Metal structure used in combination with gallium-based liquid metal, and its manufacturing method and use

A high phosphorus nickel alloy layer on metal structures prevents reactions with gallium-based liquid metals, ensuring stable thermal performance by avoiding consumption and maintaining interface integrity.

JP2024545536AInactive Publication Date: 2024-12-09YUNNAN ZHONGXUAN LIQUID METAL TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024539880
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-05-13
Filing Date
2022-08-29
Publication Date
2024-12-09
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Gallium-based liquid metals react with materials like copper and aluminum, forming intermetallic compounds and leading to consumption, which deteriorates thermal performance in heat sinks and other electronic devices.

Method used

A high phosphorus nickel alloy layer is formed on the surface of metal structures to prevent reactions with gallium-based liquid metals, ensuring long-term stability and thermal conductivity.

Benefits of technology

The high phosphorus nickel alloy layer effectively prevents the consumption of gallium-based liquid metals, maintaining thermal performance and integrity of the interface over time, even under extreme conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024545536000001_ABST
    Figure 2024545536000001_ABST
Patent Text Reader

Abstract

The present invention discloses a metal structure for use in combination with a gallium-based liquid metal, the metal structure having a high phosphorus nickel alloy layer on the surface in contact with the gallium-based liquid metal. When the metal structure contacts the gallium-based liquid metal, the metal structure does not react with the gallium-based liquid metal, so that the deterioration of heat dissipation performance caused by the consumption of the gallium-based liquid metal is avoided. The present invention further discloses a method for manufacturing the metal structure and its application in heat dissipation of computer chips, mobile phone chips, communication products, high power LEDs, insulated gate bipolar transistors, and high power electronic products.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] [CROSS REFERENCE TO RELATED APPLICATIONS] This application claims priority to the Chinese patent application filed with the China Patent Office on May 13, 2022, bearing application number 202210524894.9 and titled "Metal structure used in combination with gallium-based liquid metal, and its manufacturing method and use", and the Chinese patent application bearing application number 202221152744.1 and titled "Metal structure used in combination with gallium-based liquid metal", the entire contents of which are incorporated herein by reference. The present invention relates to the field of heat transfer in electronic devices, and in particular to a metal structure for use in combination with a gallium-based liquid metal, and to a method for producing the same and its use. [Background technology]

[0002] There are fine uneven gaps between the surface of the electronic material and the heat sink, and when they are directly attached, the actual contact area of ​​these is only 10% of the base area of ​​the heat sink, and the rest is all air gaps. Because the thermal conductivity of air is only 0.024w / (mk), the contact thermal resistance between the electronic device and the heat sink becomes very large, which significantly hinders the conduction of heat and causes the performance of the heat sink to deteriorate. Therefore, we need a thermal interface material with high thermal conductivity to fill these gaps, remove the air in them, and create a heat conduction path between the electronic device and the heat sink, thereby greatly increasing the contact area between the heat source and the heat sink, reducing the contact thermal resistance, and allowing the heat sink to play its role well.

[0003] Thermally conductive silicone grease is a traditional thermal interface material that is widely used at present. However, with the development of emerging fields such as 5G communication, Internet of Things, new energy automotive electronics, wearable devices, and smart cities, the related electronic devices are developing toward miniaturization, high power density, multi-functionality, etc., which continues to increase the risk of overheating of related electronic devices, and traditional silicone grease has low thermal conductivity and cannot meet the demand for use. The development of high-performance thermal interface materials is very important in terms of improving the heat dissipation of electronic devices, and has become the biggest challenge faced by academia and the application industry of electronic devices. Gallium-based liquid metal thermal interface materials have high thermal conductivity, which can meet the modern high power density application field, and have attracted more and more attention in recent years.

[0004] However, gallium-based liquid metal can react with aluminum or its alloy, and therefore also forms intermetallic compounds with copper or its alloy, but most of the materials of heat sinks are copper, aluminum or its alloy. In this case, the interface will eventually dry out due to the reaction consumption of liquid gallium, and the filling effect will be ineffective. Therefore, avoiding the reaction between gallium-based liquid metal and copper, aluminum or its alloy is an issue that must be solved immediately if liquid metal is to be widely used as a thermal interface material.

