Atomic layer deposition derived protective coatings for calcium fluoride optics

Atomic layer deposition (ALD) coatings on calcium fluoride optical components address the challenges of PVD by providing uniform and conformal protection, enhancing mechanical stability and longevity, and improving performance in DUV applications.

JP2024537029APending Publication Date: 2024-10-10CORNING INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024518649
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-19
Filing Date
2022-09-27
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Current PVD coating processes face challenges in applying uniform and conformal coatings on optical components with steeply curved surfaces, leading to mechanical stability issues, surface cleanliness problems, and non-uniform thickness, which affect the performance and longevity of calcium fluoride-based optical components used in deep ultraviolet (DUV) applications.

Method used

The use of atomic layer deposition (ALD) processes to apply conformal coatings of metal fluorides, such as magnesium fluoride (MgF2), metal oxides, and metalloid oxides directly onto calcium fluoride optical components, ensuring uniform thickness and improved adhesion without the need for fixtures, thereby enhancing surface protection and reducing mechanical stress.

Benefits of technology

ALD coatings provide a uniform, pinhole-free, and atomically dense film that increases the lifetime of optical components, reduces rework rates, and improves product yield by sealing calcium fluoride surfaces, while maintaining high transmittance and reflectance properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024537029000001_ABST
    Figure 2024537029000001_ABST
Patent Text Reader

Abstract

The coated optical component includes an optical component and a conformal coating. The optical component is crystalline calcium fluoride, and the conformal coating is an atomic layer deposition (ALD) coating in contact with a surface of the optical component. The ALD coating includes a metal fluoride ALD coating having a metal different from calcium. The ALD coating can include other metal oxide or metalloid oxide ALD coating layers. The method of making a coated optical component includes depositing an atomic layer deposition (ALD) coating on a surface of the optical component, where the ALD coating can be a metalloid oxide, a metal oxide, a metal fluoride having a metal different from calcium, or a combination thereof. Sulfur hexafluoride is used as a fluorine source in the ALD process.
Need to check novelty before this filing date? Find Prior Art

Description

Priority

[0001] This application claims the benefit of priority under 35 U.S.C. §119 of U.S. Provisional Patent Application No. 63 / 257,486, filed October 19, 2021, the contents of which are relied upon and incorporated herein by reference in their entirety. [Technical field]

[0002] The present disclosure relates generally to optical components, and more particularly to optical components having coated calcium fluoride structures for deep ultraviolet (DUV) optics. [Background technology]

[0003] Optical technologies that utilize ultraviolet light are widely used in semiconductor manufacturing. Although extreme ultraviolet (EUV)-based advanced lithography has made progress, deep ultraviolet (DUV)-based optical technologies still play a major role in semiconductor manufacturing. Most DUV-based optical lithography techniques require laser-durable calcium fluoride (CaF2) optics for the laser optics that enable high-power light sources and precision optics that enable high-resolution inspection and patterning. Surface quality and surface scratch mitigation technologies help improve the performance of CaF2 optics. Developments in optical surface and coating technologies, such as PVD coatings, enable mitigation of surface defects and reduced surface degradation of CaF2 optics, thus extending their useful life. Summary of the Invention

[0004] According to a first aspect of the present disclosure, a coated optical component comprises an optical component including crystalline calcium fluoride and an atomic layer deposition (ALD) coating in contact with a surface of the optical component, the ALD coating including a metal fluoride having a metal different from calcium.

[0005] A second aspect of the present disclosure may include the first aspect, in which the ALD coating may include magnesium fluoride (MgF2).

[0006] A third aspect of the disclosure may include either the first or second aspect, in which the metal fluoride of the ALD coating may be directly bonded to the calcium fluoride of the optical component, such that the metal fluoride of the ALD coating contacts the calcium fluoride at the surface of the optical component.

[0007] A fourth aspect of the present disclosure can include any one of the first to third aspects, wherein the ALD coating can have a thickness of 10 nanometers (nm) or less.

[0008] A fifth aspect of the present disclosure can include any one of the first through fourth aspects, where the ALD coating can include a first ALD coating layer in direct contact with a surface of the optical component, the first ALD coating layer including a metal fluoride. The ALD coating can further include a second ALD coating layer in direct contact with the first ALD coating layer, the second ALD coating layer being made from a different material than the first ALD coating layer.

[0009] A sixth aspect of the present disclosure can include the fifth aspect, in which the first ALD coating layer can be magnesium fluoride and the second ALD coating layer can be silica (SiO2) or alumina (Al2O3).

[0010] A seventh aspect of the present disclosure can include either the fifth or sixth aspects, in which the first ALD coating layer can have a thickness of less than 10 nanometers (nm) and the second ALD coating layer can have a thickness of less than 10 nm.

[0011] An eighth aspect of the present disclosure can include any one of the first through seventh aspects, where the ALD coating can include an antireflective coating, and the antireflective coating can have a reflectivity of less than 1% over a wavelength range of 190 nm to 266 nm, where the reflectivity refers to the percentage of an incident beam power that is reflected back from the antireflective coating.

[0012] A ninth aspect of the present disclosure can include any one of the first through eighth aspects, wherein the ALD coating can include sulfur.

[0013] A tenth aspect of the present disclosure can include the ninth aspect, in which the ALD coating can have a sulfur content greater than zero, such as from greater than zero ppm to 300 ppm.

[0014] An eleventh aspect of the present disclosure can include any one of the first through tenth aspects, wherein the ALD coating can be in contact with at least 95%, at least 98%, at least 99%, or at least 99.5% of the optical surfaces of the uncovered optical component.

[0015] A twelfth aspect of the present disclosure can include any one of the first to eleventh aspects, wherein the ALD coating can be a conformal coating.

[0016] A thirteenth aspect of the present disclosure can include any one of the first through twelfth aspects, wherein the ALD coating has a thickness that varies by no more than 5% from an average thickness of the ALD coating, the average thickness of the ALD coating being the thickness of the ALD coating averaged over a surface in contact with the ALD coating.

[0017] A fourteenth aspect of the present disclosure can include any one of the first through thirteenth aspects, wherein the ALD coating can include 1000 ppm or less of carbon based on a total weight of the ALD coating.

[0018] A fifteenth aspect of the present disclosure can include any one of the first through fourteenth aspects, wherein the ALD coating can be in contact with at least 90%, at least 95%, at least 98%, at least 99%, or at least 99.5% of the surface of the optical component.

[0019] A sixteenth aspect of the present disclosure may include any one of the first to fifteenth aspects, wherein the optical component may be a prism, a lens, a beam splitter, or a window.

[0020] A seventeenth aspect of the present disclosure is a method for manufacturing a reflective optical component, the reflective optical component having a steepness ratio R of 0.5 to 0.85. c / #, and the steepness ratio R c / # is the radius of curvature of the steep surface (R c 16. The present invention may include any one of the first to sixteenth aspects, wherein

[0021] An eighteenth aspect of the present disclosure may include a method of coating an optical component. The method may include depositing an atomic layer deposition (ALD) coating on a surface of the optical component. The optical component may include crystalline calcium fluoride (CaF2), and the ALD coating may include a semi-metal oxide, a metal oxide, a metal fluoride having a metal different from calcium, or a combination thereof.

[0022] A nineteenth aspect of the present disclosure can include the eighteenth aspect, in which the ALD coating can include a metal fluoride and depositing the ALD coating can include exposing a surface of the optical component to alternating pulses of a metal precursor and a fluorine source.

[0023] A twentieth embodiment of the present disclosure may include the nineteenth embodiment, wherein the fluorine source may be selected from the group consisting of sulfur hexafluoride (SF6), nitrogen trifluoride (NF3), trifluoroiodomethane (CF3I), hydrogen fluoride (HF), and combinations thereof.

[0024] A twenty-first embodiment of the present disclosure can include either the nineteenth or twentieth embodiment, where the fluorine source can include sulfur hexafluoride (SF6).

[0025] A twenty-second aspect of the present disclosure can include any one of the nineteenth to twenty-first aspects, wherein the fluorine source can include a plasma formed from sulfur hexafluoride.

[0026] A twenty-third aspect of the present disclosure can include any one of the nineteenth to twenty-second aspects, wherein the metal precursor can include a metal-ligand complex including magnesium.

[0027] A twenty-fourth embodiment of the present disclosure can include any one of the nineteenth through twenty-third embodiments, wherein the metal precursor can be selected from the group consisting of bis(ethylcyclopentadienyl)magnesium, bis(cyclopentadienyl)magnesium, bis(2,2,6,6-tetramethyl-3,5-heptanedionato)magnesium, bis(N,N'-di-sec-butylacetamidinato)magnesium, bis(pentamethylcyclopentadienyl)magnesium, and combinations thereof.

[0028] A twenty-fifth aspect of the present disclosure may include any one of the nineteenth through twenty-fourth aspects, in which exposing the surface of the optical component to alternating pulses of a metal precursor and a fluorine source may include exposing the surface of the optical component to a pulse containing a metal precursor. The metal precursor may react with calcium fluoride at the surface of the optical component to deposit a monolayer of ligated metal on the surface of the optical component. The method may further include terminating the pulse containing the metal precursor and exposing the surface of the optical component to a pulse containing a fluorine source. The fluorine source may react with the monolayer of ligated metal to form a metal fluoride. The method may further include terminating the pulse containing the fluorine source.

[0029] A twenty-sixth embodiment of the present disclosure may include the twenty-fifth embodiment, further including repeatedly exposing the surface to alternating pulses of a metal precursor and a fluorine source to increase the thickness of the ALD coating.

[0030] A twenty-seventh embodiment of the present disclosure may include any one of the twenty-fifth or twenty-sixth embodiments, further comprising exposing the surface of the optical component to a pulse containing an oxygen source after terminating the pulse containing the metal precursor and before exposing the surface of the optical component to a pulse containing a fluorine source. The oxygen source may include water, water plasma, oxygen, oxygen plasma, ozone, ozone plasma, hydrogen peroxide, hydrogen peroxide plasma, an oxygen-containing liquid, an oxygen-containing gas, or a combination thereof. The oxygen source may oxidize the coordinated metal to form a metal oxide. The method may further include terminating the pulse containing the oxygen source. After the pulse containing the oxygen source, the fluorine source may reduce the metal oxide to form a metal fluoride.

[0031] A twenty-eighth embodiment of the present disclosure can include the twenty-seventh embodiment, wherein the pulse containing an oxygen source can remove carbon from the monolayer of the coordinated metal.

[0032] A twenty-ninth aspect of the present disclosure can include the eighteenth aspect, in which the ALD coating can include a metal oxide, and in which depositing the ALD coating on a surface of the optical component can include exposing the surface to alternating pulses of a metal precursor and an oxygen source.

[0033] A thirtieth embodiment of the present disclosure may include the twenty-ninth embodiment, wherein the oxygen source may be selected from the group consisting of water, water plasma, ozone, ozone plasma, oxygen, oxygen plasma, hydrogen peroxide, hydrogen peroxide plasma, oxygen-containing gases, oxygen-containing liquids, and combinations thereof.

[0034] A thirty-first embodiment of the present disclosure can include any one of the twenty-ninth to thirtieth embodiments, wherein the metal precursor can include an aluminum precursor selected from the group consisting of trimethylaluminum (TMA), triethylaluminum (TEA), and combinations thereof.

[0035] A thirty-second embodiment of the present disclosure can include the eighteenth embodiment, which can include an ALD coating a metalloid oxide, and in which depositing the ALD coating on a surface of the optical component can include exposing the surface of the optical component to alternating pulses of a metalloid precursor and an oxygen source.

[0036] A thirty-third embodiment of the present disclosure may include the thirty-second embodiment, wherein the oxygen source may be selected from the group consisting of water, water plasma, ozone, ozone plasma, oxygen, oxygen plasma, hydrogen peroxide, hydrogen peroxide plasma, oxygen-containing gases, oxygen-containing liquids, and combinations thereof.

[0037] A thirty-fourth embodiment of the present disclosure can include either the thirty-second or thirty-third embodiment, wherein the metalloid oxide can be silica and the metalloid precursor can be selected from the group consisting of bis(tert-butylamino)silane; di(sec-butylamino)silane; diisopropylaminotrisilylamine; a compound having the formula SiH2(NR R')2, where each of R and R' is independently a methyl group, an ethyl group, or both; and combinations thereof.

[0038] A thirty-fifth aspect of the present disclosure can include any one of the eighteenth to thirty-fourth aspects, comprising depositing the ALD coating on a surface of the optical component at a process temperature of 120° C. to 250° C.

[0039] A thirty-sixth aspect of the present disclosure can include any one of the eighteenth through thirty-fifth aspects, wherein depositing the ALD coating can include applying a first ALD coating layer on a surface of the optical component and applying a second ALD coating layer on the first ALD coating layer, the second ALD coating layer being made from a different material than the first ALD coating layer.

[0040] A thirty-seventh aspect of the present disclosure can include the thirty-sixth aspect, in which the first ALD coating layer can include a metal fluoride and the second ALD coating layer can include silica or alumina.

[0041] A thirty-eighth aspect of the present disclosure can include any one of the eighteenth to thirty-seventh aspects, wherein the step of depositing the ALD coating can be performed without rotating the optical component.

[0042] A thirty-ninth aspect of the present disclosure may include any one of the eighteenth to thirty-eighth aspects, wherein the method does not include holding the optical component in a fixture.

[0043] A fortieth aspect of the present disclosure may include any one of the eighteenth to thirty-ninth aspects, wherein the optical component comprises a plurality of surfaces, and the step of depositing the atomic layer deposition (ALD) coating is performed simultaneously on at least two of the plurality of surfaces.

[0044] Additional features and advantages of the optical components, ALD coatings, and methods of coating optical components with ALD coatings described herein are set forth in the following detailed description, and in part will be readily apparent to those skilled in the art from that description, or may be learned by practicing the embodiments described herein, including the following detailed description, claims, and accompanying drawings.

