Low modulus ion-exchangeable glasses with enhanced thermal properties for fabrication - Patents.com

Ion-exchangeable glass compositions with high compressive stress to Young's modulus ratios provide enhanced mechanical properties, ensuring durability and flexibility for cover glasses in consumer electronics, addressing the need for damage resistance in flexible displays.

JP2024538127APending Publication Date: 2024-10-18CORNING INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024522492
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-14
Filing Date
2022-09-21
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

There is a need for ion-exchangeable glass compositions with desirable mechanical properties, particularly for cover glass applications in consumer electronics, that can withstand bending without breaking and maintain touch functionality.

Method used

The development of ion-exchangeable glass compositions with a high ratio of peak compressive stress to Young's modulus, combined with suitable thermal properties, to enhance strength and flexibility, preventing breakage during use.

Benefits of technology

The glass compositions exhibit high compressive stress values and low modulus, allowing for flexible and durable cover glasses that can withstand bending stresses, reducing the risk of breakage and maintaining functionality in electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024538127000001_ABST
    Figure 2024538127000001_ABST
Patent Text Reader

Abstract

An ion-exchanged alkali aluminosilicate glass article having a peak compressive stress to Young's modulus ratio of 15 or greater. The glass article may have the following condition: Al2O3 mol% + RO mol% ≥ 17 mol%, where RO mol% = MgO mol% + CaO mol%; and be substantially free of ZnO, SrO, BaO, BO, PO, Li2O, and KO. The glass article may have a peak compressive stress ranging from 500 MPa to 1300 MPa. The glass article is suitable for a variety of high-strength applications, including cover glass applications that experience high bending stresses during use, such as cover glass for flexible displays.
Need to check novelty before this filing date? Find Prior Art

Description

CROSS-REFERENCE TO RELATED APPLICATIONS

[0001] This application claims the benefit of priority under 35 U.S.C. § 119 to U.S. Provisional Patent Application No. 63 / 255,625, filed October 14, 2021, the contents of which are relied upon and incorporated by reference herein in their entirety. [Technical field]

[0002] The present disclosure relates to ion-exchangeable glass compositions. In particular, embodiments described herein relate to ion-exchangeable glass compositions for use in various industries, such as consumer electronics, transportation, construction, defense, pharmaceuticals, and packaging. Additionally, the present disclosure relates to glass compositions for cover glass applications, such as cover glass for flexible displays. [Background technology]

[0003] Many consumer products, such as smartphones, tablets, portable media players, personal computers, and cameras, incorporate a cover glass that can act as a cover for a display and may incorporate touch functionality. These devices are often dropped by users onto hard surfaces, which can shatter the cover glass and adversely affect the use of the device, for example compromising the touch functionality.

[0004] Foldable or flexible displays for consumer electronics applications can benefit from thin, flexible ion-exchanged glass. Glass can be made resistant to bending failure through the ion-exchange process, which involves the creation of compressive stresses at the glass surface. The compressive stresses introduced using the ion-exchange process specifically serve to stop scratches that could otherwise cause glass breakage. Summary of the Invention [Problem to be solved by the invention]

[0005] Thus, there is a continuing need for ion-exchangeable glass compositions that have desirable mechanical properties for use in a variety of applications, including cover glass applications. [Means for solving the problem]

[0006] The present disclosure relates to ion-exchangeable glass compositions having strength and flexibility suitable for various applications, such as electronic device cover glass. The glass compositions are designed to maximize the ratio of peak compressive stress value to Young's modulus value. A high ratio, such as 15 or more, allows the glass composition to avoid breakage when bent. In addition, the strength imparted to the glass composition by the ion exchange process also provides the glass composition with desirable mechanical properties to prevent fracture during use. The glass compositions may also exhibit desirable thermal properties (e.g., liquidus temperature and / or liquidus viscosity) to optimize some manufacturing techniques used to form the composition into glass articles. In addition, the glass compositions may also prevent the ion exchange rate from becoming undesirably too fast, thereby aiding in the control of ion exchange within the glass composition during some ion exchange processes.

[0007] A first aspect (1) of the present application relates to an ion-exchanged alkali aluminosilicate glass article, the glass article comprising: at least 55 mol% SiO; at least 12.5 mol% and no more than 16.0 mol% AlO; at least 1 mol% and no more than 3.88 mol% MgO; at least 0.78 mol% and no more than 3 mol% CaO; and NaO; where mol% AlO+mol% RO≧17 mol%, and mol% RO=mol% MgO+mol% CaO; and the glass article is substantially free of ZnO, SrO, BaO, BO, PO, LiO, and KO.

[0008] In a second aspect (2), the alkali aluminosilicate glass article according to the first aspect (1) comprises a Young's modulus value measured in GPa before being ion-exchanged, and a compressive stress layer extending from the surface of the glass article to a compression depth and having a peak compressive stress value measured in MPa, wherein the ratio of the peak compressive stress value to the Young's modulus value is 15 or greater.

[0009] In the third embodiment (3), the ratio of the peak compressive stress value to the Young's modulus value according to the second embodiment (2) is from 15 or more to 18 or less.

[0010] In the fourth embodiment (4), the Young's modulus value according to the second embodiment (2) or the third embodiment (3) is in the range of 70 MPa or more and 80 MPa or less.

[0011] In a fifth aspect (5), the peak compressive stress value according to any one of aspects (2) to (4) ranges from 500 MPa or more to 1300 MPa or less.

[0012] In a sixth embodiment (6), the compression depth according to any one of embodiments (2) to (5) ranges from 5 micrometers to 30 micrometers.

[0013] In a seventh embodiment (7), the compression depth according to any one of embodiments (2) to (6) ranges from 5% to 20% of the thickness of the glass article.

[0014] In an eighth aspect (8), there is provided an alkali aluminosilicate glass article according to any one of aspects (1) to (7), wherein the mol% NaO+mol% RO≧20 mol%.

[0015] In a ninth aspect (9), there is provided an alkali aluminosilicate glass article according to any one of aspects (1) to (8), wherein (mol % Na2O+mol % RO-mol % Al2O3>=4 mol %.

[0016] In a tenth aspect (10), there is provided an alkali aluminosilicate glass article according to any one of aspects (1) to (8), wherein 11 mol% > (mol % NaO + mol % RO - mol % AlO) > 4 mol%.

[0017] In an eleventh aspect (11), there is provided an alkali aluminosilicate glass article according to any one of aspects (1) to (10), wherein 21 mol%≧mol% Al2O3+mol% RO≧17 mol%.

[0018] In a twelfth aspect (12), there is provided an alkali aluminosilicate glass article according to any one of aspects (1) to (11), wherein 37 mol%≧mol% Al2O3+mol% Na2O≧28 mol%.

[0019] In a thirteenth aspect (13), there is provided an alkali aluminosilicate glass article according to any one of aspects (1) to (12), wherein (mol% MgO / (mol% MgO+mol% CaO)≧0.5.

[0020] In a fourteenth aspect (14), there is provided an alkali aluminosilicate glass article according to any one of aspects (1) to (12), wherein 0.8 > (mol% MgO / (mol% MgO+mol% CaO) > 0.5.

[0021] In a fifteenth embodiment (15), the alkali aluminosilicate glass article according to any one of embodiments (1) to (14) comprises, greater than or equal to 1.92 mol % and less than or equal to 3.88 mol % MgO.

[0022] In a sixteenth embodiment (16), the alkali aluminosilicate glass article according to any one of embodiments (1) to (15) comprises, greater than or equal to 0.78 mol % and less than or equal to 2.52 mol % CaO.

[0023] In a seventeenth embodiment (17), the alkali aluminosilicate glass article according to any one of embodiments (1) to (16) comprises greater than or equal to 59 mol% and less than or equal to 66 mol% SiO2 and greater than or equal to 16 mol% and less than or equal to 21 mol% Na2O.

[0024] In an eighteenth embodiment (18), the alkali aluminosilicate glass article according to any one of embodiments (1) to (14) includes from about 64 mol% to about 66 mol% SiO, from about 13 mol% to about 15 mol% AlO, from about 2 mol% to about 3.88 mol% MgO, from about 0.78 mol% to about 2 mol% CaO, and from about 15.5 mol% to about 17.5 mol% NaO.

[0025] In a nineteenth embodiment (19), the alkali aluminosilicate glass article according to any one of embodiments (1) to (14) includes from about 59.6 mol% to about 65.5 mol% SiO, from about 12.78 mol% to about 15.96 mol% AlO, from about 1.92 mol% to about 3.88 mol% MgO, from about 0.78 mol% to about 2.52 mol% CaO, and from about 16.09 mol% to about 20.2 mol% NaO.

[0026] In a twentieth embodiment (20), the alkali aluminosilicate glass article according to any one of embodiments (1) to (19) has a thickness of less than or equal to 4 millimeters.

[0027] In a twenty-first embodiment (21), the alkali aluminosilicate glass article according to any one of embodiments (1) to (19) has a thickness in the range of 15 micrometers or more and 300 micrometers or less.

[0028] In a twenty-second embodiment (22), the alkali aluminosilicate glass article according to any one of embodiments (1) to (21) has a liquidus viscosity in the range of 500 kP or more and 2300 kP or less, measured before being ion-exchanged.

[0029] In a twenty-third embodiment (23), the alkali aluminosilicate glass article according to any one of embodiments (1) or (8) through (22) comprises a compressive stress layer extending from the surface of the glass article to a compression depth and having a peak compressive stress value in the range of from 500 MPa or more to 1300 MPa or less.

[0030] A twenty-fourth aspect (24) of the present application relates to an ion-exchanged alkali aluminosilicate glass article, comprising an electronic display and a glass article according to any one of aspects (1) to (23) disposed over the electronic display.

[0031] In a twenty-fifth embodiment (25), the electronic device according to the twenty-fourth embodiment (24) further includes a housing having a front, a rear, and a side, and electrical components at least partially within the housing, including a controller, memory, and an electronic display at or adjacent to the front of the housing, and the glass article forms at least a portion of the housing.

[0032] A twenty-sixth aspect (26) of the present application relates to an ion-exchanged alkali aluminosilicate glass article comprising: 59 mol% to 66 mol% SiO; 12.5 mol% to 16.0 mol% AlO; 1 mol% to 3.88 mol% MgO; 0.78 mol% to 3 mol% CaO; and 16 mol% to 21 mol% NaO; a Young's modulus value measured in GPa prior to ion exchanging the glass article; and a compressive stress layer extending from a surface of the ion-exchanged glass article and having a peak compressive stress value measured in MPa, wherein mol% AlO+mol% RO≧17 mol%, mol% RO=mol% MgO+mol% CaO; and is substantially free of ZnO, SrO, BaO, BO, PO, LiO, and KO; and a ratio of the peak compressive stress value to the Young's modulus value is 15 to 18.

[0033] A twenty-seventh aspect (27) of the present application relates to an ion-exchanged alkali aluminosilicate glass article comprising: at least 55 mol% SiO; at least 12.5 mol% and no more than 16 mol% AlO; at least 1 mol% and no more than 4 mol% MgO; at least 0.5 mol% and no more than 3 mol% CaO; and NaO; where mol% AlO+mol% RO≧17 mol%, and mol% RO=mol% MgO+mol% CaO; and the glass article is substantially free of ZnO, SrO, BaO, BO, PO, LiO, and KO.

[0034] In a twenty-eighth embodiment (28), the ion exchanged alkali aluminosilicate glass article according to the twenty-seventh embodiment (27) comprises a Young's modulus value measured in GPa before being ion exchanged, and a compressive stress layer extending from the surface of the glass article to a compression depth and having a peak compressive stress value measured in MPa, wherein the ratio of the peak compressive stress value to the Young's modulus value is 15 or greater.

[0035] A twenty-ninth aspect (29) of the present application relates to a method of strengthening an alkali aluminosilicate glass article, the method comprising immersing an alkali aluminosilicate glass article in an ion exchange solution comprising at least 50% by weight of a potassium salt, the glass article comprising at least 55 mol% SiO, at least 12.5 mol% to at most 16.0 mol% Al2O3, at least 1 mol% to at most 3.88 mol% MgO, at least 0.78 mol% to at most 3 mol% CaO, and at most 3 mol% Na2O, where mol% Al2O3+mol% RO≧17 mol%, and mol% RO=mol% MgO+mol% CaO, and the glass article is substantially free of ZnO, SrO, BaO, BO, PO, Li2O, and KO. The method includes ion exchanging the glass article with an ion exchange solution for a time ranging from 5 minutes to 24 hours at a temperature ranging from 350° C. to 480° C. to extend from the surface of the glass article to a compression depth to achieve a compressive stress layer comprising a peak compressive stress value ranging from 500 MPa to 1300 MPa.

