CVD single crystal diamond

The method addresses the challenge of producing high-quality, uniform CVD single crystal diamonds by controlling growth conditions and annealing processes, achieving high yield and reduced cracking for quantum and gemstone applications.

JP2024538212AActive Publication Date: 2024-10-18ELEMENT SIX TECH LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024523807
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-19
Filing Date
2022-10-19
Publication Date
2024-10-18
Estimated Expiration
2042-10-19

AI Technical Summary

Technical Problem

Existing methods struggle to produce large quantities of high-quality, uniform CVD single crystal diamond with controlled nitrogen vacancy centers for applications like quantum technology and fancy colored gemstones, often facing issues with cracking, twinning, and non-uniformity in crystal morphology and impurity distribution.

Method used

A method involving controlled growth conditions using specific gas ratios and annealing processes to achieve CVD single crystal diamonds with targeted nitrogen vacancy centers, low birefringence, and uniform properties, including concentrations of NV centers and low silicon impurities, through a continuous growth cycle.

Benefits of technology

Enables the production of large quantities of CVD single crystal diamonds with predictable properties, high yield, and reduced cracking, suitable for quantum applications and fancy colored gemstones, with enhanced growth rates and uniformity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024538212000001_ABST
    Figure 2024538212000001_ABST
Patent Text Reader

Abstract

A single substituted nitrogen atom, N, in the neutral charge state as measured by EPR s 0 CVD single crystal diamond with a concentration of 0.25 to 3 ppm, and nitrogen vacancy centers (NV 0 and N.V. - ) is the total concentration of N s 0 CVD single crystal diamond, with a concentration of 0.1 to 0.8 times that of
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to CVD single crystal diamond and a method for making CVD single crystal diamond. [Background technology]

[0002] In the 1980s and 90s, many experiments directed to the synthesis of single crystal CVD diamond material were carried out by various groups around the world. Much of this work disclosed the growth of thin layers of single crystal CVD diamond material on single crystal diamond substrates by homoepitaxial growth. Although there was a desire to produce relatively thick layers of high quality single crystal CVD synthetic diamond material, it proved difficult to achieve in practice. The synthesis of single crystal CVD diamond material requires extreme conditions. In order to successfully grow thick layers of high quality single crystal CVD synthetic diamond material, these conditions must be generated and then maintained stably over long periods of time. Furthermore, the properties of the diamond material synthesized are influenced by a number of synthesis parameters that form a complex multi-dimensional synthesis parameter space. Only a small range of this multi-dimensional synthesis parameter space can achieve thick layers of high quality single crystal CVD diamond material. Finding these synthesis regions and developing methods to generate the correct combination of parameters required to produce and maintain stable growth within one of these synthesis regions is by no means trivial. The synthesis parameters important for single crystal CVD diamond growth include the substrate type (e.g., whether produced by CVD, high pressure / high temperature, or natural geosynthetic), the method of preparing the substrate from the original host crystal, the substrate geometry (including the crystal orientation of the faces and / or edges), the substrate temperature during growth and thermal management of the growing crystal, and the gas-phase synthesis environment itself. The latter are influenced by the process gas composition (including impurities), the gas pressure in the process chamber, and the amount of microwave power supplied to the synthesis process, in addition to various equipment-dependent factors such as the size of the process chamber, the process gas inlet / outlet geometry, and the process gas flow rates. For a suitable growth region, many of these parameters are interrelated such that changing one parameter will change the other parameters correctly. Failure to select and maintain suitable process conditions for the entire deposition region throughout the duration of the synthesis process can result in high levels of uncontrolled process variability, unusable products with inappropriate material properties, and even complete destruction of the crystal due to catastrophic cracking, twinning, or graphitization.

