Etching method using silicon-containing hydrofluorocarbons
A Si-containing hydrofluorocarbon-based dry etching process addresses the challenges of high selectivity and polymer deposition in semiconductor manufacturing, ensuring precise etching profiles and reduced chamber contamination.
Patent Information
- Application Number
- JP2024522435
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-18
- Filing Date
- 2022-10-18
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2042-10-18
AI Technical Summary
Current etching processes face challenges in achieving high selectivity and controlling polymer deposition during the formation of high aspect ratio structures in semiconductor devices, leading to potential damage and modification of non-etched films.
A dry etching method using a Si-containing hydrofluorocarbon compound, particularly methylsilyl hydrofluorocarbons, is employed in a cyclic process to enhance selectivity and control polymer growth, ensuring precise etching profiles and minimal chamber contamination.
The method achieves high selectivity and controlled etching rates, reducing polymer deposition on non-etched materials and maintaining the integrity of semiconductor structures, thereby improving manufacturing efficiency and reducing additional cleaning steps.
Smart Images

Figure 2024538795000001_ABST
Abstract
Description
[Technical Field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of the filing date of U.S. Provisional Application No. 63 / 256,698, filed October 18, 2021, the teachings of which are incorporated herein by reference.
[0002] The present invention relates to a method for dry etching films, such as silicon-containing films, metal-containing films, and organic films, and in particular to a method for dry etching films, such as silicon-containing films, metal-containing films, and organic films, comprising etching a compound represented by the general formula: C x H y F z Si n (I) The present invention relates to a dry etching method, a selective dry etching method, and a cyclic selective dry etching method for dry etching films using an etching gas mixture including a Si-containing hydrofluorocarbon compound having (1≦x≦6, 1≦y≦9, 1≦z≦15, n=1 or 2). In some embodiments, the Si-containing hydrofluorocarbon includes at least one methyl group or includes at least one methyl group bonded to a Si atom. [Background technology]
[0003] In recent years, profile control (e.g., shape control, reduction of defects and damage to structures) and etch rate control during the formation of high aspect ratio structures (e.g., holes, pillars) have become key challenges in the fabrication of new semiconductor devices (e.g., 3D NAND and DRAM memories, low-k dielectrics in BEOL). These devices are based on thick stacks of silicon oxide and / or alternating layers of silicon nitride and silicon oxide, which need to be etched at high etch rates and maintaining a defined profile (no etch stops, bowing, twisting, or other pattern distortions).
[0004] Advanced patterning requires selective etching of various Si-containing compounds with high selectivity relative to one another within the same process. Most desirable is the so-called "infinite selectivity" regime, where the material to be etched is effectively removed during the etching process while the non-etched material is not etched or some polymer deposits on it. The main drawback of this process is the deposition of polymer on the non-etched material and the growth of the polymer thickness with increasing process time. For advanced patterning, the presence of a thick polymer film after the process requires additional cleaning steps, which can unintentionally modify or damage films on the substrate, further limiting the applicability of certain etching processes with infinite selectivity. The present invention provides a new cyclical etching process that utilizes Si-containing chemistries to achieve infinite selectivity for etching without growing a thick polymer film on the non-etched material or chamber walls. In this disclosure, we have demonstrated that adding a Si-containing hydrofluorocarbon to the process gas mixture during at least one step of a cyclic etch can increase selectivity through polymer growth on the non-etched material, effectively controlling the thickness of the deposited polymer when using a less selective etching process during another step of the cyclic etch. In particular, we have demonstrated that Si3N4 (or SiO2) can be etched with high selectivity relative to other tested materials when a thin film or thin interfacial layer of polymer is formed on the surface of the non-etched material after the cyclic etch.
[0005] Plasma etching using etching gases is an important process in the fabrication of semiconductor devices on substrates. Etching can remove material from the surface of a substrate; in certain cases, dry etching processes can be used to selectively remove one material over another, forming fine patterns on the surface of a substrate. Various thin films can be patterned on a workpiece or substrate to form semiconductor device components (e.g., transistors and capacitors, interconnects, signal lines, and insulators). Examples of thin films commonly used in semiconductor device fabrication include silicon-containing compounds (e.g., polycrystalline silicon, silicon oxide, or silicon nitride), organic films (containing carbon as a primary component), metals, metal oxides, or metal nitrides. For cutting-edge semiconductor devices with the most advanced technology nodes, patterning on the order of nanometers or tens of nanometers is required.
[0006] The extremely fine patterns and complex structures at the front end of semiconductor devices require highly selective etching processes relative to materials not targeted for etching. An example of such a process is the so-called "multicolor etch" or "low-contrast etch," in which a substrate containing multiple line layers of several materials is exposed to an etching process in which only one or some of the materials in the multiple line layers are targeted for etching. Multicolor etch and similar selective etching processes are critical to the formation of active components at the front end of lines, interconnects, self-aligned patterning (e.g., self-aligned multiple patterning for lithography and self-aligned contact hole etching), and other microstructures in the substrate. Therefore, poor selectivity, and associated etching defects, can degrade or even impair the performance of fabricated semiconductor devices.
[0007] To address the challenge of selective etching in multi-color etching processes, various etching processes (e.g., plasma etching, atomic layer etching, thermal etching, and wet etching) and chemistries (e.g., etchants containing fluorocarbons, Cl, or Br) have been developed.
[0008] Koyagura et al. (Chemical Etching Treatment of Polydimethylsiloxane for Smoothing Microchannel Surface, Journal of Photopolymer Science and Technology Volume 33, Number 5 (2020) 485-490) disclose a wet etching process in which Si-containing fluorocarbons (C4H9F3Si) were found in the etching mixture as a by-product. U.S. Patent Application Publication No. 2021 / 0054286 to Lim et al. discloses a wet etching method using Si-containing hydrofluorocarbons as part of the solvent. U.S. Patent Application Publication No. 2005 / 0263901 to America discloses a method for modifying a layer of material during a deposition process using the addition of Si-containing hydrofluorocarbons to the process gas mixture. U.S. Patent No. 6,107,166 to Butterbaugh et al. discloses an alkali and alkaline earth metal etching method based on using HF as the primary etchant, where Si-containing hydrofluorocarbons can be used as an additive to the primary etchant. U.S. Patent Application Publication No. 2021 / 0193477 to Ishikawa et al. discloses Si-containing compounds used as process gases for depositing passivation layers during a cyclic etching process. International Publication No. WO 2009 / 019219 to Uenveren et al. discloses a method for etching SiO2 in self-aligned contacts using hydrofluorocarbons. Several Si-containing hydrofluorocarbons (i.e., CH2F6Si2, C3H4F6Si, C3H7F3Si, C3H4F6Si) are listed, but these Si-containing hydrofluorocarbons do not have methyl groups bonded to the silicon atom, and no supporting etching examples are disclosed. U.S. Patent Application Publication No. 2003 / 0232504 to Eppler et al. discloses a process for etching openings in a dielectric layer, where the etchant gas is a fluorocarbon gas (C x F y H z, where x>=1, y>=1, and z>=0), and a silane-containing gas, hydrogen or a hydrocarbon gas (C x H y , where x>=1 and y>=4).
[0009] Patterning a substrate containing several thin films of various materials is an important process in the fabrication of semiconductor devices. During substrate patterning, some of the material to be etched can be completely or partially removed from the substrate, resulting in the formation of fine patterns that can form semiconductor device components (e.g., transistors and capacitors, interconnects, signal lines, and insulators) after several iterations of thin film and patterning. Generally, various etching processes are used to remove the material to be etched or portions of the material to be etched during substrate patterning. When partial removal of the material to be etched (wherein a portion of the material is to be etched and another portion of the material present on the substrate needs to remain after the etching process) is desired, a protective film (e.g., a hard mask) is typically used over the non-etched film. Considering the extremely small feature sizes of patterns in modern semiconductor devices, it is important to note that the hard mask must have the same order of magnitude of critical dimensions of the pattern (e.g., diameter of hole openings, width of trenches) as the pattern formed in the layer to be etched. This creates a need to form patterns in hard mask materials with the same feature size as those occurring in the material being etched, while maintaining high selectivity of the etching process relative to other materials during mask patterning to avoid damage and undesired modification of the films being etched and unetched. However, some patterning processes require long durations, such as the high-aspect-ratio etching of 3D NAND channels and DRAM capacitors. Long-duration processes require the use of thicker hard masks and more resistant mask materials. Using thicker masks increases the aspect ratio of the patterns in the mask, creating additional challenges during the patterning process. Typically, thick amorphous carbon, amorphous silicon, or doped amorphous carbon or amorphous silicon are used as hard masks in high-aspect-ratio etching processes. Therefore, to avoid damage to films other than the hard mask for semiconductor device formation, an etching process is needed that can remove mask materials with an appropriate etch rate and high selectivity relative to other materials present on the substrate.
[0010] Further development of semiconductor devices requires more complex processes for forming and patterning thin films to continue shrinking components such as transistors, signal lines, and power lines. While shrinking feature sizes of semiconductor device components is necessary to improve the performance, efficiency, and size of final devices, the dramatic reduction in feature sizes over the past few decades has placed extremely stringent requirements on manufacturing processes. In addition to shrinking feature sizes, the significantly increased portfolio of materials used has introduced new manufacturing challenges. While there are few well-established processes for selectively etching, for example, SiO2 relative to Si3N4 using common gas mixtures (e.g., fluorocarbon or hydrofluorocarbon gases, Cl- or Br-containing compounds), significant room for improvement remains due to the increasing complexity of new semiconductor devices and the need for an increasing number of materials in multi-material etch processes, along with the possibility of etching each of these materials highly selectively relative to other materials. Summary of the Invention [Means for solving the problem]
[0011] An etching method for forming an aperture in a substrate is disclosed, the method comprising: loading a substrate on a loading table in a reactor, the substrate including a silicon-containing film deposited thereon and a patterned mask layer deposited on the silicon-containing film; introducing an etching gas containing vapor of a Si-containing hydrofluorocarbon into a reactor; converting the etching gas into a plasma; and etching the silicon-containing film against the patterned mask layer by causing an etching reaction between the plasma and the silicon-containing film, thereby forming an aperture. The disclosed etching method may include one or more of the following aspects: ·CF4, C2F6, C3F6, C4F6, C4F8, C5F8, C5F 10 , C6F 12 , C7F 14 , C8F 16 an etching gas comprising fluorocarbon or hydrofluorocarbon vapor selected from one or more of CH2F2, CH3F, CHF3, C2H5F, C3H7F, C5HF7, C3H2F6, C3H4F2, C3H2F4, C4H2F6, or C4H3F7; an etching gas comprising vapor of a fluorocarbon or hydrofluorocarbon selected from one or more of C4F6, C4F8, and CH2F2; an etching gas comprising an oxidizing gas selected from O2, O3, CO, CO2, SO, SO2, FNO, NO, N2O, NO2, H2O, COS or a combination thereof; an etching gas comprising an inert gas selected from He, Ar, Xe, Kr, or Ne; an etching gas comprising an additional gas selected from H2, SF6, NF3, N2, NH3, Cl2, BCl3, BF3, Br2, F2, HBr, HCl or a combination thereof; ·General formula C x H y F z Si n (1≦x≦6, 1≦y≦9, 1≦z≦15, n=1 or 2), The Si-containing hydrofluorocarbon contains at least one methyl group; Si-containing hydrofluorocarbons containing at least one methyl group bonded to a Si atom; The Si-containing hydrofluorocarbon is a methylsilyl hydrofluorocarbon. Si-containing hydrofluorocarbons are those in which at least one methyl group is bonded to the Si atom, such as CH4F2Si, CH3F3Si, C2H6F2Si, C3H9FSi, C4H9F3Si, C5H9F5Si, and C4H 10 selected from F4Si2, C2H6F4Si2, C3H9F3Si2, C6H9F7Si, or isomers thereof; Si-containing hydrofluorocarbons selected from CH3F3Si, C2H6F2Si, C4H9F3Si, C5H9F5Si, or isomers thereof; The Si-containing hydrofluorocarbon is CH3F3Si or an isomer thereof. The Si-containing hydrofluorocarbon is C2H6F2Si or an isomer thereof. The Si-containing hydrofluorocarbon is C4H9F3Si or an isomer thereof. The Si-containing hydrofluorocarbon is C5H9F5Si or an isomer thereof. · Si-containing hydrofluorocarbons that do not contain methyl groups, Si-containing hydrofluorocarbons that contain a methyl group but do not contain a methyl group bonded to the Si element; ·CHF3Si, CH2F2Si, CH3FSi, CHF5Si, CH2F4Si, C2HF7Si, C2H2F6Si, C2H3F5Si, C2H4F4Si, C2H4F2Si, C2H3F3Si, C2H2F4Si, C2HF5Si, C3H4F6Si, C3HF9Si, C3HF7Si, C3H3F5Si, C3H4F4Si, C3H5F3Si, C4H5F7Si, C4H3F9Si, C4H2F 10 Si, C4HF 11 Si, C5H8F6Si, C5H7F7Si, C6HF 15 Si, C6H4F 12 Si, C6H7F9Si, CH5FSi2, CH3F3Si2, CH2F6Si2, C2H7F3Si2, C2H9FSi2, C2H4F6Si2, C2HF7Si2, C2H2F6Si2, C2H3F5Si2, C2H4F4Si2, C3H4F8Si2, C3H6F4Si2, C4H 10 F4Si2, C4H6F6Si2, C4H 11 Si-containing hydrofluorocarbons selected from FSi2, or C4H8F2Si2, which do not have a methyl group or do not have a methyl group bonded to the Si element; Selected from silicon oxide, silicon nitride, crystalline silicon, polysilicon, polycrystalline silicon, amorphous silicon, low-k SiCOH, SiOCN, SiC, SiON, Si a O b H c C d N e a silicon-containing film comprising layers of (a>0, b, c, d, and e≧0), or layers of alternating silicon oxide and silicon nitride (ONON) layers, or layers of alternating silicon oxide and polysilicon (OPOP) layers; silicon-containing films, optionally containing dopants such as B, C, P, As, Ga, In, Sn, Sb, Bi and / or Ge, and combinations thereof; silicon-containing films, optionally containing dopants such as B, C, P, As, Ga, In, Sn, Sb, Bi and / or Ge, and combinations thereof; · Apertures formed in the substrate having an aspect ratio of about 1:1 to about 500:1.
[0012] Also disclosed is an etching method for forming an aperture in a substrate, the method comprising: loading a substrate on a loading table in a reactor, the substrate having a silicon-containing film deposited thereon and a patterned mask layer deposited on the silicon-containing film; introducing an etching gas containing C5H9F5Si into a reactor; converting the etching gas into a plasma; and etching the silicon-containing film against the patterned mask layer to form an aperture by causing an etching reaction between the plasma and the silicon-containing film.
[0013] Also disclosed is an etching method for forming an aperture in a substrate, the method comprising: loading a substrate on a loading table in a reactor, the substrate having a silicon-containing film deposited thereon and a patterned mask layer deposited on the silicon-containing film; introducing an etching gas containing C4H9F3Si into a reactor; converting the etching gas into a plasma; and etching the silicon-containing film against the patterned mask layer to form an aperture by causing an etching reaction between the plasma and the silicon-containing film.
[0014] Also disclosed is an etching method for forming an aperture in a substrate, the method comprising: loading a substrate on a loading table in a reactor, the substrate having a silicon-containing film deposited thereon and a patterned mask layer deposited on the silicon-containing film; introducing an etching gas containing C2H6F2Si into a reactor; converting the etching gas into a plasma; and etching the silicon-containing film against the patterned mask layer to form an aperture by causing an etching reaction between the plasma and the silicon-containing film.
[0015] Also disclosed is an etching method for forming an aperture in a substrate, the method comprising: loading a substrate on a loading table in a reactor, the substrate having a silicon-containing film deposited thereon and a patterned mask layer deposited on the silicon-containing film; introducing an etching gas containing CH3F3Si into a reactor; converting the etching gas into a plasma; and etching the silicon-containing film against the patterned mask layer to form an aperture by causing an etching reaction between the plasma and the silicon-containing film.
[0016] Also disclosed is an etching gas composition suitable for use in semiconductor etching reactions, the etching gas composition comprising: formula C x H y Fz Si n (1≦x≦6, 1≦y≦9, 1≦z≦15, n=1 or 2) The first etchant vapor is a Si-containing hydrofluorocarbon selected from the group consisting of: Si-containing hydrofluorocarbons containing at least one methyl group, Si-containing hydrofluorocarbons containing at least one methyl group bonded to a Si atom; CH4F2Si, CH3F3Si, C2H6F2Si, C3H9FSi, C4H9F3Si, C5H9F5Si, C4H 10 Si-containing hydrofluorocarbons selected from F4Si2, C2H6F4Si2, C3H9F3Si2, C6H9F7Si, or isomers thereof; The Si-containing hydrofluorocarbon contains at least one methyl group; Si-containing hydrofluorocarbons containing at least one methyl group bonded to a Si atom; The Si-containing hydrofluorocarbon is a methylsilyl hydrofluorocarbon. Si-containing hydrofluorocarbons are those in which at least one methyl group is bonded to the Si atom, such as CH4F2Si, CH3F3Si, C2H6F2Si, C3H9FSi, C4H9F3Si, C5H9F5Si, and C4H 10 selected from F4Si2, C2H6F4Si2, C3H9F3Si2, C6H9F7Si, or isomers thereof; Si-containing hydrofluorocarbons selected from CH3F3Si, C2H6F2Si, C4H9F3Si, C5H9F5Si, or isomers thereof; The Si-containing hydrofluorocarbon is CH3F3Si or an isomer thereof. The Si-containing hydrofluorocarbon is C2H6F2Si or an isomer thereof. The Si-containing hydrofluorocarbon is C4H9F3Si or an isomer thereof. The Si-containing hydrofluorocarbon is C5H9F5Si or an isomer thereof. · Si-containing hydrofluorocarbons that do not contain methyl groups, Si-containing hydrofluorocarbons that contain a methyl group but do not contain a methyl group bonded to the Si element; ·CHF3Si, CH2F2Si, CH3FSi, CHF5Si, CH2F4Si, C2HF7Si, C2H2F6Si, C2H3F5Si, C2H4F4Si, C2H4F2Si, C2H3F3Si, C2H2F4Si, C2HF5Si, C3H4F6Si, C3HF9Si, C3HF7Si, C3H3F5Si, C3H4F4Si, C3H5F3Si, C4H5F7Si, C4H3F9Si, C4H2F 10 Si, C4HF 11 Si, C5H8F6Si, C5H7F7Si, C6HF 15 Si, C6H4F 12 Si, C6H7F9Si, CH5FSi2, CH3F3Si2, CH2F6Si2, C2H7F3Si2, C2H9FSi2, C2H4F6Si2, C2HF7Si2, C2H2F6Si2, C2H3F5Si2, C2H4F4Si2, C3H4F8Si2, C3H6F4Si2, C4H 10 F4Si2, C4H6F6Si2, C4H 11 Si-containing hydrofluorocarbons selected from FSi2, or C4H8F2Si2, which do not have a methyl group or do not have a methyl group bonded to the Si element; Further comprising a second etchant vapor selected from a hydrofluorocarbon or a fluorocarbon; ·CF4, C2F6, C3F6, C4F6, C4F8, C5F8, C5F 10 , C6F 12 , C7F 14 , C8F 16 a hydrofluorocarbon or fluorocarbon selected from CH2F2, CH3F, CHF3, C2H5F, C3H7F, C5HF7, C3H2F6, C3H4F2, C3H2F4, C4H2F6, or C4H3F7; further comprising an oxidizing gas selected from O2, O3, CO, CO2, SO, SO2, FNO, NO, N2O, NO2, H2O or COS, further comprising an inert gas selected from He, Ar, Xe, Kr or Ne, further comprising an additional gas selected from H2, SF6, NF3, N2, NH3, Cl2, BCl3, BF3, Br2, F2, HBr, HCl or a combination thereof; a purity of the first etching gas greater than 95% v / v; a purity of the first etching gas greater than 99.99% v / v; the boiling point of the first etching gas being approximately -50 to 250°C; and Use of the etching gas composition in a semiconductor etching process.
[0017] Also disclosed is a selective etching method for forming structures on a substrate, the selective etching method comprising: placing a substrate on a loading table in a reactor, the substrate having a pattern including an etched film and at least one non-etched film deposited thereon; introducing vapor of a Si-containing hydrofluorocarbon into a reactor; igniting the plasma to produce activated Si-containing hydrofluorocarbons; and forming a structure by selectively etching the silicon-containing film relative to at least one non-etched film by causing an etching reaction between the activated Si-containing hydrofluorocarbon and the silicon-containing film. The disclosed etching method may include one or more of the following aspects: ·CF4, C2F6, C3F6, C4F6, C4F8, C5F8, C5F 10 , C6F 12 , C7F 14 , C8F 16, CH2F2, CH3F, CHF3, C2H5F, C3H7F, C5HF7, C3H2F6, C3H4F2, C3H2F4, C4H2F6, or C4H3F7, further comprising the step of introducing into the reactor an oxidizing gas selected from O2, O3, CO, CO2, SO, SO2, FNO, NO, N2O, NO2, H2O or COS, Further comprising the step of introducing an inert gas selected from He, Ar, Xe, Kr, or Ne into the reactor, further comprising the step of introducing an additional gas into the reaction chamber, wherein the additional gas is selected from H2, SF6, NF3, N2, NH3, Cl2, BCl3, BF3, Br2, F2, HBr, HCl, or a combination thereof; ·General formula C x H y F z Si n (1≦x≦6, 1≦y≦9, 1≦z≦15, n=1 or 2), Si-containing hydrofluorocarbons containing at least one methyl group, Si-containing hydrofluorocarbons containing at least one methyl group bonded to a Si atom; The Si-containing hydrofluorocarbon is a methylsilyl hydrofluorocarbon. Si-containing hydrofluorocarbons are those in which at least one methyl group is bonded to the Si atom, such as CH4F2Si, CH3F3Si, C2H6F2Si, C3H9FSi, C4H9F3Si, C5H9F5Si, and C4H 10 selected from F4Si2, C2H6F4Si2, C3H9F3Si2, C6H9F7Si, or isomers thereof; Si-containing hydrofluorocarbons selected from CH3F3Si, C2H6F2Si, C4H9F3Si, C5H9F5Si, or isomers thereof; The Si-containing hydrofluorocarbon is CH3F3Si or an isomer thereof. The Si-containing hydrofluorocarbon is C2H6F2Si or an isomer thereof. The Si-containing hydrofluorocarbon is C4H9F3Si or an isomer thereof. The Si-containing hydrofluorocarbon is C5H9F5Si or an isomer thereof. · Si-containing hydrofluorocarbons that do not contain methyl groups, Si-containing hydrofluorocarbons that contain a methyl group but do not contain a methyl group bonded to the Si element; ·CHF3Si, CH2F2Si, CH3FSi, CHF5Si, CH2F4Si, C2HF7Si, C2H2F6Si, C2H3F5Si, C2H4F4Si, C2H4F2Si, C2H3F3Si, C2H2F4Si, C2HF5Si, C3H4F6Si, C3HF9Si, C3HF7Si, C3H3F5Si, C3H4F4Si, C3H5F3Si, C4H5F7Si, C4H3F9Si, C4H2F 10 Si, C4HF 11 Si, C5H8F6Si, C5H7F7Si, C6HF 15 Si, C6H4F 12 Si, C6H7F9Si, CH5FSi2, CH3F3Si2, CH2F6Si2, C2H7F3Si2, C2H9FSi2, C2H4F6Si2, C2HF7Si2, C2H2F6Si2, C2H3F5Si2, C2H4F4Si2, C3H4F8Si2, C3H6F4Si2, C4H 10 F4Si2, C4H6F6Si2, C4H 11 Si-containing hydrofluorocarbons selected from FSi2, or C4H8F2Si2, which do not have a methyl group or do not have a methyl group bonded to the Si element; a pattern in the substrate, which is a 2D pattern or a 3D pattern, a selectivity of the Si-containing film relative to at least one unetched film greater than 5; a selectivity of the Si-containing film relative to at least one unetched film greater than 10; selectivity of the Si-containing film relative to etching of at least one non-etched film, which is infinite; Selected from silicon oxide, silicon nitride, crystalline silicon, polysilicon, polycrystalline silicon, amorphous silicon, low-k SiCOH, SiOCN, SiC, SiON, Si a O b H c C d N e a silicon-containing film comprising layers of (a>0, b, c, d, and e≧0), or layers of alternating silicon oxide and silicon nitride (ONON) layers, or layers of alternating silicon oxide and polysilicon (OPOP) layers; and A non-etching film selected from a Si-containing film, an organic film, or a metal-containing film that is different from the Si-containing film to be etched.
