Metal plate and deposition mask for OLED pixel deposition including the same

A metal plate with controlled residual stress and surface corrugation, made of iron and nickel, addresses warpage issues in deposition masks, enhancing deposition efficiency and uniformity by minimizing lifting and non-uniformity in OLED pixel deposition.

JP2024544275AInactive Publication Date: 2024-11-28LG INNOTEK CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024535555
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-14
Filing Date
2022-11-25
Publication Date
2024-11-28
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The warpage and surface corrugation of metal plates used in deposition masks for OLED pixel deposition, caused by uneven stress distribution during pretreatment processes, lead to decreased deposition efficiency and non-uniformity of organic material patterns.

Method used

A metal plate with controlled residual stress and surface waviness is developed, composed of iron and nickel, with specific etching patterns to minimize warpage and corrugation, ensuring the metal plate maintains a residual stress of 5 mm or less and surface corrugation of 25 ppm or less.

Benefits of technology

The controlled residual stress and surface waviness improve the deposition efficiency by preventing lifting between the deposition mask and substrate, ensuring uniform organic material deposition and reducing the need for additional flattening processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024544275000001_ABST
    Figure 2024544275000001_ABST
Patent Text Reader

Abstract

A metal plate used for manufacturing a deposition mask for OLED pixel deposition according to an embodiment has a first direction and a second direction crossing the first direction, the metal plate includes Invar containing iron and nickel, a first residual stress in the first direction and a second residual stress in the second direction are 5 mm or less, a ratio of the first residual stress to the second residual stress is 1:0.4 to 0.5, the first residual stress is a residual stress of an arbitrary first sample metal plate having a size of X mm x Y mm (horizontal x vertical) in which the first direction is a horizontal direction, and the second residual stress is , the residual stress of an arbitrary second sample metal plate having a size of Y mm x X mm (width x height) in which the second direction is the horizontal direction, where X is 200 mm to 220 mm and Y is 140 mm to 160 mm, and the residual stress is defined as the following mathematical formula 1 when the first sample metal plate and the second sample metal plate are etched so that the thickness of the region from one end in the long width direction to 5% to 10% of the long width direction length of each of them is 30% to 70% of the metal plate thickness, and the etched sample metal plate is placed on a horizontal table. [Number 1] Residual stress=H / L (H: maximum height (mm) that the etching area of ​​the sample metal plate rises above the top surface of the horizontal table
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The examples relate to deposition masks for metal plates and OLED pixel deposition. [Background technology]

[0002] Display devices are applied to a variety of devices. For example, display devices are applied to large devices such as televisions, monitors, and public displays (PDs) as well as small devices such as smartphones and tablet PCs. In particular, as the demand for ultra-high resolution UHD (Ultra High Definition) of 500 PPI (Pixel Per Inch) or more has increased recently, high-resolution display devices have been applied to small and large devices. As a result, there has been growing interest in technologies for achieving low power consumption and high resolution.

[0003] Generally used display devices can be largely classified into liquid crystal displays (LCDs) and organic light emitting diodes (OLEDs) according to driving methods.

[0004] An LCD is a display device that is driven using liquid crystal, and has a structure in which a light source, such as a cold cathode fluorescent lamp (CCFL) or a light emitting diode (LED), is arranged below the liquid crystal. The LCD is driven by adjusting the amount of light emitted from the light source using the liquid crystal arranged above the light source.

[0005] OLED is a display device that uses organic materials and does not require a separate light source, but can be driven with low power because the organic material itself acts as the light source. OLED can express infinite brightness and darkness, has a response speed about 1000 times faster than LCD, and has a superior viewing angle, so it is attracting attention as a display device that can replace LCD.

[0006] In particular, the organic material included in the light-emitting layer in an OLED may be deposited on a substrate using a deposition mask called a fine metal mask (FMM), and the deposited organic material may be formed in a pattern corresponding to the pattern formed on the deposition mask to function as a pixel. The deposition mask is generally manufactured using an Invar alloy metal plate containing iron (Fe) and nickel (Ni). At this time, through holes penetrating one side and the other side of the metal plate may be formed at positions corresponding to pixel patterns. Thus, organic materials such as red, green, and blue may be deposited on the substrate through the through holes of the metal plate, and a pixel pattern may be formed on the substrate.

[0007] Meanwhile, the Invar alloy metal plate used as the deposition mask may be subjected to a pretreatment process for modifying the thickness and surface of the metal plate, and then through holes may be formed in the metal plate.

[0008] At this time, the pretreatment process may change the stress distribution inside the metal sheet, which may cause the metal sheet to warp due to the uneven stress distribution inside the metal sheet, and may increase the waviness of the surface of the metal sheet.

[0009] Therefore, when the deposition masks are cut into unit sizes after the through holes are formed in the metal plate that has been subjected to the pretreatment process, the deposition masks may be warped due to such stress.

[0010] Therefore, when an organic material is deposited through a deposition mask, the deposition mask and the substrate on which the organic material is deposited may be lifted up, which may reduce deposition efficiency.