[0045] It should be understood that both the foregoing general description and the following detailed description describe various embodiments and are intended to provide an overview or framework for understanding the nature and character of the claimed subject matter. The accompanying drawings are included to provide a further understanding of the various embodiments, and are incorporated in and constitute a part of this specification. The drawings illustrate various embodiments described herein and, together with the description, serve to explain the principles and operation of the claimed subject matter. [Brief description of the drawings]

[0046] [Figure 1A] FIG. 1 is a perspective view of a prism according to one or more embodiments shown and described herein; [Figure 1B] 1B is a cross-sectional view of a portion of the prism of FIG. 1A taken along reference line 1B-1B, in accordance with one or more embodiments shown and described herein; [Figure 1C] FIG. 1B is a top view of the prism of FIG. 1A according to one or more embodiments shown and described herein. [Figure 1D] FIG. 1B is a schematic diagram illustrating a surface of the prism of FIG. 1A according to one or more embodiments shown and described herein. [Figure 2A] FIG. 1 is a schematic diagram showing a fixture for holding and rotating an optical component during physical vapor deposition (PVD) coating according to the prior art. [Figure 2B] FIG. 1 is a schematic diagram showing a fixture for holding and rotating an optical component during physical vapor deposition (PVD) coating according to the prior art. [Figure 2C] FIG. 1 is a schematic diagram showing a fixture for holding and rotating an optical component during physical vapor deposition (PVD) coating according to the prior art. [Figure 2D] FIG. 1 is a schematic diagram showing a fixture for holding and rotating an optical component during physical vapor deposition (PVD) coating according to the prior art. [Figure 3A] FIG. 1 is a perspective view of another prism according to one or more embodiments shown and described herein; [Figure 3B] FIG. 3B is a front view of a first total internal reflection (TIR) ​​surface of the prism of FIG. 3A according to one or more embodiments shown and described herein. [Figure 3C] FIG. 3B is a front view of a second TIR surface of the prism of FIG. 3A according to one or more embodiments shown and described herein; [Figure 4] FIG. 1 is a side view of a right angle prism according to one or more embodiments shown and described herein; [Diagram 5] FIG. 1 is a side view of an optical inspection system having a high numerical aperture objective lens according to one or more embodiments shown and described herein; [Figure 6] 1 is a cross-sectional view of a portion of a coated optical component having a first ALD coating layer including a metal fluoride ALD coating and a second ALD coating layer including an oxide ALD coating deposited on the first ALD coating layer in accordance with one or more embodiments shown and described herein; [Figure 7]1 is a graph showing the thickness of each of a first ALD coating layer and a second ALD coating layer for a coated optical component of Example 1, according to one or more embodiments shown and described herein; [Figure 8] 1 is a graph showing the percentage transmission (y-axis) as a function of incidence angle (x-axis) for a coated optical component of Example 1 and a comparative uncoated optical component having the same geometry, according to one or more embodiments shown and described herein. [Figure 9] 1 is a graph showing the percentage transmission (y-axis) as a function of incidence angle (x-axis) for a coated optical component of Example 1, according to one or more embodiments shown and described herein. [Figure 10] 1 is a graph showing the percentage of internal reflectance (y-axis) as a function of incidence angle (x-axis) for a comparative uncoated optical component having the same geometry as the coated optical component of Example 1, in accordance with one or more embodiments shown and described herein; [Figure 11] 1 is a graph showing the percentage of internal reflectance (y-axis) as a function of incidence angle (x-axis) for a coated optical component of Example 1, according to one or more embodiments shown and described herein. [Figure 12] 1 is a graph showing the percentage transmission (y-axis) as a function of incidence angle (x-axis) for a coated optical component of Example 2 and a comparative uncoated optical component having the same geometry, according to one or more embodiments shown and described herein. [Figure 13] 1 is a graph showing the percentage of internal reflectance (y-axis) as a function of incidence angle (x-axis) for a coated optical component of Example 2 and a comparative uncoated optical component having the same geometry, according to one or more embodiments shown and described herein. [Figure 14] 1 is a graph showing the percentage of internal reflectance (y-axis) as a function of incidence angle (x-axis) for a coated optical component of Example 3 and a comparative uncoated optical component having the same geometry, according to one or more embodiments shown and described herein; [Figure 15]1 is a graph showing the percentage surface reflectance of the incident surface (y-axis) as a function of wavelength of incident light (x-axis) for a coated optical component of Example 3 and a comparative uncoated optical component having the same geometry, according to one or more embodiments shown and described herein; [Figure 16] Graph showing normalized intensity (y-axis) as a function of fluorine 1s binding energy (x-axis) determined by X-ray photoelectron spectroscopy for MgF2 ALD coatings of Examples 4 and 5 according to one or more embodiments shown and described herein. [Figure 17] Graph showing normalized intensity (y-axis) as a function of carbon 1s binding energy (x-axis) as determined by X-ray photoelectron spectroscopy for MgF2 ALD coatings of Examples 4 and 5 according to one or more embodiments shown and described herein. [Figure 18] Graph showing normalized intensity (y-axis) as a function of magnesium 2p binding energy (x-axis) as determined by X-ray photoelectron spectroscopy for MgF2 ALD coatings of Examples 4 and 5 according to one or more embodiments shown and described herein. [Figure 19] Graph showing refractive index (y-axis) as a function of wavelength (x-axis) for coated optical components prepared by various ALD and PVD processes according to one or more embodiments shown and described herein. [Figure 20] Graph showing normalized intensity (y-axis) as a function of depth in the coating (x-axis) for various atomic constituents of the PVD coating of Comparative Example 7. [Figure 21] 1 is a graph showing normalized intensity (y-axis) as a function of depth in the coating (x-axis) for various atomic components of the ALD coating of the ALD coated optical component of Sample 9C of Example 8, in accordance with one or more embodiments shown and described herein. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0047] Reference will now be made in detail to various embodiments of optical components and ALD coatings of the present disclosure, examples of which are illustrated generally in the accompanying drawings. Whenever possible, the same reference numbers are used throughout the drawings to refer to the same or similar parts. Referring now to FIGS. 1A and 1B, one embodiment of a coated optical component 100 according to the present disclosure is illustrated generally. Referring to FIG. 1B, the coated optical component 100 comprises an optical component 101 including crystalline calcium fluoride and a conformal coating in contact with a surface of the optical component 100. The conformal coating is an ALD coating 120 in contact with a surface of the optical component 100. The ALD coating 120 may be a metal oxide, a metalloid oxide, a metal fluoride having a metal different from calcium, or a combination thereof. In an embodiment, the ALD coating 120 may be a magnesium fluoride ALD coating.

[0048] The coated optical component 100 may be prepared by a method that may include depositing an atomic layer deposition (ALD) coating 120 on a surface of the optical component 101. The optical component 101 may include crystalline calcium fluoride (CaF2), and the ALD coating 120 may include a metalloid oxide, a metal oxide, a metal fluoride having calcium and a different metal, or a combination thereof. In an embodiment, the ALD coating 120 may include a metal fluoride ALD coating, and the method may include exposing the surface of the optical component 101 to alternating pulses of a metal precursor and a fluorine source. In an embodiment, the fluorine source may be an SF6-based fluorine source, and the ALD process may include an additional oxygen source to convert the metal precursor to a metal oxide, which may then be converted to a metal fluoride by a subsequent fluorine source. The ALD coating 120 may also include a metal oxide ALD coating, a metalloid oxide ALD coating, or both.

[0049] Various embodiments of a coated optical component 100 having an ALD coating 120 formed thereon and a method of coating an optical component with an ALD coating 120 to produce the coated optical component 100 are described herein with particular reference to the accompanying drawings.

[0050] As used herein, the term "substantially free" of a component may refer to a composition, fiber, or atmosphere that contains less than 0.01 weight or mole percent of the component. For example, an ALD coating that is substantially free of carbon may contain less than 0.01 weight or mole percent carbon.

[0051] The terms "micrometer" and "μm" are used interchangeably herein. The terms "nanometer" and "nm" are used interchangeably herein.

[0052] As used herein, the term "plasma" refers to a gas of ions, including positive ions and electrons, produced from a starting material by the application of heat and electric current.

[0053] As used herein, the term "ppm" means parts per million on a molar basis and represents atomic concentration. For example, a layer of MgF2 containing 1 ppm carbon contains 1 mole of carbon per million moles of MgF2.

[0054] As used herein, the term "conformal coating" refers to a coating that conforms to the contours of the surface of an article and has a generally uniform thickness over all of the surface contacted by the coating.

[0055] Laser-durable calcium fluoride (CaF2) optics enable the use of high-power light sources for semiconductor manufacturing, providing precision optics that enable high-resolution inspection and patterning. Surface quality and surface scratch mitigation techniques can improve the performance of CaF2 optics. These surface treatment technology advances enable the mitigation of surface defects and reduced surface degradation of CaF2 optics, thereby extending their useful life. Such surface scratch mitigation techniques include subsurface damage (SSD) detection and SSD-free surface finishing processes; surface cleaning techniques such as, but not limited to, megasonic cleaning, ultraviolet ozone (UVO) cleaning, and reactive plasma cleaning; and physical vapor deposition (PVD)-based protective coatings (PCCF) for CaF2 components.

[0056] Specifically, protective PVD-based coatings are applied to the total internal reflection (TIR) ​​and Brewster angle surfaces (input / output surfaces) of CaF2 prisms as well as the surfaces of other CaF2 optical components such as lenses, windows, etc., to extend the life of the CaF2 optical components. Currently, all of the protective coatings are based on PVD coating processes. Examples of these PVD-based coatings include, but are not limited to, silica PVD coatings, or magnesium fluoride (MgF2) PVD coatings in combination with silica PVD coatings applied on top of MgF2 PVD coatings. The total thickness of these PVD coatings is generally greater than 50 nanometers (nm) or even greater than 60 nm. These thickness ranges of the PVD coatings are necessary to ensure that the surfaces are sealed with the PVD coating within the coated area and that there are no gaps or pinholes in the PVD coating.

[0057] While these advanced techniques, especially PVD coatings, have been successfully used in many laser optics and precision optics applications, these PVD coatings can be a challenge to properly apply to CaF2 prisms and other optical components with steeply curved surfaces. These types of optical components (prisms and components with steeply curved surfaces) have characteristics that present challenges compared to certain windows and lenses. Specifically, prisms may have multiple surfaces that require coating. In addition, prisms can have small sizes and complex geometries necessitated by the Brewster's angle and positioning of the TIR surfaces of the prism.

[0058] These characteristics and properties of CaF2 prisms pose additional challenges to producing laser-durable optics with PVD-based coating processes. For example, multiple PVD coating runs are typically required to complete a protective coating on a CaF2 prism. In addition, the use of fixtures to hold and rotate the prisms at high temperatures during the PVD process can cause mechanical stability and surface cleanliness issues. These mechanical stability and surface cleanliness issues can increase the risk of mechanical and thermal damage to the optic during the PVD coating process. Referring now to Figures 2A-2D, various configurations of prior art tool fixtures 20 for holding and rotating the optic 10 during PVD coating are shown generally. The tool fixture 20 generally includes a rotational stage 22 and one or more support features 24 that contact the optic 10 to secure the optic 10 while rotating it during the PVD coating process. The tooling fixture 20 used for PVD coating has a high risk of scratching the precision-polished optical surfaces of the optical component 10 due to contact with the tooling fixture 20 at high rotational speeds. The PVD coating process also has a high risk of particle contamination and high rework rates for the prisms due to multiple surface coatings, multiple pump-to-vent events, and cleaning and re-cleaning of surfaces. PVD-based protective coatings can also have a non-uniform coating thickness, which can limit the minimum thickness required to achieve the desired average thickness and sealing ability of the PVD-based protective coating.

[0059] In addition to prisms, optical components with steeply curved surfaces can also present challenges for PVD coatings, such as protective coatings, high performance anti-reflective (AR) coatings, etc., over a wide angular range and / or broad spectral band. As used throughout this disclosure, "anti-reflective coating" may refer to a coating that has a reflectivity of less than 1%, where "reflectivity" refers to the percentage of an incident beam power that is reflected back from a given surface. The reflectivity (Rx) of a surface is given by Rx=P r / P0, where P0 is the incident beam power and P r is the power of the beam returned from the surface.

[0060] Current PVD processes have poor thickness uniformity on steeply curved surfaces due to the vapor flow of the PVD coating process and line of sight changes between points on the steeply curved surface. Therefore, PVD coating processes cannot provide uniform conformal coatings on all coating surfaces of an optical component. To address this issue, complex motion and screening of the target surface is often used to deliver a coating with a more consistent thickness. However, the complex motion and screening significantly increase the processing time and cost of PVD coating steeply curved surfaces.

[0061] The coated optical components and methods of the present disclosure overcome these problems by applying a conformal coating to a surface of an optical component, such as a prism or an optical component having a sharp curve, using an atomic layer deposition process to produce the coated optical component. The coated optical components of the present disclosure may comprise an optical component comprising, consisting of, or consisting essentially of calcium fluoride. The calcium fluoride may be crystalline calcium fluoride. The coated optical component further comprises a conformal coating comprising an ALD coating in contact with one or more surfaces of the optical component. The ALD coating may comprise a metal oxide, a metalloid oxide, a metal fluoride having a metal different from calcium, or a combination thereof. In embodiments, the ALD coating may comprise magnesium fluoride (MgF2) (e.g., an MgF2 ALD coating). Additionally or alternatively, in embodiments, the ALD coating may comprise a silica ALD coating, an alumina ALD coating, or a combination thereof. Methods of applying an ALD coating to an article to produce a coated optical component are also disclosed herein.

[0062] The ALD coating process can coat all of the surfaces of the optical component with atomic layer precision in a single deposition operation. In other words, the ALD coating process allows for conformal coating of all surfaces of the optical component simultaneously. The ALD coating process can produce atomically dense and pinhole-free films even at very small thicknesses, such as thicknesses of up to a few nanometers. Therefore, the ALD coating process can reduce the thickness of coatings, such as but not limited to protective coatings and anti-reflective (AF) coatings, to less than one-fifth the thickness of PVD-based coatings. The ALD coating can allow control of the coating thickness down to a few nanometers, such as 10 nm or less. The ALD coating process can reduce the stress of the coating and increase the lifetime of the coated optical component. In particular, the ALD coating seals the calcium fluoride and reduces the depletion of fluoride ions from the calcium fluoride surface. The ALD coating process may also improve product yield and reduce rework rates, among other features.

[0063] 1A and 1B, a coated optical component 100 is shown in schematic form. Referring to FIG. 1B, the coated optical component 100 comprises an optical component 101 and an ALD coating 120 applied to the surfaces of the optical component 101 (e.g., first surface 102, TIR surfaces 104 and 106, top surface 108, etc.). The optical component 101 may be a prism, a lens, an objective lens, a window, or other type of optical component. The optical component 101 may be a structure made from calcium fluoride (CaF2). In embodiments, the optical component 101 may comprise, consist of, or consist essentially of crystalline CaF2. The optical component 101 may be small in size, such as having a maximum dimension as small as 10 mm, and may have a complex shape. Optical components 101 having complex shapes may include optical components with many faceted sides, such as prisms, beam splitters, windows, or optical components with steeply curved surfaces, such as, but not limited to, high numerical aperture objective lenses or other lenses.

[0064] In an embodiment, the optical component 101 can be a prism having multiple sides. Referring to Figures 1A-1D, one embodiment of a coated optical component 100 including a prism as the optical component 101 is shown in schematic form. The coated optical component 100 in Figure 1A is a calcium fluoride (CaF2) prism made as an argon fluoride laser beam reverser. The coated optical component 100 in Figures 1A-1D has a first surface 102, which is a Brewster angle surface made to allow the laser beam 110 to enter and exit the prism at the Brewster angle. The coated optical component 100 may have a first TIR surface 104 and a second TIR surface 106 made to reflect the laser beam 110 back through the prism. The first TIR surface 104 and the second TIR surface 106 may be angled and positioned to reflect the laser beam 110 from the first TIR surface 104 to the second TIR surface 106 and then from the second TIR surface 106 back through the first surface 102. The angle of incidence (AOI) of the laser beam 110, the Brewster angle of calcium fluoride, and the angles of the first TIR surface 104 and the second TIR surface 106 are designed to cause the laser beam 110 to follow a specific path through the prism, which may cause the coated optic 100 to have a complex shape with sides at specific non-normal angles relative to other sides of the coated optic 100.