[0018] Also disclosed is a selective etching method for forming structures on a substrate, the selective etching method comprising: placing a substrate on a loading table in a reactor, the substrate having a pattern including an etched film and at least one non-etched film deposited thereon; introducing vapor of C4H9F3Si into a reactor; igniting a plasma to produce activated C4H9F3Si; and forming a structure by selectively etching the silicon-containing film relative to at least one non-etched film by causing an etching reaction between the activated C4H9F3Si and the silicon-containing film. The disclosed etching method may include one or more of the following aspects:
[0019] Also disclosed is a selective etching method for forming structures on a substrate, the selective etching method comprising: placing a substrate on a loading table in a reactor, the substrate having a pattern including an etched film and at least one non-etched film deposited thereon; introducing vapor of C5H9F5Si into a reactor; igniting a plasma to produce activated C5H9F5Si; and causing an etching reaction between the activated C5H9F5Si and the silicon-containing film to proceed, thereby selectively etching the silicon-containing film relative to at least one non-etched film to form a structure.
[0020] Also disclosed is a selective etching method for forming structures on a substrate, the selective etching method comprising: placing a substrate on a loading table in a reactor, the substrate having a pattern including an etched film and at least one non-etched film deposited thereon; introducing CH3F3Si vapor into a reactor; igniting a plasma to produce activated CH3F3Si; and causing an etching reaction between the activated CH3F3Si and the silicon-containing film to proceed, thereby selectively etching the silicon-containing film relative to at least one non-etched film to form a structure.
[0021] Also disclosed is a selective etching method for forming structures on a substrate, the selective etching method comprising: placing a substrate on a loading table in a reactor, the substrate having a pattern including an etched film and at least one non-etched film deposited thereon; introducing vapor of C2H6F2Si into a reactor; igniting a plasma to produce activated C2H6F2Si; and causing an etching reaction between the activated C2H6F2Si and the silicon-containing film to proceed, thereby selectively etching the silicon-containing film relative to at least one non-etched film to form a structure.
[0022] Also disclosed is a selective etching method for forming structures on a substrate, the selective etching method comprising: placing a substrate on a loading table in a reactor, the substrate having a pattern including an etched film and at least one non-etched film deposited thereon; introducing an etching gas containing vapor of a Si-containing hydrofluorocarbon and an oxidizing gas into a reactor; igniting a plasma to generate an activated etching gas; and causing an etching reaction between the activated etching gas and the etching film, thereby selectively etching the etching film relative to at least a non-etching film to form a structure. The disclosed etching method may include one or more of the following aspects: an oxidizing gas selected from O2, O3, CO, CO2, SO, SO2, FNO, NO, N2O, NO2, H2O or COS, an etching gas comprising an inert gas selected from He, Ar, Xe, Kr, or Ne; ·General formula C x H y F z Si n (1≦x≦6, 1≦y≦9, 1≦z≦15, n=1 or 2), Si-containing hydrofluorocarbons containing at least one methyl group, Si-containing hydrofluorocarbons containing at least one methyl group bonded to a Si atom; The Si-containing hydrofluorocarbon is a methylsilyl hydrofluorocarbon. Si-containing hydrofluorocarbons are those in which at least one methyl group is bonded to the Si atom, such as CH4F2Si, CH3F3Si, C2H6F2Si, C3H9FSi, C4H9F3Si, C5H9F5Si, and C4H 10 selected from F4Si2, C2H6F4Si2, C3H9F3Si2, C6H9F7Si, or isomers thereof; Si-containing hydrofluorocarbons selected from CH3F3Si, C2H6F2Si, C4H9F3Si, C5H9F5Si, or isomers thereof; The Si-containing hydrofluorocarbon is CH3F3Si or an isomer thereof. The Si-containing hydrofluorocarbon is C2H6F2Si or an isomer thereof. The Si-containing hydrofluorocarbon is C4H9F3Si or an isomer thereof. The Si-containing hydrofluorocarbon is C5H9F5Si or an isomer thereof. · Si-containing hydrofluorocarbons that do not contain methyl groups, Si-containing hydrofluorocarbons that contain a methyl group but do not contain a methyl group bonded to the Si element; ·CHF3Si, CH2F2Si, CH3FSi, CHF5Si, CH2F4Si, C2HF7Si, C2H2F6Si, C2H3F5Si, C2H4F4Si, C2H4F2Si, C2H3F3Si, C2H2F4Si, C2HF5Si, C3H4F6Si, C3HF9Si, C3HF7Si, C3H3F5Si, C3H4F4Si, C3H5F3Si, C4H5F7Si, C4H3F9Si, C4H2F 10 Si, C4HF 11 Si, C5H8F6Si, C5H7F7Si, C6HF 15 Si, C6H4F 12 Si, C6H7F9Si, CH5FSi2, CH3F3Si2, CH2F6Si2, C2H7F3Si2, C2H9FSi2, C2H4F6Si2, C2HF7Si2, C2H2F6Si2, C2H3F5Si2, C2H4F4Si2, C3H4F8Si2, C3H6F4Si2, C4H 10 F4Si2, C4H6F6Si2, C4H 11 Si-containing hydrofluorocarbons selected from FSi2, or C4H8F2Si2, which do not have a methyl group or do not have a methyl group bonded to the Si element; The etching film is an organic film. an organic film, which is an aC film, a doped aC film, an a-Si film, or a doped a-Si film; Etching film, which is a metal-containing film; A non-etching film that is an organic film different from the etching film, a metal-containing film different from the etching film, or a silicon-containing film; a selectivity of the Si-containing film relative to at least one unetched film greater than 5; a selectivity of the Si-containing film relative to at least one unetched film greater than 10; · The selectivity of the Si-containing film relative to etching of at least one non-etched film is infinite.
[0023] Also disclosed is a selective etching method for forming structures on a substrate, the selective etching method comprising: placing a substrate on a loading table in a reactor, the substrate having a pattern including an etched film and at least one non-etched film deposited thereon; introducing an etching gas containing CH3F3Si and vapor of an oxidizing gas into a reactor; igniting a plasma to generate an activated etching gas; and a step of causing an etching reaction between the activated etching gas and the etching film, thereby selectively etching the etching film relative to at least the non-etching film to form a structure.
[0024] Also disclosed is a selective etching method for forming structures on a substrate, the selective etching method comprising: placing a substrate on a loading table in a reactor, the substrate having a pattern including an etched film and at least one non-etched film deposited thereon; introducing an etching gas containing vapor of C2H6F2Si and an oxidizing gas into a reactor; igniting a plasma to generate an activated etching gas; and a step of causing an etching reaction between the activated etching gas and the etching film, thereby selectively etching the etching film relative to at least the non-etching film to form a structure.
[0025] Also disclosed is a selective etching method for forming structures on a substrate, the selective etching method comprising: placing a substrate on a loading table in a reactor, the substrate having a pattern including an etched film and at least one non-etched film deposited thereon; introducing an etching gas containing vapor of C4H9F3Si and an oxidizing gas into a reactor; igniting a plasma to generate an activated etching gas; and a step of causing an etching reaction between the activated etching gas and the etching film, thereby selectively etching the etching film relative to at least the non-etching film to form a structure.
[0026] Also disclosed is a selective etching method for forming structures on a substrate, the selective etching method comprising: placing a substrate on a loading table in a reactor, the substrate having a pattern including an etched film and at least one non-etched film deposited thereon; introducing an etching gas containing vapor of C5H9F5Si and an oxidizing gas into a reactor; igniting a plasma to generate an activated etching gas; and a step of causing an etching reaction between the activated etching gas and the etching film, thereby selectively etching the etching film relative to at least the non-etching film to form a structure.
[0027] Also disclosed is a cyclical selective etching method for removing a film, the method comprising: i) introducing a first etching gas comprising vapor of a Si-containing hydrofluorocarbon compound into a reactor containing a substrate having a pattern comprising an etched film and at least one unetched film deposited thereon; ii) initiating a plasma to form an activated first etching gas; iii) allowing an etching reaction to proceed between the activated first etching gas and the etching film, so that the etching film is selectively etched relative to the at least one non-etching film, and simultaneously a polymer layer is deposited on the at least one non-etching film; iv) introducing a second etching gas into the reactor; v) initiating a plasma to form an activated second etching gas; vi) causing an etching reaction between the activated second etching gas and the etching film and the polymer layer to etch the etching film and the polymer layer; and vii) repeating steps i) to vi) until the etching film is removed. The disclosed etching method may include one or more of the following aspects: further comprising the step of inertizing the plasma and purging the reactor with an inert gas selected from N2, He, Ar, Xe, Kr or Ne after steps iii) and vi), respectively; ·General formula C x H y F z Si n (1≦x≦6, 1≦y≦9, 1≦z≦15, n=1 or 2), Si-containing hydrofluorocarbons containing at least one methyl group, Si-containing hydrofluorocarbons containing at least one methyl group bonded to a Si atom; The Si-containing hydrofluorocarbon is a methylsilyl hydrofluorocarbon. Si-containing hydrofluorocarbons are those in which at least one methyl group is bonded to the Si atom, such as CH4F2Si, CH3F3Si, C2H6F2Si, C3H9FSi, C4H9F3Si, C5H9F5Si, and C4H 10 selected from F4Si2, C2H6F4Si2, C3H9F3Si2, C6H9F7Si, or isomers thereof; Si-containing hydrofluorocarbons selected from CH3F3Si, C2H6F2Si, C4H9F3Si, C5H9F5Si, or isomers thereof; The Si-containing hydrofluorocarbon is CH3F3Si or an isomer thereof. The Si-containing hydrofluorocarbon is C2H6F2Si or an isomer thereof. The Si-containing hydrofluorocarbon is C4H9F3Si or an isomer thereof. The Si-containing hydrofluorocarbon is C5H9F5Si or an isomer thereof. · Si-containing hydrofluorocarbons that do not contain methyl groups, Si-containing hydrofluorocarbons that contain a methyl group but do not contain a methyl group bonded to the Si element; ·CHF3Si, CH2F2Si, CH3FSi, CHF5Si, CH2F4Si, C2HF7Si, C2H2F6Si, C2H3F5Si, C2H4F4Si, C2H4F2Si, C2H3F3Si, C2H2F4Si, C2HF5Si, C3H4F6Si, C3HF9Si, C3HF7Si, C3H3F5Si, C3H4F4Si, C3H5F3Si, C4H5F7Si, C4H3F9Si, C4H2F 10 Si, C4HF 11 Si, C5H8F6Si, C5H7F7Si, C6HF 15 Si, C6H4F 12 Si, C6H7F9Si, CH5FSi2, CH3F3Si2, CH2F6Si2, C2H7F3Si2, C2H9FSi2, C2H4F6Si2, C2HF7Si2, C2H2F6Si2, C2H3F5Si2, C2H4F4Si2, C3H4F8Si2, C3H6F4Si2, C4H 10 F4Si2, C4H6F6Si2, C4H 11 Si-containing hydrofluorocarbons selected from FSi2, or C4H8F2Si2, which do not have a methyl group or do not have a methyl group bonded to the Si element; a first etching gas comprising vapors of a hydrofluorocarbon or fluorocarbon compound; ·CF4, C2F6, C3F6, C4F6, C4F8, C5F8, C5F 10 , C6F 12 , C7F 14 , C8F 16 , a fluorocarbon or hydrofluorocarbon selected from CH2F2, CH3F, CHF3, C2H5F, C3H7F, C5HF7, C3H2F6, C3H4F2, C3H2F4, C4H2F6 or C4H3F7, a first etching gas comprising an oxidizing gas selected from O2, O3, CO, CO2, SO, SO2, FNO, NO, N2O, NO2, or H2O, COS; a first etching gas comprising an inert gas selected from the group consisting of He, Ar, Xe, Kr, or Ne; a first etching gas comprising an additional gas selected from H2, SF6, NF3, N2, NH3, Cl2, BCl3, BF3, Br2, F2, HBr, HCl or a combination thereof; a second etching gas comprising vapor of a hydrofluorocarbon or a fluorocarbon, or a combination thereof; ·CF4, C2F6, C3F6, C4F6, C4F8, C5F8, C5F 10 , C6F 12 , C7F 14 , C8F 16 , a fluorocarbon or hydrofluorocarbon selected from CH2F2, CH3F, CHF3, C2H5F, C3H7F, C5HF7, C3H2F6, C3H4F2, C3H2F4, C4H2F6 or C4H3F7, a second etching gas comprising an oxidizing gas selected from O2, O3, CO, CO2, SO, SO2, FNO, NO, N2O, NO2, or H2O, COS; a second etching gas comprising an inert gas selected from the group consisting of He, Ar, Xe, Kr, or Ne; a second etching gas comprising an additional gas selected from H2, SF6, NF3, N2, NH3, Cl2, BCl3, BF3, Br2, F2, HBr, HCl or a combination thereof; · between step vi) and step vii), introducing a third etching gas into the reactor; igniting a plasma to generate an activated third etching gas; and causing an etching reaction between the activated third etching gas and the etching film and the polymer layer to etch the etching film and the polymer layer. a third etching gas that is the same as the second etching gas, but both do not have the same combination of gas compositions in one or each cycle; Selected from silicon oxide, silicon nitride, crystalline silicon, polysilicon, polycrystalline silicon, amorphous silicon, low-k SiCOH, SiOCN, SiC, SiON, Si a O b H c C d N e An etching film comprising a layer of (a>0, b, c, d and e≧0), or a layer of alternating silicon oxide and silicon nitride (ONON) layers, or a layer of alternating silicon oxide and polysilicon (OPOP) layers; Etching films, including Si-containing films, organic films, or metal-containing films.
[0028] Also disclosed is a cyclical selective etching method for removing a film, the method comprising: i) introducing a first etching gas comprising vapor of C4H9F3Si into a reactor containing a substrate having a pattern comprising an etched film and at least one non-etched film deposited thereon; ii) initiating a plasma to form an activated first etching gas; iii) allowing an etching reaction to proceed between the activated first etching gas and the etching film, so that the etching film is selectively etched relative to the at least one non-etching film, and simultaneously a polymer layer is deposited on the at least one non-etching film; iv) introducing a second etching gas into the reactor; v) initiating a plasma to form an activated second etching gas; vi) causing an etching reaction between the activated second etching gas and the etching film and the polymer layer to etch the etching film and the polymer layer; vii) repeating steps i) to vi) until the etching film is removed.
[0029] Also disclosed is a cyclical selective etching method for removing a film, the method comprising: i) introducing a first etching gas comprising vapor of C5H9F5Si into a reactor containing a substrate having a pattern comprising an etched film and at least one non-etched film deposited thereon; ii) initiating a plasma to form an activated first etching gas; iii) allowing an etching reaction to proceed between the activated first etching gas and the etching film, so that the etching film is selectively etched relative to the at least one non-etching film, and simultaneously a polymer layer is deposited on the at least one non-etching film; iv) introducing a second etching gas into the reactor; v) initiating a plasma to form an activated second etching gas; vi) causing an etching reaction between the activated second etching gas and the etching film and the polymer layer to etch the etching film and the polymer layer; vii) repeating steps i) to vi) until the etching film is removed.
[0030] Also disclosed is a cyclical selective etching method for removing a film, the method comprising: i) introducing a first etching gas comprising vapor of CH3F3Si into a reactor containing a substrate having a pattern comprising an etched film and at least one non-etched film deposited thereon; ii) initiating a plasma to form an activated first etching gas; iii) allowing an etching reaction to proceed between the activated first etching gas and the etching film, so that the etching film is selectively etched relative to the at least one non-etching film, and simultaneously a polymer layer is deposited on the at least one non-etching film; iv) introducing a second etching gas into the reactor; v) initiating a plasma to form an activated second etching gas; vi) causing an etching reaction between the activated second etching gas and the etching film and the polymer layer to etch the etching film and the polymer layer; vii) repeating steps i) to vi) until the etching film is removed.
[0031] Also disclosed is a cyclical selective etching method for removing a film, the method comprising: i) introducing a first etching gas comprising vapor of C2H6F2Si into a reactor containing a substrate having a pattern comprising an etched film and at least one non-etched film deposited thereon; ii) initiating a plasma to form an activated first etching gas; iii) allowing an etching reaction to proceed between the activated first etching gas and the etching film, so that the etching film is selectively etched relative to the at least one non-etching film, and simultaneously a polymer layer is deposited on the at least one non-etching film; iv) introducing a second etching gas into the reactor; v) initiating a plasma to form an activated second etching gas; vi) causing an etching reaction between the activated second etching gas and the etching film and the polymer layer to etch the etching film and the polymer layer; vii) repeating steps i) to vi) until the etching film is removed.
[0032] Also disclosed is an apparatus for supplying an etching gas composition to a semiconductor etching process, the apparatus comprising: a) a source of a first etchant; b) a source of a second etchant; c) at least two fluid conduits connecting sources a) and b) to a common fluid conduit; d) optionally a mixing element adapted to mix the first etching gas and the second etching gas, the mixing element being fluidly connected to the common fluid conduit; e) optionally, a thermal element adapted to adjust the temperature of the first etching gas, the temperature of the second etching gas, and the temperature of the mixture thereof; f) optionally, a vaporizer element fluidly connected to one or more of the at least two fluid conduits and / or the common fluid conduit and adapted to generate vapors of the first etching gas, the second etching gas, and mixtures thereof; g) optionally, a PLC controller adapted to control the vaporizer element and a valve connected to the source. The disclosed etching method can include one or more of the following aspects: an apparatus adapted to adjust the flow of the first etching solution and the second etching solution to form an etching gas composition having a predetermined ratio of the first etching solution to the second etching solution based on a chemical formulation of the first etching solution and the second etching solution; a vessel containing a first etching solution, the vessel being adapted to be connected to a device used in a semiconductor etching process; An apparatus including a vessel operably connected to a device used in a semiconductor etching process. a first etchant which is a Si-containing hydrofluorocarbon; ·General formula C x H y F z Si n(1≦x≦6, 1≦y≦9, 1≦z≦15, n=1 or 2), Si-containing hydrofluorocarbons containing at least one methyl group, Si-containing hydrofluorocarbons containing at least one methyl group bonded to a Si atom; The Si-containing hydrofluorocarbon is a methylsilyl hydrofluorocarbon. Si-containing hydrofluorocarbons are those in which at least one methyl group is bonded to the Si atom, such as CH4F2Si, CH3F3Si, C2H6F2Si, C3H9FSi, C4H9F3Si, C5H9F5Si, and C4H 10 selected from F4Si2, C2H6F4Si2, C3H9F3Si2, C6H9F7Si, or isomers thereof; Si-containing hydrofluorocarbons selected from CH3F3Si, C2H6F2Si, C4H9F3Si, C5H9F5Si, or isomers thereof; The Si-containing hydrofluorocarbon is CH3F3Si or an isomer thereof. The Si-containing hydrofluorocarbon is C2H6F2Si or an isomer thereof; The Si-containing hydrofluorocarbon is C4H9F3Si or an isomer thereof. The Si-containing hydrofluorocarbon is C5H9F5Si or an isomer thereof. · Si-containing hydrofluorocarbons that do not contain methyl groups, Si-containing hydrofluorocarbons that contain a methyl group but do not contain a methyl group bonded to the Si element; ·CHF3Si, CH2F2Si, CH3FSi, CHF5Si, CH2F4Si, C2HF7Si, C2H2F6Si, C2H3F5Si, C2H4F4Si, C2H4F2Si, C2H3F3Si, C2H2F4Si, C2HF5Si, C3H4F6Si, C3HF9Si, C3HF7Si, C3H3F5Si, C3H4F4Si, C3H5F3Si, C4H5F7Si, C4H3F9Si, C4H2F 10 Si, C4HF 11Si, C5H8F6Si, C5H7F7Si, C6HF 15 Si, C6H4F 12 Si, C6H7F9Si, CH5FSi2, CH3F3Si2, CH2F6Si2, C2H7F3Si2, C2H9FSi2, C2H4F6Si2, C2HF7Si2, C2H2F6Si2, C2H3F5Si2, C2H4F4Si2, C3H4F8Si2, C3H6F4Si2, C4H 10 F4Si2, C4H6F6Si2, C4H 11 Si-containing hydrofluorocarbons selected from FSi2, or C4H8F2Si2, which do not have a methyl group or do not have a methyl group bonded to the Si element; a second etching solution comprising vapors of a hydrofluorocarbon, or a fluorocarbon, or a combination thereof; ·CF4, C2F6, C3F6, C4F6, C4F8, C5F8, C5F 10 , C6F 12 , C7F 14 , C8F 16 , a fluorocarbon or hydrofluorocarbon selected from CH2F2, CH3F, CHF3, C2H5F, C3H7F, C5HF7, C3H2F6, C3H4F2, C3H2F4, C4H2F6 or C4H3F7, a second etching gas comprising an oxidizing gas selected from O2, O3, CO, CO2, SO, SO2, FNO, NO, N2O, NO2, or H2O, COS; a second etching gas comprising an inert gas selected from the group consisting of He, Ar, Xe, Kr, or Ne; and A second etching gas comprising an additional gas selected from H2, SF6, NF3, N2, NH3, Cl2, BCl3, BF3, Br2, F2, HBr, HCl or combinations thereof.
[0033] Notation and Nomenclature In the following detailed description and claims, certain abbreviations, symbols and terms that are commonly known in the art are used.
[0034] As used herein, the indefinite article "a" or "an" means one or more.
[0035] As used herein, in the text or claims, "about" or "roughly" or "approximately" means ±10% of the stated value.
[0036] As used herein, "room temperature" in the text or claims means from about 20°C to about 25°C.
[0037] The term "wafer" or "patterned wafer" refers to a wafer having a patterned hard mask layer in any pre-existing film stack, including silicon-containing films, in a substrate, and any pre-existing film stack, including silicon-containing films, formed for pattern etching.
[0038] The term "substrate" refers to the material on which a process is performed. A substrate can refer to a wafer or patterned wafer having the material on which the etching process is performed. A substrate can be any suitable wafer used in the manufacture of semiconductor, photovoltaic, flat panel, or LCD-TFT devices. A substrate can also have one or more layers of different materials already deposited thereon in a previous manufacturing step. For example, a wafer can include a silicon layer (e.g., crystalline, amorphous, porous, etc.), a silicon-containing layer (e.g., SiO2, SiN, SiON, SiCOH, etc.), a metal-containing layer (e.g., copper, cobalt, ruthenium, tungsten, indium, platinum, palladium, nickel, ruthenium, gold, etc.), or a combination thereof. Furthermore, a substrate can be planar or patterned. A substrate can be an organic patterned photoresist film. The substrate may contain oxide layers (e.g., ZrO2-based materials, HfO2-based materials, TiO2-based materials, rare earth oxide-based materials, ternary oxide-based materials, etc.) used as dielectric materials in MEMS, 3D NAND, MIM, DRAM, or FeRAM device applications, nitride-based films (e.g., TaN, TiN, NbN) used as electrodes, or metal-containing or metal alloy-based films (e.g., InGaAs, In) that are potential candidates as future silicon replacements in CMOS systems. x O y (x=0.5-1.5, y=0.5-1.5), InSnO (ITO), InGaZnO (IGZO), InN, InP, InAs, InSb, In2S3, or In(OH)3, etc. Those skilled in the art will recognize that the term "film" or "layer" as used herein refers to a thickness of some material placed on or spread across a surface, which may be a trench or line. Throughout this specification and claims, the wafer and any associated layers thereon will be referred to as the substrate.
[0039] It should be noted that films or layers to be etched, such as silicon oxide or silicon nitride, may be recited throughout the specification and claims without reference to their appropriate stoichiometry (i.e., SiO2, SiO3, Si3N4). These layers may be pure (Si) layers, such as crystalline Si, polysilicon (p-Si or polycrystalline Si), or amorphous silicon; silicon carbide (Si o C p ) layer, silicon nitride (Si k N l ) layer, silicon oxide (Si n O m ) layer, or a mixture thereof, where k, l, m, n, o, and p are in the range of 0.1 to 6, inclusive. For example, silicon nitride can be Si k N l In this case, the ranges of k and l are each 0.5 to 1.5. More preferably, the silicon nitride is Si3N4. In the following description of this specification, SiN is used to refer to Si k N l can be used to represent a containing layer. For example, silicon oxide is Si n O m In this case, n is in the range of 0.5 to 1.5, and m is in the range of 1.5 to 3.5. Preferably, the silicon oxide layer is SiO2. In the following description, SiN and SiO are respectively used to refer to Si k N l and Si n O m The term "silicon-containing layer" is used to refer to a silicon-containing layer. The silicon-containing film may also be a silicon oxide-based dielectric material, such as an organic-based or silicon oxide-based low-k dielectric material, such as Black Diamond II or III material by Applied Materials, Inc., having a SiOCH formulation. Alternatively, any silicon-containing layer referred to may be pure silicon. The silicon-containing film may also refer to a silicon-containing layer containing Si. a O b C c N d H ewhere a, b, c, d, and e range from 0.1 to 6, and independently b, c, d, and e > 0. The silicon-containing film can also include dopants such as B, C, P, As, Ga, In, Sn, Sb, Bi, and / or Ge.
[0040] The terms "pattern etching" or "patterned etching" refer to etching a non-planar structure, such as a stack of silicon-containing films underneath a patterned hard mask layer.
