Membrane electrode assembly, its manufacturing method, and fuel cell including same

The membrane electrode assembly with directly coated subgaskets addresses electrode damage and thickness variability issues, enhancing fuel cell productivity and performance by minimizing air gaps and improving workability.

JP7551796B2Active Publication Date: 2024-09-17KOLON INDUSTRIES INC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023013332
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-11-19
Filing Date
2023-01-31
Publication Date
2024-09-17
Estimated Expiration
2040-06-18

AI Technical Summary

Technical Problem

Conventional methods for preventing hydrogen and oxygen permeation through the electrolyte membrane in polymer electrolyte membrane fuel cells cause electrode damage, vary in subgasket thickness, and create stepped portions that reduce workability and gas leakage prevention.

Method used

A membrane electrode assembly with subgaskets formed by direct coating, ensuring no or minimal stepped portions and air gaps, using elastic materials with adjustable thicknesses, and integrated manufacturing to enhance productivity and performance.

Benefits of technology

The solution prevents electrode damage, allows for easy thickness adjustment, minimizes air gaps, and improves workability, resulting in reduced gas leakage and enhanced fuel cell performance and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007551796000035
    Figure 0007551796000035
  • Figure 0007551796000005
    Figure 0007551796000005
  • Figure 0007551796000030
    Figure 0007551796000030
Patent Text Reader

Abstract

A membrane electrode assembly including a subgasket that has no or almost no steps that reduce the workability of subsequent processes, a method for manufacturing the same, and a fuel cell including the same are provided. [Solution] The method for manufacturing a membrane electrode assembly of the present invention includes the steps of forming a first electrode 121 on a first surface 111 of an electrolyte membrane 110, forming a first subgasket 131 on the first surface of the electrolyte membrane by coating with a first liquid material, forming a second electrode 122 on a second surface 112 of the electrolyte membrane, and forming a second subgasket 132 on the second surface of the electrolyte membrane.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a membrane electrode assembly, a method for producing the same, and a fuel cell including the same. [Background technology]

[0002] A Polymer Electrolyte Membrane Fuel Cell (PEMFC) is a device that generates electricity by using a stacked structure of unit cells, each of which includes a membrane-electrode assembly (MEA) and a separator. Since it has high energy efficiency and environmentally friendly characteristics, it is attracting attention as a next-generation energy source that can replace fossil energy.

[0003] A membrane electrode assembly generally includes an anode (also called a fuel electrode), a cathode (also called an air electrode), and an electrolyte membrane between them. A polymer electrolyte membrane is generally used as the electrolyte membrane.

[0004] FIG. 1 is a schematic diagram of the operation of a fuel cell.

[0005] When a fuel such as hydrogen gas is supplied to the oxidizing electrode 21, hydrogen ions (H + ) and electrons (e - ) is generated. The generated hydrogen ions are transferred to the reduction electrode 22 through the electrolyte membrane 10, and the generated electrons are transferred to the reduction electrode via an external circuit. At the reduction electrode 22, to which air containing oxygen is supplied, a reduction reaction of oxygen occurs. At the reduction electrode 22, oxygen combines with the hydrogen ions and electrons to generate water, and heat is generated.

[0006] Here, if the phenomenon occurs in which hydrogen flowing into the oxidizing electrode 21 and air (oxygen) flowing into the reducing electrode 22 permeate to the counter electrode, the performance of the battery will deteriorate, so it is necessary to prevent hydrogen and air (oxygen) from permeating through the electrolyte membrane 10 and becoming mixed. The ability to prevent hydrogen and air (oxygen) from permeating through the electrolyte membrane 10 and becoming mixed is directly linked to the performance of the electrolyte membrane 10. Therefore, in the past, hydrogen and air (oxygen) were prevented from permeating through the electrolyte membrane 10 and moving to the counter electrode by overlapping a gasket on the periphery of the electrolyte membrane 10 corresponding to the periphery of the membrane electrode assembly, excluding the electrode portion.