[0011] Therefore, a new deposition mask is required that can control the warping of the metal plate caused by the pretreatment process and the resulting surface corrugation. Summary of the Invention [Problem to be solved by the invention]

[0012] The embodiments are intended to provide a metal plate with reduced warping and surface waviness, and a deposition mask manufactured therefrom. [Means for solving the problem]

[0013] A metal plate used for manufacturing a deposition mask for OLED pixel deposition according to an embodiment has a first direction and a second direction crossing the first direction, the metal plate includes Invar containing iron and nickel, a first residual stress in the first direction and a second residual stress in the second direction are 5 mm or less, a ratio of the first residual stress to the second residual stress is 1:0.4 to 0.5, the first residual stress is a residual stress of an arbitrary first sample metal plate having a size of X mm x Y mm (horizontal x vertical) in which the first direction is a horizontal direction, and the second residual stress is , the residual stress of an arbitrary second sample metal plate having a size of Y mm x X mm (width x height) in which the second direction is the horizontal direction, where X is 200 mm to 220 mm and Y is 140 mm to 160 mm, and the residual stress is defined as the following mathematical formula 1 when the first sample metal plate and the second sample metal plate are etched so that the thickness of the region from one end in the long width direction to 5% to 10% of the long width direction length of each of them is 30% to 70% of the metal plate thickness, and the etched sample metal plate is placed on a horizontal table.

[0014] [Number 1]

[0015] Residual stress=H / L

[0016] (H: maximum height (mm) of the etching area of ​​the sample metal plate warped up from the upper surface of the horizontal table, L: length (mm) of the sample metal plate in the first direction in which the etching area is formed) Effect of the Invention

[0017] The metal plate according to the embodiment can improve the floating phenomenon between a deposition mask manufactured from the metal plate and a deposition substrate by controlling the residual stress and surface waviness of the metal plate remaining after a pretreatment process within a set range, and therefore, when an organic material is deposited on a deposition substrate through a deposition mask manufactured from the metal plate, deposition efficiency is improved. [Brief description of the drawings]

[0018] [Figure 1] FIG. 1 is a cross-sectional view showing an organic deposition apparatus to which a deposition mask according to an embodiment is applied. [Diagram 2] FIG. 2 is a cross-sectional view for explaining a contact relationship between an evaporation mask and an evaporation substrate in the embodiment. [Diagram 3] 1A to 1C are diagrams for explaining a pretreatment process of a metal plate for manufacturing an evaporation mask according to an embodiment. [Figure 4] 4A to 4C are diagrams for explaining a sample metal plate manufactured from the metal plate for manufacturing the deposition mask according to the embodiment. [Diagram 5] 4A to 4C are diagrams for explaining a sample metal plate manufactured from the metal plate for manufacturing the deposition mask according to the embodiment. [Figure 6] 1A to 1C are diagrams for explaining a method for measuring residual stress of a metal plate for manufacturing an evaporation mask according to an embodiment. [Figure 7] 1A to 1C are diagrams for explaining a method for measuring surface waviness of a metal plate for manufacturing an evaporation mask according to an embodiment. [Figure 8] FIG. 2 is a plan view of an evaporation mask according to an embodiment of the present invention. [Figure 9] FIG. 13 is a diagram for explaining T / P (Total Pitch) and straightness of the deposition mask according to the embodiment. MODE FOR CARRYING OUT THEINVENTION

[0019] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings. However, the technical idea of ​​the present invention is not limited to some of the embodiments described, and may be realized in various different forms, and one or more of the components of the embodiments may be selectively combined or substituted within the scope of the technical idea of ​​the present invention. In addition, terms (including technical and scientific terms) used in the embodiments of the present invention may be interpreted as meanings commonly understood by those having ordinary skill in the art to which the present invention belongs, unless otherwise clearly and specifically defined and described, and commonly used terms such as predefined terms may be interpreted in consideration of the contextual meaning of the related art.

[0020] In addition, the terms used in the examples of the present invention are intended to describe the examples and are not intended to limit the present invention. In the present specification, the singular form can include the plural form unless otherwise specified in the phrase, and when described as "A and (and) at least one (or more) of B and C", it can include one or more of all combinations that can be combined with A, B, and C.

[0021] In addition, in describing the components of the present invention, terms such as first, second, A, B, (a), (b), etc. are used. Such terms are merely used to distinguish the components from other components, and are not intended to limit the essence, order, or sequence of the components.

[0022] Furthermore, when a component is described as being "coupled," "coupled," or "connected" to another component, it includes not only cases where the component is directly coupled, coupled, or connected to the other component, but also cases where the component is "coupled," "coupled," or "connected" by another component between the component and the other component.

[0023] In addition, when it is described as being formed or disposed "on or under" each component, "on or under" includes not only the case where the two components are in direct contact with each other, but also the case where one or more other components are formed or disposed between the two components.

[0024] In addition, when it is expressed as "above" or "below," it can mean not only the upward direction but also the downward direction based on one component.

[0025] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, deposition masks according to embodiments will be described with reference to the drawings.

[0026] FIG. 1 is a diagram showing an organic deposition apparatus to which a deposition mask according to the embodiment is applied.

[0027] Referring to FIG. 1, the organic deposition apparatus 1000 includes a deposition mask 1100 , a mask frame 1200 , a deposition substrate 1300 , an organic deposition container 1400 , and a vacuum chamber 1500 .