[0065] 3A-3C, another embodiment of a coated optic 200 comprising a prism is shown in schematic form. The coated optic 200 of FIG. 3A-3C comprises a small complex-shaped CaF2 corner prism made to operate at a laser wavelength of 213 nm. Referring to FIG. 3A, the coated optic 200 has four optical surfaces, including an entrance surface 202 and an exit surface 204 at Brewster's angle, a first TIR surface 206 at an incidence angle of 56.1°, and a second TIR surface 208 at an incidence angle of 45°. The Brewster's angle and the incidence angles of the two TIR surfaces 206, 208 result in the coated optic 200 having a complex multi-faceted shape. FIG. 3B and 3C show schematic views of two faces of the coated optic 200 of FIG. 3A, illustrating the complex shape of the coated optic 200.

[0066]

[0033] Referring now to Figure 4, another embodiment of a coated optic 400 comprising a right angle prism is shown generally. The coated optic 400 of Figure 4 may be made to reflect a beam of light 410, such as, but not limited to, a laser beam having a wavelength of 266 nm, to an inspection device 420, such as an inspection objective. The coated optic 400 of Figure 4 may comprise an entrance surface 402, an exit surface 404, and at least one TIR surface 406. The TIR surface 406 may reflect at least a portion of the beam of light 410 from a path through the exit surface 404 to the inspection device 420. The coated optic 400 of Figure 4 comprising a right angle prism may also have a complex shape.

[0067] 5, an optical inspection system 500 for optical inspection using DUV or broadband spectrum wavelengths is shown generally. The optical inspection system 500 may include many different elements such as lenses, windows, prisms, beam splitters, wavelength filters, mirrors, etc., which may have small sizes and complex shapes. In particular, the optical inspection system may include a high numerical aperture (NA) objective lens 502, which may have one or more surfaces 504 with very steep curvatures. The steepness of the curvature of the surface 504 is calculated by the radius of curvature (R) of the steep surface divided by the diameter (#) of the aperture of the optic. c ) steepness ratio R c The surface 504 having a steep curvature can be characterized by a steepness ratio R of 0.75 to 0.85. c A surface 504 having a very steep curvature may have a steepness ratio R less than 0.75, such as between 0.5 and 0.75. cOther features of optical inspection systems may also have steep curvatures. As mentioned previously, these steep curvatures may present challenges in applying anti-reflective and other coatings using PVD processes. In particular, steep curvatures may present line-of-sight issues during the PVD coating process, which may require complex process modifications, such as repositioning elements when a PVD coating is applied to the steep curved surface, and / or may result in poor coating uniformity. In particular, the steepness ratio R of the curved surface may be increased by 1 / 2 mm. c When / # is less than 1, the PVD deposition process may produce a PVD coating that has a thickness falloff of more than 5% across the curved surface. This thickness inconsistency due to falloff increases with increasing steepness of the curvature of the curve. Therefore, the PVD process cannot provide a conformal coating on steeply curved or irregular surfaces.

[0068] The ALD coating 120 and the ALD process for producing the coating will now be described with reference to the coated optical components of Figures 1A-1D. However, it will be understood that the ALD coating 120 and the ALD process disclosed herein may be applied equally well to any of the optical components of Figures 3A-3C, 4, and 5, as well as to any other optical components. The ALD coating 120 and / or the ALD coating process disclosed herein may also be applied to types of CaF2 components other than optical components.

[0069] 1B, coated optical component 100 includes one or more ALD coatings 120 deposited on a surface of optical component 101 such that ALD coating 120 contacts one or more of the surfaces of optical component 101. In embodiments, ALD coating 120 may be a protective coating that provides a barrier on the surface of optical component 101 that functions to reduce or prevent CaF2 from corroding from the surface of optical component 101. In embodiments, ALD coating 120 may be an anti-reflective coating. ALD coating 120 may include a metal oxide, a metalloid oxide, a metal fluoride having a metal different from calcium, or a combination thereof. In embodiments, ALD coating 120 may be a magnesium fluoride (MgF2) ALD coating or coating layer. In embodiments, ALD coating 120 may include other high refractive index fluorides, such as, but not limited to, a lanthanum fluoride (LaF3) ALD coating or a gadolinium fluoride (GdF3) ALD coating. Additionally or alternatively, in embodiments, the ALD coating may include a silica coating, an alumina coating, or a combination thereof.

[0070] In an embodiment, the coated optical component 100 may include an ALD coating 120 that includes magnesium fluoride (MgF2). The MgF2 ALD coating is well suited for coated optical components 100 in deep ultraviolet (DUV) optical applications due to the low refractive index, high transmission, and chemical and mechanical stability of the MgF2 ALD coating at laser wavelengths in the deep ultraviolet range, such as, but not limited to, wavelengths from 193 to 266 nm. The MgF2 ALD coating may also be suitable for use in wavelength ranges longer than 266 nm. When the ALD coating 120 is a metal oxide ALD coating, such as, but not limited to, an MgF2 ALD coating, the metal fluoride compound of the ALD coating 120 may be directly bonded to the CaF2 of the optical component 101 such that the metal fluoride of the ALD coating 120 is in contact with the CaF2 at the surface of the optical component 101. As used herein, the term "directly bonded" means that the ALD coating 120 is in contact with and bonded to the surface of the optical component 101 without any intervening coating or layer disposed between the ALD coating 120 and the surface of the optical component 101. In embodiments, the coated optical component 100 may include a metal oxide ALD coating, such as, but not limited to, a MgF2 ALD coating, with no alumina coating disposed between the CaF2 of the optical component 101 and the metal fluoride of the ALD coating 120. In embodiments, the ALD coating 120 may include a silica ALD coating, an alumina ALD coating, or both. Referring now to FIG. 6, the coated optical component 100 may include multiple ALD coating layers (e.g., a first ALD coating layer 130, a second ALD coating layer 140, etc.) applied to the surface of the optical component 101.

[0071] Referring again to FIG. 1B, the ALD coating 120 may be applied to the surface of the optical component 101 by an atomic layer deposition (ALD) process. During an ALD process, the optical component 101 is exposed to alternating pulses of one or more precursor compounds, and the exposure to the alternating pulses of precursor compounds deposits the ALD coating 120 on the surface of the optical component 101 layer by layer, with each layer having a thickness comparable to the size of a single molecule of the ALD coating material (e.g., monolayer coverage of the surface). The ALD process can coat the entire surface of the optical component 101 with atomic layer precision in a single deposition run. The first precursor may be a metal precursor or a metalloid precursor, and the second precursor may be a reducing compound (e.g., a fluorine source), an oxidizing compound (e.g., an oxygen source), or a combination thereof. In an embodiment, the ALD process may include a first pulse of a first precursor comprising a metal precursor or a metalloid precursor, a second pulse of a second precursor comprising an oxygen source, and a third pulse of a third precursor comprising a fluorine source.

[0072] In embodiments, the ALD process may be a direct reduction ALD process during which a metal or metalloid precursor is deposited on the surface of the optical component 101 and then directly reduced using a reducing agent, such as a fluorine source, to produce an ALD coating. When the ALD coating 120 is a metal fluoride ALD coating, the ALD process for applying the ALD coating 120 may include exposing the surface of the optical component 101 to alternating pulses of a metal precursor and a fluorine source. The exposing of the surface to alternating pulses of a metal precursor and a fluorine source may occur in an ALD chamber, which may be a sealed chamber. The pulses of metal precursor may include a metal precursor. In some embodiments, the pulses of metal precursor may include a metal precursor and one or more inert gases. The inert gas may include a non-reactive gas, such as, but not limited to, a noble gas (e.g., Ar, He, Ne, etc.). The inert gas may act as a carrier to transport the precursor to the ALD chamber. Each pulse of the metal precursor and fluorine source may be of sufficient duration to allow the metal precursor and fluorine source to react with at least 90%, at least 95%, at least 98%, at least 99%, or even at least 99.9% of the reactive sites on the surface of the optical component 101 or the outer surface of a previously applied metal precursor or coating layer during the respective pulse. Between injection of each pulse of the metal precursor and fluorine source, the ALD chamber may be purged with an inert gas (e.g., Ar, He, Ne, etc.) to remove any remaining metal precursor and / or fluorine source before the next pulse.

[0073] In an embodiment, the ALD coating 120 may be a metal fluoride coating, and the ALD process may include exposing the surface of the optical component 101 to a pulse containing a metal precursor, purging the chamber after the metal precursor pulse, and then exposing the optical component 101 to a subsequent pulse of a fluorine source. During the pulse of metal precursor, the metal precursor in the form of a vapor, plasma, or atomized liquid may be injected into the ALD chamber housing the optical component 101. The ALD process may further include heating a metal precursor, such as a magnesium precursor, to a temperature of 95° C. or higher before introducing the metal precursor to the optical component in the ALD chamber. When the surface of the optical component is exposed to the pulse containing the metal precursor, the metal precursor may react with calcium fluoride at the surface of the optical component 101 to bond a monolayer of coordinated metal on the surface of the optical component 101.

[0074] The monolayer of coordinated metal bound to the surface may have a thickness approximately equal to the size of a single molecule of the coordinated metal. For subsequent pulses of metal precursor following the first coating layer, the metal precursor may react with the previously deposited metal fluoride to bond subsequent monolayers of coordinated metal to the exterior surface of the previously deposited ALD coating 120. After depositing and bonding a monolayer of coordinated metal to the exterior surface of the optical component 101, the ALD coating process may further include terminating exposure of the optical component 101 to the metal precursor. Terminating exposure of the optical component 101 to the metal precursor may include stopping the flow of the metal precursor into the ALD chamber. The pulse of metal precursor may have a pulse duration sufficient to cause the metal precursor to react with at least 90%, at least 95%, at least 98%, at least 99%, or at least 99.9% of the reactive calcium fluoride sites at the surface of the optical component. In embodiments, the pulse of metal precursor may have a pulse duration of 10 milliseconds (ms) to 10 seconds (s), or about 1 second. Factors that influence the pulse duration include the vapor pressure of the precursor, the flow rate of the precursor, the reactivity of the precursor with the surface, the volume of the ALD chamber, and the dimensions of the optical components. It is preferable to set the pulse duration to achieve at least 90%, or at least 95%, or at least 98%, or at least 99%, or at least 99.9% coverage, preferably conformal coverage, of the surface area by the precursor or its reaction product. The ALD chamber may then be purged with an inert gas to remove any remaining metal precursor from the ALD chamber before continuing with the ALD process.

[0075] After purging the chamber, the optical component 101 may be exposed to a pulse containing a fluorine source. During the pulse of the fluorine source, the fluorine source may be injected into the chamber housing the optical component 101. The pulse of the fluorine source may include a fluorine source or a fluorine source combined with an inert gas, such as any of the inert gases described herein. By exposing the surface of the optical component 101 to a subsequent pulse containing a fluorine source, the fluorine source may react with the coordinated metal bound to the surface and reduce the coordinated metal to form a metal fluoride (e.g., via a chemical reduction reaction between the fluorine source and the coordinated metal to replace the ligand with fluorine to produce the metal fluoride of the ALD coating). The injection of the fluorine source may be stopped at the end of the pulse when at least 90%, at least 95%, at least 98%, at least 99%, or even at least 99.9% of the metal coordinated at the surface of the optical component 101 has reacted with the fluorine source to form a metal fluoride. In embodiments, the fluorine source pulse may have a pulse duration of 10 ms to 30 s, e.g., 10 ms to 20 s, 10 ms to 10 s, 1 s to 30 s, 1 s to 20 s, 1 s to 10 s, 3 s to 30 s, 3 s to 20 s, or 3 s to 10 s. The fluorine source pulse may be stopped by stopping the flow of the fluorine source into the ALD chamber. The ALD process may be repeated multiple times with a series of alternating pulses of the metal precursor and fluorine source to add additional layers of metal fluoride and increase the thickness of the ALD coating 120.

[0076] In an embodiment, the ALD coating 120 may be a MgF2 ALD coating. In the case of a MgF2 ALD coating, the metal precursor may be a metal-ligand complex containing magnesium as the metal. In an embodiment, the metal precursor may be selected from the group consisting of bis(ethylcyclopentadienyl)magnesium, bis(cyclopentadienyl)magnesium(II), bis(2,2,6,6-tetramethyl-3,5-heptanedionato)magnesium, bis(N,N'-di-sec-butylacetamidinato)magnesium, bis(pentamethylcyclopentadienyl)magnesium, and combinations thereof. Other magnesium-containing compounds may also be suitable as metal precursors for forming the MgF2 ALD coating. The metal precursor may be in the form of a vapor, plasma, liquid, or atomized liquid.

[0077] In embodiments, the ALD coating may be a metal fluoride having a metal other than magnesium. In these cases, similar metal-ligand complexes may be used where the metal is different from magnesium. For example, in embodiments, the metal of the metal precursor may be calcium (Ca), lithium (Li), aluminum (Al), or combinations thereof. In embodiments, the ALD coating may be a CaF2 ALD coating. When the ALD coating is a CaF2 ALD coating, the metal precursor may be selected from the group consisting of Ca(2,2,6,6-tetramethyl-3,5-heptanedionato)2, bis(N,N'-diisopropylformamidinato)calcium(II), bis(N,N'-diisopropylacetamidinato)calcium(II), [Ca3(2,2,6,6-tetramethyl-3,5-heptanedionato)6], Ca(1,2,4-triisopropylcyclopentadienyl)2, and combinations thereof. In an embodiment, the ALD coating may be a LiF ALD coating. When the ALD coating is a LiF ALD coating, the metal precursor may be selected from the group consisting of lithium tert-butoxide, lithium 2,2,6,6-tetramethyl-3,5-heptanedionate, and combinations thereof. In an embodiment, the ALD coating may be an AlF3 ALD coating. The AlF3 ALD coating may be amorphous instead of polycrystalline. When the ALD coating 120 is an AlF3 ALD coating, the metal precursor may be selected from the group consisting of trimethylaluminum (TMA), triethylaluminum (TEA), and combinations thereof. Other aluminum compounds may also be suitable for use as the metal precursor. The metal precursor pulse may include a metal precursor or a mixture of a metal precursor and an inert gas, which may be any of the inert gases previously described herein.

[0078] In embodiments, the ALD coating 120 may be an alloy including multiple different metals. X M Y F Z where A is a first metal selected from the group consisting of Mg, Ca, Li, and Al, M is a second metal different from the first metal A and selected from the group consisting of Mg, Ca, Li, and Al, X is the number of moles of the first metal A, Y is the number of moles of the second metal, and Z is the number of moles of fluorine (F). In an embodiment, the ALD coating 120 is X Al Y F Z or Ca X Al Y F Z where X is the number of moles of Li or Ca, respectively, Y is the number of moles of Al, and Z is the number of moles of F. Other metal fluorides containing mixtures of different metals are possible. Metal fluoride ALD coatings containing multiple different metals may be made by exposing an optical component to metal precursor pulses having multiple different metal precursors, each with a different metal.