[0041] As used herein, the term "etch" or "etching" refers to the removal of material using an etching compound and / or plasma by ion bombardment, remote plasma, or chemical vapor reaction between an etching gas and a substrate, and refers to isotropic and / or anisotropic etching processes. Isotropic etching processes involve a chemical reaction between an etching compound and a substrate that results in the removal of a portion of the material in the substrate. This type of etching process includes chemical dry etching, gas-phase chemical etching, thermal dry etching, etc. Isotropic etching processes produce lateral or horizontal etching profiles in the substrate. Isotropic etching processes produce recesses or horizontal recesses in the sidewalls of pre-formed apertures in the substrate. Anisotropic etching processes involve plasma etching processes (i.e., dry etching processes) in which ion bombardment accelerates chemical reactions in the vertical direction, resulting in the formation of vertical sidewalls along the edges of features masked normal to the substrate (Manos and Flamm, Thermal Etching: An Introduction, Academic Press, Inc. 1989 pp.12-13). The plasma etching process produces vertical etch profiles in the substrate. The plasma etching process produces vertical vias, apertures, trenches, channel holes, gate trenches, step contacts, capacitor holes, contact holes, slit etching, self-aligned contacts, self-aligned vias, supervias, etc. in the substrate.
[0042] The term "mask" refers to a layer that resists etching. A mask layer can be disposed on a layer to be etched. A mask layer is also called a hard mask layer. A mask layer can be an amorphous carbon (aC) layer, a doped aC layer, a photoresist layer, an anti-reflective layer, an amorphous silicon (a-Si) layer, an organic planarization layer, and combinations thereof. A mask layer can also be a silicon layer such as poly-Si, a metal oxide such as Ti, Al, Zr, Hf, an oxide, and combinations thereof.
[0043] The term "aspect ratio" refers to the ratio of the height of the trench (or aperture) to the width of the trench (or diameter of the aperture).
[0044] As used herein, the term "high aspect ratio" or "HAR" refers to an aspect ratio greater than 5.
[0045] As used herein, the term "high aspect ratio etching" or "HAR etching" refers to the formation of a pattern of vertical holes or apertures in a film being etched by the disclosed plasma etching methods, where the aspect ratio of the vertical apertures formed exceeds a value of 5.
[0046] The term "etch stop" refers to a layer that is underneath the layer to be etched and protects the underlying layer.
[0047] The term "device channel" refers to a layer that is part of the actual device, and which, if damaged in any way, affects the performance of the device.
[0048] The term "selectivity" refers to the ratio of the etch rate of one material to the etch rate of another material. The terms "selective etch" or "selectively etch" mean etching one material more than another, or in other words, having an etch selectivity between two materials that is greater than or less than 1:1.
[0049] The terms "via," "aperture," "trench," and "hole" are sometimes used interchangeably and generally refer to an opening in an interlayer dielectric.
[0050] As used herein, the term "hydrocarbon" refers to a saturated or unsaturated functional group containing only carbon and hydrogen atoms. As used herein, the term "alkyl group" refers to a saturated functional group containing only carbon and hydrogen atoms. An alkyl group is a type of hydrocarbon. Furthermore, the term "alkyl group" refers to a straight-chain, branched, or cyclic alkyl group. Examples of straight-chain alkyl groups include, but are not limited to, methyl, ethyl, propyl, butyl, and the like. Examples of branched alkyl groups include, but are not limited to, t-butyl. Examples of cyclic alkyl groups include, but are not limited to, cyclopropyl, cyclopentyl, cyclohexyl, and the like.
[0051] As used herein, the term "organic film" refers to films formed from organic precursors, including layers of amorphous carbon (aC) and amorphous silicon (a-Si).
[0052] As used herein, the term "Si-containing hydrofluorocarbon compound" refers to a compound having the general formula: C x H y F z Si n (I) (1≦x≦6, 1≦y≦9, 1≦z≦15, n=1 or 2), which compound contains at least one methyl group. In some embodiments, at least one methyl group is bonded to a Si atom in the Si-containing hydrofluorocarbon compound. In some embodiments, at least one methyl group is not bonded to a Si atom in the Si-containing hydrofluorocarbon compound.
[0053] As used herein, the term "plasma etching" refers to etching methods that involve the use of plasma to remove films to be etched that are not protected by a mask using ion bombardment or interactions with reactive species formed in the plasma or plasma afterglow, which results in the formation of volatile by-products that can be effectively removed from the substrate.
[0054] It should be noted that the terms "film," "layer," and "material" may be used interchangeably herein. It is understood that a film may correspond to or relate to a layer or material, and a layer or material may refer to a film. Furthermore, those skilled in the art will recognize that the term "film" or "layer" as used herein refers to a thickness of some material placed on or spread across a surface, which may range from as large as an entire wafer to as small as a trench or line.
[0055] It should be noted that, herein, the terms "etching compound," "etchant," "etching gas," "etch gas," and "process gas" may be used interchangeably when the etching compound is in a gaseous state at room temperature and ambient pressure. It is understood that an etching compound may correspond to or relate to an etching gas or an etching solution or a process gas, and that an etching gas or an etching solution or a process gas may refer to an etching compound.
[0056] It should be noted that the terms "etch film," "etch material," "film to be etched," "film to be etched," "process film," and "process material" can be used interchangeably herein. It is understood that an etch film can correspond to or relate to an etch material or a film to be etched or a process film or a process material, and a film to be etched or a process film or a process material can refer to an etch film.
[0057] The terms "via," "aperture," "slit," "hole," and "structure" are used interchangeably and generally refer to an opening or recess in an interlayer dielectric or an opening or recess in a substrate or wafer.
[0058] As used herein, the abbreviation "NAND" refers to a "Negated AND" or "Not AND" gate, the abbreviation "2D" refers to a two-dimensional gate structure on a planar substrate, and the abbreviation "3D" refers to a three-dimensional or vertical gate structure in which gate structures are stacked vertically.
[0059] Standard abbreviations for elements in the periodic table of the elements are used herein, and it is understood that elements may be referred to by these abbreviations (e.g., Si refers to silicon, N refers to nitrogen, O refers to oxygen, C refers to carbon, H refers to hydrogen, F refers to fluorine, etc.).
[0060] Unique CAS Registry Numbers assigned by the Chemical Abstract Service (i.e., "CAS") are provided to help better identify the disclosed molecules.
[0061] When used in the context of describing R groups, the term "independently" should be understood to mean that the subject R group is independently selected not only with respect to other R groups having the same or different subscripts or superscripts, but also with respect to any additional species of that same R group. For example, the formula MR 1 x (NR 2 R 3 ) (4-x) In the formula, M is an atom, x is 2 or 3, and two or three R 1 The groups may be mutually or mutually linked. 2 and, or R 3 and R, ...
[0062] Ranges may be expressed herein as from about one particular value and / or to about another particular value. When such a range is expressed, it is to be understood that another embodiment is from the one particular value and / or to the other particular value, along with all combinations within the stated ranges. Any and all ranges described herein include their endpoints (i.e., a range of x=1 to 4 or x=1 to 4 includes x=1, x=4, and any number therebetween).
[0063] References herein to "one embodiment" or "an embodiment" mean that a particular feature, structure, or characteristic described in connection with that embodiment may be included in at least one embodiment of the invention. Appearances of the phrase "in one embodiment" in various places throughout this specification do not necessarily all refer to the same embodiment, nor are separate or alternative embodiments necessarily mutually exclusive of other embodiments. The same applies to the term "implementation."
[0064] For a better understanding of the nature and objects of the present invention, reference should be made to the following detailed description taken in conjunction with the accompanying drawings, in which like elements are given the same or similar reference numerals, and in which: [Brief explanation of the drawings]
[0065] [Figure 1] Figure 1 shows the signals of C4H9F3Si and C5H9F5Si recorded using a quadrupole mass spectrometer in residual gas analysis mode with an electron energy of 20 eV during the scan. [Figure 2a] FIG. 2a is an exemplary substrate with a patterned film before etching and an unetched film. [Figure 2b] FIG. 2b is an exemplary substrate with a patterned film after etching and an unetched film. [Figure 3a] FIG. 3a is an exemplary substrate having a patterned film before etching and multiple unetched films. [Figure 3b] FIG. 3b is an exemplary substrate having a patterned film after etching and multiple unetched films. [Figure 4a] FIG. 4a is an exemplary substrate having an etched organic film with a pattern before etching. [Figure 4b] FIG. 4b is an exemplary substrate with an etched organic film having a pattern after etching. [Figure 5a] FIG. 5a is a cross-sectional side view of an exemplary stack of layers having multiple materials. [Figure 5b] FIG. 5b is a cross-sectional side view of the exemplary stack of layers having multiple materials of FIG. 5a showing one of the materials being selectively etched. [Figure 5c] FIG. 5c is a cross-sectional side view of the exemplary stack of layers having multiple materials of FIG. 5a illustrating successive etching steps. [Figure 5d] FIG. 5d is a cross-sectional side view of the exemplary stack of layers having multiple materials of FIG. 5a illustrating a repetition of the etching process. [Figure 6a] FIG. 6a is an SEM image of a cross section of the substrate after plasma etching (a) using the process conditions of Example 1. [Figure 6b] FIG. 6b is an SEM image of a cross section of the substrate after plasma etching (a) using the process conditions of Comparative Example 1. [Figure 6c] FIG. 6c is an SEM image of a cross section of the substrate after plasma etching (a) using the process conditions of Example 2. [Figure 6d] FIG. 6d is an SEM image of a cross section of the substrate after plasma etching (a) using the process conditions of Comparative Example 2. [Figure 7a] FIG. 7a is an SEM image of a cross section of the substrate after plasma etching (a) using the process conditions of Example 3. [Figure 7b] FIG. 7b is an SEM image of a cross section of the substrate after plasma etching (a) using the process conditions of Comparative Example 3. [Figure 7c] FIG. 7c is an SEM image of a cross section of the substrate after plasma etching (a) using the process conditions of Comparative Example 4. [Figure 8a] FIG. 8a is an SEM image of a cross section of the substrate after plasma etching (a) using the process conditions of Example 4. [Figure 8b] FIG. 8b is an SEM image of a cross section of the substrate after plasma etching (a) using the process conditions of Comparative Example 5. [Figure 8c] FIG. 8c is an SEM image of a cross section of the substrate after plasma etching (a) using the process conditions of Comparative Example 6. [Figure 9] FIG. 9 is an SEM image of a cross section of a substrate after plasma etching (a) using the process conditions of Example 8. [Figure 10] FIG. 10 is an SEM image of a cross section of a substrate after plasma etching (a) using the process conditions of Example 9. [Figure 11] FIG. 11 is an SEM image of a cross section of a substrate after plasma etching (a) using the process conditions of Example 10. [Figure 12] FIG. 12 is an SEM image of a cross section of a substrate after plasma etching (a) using the process conditions of Example 11. [Figure 13] FIG. 13 is the estimated etch rate as a function of O 2 flow rate for substrates containing one of the following plasma etch materials: SiO 2 , Si 3 N 4 , aC, poly-Si, and W (Example 12). [Figure 14] FIG. 14 is an estimated etch rate as a function of C5H9F5Si flow rate for substrates containing one of the following plasma etch materials: SiO2, Si3N4, aC, poly-Si, and W (Example 13). [Figure 15] FIG. 15 is the estimated etch rate as a function of C4H9F3Si flow rate for substrates containing one of the following plasma etch materials: SiO2, Si3N4, aC, poly-Si, and W (Example 14). [Figure 16]FIG. 16 shows the estimated etch rate as a function of CH2F2 flow rate for substrates containing one of the following plasma etch materials: SiO2, Si3N4, aC, poly-Si, W, SiC, SiCN, SiON (Example 15). [Figure 17] FIG. 17 shows the estimated etch rate as a function of C4H9F3Si flow rate for substrates containing one of the following plasma etch materials: SiO2, Si3N4, aC, poly-Si, W, SiC, SiCN, SiON (Example 16). [Figure 18] FIG. 18 is the estimated etch rate as a function of C2H6F2Si flow rate for substrates containing one of the following plasma etch materials: SiO2, Si3N4, aC, poly-Si, and W (Example 17). [Figure 19] FIG. 19 is the estimated etch rate as a function of CH 3 F 3 Si flow rate for substrates containing one of the following plasma etch materials: SiO 2 , Si 3 N 4 , aC, poly-Si, and W (Example 18). [Figure 20] FIG. 20 shows the estimated etch rate of O 2 flow rates for substrates containing one of the following plasma etch materials: SiO 2 , Si 3 N 4 , aC, poly-Si, and W (Example 19). [Figure 21] FIG. 21 is the estimated etch rate as a function of O 2 flow rate for substrates containing one of the following plasma etch materials: SiO 2 , Si 3 N 4 , aC, W-doped aC, poly-Si, and W (Example 20). [Figure 22] FIG. 22 shows the estimated etch rate as a function of O 2 flow rate for substrates containing one of the following plasma etch materials: SiO 2 , Si 3 N 4 , aC, W-doped aC, poly-Si, and W (Comparative Example 7). [Figure 23] FIG. 23 is the estimated etch rate as a function of O 2 flow rate for substrates containing one of the following plasma etch materials: SiO 2 , Si 3 N 4 , aC, poly-Si, and W (Example 21). [Figure 24]FIG. 24 is the estimated etch rate as a function of O 2 flow rate for substrates containing one of the following plasma etch materials: SiO 2 , Si 3 N 4 , aC, poly-Si, and W (Example 22). [Figure 25] FIG. 25 is the estimated deposition rate as a function of O 2 flow rate for substrates containing one of the following plasma etch materials: SiO 2 , Si 3 N 4 , aC, poly-Si, and W (Example 23). [Figure 26] FIG. 26 is the estimated deposition rate as a function of C5H9F5Si flow rate for substrates containing one of the following plasma etch materials: SiO2, Si3N4, aC, poly-Si, and W (Example 24). [Figure 27] FIG. 27 is the estimated polymer deposition rate as a function of C5H9F5Si flow rate for substrates containing one of the following plasma etch materials: SiO2, Si3N4, aC, poly-Si, and W (Example 25). [Figure 28] FIG. 28 is the estimated deposition rate as a function of O 2 flow rate for substrates containing one of the following plasma etch materials: SiO 2 , Si 3 N 4 , aC, poly-Si, and W (Example 26). [Figure 29] FIG. 29 is the estimated deposition rate as a function of C4H9F3Si flow rate for substrates containing one of the following plasma etch materials: SiO2, Si3N4, aC, poly-Si, W, SiC, SiCN, SiON (Example 27). [Figure 30] FIG. 30 is the estimated deposition rate as a function of CH2F2 flow rate for substrates containing one of the following plasma etch materials: SiO2, Si3N4, aC, poly-Si, W, SiC, SiCN, SiON (Example 28). [Figure 31] FIG. 31 is the estimated deposition rate as a function of C4H9F3Si flow rate for substrates containing one of the following plasma etch materials: SiO2, Si3N4, aC, poly-Si, W, SiC, SiCN, SiON (Example 29). [Figure 32]FIG. 32 shows the thickness results for SiO2, Si3N4, aC, poly-Si, W, SiC, SiCN, and SiON films after the cyclic etching process as a function of the number of cycles (Example 30). [Figure 33] FIG. 33 shows the estimated thickness results (reflecting etching of the film or deposition of polymer on the surface of the film) of the studied material film for the same Si3N4 thickness shown in FIG. 32 when a continuous infinite selectivity etching recipe for Si3N4 is used instead of the cyclical process. [Figure 34] FIG. 34 summarizes the thickness results of Pt, aC, poly-Si, and SiC films after a single etching cycle as described in Example 31 and the sequential process as described in Example 32. [Figure 35] FIG. 35 is an exemplary etching gas supply apparatus or system. DETAILED DESCRIPTION OF THE INVENTION
[0066] Disclosed is a plasma dry etching method or process using vapor of a Si-containing hydrofluorocarbon etching compound, preferably a methylsilyl hydrofluorocarbon etching compound, as an etching gas for plasma etching processes, including, but not limited to, high aspect ratio (HAR) plasma etching processes, selective plasma etching processes, and cyclical plasma etching processes for fabricating semiconductor structures such as 3D NAND structures, contact holes, and DRAM capacitors. The disclosed plasma dry etching method etches away silicon-containing films, organic films, metal-containing films, and the like, and provides a novel chemical approach for controlling the profile of the structures formed in the plasma etching process. Sidewall protection by controlling plasma-deposited polymers during plasma dry etching is an important mechanism for maintaining a defined profile without distortion. The disclosed plasma dry etching method also provides a novel chemical approach for controlling the profile of plasma-deposited polymers during the plasma etching process. Furthermore, the use of the disclosed Si-containing hydrofluorocarbon compounds in cyclical plasma etching processes can enhance control of the shape or profile of the etched structures while maintaining comparable etch rates.
[0067] The disclosed methods of plasma dry etching include a method for selectively HAR plasma dry etching silicon-containing films over patterned mask layers using the disclosed Si-containing hydrofluorocarbon etch compounds, preferably methylsilyl hydrofluorocarbon etchants, a method for selective plasma dry etching silicon-containing films over other non-etch films, a method for selective plasma dry etching organic films or metal-containing films over other non-etch films, and a method for cyclically selective plasma dry etching silicon-containing films, organic films, and metal-containing films over other non-etch films.
[0068] Most semiconductor devices are formed using processes that form thin films on substrates and pattern those films to accommodate desired structures and devices. Patterning includes lithography processes that can define the formed pattern and etching processes that are used to remove unwanted material or films from the substrate through the formed pattern. One commonly used etching process is plasma dry etching, where the substrate is exposed to plasma or reactive species formed inside a process chamber. The combination of physical (e.g., sputtering due to ion bombardment) and chemical (e.g., surface interaction with reactive species) mechanisms in plasma etching allows for the selective and preferential etching of certain materials over other materials, depending on the chemistry and process conditions used.
[0069] Disclosed herein is a selective plasma etching process, which is one of the key processes for patterning thin films during the fabrication of advanced semiconductor devices. The selective plasma etching process can selectively etch unwanted materials vertically, such as in 3D NAND structures and contact holes, and horizontally, such as in multiple materials at the surface of a substrate. Plasma etching is used in almost every step of semiconductor chip manufacturing that requires patterning (e.g., front-end of the line, back-end of the line, and mid-end of the line). The most important parameters of plasma etching are etch rate (to maintain high throughput during semiconductor device fabrication), selectivity (to reduce damage or unintentional modification of unetched films), ongoing process development to achieve high etch rates while maintaining high selectivity, and an increasing portfolio of etch materials / gases that can be selectively processed with each other.
[0070] In particular, in some cases it is possible to achieve so-called infinite selective etching, when the material to be etched is etched but some polymer is deposited on the non-etched material and protects it from etching.
[0071] Typically, achieving infinite selectivity results in a slower etch rate compared to processes with lower selectivity. Additionally, if a long etching process is required, infinite selectivity can result in the deposition of thick polymer films on the surfaces of the non-etched materials, the electrodes of the plasma etching device, and the plasma etching chamber itself, necessitating further processing or cleaning to remove the deposited polymer film. In some cases, polymer deposition can limit the applicability of infinite selectivity etching processes. A possible solution to the problem of excess polymer deposition during etching with infinite selectivity is to use a cyclic etching process that removes the unwanted deposited polymer between one of the steps in the etching cycle. The method disclosed herein includes a cyclic etching process characterized by introducing a Si-containing hydrofluorocarbon into at least one of the steps in the etching cycle, which allows the material to be etched to be highly selective to the non-etched material, and allows the non-etched material and the chamber walls to remain close to their initial state after the cyclic etching process.
[0072] The disclosed Si-containing hydrofluorocarbon compounds have the general formula: C x H y F z Si n (I) (1≦x≦6, 1≦y≦9, 1≦z≦15, n=1 or 2).
[0073] In some embodiments, the Si-containing hydrofluorocarbon compound of formula (I) can be a methylsilyl hydrofluorocarbon containing one or more methyl groups.
[0074] In some embodiments, the Si-containing hydrofluorocarbon compound of formula (I) can be a methylsilyl hydrofluorocarbon containing one or more methyl groups, at least one of which is bonded to a Si atom.
[0075] In some embodiments, the Si-containing hydrofluorocarbon compound of formula (I) can be a methylsilyl hydrofluorocarbon containing one or more methyl groups, none of which is bonded to a Si atom.
[0076] In some embodiments, the Si-containing hydrofluorocarbon compound may not contain a methyl group.
[0077] The disclosed Si-containing hydrofluorocarbon compounds can be used to enhance the passivation process during HAR etching. A key feature of the disclosed Si-containing hydrofluorocarbon compounds is at least one methyl group bonded to the Si atom, which promotes the formation of Si-containing species and Si-containing polymers at the surface of the substrate under plasma conditions. Figure 1 shows the signals for exemplary Si-containing hydrofluorocarbon compounds, trimethyl(trifluoromethyl)silane (C4H9F3Si) and pentafluoroethyl(trimethyl)silane (C5H9F5Si), recorded using a quadrupole mass spectrometer in residual gas analysis mode with an electron energy of 20 eV during scanning. As shown, dissociation of C4H9F3Si and C5H9F5Si primarily results in the formation of C3H9Si, C2H6FSi, C3H9FSi, CH5Si, and C2F4 fragments. All of the Si-containing fragments observed in the spectra have methyl groups attached to the Si atom: three methyl groups in the case of CHSi, two methyl groups in the case of CHFSi, three methyl groups in the case of CHFSi, and one methyl group in the case of CHSi. Therefore, in the presence of plasma, the formation of radicals with at least one methyl group attached to the Si atom is expected through electron impact dissociation, collisional dissociation, and vibrational excitation. All of the Si-containing radicals with methyl groups produced by dissociation of the initial Si-containing hydrofluorocarbons are effective in forming Si-containing films on all surfaces of the substrate. In this case, CF is typically one of the fragments produced by dissociation of common fluorocarbon gases (e.g., CF and CF) and may be valuable for etching processes.
[0078] The robust polymer-rich deposition on the surface of the substrate achieved by the use of Si-containing hydrofluorocarbons can be used to facilitate the passivation process during HAR etching. Thus, vapor of any Si-containing hydrofluorocarbon compound encompassed by formula (I) having at least one methyl group bonded to Si, such as CH4F2Si, CH3F3Si, CH2H6F2Si, CH9FSi, CH9F3Si, CH5H9F5Si, CH4F5Si,10 F4Si2, C2H6F4Si2, C3H9F3Si2, and C6H9F7Si can be used for selective plasma etching. While Si-containing hydrofluorocarbons with at least one methyl group bonded to Si can be used to deposit robust polymers at high deposition rates, the presence of Si atoms in the hydrofluorocarbon generally results in the deposition of more robust polymers compared to commonly used hydrofluorocarbon or fluorocarbon gases due to the incorporation of Si into the deposited polymer, even when there are no methyl groups bonded to silicon, or even when the Si-containing hydrofluorocarbon molecule contains a methyl group not bonded to a Si atom.
[0079] Exemplary disclosed Si-containing hydrofluorocarbon etching compounds are listed in Table 1, along with their structural formulas, CAS numbers, and boiling points. These molecules are commercially available or can be synthesized by methods known in the art. The disclosed Si-containing hydrofluorocarbon etching compounds can also include their isomers.
[0080] As summarized in Table 1, not only Si-containing hydrofluorocarbons with a methyl group bonded to Si, such as C4H9F3Si and C5H9F5Si, can be used in plasma etching processes, but also their isomers and isomers of other Si-containing hydrofluorocarbons with at least one methyl group bonded to Si, such as CH4F2Si, CH3F3Si, C2H6F2Si, C3H9FSi, C4H9F3Si, C5H9F5Si, C6H9F7Si, and C4H 10 F4Si2, a molecular formula from the list C2H6F4Si2 that can be used in plasma etching processes.
[0081] Furthermore, in addition to the Si-containing hydrofluorocarbons containing methyl groups and having at least one methyl group bonded to the Si atom that are used as etching gases in dry etching processes, vapors of Si-containing hydrofluorocarbons that may not have an isomer in which at least one methyl group is bonded to the Si atom, or vapors of Si-containing hydrofluorocarbons that may not have an isomer having one or more methyl groups, can be used, for example, CHF3Si, CH2F2Si, CH3FSi, CHF5Si, CH2F4Si, C2HF7Si, C2H2F6Si, C2H3F5Si, C2H4F4Si, C2H4F2Si, C2H3F3Si, C2H2F4Si, C2HF5Si, C3H4F6Si, C3HF9Si, C3HF7Si, C3H3F5Si, C3H4F4Si, C3H5F3Si, C4H5F7Si, C4H3F9Si, C4H2F 10 Si, C4HF 11 Si, C5H8F6Si, C5H7F7Si, C6HF 15 Si, C6H4F 12 Si and C6H7F9Si can be used as etching gases in dry etching processes. Furthermore, Si-containing hydrofluorocarbons include CH5FSi2, CH3F3Si2, CH2F6Si2, C2H7F3Si2, C2H9FSi2, C2H4F6Si2, C2HF7Si2, C2H2F6Si2, C2H3F5Si2, C2H4F4Si2, C3H4F8Si2, C3H6F4Si2, and C4H 10 F4Si2, C4H6F6Si2, C4H 11Some of the Si-containing hydrofluorocarbons may contain two Si atoms, such as FSi2 and C4H8F2Si2, which may not have an isomer with a methyl group bonded to the Si atom. The Si-containing hydrofluorocarbons described above can be used as etching gases in dry etching processes due to the presence of Si atoms in the hydrofluorocarbons, which can deposit more robust polymers compared to commonly used hydrofluorocarbon or fluorocarbon gases, even in the absence of methyl groups bonded to silicon, due to the incorporation of Si into the deposited polymer. As described above, other Si-containing hydrofluorocarbons that do not have an isomer with a methyl group bonded to Si, or that do not have an isomer with a methyl group, can be used as etching gases in dry etching processes to improve selectivity and etch profile control in the case of HAR etching.
