Molybdenum target and manufacturing method of the same

A high-density, precisely controlled molybdenum target with optimized manufacturing processes addresses particle generation issues, ensuring stable and high-quality film formation in semiconductor manufacturing.

JP2024164771AActive Publication Date: 2024-11-27ULVAC INC
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2023080476
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-15
Publication Date
2024-11-27
Estimated Expiration
2043-05-15

AI Technical Summary

Technical Problem

Existing molybdenum targets used in semiconductor manufacturing generate a high number of particles during sputtering, leading to reduced yield and quality issues, despite efforts to improve purity and density, as pores and uncontrolled crystal grain size contribute to particle generation.

Method used

A molybdenum target with a relative density of 99% or more, controlled pore size and distribution, and precise grain size and hardness variations, manufactured through specific hot pressing and hot isostatic pressing processes, to minimize particle generation.

Benefits of technology

The solution significantly reduces particle generation, enabling stable production of high-quality molybdenum films with low resistivity and consistent film formation rates, improving yield and reducing particle counts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024164771000004
    Figure 2024164771000004
  • Figure 2024164771000005
    Figure 2024164771000005
  • Figure 2024164771000006
    Figure 2024164771000006
Patent Text Reader

Abstract

To provide a molybdenum target suppressing a generation of a pore as a cause of the generation of particles, and controlling a size and a distribution of the pore with high precision, and a manufacturing method of the target.SOLUTION: A molybdenum target formed with a sintered body of a molybdenum powder has a relative density of 99% or more, an oxygen content of 25 ppm or less, a carbon content of 30 ppm or less, a tungsten content of 10 ppm to 100 ppm, and a molybdenum content excluding the oxygen content, the carbon content, and the tungsten content of 99.999 mass% or more. In an observation area of 0.15 mm2, the molybdenum target has 20 or less pores with a size of 0.01 μm2 or more and less than 0.2 μm2, 5 or less pores with a size of 0.2 μm2 or more and less than 1.8 μm2, and one or less pores with a size of 1.8 μm2 or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a molybdenum target formed of a sintered body of molybdenum powder and a method for producing the same. [Background technology]

[0002] In recent years, in the field of semiconductor device manufacturing, tungsten, which has heat resistance and low resistance characteristics, is widely used as a wiring material or electrode material. Tungsten films are generally formed by sputtering. In sputtering of tungsten films, argon ions generated by plasma discharge are collided with a tungsten target to knock out tungsten atoms from the target surface, and the tungsten atoms are deposited on a substrate arranged opposite the target. At this time, it is known that a major problem in the process is that particles generated from the target surface adhere to the substrate, reducing the yield. For this reason, it is essential that the tungsten target has extremely low particle generation, fine and uniform crystal grains, and high relative density.

[0003] However, even if a high-purity tungsten film can be formed, there is a concern that it may not be able to meet the future demand for even lower resistance. Therefore, it is necessary to find a promising material to replace tungsten. In this regard, molybdenum films have attracted attention as they may be able to achieve sufficiently low electrical resistance values. However, they are also known to have a problem in that they generate a high rate of particles during sputtering, which reduces the material yield.

[0004] Thus, a molybdenum sputtering target capable of effectively reducing particles during sputtering has been proposed, which has a molybdenum content of 99.99 mass % or more, a relative density of 98% or more, and an average crystal grain size of 400 μm or less, and a method for manufacturing a sputtering target has been proposed, which includes the steps of preparing molybdenum powder, hot pressing the molybdenum powder under a load at a temperature of 1350°C to 1500°C, and hot isostatically pressing the compact obtained by the hot pressing at a temperature of 1300°C to 1850°C (see Patent Document 1). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2022-125041 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, it has been found that even the technique of Patent Document 1 cannot sufficiently reduce the generation of particles from the molybdenum target. In particular, as wiring and the like using molybdenum becomes finer, particles generated from the molybdenum target have a significant effect on yield, and therefore there is a demand for further suppression of particle generation.

[0007] Therefore, the researchers studied the causes of particles that occur when forming a film by sputtering a molybdenum target, and found that, although the target manufactured by the above-mentioned manufacturing method has a relative density of the sintered body that reaches just under 100%, pores are inevitably present and, because the size and distribution of pores are not controlled, particle generation cannot be suppressed, resulting in reduced yields.

[0008] Therefore, in order to improve the yield, a molybdenum target that generates as few particles as possible is required, and a manufacturing method that can obtain such a molybdenum target is required.

[0009] In view of the above circumstances, an object of the present invention is to provide a molybdenum target in which the generation of pores, which are a cause of particle generation, is suppressed and the size and distribution of the pores are controlled with high precision, and a method for manufacturing the same. [Means for solving the problem]

[0010] In order to achieve the above object, a first aspect of the present invention is a molybdenum target formed of a sintered body of molybdenum powder, the molybdenum target having a relative density of 99% or more, an oxygen content of 25 ppm or less, a carbon content of 30 ppm or less, a tungsten content of 10 ppm to 100 ppm, a molybdenum content excluding the oxygen content, the carbon content, and the tungsten content of 99.999 mass% or more, and a surface roughness of 0.15 mm 2 In the observation area, 0.01 μm 2 More than 0.2μm 2 There are 20 or less pores with a size of less than 0.2 μm 2 More than 1.8μm 2 There are 5 or fewer pores with a size of less than 1.8 μm 2 The molybdenum target has one or less pores of a size equal to or larger than the diameter of the target.

