Lamination type electron component and manufacturing method of lamination type electron component
The multilayer electronic component addresses moisture resistance reliability issues by optimizing the design and manufacturing process of side margin portions, ensuring uniformity and durability through specific distance ratios and controlled pressing and punching techniques.
Patent Information
- Application Number
- JP2024018591
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-21
- Filing Date
- 2024-02-09
- Publication Date
- 2024-10-31
Smart Images

Figure 2024155731000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a multilayer electronic component and a method for manufacturing a multilayer electronic component. [Background technology]
[0002] Multi-Layered Ceramic Capacitor (MLCC), a type of multi-layered electronic component, is a chip-type capacitor that is mounted on the printed circuit boards of various electronic products such as visual devices such as liquid crystal displays (LCDs) and plasma display panels (PDPs), computers, smartphones, and mobile phones to charge and discharge electricity.
[0003] In a conventional method for miniaturizing a multilayer ceramic capacitor while increasing its capacitance, the internal electrodes are exposed in the width direction of the body, thereby maximizing the area of the internal electrodes in the width direction through a margin-free design. After manufacturing such unit chips and before firing, a process is used in which a side margin portion is separately attached to the exposed surface of the internal electrodes in the width direction of the unit chips.
[0004] In the conventional method of attaching and punching the side margin portion, a sheet for the side margin portion peeled from a molded film is attached to the side of a unit chip and pressurized. In the process of pressing and punching, there is a risk of the sheet being stretched by heat and the physical properties being changed due to the volatilization of the organic solvent, which may cause the sheet to peel off, an increase in the process time, and non-uniformity of the fracture surface.
[0005] Such peeling of the sheet and non-uniformity of the fracture surface form moisture permeation paths in the multilayer electronic component, which can be a major cause of deterioration in moisture resistance reliability.
[0006] Therefore, there is a need to study a multilayer electronic component and a method for manufacturing the multilayer electronic component that can minimize damage to the side margins during attachment and punching of the side margins. Summary of the Invention [Problem to be solved by the invention]
[0007] One of the various objects of the present invention is to provide a multilayer electronic component having side margins, which can suppress a decrease in moisture resistance reliability due to damage to the side margins.
[0008] One of the various objects of the present invention is to provide a manufacturing method that can prevent damage to the side margin when a side margin sheet is attached to the attachment surface of the side margin and punched out to form the side margin.
[0009] However, the object of the present invention is not limited to the above-mentioned contents, and can be more easily understood in the course of describing specific embodiments of the present invention. [Means for solving the problem]
[0010] According to an embodiment of the present invention, there is provided a multilayer electronic component comprising: a body including dielectric layers and internal electrodes alternately arranged in a first direction, the dielectric layers and the internal electrodes overlapping in the first direction, the body including an active portion, and a cover portion arranged on one side and the other side of the active portion in the first direction; external electrodes arranged on one side and the other side of the body in a second direction perpendicular to the first direction; and side margin portions arranged on one side and the other side of the body in a third direction perpendicular to the first direction and the second direction, the boundary between the active portion and the cover portion being defined as an active-cover portion in cross sections in the first direction and the third direction. When the bar boundary and the boundary between the main body and the side margin portion are defined as a first main body-side margin boundary, the average distance in the first direction from the active-cover boundary to the first direction end of the side margin portion that is closest to the active-cover boundary among the ends of the side margin portion in the first direction is defined as A1, and the average distance in the third direction from the first main body-side margin boundary to the third direction end of the side margin portion that is closest to the first body-side margin boundary among the ends of the side margin portion in the third direction is defined as A2, A1 / A2 satisfies more than 1.5 and less than 2.5.
[0011] A method for manufacturing a multilayer electronic component according to one embodiment includes a main body including an active portion, the active portion being an area where the dielectric layers and the internal electrodes overlap in the first direction, and a cover portion arranged on one side and the other side of the active portion in the first direction, external electrodes arranged on one side and the other side of the main body in a second direction perpendicular to the first direction, and side margin portions arranged on one side and the other side of the main body in a third direction perpendicular to the first direction and the second direction, and a boundary between the active portion and the cover portion in a cross section in the first direction and the third direction is defined as an active-cover portion. When the bar boundary and the boundary between the main body and the side margin portion are defined as a first main body-side margin boundary, the average distance in the first direction from the active-cover boundary to the first direction end of the side margin portion that is closest to the active-cover boundary among the ends of the side margin portion in the first direction is defined as A1, and the average distance in the third direction from the first main body-side margin boundary to the third direction end of the side margin portion that is closest to the first body-side margin boundary among the ends of the side margin portion in the third direction is defined as A2, A1 / A2 satisfies more than 1.5 and less than 2.5. Effect of the Invention
[0012] One of the various objects of the present invention is to provide a multilayer electronic component having side margins, which can suppress a decrease in moisture resistance reliability due to damage to the side margins.
[0013] One of the various objects of the present invention is to provide a manufacturing method that can prevent damage to the side margin when a ceramic green sheet for the side margin is attached to the attachment surface of the side margin and then punched out to form the side margin. [Brief description of the drawings]
[0014] [Figure 1] 1 is a perspective view showing a multilayer electronic component according to an embodiment of the present invention; [Diagram 2] FIG. 2 is a schematic perspective view of a main body according to one embodiment. [Diagram 3] 2 is a cross-sectional view taken along line II' in FIG. [Figure 4] 2 is a cross-sectional view taken along line II-II' in FIG. [Diagram 5] FIG. 2 is a cross-sectional view taken along line III-III' in FIG. [Figure 6a] 2 is a perspective view showing a lamination step in a method for manufacturing a multilayer electronic component according to an embodiment; FIG. [Figure 6b] 1 is a perspective view showing a state immediately after a lamination step in a method for manufacturing a multilayer electronic component according to one embodiment. FIG. [Figure 6c] 2 is a perspective view showing a cutting step in a method for manufacturing a multilayer electronic component according to an embodiment; FIG. [Figure 7a] 1 is a perspective view showing an expansion step in a method for manufacturing a multilayer electronic component according to an embodiment; [Figure 7b] 2 is a perspective view illustrating a release step in a method for manufacturing a multilayer electronic component according to an embodiment; [Figure 8a] 1 is a plan view showing a state immediately before a side margin portion is formed in a method for manufacturing a multilayer electronic component according to one embodiment. FIG. [Figure 8b] 1 is a plan view showing a state immediately after pressing and punching a ceramic green sheet for a side margin portion in a method for manufacturing a multilayer electronic component according to one embodiment. FIG. [Figure 9] 4 is a plan view illustrating a shape of a corner of a laminate during a process in which a ceramic green sheet for a side margin portion is pressed and punched in a method for manufacturing a multilayer electronic component according to an embodiment. FIG. [Figure 10a] 13 is a graph showing the results of a composite reliability evaluation of a multilayer electronic component according to a comparative example. [Figure 10b] 11 is a graph showing the results of a composite reliability evaluation of the multilayer electronic component according to the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, the embodiments of the present invention will be described with reference to specific embodiments and the accompanying drawings. However, the embodiments of the present invention can be modified into several other forms, and the scope of the present invention is not limited to the embodiments described below. Furthermore, the embodiments of the present invention are provided to more completely explain the present invention to those skilled in the art. Therefore, the shapes and sizes of elements in the drawings may be enlarged or reduced (or highlighted or simplified) for clearer explanation, and elements indicated by the same reference numerals in the drawings are the same elements.