[0036] In a thirtieth aspect (30), the method of strengthening an alkali aluminosilicate glass article according to the twenty-ninth aspect (29) comprises a Young's modulus value measured in GPa before being ion-exchanged, and a ratio of a peak compressive stress value to a Young's modulus value of 15 or greater.

[0037] In a thirty-first aspect (31), the method of strengthening an alkali aluminosilicate glass article according to the twenty-ninth aspect (29) comprises a Young's modulus value measured in GPa before being ion-exchanged, and a ratio of a peak compressive stress value to a Young's modulus value of from 15 to 18 inclusive.

[0038] In a thirty-second embodiment (32), the Young's modulus value according to the thirtieth embodiment (30) or the thirty-first embodiment (31) is in the range of 70 MPa or more and 80 MPa or less.

[0039] In a thirty-third embodiment (33), the compression depth according to any one of embodiments (29) to (32) ranges from 5 micrometers or more to 30 micrometers or less.

[0040] In a thirty-fourth embodiment (34), the compression depth according to any one of embodiments (29) to (33) ranges from 5% to 20% of the thickness of the glass article.

[0041] In a thirty-fifth embodiment (35), there is provided a method according to any one of embodiments (29) to (34), wherein the glass article comprises the condition: Na2O mol% + RO mol% > 20 mol%.

[0042] In a thirty-sixth aspect (36), there is provided a method according to any one of aspects (29) to (35), wherein the glass article comprises the condition: (mol % Na2O+mol % RO-mol % Al2O3>4 mol %.

[0043] In a thirty-seventh aspect (37), there is provided a method according to any one of aspects (29) to (35), wherein the glass article comprises the condition: 11 mol% > (mol% NaO + mol% RO - mol% AlO) > 4 mol%.

[0044] In a thirty-eighth embodiment (38), there is provided a method according to any one of embodiments (29) to (37), wherein the glass article comprises the condition: 21 mol%≧mol% Al2O3+mol% RO≧17 mol%.

[0045] In a thirty-ninth aspect (39), there is provided a method according to any one of aspects (29) to (38), wherein the glass article comprises the condition: 37 mol% > Al2O3 mol% + Na2O mol% > 28 mol%.

[0046] In a fortieth embodiment (40), there is provided a method according to any one of embodiments (29) to (39), wherein (mol% MgO / (mol% MgO+mol% CaO)≧0.5.

[0047] In a forty-first aspect (41), there is provided a method according to any one of aspects (29) to (39), wherein the glass article comprises the condition: 0.8≧(mol% MgO / (mol% MgO+mol% CaO)≧0.5.

[0048] In a forty-second embodiment (42), there is provided a method of strengthening an alkali aluminosilicate glass article according to any one of embodiments (29) to (41), wherein the glass article comprises from 1.92 mol % to 3.88 mol % MgO, inclusive.

[0049] In a forty-third aspect (43), there is provided a method of strengthening an alkali aluminosilicate glass article according to any one of aspects (29) to (42), wherein the glass article comprises greater than or equal to 0.78 mol % and less than or equal to 2.52 mol % CaO.

[0050] In a forty-fourth aspect (44), there is provided a method of strengthening an alkali aluminosilicate glass article according to any one of aspects (29) to (43), wherein the glass article comprises greater than or equal to 59 mol% and less than or equal to 66 mol% SiO2 and greater than or equal to 16 mol% and less than or equal to 21 mol% Na2O.

[0051] In a forty-fifth embodiment (45), there is provided a method of strengthening an alkali aluminosilicate glass article according to any one of embodiments (29)-(41), wherein the glass article comprises: greater than or equal to 64 mol% to less than or equal to 66 mol% SiO2; greater than or equal to 13 mol% to less than or equal to 15 mol% Al2O3; greater than or equal to 2 mol% to less than or equal to 3.88 mol% MgO; greater than or equal to 0.78 mol% to less than or equal to 2 mol% CaO; and greater than or equal to 15.5 mol% to less than or equal to 17.5 mol% Na2O.

[0052] In a forty-sixth embodiment (46), there is provided a method of strengthening an alkali aluminosilicate glass article according to any one of embodiments (29)-(41), wherein the glass article comprises from about 59.6 mol% to about 65.5 mol% SiO2, from about 12.78 mol% to about 15.96 mol% Al2O3, from about 1.92 mol% to about 3.88 mol% MgO, from about 0.78 mol% to about 2.52 mol% CaO, and from about 16.09 mol% to about 20.2 mol% Na2O.

[0053] In a forty-seventh embodiment (47), there is provided a method of strengthening an alkali aluminosilicate glass article according to any one of embodiments (29) to (46), wherein the glass article has a thickness of 4 millimeters or less.

[0054] In a forty-eighth embodiment (48), there is provided a method of strengthening an alkali aluminosilicate glass article according to any one of embodiments (29) to (46), wherein the glass article has a thickness in the range of 15 micrometers or more and 300 micrometers or less.

[0055] In a forty-ninth embodiment (49), there is provided a method of strengthening an alkali aluminosilicate glass article according to any one of embodiments (29) to (48), wherein the glass article has a liquidus viscosity in the range of from 500 kP or more to 2300 kP or less, measured before being ion-exchanged.

[0056] The accompanying drawings, which are incorporated in and form a part of this specification, illustrate aspects of the present disclosure. The drawings, together with the description, serve to further explain the principles and enable those skilled in the art to make and use the disclosed aspects. These drawings are intended to be illustrative, not limiting. While the present disclosure will generally be described in the context of these aspects, it should be understood that it is not intended to limit the scope of the disclosure to these particular aspects. In the drawings, like reference numbers indicate identical or functionally similar elements. [Brief description of the drawings]

[0057] [Figure 1] 1 illustrates a cross-section of a glass article having compressive stress regions according to the present embodiment. [Diagram 2] 1 shows a cross-sectional view of a glass article according to the present embodiment when the glass article is bent. [Figure 3A] FIG. 1 is a plan view of an exemplary electronic device incorporating a glass article according to any of the glass articles disclosed herein. [Figure 3B] FIG. 3B is a perspective view of the example electronic device of FIG. 3A. [Figure 4] 1 is a graph of calculated glass strength versus CS / E ratio for various exemplary ion-exchanged glass compositions. [Diagram 5] 1 is a graph of CS / E ratio versus liquidus viscosity for various exemplary ion-exchanged glass compositions. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0058] The following examples are illustrative only and are not intended to limit the disclosure. Other suitable modifications and adaptations of the variety of conditions and parameters normally encountered in the art will be apparent to those skilled in the art and are within the spirit and scope of the disclosure.

[0059] The glasses described herein are a family of ion-exchangeable alkali aluminosilicate glasses that can be ion-exchanged to achieve high peak compressive stress. As used herein, "ion-exchangeable" refers to a glass composition or glass article that includes a composition in which a first cation located at or near the surface of the substrate can be replaced with a second cation having the same valence. The first ion can be a sodium ion. The second ion can be one of potassium, rubidium, and cesium, provided that the second ion has a larger ionic radius than the first ion. The first ion is present in the glass-based substrate as its oxide (e.g., Na2O). As used herein, "ion-exchanged glass" or "chemically strengthened glass" refers to glass that has been subjected to at least one ion-exchange process to exchange a cation located at or near the surface of the glass with a cation having the same valence.

[0060] The glass compositions described herein may be ion-exchanged to achieve high peak compressive stress. In embodiments, the glasses described herein may be ion-exchanged to achieve peak compressive stresses of from about 500 MPa or more to about 1400 MPa. The high peak compressive stress imparted during ion-exchange processing may impart high strength to the glass with a shallow flaw size distribution, thereby preventing breakage during bending. The high peak compressive stress may allow the glass to remain in a net compression, thus allowing the glass to retain surface flaws when bent at tight bend radii. The glasses of the embodiments described herein have a low Young's modulus, which may result in lower bending stress values ​​during bending, preventing breakage during bending.

[0061] Furthermore, the glass compositions described herein have a ratio of peak compressive stress to Young's modulus (CS / E, where CS is in MPa and E is in GPa) of 15 or more over a wide range of compression depths for the compressed regions created by the ion exchange process. This ratio is difficult to increase because the surface compressive stress imparted during the ion exchange process can be strongly influenced by Young's modulus, and increasing Young's modulus is the usual way to improve the compressive stress. That is, Young's modulus is a measure of the stiffness of the network. For example, substituting K+ ions into Na+ sites imparts compressive stress, but the network becomes stiffer (due to the increase in Young's modulus), which in turn leads to higher expansive stress. Thus, one common way to obtain higher CS is simply to increase Young's modulus, but in the present disclosure, CS is increased without significantly increasing Young's modulus. With a high CS / E ratio, the glass composition can remain flexible even after ion exchange. The glass compositions described herein have a sufficiently low Young's modulus before being ion-exchanged, and the value of compressive stress that can be imparted during the ion-exchange process is high enough to achieve a high CS / E ratio over a wide range of compression depths. This results in a glass composition that is flexible and can accept high surface compressive stress values. Because the glass composition resists stress relaxation that can occur during the ion-exchange process, the glass composition can accept high surface compressive stresses at large compression depths, for example, as deep as 50 micrometers (microns and / or μm). Stress relaxation, which can become more pronounced at high temperatures and over time, is likely to occur during ion-exchange processes designed to impart large compression depths. These characteristics of the glass compositions described herein make the glass compositions suitable for a variety of industrial applications, including high strength cover glass applications that are subject to large bending stresses during use, for example, as cover glass for flexible and foldable displays.

[0062] As used herein, "peak compressive stress" refers to the highest compressive stress (CS) value measured within the compressive stress region. In embodiments, the peak compressive stress is located at the surface of the glass. In other embodiments, the peak compressive stress may occur at a depth below the surface, resulting in a compressive stress profile that appears as a "buried peak." Unless otherwise noted, compressive stress (including surface CS) is measured by a surface stress meter (FSM) using a commercially available instrument, for example, an FSM-6000 manufactured by Orihara Seisakusho Co., Ltd. (Japan). Surface stress measurements rely on accurate measurement of the stress optical coefficient (SOC), which is related to the birefringence of the glass. SOC is then measured by Procedure C (glass disk method) as described in ASTM Standard C770-16, entitled "Standard Test Method for Measurement of Glass Stress-Optical Coefficient."

[0063] As used herein, "depth of compression" (DOC) refers to the depth at which stress in a glass article changes from compressive to tensile stress. At DOC, stress transitions from compressive to tensile stress, thus exhibiting a stress value of zero. Depth of compression and depth of layer may be measured by a surface stress meter, for example, an FSM-6000 surface stress meter. As used herein, "depth of layer" (DOL) refers to the depth in a glass article at which metal oxide ions diffuse into the glass article, where the ion concentration is at a minimum. For example, with only potassium ion-exchanged into the glass article, DOC may be equal to DOL. Unless otherwise noted, DOC and DOL are used interchangeably herein.

[0064] It may also be possible to produce the glass compositions described herein at reasonable cost. The glass compositions exhibit suitably high liquidus temperatures and suitably low liquidus viscosities for certain manufacturing techniques, such as slot draw. These thermal properties may increase the manufacturability of glass articles made from the compositions, thereby reducing costs. The glass compositions of the present disclosure have aluminum oxide, magnesium oxide, calcium oxide, and sodium oxide contents, among others, that facilitate melting during manufacturing. In an embodiment, the glass compositions may have a liquidus viscosity ranging from 500 kP (kilopoise) or more to 2300 kP or less. In an embodiment, the glass compositions may have a liquidus temperature of 500° C. or more.