[0011] The second aspect of the present invention is an average particle diameter d calculated based on a circle equivalent diameter. Ave is 20μm or more and 100μm or less, and the standard deviation 3σ of the particle size calculated using the circle equivalent diameter and the average particle size d Ave Ratio to (3σ / d Ave ) is 1.2 or less.

[0012] A third aspect of the present invention is the molybdenum target according to the second aspect, in which the average aspect ratio of the grain size is less than 1.2.

[0013] In the fourth aspect of the present invention, the average Vickers hardness is 180 or less, and the standard deviation 3σ of the Vickers hardness and the average Vickers hardness H Ave Ratio to (3σ / H Ave ) is 0.07 or less.

[0014] The fifth aspect of the present invention is a method for producing a granular material having an average particle size D obtained by a laser diffraction / scattering method. Ave The median diameter D90 and the average particle diameter D Ave Ratio to (D90 / D Ave ) is 1.7 or less, and the median diameter D95 and the average particle diameter D Ave Ratio to (D95 / D Ave ) is 2.0 or less, hot-pressed at a temperature of 1400°C to 1500°C, and then sintered by hot isostatic pressing at a temperature of 1500°C to 1600°C.

[0015] A sixth aspect of the present invention is the method for producing a molybdenum target according to the fifth aspect, wherein the molybdenum powder has a tungsten content of 10 ppm to 100 ppm, and a molybdenum content excluding the oxygen content, the carbon content, and the tungsten content is 99.999 mass % or more.

[0016] A seventh aspect of the present invention is the method for producing a molybdenum target according to the fifth or sixth aspect, wherein the hot pressing is carried out under high vacuum at a holding temperature of 1400 to 1500° C. for a holding time of 360 to 600 minutes. Effect of the Invention

[0017] According to the present invention, it is possible to realize a molybdenum target and a manufacturing method thereof in which the generation of pores, which are a cause of particle generation, is suppressed and the size and distribution of the pores are controlled with high precision. [Brief description of the drawings]

[0018] [Figure 1]FIG. 2 is a diagram showing the relationship between the number of pores of 0.01 to 0.2 μm 2 and the number of particles in the examples of the present invention and the comparative examples. [Diagram 2] FIG. 2 is a graph showing the relationship between the number of pores of 0.2 to 1.8 μm2 and the number of particles in the examples of the present invention and the comparative examples. [Diagram 3] FIG. 1 is a diagram showing the relationship between the number of pores having a size of 1.8 μm or more and the number of particles in an embodiment of the present invention and a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The molybdenum target of the present invention has a molybdenum purity (content) of 5N (99.999 mass%) or more, a relative density of 99% or more, an oxygen content of 25 ppm or less, a carbon content of 30 ppm or less, a tungsten content of 10 ppm to 100 ppm, and a thickness of 0.15 mm. 2 In the observation area, 0.01 μm 2 More than 0.2μm 2 There are 20 or less pores with a size of less than 0.2 μm 2 More than 1.8μm 2 There are 5 or fewer pores with a size of less than 1.8 μm 2 The number of pores of a size equal to or larger than 1. Note that the 5N purity of molybdenum means that the molybdenum content excluding the oxygen content, carbon content, and tungsten content is 99.999 mass% or more.

[0020] (purity) To form a molybdenum film with low resistivity, it is necessary to suppress the impurities contained in the molybdenum film, and therefore it is essential to highly purify the molybdenum target. Specifically, it is necessary for the molybdenum target to have a purity of 99.999 mass% (5N) or more.

[0021] (Gas composition) Gas components such as carbon and oxygen contained in a molybdenum target adversely affect the resistivity of a molybdenum film. These gas components are incorporated into the molybdenum film during film formation, and the resistivity of the molybdenum film tends to increase as the content of these gas components increases. Therefore, the carbon content of the molybdenum target is preferably 30 ppm by mass or less, and the oxygen content is preferably 25 ppm by mass or less.

[0022] (tungsten content) The molybdenum target of the present invention has a tungsten content of 10 ppm to 100 ppm, and preferably 20 ppm to 50 ppm.

[0023] The reason for setting the tungsten content in this range is as follows. Normally, the tungsten content is reduced to an unavoidable level, but in the present invention, the tungsten content is set within a predetermined range. If the tungsten content is too low, grain growth is likely to occur during sintering, the crystal grain size becomes large, and large pores are likely to be formed. On the other hand, if the tungsten content is too high, sinterability becomes poor, and it tends to be difficult to achieve high density.

[0024] (crystal grain size) The molybdenum target of the present invention has an average crystal grain size d calculated based on the circle equivalent diameter. Ave is 20 μm or more and 100 μm or less.

