Manufacturing method of print circuit board and lamination body

The use of a laminate with polyimide resin and fumed metal oxide particles addresses adhesion and stability issues in forming fine circuit patterns, resulting in printed wiring boards with improved adhesion, low surface roughness, and heat resistance.

JP2024156378APending Publication Date: 2024-11-06KANEKA CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023070787
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-24
Publication Date
2024-11-06

AI Technical Summary

Technical Problem

Conventional methods for forming fine circuit patterns on printed wiring boards face challenges in achieving stable adhesion, low surface roughness, good etching properties, and excellent heat resistance, particularly in the formation of narrow pitch circuits.

Method used

A method involving a laminate with a layer containing polyimide resin and metal oxide particles is used, where the polyimide resin has a linear expansion coefficient of 30 ppm to 100 ppm and is non-soluble, and the metal oxide is fumed, to enhance adhesion and stability of the electroless copper plating layer.

Benefits of technology

The method enables the stable production of printed wiring boards with narrow pitch circuits that have low surface roughness, high adhesion, good etching properties, and excellent heat resistance, ensuring reliable circuit formation and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024156378000001_ABST
    Figure 2024156378000001_ABST
Patent Text Reader

Abstract

To provide a manufacturing method of a print circuit board, for stably manufacturing a narrow pitch circuit pattern having a low surface roughness, a high adhesiveness, an excellent etching property, and a heat resistance property, and provide a lamination body that is suitable for the same.SOLUTION: A manufacturing method of a print circuit board, using a lamination body L10 in which a layer A2 containing a polyimid resin and a metal oxide particle is directly formed on a copper foil 1, includes: a step (1) of performing heat crimping by causing a surface on the layer A side of the lamination body L to face a circuit formation surface of a circuit substrate B3 in which a circuit is formed, and laminating them in an order that a heat resistance adhesive material C4 is inserted therein, and obtaining a lamination body M20; a step (2) of removing the copper foil of the obtained lamination body M, and exposing the layer A; and a step (3) of forming an electroless copper plating layer D onto the exposed layer A. A linear expansion coefficient of a polyimide resin of the layer A is 30 ppm or more and 100 ppm or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a printed wiring board and a laminate. [Background technology]

[0002] Printed wiring boards, which have circuits made of metal conductors on an insulating substrate, are widely used as components that realize the functions of electronic devices, with various electronic components mounted on the printed wiring board. As electronic devices become more functional, more powerful, and more compact, printed wiring boards are required to have narrower pitches for circuit wiring. Printed wiring boards, such as HDI (High Density Interconnect) used in motherboards of mobile devices and semiconductor package boards that mount high-performance semiconductor bare chips, are particularly in need of narrower pitches, and instead of the conventional subtractive method, SAP (Semi Additive Process) and MSAP (Modified Semi Additive Process) methods are being adopted. These additive methods form a thin copper layer that serves as a power supply layer, a pattern is formed on the power supply layer using a photosensitive resist, and the openings of the resist pattern are pattern-plated using electrolytic copper plating, followed by seed etching to form a conductor pattern. Compared to the subtractive method, the MSAP method is more suitable for forming narrow-pitch circuits, but the copper foil with carrier used in the MSAP method is currently available in a grade with a thickness of about 3 microns, and a grade with a thickness of 1.5 microns has also been developed. However, since it is advantageous to have a thickness as thin as possible for forming narrow-pitch circuits, the SAP method, in which electroless copper plating is applied directly onto insulating resin, is more suitable for forming narrow-pitch circuits. Patent Documents 1 and 2 disclose the SAP method and materials that are the premise of it. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2019-108557 A [Patent Document 2] Republished patent WO2020 / 105289 Summary of the Invention [Problem to be solved by the invention]

[0004] However, as a result of intensive research, the present inventors have found that the above-mentioned conventional techniques have both advantages and disadvantages, and there is room for improvement or problems as described below.

[0005] In order to stably form a fine circuit pattern on the insulating resin layer, the higher the adhesion strength at the interface between the insulating resin layer and the electroless copper plating layer, the more preferable. Patent Documents 1 and 2 describe the adhesion strength at the interface between the insulating resin layer and the electroless copper plating layer, but further improvements are desired in order to stably form a fine circuit pattern on the insulating resin layer.

[0006] The present invention has been made in consideration of the above-mentioned problems, and an object of the present invention is to provide a method for producing a printed wiring board for stably producing a narrow-pitch circuit pattern having low surface roughness, high adhesion, good etching properties, and excellent heat resistance, and a laminate suitable for the method. [Means for solving the problem]

[0007] As a result of extensive investigations, the present inventors have found that the above problems can be overcome by the following configuration.

[0008] 1) A method for producing a printed wiring board using a laminate L in which a layer A containing a polyimide resin and metal oxide particles is formed directly on a copper foil, Step (1) A step of laminating the layer A side of the laminate L in the order of inserting a heat-resistant adhesive material C between the layer A side and the circuit-forming side of a circuit board B on which a circuit is formed, and then performing heat-pressure bonding to obtain a laminate M; Step (2) A step of removing the copper foil from the product obtained in step (1) to expose layer A. Step (3) A step of forming an electroless copper plating layer D on the layer A exposed in step (2). Including, 1. A method for producing a printed wiring board, wherein the linear expansion coefficient of the polyimide resin of layer A is 30 ppm or more and 100 ppm or less.

[0009] 2) The method for producing a printed wiring board according to 1), wherein the polyimide resin is a non-soluble polyimide resin.

[0010] 3) The method for producing a printed wiring board according to 1) or 2), wherein the metal oxide is a fumed metal oxide.

[0011] 4) A laminate (L) in which layer A containing polyimide resin and metal oxide particles is formed directly on copper foil.

[0012] 5) The laminate (L) according to 4), wherein the polyimide resin is a non-soluble polyimide resin.

[0013] 6) The laminate (L) according to 4) or 5), wherein the metal oxide is a fumed metal oxide. Effect of the Invention

[0014] According to the present invention, it is possible to provide a method for stably producing a printed wiring board having a narrow-pitch circuit pattern that has low surface roughness, high adhesion, good etching properties, and excellent heat resistance, and a laminate suitable for the manufacturing method. [Brief description of the drawings]

[0015] [Figure 1] FIG. 1 is a diagram illustrating step (1) of the present invention. [Diagram 2] FIG. 2 is a diagram showing steps (2) and (3) of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] <Laminated body (L)> A laminate (L) (sometimes referred to as laminate L) according to one embodiment of the present invention is characterized in that a layer A containing a polyimide resin and metal oxide particles is formed on a copper foil, and has a layer A / copper foil structure. With this structure, the layer A exposed by removing the copper foil during the manufacture of a printed wiring board has the advantages of low surface roughness, high adhesion to electroless copper plating, good etching properties, and excellent heat resistance.

[0017] The present invention relates to a method for producing a printed wiring board, and it is important that high adhesion is exhibited with the electroless copper plating layer formed on the surface of Layer A. The mechanism by which this adhesion is exhibited will be described.

[0018] The electroless copper plating process is composed of multiple independent chemical baths. These chemical baths are controlled under predetermined conditions (concentration, temperature, etc.), and the surface of the plated object is contacted with these chemicals for a predetermined time by methods such as immersion and showering, and the surface undergoes chemical changes and, in some cases, physical changes in shape. These chemicals contain various components, and the pH varies depending on the type of chemical, with some chemicals exhibiting strong alkalinity and strong acidity. On the other hand, the polyimide resin and metal oxide particles that constitute layer A, which are essential to one embodiment of the present invention, both interact with these chemicals, causing changes in their chemical structure and physical shape, which is thought to affect the improvement of adhesion with electroless copper plating. Both the polyimide resin and the metal oxide particles undergo chemical changes in an alkaline environment. For example, the metal oxide particles react in an alkaline environment to generate ionic functional groups on the solid surface of the metal oxide particles. In addition, the imide ring of the polyimide resin opens in an alkaline environment to generate ionic carboxyl groups. Layer A of the present invention contains a polyimide resin and metal oxide particles, and generates ionic functional groups in an alkaline environment.

[0019] These ionic functional groups formed on the surface of Layer A ionically bond with the copper ions in the electroless copper plating bath, and a copper-containing compound derived from the three components "metal oxide particles", "ionic copper", and "polyimide resin" is formed in a layer on the surface of Layer A, and an electroless copper plating layer D is formed and grows on the surface of the formed layer. The layer containing ionic copper, which is derived from the three components of "metal oxide particles," "copper ions," and "polyimide resin," is believed to be firmly adhered to Layer A through ionic bonds, and also to the electroless copper plating layer through metallic bonds between the ionic copper and metallic copper.