[0016] In addition, in the drawings, parts that are not relevant to the description are omitted in order to clearly explain the present invention, and the size and thickness of each component shown in the drawings are arbitrarily shown for convenience of explanation, so the present invention is not necessarily limited by the drawings. Furthermore, components having the same function within the same concept may be described using the same reference numerals. Furthermore, throughout the specification, when a part "includes" a certain component, it does not mean that the part excludes other components, but that the part may further include other components, unless otherwise specified to the contrary.
[0017] In the drawings, the first direction is the direction in which a plurality of green sheets are stacked or the thickness (T) direction, and among the second and third directions perpendicular to the first direction, the second direction can be defined as the length (L) direction and the third direction can be defined as the width (W) direction.
[0018] Multilayer Electronic Components FIG. 1 is a perspective view generally showing a multilayer electronic component according to one embodiment of the present invention, FIG. 2 is a perspective view generally showing a main body according to one embodiment, FIG. 3 is a cross-sectional view taken along line I-I' in FIG. 1, FIG. 4 is a cross-sectional view taken along line II-II' in FIG. 1, and FIG. 5 is a cross-sectional view taken along line III-III' in FIG. 1.
[0019] A multilayer electronic component 100 according to one embodiment of the present invention and various embodiments thereof will be described in detail below with reference to FIGS. 1 to 5.
[0020] A multilayer electronic component according to an embodiment of the present invention includes a body 110 including dielectric layers 111 and internal electrodes 121, 122 alternately arranged in a first direction, an active portion Ac being a region where the dielectric layers and the internal electrodes overlap in the first direction, and cover portions 112, 113 arranged on one side and the other side of the active portion in the first direction, external electrodes 131, 132 arranged on one side and the other side of the body in a second direction perpendicular to the first direction, and side margin portions 114, 115 arranged on one side and the other side of the body in a third direction perpendicular to the first direction and the second direction, and in cross sections in the first direction and the third direction, When the boundary between the active portion and the cover portion is defined as an active-cover boundary, the boundary between the main body and the side margin portion is defined as a first body-side margin boundary, and the average distance in the first direction from the active-cover boundary to the first direction end of the side margin portion that is closest to the active-cover boundary among the ends of the side margin portion in the first direction is defined as A1, and the average distance in the third direction from the first body-side margin boundary to the third direction end of the side margin portion that is closest to the first body-side margin boundary among the ends of the side margin portion in the third direction, A1 / A2 satisfies a ratio greater than 1.5 and less than 2.5.
[0021] The main body 110 includes dielectric layers 111 and internal electrodes 121, 122 arranged alternately in a first direction, an active portion Ac which is a region where the dielectric layers and the internal electrodes overlap in the first direction, and cover portions 112, 113 arranged on one and the other sides of the active portion in the first direction.
[0022] Although there is no particular limitation on the specific shape of the body 110, the body 110 may be hexahedral or a similar shape as shown in Fig. 2. Due to shrinkage of the ceramic powder contained in the body 110 during the firing process, the body 110 may have a substantially hexahedral shape rather than a hexahedral shape having perfectly straight lines.
[0023] The body 110 may include one side and the other side 1, 2 facing each other in a first direction, one side and the other side 3, 4 in a second direction, and one side and the other side 5, 6 in a third direction. In this case, the first direction may be defined as a direction in which the plurality of dielectric layers 111 and the plurality of internal electrodes 121, 122 are stacked, the second direction may be perpendicular to the first direction and may refer to a direction in which an end of the first internal electrode 121 and an end of the second internal electrode 122 among the plurality of internal electrodes 121, 122 are alternately exposed on a surface of the body 110, and the third direction may refer to a direction perpendicular to the first and second directions.
[0024] The body 110 may include corners connecting one side and the other side facing each other in the first to third directions. The corners of the body may be formed due to shrinkage behavior during a sintering process. In one embodiment, the corners of the body 110 may be rounded. This may prevent chipping defects of the multilayer electronic component 100.
[0025] The method for forming the corners of the body 110 into a round shape is not particularly limited, but the corners may be rounded by pressing and punching a ceramic green sheet for a side margin portion onto one side and the other side of the laminate in the third direction in a manufacturing method of a multilayer electronic component described later, while the pressing and punching are performed with a carrier film attached.
[0026] The dielectric layers 111 are in a fired state, and the boundaries between adjacent dielectric layers 111 can be integrated to such an extent that they are difficult to confirm without using a scanning electron microscope (SEM).
[0027] The raw material for forming the dielectric layer 111 is not particularly limited as long as sufficient capacitance can be obtained. For example, a barium titanate-based material, a lead composite perovskite-based material, a strontium titanate-based material, or the like can be used. The barium titanate-based material can include BaTiO3-based ceramic powder. Examples of the ceramic powder include BaTiO3, (Ba 1-x Ca x )TiO3 (0 < x < 1) in which Ca (calcium), Zr (zirconium), etc. are partially solid-solved in BaTiO3, Ba(Ti 1-y Ca y )O3 (0 < y < 1), (Ba 1-x Ca x )(Ti 1-y Zr y )O3 (0 < x < 1, 0 < y < 1), or Ba(Ti 1-y Zr y )O3 (0 < y < 1), etc.
[0028] In addition, various ceramic additives, organic solvents, binders, dispersants, etc. can be added to the powder such as barium titanate (BaTiO3) according to the purpose of the present invention as the raw material for forming the dielectric layer 111.
[0029] On the other hand, the average thickness td of the dielectric layer 111 does not need to be particularly limited. However, generally, when the dielectric layer 111 is formed thinly with a thickness of less than 0.6 μm, especially when the average thickness td of the dielectric layer 111 is 0.35 μm or less, the reliability may decrease.