[0065] The glass compositions described herein may provide one or more of the following advantages: (1) The compositions are lithium-free, yet achieve high compressive stress values ​​(e.g., up to 1400 MPa) at small depths of compression (DOC) during ion exchange, with compressive stress values ​​of up to about 1100 MPa achievable at DOCs of 20 microns (micrometers, μm) and even higher at DOCs of about 40 microns. (2) The compositions have low elastic modulus, thereby enabling high CS / E ratios and improving bendability for thin foldable applications. (3) The materials for making these glasses are inexpensive and readily available. (4) The compositions may have higher excess modifier content, making them easier to melt. For a glass composition, "excess modifier" content means that the value of (mol% RO+mol% RO-mol% Al2O3) is greater than 0 mol%, where mol% RO is the total mol% of all alkali metal oxides in the composition, and mol% RO is the total mol% of all alkaline earth metal oxides in the composition. (5) The composition has a low liquidus temperature, high liquidus viscosity, and a slow growing liquidus, all of which are advantageous for sheet formation. (6) The composition may prevent fast ion exchange rates when exposed to a molten salt bath, thereby allowing for improved manufacturing process control. In other words, the composition is ion exchanged relatively slowly, which may be advantageous for controlling ion exchange in the composition. For example, the DOC of an ion-exchanged glass article may be more precisely controlled due to the relatively slow ion exchange rate in the composition. Particularly for thin glass articles (e.g., glass articles having a thickness of 500 micrometers or less), a precisely controlled DOC can be advantageous because the DOC can rapidly approach the desired depth in the glass article.

[0066] Total stress (δ net ), flaw size (a), and the fracture toughness of the material (K IC Starting with the fundamental fracture toughness equation that governs the relationship between CS and E, the advantage of the CS / E ratio described herein can be shown. Fracture toughness can be expressed as:

[0067]

number

[0068] In Equation 1, "Y" is a geometric factor, and δ net = δ bend -δ IOX where δ bend is the bending stress applied to the glass article, and δ IOX is the compressive stress exerted on the glass article by ion exchange. For small flaw sizes, δ IOX can be equal to the peak compressive stress (SC). For the plate separation distance (D) measured in millimeters during the bending test, δ bend may be expressed using the following formula, where E=Young's modulus of the glass composition measured in Pascals, v is the Poisson's ratio of the glass composition, and h is the thickness of the glass article measured in micrometers.

[0069]

number

[0070] By a series of substitutions, the glass strength (δ net ) The Poisson's ratio of alkali aluminosilicate glass is about 0.21, so Z h,D can be considered to be substantially constant.

[0071]

number

[0072] Graph 400 of FIG. 4 illustrates the thermal expansion coefficient for 80 exemplary glass compositions. TIFF2024538127000005.tif11114

[0073] 4 shows a plot of CS / E ratio of 0.01 to 0.01. The CS / E ratios in graph 400 were measured for a 30 micrometer thick glass article having a DOC of 20 micrometers. The glass strength values ​​in FIG. 4 were calculated based on a 30 micrometer thick glass article and a plate separation distance (D) of 3 millimeters. As graph 400 shows, TIFF2024538127000006.tif11114

[0074] is directly proportional to the CS / E ratio, and the following relationship can be derived:

[0075]

number

[0076] Therefore, according to the following relationship, (δ net ) can be said to be directly proportional to CS / E.

[0077]

number

[0078] Therefore, by increasing the CS / E ratio, the glass strength (δ net ) can be enhanced. Increasing the CS / E ratio can improve manufacturing yields by, among other things, allowing tighter bend radii for the same thickness of glass, allowing thicker glass to be bent to the same plate separation distance (D) without glass breakage, and increasing scratch tolerance. These benefits can be further quantified using Equations 1-5 by considering the following comparison of two glass compositions having Young's modulus and peak compressive stress values ​​summarized in Table 1. Composition A (CA) in Table 1 is a composition containing 68.95 mol% SiO2, 10.27 mol% Al2O3, 5.36 mol% MgO, 0.06 mol% CaO, 15.20 Na2O, and 0.17 mol% SnO2. Composition 44 (C44) in Table 1 is composition C44 described in Table 2G.

[0079] [Table 1]

[0080] It is made of CA, 0.264 micrometers, 30% K 1C A 30 micrometer thick glass article with a flaw size can be safely bent to a plate separation distance (D) of about 3 mm with a bending stress of about 901 MPa, resulting in a δ of 201 MPa. net In comparison, a 30 micrometer thick glass article made of C44 and with the same flaw size achieved a δ of 201 MPa. net In this context, a 34 micrometer thick glass article constructed from C44 and having the same flaw size can be safely bent at a δ of 201 MPa. net It can be safely bent up to a plate spacing distance (D) of 3 mm while maintaining the same.

[0081] Furthermore, a 30 micrometer thick glass article constructed from CA can be safely bent to a plate separation (D) of 3 mm, resulting in a δ net We obtained a 30% K value of 0.264 micrometers. 1C In comparison, a 30 micrometer thick glass article constructed from C44 can be safely bent to a plate separation distance (D) of 3 mm, resulting in a δ net A mere δ of 81 MPa was obtained. net Glass articles made of C44 have a 30% K range up to 1.626 micrometers. 1C Can withstand the size of the wound.

[0082] As used herein, the term "glass" is meant to include any material made at least in part from glass, including glasses and glass-ceramics. "Glass-ceramics" includes materials produced through controlled glass crystallization. One or more nucleating agents, such as titanium dioxide (TiO2), zirconium dioxide (ZrO2), sodium oxide (Na2O), and phosphorus oxide (P2O5), may be added to the glass-ceramic composition to facilitate uniform crystallization.

[0083] Unless otherwise stated, for glass compositions described herein, concentrations of components (e.g., SiO2, Al2O3, Na2O, etc.) are given in mole percent (mol%) on an oxide basis. Next, the components of the glass compositions according to the present embodiment are individually described. It should be understood that any of the various recited ranges of one component may be individually combined with any of the various recited ranges of any other component. As used herein, a zero at the end of a numerical value is intended to represent a significant digit for that numerical value. For example, the numerical value "1.0" includes two significant digits, and the numerical value "1.00" includes three significant digits. As used herein, a composition described as including an oxide within a range defined by 0 mol% as the lower limit means that the composition includes any amount of oxide greater than 0 mol% (e.g., 0.01 mol%, or 0.1 mol%) up to the upper limit of the range.

[0084] SiO2 may be the largest component in a glass composition and is therefore the main component of the glass network formed from the glass composition. Pure SiO2 has a relatively low coefficient of thermal expansion (CTE - as used herein, this property is measured at temperatures from 0°C to 300°C) and is alkali-free. However, pure SiO2 has a high melting point. Thus, if the concentration of SiO2 in a glass composition is too high, the formability of the glass composition may be reduced, as a higher concentration of SiO2 makes it difficult to melt the glass, adversely affecting the formability of the glass.

[0085] In an embodiment, the glass composition may include 55 mol% or more SiO2, 56 mol% or more SiO2, 57 mol% or more SiO2, 58 mol% or more SiO2, 59 mol% or more SiO2, 60 mol% or more SiO2, 61 mol% or more SiO2, 62 mol% or more SiO2, 63 mol% or more SiO2, 64 mol% or more SiO2, 65 mol% or more SiO2, or 66 mol% or more SiO2. In an embodiment, the glass composition may include 70 mol% or less SiO2, 69 mol% or less SiO2, 68 mol% or less SiO2, 67 mol% or less SiO2, 66 mol% or less SiO2, 65 mol% or less SiO2, 64 mol% or less SiO2, 63 mol% or less SiO2, 62 mol% or less SiO2, 61 mol% or less SiO2, or 60 mol% or less SiO2.

[0086] Any of the above SiO2 ranges may be combined with other ranges. For example, in embodiments, the glass composition may include 55 mol% to 70 mol% SiO2, 55 mol% to 69 mol% SiO2, 55 mol% to 68 mol% SiO2, 55 mol% to 67 mol% SiO2, 55 mol% to 66 mol% SiO2, 55 mol% to 65 mol% SiO2, 55 mol% to 64 mol% SiO2, 55 mol% to 63 mol% SiO2, 55 mol% to 62 mol% SiO2, 55 mol% to 61 mol% SiO2, 55 mol% to 62 mol% SiO2, 55 mol% to 63 mol% SiO2, 55 mol% to 64 mol% SiO2, 55 mol% to 65 ... It may contain from the top 60 mol% or less of SiO2, 56 mol% to 70 mol% of SiO2, 57 mol% to 70 mol% of SiO2, 58 mol% to 70 mol% of SiO2, 59 mol% to 70 mol% of SiO2, 60 mol% to 70 mol% of SiO2, 61 mol% to 70 mol% of SiO2, 62 mol% to 70 mol% of SiO2, 63 mol% to 70 mol% of SiO2, 64 mol% to 70 mol% of SiO2, or 65 mol% to 70 mol% of SiO2.

[0087] In embodiments, the glass composition comprises 59 mol% to 66 mol% SiO2, including subranges. For example, in embodiments, the glass composition may comprise 60 mol% to 66 mol% SiO2, 61 mol% to 66 mol% SiO2, 62 mol% to 66 mol% SiO2, 63 mol% to 66 mol% SiO2, 64 mol% to 66 mol% SiO2, 65 mol% to 66 mol% SiO2, 59 mol% to 65 mol% SiO2, 59 mol% to 64 mol% SiO2, 59 mol% to 63 mol% SiO2, 59 mol% to 62 mol% SiO2, 59 mol% to 61 mol% SiO2, or 59 mol% to 60 mol% SiO2.

[0088] In embodiments, the glass composition comprises greater than or equal to 59.6 mol % to less than or equal to 65.5 mol % SiO2, including subranges. For example, in embodiments, the glass composition may include 60.0 mol% to 65.5 mol% SiO2, 60.5 mol% to 65.5 mol% SiO2, 61.0 mol% to 65.5 mol% SiO2, 61.5 mol% to 65.5 mol% SiO2, 62.0 mol% to 65.5 mol% SiO2, 62.5 mol% to 65.5 mol% SiO2, 63.0 mol% to 65.5 mol% SiO2, 59.6 mol% to 65.0 mol% SiO2, 59.6 mol% to 64.5 mol% SiO2, 59.6 mol% to 64.0 mol% SiO2, 59.6 mol% to 63.5 mol% SiO2, 59.6 mol% to 63.0 mol% SiO2, or 59.6 mol% to 62.5 mol% SiO2.

[0089] The glass compositions described herein include Al2O3. Added Al2O3 can act as a glass network former. Furthermore, when the concentration of Al2O3 is balanced with the concentration of SiO2 and the concentration of alkali oxides in the composition, it can lower the liquidus temperature of the molten glass, thereby increasing the liquidus viscosity.

[0090] In embodiments, the sum of the mole % Al2O3 and the mole % RO in the composition (mol % Al2O3+mol % RO) can be 17 mol % or greater. In embodiments, the mole % Al2O3+mol % RO can be from 17 mol % or greater to 21 mol % or less (e.g., 21 mol %≧mol % Al2O3+mol % RO≧17 mol %), including subranges. In embodiments, the mole % Al2O3+mol % RO can be 18 mol % or greater, 19 mol % or greater, or 20 mol % or greater. In embodiments, the mole % Al2O3+mol % RO can be 20 mol % or less, 19 mol % or less, or 18 mol % or less. In the above formula, the mole % RO is equal to the sum of the mole % MgO and the mole % CaO.

[0091] Any of the above ranges may be combined with any other range. For example, in embodiments, the mol% Al2O3 + mol% RO may be 17 mol% to 21 mol%, 18 mol% to 21 mol%, 19 mol% to 21 mol%, 17 mol% to 20 mol%, or 17 mol% to 19 mol%.

[0092] The above (mol% Al2O3+mol% RO) values ​​are beneficial for the glass compositions described herein. With the above (mol% Al2O3+mol% RO), the glass compositions can achieve high peak compressive stress over a wide compression depth as described herein. If (mol% Al2O3+mol% RO) is lower than 17 mol%, then a desirably high ion-exchange stress may not be formed. If (mol% Al2O3+mol% RO) is higher than 21 mol%, then the ion-exchange process may be too slow and / or the Young's modulus may be undesirably high. Additionally, at values ​​higher than 21 mol%, the manufacturability of the glass compositions may be reduced.

[0093] In embodiments, the glass composition may include 12.5 mol% to 16.0 mol% Al2O3, including subranges. For example, in embodiments, the glass composition may include 13.0 mol% to 16.0 mol% Al2O3, 13.5 mol% to 16.0 mol% Al2O3, 14.0 mol% to 16.0 mol% Al2O3, 14.5 mol% to 16.0 mol% Al2O3, 15.0 mol% to 16.0 mol% Al2O3, 12.5 mol% to 15.5 mol% Al2O3, 12.5 mol% to 15.0 mol% Al2O3, 12.5 mol% to 14.5 mol% Al2O3, 12.5 mol% to 14.0 mol% Al2O3, or 12.5 mol% to 13.5 mol% Al2O3.