[0025] The reason for setting such an average value of the crystal grain size (average grain size) is as follows. The smaller the average grain size of the molybdenum target, the smaller the difference in the amount of erosion caused by the orientation difference of each crystal grain on the target surface can be, so that the number of abnormal discharges caused by unevenness is reduced and the generation of particles during film formation can be suppressed.

[0026] On the other hand, if the average grain size is too small, the film formation rate becomes too slow, resulting in a decrease in productivity.

[0027] In addition, the standard deviation 3σ of the particle size calculated using the circle equivalent diameter and the average particle size d Ave Ratio to (3σ / d Ave ) is 1.2 or less. This ratio is calculated by dividing the standard deviation 3σ by the average particle size. In addition, the aspect ratio of the particle size is less than 1.2. This aspect ratio is the value obtained by dividing the long diameter of the particle image by the short diameter to determine the "particle size calculated using the circle equivalent diameter," and was calculated using the image analysis software "Image-j."

[0028] Standard deviation 3σ of grain size and average grain size d Ave Ratio to (3σ / d Ave ) is preferably 1.2 or less for the following reasons. There is a correlation between the variation in crystal grain size and the number and size of pores. The smaller the variation in crystal grain size, the fewer the number of pores in the target and the smaller their size. Therefore, within the above range, the generation of particles during film formation can be suppressed. The aspect ratio of the grain size is preferably less than 1.2 because it provides a stable deposition rate that does not adversely affect production, and the deposition rate is unlikely to change even when the target is replaced.

[0029] (Relative Density) The relative density of the molybdenum target is preferably 99% or more. If the relative density of the target is 99% or more, the amount of gas components contained in the target is small, so that when a film is formed, the increase in the resistivity of the film can be suppressed. In addition, the higher the relative density of the target, the fewer the number of pores, so that the number of abnormal discharges caused by the unevenness of the target surface is reduced, and the generation of particles during film formation can be suppressed.

[0030] (Vickers hardness) The average Vickers hardness of the molybdenum target is preferably 160 or more and 180 or less, and more preferably 165-175.

[0031] The reason why the average value of the Vickers hardness is preferably within the above range is as follows. There is a correlation between the average Vickers hardness and the number and size of pores in a target. The higher the average Vickers hardness, the fewer the number and smaller the size of pores in the target, making it possible to suppress particle generation during film formation.

[0032] On the other hand, if the average Vickers hardness is very high, it is highly likely that the heat treatment conditions were not appropriate and that the internal strain in the molybdenum was not removed. This internal strain can become the starting point for cracks due to thermal stress during target processing or deposition by sputtering.

[0033] In addition, the standard deviation 3σ of Vickers hardness and the average value H Ave Ratio to (3σ / H Ave ) is preferably 0.07 or less. The calculation method is to divide the standard deviation 3σ by the average value of the Vickers hardness.

[0034] The reason why the ratio of three times the standard deviation (3σ) of the Vickers hardness to the average value of the Vickers hardness is preferably within the above-mentioned range is as follows.

[0035] There is a correlation between the variation in Vickers hardness and the number and size of pores. The smaller the variation in Vickers hardness, the fewer the number and size of pores in the target, making it possible to suppress particle generation during film formation.

[0036] (Poa) The molybdenum target of the present invention is 0.15 mm 2 In the observation area, 0.01 μm 2 More than 0.2μm 2 There are 20 or less pores with a size of less than 0.2 μm 2 More than 1.8μm 2 There are 5 or fewer pores with a size of less than 1.8 μm 2 There is less than one pore of this size or larger.

[0037] The reasons for setting the size and number of the particles in the above-mentioned ranges in the present invention are as follows. By controlling the size and number of pores, the electric field is concentrated in the pores, which suppresses the generation of particles due to localized dissolution and scattering, improving yield. In addition, the number of particles generated remains low until the end of the target's life, realizing stable production.

[0038] A molybdenum target having extremely few coarse pores and suppressed pore localization in the surface direction and thickness direction of the molybdenum target has not been realized so far, but it can be realized by having the above-mentioned relative density, hardness and crystal grain size characteristics. Also, the molybdenum target of the present invention having extremely few coarse pores and suppressed pore localization in the surface direction and thickness direction of the molybdenum target can be realized by the manufacturing method described below.

[0039] As described above, the molybdenum target of the present invention has small and few pores. Therefore, by using this molybdenum target, the amount of particles generated can be significantly reduced, and a high-quality molybdenum film can be stably formed.

[0040] A method for producing a molybdenum target according to an embodiment of the present invention will be described.

[0041] The molybdenum target of the present invention has an average grain size D Ave It can be manufactured by hot pressing molybdenum powder having a diameter of 2.5 to 4.0 μm and a median diameter D50 of 2.0 to 3.5 at a temperature of 1400°C to 1500°C (HP process), and then sintering the same by hot isostatic pressing at a temperature of 1500°C to 1600°C (HIP process).

[0042] The method for producing a sputtering target of the present invention is to obtain an average particle diameter D AveThe first point is to use molybdenum powder having a particle size of 2.5 to 4.0 μm, preferably 2.8 to 3.7 μm, and a median diameter D50 of 2.0 to 3.5, preferably 2.2 to 3.3 μm.