[0030] According to one embodiment of the present invention, in order to improve the moisture resistance reliability by adjusting the shapes of the side margin portions 114 and 115, even when the average thickness te of the dielectric layer 111 is 0.35 μm or less, excellent moisture resistance reliability of the multilayer electronic component 100 can be ensured.
[0031] Therefore, when the average thickness td of the dielectric layer 111 is 0.35 μm or less, the effect according to the present invention can become more remarkable, and miniaturization and high capacitance of the multilayer electronic component 100 can be more easily achieved.
[0032] The average thickness td of the dielectric layer 111 may refer to an average size in the first direction of the dielectric layer 111 disposed between the first internal electrode 121 and the second internal electrode 122. Meanwhile, when the body 110 includes a plurality of dielectric layers 111, the average thickness td of the dielectric layer 111 may refer to an average thickness of at least one of the plurality of dielectric layers 111.
[0033] The average thickness td of the dielectric layer 111 may be measured by scanning an image of a cross section of the body 110 in the length and thickness direction (LT) using a scanning electron microscope (SEM) with a magnification of 10,000. More specifically, the thickness of one dielectric layer may be measured at 30 equally spaced points in the length direction in the scanned image, and an average value may be measured. The 30 equally spaced points may be designated as active parts Ac. Furthermore, if such an average value measurement is extended to 10 dielectric layers to measure the average value, the average thickness of the dielectric layer may be further generalized.
[0034] 2 to 4, the active portion Ac of the present invention means a region where the dielectric layer 111 and the internal electrodes 121 and 122 overlap in the first direction.
[0035] The active portion Ac is a portion that contributes to forming the electrostatic capacitance of the multilayer electronic component, and can be formed by repeatedly laminating a plurality of internal electrodes 121, 122 with a dielectric layer 111 sandwiched therebetween.
[0036] Cover portions 112 and 113 are disposed on one and the other surfaces of the active portion Ac in the first direction.
[0037] The cover parts 112, 113 may be formed by stacking a single dielectric layer or two or more dielectric layers on one side and the other side of the first direction of the active part Ac, respectively, and may essentially serve to prevent damage to the internal electrodes due to physical or chemical stress.
[0038] The cover portions 112 , 113 do not include an internal electrode and may comprise substantially the same material as the dielectric layer 111 .
[0039] The average thickness tc of the cover parts 112, 113 does not need to be particularly limited. However, in order to more easily achieve miniaturization and high capacity of the multilayer electronic component, the average thickness tc of the cover parts 112, 113 may be 15 μm or less. Here, the average thickness of the cover parts 112, 113 may mean the average thickness of each of the first cover part 112 and the second cover part 113.
[0040] The average thickness tc of the cover parts 112, 113 may mean the size in the first direction, and may be the average value of the sizes in the first direction of the cover parts 112, 113 measured at five equally spaced points on the upper or lower part of the active part Ac.
[0041] The internal electrodes 121, 122 and the dielectric layers 111 are alternately arranged in the first direction.
[0042] The internal electrodes 121, 122 may include a first internal electrode 121 and a second internal electrode 122. Referring to Figures 2 and 3, the first internal electrodes 121 and the second internal electrodes 122 are alternately arranged to face each other with a dielectric layer 111 constituting the body 110 interposed therebetween, and may be connected to one surface and the other surface of the body 110 in the second direction, respectively. Specifically, one end of the first internal electrode 121 may be connected to one surface 3 of the body 110 in the second direction, and one end of the second internal electrode 122 may be connected to the other surface 4 of the body 110 in the second direction.
[0043] That is, the first internal electrode 121 is connected to the first external electrode 131 but not to the second external electrode 132, and the second internal electrode 122 is connected to the second external electrode 132 but not to the first external electrode 131. Thus, the first internal electrodes 121 may be formed at a predetermined distance apart on the other surface 4 in the second direction of the body 110, and the second internal electrodes 122 may be formed at a predetermined distance apart on one surface 3 in the second direction of the body 110. At this time, the first internal electrode 121 and the second internal electrode 122 may be electrically isolated from each other by the dielectric layer 111 disposed therebetween.
[0044] 2, in one embodiment, one end in the third direction of the internal electrodes 121, 122 may contact one surface 5 in the third direction of the body 110, and the other end in the third direction of the internal electrodes 121, 122 may contact the other surface 6 in the third direction of the body 110. This increases the specific gravity of the active parts Ac in the entire component, thereby maximizing the capacitance per unit volume of the multilayer electronic component 100.
[0045] There are no particular limitations on the material forming the internal electrodes 121 and 122, and any material having excellent electrical conductivity can be used. For example, the internal electrodes 121 and 122 can include one or more of nickel (Ni), copper (Cu), palladium (Pd), silver (Ag), gold (Au), platinum (Pt), tin (Sn), tungsten (W), titanium (Ti), and alloys thereof.
[0046] The internal electrodes 121 and 122 may be formed by printing a conductive paste for internal electrodes, which includes at least one of nickel (Ni), copper (Cu), palladium (Pd), silver (Ag), gold (Au), platinum (Pt), tin (Sn), tungsten (W), titanium (Ti), and alloys thereof, on the ceramic green sheet. The method for printing the conductive paste for internal electrodes may be a screen printing method or a gravure printing method, but the present invention is not limited thereto.
[0047] On the other hand, the average thickness te of the internal electrodes 121, 122 does not need to be particularly limited.
[0048] However, in general, when the internal electrodes 121, 122 are formed to a thickness of less than 0.6 μm, particularly when the average thickness te of the internal electrodes 121, 122 is 0.35 μm or less, there is a risk of the reliability decreasing.
[0049] According to one embodiment of the present invention, the moisture resistance reliability is improved by adjusting the shape of the side margin portions 114, 115, so that excellent moisture resistance reliability of the multilayer electronic component 100 can be ensured even when the average thickness te of the internal electrodes 121, 122 is 0.35 μm or less.
[0050] Therefore, when the average thickness te of the internal electrodes 121, 122 is 0.35 μm or less, the effects of the present invention become more pronounced, and the multilayer electronic component 100 can be more easily reduced in size and increased in capacity.
[0051] The average thickness te of the internal electrodes 121, 122 may refer to an average size of the internal electrodes 121, 122 in a first direction. Meanwhile, when the body 110 includes a plurality of internal electrodes 121, 122, the average thickness td of the internal electrodes 121, 122 may refer to an average thickness of at least one of the plurality of internal electrodes 121, 122.
