Electrostatic assistant coating method using backing roll having internal electrode capable of applying high voltage
The three-layer backing roll structure with high-insulating and conductive layers addresses the issue of entrained air layers in electrostatic coating, enabling stable high-speed coating with uniformity and preventing discharge, thus overcoming conventional limitations.
Patent Information
- Application Number
- JP2023079864
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-15
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2043-05-15
AI Technical Summary
Conventional electrostatically assisted coating methods face limitations in increasing coating speed and uniformity due to entrained air layers on both sides of the web, leading to web instability and coating failures, especially when high voltages are applied, which can cause spark discharge and short-circuit currents.
A three-layer backing roll structure with a highly insulating outermost layer, a conductive internal electrode layer, and an insulating layer, allowing for the application of high DC voltages up to 6kV without spark discharge, and utilizing electrostatic forces to polarize the web surfaces to eliminate entrained air layers, ensuring stable web adhesion and increased coating speed.
The method enables stable coating at speeds over 400 m/min with uniform thickness and prevents spark discharge and short-circuit currents, enhancing coating uniformity and web stability by effectively managing air layers on both sides of the web.
Smart Images

Figure 2024164412000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for increasing the uniformity of coating thickness and coating speed in a process for applying one or more layers of a coating liquid consisting of a liquid composition, particularly a water-soluble composition, to the surface of a flexible, strip-like support (hereinafter referred to as a web) that is supported by a backing roll and runs continuously, by a method such as curtain coating or bead coating, by applying an electrostatic force to a contact line portion (hereinafter referred to as a coating point) where the coating liquid comes into contact with the web, thereby preventing an air layer accompanying the front side (coating surface) of the web from being trapped between the coating liquid and the web and promoting uniform wetting of the coating liquid into the web.
[0002] The present invention also relates to a method for preventing an air layer accompanying the back side of the web and the roll surface from penetrating between the web and the roll by bringing the back side of the web (the back side of the backing roll) into contact with the surface of the backing roll, thereby enabling the upper limit of the web speed to be increased before running troubles such as fluctuations in web tension and speed, and oscillation occur.
[0003] The present invention is applicable to improvements in coating methods for liquid compositions, mainly water-soluble compositions, in the production of photographic films, photographic printing papers, magnetic recording tapes, adhesive tapes, pressure-sensitive and heat-sensitive recording papers, coated papers, and the like. [Background technology]
[0004] In curtain coating or bead coating, air layers are entrained on both the front and back sides of the web moving at high speed.
[0005] Since the thickness of the entrained air layers on the front and back sides increases in response to the moving speed of the web, when a certain limit speed is reached, the coating uniformity decreases or web slippage and oscillation occur, making it impossible to perform stable coating and making it impossible to increase the coating speed beyond the respective limit speed. In order to increase the speed while maintaining the coating uniformity, a method is required that can simultaneously deal with the effects of the entrained air layers on the front and back sides of the web.
[0006] On the front side of the web, when the moving speed of the web increases and the accompanying air layer increases beyond a certain limit, the air layer penetrates under the coating liquid transferred to the web at the coating point and cannot be pushed out by the coating liquid. When the air layer penetrates under the coating layer, the coating liquid is prevented from wetting and spreading on the front side of the web, or the air layer is taken up by the coating liquid and turns into bubbles, which reduces the uniformity of the coating layer, making it impossible to increase the coating speed.
[0007] It has been well known that in conventional curtain coating and bead coating, when an electrostatic field is assisted at the coating point, the electrostatic force of the ions and dipolar molecules in the coating liquid makes it possible to attract and adhere the coating liquid to the web surface, thereby increasing the upper limit of the coating speed. As methods for assisting an electrostatic field at the coating point, the following have been disclosed: 1) a method in which an electrostatic charge is applied to the web from a corona discharge electrode arranged in space, and then the web is passed through the coating point while being supported by a grounded coating backing roll; 2) a method in which a DC voltage is applied to a conductive coating backing roll (hereinafter referred to as a backing roll) insulated from the earth, to form an electric field between the surface of the web and the coating liquid at the coating point; and 3) or a combination of these two methods.
[0008] For example, Patent Documents 1 to 4 disclose a method 1) in which a dielectric web such as polyester is charged. When a dielectric web, which is given a polar charge bound between the opposing back and front surfaces, is supported on a grounded conductive backing roll surface and transported to a coating point, the polar charge remaining on the front side of the web attracts the coating liquid and acts to more strongly remove the air layer below the coating liquid, thereby increasing the coating speed. Patent Documents 5 to 7 disclose a method 2) in which a direct current voltage is applied to a conductive backing roll insulated from the earth to charge its surface, the web is supported on the surface and transported to a coating point, and an electric field is applied between the web and the coating liquid to make the coating liquid adhere to the web. Patent Document 7 also discloses a method that combines 2) and 3).
[0009] The effect of imparting electrostatic charge to the web or the effect of assisting electrostatic charge on the surface of the conductive backing roll is to suppress the phenomenon in which the air layer accompanying the web is caught between the front side of the web and the coating liquid, preventing the coating liquid from becoming wet, and to raise the limit speed at which the transparency and thickness of the coating become non-uniform. In the conventional electrostatic auxiliary coatings 1) to 3), the higher the adhesion of the coating liquid to the front side of the web, the stronger the accompanying air layer is eliminated, so it is known that the higher the electrostatic charge potential of the front side of the web or the voltage of the backing roll surface is, the higher the coating speed is. However, in electrostatic auxiliary coatings in which a voltage is applied to a conductive backing roll, it is known that when the applied voltage exceeds 1500V, spark discharge from the backing roll to peripheral devices and short-circuit currents penetrating the web are likely to occur. Also, in the method of imparting electrostatic charge to the web, when the electrostatic charge potential of the front side of the web becomes high, short-circuit currents penetrating the web may occur between the coating liquid and the surface of the conductive backing roll at pinholes or places where the insulation resistance of the web is reduced. For this reason, the surface potential of the web due to the electrostatic charge disclosed in Patent Document 1 is 1200 V or less. In addition, for example, Patent Document 4 discloses an electrostatic auxiliary coating technique in which the polarization effect of a coating solution containing a surfactant is used in combination, and Patent Document 2 discloses a method of charging the web with a conductive brush in combination, thereby setting the surface potential of the web lower than 700 to 800 V, but the standard recommended surface potential is even lower, at 400 to 500 V. In this way, the conventional electrostatic auxiliary coating using a conductive backing roll is unable to apply a sufficient potential to the coating point, and is insufficient in terms of the effect of raising the limit speed before coating problems occur due to an increase in entrained air.
[0010] In addition, the backside of the web and the surface of the backing roll each have an air layer. Therefore, the combined air causes the web to float, and the amount of floating increases as the web speed increases. When the amount of floating of the web exceeds a certain limit, there is a problem that the web transport becomes unstable, and the increase in the air layer on the backside of the web also causes the coating speed to be unable to be increased.