[0028] The deposition mask 1100, the mask frame 1200, the deposition substrate 1300, and the organic material deposition container 1400 are housed in the vacuum chamber 1500. Thus, a deposition process through the deposition mask 1100 may be performed in a vacuum atmosphere.

[0029] The deposition substrate 1300 is a substrate used in manufacturing a display device. For example, the deposition substrate 1300 may be an organic deposition substrate on which an OLED pixel pattern is formed. On the deposition substrate 1300, red, green, and blue organic patterns are formed to form pixels that are the three primary colors of light. That is, an RGB pattern is formed on the deposition substrate 1300.

[0030] The deposition mask 1100 is disposed on one surface of the deposition substrate 1300. In particular, the deposition mask 1100 is disposed on a deposition surface on which an organic material is deposited, among both surfaces of the deposition substrate 1300. In addition, the deposition mask 1100 is fixed by the mask frame 1200.

[0031] As a result, the organic material passes through the through holes TH formed in the deposition mask 1100, and thus the organic material is deposited on the deposition surface of the deposition substrate 1300, thereby forming an RGB pattern on the deposition surface of the deposition substrate 1300.

[0032] The organic material deposition container 1400 may be a crucible. An organic material is placed inside the crucible. A heat source and / or an electric current is supplied to the crucible, which is the organic material deposition container 1400, in the vacuum chamber 1500. As a result, the organic material passes through the deposition mask 1100, and is deposited on the deposition surface of the deposition substrate 1300.

[0033] FIG. 2 is a diagram for explaining the positional relationship between the deposition mask 1100 and the deposition substrate 1300. As shown in FIG.

[0034] Referring to FIG. 2, the deposition mask 1100 is disposed on a deposition surface of the deposition substrate 1300. In particular, the deposition mask 1100 is disposed in direct or indirect contact with the deposition surface of the deposition substrate 1300.

[0035] The deposition mask 1100 is formed by forming a plurality of through holes TH in a metal plate 100 including iron and nickel. In particular, the deposition mask 1100 is formed by forming a plurality of through holes TH through an etching process in a metal plate 100 including an Invar alloy including iron and nickel.

[0036] In detail, the metal plate 100 includes a first surface 101 and a second surface 102 that are opposite to each other. A first surface hole V1 is formed in the first surface 101 of the metal plate 100, and a second surface hole V2 is formed in the second surface 102 of the metal plate 100. The size of the first surface hole V1 is smaller than the size of the second surface hole V2. That is, the diameter of the first surface hole V1 is smaller than the diameter of the second surface hole V2.

[0037] The second surface hole V2 is disposed opposite the organic material deposition container 1400. Thus, the deposition material from the organic material deposition container 1400 flows in. The first surface hole V1 is an area through which the deposition material flowing in from the second surface hole V2 passes. Thus, the organic material exiting from the first surface hole V1 is deposited on the deposition substrate 1300.

[0038] The first surface hole V1 and the second surface hole V2 are formed by partially penetrating the metal plate 100. For example, the depth of the first surface hole V1 is smaller than the depth of the second surface hole V2. Furthermore, the first surface hole V1 and the second surface hole V2 are arranged at positions overlapping each other in the thickness direction of the metal plate 100 and are formed to communicate with each other.

[0039] As a result, a plurality of through holes TH are formed in the metal plate 100, the through holes TH being formed by communicating the first surface holes V1 and the second surface holes V2.

[0040] The deposition mask 1100 is manufactured by cutting the metal plate 100 having a plurality of through holes TH into a set unit area size. For example, the deposition mask 1100 may be cut into a stick shape having a set unit area size.

[0041] The deposition mask 1100 is disposed such that a first surface hole V1 of the deposition mask 1100 contacts a deposition surface of the deposition substrate 1300.

[0042] Before forming the through holes TH, the metal plate 100 is subjected to a pretreatment process for reducing the thickness of the metal plate 100. The pretreatment process may change the distribution of internal stress, i.e., tensile stress and compressive stress, of the metal plate 100, and the metal plate may be warped due to the internal stress distribution. This may change the waviness of the surface of the metal plate, i.e., the surface waveform.

[0043] Such warping and increased surface corrugation of the metal plate 100 affect the straightness of the deposition mask 1100 manufactured using the metal plate 100 .

[0044] That is, when performing an etching process to form the through holes TH in the metal plate 100, a process of pulling the metal plate is performed to flatten the warped metal plate. At this time, the greater the warp of the metal plate, the greater the tensile force for pulling the metal plate. As a result, when forming the through holes in the metal plate 100 and cutting it to a set size to form a deposition mask, residual stress due to tension increases, which may increase the straightness of the deposition mask, i.e., warpage.

[0045] Therefore, when a deposition process is performed on a deposition substrate using the deposition mask, a gap g may be formed between the deposition mask and the deposition substrate, which reduces deposition efficiency of the deposition mask. In addition, since the thickness of the organic material through the deposition region of the deposition mask varies from region to region, there is a problem that the thickness of the organic material pattern deposited on the deposition substrate becomes non-uniform.

[0046] A metal plate that can solve the above problems and a deposition mask manufactured using the same will be described below.

[0047] FIG. 3 is a diagram for explaining a pretreatment step of a metal plate according to the embodiment.