[0052] The average thickness te of the internal electrodes 121, 122 may be measured by scanning an image of a cross section of the body 110 in the length and thickness direction (LT) using a scanning electron microscope (SEM) with a magnification of 10,000. More specifically, the thickness of one internal electrode may be measured at 30 equally spaced points in the length direction in the scanned image, and an average value may be measured. The 30 equally spaced points may be designated as active parts Ac. Furthermore, if such an average value measurement is extended to 10 internal electrodes and an average value is measured, the average thickness of the internal electrodes may be further generalized.
[0053] 1, 3 and 4, side margins 114 and 115 may be disposed on one and other surfaces 5 and 6 of the body 110 in the third direction.
[0054] The side margins 114 and 115 essentially serve to prevent damage to the internal electrodes due to physical or chemical stress.
[0055] The method for forming the side margin portions 114 and 115 is not particularly limited. For example, they may be formed by applying a ceramic slurry for the side margin portions to the side surfaces of the laminate 200 and then firing the ceramic slurry, or by pressurizing and adhering a ceramic green sheet for the side margin portions to the side surfaces and then firing the ceramic green sheet. The material for forming the side margin portions 114 and 115 does not need to be particularly limited, and may be the same material as that of the dielectric layer 111, but is not limited thereto, and may be formed of a different material from that of the dielectric layer 111, resulting in a different composition.
[0056] On the other hand, there is no need to particularly limit the width of the marginal portions 114, 115. However, in order to more easily achieve a smaller size and higher capacity of the multilayer electronic component, the average width of the marginal portions 114, 115 can be 15 μm or less.
[0057] In addition, according to an embodiment of the present invention, in the side margin portions 114, 115, the shape of the side margin portions 114, 115 is adjusted to improve the moisture resistance reliability, so that excellent reliability can be ensured even when the average width of the side margin portions 114, 115 is 15 μm or less. The average width of the side margin portions 114, 115 may mean the average size of the side margin portions 114, 115 in the third direction, and may be an average value of the sizes of the side margin portions 114, 115 in the third direction measured at five equally spaced points on a side of the active portion Ac.
[0058] The external electrodes 131 and 132 may be disposed on a third or fourth surface of the body 110. Specifically, the first external electrode 131 is disposed on one surface 3 in the second direction of the body 110 and connected to the first internal electrode 121, and the second external electrode 132 is disposed on the other surface 4 in the second direction of the body 110 and connected to the second internal electrode 122.
[0059] In this embodiment, a structure in which the multilayer electronic component 100 has two external electrodes 131, 132 is described, but the number and shapes of the external electrodes 131, 132 can be changed depending on the shape of the internal electrodes 121, 122 and other purposes.
[0060] Meanwhile, the external electrodes 131 and 132 may be formed using any material that has electrical conductivity, such as a metal, and the specific material may be determined taking into consideration electrical characteristics, structural stability, etc., and may further have a multi-layer structure.
[0061] Meanwhile, the external electrodes 131, 132 may be formed on one surface and the other surface of the body 110 in the second direction, and may be arranged to extend on one surface and the other surface in the first direction or on a part of one surface and the other surface in the third direction. In this case, the external electrodes 131, 132 may be arranged to cover the ends of the side margin parts 114, 115. In this case, the areas of the external electrodes 131, 132 arranged on the ends of the side margin parts 114, 115 may be rounded, thereby ensuring the coverage of the external electrodes 131, 132 even on the corners of the body 110 or the side margin parts 114, 115.
[0062] The external electrodes 131 and 132 may include electrode layers 131a and 132a disposed on the body 110 and plating layers 131b and 132b formed on the electrode layers 131a and 132a.
[0063] As a more specific example of the electrode layers 131a and 132a, the electrode layers may be fired electrodes containing a conductive metal and glass, or resin-based electrodes containing a conductive metal and resin.
[0064] Also, the electrode layers 131a and 132a may be in a form in which a fired electrode and a resin-based electrode are sequentially formed on the body 110. Also, the electrode layers 131a and 132a may be formed by transferring a sheet containing a conductive metal onto the body 110, or by transferring a sheet containing a conductive metal onto a fired electrode.
[0065] The conductive metal contained in the electrode layers 131a and 132a may be a material having excellent electrical conductivity, and is not particularly limited. For example, the conductive metal may be one or more of nickel (Ni), copper (Cu), and alloys thereof.
[0066] The plating layers 131b and 132b may serve to improve the sealing property or mounting characteristics of the multilayer electronic component 100. The type of the plating layers 131b and 132b is not particularly limited, and may be a plating layer containing one or more of Ni, Sn, Pd, and alloys thereof, and may be formed of a plurality of layers.
[0067] As a more specific example of the plating layers 131b, 132b, the plating layers 131b, 132b may be Ni-containing plating layers or Sn-containing plating layers, and may have a form in which a Ni-containing plating layer and a Sn-containing plating layer are sequentially formed on the electrode layers 131a, 132a, or a form in which a Sn-containing plating layer, a Ni-containing plating layer, and a Sn-containing plating layer are sequentially formed. Also, the plating layers may include a plurality of Ni plating layers and / or a plurality of Sn plating layers.
[0068] Conventionally, one example of a method for forming side margin portions is a method in which, in order to suppress steps caused by internal electrodes 121, 122, after lamination, the internal electrodes are cut so that they are exposed on one side and the other side 5, 6 in the third direction of the main body, and then a single dielectric layer or two or more dielectric layers are laminated on one side and the other side in the third direction of active portion Ac to form side margin portions 114, 115.
[0069] However, in order to form such side margins 114, 115 firmly, it may not be sufficient to simply laminate the dielectric layers on one surface and the other surface in the third direction of the active portion Ac, and a separate high-temperature and high-pressure treatment may be required. For example, in one embodiment, a pressurizing and punching process may be performed on one surface and the other surface in the third direction of the unit chip 210, which is in a state before the firing of the main body 110, of the ceramic green sheet for the side margins. As a result, the ends of the side margins 114, 115 that have undergone the firing process may be formed unevenly, which may be a major cause of a decrease in the moisture resistance reliability of the multilayer electronic component 100.
[0070] Therefore, in the present invention, the moisture resistance reliability of the multilayer electronic component 100 is improved by adjusting the positional relationship between the active-cover boundary and the body-side margin boundary, and the ends of the side margin portions in the first direction and the third direction, among the parameters indicating the shape of the ends of the side margin portions 114 and 115.