[0094] In embodiments, the glass composition includes from 13 mol% to 15 mol% Al2O3, including subranges. For example, in embodiments, the glass composition may include from 13.5 mol% to 15 mol% Al2O3, from 14 mol% to 15 mol% Al2O3, from 14.5 mol% to 15 mol% Al2O3, from 13 mol% to 14.5 mol% Al2O3, from 13 mol% to 14.0 mol% Al2O3, or from 13 mol% to 13.5 mol% Al2O3.

[0095] In an embodiment, the glass composition comprises from 12.78 mol% to 15.96 mol% Al2O3, including subranges. For example, in an embodiment, the glass composition comprises from 13.0 mol% to 15.96 mol% Al2O3, from 13.25 mol% to 15.96 mol% Al2O3, from 13.5 mol% to 15.96 mol% Al2O3, from 13.75 mol% to 15.96 mol% Al2O3, from 14.0 mol% to 15.96 mol% Al2O3, from 14.25 mol% to 15.96 mol% Al2O3, from 14.5 mol% to 15.96 mol% Al2O3, from 14.75 mol% to 15.96 mol% Al2O3, from 15.0 mol% to 15.96 mol% A2O3, from 15.0 mol% to 15.96 mol% B2O3, from 15.0 mol% to 15.96 mol% C ... % to 15.75 mol% Al2O3, 12.78 mol% to 15.5 mol% Al2O3, 12.78 mol% to 15.25 mol% Al2O3, 12.78 mol% to 15.0 mol% Al2O3, 12.78 mol% to 14.75 mol% Al2O3, 12.78 mol% to 14.5 mol% Al2O3, 12.78 mol% to 14.25 mol% Al2O3, 12.78 mol% to 14.0 mol% Al2O3, or 12.78 mol% to 13.75 mol% Al2O3.

[0096] In embodiments, the glass composition may include from 12.5 mol% to 16 mol% Al2O3, including subranges. For example, in embodiments, the glass composition may include from 13 mol% to 16 mol% Al2O3, from 14 mol% to 16 mol% Al2O3, from 12.5 mol% to 15 mol% Al2O3, or from 12.5 mol% to 14 mol% Al2O3.

[0097] The glass compositions described herein include Na2O. Na2O can promote the ion exchangeability and improve the formability of the glass composition, thereby improving the manufacturability of the glass composition. However, if too much Na2O is added to the glass composition, the CTE can become too low and the melting point can become too high. Furthermore, if too much Na2O is added to the glass composition, the ion exchange rate of the glass can, in some cases, be too fast to precisely control the ion exchange in the composition.

[0098] In embodiments, the glass composition includes from 16 mol% to 21 mol% Na2O, including subranges. For example, in embodiments, the glass composition includes from 16.5 mol% to 21 mol% Na2O, from 17 mol% to 21 mol% Na2O, from 17.5 mol% to 21 mol% Na2O, from 18 mol% to 21 mol% Na2O, from 18.5 mol% to 21 mol% Na2O, from 19 mol% to 21 mol% Na2O, from 19.5 mol% to 21 mol% Na2O, from 20 ... It may contain from the top 21 mol% or less Na2O, 16 mol% or more to 20.5 mol% or less Na2O, 16 mol% or more to 20 mol% or less Na2O, 16 mol% or more to 19.5 mol% or less Na2O, 16 mol% or more to 19 mol% or less Na2O, 16 mol% or more to 18.5 mol% or less Na2O, 16 mol% or more to 18 mol% or less Na2O, or 16 mol% or more to 17.5 mol% or less Na2O.

[0099] In embodiments, the glass composition includes greater than or equal to 15.5 mol % NaO, inclusive, and can include subranges. For example, in embodiments, the glass composition may include 15.75 mol% to 17.5 mol% NaO, 16.0 mol% to 17.5 mol% NaO, 16.25 mol% to 17.5 mol% NaO, 16.5 mol% to 17.5 mol% NaO, 16.75 mol% to 17.5 mol% NaO, 17.0 mol% to 17.5 mol% NaO, 15.5 mol% to 17.25 mol% NaO, 15.5 mol% to 17.0 mol% NaO, 15.5 mol% to 16.75 mol% NaO, 15.5 mol% to 16.5 mol% NaO, 15.5 mol% to 16.25 mol% NaO, or 15.5 mol% to 16.0 mol% NaO.

[0100] In embodiments, the glass composition includes from 16.09 mol% to 20.2 mol% Na2O, including subranges. For example, in embodiments, the glass composition includes from 16.5 mol% to 20.2 mol% Na2O, from 17.0 mol% to 20.2 mol% Na2O, from 17.5 mol% to 20.2 mol% Na2O, from 18.0 mol% to 20.2 mol% Na2O, from 18.5 mol% to 20.2 mol% Na2O, from 19.0 mol% to 20.2 mol% Na2O, from 16.09 ...6.09 mol% to 20.2 mol% Na2O, from 16.09 mol% to 20.2 mol% Na2O, from 16.09 mol% to 20.2 mol% Na2O, from 16.09 mol% to 20.2 mol% Na2O, from 16.09 mol% to 20.2 mol% Na2O, from 16.09 mol% to 20.2 mol% Na2O, from 16.09 mol% to 20.2 mol% Na2O, from 16.09 mol% to 20.2 % to 20.0 mol% NaO, 16.09 mol% to 19.5 mol% NaO, 16.09 mol% to 19.0 mol% NaO, 16.09 mol% to 18.5 mol% NaO, 16.09 mol% to 18.0 mol% NaO, 16.09 mol% to 17.5 mol% NaO, or 16.09 mol% to 17.0 mol% NaO.

[0101] In embodiments, the molar % of Na2O+mol % of RO-mol % of Al2O3 (mol % of Na2O+mol % of RO-mol % of Al2O3) for the glass composition can be 4 mol % or greater. In embodiments, the molar % of Na2O+mol % of RO-mol % of Al2O3 can be 4 mol % or greater to 11 mol % or less (e.g., 11 mol %≧(mol % of Na2O+mol % of RO-mol % of Al2O3≧4 mol %), including subranges. In embodiments, the molar % of Na2O+mol % of RO-mol % of Al2O3 can be 5 mol % or greater, 6 mol % or greater, 7 mol % or greater, 8 mol % or greater, 9 mol % or greater, or 10 mol % or greater. In embodiments, the mole % Na2O+mol % RO-mol % Al2O3 can be 11 mol % or less, 10 mol % or less, 9 mol % or less, 8 mol % or less, 7 mol % or less, 6 mol % or less, or 5 mol % or less, where the mole % RO is equal to the sum of the mole % MgO and the mole % CaO.

[0102] Any of the above ranges may be combined with any other range. For example, in embodiments, the mol% Na2O+mol% RO-Al2O3 may be 4 mol% to 10 mol%, 4 mol% to 9 mol%, 4 mol% to 8 mol%, or 4 mol% to 7 mol%.

[0103] The above (mol% Na2O+mol% RO-mol% Al2O3) values ​​are beneficial to the glass compositions described herein. With the above (mol% Na2O+mol% RO-mol% Al2O3) values, the glass compositions exhibit the following advantageous physical properties: First, adjusting the (mol% Na2O+mol% RO-mol% Al2O3) values ​​as described above improves the meltability of the glass composition. As described herein, the (mol% Na2O+mol% RO-mol% Al2O3) values ​​result in advantageous thermal physical properties, such as liquidus temperature and liquidus viscosity, that facilitate the manufacture of glass articles from the composition. If the (mol% Na2O+mol% RO-mol% Al2O3) values ​​are less than 4 mol%, the meltability of the glass composition may be impaired. Second, adjusting the (mol % Na2O+mol % RO-mol % Al2O3) value as described above may ensure an ion-exchange range that may produce a desirable compositional gradient while preventing significant stress relaxation in the glass article that would offset the compressive stress imparted by the ion-exchange process. Values ​​of (mol % Na2O+mol % RO-mol % Al2O3) greater than 11 mol % may result in a significant amount of stress relaxation in the glass article during the ion-exchange process. Such stress relaxation may reduce the compressive stress imparted during ion-exchange, particularly the peak compressive stress.

[0104] In embodiments, for the glass composition, the Na2O mol% + RO mol% (Na2O mol% + RO mol%) can be 20 mol% or greater. In embodiments, the Na2O mol% + RO mol% can be 20 mol% or greater to 25 mol% or less (e.g., 25 mol% > (Na2O mol% + RO mol%) > 20 mol%). The above Na2O mol% + RO mol% values ​​can be beneficial for the glass compositions described herein. With the above Na2O mol% + RO mol% values, the glass composition can exhibit a desired liquidus temperature, a desired liquidus viscosity, or both, for some manufacturing techniques for forming the composition into a glass article, such as slot draw. Additionally, the above Na2O mol% + RO mol% values ​​can facilitate the formation of high peak compressive stresses during ion exchange.

[0105] In embodiments, for a glass composition, the mol% Al2O3 + mol% Na2O (mol% Al2O3 + mol% Na2O) can be 28 mol% or greater. In embodiments, the mol% Al2O3 + mol% Na2O can be 28 mol% or greater to 37 mol% or less (e.g., 37 mol% > (mol% Na2O + mol% RO > 28 mol%), including subranges. For example, in embodiments, the mol% Al2O3 + mol% Na2O can be 30 mol% or greater to 37 mol% or less, 32 mol% or greater to 37 mol% or less, 28 mol% or greater to 35 mol% or less, or 28 mol% or greater to 33 mol% or less. The above (mol% Al2O3 + mol% Na2O) values ​​can be beneficial for the glass compositions described herein. Using the above (mol % AlO+mol % NaO) values, the glass composition may exhibit a desired liquidus temperature, a desired liquidus viscosity, or both, for a number of manufacturing techniques for forming the composition into a glass article, such as slot drawing.

[0106] The glass compositions described herein include MgO. MgO can reduce the viscosity of the glass, thereby increasing the formability and manufacturability of the glass. Including MgO in the glass composition can improve the strain point and Young's modulus of the glass composition, as well as the ion exchangeability of the glass. However, adding too much MgO to the glass composition can increase the density and CTE of the glass composition to undesirable levels. Furthermore, adding too much MgO can result in too high a liquidus temperature and too low a liquidus viscosity for some manufacturing processes.

[0107] In embodiments, the glass composition includes from 1 mol% to 3.88 mol% MgO, including subranges. For example, in embodiments, the glass composition includes from 1.25 mol% to 3.88 mol% MgO, from 1.5 mol% to 3.88 mol% MgO, from 1.75 mol% to 3.88 mol% MgO, from 2.0 mol% to 3.88 mol% MgO, from 2.25 mol% to 3.88 mol% MgO, from 2.5 mol% to 3.88 mol% MgO, from 2.75 mol% to 3.88 mol% MgO, from 3.0 mol% to 3.88 mol% MgO, from 3.25 ... % to 3.88 mol% MgO, 1 mol% to 3.5 mol% MgO, 1 mol% to 3.25 mol% MgO, 1 mol% to 3.0 mol% MgO, 1 mol% to 2.75 mol% MgO, 1 mol% to 2.5 mol% MgO, 1 mol% to 2.25 mol% MgO, 1 mol% to 2.0 mol% MgO, 1 mol% to 1.75 mol% MgO, or 1 mol% to 1.5 mol% MgO.

[0108] In embodiments, the glass composition includes from 1.92 mol% to 3.88 mol% MgO, including subranges. For example, in embodiments, the glass composition includes from 2.0 mol% to 3.88 mol% MgO, from 2.2 mol% to 3.88 mol% MgO, from 2.4 mol% to 3.88 mol% MgO, from 2.6 mol% to 3.88 mol% MgO, from 2.8 mol% to 3.88 mol% MgO, from 3.0 mol% to 3.88 mol% MgO, from 3.2 mol% to 3.88 mol% MgO, % to 3.6 mol % MgO, 1.92 mol % to 3.4 mol % MgO, 1.92 mol % to 3.2 mol % MgO, 1.92 mol % to 3.0 mol % MgO, 1.92 mol % to 2.8 mol % MgO, 1.92 mol % to 2.6 mol % MgO, or 1.92 mol % to 2.4 mol % MgO.