[0007] A commonly used method for disposing a gasket on the electrolyte membrane 10 is to laminate a film-type subgasket to the electrolyte membrane 10 by applying heat and pressure. However, this method has the following problems: (i) the electrodes 21 and 22 may be damaged during the heating and pressure process for laminating the subgasket; (ii) since the final thickness of the subgasket is determined by the thickness of the film, subgaskets with various film thicknesses must be separately prepared in order to adjust the thickness of the subgasket; (iii) when a part of the film-type subgasket is attached to the periphery of an electrode, a step corresponding to the thickness of the electrode is formed on the subgasket. Such a step on the subgasket reduces the workability of subsequent processes [e.g., gas diffusion layer (GDL) formation / assembly process]; and (iv) the step generates an air gap between the subgasket film and the side of the electrode, significantly reducing the gas leakage prevention function of the subgasket film. Summary of the Invention [Problem to be solved by the invention]

[0008] SUMMARY OF THE PRESENT EMBODIMENT An embodiment of the present invention provides a membrane electrode assembly capable of solving the above problems, a method for manufacturing the same, and a fuel cell including the same.

[0009] One aspect of the present invention is to provide a membrane electrode assembly including a subgasket that has no or almost no steps that reduce the workability of subsequent processes.

[0010] Another aspect of the present invention is to provide a method for manufacturing a membrane electrode assembly having excellent performance with high productivity without causing electrode damage. Still another aspect of the present invention is to provide a fuel cell manufactured using a membrane electrode assembly including a subgasket that has no or almost no steps that reduce the workability of subsequent processes. [Means for solving the problem]

[0011] According to one aspect of the present invention, there is provided an electrolyte membrane having a first surface and a second surface opposite thereto, the electrolyte membrane including an active region and a non-active region surrounding the active region; a first electrode disposed on the first surface of the electrolyte membrane and covering the active region; a first subgasket disposed on the first surface of the electrolyte membrane and having a first window exposing a central portion of the first electrode; a second electrode disposed on the second surface of the electrolyte membrane and covering the active region; and a second subgasket disposed on the second surface of the electrolyte membrane and having a second window exposing the central portion of the second electrode, the first subgasket being configured to contact a peripheral portion of the first electrode and The second subgasket includes a second overlapping region overlapping a peripheral portion of the second electrode and a second non-overlapping region covering the non-active region, and the second subgasket includes a second overlapping region overlapping a peripheral portion of the second electrode and a second non-overlapping region covering the non-active region, and the second subgasket includes a first overlapping region overlapping with the peripheral portion of the second electrode and a first ...

[0012] Even if there is no air gap between the first subgasket and the first electrode or a first air gap exists between the first subgasket and the first electrode, the volume of the first air gap can satisfy the following formula 1, and even if there is no air gap between the second subgasket and the second electrode or a second air gap exists between the second subgasket and the second electrode, the volume of the second air gap can satisfy the following formula 2.

[0013] Formula 1: V1≦0.5×T1 2 ×(W1+L1)

[0014] Formula 2: V2≦0.5×T2 2 ×(W2+L2)

[0015] where V1 and V2 are the volumes of the first and second air gaps, respectively, T1 and T2 are the thicknesses of the first and second electrodes, respectively, W1 and W2 are the widths of the first and second electrodes, respectively, and L1 and L2 are the lengths of the first and second electrodes, respectively.

[0016] In accordance with another aspect of the present invention, there is provided a method for manufacturing a membrane electrode assembly, the method including the steps of forming a first electrode on a first surface of an electrolyte membrane, forming a first subgasket on the first surface of the electrolyte membrane by coating with a first liquid material, forming a second electrode on a second surface of the electrolyte membrane, and forming a second subgasket on the second surface of the electrolyte membrane by coating with a second liquid material.

[0017] The method for manufacturing the membrane electrode assembly may further include at least one of the steps of disposing a first protective layer on the first electrode prior to forming the first subgasket, and disposing a second protective layer on the second electrode prior to forming the second subgasket.

[0018] The method for manufacturing the membrane electrode assembly may include removing at least one of the first protective layer and the second protective layer.