[0082] [Table 1]
[0083] [Table 2]
[0084] [Table 3]
[0085] [Table 4]
[0086] [Table 5]
[0087] [Table 6]
[0088] Considering the examples of Si-containing hydrofluorocarbon etching compounds and their isomers listed in Table 1, as well as the discussion in the Examples below, it can be summarized that any Si-containing hydrofluorocarbon vapor and Si-containing hydrofluorocarbon can be used as an etching gas, particularly any Si-containing hydrofluorocarbon encompassed by formula (I), in a plasma etching process. Preferably, the Si-containing hydrofluorocarbon has at least one methyl group attached to the Si atom, as this can deposit a robust polymer and enhance the selectivity of the etching process.
[0089] The disclosed Si-containing hydrofluorocarbon compounds encompassed by formula (I) include CH4F2Si, CH3F3Si, C2H6F2Si, C3H9FSi, C4H9F3Si, C5H9F5Si, C4H 10 These include F4Si2, C2H6F4Si2, C3H9F3Si2, C6H9F7Si, or their isomers.
[0090] The disclosed Si-containing hydrofluorocarbon compounds are CH3F3Si, C2H6F2Si, C4H9F3Si, C5H9F5Si, or isomers thereof.
[0091] The disclosed Si-containing hydrofluorocarbon compound is CH3F3Si, or an isomer thereof.
[0092] The disclosed Si-containing hydrofluorocarbon compound is C2H6F2Si, or an isomer thereof.
[0093] The disclosed Si-containing hydrofluorocarbon compound is C4H9F3Si, or an isomer thereof.
[0094] The disclosed Si-containing hydrofluorocarbon compound is C5H9F5Si, or an isomer thereof.
[0095] In some embodiments, the disclosed Si-containing hydrofluorocarbon compounds and their isomers are encompassed by formula (I) but do not contain a methyl group. Compounds of this type include CHFSi, CHFSi, CHFSi, CHFSi, CHHFSi, CHFSi, CHFSi, CHFSi, CHFSi, CHFSi, CHFSi, CHFSi, CHFSi, CHFSi, CHFSi, CHFSi, CHFSi, CHFSi, CHF 10 Si, C4HF 11 Si, C5H8F6Si, C5H7F7Si, C6HF 15 Si, C6H4F 12 Some of the isomers of Si, C6H7F9Si, may be included, which may be used as etching gases in the disclosed plasma dry etching process, even though they do not contain a methyl group.
[0096] The boiling point of the disclosed Si-containing hydrofluorocarbon compound can be in the range of about -50°C to about 250°C, preferably in the range of about -30°C to about 200°C, more preferably in the range of about -20°C to about 150°C. Even more preferably, the boiling point of the disclosed Si-containing hydrofluorocarbon compound can be in the range of about 20°C to about 150°C.
[0097] The disclosed Si-containing hydrofluorocarbon etching compounds are provided with a purity of greater than 95% v / v, preferably greater than 99.99% v / v, and more preferably greater than 99.999% v / v. The disclosed Si-containing hydrofluorocarbon etching compounds contain less than 5% by volume of trace gas impurities, and the trace gas impurities include less than 150 ppm by volume of impurity gases such as N2 and / or HO and / or CO2. Preferably, the water content in the plasma etching gas is less than 20 ppm by weight. Purified products can be produced by distillation and / or passing the gas or liquid through a suitable adsorbent, such as a 4 Å molecular sieve. The disclosed Si-containing hydrofluorocarbon etching compounds contain less than 10% v / v, preferably less than 1% v / v, more preferably less than 0.1% v / v, and even more preferably less than 0.01% v / v of any of their isomers, which can be purified by distilling the gas or liquid to remove the isomers, resulting in good process reproducibility.
[0098] Alternatively, the disclosed Si-containing hydrofluorocarbon etching compounds can contain 0.01% v / v to 99.99% v / v of an isomer of interest, particularly when the isomer mixture provides improved process parameters or when isolation of the isomer is too difficult or expensive. The isomer mixture can also reduce the need for two or more gas lines to the reaction chamber. Some of the disclosed Si-containing hydrofluorocarbon etching compounds are gases at room temperature and atmospheric pressure. For non-gaseous (i.e., liquid or solid) compounds, these gases can be formed by vaporizing the compound using conventional evaporation processes, such as direct evaporation, or by bubbling with an inert gas (e.g., N, Ar, He). Non-gaseous compounds can be supplied in liquid form to an evaporator, where they are vaporized and then introduced into the reactor.
[0099] In the disclosed method of plasma dry etching, the plasma etching gas is a gas mixture containing at least one of the following substances: a Si-containing hydrofluorocarbon, an oxidizing gas, an inert gas, a fluorocarbon and / or hydrofluorocarbon-based chemical, or another additional gas. The inert gas can be selected from He, Ar, Kr, Xe, or Ne; the oxidizing gas can be selected from O, O, CO, CO, COS, SO, SO, FNO, NO, NO, NO, NO, or H2O; and the additional gas can be selected from H, SF, NF, N, NH, Cl, BCl, BF, Br, F, HBr, HCl, or a combination thereof. The Si-containing hydrofluorocarbon is preferably a hydrofluorocarbon compound gas containing a Si atom with at least one methyl group (—CH) attached to the Si atom, forming molecular fragments containing Si atoms with several methyl groups attached to facilitate the deposition process on non-etched materials to enhance selectivity. This is preferable because it allows etching of a list of materials to be etched while depositing on other non-etched materials (implying infinite selectivity). Furthermore, in the disclosed plasma etching method, the Si-containing hydrofluorocarbon is preferably a gas of a compound represented by formula (I). The use of an inert gas is intended to promote plasma generation and ion bombardment during the etching process, and depending on the gas ratio, it promotes or suppresses dissociation of other gases in the etching gas mixture, thereby directly affecting the etching rate and anisotropy of the etching process. The addition of an oxidizing gas to the etching gas mixture can improve the etching rate, promote isotropic etching and surface or gas-phase chemical reactions, and improve the selectivity of the etching process, depending on the etching gas mixture and the type of etching and non-etching materials. The aforementioned additional gases can improve process control or increase the etching rate. Fluorocarbon or hydrofluorocarbon gases can promote both the anisotropic etching process of etching films and vertical surfaces and / or passivation of non-etched films.Examples of fluorocarbon gases that can be used in the disclosed plasma etching method include, but are not limited to, CF4, C2F6, C3F6, C4F6, C4F8, C5F8, and C5F. 10 , C6F 12 , C7F 14 , C8F 16 Examples of hydrofluorocarbon gases that can be used in the disclosed plasma etching methods include, but are not limited to, CH2F2, CH3F, CHF3, C2H5F, C3H7F, C5HF7, C3H2F6, C3H4F2, C3H2F4, C4H2F6, C4H3F7, and the like.
[0100] Under plasma conditions, various reactive species and ions are generated directly by the dissociation of these compounds and chemical reactions due to interactions between species present in the gas phase. Typically, plasma etching effects can be achieved using any of the compounds represented by the above formulas, whether used individually or in mixtures with each other. Depending on the structure of each compound, etching performance (including increasing the etch rate of certain etching materials) or passivation during high aspect ratio etching processes can be enhanced. In particular, a mixture of CF and CF is one of the commonly used mixtures, since CF is efficient at promoting passivation and CF is efficient at increasing the etch rate, resulting in a highly anisotropic etching process, as described in Comparative Example 6 below. Furthermore, if necessary, a hydrofluorocarbon gas such as CHF can be added to enhance the etch rate of silicon nitride films.
[0101] To achieve HAR of the etched structures and improve etch selectivity for a particular material or film while maintaining a high etch rate, etch gases can be selected to preferentially produce volatile by-products with the etched material without reacting with the non-etched material to form less volatile by-products. Throughout the disclosed methods of plasma dry etching, it has been discovered that the addition of Si-containing hydrofluorocarbons encompassed by formula (I) to the process etch gas mixture can dramatically improve selectivity and aspect ratio during etching of Si-containing compound materials.
[0102] In the plasma etching process disclosed herein, chemical reaction-based etching can be combined with physical sputtering due to ion bombardment. Gases used in plasma etching are typically dissociated by the plasma, resulting in the presence of numerous reactive species capable of deposition, etching, or surface functionalization. This provides a further method of selective etching, in which material is removed while depositing some film on the non-etched material. This approach can achieve high selectivity during the etching process, and the deposited film can be removed either after or during the etching process.
[0103] The disclosed plasma etching method uses Si-containing hydrofluorocarbons in the etching gas mixture to achieve high or even infinite selectivity of the material being etched relative to other non-etched materials while maintaining a relatively high etch rate. Selectivity is achieved by depositing a robust polymer on the non-etched material while preventing the polymer from depositing on (or reacting with) the material being etched. The ability to deposit a robust polymer during the etching process is attributed to the dissociation of the Si-containing hydrofluorocarbon to form a Si-containing fragment with a methyl group directly bonded to the Si atom. Molecules containing Si and a methyl group, where the methyl group is bonded to the Si atom, are commonly used as precursors for the deposition of Si-containing films, which correlates well with the results observed in the disclosed method, for example, using trifluoromethylsilane (C4H9F3Si), where the trimethylsilane fragment (C3H9Si) is generated by dissociation of the parent molecule in the plasma due to the weak bond between the Si atom and the trifluoromethyl group in the trimethylsilane molecule.
[0104] Various disclosed methods of plasma dry etching that apply the above description are described herein below.
[0105] HAR plasma dry etching In some embodiments, the disclosed methods of plasma dry etching silicon-containing films are applied to etch substrates having one or more treated or etched films (e.g., silicon oxide, silicon nitride, or a combination thereof) and one or more non-etched films (e.g., amorphous carbon, amorphous silicon, doped amorphous carbon, doped amorphous silicon, metal, etc.) in HAR etching processes for fabricating semiconductor structures such as, but not limited to, 3D NAND structures, contact holes, DRAM capacitors, etc. The disclosed methods of plasma dry etching one or more treated films to form HAR apertures in a substrate include: loading a substrate onto a loading table within a processing or reaction chamber, the substrate having one or more processing films deposited thereon and a non-etching film deposited on the one or more processing films; introducing an etching gas comprising a Si-containing hydrofluorocarbon vapor into a processing chamber; igniting the etching gas to generate a plasma; and causing an etching reaction between the plasma and the one or more treatment films to etch the one or more treatment films relative to the non-etching film, thereby forming an aperture.
[0106] One or more treatment films may be Si a O b C c N d H e where a, b, c, d, and e are in the range of 0.1 to 6, and b, c, d, and e can each independently be 0. Additionally, one or more of the treatment films can include dopants such as B, C, P, As, Ga, In, Sn, Sb, Bi, and / or Ge. The non-etch film can be, for example, a patterned hard mask layer of amorphous carbon, amorphous silicon, doped amorphous carbon, doped amorphous silicon, a metal, or the like.
[0107] As used herein, the term "high aspect ratio aperture" or "HAR aperture" refers to the formation of an aperture pattern in a film to be etched by the disclosed plasma etching method when the aspect ratio of the formed aperture structure exceeds a value of 5. Achieving HAR in the etched aperture requires high anisotropy of the plasma etching process (preferentially etching the exposed target material in a substantially vertical direction) (see FIG. 2b). To achieve anisotropy in the etching, i.e., directional vertical etching with minimal lateral etching, polymer typically forms on the sidewalls of the etched structure or aperture. The preferential formation of polymer on the sidewalls of the etched structure is achieved by competition between the etching process (polymer removal) and the deposition process (polymer formation). The presence of directional (vertical) etching by ion bombardment allows for more effective removal of polymer from horizontal surfaces than vertical surfaces, thereby promoting polymer formation on the vertical sidewalls. Furthermore, by fine tuning the etching and deposition processes, preferential etching of the substrate in the vertical direction can be achieved while lateral etching is suppressed, thereby preserving the horizontal dimensions of the structure.
[0108] An example of the initial structure of a substrate, including a plasma-etched film with several openings and an unetched film, is shown in Figure 2a, and the HAR structure formed after the plasma etching process is shown in Figure 2b. As shown, a single-crystal silicon wafer 102 with the structure shown in Figure 2a formed on top was used as the substrate. A silicon dioxide film 104 with a unique thickness, such as 3000 nm (arrow 3), was used as the membrane. A patterned film of amorphous carbon 106 with a thickness, such as 868 nm (arrow 5), was used as the unetched material. The opening pattern in the amorphous carbon film (arrow 6) has a bottom diameter, such as approximately 120 nm. An example of the profile of the substrate after the etching process is shown in Figure 2b. Arrow 7 is the thickness of the unetched film 206 (here amorphous carbon) after the etching process, arrow 8 is the depth of the etched HAR hole in the plasma-etched film 204, arrow 9 is the diameter of the top of the HAR hole 208 in the plasma-etched film 204 (hereinafter "top CD"), arrow 10 is the diameter of the middle of the HAR hole 208 in the plasma-etched film 204 (hereinafter "middle CD"), and arrow 11 is the diameter of the HAR hole 208 at the bottom (hereinafter "bottom CD"), where "CD" stands for critical dimension.
[0109] The selection of etching gases and the ratio of each gas concentration in the etching gas mixture is necessary to achieve a balance between the deposition process to protect vertical surfaces (hereafter "passivation") and the etching process for anisotropic removal of material. Typically, a combination or mixture of etching gases is used, with each gas type playing a different role. The process etch gas mixture used in the disclosed method of plasma dry etching silicon-containing films can include at least one disclosed Si-containing hydrofluorocarbon (e.g., CH3F3Si, C2H6F2Si, C4H9F3Si, C5H9F5Si), at least one fluorocarbon or hydrofluorocarbon gas (e.g., C4F8, C4F6, CF4, CH2F2), optionally at least one inert gas (e.g., He, Ar, Kr, Xe, Ne), optionally an oxidizing gas (e.g., O2, O3, CO, CO2, COS, SO, SO2, FNO, NO, NO, NO2, H2O, Cl2, F2), and optionally an additional gas selected from H2, SF6, NF3, N2, NH3, Cl2, BCl3, BF3, Br2, F2, HBr, HCl, or combinations thereof, which are used to form reactive species and ions within the plasma. In addition, CF4, C2F6, C3F6, C4F6, C4F8, C5F8, C5F 10 , C6F 12 , C7F 14 , C8F 16 At least one fluorocarbon or hydrofluorocarbon gas selected from CH2F2, CH3F, CHF3, C2H5F, C3H7F, C5HF7, C3H2F6, C3H4F2, C3H2F4, C4H2F6, C4H3F7, and the like may be added to the etching gas mixture.
[0110] More specifically, the disclosed plasma etching method includes the following steps: In the first step, a substrate containing one or more films, optionally including a non-etched film, that can be patterned, i.e., have some pattern, such as openings or apertures, is placed on a loading table or substrate holder in a plasma etching chamber or reactor. The substrate can be any type of material to be etched, as long as it can be processed by plasma etching. For example, a single-crystal Si wafer containing at least one Si-containing film, an organic film, or a metal-containing film, or multiple films, some of which can be patterned. An example of a substrate with a patterned film and a non-etched film is shown in Figure 2a. The reactor includes a vessel capable of creating a low pressure within the vessel by evacuation, a plasma generator capable of generating a plasma within the reactor, and a substrate holder capable of holding a substrate within the reactor, where it is exposed to the plasma while its temperature is controlled using a cooling device or a gas flow, such as a helium flow. An etching gas mixture containing certain vapors or gases in specific proportions that can change during the etching process is then introduced into the reactor, and the pressure within the reactor is maintained at a predetermined value or at some other value that can change during the process. The etching gas mixture can be a Si-containing hydrofluorocarbon, or a Si-containing hydrofluorocarbon mixed with a hydrofluorocarbon or a fluorocarbon and / or an oxidizing gas and / or an inert gas. A plasma generator then applies a high frequency electromagnetic field to the etching gas mixture to generate a glow discharge. When the substrate is exposed to the plasma generated in the reactor, the film to be etched is removed by a combination of ion bombardment and interactions with reactive species, forming volatile by-products.
[0111] The disclosed plasma etching methods using the disclosed Si-containing hydrofluorocarbon compounds as etching gases produce apertures in silicon-containing films, such as channel holes, gate trenches, staircase contacts, capacitor holes, contact holes, contact etch, slit etch, self-aligned contacts, self-aligned vias, and supervias. The resulting apertures can have aspect ratios ranging from about 5:1 to about 500:1, preferably from about 20:1 to about 400:1, and diameters ranging from about 5 nm to about 500 nm, preferably less than 100 nm. For example, those skilled in the art will recognize that channel hole etching produces apertures in silicon-containing films with aspect ratios greater than 50:1.
[0112] Selective plasma dry etching of Si-containing films In some embodiments, the disclosed methods of plasma dry etching include selective plasma dry etching of silicon-containing films using the disclosed Si-containing hydrofluorocarbon etching compounds. The disclosed methods of selective plasma dry etching of silicon-containing films can process substrates having one or more films to be etched, such as silicon oxide, silicon nitride, or a combination thereof, and non-etch films, such as amorphous silicon, SiCN, SiC, doped amorphous silicon, etc., deposited thereon. The disclosed methods of selective plasma dry etching of silicon-containing films provide a process for etching Si-containing materials or films with high selectivity relative to other materials or films. The disclosed methods of selective plasma dry etching of silicon-containing films can be isotropic and anisotropic etching applied to form 2D and 3D active devices in logic substrates, such as FinFETs, gate-all-around (GAA)-FETs, or fork-sheet FETs.
[0113] The disclosed method for selective plasma dry etching of silicon-containing films provides a novel chemical approach to increasing the selectivity of the material to be etched relative to the non-etched material by promoting polymer formation in the non-etched material using the addition of a Si-containing hydrofluorocarbon to the etching gas mixture. The disclosed plasma etching method maintains an adequate etch rate for the material to be etched while inhibiting the etching of the non-etched material by depositing a polymer thereon, resulting in high or even infinite selectivity. In particular, it is demonstrated that silicon-containing films such as SiO2 and Si3N4 can be etched with infinite selectivity to each other and to amorphous carbon, polycrystalline silicon, W, SiC, SiON, and SiCN, materials commonly used in multi-color etching and advanced patterning. Examples 12-18 below are promising for the selective etching of Si-containing compounds. The disclosed method for selective plasma dry etching of Si-containing films to form structures on a substrate includes: introducing a vapor of a Si-containing hydrofluorocarbon into a reaction chamber containing a substrate having a pattern comprising one or more treatment films and at least one non-etch film deposited thereon; igniting the plasma to produce activated Si-containing hydrofluorocarbons; and (b) allowing an etching reaction to proceed between the activated Si-containing hydrofluorocarbon and the one or more treated films, thereby selectively etching the one or more treated films relative to at least one non-etched film.
[0114] One or more treatment films may be Si a O b C c N d H ewhere a, b, c, d, and e range from 0.1 to 6, and b, c, d, and e can each independently be 0. One or more of the treatment films can also contain dopants such as B, C, P, As, Ga, In, Sn, Sb, Bi, and / or Ge. The non-etch film can be any other material used in the fabrication of semiconductor devices at a particular level, such as organic films (aC or doped aC films, a-Si, photoresist (PR), etc.), metal films, metal-containing films, etc. The non-etch film is different from the silicon-containing film to be etched, but has the same formula as the silicon-containing film to be etched, i.e., Si a O b C c N d H e (a, b, c, d, and e are in the range of 0.1 to 6, and b, c, d, and e may each independently be 0).
[0115] An example of the initial structure of a substrate with multiple films, including plasma-etched and non-etched films with some openings, is shown in FIG. 3a, and the structure formed after the selective plasma etching process is shown in FIG. 3b. As shown, a single-crystal silicon wafer 302 with a multiple-film structure formed thereon can be used as the substrate shown in FIG. 3a. Multiple films 304 (e.g., 304a, 304b, 304c, 304d, and 304e) are deposited on the single-crystal silicon wafer 302, and one of the multiple films 304 is used as the non-etched material. A patterned film of amorphous carbon 306 is used as the non-etched material. The opening pattern in the amorphous carbon film allows portions of the multiple films 304 to be exposed to the etching gas. An example profile of the substrate after the selective etching process is shown in FIG. 3b, where film 404c is selectively etched relative to the other films 404a, 404b, 404d, and 404e.
[0116] Specifically, the disclosed method is directed to selectively etching specific Si-containing compounds (e.g., silicon oxide, silicon nitride) relative to all other materials used in the fabrication of semiconductor devices at a specific level (e.g., front-end or mid-end of the line) using a gas mixture containing at least one of the following substances: a process etch gas mixture containing at least one Si-containing hydrofluorocarbon, an inert gas, an oxidizer, optionally fluorocarbons and / or hydrofluorocarbons, and additional gases. The use of silicon-containing hydrofluorocarbons in the process etch gas mixture can achieve high or even infinite selectivity of silicon-containing films relative to other materials while maintaining a relatively high etch rate. The at least one Si-containing hydrofluorocarbon is encompassed by formula (I). The inert gas can be selected from He, Ar, Kr, Xe, and Ne. The oxidizing gas can be selected from O2, O3, CO, CO2, SO2, SO2, FNO, NO, NO2, NO2, HO, H2, or NO2. The additional gas can be any of the following gases: H2, SF6, NF3, N2, NH3, Cl2, BCl3, BF3, Br2, F2, HBr, HCl, or a combination thereof. Optionally, the fluorocarbon and / or hydrofluorocarbon is CF4, C2F6, C3F6, C4F6, C4F8, C5F8, C5F 10 , C6F 12 , C7F 14 , C8F 16 , CH2F2, CH3F, CHF3, C2H5F, C3H7F, C5HF7, C3H2F6, C3H4F2, C3H2F4, C4H2F6, C4H3F7, etc. The selectivity of the etched film relative to at least one non-etched film may be greater than 5, preferably greater than 10.
[0117] As mentioned above, for example, when trifluoromethylsilane (C4H9F3Si) is used, dissociation of the parent molecule in the plasma due to the weak bond between the Si atom and the trifluoromethyl group in the trimethylsilane molecule generates trimethylsilane fragments (C3H9Si), which allows for the deposition of the polymer in Example 14, which results in the infinite selectivity discussed in this disclosure.
[0118] Selective plasma dry etching of organic or metal-containing films In some embodiments, the disclosed methods of plasma dry etching include selective plasma dry etching of organic or metal-containing films using the disclosed Si-containing hydrofluorocarbon etching compounds. The disclosed methods of selective plasma dry etching of organic or metal-containing films etch a substrate having one or more etching films (e.g., amorphous carbon and W-doped amorphous carbon) and non-etching films (e.g., polycrystalline silicon, silicon nitride, silicon oxide, metal, etc.) deposited thereon. In particular, the disclosed selective etching methods are aimed at selectively etching specific organic materials (e.g., aC and doped aC, a-Si, PR, etc.) or metal-containing films relative to all other materials (e.g., Si-containing films, doped Si-containing films, etc.) used in the fabrication of semiconductor devices at a specific level (e.g., front-end or mid-end of the line) using at least one Si-containing hydrofluorocarbon, an oxidizer, an inert gas, and optionally a mixture of fluorocarbon and hydrofluorocarbon gases as etching gases. The disclosed methods of selective plasma dry etching of organic or metal-containing films include: introducing vapors of a Si-containing hydrofluorocarbon and an oxidizing gas and optionally an inert gas (He, Ar, Xe, Kr, Ne) into a reaction chamber containing a substrate having a pattern deposited thereon, the pattern comprising an organic film or a metal-containing film and at least one non-etching film; igniting a plasma to produce an activated Si-containing hydrofluorocarbon and an activated oxidizing gas; and a step of causing an etching reaction between the activated Si-containing hydrofluorocarbon and the activated oxidizing gas and the organic film or the metal-containing film to proceed, thereby selectively etching the organic film or the metal-containing film relative to at least one non-etched film.