[0003] It is known to intentionally add defects in the form of dopants. Nitrogen is one of the most important dopants in the synthesis of CVD diamond materials, since it has been found that providing nitrogen to the CVD process gas can increase the growth rate of the material and also affect the formation of crystal defects such as dislocations. Thus, nitrogen doping of single crystal CVD synthetic diamond materials has been extensively explored and reported in the literature. For some applications, such as electronic applications, it has proven advantageous to develop techniques to intentionally exclude nitrogen from the CVD process gas. However, for other applications, substantial levels of nitrogen doping can provide advantageous properties and / or can be useful in achieving the growth of thick layers of CVD synthetic diamond materials. Patent literature relating to such nitrogen-doped single crystal CVD synthetic diamond materials includes WO 2003 / 052177. Native diamond material has an indirect band gap of 5.5 eV and is transparent in the visible portion of the spectrum. By introducing defects, or color centers, with associated energy levels within the band gap, diamond exhibits a unique color depending on the type and concentration of the color center. This color can be due to either absorption or photoluminescence, or some combination of the two. Generally, absorption is the dominant factor. One example of a common color center present in synthetic diamond material is nitrogen. When nitrogen is in a substitutional lattice site in its neutral charge state, it has an associated energy level of 1.7 eV below the conduction band which causes absorption at the blue end of the visible spectrum, and alone diamond has a unique yellow color. When the nitrogen atom is in a substitutional lattice site in its neutral charge state, N s 0 defects, and their concentration is [N s 0 ] is indicated.

[0004] For example, according to WO 2010 / 149775, monosubstituted nitrogen N s 0 It is known that irradiation and annealing of CVD diamond material containing can produce pink colored diamonds. The term "fancy color diamond" is an established gem trade classification and is used to refer to unusually colored diamonds. Examples of synthetic and natural diamonds with fancy colors are known in the art, which are created by introducing color centers into diamond. For example, EP-A-0615954 and EP-A-0316856 describe irradiating synthetic diamond material with an electron beam or neutron beam to form lattice defects (interstitial atoms and vacancies) in the crystal. The diamond crystal is then annealed at a predetermined temperature range to form color centers. One color center described is a substitutional nitrogen atom adjacent to a vacancy called "NV center", which can give the diamond material a desired fancy color, such as purple (as described in EP-A-0316856) or red / pink (as described in EP-A-0615954). Not only are NV centers useful for imparting pink color to diamonds, but they also have many important applications in other fields. NV centers are being investigated for use in various imaging, sensing and processing applications, including, for example, luminescence tags; magnetic sensors; spin resonance devices such as nuclear magnetic resonance (NMR) and electron spin resonance (ESR) devices; spin resonance imaging devices for magnetic resonance imaging (MRI); quantum information processing devices such as for quantum communication and computing; magnetic communication devices; and gyroscopes. NV centers have attracted interest as useful quantum spin defects because they have several desirable characteristics: (i) its electron spin state can be coherently manipulated with high fidelity and has extremely long coherence times (transverse relaxation times T and / or T * can be used to quantify and compare; (ii) its electronic structure allows the defect to be optically injected into its electronic ground state and places such defects into specific electronic spin states even at non-cryogenic temperatures, thereby eliminating the need for expensive and bulky cryogenic cooling equipment for certain applications where miniaturization is desired. Furthermore, the defect can act as a source of photons that all have the same spin state; and (iii) Its electronic structure contains luminescent and non-luminescent electron spin states, and the electron spin state of the defect can be read out by photons. This is useful for reading out information from synthetic diamond materials used in sensing applications such as magnetometry, spin resonance spectroscopy and imaging. Furthermore, it is a key ingredient for using NV-defects as qubits for long-distance quantum communication and scalable quantum computing. These results make the NV-defect a competitive candidate for solid-state quantum information processing (QIP).

[0005] Multiple single crystal CVD synthetic diamonds can be produced in a single CVD growth cycle or run (meaning a single uninterrupted growth operation in a CVD reactor) by providing multiple single crystal diamond substrates on a substrate carrier, introducing process gases, and forming a plasma to deposit carbon on the substrates and grow diamonds. The problem with this approach to synthesizing multiple single crystal CVD diamonds is that of uniformity and yield. Non-uniformity can exist in terms of crystal morphology, growth rate, cracking, and impurity content and distribution. For example, as described in WO 2013 / 087697, even with careful control of the CVD diamond growth chemistry, non-uniform incorporation of impurities can occur due to temperature variations at the growth surface that affect the impurity incorporation rate. Temperature variations also cause variations in crystal morphology, growth rate, and cracking issues. These temperature variations can be transverse (spatially distributed) to the growth direction at certain points in the growth run, or parallel (temporally distributed) to the growth direction due to temperature variations over the duration of the growth run. Variations can occur within a single CVD diamond crystal, and also between crystals when multiple crystals are provided to the synthesis process. Thus, in many crystal synthesis processes, only a portion of the product diamond crystals from a single growth run may meet the desired specifications.