[0019] The first electrode can be formed by coating or transferring.

[0020] In the step of forming the first electrode, the electrolyte membrane may be supported by a support substrate.

[0021] The coating for forming the first subgasket and the coating for forming the second subgasket can be performed by any one of spray coating, comma coating, and slot die coating using a liquid material.

[0022] At least one of a 3D printer and a partial coating device may be used in the steps of forming the first subgasket and forming the second subgasket.

[0023] The first liquid material and the second liquid material may each be a crosslinkable or curable elastic material.

[0024] The first liquid material and the second liquid material may be the same as each other, or the first liquid material and the second liquid material may be different from each other.

[0025] The first subgasket and the second subgasket may include at least one of polyethylene terephthalate (PET), polyamide, tetrafluoroethylene / hexafluoropropene (FEP), fluororubber, silicone rubber, hydrocarbon-based elastomers (EPDM, EPR, etc.), and polyurethane.

[0026] In at least one of the steps of forming the first subgasket and forming the second subgasket, the first subgasket or the second subgasket may be left for 10 to 600 seconds after the coating.

[0027] In at least one of the steps of forming the first subgasket and forming the second subgasket, the first subgasket or the second subgasket may be heated to a temperature of 40 to 150° C. after the coating.

[0028] In at least one of the steps of forming the first subgasket and forming the second subgasket, after the coating, the first subgasket or the second subgasket may be heat-treated with hot air for 3 to 300 seconds.

[0029] The first protective layer and the second protective layer may each include at least one of polyethylene terephthalate (PET), polyimide (PI), tetrafluoroethylene, polyethylene (PE), rubber, and silicone.

[0030] 4. The method for producing a membrane electrode assembly according to claim 3, further comprising the step of cutting at least a portion of the electrolyte membrane prior to the step of forming the first subgasket.

[0031] According to yet another aspect of the present invention, there is provided a fuel cell including the membrane electrode assembly, a gas diffusion layer on the membrane electrode assembly, and a separator on the gas diffusion layer. Effect of the Invention

[0032] According to an embodiment of the present invention, since the subgasket is formed by coating, the thickness of the subgasket can be easily adjusted by adjusting the coating thickness, and mass production and automation can be realized by applying a direct coating process. In addition, since the subgasket is formed by a direct coating method without a heating and pressurizing process for film lamination, not only does it not cause damage to the electrode, but the subgasket has no or almost no step, so that the workability of subsequent processes such as a gas diffusion layer formation / assembly process can be improved. In addition, it is possible to prevent or minimize the occurrence of an air gap between the side of the electrode and the subgasket, so that the original function of the subgasket to prevent gas leakage can be reliably guaranteed.

[0033] The liquid material used in the direct coating according to an embodiment of the present invention has room temperature crosslinking or thermal crosslinking properties, and the subgasket formed from the liquid material can have excellent gas barrier properties and elasticity.

[0034] According to one embodiment of the present invention, the subgasket and the membrane electrode assembly are manufactured as an integrated unit, which reduces leakage of gases such as hydrogen or air (oxygen) during operation of the fuel cell, and the manufacturing process is simplified, facilitating mass production of fuel cells.

[0035] According to an embodiment of the present invention, an elastic body can be used as a material for the subgasket. As a result, when assembling a fuel cell stack, the elastic body absorbs thickness deviations between components, making it possible to manufacture a stable stack structure. In addition, since the thickness of the subgasket can be easily adjusted, the interfacial bonding strength between the membrane electrode assembly and the gas diffusion layer can be optimized and increased, thereby improving the performance and durability of the fuel cell. In addition, since there is no need to prepare subgasket materials for different thicknesses, production costs can be reduced. [Brief description of the drawings]

