, and more preferably 0.01 to 10 parts by mass, based on 100 parts by mass of the metal nanoparticles (c).
[0082] Furthermore, when the dispersant is removed by firing to form a porous plating base layer (C) for the purpose of further improving adhesion between the plating base layer (C) and the metal plating layer (D) described later, the amount of the dispersant is preferably 0.1 to 10 parts by mass, and more preferably 0.1 to 5 parts by mass, per 100 parts by mass of the nano-sized metal powder.
[0083] The solvent used for the fluid may be an aqueous medium or an organic solvent. Examples of the aqueous medium include distilled water, ion-exchanged water, pure water, and ultrapure water. Examples of the organic solvent include alcohol compounds, ether compounds, ester compounds, and ketone compounds.
[0084] Examples of the alcohol include methanol, ethanol, n-propanol, isopropyl alcohol, n-butanol, isobutyl alcohol, sec-butanol, tert-butanol, heptanol, hexanol, octanol, nonanol, decanol, undecanol, dodecanol, tridecanol, tetradecanol, pentadecanol, stearyl alcohol, allyl alcohol, cyclohexanol, terpineol, terpineol, dihydroterpineol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monoethyl ether, diethylene glycol monomethyl ether, diethylene glycol monobutyl ether, tetraethylene glycol monobutyl ether, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, tripropylene glycol monomethyl ether, propylene glycol monopropyl ether, dipropylene glycol monopropyl ether, propylene glycol monobutyl ether, dipropylene glycol monobutyl ether, and tripropylene glycol monobutyl ether.
[0085] In addition to the above-mentioned metal powder and solvent, the fluid may contain ethylene glycol, diethylene glycol, 1,3-butanediol, isoprene glycol, or the like, if necessary.
[0086] As the surfactant, a general surfactant can be used, and examples thereof include di-2-ethylhexyl sulfosuccinate, dodecylbenzenesulfonate, alkyldiphenyletherdisulfonate, alkylnaphthalenesulfonate, and hexametaphosphate.
[0087] As the leveling agent, a general leveling agent can be used, and examples thereof include silicone-based compounds, acetylene diol-based compounds, and fluorine-based compounds.
[0088] As the viscosity modifier, a general thickening agent can be used, and examples thereof include acrylic polymers and synthetic rubber latexes which can be thickened by adjusting the alkalinity, urethane resins which can be thickened by molecular association, hydroxyethyl cellulose, carboxymethyl cellulose, methyl cellulose, polyvinyl alcohol, water-added castor oil, amide wax, oxidized polyethylene, metal soaps, and dibenzylidene sorbitol.
[0089] As the film-forming aid, a general film-forming aid can be used, for example, anionic surfactants (such as dioctyl sulfosuccinate sodium salt), hydrophobic nonionic surfactants (such as sorbitan monooleate), polyether-modified siloxane, silicone oil, etc.
[0090] As the defoaming agent, a general defoaming agent can be used, for example, a silicone-based defoaming agent, a nonionic surfactant, a polyether, a higher alcohol, a polymer-based surfactant, and the like.
[0091] As the preservative, a general preservative can be used, and examples thereof include isothiazolinone-based preservatives, triazine-based preservatives, imidazole-based preservatives, pyridine-based preservatives, azole-based preservatives, iodine-based preservatives, and pyrithione-based preservatives.
[0092] The viscosity of the fluid (measured at 25° C. using a Brookfield viscometer) is preferably in the range of 0.1 to 500,000 mPa s, and more preferably in the range of 0.5 to 10,000 mPa s. When the fluid is applied (printed) by a method such as inkjet printing or letterpress reverse printing, which will be described later, the viscosity is preferably in the range of 5 to 20 mPa s.
[0093] Examples of methods for coating or printing the fluid on the primer layer (B) include inkjet printing, reverse printing, screen printing, offset printing, spin coating, spray coating, bar coating, die coating, slit coating, roll coating, dip coating, pad printing, gravure printing, and flexographic printing.
[0094] Among these coating methods, when forming the plating underlayer (C) patterned in fine lines of about 0.01 to 100 μm, which is required to realize high density electronic circuits, etc., it is preferable to use an inkjet printing method or a reverse printing method.
[0095] The inkjet printing method can be performed using a printer generally known as an inkjet printer. Specific examples include Konica Minolta EB100, XY100 (manufactured by Konica Minolta IJ Co., Ltd.), Dimatix Material Printer DMP-3000, and Dimatix Material Printer DMP-2831 (manufactured by Fuji Film Corporation).
[0096] In addition, as reverse printing methods, letterpress reverse printing and intaglio reverse printing are known, and examples of such methods include a method in which the fluid is applied to the surface of various blankets, which is then brought into contact with a plate having protruding non-image areas, and the fluid corresponding to the non-image areas is selectively transferred to the surface of the plate to form the pattern on the surface of the blanket, etc., and then the pattern is transferred onto the top (surface) of the support (A).
[0097] For printing a pattern when the support (A) is a molded product, a pad printing method is known, which involves placing ink on an intaglio plate, writing it down with a squeegee to uniformly fill the ink in the recesses, pressing a pad made of silicone rubber or urethane rubber onto the plate on which the ink has been placed, and transferring the pattern onto the pad, which is then transferred to the molded product.
[0098] The plating underlayer (C) may be one layer or two or more layers. When two or more plating underlayers (C) are formed, for example, a coating defect occurring in the first plating underlayer (C) is covered by the second plating underlayer (C), thereby eliminating the coating defect.
[0099] The drying temperature after coating or printing the fluid is preferably in the range of 50°C to 400°C, more preferably in the range of 80°C to 340°C, preferably in the range of 120°C to 320°C, preferably in the range of 150°C to 300°C, and even more preferably in the range of 180°C to 280°C.
[0100] The mass per unit area of the plating underlayer (C) is 1 to 10,000 mg / m 2 The range is preferably 1 to 5,000 mg / m 2 In the case where electroless plating is performed on the plating underlayer (C), the plating underlayer (C) is used as a catalyst, so the thickness of the plating underlayer (C) may be thin, specifically, 1 to 5,000 mg / m 2 is preferable, and 10 to 1,000 mg / m 2 is preferable, and 10 to 500 mg / m 2 is preferable, and 50 to 500 mg / m 2 On the other hand, when electrolytic plating is performed on the plating underlayer (C), it is preferable that the plating underlayer (C) has conductivity and low resistance, so that the film thickness is preferably thicker, and is preferably 100 to 10,000 mg / m 2 is preferable, and 300 to 5,000 mg / m 2 is preferable. In order to improve the adhesion between the metal plating layer (D) and the plating underlayer (C) described later and to reduce the cost by making the plating underlayer (C) thin, the plating concentration is preferably 500 to 2,000 mg / m2 is more preferred.
[0101] When electrolytic plating is performed on the plating underlayer (C), the surface resistance of the plating underlayer (C) is preferably low in order to form the electrolytic plating uniformly. The surface resistance is preferably in the range of 0.1 to 10,000 Ω / □, more preferably in the range of 0.15 to 1,000 Ω / □, more preferably in the range of 0.15 to 500 Ω / □, more preferably in the range of 0.2 to 100 Ω / □, more preferably in the range of 0.2 to 10 Ω / □, and even more preferably in the range of 0.2 to 5 Ω / □.
[0102] As described above, the surface of the plating underlayer (C) is preferably smooth. Therefore, the surface roughness (maximum height Sz) measured by a laser microscope is preferably in the range of 0.001 to 30 μm, more preferably in the range of 0.01 to 20 μm, and more preferably in the range of 0.05 to 10 μm. The surface roughness (maximum height Sz) is measured by the evaluation method described in ISO 25178, and represents the distance from the highest point to the lowest point on the surface.
[0103] In addition, as a method for forming the primer layer (B) and the plating base layer (C) on the support (A), there is a method in which the plating base layer (C) and the primer layer (B) are sequentially laminated on a temporary support (G) to produce a transfer laminate, and the surface of the primer layer (B) of the transfer laminate is bonded to at least one surface of the support (A).
[0104] The method of laminating by the transfer method is a simple method that enables the primer layer (B) and the plating underlayer (C) to be formed on the support (A) in one step by thermocompression bonding, and therefore has excellent productivity and reduces manufacturing costs, compared with the existing methods of applying a coating by a sputtering method or a wet process carried out on the support (A). Furthermore, it is preferable from the viewpoint of strengthening the adhesion at the interface between the primer layer (B) and the plating underlayer (C) by applying pressure by thermocompression bonding to bury the plating underlayer (C) in the primer layer (B).
[0105] Since the temporary support (G) needs to be finally peeled off after the transfer laminate is bonded, it is preferable to select one that can be easily peeled off at the interface between the temporary support (G) and the plating underlayer (C). For example, examples of polymer films include aromatic polyesters such as polyethylene terephthalate, polybutylene terephthalate (PBT), polyethylene naphthalate, and polybutylene naphthalate; fluorine-based resins such as polytetrafluoroethylene, tetrafluoroethylene perfluoroalkyl vinyl ether copolymer, tetrafluoroethylene-hexafluoropropylene copolymer, tetrafluoroethylene-ethylene copolymer, vinylidene fluoride resin, trifluorochloroethylene resin, trifluorochloroethylene-ethylene copolymer, tetrafluoroethylene-perfluorodioxysol copolymer, vinyl fluoride resin, and polyvinylidene fluoride; polymethylpentene (TPX), polypropylene (PP) [including biaxially oriented polypropylene (OPP) and nonaxially oriented polypropylene (CPP)], and polyethylene (PE) [high density poly Examples of the suitable materials include olefin resins such as ethylene (HDPE), low density polyethylene (LDPE), linear low density polyethylene (LLDPE), etc.; polystyrene (PS); polyimide resins such as polyvinyl chloride (PVC), polyimide, transparent polyimide, etc.; polyamide resins such as polyamideimide and polyamide; polycarbonate, acrylonitrile-butadiene-styrene (ABS) resin, polymer alloy of ABS and polycarbonate, acrylic resins such as poly(methyl meth)acrylate, polyvinyl chloride, polyvinylidene chloride, polyvinyl alcohol, polycarbonate, polyethylene, polypropylene, polyurethane, liquid crystal polymer (LCP), polyether ether ketone (PEEK), polyphenylene sulfide (PPS), polyphenylene sulfone (PPSU), epoxy resins, etc. Among them, aromatic polyester, polyethylene, olefin resin, fluorine-based resin, polyimide resin, LCP, polyphenylene sulfide, and polystyrene are preferably used as the temporary support (G).