[0079] The fluorine source may be derived from a fluorine-containing precursor selected from the group consisting of sulfur hexafluoride (SF6), nitrogen trifluoride (NF3), trifluoroiodomethane (CF3I), hydrogen fluoride (HF), and combinations thereof. In embodiments, the ALD process may be a plasma fluorine source, where the fluorine source is derived from a fluorine-containing precursor or a fluorine-containing precursor and argon (Ar) plasma. In embodiments, the fluorine source may be a plasma including SF6, SF6 and Ar (SF6 / Ar), or NF6 and Ar (NF6 / Ar). In embodiments, the fluorine source may be derived from one or more organic fluorine sources, such as, but not limited to, hexafluoroacetylacetone or other fluorine-containing organic compounds. However, for organic fluorine sources, an additional pulse step, such as a long ozone pulse, may be required in the ALD process to remove carbon compounds from the ALD coating contributed by the organic fluorine source.

[0080] HF is commonly used as a fluorine source in ALD coating operations. However, HF is dangerous to handle and highly corrosive, especially when in contact with water. Therefore, safer alternatives to HF are desirable. SF6 fluorine precursors are significantly safer to use compared to HF and are more productive than organic fluorine sources, which require a four-step process and long ozone pulses to form metal fluoride ALD coatings. In embodiments, the fluorine source may include SF6 or a plasma derived from SF6 (i.e., an SF6-based plasma). In embodiments, the fluorine source may include, consist of, or consist essentially of an SF6-based fluorine source, such as SF6 or an SF6-based plasma. In embodiments, the fluorine source may include, consist of, or consist essentially of a plasma derived from SF6 and Ar (i.e., an SF6 / Ar plasma) or SF6 and other inert gases. When the fluorine source comprises an SF6 / Ar plasma, the flow ratio of Ar to SF6 can be 0.1:1 to 10:1, 0.1:1 to 5:1, 0.1:1 to 2:1, 0.5:1 to 10:1, 0.5:1 to 5:1, 0.5:1 to 2:1, 1:1 to 10:1, 1:1 to 5:1, 1:1 to 2:1, 2:1 to 10:1, 2:1 to 5:1, or about 2:1, where the flow rates are volumetric flow rates in units of sccm (standard cubic centimeters per minute).

[0081] As previously mentioned, the ALD process may be a direct reduction process in which the ALD coating is deposited by attaching a coordinated metal or coordinated metalloid to the surface of the optical component and then directly reducing the coordinated metal or coordinated metalloid with a fluorine source to produce a metal (or metalloid) fluoride ALD coating. However, when SF6, SF6 plasma, or SF6 / Ar plasma is used as the fluorine source, the resulting ALD coating may have a high concentration of carbon impurities originating from the ligands of the coordinated metal. Without intending to be bound by any particular theory, it is believed that sulfur from SF6 reacts with the ligands to damage or fragment them during the reaction of the coordinated metal with the fluorine source to produce the metal fluoride, thus leaving carbon or carbon-containing fragments of the ligand in the ALD coating.

[0082] The concentration of carbon deposits in a metal fluoride ALD coating can be reduced or eliminated by performing an oxide formation step between the metal precursor pulse and the fluorine source pulse. The oxide formation step can include exposing an optical component having a layer of coordinated metal deposited on its surface to an oxygen source for a pulse duration sufficient to oxidize or convert the coordinated metal to a metal oxide. Exposing the coordinated metal to a pulse containing an oxygen source causes the ligands of the coordinated metal to react with oxygen from the oxygen source, replacing the ligands with oxygen, which becomes bonded to the metal or metalloid (e.g., the coordinated metal undergoes an oxidation reaction to convert the coordinated metal layer to a metal oxide layer). After the oxide is formed, the ALD chamber can be purged of residual oxygen source, and the optical component having a layer of metal oxide on its surface can then be exposed to a pulse containing a fluorine source. Exposing the metal oxide to a fluorine source can convert the metal oxide to a metal fluoride ALD coating. The oxygen source may be water (H2O), H2O plasma, ozone (O3), O3 plasma, oxygen (O2), O2 plasma, hydrogen peroxide, other oxygen-containing gases, other oxygen-containing liquids, or combinations thereof. The oxygen source may be in a liquid, gaseous, or plasma state. In an embodiment, the oxygen source pulse may include an oxygen source or an oxygen source in combination with one or more inert gases, which may be any of the inert gases previously described herein.

[0083] When an SF6-based fluorine source is used, metal fluoride ALD coatings prepared by first converting the metal ligands to metal oxides with an oxygen source pulse and then converting the metal oxides to metal fluorides with a fluorine source pulse may yield metal fluoride ALD coatings with lower concentrations of carbon compared to direct reduction of the metal ligands with a fluorine source. Without being bound by any particular theory, it is believed that oxidation of the ligands of a coordinated metal may completely remove the ligands from the metal without decomposing the ligands, thereby eliminating or greatly reducing the fragmentation of organic (carbon-containing) components that remain bound to the metal or that otherwise remain present in the ALD coating. Metal fluoride ALD coatings prepared by oxidation of the metal ligands with an oxygen source pulse and then reduction of the metal oxide with a fluorine source pulse will have a higher oxygen content than metal fluoride ALD coatings produced by direct reduction of the metal ligands with a fluorine source pulse. However, the concentration of oxygen in metal fluoride ALD coatings prepared by the formation of an oxide intermediate was found to be comparable to the oxygen concentration in existing PVD metal fluoride coatings.

[0084] In an embodiment, the ALD coating 120 may be a metal fluoride coating, and the ALD process may include exposing the surface of the optical component 101 to a pulse containing a metal precursor, followed by a pulse containing an oxygen source, and then a pulse containing a fluorine source. The ALD process may include first exposing the optical component to the metal precursor. During the pulse of the metal precursor, the metal precursor, in the form of a vapor, plasma, or atomized liquid, may be introduced, such as by injection, into the ALD chamber housing the optical component 101. When the surface of the optical component is exposed to the pulse containing the metal precursor, the metal precursor may react with CaF2 at the surface of the optical component 101 to bond a monolayer (monolayer) of coordinated metal to the surface of the optical component 101. The metal precursor may be any of the metal precursors previously described herein. The metal precursor pulse may have a duration sufficient for the metal precursor to react with at least 90%, at least 95%, at least 98%, at least 99%, or even at least 99.9% of the reactive calcium fluoride sites on the surface of the optical component. The metal precursor pulse may have a pulse duration of 10 ms to 10 s, or about 1 second. The monolayer of coordinated metal bound to the surface may have a thickness equal to the size of a single molecule of the metal ligand. For pulses of metal precursor subsequent to the first coating layer, the metal precursor may react with the previously deposited metal fluoride ALD coating to bond a subsequent monolayer of coordinated metal to the outer surface of the metal fluoride ALD coating. After depositing and bonding a monolayer of coordinated metal to the outer surface of the optical component 101, the ALD coating process may further include stopping exposure of the optical component 101 to the metal precursor. Stopping exposure of the optical component 101 to the metal precursor may include stopping the flow of metal precursor into the ALD chamber. The ALD chamber may then be purged with an inert gas to remove any remaining metal precursor from the chamber before continuing with the ALD process.

[0085] After exposing the optical component to the metal precursor and purging the ALD chamber, the ALD process may include exposing the optical component with a layer of coordinated metal bonded thereto to an oxygen source. The oxygen source may include water, water plasma, oxygen, oxygen plasma, ozone, ozone plasma, hydrogen peroxide, hydrogen peroxide plasma, an oxygen-containing liquid, an oxygen-containing gas, or a combination thereof. The oxygen source may be in a liquid state, a gas state, or a plasma state. Exposing the optical component to an oxygen source may include introducing a pulse containing an oxygen source into the ALD chamber housing the optical component. In an embodiment, the oxygen source pulse may include an oxygen source or an oxygen source in combination with one or more inert gases, which may be any of the inert gases previously described herein. Exposing the optical component to the oxygen-containing pulse may oxidize the coordinated metal to form a metal oxide on the surface of the optical component. The oxygen source pulse may have a pulse duration sufficient for the oxygen source to react with at least 90%, at least 95%, at least 98%, at least 99%, or even at least 99.9% of the coordinated metals bound to the surface of the optical component (or the surface of the ALD coating for the application of a subsequent coating layer). The oxygen source pulse may have a pulse duration of 0.1 seconds to 1 second, or about 0.3 seconds. The ALD process may further include, at the end of the oxygen source pulse, stopping exposure of the optical component to the oxygen source pulse, such as by stopping the flow of oxygen source to the ALD chamber. In an embodiment, the ALD chamber may then be purged with an inert gas after the oxygen source pulse, which will remove any remaining oxygen and organic compounds from the ALD chamber.

[0086] The ALD process may further include exposing the optical component having a metal oxide layer deposited thereon to a fluorine source after the oxygen source pulse. Exposing the optical component to the fluorine source may include introducing a pulse containing a fluorine source into the ALD chamber housing the optical component. The fluorine source may be any of the compositions previously described herein for fluorine sources. In embodiments, the fluorine source is an SF6-based fluorine source, such as, but not limited to, SF6, SF6 plasma, SF6 / Ar plasma, or combinations thereof. The fluorine from the fluorine source may reduce the metal oxide to form a metal fluoride ALD coating on the surface of the optical component. The fluorine source pulse may have a pulse duration sufficient for the fluorine to react with at least 90%, at least 95%, at least 98%, at least 99%, or even at least 99.9% of the metal oxide on the surface of the optical component (or on the surface of the ALD coating for the application of a subsequent coating layer). The fluorine source pulse may have a pulse duration of 10 ms to 30 s, e.g., 10 ms to 20 s, 10 ms to 10 s, 1 s to 30 s, 1 s to 20 s, 1 s to 10 s, 3 s to 30 s, 3 s to 20 s, or 3 s to 10 s. The process may further include stopping exposure of the optical component to the fluorine source at the end of the fluorine source pulse, such as by stopping the flow of the fluorine source into the ALD chamber. As noted above, exposing the optical component to an oxygen source after exposure to the metal precursor but before exposure to the fluorine source will result in a lower concentration of carbon in the ALD coating applied to the optical component compared to alternating pulses of the metal precursor and fluorine source without a pulse containing an oxygen source.

[0087] The optical component may be contacted / exposed to a metal precursor and a fluorine source, or a metal precursor, an oxygen source, and a fluorine source, at operating conditions sufficient for the metal precursor, the fluorine source, the oxygen source, or a combination thereof to undergo a chemical reaction at the surface of the optical component. The ALD process may be performed at a process temperature sufficient for the metal precursor, the oxygen source, the fluorine source, or a combination thereof to undergo a reaction at the surface of the optical component. In an embodiment, the ALD process may be a plasma-assisted ALD process in which a plasma material is utilized in one or more of the metal precursor pulses, the oxygen source pulses, the fluorine source pulses, or a combination thereof, and the ALD process may be performed at a process temperature sufficient to generate and maintain the material in a plasma state during the pulse. In an embodiment, the ALD process may include depositing an ALD coating on the surface of the optical component at a process temperature of 120° C. to 250° C. The optical component may be exposed / exposed to a metal precursor, an oxygen source, a fluorine source, or a combination thereof to undergo a chemical reaction at the surface of the optical component.

[0088] In embodiments, the ALD process may be a plasma-assisted ALD process in which plasma materials are utilized in one or more of a metal precursor pulse, an oxygen source pulse, a fluorine source pulse, or a combination thereof. The metal precursor, oxygen source, fluorine source, or a combination thereof may be converted into a plasma by heating the material and exposing the material to an electric current or a strong electromagnetic field. The material (e.g., the metal precursor, oxygen source, fluorine source, or a combination thereof) may be heated to an ALD process temperature and exposed to an electric current sufficient to convert the material into a plasma. In embodiments, converting the material (e.g., the metal precursor, oxygen source, fluorine source, or a combination thereof) into a plasma may include heating the material to a temperature of 120° C. to 250° C. and applying an electric current having a power of 100 watts (W) to 300 W, or about 200 W.

[0089] The ALD process may be repeated multiple times to increase the thickness of the ALD coating. Each iteration of the ALD process may add another molecular layer of the ALD coating material to the ALD coating. The thickness of the ALD coating may be controlled by controlling the number of iterations of the ALD process, i.e., controlling the number of molecular layers of the ALD coating material in the ALD coating.

[0090] In embodiments, the ALD coating 120 may be a metal fluoride ALD coating that comprises a stack of distinct layers, where each distinct layer comprises a metal fluoride having a different metal than the metal fluoride in an adjacent layer of the stack. In embodiments, the ALD coating 120 may comprise a stack of metal fluorides, including an amorphous AlF3 ALD coating disposed between layers of a polycrystalline metal fluoride ALD coating, such as, but not limited to, a CaF2, MgF2, or LiF2 ALD coating. Other combinations of distinct metal fluoride layers formed in a stack are also contemplated.

[0091] An ALD process for forming an ALD coating on an optical component may further include cleaning the surface of the optical component prior to forming the ALD coating thereon. In embodiments, the ALD process does not require or include rotating the optical component during the coating process. In embodiments, the ALD process does not require or include holding the optical component in a fixture that masks at least a portion of the surface of the optical component. In embodiments, one or more, or two or more, or three or more surfaces, or up to the entire surface of an optical component are simultaneously coated with an ALD coating in an ALD process.

[0092] 1B, an ALD coating 120 may be bonded to a surface of the optical component 101 (e.g., optical surfaces 102, 104, and 106 of the coated optical component 100 of FIGS. 1A-1D), such as bonded to CaF2 at the surface of the optical component 101. The ALD coating 120 may include a metal fluoride, such as, but not limited to, magnesium fluoride. In embodiments, the ALD coating may include a metal fluoride ALD coating or metal fluoride ALD coating layer that includes 90% or more, 95% or more, 98% or more, 99% or more, or 99.9% or more metal fluoride, based on the total weight of the ALD coating or metal fluoride ALD coating layer, respectively.

[0093] In embodiments, the ALD coating or ALD coating layer can be a metal fluoride ALD coating and can include sulfur in addition to the metal fluoride. In embodiments, the ALD coating or ALD coating layer can include a metal fluoride ALD coating and can have a sulfur content in the metal fluoride ALD coating greater than zero parts per million (ppm), e.g., greater than zero ppm to 300 ppm, or greater than 1 ppm to 250 ppm, or greater than 5 ppm to 200 ppm, or greater than 10 ppm to 150 ppm, or greater than 25 ppm to 125 ppm.

[0094] In embodiments, an ALD coating or ALD coating layer can include a metal fluoride ALD coating, which can be substantially free of carbon. In embodiments, the metal fluoride ALD coating can have a concentration of carbon in the metal fluoride ALD coating of 10,000 ppm or less, or 5,000 ppm or less, or 1,000 ppm or less, or less than 500 ppm.