[0006] There is little prior art that describes either growing multiple CVD single crystal diamonds or the resulting distribution of properties (hardness and other) among the diamonds. The conditions required to grow multiple single crystal diamonds with desirable properties for specific applications in high yields are still largely unknown. Considerations regarding uniformity in a region are known in terms of polycrystalline diamond wafers or thin films, but nothing disclosed in this regard has anything to do with the requirement to grow multiple relatively large, substantially separated single crystal diamonds. Summary of the Invention

[0007] It is an object of the present invention to provide a method for synthesizing CVD single crystal diamond that produces large quantities of CVD single crystal diamond having a uniform concentration of NV centres for desired applications such as quantum applications or pink gemstones.

[0008] According to a first embodiment, a single substituted nitrogen atom N in a neutral charge state as measured by EPR is provided. s 0 The present invention provides a CVD single crystal diamond having a nitrogen vacancy center (NV ) in a neutral and negative charge state. 0 and N.V. - ) is the total concentration of N s 0 It is 0.1 to 0.8 times the concentration. Optionally, the CVD single crystal diamond has at least one linear dimension of 3.5mm or greater. As an option, CVD single crystal diamonds can be manufactured with a hue angle selected from -45 to 45°, -10 to 40° and 10 to 40°. ab has. CVD single crystal diamond is arbitrarily measured using an excitation wavelength of 660 nm at a temperature of 77 K, and the ratio of SiV to the peak area of ​​the primary Raman signal of diamond in photoluminescence measurements is - SiV, quantified by the ratio of the total peak areas of the zero phonon line, selected from the group consisting of less than 0.5; less than 0.1; less than 0.05; and less than 0.01. -Such values ​​indicate diamond material with very little silicon impurities. CVD single crystal diamond has low optical birefringence, optionally exhibiting low strain at a temperature of 20°C, and has a third quartile value of the refractive index difference for light polarized parallel to the slow and fast axes, averaged over the thickness of the sample, of 1×10 when measured over an area of ​​at least 3 mm × 3 mm. -4 and 5 x 10 -5 These low birefringence values ​​are indicative of a sample suitable for producing a single crystal CVD diamond that does not have "grain" that could otherwise affect its perceived clarity.

[0009] Alternatively, the total volume of the single crystal CVD diamond material is at least 0.1mm 2 , at least 1 mm 2 , at least 10 mm 2 , at least 20 mm 2 , at least 40mm 3 , at least 60mm 3 , at least 80mm 3 and at least 100 mm 3 The above formula is selected from the following formula: The CVD single crystal diamond is optionally gem-like and has a saturation C selected from any of 5 to 40, 10 to 35, and 15 to 30. * ab has. The resulting diamond is used in applications that exploit the spin nature of the NV centers, but in any CVD single crystal diamond, the measured inhomogeneous dephasing time T of the ensemble NVs is 2 * is more than 5 μs. The CVD single crystal diamond is optionally gem-like and has a color grade selected from any of Fancy Light, Fancy, Fancy Intense, Fancy Vivid and Fancy Deep, along with any of pinkish orange, orange-pink, pink, purplish pink, purple-pink and pink-purple, according to the Gemological Institute of America (GIA) scale and method. CVD single crystal diamonds are optionally gem-like and are graded according to the Gemological Institute of America (GIA) scale and methodology and are VS 2 , V.S. 1 , V.V.S. 2 , V.V.S. 1 The clarity grades are selected from the group consisting of IF, IF and FL. These clarity grades correspond to samples that are free of or have clarity defects. However, they can only be observed under magnification and are not visible to the naked eye. Some embodiments of the present invention provide single crystal diamonds that would normally fit into one of these grades, and gemstones formed therefrom can be sold, including but not limited to, as commercial or high-quality products.

[0010] CVD single crystal diamond is optionally classified as H3, NVN 0 Upon heat treatment, H3 centers can be formed within the disclosed materials. Alternatively, CVD single crystal diamond should have a minimum of 50 (NV) in photoluminescence measurements performed at 77K using an excitation wavelength of 455 to 459 nm. 0 +NV - ) / H3 ratio. NV 0 , N.V. - and H3 defects are quantified by the peak area ratio of the zero phonon line to the primary Raman signal of diamond. The CVD single crystal diamond is optionally selected from any of at least 100, at least 150, at least 200, at least 300 and at least 400 (NV 0 +NV - ) / H3 ratio.