[0119] Amorphous carbon and W-doped amorphous carbon are common materials for 3D NAND high-aspect-ratio etch masks, self-aligned patterning masks, and contact etch masks. The use of Si-containing hydrofluorocarbons can dramatically increase the selectivity of the etch process relative to other materials. Adding oxidizing gases (e.g., O2, O3, CO, CO2, SO2, SO2, FNO, NO, NO2O, NO2, HO, H2O, or NO2O) and / or inert gases (e.g., He, Ar, Kr, Xe, Ne) to the etch gas can promote polymer deposition on non-etched materials. The highly selective etching of amorphous carbon and W-doped amorphous carbon relative to non-etched films is promising for patterning and stripping organic masks and for patterning other materials on substrates.
[0120] Thus, the disclosed method of selective plasma dry etching of organic or metal-containing films can enable high selectivity of amorphous carbon and W-doped amorphous carbon over non-etched materials while maintaining high etch rates of organic or metal-containing materials present on the substrate or mask material to form patterns in the mask material without damaging the underlying materials.
[0121] The disclosed method for selective plasma dry etching of organic or metal-containing films can be used for forming patterns in organic hard masks, selectively etching for stripping or patterning other organic films on a substrate. The disclosed method for selective plasma dry etching of organic or metal-containing films is a method for processing substrates containing one or more films to be etched (e.g., amorphous carbon and doped amorphous carbon) and films to be etched (e.g., polycrystalline silicon, silicon nitride, silicon oxide, metal) when the etching gas mixture includes at least one Si-containing hydrofluorocarbon (C4H9F3Si), an inert gas (e.g., Ar), an oxidizing gas (e.g., O2), and an additional gas selected from H2, SF6, NF3, N2, NH3, Cl2, BCl3, BF3, Br2, F2, HBr, HCl, or a combination thereof, which are used to form reactive species and ions within the plasma. Here, hydrofluorocarbon or fluorocarbon gases do not necessarily need to be included in the etching gas mixture. The substrate can be any type of material that can be processed by plasma etching. The selectivity of etching an organic or metal-containing film relative to at least one non-etched film may be greater than 5, preferably greater than 10.
[0122] Depending on the etching process, selectivity to specific materials can be achieved by utilizing the physical or chemical properties of the materials present on the substrate and the etching gas. Adding a Si-containing hydrofluorocarbon to the etching gas mixture can dramatically increase selectivity during etching of organic materials or metal-containing films by depositing a polymer on the non-etching material. An example of the initial structure of a substrate with an organic etching film or metal-containing film and a non-etching film with several openings is shown in Figure 4a, and the high selectivity after the selective plasma etching process is shown in Figure 4b. As shown in Figure 4a, a single-crystal silicon wafer 502 with multiple film structures formed on top was used as the substrate. An underlayer 504 was deposited on the single-crystal silicon wafer 502, and a mask material layer 506 was deposited on top of the underlayer 504. A patterned initial mask 508, e.g., a photoresist layer on top of the mask material layer 506, was used as the non-etching material. The opening pattern in the patterned initial mask 508 allowed portions of the mask material layer 506 to be exposed to the etching gas. An example profile of the substrate after the selective etching process is shown in FIG. 4 b , where the mask material layer 606 is selectively etched relative to the patterned initial mask 608 .
[0123] Cyclic selective plasma dry etching In some embodiments, the disclosed methods of plasma dry etching include methods of cyclic selective plasma dry etching of silicon-containing and metal-containing films using the disclosed Si-containing hydrofluorocarbon etching compounds.
[0124] The disclosed method for cyclical selective plasma dry etching of silicon-containing or metal-containing films etches substrates containing one or more target films, such as metals (e.g., platinum), silicon oxide, silicon nitride, or combinations thereof, and non-etchable materials or films (e.g., amorphous silicon, SiCN, SiC, doped amorphous silicon), when an etching gas mixture containing at least one Si-containing hydrofluorocarbon, optionally an oxidizer, optionally a fluorocarbon or hydrofluorocarbon gas, and optionally at least one inert gas is used to generate reactive species and ions in at least one step of the cyclical plasma etching. The etching process is carried out in a cyclical manner, involving several etching steps that are repeated sequentially over time, where the conditions for each etching step can be varied depending on the number of cycles. The substrate can be any type of material that can be processed by plasma etching. The disclosed method for cyclical selective plasma dry etching of silicon-containing or metal-containing films achieves high selectivity to non-etched materials while maintaining high etch rate throughput for the film being etched and low rates of polymer deposition on the non-etched materials and the interior of the etch chamber using a cyclical etching process. The disclosed method for cyclical selective plasma dry etching of silicon-containing or metal-containing films can be used for forming structures by selective etching at the front end of the line, self-aligned multi-patterning, opening and etching hard masks, etc. The disclosed method for cyclical selective plasma dry etching of etched films (such as silicon-containing or metal-containing films) includes: i) introducing a first etching gas comprising vapor of a Si-containing hydrofluorocarbon compound into a reaction chamber containing a substrate having a pattern comprising an etched film and at least one unetched film deposited thereon; ii) applying power to generate a plasma of the activated first etching gas; iii) allowing an etching reaction to proceed between the activated first etching gas and the etching film, so that the etching film is selectively etched relative to at least one non-etching film, and simultaneously depositing a polymer on the at least one non-etching film by the activated first etching gas; iv) introducing a second etching gas into the reaction chamber; v) allowing an etching reaction to proceed between the activated second etching gas and both the etching film and the polymer deposited on the at least one non-etching film, thereby etching both the etching film and the polymer deposited on the at least one non-etching film; vi) repeating steps i) to v) until the etching film is removed.
[0125] Here, the first etching gas can include the disclosed Si-containing hydrofluorocarbon, one or more hydrofluorocarbons or fluorocarbons, an oxidizing gas, an inert gas, and / or an additional gas. The second etching gas can include one or more hydrofluorocarbons or fluorocarbons, an oxidizing gas, an inert gas, and / or an additional gas. The disclosed method for cyclically selective plasma dry etching of silicon-containing films can further include introducing a third etching gas after step v). Here, the third etching gas is the same as the second etching gas, which includes one or more hydrofluorocarbons or fluorocarbons, an oxidizing gas, an inert gas, and / or an additional gas. However, within a cycle or each cycle, the third etching gas and the second etching gas do not have the same combination of etching gas compositions. For example, if the second etching gas is a combination of CF, O, Ar, and CO, the third etching gas can be a combination of CH, F, O, Ar, and SF, or CH, F, O, He, and SF. A purge step is applied after each use of etching gas, i.e., a purge step is applied after steps iii) and v). During the purge, the power for generating the plasma can remain on or can be turned off. After the purge, the power for generating the plasma is turned on. Here, the one or more hydrofluorocarbons or fluorocarbons can be CF4, C2F6, C3F6, C4F6, C4F8, C5F8, C5F 10 , C6F 12 , C7F 14 , C8F 16 , CH2F2, CH3F, CHF3, C2H5F, C3H7F, C5HF7, C3H2F6, C3H4F2, C3H2F4, C4H2F6 or C4H3F7, the oxidizing gas can be selected from O2, O3, CO, CO2, SO, SO2, FNO, N2, NO, N2O, NO2, or H2O, COS, the inert gas can be selected from the group consisting of He, Ar, Xe, Kr or Ne, and the additional gas can be selected from H2, CO2, SF6, NF3, N2, NH3, Cl2, BCl3, HCl, HBr or Br2.
[0126] The possibility of polymer formation on the surface of a substrate, depending on the material being exposed, provides another method for highly selective etching, where some film is deposited on non-etching plasma-etched materials while material is removed during the etching process. This approach can achieve high selectivity, and the deposited film can be removed after the etching process or during etching if a cyclical process is used. The disclosed cyclical etching method improves the etch selectivity of the film being etched while maintaining a high etch rate and a low amount of polymer deposition on non-etched materials. The addition of Si-containing hydrofluorocarbons to the process gas mixture can dramatically improve selectivity during etching of Si-containing and / or metal-containing films, while the use of a cyclical process can significantly reduce polymer growth while maintaining a high etch rate.
[0127] The disclosed cyclical etching process refers to a process in which a substrate is processed in an etching chamber using sequentially repeated etching steps. Examples of substrates processed using cyclical etching are shown in Figures 5a-5d. Figure 5a shows an example of an initial substrate consisting of substrate 702 having multiple thin films thereon, where film 704 serves as a mask, films 706, 708, and 710 are films of non-etched material, and film 712 is a film of the material to be etched. Figure 5b shows the substrate after the first step of an etching cycle. During the first step, material is partially removed 716 using a selective etching recipe, resulting in the deposition of polymer 714 on the non-etched material, resulting in a mask with a polymer thickness depending on the film material. Figure 5c shows the substrate after the second step of the cycle. In the second step, an etching recipe with non-infinite selectivity to the polymer deposited during the first step was used, resulting in further etching of the material to be etched 718 and removal of the polymer from the non-etched material. As shown in FIG. 5d, depending on the non-etched material and process conditions, some polymer may remain in the non-etched material film 720, or some of the non-etched material film may be etched during a second step after completely removing the polymer (not shown).
[0128] The disclosed method for cyclically selective plasma dry etching of silicon-containing films includes using at least one Si-containing hydrofluorocarbon, optionally a mixture of an inert gas, an oxidizing gas, and a fluorocarbon and / or a hydrofluorocarbon gas as an etching gas to selectively etch specific materials, such as silicon nitride, silicon oxide, and aC-containing Si-containing films, relative to any other materials used in the fabrication of semiconductor devices at a specific level (e.g., front-end or mid-end of the line), while the etching process further includes several steps using various cyclically repeated etching recipes. The use of a cyclical etching process consisting of several steps can achieve high or infinite selectivity while depositing a small amount of polymer on the surface of the non-etched material or simply forming a thin film interface.
[0129] The disclosed cyclic plasma etching method can achieve preferential etching of Si-containing compounds with high selectivity over other materials, such as mask materials and non-etch materials, without altering the non-etch materials.
[0130] In the disclosed cyclic plasma etching method, the plasma etching gas is a gas mixture containing at least one of the following: a Si-containing hydrofluorocarbon, an inert gas, an oxidizer, a fluorocarbon and / or hydrofluorocarbon, and an additional gas. Again, the inert gas can be selected from He, Ar, Kr, Xe, Ne, the oxidizer can be selected from O2, O3, CO, CO2, COS, SO, SO2, FNO, NO, NO2O, NO2, NO2O, Cl2, F2, and the hydrofluorocarbon or fluorocarbon can be CF4, C2F6, C3F6, C4F6, C4F8, C5F8, C5F 10 , C6F 12 , C7F 14 , C8F 16, CH2F2, CH3F, CHF3, C2H5F, C3H7F, C5HF7, C3H2F6, C3H4F2, C3H2F4, C4H2F6 or C4H3F7, and the additional gas can be selected from H2, SF6, NF3, N2, NH3, Cl2, BCl3, BF3, Br2, F2, HBr, HCl or a combination thereof. The selectivity of the etched film relative to at least one non-etched film may be greater than 5, preferably greater than 10.
[0131] In summary, in the disclosed plasma dry etching methods described above, the etching gas mixture includes at least one disclosed Si-containing hydrofluorocarbon compound. Additionally, at least one hydrofluorocarbon or fluorocarbon gas, at least one oxidizing gas, at least one inert gas, and / or at least one additional gas can be added to the disclosed Si-containing hydrofluorocarbon compound prior to etching to form the etching gas mixture. In some embodiments, the at least one hydrofluorocarbon or fluorocarbon gas, at least one oxidizing gas, at least one inert gas, and / or at least one additional gas can be optional. For example, in the disclosed plasma etching methods for selectively plasma dry etching organic films, the at least one hydrofluorocarbon or fluorocarbon gas is optional and may or may not be included in the etching gas mixture.
[0132] Under plasma conditions, various reactive species and ions are generated directly by the dissociation of these compounds and by chemical reactions due to interactions between species present in the gas phase. Typically, plasma etching effects can be achieved using any of the compounds represented by the above formulas, whether used individually or in mixtures with each other. Depending on the structure of each compound, etching performance (including increasing the etch rate of a specific material to be etched) or passivation during high aspect ratio etching processes can be enhanced. In particular, a mixture of CF and CF is one of the commonly used mixtures, because CF is efficient at promoting passivation, and CF is efficient at increasing the etch rate, resulting in a highly anisotropic etching process, as described in Comparative Example 6 below. Furthermore, hydrofluorocarbon gases such as CHF can be added, if necessary, to enhance the etch rate of silicon nitride films.
[0133] Other gases, such as inert or oxidizing gases, can be added to the etching gas mixture. The use of inert gases increases ion bombardment during the etching process and, depending on the gas ratio, promotes or inhibits the dissociation of other gases in the etching gas mixture, thereby directly affecting the etching rate and anisotropy of the etching process. Furthermore, the addition of oxidizing gases to the etching gas mixture can increase the etching rate, isotropy, and selectivity of the etching process, depending on the etching gas mixture and the type of target and non-etched materials. Furthermore, additional gases selected from H2, SF6, NF3, N2, NH3, Cl2, BCl3, BF3, Br2, F2, HBr, HCl, or combinations thereof can be added to the etching gas mixture to improve process control or increase the etching rate.
[0134] The disclosed etching gas mixture is suitable for plasma etching semiconductor structures such as channel holes, gate trenches, step contacts, slits, capacitor holes, contact holes, self-aligned contacts, self-aligned vias, and supervias in silicon-containing films. The disclosed etching gas mixture is compatible with not only currently available mask materials but also future generations of mask materials because the disclosed Si-containing etching compounds induce little or no damage to the mask, along with good profiling of high-aspect-ratio structures. In other words, the disclosed etching gas mixture can produce vertical etched patterns with minimal or no bowing, pattern collapse, or roughness. To achieve these properties, the disclosed etching gas mixture can deposit an etch-resistant polymer layer during etching to help mitigate the direct effects of oxygen and fluorine radicals during the etching process. The disclosed etching gas mixture can also mitigate damage to p-Si or crystalline Si channel structures during etching.
[0135] Material compatibility testing is important to determine whether any of the disclosed etching gas mixtures will react with chamber materials and degrade chamber performance over short or long-term use. Typical materials used in chambers, valves, and other components include stainless steel, aluminum, nickel, PCTFE, PVDF, PTFE, PFA, PP, Kalrez, Viton, and other metals and polymers. In some cases, these materials are exposed to high temperatures, e.g., above 20°C, and high pressures, e.g., above 1 atmosphere, which can accelerate degradation. Measurement methods can include visual inspection, weight measurement, nanometer-scale changes measured with a scanning electron microscope (SEM), tensile strength, hardness, and the like.
[0136] The disclosed etching gas mixtures can be used to plasma etch silicon-containing films on substrates. The disclosed plasma etching methods can be useful in the fabrication of semiconductor devices such as NAND or 3D NAND gates, flash or DRAM memory capacitors, or transistors such as fin field-effect transistors (FinFETs), gate-all-around (GAA)-FETs, nanowire FETs, nanosheet FETs, fork-sheet FETs, complementary FETs (CFETs), bulk complementary metal-oxide-semiconductor (Bulk CMOS), MOSFETs, and fully depleted silicon-on-insulator (FD-SOI) structures. The disclosed etching gas mixtures can be used in various front-end-of-the-line (FEOL) and back-end-of-the-line (BEOL) etching applications, such as patterning metal films, forming metal interconnects, and buried power and signal lines. Additionally, the disclosed etching gas mixtures can be used to etch silicon in 3D via-silicon (TSV) etching applications for interconnecting memory to logic in a substrate and in MEMS applications.
[0137] The disclosed plasma etching method includes providing a reaction chamber within which a substrate is placed. The reaction chamber can be any enclosure or chamber within a device in which an etching method is performed, such as, but not limited to, reactive ion etching (RIE), capacitively coupled plasma (CCP) with single or multiple frequency RF sources, inductively coupled plasma (ICP), or microwave plasma reactors, or other types of etching systems capable of selectively removing portions of silicon-containing films or generating activated species. Those skilled in the art will recognize that various plasma reaction chamber designs provide different electron density and temperature control. Suitable commercially available plasma reaction chambers include, but are not limited to, Applied Materials' magnetically enhanced reactive ion etcher, sold under the trademark eMAX™, or Lam Research's Dual CCP reactive ion etcher dielectric etch product family, sold under the trademark 2300® Flex™. In such cases, RF power can be pulsed to control plasma characteristics, thereby further improving etch performance (selectivity and damage).
[0138] In the disclosed plasma etching method, a plasma etching chamber is equipped with a parallel-plate electrode plasma generator, in which a high-frequency electromagnetic field with a frequency ranging from 2 to 100 MHz is applied to either the upper electrode or the lower electrode, or both, while a low-frequency electromagnetic field with a frequency ranging from 40 kHz to 2 MHz is applied to the lower electrode, with the gap between the electrodes maintained in the range of 10 to 35 mm. These electromagnetic fields can be combined to apply power ranging from 0 to 10,000 W to the upper electrode and from 0 to 100,000 W to the lower electrode. The pressure within the etching chamber during the plasma etching process is maintained in the range of 5 to 100 mTorr, and the etching gas mixture is introduced. Alternatively, the plasma-treated reactants of the disclosed etching gas mixture can be generated outside the reaction chamber. For example, the reactants can be treated before entering the reaction chamber using an MKS Instruments ASTRONi® reactive gas generator, etc. For example, when operating at 2.45 GHz, 7 kW plasma power, and a pressure ranging from approximately 0.5 Torr to approximately 10 Torr, the reactant O2 can be decomposed into two O radicals. Preferably, the remote plasma can be generated at a power ranging from approximately 1 kW to approximately 10 kW, more preferably from approximately 2.5 kW to approximately 7.5 kW. The reaction chamber can contain one or more substrates. For example, the reaction chamber can accommodate 1 to 200 silicon wafers having diameters ranging from 25.4 mm to 450 mm. The substrate can be any suitable substrate used in the manufacture of semiconductor, photovoltaic, flat panel, or LCD-TFT devices. Examples of suitable substrates include wafers such as silicon, silica, glass, Ge, SiGe, GeSn, InGaAs, GaSb, InP, or GaAs wafers. The wafer has multiple films or layers thereon, including silicon-containing films or layers, obtained from previous manufacturing processes. The layers can be patterned or unpatterned.Examples of suitable layers include, but are not limited to, silicon (amorphous silicon, p-Si, crystalline silicon, etc., any of which can be further p-doped or n-doped with B, C, P, As, Ga, In, Sn, Sb, Bi and / or Ge), silica, silicon nitride, silicon oxide, silicon oxynitride, Si. a O b H c C d N e (a>0, b, c, d, e≧0), mask layer materials such as Ge, SiGe, GeSn, InGaAs, GaSb, InP, amorphous carbon with or without dopants, anti-reflective coatings, photoresist materials, metal oxides such as AlO, TiO, HfO, ZrO, SnO, TaO, or metal nitride layers such as AlN, ZrN, SnN, HfN, titanium nitride, tantalum nitride, or the like, or combinations thereof, Si selected from silicon nitride, polysilicon, crystalline silicon, silicon carbide, SiON, SiCN, or combinations thereof. a O b H c C d N e (a>0, b, c, d, e≧0), or device channel materials such as crystalline silicon, epitaxial silicon, doped silicon, or combinations thereof. The silicon oxide layer can form a dielectric material such as an organic-based or silicon oxide-based low-k dielectric material (e.g., porous SiCOH film). Exemplary low-k dielectric materials are sold by Applied Materials under the trade names Black Diamond II or III. Additionally, layers containing tungsten, cobalt, copper, or noble metals (e.g., platinum, palladium, rhodium, or gold) can be used. Further examples of silicon-containing films include Si a O b H c C d N e (a>0, b, c, d, e≧0). Throughout this specification and claims, the wafer and any associated layers thereon are referred to as the substrate.
[0139] Vapor of the disclosed etching gas mixture is introduced into a reaction chamber containing a substrate having a silicon-containing film deposited thereon. Vapor of the disclosed etching gas mixture, or vapor of each component of the disclosed etching gas mixture, can be introduced into the chamber at a flow rate ranging from approximately 0.1 sccm to approximately 1 slm. For example, for a 300 mm wafer size, vapor can be introduced into the chamber at a flow rate ranging from approximately 1 sccm to approximately 50 sccm. Alternatively, for a 450 mm wafer size, vapor can be introduced into the chamber at a flow rate ranging from approximately 25 sccm to approximately 250 sccm. Those skilled in the art will recognize that flow rates may vary from tool to tool. The disclosed Si-containing hydrofluorocarbon etching compounds and hydrofluorocarbon or fluorocarbon compounds can be supplied neat or in blends with inert gases such as N2, Ar, Kr, Ne, He, Xe, etc., or with solvents. The disclosed Si-containing hydrofluorocarbon etching compounds and hydrofluorocarbon or fluorocarbon compounds can be present in various concentrations in the blends. In the case of liquid Si-containing hydrofluorocarbon etchant compounds and hydrofluorocarbon or fluorocarbon compounds, vapor forms of the Si-containing hydrofluorocarbon etchant compounds and hydrofluorocarbon or fluorocarbon compounds can be produced by evaporating neat or blended Si-containing hydrofluorocarbon etchant compound solutions and hydrofluorocarbon or fluorocarbon compound solutions by a conventional evaporation process such as direct evaporation or by aeration. The neat or blended Si-containing hydrofluorocarbon etchant compounds and neat or blended hydrofluorocarbon or fluorocarbon compounds are fed in liquid form to an evaporator where they are evaporated before being introduced into the reactor.
[0140] Alternatively, neat or blended Si-containing hydrofluorocarbon etching compounds can be vaporized by passing a carrier gas through a vessel containing the disclosed Si-containing hydrofluorocarbon etching compound and a hydrofluorocarbon or fluorocarbon compound, or by bubbling a carrier gas through the disclosed Si-containing hydrofluorocarbon etching compound and a hydrofluorocarbon or fluorocarbon compound. Carrier gases can include, but are not limited to, Ar, He, N2, Kr, Xe, Ne, and mixtures thereof. Bubbling with a carrier gas can also remove any dissolved oxygen present in the neat or blended Si-containing hydrofluorocarbon etching compound solution and the hydrofluorocarbon or fluorocarbon compound solution. The carrier gas and the disclosed Si-containing hydrofluorocarbon etching compound are then introduced into a reactor as a vapor.
[0141] If necessary, the container containing the disclosed Si-containing hydrofluorocarbon etching compound can be heated to a temperature that allows the Si-containing hydrofluorocarbon etching compound to reach a liquid phase and have sufficient vapor pressure to be delivered to an etching tool. The container can be maintained at a temperature ranging from about 0°C to about 150°C, preferably from about room temperature to about 100°C, and more preferably from about room temperature to about 50°C. More preferably, the container is maintained at room temperature to avoid heat lines to the etching tool. Those skilled in the art will recognize that the temperature of the container can be adjusted in known ways to control the amount of vaporized Si-containing hydrofluorocarbon etching compound.
[0142] For 3D NAND applications, the plasma-activated vapor of the disclosed etching gas mixture or the disclosed plasma-activated etching gas exhibits high selectivity to the mask, preferably etching through alternating layers of SiO and SiN or alternating layers of polysilicon and SiO, resulting in a vertical etch profile without profile distortion (e.g., curvature or roughness), which is important for 3D NAND applications. In addition, the plasma-activated vapor deposits polymer on the sidewalls, minimizing deformation of the feature profile. For other applications, such as DRAM and 2D NAND, for example, under various process conditions, the plasma-activated vapor of the disclosed etching gas mixture can selectively etch SiO from SiN. The disclosed plasma-activated etching gas can selectively etch SiO and / or SiN from mask layers such as aC, photoresist, a-Si, p-Si, or silicon carbide, or from metal contact layers such as Cu, W, or Ru, or from channel regions made of SiGe or polysilicon regions. The disclosed plasma activated etching gases can selectively etch organic films from other films such as aC, photoresist, a-Si, p-Si, or silicon carbide, or from metal contact layers such as Cu, W, Ru, or from channel regions made of SiGe or polysilicon regions.
[0143] The disclosed activated etching gas mixture, including a Si-containing hydrofluorocarbon etching gas (e.g., by igniting a plasma of the etching gas mixture), reacts with a silicon-containing film deposited on a substrate to form volatile by-products that are removed from the reaction chamber. The aC mask, anti-reflective coating, and photoresist layer on the substrate become less reactive with the activated etching gas. Thus, the activated etching gas selectively reacts with the silicon-containing film to form volatile by-products.
[0144] Alternatively, the disclosed activated etching gas mixture (e.g., by igniting a plasma of the etching gas mixture) containing a Si-containing hydrofluorocarbon etching gas reacts with organic films deposited on a substrate to form volatile by-products that are removed from the reaction chamber. In this case, organic films, such as aC masks, are more reactive with the activated etching gas in various processes and under various etching conditions. Thus, the activated etching gas selectively reacts with the organic films to form volatile by-products.