[0020] <Polyimide resin> Next, the polyimide resin used in layer A will be described. Since the laminate L of one embodiment of the present invention is used for a printed wiring board, it is preferable that the polyimide resin in layer A is resistant to the high temperature process temperature during the processing and the high temperature when components are mounted. Therefore, the polyimide resin used in layer A preferably has a high glass transition temperature and a high elastic modulus at high temperatures. These are preferable because the adhesion between layer A and the electroless copper plating layer at high temperatures can be maintained high, which makes it possible to withstand the high temperature process temperature and the component mounting process, which is preferable. There is no particular inconvenience in that these are too high. From the above perspective, it is preferable that the glass transition temperature of the heat-resistant resin, which is an index of heat resistance, is as high as possible, for example, preferably 180°C or higher, more preferably 210°C or higher, and particularly preferably 230°C or higher. In addition, in order to exhibit good solder heat resistance, it is preferable that the polyimide resin used in layer A has a certain elastic modulus or higher even near the melting point of the solder. Specifically, the polyimide resin contained in layer A has a storage elastic modulus of 0.02×10 at 300°C. 9 Pa or more, 0.05×10 9 Pa or more, and 0.08×10 9 Pa or more is more preferable, and 0.1×10 9 Pa or more is even more preferable.

[0021] Polyimide resin is characterized by the inclusion of imide groups in its chemical skeleton. It is believed that the imide groups (functional groups) in the polyimide resin, and the polyamic acid groups generated in an alkaline environment, bond with copper ions, improving adhesion to the electroless copper plating layer.

[0022] On the other hand, the present inventors, in the course of intensive investigation, independently found that the linear expansion coefficient of the polyimide resin used in layer A affects adhesion, specifically, good adhesion is exhibited when the linear expansion coefficient is 30 ppm / °C or more, and arrived at one embodiment of the present invention. In this specification, the linear expansion coefficient of the polyimide resin is the linear expansion coefficient in the plane direction when the polyimide resin used in layer A is formed into a film, and reflects the degree of in-plane orientation of the polyimide molecular chains in layer A. The smaller the linear expansion coefficient of the polyimide resin, the more the polyimide molecular chains are oriented in the plane direction, and conversely, the larger the linear expansion coefficient, the more the polyimide molecular chains are oriented in the thickness direction as well.

[0023] The linear expansion coefficient of polyimide resin can be controlled by the type of monomer used. In order to reduce the linear expansion coefficient of polyimide resin, it is effective to use a monomer having a rigid chemical structure and increase its composition ratio. By using a monomer having a rigid chemical structure and increasing its composition ratio, when processed (molded) into a film, the polyimide molecular chains are oriented in the plane direction, and further the molecular chains can be accumulated in the thickness direction.

[0024] As described above, the present inventors have independently found that when the linear expansion coefficient of the polyimide resin of layer A is too small, the adhesion between the resin film and the electroless copper plating layer decreases. The reason for this is speculated as follows. When a polyimide obtained from a monomer mixture in which a monomer having a rigid chemical structure is used and the composition ratio of the monomer is increased is exposed to an alkaline chemical solution, the polyimide molecules near the surface are modified to polyamic acid by the cleavage reaction of the imide ring, and a state in which polyamic acid molecules oriented in the plane direction are deposited in the thickness direction is formed. The cohesive force between polyamic acid molecular chains is weaker than the cohesive force between polyimide molecular chains. Therefore, when an electroless copper plating layer (film) is formed on the surface of a film obtained by exposing the polyimide to an alkaline chemical solution and the adhesion is evaluated, it is speculated that peeling occurs at the interface where the polyamic acid molecular chains with weak cohesive force are broken into layers, and as a result, the adhesion strength between the film and the plating layer (film) tends to be low. Note that the present invention is not limited to such a speculation.

[0025] Conversely, in order to increase the linear expansion coefficient of polyimide resin, it is effective to use a monomer having a flexible chemical structure and increase its composition ratio. By using a monomer having a flexible chemical structure and increasing its composition ratio, when molded into a film, the polyimide molecular chains tend to be oriented not only in the plane direction but also in the thickness direction, that is, to show a random orientation.

[0026] As described above, the present inventors have independently found that when the linear expansion coefficient of the polyimide resin of layer A is large (for example, 30 ppm / °C or more), the adhesion between the resin film and the electroless copper plating layer is enhanced. The reason for this is speculated as follows. When a polyimide obtained from a monomer mixture in which a monomer having a flexible chemical structure is used and the composition ratio of the monomer is increased is exposed to an alkaline chemical solution, the polyimide molecules near the surface are modified to polyamic acid by the cleavage reaction of the imide ring, but there are many covalent bonds of the polymer chains in the thickness direction, and therefore the cohesive force between the molecular chains remains high. Therefore, when an electroless copper plating film is formed on the surface of a film obtained by exposing the polyimide to an alkaline chemical solution and the adhesion is evaluated, it is speculated that the linear expansion coefficient of the polyimide resin is small as described above, and there is no peeling in layers between the polyamic acid molecular chains as in the case of a polyimide with advanced in-plane molecular orientation, and as a result, the adhesion strength with the electroless copper plating tends to be large. It is to be noted that the present invention is not limited to such a speculation.

[0027] In view of the above, from the viewpoint that the cohesive strength of the polyimide resin itself is not reduced even when the polyimide resin is exposed to an alkaline chemical solution, it is preferable that the polyimide resin used in Layer A is a polyimide resin that tends to be randomly oriented, that is, a polyimide resin that tends to be isotropically oriented, rather than a polyimide resin with advanced in-plane molecular orientation.

[0028] Regarding polyimide resin, there is a correlation between the degree of in-plane molecular orientation and the linear expansion coefficient. Regarding polyimide resin, when the in-plane molecular orientation is highly advanced, and as a result, the peel strength between the plane-oriented polymer chains is also weakened, the linear expansion coefficient is smaller than 30 ppm / °C. It is preferable that the polyimide resin used in layer A has a random orientation tendency, which is oriented not only in the plane direction but also in the thickness direction, and this also improves the adhesion with electroless copper plating. The linear expansion coefficient of the polyimide resin is 30 ppm / °C or more, preferably larger than 30 ppm / °C, more preferably 35 ppm / °C or more, even more preferably 40 ppm / °C or more, even more preferably 45 ppm / °C or more, and particularly preferably 50 ppm / °C or more. On the other hand, if the linear expansion coefficient is too high, it will have a negative effect on heat resistance, dimensional stability, etc., so the linear expansion coefficient is 100 ppm / °C or less, and preferably 80 ppm / °C or less.

[0029] <Polyimide resin formulation for layer A> Next, the monomer species and polymerization method used for the polyimide resin used in Layer A will be described. It is preferable that the physical properties of the polyimide resin, such as the glass transition temperature, storage modulus at high temperatures, and the ability to generate ionic functional groups in an alkaline chemical environment, are appropriately controlled. One method for controlling these physical properties within an appropriate range is to select the raw material monomers used. Raw material monomers for polyimide resins include monomers with flexible skeletons and monomers with rigid skeletons, and by appropriately selecting these and further adjusting the compounding ratio, it is possible to achieve the desired physical properties.

[0030] Diamines having a flexible skeleton include 4,4'-oxydianiline, 3,3'-oxydianiline, 3,4'-oxydianiline, bis{4-(4-aminophenoxy)phenyl}sulfone, 2,2'-bis{4-(4-aminophenoxy)phenyl}propane, bis{4-(3-aminophenoxy)phenyl}sulfone, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl ether, 4,4'-diaminodiphenyl Phenyl thioether, 3,4'-diaminodiphenyl thioether, 3,3'-diaminodiphenyl thioether, 4,4'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 3,3'-diaminodiphenylmethane, 4,4'-diaminodiphenylpropane, 3,4'-diaminodiphenylpropane, 3,3'-diaminodiphenylpropane, 4,4'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl Nilsulfone, 4,4'-diaminobenzophenone, 3,4'-diaminobenzophenone, 3,3'-diaminobenzophenone, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(3-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[4-(4-aminophenoxy)phenyl]sulfone, 2,2-bis[4- (3-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[3-(3-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 4,4'-bis(4-aminophenoxy)biphenyl, 4,4'-bis(3-aminophenoxy)biphenyl, and the like.

[0031] On the other hand, examples of diamines having a rigid skeleton include 1,4-diaminobenzene (p-phenylenediamine), 1,3-diaminobenzene, 1,2-diaminobenzene, benzidine, 3,3'-dichlorobenzidine, 3,3'-dimethylbenzidine, 2,2'-dimethylbenzidine, 3,3'-dimethoxybenzidine, 2,2'-dimethoxybenzidine, 3,3'-dihydroxy-4,4'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)benzidine, 1,5-diaminonaphthalene, 4,4'-diaminobenzanilide, 3,4'-diaminobenzanilide, and 3,3'-diaminobenzanilide.