[0011] The web lift h (μm) is determined by the backing roll radius R (m) and roller speed U when the air temperature is 25°C. R (m / s), web speed U W (m / s) and web tension T (N / m) are given by the following equation (1).
[0012]
number
[0013] ("Basic Theory and Applications of Web Handling" by Kyo Hashimoto, p. 73, published by the Processing Technology Research Association)
[0014] According to equation (1), the thickness of the entrained air layer entrained between the back side of the web and the roll surface decreases as the web tension T increases, and the roll radius R and web speed U W or backing roll speed U R It increases as W ≒U R ).
[0015] In electrostatic assisted coating, where a voltage is applied to a conductive backing roll, when the web travel speed increases and the web floats due to the accompanying air layer between the web and the backing roll, the distance from the backing roll surface to the front side of the web increases, and the electrostatic capacitance decreases due to the air layer between the conductive backing roll and the back side of the web, which reduces the amount of polar charge stored on the web and the electrostatic force between the web and the coating solution.
[0016] Furthermore, if the thickness of the entrained air layer on the backside of the web exceeds the sum of the surface roughness of the roll and the surface roughness of the backside of the web, the contact between the web and the backing roll surface decreases, and the force pulling the web decreases. When the web pulling force decreases, the tension and speed of the web fluctuate, causing problems such as the web meandering and scratches on the backside of the web. Therefore, in order to increase the coating speed, it is absolutely necessary to take measures to prevent the web from floating up by the entrained air layer sandwiched between the backside of the web and the backing roll.
[0017] The relationship between the web transport speed and the amount of web lift calculated from equation (1) is shown in Figures 7 and 8. As shown in Figure 7, it is possible to suppress web lift by increasing the web tension T. However, increasing the web tension increases the load on the web transport system, and increases the amount of deflection of the backing roll and the guide rolls in the web transport path. In addition, when the web is thin, wrinkles are likely to occur, so there is a limit to how much the web tension can be increased.
[0018] As shown in Figure 8, the web lift amount decreases when the diameter of the backing roll is reduced. However, when the diameter of the backing roll is reduced, the rigidity of the roll decreases and the amount of deflection increases. Furthermore, when the roll diameter is reduced, the number of rotations of the roll increases proportionally, so the faster the web is and the wider the web is, the more the roll vibrates, and vibration patterns occur on the coating film. In roller curtain coating and bead coating for wide webs of 1500 mm or more, the diameter of the backing roll is preferably 100 mm or more, taking into consideration the roll's deflection strength and the area required to install the coating head (applicator). The tension of the web depends on the strength and thickness of the web, but is usually around 75 to 300 N / m, taking into consideration the stretching and deformation of the web. According to Figure 7, when a backing roll with a diameter of 100 mm is used, even if the web tension is set to 150 N / m, the web lift amount is already 6 μm at a moving speed of 100 m / min, and in rolls with a smooth surface, the traction force decreases, causing fluctuations in tension and speed. Judging from the web floating amounts shown in Figures 7 and 8, when the diameter of the backing roll is made 100 mm or more, in order to increase the web conveying speed to 100 m / min or more, it is necessary to prevent the web from floating by an air layer entrained on the back side of the web.
[0019] In electrostatically assisted curtain coating in which a DC voltage is applied to a conductive backing roll with a diameter of 100 mm or more, a measure against the floating of the web due to the accompanying air layer on the back side of the web is disclosed in Patent Document 7. In the examples of Patent Document 7, a circumferential groove (groove depth 0.15 mm, width 0.43 mm, pitch 1 mm) is formed on the surface of a backing roll with a diameter of 200 mm at a ratio of 10 to 30% of the roll surface area, and the accompanying air layer is discharged into the microgroove, making it possible to suppress the floating of the web and increase the conveying speed. However, the voltage applied to the conductive backing roll is 800 V or less, and furthermore, the electrostatic auxiliary effect is reduced in the groove portion, making it easy for coating unevenness to occur. Therefore, the increase in coating speed when microgrooves and electrostatic assistance are used in combination is a maximum of 144 m / min, which is not very large. [Prior art documents] [Patent documents]
[0020] [Patent Document 1] Patent No. 2835659 [Patent Document 2] Special Publication No. 01-035702 [Patent Document 3] Japanese Patent Application Publication No. 08-252517 [Patent Document 4] Patent No. 2509316 [Patent Document 5] Special Publication No. 06-009671 [Patent Document 6] Special Publication No. 46-027423 [Patent Document 7] U.S. Patent No. 6,177,141 [Non-patent literature]
[0021] [Non-Patent Document 1] "Basic Theory and Applications of Web Handling" by Kyo Hashimoto, published by the Processing Technology Research Association, p.73 Summary of the Invention [Problem to be solved by the invention]
[0022] In curtain coating and bead coating, air layers are entrained on both the front side (coating side) and the back side (backing roll side) of the web moving at high speed, and the thickness of these layers increases on both sides as the web moves faster. However, the problems caused by the entrained air layers are different on the front side and the back side. On the front side, the coating liquid does not wet the web, but on the back side, the entrained air layer that penetrates between the back side of the web and the backing roll causes the web to float, making the web run unstable. There is a demand for high-speed coating technology that can simultaneously address these different problems caused by entrained air flows on the front and back sides of the web.
[0023] By using a backing roll that can apply a voltage to the roll surface of 1.5 kV or more, preferably up to about 3.5 kV, the dielectric web is polarized more strongly, and the electric field between the web surface and the coating liquid at the contact line between the coating liquid and the web (coating point) can be made much stronger than with conventional methods, so that the coating speed can be increased as needed simply by adjusting the applied voltage.
[0024] At the same time, the backside of the web, which is strongly polarized by the high voltage of the backing roll, is strongly attracted to the backing roll by the electric field caused by the positive charge on the surface of the backing roll, pushing out the accompanying air layer and adhering to the surface of the backing roll, making it possible to raise the limit speed at which running problems occur with the web. [Means for solving the problem]
[0025] In order to achieve the above object, the present invention employs the following method.
[0026] The present invention provides an electrostatic auxiliary coating method using a highly safe backing roll that does not cause spark discharge to peripheral devices, does not cause short circuit current in the web, and does not cause electric shock even if a high DC voltage of up to 6 kV is applied in a process of applying a liquid composition (particularly a water-soluble composition) to a web that is supported by the roll and runs continuously. This backing roll uses highly insulating ceramics in the bottom layer, conductive metal in the internal electrode layer, and a highly resistive ceramic material layer in the outermost layer, and a gap-free three-layer structure consisting of the outermost layer / internal electrode layer / bottom layer is formed on the roll surface. The internal electrode layer is completely electrically shielded from the core metal of the backing roll and peripheral devices by the outermost layer and the bottom layer. Since the insulation withstand voltage of the outermost layer and the bottom layer is 6 kV or more, spark discharge to peripheral devices and short circuit current in the web are completely prevented even if a high DC voltage of up to 6 kV is applied to the internal electrode layer.