[0109] In embodiments, the glass composition may include from ≧1 mol% to ≦4 mol% MgO, including subranges. For example, in embodiments, the glass composition may include from ≧1.5 mol% to ≦4 mol% MgO, from ≧2 mol% to ≦4 mol% MgO, from ≧2.5 mol% to ≦4 mol% MgO, from ≧1 mol% to ≦3.5 mol% MgO, from ≧1 mol% to ≦3 mol% MgO, or from ≧1 mol% to ≦2.5 mol% MgO.

[0110] The glass compositions described herein include CaO. CaO reduces the viscosity of the glass, which increases the formability, strain point, and Young's modulus, and may improve the ion exchangeability of the glass. However, if too much CaO is added to the glass composition, the density and CTE of the glass composition may increase to undesirable levels. Furthermore, the amount of CaO described herein helps to slow down the ion exchange process in the composition, which may allow for more precise control of the ion exchange process. For example, the amount of CaO may allow for more precise control of the DOC.

[0111] In embodiments, the glass composition includes greater than or equal to 0.78 mol % CaO, inclusive, and can include subranges. For example, in embodiments, the glass composition may include 1.0 mol% to 3 mol% CaO, 1.25 mol% to 3 mol% CaO, 1.5 mol% to 3 mol% CaO, 1.75 mol% to 3 mol% CaO, 2.0 mol% to 3 mol% CaO, 2.25 mol% to 3 mol% CaO, 2.5 mol% to 3 mol% CaO, 0.78 mol% to 2.75 mol% CaO, 0.78 mol% to 2.5 mol% CaO, 0.78 mol% to 2.25 mol% CaO, 0.78 mol% to 2.0 mol% CaO, 0.78 mol% to 1.75 mol% CaO, 0.78 mol% to 1.5 mol% CaO, or 0.78 mol% to 1.25 mol% CaO.

[0112] In embodiments, the glass composition includes greater than or equal to 0.78 mol % CaO, inclusive, and can include subranges. For example, in embodiments, the glass composition may include 0.9 mol% to 2 mol% CaO, 1.0 mol% to 2 mol% CaO, 1.1 mol% to 2 mol% CaO, 1.2 mol% to 2 mol% CaO, 1.3 mol% to 2 mol% CaO, 1.4 mol% to 2 mol% CaO, 1.5 mol% to 2 mol% CaO, 0.78 mol% to 1.9 mol% CaO, 0.78 mol% to 1.8 mol% CaO, 0.78 mol% to 1.7 mol% CaO, 0.78 mol% to 1.6 mol% CaO, 0.78 mol% to 1.5 mol% CaO, 0.78 mol% to 1.4 mol% CaO, 0.78 mol% to 1.3 mol% CaO, or 0.78 mol% to 1.2 mol% CaO.

[0113] In embodiments, the glass composition includes from greater than or equal to 0.78 mol % to less than or equal to 2.52 mol % CaO, including subranges. For example, in embodiments, the glass composition may include 1.0 mol% to 2.52 mol% CaO, 1.2 mol% to 2.52 mol% CaO, 1.4 mol% to 2.52 mol% CaO, 1.6 mol% to 2.52 mol% CaO, 1.8 mol% to 2.52 mol% CaO, 2.0 mol% to 2.52 mol% CaO, 0.78 mol% to 2.4 mol% CaO, 0.78 mol% to 2.2 mol% CaO, 0.78 mol% to 2.0 mol% CaO, 0.78 mol% to 1.8 mol% CaO, 0.78 mol% to 1.6 mol% CaO, 0.78 mol% to 1.4 mol% CaO, or 0.78 mol% to 1.2 mol% CaO.

[0114] In embodiments, the glass composition may include from 0.5 mol% to 3 mol% CaO, including subranges, For example, in embodiments, the glass composition may include from 1 mol% to 3 mol% CaO, from 2 mol% to 3 mol% CaO, or from 0.5 mol% to 2 mol% CaO.

[0115] In embodiments, for a glass composition, the ratio of the mole % MgO to the sum of the mole % MgO and the mole % CaO (mol % MgO / (mol % MgO+mol % CaO)) can be 0.5 or greater. In embodiments, the mole % MgO / (mol % MgO+mol % CaO) can be 0.55 or greater, 0.6 or greater, 0.65 or greater, 0.7 or greater, 0.75 or greater, or 0.8 or greater. In embodiments, the mole % MgO / (mol % MgO+mol % CaO) can be 0.8 or less, 0.75 or less, 0.7 or less, 0.65 or less, 0.6 or less, 0.55 or less, or 0.5 or less.

[0116] In embodiments, the mol% MgO / (mol% MgO+mol% CaO) is from 0.5 to 0.8 (e.g., 0.8≧(mol% MgO / (mol% MgO+mol% CaO)≧0.5), including all ranges and subranges therebetween. For example, in embodiments, the mol% MgO / (mol% MgO+mol% CaO) can be from 0.55 to 0.8, from 0.6 to 0.8, from 0.65 to 0.8, from 0.7 to 0.8, from 0.5 to 0.75, from 0.5 to 0.7, from 0.5 to 0.65, or from 0.5 to 0.6.

[0117] The glass compositions described herein may be free or substantially free of one or more of ZnO, SrO, BaO, B2O3, P2O5, Li2O, and K2O. In embodiments, the glass compositions may be substantially free or substantially free of all of ZnO, SrO, BaO, B2O3, P2O5, Li2O, and K2O. Some of these oxides may be expensive and / or in limited supply. Alkaline earth metal oxides may undesirably increase the Young's modulus and slow the ion-exchange process. B2O3, P2O5, and K2O may reduce the amount of compressive stress imparted during the ion-exchange process. The glass articles described herein can achieve advantageous physical properties without the need for these oxides. Thus, these oxides may be excluded from the composition. As used herein, the term "substantially free" means that the component may be present in the final glass in very small amounts as an impurity, but is not added as a component of the batch materials. Due to the raw materials and / or equipment used to make the glass compositions of the present disclosure, some impurities or components not intentionally added may be present in the final glass composition. Such materials are present in small amounts in the glass composition and are referred to as "contaminant materials." A composition that is "substantially free" of a component means that the component was not intentionally added to the composition, but the composition may still contain the component in a contaminant or trace amount. A composition that is "substantially free" of an oxide means that the oxide is present in an amount of 0.1 mol % or less, e.g., 0 mol % to 0.1 mol %. As used herein, a glass composition that is "totally free" of a component is defined to mean that the component (e.g., oxide) is not present in the composition, either contaminantly or in a trace amount.

[0118] In embodiments, the glass composition may optionally include one or more fining agents. In embodiments, the fining agent may include, for example, SnO2. In such embodiments, SnO2 may be present in the glass composition in an amount of 2 mol% or less, such as 0 mol% to 2 mol%, including subranges. For example, in embodiments, SnO2 may be present in the glass composition in an amount of 0.1 mol% to 2 mol%, 0.1 mol% to 1.5 mol%, 0.1 mol% to 1 mol%, 0.1 mol% to 0.5 mol%, or 0.1 mol% to 0.25 mol%.

[0119] Next, the physical properties of the glass compositions described herein and glass articles fabricated therefrom are described. As described in more detail in the Examples, these physical properties can be achieved by adjusting the amounts of the components of the glass compositions.

[0120] In embodiments, the Young's modulus (E) of the glass composition is from 70 GPa to 80 GPa, including all ranges and subranges therebetween. For example, in embodiments, the Young's modulus (E) of the glass composition can be from 70 GPa to 79 GPa, from 70 GPa to 78 GPa, from 70 GPa to 77 GPa, from 70 GPa to 76 GPa, from 70 GPa to 75 GPa, from 70 GPa to 74 GPa, or from 70 GPa to 73 GPa.

[0121] Unless otherwise indicated, the Young's modulus and Poisson's ratio values ​​disclosed herein refer to values ​​measured by the typical resonant ultrasonic spectroscopy technique set forth in ASTM standard E2001-13 entitled "Standard Guide for Resonant Ultrasound Spectroscopy for Defect Detection in Both Metallic and Non-Metallic Parts". Furthermore, unless otherwise indicated, the Young's modulus and Poisson's ratio of a glass composition or article are measured before the composition or article is subjected to any ion exchange treatment or any other strengthening treatment. In particular, the Young's modulus and Poisson's ratio of a glass composition or article are measured before the composition or article is exposed to, e.g., immersed in, an ion exchange solution. The Poisson's ratio value (v) is calculated from the Young's modulus value (E) and the shear modulus (G) obtained from the ASTM E2001-13 test using the formula E=2G(1+v).

[0122] In embodiments, the liquidus viscosity of the glass composition can be in the range of 500 kP (kilopoise) or more. In embodiments, the liquidus viscosity of the glass composition can be in the range of 500 kP or more to 2300 kP or less, including subranges. For example, in embodiments, the liquidus viscosity of the glass composition can be in the range of 750 kP or more to 2300 kP or less, 1000 kP or more to 2300 kP or less, 1500 kP or more to 2300 kP or less, 500 kP or more to 2000 kP or less, 500 kP or more to 1750 kP or less, 500 kP or more to 1500 kP or less, 500 kP or more to 1250 kP or less, or 500 kP or more to 1000 kP or less. In embodiments, the liquidus viscosity of the glass composition can be in the range of 1000 kP or more to 1500 kP or less.

[0123] In an embodiment, the glass composition can have a liquidus temperature of 500° C. or more. In an embodiment, the glass composition can have a liquidus temperature of 500° C. or more and 1200° C. or less.

[0124] As used herein, the term "liquidus viscosity" refers to the viscosity of a molten glass at its liquidus temperature, which refers to the temperature at which crystals first appear as the molten glass cools from its melting point, or at which the last crystals melt as the temperature is increased from room temperature. Unless otherwise noted, the liquidus viscosity values ​​disclosed herein are determined by the following method. First, the liquidus temperature of the glass is measured by ASTM standard C829-81 (2015), entitled "Standard Practice for Measurement of Liquidus Temperature of Glass by the Gradient Furnace Method." Second, the viscosity at the liquidus temperature of the glass is measured by ASTM standard C965-96 (2012), entitled "Standard Practice for Measuring Viscosity of Glass above the Softening Point." Unless otherwise noted, the liquidus viscosity and temperature of a glass composition or article are measured before the composition or article is subjected to any ion exchange treatment or any other strengthening treatment. In particular, the liquidus viscosity and temperature of the glass composition or article are measured before exposing the composition or article to the ion exchange solution, e.g., before immersing it in the ion exchange solution.

[0125] Glass articles according to the present embodiment may be formed from the compositions described above by any suitable method, such as slot forming, float forming, rolling, fusion forming processes, etc. Glass compositions, and articles made therefrom, may be characterized by the method by which they may be formed. For example, glass compositions may be characterized as float formable (i.e., formed by a float process), downdrawable, and, particularly, fusion formable or slot drawable (e.g., formed by a downdraw process, such as a fusion draw process or a slot draw process).

[0126] In an embodiment, the glass articles described herein can be formed, for example, by a down-draw process. The down-draw process produces glass articles having uniform thickness with relatively flawless surfaces. Since the average bending strength of a glass article is controlled by the amount and size of surface flaws, flawless surfaces that produce minimal contact have higher initial strength. Furthermore, down-drawn glass articles have very flat and smooth surfaces that can be used without expensive grinding and polishing in their final applications.

[0127] In embodiments, the glass article may be described as fusion formable (i.e., formable using a fusion draw process). The fusion process employs a draw vessel having a channel for receiving molten glass frit. The channel has weirs on either side of the channel that open at the top and run along the length of the channel. When the channel is filled with molten material, the molten glass overflows the weirs. Gravity causes the molten glass to flow down the exterior surface of the draw vessel as two flowing glass films. These exterior surfaces of the draw vessel extend downward and inward to meet at the lower edge of the draw vessel. The two flowing glass films meet and fuse at this edge to form a single flowing glass article. The fusion draw process offers the advantage that the exterior surface of the resulting glass article does not come into contact with any part of the apparatus as the two glass films flowing over the channels fuse together. Thus, the surface properties of the fusion drawn glass article are not affected by such contact.

[0128] In embodiments, the glass articles described herein may be formed by a slot-draw process. The slot-draw process is distinct from the fusion draw process. In the slot-draw process, molten raw glass is fed into a draw vessel. The bottom of the draw vessel has an open slot and a nozzle extends the length of the slot. The molten glass flows through the slot and / or nozzle and is drawn downward into an annealing zone as a continuous glass article.