[0005] The information disclosed in this Background is intended only to enhance the understanding of the general context of the present invention and should not be construed as an admission or in any manner suggesting that this information constitutes prior art well known to those skilled in the art. Summary of the Invention [Problem to be solved by the invention]

[0006] The objective of the present invention is to provide a metal structure for use in combination with a gallium-based liquid metal, which does not react with the gallium-based liquid metal when it comes into contact with the gallium-based liquid metal, thereby avoiding the deterioration of heat dissipation performance caused by the consumption of the gallium-based liquid metal, and solving the technical problem in the prior art that the gallium-based liquid metal reacts with aluminum or its alloy in the heat sink material, causing the liquid phase gallium to react and be consumed, eventually drying up the interface and losing the filling effect. [Means for solving the problem]

[0007] To achieve the above object, the present invention provides a metal structure for use in combination with a gallium-based liquid metal, the metal structure having a high phosphorus nickel alloy layer on a surface in contact with the gallium-based liquid metal.

[0008] In one embodiment of the present invention, the phosphorus content in the high phosphorus nickel alloy layer is ≧10%.

[0009] In one embodiment of the present invention, the thickness of the high phosphorus nickel alloy layer is ≧1 μm, preferably, the thickness of the high phosphorus nickel alloy layer is ≧3 μm, more preferably, the thickness of the high phosphorus nickel alloy layer is ≧5 μm, and most preferably, the thickness of the high phosphorus nickel alloy layer is ≧10 μm.

[0010] In one embodiment of the present invention, the metal structure is a heat dissipation assembly in contact with a gallium-based liquid metal, a container or cavity for containing a gallium-based liquid metal, or a gallium-based liquid metal flow pipe, and preferably the metal structure is a fin heat sink, a heat pipe heat sink, a phase change heat sink, a heat sink, a vapor chamber, a microchannel heat sink, a liquid metal fluid heat sink, a liquid metal pressure sensor, a liquid metal pressure transmitter, a liquid metal containing container, or a part thereof in contact with a gallium-based liquid metal.

[0011] In one embodiment of the present invention, the surface of the metal structure that is in contact with the gallium-based liquid metal is flat or curved.

[0012] In one embodiment of the present invention, the material of the metal structure is at least one selected from copper, aluminum, iron, nickel, stainless steel, titanium, zinc, gold, or an alloy thereof.

[0013] In one embodiment of the invention, the metal structure further comprises a composite ceramic protective layer on the surface in contact with the gallium-based liquid metal.

[0014] In one embodiment of the invention, the gallium-based liquid metal is selected from gallium metal, gallium-containing liquid alloys, gallium-containing metal oxides, gallium-containing thermal interface materials, and gallium-containing composite materials.

[0015] Another object of the present invention is to provide a method for manufacturing the above-mentioned metal structure, which is to carry out high phosphorus chemical nickel plating treatment on the surface of the metal structure that contacts with the gallium-based liquid metal thermal interface material, thereby forming a high phosphorus nickel alloy layer on the surface of the metal structure that contacts with the gallium-based liquid metal, the technology of which is mature and stable, and the cost is low.

[0016] Another object of the present invention is to provide a method for the application of the above-mentioned metal structure or the metal structure manufactured by the above-mentioned manufacturing method to heat dissipation in computer chips, mobile phone chips, communication products, high power LEDs, insulated gate bipolar transistors, high power electronic products, etc. The present invention forms a high phosphorus nickel alloy layer on the surface of the metal structure that contacts with the gallium-based liquid metal, thereby preventing the alloying reaction between the gallium-based liquid metal and the metal structure, thereby making it possible to use the high thermal conductivity gallium-based liquid metal in products such as computer chips, mobile phone chips, communication products, high power LEDs, insulated gate bipolar transistors, and high power electronic products for aviation or military use. Effect of the Invention

[0017] Compared with the prior art, the present invention has the following beneficial effects:

[0018] (1) In the present invention, a high phosphorus nickel alloy layer is formed on the surface of the metal structure, which provides effective protection against metals such as copper and aluminum, and does not react with gallium-based liquid metal for a long time under extreme conditions. Experimental results show that a high phosphorus nickel plating layer of 1 μm or more can prevent the reaction between the metal sheet and the gallium-based liquid metal, thereby avoiding the gradual consumption of the gallium-based liquid metal due to the reaction, and avoiding the deterioration of the thermal conductivity performance caused by the consumption of the gallium-based liquid metal thermal interface material.