[0106] The temporary support (G) may be made of a metal, such as copper, aluminum, an aluminum alloy, titanium, stainless steel, beryllium copper, phosphor bronze, nickel, nichrome, a nickel alloy, tin, zinc, lead, gold, zinc, lead, tantalum, molybdenum, niobium, iron, or silver. In addition, the temporary support (G) may be made of an inorganic base material such as silicon, ceramics, or glass.
[0107] The shape of the temporary support (G) is not particularly limited, but a film or sheet is easy to handle. The film thickness of the temporary support (G) is usually preferably in the range of 1 to 5,000 μm, more preferably in the range of 1 to 300 μm, more preferably in the range of 1 to 200 μm, more preferably in the range of 1 to 100 μm, and even more preferably in the range of 1 to 50 μm. The temporary support (G) is attached to the support (A), and after the plating underlayer (C) and the primer layer (B) are transferred and laminated to the support (A), it becomes unnecessary, so it is preferable that the temporary support is thin enough not to lose workability.
[0108] The surface of the temporary support (G) is preferably smooth so as to facilitate the transfer of the plating underlayer (C) and the primer layer (B) from the transfer laminate. Specifically, the surface roughness (maximum height Sz) measured by a laser microscope is preferably in the range of 0.001 to 50 μm, more preferably in the range of 0.01 to 20 μm, and more preferably in the range of 0.05 to 10 μm. The surface roughness (maximum height Sz) is measured by the evaluation method described in ISO 25178, and represents the distance from the highest point to the lowest point on the surface.
[0109] In addition, a release layer formed on the surface of the temporary support (G) can be used. The release layer can be formed by applying a silicone-based release agent or a non-silicone-based release agent to the temporary support (G). As the non-silicone-based release agent, an alkyd resin, a melamine resin, an acrylic resin, a cellulose resin, a urea resin, a polyolefin, a paraffin, a silica composite acrylic resin, a silica composite melamine resin, a silica composite urethane resin, a silica composite epoxy-based resin, a silica composite phenolic resin, a silica composite poval resin, a silica composite polystyrene-based resin, a silica composite polyvinyl acetate-based resin, a silica composite polyimide-based resin, and a silica composite polyamideimide-based resin can be used. When the temporary support (G) of the transfer laminate is peeled off, the silicone resin of the release layer of the silicone resin migrates to the surface of the plating base layer (C), and when a metal plating layer (D) is formed on the plating base layer (C) described later, the silicone resin inhibits the adhesion between the plating base layer (C) and the metal plating layer (D). For this reason, it is preferable to use a non-silicone-based release agent for the release layer, and it is preferable to use polyolefin, acrylic resin, melamine resin, urethane resin, silica composite acrylic resin, silica composite melamine resin, silica composite urethane resin, silica composite epoxy-based resin, silica composite phenolic resin, silica composite poval resin, silica composite polystyrene-based resin, silica composite polyvinyl acetate-based resin, silica composite polyimide-based resin, or silica composite polyamideimide-based resin.
[0110] The thickness of the release layer is not particularly limited as long as it can secure releasability, but it is preferably a thin film to prevent the release layer from adhering to the surface of the plating underlayer (C). Specifically, the thickness is preferably 0.01 to 50 μm, more preferably 0.01 to 10 μm, and even more preferably 0.01 to 1 μm.
[0111] It is preferable to use a metal as the temporary support (G). When forming the plating underlayer (C) using metal nanoparticles on the surface of the temporary support (G) described later, the plating underlayer (C) can be dried at a higher temperature than when a polymer film is used, and the surface resistance of the plating underlayer (C) can be reduced, thereby increasing the conductivity of the plating underlayer itself. In addition, in the process of forming a conductive pattern, after laminating the surface of the primer layer (B) of the transfer laminate described later to the support (A), when forming through holes penetrating both sides from the surface of the temporary support (G) or non-through holes to the conductive pattern of the inner layer, holes are formed with a drill or laser, but when a polymer film is used as the temporary support (G), polymer smears occur during hole drilling, and plating precipitation problems may occur in the process of making the through holes or non-through holes conductive. On the other hand, when a metal is used, a conventional drilling method using a laser for printed circuit boards can be applied, and it is preferable to use copper or aluminum as the temporary support (G).
[0112] When the plating underlayer (C) described later is applied to the temporary support (G), the surface of the temporary support (G) may be subjected to a surface treatment, if necessary, for the purpose of making the surface of the temporary support (G) more easily wetted with a coating material. Specifically, methods such as plasma discharge treatment such as corona discharge treatment, dry treatment such as ultraviolet treatment, and wet treatment using water, an aqueous solution of an acid or alkali, or an organic solvent, etc., may be mentioned. If the temporary support (G) is subjected to an excessive surface treatment, peeling at the interface between the temporary support (G) and the plating underlayer (C) described later becomes difficult, so it is preferable to perform the surface treatment appropriately.
[0113] Examples of a method for coating or printing the plating underlayer (C) on the temporary support (G) include inkjet printing, reverse printing, screen printing, offset printing, gravure printing, flexographic printing, pad printing, spin coating, spray coating, bar coating, die coating, slit coating, roll coating, dip coating, rotary coating, capillary coating, microgravure coating, and doctor roll methods.
[0114] The plating underlayer (C) may be one layer or two or more layers. When two or more plating underlayers (C) are formed, for example, a coating defect occurring in the first plating underlayer (C) is covered by the second plating underlayer (C), thereby eliminating the coating defect.
[0115] When the plating underlayer (C) is applied onto the temporary support (G), the drying temperature after coating or printing is preferably in the range of 50°C to 400°C, more preferably in the range of 80°C to 340°C, preferably in the range of 120°C to 320°C, preferably in the range of 150°C to 300°C, and even more preferably in the range of 180°C to 280°C.
[0116] The primer layer (B) can be formed by applying the primer layer (B) to a part or all of the plating base layer (C) formed on the surface of the temporary support (G), and removing the organic solvent contained in the coating material for the primer layer (B).
[0117] Examples of the method for applying the paint for the primer layer (B) include a gravure method, a coating method, a screen method, a roller method, a rotary method, a spray method, a capillary method, and a doctor roll method.
[0118] The coating material of the primer layer (B) is applied to the surface of the plating underlayer (C) formed on the surface of the temporary support (G), and then the organic solvent contained in the coating layer is generally removed by, for example, drying the coating layer using a dryer to volatilize the organic solvent. The drying temperature must be set within a range that allows the organic solvent used to volatilize.
[0119] The drying temperature for the primer layer (B) is preferably in the range of 50°C to 400°C, more preferably in the range of 80°C to 340°C, preferably in the range of 120°C to 280°C, and further preferably in the range of 150°C to 200°C.
[0120] Next, a method for transferring the transfer laminate onto the support (A) will be described. As a transfer method, a method of laminating the surface of the primer layer (B) of the transfer laminate to the support (A) using heat and pressure can be used. Although not particularly limited, for example, a thermal lamination method, a solventless lamination method, an extrusion lamination method, a wet lamination method, a hot roll transfer method, an in-mold transfer method, a pressing method, a vacuum pressing method, a hydraulic transfer method, etc. can be used.
[0121] When the support (A) is a flexible material and a roll film, it is preferable to use a hot roll lamination method, a solventless lamination method, an extrusion lamination method, or a wet lamination method. In particular, the hot roll lamination method is more preferable because it can be easily processed. On the other hand, when the support (A) is a rigid material, it is preferable to use a press method, a vacuum press method, or a vacuum hot lamination method because it is often thermocompressed in a sheet-like manner.
[0122] Regarding the thermocompression bonding conditions, the heating conditions are preferably in the range of 50° C. to 400° C., more preferably in the range of 80° C. to 350° C., more preferably in the range of 80° C. to 280° C., more preferably in the range of 100° C. to 200° C., and more preferably in the range of 120 to 180° C. The pressure conditions are preferably in the range of 0.05 MPa to 35 MPa, and more preferably in the range of 0.3 MPa to 20 MPa.
[0123] In the case of hot roll lamination, the processing time for thermocompression bonding is within 1 second because the thermocompression bonding is performed by the linear pressure of the roll while the film is being transported. On the other hand, in the case of pressing, vacuum pressing, and vacuum hot lamination which process the film sheet by sheet, the processing time is preferably in the range of 1 second to 120 minutes, more preferably in the range of 30 seconds to 60 minutes, and more preferably in the range of 30 seconds to 15 minutes, and from the viewpoint of productivity, the processing time is preferably in the range of 1 minute to 5 minutes.
[0124] In addition, when performing thermocompression bonding, air may get between the transfer laminate and the support (A), or the gas generated from the support (A) or the transfer laminate may accumulate between the transfer laminate and the support (A), resulting in a decrease in the transfer rate. Therefore, it is preferable to perform thermocompression bonding under vacuum using a vacuum press. As for the vacuum conditions, the absolute pressure is preferably 100 hPa or less, more preferably 50 hPa or less, and more preferably 13 hPa or less. It is preferable to perform the treatment under the same heating and pressure conditions as described above.