[0071] Referring to FIG. 3, the positional relationship between the active-cover boundary and the body-side margin boundary and the first direction end and third direction end of the side margin portion can be defined in the cross sections of the laminated electronic component 100 in the first direction and the third direction.
[0072] First, in the cross sections of the multilayer electronic component 100 in the first and third directions, the boundary between the active portion Ac and the cover portions 112 and 113 may be defined as an active-cover boundary, and the boundary between the body 110 and the side margin portions 114 and 115 may be defined as a body-side margin boundary. In this case, the body-side margin boundary may be defined as a first body-side margin boundary in order to distinguish it from the boundary in the cross sections of the multilayer electronic component 100 in the first and second directions, which will be described later. Specifically, the active-cover boundary may be defined as a straight line connecting the ends of the internal electrodes 121 and 122 included in the active portion Ac in the first direction in the third direction, and the first body-side margin boundary may be defined as a straight line connecting the ends of the internal electrodes 121 and 122 included in the active portion Ac in the third direction in the first direction.
[0073] Meanwhile, the side margin portions 114, 115 may have ends because they are disposed on one surface and the other surface in the third direction of the main body 110. The ends of the side margin portions 114, 115 correspond to the boundaries between the main body 110 and the side margin portions 114, 115, and may become the main path for penetration of external moisture. Therefore, the moisture resistance reliability of the multilayer electronic component 100 may be significantly affected by the shape of the ends of the side margin portions 114, 115.
[0074] On the end faces in the first and third directions of the multilayer electronic component 100, the side margin portions 114, 115 may have an end in the first direction and an end in the third direction. Here, the end in the first direction may refer to an end located at the outermost position in the first direction based on a central region in the first direction of the side margin portions 114, 115, and the end in the third direction may refer to an end located at the outermost position in the third direction based on a central region in the third direction of the side margin portions 114, 115.
[0075] In one embodiment of the present invention, the average distance in the first direction from the active-cover boundary to the first direction end of the side margin portion that is closest to the active-cover boundary among the ends of the side margin portion in the first direction is defined as A1, and the average distance in the third direction from the first body-side margin boundary to the third direction end of the side margin portion that is closest to the first body-side margin boundary among the ends of the side margin portion in the third direction is defined as A2, and the value of A1 / A2 is adjusted.
[0076] If the A1 / A2 value is 1.5 or less, the moisture-resistant path becomes shorter, which may result in a decrease in reliability. If the A1 / A2 value is 2.5 or more, thickness asymmetry occurs between the cover and side margin, which may result in a mismatch in the shrinkage rate during firing, which may cause the side margin or cover to peel off.
[0077] Therefore, in one embodiment of the present invention, the moisture resistance reliability of the multilayer electronic component 100 can be improved by ensuring that the A1 / A2 value is greater than 1.5 and less than 2.5.
[0078] Meanwhile, since the shape of the side margin portions 114, 115, particularly the shape of the ends of the side margin portions 114, 115, has a three-dimensional shape, simultaneously adjusting the active-side margin boundary and the relationship between the second direction ends of the active portion Ac and the ends of the side margin portions 114, 115 not only in the first direction and second direction cross sections of the multilayer electronic component 100 but also in the second direction and third direction cross sections can be a method that can more significantly improve the moisture resistance reliability of the multilayer electronic component 100.
[0079] Specifically, in the cross sections of the multilayer electronic component 100 in the second and third directions, the boundaries between the main body 110 and the side margin portions 114, 115 can be defined as second main body-side margin boundaries.
[0080] Furthermore, at the end faces in the second and third directions of the multilayer electronic component 100, the side margin portions 114, 115 may have ends in the second direction and ends in the third direction.
[0081] Here, the end in the third direction may refer to the end located outermost in the third direction based on the central region in the third direction of the side margin portions 114, 115, and the end in the second direction may refer to the end located outermost in the second direction based on the central region in the second direction of the side margin portions 114, 115.
[0082] In one embodiment, the average distance in the second direction from the end of the active part in the second direction to the face of the second direction surface of the main body that is closest to the end of the active part in the second direction is B1, and the average distance in the third direction from the second main body-side margin boundary to the end of the side margin part in the third direction that is closest to the second main body-side margin boundary among the ends of the side margin part in the third direction, is B2, and the B1 / B2 value is adjusted.
[0083] If the B1 / B2 value is 0.35 or less, the round will not be formed properly, which may result in chipping and scratch-related cosmetic defects, and if the B1 / B2 value is 0.55 or more, the round will exceed the appropriate range, shortening the moisture-resistant path and potentially causing reliability problems.
[0084] Therefore, in one embodiment, the moisture resistance reliability of the multilayer electronic component 100 can be improved by adjusting the B1 / B2 value to be greater than 0.35 and less than 0.55.
[0085] In addition, when the A1 / A2 value satisfies the range of more than 1.5 and less than 2.5, and at the same time the B1 / B2 value satisfies the range of more than 0.35 and less than 0.55, the effect of improving the moisture resistance reliability can be more remarkable.
[0086] Meanwhile, A1 and A2 indicating the average distances may be average values measured using an optical microscope (OM) or a scanning electron microscope (SEM) on cross sections in the first and third directions polished to 1 / 3, 1 / 2, and 2 / 3 points in the second direction of the multilayer electronic component 100. If such measurements are performed in the four end regions of the margin portions 114 and 115 shown in the cross sections and averaged, the A1 and A2 values can be further generalized.
[0087] The average distances B1 and B2 may be average values measured using an optical microscope (OM) or a scanning electron microscope (SEM) on cross sections in the second and third directions polished to 1 / 3, 1 / 2, and 2 / 3 points in the first direction of the multilayer electronic component 100. If such measurements are performed in the four end regions of the margins 114 and 115 shown in the cross sections and the average values are calculated, the B1 and B2 values can be further generalized.
[0088] In one embodiment, the side margin portions 114, 115 may be disposed so as not to extend beyond one surface 1, 2 in the first direction of the body 110. From another perspective, the side margin portions 114, 115 may be disposed so as not to extend beyond one surface 5, 6 in the third direction of the body 110. As a result, the side margin portions 114, 115 are formed with a minimum specific gravity required to ensure moisture resistance reliability, thereby improving the capacitance per unit volume of the multilayer electronic component 100. Additionally, a uniform thickness can be ensured when forming the external electrodes.