[0032] Among these, from the viewpoints of control of thermal properties and industrial ease of availability, one or more selected from the group consisting of 4,4'-oxydianiline, 4,4'-diaminodiphenylpropane, 4,4'-diaminodiphenylmethane, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 3,3'-oxydianiline, 3,4'-oxydianiline, 1,3-bis(4-aminophenoxy)benzene, bis{4-(4-aminophenoxy)phenyl}sulfone, 2,2'-bis{4-(4-aminophenoxy)phenyl}propane, bis{4-(3-aminophenoxy)phenyl}sulfone, 1,3-bis(3-aminophenoxy)benzene, 3,3'-diaminobenzophenone, and 4,4'-diaminobenzophenone can be preferably used as the diamine having a flexible skeleton. In particular, one or more selected from the group consisting of 4,4'-oxydianiline, 1,3-bis(4-aminophenoxy)benzene, and 2,2'-bis{4-(4-aminophenoxy)phenyl}propane may be preferably used. As a diamine having a rigid skeleton, one or more selected from the group consisting of 1,4-diaminobenzene (p-phenylenediamine), 1,3-diaminobenzene, and 2,2'-dimethylbenzidine may be preferably used, since it exerts the effect of hardening the polymer chain with a relatively small amount and is easily available industrially. In particular, at least one of 1,4-diaminobenzene (p-phenylenediamine) and 2,2'-dimethylbenzidine may be preferably used. These diamines may be used alone or in combination of two or more.

[0033] Examples of tetracarboxylic dianhydrides having a flexible skeleton include 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,3,3',4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 3,4'-oxydiphthalic anhydride, 4,4'-oxydiphthalic anhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, 4,4'-(hexafluoroisopropylidene)phthalic anhydride, 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride, 2,2-bis(3,4-dicarboxyphenyl)propane, and 2,2-bis(3,4-dicarboxyphenyl)propane. Examples of suitable anhydrides include 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride, 1,1-bis(3,4-dicarboxyphenyl)ethane dianhydride, bis(2,3-dicarboxyphenyl)methane dianhydride, bis(3,4-dicarboxyphenyl)ethane dianhydride, bis(3,4-dicarboxyphenyl)sulfone dianhydride, p-phenylene bis(trimellitic acid monoester anhydride), ethylene bis(trimellitic acid monoester anhydride), and bisphenol A bis(trimellitic acid monoester anhydride).

[0034] On the other hand, examples of tetracarboxylic dianhydrides having a rigid skeleton include pyromellitic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, and 3,4,9,10-perylenetetracarboxylic dianhydride.

[0035] Among these, from the viewpoints of control of thermal properties and industrial availability, one or more selected from the group consisting of 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,3,3',4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, and 4,4'-oxydiphthalic anhydride may be preferably used as the tetracarboxylic dianhydride having a flexible skeleton. Among these, 3,3',4,4'-biphenyltetracarboxylic dianhydride is more preferable, and can be effectively used to achieve a good balance of various physical properties desired in a preferred embodiment of the present invention, i.e., adhesion to electroless plating film, elastic modulus at high temperatures, glass transition temperature, linear expansion coefficient of polyimide resin, etc.

[0036] As the tetracarboxylic dianhydride having a rigid skeleton, pyromellitic dianhydride is preferably used because it exerts the effect of hardening the polymer chain with a relatively small amount and is easily available industrially. Two or more of these tetracarboxylic dianhydrides may be mixed and used.

[0037] There are many unclear points regarding the relationship between adhesion and the chemical structure of the polyimide resin of layer A in one embodiment of the present invention, and a clear explanation is difficult. Empirically obtained during the course of the inventors' intensive research, it has been found that the use of a combination of acid dianhydrides and diamines that reduce the polarization of the imide ring of the polyimide resin tends to show good adhesion. Specifically, a combination of at least one of 4,4'-oxydiphthalic dianhydride and 3,3',4,4'-biphenyltetracarboxylic dianhydride as the acid dianhydride and 2,2'-bis(trifluoromethyl)benzidine as the diamine is effective. The combination of the preferred diamine and acid dianhydride is not particularly limited. It is preferable to select a combination of at least one selected from the group consisting of 2,2'-bis(trifluoromethyl)benzidine, 4,4'-oxydianiline, 1,3-bis(4-aminophenoxy)benzene, 2,2'-bis{4-(4-aminophenoxy)phenyl}propane, and 2,2'-dimethylbenzidine as the diamine, and at least one of 4,4'-oxydiphthalic dianhydride and 3,3',4,4'-biphenyltetracarboxylic dianhydride as the acid dianhydride, and further combine metal oxide particles with an appropriate type and amount. This configuration (combination) can improve the adhesion with the electroless copper plating layer of one embodiment of the present invention, and in particular, can greatly improve the initial state after the formation of the electroless copper plating layer, which is preferable. In addition, in order to achieve a good balance between the elastic modulus at high temperatures, the glass transition temperature, and the linear expansion coefficient, it is also preferable to use other diamines and acid dianhydrides in combination with the above-mentioned preferable diamines and acid dianhydrides.

[0038] The polyamic acid, which is a precursor of the polyimide of the layer A, is obtained by mixing the diamine and the acid dianhydride in an organic solvent so that they are substantially equimolar or approximately equimolar, and reacting them. Any organic solvent can be used as long as it can dissolve the polyamic acid. As the organic solvent, amide-based solvents, i.e., N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, etc. are preferred, and at least one of N,N-dimethylformamide and N,N-dimethylacetamide can be particularly preferably used. The solid content concentration of the polyamic acid is not particularly limited, and if it is within the range of 5% by weight to 35% by weight, a polyamic acid having sufficient mechanical strength when made into a polyimide can be obtained.

[0039] The order of addition of the diamine and the acid dianhydride raw materials is not particularly limited. By controlling not only the chemical structures of the diamine and the acid dianhydride raw materials but also the order of addition of these raw materials, it is possible to control the properties of the resulting polyimide.

[0040] In addition, when 1,4-diaminobenzene and pyromellitic dianhydride are used as raw materials, a polyimide structure obtained by binding the two has low durability against a desmear solution, so it is preferable to adjust the order of addition of 1,4-diaminobenzene and pyromellitic dianhydride so as not to form a structure in which the two are directly bound to each other.

[0041] Layer A may contain a resin other than the above-mentioned polyimide resin as a resin component. The content ratio of polyimide resin in the resin component contained in layer A is preferably high. For example, in 100% by weight of the resin component contained in layer A, the polyimide resin is preferably 50% by weight or more, more preferably 60% by weight or more, more preferably 70% by weight or more, more preferably 80% by weight or more, even more preferably 90% by weight or more, and particularly preferably 95% by weight or more. In 100% by weight of the resin component contained in layer A, the polyimide resin is most preferably 100% by weight, in other words, layer A most preferably contains only polyimide resin as a resin component.

[0042] <Solubility of polyimide resin in layer A> It is possible to manufacture the laminate L of one embodiment of the present invention by using a soluble polyimide soluble in an organic solvent as the polyimide resin of layer A. Specifically, a soluble polyimide is dissolved in an organic solvent, and a fumed metal oxide is further dispersed in the obtained solution, and the obtained dispersion is applied to a copper foil, and then layer A is dried to obtain the laminate L of one embodiment of the present invention. However, it is preferable that the polyimide resin used in layer A is insoluble so that problems such as resin dissolution do not occur in the process in which an organic solvent is used in the manufacturing process and mounting process of the printed wiring board obtained by the present invention. Insoluble means that the polyimide resin has a solubility of less than 1% by weight in amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone.

[0043] As described above, the present invention can be achieved whether the solvent for the polyimide resin used in Layer A is soluble or non-soluble, but is preferably non-soluble. In this case, the laminate L of the present invention can be obtained by applying the polyimide resin in a precursor state to copper foil, drying, and imidizing it. This makes it possible to obtain the laminate L having excellent durability against solvents, and further a printed wiring board using the laminate L, which is preferably carried out.

[0044] Here, insolubility will be described. In general, it means that the substance is not dissolved in organic solvents used in industrial applications. Specifically, it is preferable that the substance is not dissolved in 10% by weight or more, and more preferably, it is not dissolved in 5% by weight or more. The types of organic solvents include, but are not limited to, alcohol-based solvents such as methanol, ethanol, and propanol; ketone-based solvents such as acetone and methyl ethyl ketone; aromatic solvents such as toluene, xylene, cresol, and benzene; ether-based solvents such as dioxolane, dioxane, tetrahydrofuran, and diethyl ether; and aprotic polar solvents such as N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethylsulfoxide, and acetonitrile.

[0045] [Metal oxide particles] <Metal oxide particles in layer A> The metal oxide particles of the present invention are metal oxide particles mainly composed of silica, alumina, titania, copper, iron, zirconia, magnesium, barium, etc. As these metal oxide particles, spherical or amorphous metal oxide particles in which primary particles exist independently, and fumed metal oxide particles in which structures formed by agglomeration of primary particles form structural units can be used.

[0046] The metal oxide particles of layer A constitute layer A together with the polyimide resin, and in order for layer A to adhere firmly to the electroless copper plating layer, it is preferable that the metal oxide particles adhere firmly to the polyimide resin and that the number of functional groups generated by the metal oxide particles in an alkaline environment is large. To meet this requirement, it is preferable that the metal oxide particles have a structurally complex shape, which increases the interaction with the heat-resistant resin and enables strong adhesion to the heat-resistant resin, and also increases the specific surface area, thereby increasing the number of functional groups generated. Fumed metal oxides meet these requirements and can be used preferably.