[0043] In addition, the method for producing a sputtering target of the present invention is capable of determining the median diameter D90 and the average particle diameter D Ave Ratio to (D90 / D Ave The second point is to use molybdenum powder having a molybdenum content of 1.7 or less, preferably 1.5 or less.

[0044] In addition, the method for producing a sputtering target of the present invention is similar to the method for producing a sputtering target of the present invention. Ave and ratio (D95 / D Ave The third point is to use tungsten powder with a refractive index of 2.0 or less, preferably 1.8 or less.

[0045] In this way, the present invention uses a molybdenum powder having a particle size within a specified range and an extremely narrow particle size distribution range, i.e., a small variation in particle size from the average particle size, thereby making it possible to realize a molybdenum target having extremely small and few pores. In the present invention, such a feature of a narrow particle size distribution is realized by multiplying the median diameter D90 by the average particle size D obtained by a laser diffraction / scattering method. Ave The value divided by the median diameter D95 and the average particle size D obtained by the laser diffraction / scattering method are Ave It is defined that the value obtained by dividing the particle size distribution by the particle diameter is equal to or less than a predetermined value. Note that powders having a wide particle size distribution outside this range cannot achieve the effects of the present invention.

[0046] Furthermore, if the average particle size of the powder is too large, a sintered body with the specified density cannot be obtained, whereas if it is too small, the density will rise rapidly during hot pressing (HP) and oxides will be trapped, so it is necessary to keep the particle size within a specified range.

[0047] The molybdenum powder used in the present invention has a tungsten content of 10 ppm to 100 ppm, and a molybdenum content excluding the oxygen content, the carbon content, and the tungsten content is 99.999 mass % or more.

[0048] In addition, since the oxygen content affects the oxygen content of the molybdenum target, it is preferable that the oxygen content of the raw material powder is, for example, 3000 mass ppm or less, since the amount of oxide sublimation increases, which may damage the hot press device.

[0049] The sputtering target of the present invention can be produced by hot pressing the above-mentioned molybdenum powder at a temperature of 1400°C or higher and 1500°C or lower, and then sintering it by hot isostatic pressing at a temperature of 1500°C or higher and 1600°C or lower.

[0050] By vacuum hot pressing in a high vacuum region, degassing and sintering can be promoted, and a high-density sintered body can be obtained while reducing the amount of oxygen contained in the molybdenum target. If the oxygen content of the molybdenum powder is high, the number of oxides in the molybdenum target increases, and the frequency of particle generation increases. In addition, sintering is inhibited by a thick surface oxide film, making it impossible to obtain a high-density sintered body.

[0051] Here, high vacuum is 1×10 -2 Pa or less, preferably 1×10 -3 Pa or less, more preferably 1×10 -4 Pa or less.

[0052] As described above, gas components such as carbon and oxygen contained in the molybdenum target adversely affect the resistivity of the molybdenum film, so the carbon content in the molybdenum target is preferably 30 ppm by mass or less, and the oxygen content is preferably 25 ppm by mass or less.

[0053] The oxygen concentration can be achieved by vacuum hot pressing as described above.

[0054] On the other hand, regarding the carbon concentration, during hot pressing, carbon diffuses from the graphite members constituting the hot pressing apparatus into the molybdenum sintered body, causing an increase in the carbon content. Therefore, the lower the hot pressing temperature, the better, and at 1500°C or less, a stable carbon concentration of 30 mass ppm or less, preferably 20 mass ppm or less, can be achieved.

[0055] In the HP process, a sintered body having a relative density of 95% or more is produced. The HP temperature for producing a sintered body having such characteristics is preferably 1400°C or higher and 1500°C or lower. If the HP temperature is too low, the density does not rise to a level at which HIP treatment is possible, and if it is too high, coarse pores are formed locally due to rapid grain growth, which is undesirable. If the HP pressure is too low, the density does not rise to a level at which HIP treatment is possible. If it is too high, the HP equipment will wear out rapidly. For example, the pressure during HP treatment is 39.2 MPa (400 kg / cm 2 ) or more 44.1MPa (450kg / cm 2 ) or less. The HP holding time in this process is 360 minutes or more and 600 minutes or less. If the HP holding time is too short, the density will not increase to a level at which HIP processing is possible, and if it is too long, productivity will decrease. In the present invention, it is essential to control the powder particle size and particle size distribution, set the HP temperature to 1400°C or more and 1500°C or less, and set the HP holding time to 360 minutes or more and 600 minutes or less. This makes it possible to prevent the pores in the sintered body from becoming coarse and to uniformly disperse fine pores in the sintered body.

[0056] Hot isostatic pressing (HIP) is applied to the sintered body after HP treatment to reduce pores in the sintered body and to increase density.