[0027] That is, the method of the present invention comprises: (1) A method for applying a coating liquid comprising a liquid composition to a first surface of a continuously moving flexible plastic web having first and second opposing surfaces, the method comprising the steps of: a step of conveying the web along a path to a backing roll for coating, and passing the web through a coating point while supporting a second surface of the web in close contact with a portion of the surface of the rotating backing roll to which a DC voltage is applied by an electrostatic field of the backing roll; and applying the coating liquid to the first surface of the web by electrostatic force generated by the arrangement of charges of the same polarity as the DC voltage applied to the backing roll on the first surface of the web, by attracting the coating liquid at the coating point, The backing roll is provided with an outermost layer to which the web is in close contact, a conductive monopolar internal electrode layer adjacent to the inner side of the outermost layer, and an insulating layer adjacent to the inner side of the internal electrode layer, and the backing roll is configured to be able to apply a predetermined voltage to the internal electrode layer, and the outermost layer has a volume resistivity of 10 7 ~10 13 a ceramic material layer of Ωcm, the surface of the backing roll being charged with a charge of the same sign as the voltage applied to the internal electrode when the predetermined voltage is applied to the internal electrode layer, the second surface of the web in contact with the outermost layer by the electrostatic force of the charge is brought into close contact with the outermost layer and rotated and transported, and the coating liquid is attracted to and brought into contact with a first surface of the web during rotation and transport, and deposited on the first surface of the web.
[0028] In the coating method, (2) applying a charge having a polarity opposite to that of the DC voltage applied to the internal electrode layer to a first surface of the web opposite to a second surface of the web before the coating liquid comes into contact with the web during rotational transport; (3) A DC voltage applied to the internal electrode layer is 0.3 to 6.0 KV. (4) The diameter of the backing roll is 100 mm or more. (5) At least one of the insulating layer, the internal electrode layer, and the outermost layer is made of a material formed by a thermal spraying method or a material using either an inorganic or organic binder, and at least one of the insulating layer, the internal electrode layer, and the outermost layer of the backing roll is subjected to a sealing treatment. (6) The outermost layer is made of a ceramic material, and the ceramic material is an alumina-based, zirconium oxide-based, or magnesium oxide-based ceramic containing a compound selected from titanium oxide, chromium oxide, silicon oxide, manganese oxide, nickel oxide, and iron oxide, or an aluminum oxide-based ceramic containing 5 to 17% by weight of titanium oxide. (7) The ceramic material contains at least one selected from an aluminum nitride material, a silicon carbide material, and a silicon nitride material, and an organic or inorganic binder. (8) The thickness of the outermost layer is 50 to 500 μm. (9) The center line average surface roughness Ra of the outermost layer is 0.01 to 5 μm. (10) The internal electrode layers are made of a conductive material containing tungsten or molybdenum. (11) The thickness of the internal electrode layer is 5 to 50 μm. (12) The insulating layer includes at least one highly insulating material selected from aluminum oxide, aluminum oxide-based materials containing 2 to 4% by weight of titanium oxide, magnesium oxide-based materials, beryllium oxide-based materials, aluminum nitride-based materials, ceramic materials containing silicon nitride, porcelain, and enamel. (13) The volume resistivity of the insulating layer is 10 13 Ωcm or more, (14) The thickness of the insulating layer is 50 to 500 μm. It is characterized by: Effect of the Invention
[0029] The present invention relates to an electrostatic auxiliary coating method using a highly safe backing roll that does not generate spark discharge to peripheral devices, does not generate short circuit current in the web, and does not cause electric shock even if a high DC voltage of up to 6 kV is applied in a process of applying a liquid composition (particularly a water-soluble composition) to a web that is supported by the roll and runs continuously. This backing roll uses highly insulating ceramics in the bottom layer, conductive metal in the internal electrode layer, and a highly resistive ceramic material layer in the outermost layer, and a gap-free three-layer structure consisting of the outermost layer / internal electrode layer / insulating layer is formed on the roll surface. The internal electrode layer is completely electrically shielded from the core metal of the backing roll and peripheral devices by the outermost layer and the bottom layer. Since the insulation withstand voltage of the outermost layer and the bottom layer is 6 kV or more, spark discharge to peripheral devices is completely prevented even if a high DC voltage of up to 6 kV is applied to the internal electrode layer.
[0030] The volume resistivity of the outermost layer, the high-resistance semiconductor ceramic, is 10 7 ~10 13 Since the internal electrode has a resistivity of Ωcm, when a DC voltage is applied to the internal electrode, charges move from the internal electrode to the outermost surface, and the surface of the outermost layer is charged with the same polarity as the internal electrode. At the same time, the web in contact with the outermost surface of the backing roll is dielectrically polarized by the electric field of the internal electrode, and the internal electric dipole is arranged so that the back side direction is charged with a charge of the opposite polarity to the potential of the internal electrode, and the front side direction is charged with a charge of the same polarity. Then, the coating liquid is attracted to the web surface and adheres to the web by the electrostatic charge of the same polarity as the internal electrode arranged on the web surface side, eliminating the air layer accompanying the front side of the web, and promoting the wetting of the coating liquid by the web. At the same time, the charge of the opposite polarity to the internal electrode arranged on the back side of the web is attracted to the free charge of the same polarity as the internal electrode that is charged on the surface of the high-resistance semiconductor ceramic, which is the outermost layer of the backing roll, so that the web adheres to the backing roll surface. In this way, in the present invention, the influence of the accompanying air layer is eliminated on both the front and back sides of the web, making it possible to greatly increase the coating speed on the web.
[0031] The present invention provides the following effects. 1. By applying a high DC voltage of up to 6 kV to the internal electrode installed on the outer surface of the backing roll, it is possible to coat liquid compositions (especially water-soluble compositions) with electrostatic assistance without generating spark discharge to surrounding equipment or damaging the web due to short circuit current. 2. While applying a high DC voltage to the internal electrode of the backing roll, an external auxiliary electrode is simultaneously placed in the space above the front surface of the web and a DC voltage of 1.5 to 6 kV of opposite polarity to the internal electrode is applied, enabling electrostatic auxiliary coating in which a charge of opposite polarity to the internal electrode is applied to the front surface of the web. 3. Even if the diameter of the backing roll is 100 mm or more, the electrostatic force due to the static charge on the surface of the high-resistance semiconductor ceramic on the outermost surface makes it possible to completely adhere the web to the backing roll, effectively performing electrostatic auxiliary coating on the web surface, and preventing rocking and slipping due to the web floating, making it possible to increase the web transport speed to 400 m / min or more. 4. The diameter of the backing roll can be increased according to the length of the roll, which makes it possible to increase the rigidity of the roll and facilitates the production of wider webs. [Brief description of the drawings]
[0032] [Figure 1] FIG. 2 is a cross-sectional view of an example of the method of the present invention for electrostatically assisted coating using only a backing roll with a high voltage applied to the internal electrode. [Diagram 2] 2 is a diagram showing a schematic diagram of charge distribution in part A of FIG. 1. FIG. [Diagram 3] FIG. 2 is an external view of the method of the present invention seen from an oblique direction. [Figure 4] FIG. 11 is a cross-sectional view of an alternative method of the present invention for electrostatically assisted coating using a backing roll with a high voltage applied to the internal electrode in combination with the application of an electrostatic charge to the web. [Diagram 5] 5 is a diagram showing a schematic diagram of the charge distribution state in part B of FIG. 4. FIG. [Figure 6] FIG. 13 is an external view of a method according to a modified example of the present invention, as viewed from an oblique direction. [Figure 7] 1 is a graph showing the change in web lift amount versus tension and web speed for a backing roll having a diameter of φ200 mm. [Figure 8] 1 is a graph showing the change in web lift with respect to backing roll diameter and web speed at a web tension of 150 N / m. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0033] The method of the present invention is shown in Figures 1 to 3. Figure 2 shows a schematic diagram of the charge distribution state in part A shown in Figure 1.