[0125] Next, a method of laminating the surface of the primer layer (B) of the transfer laminate to the support (A) and peeling off the temporary support (G) will be described. The method of peeling off the temporary support (G) is not particularly limited, but when the adhesion between the support (A) and the primer layer (B) is low during the thermocompression bonding (temporary adhesion state), the primer layer (B) and the plating underlayer (C) may not be sufficiently transferred to the support (A) and may remain partially on the transfer laminate side, so the direction and speed of peeling off the temporary support (G) when peeling off is important. Specifically, it is preferable to peel off the support (A) in a direction of 90 degrees to 180 degrees, preferably in a range of 120 degrees to 180 degrees, and preferably in a direction of 150 degrees to 180 degrees. When peeling off, it is preferable to peel off the temporary support (G) side at the above-mentioned angle, not the support (A) side. The peeling speed is preferably in the range of 0.01 m / min to 20 m / min, more preferably in the range of 0.05 to 10 m / min, and even more preferably in the range of 0.5 to 5 m / min.
[0126] Next, the surface of the primer layer (B) of the transfer laminate is laminated onto the support (A), and then the temporary support (G) of the transfer laminate is peeled off. The post-treatment of the laminate will be described below. To further improve the adhesion between the support (A) and the primer layer (B), a heat treatment may be performed. The heat treatment conditions are preferably in the range of 80° C. to 400° C., more preferably in the range of 100° C. to 350° C., more preferably in the range of 120° C. to 325° C., and still more preferably in the range of 150° C. to 300° C. The heat treatment time is preferably in the range of 1 second to 168 hours, more preferably in the range of 30 seconds to 72 hours, and further preferably in the range of 1 minute to 30 minutes from the viewpoint of productivity.
[0127] In the next step, a metal plating layer (D) or a pattern resist is formed on the surface of the plating underlayer (C), so it is preferable to carry out a cleaning treatment to clean off components that reduce the adhesion of these layers. Examples of components that reduce adhesion include oligomer components that are present in the film and bleed onto the film surface when the temporary support (G) is a resin film, components of the release agent that are partially transferred to the plating underlayer (C) when a release layer is formed on the temporary support (G), and a metal oxide film on the temporary support when the temporary support (G) is made of metal. Examples of the cleaning treatment include oxidative decomposition of organic matter present on the surface of the plating underlayer (C) by heating, plasma discharge treatment such as corona discharge treatment, dry treatment such as ultraviolet treatment, and wet treatment using water, an aqueous solution of an acid or alkali, water containing ozone (ozone nanobubbles), or an organic solvent.
[0128] When the laminate of the present invention is used as metal wiring described later, the plating underlayer (C), metal plating layer (D), etc. may be removed by etching described later, and a metal wiring pattern may be formed to produce the metal wiring.
[0129] The metal plating layer (D) constituting the laminate of the present invention is a layer provided for the purpose of forming a highly reliable wiring pattern capable of maintaining good electrical conductivity for a long period of time without causing breaks or the like, for example, when the laminate is used for a conductive pattern or the like.
[0130] Examples of metals constituting the metal plating layer (D) include copper, nickel, chromium, cobalt, tin, etc. Among these, copper is preferred because it has low electrical resistance and can provide a conductive pattern that is resistant to corrosion.
[0131] In the laminate of the present invention, it is preferable that the voids present in the plating base layer (C) are filled with the metal constituting the metal plating layer (D), and it is preferable that the metal constituting the metal plating layer (D) is filled up to the voids in the plating base layer (C) present in the vicinity of the interface between the support (A) and the plating base layer (C), because this further improves the adhesion between the plating base layer (C) and the metal plating layer (D).
[0132] The metal plating layer (D) is a layer formed on the plating underlayer (C), and is preferably formed by a plating process. Examples of the plating process include wet plating methods such as electrolytic plating and electroless plating, and dry plating methods such as sputtering and vacuum deposition. The metal plating layer (D) may be formed by combining two or more of these plating methods.
[0133] The electroless plating method is, for example, a method in which an electroless plating solution is brought into contact with a metal constituting the plating underlayer (C), thereby precipitating a metal such as copper contained in the electroless plating solution and forming an electroless plating layer (film) consisting of a metal film.
[0134] The electroless plating solution may contain, for example, a metal such as copper, nickel, chromium, cobalt, or tin, a reducing agent, and a solvent such as an aqueous medium or an organic solvent.
[0135] Examples of the reducing agent include dimethylaminoborane, hypophosphorous acid, sodium hypophosphite, dimethylamineborane, hydrazine, formaldehyde, sodium borohydride, and phenol.
[0136] The electroless plating solution may contain, as necessary, a complexing agent such as a monocarboxylic acid, such as acetic acid or formic acid; a dicarboxylic acid compound, such as malonic acid, succinic acid, adipic acid, maleic acid or fumaric acid; a hydroxycarboxylic acid compound, such as malic acid, lactic acid, glycolic acid, gluconic acid or citric acid; an amino acid compound, such as glycine, alanine, iminodiacetic acid, arginine, aspartic acid or glutamic acid; an aminopolycarboxylic acid compound, such as iminodiacetic acid, nitrilotriacetic acid, ethylenediaminediacetic acid, ethylenediaminetetraacetic acid or diethylenetriaminepentaacetic acid; or a soluble salt (sodium salt, potassium salt, ammonium salt, etc.) of these organic acids, or an amine compound, such as ethylenediamine, diethylenetriamine or triethylenetetramine.
[0137] The electroless plating solution is preferably used at a temperature in the range of 20 to 98°C.
[0138] The electrolytic plating method is a method in which, for example, an electric current is passed through an electrolytic plating solution in contact with a metal constituting the plating base layer (C) or the surface of the electroless plating layer (film) formed by the electroless treatment, thereby precipitating a metal such as copper contained in the electrolytic plating solution onto the surface of a conductive material constituting the plating base layer (C) placed at a cathode or the electroless plating layer (film) formed by the electroless treatment, thereby forming an electrolytic plating layer (metal film).
[0139] The electrolytic plating solution may contain, for example, a sulfide of a metal such as copper, nickel, chromium, cobalt, or tin, sulfuric acid, and an aqueous medium. Specifically, the electrolytic plating solution may contain copper sulfate, sulfuric acid, and an aqueous medium.
[0140] The electrolytic plating solution is preferably used at a temperature in the range of 20 to 98°C.
[0141] The electrolytic plating method does not use highly toxic substances and has good workability, so it is preferable to form the metal plating layer (D) made of copper using an electrolytic plating method.
[0142] The dry plating process may be performed by sputtering, vacuum deposition, etc. The sputtering method is a method in which an inert gas (mainly argon) is introduced in a vacuum, negative ions are applied to the material for forming the metal plating layer (D) to generate a glow discharge, the inert gas atoms are then ionized, and the gas ions are violently bombarded at high speed onto the surface of the material for forming the metal plating layer (D), ejecting atoms and molecules constituting the material for forming the metal plating layer (D) and causing them to adhere vigorously to the surface of the plating underlayer (C), thereby forming the metal plating layer (D).
[0143] Examples of materials for forming the metal plating layer (D) by the sputtering method include chromium, copper, titanium, silver, platinum, gold, nickel-chromium alloy, stainless steel, copper-zinc alloy, indium tin oxide (ITO), silicon dioxide, titanium dioxide, niobium oxide, and zinc oxide.
[0144] When plating by the sputtering method, for example, a magnetron sputtering device or the like can be used.
[0145] The thickness of the metal plating layer (D) is preferably in the range of 0.05 to 100 μm, more preferably 1 to 50 μm, and further preferably 5 to 18 μm. The thickness of the metal plating layer (D) can be adjusted by controlling the treatment time, current density, amount of plating additives used, etc. in the plating treatment step when forming the metal plating layer (D).
[0146] As described above, the surface of the metal plating layer (D) is preferably smooth. Therefore, the surface roughness (maximum height Sz) measured by a laser microscope is preferably in the range of 0.001 to 20 μm, more preferably in the range of 0.01 to 15 μm, and more preferably in the range of 0.05 to 10 μm. The surface roughness (maximum height Sz) is measured by the evaluation method described in ISO 25178, and represents the distance from the highest point to the lowest point on the surface.
[0147] Examples of the method for patterning the metal plating layer (D) include photolitho-etching methods such as a subtractive method and a semi-additive method, and a method of plating on the printed pattern of the plating underlayer (C).
[0148] The subtractive method is a method in which an etching resist layer having a shape corresponding to a desired pattern shape is formed on the metal plating layer (D) constituting the laminate of the present invention that has been previously produced, and then a developing process is performed to dissolve and remove the plating underlayer (C), the metal plating layer (D), etc., from the portion where the resist has been removed, with a chemical solution, thereby forming a desired pattern. As the chemical solution, a chemical solution containing copper chloride, iron chloride, etc. can be used.
[0149] The semi-additive method is a method in which the primer layer (B) and the plating underlayer (C) are formed on both sides or one side of the support (A), a plating resist layer having a shape corresponding to a desired pattern is formed on the surface of the plating underlayer (C), a metal plating layer (D) is then formed by an electrolytic plating method, an electroless plating method or a combination thereof, and the plating resist layer and the plating underlayer (C) in contact therewith are then dissolved and removed in a chemical solution or the like to form a desired pattern.
[0150] In addition, the method of plating on the printed pattern of the plating base layer (C) is a method in which the pattern of the plating base layer (C) is printed on the primer layer (B) formed on both sides or one side of the support (A) by an inkjet method, a reverse printing method, or the like, and the metal plating layer (D) is formed on the surface of the plating base layer (C) by an electrolytic plating method, an electroless plating method, or a combination thereof, thereby forming a desired pattern.
[0151] By using the above-mentioned technique, the metal plating layer (D) is patterned to form copper wiring, and then an adhesive layer (E) is formed on the surface of the copper wiring, making it possible to produce a highly reliable laminate that has excellent adhesion to the interlayer resin layer (F) described below without the need for roughening treatment of the wiring.
[0152] The adhesive layer (E) can be formed by applying a solution containing the composition described below to part or all of the surface of the patterned metal plating layer (D) and removing the solvent, such as the aqueous medium or organic solvent, contained in the solution.
[0153] Examples of the method for applying the adhesive layer (E) to the surface of the patterned metal plating layer (D) include a coating method, a dipping method, a roller coating method, a spin coating method, a rotary method, a spray method, a dispenser method, an inkjet printing method, a pad printing method, a reverse printing method, a flexographic printing method, a screen printing method, a gravure printing method, a gravure offset printing method, etc. Specifically, a method of immersion by a dipping method is exemplified.