[0048] Referring to FIG. 3, the metal plate 100 includes one surface 101 and another surface 102 opposite to the one surface 101 .

[0049] The metal plate 100 includes iron (Fe) and nickel (Ni). In particular, the metal plate 100 may include about 60% to about 65% by weight of iron and about 35% to about 40% by weight of nickel. In particular, the metal plate 100 may include about 63.5% to about 64.5% by weight of iron and about 35.5% to about 36.5% by weight of nickel. The metal plate 100 may further include about 1% by weight or less of at least one element selected from the group consisting of carbon (C), silicon (Si), sulfur (S), phosphorus (P), manganese (Mn), titanium (Ti), cobalt (Co), copper (Cu), silver (Ag), vanadium (V), niobium (Nb), indium (In), and antimony (Sb).

[0050] One surface 101 and the other surface 102 of the metal plate 100 are etched. In particular, both surfaces of the metal plate 100 are etched through a chemical polishing process using an etching solution capable of etching the metal plate 100. For example, the one surface 101 of the metal plate 100 is etched to a thickness t1 in the range of 20% to 30% of the total thickness T of the metal plate 100, and the other surface 102 of the metal plate 100 is etched to a thickness t2 in the range of 20% to 30% of the total thickness T of the metal plate 100.

[0051] Thus, the metal plate 100 includes a first surface 110 and a second surface 120 opposite to the first surface 110 through the pretreatment process. The thickness of the metal plate 100 is reduced through the pretreatment process. Specifically, the metal plate 100 has a thickness t3 of 5 μm to 30 μm after the pretreatment process. More specifically, the metal plate 100 has a thickness of 15 μm to 25 μm after the pretreatment process.

[0052] By pretreating the metal plate 100 through a chemical polishing process, it is possible to prevent an increase in warpage or surface waviness of the metal plate 100 that occurs during the pretreatment process.

[0053] That is, the internal stresses such as compressive stress and tensile stress contained in the raw material of the metal plate 100 are not changed by other forces, and the internal stresses are removed by the etching process, thereby minimizing the occurrence of residual stress inside the metal plate 100 after the pretreatment process.

[0054] As a result, residual stress inside the metal plate 100 after the pretreatment process can be minimized, and waviness on the surface of the metal plate 100 can be minimized.

[0055] Fig. 4 and Fig. 5 are diagrams for explaining a sample metal plate made from the metal plate according to the embodiment. Fig. 6 is a diagram for explaining a method for measuring the residual stress of the metal plate according to the embodiment. That is, Fig. 6 is a diagram for explaining a method for measuring the residual stress of the metal plate after the pretreatment process.

[0056] 4 and 5, the metal plate 100 may have a thickness of about 30 μm or less as a metal plate for manufacturing a deposition mask 100 to realize a high resolution of 400 PPI or more. In particular, the metal plate 100 may have a thickness of 5 μm to 30 μm through the above-mentioned pretreatment process. More particularly, the metal plate 100 may have a thickness of 15 μm to 25 μm through the above-mentioned pretreatment process.

[0057] In order to measure the residual stress of the metal plate 100, a sample metal plate 150 of a set size is separated from the metal plate 100. The sample metal plate 150 is a sample taken at an arbitrary point of the metal plate 100. In this case, the sample metal plate 150 may be at least one sample taken at an arbitrary point of the metal plate 100, and the residual stress is measured using the at least one sample.

[0058] In detail, a strip-shaped sample metal plate whose width is greater than its length is extracted at any point on the metal plate 100. In detail, a first sample metal plate extracted so that its long width direction is in a first direction as shown in Fig. 4 and a second sample metal plate extracted so that its long width direction is in a second direction as shown in Fig. 5 are extracted.

[0059] The sample metal plate 150 has a set size. In detail, the first sample metal plate has a length in a first direction of X mm and a length in a second direction of Y mm. The second sample metal plate has a length in a first direction of about Y mm and a length in a second direction of about X mm.

[0060] In this case, the X is 200 mm to 220 mm, and the Y is 140 mm to 160 mm.

[0061] For example, the first sample metal plate may be a sample having a size of 210 mm×150 mm (width×length), and the second sample metal plate may be a sample having a size of 150 mm×210 mm (width×length).

[0062] Next, the sample metal plate 150 is etched. In particular, one surface of the sample metal plate 150 is partially etched. For example, one surface of each of the first sample metal plate and the second sample metal plate is partially etched.

[0063] Specifically, the sample metal plate 150 is partially etched such that a region from one end in the long width direction of the sample metal plate 150 to 5% to 10% of the long width direction length is left, and a region beyond 5% to 10% of the long width direction length is partially etched. Specifically, the sample metal plate 150 can be partially etched such that a thickness of a region beyond 5% to 10% of the long width direction length of the sample metal plate 150 is about 30% to about 70% of the thickness of the sample metal plate 150. More specifically, the sample metal plate 150 can be partially etched such that a thickness of a region beyond 5% to 10% of the long width direction size of the sample metal plate 150 is 50% of the thickness of the sample metal plate 150.

[0064] Next, the residual stress of the metal plate 100 is measured using the sample metal plate 150. Referring to Fig. 6, in order to measure the residual stress of the sample metal plate 150, the sample metal plate 150 is placed on a horizontal table 200. In particular, the first and second sample metal plates on which the partial etching has been performed are placed on the horizontal table.