[0047] The fumed metal oxide used in one embodiment of the present invention is preferably a metal oxide particle obtained by gas phase synthesis. When obtained by gas phase synthesis, the fumed metal oxide obtained has a feature that the structural unit is a structure in which primary particles are aggregated due to the characteristics of the manufacturing method. In other words, the fumed metal oxide preferably has a structural unit in which primary particles are aggregated (for example, has an aggregate structure like a bunch of grapes). The fumed metal oxide is mixed with a polyimide resin to form layer A in one embodiment of the present invention. As a result of various studies by the present inventors, it is preferable that layer A is in a state in which (i) the structural unit of the fumed metal oxide is embedded in the polyimide resin with low voids, (ii) the structural unit is present on the surface and / or near the surface of layer A in the bulk direction, and (iii) the structural unit is evenly present and dispersed in layer A, and it is believed that such a state is effective for developing adhesion, which is the object of one embodiment of the present invention.

[0048] In the blending of polyimide resin and fumed metal oxide, the porosity in layer A tends to increase when the blending ratio of fumed metal oxide is increased. When the porosity in layer A is not too high, the binding strength between polyimide resin and fumed metal oxide does not decrease, and the strength of layer A itself tends to be good, and as a result, the adhesion to electroless copper plating tends to be good. Therefore, in the blending of polyimide resin and fumed metal oxide, it is preferable that the blending ratio of fumed metal oxide is not too high. Conversely, in the blending of polyimide resin and fumed metal oxide, when the blending ratio of fumed metal oxide is low, the porosity tends to be low. When the porosity in layer A is not too low, it is preferable because sufficient adhesion to electroless copper plating is easily exhibited. It is believed that the reason for this is that the ratio of fumed metal oxide is not too low, and the amount of compounds derived from the three components of "fumed metal oxide"-"copper ion"-"polyimide resin" is sufficient. However, the present invention is not limited to such a speculation.

[0049] From the above, in order to realize good adhesion, it is preferable to control the compounding ratio of polyimide resin to fumed metal oxide within an appropriate range. On the other hand, there are various grades of fumed metal oxides that differ in primary particle size, structure of the structure formed by aggregation of primary particles, and surface treatment type, and it is believed that there is an appropriate compounding ratio that is influenced by these factors.

[0050] <Primary particle size and specific surface area of ​​fumed metal oxides> Although the fumed metal oxide near the surface is partially dissolved by the chemical solution of the electroless copper plating process, it is preferable that the surface roughness of layer A does not become too large even if it is dissolved. For this reason, it is preferable that the primary particle size of the fumed metal oxide is small, specifically, preferably 5 nanometers to 1,000 nanometers, more preferably 5 nanometers to 100 nanometers, even more preferably 5 nanometers to 50 nanometers, and even more preferably 10 nanometers to 20 nanometers. In addition, the specific surface area of ​​the fumed metal oxide is also a physical property value that expresses the primary particle size, and the larger the primary particle size, the smaller the specific surface area. The specific surface area of ​​the fumed metal oxide is preferably 30 square meters / gram to 400 square meters / gram, more preferably 100 square meters / gram to 250 square meters / gram.

[0051] <Apparent density of fumed metal oxides> Fumed metal oxides are structures in which the primary particle size is aggregated, and the apparent density can be used as an index of the state of the structure of the fumed metal oxide. If the apparent density of the fumed metal oxide is low, the fumed metal oxide structure has a bulky structure and has large voids. Conversely, if the apparent density of the fumed metal oxide is high, the fumed metal oxide structure has a less bulky structure and has small voids.

[0052] By filling the voids in the structure formed by agglomeration of the primary particle diameter of the fumed metal oxide with a heat-resistant resin component, a layer A having a low porosity can be produced. The smaller the apparent density of the fumed metal oxide, the more voids there are in the fumed metal oxide structure, and the more polyimide resin component can be used to fill the voids. The larger the apparent density of the fumed metal oxide, the more the heat-resistant resin component can fill the voids in the fumed metal oxide structure. In other words, when a certain amount of polyimide resin is mixed with a fumed metal oxide to produce a layer A having a low porosity, (i) in the case of a fumed metal oxide having a small apparent density, the upper limit of the amount of the fumed metal oxide to be mixed is low, and conversely, (ii) in the case of a fumed metal oxide having a large apparent density, a large amount of the fumed metal oxide can be mixed, that is, the upper limit of the amount of the fumed metal oxide to be mixed is high. As mentioned above, if the amount of fumed metal oxide is not too large, there is no risk of excessive voids occurring in layer A. As a result, the binding strength between the polyimide resin and the fumed metal oxide is not reduced, and the strength of layer A itself tends to be good, and as a result, the adhesion to electroless copper plating also tends to be good, and the adhesion between layer A and the electroless copper plating layer also tends to be good. Therefore, in the blending of the polyimide resin and the fumed metal oxide, it is preferable that the blending ratio of the fumed metal oxide is not too high. Conversely, if the ratio of the fumed metal oxide is not too low, sufficient adhesion to electroless copper plating is easily achieved. In other words, in the blending of the polyimide resin and the fumed metal oxide, blending the fumed metal oxide near the upper limit of the blending amount is effective in achieving good adhesion.

[0053] The upper limit of the amount of fumed metal oxide to be mixed with a certain amount of polyimide resin to produce a layer A with a small porosity varies depending on the apparent specific gravity of the fumed metal oxide and the type of surface treatment. In other words, the adhesion can be further improved by adjusting the amount of fumed metal oxide to be mixed with a certain amount of polyimide resin according to the apparent specific gravity and the type of surface treatment of the fumed metal oxide. In one embodiment of the present invention, the apparent specific gravity of the fumed metal oxide is preferably 20 g / L or more and 250 g / L or less, and more preferably 20 g / L or more and 220 g / L or less. In addition, the higher the apparent specific gravity of the fumed metal oxide, the higher the upper limit of the amount of fumed metal oxide to be mixed with, and the adhesion tends to be further improved. For this reason, the apparent specific gravity of the fumed metal oxide is preferably greater than 50 g / L and equal to or less than 250 g / L, more preferably between 60 g / L and 250 g / L, even more preferably between 70 g / L and 250 g / L, and even more preferably between 70 g / L and 220 g / L. The apparent specific gravity of the fumed metal oxide can also be changed by modifying the structure of the fumed metal oxide by mechanically applying a stress such as shear to the fumed metal oxide.

[0054] Various surface treatments can be performed on the fumed metal oxide. The surface state of the fumed metal oxide can be silanol (untreated), dimethylsilyl, octylsilyl, trimethylsilyl, dimethylsiloxane, dimethylpolysiloxane, aminoalkylsilyl, methacrylsilyl, etc., and all of them are industrially available. When the polarity of the surface treatment type of the fumed metal oxide is similar to that of the polyimide resin component, the upper limit of the amount of the fumed metal oxide to be mixed tends to be high. In addition, when the surface of the fumed metal oxide is untreated, the wettability with the alkaline chemical solution during the electroless copper plating process is too good, so the amount of the fumed metal oxide dissolved tends to increase, and the surface roughness of the layer A tends to increase. Therefore, it is preferable that the surface of the fumed metal oxide is subjected to an appropriate hydrophobic treatment. The apparent specific gravity of the fumed metal oxide can be measured according to ISO787 / XI.

[0055] <Specific examples of fumed metal oxides> The following describes fumed metal oxides that can be preferably used in one embodiment of the present invention. Specific examples are shown below, but are not limited to these. Fumed metal oxides that satisfy the requirements of various properties including apparent density can be more suitably used in one embodiment of the present invention. Fumed metal oxides of various grades with different primary particle size, specific surface area, surface treatment type, apparent density, and metal oxide type are available from Nippon Aerosil Co., Ltd., Wacker Asahi Kasei Silicone Co., Ltd., and Cabot Corporation, and can be preferably used. The following is a specific explanation using the fumed metal oxides of Nippon Aerosil Co., Ltd. as an example. Aerosil R972, R972CF, R972V, etc., which are approximately the same except for the apparent density, can be preferably used, and among these, R972 (50 grams / liter) with a high apparent density can be more preferably used. Similarly, Aerosil R974, R9200, VP RS920, etc., which are equivalent except for the apparent density, can be preferably used, and among these, Aerosil R9200 (200 g / L) and Aerosil VP RS920 (80 g / L to 120 g / L), which have a high apparent density, can be more preferably used. In addition to these, Aerosil NX130, RY200S, R976, NAX50, NX90G, NX90S, RX200, RX300, R812, R812S, etc. can be preferably used as fumed metal oxides manufactured by Nippon Aerosil Co., Ltd., which have a relatively low apparent density of 70 g / L or less, which is one of the preferred physical properties of one embodiment of the present invention. In addition, as fumed metal oxides manufactured by Nippon Aerosil Co., Ltd. having a relatively high apparent specific gravity of 70 grams / liter or more, Aerosil 200V, AEROIDE TiO2 P90, AEROIDE TiO2 NKT90, OX50, RY50, RY51, AEROIDE TiO2 P25, R8200, RM50, RX50, AEROIDE TiO2 T805, R7200, etc. can also be preferably used. In addition, Aerosil VP RS920 has been sold under the name "Aerosil E9200" since November 2021.