[0089] Manufacturing method for multilayer electronic components 6a is a perspective view showing a lamination step in a method for manufacturing a multilayer electronic component according to an embodiment, FIG. 6b is a perspective view showing a state immediately after the lamination step in a method for manufacturing a multilayer electronic component according to an embodiment, FIG. 6c is a perspective view showing a cutting step in a method for manufacturing a multilayer electronic component according to an embodiment, FIG. 7a is a perspective view showing an expansion step in a method for manufacturing a multilayer electronic component according to an embodiment, FIG. 7b is a perspective view showing an opening step in a method for manufacturing a multilayer electronic component according to an embodiment, FIG. 8a is a plan view showing a state immediately before forming a side margin portion in a method for manufacturing a multilayer electronic component according to an embodiment, FIG. 8b is a plan view showing a state immediately after pressing and punching a ceramic green sheet for a side margin portion in a method for manufacturing a multilayer electronic component according to an embodiment, and FIG. 9 is a plan view showing the shape of a corner of a laminate in the process of pressing and punching a ceramic green sheet for a side margin portion in a method for manufacturing a multilayer electronic component according to an embodiment.
[0090] A method for manufacturing a multilayer electronic component will be described in detail below with reference to Figures 6a to 9. The method for manufacturing a multilayer electronic component described below is an example for manufacturing the multilayer electronic component 100 described above, and therefore it is not necessary to manufacture the multilayer electronic component 100 only by the manufacturing method described below.
[0091] Laminate manufacturing stages First, in the multilayer electronic component according to an embodiment, a multilayer body may be fabricated. The multilayer body 200 may become a part that forms the body 110 of the present invention after firing.
[0092] In the manufacturing process of the laminate 200, first, a plurality of ceramic green sheets 201, 202 having conductive patterns 221, 222 arranged thereon are laminated on a support film 310.
[0093] The support film 310 may play a role in supporting the laminate 200 in which the conductive patterns 221, 222 and the plurality of ceramic green sheets 201, 202 are laminated. In this case, the support film 310 may include an adhesive material such as latex, starch, cellulose, protein, IR (Isoprene Rubber), NBR (Nitrile Butadiene Rubber), SBR (Styrene Butadiene Rubber), CR (Chloroprene Rubber), Silicon Rubber, Silicon-based, Urethane-based, Acrylic-based, and mixtures thereof, in order to effectively support and attach the laminate 200.
[0094] The plurality of ceramic green sheets 201, 202 may be formed from a ceramic paste containing ceramic powder, an organic solvent, a dispersant, and a binder. The ceramic powder may be a raw material for forming the dielectric layer 111 of the multilayer electronic component 100, and may be a barium titanate-based material, a lead composite perovskite-based material, a strontium titanate-based material, or the like. The barium titanate-based material may contain BaTiO3-based ceramic powder, and examples of the ceramic powder include BaTiO3, BaTiO3 partially solid-dissolved with Ca (calcium), Zr (zirconium), and the like. 1-x Ca x )TiO3(0 <x<1)、Ba(Ti 1-y Ca y )O3(0 <y<1)、(Ba 1-x Ca x )(Ti 1-y Zry ) O3 (0 < x < 1, 0 < y < 1) or Ba(Ti 1-y Zr y ) O3 (0 < y < 1), etc. When a plurality of ceramic green sheets 201, 202 are fired, a dielectric layer 111 constituting the main body 110 is formed.
[0095] On the other hand, in one embodiment, the laminate 200 can further include a cover - part ceramic green sheet 203 that forms cover parts 112, 113. The cover - part ceramic green sheet 203 can be composed of the same material and components as the ceramic green sheets 201, 202, but is not limited thereto, and can form the upper and lower cover parts 112, 113 of the main body 110 through a firing process. At this time, the cover - part ceramic green sheet 203 can be formed on one surface and the other surface of the laminate in the first direction, and can be formed as a single layer or a plurality of layers.
[0096] The conductive patterns 221, 222 can be formed on the ceramic green sheets 201, 202 by an internal - electrode paste containing a conductive metal. The conductive metal contained in the conductive patterns 221, 222 is not particularly limited, and a material with excellent electrical conductivity can be used. For example, the above - mentioned conductive metal can include one or more of nickel (Ni), copper (Cu), palladium (Pd), silver (Ag), gold (Au), platinum (Pt), tin (Sn), tungsten (W), titanium (Ti), and alloys thereof. The method of forming the conductive patterns 221, 222 on the ceramic green sheets 201, 202 is not particularly limited. For example, the conductive paste for internal electrodes containing the above - mentioned conductive metal can be screen - printed or gravure - printed on the ceramic green sheets 201, 202 to form them.
[0097] The conductive patterns 221, 222 can be in a stripe shape. Specifically, the internal - electrode pattern can be formed to be in contact with both ends of the ceramic green sheets 201, 202 in the third direction at regular intervals in the second direction.
[0098] The conductive patterns 221, 222 may include a first conductive pattern 221 formed on a ceramic green sheet 201 and a second conductive pattern 222 formed on another ceramic green sheet 202. In this case, the ceramic green sheet on which the first conductive pattern 221 is formed may be referred to as the first ceramic green sheet 201, and the ceramic green sheet on which the second conductive pattern 222 is formed may be referred to as the second ceramic green sheet 202.
[0099] Meanwhile, in the present invention, for convenience of explanation, the direction in which a plurality of ceramic green sheets arranged on the support film 310 are stacked will be described as a first direction.
[0100] Cutting the laminate After the step of fabricating the laminate, a step of cutting the laminate may be performed.
[0101] 6b, the laminate 200 may be cut along cutting lines C1-C1 and C2-C2 that are perpendicular to each other. The C1-C1 cutting lines are parallel to the second direction and are arranged at substantially equal intervals in the third direction, and the C2-C2 cutting lines are parallel to the third direction and are arranged at substantially equal intervals in the second direction. The C1-C1 cutting lines may form unit chips 210 having a substantially constant size in the third direction, and the C2-C2 cutting lines may form unit chips 210 having a substantially constant size in the second direction.
[0102] There is no particular limitation on the means for cutting the laminate 200. For example, the laminate 200 can be cut using a blade cutting method such as a doctor blade or a dicing blade, a guillotine cutting method, or a laser cutting method.
[0103] 6c, it can be seen that immediately after the cutting step of the laminate, the laminate 200 is formed of a plurality of unit chips 210. The plurality of unit chips 210 may remain attached to the support film 310 even after cutting due to the adhesiveness of the support film 310.
[0104] Expansion Phase After the cutting step of the laminate, an expansion step may be performed by stretching the support film 310 in the second and third directions, but is not limited thereto, and may be performed by transferring a plurality of unit chips 210 to another separate film.