[0095] The ALD coating 120 may have a thickness sufficient to cover the surface of the optical component 101 without substantially exposing the surface of the optical component to the atmosphere within the coverage area. In embodiments, the ALD coating may include a metal fluoride ALD coating or metal fluoride ALD coating layer having a thickness of 10 nanometers (nm) or less, e.g., 8 nm or less, or even 5 nm or less. In embodiments, the ALD coating may include a metal fluoride ALD coating or metal fluoride ALD coating layer having a thickness of 0.25 nm or more, 0.50 nm or more, or even 1.0 nm or more. In embodiments, the ALD coating may include a metal fluoride ALD coating or a metal fluoride ALD coating layer having a thickness of 0.25 nm to 10 nm, 0.25 nm to 8 nm, 0.25 nm to 5 nm, 0.35 nm to 10 nm, 0.35 nm to 8 nm, 0.35 nm to 5 nm, 0.5 nm to 10 nm, 0.5 nm to 8 nm, 0.5 nm to 5 nm, 1 nm to 10 nm, 1 nm to 8 nm, 1 nm to 5 nm, 0.25 nm to 1 nm, or 5 nm to 10 nm. In embodiments, the ALD coating may include multiple ALD coating layers, where each of the multiple ALD coating layers is made from a different coating material. In these embodiments, each of the multiple ALD coating layers can have a thickness of 0.25 nm to 10 nm, 0.25 nm to 8 nm, 0.25 nm to 5 nm, 0.35 nm to 10 nm, 0.35 nm to 8 nm, 0.35 nm to 5 nm, 0.5 nm to 10 nm, 0.5 nm to 8 nm, 0.5 nm to 5 nm, 1 nm to 10 nm, 1 nm to 8 nm, 1 nm to 5 nm, 0.25 nm to 1 nm, or 5 nm to 10 nm. The total thickness of the ALD coating can be the sum of the thicknesses of the individual ALD coating layers.

[0096] The ALD coating 120 may be a conformal coating having a uniform thickness across the entire covered surface. In embodiments, the ALD coating 120 may have a thickness that varies by 5% or less, 4% or less, 3% or less, 2% or less, 1% or less, or even 0.5% or less from the average thickness of the ALD coating 120. The average thickness of the ALD coating is the thickness of the ALD coating averaged over all of the surface area of ​​the surface in contact with the ALD coating 120.

[0097] As previously mentioned, the ALD coating process does not require holding the optical component in a fixture and rotating the optical component during the coating process. Thus, the ALD coating process may deposit an ALD coating uniformly on one, multiple, or all of the surfaces of the optical component. In embodiments, the coated optical component may include an ALD coating deposited on and / or in contact with at least 95%, at least 98%, at least 99%, or even at least 99.5% of the optical surface of the optical component 101 intended to be coated (e.g., surfaces 102, 104, and 106 of the coated optical component 100 of FIGS. 1A-1D; surfaces 202, 204, 206, and 208 of the coated optical component 200 of FIGS. 3A-3C; surfaces 402, 404, and 406 of the coated optical component 400 of FIG. 4; surface 504 of the high NA objective lens 502 of FIG. 5; or other optical surfaces). The surfaces of the optical component 101 that are intended to be coated are those surfaces that are not intentionally masked to prevent ALD coating. The ALD coating may also be deposited on and / or in contact with other non-optical surfaces of the optical component, such as surfaces on which a laser beam or light beam is not expected to be incident. In embodiments, the coated optical component 100 does not include optical surfaces that have more than 10%, more than 5%, or even more than 1% of their surface area uncoated.

[0098] In embodiments, a coated optical component (e.g., coated optical component 100, 200, 400; high NA objective lens 500, or other optical component) may have an ALD coating or ALD coating layer, including a metal oxide ALD coating and / or a semi-metal oxide ALD coating. In embodiments, the ALD coating 120 may be a metal oxide coating, such as, but not limited to, an alumina (Al2O3) ALD coating, a hafnium oxide (HfO2) ALD coating, a lanthanum oxide (La2O3) ALD coating, or a gadolinium oxide (Gd2O3) ALD coating. When the ALD coating is a metal oxide ALD coating, an ALD process for depositing the metal oxide ALD coating on a surface of the optical component may include exposing the surface of the optical component to alternating pulses of a metal precursor and an oxygen source. The metal precursor may be a metal bonded to one or more organic groups. In embodiments, the metal oxide ALD coating may be an alumina ALD coating. For alumina ALD coatings, the metal precursor of the metal precursor pulse may be an aluminum precursor selected from the group consisting of trimethylaluminum (TMA), triethylaluminum (TEA), and combinations thereof. Other aluminum compounds may also be suitable for use as the metal precursor. The metal precursor may be in the form of a vapor, plasma, liquid, or atomized liquid. In embodiments, the metal precursor pulse may include a metal precursor in combination with one or more inert gases, which may be any of the inert gases previously described herein.

[0099] The oxygen source for preparing metal oxide ALD coatings may be the same as the oxygen sources previously described herein in the context of preparing metal fluoride coatings using SF6-based fluorine sources. Specifically, the oxygen source may be water (H2O), H2O plasma, ozone (O3), O3 plasma, oxygen (O2), O2 plasma, hydrogen peroxide (H2O2), hydrogen peroxide plasma, other oxygen-containing gases, other oxygen-containing liquids, or combinations thereof. The oxygen source may be selected from the group consisting of water (H2O), H2O plasma, ozone (O3), O3 plasma, oxygen (O2), O2 plasma, hydrogen peroxide, hydrogen peroxide plasma, other oxygen-containing gases, other oxygen-containing liquids, and combinations thereof. The oxygen source may be in a liquid state, a gas state, or a plasma state. In an embodiment, the oxygen source pulse may include an oxygen source or an oxygen source combined with one or more inert gases, which may be any of the inert gases previously described herein. By exposing the metal precursor bound to the surface of the optical component to a pulse containing an oxygen source, the metal precursor may react with oxygen from the oxygen source to replace organic components of the metal precursor with oxygen, which bonds with the metal or metalloid (e.g., the coordinated metal undergoes an oxidation reaction to oxidize or convert the metal precursor to a metal oxide layer).

[0100] An ALD process for preparing a metal oxide ALD coating or coating layer may first include exposing the optical component to a metal precursor. During a pulse of the metal precursor, the metal precursor in the form of a vapor, plasma, or atomized liquid may be introduced, such as by injection, into an ALD chamber housing the optical component 101. By exposing the surface of the optical component to a pulse containing the metal precursor, the metal precursor may react with a component on the surface of the optical component 101 such that a monolayer of the metal precursor (or a reaction product thereof) is bonded to the surface of the optical component 101. The component on the surface of the optical component 101 may include calcium fluoride, a metal oxide previously deposited on the optical component 101, a metal fluoride previously deposited on the optical component, or a metalloid oxide previously deposited on the surface of the optical component. The metal precursor may be any of the metal precursors previously described herein. The metal precursor pulse may have a sufficient duration to allow the metal precursor to react with at least 90%, at least 95%, at least 98%, at least 99%, or even at least 99.9% of the reactive sites on the surface of the optical component. The metal precursor pulse may have a pulse duration of 10 ms to 10 s, or about 1 second. The monolayer of metal precursor bound to the surface may have a thickness approximately equal to the size of one molecule of the metal precursor. For pulses of metal precursor subsequent to the first coating layer, the metal precursor may react with the previously deposited metal oxide ALD coating to bond a subsequent monolayer of metal precursor to the outer surface of the metal oxide ALD coating. After depositing and bonding a monolayer of metal precursor to the outer surface of the optical component 101, the ALD coating process may further include stopping exposure of the optical component 101 to the metal precursor. Stopping exposure of the optical component 101 to the metal precursor may include stopping the flow of the metal precursor to the ALD chamber. The ALD chamber may then be purged with an inert gas to remove any remaining metal precursor from the chamber before continuing the ALD process.

[0101] After stopping the exposure of the optical component to the metal precursor and purging the ALD chamber, the ALD process for preparing a metal oxide ALD coating may include exposing the optical component having a layer of metal precursor bound thereto to an oxygen source. Exposing the optical component to the oxygen source may include introducing a pulse containing an oxygen source into the ALD chamber housing the optical component. Exposing the optical component to the oxygen-containing pulse may oxidize the metal precursor to form a metal oxide on the surface of the optical component. The oxygen source pulse may have a pulse duration sufficient for the oxygen source to react with at least 90%, at least 95%, at least 98%, at least 99%, or even at least 99.9% of the metal precursor bound to the surface of the optical component (or the surface of the ALD coating for the application of a subsequent coating layer). The oxygen source pulse may have a pulse duration of 0.1 seconds to 1 second, or about 0.3 seconds. The ALD process may further include stopping the exposure of the optical component to the oxygen source pulse, such as by stopping the flow of the oxygen source to the ALD chamber at the end of the pulse. In an embodiment, the ALD chamber may then be purged with an inert gas after the oxygen source pulse, which will remove any residual oxygen and organic compounds or fractions from the ALD chamber. The ALD process for depositing a metal oxide ALD coating on an optical component may be carried out under the same operating conditions described above in the context of depositing a metal fluoride ALD coating. The ALD process for depositing a metal oxide ALD coating may be repeated multiple times to increase the thickness of the metal oxide ALD coating.

[0102] In embodiments, an ALD coating may comprise primarily a metal oxide, such as, but not limited to, alumina. In embodiments, an ALD coating may comprise a metal oxide ALD coating or metal oxide ALD coating layer that comprises 90% or more, 95% or more, 98% or more, 99% or more, or 99.9% or more by weight metal oxide, based on the total weight of the metal oxide ALD coating or metal oxide ALD coating layer, respectively.

[0103] In an embodiment, the ALD coating 120 may be a metalloid oxide coating, such as, but not limited to, a silica (SiO2) ALD coating. When the ALD coating is a metalloid oxide coating, an ALD process for depositing a metalloid oxide ALD coating on a surface of an optical component may include exposing the surface of the optical component to alternating pulses of a metalloid precursor and an oxygen source. The metalloid precursor may be a metalloid bonded to one or more organic groups, such as, but not limited to, silicon (Si), boron (B), germanium (Ge), etc. In an embodiment, the metalloid oxide ALD coating may be a silica ALD coating. For silica ALD coatings, the metalloid precursor may be a silica precursor selected from the group consisting of bis(tert-butylamino)silane (i.e., SiH2(NHtBu)2, BTBAS); di(sec-butylamino)silane (i.e., SiH3(NsecBu2), DSBAS); diisopropylaminotrisilylamine; a compound having the formula SiH2(NRR')2, where each of R and R' is independently a methyl group, an ethyl group, or both, and combinations thereof. Other silica compounds may also be suitable for use as the metalloid precursor. The metalloid precursor may be in the form of a vapor, plasma, liquid, or atomized liquid. In embodiments, the pulse of metalloid precursor may include the metalloid precursor in combination with one or more inert gases, which may be any of the inert gases previously described herein.

[0104] The oxygen source for preparing the metalloid oxide ALD coating may be the same as the oxygen sources previously described herein. In particular, the oxygen source may be water (H2O), H2O plasma, ozone (O3), O3 plasma, oxygen (O2), O2 plasma, hydrogen peroxide, hydrogen peroxide plasma, other oxygen-containing gases, other oxygen-containing liquids, and combinations thereof. The oxygen source may be in a liquid state, a gas state, or a plasma state. In an embodiment, the oxygen source pulse may include an oxygen source or an oxygen source combined with one or more inert gases, which may be any of the inert gases previously described herein. By exposing the metalloid precursor bound to the surface of the optical component to a pulse containing an oxygen source, the metalloid precursor may react with oxygen from the oxygen source to replace organic components of the metalloid precursor with oxygen, which bonds to the metalloid (e.g., the metalloid precursor undergoes an oxidation reaction to convert the metalloid precursor to a metalloid oxide layer).

[0105] An ALD process for preparing a metalloid oxide ALD coating or coating layer may first include exposing the optical component to a metalloid precursor. During a pulse of metalloid precursor, the metalloid precursor in the form of a vapor, plasma, or atomized liquid may be introduced, such as by injection, into an ALD chamber housing the optical component 101. By exposing the surface of the optical component to a pulse containing the metalloid precursor, the metalloid precursor may react with components at the surface of the optical component 101 to bond a monolayer of the metalloid precursor to the surface of the optical component 101. The components at the surface of the optical component 101 may include calcium fluoride, a metal oxide previously deposited on the optical component 101, a metal fluoride previously deposited on the optical component, or a metalloid oxide previously deposited on the surface of the optical component. The metalloid precursor may be any of the metalloid precursors previously described herein. The metalloid precursor pulse may have a sufficient duration to allow the metalloid precursor to react with at least 90%, at least 95%, at least 98%, at least 99%, or even at least 99.9% of the reactive sites on the surface of the optical component. The metalloid precursor pulse may have a pulse duration of 10 ms to 10 s, or about 1 second. The monolayer of metalloid precursor bound to the surface may have a thickness approximately equal to the size of one molecule of the metalloid precursor. For pulses of metalloid precursor subsequent to the first coating layer, the metalloid precursor may react with the previously deposited metalloid oxide ALD coating to bond a subsequent monolayer of the metalloid precursor to the outer surface of the metalloid oxide ALD coating. After depositing and bonding a monolayer of the metalloid precursor to the outer surface of the optical component 101, the ALD coating process may further include terminating the exposure of the optical component 101 to the metalloid precursor. Terminating the exposure of the optical component 101 to the metalloid precursor may include stopping the flow of the metalloid precursor to the ALD chamber. The ALD chamber may then be purged with an inert gas to remove any remaining metalloid precursor from the chamber before continuing with the ALD process.

[0106] After stopping exposure of the optical component to the metalloid precursor and purging the ALD chamber, the ALD process for preparing a metalloid oxide ALD coating may include exposing the optical component having a layer of metalloid precursor bound thereto to an oxygen source. Exposing the optical component to the oxygen source may include introducing a pulse containing an oxygen source into the ALD chamber housing the optical component. Exposing the optical component to the oxygen-containing pulse may oxidize the metalloid precursor to form a metalloid oxide such as silica on the surface of the optical component. The oxygen source pulse may have a pulse duration sufficient for the oxygen source to react with at least 90%, at least 95%, at least 98%, at least 99%, or even at least 99.9% of the metalloid precursor bound to the surface of the optical component (or the surface of the ALD coating for the application of a subsequent coating layer). The oxygen source pulse may have a pulse duration of 0.1 to 1 second, or about 0.3 seconds. The ALD process may further include stopping the exposure of the optical component to the oxygen source pulse, such as by stopping the flow of the oxygen source to the ALD chamber at the end of the pulse. In an embodiment, the ALD chamber may then be purged with an inert gas after the oxygen source pulse, which will remove any residual oxygen and organic compounds from the ALD chamber. The ALD process for depositing a half-metal oxide ALD coating on an optical component may be performed under the same operating conditions described above in the context of depositing a metal fluoride ALD coating. The ALD process for depositing a half-metal oxide ALD coating may be repeated multiple times to increase the thickness of the half-metal oxide ALD coating.

[0107] In embodiments, an ALD coating may comprise primarily a metalloid oxide, such as, but not limited to, a silica ALD coating. In embodiments, an ALD coating may comprise a metalloid oxide ALD coating or a metalloid oxide ALD coating layer that comprises 90% or more, 95% or more, 98% or more, 99% or more, or 99.9% or more by weight of a metalloid oxide, based on the total weight of the metalloid oxide ALD coating or a metalloid oxide ALD coating layer, respectively.