[0154] In order to form the adhesive layer (E), in order to further improve adhesion with the metal plating layer, it is preferable that the surface is treated by, for example, a plasma discharge treatment method such as a corona discharge treatment method, a dry treatment method such as an ultraviolet treatment method, or a wet treatment method using water, an acidic or alkaline chemical solution, an organic solvent, or the like.
[0155] A typical method for removing the solvent contained in the coating layer after applying the adhesive layer (E) to the surface of the patterned metal plating layer (D) is, for example, drying the coating layer with a dryer to volatilize the solvent. The drying temperature may be set within a range that allows the solvent to volatilize and does not adversely affect the support (A), the primer layer (B), the plating underlayer (C), and the metal plating layer (D), such as thermal deformation.
[0156] The film thickness of the adhesive layer (E) consisting of the compositions (e), (e'), (e'') and (e''') described below varies depending on the application of the laminate of the present invention, but is preferably in a range that further improves the adhesion between the patterned metal plating layer (D) and the interlayer resin layer (F) described below without reducing the adhesion to the resin, and the film thickness of the adhesive layer (E) is preferably 0.001 to 1 μm, more preferably 0.005 to 0.8 μm, and even more preferably 0.01 to 0.5 μm.
[0157] As described above, the surface of the adhesive layer (E) is preferably smooth. Therefore, the surface roughness (maximum height Sz) measured by a laser microscope is preferably in the range of 0.001 to 20 μm, more preferably in the range of 0.01 to 15 μm, and more preferably in the range of 0.05 to 10 μm. The surface roughness (maximum height Sz) is measured by the evaluation method described in ISO 25178, and represents the distance from the highest point to the lowest point on the surface.
[0158] The adhesive layer composition (e) used to form the adhesive layer (E) may contain various organic compounds and a solvent.
[0159] As the composition (e), an organic silane compound is most suitable for adhesion with organic and inorganic materials. For example, mercaptosilane compounds, vinyl silane compounds, vinylphenyl silane compounds, epoxy silane compounds, acryloxy silane compounds, methacryloxy silane compounds, amino silane compounds, ureido silane compounds, chloropropyl silane compounds, sulfido silane compounds, isocyanate silane compounds, triazole silane compounds, thiadiazole silane compounds, isocyanatopropyl silane compounds, styryl silane compounds, carboxy silane compounds, alkoxy silane compounds, triazine silane compounds, imidazole silane compounds, azole silane compounds, pyrrole silane compounds, pyrazole silane compounds, tetrazole silane compounds, indole silane compounds, isoindole silane compounds, indazole silane compounds, benzimidazole silane compounds, benzotriazole silane compounds, etc. can be mentioned. In addition, these silane compounds can be used alone or in combination of two or more kinds. For example, Glicap treatment by Shikoku Chemical Industry Co., Ltd. can be used.
[0160] As the composition (e'), an organic resin composition is also suitable for adhesion to organic and inorganic materials. For example, urethane resin, acrylic resin, core-shell type composite resin having urethane resin as the shell and acrylic resin as the core, epoxy resin, phenoxy resin, imide resin, amide resin, melamine resin, phenol resin, urea formaldehyde resin, blocked isocyanate polyvinyl alcohol obtained by reacting a blocking agent such as phenol with polyisocyanate, polyvinylpyrrolidone, etc. are mentioned. In addition, a core-shell type composite resin having urethane resin as the shell and acrylic resin as the core can be obtained, for example, by polymerizing an acrylic monomer in the presence of urethane resin. In addition, these resins can be used alone or in combination of two or more kinds.
[0161] The organic compound used for molecular bonding in the composition (e'') is also suitable for adhesion between organic and inorganic materials. Examples include triazine thiol compounds, triazine azide compounds, triazine amino compounds, triazine isoyanate compounds, triazine urethane compounds, triazine ester compounds, and triazine silane compounds. These resins can be used alone or in combination of two or more. For example, molecular bonding treatment manufactured by Io Chemical Laboratory Co., Ltd. can be used.
[0162] In addition, since the coating material for the adhesive layer (E) made of the composition (e) is applied to the surface of the patterned metal plating layer (D), it is preferable to mix an aqueous medium or an organic solvent to obtain a viscosity that is easy to apply. Examples of the aqueous medium include distilled water, ion-exchanged water, pure water, and ultrapure water. Examples of the organic solvent include alcohol compounds, ether compounds, ester compounds, and ketone compounds.
[0163] Examples of the alcohol include methanol, ethanol, n-propanol, isopropyl alcohol, n-butanol, isobutyl alcohol, sec-butanol, tert-butanol, heptanol, hexanol, octanol, nonanol, decanol, undecanol, dodecanol, tridecanol, tetradecanol, pentadecanol, stearyl alcohol, allyl alcohol, cyclohexanol, terpineol, terpineol, dihydroterpineol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monoethyl ether, diethylene glycol monomethyl ether, diethylene glycol monobutyl ether, tetraethylene glycol monobutyl ether, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, tripropylene glycol monomethyl ether, propylene glycol monopropyl ether, dipropylene glycol monopropyl ether, propylene glycol monobutyl ether, dipropylene glycol monobutyl ether, and tripropylene glycol monobutyl ether.
[0164] In addition, the coating material for the adhesive layer (E) made of the composition (e) may contain, as necessary, known additives such as film-forming assistants, leveling agents, thickeners, water repellents, defoamers, and antioxidants.
[0165] A coating material for the adhesive layer (E) made of the composition (e) is formed on the surface of the patterned metal plating layer (D), and then the solvent contained in the coating layer is generally removed by, for example, drying using a dryer to volatilize the organic solvent.
[0166] The drying temperature of the coating material for the adhesive layer (E) made of the composition (e) is preferably in the range of 10°C to 200°C, more preferably in the range of 20°C to 150°C, and even more preferably in the range of 30°C to 120°C.
[0167] Furthermore, since the coating material for the adhesive layer (E) made of the composition (e') or the composition (e'') is applied to the surface of the patterned metal plating layer (D), it is preferable to blend an organic solvent in order to give it a viscosity that is easy to apply. Examples of the organic solvent include ethyl acetate, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, isopropyl alcohol, diacetone alcohol, ethylene glycol, toluene, and the like. These solvents can be used alone or in combination of two or more.
[0168] In addition, the coating material for the adhesive layer (E) made of the composition (e') or the composition (e'') may contain, as necessary, known additives such as film-forming aids, leveling agents, thickeners, water repellents, defoamers, and antioxidants.
[0169] A coating material of the adhesive layer (E) made of the composition (e') or the composition (e'') is formed on the surface of the patterned metal plating layer (D), and then the organic solvent contained in the coating layer is generally removed by, for example, drying using a dryer to volatilize the organic solvent.
[0170] The drying temperature of the adhesive layer (E) made of the composition (e') or the composition (e'') is preferably in the range of 50°C to 400°C, more preferably in the range of 80°C to 340°C, preferably in the range of 120°C to 280°C, and even more preferably in the range of 150°C to 200°C.
[0171] The adhesive layer composition (e''') used to form the adhesive layer (E) may contain various metal ions and a solvent.
[0172] As the composition (e'''), a composition of an alloy consisting of multiple metals is also suitable for adhesion to organic and inorganic materials. Examples include copper, nickel, chromium, cobalt, tin, silver, bismuth, zinc, aluminum, titanium, iron, manganese, indium, molybdenum, gold, palladium, platinum, zirconium, tungsten, and ruthenium. These metals can be used alone or in combination of two or more. For example, a flat bond treatment manufactured by MEC Co., Ltd. can be used.
[0173] The method for forming the adhesive layer (E) made of the composition (e''') includes, for example, a method containing a sulfide of a metal such as copper, nickel, chromium, cobalt, or tin, sulfuric acid, and an aqueous medium. Specifically, an aqueous solution containing an inorganic acid such as sulfuric acid or an organic acid such as acetic acid, a stannous salt such as stannous sulfate, a metal salt such as silver acetate, a reaction accelerator such as thiourea, and a diffusion-type retention solvent such as diethylene glycol is used. By contacting this mixed aqueous solution with the patterned metal plating layer (D), the metal of the metal plating layer (D) is replaced by the metal of the composition (e'''), thereby forming the adhesive layer (E) (substitution plating method). Therefore, when the composition (e''') is used, the adhesive layer (E) can be formed only on the surface of the patterned metal plating layer (D) and the patterned plating base layer (C).
[0174] The surface treatment temperature during the surface treatment using the treatment liquid for forming the adhesive layer (E) made of the composition (e''') is preferably in the range of 10°C to 70°C, more preferably in the range of 20°C to 60°C, and even more preferably in the range of 30°C to 50°C.
[0175] The adhesive layer (E) made of the compositions (e), (e'), (e'') and (e''') may be one layer or two or more layers. For example, by forming an adhesive layer (E) made of the composition (e''') and then further forming an adhesive layer (E) made of the composition (e), the metal plating layer (D) and the interlayer resin layer (F) described below can be more firmly adhered to each other. It is also preferable to use an organosilane compound of the composition (e).
[0176] Next, a method for laminating the laminate having the adhesive layer (E) formed thereon and the interlayer resin layer (F) will be described.
[0177] The interlayer resin layer (F) can be suitably adhered to the adhesive layer (E) on the wiring surface and the primer layer (B) on the substrate surface when the laminate having the adhesive layer (E) laminated thereon is formed into a multilayer structure.