[0011] According to a second aspect, there is provided a method of making a plurality of single crystal CVD diamonds as described above in the first aspect, the method comprising: placing a plurality of single crystal diamond substrates on a substrate carrier in a chemical vapor deposition reactor; Supplying a process gas to the reactor, the process gas comprising a hydrogen-containing gas, a carbon-containing gas and a nitrogen-containing gas, the relative amount of the process gas being 1% to 4% C 2 H 2 / H 2 ratio, and 30 ppm to 300 ppm N 2 / C 2 H 2 and supplying a ratio that is stoichiometrically equal to; growing a plurality of single crystal CVD diamonds on at least some surfaces of the plurality of single crystal diamond substrates at a temperature of 750°C to 1000°C; first annealing at least a portion of the resulting plurality of single crystal CVD diamonds at a temperature of 1500°C to 1800°C; irradiating a plurality of single crystal CVD diamonds to form vacancies in the diamond crystal lattice; and second annealing the resulting plurality of single crystal CVD diamonds at a temperature of 700°C to 1100°C.

[0012] The relative amounts of the process gas are optionally selected from any of 50 to 200 ppm, 60 to 180 ppm, and 70 to 150 ppm N 2 / C 2 H 2 The ratio is selected to be stoichiometrically equal. The relative amount of the process gas is optionally selected from any of 1 to 3%, 1.5 to 2.5%, and 1.5 to 2% C 2 H 2 / H 2 The ratio is selected to be stoichiometrically equal. Alternatively, the first annealing is carried out at a temperature of 1550°C to 1750°C. Optionally, the first annealing is carried out under diamond stabilizing pressure, which allows for the use of higher temperatures and / or longer annealing times without any loss or damage of the CVD single crystal material due to graphitization. The irradiation is optionally electron irradiation carried out with an electron energy of 1 MeV to 10 MeV. The second annealing optionally includes annealing at a temperature range selected from any of 700 to 1000°C, 800 to 1000°C, and 850 to 950°C. Optionally, the method further comprises cutting and polishing at least one of the plurality of single crystal diamonds to form a gemstone. Optionally, growth on the substrate is carried out uninterrupted as a single CVD synthesis cycle. Optionally, the process of growing a plurality of single crystal CVD diamonds comprises growing a diamond layer of at least 10 mm 3 / h, at least 20mm 3 / h, at least 30mm 3 / h, at least 40mm 3 / h and at least 50 mm 3 / h. The multiple CVD single crystal diamonds are optionally grown at a temperature selected from any of: 800°C to 1000°C; 800°C to 950°C; and 800°C to 900°C.

[0013] According to a third aspect, there is provided a device comprising a CVD single crystal diamond as defined above in the first aspect, the device being selected from any of an imaging device, a sensing device, a magnetic sensor; a spin resonance device, a quantum information processing device and a gyroscope device.

[0014] The invention will now be described in more detail by way of example with reference to the accompanying drawings, in which: FIG. [Brief description of the drawings]

[0015] [Figure 1] FIG. 1 is a flow chart showing exemplary steps for making CVD single crystal diamond. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The present inventors have developed a mass-manufacturable lab-grown diamond gemstone product. The present invention produces dozens of pieces of single crystal diamond material in a single run with predictable properties, such as the concentration of NV centers. For example, these properties are such that when cut and polished into round brilliant lab-grown gemstones, the diamonds will have a high yield and have a pink or related GIA color grade. The conditions developed by the inventors provide diamond material with a relatively high growth rate and low internal strain, resulting in a high yield of diamond with less cracking. This is in part due to the use of a substrate with few surface defects, such as etch puts, which would otherwise occur as nucleation points for a group of extended defects, increasing strain as described in WO2004 / 046427. A preferred method for achieving this is to use a vertically cut substrate, as described in WO2004 / 027123, the contents of which are incorporated herein by reference. In this disclosure, a method for producing a single crystal diamond plate is described, which includes the steps of providing a diamond substrate with a surface that is substantially free of surface defects, growing diamond homoepitaxially on the surface by chemical vapor deposition (CVD), and cutting the homoepitaxial CVD grown diamond and substrate transversely, usually perpendicular (i.e., 90° or nearly 90°) to the surface of the substrate on which diamond growth occurs, to produce a single crystal CVD diamond plate. This single crystal diamond plate is then used as a substrate for further growth. Since extended defects tend to follow the growth direction, slicing the diamond perpendicular to the growth direction ensures that the new slicing faces have a very low surface defect concentration.