[0056] In addition, "Aerosil" or "AEROSIL" is a registered trademark of Evonik Operations GmbH. In addition, as the fumed metal oxide, a fumed metal oxide that is synthesized by gas phase synthesis and thus has a structure in which the primary particle size is aggregated can be preferably used.

[0057] Among these fumed metal oxides, fumed silica such as Aerosil R972, 972V, NX130, R9200, VP RS920, R974, R976, and R8200 are preferred in that the surface shape of layer A formed by dissolution in an alkaline environment is good and the surface roughness is within an appropriate range.

[0058] In addition to the fumed metal compounds, spherical or amorphous metal oxide particles can also be used. Specific examples of the particles that can be preferably used include the Admanano, Admafine, and Admafuse products manufactured by Admatechs Co., Ltd.

[0059] <Parts of metal oxide particles> The number of parts of the metal oxide particles is preferably 10 parts by weight or more and 130 parts by weight or less relative to 100 parts by weight of the heat-resistant resin of Layer A. When the metal oxide particles are fumed metal oxide, as described above, the preferred number of parts of the fumed metal oxide relative to the heat-resistant resin of Layer A can be adjusted to some extent depending on the apparent specific gravity of the fumed metal oxide, but due to the influence of the surface treatment of the fumed metal oxide, etc., it is not possible to state anything definite. Here, the preferred number of parts of the fumed metal oxide is described as an index.

[0060] When the apparent specific gravity of the fumed metal oxide is from 20 to 70 g / L, the amount of the fumed metal oxide is preferably from 15 to 80 parts by weight, and more preferably from 20 to 60 parts by weight, relative to 100 parts by weight of the heat-resistant resin.When the apparent specific gravity of the fumed metal oxide is from 70 to 250 g / L, the amount of the fumed metal oxide is preferably from 10 to 130 parts by weight, and more preferably from 15 to 120 parts by weight, even more preferably from 20 to 100 parts by weight, and particularly preferably from 30 to 90 parts by weight.

[0061] As mentioned above, the preferred number of parts varies depending on the apparent specific gravity of the fumed metal oxide, and the larger the apparent specific gravity of the fumed metal oxide, the more the amount of the fumed metal oxide can be increased, and the preferred amount tends to be increased. By mixing the fumed metal oxide in the above range with 100 parts by weight of the polyimide resin precursor, it is possible to achieve better adhesion strength, and in particular to achieve stronger adhesion in the initial state after the formation of the electroless copper plating film. It is also possible to mix (combine) multiple types of fumed metal oxides with different primary particle sizes, specific surface areas, surface treatment types, apparent specific gravity, metal oxide types, etc.

[0062] <Method of mixing polyimide resin and metal oxide particles, and method of producing layer A> As a method for producing the layer A, an appropriate method can be selected depending on the characteristics of the polyimide resin. i) When the polyimide resin of Layer A is soluble in a solvent, metal oxide particles are dispersed in an organic solvent, and the dispersion is added to a solution of a polyimide resin to obtain a Layer A dispersion, and then the Layer A dispersion is applied onto a copper foil and dried to obtain a laminate L consisting of Layer A and a copper foil; ii) A method in which a solution of polyamic acid, which is a precursor of the polyimide resin of Layer A, is mixed and dispersed with metal oxide particles, and then coated on a copper foil and heated to imidize the polyamic acid into a polyimide resin, thereby obtaining a laminate L consisting of Layer A and copper foil; iii) When the polyimide resin exhibits thermoplasticity, metal oxide particles are kneaded at a temperature equal to or higher than the melting point of the heat-resistant resin to obtain a resin bulk for layer A, which is then molded into a film shape while applying heat and pressure or by using a melt extruder to form layer A on copper foil, thereby obtaining a laminate L consisting of layer A and copper foil. Among these methods, method ii) is preferably implemented because a non-soluble polyimide resin can be used.

[0063] In order to achieve high adhesion strength, it is preferable that the metal oxide particles are uniformly dispersed. In particular, when fumed metal oxide is used as the metal oxide particles, it is preferable to disperse the particles down to the structural unit of the structure in which the primary particles are aggregated, and it is preferable to select an appropriate method in accordance with the type and properties of the heat-resistant resin and metal oxide particles used.

[0064] In the case of method i), the dispersion method may be a disperser, a homogenizer, a planetary mixer, a bead mill, a rotation / revolution mixer, a roll, a kneader, a high-pressure disperser, an ultrasonic wave, a resolver, a liquid-liquid shear type disperser Clearmix, etc. In the case of method iii), devices such as a screw extruder and a melt kneader may be used.

[0065] As long as the effect of one embodiment of the present invention can be obtained, the fumed metal oxide does not have to be dispersed to the structural unit. If the fumed metal oxide can be dispersed to the structural unit, the fumed metal oxide will not be present in the layer A in a solid form, and in that case, the surface roughness of the layer A is small, which is advantageous for the fine wiring formation, which is the aim of one embodiment of the present invention, and is preferable. It is also possible to disperse and grind the fumed metal oxide under conditions that make the structural unit of the fumed metal oxide even smaller. The organic solvent can be a solvent used for polymerization of polyamic acid, and amide-based solvents, i.e., N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, etc., can be preferably used, but are not limited thereto.

[0066] The laminate L according to one embodiment of the present invention is characterized in that a layer A containing a polyimide resin and metal oxide particles is formed on a copper foil. The laminate L according to the present invention can be obtained by applying and heating a solution containing a polyimide resin and metal oxide particles constituting the layer A or a solution containing a polyamic acid and metal oxide particles, which are precursors of the polyimide resin constituting the layer A, on a copper foil. When the solution to be applied is a solution containing a polyamic acid and metal oxide particles, it is also possible to preferably imidize the polyamic acid into a polyimide resin, and it is preferable to heat at an appropriate temperature and time to promote the imidization reaction. That is, the temperature is preferably in the range of 200°C to 450°C, and the time is preferably in the range of 1 second to 10 minutes. When the solution to be applied is a solution containing a polyimide and metal oxide particles, there is no particular limitation on the temperature and time as long as the solvent can be dried, and they can be appropriately set according to the type of solvent and drying equipment.

[0067] The thickness of layer A is not particularly limited, and the effects of the present invention are exhibited regardless of the thickness. In view of the recent demand for thinner printed wiring boards, the thickness is preferably 10 microns or less, more preferably 5 microns or less, and even more preferably 2 microns or less. In addition, for industrially stable production, the thickness is preferably 0.1 microns or more, more preferably 0.5 microns or more, and even more preferably 1 micron or more.

[0068] The laminate L according to one embodiment of the present invention is characterized in that a layer A containing a polyimide resin and metal oxide particles is formed on a copper foil. The copper foil is not particularly limited, and industrially available electrolytic copper foil and rolled copper foil can be used. In order to form fine wiring, it is preferable that the surface roughness of the surface of the copper foil on which the layer A is formed is as small as possible, and the surface roughness Ra is preferably 400 microns or less, more preferably 200 microns or less, and particularly preferably 100 microns or less. The thickness of the copper foil is also not particularly limited, but from the viewpoint of performing the step of removing the copper foil with good productivity in the method for producing printed wiring of the present invention and industrial availability, it is preferably about 18 microns or less, and a copper foil with a thickness of 9 microns can also be preferably used. In addition, from the viewpoint that the handleability is deteriorated if the copper foil thickness is too thin, it is preferably 5 microns or more. When a copper foil thinner than 5 microns is used for the laminate L of the present invention, a copper foil with a carrier can also be preferably used, and in this case, an ultra-thin copper foil with a thickness of 3 microns or less can be used. It is also possible and preferable to laminate a protective film onto the surface of Layer A of the laminate L according to one embodiment of the present invention.

[0069] <Manufacturing method for printed wiring boards> The method for producing a printed wiring board of the present invention is a method for producing a printed wiring board using a laminate in which a layer A containing a polyimide resin and metal oxide particles is formed directly on a copper foil, Step (1): A step of placing the surface of the layer A side of the laminate L opposite to the circuit formation surface of a circuit board B on which a circuit is formed, laminating them in the order in which the heat-resistant adhesive material C is inserted between them, and heat-pressing them (a step of producing a laminate M); Step (2): A step of removing the copper foil from the product (laminate M) obtained in step (1) to expose layer A (a step of producing laminate M'). Step (3): A step of forming an electroless copper plating layer D on the layer A exposed in step (2) (a step of producing a laminate N), wherein the linear expansion coefficient of the polyimide resin of layer A is 30 ppm or more and 100 ppm or less.