[0108] The metal oxide ALD coatings and metalloid oxide ALD coatings may have similar properties to those described above for metal fluoride ALD coatings. Specifically, the ALD coatings (e.g., metal oxides and / or metalloid oxides) may be bonded to the surfaces of the optical component 101 (e.g., surface 102 and other surfaces), such as to CaF2 at the surface of the optical component. In embodiments, the ALD coatings or ALD coating layers that include metal oxides and / or metalloid oxides may be substantially free of carbon. In embodiments, the metal oxide ALD coatings and / or metalloid oxide ALD coatings may have concentrations of carbon in the metal oxide ALD coatings and / or metalloid oxide ALD coatings, respectively, of less than 10,000 ppm, or less than 5,000 ppm, or less than 1,000 ppm, or less than 500 ppm.

[0109] An ALD coating or ALD coating layer comprising a metal oxide and / or a metalloid oxide may have a thickness of 0.25 nm to 10 nm, 0.25 nm to 8 nm, 0.25 nm to 5 nm, 0.5 nm to 10 nm, 0.5 nm to 8 nm, 0.5 nm to 5 nm, 1 nm to 10 nm, 1 nm to 8 nm, 1 nm to 5 nm, 0.25 nm to 1 nm, or 5 nm to 10 nm. In embodiments, an ALD coating may include multiple ALD coating layers, where each of the multiple ALD coating layers is made from a different material. In these embodiments, each of the multiple ALD coating layers can have a thickness of 0.25 nm to 10 nm, 0.25 nm to 8 nm, 0.25 nm to 5 nm, 0.5 nm to 10 nm, 0.5 nm to 8 nm, 0.5 nm to 5 nm, 1 nm to 10 nm, 1 nm to 8 nm, 1 nm to 5 nm, 0.25 nm to 1 nm, or 5 nm to 10 nm. The total thickness of the ALD coating can be the sum of the thicknesses of the individual ALD coating layers.

[0110] In embodiments, the coated optic may include an ALD coating and / or ALD coating layer comprising metal oxides and / or metalloid oxides deposited on and / or in contact with at least 95%, at least 98%, at least 99%, or even at least 99.5% of the optical surfaces of the optical component 101 intended to be coated (e.g., surfaces 102, 104, and 106 of the coated optic 100 of FIGS. 1A-1D; surfaces 202, 204, 206, and 208 of the coated optic 200 of FIGS. 3A-3C; surfaces 402, 404, and 406 of the coated optic 400 of FIG. 4; surface 504 of the high NA objective lens 502 of FIG. 5; or surfaces that are not intentionally masked, which non-limiting examples may include one or more of: surfaces 102, 104, and 106 of the coated optic 100 of FIGS. 1A-1D; surfaces 202, 204, 206, and 208 of the coated optic 200 of FIGS. 3A-3C; surfaces 402, 404, and 406 of the coated optic 400 of FIG. 4; surface 504 of the high NA objective lens 502 of FIG. 5; or other optical surfaces). ALD coatings may also be deposited on other non-optical surfaces of the optical component, such as surfaces on which a laser beam or light beam is not expected to be incident.

[0111] As mentioned above, and referring again to FIG. 6, coated optical component 100 may have an ALD coating 120 including multiple ALD coating layers (e.g., first ALD coating layer 130, second ALD coating layer 140, etc.) applied to a surface of optical component 101. In an embodiment, coated optical component 100 may have a first ALD coating layer 130 in direct contact with one or more of the surfaces of optical component 101 (e.g., surfaces 102, 104, and 106 of coated optical component 100 of FIGS. 1A-1D; surfaces 202, 204, 206, and 208 of coated optical component 200 of FIGS. 3A-3C; surfaces 402, 404, and 406 of coated optical component 400 of FIG. 4; surface 504 of high NA objective lens 502 of FIG. 5; or other optical surfaces) and at least one second ALD coating layer 140 applied over first ALD coating layer 130. The first ALD coating layer 130 may have an inner surface 132 directly bonded to the CaF2 at a surface of the optical component 101 (e.g., first surface 102) and an outer surface 134 facing away from the surface of the optical component 101. The second ALD coating layer 140 may be a different material than the first ALD coating layer 130. The second ALD coating layer 140 may have an inner surface 142 directly bonded to the outer surface 134 of the first ALD coating layer 130. The second ALD coating layer 140 may have an outer surface 144 facing away from the first ALD coating layer 130. The second ALD coating layer 140 may be bonded directly to the first ALD coating layer 130 such that an inner surface 142 of the second ALD coating layer 140 contacts and bonds with an outer surface 134 of the first ALD coating layer 130 without any intervening layers or coatings disposed between the first ALD coating layer 130 and the second ALD coating layer 140. One or more additional ALD coating layers may be applied over the second ALD coating layer 140 to provide a stack of ALD coating layers. The first ALD coating layer 130, the second ALD coating layer 140, a subsequent ALD coating layer, or a combination thereof, may have a thickness of less than 10 nm, such as 0.25 nm to 10 nm, as previously discussed.

[0112] Specific examples of laminates A coated optical component 100 having an ALD coating 120 comprising multiple ALD coating layers may be prepared by applying a first ALD coating layer 130 to a surface of the optical component (e.g., surfaces 102, 104, and 106 of coated optical component 100 of FIGS. 1A-1D; surfaces 202, 204, 206, and 208 of coated optical component 200 of FIGS. 3A-3C; surfaces 402, 404, and 406 of coated optical component 400 of FIG. 4; surface 504 of high NA objective lens 502 of FIG. 5; or other optical surface) and applying a second ALD coating layer 140 over first ALD coating layer 130 such that the first ALD coating layer 130 is disposed between the optical component 101 and the second ALD coating layer 140. First ALD coating layer 130 and second ALD coating layer 140 may be deposited on one or more surfaces of optical component 101 according to any of the ALD processes previously described herein.

[0113] Referring again to FIG. 6, in an embodiment, the first ALD coating layer 130 can be a metal fluoride ALD coating having a metal different from calcium, and the second ALD coating layer 140 can be a metal oxide or semi-metal oxide coating. In an embodiment, the first ALD coating layer 130 can be a MgF2 ALD coating, and the second ALD coating layer 140 can be a silica ALD coating, an alumina ALD coating, or both. In an embodiment, the first ALD coating layer 130 comprised of a metal fluoride ALD coating can be a buffer layer, and the second ALD coating layer 140 comprised of a silica ALD coating, an alumina ALD coating, or both can be a capping layer. The MgF2 ALD coating can have a thickness of 0.25 nm to 10 nm, or 0.25 nm to 5 nm, and the capping layer can have a thickness of 1 nm to 10 nm. A buffer layer comprised of an MgF2 ALD coating may be disposed between the optical component 101 and a capping layer comprised of a silica ALD coating, an alumina ALD coating, or both. In an embodiment, the first ALD coating layer 130 may be comprised of an MgF2 ALD coating, which may have a thickness of 0.25 nm to 5 nm, and the second ALD coating layer 140 is a capping layer and may be a silica ALD coating, which may have a thickness of 1 nm to 10 nm. A buffer layer comprised of an MgF2 ALD coating may be disposed between the optical component 101 and a buffer layer comprised of a silica ALD coating. In an embodiment, the second ALD coating layer 140 is a capping layer and may be an alumina ALD coating, which may have a thickness of 0.35 nm to 10 nm.

[0114] In embodiments, coated optic 100 can include, consist of, or consist essentially of optical component 101 and an ALD coating 120 deposited on and / or in contact with one or more of the surfaces of optical component 101. In embodiments, ALD coating 120 can include, consist of, or consist essentially of a first ALD coating layer 130 and a second ALD coating layer 140. First ALD coating layer 130 can consist of, or consist essentially of, a metal fluoride ALD coating and is in direct contact with a surface of the optical component (e.g., surfaces 102, 104, and 106 of coated optic 100 of FIGS. 1A-1D; surfaces 202, 204, 206, and 208 of coated optic 200 of FIGS. 3A-3C; surfaces 402, 404, and 406 of coated optic 400 of FIG. 4; surface 504 of high NA objective lens 502 of FIG. 5; or other optical surface). Second ALD coating layer 140 may consist of, or consist essentially of, a metal oxide ALD coating, a metalloid oxide ALD coating, or both, and may be bonded directly to outer surface 134 of first ALD coating layer 130 such that first ALD coating layer 130 is disposed between the surface of optical component 101 and second ALD coating layer 140. In embodiments, first ALD coating layer 130 may consist of, or consist essentially of, magnesium fluoride. In embodiments, second ALD coating layer 140 may consist of, or consist essentially of, silica, alumina, or both.

[0115] The coated optics 100, 300, 400, 500 of the present disclosure having an ALD coating 120 deposited thereon may be used as an optical component in various DUV applications, such as DUV lithography or DUV inspection systems. The coated optics may be used with lasers having wavelengths in the DUV range, such as, but not limited to, beams having wavelengths from 190 nm to 266 nm. In embodiments, the coated optics of the present disclosure may be used with beams having wavelengths longer than 266 nm. EXAMPLES

[0116] Embodiments of the coated optical components and ALD processes for producing the coated optical components described herein will be further elucidated by the following examples.

[0117] Example 1 In Example 1, an optical component was coated with a first ALD coating layer and a second ALD coating layer on the first ALD coating layer to prepare a coated optical component. The optical component used in Example 1 was a CaF2 prism as shown in Figures 1A-1D, which had a first surface 102 (e.g., beam entrance and exit surfaces), a first TIR surface 104, and a second TIR surface 106. The first surface 102 had a length of 30 mm and a height of 20 mm. The first TIR surface 104 had a length of 20 mm and a height of 20 mm. The second TIR surface 106 had a width of 25 mm and a height of 20 mm.

[0118] The first ALD coating layer was a MgF2 ALD coating having a thickness of 4 nm. The MgF2 ALD coating was applied to the first surface 102, the first TIR surface 104, and the second TIR surface 106. The MgF2 ALD coating was prepared according to the ALD process disclosed herein using an ALD chamber maintained at a reactor temperature of 150° C. The magnesium precursor was (EtCp)2Mg (i.e., bis(ethylcyclopentadienyl)magnesium). The bubbler temperature was set at 92° C. and the ICP plasma power was 200 W. The metal precursor pulse, including (EtCp)2Mg, had a pulse duration of 0.5 seconds, followed by an inert gas purge for 9 seconds. The metal precursor pulse and purge were followed by a water pulse having a duration of 40 milliseconds, followed by an inert gas purge for 8 seconds. After the water pulse and purge, the optics were subjected to a fluorine source pulse containing a mixture of SF6 and argon. The SF6 / argon flow ratio was 30 / 15 and the fluorine source pulse had a duration of 7 seconds. The fluorine source pulse was followed by a purge pulse. The sequence of metal precursor pulse / water pulse / fluorine source pulse was repeated until the MgF2 ALD coating had a thickness of 4 nm.

[0119] The second ALD coating layer was a silica (SiO2) ALD coating applied to the outer cladding surface of the MgF2 ALD coating layer. The second ALD coating layer had a thickness of 6 nm. The SiO2 ALD coating layer was prepared according to the ALD process disclosed herein in an ALD chamber maintained at a reactor temperature of 150°C. The silica precursor was an alkylaminosilylamine (ORTHRUS™ alkylaminosilylamine available from Air Liquide). The bubbler temperature was set at 60°C and the ICP plasma power was 300 W. The optical component was first exposed to a silica precursor pulse containing a silica precursor with a pulse duration of 0.4 seconds. The silica precursor pulse was followed by an 8 second purge of inert gas. Argon (Ar) was used as the inert gas to purge the ALD chamber throughout the examples. After the silica precursor pulse and purge, the optical component was subjected to an O2 plasma and an O2 plasma pulse containing argon. The O2 plasma pulse had a ratio of Ar / O2 flows of 35 / 15. The O2 plasma pulse had a duration of 9 seconds, followed by an 8 second purge of inert gas. The series of silica precursor pulses followed by O2 pulses were repeated until the thickness of the SiO2 ALD coating layer was 6 nm. Referring to FIG. 7, the physical thickness of each of the first and second ALD coating layers is shown in a graph. A comparative uncoated optical component having the same shape and the same dimensions as shown in FIGS. 1A-1D was used as a comparative example.

[0120] The CaF2 prism of Example 1 is used to change the laser beam direction of a laser beam with a wavelength of 193 nm. The transmittance of the first surface (e.g., surface 102, which is the beam entrance / exit surface) of the coated optical component of Example 1 was then compared to the transmittance of the first surface of an uncoated CaF2 optical component having the same shape. The first surface of this optical component is the surface where the laser beam enters and exits the prism. The uncoated CaF2 optical component provides a comparative example. The uncoated optical component and the coated optical component of Example 1 were each irradiated with an ArF laser beam having a wavelength of 193.4 nm, and the transmittance of P-polarized light as a function of the angle of incidence (AOI) was determined. The transmittance of a surface is defined as the fraction of the beam power of the laser beam incident on the first surface 102 that passes through the first surface 102, and is expressed as a percentage. The transmittance percentage can be determined using a spectrophotometer or an optical transmittance meter according to known methods. For a flat surface, the angle of incidence (AOI) refers to the acute angle between the ArF laser beam path and a line perpendicular to the plane of the surface on which the ArF laser beam is incident.

[0121] Referring now to Figure 8, the percentage transmission (y-axis) as a function of AOI (x-axis) for the comparative uncoated optic shows 100% transmission for a P-polarized laser beam at Brewster's angle of 55.6° for a calcium fluoride prism. Referring now to Figure 9, the percentage transmission (y-axis) as a function of AOI (x-axis) for the coated optic of Example 1 also shows 100% transmission for a P-polarized laser beam at Brewster's angle of 55.6°. This indicates that the ALD coating of Example 1, which includes a first ALD coating layer of MgF2 and a second ALD coating layer of silica, does not change the transmission of the beam through the first surface (e.g., beam entrance / exit surface) compared to the comparative uncoated optic having the same geometry.

[0122] The internal reflectance of P-polarized light of a 193.4 nm wavelength ArF laser beam was determined for the TIR surfaces (e.g., the first TIR surface 104 and the second TIR surface 106 in FIG. 1A) as a function of the TIR angle of incidence (AOI) for the coated optical component of Example 1 and the comparative uncoated optical component. The internal reflectance of a surface is defined as the fraction of the beam power of the laser beam incident on the TIR surface that is reflected off the TIR surface, expressed as a percentage. The internal reflectance can be determined using a spectrophotometer or optical transmittance meter according to known methods. FIG. 10 plots the percentage of internal reflectance (y-axis) as a function of the AOI (x-axis) for the comparative uncoated optical component, and FIG. 11 plots the percentage of internal reflectance (y-axis) as a function of the TIR AOI (x-axis) for the coated optical component of Example 1. In Figures 10 and 11, the TIR AOI refers to the acute angle between the ArF laser beam path through the optic and a line perpendicular to the plane of the TIR surface. The TIR AOI is relative to the TIR surface, not the first surface where the laser beam first enters the optic. If the TIR AOI from the CaF2 side is greater than the critical angle, which is 41.7 degrees for CaF2, total internal reflection occurs at the TIR surface. A comparison of Figures 10 and 11 shows that the ALD coating of Example 1, which includes a first ALD coating layer of MgF2 and a second ALD coating layer of silica, does not change the internal reflectance of the TIR surface of the coated optic compared to a comparative uncoated optic having the same geometry.