[0178] As the composition used for forming the interlayer resin layer (F), a resin having excellent insulating properties can be used. For example, a composite substrate of glass fiber and epoxy resin (glass epoxy resin, FR-4, FR-5), a composite substrate of paper and epoxy resin (FR-3), a composite substrate of glass nonwoven fabric and epoxy resin (CEM-3), a composite substrate of paper, glass nonwoven fabric and epoxy resin (CEM-1), a composite substrate of paper and phenolic resin (paper phenolic resin, FR-1, FR-2), a composite substrate of glass fiber and PPE resin (e.g., Megtron 6, Megtron 7, Megtron 8 manufactured by Panasonic), a composite substrate of glass fiber and maleimide resin, a bismaleimide triazine resin (BT resin), a composite substrate of ceramic and fluororesin (e.g., RO3003 manufactured by Rogers), a composite substrate of silica and epoxy resin (e.g., Buildup Fill manufactured by Ajinomoto Co., Inc.), Examples of such materials include polyimide resin, liquid crystal polymer, polyether ether ketone, polyphenylene sulfide, polystyrene, polycarbonate, polyester resin, polypropylene, polyethylene, acrylic resin, urethane resin, cycloolefin resin, modified polyimide resin (MPI), polytetrafluoroethylene resin, liquid crystal polymer (LCP), polyphenylene sulfide (PPS), fluororesin composite polyimide resin (film with a fluororesin layer formed on the surface of a polyimide resin, multilayer film with polyimide resin and fluororesin alternately laminated), thermoplastic polyimide resin composite polyimide resin (film with a thermoplastic polyimide resin layer formed on the surface of a polyimide resin).
[0179] Examples of the interlaminar resin layer (F) include synthetic fibers such as polyester fibers, polyamide fibers, and polyaramid fibers, inorganic fibers such as carbon fibers, and natural fibers such as cellulose nanofibers.
[0180] The interlaminar resin layer (F) may be a prepreg, an electroless plating adhesive, a film-like resin, a liquid resin, a photosensitive resin, a thermosetting resin, or a thermoplastic resin. The adhesive layer (E) also improves adhesion to solder resist, etching resist, conductive resin, conductive paste, conductive adhesive, resin for dielectrics, resin for filling holes, flexible coverlay film, etc.
[0181] As a method for forming the interlaminar resin layer (F) on the laminate formed by the adhesive layer (E), when the support (A) is a flexible material and a roll film, it is preferable to use a hot roll lamination method, a solventless lamination method, an extrusion lamination method, or a wet lamination method. In particular, the hot roll lamination method is more preferable because it can be easily processed. On the other hand, when the support (A) is a rigid material, it is often thermocompressed in a sheet, so it is preferable to use a press method, a vacuum press method, or a vacuum heat lamination method.
[0182] Regarding the thermocompression bonding conditions, the heating conditions are preferably in the range of 50° C. to 400° C., more preferably in the range of 80° C. to 350° C., more preferably in the range of 80° C. to 280° C., more preferably in the range of 100° C. to 200° C., and more preferably in the range of 120 to 180° C. The pressure conditions are preferably in the range of 0.05 MPa to 35 MPa, and more preferably in the range of 0.3 MPa to 20 MPa.
[0183] In the case of hot roll lamination, the processing time for thermocompression bonding is within 1 second because the thermocompression bonding is performed by the linear pressure of the roll while the film is being transported. On the other hand, in the case of pressing, vacuum pressing, and vacuum hot lamination which process the film sheet by sheet, the processing time is preferably in the range of 1 second to 120 minutes, more preferably in the range of 30 seconds to 60 minutes, and more preferably in the range of 30 seconds to 15 minutes, and from the viewpoint of productivity, the processing time is preferably in the range of 1 minute to 5 minutes.
[0184] In addition, when performing thermocompression bonding, air may get between the laminate having the adhesive layer (E) and the interlayer resin layer (F), or the gas generated from the laminate having the adhesive layer (E) or the interlayer resin layer (F) may accumulate between the laminate having the adhesive layer (E) and the interlayer resin layer (F), resulting in a decrease in the transfer rate. Therefore, it is preferable to perform thermocompression bonding under vacuum using a vacuum press. As for the vacuum conditions, absolute pressure is preferably 100 hPa or less, more preferably 50 hPa or less, and more preferably 13 hPa or less. It is preferable to perform the heating conditions and pressure conditions under the same conditions as those described above.
[0185] In addition, when bonding the laminate having the adhesive layer (E) and the interlayer resin layer (F), a multilayer wiring board can be formed by laminating a conductive layer or a wiring board on the interlayer resin layer to form a multilayer wiring board.
[0186] By laminating copper foil when forming the interlayer resin layer (F), a multilayer structure of the laminate can be formed. Therefore, a multilayer wiring board can be formed by sequentially bonding the laminate on which the adhesive layer (E) is formed, the interlayer resin layer (F), and the copper foil.
[0187] By stacking wiring boards when forming the interlayer resin layer (F), a multilayer structure of a laminate can be formed. Therefore, a multilayer wiring board can be formed by sequentially bonding together a laminate having an adhesive layer (E), the interlayer resin layer (F), and a wiring board.
[0188] After forming the interlayer resin layer (F), a conductive treatment is performed by sputtering or electroless plating to connect the multilayer wiring, thereby forming a multilayer wiring board with a conductive layer.
[0189] In the multilayer wiring board having the conductive layer formed thereon, the metal layer and the conductive layer can be electrically connected by forming a through hole in the interlayer resin layer and then performing the conductive treatment prior to the conductive treatment.
[0190] In contrast to the multilayer wiring board formed by the conventional roughening treatment, the present invention forms a thin adhesive layer on the surface of a smooth substrate and smooth copper wiring, thereby achieving high adhesion with the interlayer resin of the multilayer wiring board, and can provide a metal circuit board with excellent transmission characteristics and high reliability. Therefore, the laminate of the present invention can be suitably used as electronic components such as printed wiring boards, rigid printed wiring boards, flexible printed wiring boards, package substrates, metal substrates, metal meshes for touch panels, organic solar cells, organic EL elements, LED electrode wiring substrates, organic transistors, RFID such as non-contact IC cards, electromagnetic wave shields, LED lighting substrates, digital signage, photoelectric convergence devices, and interposers. EXAMPLES
[0191] The present invention will be described in more detail below with reference to examples and comparative examples. In the following examples and comparative examples, "parts" and "%" are all based on mass.
[0192] [Preparation Example 1: Preparation of Coating Liquid (1) for Forming Primer Layer (B)] 60 parts by mass of phenoxy resin 4250 (Mitsubishi Chemical Corporation bisphenol A / bisphenol F mixed type, molecular weight 60,000, solid content 100 mass%), 33 parts by mass of aminotriazine novolak resin (DIC Corporation "Phenolite LA-7052", solid content 60 mass%), 17 parts by mass of epoxy resin (DIC Corporation "EPICLON EXA-830CRP"; bisphenol F type epoxy resin, epoxy group equivalent 162 g / equivalent), 3 parts by mass of trimellitic anhydride, and 0.5 parts by mass of "TBZ" manufactured by Shikoku Kasei Co., Ltd. as a curing catalyst were mixed, diluted with cyclohexanone so that the non-volatile content was 2 mass%, and mixed uniformly to obtain a coating liquid (1) for forming a primer layer (B).
[0193] [Preparation Example 2: Preparation of coating solution (1) for forming plating underlayer (C)] Under a nitrogen atmosphere, a solution of p-toluenesulfonic acid chloride in chloroform (30 ml) containing 9.6 parts by mass was added dropwise to a mixture containing 20 parts by mass of methoxypolyethylene glycol (number average molecular weight 2,000), 8.0 parts by mass of pyridine, and 20 ml of chloroform while stirring on ice for 30 minutes, and the mixture was then stirred for 4 hours at a bath temperature of 40°C and mixed with 50 ml of chloroform. The obtained product was then washed with 100 ml of a 5 mass% aqueous hydrochloric acid solution, then washed with 100 ml of a saturated aqueous sodium hydrogencarbonate solution, and then washed with 100 ml of a saturated saline solution, and then dried over anhydrous magnesium sulfate, filtered, concentrated under reduced pressure, washed several times with hexane, filtered, and dried under reduced pressure at 80°C to obtain a methoxypolyethylene glycol having a p-toluenesulfonyloxy group. 5.39 parts by mass of methoxypolyethylene glycol having a p-toluenesulfonyloxy group, 20 parts by mass of polyethyleneimine (manufactured by Aldrich, molecular weight 25,000), 0.07 parts by mass of potassium carbonate, and 100 ml of N,N-dimethylacetamide were mixed and stirred at 100° C. for 6 hours under a nitrogen atmosphere. Next, 300 ml of a mixed solution of ethyl acetate and hexane (volume ratio of ethyl acetate / hexane = 1 / 2) was added, and the mixture was stirred vigorously at room temperature, after which the product solid was filtered. The solid was washed with 100 ml of a mixed solution of ethyl acetate and hexane (volume ratio of ethyl acetate / hexane = 1 / 2), and then dried under reduced pressure to obtain a compound in which polyethylene glycol was bound to polyethyleneimine. 138.8 parts by mass of an aqueous solution containing 0.592 parts by mass of the compound in which polyethylene glycol is bound to polyethyleneimine obtained was mixed with 10 parts by mass of silver oxide, and the mixture was stirred for 30 minutes at 25° C. Then, 46 parts by mass of dimethylethanolamine was gradually added with stirring, and the mixture was stirred for 30 minutes at 25° C. Next, 15.2 parts by mass of a 10% by mass aqueous ascorbic acid solution was gradually added with stirring, and stirring was continued for 20 hours to obtain a silver dispersion. A mixed solvent of 200 ml of isopropyl alcohol and 200 ml of hexane was added to the obtained silver dispersion and stirred for 2 minutes, and then centrifugal concentration was performed at 3,000 rpm for 5 minutes. After removing the supernatant, a mixed solvent of 50 ml of isopropyl alcohol and 50 ml of hexane was added to the precipitate and stirred for 2 minutes, and then centrifugal concentration was performed at 2,000 rpm for 10 minutes. After removing the supernatant, 20 parts by mass of water was further added to the precipitate and stirred for 2 minutes to remove the organic solvent under reduced pressure. After adding 10 parts by mass of water and stirring and dispersing, the dispersion was left in a freezer at -40 ° C for 1 day and night to freeze, and this was treated with a freeze dryer (FDU-2200 manufactured by Tokyo Rikakikai Co., Ltd.) for 24 hours to obtain silver particles containing a dispersant having a basic nitrogen atom-containing group consisting of flake-shaped lumps with a gray-green metallic luster. The obtained powder of silver particles containing a dispersant having a basic nitrogen atom-containing group was dispersed in a mixed solvent of 45 parts by mass of ethanol and 55 parts by mass of ion-exchanged water to prepare a 5% by mass coating solution (1) for forming a plating underlayer (C). The proportion of the dispersant was calculated from the ash content after heating the obtained silver particles in an electric furnace at 500°C for 1 hour, and it was confirmed that the proportion was 5% by mass relative to 100% by mass of silver solids.