[0070] The circuit board B on which the circuit is formed can be exemplified by a rigid circuit board in which a circuit made of copper is formed on the surface of an insulating substrate made of a glass substrate and a heat-resistant resin, or a flexible circuit board in which a circuit made of copper is formed on the surface of a heat-resistant insulating substrate such as a polyimide film or a liquid crystal polymer film. The circuit-forming surface of the circuit board B and the layer A-forming surface of the laminate L according to the present invention are opposed to each other, and the heat-resistant adhesive material C is inserted between them in the order of lamination and heat-pressure bonding. The heat-resistant adhesive material C needs to embed the circuit of the circuit board B without any gaps and to adhere well to the circuit board B and the layer A according to the present invention, and there is no particular restriction as long as this is satisfied. For example, glass cloth-epoxy resin prepreg and bonding sheet can be exemplified, and are preferably usable. In addition, it is preferable to select the heat-pressure bonding conditions according to the characteristics of the heat-resistant adhesive material C. It is preferable to laminate using a heat-pressure bonding device such as a heat press device, a vacuum heat press device, or a vacuum laminator. In addition, when the heat-resistant adhesive material C exhibits thermosetting properties, the curing reaction can be progressed by a method of performing heat pressing with a device such as the above-mentioned heat press device, vacuum heat press device, or vacuum laminator, maintaining the state and performing a heat curing reaction, or a method of performing heat pressing with a device such as a heat press, vacuum heat press, or vacuum laminator, embedding the circuit of the circuit board B, i.e., a temporary pressure-bonded state, and then releasing the heat pressing and performing a heat curing reaction in another heating furnace or another heat pressing device. When a heat press device or a vacuum heat press device is used, it is possible to insert multiple objects to be laminated (works) between the hot plates of the press device, and it is possible to laminate and heat press multiple workpieces at the same time. Therefore, even if the heat curing reaction takes a long time, lamination and heat pressing can be performed with good productivity. On the other hand, when a vacuum laminator is used, since the vacuum laminator can only laminate one set of laminated objects, it is preferable to perform lamination and temporary pressure bonding in a relatively short time, and perform the heat curing reaction in another heating furnace or another heat pressing device.

[0071] The method for removing the copper foil from the product (laminate M) obtained in step (1) can be preferably performed by etching. Copper chloride solution, ferric chloride solution, alkaline etching, and acid / hydrogen peroxide (hydrogen peroxide) etching can be preferably used, and by removing the copper foil with these etching solutions, the layer A according to the present invention can be exposed (laminate M': step (2)).

[0072] As shown in FIG. 2, if necessary, between steps (2) and (3), a via hole (VIA) or through hole (hole formation) may be formed (hole formation) using a laser processing device, mechanical drill, plasma etching, or the like, and then step (3) may be performed to ensure electrical conductivity between the layers.

[0073] Next, an electroless copper plating layer D is formed on the surface of the exposed layer A to produce a laminate N. The electroless copper plating of one embodiment of the present invention can preferably be applied to reduction-type electroless plating using a chemical reaction. The electroless copper plating process, which is widely used for printed wiring boards, can utilize the chemical processes of various plating chemical manufacturers. In addition, desmearing is also generally performed before electroless copper plating. The desmearing is originally performed for the purpose of removing smears generated on the copper surface generated in the through-hole formation process and the laser via formation process. The desmearing also gives a chemical change to the surface of the resin film of one embodiment of the present invention, and is preferably usable. The desmearing process and the electroless copper plating process are each performed by treating the plated object with multiple chemicals in sequence. For example, the desmearing process is composed of a chemical solution responsible for swelling, a chemical solution responsible for etching, and a chemical solution responsible for reduction. The electroless copper plating process is composed of chemical solutions each playing a series of roles, such as a chemical solution responsible for cleaning and conditioning, a chemical solution responsible for soft etching, a chemical solution responsible for pre-dip, a chemical solution responsible for catalyst application, a chemical solution responsible for activation, and a chemical solution responsible for electroless copper plating. As a series of these processes, chemical processes of various plating chemical manufacturers can be used. For example, chemicals manufactured by Atotech, Adcopper IW manufactured by Okuno Chemical Industries Co., Ltd., Sulcup PEA manufactured by Uemura Kogyo Co., Ltd., chemicals manufactured by Rohm and Haas Electronic Materials Co., Ltd., chemicals manufactured by Meltex Inc., and other chemicals and processes can be applied, and they can also be appropriately combined. Although a small amount of nickel component may be added to these electroless copper platings, these electroless copper platings can be used within a range that does not impair the effects of one embodiment of the present invention. When electroless plating is performed on layer A, electroless plating may be performed directly on layer A, or pretreatment such as alkali treatment and desmear treatment may be performed on layer A as a pretreatment, and then electroless plating may be performed on layer A after the pretreatment. Examples of the alkaline aqueous solution for the alkaline treatment include an aqueous sodium hydroxide solution and an aqueous potassium hydroxide solution.

[0074] <Electroless copper plating layer D (layer D)> In the present invention, an electroless copper plating layer D is formed on the surface of layer A. The electroless copper plating layer (film) obtained by electroless copper plating can be thinner than a general copper foil. The thickness of the electroless copper plating layer is preferably 0.01 microns to 10.00 microns, more preferably 0.05 microns to 2.00 microns, and even more preferably 0.10 microns to 1.00 microns. When manufacturing a printed wiring board, via holes or through holes are formed (hole formation) to ensure electrical continuity in the thickness direction, and a desmearing process is performed to remove smears from within the holes. The hole formation and desmearing process in the manufacturing method of the present invention can be performed using the following three types of methods (X, Y, and Z). (X); step (1), hole formation, desmear treatment, step (2), step (3) (Y); step (1), step (2), hole formation, desmear treatment, step (3) (Z); step (1), hole formation, step (2), desmear treatment, step (3) In all of the methods, the desmear treatment is performed after the hole formation, and the smear in the hole can be removed. (X) is a method in which the process (2) is performed after the desmear treatment, that is, the copper foil is not removed during the desmear treatment, that is, the layer A is not exposed and the desmear treatment is not performed. In this case, since the functional group generation in the alkaline environment of the layer A described in (Mechanism of adhesion development) does not occur, the adhesion to the electroless copper plating tends to be inferior, but the change in the surface shape due to the desmear treatment is small and the surface roughness tends to be small, which tends to be advantageous for the formation of fine wiring. In addition, (Y) and (Z) are methods in which the desmear treatment is performed after the process (2), that is, the copper foil is removed during the desmear treatment, the layer A is exposed, and the desmear treatment is performed. In this case, the functional group generation in the alkaline environment of the layer A occurs, and the adhesion to the electroless copper plating tends to be excellent, but the change in the surface shape due to the desmear treatment tends to be larger than that of (X). In the present invention, it is preferable to select any one of the methods (X), (Y) and (Z) appropriately depending on the width of the circuit and the adhesive strength. For forming the holes, a laser processing device, a mechanical drill, plasma etching, or the like can be preferably used.

[0075] In step (3), an electroless copper plating layer is formed on the surface of layer A, and the subtractive method and additive method can be preferably used for the subsequent circuit formation. In particular, when the additive method is used, narrow-pitch circuit formation is possible and can be preferably performed. Furthermore, multi-layering treatment, protective film formation treatment, surface treatment, etc. can be preferably performed by known methods.

[0076] In order to form a narrow-pitch circuit, the surface roughness of the layer A in one embodiment of the present invention is preferably small. In one embodiment of the present invention, the surface roughness Ra of the layer A exposed by removing the electroless copper plating layer D by etching is preferably 200 nanometers or less, more preferably 150 nanometers or less, and even more preferably 100 nanometers or less. The surface roughness can be adjusted by changing the number of metal oxide particles added to the polyimide precursor, the type of metal oxide particles (apparent specific gravity, surface treatment, etc.), the chemical structure of the polyimide resin of the layer A, the desmear conditions, the conditions of the electroless copper plating layer formation treatment, etc.

[0077] In addition, in the present invention, since the electroless copper plating layer (layer D) is formed directly on the surface of the insulating layer, layer A, without the intervention of a metal layer such as nickel or chromium, there is no need to use a special etching solution for dissolving and removing metal components such as nickel and chromium, and a circuit can be formed and a printed wiring board can be manufactured by using a general etching solution for dissolving and removing copper, and the etching property is good. The general etching solution refers to an etching solution that is widely used in printed wiring board applications and is mainly used to etch copper, and specific examples of such etching solutions include iron (ferric chloride), cupric chloride (ferric chloride), alkaline ammonia (alkaline ammonia), sulfuric acid hydrogen peroxide (sulfuric acid + hydrogen peroxide) etching solution, ammonium persulfate, sulfuric acid (chromic acid etching solution), and potassium persulfate. Furthermore, since it is possible to set the surface roughness Ra to a relatively small value of 200 nanometers or less, layer D on layer A also does not have a complex uneven shape, and when removing layer D with an etching solution, it is not necessary to make the etching conditions stronger than necessary (prolonging the etching time, increasing the etching rate by increasing the temperature, increasing the etching rate by adjusting the concentration of the chemical solution, etc.).Therefore, the metallized resin film of the present invention has good etching properties. In addition, from the viewpoint of reliability required for printed wiring board applications and from the viewpoint of forming fine wiring without circuit peeling, it is preferable that the peel strength is as high as possible. Specifically, it is preferably 4 N / cm or more, more preferably 6 N / cm or more, and even more preferably 9 N / cm or more. EXAMPLES

[0078] Hereinafter, one embodiment of the present invention will be described in more detail with reference to examples and comparative examples. However, the present invention is not limited to the following examples.