[0019] (2) Although a high phosphorus nickel plating layer of 1 μm or more has a good protective effect on a metal structure, for metal structures such as heat sinks and vapor chambers where the high phosphorus nickel plating layer is exposed on the surface, the high phosphorus nickel plating layer may be worn or damaged during packaging, transportation and use, so the thickness of the high phosphorus nickel plating layer is preferably 3 μm or more, more preferably 5 μm or more. In cases where there is severe wear or special requirements such as high requirements for stability and long usage cycles, a high phosphorus nickel plating layer of 10 μm or more can be formed on the surface of the metal structure to ensure sufficient protective effect to avoid unexpected situations.

[0020] (3) Furthermore, the phosphorus content in the high phosphorus nickel alloy layer is also extremely important. In Comparative Example 2, protection was provided with medium phosphorus nickel plating with a phosphorus content of 9%. Experimental results showed that although covering with the medium phosphorus nickel plating layer provided a certain degree of protection in preventing the reaction between the metal sheet and the gallium-based liquid metal, the protective effect was not sufficient, and it was discovered that the gallium-based liquid metal ultimately reacted with the metal sheet. [Brief description of the drawings]

[0021] [Figure 1] 1 is a cross-sectional schematic diagram of a fin heat sink according to one embodiment of the present invention; [Diagram 2] 2 is a cross-sectional schematic diagram of a heat pipe of a heat pipe radiator according to one embodiment of the present invention; [Diagram 3] 1 is a cross-sectional schematic view of a liquid metal containment vessel according to one embodiment of the present invention; [Figure 4] 1 is a photograph of metal sheets treated according to the methods of Example 3 of the present invention and Comparative Examples 1 to 5 after testing the protective effect of the plating layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, specific embodiments of the present invention will be described in detail with reference to the accompanying drawings in the specification, but it should be understood that the protection scope of the present invention is not limited to the specific embodiments.

[0023] Unless otherwise expressly stated, throughout the specification and claims, the term "comprises" or variations thereof, such as "containing" or "comprising," is to be understood to include stated elements or components and not to exclude other elements or components.

[0024] Example 1 What is shown in Figure 1 is a metal structure 1, specifically a copper fin heat sink, which has a high phosphorus nickel alloy layer 2 on its bottom surface that comes into contact with a gallium-based liquid metal 3. The manufacturing method was to thoroughly clean the bottom surface of the copper fin heat sink that comes into contact with the gallium-based liquid metal, perform a high phosphorus chemical nickel plating process for 5 minutes, and then remove and dry it.

[0025] According to the measurement results, the thickness of the high phosphorus nickel alloy layer formed on the bottom surface of the copper fin heat sink was 1.2 μm, and the phosphorus content in the high phosphorus nickel alloy layer was 10%. In order to facilitate subsequent experiments, a 2 mm copper sheet was simultaneously used to perform high phosphorus chemical nickel plating treatment, and then the treated copper sheet was used as the test subject of Example 1 instead of the copper fin heat sink.

[0026] Example 2 What is shown in Figure 2 is a metal structure 1, specifically, a heat pipe of a copper heat pipe radiator, which has a high phosphorus nickel alloy layer 2 on its inner surface that comes into contact with a gallium-based liquid metal 3. The manufacturing method of this metal structure was to thoroughly clean the inner surface of the heat pipe of the copper heat pipe radiator that comes into contact with the gallium-based liquid metal, perform a high phosphorus chemical nickel plating treatment for 18 minutes, and then remove and dry it.

[0027] According to the measurement results, the thickness of the high phosphorus nickel alloy layer formed on the surface of the vapor chamber was 3 μm, and the phosphorus content in the high phosphorus nickel alloy layer was 12%. In order to facilitate subsequent experiments, a 2 mm copper sheet was simultaneously used to perform high phosphorus chemical nickel plating treatment, and then the treated copper sheet was used as the test subject of Example 2 instead of the copper heat pipe.

[0028] Example 3 What is shown in Figure 3 is a metal structure 1, specifically a copper liquid metal container, which has a high phosphorus nickel alloy layer 2 on its inner surface that comes into contact with a gallium-based liquid metal 3. The manufacturing method of this metal structure was to thoroughly clean the inner surface of the copper liquid metal container that comes into contact with the gallium-based liquid metal, perform a high phosphorus chemical nickel plating process for 24 minutes, and then remove and dry it.