[0065] The sample metal plate 150 includes one side and another side. In particular, the sample metal plate 150 includes one side that is partially etched and another side that is not partially etched. The sample metal plate 150 is disposed such that the other side of the sample metal plate 150 faces the upper surface of the horizontal table 200.

[0066] Next, a first residual stress and a second residual stress are measured, the first residual stress being the residual stress of the first sample metal plate, and the second residual stress being the residual stress of the second sample metal plate.

[0067] In detail, the first residual stress is the residual stress of the first sample metal plate in which the first direction is the long width direction, and the second residual stress is the residual stress of the first sample metal plate in which the second direction is the long width direction.

[0068] The sample metal plate 150 placed on the horizontal platform may be warped in one direction due to the internal stress of the metal plate itself and the internal stress that changes due to the pre-treatment process. In particular, at least one end of the etched region of the sample metal plate 150 may be warped in a direction away from the upper surface of the horizontal platform 200. More particularly, at least one end of one surface of the half-etched sample metal plate 150 may be warped toward the center of the sample metal plate 150, moving away from the upper surface of the horizontal platform 200. That is, one end of the sample metal plate 150 may be warped in a direction away from the horizontal platform due to the internal stress, and the one end may be warped in a roll shape depending on the magnitude of the internal stress.

[0069] That is, the residual stress of the metal plate 100 is calculated by measuring the height at which the partially etched region of the sample metal plate 150 is spaced from the upper surface of the horizontal table.

[0070] Specifically, the residual stress of the metal plate 100 is defined as the maximum height of the etched area of ​​the sample metal plate warped up from the upper surface of the horizontal table. Specifically, the residual stress of the metal plate 100 can be defined as the following Equation 1.

[0071] [Number 1]

[0072] Residual stress=H / L

[0073] (H: maximum height of the etching area of ​​the sample metal plate from the upper surface of the horizontal table, L: length of the sample metal plate in the first direction in which the etching area is formed)

[0074] According to Equation 1, when the length of the first sample metal plate in the first direction is X mm and the length of the second direction is Y mm, and the length of the second sample metal plate in the first direction is about Y mm and the length of the second direction is about X mm, the metal plate 100 has a first residual stress of H / X in the first direction and a second residual stress of H / Y in the second direction.

[0075] For example, when the first sample metal plate is a sample having a size of 210 mm x 150 mm (width x height) and the second sample metal plate is a sample having a size of 150 mm x 210 mm (width x height), the metal plate 100 has a first residual stress of H / 210 in a first direction and a second residual stress of H / 150 in a second direction.

[0076] The residual stress of the metal plate 100 is calculated using a plurality of sample metal plates 150. For example, the first residual stress of the first sample metal plate is a value derived from an average value obtained by measuring a plurality of first sample metal plates using the above-mentioned method. Also, the second residual stress of the second sample metal plate is a value derived from an average value obtained by measuring a plurality of second sample metal plates using the above-mentioned method. In other words, the residual stress is an average residual stress.

[0077] The method measures a first residual stress in a first direction and a second residual stress in the second direction of the metal plate 100. In particular, the first residual stress is measured through the first sample metal plate, and the second residual stress is measured through the second sample metal plate.

[0078] The magnitude of the first residual stress and the magnitude of the second residual stress have a set magnitude.

[0079] The first residual stress and the second residual stress may be 10 mm or less. In particular, the first residual stress and the second residual stress may be 7 mm or less. More particularly, the first residual stress and the second residual stress may be 5 mm or less. More particularly, the first residual stress and the second residual stress may be 1 mm to 5 mm.

[0080] When the magnitude of the first residual stress and the second residual stress exceeds 10 mm, the residual stress inside the metal plate may increase the surface waviness of the metal plate, and when a deposition mask is manufactured using the metal plate, the straightness characteristic of the manufactured deposition mask may be degraded.

[0081] Furthermore, the magnitude of the first residual stress is different from the magnitude of the second residual stress. More specifically, the magnitude of the first residual stress is greater than the magnitude of the second residual stress. For example, the ratio of the magnitude of the first residual stress to the magnitude of the second residual stress may be 1:(0.2 to 0.7). More specifically, the ratio of the magnitude of the first residual stress to the magnitude of the second residual stress may be 1:(0.3 to 0.6). More specifically, the ratio of the magnitude of the first residual stress to the magnitude of the second residual stress may be 1:(0.4 to 0.5).

[0082] For example, the magnitude of the first residual stress may be 1 mm to 10 mm. In particular, the magnitude of the first residual stress may be 1.5 mm to 7.5 mm. More particularly, the magnitude of the first residual stress may be 2 mm to 5 mm.

[0083] Furthermore, the magnitude of the second residual stress may be 0.5 mm to 8 mm. More specifically, the magnitude of the second residual stress may be 0.5 mm to 5 mm. More specifically, the magnitude of the second residual stress may be 1 mm to 3 mm.

[0084] The metal plate according to the embodiment can reduce warpage of a deposition mask manufactured using the metal plate by controlling the residual stress of the metal plate remaining after the pretreatment process within the above range, thereby improving deposition efficiency when depositing an organic material on a deposition substrate through a deposition mask manufactured using the metal plate.