[0123] Example 2 In Example 2, an optical component was prepared by coating a first ALD coating layer and a second ALD coating layer on the first ALD coating layer. The optical component used in Example 2 was a CaF2 prism having the shape of prism 200 shown in Figures 3A-3C, which had an entrance surface 202 and an exit surface 204 at Brewster's angle, a first TIR surface 206 at an incidence angle of 56.1°, and a second TIR surface 208 at an incidence angle of 45°. The longest dimension of the CaF2 prism in Example 2 was less than 20 mm. The first ALD coating layer was a MgF2 ALD coating having a thickness of 4 nm. The MgF2 ALD coating was formed according to the method and conditions described in Example 1.

[0124] The second ALD coating layer was an alumina (Al2O3) ALD coating applied to the outer coating surface of the first ALD coating layer. The second ALD coating layer had a thickness of 6 nm. The second ALD coating layer constituting the alumina ALD coating was applied in an ALD chamber maintained at a reactor temperature of 150° C. The alumina precursor was trimethylaluminum (TMA). The bubbler temperature was set to room temperature. The optical component was first exposed to an alumina precursor pulse having a duration of 40 ms and including an alumina precursor. The alumina precursor pulse was followed by a 10 second inert gas purge. After the alumina precursor pulse and purge, the optical component was subjected to a water pulse including water. The water pulse had a duration of 40 ms and was followed by a 7 second inert gas purge. The series of alumina precursor and water pulses was repeated until the alumina ALD coating layer had a thickness of 6 nm. A comparative uncoated optical component having the same shape and dimensions as shown in FIG. 3A was used as a comparative example.

[0125] A laser beam having a wavelength of 213 nm was redirected using the CaF2 prism of Example 2. Each of the comparative uncoated optic and the coated optic of Example 2 was irradiated with an ArF laser beam having a wavelength of 213 nm, and the transmission and internal reflectance of the P-polarized light of the ArF laser beam were measured as a function of the angle of incidence (AOI) according to the method disclosed herein. Referring to FIG. 12, the percentage transmission of the comparative uncoated optic is shown as a solid line, and the percentage transmission of the coated optic of Example 2 is shown as a dashed line. As shown in FIG. 12, the percentage transmission of the coated optic of Example 2 corresponds closely to the percentage transmission of the comparative uncoated optic. This demonstrates that the ALD coating of Example 2, which includes a first ALD coating layer of MgF2 and a second ALD coating layer of alumina, does not substantially change the transmission of a 213 nm beam through a first surface (e.g., beam entrance / exit surface) compared to the comparative uncoated optic having the same shape.

[0126] Referring now to Figure 13, the percentage internal reflectance of a 213 nm beam for the TIR surface 206 of the comparative uncoated optic is shown as a solid line, and the percentage internal reflectance of a 213 nm beam for the TIR surface 206 of the coated optic of Example 2 is shown as a dashed line. As shown in Figure 13, the percentage internal reflectance of the coated optic of Example 2 corresponds closely to the percentage internal reflectance of the comparative uncoated optic. This demonstrates that the ALD coating of Example 2, which includes a first ALD coating layer of MgF2 and a second ALD coating layer of alumina, does not substantially alter the internal reflectance of a 213 nm beam through the TIR surface (e.g., beam entrance / exit surfaces) of the coated optic compared to the TIR surface of the comparative uncoated optic having the same geometry.

[0127] Example 3 In Example 3, an optical component was prepared by coating with a first ALD coating layer and a second ALD coating layer on the first ALD coating layer. The optical component used in Example 3 was a CaF2 prism having the shape of a right-angle prism 400 shown in FIG. 4, which had an entrance surface 402, an exit surface 404, and one TIR surface 406 (hypothetic side). The height of the right-angle prism in Example 3 was less than 10 mm. An ALD-based protective anti-reflective (AR) coating was applied to all three surfaces 402, 404, and 406. The ALD coating comprised a 4 nm thick MgF2 ALD coating deposited directly on the CaF2 prism, followed by four additional coating layers. The four additional coating layers were an Al2O3 ALD coating layer having a thickness of 19 nm, a SiO2 ALD coating layer having a thickness of 52 nm, an Al2O3 ALD coating layer having a thickness of 41 nm, and a SiO2 ALD coating layer having a thickness of 45 nm. The MgF2 ALD coating layer and the SiO2 ALD coating layer were applied according to the method and conditions described in Example 1. The Al2O3 ALD coating layer was applied according to the method in Example 2. The prism was used to direct a laser beam having a wavelength of 266 nm into the objective lens of the inspection system. A comparative uncoated optical part having the same shape and dimensions as shown in FIG. 4 was used as a comparative example.

[0128] Each of the comparative uncoated optic and the coated optic of Example 3 was irradiated with an ArF laser beam having a wavelength of 266 nm, and the internal reflectance of the P-polarized light of the ArF laser beam was measured as a function of the angle of incidence (AOI) at the TIR surface 406 according to the methods disclosed herein. Referring now to FIG. 14, the percentage of internal reflectance of the comparative uncoated optic is shown in solid line, and the percentage of internal reflectance of the coated optic of Example 3 is shown in dashed line. As shown in FIG. 14, the percentage of internal reflectance of the coated optic of Example 3 corresponds closely to that of the comparative uncoated optic, as shown by the overlap of the dashed and solid lines in FIG. 14. This demonstrates that the ALD coating of Example 3, which includes a first ALD coating layer of MgF2 and a second oxide ALD coating layer (alternating alumina and silica), does not substantially alter the internal reflectance of a 266 nm beam by the TIR surface.

[0129] The ALD coating of Example 3 has been shown to not reduce reflection losses at the input surface 402 and output surface 404 as compared to a comparative uncoated optic having the same dimensions. Referring now to FIG. 15, a graph is shown of the % reflectance of input surface 402 as a function of wavelength of light incident on input surface 402. In FIG. 15, reference numeral 1502 refers to the reflectance of the comparative uncoated optic and reference numeral 1504 refers to the reflectance of the ALD coated optic of Example 3. As shown in FIG. 15, for input surface 402, the ALD protective AR coating of Example 3 (reference numeral 1504) reduces the surface reflectance to less than 0.2% as compared to a surface reflectance of 3.5% for the comparative uncoated optic (reference numeral 1502).

[0130] Example 4 - SF as fluorine source 6 MgF applied using / Ar plasma 2 ALD Coating In Example 4, a CaF2 optical component was coated with a MgF2 ALD coating using SF6 / Ar plasma as the fluorine source. The optical component in Example 4 was a right angle prism similar to that in FIG. 4 with dimensions between 10 mm and 30 mm. The ALD process in Example 4 included exposing the CaF2 optical component to alternating pulses of magnesium precursor and SF6 / Ar plasma. In Example 4, the optical component was not subjected to an oxygen source pulse between the magnesium precursor pulse and the fluorine source pulse. The ALD process was carried out while the ALD chamber was maintained at a temperature of 150° C. The magnesium precursor was (EtCp)2Mg (i.e., bis(ethylcyclopentadienyl)magnesium). The magnesium precursor was heated to 95° C. and the optical component was exposed to the magnesium precursor for 1 second during each pulse of magnesium precursor to saturate the surface. After the magnesium precursor pulse, the ALD chamber was purged with inert gas (Ar, N2) to remove any remaining magnesium precursor. The optics were then exposed to a SF6 / Ar plasma fluorine pulse. The power of the current used to generate the SF6 / Ar plasma was 200 W and the Ar to SF6 flow ratio was 2:1, where the flow rates were volumetric flows in sccm. The duration of the SF6 / Ar plasma fluorine pulse was 7 seconds.

[0131] Example 5-H 2 SF as a fluorine source, including an O pulse 6 MgF applied using / Ar plasma 2 ALD Coating For Example 5, a CaF2 optical component was coated with a MgF2 ALD coating using SF6 / Ar plasma as the fluorine source and an oxygen source pulse between the magnesium precursor pulse and the fluorine source pulse. The CaF2 optical component of Example 5 was the same as the CaF2 optical component described in Example 4. The ALD process of Example 5 included exposing the CaF2 optical component to a pulse containing a magnesium precursor, a second pulse containing an oxygen source, and a third pulse containing an SF6 / Ar plasma. Thus, in Example 5, the magnesium precursor is first converted to magnesium oxide with an oxygen source, and then the magnesium oxide is converted to MgF2 by SF6 / Ar plasma (fluorine source). The magnesium precursor pulse and the fluorine source pulse were the same as those previously described in Example 4. For the oxygen source pulse, water (H2O) was used as the oxygen source. After exposure to the magnesium precursor, the optical component was exposed to an oxygen source pulse having a duration of 0.3 seconds. The optical component was then exposed to the oxygen source followed by the fluorine source. The ALD chamber was maintained at a temperature of 150° C. throughout the ALD process and purged with an inert gas between each pulse.

[0132] Example 6 - MgF of Examples 4 and 5 2 XPS analysis of ALD coatings In Example 6, the MgF2 ALD coatings of Examples 4 and 5 were analyzed by X-ray photoelectron spectroscopy (XPS) to elucidate the relative concentrations of different chemical elements at the surface of the MgF2 ALD coating. To accurately quantify the surface concentrations of various elements in the MgF2 ALD coating using X-ray photoelectron spectroscopy (XPS), relative sensitivity factors calculated from standard reference materials were utilized. The analysis volume for XPS measurements of ALD coatings is the product of the analysis area (XPS spot size or aperture size at the surface of the ALD coating) and the depth of the ALD coating investigated. Photoelectrons are generated within the X-ray penetration depth of the ALD coating (typically a few micrometers), but only photoelectrons with enough kinetic energy to escape from the surface of the ALD coating (approximately three times the photoelectron escape depth) are detected. The photoelectron escape depth is on the order of 15-35 Å, which results in an analysis depth of approximately 50-100 Å. Typically, 95% of the signal originates from within this depth. An electron energy analyzer and detector were used to collect and measure the kinetic energy of photoelectrons emitted from the surface of the ALD coating. The specific kinetic energy of each emitted photoelectron is characteristic of the element and the core electron level originating from that particular bonding configuration of the element. The number of emitted photoelectrons is counted (signal intensity) and plotted as a function of kinetic energy to produce a photoelectron spectrum. Peaks in the spectrum are characteristic of the core electron levels of individual elements. To quantify the atomic percentage of each element in the analyzed volume of the ALD coating, the area under each peak is integrated and then divided by an appropriate relative sensitivity factor (calculated from a standard reference material). When analyzing data from an ALD coating with XPS, there are many XPS lines associated with each element, one for each core electron level in each particular bonding configuration of the element. The atomic percentages of elements in the MgF2 ALD coating are given in Table 1. For elements in low concentrations, the XPS line with the highest signal-to-noise ratio should be used. The surface of the ALD coating may be cleaned with UV / ozone, alcohol, or other non-aqueous means. Photoelectron spectra in various energy ranges for the MgF2 coatings of Examples 4 and 5 are provided in Figures 16, 17, and 18.The photoelectron spectra in Figures 16, 17, and 18 are reported in terms of binding energy, where binding energy is equal to hv-KE, where hv is the photon energy, and the term KE is the measured kinetic energy of the emitted electron.

[0133] Referring to Figure 16, photoelectron spectra in the energy range representative of the fluorine 1s core level are graphically shown for the MgF2ALD coating of Example 4 (reference number 1602) and the MgF2ALD coating of Example 5 (reference number 1604). As shown in Figure 16, the photoelectron spectrum for the MgF2ALD coating of Example 4 (reference number 1602) has a major peak (reference number 1610) at about 688 eV and a minor peak (reference number 1611) at about 685 eV. The major peak 1610 represents a significant bond between fluorine and an organic component, such as a carbon or fragment of a ligand, and the minor peak 1611 represents fluorine bonding to an inorganic species, such as magnesium. In contrast, the photoelectron spectrum for the MgF2ALD coating of Example 5 (reference number 1604) shows a single peak at around 685 eV (reference number 1612), indicating that substantially all of the fluorine is bonded to inorganic components such as magnesium, with very few fluorine-carbon bonds present.

[0134] 17, photoelectron spectra in the energy range representative of the carbon 1s core electron level are graphically shown for the MgF2ALD coating of Example 4 (reference number 1602) and the MgF2ALD coating of Example 5 (reference number 1604). As shown in FIG. 17, the photoelectron spectrum for the MgF2ALD coating of Example 4 (reference number 1602) has a major peak (reference number 1710) at about 291 eV and a minor peak (reference number 1711) at about 289 eV. The major peak 1710 represents the significant bonding of carbon to two fluorine atoms (CF2) and the minor peak 1711 represents a carbon atom bonded to fluorine and hydrogen (CF y H z) In contrast, the photoelectron spectrum for the MgF2ALD coating of Example 5 (reference number 1604) shows a single peak (reference number 1712) at around 285 eV, indicating that substantially all of the carbon is in the form of carbon-carbon bonds and that there are very few bonds between carbon and fluorine. Thus, Figures 16 and 17 show that (1) the MgF2ALD coating of Example 5, prepared by including an oxygen source pulse between the magnesium precursor pulse and the fluorine source pulse, has fewer fluorine-carbon bonds compared to the MgF2ALD coating of Example 4, which does not have an oxygen source pulse, (2) substantially all of the fluorine in the MgF2ALD coating of Example 5 is bonded to Mg, and (3) the carbon detected in the MgF2ALD coating of Example 5 is not incorporated within the MgF2ALD coating, but rather forms isolated regions on the surface.

[0135] Referring now to FIG. 18, photoelectron spectra in the energy range representative of magnesium 2p core electron levels are graphically shown for the MgF2 ALD coating of Example 4 and the MgF2 ALD coating of Example 5. Peak 1802 in FIG. 18 represents a magnesium bond with a higher bond energy, indicative of magnesium bonding to fluorine. Peak 1804 in FIG. 18 represents a magnesium bond with a lower bond energy, corresponding to magnesium-oxygen and / or magnesium-carbon bonds. The Mg2p data shows asymmetric peaks strongly suggestive of two different Mg species. The lower bond energy (shifted to the right) with asymmetric peaks indicates MgF2, with oxygen and carbon included in the film.

[0136] Photoelectron spectroscopy was used to determine the atomic percentages of each of magnesium, fluorine, carbon, and oxygen in the analyzed volumes of the MgF2ALD coatings of Examples 4 and 5. The atomic percentages are given in Table 1. As shown in Table 1, the MgF2ALD coating of Example 5 had a smaller percentage of carbon and a larger percentage of magnesium compared to the MgF2ALD coating of Example 4. Therefore, when an SF6-based fluorine source is used, the concentration of carbon in the MgF2ALD coating can be reduced, as in Example 5, by incorporating an oxygen source pulse between the magnesium precursor and fluorine source pulses.