[0036] The accompanying drawings are intended to aid in the understanding of the invention and are incorporated in and constitute a part of this specification, illustrate embodiments of the invention and, together with the description, serve to explain the principles of the invention. [Figure 1] FIG. 2 is a schematic diagram of the operation of a fuel cell. [Diagram 2] FIG. 2 is an exploded perspective view of a fuel cell. [Diagram 3] 1 is an exploded perspective view of a membrane electrode assembly according to an embodiment of the present invention; [Figure 4a] 1 is a cross-sectional view of a membrane electrode assembly according to an embodiment of the present invention. [Figure 4b] FIG. 4 is a cross-sectional view of a membrane electrode assembly according to another embodiment of the present invention. [Figure 5a] 3A to 3C are diagrams illustrating a process for manufacturing a membrane electrode assembly according to an embodiment of the present invention. [Figure 5b] 1 is a process diagram illustrating a manufacturing process of a membrane electrode assembly according to an embodiment of the present invention. [Figure 5c] 1 is a process diagram illustrating a manufacturing process of a membrane electrode assembly according to an embodiment of the present invention. [Figure 5d] 1 is a process diagram illustrating a manufacturing process of a membrane electrode assembly according to an embodiment of the present invention. [Figure 5e] 1 is a process diagram illustrating a manufacturing process of a membrane electrode assembly according to an embodiment of the present invention. [Figure 5f] 1 is a process diagram illustrating a manufacturing process of a membrane electrode assembly according to an embodiment of the present invention. [Figure 5g] 1 is a process diagram illustrating a manufacturing process of a membrane electrode assembly according to an embodiment of the present invention. [Figure 5h] 1 is a process diagram illustrating a manufacturing process of a membrane electrode assembly according to an embodiment of the present invention. [Figure 6] FIG. 4 is a cross-sectional view of a membrane electrode assembly according to another embodiment of the present invention. [Figure 7a] 5A to 5C are diagrams illustrating a process for manufacturing a membrane electrode assembly according to another embodiment of the present invention. [Figure 7b] 5A to 5C are diagrams illustrating a process for manufacturing a membrane electrode assembly according to another embodiment of the present invention. [Figure 7c] 5A to 5C are diagrams illustrating a process for manufacturing a membrane electrode assembly according to another embodiment of the present invention. [Figure 7d] 5A to 5C are diagrams illustrating a process for manufacturing a membrane electrode assembly according to another embodiment of the present invention. [Figure 7e] 5A to 5C are diagrams illustrating a process for manufacturing a membrane electrode assembly according to another embodiment of the present invention. [Figure 7f] 5A to 5C are diagrams illustrating a process for manufacturing a membrane electrode assembly according to another embodiment of the present invention. [Figure 7g] 5A to 5C are diagrams illustrating a process for manufacturing a membrane electrode assembly according to another embodiment of the present invention. [Figure 7h] 5A to 5C are diagrams illustrating a process for manufacturing a membrane electrode assembly according to another embodiment of the present invention. [Figure 8] FIG. 2 is a perspective view of a membrane electrode assembly wound into a roll. [Figure 9a] 5A to 5C are diagrams illustrating a process for manufacturing a membrane electrode assembly according to still another embodiment of the present invention. [Figure 9b] 5A to 5C are diagrams illustrating a process for manufacturing a membrane electrode assembly according to still another embodiment of the present invention. [Figure 9c] 4A to 4C are diagrams illustrating a process for manufacturing a membrane electrode assembly according to still another embodiment of the present invention. [Figure 9d] 5A to 5C are diagrams illustrating a process for manufacturing a membrane electrode assembly according to still another embodiment of the present invention. [Figure 9e] 5A to 5C are diagrams illustrating a process for manufacturing a membrane electrode assembly according to still another embodiment of the present invention. [Figure 9f] 5A to 5C are diagrams illustrating a process for manufacturing a membrane electrode assembly according to still another embodiment of the present invention. [Figure 10a] FIG. 2 is a manufacturing process diagram of a membrane electrode assembly according to Comparative Example 1. [Figure 10b] FIG. 2 is a manufacturing process diagram of a membrane electrode assembly according to Comparative Example 1. [Figure 10c] FIG. 2 is a manufacturing process diagram of a membrane electrode assembly according to Comparative Example 1. [Figure 10d] FIG. 2 is a manufacturing process diagram of a membrane electrode assembly according to Comparative Example 1. [Figure 10e] FIG. 2 is a manufacturing process diagram of a membrane electrode assembly according to Comparative Example 1. [Figure 10f] FIG. 2 is a manufacturing process diagram of a membrane electrode assembly according to Comparative Example 1. [Figure 10g] FIG. 2 is a manufacturing process diagram of a membrane electrode assembly according to Comparative Example 1. [Figure 10h] FIG. 2 is a manufacturing process diagram of a membrane electrode assembly according to Comparative Example 1. [Figure 11] FIG. 4 is a cross-sectional view of a membrane electrode assembly according to Comparative Example 2. [Figure 12a] 1 is a photograph of a membrane electrode assembly. [Figure 12b] 1 is a photograph of a membrane electrode assembly. [Figure 12c] 1 is a photograph of a membrane electrode assembly. [Figure 13] 4 is a cross-sectional view of a fuel cell according to yet another embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0037] Hereinafter, the embodiments of the present invention will be described in detail with reference to the accompanying drawings. However, the embodiments described below are presented for illustrative purposes only to help a clear understanding of the present invention, and are not intended to limit the scope of the present invention.