[0079] <Preparation of a single layer film of polyimide resin for Layer A> The polyamic acid solution obtained in the synthesis example was applied to an aluminum foil, and the polyamic acid solution was heated at 120°C for 360 seconds, 200°C for 60 seconds, 350°C for 200 seconds, and 450°C for 30 seconds in sequence to carry out imidization. The aluminum foil was then dissolved and removed using an etching solution to obtain a monolayer film of polyimide resin of layer A having a thickness of 30 microns. The monolayer film was used to evaluate the storage modulus, glass transition temperature, and linear expansion coefficient.

[0080] <Measurement of storage modulus and glass transition temperature of polyimide resin of layer A> The monolayer film obtained in the above section <Preparation of monolayer film of polyimide resin of layer A> was used as a sample to measure the storage modulus and glass transition temperature using a DMS6100 manufactured by Seiko Electronics Co., Ltd. The sample size was 9 mm in width and 50 mm in length. The measurement was performed at frequencies of 1, 5 and 10 Hz, at a heating rate of 3°C / min in the temperature range from 20°C to 400°C, and the storage modulus value at 300°C was read. The glass transition temperature (hereinafter referred to as "Tg") was determined from the inflection point value of the storage modulus.

[0081] <Measurement of linear expansion coefficient> The monolayer film obtained in the above <Preparation of monolayer film of polyimide resin of layer A> was used as a specimen (sample) and TMA120C manufactured by Seiko Electronics Co., Ltd. The sample size was 3 mm in width and 10 mm in length. The temperature of the sample was once raised from 10°C to 400°C at 10°C / min with a load of 3 g, then cooled to 10°C, and further raised at 10°C / min, and the average value was calculated from the thermal expansion coefficient from 100°C to 200°C during the second heating.

[0082] <Solvent resistance> The polyimide resin monolayer film of Layer A obtained from the polyamic acid solution of the synthesis example was evaluated for solubility in the following organic solvents. If any of the organic solvents was soluble at a concentration of 10% by weight or more, it was rated as soluble x (bad), and if it was not soluble at 10% by weight or more, it was rated as insoluble o (good). The solvent resistance of the printed wiring board obtained by the method for producing a printed wiring board of the present invention is in accordance with this evaluation result. In other words, if the solubility evaluation result is o (good), the solvent resistance of the printed wiring board is considered to be good, and conversely, if the solubility evaluation result is x (bad), the solvent resistance of the printed wiring board is also considered to be poor. Organic solvents: methanol, methyl ethyl ketone, toluene, tetrahydrofuran, N,N-dimethylformamide

[0083] <Peel strength> In one embodiment of the present invention, sufficient adhesion can be exhibited between the layer A on the surface of the printed wiring board and the electroless copper plating layer D. This makes it possible to avoid problems of reduced reliability such as peeling of the circuit during the circuit formation process, and to obtain a highly reliable printed wiring board. In view of the above, in order to evaluate the adhesion, the peel strength was measured according to the following procedure.

[0084] (Preparation of samples for measuring peel strength) A 1 mm wide copper pattern was made on the copper layer on one side of the double-sided laminates obtained in the examples and comparative examples by etching using masking tape, and an evaluation pattern was made on the back side with a copper layer covering the entire surface. The peel strength was measured according to the following procedure.

[0085] After the pattern etching, the water droplets on the double-sided copper-clad laminate were wiped off, the masking tape was removed, and the peel strength was immediately measured. This was carried out to evaluate the adhesion of the double-sided copper-clad laminate in a state without drying or high temperature heating, that is, immediately after only the formation of the electroless plating layer.

[0086] (Peel strength measurement) The six types of peel strength measurements were carried out on one double-sided copper-clad laminate. The peel strength was measured by peeling at a crosshead speed of 50 mm / min and a peel angle of 180°, and the resulting load was measured.

[0087] <Moisture absorption and solder heat resistance> The double-sided copper-clad laminates for evaluation obtained in the examples and comparative examples were cut into 3.5 cm squares. Next, 15 samples were prepared by removing excess copper foil layers from the 3.5 cm square double-sided copper-clad laminates for evaluation by etching so that a 2.5 cm square copper foil layer remained in the center of the sample on one side (conveniently referred to as side A) and the copper foil layer remained on the entire surface on the other side (conveniently referred to as side B). The obtained samples were left for 96 hours under humidified conditions of 40°C and 90% RH, and moisture absorption treatment was performed. After the moisture absorption treatment, five samples each were immersed in a solder bath at 260°C, 280°C, or 300°C for 10 seconds. In other words, five samples were used under one temperature condition. For the samples after solder immersion, the copper foil layer on side B was completely removed by etching, and the appearance of the part where the copper foil had overlapped was observed. If any of whitening, swelling, and peeling of the copper foil layer was confirmed in the appearance, it was determined that there was a change in the appearance. If there was no change in appearance for all five samples at 300°C, the sample was rated as ○ (good); if there was a change in appearance for one or more of the five samples at 300°C but no change in appearance at 260°C, the sample was rated as △ (pass); and if there was a change in appearance for one or more of the five samples at 260°C, the sample was rated as × (poor).

[0088] <Surface roughness Ra> The copper layer of the double-sided copper-clad laminate for evaluation obtained in the examples and comparative examples was dissolved and removed by etching. The surface roughness (Ra) of the exposed resin film was measured using a scanning probe microscope (SPM, Dimension Icon manufactured by Bruker AXS) in accordance with JIS C 0601-2001.

[0089] <Circuit formability> The circuit formability was evaluated by observing the circuit patterns for evaluation of the printed wiring boards obtained in the examples and comparative examples. The circuit formability was evaluated according to the peeling rate of the produced circuit pattern, and the following evaluation criteria were used. ◎: Peeling rate 0%-5%, 〇: Peeling rate 5%-10%, △: Peeling rate 10%-30%, ×: Peeling rate 30% or more

[0090] (Synthesis Example 1: Synthesis of polyimide resin precursor of layer A) 322.3 g of N,N-dimethylformamide (hereinafter also referred to as DMF) and 33.9 g of 1,3-bis(4-aminophenoxy)benzene (hereinafter also referred to as TPE-R) were added to a glass flask with a capacity of 2000 ml. Next, while stirring the solution in the flask under a nitrogen atmosphere, 33.6 g of 3,3',4,4'-biphenyltetracarboxylic dianhydride (hereinafter also referred to as BPDA) was added to the flask, and the solution in the flask was stirred at 25°C for 1 hour. A solution (hereinafter also referred to as BPDA solution (1)) in which 0.51 g of BPDA was dissolved in 9.7 g of DMF was separately prepared. The BPDA solution (1) was gradually added to the reaction solution while paying attention to the viscosity, and the reaction solution in the flask was stirred. When the viscosity of the reaction solution reached 1000 poise, the addition of the BPDA solution (1) and the stirring of the reaction solution were stopped. By this operation, a polyamic acid solution, which is a polyimide precursor, was obtained.

[0091] (Synthesis Example 2: Synthesis of polyimide resin precursor of layer A) 320.9 g of N,N-dimethylformamide (hereinafter also referred to as DMF), 10.4 g of ODA, and 18.7 g of KF-8010 manufactured by Shin-Etsu Chemical Co., Ltd. were added to a glass flask with a capacity of 2000 ml. Next, 38.1 g of 4,4'-(4,4'-isopropylidenediphenoxy)bis(phthalic anhydride) (hereinafter also referred to as BPADA) was added to the flask while stirring the solution in the flask under a nitrogen atmosphere, and the solution in the flask was stirred at 25°C for 1 hour. A solution in which 0.58 g of BPADA was dissolved in 11.0 g of DMF was separately prepared (hereinafter also referred to as BPADA solution). The BPADA solution was gradually added to the reaction solution while paying attention to the viscosity, and the reaction solution in the flask was stirred. When the viscosity of the reaction solution reached 1000 poise, the addition of the BPADA solution and the stirring of the reaction solution were stopped. By this operation, a polyamic acid solution, which is a polyimide precursor, was obtained. The chemical structural formula of KF-8010 manufactured by Shin-Etsu Chemical Co., Ltd. is shown in general formula (1).

[0092] [ka] (Synthesis Example 3: Synthesis of polyimide resin precursor of layer A) 321.3 g of N,N-dimethylformamide (hereinafter also referred to as DMF), 25.8 g of ODA, and 4.6 g of p-PDA were added to a glass flask with a capacity of 2000 ml. Next, 36.9 g of PMDA was added to the flask while stirring the solution in the flask under a nitrogen atmosphere, and the solution in the flask was stirred at 25°C for 1 hour. A solution in which 0.56 g of PMDA was dissolved in 10.6 g of DMF was separately prepared (hereinafter also referred to as PMDA solution). The PMDA solution was gradually added to the reaction solution while paying attention to the viscosity, and the reaction solution in the flask was stirred. When the viscosity of the reaction solution reached 1000 poise, the addition of the PMDA solution and the stirring of the reaction solution were stopped. By this operation, a polyamic acid solution, which is a polyimide precursor, was obtained.