[0057] The HIP temperature is 1500°C or higher and 1600°C or lower. If the HIP temperature is lower than 1500°C, it is difficult to obtain a high relative density of 99% or higher within a processing time suitable for mass production due to the low processing temperature. In particular, in the present invention, since a molybdenum powder with a tungsten content within a specified range is used, a sintered body with a relative density of 99% or higher cannot be obtained at a temperature lower than 1500°C. In addition, if the HIP temperature exceeds 1600°C, the high processing temperature leads to rapid coarsening of the crystal grains, and coarse pores are formed locally, which is not preferable. The pressure is not particularly limited and is, for example, 100 to 200 MPa, and in this embodiment, it is 176.4 MPa (1800 kg / cm 2 ).

[0058] According to the above manufacturing method, a molybdenum target having the characteristics of the present invention can be obtained. In particular, the number of pores in the molybdenum target can be reduced, the size of the pores can be reduced, and localization of the pores can be suppressed. Therefore, by using the sputtering target of this embodiment, it is possible to reduce particle generation during film formation, and it is possible to stably form a high-quality molybdenum film.

[0059] The presence of pores in a sputtering target is strongly correlated with the size of the raw material powder and its particle size distribution, the relative density of the sintered body, the size and distribution of the crystal grain size of the target, and the size and distribution of hardness. The finer the size of the raw material powder and the narrower the range of its particle size distribution, the higher the relative density of the sintered body, and the smaller the variation in crystal grain size and hardness, the more significantly the occurrence of pores is reduced and the size of the pores becomes extremely small.

[0060] On the other hand, even if the crystal grain size is fine, if the variation is large, the generation of coarse pores cannot be suppressed. The present invention has found that the molybdenum target of the present invention can be manufactured with very few coarse pores and almost no localization of pores by optimizing the size and particle size distribution of the raw material powder, the hot pressing conditions, and the hot isostatic pressing conditions to increase the relative density of the sintered body and suppress the variation in crystal grain size and hardness.

[0061] That is, in the method for producing a molybdenum target of this embodiment, the raw material powder is hot pressed at a temperature of 1400° C. to 1500° C., and then sintered by hot isostatic pressing at a temperature of 1500° C. to 1600° C.

[0062] According to the above-mentioned method for producing a molybdenum target, it is possible to obtain a sputtering target having small and few pores. 2 In the observation area, 0.01 μm 2 More than 0.2μm 2 There are 20 or less pores with a size of less than 0.2 μm 2 More than 1.8μm 2 There are 5 or fewer pores with a size of less than 1.8 μm 2 It is possible to stably produce molybdenum targets having one or less pores of the above size.

[0063] In the method for producing a molybdenum target of the present invention, the relative density is 99% or more, the Vickers hardness is 180 or less, and the standard deviation 3σ of the Vickers hardness and the average value H Ave Ratio (3σ / H Ave ) is 0.07 or less, the average grain size is 20 μm or more and 100 μm or less, the standard deviation 3σ of the average grain size and the average grain size H Ave Ratio to (3σ / H Ave ) of 1.2 or less can be efficiently and stably produced.

[0064] This makes it possible to manufacture a molybdenum target with small and few pores. By using this molybdenum target, the amount of particles generated can be significantly reduced, making it possible to stably form a high-quality molybdenum film.

[0065] The sintered body produced as described above is processed into a predetermined target shape in a processing step. Although the processing method is not particularly limited, typically, mechanical processing methods such as grinding and cutting are applied. The processing size and shape are determined according to the specifications of the target, and are processed into, for example, a circular or rectangular shape. The processed sintered body is bonded to a backing plate to form a sputtering cathode. EXAMPLES

[0066] The present invention will be described below with reference to examples and comparative examples. The average particle size and particle size distribution of the molybdenum powder were determined using a particle size distribution measuring device "LS13320" manufactured by Microtrackbell.

[0067] (Examples 1 to 4) As shown in Table 1, the tungsten content is 10 ppm to 100 ppm, the molybdenum content excluding tungsten and gas content is 99.999 mass% or more (purity 5N), and the average particle size D obtained by the laser diffraction / scattering method is Ave The median diameter D90 and the average particle diameter D Ave Ratio to (D90 / D Ave ) is 1.7 or less, and the median diameter D95 and the average particle diameter D Ave Ratio to (D95 / D Ave A molybdenum powder having a melting point of 2.0 or less was used, and the powder was hot pressed at a temperature shown in Table 1, 1400°C or more and 1500°C or less, and then a molybdenum sintered body was obtained by HIPing at a temperature shown in Table 1, 1500°C or more and 1600°C or less. The obtained molybdenum sintered body was ground on a lathe to give a predetermined target shape (diameter 440 mm, thickness 6 mm).

[0068] Comparative Example 1 As shown in Table 1, the average particle size D obtained by the laser diffraction / scattering method Ave is smaller than 2.5 μm, the median diameter D50 is smaller than 2.0 μm, and the median diameter D90 and the average particle diameter D Ave Ratio to (D90 / DAve ) is 1.7 or less, and the median diameter D95 and the average particle diameter D Ave Ratio to (D95 / D Ave Molybdenum powder with a porosity of 2.0 or less was used and hot pressed at the temperatures shown in Table 1 to obtain a molybdenum sintered body. The particle size of the molybdenum powder was too small, causing a sudden increase in density and trapping a large amount of oxide.