[0085] Meanwhile, the metal sheet according to the embodiment has a surface waviness in a set size range. That is, the metal sheet according to the embodiment has a residual stress in a set size range. Or, the metal sheet according to the embodiment has a surface waviness in a set size range. Or, the metal sheet according to the embodiment has a residual stress and a surface waviness in a set size range.

[0086] FIG. 7 is a diagram for explaining a method for measuring the surface corrugation of a metal plate according to an embodiment.

[0087] 7, the surface corrugation of the metal plate is measured by measuring the flatness of the metal plate using a non-contact three-dimensional measuring device. That is, a plurality of coordinates are set at equal intervals on the metal plate, and the flatness is converted into a length size to measure the surface corrugation.

[0088] 7, in order to measure the surface corrugation of the metal plate 100, a sample metal plate 150 of a set size is separated from the metal plate 100. The sample metal plate 150 is a sample taken at an arbitrary point of the metal plate 100. In this case, the sample metal plate 150 may be at least one sample taken at an arbitrary point of the metal plate 100, and the surface corrugation is measured using the at least one sample.

[0089] In detail, a strip-shaped sample metal plate having a width greater than a length is extracted at an arbitrary point of the metal plate 100. In detail, a third sample metal plate is extracted such that the long width direction is in the first direction as shown in FIG.

[0090] The sample metal plate 150 has a set size. In detail, the length in the first direction of the third sample metal plate is A mm, and the length in the second direction is B mm, where A is 490 mm to 510 mm, and B is 160 mm to 180 mm.

[0091] For example, the third sample metal plate may be a sample having a size of 500 mm×170 mm (width×length).

[0092] A plurality of coordinates are set on the third sample metal plate, that is, a first coordinate (C1), a second coordinate (C2), a third coordinate (C3), and a fourth coordinate (C4) are set on the third sample metal plate.

[0093] In addition, a plurality of coordinates spaced apart at equal intervals are set within an imaginary quadrangle formed by connecting the first coordinate (C1), the second coordinate (C2), the third coordinate (C3), and the fourth coordinate (C4).

[0094] The surface corrugation of the metal plate 100 may be measured based on a ratio of a curve distance to a straight line distance of a coordinate. In particular, the first surface corrugation in the first direction and the second surface corrugation in the second direction are defined by the following Equation 2.

[0095] [Number 2]

[0096] Surface waveform (ppm)=10 6 *(L-L0) / L0

[0097] (L means the curved distance of the coordinate, and L0 means the straight line distance of the coordinate.)

[0098] The surface waviness in the first direction of the metal plate 100 is calculated as the average value of the surface waviness of a first virtual line VL1 in the first direction passing through the coordinates, and the surface waviness in the second direction is calculated as the average value of the surface waviness of a second virtual line VL2 in the second direction passing through the coordinates.

[0099] By this method, a first surface corrugation in a first direction and a second surface corrugation in the second direction of the metal plate 100 are measured.

[0100] The magnitude of the first surface corrugation and the magnitude of the second surface corrugation have set magnitudes.

[0101] The first surface corrugation and the second surface corrugation may be 25 ppm or less. In particular, the first surface corrugation and the second surface corrugation may be 20 ppm or less. More particularly, the first surface corrugation and the second surface corrugation may be 5 ppm to 25 ppm.

[0102] When the magnitude of the first surface corrugation and the second surface corrugation exceeds 25 ppm, the flatness of the surface of the metal plate is reduced, and thus, when an organic material is deposited on a deposition substrate using a deposition mask manufactured using the metal plate, the floating between the deposition mask and the deposition substrate becomes large, and deposition efficiency may be reduced.

[0103] Furthermore, the magnitude of the first surface corrugation is different from the magnitude of the second surface corrugation. More specifically, the magnitude of the first surface corrugation is greater than the magnitude of the second surface corrugation. For example, the ratio of the magnitude of the first surface corrugation to the magnitude of the second surface corrugation may be 1:(0.15 to 0.7). More specifically, the ratio of the magnitude of the first surface corrugation to the magnitude of the second surface corrugation may be 1:(0.2 to 0.6). More specifically, the ratio of the magnitude of the first surface corrugation to the magnitude of the second surface corrugation may be 1:(0.25 to 0.5).

[0104] For example, the magnitude of the first surface corrugation may be 8 ppm to 25 ppm. More specifically, the magnitude of the first surface corrugation may be 10 ppm to 20 ppm. More specifically, the magnitude of the first surface corrugation may be 12 ppm to 18 ppm.

[0105] The magnitude of the second surface corrugation may be 3 ppm to 25 ppm. More specifically, the magnitude of the second surface corrugation may be 5 ppm to 15 ppm. More specifically, the magnitude of the second surface corrugation may be 7 ppm to 10 ppm.

[0106] The metal plate according to the embodiment can improve the floating phenomenon between a deposition mask manufactured from the metal plate and a deposition substrate by controlling the surface corrugation of the metal plate remaining after the pretreatment process within the above range, and therefore has improved deposition efficiency when depositing an organic material on a deposition substrate through a deposition mask manufactured from the metal plate.

[0107] Hereinafter, with reference to FIG. 8, a deposition mask to which the above-described pretreated metal plate is applied will be described.