[0038] The shapes, sizes, ratios, angles, numbers, etc. disclosed in the drawings for explaining the embodiments of the present invention are merely illustrative, and the present invention is not limited to the illustrated matters. The same reference numerals refer to the same components throughout the specification. In addition, in the description of the present invention, if it is determined that a detailed description of related known technology may unnecessarily obscure the gist of this specification, the detailed description will be omitted.

[0039] When using words such as 'including,' 'having,' and 'consisting of,' etc. in this specification, other parts may be added unless 'only' is used. When an element is expressed in the singular, it includes the plural unless otherwise expressly stated. In addition, in interpreting an element, it is interpreted as including a margin of error, even if there is no other express description.

[0040] When describing the positional relationship of two parts, for example 'on top of', 'below', 'next to', etc., one or more other parts may be located between the two parts, unless 'directly' or 'immediately' is used.

[0041] Spatially relative terms such as "below," "beneath," "lower," "above," "upper," and the like, may be used to facilitate describing the relationship of one element or component to another element or component as illustrated in the drawings. Spatially relative terms should be understood to include different orientations of elements in use or operation in addition to the orientation depicted in the drawings. For example, if an element depicted in the drawings is turned upside down, an element described as "below" or "beneath" another element may be placed "above" the other element. Thus, the exemplary term "below" can include both below and above. Similarly, the exemplary term "upper" can include both above and below.

[0042] When describing a temporal relationship, for example, 'after', 'following', 'next to', 'before', etc., it is possible to include cases where the relationship is not consecutive, as long as 'immediately' or 'directly' is not used.

[0043] Although the terms "first", "second", etc. are used to describe various components, these components are not limited to these terms. These terms are used only to distinguish one component from another. Therefore, the first component referred to below may also be the second component within the technical spirit of the present invention.

[0044] The term "at least one" should be understood to include all possible combinations of one or more of the relevant items. For example, the meaning of "at least one of the first item, the second item, and the third item" can mean not only the first item, the second item, or the third item, respectively, but also all possible combinations of two or more of the first item, the second item, and the third item.

[0045] The technical features of the various examples of the present invention may be partially or fully combined or combined with each other, and various technical interlocking and driving are possible, and each embodiment may be implemented independently of each other, or may be implemented together in a linked relationship.

[0046] FIG. 2 is an exploded perspective view of the fuel cell.

[0047] According to one embodiment of the present invention, the fuel cell includes an electrolyte membrane 10, a first electrode 21, a second electrode 22, subgaskets 31, 32, gas diffusion layers 41, 42, gaskets 51, 52, and separators 61, 62. Figure 2 shows a single unit cell of the fuel cell.