[0034] (1) In order to increase the coating capacity, in addition to increasing the web transport speed, it is important to lengthen the backing roll to widen the web. However, when the web tension is constant, the amount of deflection of the roll increases rapidly when the backing roll is lengthened. Therefore, in order to prevent the backing roll from deflecting, it is necessary to simultaneously increase the backing roll diameter and increase the rigidity of the roll (the amount of deflection of the roll is proportional to the cube of the roll length and inversely proportional to the fourth power of the second moment of area (almost proportional to the roll diameter)). However, as shown in the above formula (1), when the roll diameter is increased, the accompanying air layer on the back side of the web also increases proportionally. The increase in the accompanying air layer lowers the upper limit of the web transport speed, so that it becomes impossible to increase the diameter of the backing roll and therefore the roll cannot be lengthened. On the other hand, the present invention can eliminate the influence of the accompanying air layer on the back side of the web, so that it is possible to increase the diameter and roll length of the backing roll as necessary to widen the web. Judging from FIG. 8, when the diameter of the web-transport roll is 100 mm or more, the effect of the entrained air layer becomes significant, so the present invention is more effective when applied to a backing roll having a diameter of 100 mm or more.
[0035] The internal electrode layer 3 of the backing roll 1 of the present invention is a conductive layer adjacent to the outermost layer 4 on the inside with no gap therebetween and in contact with the outermost layer 4. The internal electrode layer 3 is of a unipolar type and is wired for connection to a high-voltage DC power source 5 so that a DC voltage can be applied thereto, but the internal electrode layer 3 is completely insulated from the earth and the core metal 16 of the backing roll 1 by the insulating layer 2 adjacent to the inside.
[0036] Generally, there are two types of internal electrode layer 3, a monopolar type and a bipolar type, depending on the voltage application method. The monopolar type has only a single internal electrode, either positive (+) or negative (-), and a voltage is applied only between this single electrode with respect to the earth. The bipolar type has two or more internal electrodes of different polarities, but when the web, which is the object to be attracted, is connected to the earth, the charge (current) leaks to the earth side and the electrostatic attraction force becomes unstable. In the present invention, the monopolar type is used for the internal electrode layer 3. The internal electrode layer 3 is provided continuously and uniformly over a range wider than the width of the web 7 in the axial direction of the backing roll 1, and further over the entire circumference of the backing roll 1 in the rotation direction of the backing roll 1. If the internal electrode 3 is comb-shaped, band-shaped, or spiral-shaped, the coating layer will have shape unevenness. The internal electrode layer 3 may not be formed on both ends of the cylindrical surface of the backing roll 1, which are outside the support range of the web 7.
[0037] The outermost layer 4 is a high-resistance ceramic material, and the volume resistivity is 10 7 ~10 13 Ωcm, more preferably 10 8 ~10 12 In the "field of static electricity," the volume resistivity is 10 13 Materials with a volume resistivity of 10 Ωcm or more are classified as insulators because static electricity does not easily move. 6 Materials with a volume resistivity of less than Ωcm are called electrostatic conductors, and static electricity moves easily and becomes equipotential when voltage is applied. 7 ~10 13These materials are classified as intermediate between conductors and insulators, and are classified as "electrostatic semiconductors." It is known that when a voltage is applied, a minute current flows, and free charges move to the surface and become charged, just like in the case of a conductor. The amount of charge on these free charges depends on the applied voltage. Unlike conductive metal surfaces, the surface of these highly resistive semiconductor ceramic materials has a localized charge of 0.001 to 10 μA / cm2 even when a high voltage of 3.5 to 6 kV is applied. 2 Therefore, the discharge caused by the free charges on the surface becomes a minute corona and does not develop into an arc discharge, and no spark discharge occurs toward surrounding equipment.
[0038] In the present invention, as shown in Fig. 2, when a DC voltage is applied to the internal electrode layer 3, free charges 17 of the same polarity as the internal electrode 3 move to the surface of the outermost layer 4 and are charged. Then, when the second surface 13 (back side surface) of the web 7 comes into contact with the surface of the outermost layer 4, the dipoles 18 inside the web 7 are oriented with the polarity opposite to that of the free charges 17 toward the surface of the outermost layer 4 due to dielectric polarization caused by the electric field of the internal electrode. Then, the web 7 is adhered to the surface of the outermost layer 4 due to the electrostatic force between the charges 17 on the surface of the outermost layer 4 and the opposite charges of the dipoles oriented on the second surface 13 of the web 7. At this time, the first surface 12 (front side surface) of the web, which is the coating surface, is polarized and charged to the same polarity as the internal electrode by the electrostatic field of the internal electrode 3. This "polar charge" attracts the coating liquid toward the first surface 12 of the web 7 during rotational transport, making it possible to form a uniform coating layer 11 on the first surface 12 of the web 7 without the intrusion of an entrained air layer between the coating liquid 9 and the first surface 12 of the web 7. The higher the voltage applied to the internal electrode 3, the more the amount of polar charge accumulated on the first surface 12 due to dielectric polarization of the web 7 increases, and the stronger the electric field becomes, making it possible to greatly increase the coating speed.
[0039] (2) Figures 4 and 5 are side views showing an example of a modified method of the present invention. Figure 5 shows a schematic diagram of the charge distribution state in part B of Figure 4.
[0040] The method of the present invention is a method in which, in the same apparatus configuration as the method of the present invention, a spatial auxiliary electrode 14 is additionally installed at a position upstream of the coating point, and a high voltage of opposite polarity to that of the internal electrode 4 is applied to generate a corona discharge, thereby charging the first surface 12 of the web 7 with free charges 19 of opposite polarity to that of the internal electrode layer 3.