[0029] According to the measurement results, the thickness of the high phosphorus nickel alloy layer formed on the inner surface of the copper liquid metal container was 5 μm, and the phosphorus content in the high phosphorus nickel alloy layer was 11%. In order to facilitate subsequent experiments, a 2 mm copper sheet was simultaneously used to perform high phosphorus chemical nickel plating, and then the treated copper sheet was used as the test subject in Example 3 instead of the copper liquid metal container.

[0030] Example 4 The copper microchannel heat sink has a high phosphorus nickel alloy layer on its inner and outer surfaces that come into contact with the gallium-based liquid metal. The inner and outer surfaces of the copper microchannel heat sink that come into contact with the gallium-based liquid metal are cleaned, and then subjected to a high phosphorus chemical nickel plating process for 40 minutes, and then removed and dried.

[0031] According to the measurement results, the thickness of the high phosphorus nickel alloy layer formed on the inner and outer surfaces of the copper microchannel heat sink was 10 μm, and the phosphorus content in the high phosphorus nickel alloy layer was 10%. In order to facilitate subsequent experiments, a 2 mm copper sheet was simultaneously used to perform high phosphorus chemical nickel plating, and then the treated copper sheet was used as the test subject in Example 4 instead of the copper microchannel heat sink.

[0032] Example 5 The aluminum heat sink had a high phosphorus nickel alloy layer on its bottom surface that was in contact with the gallium-based liquid metal. The bottom surface of the aluminum heat sink that was in contact with the gallium-based liquid metal was cleaned, and then the high phosphorus nickel plating process was performed for 20 minutes, and the aluminum heat sink was then removed and dried.

[0033] According to the measurement results, the thickness of the high phosphorus nickel alloy layer formed on the bottom surface of the aluminum heat sink was 5 μm, and the phosphorus content in the high phosphorus nickel alloy layer was 10%. In order to facilitate subsequent experiments, a 2 mm aluminum sheet was simultaneously used to perform high phosphorus chemical nickel plating treatment, and then the treated aluminum sheet was used as the test subject in Example 5 instead of the aluminum heat sink.

[0034] Example 6 The copper alloy heat sink had a high phosphorus nickel alloy layer on its bottom surface that was in contact with the gallium-based liquid metal. The bottom surface of the copper alloy heat sink that was in contact with the gallium-based liquid metal was cleaned, and then the high phosphorus nickel plating process was performed for 20 minutes, and the heat sink was then removed and dried.

[0035] According to the measurement results, the thickness of the high phosphorus nickel alloy layer formed on the bottom surface of the copper alloy heat sink was 5 μm, and the phosphorus content in the high phosphorus nickel alloy layer was 10%. In order to facilitate subsequent experiments, a 2 mm copper alloy sheet was used as the test subject in Example 6 instead of the copper alloy heat sink.

[0036] Example 7 The aluminum alloy heat sink had a high phosphorus nickel alloy layer on its bottom surface that was in contact with the gallium-based liquid metal. The bottom surface of the aluminum alloy heat sink that was in contact with the gallium-based liquid metal was cleaned, and then the high phosphorus nickel plating process was performed for 29 minutes, and the heat sink was removed and dried.

[0037] According to the measurement results, the thickness of the high phosphorus nickel alloy layer formed on the surface of the aluminum alloy heat sink was 5 μm, and the phosphorus content in the high phosphorus nickel alloy layer was 10%. In order to facilitate subsequent experiments, a 2 mm aluminum alloy sheet was used as the test subject in Example 7 instead of the aluminum alloy heat sink.

[0038] Example 8 The stainless steel heat sink had a high phosphorus nickel alloy layer on its bottom surface in contact with the gallium-based liquid metal. The bottom surface of the stainless steel heat sink in contact with the gallium-based liquid metal was cleaned, subjected to a high phosphorus chemical nickel plating process for 29 minutes, removed and dried.

[0039] According to the measurement results, the thickness of the high phosphorus nickel alloy layer formed on the surface of the stainless steel heat sink was 5 μm, and the phosphorus content in the high phosphorus nickel alloy layer was 10%. In order to facilitate subsequent experiments, a 2 mm stainless steel sheet was used as the test subject in Example 8 instead of the stainless steel heat sink.