[0108] FIG. 8 is a plan view of an evaporation mask according to an embodiment.

[0109] Referring to FIG. 8, a deposition mask 1100 according to the embodiment includes a deposition area DA and the non-deposition area NDA.

[0110] The deposition area DA is an area for forming a deposition pattern, that is, a deposition material is deposited on a deposition substrate through the deposition mask in the deposition area DA.

[0111] The deposition mask 1100 includes a plurality of deposition areas DA. For example, the deposition areas DA include an effective portion and a non-effective portion. In detail, the deposition areas DA include a plurality of effective portions in which a plurality of through holes are formed to form a deposition pattern, and a non-effective portion UA ​​in which no through holes are formed. The above-mentioned plurality of through holes TH are formed in the effective portion.

[0112] The plurality of effective portions may include a first effective portion AA1, a second effective portion AA2, and a third effective portion AA3, and are separated from each other by isolation regions IA1 and IA2.

[0113] In the case of a small display device such as a smartphone, any one of the effective portions of the multiple deposition regions included in the deposition mask 1100 may be for forming one display device. Alternatively, in the case of a large display device such as a television, multiple effective portions included in one deposition mask 1100 may be a part for forming one display device. As a result, one deposition mask 1100 may include multiple effective portions, so that multiple display devices can be formed simultaneously. Therefore, the deposition mask 1100 according to the embodiment may improve process efficiency.

[0114] The non-deposition areas NDA are disposed on both sides of the deposition area DA in the longitudinal direction, that is, on the outer side of the deposition area DA in the longitudinal direction.

[0115] The non-deposition area NDA is an area that is not involved in deposition. The non-deposition area NDA includes frame fixing areas FA1 and FA2 for fixing the deposition mask 1100 to a mask frame 1200. The non-deposition area NDA also includes half-etched portions HF1 and HF2, open portions OA1 and OA2, and protruding portions PA1 and PA2.

[0116] The deposition mask 1100 according to the embodiment is manufactured using the above-described metal plate 100. As a result, the metal plate for manufacturing the deposition mask has low residual stress and surface waviness, and therefore, the straightness and total pitch (T / P) characteristics of the manufactured deposition mask are both improved.

[0117] FIG. 9 is a diagram for explaining the straightness and total pitch T / P (Total Pitch) of the deposition mask 1100 according to the embodiment.

[0118] 9, the deposition mask 1100 is shown before and after warping. The straightness and total pitch of the deposition mask 1100 are calculated as a position difference between the deposition mask 1100 before and after warping.

[0119] Specifically, the straightness of the deposition mask 1100 is measured as the degree of warping of the deposition mask. Specifically, the straightness of the deposition mask 1100 is measured as the degree of warping of the deposition mask after warping, when the degree of warping of the deposition mask before warping is set to zero. More specifically, the straightness of the deposition mask 1100 is measured as the maximum degree of warping of the deposition mask after warping, when the degree of warping of the deposition mask before warping is set to zero.

[0120] The deposition mask 1100 manufactured using the metal plate 100 may have a straightness size of less than 50 μm. That is, the maximum warpage size of the deposition mask 1100 may be less than 50 μm. In particular, the deposition mask 1100 manufactured using the metal plate 100 may have a straightness size of 40 μm or less. More specifically, the deposition mask 1100 manufactured using the metal plate 100 may have a straightness of 15 μm to 40 μm. More specifically, the deposition mask 1100 manufactured using the metal plate 100 may have a straightness of 25 μm to 35 μm.

[0121] In addition, the total pitch of the deposition mask 1100 is measured as a difference in length between the upper surface and the lower surface in the long axis direction or a difference in length between the upper surface and the lower surface in the short axis direction.

[0122] The deposition mask 1100 manufactured using the metal plate 100 may have a total pitch size of less than 30 μm. In particular, the deposition mask 1100 manufactured using the metal plate 100 may have a total pitch size of 20 μm or less. More particularly, the deposition mask 1100 manufactured using the metal plate 100 may have a total pitch of 15 μm to 25 μm.

[0123] The deposition mask according to the embodiment is manufactured from a metal plate with reduced residual stress and surface waviness. This can improve the straightness and total pitch characteristics of the deposition mask manufactured from the metal plate. In particular, the straightness size and total pitch size of the deposition mask can be reduced.

[0124] As a result, in the deposition mask according to the embodiment, warping of the deposition mask is reduced, and thus it is possible to minimize lifting of the deposition region of the deposition mask and the deposition substrate when the deposition mask and the deposition substrate come into contact with each other.

[0125] Accordingly, the deposition mask according to the embodiment can minimize the gap between the deposition mask and the deposition substrate, thereby minimizing non-uniformity in the deposition thickness and improving deposition efficiency.

[0126] In addition, after forming the deposition mask, a separate tensioning process for reducing the surface corrugation of the deposition mask can be omitted.

[0127] The features, structures, effects, etc. described in the above-mentioned embodiments are included in at least one embodiment of the present invention, and are not necessarily limited to only one embodiment. Furthermore, the features, structures, effects, etc. exemplified in each embodiment can be combined or modified in other embodiments by a person having ordinary skill in the art to which the embodiment belongs. Therefore, the contents related to such combinations and modifications should be interpreted as being included in the scope of the present invention.