[0145] The temperature and pressure within the reaction chamber are maintained at conditions suitable for the silicon-containing film to react with the activated etching gas. For example, the pressure within the chamber may be maintained at about 0.1 mTorr to about 1000 Torr, preferably about 1 mTorr to about 10 Torr, more preferably about 10 mTorr to about 1 Torr, and more preferably about 10 mTorr to about 100 mTorr, as required by the etching parameters. Similarly, the temperature of the substrate within the chamber may range from about −196° C. to about 500° C., preferably about −120° C. to about 300° C., more preferably about −100° C. to about 50° C., and more preferably about −70° C. to about 40° C. The temperature of the chamber walls may range from about −196° C. to about 300° C., depending on the process requirements.
[0146] Alternatively, the temperature and pressure within the reaction chamber are maintained at conditions suitable for the organic film to react with the activated etching gas. For example, the pressure within the chamber may be maintained at approximately 0.1 mTorr to approximately 1000 Torr, preferably approximately 1 mTorr to approximately 10 Torr, more preferably approximately 10 mTorr to approximately 1 Torr, and more preferably approximately 10 mTorr to approximately 100 mTorr, as required by the etching parameters. Similarly, the temperature of the substrate within the chamber may range from approximately −196° C. to approximately 500° C., preferably approximately −120° C. to approximately 300° C., more preferably approximately −100° C. to approximately 50° C., and more preferably approximately −70° C. to approximately 40° C. The temperature of the chamber walls may range from approximately −196° C. to approximately 300° C., depending on the process requirements.
[0147] Reactions between the silicon-containing film and the activated etching gas, and between the organic film and the activated etching gas, result in anisotropic removal of the silicon-containing and organic films from the substrate, depending on the process parameters. Nitrogen, oxygen, and / or carbon atoms may also be present in the silicon-containing and organic films. Removal may occur by physical sputtering of the silicon-containing and organic films from plasma ions (accelerated by the plasma) and / or by removing Si from SiF x (x ranges from 1 to 4) by chemical reactions of plasma species that convert them into volatile species such as
[0148] The disclosed plasma etching method using the disclosed Si-containing hydrofluorocarbon compounds as etching gases produces apertures in silicon-containing films, such as channel holes, gate trenches, step contacts, capacitor holes, contact holes, contact etch, slit etch, self-aligned contacts, self-aligned vias, and supervias. The resulting apertures can have aspect ratios ranging from about 5:1 to about 500:1, preferably from about 20:1 to about 400:1, and diameters ranging from about 5 nm to about 500 nm, preferably less than 100 nm. For example, those skilled in the art will recognize that channel hole etching produces apertures in silicon-containing films with aspect ratios greater than 50:1.
[0149] A typical material that needs to be etched can be SiO. The process of etching SiO can involve etching trenches in borophosphosilicate glass (BPSG), tetraethyl orthosilicate (TEOS), or low-deposition-rate TEOS (LDTEOS). The etch stop layer can be silicon nitride or silicon oxynitride (SiON), polysilicon, or a metal or metal nitride (e.g., W or TiN). The mask material used can be aC, p-Si, amorphous silicon B-doped aC, W-doped aC, B-doped amorphous silicon, or a photoresist material. The disclosed Si-containing hydrofluorocarbon etching compounds are applied to etch SiO, SiN, p-Si, and / or aC substrate films.
[0150] The disclosed etching method is not limited to the above experimental conditions in any way and type of plasma etching tool (capacitively coupled plasma or inductively coupled plasma), process conditions (pressure, power, temperature, duration of process), process gas mixture, combination and proportion of gases in the gas mixture, gas flow, workpiece or substrate, and plasma etching chamber itself can be varied from process to process and during the process.
[0151] Also disclosed is an etching gas supply system. FIG. 35 illustrates an exemplary etching gas supply apparatus or system. As shown, two fluid conduits 814 and 816 connect a first etchant source 802 and a second etchant source 804, respectively, to a common fluid conduit 818. The first etchant source 802 contains a first etchant, and the second etchant source 804 contains a second etchant. Thermal elements 810a, 810b, and 810c are connected to the first etchant source 802, the second etchant source 804, and the gas mixer 806, respectively, and are configured and adapted to regulate the temperature of the first etchant, the second etchant, and / or a mixture of the first and second etchants. Optionally, the vaporizer elements 808a, 808b, and 808c are fluidly connected to one or more of the at least two fluid conduits 814 and 816 and / or a common fluid conduit 818. The vaporizer elements 808a, 808b, and 808c are configured and adapted to generate vapor of the first etchant, the second etchant, and / or a mixture thereof, respectively. The mixing element 806 is optionally connected to the two fluid conduits 814 and 816 and the common fluid conduit 818. The mixing element 806 is configured and adapted to mix the first etchant and the second etchant. Valves 812a, 812b, 812c, 812d, 812e, and 812f are installed in conduits 814, 816, 818 and steam elements 808a, 808b, and 808c to control the use of steam elements 808a, 808b, and 808c. When steam elements 808a, 808b, and 808c are not in use, valves 812a, 812c, and 812e are shut off and valves 812b, 812d, and 812f are open, and vice versa.
[0152] Here, a programmable logic controller (PLC) (not shown) can be installed in the system and configured and adapted to control all elements, valves, gas sources, etc. in the apparatus. The etching gas supply device is specifically adapted to adjust the flow of the first etching solution and the second etching solution to form an etching gas composition having a predetermined ratio of the first etching solution to the second etching solution based on the chemical formulas of the first etching solution and the second etching solution. The first etching solution and the second etching solution may or may not be mixed before being introduced into the etching process chamber or reactor. The first etching solution and the second etching solution may be mixed in mixing element 806 before being introduced into the etching process chamber or reactor. The first etching solution and the second etching solution may be introduced into the etching process chamber or reactor independently and mixed therein. Dashed lines 820 and 822 indicate that the first etching solution and the second etching solution, respectively, are directly introduced into the etching process chamber or reactor without being mixed. In some embodiments, the first etchant is a disclosed Si-containing hydrofluorocarbon, and the container of the first etchant can be operably connected to a device used in a semiconductor etching process.
[0153] In some embodiments, the second etchant is a mixture of Ar, Kr, Xe, N 2、The etching gas supply system shown in FIG. 35 may be an inert gas selected from He, Ne, or a combination thereof; an oxidizer or oxidizing gas selected from O, O, CO, CO, COS, SO, SO, FNO, NO, NO, NO, NO, H, NO, Cl, F, etc.; or an additional gas selected from H, SF, NF, N, NH, Cl, BCl, BF, Br, F, HBr, HCl, or a combination thereof. In addition, the etching gas supply system shown in FIG. 35 is not limited to the first and second etching solution sources 802 and 804; one or more etching solution sources can be added in parallel to the first and second etching solution sources 802 and 804 and mixed in the mixing element 806 with the first and second etching solutions. For example, when the disclosed etching gas mixture includes a Si-containing hydrofluorocarbon, an inert gas, an oxidizer, and an additional gas, four etching solution sources are installed in the etching gas supply system. [Example]
[0154] To further illustrate embodiments of the present invention, a detailed description of the present disclosure is provided below through examples and comparative examples. However, the present disclosure is in no way limited to the presented examples, and etching conditions, etching gas mixtures, combinations and proportions of gases or vapors in the etching gas mixtures, substrates, and the plasma etching chamber itself may vary.
[0155] Examples 1 to 11 and Comparative Examples 1 to 6 have the following conditions.
[0156] Plasma Etching Device: In the disclosed method, a parallel-plate (capacitively coupled plasma) plasma generator was used as the plasma etching device. The parallel-plate configuration included an upper electrode and a lower electrode on which the substrate was placed (the lower electrode was used as a sample holder with cooling capabilities). The distance between the electrodes was 13 mm or 30 mm. When the lower electrode was connected to a 2 MHz generator, the upper electrode was connected to a 27 MHz or 60 MHz generator.
[0157] Plasma Etching Conditions: During the plasma etching process, the power supplied to the upper electrode varied from 500 to 2000 W, and the power applied to the lower electrode varied from 750 to 7000 W. The pressure was maintained constant between 5 and 100 mTorr during the process. The plasma etching time was set to a value between 30 and 300 seconds. The etching rate was estimated in nanometers per minute. The plasma etching gas mixture included Ar, O, C4F6 and / or C4F8 used as the fluorocarbon gas, and C2H6F2Si or CH3F3Si, C4H9F3Si, or C5H9F5Si used as the Si-containing hydrofluorocarbon gas, with CH2F2 optionally used as the hydrofluorocarbon gas.
[0158] Substrate: The substrates used in Examples 1 to 11 and Comparative Examples 1 to 6 are shown in Figures 2a-2b. The substrates in Examples 5-7 were single crystal silicon wafer pieces having a thin film of one of the following materials on top of the silicon wafer: SiO2, Si3N4, amorphous carbon (hereinafter "aC"), W, Ru, Co, Mo, TiN, TiO2.
[0159] Plasma Etch Profile and Selectivity: Selectivity, top CD, mid CD, and bottom CD were selected as metrics for comparing the high aspect ratio etch performance of the disclosed plasma etch process with a reference plasma etch process using a typical etch gas mixture, e.g., a mixture of Ar, O2, CF6, and / or CF8, because they reflect control of the etched pattern profile. Selectivity was calculated as the ratio of the silicon dioxide etch depth (arrow 8 in Figure 2b) to the difference between the initial amorphous carbon mask thickness (arrow 5 in Figure 2a, 868 nm) and the mask thickness after the etch process (arrow 7 in Figure 2b). If the resulting selectivity value becomes negative, i.e., if the amorphous carbon mask thickness increases after the etch process, this condition is referred to as "infinite selectivity," meaning that the mask thickness has increased due to polymer deposition during the etch process. If the width of an etched hole in SiO2 increases compared to the top CD at a certain depth, the bow CD can be used instead of the mid CD. The bow CD represents the widest area of the etched hole in the SiO2 film. In addition, the neck CD (which is the smallest width of the hole in the aC mask) can be used as a measure of the reduction in the diameter of the hole in the aC mask due to polymer deposition on the mask during the etching process.
[0160] During the comparison, higher values of selectivity or infinite selectivity were targeted when the neck CD, top CD, bottom CD, bow CD, and middle CD were targeted to be as close as possible to the value of the diameter of the bottom of the opening in the amorphous carbon mask (120 nm, arrow 3 in Figure 2a).
[0161] Example 1 Plasma etching was performed in a plasma etching chamber with 750 W of power applied to the top electrode at a frequency of 27 MHz and 1500 W of power applied to the bottom electrode at a frequency of 2 MHz. The pressure in the chamber was maintained at 30 mTorr, and the gap between the electrodes was set to 13 mm. An etching gas mixture containing the following gas flows was introduced into the plasma etching chamber: 150 sccm Ar, 12 sccm C4F8, 12 sccm O2, and 1.2 sccm C5H9F5Si. The plasma etching process was performed for 2 minutes. The resulting cross-sectional structure of the substrate after the plasma etching process is shown in Figure 6a, and the parameters for comparison are summarized in Table 2.
[0162] [Table 7]
[0163] Example 2 Plasma etching was performed in the same manner as in Example 1, except that the process gas mixture was replaced with the following: 75 sccm Ar, 15 sccm C4F6, 10 sccm O2, and 0.6 sccm C5H9F5Si. The resulting cross-sectional structure of the substrate after the etching process is shown in Figure 6c, and the parameters for comparison are summarized in Table 2.
[0164] Example 3 Plasma etching was performed in a plasma etching device with a power of 1000 W applied to the top electrode at a frequency of 60 MHz and a power of 7000 W applied to the bottom electrode at a frequency of 2 MHz. The pressure in the chamber was maintained at 20 mTorr, and the gap between the electrodes was set to 20 mm. A process gas mixture containing the following gas flows was introduced into the plasma etching chamber: 150 sccm Ar, 60 sccm C4F8, 30 sccm O2, and 5 sccm C4H9F3Si. The plasma etching process was performed for 2 minutes. The resulting cross-sectional structure of the substrate after the etching process is shown in Figure 7a, and the parameters for comparison are summarized in Table 2.
[0165] Example 4 Plasma etching was performed in a plasma etching device with a power of 1000 W applied to the top electrode at a frequency of 60 MHz and a power of 7000 W applied to the bottom electrode at a frequency of 2 MHz. The pressure in the chamber was maintained at 20 mTorr, and the gap between the electrodes was set to 20 mm. A process gas mixture containing the following gas flows was introduced into the plasma etching chamber: 150 sccm Ar, 60 sccm C4F8, 35 sccm O2, and 5 sccm C4H9F3Si. The plasma etching process was performed for 5 minutes. The resulting cross-sectional structure of the substrate after the etching process is shown in Figure 8a, and the parameters for comparison are summarized in Table 3.
[0166] Example 5 Plasma etching was performed in a plasma etching device with a power of 1000 W applied to the top electrode at a frequency of 60 MHz and a power of 7000 W applied to the bottom electrode at a frequency of 2 MHz. The pressure in the chamber was maintained at 20 mTorr, and the gap between the electrodes was set to 20 mm. A process gas mixture containing the following gas flows was introduced into the plasma etching chamber: 150 sccm Ar, 60 sccm C4F8, 30 sccm O2, and 5 sccm C4H9F3Si. The plasma etching process was performed for 30 seconds. The etch rates for each of the studied materials are summarized in Table 3.
[0167] [Table 8]
[0168] Example 6 Plasma etching was performed in a similar manner to Example 5, except that the process gas mixture was replaced with the following: 150 sccm Ar, 40 sccm C4F8, 20 sccm CH2F2, 30 sccm O2, and 5 sccm C4H9F3Si. The plasma etching process was carried out for 30 seconds. The etch rates for each of the studied materials are summarized in Table 3.
[0169] Example 7 Plasma etching was performed in a similar manner to Example 5, except that the process gas mixture was replaced with the following: 150 sccm Ar, 30 sccm C4F8, 30 sccm CH2F2, 30 sccm O2, and 5 sccm C4H9F3Si. The plasma etching process was carried out for 30 seconds. The etch rates for each of the studied materials are summarized in Table 3.
[0170] Comparative Example 1 Plasma etching was carried out in the same manner as in Example 1, except that C5H9F5Si was not added to the process gas mixture. The resulting cross-sectional structure of the substrate after the etching process is shown in Figure 6b, and the parameters for comparison are summarized in Table 2.
[0171] Comparative Example 2 Plasma etching was carried out in the same manner as in Example 2, except that C5H9F5Si was not added to the process gas mixture. The resulting cross-sectional structure of the substrate after the etching process is shown in Figure 6d, and the parameters for comparison are summarized in Table 2.
[0172] Comparative Example 3 Plasma etching was carried out in the same manner as in Example 3, except that C4H9F3Si was not added to the process gas mixture. The resulting cross-sectional structure of the substrate after the etching process is shown in Figure 7b, and the parameters for comparison are summarized in Table 2.
[0173] Comparative Example 4 Plasma etching was performed in the same manner as in Example 3, except that the 5 sccm flow rate of C4H9F3Si was replaced with a 5 sccm flow rate of C4F6: the resulting cross-sectional structure of the substrate after etching is shown in Figure 7c, and the parameters for comparison are summarized in Table 2.
[0174] Comparative Example 5 Plasma etching was carried out in the same manner as in Example 4, except that C4H9F3Si was not added to the process gas mixture. The resulting cross-sectional structure of the substrate after the etching process is shown in Figure 8b, and the parameters for comparison are summarized in Table 2.
[0175] Comparative Example 6 Plasma etching was performed in the same manner as in Example 4, except that the 5 sccm flow rate of C4H9F3Si was replaced with a 5 sccm flow rate of C4F6. The resulting cross-sectional structure of the substrate after the etching process is shown in Figure 8c, and the comparative parameters are summarized in Table 2. Table 2 clearly shows that the addition of 0.6-1.2 sccm of C5H9F5Si or 5 sccm of C4H9F3Si can improve most of the comparative criteria under all of the conditions studied. For example, in all cases where a Si-containing hydrofluorocarbon was added to the process gas mixture, the selectivity improved and the top CD approached the initial value.
[0176] Specifically, in Example 1, 1.3 sccm of C5H9F5Si was added to a working gas mixture of Ar, O2, and C4F8, and the selectivity to the mask material was 13, which is much higher than Comparative Example 1 under the same conditions without C5H9F5Si, where the selectivity value was 7, which is almost twice as low. In Examples 2 and 3, 0.6 sccm of C5H9F5Si or 5 sccm of C4H9F3Si was added to a process gas mixture of Ar, O2, and C4F6 or C4F8, respectively, and under the same conditions without the Si-containing hydrofluorocarbon, or when the Si-containing hydrofluorocarbon was replaced with C4F6, the selectivity to the mask material was infinite (the thickness of the mask after processing increased), and the selectivity value was in the range of 5 to 20, which was significantly lower. Furthermore, as can be seen in the cross-sectional images of the substrates taken by a scanning electron microscope, in Comparative Example 2, the material to be plasma etched was not etched due to excessive passivation ( FIG. 6d ), whereas in Comparative Example 1, the etching of the material to be plasma etched was occasionally interrupted and stopped due to excessive passivation ( FIG. 6b ). This clearly demonstrates that when the etching process of the target material is not possible under the same conditions without the Si-containing hydrofluorocarbon (e.g., Comparative Example 2), the fluorocarbon fragments (e.g., CF) generated by the dissociation of the initial Si-containing hydrofluorocarbon can enhance the etching process and achieve an acceptable etching profile (e.g., Example 2).
[0177] The most important comparison criteria for etch profile control are the top and mid CDs because both directly affect the etch profile at greater depths. The bottom CD, while important, is a less critical criterion because, by comparison, if top CD expansion or clogging is irreversible, profile distortions such as bottom taper can be corrected by overetching (continuing the etching process after reaching the desired depth or stop layer). From Table 2, it can be clearly seen that when Si-containing hydrofluorocarbons (C4H9F3Si or C5H9F5Si) were added to the working gas mixtures of Examples 1-4, both the top and mid CDs were close to or identical to the initial value of the mask opening (120 nm, arrow 3 in Figure 2a). It can also be seen that Comparative Examples 1-6, where Si-containing hydrofluorocarbons were not used or were replaced with C4F6, exhibited significant increases in the top and mid CDs compared to Examples 1-4, which would be unacceptable in semiconductor device manufacturing processes. Even though the bottom CD of the comparative example was rarely close to the CD value of the initial mask opening (120 nm, arrow 3 in Figure 2a) compared to Examples 1-4 where Si-containing hydrofluorocarbons were used, this came at the high cost of large lateral recession of the top etched structures, which cannot be corrected if the shrunken bottom CD can be compensated for by overetching.
[0178] As can be seen from Table 3, when 20 or 30 sccm of CH2F2 was added to the process gas mixture, it was possible to etch SiO2 selectively to aC and polycrystalline silicon, as well as to selectively etch Si3N4. Specifically, in Example 7, when 30 sccm of CH2F2 was added to the process gas mixture, it was possible to etch SiO2 and Si3N4 with comparable etch rates and infinite selectivity to aC and polycrystalline silicon, which are commonly used as mask materials. The results suggest that when CH2F2 is added to the process gas mixture, the same process for high aspect ratio etching of SiO2 demonstrated in Examples 1-4 can also be performed for high aspect ratio etching of Si3N4 or alternating layers of SiO2 and Si3N4 (ONON stack). Furthermore, the infinite selectivity observed for etching SiO2 or Si3N4 relative to the metal films (Ru, Co, Mo, W) tested in Examples 5-7 indicates that these metals or other metal films (e.g., Al, Pt, Au) can be used as a stop layer for the etching process. This means that if a thin metal film (e.g., contact pads, buried power rails, etc.) is present below the target plasma etching material (e.g., SiO2 or Si3N4), the high aspect ratio etching process will stop when the etched opening reaches the metal film, and infinite selectivity minimizes damage to the metal film. In addition, the etch rates of metal oxide and metal nitride films (TiO2 and TiN) in Example 7 are significantly smaller than those of SiO2 and Si3N4, meaning that a soft landing can be achieved even on metal oxide or metal nitride films if the etching process is properly optimized. This effect can be useful for etching high aspect ratio contact holes or other high aspect ratio structures landing on metal, metal nitride or metal oxide films (e.g., high aspect ratio etching of 3D NAND channels or DRAM capacitors).Summarizing the results observed in Examples 1-4 and Comparative Examples 1-6, it can be concluded that the addition of a Si-containing hydrofluorocarbon, preferably having at least one methyl group bonded to Si, more preferably C4H9F3Si or C5H9F5Si, to the process gas mixture can improve selectivity and maintain the lateral dimensions of features during high-aspect-ratio etching. Additionally, as observed in Examples 1 and 2 and Comparative Examples 1 and 2, the formation of fluorocarbon fragments (such as C2F4 as seen in quadrupole mass spectrometry) during dissociation of the Si-containing hydrofluorocarbon can enhance the plasma etching of the material. Furthermore, as demonstrated in Examples 5-7, the addition of CH2F2 to the process gas mixture is effective in improving the etching of Si3N4, enabling high-aspect-ratio etching of Si3N4 films or alternating SiO2 and Si3N4 films while maintaining high selectivity to metals.
[0179] Example 8 Plasma etching was performed in a plasma etching device with 1000 W of power applied to the top electrode at a frequency of 60 MHz and 7000 W of power applied to the bottom electrode at a frequency of 2 MHz. The pressure in the chamber was maintained at 20 mTorr, and the gap between the electrodes was set to 20 mm. A process gas mixture containing the following gas flows was introduced into the plasma etching chamber: 150 sccm Ar, 60 sccm C4F8, 30 sccm O2, and 5 sccm C2H6F2Si. The plasma etching process was performed for 2 minutes. The resulting cross-sectional structure of the substrate after the etching process is shown in Figure 9, and the parameters for comparison are summarized in Table 4.
[0180] [Table 9]
[0181] Example 9 Plasma etching was performed in the same manner as in Example 8, except that the plasma etching process was carried out for 5 minutes. The resulting cross-sectional structure of the substrate after the etching process is shown in Figure 10, and the parameters for comparison are summarized in Table 4.
[0182] Example 10 Plasma etching was performed in the same manner as in Example 8, except that the process gas mixture was replaced with the following: 150 sccm Ar, 60 sccm C4F8, 30 sccm O2, and 5 sccm CH3F3Si. The resulting cross-sectional structure of the substrate after the etching process is shown in Figure 11, and the parameters for comparison are summarized in Table 4.
[0183] Example 11 Plasma etching was performed in the same manner as in Example 9, except that the process gas mixture was replaced with the following: 150 sccm Ar, 60 sccm C4F8, 30 sccm O2, and 5 sccm CH3F3Si. The resulting cross-sectional structure of the substrate after the etching process is shown in Figure 12, and the parameters for comparison are summarized in Table 4.
[0184] The most important comparison criteria for etch profile control are the top and mid CDs because they both directly affect the etch profile at greater depths. The bottom CD, while important, is a less critical criterion because, by comparison, profile distortions such as bottom taper can be corrected by overetching (continuing the etching process after reaching the desired depth or stop layer) while expansion or occlusion of the top CD is irreversible. When C2H6F2Si or CH3F3Si was added to the working gas mixtures of Examples 8-11, both the top and mid CDs were close to or identical to the initial value of the mask opening (120 nm, arrow 3 in Figure 2a). It can be clearly seen from Table 2 that, in Comparative Examples 1-6 where the Si-containing hydrofluorocarbon was not used or was replaced with C4F6, the top and mid CDs increased significantly compared to Examples 8-11, which would be unacceptable in semiconductor device manufacturing processes due to pattern degradation and possible structural collapse during the prolonged etching process. Even though there were few cases where neck CD was not a desirable effect when using C2H6F2Si or CH3F3Si, it is still more reliable in the fabrication of semiconductor devices than the significant neck CD expansion in Comparative Examples 1 to 6. In the case of neck shrinkage during the etching process, the neck CD can be opened by a short cleaning step, while it is more complicated to recover the expanded neck CD seen in Comparative Examples 1 to 6 without using Si-containing hydrofluorocarbons.
[0185] Examples 12 to 18 have the following conditions.
[0186] Plasma Etching Device: In the disclosed method, a parallel-plate (capacitively coupled plasma) plasma generator was used as the plasma etching device. The parallel-plate configuration included an upper electrode and a lower electrode, on which the substrate was placed (the lower electrode was used as a sample holder with cooling capabilities). The distance between the electrodes was 13 mm or 20 mm. When the lower electrode was connected to a 2 MHz generator, the upper electrode was connected to a 27 MHz or 60 MHz generator.
[0187] Plasma etching conditions: During the plasma etching process, the power supplied to the upper electrode varied from 500 to 2000 W, and the power applied to the lower electrode varied from 750 to 7000 W. The pressure was maintained constant in the range of 1 to 100 mTorr during the process. The plasma etching time was set to a value between 30 and 300 seconds. The etching rate was estimated in nanometers per minute. The plasma etching gas mixture included Ar, O, C4F8 used as the fluorocarbon gas, and C2H6F2Si, CH3F3Si, C4H9F3Si, or C5H9F5Si used as the Si-containing hydrofluorocarbon gas.