[0069] Comparative Example 2 As shown in Table 1, the average particle size D obtained by the laser diffraction / scattering method Ave The median diameter D90 and the average particle diameter D Ave Ratio to (D90 / D Ave ) is 1.7 or less, and the median diameter D95 and the average particle diameter D Ave Ratio to (D95 / D Ave ) of 2.0 or less was used, and a molybdenum sintered body was obtained by hot pressing the molybdenum powder at the temperature shown in Table 1. Since HIP was not performed, a sintered body with sufficient density was not obtained.

[0070] (Comparative Example 3-8) As shown in Table 1, the average particle size D obtained by the laser diffraction / scattering method Ave is smaller than 2.5 μm, the median diameter D50 is smaller than 2.0 μm, and the median diameter D90 and the average particle diameter D Ave Ratio to (D90 / D Ave ) is 1.7 or less, and the median diameter D95 and the average particle diameter D Ave Ratio to (D95 / D Ave Molybdenum powder having a porosity of 2.0 or less was used, hot pressed at the temperatures shown in Table 1, and then HIP was performed to obtain a molybdenum sintered body. The obtained molybdenum sintered body was ground on a lathe to give the specified target shape (diameter 440 mm, thickness 6 mm).

[0071] Comparative Example 9 As shown in Table 1, the average particle size D obtained by the laser diffraction / scattering method AveThe median diameter D90 and the average particle diameter D Ave Ratio to (D90 / D Ave ) is 1.7 or more, and the median diameter D95 and the average particle diameter D Ave Ratio to (D95 / D Ave Molybdenum powder having a porosity of 2.0 or more was used, hot pressed at the temperatures shown in Table 1, and then HIP was performed to obtain a molybdenum sintered body. The obtained molybdenum sintered body was ground on a lathe to give the specified target shape (diameter 440 mm, thickness 6 mm).

[0072] Comparative Example 10 As shown in Table 1, the average particle size D obtained by the laser diffraction / scattering method Ave is greater than 4.0 μm, the median diameter D50 is 2.0 to 3.5 μm, and the median diameter D90 and the average particle diameter D Ave Ratio to (D90 / D Ave ) is 1.7 or less, and the median diameter D95 and the average particle diameter D Ave Ratio to (D95 / D Ave Molybdenum powder having a porosity of 2.0 or more was used, hot pressed at the temperatures shown in Table 1, and then HIP was performed to obtain a molybdenum sintered body. The obtained molybdenum sintered body was ground on a lathe to give the specified target shape (diameter 440 mm, thickness 6 mm).

[0073] (Comparative Examples 11-13) As shown in Table 1, the average particle size D obtained by the laser diffraction / scattering method Ave is larger than 4.0 μm, the median diameter D50 is larger than 3.5 μm, and the median diameter D90 and the average particle diameter D Ave Ratio to (D90 / D Ave ) is 1.7 or more, and the median diameter D95 and the average particle diameter D Ave Ratio to (D95 / D AveMolybdenum powder having a porosity of 2.0 or more was used, hot pressed at the temperatures shown in Table 1, and then HIP was performed to obtain a molybdenum sintered body. The obtained molybdenum sintered body was ground on a lathe to give the specified target shape (diameter 440 mm, thickness 6 mm).

[0074] (Examples and Comparative Examples) The obtained targets were subjected to measurements of relative density, Vickers hardness, crystal grain size, tungsten content, oxygen content, carbon content, and pores according to the following procedures. The results are shown in Tables 2 and 3.

[0075] (Relative Density) Samples measuring 10 × 10 × 6 mm were taken from the center, edge, and halfway along the line connecting the center and edge of the obtained molybdenum target. The cross section of each sample was polished and etched, and the specific gravity was calculated using the Archimedes method to obtain the theoretical density of molybdenum (10.23 g / cm 3 The relative density of each sample was added and divided by the number of samples to obtain a value, which was defined as the relative density of the molybdenum target according to the present invention.

[0076] (Vickers hardness) Samples of 10×10×6 mmt were taken from the center, end, and halfway along the line connecting the center and end of the obtained molybdenum target, and the cross section of each sample was polished, and hardness was measured three times at 1 mm intervals in the depth direction of the target using a Mitutoyo Vickers hardness tester "HM-200" under a load of 1 kg and a load time of 15 seconds, using a Mitutoyo Vickers hardness tester "HM-200". The average value of the obtained values ​​was calculated by adding up the average values ​​calculated for each sample and dividing the result by the number of samples, which was taken as the hardness of the molybdenum target according to the present invention. Furthermore, the standard deviation of the molybdenum target was calculated by adding up the standard deviations calculated from each sample and dividing the result by the number of samples, which was taken as the standard deviation according to the present invention.