[0017] An additional problem when attempting to grow lab-grown gem stones in large quantities is the perceived color non-uniformity of diamonds. Process conditions that provide perceptibly uniform color within a given gemstone, and between different gemstones produced to nominally common specifications, are desirable. As mentioned above, the presence of nitrogen can result in a yellow color. Furthermore, CVD single crystal materials grown with significant nitrogen additions usually contain vacancy complexes (e.g., clusters and chains) that grow quickly and result in a brown hue. This brown color can be reduced or eliminated by heat treating the diamond, as described in WO 2004 / 022821, the contents of which are incorporated herein by reference. This document describes heating the diamond at diamond stabilizing pressures, temperatures above 1400°C. This is known as high pressure / high temperature (HPHT) annealing. To create a sufficient number of NV centers capable of producing the pink coloration, an irradiation step is typically carried out prior to annealing to incorporate more vacancies into the diamond lattice than the relatively small number that are typically incorporated during growth. Upon subsequent annealing, the vacancies can migrate to nitrogen in the diamond crystal lattice and form NV centers. Nitrogen can be incorporated into the diamond crystal lattice in a number of different ways. Some important methods are: Single substituted nitrogen (N s 0 ) is a single nitrogen atom substituting for a carbon atom in the diamond lattice. -1 (0.140 eV) and typically has a brown color. Negatively charged nitrogen vacancy center (NV - NV) is a defect in which vacancies and substitutional nitrogen form pairs in the crystal lattice resulting in an overall negative charge state. - It exhibits an absorption line at 637 nm (1.945 eV) and related bands, and is usually pink or purple in color. The H3 center is in a globally neutral charge state (NVN). 0H3 consists of two substitutional nitrogen atoms separated by a vacancy at 503.2 nm (2.463 eV). H3 exhibits an absorption line at 503.2 nm (2.463 eV) and related bands, giving it a yellow color. EXAMPLES

[0018] A plurality of single crystal diamond substrates were obtained using plates of cross-cut CVD single crystal diamond as described in WO 2004 / 027123. These were mounted on a carrier and placed in a CVD reactor. A process gas was supplied to the CVD reactor. The process gas included hydrogen, a carbon-containing gas (methane in this example) and a nitrogen-containing gas (molecular nitrogen herein). A plasma of the process gas was formed in the reactor and single crystal CVD diamond material was grown on the surface of each of the plurality of single crystal diamond substrates to a thickness of 4 to 6 mm. The resulting single crystal diamond was then annealed at a pressure above 6 GPa and a temperature of 1550°C to 1750°C to ensure it was in the diamond stability field. Prior to annealing, any polycrystalline material was removed, along with surface cracks and defects, which would otherwise increase the risk of failure during annealing. The annealing temperature was maintained between 1550°C and 1750°C for the selected time to maximize NV retention and avoid H3 formation. This maximizes the pink color resulting from the NV centers and slight yellow color from the H3 centers. Below a temperature of 1750°C, the NV centers are largely immobile but the vacancies are mobile, resulting in a low tendency to form H3 centers. After the first (HPHT) annealing, the single crystal diamond was electron irradiated using electron energies between 1 MeV and 10 MeV and then annealed again, this time at temperatures between 700 and 1000°C to form NV centers. Due to the lower temperatures required for the second annealing, it does not need to be performed under diamond stabilization pressure, and in this example was performed in a vacuum furnace. The resulting single crystal diamonds were cut and polished to form round brilliant gemstones with GIA fancy color grades of either "Fancy Intense Orange-Pink" or "Fancy Vivid Pink", depending on the exact synthesis and processing conditions. Note that the gemstones can be cut to contain the substrate, which reduces the time required to grow the diamond. It is particularly favorable if the substrate is made using the same process as the final diamond, resulting in no visible discontinuities.