[0188] Substrate: Referring to Figures 3a and 3b, a single-crystal silicon wafer fragment with a thin film of the target plasma etching material on the wafer was used as the substrate. The target plasma etching material was one from the following list: SiO2, Si3N4, amorphous carbon (hereinafter "aC"), polycrystalline silicon (hereinafter "poly-Si"), and W. The initial thickness of each target plasma etching material was as follows: 300 nm aC, 110 nm W, 550 nm poly-Si, 300 nm Si3N4, and 2000 nm SiO2. Plasma Etch Rate and Selectivity: The plasma etch rate was estimated as the difference between the initial thickness of the plasma etched material film and the thickness of the film after the etching process divided by time, and the etch rate was obtained in nm / min. Selectivity was estimated as the ratio of the etch rates calculated for two different plasma etch materials. An etch rate of 0 nm / min corresponds to a condition where the target material is not etched or has a polymer deposited on it, which in certain instances results in a selectivity of infinite value if this material is a non-etchable material.
[0189] Example 12 Plasma etching was performed in a plasma etching device with 750 W of power applied to the top electrode at a frequency of 27 MHz and 1500 W of power applied to the bottom electrode at a frequency of 2 MHz. The pressure in the chamber was maintained at 30 mTorr, and the gap between the electrodes was set to 13 mm. A process gas mixture containing the following gas flows was introduced into the plasma etching chamber: 75 sccm Ar, 7.6 sccm C5H9F5Si, and an O2 flow rate varying from 0 to 20 sccm. The plasma etching process was performed for 1 minute. Figure 13 summarizes the estimated etch rates as a function of O2 flow rate for substrates containing one of the following plasma etch materials: SiO2, Si3N4, aC, poly-Si, and W. Table 5 summarizes the experimental conditions that exhibited high selectivity etching windows along with the recorded etch rates for the tested materials.
[0190] Example 13 Plasma etching was performed in a manner similar to Example 12, except that the process gas mixture was replaced with the following: 125 sccm Ar, 9 sccm C4F6, 14 sccm O2, and a C5H9F5Si flow rate varying from 0 to 2.5 sccm. Figure 14 summarizes the estimated etch rate as a function of C5H9F5Si flow rate for substrates containing one of the following plasma etch materials: SiO2, Si3N4, aC, poly-Si, and W. Table 5 summarizes the experimental conditions that exhibited high selectivity etch windows along with the recorded etch rates for the tested materials.
[0191] Example 14 Plasma etching was performed in a plasma etching device with 1000 W of power applied to the top electrode at a frequency of 60 MHz and 7000 W of power applied to the bottom electrode at a frequency of 2 MHz. The power to both the top and bottom electrodes was pulsed at a frequency of 500 Hz and a duty cycle of 60%. The pressure in the chamber was maintained at 20 mTorr, and the gap between the electrodes was set to 20 mm. A process gas mixture containing the following gas flows was introduced into the plasma etching chamber: 150 sccm Ar, 40 sccm O, 65 sccm C4F8, and a flow rate of C4H9F3Si varying from 0 to 10 sccm. The plasma etching process was performed for 30 seconds. Figure 15 summarizes the estimated etch rate as a function of C4H9F3Si flow rate for substrates containing one of the following plasma etching materials: SiO2, Si3N4, aC, poly-Si, and W. The experimental conditions that represent the etching window with high selectivity along with the recorded etching rates for the tested materials are summarized in Table 5.
[0192] Example 15 Plasma etching was performed in a manner similar to Example 14, except that the process gas mixture was replaced with the following: 150 sccm Ar, 30 sccm O, 5 sccm C4H9F3Si, and the flow rates of C4F8 and CH2F2 varied from 0 to 60 sccm while maintaining the total flow rate of both C4F8 and CH2F2 at 60 sccm. Figure 16 summarizes the estimated etch rates as a function of CH2F2 flow rate for substrates containing one of the following plasma etch materials: SiO2, Si3N4, aC, poly-Si, W, SiC, SiCN, and SiON. Table 5 summarizes the experimental conditions that exhibited highly selective etch windows along with the recorded etch rates for the tested materials.
[0193] Example 16 Plasma etching was performed in a manner similar to Example 14, except that the process gas mixture was replaced with the following: 150 sccm Ar, 30 sccm O, 60 sccm CHF, and a flow rate of C4H9F3Si varying from 0 to 25 sccm. Figure 17 summarizes the estimated etch rate as a function of C4H9F3Si flow rate for substrates containing one of the following plasma etch materials: SiO2, Si3N4, aC, poly-Si, W, SiC, SiCN, and SiON. Table 5 summarizes the experimental conditions that exhibited high selectivity etch windows along with the recorded etch rates for the tested materials.
[0194] As can be seen from Table 5, the etch rates vary over a wide range depending on the gas mixture selected and the type of material used to etch. There are few gas flow combinations that allow a particular material to be exclusively etched with infinite selectivity over the other tested materials. For example, in Examples 12 and 14, when the conditions listed in Table 5 were used in the etching process, it was possible to etch SiO with infinite selectivity over all other tested materials. Furthermore, as can be clearly seen from Figure 14, when C4H9F3Si was not added to the process gas mixture (0 sccm C4H9F3Si condition), all tested materials were etched during the process, resulting in a decrease in SiO2 etch selectivity. The same trend is reflected in Figure 17, where increasing the additional flow rate of C5H9F5Si gradually increased SiO2 etch selectivity, up to the point where infinite selectivity to poly-Si, Si3N4, and W was achieved, along with high selectivity to aC. The decrease in etch rates for all materials with increasing Si-containing hydrofluorocarbon flow rates seen in Figures 15 and 16 directly indicates that the inhibition of the etch process is related to polymer deposition promoted by the addition of C4H9F3Si or C5H9F5Si. Importantly, while the etching of Si3N4, poly-Si, aC, and W was suppressed, the etch rate of SiO2 remained relatively high (620 nm / min in Example 14), indicating that despite the effective promotion of polymer deposition, it is still possible to maintain the etching of certain materials at reliable etch rates even when Si-containing hydrofluorocarbons are added to the working gas mixture.
[0195] In Example 14, C4F8 was used as the primary etchant, which is effective for SiO2 etching, when C4H9F3Si was added to the gas mixture to promote polymer deposition and increased selectivity to materials other than SiO2. The same approach can be used for selective etching of other materials when a different primary etchant is used. In Example 16, CH2F2 was used as the primary etchant, which is effective for Si3N4 etching. Consequently, adding C4H9F3Si to the gas mixture suppressed etching of materials other than Si3N4 by promoting polymer deposition while maintaining an adequate etch rate for Si3N4. Furthermore, at C4H9F3Si flow rates above 10 sccm, the etch rate of Si3N4 was further enhanced by the presence of trifluoromethyl groups in the C4H9F3Si molecule, which provide a fluorocarbon to the process and can enhance etching of Si3N4 when polymer is being deposited on another material. For the conditions highlighted in Table 5 in Example 16, when 25 sccm of C4H9F3Si is added to the process gas mixture, infinite selectivity to aC, poly-Si, W, SiO2, SiC, SiCN, and SiON can be achieved; at lower flow rates of C4H9F3Si, or when C4H9F3Si is not added to the process gas mixture (0 sccm conditions in Figure 17), at least one other material from the list is etched along with Si3N4, resulting in loss of selectivity.
[0196] In addition, there were some conditions under which combinations of materials could be etched with infinite selectivity to other tested materials. For example, in Example 15, both Si3N4 and SiO2 could be etched with infinite selectivity to aC, poly-Si, W, SiC, SiCN, and SiON. In some cases, multiple materials need to be etched simultaneously with high selectivity to the remainder of the substrate, and this disclosure demonstrates that selective etching using Si-containing hydrofluorocarbons mixed with common gases (e.g., mixtures containing inert gases, fluorocarbons, hydrofluorocarbons, oxidizing gases, or combinations thereof) can be essential for this purpose.
[0197] In particular, when applying multi-color etching, several Si-containing films are typically present on the substrate and exposed during the etching process. Commonly used Si-containing films are SiO, SiN, SiC, SiCN, and SiON. Therefore, etching SiO, SiN, or both of these materials with high or infinite selectivity to another Si-containing material, achieved by the addition of Si-containing hydrofluorocarbons to the process gas mixture, has proven essential for advanced patterning of substrates using multi-color etching.
[0198] [Table 10]
[0199] Example 17 Plasma etching was performed in a plasma etching device with 1000 W of power applied to the top electrode at a frequency of 60 MHz and 7000 W of power applied to the bottom electrode at a frequency of 2 MHz. The power to both the top and bottom electrodes was pulsed at a frequency of 500 Hz and a duty cycle of 60%. The pressure in the chamber was maintained at 20 mTorr, and the gap between the electrodes was set to 20 mm. A process gas mixture containing the following gas flows was introduced into the plasma etching chamber: 150 sccm Ar, 30 sccm O, 60 sccm C4F8, and a flow rate of C2H6F2Si varying from 0 to 10 sccm. The plasma etching process was performed for 30 seconds. Figure 18 summarizes the estimated etch rate as a function of C2H6F2Si flow rate for substrates containing one of the following plasma etching materials: SiO2, Si3N4, aC, poly-Si, and W. The experimental conditions that represent the etching window with high selectivity along with the recorded etching rates for the tested materials are summarized in Table 6.
[0200] Example 18 Plasma etching was performed in a manner similar to Example 17, except that the process gas mixture was replaced with the following: 150 sccm Ar, 30 sccm O, 60 sccm C4F8, and a flow rate of CH3F3Si varying from 0 to 13 sccm. Figure 19 summarizes the estimated etch rate as a function of CH2F2 flow rate for substrates containing one of the following plasma etch materials: SiO2, Si3N4, aC, poly-Si, and W. Table 6 summarizes the experimental conditions that exhibited high selectivity etch windows along with the recorded etch rates for the tested materials.
[0201] [Table 11]
[0202] As can be seen from Table 6, the etch rates vary over a wide range depending on the gas mixture selected and the type of material used to etch. There are few gas flow combinations that allow a particular material to be etched exclusively with high selectivity or even infinite selectivity to the other tested materials. For example, in Examples 17 and 18, when the conditions listed in Table 6 were used in the etching process, it was possible to etch SiO with high selectivity or infinite selectivity to all other tested materials. Furthermore, as can be clearly seen from Figure 18, when C2H6F2Si was not added to the process gas mixture (0 sccm C2H6F2Si condition), all tested materials were etched during the process, resulting in a decrease in SiO2 etch selectivity. The same trend is reflected in Figure 19, where increasing the additional flow rate of CH3F3Si gradually increased SiO2 etch selectivity, up to the point where infinite selectivity to poly-Si, aC, and W was achieved, along with high selectivity to Si3N4. The decrease in etch rate for all materials with increasing Si-containing hydrofluorocarbon flow rate seen in Figures 18 and 19 directly indicates that the inhibition of the etch process is related to polymer deposition promoted by the addition of CH3F3Si or CH3F5Si, similar to that seen with C4H9F3Si and C5H9F5Si.
[0203] Examples 19 to 22 and Comparative Example 7 have the following conditions.
[0204] Plasma Etching Device: In the disclosed method, a parallel-plate (capacitively coupled plasma) plasma generator was used as the plasma etching device. The parallel-plate configuration included an upper electrode and a lower electrode, on which the substrate was placed (the lower electrode was used as a sample holder with cooling capability). The distance between the electrodes was 13 mm or 20 mm. When the lower electrode was connected to a 2 MHz power generator, the upper electrode was connected to a 27 MHz or 60 MHz power generator.
[0205] Plasma etching conditions: During the plasma etching process, the power supplied to the top electrode varied between 500 and 1000 W, the power applied to the bottom electrode varied between 750 and 7000 W, and the power applied to both the top and bottom electrodes could be pulsed at a lower frequency (e.g., 1 to 1000 Hz) and a duty cycle ranging from 10 to 99%. During the process, the pressure was maintained constant at a selected value ranging from 5 to 100 mTorr. The plasma etching time was set to a value between 30 and 60 seconds. The plasma process gas mixture included Ar, O, and a Si-containing hydrofluorocarbon gas such as CHFSi, CHFSi, or CHFSi.
[0206] Substrate: Referring to Figures 4a and 4b, a single-crystal silicon wafer piece with a thin film of the target plasma etching material on the wafer was used as the substrate. The target plasma etching material was one from the following list: SiO2, Si3N4, amorphous carbon (hereinafter "aC"), polycrystalline silicon (hereinafter "poly-Si"), and W. The initial thickness of each target plasma etching material was as follows: 300 nm of aC, 110 nm of W, 550 nm of poly-Si, 300 nm of Si3N4, and 2000 nm of SiO2.
[0207] Plasma etch rate and selectivity: The plasma etch rate was estimated as the difference between the initial thickness of the material film to be plasma etched and the thickness of the film after the etching process divided by the duration of the etching process in minutes, resulting in an etch rate in nm / min. Selectivity was estimated as the ratio of the etch rates calculated for two different plasma etched materials. The term "infinite selectivity" refers to the case where material is removed from the substrate during the etching process while the unetched material remains intact or a thin film is deposited on the unetched material.
[0208] Example 19 Plasma etching was performed in a plasma etching device with 750 W of power applied to the top electrode at a frequency of 27 MHz and 1500 W of power applied to the bottom electrode at a frequency of 2 MHz. The pressure in the chamber was maintained at 30 mTorr, and the gap between the electrodes was set to 13 mm. A process gas mixture containing the following gas flows was introduced into the plasma etching chamber: 75 sccm Ar, 7.6 sccm C4H9F4Si, and an O2 flow rate varying from 0 to 20 sccm. The plasma etching process was performed for 1 minute. Figure 20 summarizes the estimated etch rates for O2 flow rates on substrates containing one of the following plasma etching materials: SiO2, Si3N4, aC, poly-Si, and W. Table 7 summarizes the experimental conditions that represent the etch window for aC with high selectivity, along with the recorded etch rates for the tested materials. An etch rate value of 0 nm / min indicates polymer deposition on the investigated film, meaning the film was not etched; infinite selectivity was obtained for non-etched material films.
[0209] [Table 12]
[0210] Example 20 Plasma etching was performed in a plasma etching device with 700 W of power applied to the top electrode at a frequency of 60 MHz and 7000 W of power applied to the bottom electrode at a frequency of 2 MHz. The power applied to both the top and bottom electrodes was pulsed at a frequency of 500 Hz and a duty cycle of 60%. The pressure in the chamber was maintained at 25 mTorr, and the gap between the electrodes was set to 30 mm. A process gas mixture containing the following gas flows was introduced into the plasma etching chamber: 150 sccm Ar, 20 sccm C4H9F3Si, and an O2 flow rate varying from 5 to 90 sccm. The plasma etching process was performed for 30 seconds. Figure 21 summarizes the estimated etch rate as a function of O2 flow rate for substrates containing one of the following plasma etching materials: SiO2, Si3N4, aC, W-doped aC, poly-Si, and W. The experimental conditions that represent the etching window for aC and W-doped aC with high selectivity along with the recorded etching rates for the tested materials are summarized in Table 7. An etching rate value of 0 nm / min indicates that polymer was deposited on the studied film, meaning that the film was not etched, and infinite selectivity was obtained for the unetched material film.
[0211] Comparative Example 7 Plasma etching was performed in a manner similar to Example 20, except that the 15 sccm flow rate of C4H9F3Si was replaced with a 15 sccm flow rate of C4F6 in the process gas mixture. Figure 22 summarizes the estimated etch rates as a function of O2 flow rate for substrates containing one of the following plasma etch materials: SiO2, Si3N4, aC, W-doped aC, poly-Si, and W. Table 7 summarizes the recorded etch rates for each material compared to the same conditions in Example 20 with the addition of C4H9F3Si.
[0212] As can be seen from Table 7 and Figures 21 and 22, there is good consistency between the results of Experiments 1 and 2. Increasing the O2 flow rate while keeping other parameters the same increases the aC etch rate while maintaining high or infinite selectivity to the other tested materials due to polymer deposition. In particular, in Example 19, where the O2 flow rate was 12 sccm, and Example 20, where the O2 flow rate exceeded 65 sccm, amorphous carbon was observed to be etched with infinite selectivity to poly-Si, SiO2, Si3N4, and W. These conditions appear promising for patterning aC hard masks or other organic materials due to the infinite selectivity to materials typically protected by hard masks. Infinite selectivity allows for rapid etching of the mask without concern for damaging layers below the mask and distorting the mask pattern after etching (e.g., undercutting). The difference in aC etch rate at low O2 flow rates between Examples 19 and 20 can be explained by the stronger ion bombardment in Example 20 as a result of the higher applied power, resulting in additional etch rate due to sputtering. It should also be noted that under certain conditions it is possible to etch both aC and W selectively to all other tested materials, suggesting that etching of W-doped aC is possible under these conditions.
[0213] Furthermore, in Example 20, where the O2 flow rate exceeded 45 sccm, it was possible to etch W-doped aC, which may be essential for high aspect ratio etching applications (such as ONON channel etching or step contact etching in 3D NAND), where a robust mask is required for the long process where the doped aC is used as a hard mask. The infinite selectivity observed over other tested materials ensures that films covered by the mask (such as Si3N4 or SiO2) are not damaged during the patterning of the mask itself.
[0214] Another potential application is selective mask removal using the gas mixtures discussed in this disclosure. The use of Si-containing hydrofluorocarbons in the process gas mixture allows for selective removal of aC masks from substrates without damaging other materials. On the other hand, as seen in Comparative Example 19, when C4H9F3Si is not added to the process gas mixture and CF6 is added instead at the same flow rate, it is possible to etch aC and W-doped aC. However, even though CF6 is a gas commonly used to promote polymerization to protect hard masks or sidewalls during high-aspect-ratio etch processes, the selectivity to other tested materials is significantly reduced when CF6 is used. The low selectivity of aC and doped aC etching limits the process window for mask patterning or removal, potentially making the process impractical for certain applications.
[0215] Therefore, it can be concluded that adding Si-containing hydrofluorocarbon gases to a process gas mixture can significantly increase selectivity to non-etched materials through robust polymer deposition, which can be compared to the typical Ar+O2+C4F6 gas mixture, while maintaining adequate etch rates for the target organic films. The benefits of using Si-containing hydrofluorocarbons are expected to be the same compared to using an Ar+O2 gas mixture to selectively etch organic films.
[0216] Example 21 Plasma etching was performed in a plasma etching device with 700 W of power applied to the top electrode at a frequency of 60 MHz and 7000 W of power applied to the bottom electrode at a frequency of 2 MHz. The power applied to both the top and bottom electrodes was pulsed at a frequency of 500 Hz and a duty cycle of 60%. The pressure in the chamber was maintained at 25 mTorr, and the gap between the electrodes was set to 20 mm. A process gas mixture containing the following gas flows was introduced into the plasma etching chamber: 150 sccm Ar, 20 sccm C2H6F2Si, and an O2 flow rate varying from 0 to 90 sccm. The plasma etching process was performed for 30 seconds. Figure 23 summarizes the estimated etch rate as a function of O2 flow rate for substrates containing one of the following plasma etching materials: SiO2, Si3N4, aC, and W. Table 8 summarizes the experimental conditions, which represent the etch window for aC with high selectivity, along with the recorded etch rates for the tested materials. An etch rate value of 0 nm / min indicates that polymer was deposited on the studied film, meaning that the film was not etched, resulting in infinite selectivity for the non-etched material film.
[0217] [Table 13]
[0218] Example 22 Plasma etching was performed in a manner similar to Example 21, except that the process gas mixture was replaced with the following: 150 sccm Ar, 25 sccm CH3F3Si, and O2 flow rates varying from 0 to 90 sccm. Figure 24 summarizes the estimated etch rates as a function of O2 flow rate for substrates containing one of the following plasma etch materials: SiO2, Si3N4, aC, poly-Si, and W. Table 8 summarizes the experimental conditions that represent an etch window for aC with high selectivity, along with the recorded etch rates for the tested materials. An etch rate value of 0 nm / min indicates polymer deposition on the studied film, meaning that the film was not etched; infinite selectivity was obtained for the unetched material film.
[0219] As can be seen from Table 8 and Figures 23-24, there is good consistency between the results of Experiments 21-22, which used gas mixtures containing Si-containing hydrofluorocarbons. Increasing the O2 flow rate while keeping other parameters the same increases the aC etch rate while maintaining high or infinite selectivity to the other tested materials due to polymer deposition. In particular, in Example 21, where the O2 flow rate exceeded 65 sccm, and in Example 22, where the O2 flow rate exceeded 45 sccm, amorphous carbon was observed to be etched with infinite selectivity to poly-Si, SiO2, Si3N4, and W. These conditions appear promising for patterning aC hard masks or other organic materials due to the infinite selectivity to materials typically protected by hard masks. Infinite selectivity allows for rapid etching of the mask without concern for damage to layers below the mask and distortion of the mask pattern after etching (e.g., undercutting). The results observed with CH3F3Si and C2H6F2Si demonstrate the same trends as those described in Examples 19-20 for C4H9F3Si, confirming the promise of Si-containing hydrofluorocarbons for the development of selective etching processes for organic materials.
[0220] Examples 23 to 32 relating to the circulating plasma dry etching method have the following conditions.
[0221] Plasma Etching Device: In the disclosed method, a parallel-plate (capacitively coupled plasma) plasma generator was used as the plasma etching device. The parallel-plate configuration included an upper electrode and a lower electrode, on which the substrate was placed (the lower electrode was used as a sample holder with cooling capabilities). The distance between the electrodes was 13 mm or 20 mm. When the lower electrode was connected to a 2 MHz generator, the upper electrode was connected to a 27 MHz or 60 MHz generator.
[0222] Plasma Etching Conditions: During the plasma etching process, the power supplied to the top electrode varied between 500 and 2000 W, and the power applied to the bottom electrode varied between 750 and 7000 W. The power applied to both the top and bottom electrodes could be pulsed at a lower frequency (e.g., 1 to 1000 Hz) and a duty cycle ranging from 199%. During the process, the pressure was maintained constant at a selected value ranging from 5 to 100 mTorr. The plasma etching time was set to a value between 10 and 60 seconds. The deposition rate was estimated in nanometers per minute. Negative deposition rates represent the state when the substrate material is etched. The plasma process gas mixture included at least one of the following gases: Ar, O, C4F6 and / or C4F8 as fluorocarbon gases, C4H9F3Si or C5H9F5Si as Si-containing hydrofluorocarbon gases, and CH2F2 as hydrofluorocarbon gases.
[0223] Substrate: Referring to Figures 5a and 5d, a single-crystal silicon wafer piece with a thin film of the target plasma etching material on the wafer was used as the substrate. The target plasma etching material was one from the following list: SiO2, Si3N4, amorphous carbon (hereinafter "aC"), polycrystalline silicon (hereinafter "poly-Si"), W, SiC, SiCN, or SiON. The initial thickness of each target plasma etching material was as follows: 300 nm aC, 110 nm W, 550 nm poly-Si, 2050 nm Si3N4, 200 nm SiO2, 105 nm SiC, 300 nm SiCN, and 315 nm SiON.
[0224] Plasma Etch Rate and Selectivity: The plasma deposition or etch rate was estimated as the difference between the initial thickness of the material film being plasma etched and the thickness of the film after the etching process, divided by time, to give the etch or deposition rate in nm / min. In some instances, a negative deposition rate represents etching of the sample (and is actually equivalent to the etch rate value).
[0225] Cyclic Etching Process: The disclosed cyclic etching process refers to a process where a substrate is processed in an etching chamber using several etching steps that are repeated in sequence. An example of a substrate processed using cyclic etching is shown in Figures 5a-5d. An example of an initial substrate consisting of substrate 702 having multiple thin films thereon is shown in Figure 5a, where film 704 acts as a mask, films 706, 708, and 710 are films of a material not to be etched, and film 712 is a film of a material to be etched.
[0226] The substrate after the first step of the etching cycle is shown in FIG. 5b. During the first step, material was partially removed 716 using a selective etching recipe, resulting in the deposition of polymer 714 on the unetched material, creating a mask with a polymer thickness depending on the film material. The substrate after the second step of the cycle is shown in FIG. 5c. In the second step, an etching recipe with non-infinite selectivity to the polymer deposited in the first step was used, resulting in further etching of the target material 718 and removal of the polymer from the unetched material. Depending on the unetched material and process conditions, some polymer may remain in the unetched material film, as shown in FIG. 5d, or a portion of the unetched material film may be etched in the second step after the polymer has been completely removed. However, the cyclical process in this disclosure is not limited in any way to the presented examples, and the process steps, the number of process steps in the cycle, the substrate, and the plasma etching process may vary. For example, some steps in a cycle may be only deposition steps without etching, and the substrate may have a single film of material instead of the multiple films 706, 708, 710, 712 shown in the example.