[0129] Draw processes to form glass articles, such as glass sheets, are desirable because they allow thin glass articles to be formed with few defects. Previously, it was believed that glass compositions needed to have relatively high liquidus viscosities, such as greater than 1000 kP, greater than 1100 kP, or greater than 1200 kP, to be formed by a draw process, such as fusion draw or slot draw. However, developments in draw processes may allow glasses having lower liquidus viscosities (e.g., liquidus viscosities as low as 500 kP) to be used in the draw process.

[0130] In aspects, the glass articles described herein may exhibit an amorphous microstructure and be substantially free of crystals or crystallites. In other words, the glass articles in these aspects exclude glass-ceramic materials. In other aspects, the glass articles described herein may include glass-ceramic materials.

[0131] As described above, glass compositions and articles formed therefrom may be strengthened by ion exchange treatment. Referring to FIG. 1, the glass article 100 may have one or more compressively stressed regions. For example, the glass article 100 may have a first compressive stress region 120 and / or a second compressive stress region 122 extending from an outer surface (e.g., surfaces 110, 112) of the glass article 100 to a compression depth (DOC, d1, d2) and a second region (e.g., central region 130) of tensile stress or CT extending from the DOC to a center or interior region of the glass article 100. The ion-exchanged compressive stress regions 120, 122 have different metal oxide concentrations at two or more locations through the thickness (t) of the glass article 100.

[0132] In common practice in the art, compression or compressive stress (CS) is expressed as a negative (<0) stress, and tension or tensile stress is expressed as a positive (>0) stress. However, throughout this specification, CS is expressed as a positive or absolute value, i.e., written as CS=|CS| herein. CS has a maximum value at the surface of the glass and can vary as a function of distance d from the surface. Referring again to FIG. 1 , a first compressive stress region 120 extends from the first surface 110 to a depth d1, and a second compressive stress region 122 extends from the second surface 112 to a depth d2. Together, these compressive stress regions 120, 122 define the compressed or CS region of the glass article 100.

[0133] In embodiments, the peak compressive stress of one or more compressive stress regions of the glass article is from 500 MPa to 1300 megapascals (MPa), including subranges. For example, in embodiments, the peak compressive stress of one or more compressive stress regions of the glass article can be from 600 MPa to 1300 MPa, from 700 MPa to 1300 MPa, from 800 MPa to 1300 MPa, from 900 MPa to 1300 MPa, from 1000 MPa to 1300 MPa, from 500 MPa to 1200 MPa, from 500 MPa to 1100 MPa, from 500 MPa to 1000 MPa, from 500 MPa to 900 MPa, or from 500 MPa to 800 MPa.

[0134] In embodiments, glass articles fabricated from the glass compositions may have a ratio of peak compressive stress value to Young's modulus value (peak compressive stress value / Young's modulus value, CS / E) of 15 or greater. In embodiments, the glass articles may have a CS / E ratio in the range of 15 or greater to 18 or less, including subranges. For example, in embodiments, the glass articles may have a CS / E ratio of 15.5 or greater to 18 or less, 16 or greater to 18 or less, 16.5 or greater to 18 or less, 17 or greater to 18 or less, 15 or greater to 17.5 or less, 15 or greater to 17 or less, 15 or greater to 16.5 or less, or 15 or greater to 16 or less.

[0135] These CS / E ratios and ranges of CS / E ratios can be achieved at the peak compressive stress and compression depth described herein. For example, in embodiments, the glass article can have a CS / E ratio or ranges of CS / E ratios as described for a peak compressive stress ranging from 500 MPa or more to 1300 MPa or less. As another example, the glass article can have a CS / E ratio or ranges of CS / E ratios as described for a compression depth ranging from 5 micrometers or more to 30 micrometers or less. As another example, the glass article can have a CS / E ratio or ranges of CS / E ratios as described for a compression depth ranging from 5 micrometers or more to 20 micrometers or less. As another example, the glass article can have a CS / E ratio or ranges of CS / E ratios as described for a compression depth ranging from 5% or more to 20% or less of the thickness of the glass article.

[0136] The high peak compressive stress that can be achieved by ion exchange allows for tighter (i.e., smaller) bend radii for a given glass thickness. The high peak compressive stress allows the glass to remain in a net compression and therefore contain surface flaws when the glass is bent to a tight radius. Flaws near the surface can thus be contained in a net compression or, if located within the effective surface compression layer, not stretch to failure.

[0137] FIG. 2 illustrates two-point bending of a glass article 100 with a bending force 202 between two parallel plates 200. The bending force 202 is applied using a two-point bending test apparatus, where the two parallel plates 200 press the glass article 100 with a constant force, the bending force 202, during the bending test. If necessary, fixtures associated with the test apparatus ensure that the glass article 100 bends symmetrically about the bend line 210 as the bending force 202 is applied to the glass article 100 through the plates 200. The plates 200 may move together simultaneously until a particular plate distance (D) is achieved. As used herein, the term "failure" upon application of a bending force refers to breakage, fracture, delamination, crack propagation, permanent deformation, or other mechanisms that render the article unsuitable for its intended use.

[0138] In Figure 2, surface 110 of glass article 100 is placed under tensile stress by bending while surface 112 is placed under additional compressive stress by bending, reducing the effective DOC from surface 110 below the DOC from surface 110 when the article is unbent. The effective DOC from surface 110 increases as the plate distance increases and decreases as the plate distance decreases (when the article is bent so that surfaces 112 are closer together as shown in Figure 2). In other words, the effective DOC is the DOC in the unbent state minus the effective depth from the tensile stress induced by bending.

[0139] In embodiments, the glass article 100 avoids failure during a static two-point bend test when held between two parallel plates 200 at a plate distance (D) of 10 millimeters (mm) or less for 240 hours at 60° C. and 93% relative humidity. For example, in embodiments, the glass article 100 avoids failure during a static two-point bend test when held between two plates at a plate distance (D) of 10 mm to 1 mm for 240 hours at 60° C. and 93% relative humidity. The plate distance (D) can be, for example, 10 mm, 9 mm, 8 mm, 7 mm, 6 mm, 5 mm, 4 mm, 3 mm, 2 mm, or 1 mm.

[0140] The compressive stress in both regions 120, 122 is balanced by the tension stored in the central region 130 of the glass article 100. Unless otherwise stated, the CT value is reported as the maximum CT value. The DOC can be measured by a surface stress meter or a scattered light polarimeter (SCALP) depending on the ion exchange process and the thickness of the article being measured. If the stress in the substrate is caused by exchanging potassium ions into the substrate, a surface stress meter, for example, FSM-6000 (Orihara Seisakusho Co., Ltd., Japan), is used to measure the compression depth. If the stress in the substrate is caused by exchanging sodium ions into the substrate and the article being measured is thicker than about 400 micrometers, SCALP is used to measure the compression depth and maximum central tension (CT). If the stress in the substrate is caused by exchanging both potassium and sodium ions into the glass and the article being measured is thicker than about 400 micrometers, SCALP is used to measure the compression depth and CT. Without wishing to be bound by theory, the exchange depth of sodium may indicate the compression depth, and the exchange depth of potassium ions may indicate a change in the magnitude of the compressive stress (although the change in stress is not necessarily from compressive to tensile). As used herein, "depth of layer" refers to the depth to which ions have been exchanged (e.g., sodium, potassium) into the substrate. Throughout this disclosure, when the maximum central tension cannot be measured directly by SCALP (such as when the article being measured is thinner than about 400 micrometers), it is approximated by multiplying the maximum central tension by the maximum compressive stress and the compression depth, and then dividing by the difference between the thickness of the substrate and twice the compression depth, and the compressive stress and compression depth are measured by FSM.

[0141] If the thickness of the substrate is greater than about 400 micrometers, the refractive near-field (RNF) method may also be used to display a graph of the stress profile. When the RNF method is used to display a graph of the stress profile, the RNF method uses the maximum CT value provided by SCALP. In particular, the stress profile measured by RNF is force balanced and calibrated to the maximum CT value provided by the SCALP measurement. The RNF method is described in U.S. Pat. No. 8,854,623, entitled "Systems and Methods for Measuring a Profile Characteristic of a Glass Sample," which is incorporated herein by reference in its entirety. In particular, the RNF method includes the steps of placing a glass article adjacent to a reference block, switching between orthogonal polarizations at a rate of 1 Hz to 50 Hz to generate a polarization-switched light beam, measuring the amount of power in the polarization-switched light beam, and generating a polarization-switched reference signal, where the amount of power measured in each orthogonal polarization is within 50% of each other. The method further includes transmitting the polarization-switched light beam through the glass sample and for different depths through the reference block and into the glass sample, and then relaying the transmitted polarization-switched light beam with relay optics to a signal light detector that generates a polarization-switched detector signal. The method further includes dividing the detector signal by the reference signal to determine a normalized detector signal, and determining a profile characteristic of the glass sample from the normalized detector signal.

[0142] When performing SCALP measurements, a SCALP polariscope (e.g., SCALP-04 or SCALP-05) available from GlassStress Ltd., Talinn, Estonia is used. A precise specimen speed SS and exposure time t are selected that reduce the measurement noise in the polariscope to an acceptable level when measuring the sample to characterize at least one stress-related property. Eis dependent on a number of factors. These factors include the characteristics of the image sensing device (e.g., gain, imaging speed (frames per second), pixel size, inter-pixel averaging techniques, etc.) as well as non-stress related (NSR) scattering properties, the intensity of the incident light beam, the number of polarization states used, etc. Other factors include the measurement wavelength of the light beam from the laser source and the intensity of the scattered light beam. Exemplary measurement wavelengths include 640 nanometers (nm), 518 nm, and 405 nm. Exemplary exposure times can range from 0.05 milliseconds to 100 milliseconds. Exemplary frame rates can range from 10 to 200 frames per second. An exemplary optical delay calculation can be performed using a measurement time t of 0.1 to 10 seconds. M A range of 2 to 200 frames may be used.

[0143] In embodiments, the glass article has a maximum CT of 20 MPa to 400 megapascals (MPa), e.g., 50 MPa to 350 MPa, 75 MPa to 300 MPa, 100 MPa to 250 MPa, or 150 MPa to 200 MPa, including all ranges and subranges therebetween, including and including any two of the above values ​​as endpoints. For example, in embodiments, the maximum CT can be in the range of 20 MPa to 400 MPa, 50 MPa to 350 MPa, 75 MPa to 300 MPa, 100 MPa to 250 MPa, or 150 MPa to 200 MPa, including and including any two of these values ​​as endpoints.

[0144] In embodiments, the DOC of region 120 and / or region 122 can range from 5 micrometers to 50 micrometers, including subranges. For example, the DOC can range from 10 micrometers to 50 micrometers, 15 micrometers to 50 micrometers, 20 micrometers to 50 micrometers, 25 micrometers to 50 micrometers, 30 micrometers to 50 micrometers, 35 micrometers to 50 micrometers, 40 micrometers to 50 micrometers, 5 micrometers to 45 micrometers, 5 micrometers to 40 micrometers, 5 micrometers to 35 micrometers, 5 micrometers to 30 micrometers, 5 micrometers to 25 micrometers, 5 micrometers to 20 micrometers, or 5 micrometers to 15 micrometers. In embodiments, the DOC can range from 5 micrometers to 30 micrometers. In embodiments, the DOC can range from 5 microns or more to 20 microns or less.

[0145] In embodiments, the DOC may be reported as a fraction of the thickness (t) of the glass article 100. For example, the glass article may have a depth of compression (DOC) of 5% (0.05t) or more and 20% (0.20t) or less of the thickness of the glass article, including subranges. For example, in embodiments, the DOC may be 10% or more and 20% or less of the thickness of the glass article, 15% or more and 20% or less of the thickness of the glass article, 5% or more and 15% or less of the thickness of the glass article, or 5% or more and 10% or less of the thickness of the glass article.

[0146] The thickness (t) of the glass article 100 is measured between surface 110 and surface 112. In embodiments, the thickness of the glass article 100 can be 4 millimeters (mm) or less. In embodiments, the thickness of the glass article 100 can range from 15 micrometers or more to 4 mm or less, including subranges. For example, in embodiments, the thickness of the glass article 100 can range from 20 micrometers to 4 mm, 30 micrometers to 4 mm, 40 micrometers to 4 mm, 50 micrometers to 4 mm, 60 micrometers to 4 mm, 70 micrometers to 4 mm, 80 micrometers to 4 mm, 90 micrometers to 4 mm, 1 mm to 4 mm, 15 micrometers to 3 mm, 15 micrometers to 2 mm, 15 micrometers to 1 mm, 15 micrometers to 500 micrometers, 15 micrometers to 400 micrometers, 15 micrometers to 300 micrometers, 15 micrometers to 200 micrometers, or 15 micrometers to 100 micrometers.