[0041] The outermost layer 4 of the backing roll 1 has a maximum withstand voltage of 6 kV and a volume resistivity of 10 7 ~10 13 Since the electrical resistance is Ωcm, even if the web to which the electric charge 19 is applied has pinholes or areas with weak insulation resistance, it prevents the occurrence of short-circuit current from the coating liquid at the defective areas toward the backing roll 1. Therefore, by raising the corona discharge potential of the external auxiliary electrode 14 installed in the space upstream of the coating point as necessary, it is possible to increase the amount of free charge 19 on the first surface 12 of the web 7, making it possible to further increase the coating speed by electrostatic assistance. A voltage of DC (-) 3.5 to 6 kV applied to the external auxiliary electrode is sufficiently effective, and if it is installed at an appropriate distance from surrounding equipment, no spark discharge will occur.
[0042] Furthermore, due to the electrostatic force between the charges 17 on the surface of the outermost layer 4 and the charges 19 on the first side of the web, the web 7 adheres more strongly to the surface of the outermost layer 4, completely preventing the intrusion of the entrained air flow to the back side of the web 7. Therefore, in accordance with the increase in the coating speed, the web transport speed can also be increased significantly as necessary.
[0043] (3) Since the web 7, which is the object to be adhered in the present invention, is flexible, all contact surfaces between the web 7 and the backing roll 1 must have uniform and strong adhesion without any loose parts. To obtain the electrostatic force required for electrostatic adhesion of the web 7, a voltage of DC(+)0.3 to 3.5 kV is usually sufficient to apply to the internal electrode layer 3. The higher the applied voltage, the stronger the electrostatic auxiliary effect becomes, and the electrostatic force is insufficient when the applied voltage is 0.3 kV or less. Since the withstand voltage of the outermost layer 4 is a maximum of 6 kV or more, no spark discharge occurs even when DC+3.5 kV is applied.
[0044] (4) At least one of the insulating layer 4, the internal electrode layer 3, and the outermost layer 2 of the backing roll 1 is made of a material formed by a thermal spraying method or a material using either an inorganic or organic binder, and at least one of them has been subjected to a sealing treatment.
[0045] Thermal spraying in this invention is a coating technology in which a coating material is melted or softened by heating, turned into fine particles, accelerated, and collided with the surface of the object to be coated, and the flattened particles are solidified and deposited to form a coating. There are various methods of thermal spraying, which are classified according to the material used and the type of heat source, but in the case of this invention, the atmospheric plasma spraying method is particularly suitable.
[0046] Furthermore, when a sprayed ceramic material is used for the outermost layer 4 and the outermost layer 2, it is preferable that at least one of the insulating layer 2, the internal electrode layer 3, and the outermost layer 4 is subjected to a sealing treatment. The sprayed ceramic coating is a collection of flat sprayed particles, but there are fine gaps between these sprayed particles, and interconnected pores equivalent to 3 to 10 Vol% of the total volume of the sprayed coating are formed. In a normal atmospheric environment, air or liquid containing moisture penetrates the pores, and water molecules are adsorbed on the inner walls of the pores, so that the sprayed coating has a significantly low insulation resistance and withstand voltage. By permeating the sprayed ceramic with an insulating sealant, the interconnected pores disappear, and the sprayed ceramic becomes a ceramic material with a stable volume resistivity, high withstand voltage, and excellent corrosion resistance. Sealing the ceramic material after coating it is possible to carry out even on large backing rolls with a diameter of 200 mm or more used in actual machines, and is a practical method. As the material used for the sealing treatment, a low-viscosity silicon oligomer (e.g., viscosity 8-40 mPs, 25°C), a low-viscosity epoxy resin (e.g., viscosity 80-400 mPs, 25°C), a polyester resin, an aqueous lithium silicate solution forming an inorganic coating, a metal alkoxide forming an inorganic sol, and other liquid sealing agents can be used by diluting with a solvent to reduce the viscosity. In the present invention, low-viscosity silicon oligomers and low-viscosity epoxy resins are preferred because they exhibit excellent impregnation characteristics, insulating performance, and voltage resistance characteristics. In addition, the thickness range of the sealing treatment layer is preferably such that the entire sprayed layer is sealed. In this way, it is important to penetrate the sealing agent into the pores of the sprayed coating to seal the pores, and then heat-set the sealant to stabilize the volume resistivity and voltage resistance characteristics of the sealant. Unless the pores inside the sprayed coating are reliably sealed, both the insulating layer 2 and the outermost layer 4 cannot be adjusted to their original volume resistivity and voltage resistance.
[0047] The volume resistivity of the outermost layer 4 after the sealing treatment at 25 to 100°C is 10 7 ~10 13 Ωcm, preferably 10 8 ~10 12 Ωcm, more preferably 10 9 ~10 12 The volume resistivity is 107 If the volume resistivity is less than Ωcm, it is not possible to prevent the occurrence of short circuit current or spark discharge to peripheral devices through the web 7 that contacts the surface of the backing roll 1 from the coating solution connected to the earth. 7 Below this level, it is not preferable since it becomes impossible to carry out electrostatically assisted coating in which a high voltage of 1.5 kV or more is applied to the surface of the back roll and the web.
[0048] On the other hand, the volume resistivity of the outermost layer 4 is 10 13 If the electrical resistance exceeds Ωcm, the outermost layer 4 becomes an insulating dielectric, and the free charge 17 does not flow substantially from the internal electrode layer 3. As a result, the surface of the outermost layer 4 cannot be charged with the free charge 17 of the same polarity as the internal electrode, which is not preferable. When the electrical property of the outermost layer 4 is an insulating dielectric, the dipole 18 is oriented so that the surface direction of the outermost layer 4 becomes a charge of the same polarity as the internal electrode 3 due to the dielectric polarization caused by the voltage of the internal electrode 3. Here, the charge on the surface of the outermost layer 4 is due to the charge fixed to the dipole, and cannot be neutralized and annihilated by the free charge. When the web 7 is separated from the backing roll, a reverse charge remains on the surface of the outermost layer 4 due to peeling electrification. This reverse charge is trapped by the fixed charge at the dipole end of the outermost layer 4 when a voltage is applied to the backing roll, and although the apparent charged potential decreases, it does not disappear and remains as it is. When the surface of the outermost layer 4 becomes like this, the web 7 is repelled from the surface of the outermost layer 4. That is, the outermost layer 4 has a volume resistivity of 10 13 If the resistivity is higher than Ωcm, the material becomes an insulating dielectric, and the peeling charge of the web is not neutralized and remains on its surface, so that the web cannot adhere to the surface of the outermost layer 4, causing problems with the running of the web.
[0049] (5) The outermost layer 4 is made of a ceramic material, and the ceramic material is an alumina-based, zirconium oxide-based, or magnesium oxide-based ceramic containing a compound selected from titanium oxide, chromium oxide, silicon oxide, manganese oxide, nickel oxide, and iron oxide, or an aluminum oxide-based ceramic containing 5 to 17 weight % titanium oxide.