[0040] Comparative Example 1 The surface of a 2 mm copper sheet is cleaned and not subjected to any treatment.

[0041] Comparative Example 2 The surface of a 2 mm copper sheet is cleaned thoroughly, and then subjected to a medium phosphorus chemical nickel plating process for 18 minutes, and then removed and dried. According to the measurement results, the thickness of the medium phosphorus nickel alloy layer formed on the surface of the copper sheet is 5 μm, and the phosphorus content in the medium phosphorus nickel alloy layer is 9%.

[0042] Comparative Example 3 The surface of a 2 mm copper sheet was cleaned and electroplated with chromium. Measurements showed that the thickness of the electroplated chromium layer formed on the surface of the copper sheet was 5 μm.

[0043] Comparative Example 4 The surface of a 2 mm copper sheet was cleaned thoroughly and subjected to nickel electroplating treatment. Measurement results showed that the thickness of the nickel electroplating layer formed on the surface of the copper sheet was 5 μm.

[0044] Comparative Example 5 The surface of a 2 mm copper sheet was thoroughly cleaned and then coated with 207E high thermal conductive ceramic paint. Measurements showed that the thickness of the high thermal conductive ceramic layer formed on the surface of the copper sheet was 5 μm.

[0045] Example: Testing the protective effect of the plating layer The metal sheets treated by the methods of Examples 1-8 and Comparative Examples 1-4 were used as test subjects. The test subject metal sheets were divided into pairs, one of which was coated with gallium-based liquid metal at the middle position, and a sealant was applied around the liquid metal to prevent leakage of the liquid metal. The other metal sheet was connected to the metal sheet coated with the liquid metal, and the two metal sheets were fixed with clips while maintaining a distance of about 1 mm between them. Each pair of fixed metal sheets was placed in a programmable constant temperature and humidity test box, and the temperature of the constant temperature and humidity test box was set to -40°C and 80°C, respectively, and stabilized for 30 minutes each. This was considered as one cycle, and a high-low temperature cycle test was performed, with the number of cycle tests being 1000. After the test was completed, each pair of metal sheets was separated, the liquid metal was removed, and the reaction between the metal sheet and the liquid metal was observed. The test results are shown in Table 1 below.

[0046] Table 1 Test results JPEG2024545536000002.jpg106137The test results showed that there were no reaction marks on the surface of the metal sheets having high phosphorus nickel alloy layers treated in Examples 1-8, and the surface of the plating layer could be cleaned cleanly, while in Comparative Examples 2 and 5, there were slight reaction marks on the surface, and in Comparative Examples 1, 3 and 4, there were large reaction marks on the surface.

[0047] According to the above test results, a high phosphorus nickel plating layer of 1 μm or more can prevent the reaction between the metal sheet and the gallium-based liquid metal, thereby avoiding the gradual consumption of the gallium-based liquid metal due to the reaction, and avoiding the deterioration of the thermal conductivity performance caused by the consumption of the gallium-based liquid metal thermal interface material. Although a high phosphorus nickel plating layer of 1 μm or more has a good protective effect on the metal structure, for metal structures such as heat sinks and vapor chambers with exposed high phosphorus nickel plating layers on the surface, considering that the high phosphorus nickel plating layer may be worn or scratched during packaging, transportation and use, the thickness of the high phosphorus nickel plating layer is preferably 3 μm or more, more preferably 5 μm or more. In the case of severe wear or special requirements such as high requirements for stability and long service cycles, a high phosphorus nickel plating layer of 10 μm or more can be formed on the surface of the metal structure to ensure sufficient protective effect to avoid unexpected events.