[0077] (crystal grain size) Samples of 10 x 10 x 6 mmt were taken from the center, end, and half of the line connecting the center and end of the obtained molybdenum target, and the cross section of each sample was polished and etched. Images were taken at 1 mm intervals in the depth direction of the target using an optical microscope "Digital Microscope VHX-6000" manufactured by Keyence Corporation, and the circle equivalent diameter was obtained using image analysis software "Image-j" and the average value was calculated. The average values ​​calculated for each test piece were added together and divided by the number of samples to obtain the average grain size of the molybdenum target according to the present invention. Furthermore, the standard deviation of the molybdenum target was determined by adding the standard deviations obtained from each sample and dividing the result by the number of samples to obtain the standard deviation according to the present invention.

[0078] (oxygen content) When processing the molybdenum sintered body into a target shape, an analysis sample was taken and the oxygen content of the compact was measured. The oxygen content was analyzed using the LECO analyzer "TC-600."

[0079] (Carbon content) When processing the molybdenum sintered body into a target shape, an analysis sample was taken and the carbon content of the compact was measured. The carbon content was analyzed using the HORIBA EMIA-320V analyzer.

[0080] (Poa) Samples of 10 x 10 x 6 mmt were taken from the center, end, and halfway along the line connecting the center and end of the obtained sputtering target, and after polishing the cross section of each sample, two SEM images were taken at 1 mm intervals in the depth direction of the target using an electron microscope "TM4000Plus" manufactured by Hitachi High-Technologies Corporation. The pore area of ​​the taken SEM images was calculated using image analysis software "Image-j", and the size and number of pores in each sample were calculated. The size and number of pores calculated for each sample were added together and divided by the number of samples to determine the size and number of pores of the molybdenum target according to the present invention.

[0081] Using the obtained targets of the examples and comparative examples, films were formed as follows, and the resistivity of the films was measured as follows, and particles were evaluated as follows.

[0082] The results of Examples 1 to 4 and Comparative Examples 1 to 13 are shown in Table 3, and the relationship between the number of pores of a given size and the number of particles is shown in Figures 1 to 3. Resistivity of 11 μΩ·cm or less was marked as O, and that exceeding 11 μΩ·cm was marked as X. If the resistivity is 11 μΩ·cm or less, low-resistance LSI wiring can be formed, making it possible to realize devices with low power consumption. A film thickness distribution of 2% or less was marked as O, and a distribution exceeding 2% was marked as X. If the film thickness distribution is 2% or less, devices with little variation in performance and quality can be produced stably.

[0083] (Resistivity measurement) The obtained molybdenum target was bonded to an aluminum alloy backing plate with an In-based solder to form a sputtering cathode. The sputtering cathode was assembled in an ULVAC sputtering device "ENTRON (registered trademark)" to form a molybdenum thin film with a thickness of 10 nm on a semiconductor wafer with a diameter of 300 mm. The sputtering conditions were: ultimate pressure: 1×10 -5 Pa, discharge method: DC, power: 4 kW, gas source: Ar, gas flow rate: 150 sccm, film formation temperature: 200° C., sputtering time: 5 seconds, and distance between target and wafer: 60 mm.

[0084] The film thickness was measured at nine points on the molybdenum thin film on the wafer using a TECHNORAYS S-MAT2300, and the sheet resistance was measured using a KLATencor OmniMap RS100 to calculate the resistivity (μΩ cm) of the thin film. The average value was used as the resistivity of the molybdenum thin film.

[0085] (Particle Measurement) The surface of the molybdenum thin film on a semiconductor wafer with a diameter of 300 mm was inspected using a surface inspection device "WM-10" manufactured by TOPCON Corporation for the 10 nm thick molybdenum thin film used for resistivity measurement, and the number of particles with a size of 0.065 μm or more was counted. 2 This is the number of winning pieces, with 20 or less being considered preferable, and 15 or less being considered even more preferable.

[0086] (Measurement of film thickness distribution) The film thickness of the molybdenum thin film on the wafer was measured at 49 points using a TECHNORAYS S-MAT2300, and the film thickness was calculated using the following formula. Film thickness distribution (%) = (maximum value - minimum value) / (maximum value + minimum value) x 100

[0087] [Table 1]

[0088] [Table 2]

[0089] [Table 3]

[0090] As shown in Examples 1 to 4, the tungsten content is 10 ppm to 100 ppm, the molybdenum content excluding the tungsten and gas content is 99.999 mass% or more (purity 5N), and the average particle size D obtained by the laser diffraction / scattering method is Ave The median diameter D90 and the average particle diameter D Ave Ratio to (D90 / D Ave ) is 1.7 or less, and the median diameter D95 and the average particle diameter D Ave Ratio to (D95 / D AveA molybdenum powder having a porosity of 2.0 or less was used, and the powder was hot pressed at a temperature of 1400°C to 1500°C, and then HIPed at a temperature of 1500°C to 1600°C to obtain a molybdenum sintered body. The obtained molybdenum sintered body had a relative density of 99% or more and a porosity of 0.15 mm 2 In the observation area, 0.01 μm 2 More than 0.2μm 2 There are 20 or less pores with a size of less than 0.2 μm 2 More than 1.8μm 2 There are 5 or fewer pores with a size of less than 1.8 μm 2 It is possible to obtain a molybdenum target having one or less pores of a size equal to or larger than this. By using such a molybdenum target, it is possible to suppress particle generation and stably form a high-quality molybdenum thin film.