[0194] <Preparation Example 3: Preparation of Transfer Laminate (1)> The coating liquid (1) for forming the plating underlayer (C) obtained in Preparation Example 2 was applied to the surface of a release film ("TN-200" manufactured by Toyobo Co., Ltd., a release PET film; thickness 38 μm) on which the release layer was formed, using a small desktop coater ("K Printing Profer" manufactured by RK Print Coat Instruments Co., Ltd.), and dried at 150°C for 5 minutes to coat a silver layer corresponding to the plating underlayer (C) to a thickness of 0.1 μm after drying. Thereafter, the coating liquid (1) for forming the primer layer (B) obtained in Preparation Example 1 was applied using a small desktop coater (RK Printing Profer, manufactured by RK Print Coat Instruments Co., Ltd.) and dried at 180°C for 3 minutes, thereby coating a layer corresponding to the primer layer (B) to a dry thickness of 0.3 μm, thereby forming a plating base layer (C) and a primer layer (B) on the surface of the release film corresponding to the temporary support (G), and obtaining a transfer laminate (1).
[0195] (Preparation Example 4: Preparation of Laminate (1) of Single-Layer Circuit Board) The glossy side (non-roughened side) of copper foil (F2-WS manufactured by Furukawa Electric Co., Ltd., thickness 18 μm) was attached to both sides of a prepreg (R5670 manufactured by Panasonic Corporation, containing glass fiber, thickness 0.1 mm, surface roughness Sz: 20.815 μm), and heat-pressed at 195 ° C for 90 minutes using a hand press ("Mini Test Press" manufactured by Toyo Seiki Seisakusho Co., Ltd.). Then, the substrate was immersed in a ferric chloride etching solution (content 40 mass%) at 40 ° C for 3 minutes to etch the entire surface of the copper foil, thereby obtaining a rigid substrate in which the prepreg corresponding to the support (D) was hardened. It was confirmed that the surface roughness of the rigid substrate was Sz 4.215 μm and smoothed. Then, a corona treatment ("Corona Surface Modification Evaluation Device TEC-4AX" manufactured by Kasuga Electric Co., Ltd., electrode-substrate distance 0.5 mm, 100 W) was performed on both sides of the rigid substrate. Thereafter, the surface of the transfer laminate (1) obtained in Preparation Example 3 on which the primer layer (B) was formed was attached to both sides of the rigid substrate, and a hand press ("Mini Test Press" manufactured by Toyo Seiki Seisakusho Co., Ltd.) was used to perform thermocompression bonding for 10 minutes with the upper hot plate of the press made of SUS and the lower hot plate made of SUS, the upper hot plate temperature was set to 150°C, the lower hot plate temperature was set to 150°C, and the pressure was 5 MPa. Next, the release film of the transfer laminate (1) thermocompression bonded to both sides of the rigid substrate was peeled off, thereby forming the primer layer (B) and the plating undercoat layer (C) on both sides of the rigid substrate with the prepreg cured.
[0196] Thereafter, a conductive pattern was formed by a semi-additive method. The pattern was shaped as required for the evaluation described below. A plating resist ("RY-5125" manufactured by Showa Denko Materials Co., Ltd., thickness 25 μm) was attached to the surface of the plating underlayer (C) at 110° C., 0.4 MPa, and 1 m / min, and an exposure process was performed for 2 minutes (316 mJ / cm2) using an exposure machine ("BOX-W10" manufactured by Sanhayato Co., Ltd.), and then the plating resist was formed by immersing the plating resist in a developer (1 mass% aqueous sodium carbonate solution) for 5 minutes and developing the plating resist. Thereafter, a metal plating layer (D) having a thickness of 18 μm was formed by electrolytic copper plating on the part of the plating underlayer (C) after the plating resist was removed by development. The plating resist was then peeled off by immersing the plating resist in 3 mass% sodium hydroxide for 3 minutes. Next, the plating underlayer (C) was dissolved using an etching solution (SVE-A810 manufactured by ADEKA CORPORATION) to obtain a laminate (1) of single-layer circuit boards on which a circuit pattern was formed.
[0197] (Preparation Example 5: Preparation of Laminate (2) of Single-Layer Circuit Board) A roughened surface of copper foil (F2-WS manufactured by Furukawa Electric Co., Ltd., thickness 18 μm) was bonded to both sides of a prepreg (R5670 manufactured by Panasonic Corporation, containing glass fiber, thickness 0.1 mm, surface roughness Sz: 20.815 μm), and the resulting material was thermocompressed at 195°C for 90 minutes using a hand press ("Mini Test Press" manufactured by Toyo Seiki Seisakusho Co., Ltd.).
[0198] Thereafter, a conductive pattern was formed by a subtractive method. The pattern was shaped as required for the evaluation described below. An etching resist ("RY-5125" manufactured by Showa Denko Materials Co., Ltd., thickness 25 μm) was attached to the surface of the metal layer (D) at 110° C., 0.4 MPa, and 1 m / min, and an exposure process was performed for 2 minutes (316 mJ / cm2) using an exposure machine ("BOX-W10" manufactured by Sanhayato Co., Ltd.), and then the substrate was immersed in a developer (1 mass% sodium carbonate aqueous solution) for 5 minutes and developed to form a pattern resist. Next, the metal layer (D) was dissolved using a cupric chloride solution, and then the substrate was immersed in 3 mass% sodium hydroxide for 3 minutes to peel off the plating resist, thereby obtaining a laminate (2) of a single-layer circuit board having a circuit pattern formed thereon.
[0199] (Preparation Example 6: Preparation of Laminate (3) of Single-Layer Circuit Board) The glossy side (non-roughened side) of copper foil (F2-WS manufactured by Furukawa Electric Co., Ltd., thickness 18 μm) was attached to both sides of a prepreg (R5670 manufactured by Panasonic Corporation, containing glass fiber, thickness 0.1 mm, surface roughness Sz: 20.815 μm), and heat-pressed at 195 ° C for 90 minutes using a hand press ("Mini Test Press" manufactured by Toyo Seiki Seisakusho Co., Ltd.). Then, the substrate was immersed in a ferric chloride etching solution (content 40 mass%) at 40 ° C for 3 minutes to etch the entire surface of the copper foil, thereby obtaining a rigid substrate in which the prepreg corresponding to the support (D) was hardened. It was confirmed that the surface roughness of the rigid substrate was Sz 4.215 μm and smoothed. Then, a corona treatment ("Corona Surface Modification Evaluation Device TEC-4AX" manufactured by Kasuga Electric Co., Ltd., electrode-substrate distance 0.5 mm, 100 W) was performed on both sides of the rigid substrate. Thereafter, the coating solution (1) for forming the plating underlayer (C) of Preparation Example 2 was applied using a small desktop spin coater (Opticoat MS-A150 manufactured by Mikasa Co., Ltd.) and dried at 120°C for 5 minutes, thereby coating a silver layer corresponding to the plating underlayer (C) to a dry thickness of 0.1 μm.
[0200] Thereafter, a conductive pattern was formed by a semi-additive method. The pattern was shaped as required for the evaluation described below. A plating resist ("RY-5125" manufactured by Showa Denko Materials Co., Ltd., thickness 25 μm) was attached to the surface of the plating underlayer (C) at 110° C., 0.4 MPa, and 1 m / min, and an exposure process was performed for 2 minutes (316 mJ / cm2) using an exposure machine ("BOX-W10" manufactured by Sanhayato Co., Ltd.), and then the plating resist was formed by immersing the plating resist in a developer (1 mass% aqueous sodium carbonate solution) for 5 minutes and developing the plating resist. Thereafter, a metal plating layer (D) having a thickness of 18 μm was formed by electrolytic copper plating on the part of the plating underlayer (C) after the plating resist was removed by development. The plating resist was then peeled off by immersing the plating resist in 3 mass% sodium hydroxide for 3 minutes. Next, the plating underlayer (C) was dissolved using an etching solution (SVE-A810 manufactured by ADEKA CORPORATION) to obtain a laminate (3) of single-layer circuit boards on which a circuit pattern was formed.
[0201] Example 1 The laminate (1) for the single-layer circuit board was sprayed with 5% by mass of hydrochloric acid at room temperature for 60 seconds to clean it, and then washed with water and dried. Thereafter, the laminate was immersed in an aqueous solution consisting of 1% by mass of 3-[3-(trimethoxysilyl)propylthio]-1,2,4-triazole, 20% by mass of ethylene glycol monobutyl ether, and the remainder being ion-exchanged water at room temperature for 1 minute, washed with water, and dried to obtain a laminate (1) for a multilayer circuit board in which an adhesive layer (E) having a thickness of 100 nm was formed only on the wiring surface of the laminate (1).
[0202] Example 2 The laminate (1) for the single-layer circuit board was washed by spraying 5% by mass of hydrochloric acid at room temperature for 60 seconds, then washed with water and dried. Then, the laminate (2) for multilayer circuit board was obtained by immersing the coating liquid (1) for forming the primer layer (B) in Preparation Example 1 at room temperature for 1 minute, washing and drying, and forming an adhesive layer (E) having a thickness of 100 nm only on the wiring surface of the laminate (1).
[0203] Example 3 The laminate (1) for the single-layer circuit board was cleaned by spraying 5% by mass of hydrochloric acid at room temperature for 60 seconds, followed by rinsing with water and drying. Thereafter, the laminate was immersed at room temperature for 1 minute in an aqueous solution consisting of 0.2% by mass of 6-(3-(triethoxysilyl)propylamino)-1,3,5-triazine-2,4-dithiol monosodium, 5% by mass of ethanol, and the remainder being ion-exchanged water, followed by rinsing with water and drying to obtain a laminate (3) for a multilayer circuit board in which an adhesive layer (E) having a thickness of 100 nm was formed only on the wiring surface of the laminate (1).