[0048] A polymer electrolyte membrane known in the art can be used as the electrolyte membrane 10. A detailed description of the electrolyte membrane 10 and the polymer electrolyte membrane will be omitted.

[0049] Either the first electrode 21 or the second electrode 22 can be an oxidizing electrode, and the other can be a reducing electrode. The oxidizing electrode is also called an anode or a fuel electrode, and the reducing electrode is also called a cathode or an air electrode.

[0050] In one embodiment of the present invention, when the first electrode 21 is an oxidizing electrode, the second electrode 22 is a reducing electrode, and when the first electrode 21 is a reducing electrode, the second electrode 22 is an oxidizing electrode.

[0051] A fuel such as hydrogen gas is supplied to one of the first electrode 21 and the second electrode 22, and air containing oxygen is supplied to the other. The hydrogen gas and air are supplied to one of the first electrode 21 and the second electrode 22 through gas diffusion layers 41 and 42, respectively.

[0052] When a fuel such as hydrogen gas is supplied to the oxidizing electrode, hydrogen ions (H + ) and electrons (e -) is generated. The generated hydrogen ions are transferred to the reducing electrode through the polymer electrolyte membrane 10, and the generated electrons are transferred to the reducing electrode via an external circuit. Air containing oxygen is supplied to the reducing electrode, where the oxygen combines with the hydrogen ions and electrons, resulting in the generation of water and heat.

[0053] If hydrogen flowing into the oxidizing electrode and air (oxygen) flowing into the reducing electrode permeate through the electrolyte membrane 10 to the counter electrode, the performance of the fuel cell will deteriorate. Therefore, subgaskets 31 and 32 are provided to prevent hydrogen and air (oxygen) from permeating through the electrolyte membrane 10 to the counter electrode.

[0054] Subgaskets 31 and 32 are disposed on the edges of the electrolyte membrane 10 to prevent hydrogen from flowing into the reducing electrode without passing through the oxidizing electrode, and prevent oxygen from flowing into the oxidizing electrode through the electrolyte membrane 10.

[0055] The gaskets 51 and 52 serve to seal the space between the electrolyte membrane 10 and the separators 61 and 62 so that the supplied gas can be transferred without loss to the first electrode 21 and the second electrode 22 where the electrochemical reaction occurs. The gaskets 51 and 52 can maintain the airtightness of the fuel cell stack.

[0056] The separators 61 and 62 fix the electrolyte membrane 10, the first electrode 21, the second electrode 22, the subgaskets 31 and 32, the gas diffusion layers 41 and 42, and the gaskets 51 and 52. The separators 61 and 62 are also called bipolar plates.

[0057] FIG. 3 is an exploded perspective view of a membrane electrode assembly 100 according to one embodiment of the present invention, and FIGS. 4a and 4b are cross-sectional views of membrane electrode assemblies 100 according to different embodiments of the present invention.

[0058] Referring to Figures 4a and 4b, a subgasket-integrated membrane electrode assembly 100 according to one embodiment of the present invention includes an electrolyte membrane 110 having a first surface 111 and an opposite second surface 112, a first electrode 121 on the first surface 111 of the electrolyte membrane 110, a first subgasket 131 on the first surface 111 of the electrolyte membrane 110, a second electrode 122 on the second surface 112 of the electrolyte membrane 110, and a second subgasket 132 on the second surface 112 of the electrolyte membrane 110.

[0059] The electrolyte membrane 110 includes an active area AA that corresponds to the first and second electrodes 121 and 122 and directly contributes to electricity generation, and a non-active area NA that surrounds the active area AA. A polymer electrolyte membrane known in the art is used as the electrolyte membrane 110. A detailed description of the polymer electrolyte membrane will be omitted.

[0060] The first electrode 121 is disposed on the first surface 111 of the electrolyte membrane 110 to cover the active area AA, and the second electrode 122 is disposed on the second surface 112 of the electrolyte membrane 110 to cover the active area AA.

[0061] Either the first electrode 121 or the second electrode 122 is an oxidizing electrode, and the other is a reducing electrode. The oxidizing electrode is also called an anode or a fuel electrode, and the reducing electrode is also called a cathode or an air electrode.