[0128] In addition, although the above description has focused on the embodiments, these are merely illustrative and do not limit the present invention, and a person having ordinary skill in the art to which the present invention pertains will understand that various modifications and applications not exemplified above are possible within the scope of the essential characteristics of the present embodiments. For example, each component specifically illustrated in the embodiments can be modified and implemented. Differences related to such modifications and applications should be interpreted as being included in the scope of the present invention as defined in the appended claims.

Claims

1. A metal plate having a first direction and a second direction intersecting the first direction defined therein, The metal plate includes Invar containing iron and nickel, The first residual stress in the first direction and the second residual stress in the second direction are 5 mm or less; a ratio of the first residual stress to the second residual stress is 1:0.4 to 0.5; The first residual stress is a residual stress of an arbitrary first sample metal plate having a size of X mm x Y mm (horizontal x vertical) in which the first direction is a horizontal direction, The second residual stress is a residual stress of an arbitrary second sample metal plate having a size of Y mm x X mm (horizontal x vertical) in which the second direction is a horizontal direction, The X is 200 mm to 220 mm, and the Y is 140 mm to 160 mm, The residual stress is defined as the following Equation 1 when the thickness of a region of each of the first sample metal plate and the second sample metal plate that is 5% to 10% of the length in the long width direction from one end of the long width direction is 30% to 70% of the metal plate thickness, and the etched sample metal plate is placed on a horizontal table. [Equation 1] Residual stress = H / L (H: maximum height (mm) of the etching region of the sample metal plate warped up from the upper surface of the horizontal table, L: length (mm) of the sample metal plate in the first direction in which the etching region is formed)

2. 2. The metal plate according to claim 1, wherein a ratio of the first residual stress to the second residual stress is 1:0.3 to 0.

6.

3. 2. The metal plate according to claim 1, wherein a ratio of the first residual stress to the second residual stress is 1:0.4 to 0.

5.

4. The first residual stress is measured as an average value of a plurality of first sample metal plates; The metal plate used for manufacturing an evaporation mask for OLED pixel deposition according to claim 1 , wherein the second residual stress is measured as an average value of a plurality of second sample metal plates.

5. the first surface waviness in the first direction and the second surface waviness in the second direction are 20 ppm or less; The ratio of the first surface corrugation to the second surface corrugation is 1:0.15 to 1:0.7; The first surface corrugation is a surface corrugation in the first direction of an arbitrary third sample metal plate having a size of 500 mm x 170 mm (width x length), in which the first direction is a horizontal direction; The second surface corrugation is a surface corrugation in the second direction of the third sample metal plate, The third sample metal plate is provided with a virtual rectangle formed by a first coordinate (C1), a second coordinate (C2), a third coordinate (C3), and a fourth coordinate (C4), and a plurality of coordinates equally spaced apart within the virtual rectangle; A plurality of first virtual lines in the first direction and a plurality of second virtual lines in the second direction passing through the coordinates are set on the third sample metal plate, 2 . The metal plate according to claim 1 , wherein the first surface corrugation and the second surface corrugation are defined by Equation 2 below: [Equation 2] Surface waveform (ppm) = 106*(L-L0) / L0 (L means the curved distance of the coordinates, and L0 means the straight line distance of the coordinates.

6. 6. The metal plate according to claim 5, wherein a ratio of the first surface corrugation to the second surface corrugation is 1:0.2 to 0.

6.

7. 6. The metal plate according to claim 5, wherein a ratio of the first surface corrugation to the second surface corrugation is 1:0.25 to 0.

5.

8. The first surface waveform is calculated as an average value of the surface waveform of the first virtual line passing through the coordinates; 6. The metal plate used for manufacturing an evaporation mask for OLED pixel deposition according to claim 5, wherein the second surface corrugation is calculated as an average value of the surface corrugation of the second imaginary line passing through the coordinate.

9. 2. The metal plate used for manufacturing a deposition mask for OLED pixel deposition according to claim 1, wherein the metal plate has a thickness of 15 μm to 25 μm.

10. The first residual stress is between 2 mm and 5 mm; 2. The metal plate according to claim 1, wherein the second residual stress is in the range of 1 mm to 3 mm.

11. the first surface corrugation is between 10 ppm and 20 ppm; 3. The metal plate according to claim 2, wherein the second surface corrugation is from 5 ppm to 15 ppm.

12. The metal plate according to any one of claims 1 and 2, The metal plate is a through hole including a first surface hole on the first surface of the metal plate and a large surface hole on the second surface; a width of the first surface hole is smaller than a width of the second surface hole.

13. The deposition mask has a straightness of 25 μm to 35 μm, The deposition mask according to claim 12 , wherein the straightness is defined as a maximum degree of warping of the deposition mask after warping, when a degree of warping of the deposition mask before warping is set to zero.

14. the deposition mask has a total pitch of 15 μm to 25 μm; The deposition mask of claim 12 , wherein the total pitch is defined as a difference in length between an upper surface and a lower surface in a major axis or a minor axis direction of the deposition mask.

Citation Information

Patent Citations

  • Method for manufacturing metal plate

    JP2021059781A

  • Method for manufacturing deposition mask, method for manufacturing display device, and deposition mask intermediate