[0105] Opening stage After the expanding step, an opening step may be performed, which is a process of simultaneously opening the sides of the plurality of unit chips 210 on one and the other sides in the third direction of the body 110 to easily form side margins.
[0106] The side of the plurality of unit chips 210 may be a surface cut along the cutting line C1-C1, and may be a surface where an end of the first conductive pattern 221 and an end of the second conductive pattern 222 are simultaneously exposed. A method for releasing the side of the plurality of unit chips 210 is not particularly limited. For example, the plurality of unit chips 210 may be simultaneously rotated or moved to another film without being rotated. In this case, the plurality of unit chips 210 may be moved to a separate adhesive tape 320.
[0107] Side margin formation stage After the opening step, a side margin forming step may be performed.
[0108] In the step of forming the side margin portion, a process of pressing and punching the ceramic green sheet for the side margin portion may be performed on one side SF of the unit chip 210. In the step of forming the side margin portion described below, it is described that the side margin portion is formed only on one side SF of the unit chip 210, but the same process may be performed on the other side of the unit chip 210.
[0109] 8a and 8b, the method of attaching the ceramic green sheet 140 for the side margin to one side SF of the unit chip 210 is not particularly limited. For example, the pressure can be applied using an elastic pad 330. Specifically, the elastic pad 330 and the support plate 340 are sequentially arranged on one side of the adhesive tape 320 on which the unit chips 210 are not arranged, and the support plate 340, the elastic pad 330, the carrier film 350 and the ceramic green sheet 140 for the side margin are sequentially stacked on the open side of the unit chip 210, and then pressure is applied to the upper or lower support plate 340.
[0110] At this time, in one embodiment, in order to prevent the ceramic green sheet 140 for the side margin portion from being deformed or cracked, the ceramic green sheet 140 for the side margin portion may be attached to one side surface SF at a temperature of 50° C. to 150° C.
[0111] There is no particular limitation on the method for forming the side margin portion from the side margin ceramic green sheet 140 attached to one side surface SF of the unit chip 210.
[0112] For example, after attaching the ceramic green sheet 140 for the side margin portion, pressure is applied to the ceramic green sheet 140 for the side margin portion to the extent that the elastic pad 360 is elastically deformed, and punching is performed to cut the ceramic green sheet 140 for the side margin portion only at a portion corresponding to one side surface SF. By punching in this manner, the ceramic green sheet 140 for the side margin portion can be cut at a portion corresponding to one side surface SF to form the side margin portion. The side margin portion can be subsequently fired to form the side margin portion 114 of the multilayer electronic component.
[0113] In one embodiment, in the step of forming the side margin portion, the attachment and punching of the ceramic green sheet 140 for the side margin portion may be performed in a state in which the ceramic green sheet 140 for the side margin portion is attached to the carrier film 350. As a result, even if a separate adhesive is not applied to one side surface S1 or the ceramic green sheet 140 for the side margin portion, rapid drying of the ceramic green sheet 140 for the side margin portion can be prevented and sufficient adhesive strength for the ceramic green sheet 140 for the side margin portion to be attached to one side surface SF can be ensured.
[0114] In addition, since pressure is applied in a manner surrounding the corners of the unit chip 210 during the pressing and punching process, the end shapes of the side margin portions 114, 115 may be rounded. In addition, the A1 / A2 value or the B1 / B2 value of the multilayer electronic component 100 may be adjusted by adjusting the temperature and pressure during the pressing and punching process. That is, the A1 / A2 value or the B1 / B2 value of the multilayer electronic component 100 according to one embodiment or an example of the present invention may be adjusted by adjusting the variables of the pressing and punching process in the process of forming the side margin portions.
[0115] 9, one corner of the unit chip 210 may be rounded when the ceramic green sheet 140 for the side margins is pressed and punched with the carrier film 350 attached thereto. In addition, since the ceramic green sheet 140 for the side margins is pressed and punched with the carrier film 350 surrounding the ends of the ceramic green sheet 140 for the side margins, the ends of the side margins 114 and 115 may also have rounded shapes.
[0116] In one embodiment, the side margin ceramic green sheet 140 can be prevented from drying out too quickly, so punching can be performed at a temperature of 50° C. or less. This eliminates the need to maintain a high temperature to form the side margin, and reduces damage to the unit chips 210 or the side margin ceramic green sheet 140 caused by thermal shock.
[0117] Meanwhile, the components of the carrier film 350 are not particularly limited. In an embodiment, the carrier film 350 may include one or more of PET (Polyethylene terephthalate), PU (Polyurethane), PE (Polyethylene), PO (Polyolefin), PS (Polystyrene), PVC (Polyvinyl chloride), and PVDC (Polyvinydene chloride). This can effectively prevent the side margin ceramic green sheet 140 attached to the carrier film 350 from drying rapidly. In addition, the thickness of the carrier film 350 is not particularly limited, but it is preferable that the thickness of the carrier film 350 is 1 μm or more in order to properly form the side margin, and is preferably 50 μm or less in order to easily punch out the side margin ceramic green sheet.
[0118] Thereafter, a body forming step may be included in which the unit chip 210 having the side margin portion formed therein is sintered. The sintering temperature is not particularly limited, but may be, for example, 1000 to 1300° C. Also, the sintering may be performed in a reducing atmosphere.
[0119] Thereafter, external electrodes 131 and 132 are formed on one surface and the other surface of body 110 in the second direction, respectively, so that multilayer electronic component 100 can be manufactured.
[0120] Meanwhile, the unit chip 210 having the side margin portion formed thereon can be fired without any additional process to form the main body 110, but is not limited thereto. A conductive paste containing a metal having excellent electrical conductivity can be disposed on one side and the other side 3, 4 in the second direction, respectively, and fired simultaneously with the main body 110 to form the external electrodes 131, 132, thereby manufacturing the multilayer electronic component 100.
[0121] (Experimental Example) 10a and 10b are graphs showing the results of evaluating the composite reliability of the multilayer electronic components according to the comparative example and the embodiment.
[0122] The comparative examples correspond to cases where the A1 / A2 value does not satisfy the condition of being greater than 1.5 and less than 2.5 according to the present invention, or the B1 / B2 value does not satisfy the condition of being greater than 0.35 and less than 0.55, while the examples correspond to cases where the A1 / A2 value satisfies the condition of being greater than 1.5 and less than 2.5 and at the same time the B1 / B2 value satisfies the condition of being greater than 0.35 and less than 0.55.