[0137] [Table 1]

[0138] Comparative Example 7-PVD MgF 2 Optical components with coatings In Comparative Example 7, a comparative coated optical component was prepared by coating a crystalline CaF2 optical component with MgF2 using physical vapor deposition (PVD). In the PVD process, MgF2 was thermally evaporated from a resistive source in a vacuum chamber to provide an evaporated MgF2 flux. The evaporated MgF2 flux was then directed to the optical component in a line-of-sight manner. As a result, the PVD process of Comparative Example 7 was able to coat only one surface of a multi-surface optical component at a time.

[0139] Example 8 - MgF prepared with different fluorine sources 2 ALD Coating In Example 8, coated optical components were prepared with MgF2 ALD coatings prepared using different fluorine sources. The optical components of Example 8 had the same composition and geometry as the optical components used in Comparative Example 7. For Sample 8A, the MgF2 ALD coating was prepared using HF as the fluorine source. The MgF2 ALD coating of Sample 8A was applied using the magnesium precursor and ALD process described in Example 4, except that HF ​​was used as the fluorine source instead of SF6 / Ar plasma. The reactor temperature of the ALD chamber was 150°C. The magnesium precursor pulse was performed according to the method and operating conditions described in Example 4. The HF pulse had a pulse duration of 1 second, followed by purging with an inert gas.

[0140] For Sample 8B, an MgF2 ALD coating was prepared using an organofluorine compound as the fluorine source. The MgF2 ALD coating of Sample 8B was applied using the magnesium precursor and ALD process described in Example 4, except that an organofluorine compound was used instead of SF6 / Ar plasma as the fluorine source. The organofluorine compound for preparing Sample 8B was hexafluoroacetylacetone.

[0141] For Sample 8C, the MgF2 ALD coating was applied using a SF6 / Ar plasma as the fluorine source and including an oxygen source pulse between the magnesium precursor and fluorine source pulses. The MgF2 ALD coating for Sample 8C was applied using the materials and ALD process described in Example 5.

[0142] Referring now to FIG. 19, the refractive index of each of the coated optics of Example 8 and Comparative Example 7 as a function of wavelength, measured using a refractometer according to known methods, is shown in a graph. In FIG. 19, reference number 1902 corresponds to Comparative Example 7, reference number 1904 corresponds to the refractive index curve of Sample 8A prepared using HF, reference number 1906 corresponds to the refractive index curve of Sample 8B prepared using an organic fluorine source, and reference number 1908 corresponds to the refractive index curve of Sample 8C using SF6 / Ar plasma. As shown in FIG. 19, the coated optic of Sample 8C (1908), prepared using SF6 / Ar plasma with the addition of oxygen source pulses, exhibited a lower refractive index value compared to the coated optics of Sample 8A (1904) and Sample 8B (1906). The refractive index value of the coated optic of Sample 8C was comparable to that of the coated optic of Comparative Example 7. This demonstrates that preparing coated optics having ALD coatings prepared by an ALD process using an SF6-based fluorine source with an intermediate oxygen source pulse step can produce coated optics with refractive indices comparable to existing PVD-coated optics.

[0143] Referring now to Figures 20 and 21, the relative amounts of carbon, magnesium, oxygen, and fluorine are provided as a function of depth in the coating for the coated optics of Comparative Example 7 (Figure 20) and Sample 8C of Example 8 (Figure 21). The data in Figures 20 and 21 were generated by Secondary Ion Mass Spectroscopy (SIMS) using a secondary ion mass spectrometer. Cesium ions (Cs) with a kinetic energy of 2 kV were applied to the surface of the coating. + ) was sputtered and Bi was applied at 30 kV. 3+SIMS analysis was performed by performing the analysis in positive mode with ions. In Figures 20 and 21, the reference line 2002 represents the interface between the substrate and the coating, with the coating being shown in the data to the left of the reference line 2002. As shown in Figure 21, the ALD coated optical component of Sample 8C exhibited a similar oxygen concentration comparable to the PVD coated optical component of Comparative Example 7 (Figure 20). However, Figure 21 also shows that the ALD coated optical component of Sample 8C had a lower concentration of carbon impurities compared to the PVD coated optical component of Comparative Example 7.

[0144] It will be apparent to those skilled in the art that various modifications and variations can be made to the embodiments described herein without departing from the spirit and scope of the claimed subject matter. Thus, this specification is intended to cover modifications and variations of the various embodiments described herein, provided such modifications and variations come within the scope of the appended claims and their equivalents.

[0145] Preferred embodiments of the present invention will be described below in detail.

[0146] EMBODIMENT 1 In coated optical components, An optical component comprising crystalline calcium fluoride, and an atomic layer deposition (ALD) coating in contact with a surface of the optical component, the ALD coating comprising a metal fluoride having a metal different from calcium; A coated optical component comprising:

[0147] EMBODIMENT 2 2. The coated optical component of embodiment 1, wherein the ALD coating comprises magnesium fluoride (MgF2).

[0148] EMBODIMENT 3 3. The coated optical component of any of the preceding claims, wherein the ALD coating has a thickness of 10 nanometers (nm) or less.

[0149] EMBODIMENT 4 The ALD coating comprises: a first ALD coating layer in direct contact with a surface of the optical component, the first ALD coating layer comprising the metal fluoride; and a second ALD coating layer in direct contact with the first ALD coating layer, the second ALD coating layer being made from a different material than the first ALD coating layer; 4. The coated optical component of any one of embodiments 1 to 3, comprising:

[0150] EMBODIMENT 5 5. The coated optical component of embodiment 4, wherein the first ALD coating layer is magnesium fluoride and the second ALD coating layer is silica (SiO2) or alumina (Al2O3), the first ALD coating layer has a thickness less than 10 nanometers (nm), and the second ALD coating layer has a thickness less than 10 nm.

[0151] EMBODIMENT 6 6. The coated optical component of embodiment 5, wherein the ALD coating has a sulfur content greater than zero.

[0152] EMBODIMENT 7 7. The coated optical component of any of the preceding embodiments, wherein the ALD coating is a conformal coating.

[0153] EMBODIMENT 8 8. The coated optical component of any of the preceding claims, wherein the ALD coating has a thickness that varies by no more than 5% from an average thickness of the ALD coating, the average thickness of the ALD coating being the thickness of the ALD coating averaged over the surface in contact with the ALD coating.

[0154] EMBODIMENT 9 9. The coated optical component of any of the previous claims, wherein the ALD coating comprises 1000 ppm or less of carbon based on the total weight of the ALD coating.

[0155] EMBODIMENT 10 10. The coated optical component of any of the previous embodiments, wherein the optical component is a prism, a lens, a beam splitter, or a window.

[0156] EMBODIMENT 11 The optical component has a steepness ratio R of 0.5 to 0.85. c / #, and the steepness ratio R c / # is the radius of curvature of the steepest surface (R) divided by the diameter (#) of the aperture of the optical component. c 11. The coated optical component of any one of the preceding claims, wherein the optical component is equal to

[0157] EMBODIMENT 12 1. A method of coating an optical component, comprising depositing an atomic layer deposition (ALD) coating on a surface of the optical component; the optical component comprises crystalline calcium fluoride (CaF2); The method, wherein the ALD coating comprises a semi-metal oxide, a metal oxide, a metal fluoride having a metal different from calcium, or a combination thereof.

[0158] EMBODIMENT 13 13. The method of embodiment 12, wherein the ALD coating comprises the metal fluoride, and depositing the ALD coating comprises exposing a surface of the optical component to alternating pulses of a metal precursor and a fluorine source comprising sulfur hexafluoride (SF6).

[0159] EMBODIMENT 14 14. The method of embodiment 13, wherein the fluorine source comprises a plasma formed from sulfur hexafluoride.

[0160] EMBODIMENT 15 14. The method of embodiment 13, wherein the metal precursor comprises a metal-ligand complex comprising magnesium.

[0161] EMBODIMENT 16 exposing a surface of the optical component to alternating pulses of a metal precursor and a fluorine source; exposing the surface of the optical component to a pulse containing the metal precursor, which reacts with the calcium fluoride at the surface of the optical component to deposit a monolayer of metal coordinated to the surface of the optical component; terminating the pulse containing the metal precursor; exposing the surface of the optical component to a pulse containing the fluorine source, which reacts with the coordinated metal monolayer to form a metal fluoride; and terminating the pulse containing the fluorine source; 14. The method of embodiment 13, comprising:

[0162] EMBODIMENT 17 exposing the surface of the optical component to a pulse containing an oxygen source after the pulse containing the metal precursor is terminated and before exposing the surface to a pulse containing a fluorine source, the oxygen source comprising water, water plasma, oxygen, oxygen plasma, ozone, ozone plasma, hydrogen peroxide, hydrogen peroxide plasma, an oxygen-containing liquid, an oxygen-containing gas, or a combination thereof, which oxidizes the coordinated metal to form a metal oxide; and terminating the pulse containing the oxygen source; Further comprising: the fluorine source reduces the metal oxide to form the metal fluoride; 17. The method of embodiment 16, wherein the pulse containing the oxygen source removes carbon from the coordinated metal monolayer.

[0163] EMBODIMENT 18 the ALD coating comprises the metal oxide; depositing an ALD coating on a surface of the optical component comprises exposing the surface to alternating pulses of a metal precursor and an oxygen source; the oxygen source is selected from the group consisting of water, water plasma, ozone, ozone plasma, oxygen, oxygen plasma, hydrogen peroxide, hydrogen peroxide plasma, oxygen-containing gas, oxygen-containing liquid, and combinations thereof; 18. The method of any of embodiments 12 to 17, wherein the metal precursor comprises an aluminum precursor selected from the group consisting of trimethylaluminum (TMA), triethylaluminum (TEA), and combinations thereof.

[0164] EMBODIMENT 19 the ALD coating comprises the metalloid oxide; depositing an ALD coating on a surface of the optical component comprises exposing the surface of the optical component to alternating pulses of a metalloid precursor and an oxygen source; the oxygen source is selected from the group consisting of water, water plasma, ozone, ozone plasma, oxygen, oxygen plasma, hydrogen peroxide, hydrogen peroxide plasma, oxygen-containing gas, oxygen-containing liquid, and combinations thereof; 18. The method of any of claims 12 to 17, wherein the metalloid oxide is silica and the metalloid precursor is selected from the group consisting of bis(tert-butylamino)silane; di(sec-butylamino)silane; diisopropylaminotrisilylamine; a compound having the formula SiH2(NR R')2, where each of R and R' is independently a methyl group, an ethyl group, or both; and combinations thereof.

[0165] EMBODIMENT 20 depositing the ALD coating comprises: providing a first ALD coating layer on a surface of the optical component; and applying a second ALD coating layer over the first ALD coating layer, the second ALD coating layer being made of a different material than the first ALD coating layer; 20. The method of any one of embodiments 12 to 19, comprising: [Explanation of symbols]

[0166] 10, 101 Optical components 20 Tool fixture 22 Rotating table 24 Support Features 100, 200, 400 Coated Optics 102 Front page 104, 106, 406 TIR plane 108 Top surface 110 Laser Beam 120 ALD Coating 130 First ALD coating layer 132 Inner surface of first ALD coating layer 134 Outer surface of first ALD coating layer 140 Second ALD coating layer 142 Inner surface of second ALD coating layer 144 Outer surface of second ALD coating layer 202, 402 entrance plane 204, 404 Exit surface 206 First TIR Surface 208 Second TIR surface 410 Beam of Light 420 Inspection Equipment 500 Optical Inspection System 502 Objective Lens 504 Surfaces with Steep Curvature

Claims

1. In coated optical components, An optical component comprising crystalline calcium fluoride, and an atomic layer deposition (ALD) coating in contact with a surface of the optical component, the ALD coating comprising a metal fluoride having a metal different from calcium; A coated optical component comprising:

2. The ALD coating is magnesium fluoride (MgF 2 10. The coated optic of claim 1 , wherein the ALD coating has a thickness of 10 nanometers (nm) or less.

3. The ALD coating comprises: a first ALD coating layer in direct contact with a surface of the optical component, the first ALD coating layer comprising the metal fluoride; and a second ALD coating layer in direct contact with the first ALD coating layer, the second ALD coating layer being made of a different material than the first ALD coating layer; The coated optical component of claim 1 comprising:

4. The first ALD coating layer is magnesium fluoride and the second ALD coating layer is silica (SiO 2 ) or alumina (Al 2 O 3 4. The coated optical component of claim 3, wherein the first ALD coating layer has a thickness of less than 10 nanometers (nm) and the second ALD coating layer has a thickness of less than 10 nm.

5. The coated optical component of claim 4 , wherein the ALD coating has a sulfur content greater than zero ppm, a carbon content less than or equal to 1000 ppm, or both, based on a total weight of the ALD coating.

6. 6. The coated optical component of claim 1, wherein the ALD coating is a conformal coating having a thickness that varies no more than 5% from an average thickness of the ALD coating, the average thickness of the ALD coating being the thickness of the ALD coating averaged over the surface in contact with the ALD coating.

7. 1. A method of coating an optical component, comprising depositing an atomic layer deposition (ALD) coating on a surface of the optical component; The optical component is made of crystalline calcium fluoride (CaF 2 ), The method, wherein the ALD coating comprises a semi-metal oxide, a metal oxide, a metal fluoride having a metal different from calcium, or a combination thereof.

8. The ALD coating includes the metal fluoride, and the step of depositing the ALD coating includes treating the surface of the optical component with a metal precursor and sulfur hexafluoride (SF 6 8. The method of claim 7, further comprising exposing the fluorine source to alternating pulses of a fluorine source comprising:

9. exposing a surface of the optical component to alternating pulses of a metal precursor and a fluorine source; exposing the surface of the optical component to a pulse containing the metal precursor, which reacts with the calcium fluoride at the surface of the optical component to deposit a monolayer of metal coordinated to the surface of the optical component; terminating the pulse containing the metal precursor; exposing the surface of the optical component to a pulse containing the fluorine source, which reacts with the coordinated metal monolayer to form a metal fluoride; and terminating the pulse containing the fluorine source; The method of claim 8 , comprising:

10. exposing the surface of the optical component to a pulse containing an oxygen source after the pulse containing the metal precursor is terminated and before exposing the surface to a pulse containing a fluorine source, the oxygen source comprising water, water plasma, oxygen, oxygen plasma, ozone, ozone plasma, hydrogen peroxide, hydrogen peroxide plasma, an oxygen-containing liquid, an oxygen-containing gas, or a combination thereof, which oxidizes the coordinated metal to form a metal oxide; and terminating the pulse containing the oxygen source; Further comprising: the fluorine source reduces the metal oxide to form the metal fluoride; The method of claim 9 , wherein the pulse containing the oxygen source removes carbon from the monolayer of the coordinated metal.

Citation Information

Patent Citations

  • Production of fluoride thin coating

    JP1998008252A

  • Optical element

    JP2014531061A

  • Optical layer, optical member, and optical device

    JP2021162717A

  • Methods for coating a substrate with magnesium fluoride via atomic layer deposition

    US20210032744A1