[0204] Example 4 The laminate (1) for the single-layer circuit board was sprayed with 5% by mass of hydrochloric acid at room temperature for 60 seconds to clean it, and then washed with water and dried. Thereafter, it was immersed in an aqueous solution consisting of 20% by mass of acetic acid, 2% by mass of stannous acetate, 3% by mass of silver acetate, 15% by mass of thiourea, 30% by mass of diethylene glycol, and the remainder being ion-exchanged water at 30°C for 30 seconds, and then washed with water and dried to obtain a laminate (4) for a multilayer circuit board in which an adhesive layer (E) having a thickness of 100 nm was formed only on the wiring surface of the laminate (1).
[0205] Example 5 A laminate (5) for a multilayer circuit board was obtained in the same manner as in Example 1, except that the adhesive layer (E) was formed on the wiring surface and the substrate surface by immersing in the adjusted liquid and then drying.
[0206] Example 6 A laminate (6) for a multilayer circuit board was obtained in the same manner as in Example 5, except that an adhesive layer (E) having a thickness of 25 μm was used.
[0207] Comparative Example 1 Both sides of the single-layer circuit board laminate (1) were cleaned by spraying 5% by mass hydrochloric acid at room temperature for 60 seconds, followed by rinsing with water and drying to obtain a multilayer circuit board laminate (R1).
[0208] Comparative Example 2 Both sides of the laminate (1) for the single-layer circuit board were cleaned by spraying 5% by mass of hydrochloric acid at room temperature for 60 seconds, then washed with water and dried. Then, a roughening treatment was performed by microetching using hydrogen peroxide and sulfuric acid to obtain a laminate (R2) for a multilayer circuit board in which only the wiring was roughened.
[0209] Comparative Example 3 Both sides of the single-layer circuit board laminate (2) were cleaned by spraying 5% by mass hydrochloric acid at room temperature for 60 seconds, followed by rinsing with water and drying to obtain a multilayer circuit board laminate (R3).
[0210] Comparative Example 4 The laminate (2) for a single-layer circuit board was cleaned by spraying 5% by mass of hydrochloric acid at room temperature for 60 seconds, then washed with water and dried. Then, a roughening treatment was performed by microetching using hydrogen peroxide and sulfuric acid to obtain a laminate (R4) for a multilayer circuit board in which only the wiring was roughened.
[0211] Comparative Example 5 The single-layer circuit board laminate (2) was sprayed with 5% by mass hydrochloric acid at room temperature for 60 seconds to clean it, then washed with water and dried. Thereafter, it was immersed at room temperature for 1 minute in an aqueous solution consisting of 1% by mass of 3-[3-(trimethoxysilyl)propylthio]-1,2,4-triazole, 20% by mass of ethylene glycol monobutyl ether, and the remainder being ion-exchanged water, and washed with water and dried to obtain a multilayer circuit board laminate (R5) in which an adhesive layer (E) having a thickness of 100 nm was formed only on the wiring surface of the single-layer circuit board laminate (2).
[0212] Comparative Example 6 The single-layer circuit board laminate (3) was sprayed with 5% by mass hydrochloric acid at room temperature for 60 seconds to clean it, then washed with water and dried. Thereafter, it was immersed at room temperature for 1 minute in an aqueous solution consisting of 1% by mass of 3-[3-(trimethoxysilyl)propylthio]-1,2,4-triazole, 20% by mass of ethylene glycol monobutyl ether, and the remainder being ion-exchanged water, and washed with water and dried to obtain a multilayer circuit board laminate (R6) in which an adhesive layer (E) having a thickness of 100 nm was formed only on the wiring surface of the single-layer circuit board laminate (3).
[0213] <Substrate surface roughness: Evaluation by laser microscope> The surface roughness of the base material of the laminate for multilayer circuit board obtained above was measured by a laser microscope. The surface roughness Sz of the measurement area was 250×250 μm. From the surface roughness value of the substrate measured above, the adhesion was evaluated according to the following criteria. A: The surface roughness Sz value of the substrate is less than 3.0 μm. B: The surface roughness Sz value of the substrate is 3.0 μm or more and less than 4.0 μm. C: The surface roughness Sz value of the substrate is 4.0 μm or more and less than 6.0 μm. D: The surface roughness Sz value of the substrate is 6.0 μm or more and less than 10.0 μm. E: The surface roughness Sz value of the substrate is 10.0 μm or more.
[0214] <Copper wiring surface roughness: Evaluation using a laser microscope> The surface roughness of the wiring of the laminate for multilayer circuit board obtained above was measured by a laser microscope. The surface roughness Sz of the measurement area was 250×250 μm. From the surface roughness value of the substrate measured above, the adhesion was evaluated according to the following criteria. A: The surface roughness Sz value of the substrate is less than 3.0 μm. B: The surface roughness Sz value of the substrate is 3.0 μm or more and less than 4.0 μm. C: The surface roughness Sz value of the substrate is 4.0 μm or more and less than 6.0 μm. D: The surface roughness Sz value of the substrate is 6.0 μm or more and less than 10.0 μm. E: The surface roughness Sz value of the substrate is 10.0 μm or more.
[0215] <Normal adhesion strength: Evaluation by peel test of the interface between the substrate and prepreg> The roughened surfaces of prepreg (R5670 manufactured by Panasonic Corporation, containing glass fiber, thickness 0.1 mm, surface roughness Sz: 20.815 μm) and copper foil (F2-WS manufactured by Furukawa Electric Co., Ltd., thickness 18 μm) were attached to both sides of the laminate for multilayer circuit board obtained above, and thermocompression bonding was performed at 195 ° C for 90 minutes using a hand press ("Mini Test Press" manufactured by Toyo Seiki Seisakusho Co., Ltd.). Thereafter, the peel strength of the interface between the substrate and the prepreg was measured. The peel strength measurement was performed according to a method conforming to IPC-TM-650, NUMBER2.4.9. The lead width used for the measurement was 5 mm, and the peel angle was 90 °. From the peel strength value before heating measured above, the adhesion was evaluated according to the following criteria. A: The peel strength value is 700N / m or more. B: The peel strength value is 600N / m or more and less than 700N / m. C: The peel strength value is 500N / m or more and less than 600N / m. D: The peel strength value is 400 N / m or more and less than 500 N / m. E: The peel strength value is less than 400 N / m.
[0216] <Normal adhesion strength: Evaluation by peel test of copper wiring and prepreg interface> The roughened surfaces of prepreg (R5670 manufactured by Panasonic Corporation, containing glass fiber, thickness 0.1 mm, surface roughness Sz: 20.815 μm) and copper foil (F2-WS manufactured by Furukawa Electric Co., Ltd., thickness 18 μm) were attached to both sides of the laminate for multilayer circuit board obtained above, and thermocompression bonding was performed at 195°C for 90 minutes using a hand press ("Mini Test Press" manufactured by Toyo Seiki Seisakusho Co., Ltd.). Thereafter, the peel strength of the wiring and prepreg interface was measured. The peel strength measurement was performed according to a method conforming to IPC-TM-650, NUMBER2.4.9. The lead width used for the measurement was 5 mm, and the peel angle was 90°. From the peel strength value before heating measured above, the adhesion was evaluated according to the following criteria. A: The peel strength value is 700N / m or more. B: The peel strength value is 600N / m or more and less than 700N / m. C: The peel strength value is 500N / m or more and less than 600N / m. D: The peel strength value is 400 N / m or more and less than 500 N / m. E: The peel strength value is less than 400 N / m.
[0217] <Heat resistance test: Evaluation of the number of blisters occurring at the interface between the substrate and prepreg> The roughened surfaces of prepreg (R5670 manufactured by Panasonic Corporation, containing glass fiber, thickness 0.1 mm, surface roughness Sz: 20.815 μm) and copper foil (F2-WS manufactured by Furukawa Electric Co., Ltd., thickness 18 μm) were attached to both sides of the laminate for multilayer circuit board obtained above, and the laminate was thermocompressed at 195 ° C for 90 minutes using a hand press ("Mini Test Press" manufactured by Toyo Seiki Seisakusho Co., Ltd.). After that, the laminate was placed in a thermostatic chamber at 260 ° C for 5 minutes and then removed 10 times, and the number of blisters generated in the laminate was evaluated. The occurrence of blisters was judged visually, and the number of blisters was counted. A 100 mm × 100 mm piece was cut out from the area where the substrate and prepreg formed an interface, and the evaluation was performed. A: The number of blisters is 0. B: The number of blisters is 0 or more and less than 5. C: The number of blisters is 5 or more and less than 10. D: The number of blisters is 10 or more and less than 20. E: The number of blisters is 20 or more.
[0218] <Heat resistance test: Evaluation of the number of blisters occurring at the interface between the copper film and the prepreg> The roughened surfaces of prepreg (R5670 manufactured by Panasonic Corporation, containing glass fiber, thickness 0.1 mm, surface roughness Sz: 20.815 μm) and copper foil (F2-WS manufactured by Furukawa Electric Co., Ltd., thickness 18 μm) were attached to both sides of the laminate for multilayer circuit board obtained above, and the laminate was thermocompressed at 195 ° C for 90 minutes using a hand press ("Mini Test Press" manufactured by Toyo Seiki Seisakusho Co., Ltd.). After that, the laminate was placed in a thermostatic chamber at 260 ° C for 5 minutes and then removed, and the number of blisters generated in the laminate was evaluated. The occurrence of blisters was judged visually, and the number of blisters was counted. A 100 mm × 100 mm piece was cut out from the area where the copper film and the prepreg formed an interface, and the evaluation was performed. A: The number of blisters is 0. B: The number of blisters is 0 or more and less than 5. C: The number of blisters is 5 or more and less than 10. D: The number of blisters is 10 or more and less than 20. E: The number of blisters is 20 or more.