[0123] FIG. 10a is a graph showing the composite reliability evaluation of the multilayer electronic component according to the comparative example, and FIG. 10b is a graph showing the composite reliability evaluation of the multilayer electronic component according to the example.
[0124] The test was performed on 40 samples each of the comparative example and the embodiment, and the insulation resistance (IR) was measured under the following evaluation conditions: relative humidity 85%, 85°C, 4.8vr, 4 hours. A decrease in insulation resistance value to 10^7 (Ω) or less can be considered to be a reliability defect.
[0125] 10a, it can be seen that the moisture resistance reliability of the multilayer electronic component according to the comparative example is not ensured when there are three or more defective products. Referring to FIG 10b, it can be seen that the moisture resistance reliability is significantly improved when there is only one defective product. Therefore, when the A1 / A2 value is greater than 1.5 and less than 2.5, and the B1 / B2 value is greater than 0.35 and less than 0.55, as in one embodiment, the moisture resistance reliability of the multilayer electronic component 100 can be significantly improved. [Explanation of symbols]
[0126] 100 Multilayer electronic components 110 Main unit 111 Dielectric layer 112, 113 Cover part 114, 115 Margin 121, 122 Internal electrode 131, 132 External electrode 140 Ceramic green sheet for side margin 200 Laminate 201, 202 Ceramic green sheet 203 Ceramic green sheet for cover 210 chips 221, 222 Conductive pattern 310 Support Film 320 Adhesive Tape 330 Elastic Pad 340 Support Plate 350 Carrier Film
Claims
1. a main body including an active portion including dielectric layers and internal electrodes alternately arranged in a first direction, the dielectric layers and the internal electrodes overlapping each other in the first direction, and a cover portion arranged on one side and the other side of the active portion in the first direction; external electrodes disposed on one and the other surfaces of the body in a second direction perpendicular to the first direction; a side margin portion disposed on one surface and the other surface of the main body in a third direction perpendicular to the first direction and the second direction, In cross sections in the first direction and the third direction, a boundary between the active portion and the cover portion is defined as an active-cover boundary, a boundary between the main body and the side margin portion is defined as a first body-side margin boundary, an average distance in the first direction from the active-cover boundary to an end of the side margin portion in the first direction that is closest to the active-cover boundary among the ends of the side margin portion in the first direction is defined as A1, and an average distance in the third direction from the first body-side margin boundary to an end of the side margin portion in the third direction that is closest to the first body-side margin boundary among the ends of the side margin portion in the third direction is defined as A2. A multilayer electronic component having an A1 / A2 ratio of more than 1.5 but less than 2.
5.
2. In cross sections of the laminated electronic component in the second direction and the third direction, a boundary between the main body and the side margin portion is defined as a second main body-side margin boundary, an average distance in the second direction from an end of the active portion in the second direction to a surface of the second direction face of the main body that is closest to the end of the active portion in the second direction is defined as B1, and an average distance in the first direction from the second main body-side margin boundary to an end of the side margin portion in the third direction that is closest to the second main body-side margin boundary among ends of the side margin portion in the third direction, is defined as B2. The multilayer electronic component according to claim 1 , wherein B1 / B2 is greater than 0.35 and less than 0.
55.
3. 2. The multilayer electronic component according to claim 1, wherein ends of said side margin portions in said first direction and said third direction are rounded.
4. The multilayer electronic component according to claim 1 , wherein the corners of the body are rounded.
5. The multilayer electronic component according to claim 1 , wherein the side margin portion is disposed so as not to extend beyond one surface and the other surface of the main body in the first direction.
6. The multilayer electronic component according to claim 1 , wherein the side margin portion is disposed so as not to extend beyond one surface and the other surface of the main body in the third direction.
7. the external electrode is disposed so as to cover an end of the side margin portion, 7. The multilayer electronic component according to claim 1, wherein the regions of the external electrodes arranged on the ends of the side margin portions are rounded.
8. a main body including an active portion including dielectric layers and internal electrodes alternately arranged in a first direction, the dielectric layers and the internal electrodes overlapping each other in the first direction, and a cover portion arranged on one side and the other side of the active portion in the first direction; external electrodes disposed on one and the other surfaces of the body in a second direction perpendicular to the first direction; a side margin portion disposed on one surface and the other surface of the main body in a third direction perpendicular to the first direction and the second direction, In cross sections in the first direction and the third direction, a boundary between the active portion and the cover portion is defined as an active-cover boundary, a boundary between the main body and the side margin portion is defined as a first body-side margin boundary, an average distance in the first direction from the active-cover boundary to an end of the side margin portion in the first direction that is closest to the active-cover boundary among the ends of the side margin portion in the first direction is defined as A1, and an average distance in the third direction from the first body-side margin boundary to an end of the side margin portion in the third direction that is closest to the first body-side margin boundary among the ends of the side margin portion in the third direction is defined as A2. A method for manufacturing a multilayer electronic component, wherein A1 / A2 is greater than 1.5 and less than 2.
5.
9. In cross sections of the multilayer electronic component in the second direction and the third direction, a boundary between the main body and the side margin portion is defined as a second main body-side margin boundary, an average distance in the second direction from an end of the active portion in the second direction to a surface of the second direction surface of the main body that is closest to the end of the active portion in the second direction is defined as B1, and an average distance in the third direction from the second main body-side margin boundary to an end of the side margin portion in the third direction that is closest to the second main body-side margin boundary is defined as B2. The method for producing a multilayer electronic component according to claim 8 , wherein B1 / B2 satisfies the ratio of more than 0.35 to less than 0.
55.
10. 9. The method for manufacturing a multilayer electronic component according to claim 8, wherein the side margin portion is formed by pressing and punching a ceramic green sheet for the side margin portion onto one surface and the other surface in the third direction of the unit chip before the main body is fired.
11. The method for producing a multilayer electronic component according to claim 10, wherein the pressing and punching are performed with a carrier film attached.
12. 12. The method of claim 11, wherein the carrier film includes at least one of polyethylene terephthalate (PET), polyurethane (PU), polyethylene (PE), polyolefin (PO), polystyrene (PS), polyvinyl chloride (PVC), and polyvinydene chloride (PVDC).
13. The method for producing a multilayer electronic component according to claim 11, wherein the carrier film has a thickness of 1 mm or more and 50 mm or less.
14. The method for producing a multilayer electronic component according to claim 8 , wherein ends of the side margin portion in the first direction and the third direction are rounded.
15. The method for producing a multilayer electronic component according to claim 8 , wherein corners of the main body are rounded.