[0050] The material of the outermost layer 4 of the present invention is preferably a material having a volume resistivity of 10 7 ~10 13 It is a material that can be adjusted to Ωcm and has excellent handling properties. In terms of adhesion and density with the internal electrode layer 2, stability of the volume resistivity, ease of handling, etc., an aluminum oxide-based ceramic material layer containing 5 to 17% by weight, preferably 7 to 15% by weight, of titanium oxide by thermal spraying is the most preferable.
[0051] (6) In a similar sense, in the present invention, the outermost layer 4 and the insulating layer 2 are also preferably non-oxide ceramic material layers using organic or inorganic binders by coating. As long as the volume resistivity and withstand voltage can be ensured, the outermost layer 4 and the insulating layer 2 may be coating layers formed by coating a coating material made of a ceramic material containing an organic or inorganic binder and at least one selected from an organic binder such as polyimide or an inorganic binder such as aluminum phosphate, water glass, or silicon, which is blended to have a volume resistivity suitable for the present invention, and an organic or inorganic binder.
[0052] (7) The thickness of the outermost layer 4 is preferably 50 μm or more, more preferably 80 to 500 μm. The lower limit of this thickness is the minimum thickness necessary to ensure that there are no pinholes or the like penetrating through the outermost layer 4 to the internal electrode layer 3, and is the thickness that can ensure the withstand voltage against the minimum applied voltage necessary for stable adhesion of the web 7. The upper limit of this thickness is set in consideration of the maximum applied voltage. In order to obtain a stronger electrostatic auxiliary effect, a higher applied voltage is required, and it is necessary to increase the thickness of the outermost layer 4 to increase the withstand voltage. However, since a sufficient effect can be obtained with a voltage of 3.5 kV applied to the internal electrode layer, a maximum withstand voltage of 6 kV is sufficient in consideration of a safety factor. Increasing the thickness of the outermost layer 4 beyond 500 μm at which the withstand voltage is obtained is not preferable because it only increases the spraying time.
[0053] (8) The surface roughness of the outermost layer 4 of the backing roll 1 of the present invention is a center line average surface roughness Ra of 0.01 to 5 μm. A smooth surface of less than 0.01 μm is difficult to obtain using actual ceramic layer polishing techniques. The greater the surface roughness of the outermost layer 4, the more stable the running of the web at high speeds becomes, but if it exceeds 5 μm, it is not preferable because the surface roughness of the outermost layer 4 is transferred to the back surface of the web.
[0054] (9) As the material for the internal electrode layer 3, a sintered conductive paste such as tungsten, molybdenum, high-performance activated carbon, copper, or silver can be used. However, a sprayed coating of tungsten or molybdenum applied by a plasma spraying method has high thermal conductivity and is also preferable in terms of handling.
[0055] (10) The volume resistivity of the outermost layer 4 is 10 7 ~10 13 Since the internal electrode has a high resistivity of Ωcm, even when a high voltage of 6 kV is applied to the internal electrode, the total current flowing from the internal electrode to the web surface is very small, at several mA or less, so a thickness of 5 to 50 μm for the internal electrode layer 3 is sufficient, and it is preferable that the thickness is as thin as possible in order to smooth the boundaries of the internal electrode 3 at both ends of the roll.
[0056] (11) As the highly insulating material of the insulating layer 2, a ceramic spray coating made of high purity alumina of 99.6% or more or alumina containing 2 to 4 wt% titanium oxide is preferable, and a coating material made of a ceramic material selected from magnesium oxide, beryllium oxide (BeO), aluminum nitride (AlN), silicon nitride (Si3N4), etc. Also, a polymer resin selected from polyimide, polyphenylene oxide, polyethylene tetrafluoroethylene (Teflon (registered trademark)), polytrifluoroethylene chloride, polyethylene, polypropylene, polystyrene, etc., a SiO2-based glass film such as porcelain and enamel may be used, but in the present invention, a ceramic spray coating made of high purity alumina of 99.6% or more or alumina containing 2 to 4 wt% titanium oxide is most preferable in terms of insulation performance, thermal conductivity, handling, price, etc.
[0057] (12) The volume resistivity of the insulating layer 2, which is the innermost layer in contact with the core metal 16 of the backing roll 1 of the present invention, is 10 13 It is preferable that the resistance is Ωcm or more in order to reduce the leakage current from the internal electrode layer 3 to the core metal 16 via the insulating layer 2 to a level that has no effect.
[0058] (13) The thickness of the insulating layer 2 is preferably 50 to 500 μm, and if it is less than 50 μm, the withstand voltage is insufficient to apply the minimum voltage of 0.3 kV to obtain the necessary adhesion to the internal electrode layer 3. To enable application of a voltage of up to 6 kV to the internal electrode layer, it is desirable for the withstand voltage of the insulating layer 3 to be 6 kV or more, and a thickness of 500 μm is sufficient for this withstand voltage.
[0059] (14) The web used in the present invention includes paper, plastic film, resin-coated paper, synthetic paper, etc. Examples of materials for the plastic film include polyolefins such as polyethylene and polypropylene, vinyl polymers such as polyvinyl acetate, polyvinyl chloride, and polystyrene, polyamides such as 6,6-nylon and 6-nylon, polyesters such as polyethylene terephthalate and polyethylene-2,6-naphthalate, polycarbonates, cellulose acetates such as cellulose triacetate and cellulose diacetate, etc. Resins used for resin-coated paper are typically polyolefins such as polyethylene, but are not necessarily limited to these. The web can have one or several layers coated in advance.
[0060] (15) The term "coating liquid" includes various liquid compositions depending on the application, and can be used to form, for example, a photosensitive emulsion layer, undercoat layer, protective layer, backing layer, antistatic layer or antihalation layer of a photographic material, an ink absorbing layer in the case of an inkjet receiving medium, a magnetic layer, undercoat layer, lubricating layer, protective layer, back layer, adhesive layer, colored layer, anticorrosive layer, etc. of a magnetic recording medium. These coating liquids can contain a water-soluble binder or an organic binder.
[0061] (16) Surfactants can be used to modify the surface tension and coatability of the coating solution, including nonionic surfactants such as polyalkylene oxides and water-soluble adducts of glycidol and alkylphenols, anionic surfactants such as alkylaryl polyether sulfates and sulfonates, amphoteric surfactants such as arylalkyltaurines, N-alkyl and N-acyl β-aminopropionates, saponins, and alkylammonium sulfonate betaines.
[0062] (17) A thickener may be used in the coating solution to adjust the viscosity.
[0063] (17) Coating applicators to which the present invention can be applied include bead coating applicators, curtain coating applicators, extrusion coating applicators, and slide extrusion coating applicators.
[0064] [Measurement method] The methods for measuring physical properties used in the present invention are as follows.