[0062] When the first electrode 121 is an oxidizing electrode, the second electrode 122 is a reducing electrode, and when the first electrode 121 is a reducing electrode, the second electrode 122 is an oxidizing electrode. A fuel such as hydrogen gas is supplied to one of the first electrode 121 and the second electrode 122, and air containing oxygen is supplied to the other.

[0063] The first subgasket 131 disposed on the first surface 111 of the electrolyte membrane 110 has a first window W1 exposing a central portion of the first electrode 121, and the second subgasket 132 disposed on the second surface 112 of the electrolyte membrane 110 has a second window W2 exposing a central portion of the second electrode 122. Hydrogen gas and oxygen gas come into contact with the central portions of the first and second electrodes 121 and 122 exposed through the first and second windows W1 and W2, respectively.

[0064] The first subgasket 131 and the second subgasket 132 have elasticity and airtightness. The first subgasket 131 and the second subgasket 132 prevent hydrogen or oxygen from one electrode from flowing through the electrolyte membrane 110 to the other electrode.

[0065] The first subgasket 131 and the second subgasket 132 may be made of an elastic material. The first subgasket 131 and the second subgasket 132 may include at least one of polyethylene terephthalate (PET), polyamide, tetrafluoroethylene / hexafluoropropene (FEP), fluororubber, silicone rubber, hydrocarbon-based elastomers (EPDM, EPR, etc.), and polyurethane.

[0066] As illustrated in FIGS. 4a and 4b, the first subgasket 131 includes a first overlapping area OA1 overlapping the peripheral portion of the first electrode 121 and a first non-overlapping area NOA1 covering the non-active area NA of the electrolyte membrane 110.

[0067] Similarly, the second subgasket 132 includes a second overlapping area OA2 that overlaps the peripheral edge of the second electrode 122 and a second non-overlapping area NOA2 that covers the non-active area NA of the electrolyte membrane 110.

[0068] The first and second overlapping regions OA1, OA2 of the first and second subgaskets 131, 132 not only protect the peripheral portions of the first and second electrodes 121, 122, respectively, but also prevent gas from leaking through the boundary between the first subgasket 131 and the first electrode 121 or the boundary between the second subgasket 132 and the second electrode 122.

[0069] According to the present invention, (i) as shown in FIG. 4a, there is no step between the first overlap region OA1 and the first non-overlapping region NOA1, and between the second overlap region OA2 and the second non-overlapping region NOA2, or (ii) as shown in FIG. 4b, the height H1 of the first step formed by the first overlap region OA1 and the first non-overlapping region NOA1 is 0.5 times or less, more preferably 0.2 times or less, the thickness T1 of the first electrode 121, and the height H2 of the second step formed by the second overlap region OA2 and the second non-overlapping region NOA2 is 0.5 times or less, more preferably 0.2 times or less, the thickness T2 of the second electrode 122.

[0070] That is, according to the present invention, the first and second sub-gaskets 131 and 132 do not have a step on their upper surfaces, or even if they have a step, the height of the step is very small, such as less than 0.5 times, more preferably less than 0.2 times, the thickness T1 of the first electrode 121 or the thickness T2 of the second electrode 122, thereby improving the workability of subsequent processes such as a gas diffusion layer formation / assembly process.

[0071] 4a and 4b, the first and second sub-gaskets 131 and 132 may be closely attached to the first and second electrodes 121 and 122, respectively, to the extent that no air gap exists, thereby preventing gas leakage through the air gap.

[0072] Hereinafter, a method for manufacturing a membrane electrode assembly 100 according to an embodiment of the present invention will be described with reference to FIGS. 5a to 5h.

[0073] 5a to 5h are diagrams showing the manufacturing process of a membrane electrode assembly 100 according to an embodiment of the present invention.

[0074] First, referring to FIG. 5A, a first electrode 121 is formed on a first surface 111 of an electrolyte membrane 110. do.