[0019] Quantitative measurement of finished gemstone color is difficult due to specularity, multiple internal reflections, and dispersion within the polish. Lighting conditions primarily result in localized bright areas and apparent flashes of color that must not be taken into account when assessing the true body color of a gemstone. To make the measurement, a photographic approach was used as described in WO 2016 / 203210. This technique is a fast but more reliable alternative to the use of a spectrophotometer and integrating sphere, and is therefore particularly useful when measuring large numbers of polished gemstones. When the finished gemstone is measured, the hue angle is 25°. <h ab <35°, and most of the gemstones are in the h ab = 30°. Saturation values ​​are typically around 20 <C * ab <30, and most of the gems measured are C * ab = 25. These values ​​were chosen as an example. Note that by suitably changing synthesis and / or illumination conditions, both the hue angle and chroma can be adjusted to fall within the range of the present invention to obtain the N s The relative and / or absolute concentrations of and NV can be varied. In this way, different aesthetic preferences can be met. Excitation was performed using a 660 nm diode laser and SiV at 77 K. - Photoluminescence (PL) measurements were performed on 100 samples of 1000 SiV. The sensitivity of low-temperature PL is the highest, allowing quantifiable SiVs even in samples with orders of magnitude fewer SiVs than are detectable by absorption. -The signal is almost always observed in measurements of CVD synthetic diamond material. As with other PL measurements, SiV - The values ​​recorded are the SiV for the primary Raman line of diamond, except that the two ZPLs are at 736.5 and 736.8 nm, respectively. - is the area ratio of the PL feature of SiV - 660 = I(736.5 nm) / I(R1 660 ) + I(736.8 nm) / I(R1 660 In these samples, SiV - 660 is typically between 0.001 and 0.01, which is exceptionally small by the standards of commercially available CVD synthetic gemstones.

[0020] Birefringence measurements were performed on CVD single crystal diamond material. The grown diamond material was formed into a cube. The cube had {110} oriented sides with edge lengths equal to the diagonals of the substrate, thus limiting the area of ​​the original substrate, as well as {100} oriented top and bottom faces. After annealing the cube as described above, it was cut horizontally into a plate 0.7 mm thick and both major faces were polished. A commercially available instrument (Thorlabs LCC7201) was used to measure the birefringence (defined as the refractive index difference for light polarized parallel to the slow and fast axes, averaged over the thickness of the sample) of the plate at a wavelength of 590 nm, and found to be 10 nm for most of its area, well within the range of WO 2004 / 046427, which describes materials suitable for optical applications such as etalons. -5 The exception was the region just above the substrate edge, where dislocations tended to concentrate at the boundaries between the lateral and vertical growth regions, with local maximum birefringence of 10 -4Although inclusions in these more doubly refracting parts of the crystal may not be desirable in all technical applications, they have not been found to be detrimental to the visual clarity of CVD single crystal diamonds, taking into account that they occupy only a small fraction of the total volume, and in any given example, the maximum doubly refracting is on the order of 4.3 × 10 as cited in “Synthetic moissanite: a new diamond substitute”, Gems and Gemology volume 33, issue 4, winter 1997. -2 ) is less than 1% of the For applications using the spin state of NV centers in diamond, the decoherence time T 2 * It is possible to measure T 2 * The value of was determined by a Ramsey pulse sequence and found to be greater than 5 μsec.

[0021] Figure 1 is a flow chart illustrating an exemplary process for making CVD single crystal diamond. The numbering below corresponds to Figure 1. S1. Place multiple single crystal diamond substrates on a substrate carrier in a CVD reactor. S2. Feed a process gas into the reactor. The process gas includes a hydrogen-containing gas, a carbon-containing gas, and a nitrogen-containing gas. The relative amounts of these gases are 1% to 4% C. 2 H 2 / H 2 ratio, and 30 ppm to 300 ppm N 2 / C 2 H 2 The ratio is stoichiometrically equal to the ratio of 50 to 200 ppm, 60 to 180 ppm, and 70 to 150 ppm of N. 2 / C 2 H 2 The relative amount of the process gas may be selected from the range of 1 to 3%, 1.5 to 2.5%, and 1.5 to 2%. 2 H2 / H 2 The ratio may be selected to be stoichiometrically equivalent. S3. Grow single crystal CVD diamond on the surfaces of multiple single crystal diamond substrates at a temperature of 750°C to 1000°C. Growth is preferably carried out as a single continuous, uninterrupted CVD synthesis cycle or "run". The volumetric growth rate of this cycle is at least 10 mm 3 / h, at least 20mm 3 / h, at least 30mm 3 / h, at least 40mm 3 / h and at least 50 mm 3 The growth temperature is typically between 800°C and 1000°C, between 800°C and 950°C, or between 800°C and 900°C. S4. The resulting single crystal CVD diamonds are subjected to a first annealing at a temperature of 1500°C to 1800°C. At temperatures significantly higher than 1800°C, any nitrogen in the crystals may form H3 centers, meaning that single substitutional nitrogen is not available for subsequent processing to form NV centers. One skilled in the art may choose to perform the annealing below 1750°C, further reducing the formation of H3 centers. The annealing is preferably performed under diamond stabilizing pressure to reduce the risk of graphitization. S5. Irradiate the plurality of single crystal CVD diamonds to create vacancies in the diamond crystal lattice. This may be done, for example, using 1 to 10 MeV electron irradiation. S6. Perform a second annealing on the irradiated single crystal CVD diamond at a temperature of 700°C to 1100°C to form NV centres. The second annealing may be performed at a temperature selected from any of 700 to 1000°C, 800 to 1000°C and 850 to 950°C.