[0065] 1.Center line average roughness Ra When the surface roughness of the backing roll could be measured while it was in the rolled state, the average roughness Ra of the surface was measured with a portable surface roughness meter. The measuring device was in accordance with JIS B0651, and the stylus was a cone with an apex angle of 60 degrees and a spherical tip with a radius of curvature of 2 μm. The measuring method was in accordance with JIS B0601-2013, and measurements were taken with a cutoff value of 0.8 mm to obtain the center line average roughness Ra. The measuring device used was the Surfcoder SE1700α manufactured by Kosaka Laboratory Co., Ltd.
[0066] 2. Volume resistivity The volume resistivity of the outermost layer 4 on the surface of the backing roll 1 is measured in accordance with JISC2141-1992, a test method for ceramic materials for electrical insulation. A main electrode with an outer diameter of φ26 mm and a guard electrode with an outer diameter of φ48 mm and an inner diameter of φ38 mm are cut out from a conductive adhesive sheet, and are attached to the curved surface of the outermost layer 4 so that the guard electrode and the main electrode are concentric to conform to the three-terminal method of JISC2141. A conductor with a terminal attached with conductive adhesive tape is used as the contact point on the surface of the main electrode and the guard electrode. The internal electrode layer 3 of the backing roll is used as the counter electrode. The value measured one minute after the start of the measurement is adopted. The measuring instrument used is the Super Insulation Meter R-503 manufactured by Kawaguchi Electric Works. A DC voltage of 500 V is applied between the main electrode, the internal electrode layer 3, and the guard electrode, and the volume resistivity R is calculated from the current value I (A) flowing through the main electrode and the counter electrode (internal electrode layer 3) at that time. V (=V / I) and calculate the volume resistivity ρ V Calculate.
[0067] ρ V (Ωcm)=R V ×A / d A = π × D 2 / 4 Where: V: Applied voltage (V) R V : Volume resistivity (Ω) ρ V : Volume resistivity (Ωcm) A: Area of the main electrode (cm 2 ) D: Main electrode outer diameter (cm) d: Outermost layer thickness (cm) The thickness d is measured using a magnetic or eddy current thickness gauge, FMP20, a dual-purpose magnetic / eddy current thickness gauge manufactured by Fisher Instruments. EXAMPLES
[0068] Example 1 In the method of FIG. 1, electrostatically assisted curtain coating according to the method of the present invention was carried out by continuously conveying a web 7 to a backing roll 1 and applying a DC voltage only to the internal electrode 3 of the backing roll.
[0069] The backing roll 1 used here was produced as follows.
[0070] The entire surface of the center of the cylindrical core 16 made of steel and 200 mm in diameter was sandblasted, and then a 50 μm thick 80 wt% Ni / 20 wt% Cr alloy was plasma sprayed to form a bonding layer to improve the adhesion of the ceramic layer. Then, 250 μm of aluminum oxide (alumina) (99.6 wt% Al2O3) was plasma sprayed onto the surface of the bonding layer as a highly insulating material, and this sprayed alumina layer was then sealed with low-viscosity epoxy resin to give a volume resistivity of 10 14 An insulating layer 2 of Ωcm or more was formed. On the insulating layer 2, tungsten (W) of 30 μm thickness was laminated by plasma spraying to form the internal electrode layer 3. At this time, a masking was performed over a width of 20 mm from both ends in the width direction of the backing roll 1 so that the internal electrode layer 3 was not formed in this range. After removing the masks at both ends, an alumina-based ceramic material containing 10 wt% titanium oxide (TiO2) and the remaining 90 wt% being alumina (Al2O3) was laminated to a thickness of 400 μm as the outermost layer 4 by plasma spraying on both ends and further on the upper surface of the internal electrode layer 3, i.e., the entire cylindrical surface of the backing roll 1. Similarly, the alumina-based ceramic material layer was sealed with a low-viscosity epoxy resin together with the tungsten layer of the internal electrode layer 3, to obtain a volume resistivity of 5.6 × 10 10 An outermost layer 4 with a resistance of Ωcm was obtained.
[0071] The outermost layer 4 after the sealing treatment was polished with a diamond grindstone so that the residual thickness was 300 μm and the surface roughness Ra after polishing was 0.05 μm. In order to enable electrical connection to the internal electrode layer 3, a rectangular masking area of 20 mm x 30 mm was applied to one end of the roll during thermal spraying of the outermost layer 4, and the internal electrode layer 3 was exposed at the end of the roll with a width of 20 mm x 10 mm after thermal spraying of the outermost layer 4. A slip ring 6 was connected to the exposed internal electrode layer 3. A DC high voltage power supply 5 was connected to the slip ring 6, and a DC voltage of (+) 3.5 kV was applied to the internal electrode 3. Here, when a voltage was applied to the internal electrode, no current was felt by the human body even when the surface of the outermost layer 4 was touched with a finger.
[0072] The web 7 is a polyethylene terephthalate film having a thickness of 100 μm, and is coated with a gelatin undercoat layer having a thickness of 0.3 μm. The web 7 was placed in a heating furnace at a temperature of 90 to 100° C., and the back and front sides of the web 7 were alternately brought into contact with earthed rolls to remove the electric charge until the surface potential became ±50 V or less, and then cooled to 25° C.
[0073] The gelatin composition was applied so that the thickness of the wet coating layer 11 would be 60 μm, with a curtain height of the coating solution 9 of 10 cm, a coating angle of 30° forward from the top of the roll, a tension of the web 7 of 150 N / m, and a conveying speed of the web 7 of 400 m / min. The coating solution used was a 15% aqueous gelatin solution containing 0.1% sodium dodecyl benzene sulfonate, and the low shear viscosity was adjusted to 100 mPa s with a thickener. The flow rate of the coating solution was set to 4 cc / sec per 1 cm of coating width.
[0074] The back surface 12 of the web 7 was in close contact with the surface of the backing roll 1, and the web was running stably. Coating could be continued without any coating failure due to the air layer accompanying the surface of the web 7 being drawn under the coating liquid, and the wet coating layer 11 had good thickness uniformity and a smooth surface. No spark discharge occurred from the back roll to the surroundings, and no short circuit current was generated that penetrated the web 7 from the coating liquid 9 toward the roll surface.
[0075] Comparative Example 1 When coating was performed with the same configuration and conditions as in Example 1, with the voltage to the internal electrode 3 set to 0 (zero), the curtain of coating liquid 9 alone was unable to eliminate the entrained air layer, and the coating liquid did not wet the surface 12 of the web 7, making uniform coating impossible. In addition, the web 7 floated up from the backing roll, and the traction force of the backing roll 1 on the web 7 decreased, causing the tension and speed of the web 7 to fluctuate, making the running unstable, and therefore coating could not be sustained.
[0076] Example 2 In the same coating apparatus as in Example 1, the web 7 was transported to a backing roll 1 having a diameter of 200 mm, a voltage of +3.5 kV was applied to the internal electrode 3, and a tungsten wire electrode 14 having a diameter of 0.5 mm was additionally installed at a distance of 10 mm from the web as shown in FIG. 2, a voltage of -3 kV was applied, and a negative charge (-) was deposited from the electrode 14 on the first surface of the web 7, thereby performing electrostatically assisted curtain coating according to the method of the modified example of the present invention.