[0091] In addition, in Examples 1 to 4, the hot pressing temperature was low at 1500° C. or less, so the carbon content of the target was sufficiently low, making it possible to form a thin film having a sufficiently low resistivity of 11 μΩ·cm or less.

[0092] In Comparative Example 1, the powder was too fine and contained a large amount of oxygen, so the density rose sharply during HP and oxides were trapped, while in Comparative Example 2, the density was insufficient because HIP was not performed. In Comparative Examples 3 and 4, the tungsten content and oxygen content were high, resulting in high resistivity. In addition, the raw powder was too fine, resulting in a sudden increase in density during HP, and the HP temperature was low, resulting in oxides remaining without sublimation. In Comparative Example 3, abnormal grain growth occurred due to the high HIP temperature, and in Comparative Example 4, the density was low due to the low HIP temperature. In Comparative Examples 5 and 6, the tungsten content and oxygen content were high, resulting in high resistivity. In addition, the powder was too fine and the oxygen content was high, resulting in a sudden increase in density during HP, leading to oxide trapping. In addition, the density was low due to the low HIP temperature. In Comparative Example 7, the oxygen content was high, so the resistivity was high, and the raw powder was too fine, so the density rose sharply during HP and some oxides remained. In Comparative Example 8, the oxygen content was high, so the resistivity was high, and the raw powder was too fine, so the density rose sharply during HP, leaving some oxides behind. Also, the HIP temperature was high, so abnormal grain growth occurred, and the aspect ratio became large. In Comparative Examples 9 to 11, the raw material powder was coarse, resulting in insufficient density, and in Comparative Example 11, insufficient particle size adjustment resulted in uneven particle size and a large aspect ratio, resulting in insufficient density. In Comparative Example 12, the high HIP temperature caused abnormal grain growth, resulting in a large aspect ratio, and the raw material powder was coarse, resulting in insufficient density. In Comparative Example 13, the amount of carbon diffusion was large due to the high HP temperature. Also, due to insufficient adjustment of the raw material particle size distribution, the particle size was uneven, the aspect ratio was large, and the powder was coarse, resulting in insufficient density.

Claims

1. A molybdenum target formed of a sintered body of molybdenum powder, The relative density is 99% or more, The oxygen content is 25 ppm or less, and the carbon content is 30 ppm or less, The tungsten content is 10 ppm to 100 ppm; The molybdenum content excluding the oxygen content, the carbon content, and the tungsten content is 99.999% by mass or more, 0.15mm 2 In the observation area of ​​0.01 μm 2 0.2 μm or more 2 There are 20 or less pores with a size of less than 0.2 μm 2 More than 1.8 μm 2 There are 5 or less pores with a size of less than 1.8 μm 2 A molybdenum target having one or less pores of this size or larger.

2. Average particle diameter d calculated based on circle equivalent diameter Ave is 20 μm or more and 100 μm or less, Standard deviation 3σ of particle size calculated using circle equivalent diameter and average particle size d Ave Ratio to (3σ / d Ave 2. The molybdenum target according to claim 1, wherein the molybdenum content is 1.2 or less.

3. 3. The molybdenum target according to claim 2, wherein the aspect ratio of the grain size d is less than 1.

2.

4. The average Vickers hardness is 180 or less, Standard deviation 3σ of Vickers hardness and average value H of Vickers hardness Ave Ratio to (3σ / H Ave 4. The molybdenum target according to claim 1, wherein the molybdenum content is 0.07 or less.

5. Average particle size D obtained by laser diffraction / scattering method Ave The median diameter D50 is 2.0 to 3.5, and the median diameter D90 and the average particle diameter D AveThe ratio of D90 to D Ave ) is 1.7 or less, and the median diameter D95 and the average particle diameter D Ave The ratio of D95 / D Ave ) is 2.0 or less, A method for manufacturing a molybdenum target, comprising hot pressing at a temperature of 1400° C. to 1500° C., and then sintering by hot isostatic pressing at a temperature of 1500° C. to 1600° C.

6. The molybdenum powder has a tungsten content of 10 ppm to 100 ppm; The method for producing a molybdenum target according to claim 5, wherein the molybdenum content excluding the oxygen content, the carbon content and the tungsten content is 99.999 mass % or more.

7. 7. The method for producing a molybdenum target according to claim 5, wherein the hot pressing is carried out under high vacuum at a holding temperature of 1400 to 1500° C. for a holding time of 360 to 600 minutes.

Citation Information

Patent Citations

  • Dense sintered compact of ferroelectric oxide and its production

    JP1999240720A

  • Molybdenum sputtering target material and its production

    JP2000234167A

  • Sputtering target material

    JP2000319774A

  • Method of producing molybdenum target for sputtering and molybdenum target

    JP2003342720A

  • METHOD FOR PRODUCING INTEGRALLY SINTERED Mo BASED TARGET MATERIAL, AND INTEGRALLY SINTERED Mo BASED TARGET MATERIAL

    JP2005344136A