[0022] If it is desired to produce a gemstone, the method further comprises cutting and polishing at least one of the plurality of single crystal diamonds to form a gemstone. In this example, to produce a gemstone of over 1 ct, at least one linear dimension of the CVD single crystal diamond is 3.5 mm or more. However, for many technical applications, much smaller crystals, such as diamonds having at least one linear dimension of 0.5 mm or more, are often sufficient. The high-yield synthesis and post-growth annealing process described above produces multiple reproducible gemstones in a single run, greatly reducing energy costs. This allows diamonds to be produced with the required properties, knowing in advance what size and shape is required, with the confidence that they will be spared annealing damage after minimal processing. Such an uninterrupted process has advantages over "stop-start" or layer-by-layer processes, for example, in improving equipment utilization efficiency, avoiding the need to prepare crystals for growth multiple times, and preventing any deleterious effects of interfaces formed between grown layers in the material produced by successive growth cycles. In our preferred embodiment, growth to full thickness is always performed without interruption, as detailed by examples.

[0023] Although the present invention has been particularly shown and described with reference to embodiments, it will be understood by those skilled in the art that various changes in form and details may be made therein without departing from the scope of the invention as defined in the appended claims.

Claims

1. below, A single substituted nitrogen atom N in the neutral charge state as measured by EPR. s 0 Concentration is between 0.25 and 3 ppm; CVD single crystal diamond having the properties Nitrogen vacancy centers (NV) in neutral and negative charge states 0 and N.V. - The total concentration of s 0 CVD single crystal diamond, with 0.1 to 0.8 times the concentration.

2. 2. The CVD single crystal diamond according to claim 1, having at least one linear dimension of 3.5 mm or greater.

3. A hue angle h selected from −45 to 45°, −10 to 40°, and 10 to 40° ab 3. The CVD single crystal diamond according to claim 1 or 2, having

4. The SiV ratio relative to the peak area of ​​the primary Raman signal of diamond in photoluminescence measurements performed at a temperature of 77 K using an excitation wavelength of 660 nm. - SiV, quantified by the ratio of the total peak areas of the zero phonon line, selected from any of: less than 0.5; less than 0.1; less than 0.05; and less than 0.

01. - 4. A CVD single crystal diamond according to any one of claims 1 to 3, which exhibits luminescence.

5. It has low optical birefringence with low distortion at a temperature of 20° C., and when measuring an area of ​​at least 3 mm×3 mm, the third quartile value of the refractive index difference for light polarized parallel to the slow and fast axes, averaged over the thickness of the sample, is less than 1×10 -4 and 5 x 10 -5 5. The CVD single crystal diamond according to any one of claims 1 to 4, wherein the average molecular weight of the diamond is 100 or more.

6. The total volume of the single crystal CVD diamond material is at least 0.1 mm 2 , at least 1 mm 2 , at least 10 mm 2 , at least 20 mm 2 , at least 40 mm 3 , at least 60 mm 3 , at least 80 mm 3 and at least 100 mm 3 6. The CVD single crystal diamond according to any one of claims 1 to 5, selected from any one of

7. A gem-like color having a chroma C selected from 5 to 40, 10 to 35, and 15 to 30. * ab 7. The CVD single crystal diamond according to any one of claims 1 to 6, having

8. The inhomogeneous dephasing time T of the measured ensemble NVs, as measured by the Ramsey pulse sequence, 2 * 6. The CVD single crystal diamond according to any one of claims 1 to 5, wherein the ds is greater than 5 μsec.

9. 8. The CVD single crystal diamond according to any one of claims 1 to 7, which is in gem form and has a colour grade selected from any of Fancy Light, Fancy, Fancy Intense, Fancy Vivid and Fancy Deep, along with any of pinkish orange, orange-pink, pink, purplish pink, purple-pink and pink-purple, according to the Gemological Institute of America (GIA) scale and method.