[0219] <Transmission characteristic evaluation; Transmission characteristic evaluation of stripline structure> A roughened surface of a prepreg (R5670 manufactured by Panasonic Corporation, containing glass fiber, thickness 0.1 mm, surface roughness Sz: 20.815 μm) and a copper foil (F2-WS manufactured by Furukawa Electric Co., Ltd., thickness 18 μm) were attached to one side of the laminate for multilayer circuit board obtained above, and thermocompression bonding was performed for 90 minutes at 195 ° C. using a hand press ("Mini Test Press" manufactured by Toyo Seiki Seisakusho Co., Ltd.). After that, in order to obtain electrical continuity between the copper foil of the outermost layer and the inner layer circuit, a through hole was formed with a CO2 laser, and a desmear process was performed by permanganate treatment. After that, a Sn / Pd catalyst was used to support the catalyst, and electroless copper plating was performed, and the inner layer circuit and copper foil were connected by panel plating, and then the outermost layer was patterned by a subtractive method to prepare a coupon for evaluating the transmission characteristics of a stripline structure. The structure of the stripline for evaluating the transmission characteristics was designed to have an inner layer wiring width of 100 μm, a thickness of 35 μm, and an impedance of 50 Ω, and the transmission characteristics were evaluated by the transmission loss value at 60 GHz. The transmission characteristics were evaluated according to the following criteria based on the values measured above. A: The transmission loss value is -11 dB or more. B: The transmission loss value is less than -11 dB and greater than or equal to -12 dB. C: The transmission loss value is less than -12 dB and greater than or equal to -13 dB. D: The transmission loss value is less than -13 dB and greater than or equal to -14 dB. E: The transmission loss value is less than -14 dB.
[0220] In Examples 1 to 6, various adhesive layers (E) were formed using a single-layer circuit board laminate (1), and good results were obtained.
[0221] On the other hand, Comparative Example 1 is an example in which a laminate (1) of a single-layer circuit board is used and no adhesive layer (E) is formed, and the adhesion between the copper wiring and the prepreg is low, and many blisters are observed at the interface between the copper wiring and the prepreg. In Comparative Example 2, the surface of the copper wiring is roughened, so the surface roughness of the copper wiring is large, and the transmission loss in the transmission characteristic evaluation is large. In Comparative Examples 3 to 5, the copper wiring is made of a roughened copper foil, so the transmission loss in the transmission characteristic is large. In Comparative Example 6, a laminate (3) of a single-layer circuit board is used and a primer layer (B) is not provided. Since the primer layer (B) is not provided, the adhesion at the interface between the smooth base material and the prepreg is low. In addition, the adhesion at the interface between the copper film and the prepreg is also low, and as a result of detailed examination of the peeled portion of the sample after evaluation, it was broken at the interface between the base material and the plating underlayer (C). In addition, after the heat resistance test, many blisters occurred at both the interface between the base material and the prepreg and the interface between the copper film and the prepreg.
[0222] [Table 1]
[0223] [Table 2] [Explanation of symbols]
[0224] 1: Metal plating layer 2: Plating base layer 3: Primer layer 4:Support 5: Adhesive layer 6: Interlayer resin layer 7: Metal layer
Claims
1. A laminate comprising a primer layer (B), a patterned plating underlayer (C), and a metal plating layer (D) laminated in this order on at least one surface of a support (A), and an adhesive layer (E) having a thickness of 0.001 to 1 μm laminated only on the surfaces of the plating underlayer (C) and the metal plating layer (D).
2. A laminate comprising a primer layer (B), a patterned plating underlayer (C), and a metal plating layer (D) laminated in this order on at least one surface of a support (A), and further an adhesive layer (E) having a thickness of 0.001 to 1 μm laminated on the surfaces of the primer layer (B), the patterned plating underlayer (C), and the metal plating layer (D).
3. 3. The laminate according to claim 1, further comprising an interlayer resin layer (F) on the primer layer (B) and / or the adhesive layer (E) or on the adhesive layer (E).
4. 3. The laminate according to claim 1, wherein the surface roughness (maximum height Sz) of the support (A) as measured by a laser microscope is 0.001 to 50 μm.
5. 3. The laminate according to claim 1, wherein the surface roughness (maximum height Sz) of the primer layer (B) measured by a laser microscope is 0.001 to 30 μm.
6. 3. The laminate according to claim 1, wherein the surface roughness (maximum height Sz) of the plating underlayer (C) measured with a laser microscope is 0.001 to 30 μm.
7. 3. The laminate according to claim 1, wherein the surface roughness (maximum height Sz) of the metal plating layer (D) measured with a laser microscope is 0.001 to 20 μm.
8. 3. The laminate according to claim 1, wherein the surface roughness (maximum height Sz) of the adhesive layer (E) measured with a laser microscope is 0.001 to 20 μm.
9. 3. The laminate according to claim 1 or 2, wherein the primer layer (B) is selected from the group consisting of urethane resin, acrylic resin, core-shell type composite resin having a urethane resin as a shell and an acrylic resin as a core, epoxy resin, phenoxy resin, imide resin, amide resin, melamine resin, phenol resin, urea-formaldehyde resin, blocked isocyanate obtained by reacting a blocking agent such as phenol with a polyisocyanate, polyvinyl alcohol, and polyvinylpyrrolidone.
10. 3. The laminate according to claim 1, wherein the primer layer (B) is one or more layers.
11. 3. The laminate according to claim 1, wherein the patterned plating underlayer (C) is one or more layers.
12. The adhesive layer (E) is at least a mercaptosilane compound, a vinylsilane compound, a vinylphenylsilane compound, an epoxysilane compound, an acryloxysilane compound, a methacryloxysilane compound, an aminosilane compound, a ureidosilane compound, a chloropropylsilane compound, a sulfide silane compound, an isocyanate silane compound, a triazole silane compound, a thiadiazole silane compound, an isocyanatopropylsilane compound, a styryl silane compound, a carboxysilane compound, an alkoxysilane compound, a triazine silane compound, an imidazole silane compound, an azole silane compound, a pyrrole silane compound, a pyrazole silane compound, a tetrazole silane compound, an indole silane compound, an isoindole silane compound, an indazole ...
3. The laminate according to claim 1 or 2, characterized in that the compound is selected from one or more of the following: arylene compounds, benzimidazole silane compounds, benzotriazole silane compounds, triazine thiol compounds, triazine azide compounds, triazine amino compounds, triazine isoyanate compounds, triazine urethane compounds, triazine ester compounds, triazine silane compounds, urethane resins, acrylic resins, core-shell type composite resins having a urethane resin as the shell and an acrylic resin as the core, epoxy resins, phenoxy resins, imide resins, amide resins, melamine resins, phenolic resins, urea formaldehyde resins, blocked isocyanate polyvinyl alcohol obtained by reacting a blocking agent such as phenol with a polyisocyanate, and polyvinylpyrrolidone.
13. 3. The laminate according to claim 1 or 2, characterized in that the adhesive layer (E) is selected from one or more of copper, tin, silver, bismuth, nickel, palladium, platinum, cobalt, titanium, molybdenum, chromium, manganese, ruthenium, indium, zinc, tungsten, aluminum, and zirconium.
14. Step 1 of forming the primer layer (B) on at least one surface of the support (A); Step 2 of forming the plating underlayer (C) on the surface of the primer layer (B); Step 3: forming a metal plating layer (D) on the surface of the plating underlayer (C); Step 4: forming an adhesive layer (E) on the surface of the metal plating layer (D) The method for producing a laminate according to claim 1 or 2, further comprising the steps of:
15. Step 1 of producing a transfer laminate in which a plating underlayer (C) and a primer layer (B) are successively formed on a temporary support (G); A step 2 of laminating the surface of the transfer laminate on which the primer layer (B) is formed to at least one surface of the support (A); A step 3 of peeling off the temporary support (G) of the transfer laminate laminate bonded to the support (A) and forming the primer layer (B) and the plating underlayer (C) on at least one surface of the support (A); Step 4 of forming a metal plating layer (D) on the surface of the plating underlayer (C); Step 5: forming an adhesive layer (E) on the surface of the metal plating layer (D). The method for producing a laminate according to claim 1 or 2, further comprising the steps of:
16. Step 1 of forming the primer layer (B) on at least one surface of the support (A); Step 2 of forming the plating underlayer (C) on the surface of the primer layer (B); Step 3: forming a metal plating layer (D) on the surface of the plating underlayer (C); Step 4 of forming an adhesive layer (E) on the surface of the metal plating layer (D); Step 5 further comprises forming an interlayer resin layer (F) on the primer layer (B) and the adhesive layer (E) or on the adhesive layer (E); The method for producing a laminate according to claim 3, further comprising the steps of:
17. Step 1 of producing a transfer laminate in which a plating underlayer (C) and a primer layer (B) are successively formed on a temporary support (G); A step 2 of laminating the surface of the transfer laminate on which the primer layer (B) is formed to at least one surface of the support (A); A step 3 of peeling off the temporary support (G) of the transfer laminate laminate bonded to the support (A) and forming the primer layer (B) and the plating underlayer (C) on at least one surface of the support (A); Step 4 of forming a metal plating layer (D) on the surface of the plating underlayer (C); Step 5 of forming an adhesive layer (E) on the surface of the metal plating layer (D); Step 6 further comprises forming an interlayer resin layer (F) on the primer layer (B) and the adhesive layer (E) or on the adhesive layer (E); The method for producing a laminate according to claim 3, further comprising the steps of:
18. A printed wiring board, a package substrate, an interposer, a wiring substrate for LED electrodes, or an optoelectronic device, comprising the laminate according to claim 1 or 2.
Citation Information
Patent Citations
To-resin adhesive layer on surface of copper, wiring board, and method for forming adhesive layer
JP2012094918A
Surface treatment liquid of metal, surface treatment method and its utilization
JP2015092020A
Laminated body and circuit wiring board
WO2009154083A1
Cited By
Unequal-length soft area rigid-flex board processing method
CN121174412A