[0093] (Formulation Example 1: Dispersion of Metal Oxide Particles for Layer A) 20 g of Aerosil E9200 manufactured by Nippon Aerosil Co., Ltd. was mixed with 80 g of DMF. The resulting mixture was stirred for 5 minutes at a rotation speed of 10,000 rpm using a rotary blade homogenizer (rotary blade diameter: 20 mm) to obtain a dispersion liquid of metal oxide particles.

[0094] (Formulation Example 2: Dispersion of Metal Oxide Particles for Layer A) 20 g of Aerosil R9200 manufactured by Nippon Aerosil Co., Ltd. was mixed with 80 g of DMF. The resulting mixture was stirred for 5 minutes at a rotation speed of 10,000 rpm with a rotary blade homogenizer (rotary blade diameter: 20 mm) to obtain a dispersion liquid of metal oxide particles.

[0095] (Formulation Example 3: Dispersion of Metal Oxide Particles for Layer A) 20 g of Aerosil NX130 manufactured by Nippon Aerosil Co., Ltd. was mixed with 80 g of DMF. The resulting mixture was stirred for 5 minutes at a rotation speed of 10,000 rpm with a rotary blade homogenizer (rotary blade diameter: 20 mm) to obtain a dispersion liquid of metal oxide particles.

[0096] Example 1 40.0 g of the polyamic acid solution of Synthesis Example 1 and 17.0 g of the dispersion of Preparation Example 1 were mixed, and 40 g of DMF and 2.0 g of lutidine were further mixed with the resulting mixture to obtain a dispersion of Layer A. The dispersion of Layer A was applied to the glossy surface of a copper foil (BHY-HA manufactured by JX Metals Corporation, thickness 12 microns) so that the final thickness of Layer A on one side was 4 microns, and the dispersion of Layer A was dried under conditions of 120°C x 2 minutes, and then heated at 450°C for 12 seconds to imidize the polyamic acid of Layer A, thereby obtaining a laminate L having a configuration of Layer A (containing heat-resistant resin and metal oxide particles) / copper foil.

[0097] The surface of the layer A side of the laminate L and the circuit-formed surface of the glass epoxy base material having circuits formed on both sides were placed opposite each other, and a glass epoxy prepreg (GEA-67N manufactured by Hitachi Chemical Co., Ltd., thickness 0.15 mm) was inserted between them and laminated, and then a vacuum press was used to laminate under the conditions of a pressure of 2 MPa, a vacuum degree of 10 kPa or less, a heating time from room temperature to 180°C of about 25 minutes, 1 hour at 180°C, and a cooling time to room temperature of about 10 minutes, and a thermosetting reaction of the glass epoxy prepreg was performed to obtain a laminate M in which copper foil was exposed on both sides. Next, the copper foil on both sides was removed by etching (hydrochloric acid / iron chloride solution), and the layer A was exposed on both sides. Next, a desmear treatment and electroless copper plating were performed under the conditions shown in Tables 1 to 2, and a laminate N in which an electroless copper plating layer was formed on the layer A on both sides was obtained.

[0098] [Table 1]

[0099] [Table 2] <Preparation of double-sided copper-clad laminate for evaluation> Next, panel plating was performed on the laminate N under the conditions shown in Table 3, using the electroless copper plating layers on both sides as power supply layers, to obtain a double-sided copper-clad laminate for evaluation with a copper thickness of 30 microns. The peel strength, moisture absorption solder heat resistance, and surface roughness Ra were evaluated.

[0100] [Table 3] <Preparation of printed wiring board> A circuit was formed with a 30 micron pitch (line / space=15 microns / 15 microns) on the laminate N having an electroless copper plating layer formed on the layer A by the semi-additive process shown in Table 4 to obtain a printed wiring board. The composition and results are shown in Tables 5 to 6.

[0101] [Table 4]

[0102] Example 2 The same procedure as in Example 1 was carried out except that the dispersion liquid of Preparation Example 1 used in Example 1 was changed to the dispersion liquid of Preparation Example 2, and double-sided copper-clad laminates and printed wiring boards for evaluation were obtained and evaluated in the same manner. The compositions and results are shown in Tables 5 and 6.

[0103] Example 3 The same procedure as in Example 1 was carried out except that the dispersion liquid of Preparation Example 1 used in Example 1 was changed to the dispersion liquid of Preparation Example 3, and double-sided copper-clad laminates and printed wiring boards for evaluation were obtained and evaluated in the same manner. The compositions and results are shown in Tables 5 and 6.

[0104] Example 4 Except for changing the amount of the dispersion liquid of Preparation Example 1 used in Example 1 to 8.5 g, the same operation as in Example 1 was carried out to obtain a double-sided copper-clad laminate and a printed wiring board for evaluation, and the same evaluation was carried out. The composition and results are shown in Tables 5 and 6.

[0105] Example 5 The same procedure as in Example 1 was carried out except that the amount of the dispersion liquid of Preparation Example 1 used in Example 1 was changed to 11.9 g, and a double-sided copper-clad laminate and a printed wiring board for evaluation were obtained and evaluated in the same manner. The compositions and results are shown in Tables 5 and 6.

[0106] Example 6 Except for changing the amount of the dispersion liquid of Preparation Example 1 used in Example 1 to 28.9 g, the same operation as in Example 1 was carried out to obtain a double-sided copper-clad laminate and a printed wiring board for evaluation, and the same evaluation was carried out. The composition and results are shown in Tables 5 and 6.

[0107] Example 7 The same procedure as in Example 1 was carried out except that the amount of the dispersion liquid of Preparation Example 1 used in Example 1 was changed to 34.0 g, and a double-sided copper-clad laminate and a printed wiring board for evaluation were obtained and evaluated in the same manner. The compositions and results are shown in Tables 5 and 6.

[0108] Comparative Example 1 The same procedure as in Example 1 was carried out except that the dispersion liquid of Preparation Example 1 used in Example 1 was not used, and a double-sided copper-clad laminate and a printed wiring board for evaluation were obtained and evaluated in the same manner. The peel strength and moisture absorption solderability were not sufficient, and more than 30% of the circuit peeling occurred. The composition and results are shown in Tables 5 and 6.

[0109] Comparative Example 2 The same operations as in Example 1 were carried out except that the polyamic acid solution of Synthesis Example 1 used in Example 1 was changed to the polyamic acid solution of Synthesis Example 2, and a double-sided copper-clad laminate and a printed wiring board for evaluation were obtained and evaluated in the same manner. A good high peel strength was shown. However, the storage modulus at 300°C of the polyimide resin of Layer A was low at <0.01 GPa, and the moisture absorption solder heat resistance was also insufficient. In addition, the solvent resistance was also poor. The composition and results are shown in Tables 5 to 6.

[0110] Comparative Example 3 The same operations as in Example 1 were carried out except that the polyamic acid solution of Synthesis Example 1 used in Example 1 was changed to the polyamic acid solution of Synthesis Example 3, and double-sided copper-clad laminates and printed wiring boards for evaluation were obtained and evaluated in the same manner. The peel strength and moisture absorption solderability were not sufficient, and more than 30% of the circuit peeling occurred.

[0111] [Table 5]

[0112] [Table 6] [Explanation of symbols]

[0113] 1.Copper foil 2. Layer A 3. Circuit board B 4.Heat-resistant adhesive material C 5. Circuit Board B 6. Electroless copper plating layer D 10. Laminate L 20. Laminate M 21. Laminate M' 22. Laminate M'' 30.Laminate N

Claims

1. A method for producing a printed wiring board using a laminate L in which a layer A containing a polyimide resin and metal oxide particles is formed directly on a copper foil, Step (1) A step of laminating the layer A side of the laminate L in the order of inserting a heat-resistant adhesive material C between the layer A side and the circuit-forming side of a circuit board B on which a circuit is formed, and then performing heat-pressure bonding to obtain a laminate M; Step (2) A step of removing the copper foil from the product obtained in step (1) to expose layer A. Step (3) A step of forming an electroless copper plating layer D on the layer A exposed in step (2). Including, 1. A method for producing a printed wiring board, wherein the linear expansion coefficient of the polyimide resin of layer A is 30 ppm or more and 100 ppm or less.

2. 2. The method for producing a printed wiring board according to claim 1, wherein the polyimide resin is a non-soluble polyimide resin.

3. 3. The method for producing a printed wiring board according to claim 1, wherein the metal oxide is a fumed metal oxide.

4. A laminate (L) in which a layer A containing a polyimide resin and metal oxide particles is formed directly on a copper foil.

5. The laminate (L) according to claim 4, characterized in that the polyimide resin is a non-soluble polyimide resin.

6. 6. The laminate (L) according to claim 4 or 5, characterized in that the metal oxide is a fumed metal oxide.