[0147] The compressive stress layer may be formed on the glass article by exposing the glass article to an ion exchange solution. In an embodiment, the ion exchange solution may include a molten potassium salt. In an embodiment, the ion exchange solution may include 50% or more, 60% or more, 70% or more, 80% or more, 90% or more, or 100% of the potassium salt by weight. For example, in an embodiment, the ion exchange solution may include 50% or more to 100% or less, 60% or more to 100% or less, 70% or more to 100% or less, 80% or more to 100% or less, or 90% or more to 100% or less, of the potassium salt by weight. In an embodiment, the potassium salt may be potassium nitrate (KNO3). In an embodiment, all or a portion of the remaining weight percent of the ion exchange solution may be a molten nitrate salt, such as sodium nitrate salt (NaNO3).

[0148] The glass article may be exposed to the ion exchange solution by immersing a glass article made from the glass composition in a bath of the ion exchange solution, spraying the ion exchange solution onto a glass article made from the glass composition, or otherwise physically applying the ion exchange solution to the glass article. The ion exchange solution when exposed to the glass article according to this embodiment is at a temperature of from 350° C. to 480° C., including subranges. For example, in embodiments, the temperature may be from 360° C. to 470° C., from 370° C. to 460° C., from 380° C. to 450° C., from 390° C. to 440° C., from 400° C. to 430° C., or from 410° C. to 420° C.

[0149] In embodiments, the glass article is exposed to the ion exchange solution for a duration of from 5 minutes to 24 hours, including subranges, For example, in embodiments, the duration can be from 5 minutes to 20 hours, from 5 minutes to 16 hours, from 5 minutes to 12 hours, from 5 minutes to 6 hours, from 5 minutes to 2 hours, from 5 minutes to 1 hour, or from 5 minutes to 30 minutes.

[0150] It should be understood that after the ion exchange process, the composition at the surface of the glass article may differ from the composition of the glass article (e.g., the glass article prior to the ion exchange process) as formed. This is a result of one type of alkali metal ion, e.g., Na+, being replaced with a larger alkali metal ion, e.g., K+, in the glass as formed. However, in embodiments, the glass composition at or near the center of the depth of the glass article may remain with the composition of the glass article as formed. Unless otherwise stated, the glass composition disclosed herein is the composition of the glass article near the center of the depth of the glass article, a composition that is not affected (or is minimally affected) by the ion exchange process, i.e., the composition of the glass article as formed.

[0151] The glass articles disclosed herein may be incorporated into other articles, such as display-bearing articles (or display articles) (e.g., consumer electronics including cell phones, watches, tablets, computers, navigation systems, etc.), architectural articles, transportation articles (e.g., automobiles, trains, aircraft, ships, etc.), household appliances, or any article that may benefit from some transparency, scratch resistance, abrasion resistance, or combinations thereof. Exemplary articles incorporating any of the glass articles disclosed herein are shown in Figures 3A and 3B. In particular, Figures 3A and 3B show a consumer electronics product 300 including a housing 302 having a front surface 304, a rear surface 306, and a side surface 308. The electrical components at least partially inside the housing or entirely within the housing may include at least a control unit 320, a memory 322, and a display 310 on or adjacent to the front surface 306 of the housing 302. The display 310 may be, for example, a light-emitting diode (LED) display or an organic light-emitting diode (OLED) display.

[0152] The cover substrate 312 may be disposed on or over the front surface 304 of the housing 302 so as to overlie the display 310. The cover substrate 312 may include any glass article disclosed herein and may be referred to as a "cover glass." The cover substrate 312 may serve to protect the display 310 and other components of the consumer electronics product 300 (e.g., the control 320 and the memory 322) from damage. In embodiments, the cover substrate 312 may be bonded to the display 310 with an adhesive. In embodiments, the cover substrate 312 may define all or a portion of the front surface 304 of the housing 302. In embodiments, the cover substrate 312 may define all or a portion of the front surface 304 of the housing 302 and all or a portion of the side surface 308 of the housing 302. In embodiments, the consumer electronics product 300 may include a cover substrate that defines all or a portion of the rear surface 306 of the housing 302. EXAMPLES

[0153] The embodiments are further illustrated by the following examples, which should not be construed as limiting the above embodiments.

[0154] Glass compositions made from the oxides listed in the following Tables 2A-2H were prepared by conventional glass forming methods. Compositions 1-50 (C1-C50) in Tables 2A-2H are glass compositions according to embodiments of the present application. In Tables 2A-2H, all oxide components are listed in mole percent.

[0155] Tables 3A-3J list the material properties of Compositions 1-50 (C1-C50) of Tables 2A-2H. The Young's Modulus (E) values ​​reported in Tables 3A-3J were measured by the method disclosed herein. The shear modulus values ​​were measured by a resonant ultrasonic spectroscopy technique of the general type set forth in ASTM E2001-13, entitled "Standard Guide for Resonant Ultrasound Spectroscopy for Defect Detection in Both Metallic and Non-Metallic Parts."

[0156] Additional material properties listed in Tables 3A-3J include density, where density values ​​are determined using the buoyancy method of ASTM C693-93(2013), low temperature CTE (ranging from 0°C to 300°C) measured in parts per million (ppm) per degree Celsius (ppm / °C), strain point, annealing point, and softening point, where strain point is determined using the beam bending viscosity method of ASTM C598-93(2013), annealing point is determined using the fiber draw method of ASTM C336-71(2015), softening point is determined using the fiber draw method of ASTM C338-93(2013), and further includes tensile strength, tensile modulus, and tensile strength, measured in parts per million (ppm) per degree Celsius (ppm / °C). 11 Poise, liquidus viscosity, which is specified as described herein, and further including the stress optical coefficient (SOC), which is related to the birefringence of the glass. Unless otherwise noted, SOC was measured by Procedure C (glass disk method) as set forth in ASTM Standard C770-16 entitled "Standard Test Method for Measurement of Glass Stress-Optical Coefficient", the contents of which are incorporated herein by reference in their entirety. Unless otherwise noted, the physical properties listed in Tables 3A-3J were measured before the composition or article was subjected to any ion exchange treatment or any other strengthening treatment. The CTE values ​​reported in Tables 3A-3J were measured using the fiber drawing method. The dilatometer was set up according to ASTM E228 ("Standard Test Method for Linear Thermal Expansion of Solid Materials With a Push-Rod Dilatometer"). For fiber stretch testing, fiber samples of a particular composition mounted in a dilatometer were placed in an ice bath at 0° C. and then in an isothermal oven at 300° C. to determine the average linear thermal expansion coefficient over that temperature range. Fiber samples were prepared in a flame run.

[0157] Tables 4A-4G include the ion exchange conditions and physical properties for compositions 1-48 (C1-C48) of Tables 2A-2G. For the ion exchange treatments reported in Tables 4A-4G, samples of each composition were immersed in a molten salt bath composed of 100% KNO3 by weight. Each sample had a length of 1 inch, a width of 1 inch, and a thickness of 0.8 mm. Composition A (CA) of Tables 4A-4G is a comparative composition containing 68.95 mol% SiO2, 10.27 mol% Al2O3, 5.36 mol% MgO, 0.06 mol% CaO, 15.20 Na2O, and 0.17 mol% SnO2.

[0158] As shown in Tables 4A-4G, all of compositions 1-48 (C1-C48) achieved a CS / E ratio of at least 15 at various DOCs. Except for C30-C36, which were not ion-exchanged for longer than 30 minutes, each composition achieved a CS / E ratio of at least 15 at a DOC of about 15 micrometers or greater. Graph 500 in FIG. 5 is a plot of CS / E ratio at a DOC of about 20 micrometers versus liquidus viscosity for various ion-exchanged glass compositions. The gray diamonds in graph 500 represent various compositions from Tables 2A-2H that had DOC values ​​in the range of 20±5 micrometers, taken from the DOC values ​​reported in Tables 4A-4F. Graph 500 shows that the majority of compositions had a CS / E ratio of at least 15 and a liquidus viscosity greater than 500° C.

[0159] [Table 2A]

[0160] [Table 2B]

[0161] [Table 2C]

[0162]

Table 2D

[0163]

Table 2E

[0164]

Table 2F

[0165]

Table 2G

[0166]

Table 2H

[0167]

Table 3A

[0168]

Table 3B

[0169]

Table 3C

[0170]

Table 3D

[0171]

Table 3E

[0172]

Table 3F

[0173]

Table 3G

[0174]

Table 3H

[0175]

Table 3I

[0176]

Table 3J

[0177]

Table 4A

[0178]

Table 4B

[0179]

Table 4C

[0180]

Table 4D

[0181]

Table 4E

[0182] [Table 4F]

[0183] [Table 4G]

[0184] Various embodiments have been described herein by way of example and not limitation. It will be apparent that adaptations and modifications of the disclosed embodiments are intended to be within the meaning and range of equivalents of those embodiments, based on the teaching and guidance provided herein. Thus, it will be apparent to one skilled in the art that various changes in form and detail can be made to the embodiments disclosed herein without departing from the spirit and scope of the disclosure. The elements of the embodiments described herein are not necessarily mutually exclusive and may be interchanged to address various situations, as will be appreciated by those skilled in the art.

[0185] Aspects of the present disclosure are described in detail with respect to the aspects illustrated in the accompanying drawings, in which like reference numerals are used to indicate identical or functionally similar elements. Reference to "aspects" or "aspects" indicates that the described aspects may include a particular feature, structure, or characteristic, but not all aspects may include that particular feature, structure, or characteristic. Moreover, such terms do not necessarily refer to the same aspect. Furthermore, when a particular feature, structure, or characteristic is described in the context of one aspect, it is submitted that it is within the knowledge of one of ordinary skill in the art to affect such feature, structure, or characteristic in the context of other aspects, whether or not expressly stated.

[0186] The examples are illustrative only and are not intended to limit the disclosure. Other suitable modifications and adaptations of the variety of conditions and parameters normally encountered in the art and obvious to those skilled in the art are within the spirit and scope of the disclosure.

[0187] In describing an element or component, the indefinite article as used in the original English means that there is one or more of that element or component. Generally, these articles are used to mean that the modified noun is singular, but as used herein, they also include plural, unless otherwise stated in specific instances. Similarly, the definite article as used in the original English also indicates that the modified noun as used herein may be singular or plural, unless otherwise stated in specific instances.

[0188] As used herein, directional terms, such as up, down, right, left, front, back, top, bottom, inward, outward, refer to the drawings as illustrated and are not intended to imply absolute orientations.

[0189] The term "comprising" as used in the claims is an open-ended transitional phrase. The elements listed after the transitional phrase "comprising" are a non-exclusive list, and elements in addition to the elements specifically listed may be present. As used in the claims, the terms "consisting essentially of" or "consisting essentially of" limit the composition of the material to the specified materials and to materials that do not materially affect the basic and novel characteristics of the material. As used in the claims, the terms "consisting of" or "completely consisting of" limit the composition of the material to the specified materials and exclude any unspecified materials.

[0190] When a range of values, including upper and lower limits, is described herein, it is intended to include the endpoints of the range, and all integers and fractions within the range, unless otherwise stated in specific circumstances. It is not intended that the scope of the claims be limited to the specific values ​​described in defining the range. Furthermore, when an amount, concentration, or other value or parameter is described as a range, one or more preferred ranges, or a list of upper and lower preferred values, it should be understood that any range formed from any pair of any upper range or preferred value and any lower range or preferred value is specifically described, regardless of whether such pairs are separately disclosed. Finally, when the term "about" is used to describe a value or range endpoint, the disclosure should be understood to include that specific value or endpoint. Regardless of whether a value or range endpoint is described as "about," it is intended that the value or range endpoint includes two aspects, namely, both those modified by "about" and those not modified by "about."

[0191] As used herein, the term "about" means that amounts, sizes, formulations, parameters, and other quantities and characteristics may not be exact, or need not be exact, but may be approximate and / or may be larger or smaller as desired to reflect tolerances, conversion factors, rounding, measurement error, and the like, as well as other factors known to those of ordinary skill in the art.