10. Gem-like, according to the Gemological Institute of America (GIA) scale and method, VS 2 , V.S. 1 , V.V.S. 2 , V.V.S. 1 9. The CVD single crystal diamond according to any one of claims 1 to 8, having a clarity grade selected from any of the following: IF, FL and IF.

11. H3 (NVN 0 10. The CVD single crystal diamond according to any one of claims 1 to 9, further comprising a .sup.3) centre.

12. In photoluminescence measurements performed at a temperature of 77 K using an excitation wavelength of 455 to 459 nm, a (NV 0 + N.V. - 11. The CVD single crystal diamond according to claim 10, which exhibits a NV / H ratio, 0 , N.V. - and H3 defects are quantified by the peak area ratio of the zero phonon line to the first order Raman signal of the diamond.

13. at least 100, at least 150, at least 200, at least 300, and at least 400 (NV 0 + N.V. - 2. The CVD single crystal diamond of claim 1, wherein the diamond exhibits a ZnO / H3 ratio.

14. 13. A method of making a plurality of single crystal CVD diamonds according to any one of claims 1 to 12, comprising the steps of: placing a plurality of single crystal diamond substrates on a substrate carrier in a chemical vapor deposition reactor; Supplying a process gas to the reactor, the process gas comprising a hydrogen-containing gas, a carbon-containing gas and a nitrogen-containing gas, the relative amount of the process gas being between 1% and 4% C 2 H 2 / H 2 ratio, and 30 ppm to 300 ppm N 2 / C 2 H 2 providing a ratio that is stoichiometrically equal to; growing the plurality of single crystal CVD diamonds on at least some of the surfaces of the plurality of single crystal diamond substrates at a temperature of 750°C to 1000°C; first annealing at least a portion of the resulting plurality of single crystal CVD diamonds at a temperature of 1500°C to 1800°C; irradiating the plurality of single crystal CVD diamonds to form vacancies in the diamond crystal lattice; a second annealing of the resulting plurality of single crystal CVD diamonds at a temperature of 700°C to 1100°C; and A method comprising:

15. The relative amount of N in the process gas is selected from the group consisting of 50 to 200 ppm, 60 to 180 ppm, and 70 to 150 ppm. 2 / C 2 H 2 The method of claim 13, wherein the ratio is stoichiometrically equivalent.

16. The relative amount of the process gas is selected from the group consisting of 1 to 3%, 1.5 to 2.5%, and 1.5 to 2%. 2 H 2 / H 2 17. The method of claim 13 or 14, wherein the ratio is stoichiometrically equivalent.

17. 16. The method according to any one of claims 13 to 15, wherein the first annealing is carried out at a temperature of 1550°C to 1750°C.

18. 17. The method of any one of claims 13 to 16, wherein the first annealing is carried out under diamond stabilizing pressure.

19. 18. The method according to any one of claims 13 to 17, wherein the irradiation is carried out using electron irradiation of 1 to 10 MeV.

20. 17. The method of any one of claims 13 to 16, wherein the second annealing comprises annealing at a temperature range selected from any of 700 to 1000°C, 800 to 1000°C, and 850 to 950°C.

21. 20. The method of any one of claims 13 to 19, further comprising cutting and polishing at least one of the plurality of single crystal diamonds to form a gemstone.

22. 21. The method of any one of claims 13 to 20, wherein the growth on the substrate is carried out as a single CVD synthesis cycle without interruption.

23. The step of growing the plurality of single crystal CVD diamonds comprises growing a diamond layer of at least 10 mm 3 / h, at least 20 mm 3 / h, at least 30 mm 3 / h, at least 40 mm 3 / h and at least 50 mm 3 22. A method according to any one of claims 13 to 21, providing a volumetric growth rate of the single crystal diamond material selected from

24. 23. A method according to any one of claims 13 to 22, wherein the plurality of CVD single crystal diamonds are grown at a temperature selected from any of: 800°C to 1000°C; 800°C to 950°C; and 800°C to 900°C.

25. 13. A device comprising a CVD single crystal diamond according to any one of claims 1 to 12, the device being selected from any of an imaging device, a sensing device, a magnetic sensor; a spin resonance device, a quantum information processing device and a gyroscope device.

Citation Information

Patent Citations

  • Method for processing single-crystal CVD diamond and the resulting product

    JP2012530674A

  • Method for producing fancy pale blue or fancy pale blue / green single-crystal CVD diamond and the resulting product

    JP2012530677A