[0048] In Comparative Example 1, the surface of the untreated copper sheet was not cleaned thoroughly, and the area of ​​the marks reached about 35%, which indicated that the metal sheet reacted with a large amount of gallium-based liquid metal, causing a decrease in the thermal conductivity performance due to the consumption of the thermal interface material of the gallium-based liquid metal. In Comparative Example 2, there were slight marks on the surface of the plating layer of the metal sheet covered with a medium phosphorus nickel plating layer, and the area of ​​the marks was about 5% of the contact area with the gallium-based liquid metal, which was obviously less than that of Comparative Example 1. It was shown that the medium phosphorus nickel plating layer with a phosphorus content of 9% played a certain protective effect in preventing the reaction between the metal sheet and the gallium-based liquid metal, but the protective effect was not sufficient, and the gallium-based liquid metal eventually reacted with the metal sheet. Comparative Examples 3-5 and 2 had similar effects, and the metal sheet coated with a chromium electroplating layer in Comparative Example 3, the metal sheet coated with a nickel electroplating layer in Comparative Example 4, and the metal sheet coated with a ceramic layer in Comparative Example 5 all had slight marks on the surface of the plating layer, with the areas of the marks being 15%, 25%, and 3%, respectively, which were obviously less than those of Comparative Example 1. It was shown that the chromium electroplating layer, the nickel electroplating layer, and the ceramic layer had a certain protective effect in preventing the reaction between the metal sheet and the gallium-based liquid metal, but the protective power was obviously lower than that of the high phosphorus nickel plating layer.

[0049] The foregoing description of specific exemplary embodiments of the present invention is for purposes of explanation and illustration. It is not intended that these descriptions be construed as limiting the invention to the precise forms disclosed, and it is apparent that many modifications and variations are possible in light of the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain certain principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments and various different options and modifications of the present invention. It is intended that the scope of the present invention be limited by the claims and their equivalents. [Explanation of symbols]

[0050] 1 - metal structure, 2 - high phosphorus nickel alloy layer, 3 - gallium-based liquid metal.

Claims

1. A metal structure for use in combination with a gallium-based liquid metal, the metal structure having a high phosphorus nickel alloy layer on a surface of the metal structure that contacts the gallium-based liquid metal.

2. The high phosphorus nickel alloy layer has a phosphorus content of ≧10%. The metal structure according to claim 1 .

3. The high phosphorus nickel alloy layer has a thickness of ≧1 μm. The metal structure according to claim 1 .

4. The high phosphorus nickel alloy layer has a thickness of ≥ 3 μm. The metal structure according to claim 3 .

5. The high phosphorus nickel alloy layer has a thickness of ≧5 μm. The metal structure according to claim 4.

6. The high phosphorus nickel alloy layer has a thickness of ≧10 μm. The metal structure according to claim 5 .

7. The metal structure is an assembly that comes into contact with a gallium-based liquid metal, a container or cavity that contains a gallium-based liquid metal, or a gallium-based liquid metal flow pipe. The metal structure according to claim 1 .

8. The metal structure is a fin heat sink, a heat pipe heat sink, a phase change heat sink, a heat sink, a vapor chamber, a microchannel heat sink, a liquid metal fluid heat sink, a liquid metal pressure sensor, a liquid metal pressure transmitter, a liquid metal container, or a part in contact with a gallium-based liquid metal. The metal structure according to claim 7.

9. The surface of the metal structure that comes into contact with the gallium-based liquid metal is a flat surface or a curved surface. The metal structure according to claim 1 .

10. The material of the metal structure is at least one selected from the group consisting of copper, aluminum, iron, nickel, stainless steel, titanium, zinc, gold, and alloys thereof. The metal structure according to claim 1 .

11. The metal structure further comprises a nanocomposite ceramic coating layer on a surface that contacts the gallium-based liquid metal. The metal structure according to claim 1 .

12. The gallium-based liquid metal is at least one selected from the group consisting of gallium metal, gallium-containing liquid alloy, gallium-containing metal oxide, gallium-containing thermal interface material, and gallium-containing composite material. The metal structure according to claim 1 .

13. A high phosphorus nickel alloy layer is formed on the surface of the metal structure in contact with the gallium-based liquid metal by performing a high phosphorus chemical nickel plating process on the surface of the metal structure in contact with the gallium-based liquid metal thermal interface material. The method for producing a metal structure according to claim 1 .

14. The application is to provide heat dissipation for computer chips, mobile phone chips, communication products, high power LEDs, insulated gate bipolar transistors, and high power electronic products. A metal structure according to any one of claims 1 to 12 or produced by the method according to claim 13.

Citation Information

Patent Citations

  • Copper alloy workpiece plated with nickel-phosphorus alloy layer and application of copper alloy workpiece to corrosion prevention of stainless steel product

    CN113249713A

  • Cooling device for integrated circuit chip

    JP1986201452A

  • Method for plating cu and cu alloy with ni

    JP1993179457A

  • Optical member cooling apparatus, lens barrel, exposure apparatus and device manufacturing method

    WO2009051199A1