[0192] It should be understood that the phraseology and terminology used herein is for the purpose of description and not of limitation. The breadth and scope of the present disclosure should not be limited by any of the above exemplary embodiments, but should be defined by the following claims and their equivalents.

[0193] Preferred embodiments of the present invention will be described below in detail.

[0194] EMBODIMENT 1 In an ion-exchanged alkali aluminosilicate glass article, 55 mol% or more of SiO2; 12.5 mol% or more and 16.0 mol% or less of Al2O3; 1 mol% or more and 3.88 mol% or less of MgO; 0.78 mol% or more and 3 mol% or less of CaO; NaO and Including, % by mole of Al2O3 + % by mole of RO ≥ 17 mol%; mol% RO=mol% MgO+mol% CaO; The glass article is substantially free of ZnO, SrO, BaO, B2O3, P2O5, Li2O, and K2O.

[0195] EMBODIMENT 2 The glass article comprises: Young's modulus measured in GPa before ion exchange, a compressive stress layer extending from the surface of the glass article to a compression depth and having a peak compressive stress value measured in MPa; Including, 2. The ion-exchanged alkali aluminosilicate glass article of claim 1, wherein the ratio of the peak compressive stress value to the Young's modulus value is 15 or greater.

[0196] EMBODIMENT 3 3. The ion-exchanged alkali aluminosilicate glass article of claim 2, wherein the ratio of the peak compressive stress value to the Young's modulus value is from 15 or more to 18 or less.

[0197] EMBODIMENT 4 4. The ion-exchanged alkali aluminosilicate glass article of claim 2 or 3, wherein the Young's modulus value is in the range of 70 MPa or more and 80 MPa or less.

[0198] EMBODIMENT 5 5. The ion-exchanged alkali aluminosilicate glass article of any one of claims 2 to 4, wherein the peak compressive stress value is in the range of from 500 MPa or more to 1300 MPa or less.

[0199] EMBODIMENT 6 6. The ion-exchanged alkali aluminosilicate glass article of any one of claims 2 to 5, wherein the compression depth ranges from 5 micrometers to 30 micrometers.

[0200] EMBODIMENT 7 7. The ion-exchanged alkali aluminosilicate glass article of any one of claims 2 to 6, wherein the compression depth ranges from 5% to 20% of the thickness of the glass article.

[0201] EMBODIMENT 8 8. The ion-exchanged alkali aluminosilicate glass article of any one of the preceding claims, wherein the mol% NaO+mol% RO > 20 mol%.

[0202] EMBODIMENT 9 9. The ion-exchanged alkali aluminosilicate glass article of any one of the preceding claims, wherein (mol % NaO+mol % RO-mol % AlO)≧4 mol %.

[0203] EMBODIMENT 10 9. The ion-exchanged alkali aluminosilicate glass article of any one of the preceding claims, wherein 11 mol% > (mol% NaO + mol% RO - mol% AlO) > 4 mol%.

[0204] EMBODIMENT 11 11. The ion-exchanged alkali aluminosilicate glass article of any one of the preceding claims, wherein 21 mol% > mol% Al2O3 + mol% RO > 17 mol%.

[0205] EMBODIMENT 12 12. The ion-exchanged alkali aluminosilicate glass article of any one of the preceding claims, wherein 37 mol% > mol% Al2O3 + mol% Na2O > 28 mol%.

[0206] EMBODIMENT 13 13. The ion-exchanged alkali aluminosilicate glass article of any one of the preceding claims, wherein (mol% MgO / (mol% MgO+mol% CaO) > 0.5.

[0207] EMBODIMENT 14 13. The ion-exchanged alkali aluminosilicate glass article of any one of the preceding claims, wherein 0.8 > (mol % MgO / (mol % MgO+mol % CaO) > 0.5.

[0208] EMBODIMENT 15 1.92 mol% or more and 3.88 mol% or less of MgO, 15. The ion-exchanged alkali aluminosilicate glass article of any one of the preceding claims, comprising:

[0209] EMBODIMENT 16 0.78 mol% or more and 2.52 mol% or less of CaO, 16. The ion-exchanged alkali aluminosilicate glass article of any one of the preceding claims, comprising:

[0210] EMBODIMENT 17 SiO2 of 59 mol% or more and 66 mol% or less; 16 mol% or more and 21 mol% or less of Na2O 17. The ion-exchanged alkali aluminosilicate glass article of any one of the preceding claims, comprising:

[0211] EMBODIMENT 18 64 mol% or more and 66 mol% or less of SiO2; 13 mol% or more and 15 mol% or less of Al2O3; 2 mol% or more and 3.88 mol% or less of MgO; 0.78 mol% or more and 2 mol% or less of CaO; 15.5 mol% or more and 17.5 mol% or less of Na2O 15. The ion-exchanged alkali aluminosilicate glass article of any one of the preceding claims, comprising:

[0212] EMBODIMENT 19 SiO2 of 59.6 mol% or more and 65.5 mol% or less; 12.78 mol% or more and 15.96 mol% or less of Al2O3; 1.92 mol% or more and 3.88 mol% or less of MgO; 0.78 mol% or more and 2.52 mol% or less of CaO; 16.09 mol% or more and 20.2 mol% or less of Na2O; 15. The ion-exchanged alkali aluminosilicate glass article of any one of the preceding claims, comprising:

[0213] EMBODIMENT 20 20. The ion-exchanged alkali aluminosilicate glass article of any one of the preceding claims, having a thickness of 4 millimeters or less.

[0214] EMBODIMENT 21 20. The ion-exchanged alkali aluminosilicate glass article of any one of the preceding claims, having a thickness ranging from 15 micrometers to 300 micrometers inclusive.

[0215] EMBODIMENT 22 22. The ion-exchanged alkali aluminosilicate glass article of any one of the preceding claims, having a liquidus viscosity in the range of from 500 kP or more to 2300 kP or less, measured before being ion-exchanged.

[0216] EMBODIMENT 23 A compressive stress layer extending from the surface of the glass article to a compression depth and having a peak compressive stress value in the range of 500 MPa or more to 1300 MPa or less, 23. The ion-exchanged alkali aluminosilicate glass article of any one of claims 1 or 8 to 22, comprising:

[0217] EMBODIMENT 24 In an electronic device, An electronic display; The glass article according to any one of claims 1 to 23 disposed over the electronic display; and An electronic device comprising:

[0218] EMBODIMENT 25 a housing having a front surface, a rear surface, and a side surface; electrical components at least partially disposed within the housing, including a controller, memory, and an electronic display on or adjacent to the front surface of the housing; Further comprising: 25. The electronic device of claim 24, wherein the glass article forms at least a portion of the housing.

[0219] EMBODIMENT 26 In an ion-exchanged alkali aluminosilicate glass article, SiO2 of 59 mol% or more and 66 mol% or less; 12.5 mol% or more and 16.0 mol% or less of Al2O3; 1 mol% or more and 3.88 mol% or less of MgO; 0.78 mol% or more and 3 mol% or less of CaO; 16 mol% or more and 21 mol% or less of Na2O; the Young's modulus value measured in GPa of the glass article before ion exchange; a compressive stress layer extending from a surface of the ion exchanged glass article and having a peak compressive stress value measured in MPa; Including, mol% of Al2O3+mol% of RO≧17 mol%, mol% RO=mol% MgO+mol% CaO; It is substantially free of ZnO, SrO, BaO, B2O3, P2O5, Li2O, and K2O, A glass article having a ratio of the peak compressive stress value to the Young's modulus value of 15 or more and 18 or less.

[0220] EMBODIMENT 27 In an ion-exchanged alkali aluminosilicate glass article, 55 mol% or more of SiO2; 12.5 mol% or more and 16 mol% or less of Al2O3; 1 mol% or more and 4 mol% or less of MgO; 0.5 mol% or more and 3 mol% or less of CaO; NaO and Including, % by mole of Al2O3 + % by mole of RO ≥ 17 mol%; mol% RO=mol% MgO+mol% CaO; A glass article that is substantially free of ZnO, SrO, BaO, B2O3, P2O5, Li2O, and K2O.

[0221] EMBODIMENT 28 Young's modulus measured in GPa before ion exchange, a compressive stress layer extending from the surface of the glass article to a compression depth and having a peak compressive stress value measured in MPa; Including, 28. The ion-exchanged alkali aluminosilicate glass article of claim 27, wherein the ratio of the peak compressive stress value to the Young's modulus value is 15 or greater. [Explanation of symbols]

[0222] 100 Glass items 110, 112 surface 120, 122 Compressive stress region 130 Central area DOC, d1, d2 compression depth

Claims

1. In an ion-exchanged alkali aluminosilicate glass article, 55 mol% or more of SiO 2 and, 12.5 mol% or more and 16.0 mol% or less of Al 2 O 3 and, 1 mol % or more and 3.88 mol % or less of MgO; 0.78 mol% or more and 3 mol% or less of CaO; Na 2 Oと Including, A 2 O 3 and the mol% of RO is ≧17 mol%; mol% RO=mol% MgO+mol% CaO; The glass article contains ZnO, SrO, BaO, B 2 O 3 , P 2 O 5 , Li 2 O and K 2 A glass article that is substantially free of O.

2. The glass article comprises: the Young's modulus measured in GPa before being ion-exchanged; a compressive stress layer extending from the surface of the glass article to a compression depth and having a peak compressive stress value measured in MPa; Including, 2. The ion-exchanged alkali aluminosilicate glass article of claim 1, wherein the ratio of the peak compressive stress value to the Young's modulus value is 15 or greater.

3. 3. The ion-exchanged alkali aluminosilicate glass article of claim 2, wherein the ratio of the peak compressive stress value to the Young's modulus value is from 15 or more to 18 or less.

4. 3. The ion-exchanged alkali aluminosilicate glass article of claim 2, wherein the Young's modulus value is in the range of from 70 MPa or more to 80 MPa or less.

5. 3. The ion-exchanged alkali aluminosilicate glass article of claim 2, wherein the peak compressive stress value is in the range of from 500 MPa or more to 1300 MPa or less.

6. 3. The ion-exchanged alkali aluminosilicate glass article of claim 2, wherein the compression depth ranges from 5 micrometers to 30 micrometers.

7. 3. The ion-exchanged alkali aluminosilicate glass article of claim 2, wherein the compression depth ranges from 5% to 20% of the thickness of the glass article.

8. Na 2 8. The ion-exchanged alkali aluminosilicate glass article of any one of claims 1 to 7, wherein mol% O + mol% RO > 20 mol%.

9. (Na 2 mol% of O+mol% of RO-Al 2 O 3 8. The ion-exchanged alkali aluminosilicate glass article of claim 1 , wherein the cation exchange ratio (A) of the cation exchanger is 0.01 to 0.

01.

10. 21 mol% ≧ Al 2 O 3 8. The ion-exchanged alkali aluminosilicate glass article of claim 1, wherein the mol % of R+the mol % of RO > 17 mol %.

11. 37 mol% or more Al 2 O 3 % by mole + Na 2 8. The ion-exchanged alkali aluminosilicate glass article of any one of claims 1 to 7, wherein the mol% of O > 28 mol%.

12. 8. The ion-exchanged alkali aluminosilicate glass article of any one of claims 1 to 7, wherein (mol % MgO / (mol % MgO+mol % CaO) > 0.

5.

13. 8. The ion-exchanged alkali aluminosilicate glass article of any one of claims 1 to 7, having a thickness in the range of from 15 micrometers or more to 300 micrometers or less.

14. 8. The ion-exchanged alkali aluminosilicate glass article of claim 1 having a liquidus viscosity in the range of from 500 kP or more to 2300 kP or less, measured before being ion-exchanged.

15. A compressive stress layer extending from the surface of the glass article to a compression depth and having a peak compressive stress value in the range of 500 MPa or more to 1300 MPa or less, The ion-exchanged alkali aluminosilicate glass article of any one of claims 1 to 7, comprising:

Citation Information

Patent Citations

  • Aluminosilicate glass, aluminosilicate glass reinforcing method and reinforced aluminosilicate glass

    CN104591538A

  • Strengthened glass, strengthened glass plate and glass for strengthening

    JP2014073952A

  • Strengthened glass, and glass for strengthening

    JP2015042607A

  • Low-modulus ion-exchangeable glasses

    US20210179482A1

  • Glass plate for chemical tempering and method for producing chemically tempered glass plate

    WO2018124084A1