[0227] Example 23 Plasma etching conditions: Plasma etching was performed in a plasma etching device with 750 W of power applied to the top electrode at a frequency of 27 MHz and 1500 W of power applied to the bottom electrode at a frequency of 2 MHz. The pressure in the chamber was maintained at 30 mTorr, and the gap between the electrodes was set to 13 mm. A process gas mixture containing the following gas flows was introduced into the plasma etching chamber: 75 sccm Ar, 7.6 sccm C5H9F5Si, and an O2 flow rate varying from 0 to 20 sccm. The plasma etching process was performed for 1 minute. Figure 25 summarizes the estimated deposition rate as a function of O2 flow rate for substrates containing one of the following plasma etched materials: SiO2, Si3N4, aC, poly-Si, and W.
[0228] Example 24 Plasma etching was performed in a manner similar to Example 23, except that the process gas mixture was replaced with the following: 75 sccm Ar, 9 sccm C4F6, 14 sccm O2, and a flow rate of C5H9F5Si varying from 0 to 2.5 sccm. Figure 26 summarizes the estimated deposition rate as a function of C5H9F5Si flow rate for substrates containing one of the following plasma etch materials: SiO2, Si3N4, aC, poly-Si, and W.
[0229] Example 25 Plasma etching was performed in a manner similar to Example 23, except that the process gas mixture was replaced with the following: 125 sccm Ar, 9 sccm C4F8, 14 sccm O2, and a flow rate of C5H9F5Si varying from 0 to 2.5 sccm. Figure 27 summarizes the estimated polymer deposition rate as a function of C5H9F5Si flow rate for substrates containing one of the following plasma etch materials: SiO2, Si3N4, aC, poly-Si, and W.
[0230] Example 26 Plasma etching conditions: Plasma etching was performed in a plasma etching device with 700 W of power applied to the top electrode at a frequency of 60 MHz and 7000 W of power applied to the bottom electrode at a frequency of 2 MHz. The power to both the top and bottom electrodes was pulsed at a frequency of 500 Hz and a duty cycle of 60%. The pressure in the chamber was maintained at 20 mTorr, and the gap between the electrodes was set to 20 mm. A process gas mixture containing the following gas flows was introduced into the plasma etching chamber: 150 sccm Ar, 15 sccm C4H9F3Si, and an O2 flow rate varying from 0 to 90 sccm. The plasma etching process was performed for 30 seconds. Figure 28 summarizes the estimated deposition rate as a function of O2 flow rate for substrates containing one of the following plasma etched materials: SiO2, Si3N4, aC, poly-Si, and W.
[0231] Example 27 Plasma etching was performed in a manner similar to Example 26, except that the power applied to the top electrode was 1000 W and the process gas mixture was replaced with the following: 150 sccm Ar, 40 sccm O, 65 sccm C4F8, and a flow rate of C4H9F3Si varying from 0 to 10 sccm. Figure 29 summarizes the estimated deposition rate as a function of C4H9F3Si flow rate for substrates containing one of the following plasma etch materials: SiO2, Si3N4, aC, poly-Si, W, SiC, SiCN, SiON.
[0232] Example 28 Plasma etching was performed in a manner similar to Example 26, except that the power applied to the top electrode was 1000 W and the process gas mixture was replaced with the following: 150 sccm Ar, 30 sccm O, 5 sccm C4H9F3Si, with the flow rates of C4F8 and CH2F2 varying from 0 to 60 sccm while maintaining the total flow rate of both C4F8 and CH2F2 at 60 sccm. Figure 30 summarizes the estimated deposition rate as a function of CH2F2 flow rate for substrates containing one of the following plasma etch materials: SiO2, Si3N4, aC, poly-Si, W, SiC, SiCN, SiON.
[0233] Example 29 Plasma etching was performed in a manner similar to Example 26, except that the power applied to the top electrode was 1000 W and the process gas mixture was replaced with the following: 150 sccm Ar, 30 sccm O, 60 sccm CHF, and a flow rate of C4H9F3Si varying from 0 to 25 sccm. Figure 31 summarizes the estimated deposition rate as a function of C4H9F3Si flow rate for substrates containing one of the following plasma etch materials: SiO2, Si3N4, aC, poly-Si, W, SiC, SiCN, and SiON.
[0234] Example 30 Plasma etching conditions: The cyclic plasma etching process was performed in a plasma etching device with 1000 W of power applied to the top electrode at a frequency of 60 MHz and 7000 W of power applied to the bottom electrode at a frequency of 2 MHz, and the power to both the top and bottom electrodes was pulsed at a frequency of 500 Hz and a duty cycle of 60%. The pressure in the chamber was maintained at 20 mTorr, and the gap between the electrodes was set to 20 mm.
[0235] Each cycle included two etching steps: a first step, selective etching of Si3N4 (depositing polymer on materials other than Si3N4), and a second step, aggressive etching of Si3N4 with low selectivity (which etches the polymer deposited in the first step and materials other than Si3N4).
[0236] During the first etching cycle, the first step was performed using a process gas mixture supplied to the chamber containing the following gas flows: 150 sccm Ar, 25 sccm C4H9F3Si, 60 sccm CH2F2, and 30 sccm O2. The plasma etching process during the first step was performed for 17 seconds. The second step was performed using a process gas mixture supplied to the chamber containing the following gas flows: 150 sccm Ar, 15 sccm C4F8, 45 sccm CH2F2, and 30 sccm O2. The plasma etching process during the second step was performed for 10 seconds.
[0237] In the second and subsequent cycles, the same gas mixture was used for the first and second steps within each cycle as in the first cycle, but the duration of each step was changed: in the second and subsequent etching cycles, the duration of the first step with selective etching was set to 10 seconds, and the duration of the second step without selective etching was set to 40 seconds.
[0238] Figure 32 summarizes the thickness of SiO2, Si3N4, aC, poly-Si, W, SiC, SiCN, and SiON films after the cyclic etching process as a function of the number of cycles. While an increase in the thickness of the studied films reflects the deposition of polymer on the substrate, a decrease in the thickness of the studied films reflects the etching of the substrate. The value shown at 0 cycles represents the initial thickness of the studied films.
[0239] Example 31 Plasma etching conditions: The cyclic plasma etching process was performed in a plasma etching device with 700 W of power applied to the top electrode at a frequency of 60 MHz and 7000 W of power applied to the bottom electrode at a frequency of 2 MHz, and the power to both the top and bottom electrodes was pulsed at a frequency of 500 Hz and a duty cycle of 60%. The pressure in the chamber was maintained at 25 mTorr, and the gap between the electrodes was set to 20 mm.
[0240] Each cycle included two etching steps: a first step, a selective etch of Pt (depositing polymer on materials other than Pt) and a second step, a low selectivity etch of Pt (which etches the polymer deposited in the first step and materials other than Pt).
[0241] The first step was performed using a process gas mixture supplied to the chamber containing the following gas flows: 150 sccm Ar, 15 sccm C4H9F3Si, and 15 sccm O2. The plasma etching process during the first step was performed for 60 seconds. The second step was performed using a process gas mixture supplied to the chamber containing the following gas flows: 150 sccm Ar, 65 sccm C4F8, and 30 sccm O2. The plasma etching process during the second step was performed for 9 seconds. The estimated etch rates for each material per etching cycle are summarized in Table 9. Figure 34 summarizes the thicknesses of Pt, aC, poly-Si, SiC, and Si3N4 films after one etching cycle. While an increase in the thickness of the observed films reflects the deposition of polymer on the workpiece, a decrease in the thickness of the observed films reflects the etching of the workpiece. The value shown for cycle 0 represents the initial thickness of the observed films.
[0242] Example 32 Plasma etching conditions: Plasma etching was performed in a plasma etching device with 700 W of power applied to the top electrode at a frequency of 60 MHz and 7000 W of power applied to the bottom electrode at a frequency of 2 MHz. The power to both the top and bottom electrodes was pulsed at a frequency of 500 Hz and a duty cycle of 60%. The pressure in the chamber was maintained at 25 mTorr, and the gap between the electrodes was set to 20 mm. A process gas mixture containing the following gas flows was introduced into the plasma etching chamber: 150 sccm Ar, 15 sccm C4H9F3Si, and 15 sccm O2. The plasma etching process was performed for 30 seconds. The estimated etch rates for each material per etch cycle are summarized in Table 9. Negative etch rates correspond to the case where a polymer is deposited on the studied material and reflect the deposition rate.
[0243] Based on the assumption that the amount of etched material or deposited polymer removed increases linearly with process time, it was estimated that the process described in this example would need to be run for approximately 54 seconds to remove the same amount of Pt as reported for one etch cycle in Example 31. Figure 34 summarizes the estimated thicknesses of Pt, aC, poly-Si, SiC, and Si3N4 for the process reported in Example 32 over a 54 second period.
[0244] [Table 14]
[0245] As can be seen from Examples 23-32 in Figures 25-32, the polymer deposition or etch rate varies greatly depending on the gas mixture used and the target material. Conditions where one of the materials is etched when the polymer is deposited on the other (infinite selectivity case), or where the polymer is deposited at different rates on various materials, can be used to develop a cyclical etch process. For example, in FIG. 25, SiO2 is etched with infinite selectivity to other tested materials using 16 sccm O2; in FIG. 27, SiO2 is etched with infinite selectivity to other tested materials using 2 sccm C5H9F5Si; in FIG. 28, aC is etched with infinite selectivity to other tested materials using O2 flow rates greater than 60 sccm; in FIG. 29, SiO2 is etched with infinite selectivity to other tested materials when the C4H9F3Si flow rate is greater than 8 sccm; in FIG. 30, SiO2 or Si3N4 can be etched with infinite selectivity to other tested materials when the CH2F2 flow rate is 20-40 sccm; and in FIG. 31, Si3N4 can be etched with infinite selectivity to other processed materials when the C4H9F3Si flow rate is 25 sccm. These conditions with infinite selectivity can be used to develop cyclical recipes using at least two steps in a cycle, where the first step in the cycle is an etch of the target material with infinite selectivity and the second step is an aggressive etch of the target material with a high etch rate and low selectivity. In this case, if the aggressive etch is used to improve etch rate and throughput, the polymer deposited during the first step of the selective etch protects the non-etched material during the aggressive etch. In addition, the use of an aggressive or low-selectivity etch step can remove the polymer from the surface of the non-etched material, allowing for fine tuning to reach a state where the target material is etched at the appropriate rate after each cycle, while the non-etched material remains close to its initial state.
[0246] In Example 30, a cyclical etching process was developed using the conditions of Example 29 with infinite selectivity for etching Si3N4 in the first step within the etching cycle. As can be seen from Figure 32, using a cyclical etching recipe with selective and aggressive etching steps within each cycle, it is possible to achieve a reasonably fast etching rate for Si3N4 when very little polymer is deposited on SiO2 and SiON, and tens of nanometers of polymer are deposited on other materials. While the current etching process was optimized to selectively etch Si3N4 relative to SiO2 and SiON, the cyclical etching process can be further tuned to etch Si3N4 selectively relative to other tested materials by varying the duration of each step in the process conditions. In Example 30, the duration of steps within the cycle was changed after the first cycle due to surface modification of the non-etched material. After the first cycle, a thin film of polymer (a few nanometers) remained on the SiO2 and SiON surfaces, resulting in a change in the rate of polymer deposition starting from the second cycle. An important observation from Figure 32 is that the use of a cyclical recipe reduced polymer growth, and the polymer thickness did not grow significantly in the second and subsequent cycles.
[0247] Figure 33 shows the estimated thickness of the studied material film (reflecting etching of the film or deposition of polymer on the surface of the film) if a continuous infinitely selective etching recipe for SiN is used instead of the cyclical process, at the same SiN thickness as shown in Figure 32. The estimate was based on the conditions of Example 29, which featured an infinitely selective etching of SiN (25 sccm C4H9F3Si in Figure 31), and the assumption that the etching or deposition rate increases linearly with increasing duration of the process.
[0248] A comparison of Figures 32 and 33 clearly shows that the developed cyclical recipe can effectively reduce polymer deposition on the unetched material and maintain the unetched material close to its initial state. In the case of continuous selective etching, polymer continuously deposits during the process, resulting in a polymer thickness greater than the initial film thickness for some of the tested materials. A similar observation can be made in Examples 31 and 32. As shown in Figure 34, when Pt is etched using the cyclical recipe of Example 31, high etching selectivity of Pt relative to aC, poly-Si, and SiC (selectivity to aC: 45, selectivity to poly-Si: 18, selectivity to Si3N4: 18, selectivity to SiC: 18) can be achieved without polymer remaining on the unetched material. In contrast, etching Pt using the continuous recipe of Example 32 would result in thick polymer deposition on the unetched material, which, despite infinite selectivity, may limit the applicability of the process due to issues with further processing workpieces with thick polymer films.
[0249] The presence of thick polymers after successive selective etches requires the use of post-etch process cleaning recipes to remove the polymer, which can potentially damage exposed target materials, masks, and structures, further limiting the use of selective etch processes in the fabrication of novel semiconductor devices. In contrast, with the disclosed cyclical etch process, after the etch process, only a thin film of polymer or a thin modified layer on the surface of the non-etched material is present, which can be easily removed by selective cleaning, minimizing potential damage and reducing processing time. Additionally, a gentle cleaning step or a separate etching step can be included within each cycle or within several defined cycles to further tailor the cyclical etch process to remove the presence of polymer or modified layer on the surface of the non-etched material and maintain the non-etched material film in a state close to its original state after the cyclical etch.
[0250] Meanwhile, the different polymer deposition rates on the surfaces of various materials observed in Examples 1-7 can be used to develop cyclical etching recipes using steps within each cycle that include polymer deposition and etching. For example, in Figure 26, using 1.25 sccm of C5H9F5Si, a thinner film of polymer is deposited on aC and SiO2 compared to W, SiN, and poly-Si. In Figure 28, using 15 sccm of O2, only a few nanometers of polymer is deposited on SiO2, while more than 40 nm is deposited on aC, Si3N4, and poly-Si after a 1-minute process. If the demonstrated polymer deposition at different rates on various materials is used as the first step in a cycle followed by a non-selective etching step, the thinnest film of polymer is removed first, and the exposed material below it is etched, resulting in a thicker polymer film after the deposition step, leaving some polymer behind on the other films. If the target material is the material with the lowest polymer deposition rate from a selected group of materials, fine-tuning the cyclic etching process as in Example 30 makes it possible to etch the target material and maintain the unetched material close to its original state after the cyclic etching process.
[0251] The results demonstrated in this disclosure demonstrate that polymer deposition can be achieved at variable rates depending on the target material, and that etching certain materials with infinite selectivity, which is possible when Si-containing hydrofluorocarbons are added to the process gas mixture, appears promising for the development of cyclical etch processes (Examples 23-32). It was further demonstrated that, in the case of a continuous process with infinite selectivity, where thick polymer films would deposit and require further processing or additional cleaning, it is possible to suppress polymer deposition using a cyclical process, preserving the unetched material in a near-pristine state. The developed cyclical etch process, which uses Si-containing hydrofluorocarbons in at least one of the cycle steps, appears promising for advanced patterning of substrates during semiconductor device fabrication. In particular, in applications involving multiple patterning, multicolor etching, or low-contrast etching, several Si-containing films are typically present on the substrate and exposed during the etching process. Commonly used Si-containing films in these processes are SiO2, Si3N4, SiC, SiCN, and SiON; therefore, the ability to selectively etch SiO2, Si3N4, or both of these materials, achieved by a cyclic etching process in which a Si-containing hydrofluorocarbon is added to the process gas mixture in at least one of the cycle steps, has been demonstrated to be essential for advanced patterning of substrates using multicolor etching. In addition, the demonstrated ability to selectively etch or deposit thin polymer films over organic materials (e.g., aC) appears promising for patterning or removing organic masks, as it provides high selectivity to materials other than the processed mask and does not result in the deposition of thick films over these materials.
[0252] Although the subject matter described herein may be described in the context of example implementations for processing one or more computing application functions / operations for a computing application having a user-interactive component, the subject matter is not limited to these particular embodiments. Rather, the techniques described herein may be applied to any suitable type of user-interactive component execution management method, system, platform, and / or apparatus.
[0253] It will be understood that many additional changes in the details, materials, steps, and arrangements of parts described and illustrated herein to explain the principles of the invention may be made by those skilled in the art within the principles and scope of the invention as expressed in the appended claims. Accordingly, it is not intended that the invention be limited to the specific embodiments in the above examples and / or accompanying drawings.
Claims
1. 1. An etching method for forming an aperture in a substrate, comprising: loading the substrate on a loading table in a reactor, the substrate including a Si-containing film deposited thereon and a patterned mask layer deposited on the Si-containing film; introducing an etching gas comprising vapor of a Si-containing hydrofluorocarbon into the reactor; converting the etching gas into a plasma; and causing an etching reaction between the plasma and the Si-containing film to etch the Si-containing film against the patterned mask layer, thereby forming the aperture.
2. The etching gas is CF 4 , C 2 F 6 , C 3 F 6 , C 4 F 6 , C 4 F 8 , C 5 F 8 , C 5 F 10 , C 6 F 12 , C 7 F 14 , C 8 F 16 , C.H. 2 F 2 , C.H. 3 F, C.H.F. 3 , C 2 H 5 F.C. 3 H 7 F.C. 5 H.F. 7 , C 3 H 2 F 6 , C 3 H 4 F 2 , C 3 H 2 F 4 , C 4 H 2 F 6 or C 4 H 3 F 7 2. The method of claim 1, comprising vapor of a fluorocarbon or hydrofluorocarbon selected from the group consisting of:
3. The etching gas is O 2 , O 3 , CO, CO 2 , SO, SO 2 ,FNO,NO,N 2 O, NO 2 , H 2 10. The method of claim 1, comprising an oxidizing gas selected from O, COS, or a combination thereof.
4. The method of claim 1 , wherein the etching gas comprises an inert gas selected from He, Ar, Xe, Kr, or Ne.
5. The etching gas is H 2 , S.F. 6 , N.F. 3 , N 2 , N.H. 3 , Cl 2 , BCl 3 , B.F. 3 , B 2 , F 2 5. The method of claim 1, further comprising an additional gas selected from the group consisting of HBr, HCl, or combinations thereof.
6. The Si-containing hydrofluorocarbon is represented by the general formula C x H y F z S n 2. The method of claim 1 , wherein: (1≦x≦6, 1≦y≦9, 1≦z≦15, n=1 or 2).
7. The method of claim 6 , wherein the Si-containing hydrofluorocarbon comprises one or more methyl groups.
8. The method of claim 7, wherein the Si-containing hydrofluorocarbon comprises at least one methyl group bonded to a Si atom.
9. The Si-containing hydrofluorocarbon is a CH 4 F 2 Si, CH 3 F 3 Si, C 2 H 6 F 2 Si, C 3 H 9 FSi, C 4 H 9 F 3 Si, C 5 H 9 F 5 Si, C 4 H 10 F 4 S 2 , C 2 H 6 F 4 S 2 , C 3 H 9 F 3 S 2 , C 6 H 9 F 7 2. The method of claim 1 , wherein said first and second aryl groups are selected from the group consisting of aryl, aryloxy ...
10. The Si-containing hydrofluorocarbon is CH 3 F 3 2. The method of claim 1 , wherein said compound is selected from the group consisting of aryl, aryloxy ...
11. The Si-containing hydrofluorocarbon is 2 H 6 F 2 2. The method of claim 1 , wherein said compound is selected from the group consisting of aryl, aryloxy ...
12. The Si-containing hydrofluorocarbon is 4 H 9 F 3 2. The method of claim 1 , wherein said compound is selected from the group consisting of aryl, aryloxy ...
13. The Si-containing hydrofluorocarbon is 5 H 9 F 5 2. The method of claim 1 , wherein said compound is selected from the group consisting of aryl, aryloxy ...
14. The silicon-containing film is selected from silicon oxide, silicon nitride, crystalline Si, polysilicon, polycrystalline silicon, amorphous silicon, low-k SiCOH, SiOCN, SiC, and SiON. a O b H c C d N e 14. The method of any one of claims 1 to 13, comprising layers of (a>0, b, c, d and e≧0), or layers of alternating silicon oxide and silicon nitride (ONON) layers, or layers of alternating silicon oxide and polysilicon (OPOP) layers.
15. The method of any one of claims 1 to 13, wherein the aperture formed in the substrate has an aspect ratio of from about 1:1 to about 500:
1.
16. 1. An etching method for forming an aperture in a substrate, comprising: loading the substrate on a loading table in a reactor, the substrate having a silicon-containing film deposited thereon and a patterned mask layer deposited on the silicon-containing film; C 5 H 9 F 5 introducing an etching gas containing Si into the reactor; converting the etching gas into a plasma; and causing an etching reaction between the plasma and the silicon-containing film to proceed, thereby etching the silicon-containing film against the patterned mask layer to form the aperture.
17. 1. An etching method for forming an aperture in a substrate, comprising: loading the substrate on a loading table in a reactor, the substrate having a silicon-containing film deposited thereon and a patterned mask layer deposited on the silicon-containing film; C 4 H 9 F 3 introducing an etching gas containing Si into the reactor; converting the etching gas into a plasma; and causing an etching reaction between the plasma and the silicon-containing film to proceed, thereby etching the silicon-containing film against the patterned mask layer to form the aperture.
18. 1. An etching method for forming an aperture in a substrate, comprising: loading the substrate on a loading table in a reactor, the substrate having a silicon-containing film deposited thereon and a patterned mask layer deposited on the silicon-containing film; CH 3 F 3 introducing an etching gas containing Si into the reactor; converting the etching gas into a plasma; and causing an etching reaction between the plasma and the silicon-containing film to proceed, thereby etching the silicon-containing film against the patterned mask layer to form the aperture.
19. 1. An etching method for forming an aperture in a substrate, comprising: loading the substrate on a loading table in a reactor, the substrate having a silicon-containing film deposited thereon and a patterned mask layer deposited on the silicon-containing film; C 2 H 6 F 2 introducing an etching gas containing Si into the reactor; converting the etching gas into a plasma; and causing an etching reaction between the plasma and the silicon-containing film to proceed, thereby etching the silicon-containing film against the patterned mask layer to form the aperture.
20. 1. An etching gas composition suitable for use in a semiconductor etching reaction, comprising: Formula C x H y F z S n An etching gas composition comprising a first etchant vapor that is a Si-containing hydrofluorocarbon selected from (1≦x≦6, 1≦y≦9, 1≦z≦15, n=1 or 2).
21. 21. The etching gas composition of claim 20, wherein the first etching gas comprises one or more methyl groups.
22. 21. The etching gas composition of claim 20, wherein the first etching gas comprises at least one methyl group bonded to a Si atom.
23. The first etching gas is a CH 4 F 2 Si, CH 3 F 3 Si, C 2 H 6 F 2 Si, C 3 H 9 FSi, C 4 H 9 F 3 Si, C 5 H 9 F 5 Si, C 4 H 10 F 4 S 2 , C 2 H 6 F 4 S 2 , C 3 H 9 F 3 S 2 , C 6 H 9 F 7 21. The etching gas composition of claim 20, wherein said first and second aryl groups are selected from the group consisting of aryl, aryloxy ...
24. 21. The etching gas composition of claim 20, further comprising a second etchant vapor selected from a hydrofluorocarbon or a fluorocarbon.
25. The hydrofluorocarbon or fluorocarbon is CF 4 , C 2 F 6 , C 3 F 6 , C 4 F 6 , C 4 F 8 , C 5 F 8 , C 5 F 10 , C 6 F 12 , C 7 F 14 , C 8 F 16 , C.H. 2 F 2 , C.H. 3 F, C.H.F. 3 , C 2 H 5 F.C. 3 H 7 F.C. 5 H.F. 7 , C 3 H 2 F 6 , C 3 H 4 F 2 , C 3 H 2 F 4 , C 4 H 2 F 6 Or C 4 H 3 F 7 25. The etching gas composition of claim 24, wherein said etching gas composition is selected from:
26. O 2 , O 3 , CO, CO 2 , SO, SO 2 ,FNO,NO,N 2 O, NO 2 , H 2 21. The etching gas composition of claim 20, further comprising an oxidizing gas selected from O or COS.
27. 21. The etching gas composition of claim 20, further comprising an inert gas selected from He, Ar, Xe, Kr, or Ne.
28. H 2 , S.F. 6 , N.F. 3 , N 2 , N.H. 3 , Cl 2 , BCl 3 , B.F. 3 , B 2 , F 2 21. The etching gas composition of claim 20, further comprising an additional gas selected from HBr, HCl, or combinations thereof.
29. The etching gas composition of any one of claims 20 to 28, wherein the purity of the first etching gas is greater than 95% v / v.
30. The etching gas composition of any one of claims 20 to 28, wherein the purity of the first etching gas is greater than 99.99% v / v.
31. The etching gas composition according to any one of claims 20 to 28, wherein the boiling point of the first etching gas is approximately -50 to 250°C.
32. Use of the etching gas composition according to any one of claims 20 to 28 in a semiconductor etching process.
Citation Information
Patent Citations
Method of manufacturing water-repelling film
US20050089647A1
Chemistries for etching multi-stacked layers
US20170365487A1
Plasma treatment apparatus and plasma treatment method
US6475918B1