[0077] The web 7 is a polyethylene-coated paper having a thickness of 100 μm, and is coated with a gelatin undercoat layer having a thickness of 0.6 μm. The web 7 is placed in a heating furnace at a temperature of 90 to 100° C., and the back and front sides of the web are alternately brought into contact with earthed rolls to remove the electric charge until the surface potential becomes ±50 V or less, and then cooled to 25° C.
[0078] The gelatin composition was applied to a wet thickness of 35 μm at a curtain height of 10 cm, a coating angle of 30° forward from the roll apex, a tension of 150 N / m on the web 7, and a web conveying speed of 400 m / min. The coating solution 9 was a 12% gelatin aqueous solution containing 0.1% sodium dodecyl benzene sulfonate, and the low shear viscosity was adjusted to 21 mPa·s with a thickener. The flow rate of the coating solution was set to 2.3 cc / sec per 1 cm of coating width. The second surface 13 of the web 7 was in close contact with the surface of the backing roll 1, and the web was running stably. The first surface 12 of the web 7 was able to continue coating stably without causing coating problems due to the air layer accompanying the first surface 12 being entrained in the coating solution, and the thickness uniformity of the wet coating layer 11 and the surface smoothness were both good. No spark discharge or glow discharge occurred from the backing roll to the surroundings, and no short-circuit current was generated that penetrated the web 7 from the coating solution 9 toward the roll surface.
[0079] Comparative Example 2 Under the same configuration conditions as in Example 2, when coating was performed with the voltage to the internal electrode 3 set to 0 (zero), the coating liquid 9 was able to form a wet coating layer 11 that adhered closely to the entire surface of the first surface 12 of the web. However, an entrained air layer entered between the back surface 13 of the web and the backing roll, causing the web 7 to float, which resulted in the tension and speed of the web 7 becoming unstable and causing it to sway and run unstably, making it impossible to sustainably form a wet coating layer 11 with a smooth surface. [Explanation of symbols]
[0080] 1 Backing roll 2. Insulation layer 3 Internal electrode (+) 4 Outermost layer 5 DC high voltage power supply (for internal electrodes) 6. Slip ring 7. Belt-shaped support (web) 8 Applicator (application head) 9. Curtain of coating fluid 10 Coating liquid contact line (coating point) 11 Wet Coating Layer 12 Web 1st side (front side) 13 Web 2nd side (back side) 14 Spatial auxiliary electrode(-) 15 DC high voltage power supply (for space auxiliary electrode) 16 Roll core 17 Free charge (+) 18 Dipoles inside the web 19 Surface charge(-)
Claims
1. A method for applying a coating liquid comprising a liquid composition to a continuously moving flexible plastic-based web having opposed first and second surfaces by flowing the coating liquid from an applicator grounded on a first surface of the web, the method comprising the steps of: a step of conveying the web along a path to a backing roll for coating, and passing the web through a coating point while supporting a second surface of the web by being in close contact with a portion of the surface of the rotating backing roll to which a DC voltage is applied, by an electrostatic field of the backing roll; and applying the coating liquid to the first surface of the web by electrostatic force generated by the arrangement of charges of the same polarity as the DC voltage applied to the backing roll on the first surface of the web, by attracting the coating liquid at the coating point, The backing roll is provided with an outermost layer to which the web is in close contact, a conductive monopolar internal electrode layer adjacent to the inner side of the outermost layer, and an insulating layer adjacent to the inner side of the internal electrode layer, and the backing roll is configured to be able to apply a predetermined voltage to the internal electrode layer, and the outermost layer has a volume resistivity of 10 7 ~10 13 a ceramic material layer of Ωcm, the surface of the backing roll being charged with a charge of the same sign as the voltage applied to the internal electrode when the predetermined voltage is applied to the internal electrode layer, the second surface of the web in contact with the outermost layer by the electrostatic force of the charge is brought into close contact with the outermost layer and rotated to be transported, and the coating liquid is attracted to and brought into contact with a first surface of the web during rotation and transport, and deposited on the first surface of the web.
2. 2. The coating method according to claim 1, wherein a charge having a polarity opposite to that of the DC voltage applied to the internal electrode layer is applied to a first surface of the web opposite to the second surface before the coating liquid comes into contact with the web during rotational transport.
3. The coating method according to claim 1, wherein a DC voltage applied to the internal electrode layers is 0.3 to 6.0 KV.
4. The coating method according to claim 1 , wherein the backing roll has a diameter of 100 mm or more.
5. 2. The coating method according to claim 1, wherein at least one of the insulating layer, the internal electrode layer, and the outermost layer is made of a material formed by a thermal spraying method or a material using either an inorganic or organic binder, and at least one of the insulating layer, the internal electrode layer, and the outermost layer of the backing roll is subjected to a sealing treatment.
6. 2. The coating method according to claim 1, wherein the outermost layer is made of a ceramic material, and the ceramic material is an alumina-based, zirconium oxide-based, or magnesium oxide-based ceramic containing a compound selected from titanium oxide, chromium oxide, silicon oxide, manganese oxide, nickel oxide, and iron oxide, or an aluminum oxide-based ceramic containing 5 to 17% by weight of titanium oxide.
7. 2. The coating method according to claim 1, wherein the ceramic material comprises at least one selected from an aluminum nitride material, a silicon carbide material, and a silicon nitride material, and an organic or inorganic binder.
8. The coating method according to claim 1, wherein the outermost layer has a thickness of 50 to 500 μm.
9. The coating method according to claim 1, wherein the outermost layer of the backing roll has a center line average surface roughness Ra of 0.01 μm to 5 μm.
10. The coating method according to claim 1 , wherein the internal electrode layers are made of a conductive material containing tungsten or molybdenum.
11. The coating method according to claim 1, wherein the internal electrode layer has a thickness of 5 to 50 μm.
12. 2. The coating method according to claim 1, wherein the insulating layer comprises at least one highly insulating material selected from aluminum oxide, aluminum oxide-based materials containing 2 to 4% by weight of titanium oxide, magnesium oxide-based materials, beryllium oxide-based materials, aluminum nitride-based materials, ceramic materials containing silicon nitride, porcelain, and enamel.
13. The volume resistivity of the insulating layer is 10 13 The coating method according to claim 1 , wherein the resistivity is Ωcm or more.
14. The coating method according to claim 1, wherein the insulating layer has a thickness of 50 to 500 μm.
Citation Information
Patent Citations
Electrostatically assisted coating method and apparatus using concentrated electrode fields
JP2003530215A
Charging method, manufacturing method of web wounded body and charging apparatus
JP2020158605A
Coating process
US20030138572A1
Cooling roll and method for producing thermoplastic resin sheet using same
WO2019116600A1
JP1971027423Y1