[0075] There is no particular limitation on the method of forming the first electrode 121. According to an embodiment of the present invention, the first electrode 121 may be formed by a coating method or a transfer method. The material of the first electrode 121 may be at least one of an oxidizing electrode material or a reducing electrode material known in the art.

[0076] In the step of forming the first electrode 121, the electrolyte membrane 110 may be supported by a supporting substrate 190. There is no particular limitation on the type of the supporting substrate 190. Any material capable of supporting the electrolyte membrane 110 may be used as the supporting substrate 190. For example, a plastic film may be used as the supporting substrate 190. According to an embodiment of the present invention, a polyethylene terephthalate (PET) film may be used as the supporting substrate 190. do.

[0077] Referring to FIG. 5 b , a first protective layer 211 is disposed on the first electrode 121 .

[0078] The first protective layer 211 protects the first electrode 121. After coating for forming the first subgasket 131, the first protective layer 211 may be removed, or may be attached until the second subgasket 132 is formed, and then removed together with the second protective layer 212 after the second subgasket 132 is formed. Therefore, the first protective layer 211 is made of a material that can minimize damage to the first electrode 121 during the peeling process.

[0079] The first protective layer 211 may be made of, for example, at least one of polyethylene terephthalate (PET), polyimide (PI), tetrafluoroethylene, polyethylene (PE), rubber, and silicon.

[0080] The first protective layer 211 has a thickness of 1 to 50 μm.

[0081] 5b, the first protective layer 211 has an area smaller than that of the first electrode 121 and is disposed within the region of the first electrode 121. More specifically, the first protective layer 211 is disposed inside the edge of the first electrode 121. Thus, the first subgasket 131 is also disposed on the peripheral edge of the first electrode 121.

[0082] Referring to FIG. 5c, a first subgasket 131 is formed on the first surface 111 of the electrolyte membrane 110 by coating with a first liquid material.

[0083] The first liquid material for forming the first subgasket 131 is made of a crosslinkable or curable elastic material.

[0084] Specifically, the first subgasket 131 may include at least one of polyethylene terephthalate (PET), polyamide, tetrafluoroethylene / hexafluoropropene (FEP), fluororubber, silicone rubber, hydrocarbon-based elastomer (EPDM, EPR, etc.), and polyurethane. Thus, the first liquid material may be a material in which any one of polyethylene terephthalate (PET), polyamide, tetrafluoroethylene / hexafluoropropene (FEP), fluororubber, silicone rubber, hydrocarbon-based elastomer (EPDM, EPR, etc.), and polyurethane is dissolved or dispersed in a solvent. In this way, the first liquid material may include a polymer component.

[0085] According to an embodiment of the present invention, the first sub-gasket 131 may be formed by a direct coating method using a liquid material.

[0086] Specifically, the coating for forming the first subgasket 131 may be performed by any one of spray coating, comma coating, and slot die coating using a liquid material. For example, the first subgasket 131 may be formed by spray coating.

[0087] 5c shows a method of forming the first subgasket 131 by spray coating. As described above, according to one embodiment of the present invention, a direct coating method using a liquid material can be applied as a coating method for forming the first subgasket 131. Referring to FIG 5c, a spray coating device 250 is used for spray coating.

[0088] After coating, the first liquid material dries and crosslinks or hardens to form the first subgasket 131 .

[0089] In the step of forming the first subgasket 131, after coating, the first subgasket 131 may be left for 10 to 600 seconds, thereby allowing the first liquid material used to form the first subgasket 131 to dry and promoting crosslinking or hardening of the polymer component contained in the first liquid material.

[0090] Furthermore, in the step of forming the first subgasket 131, after coating with the first liquid material, the first subgasket 131 can be heated to a temperature of 40 to 150° C. Such heating promotes thermal crosslinking or thermal curing of the polymer component contained in the first liquid material, thereby completing the first subgasket 131.

[0091] According to an embodiment of the present invention, in the step of forming the first sub-gasket 131, after coating with the first liquid material, the first sub-gasket 131 may be heat-treated with hot air for 3 to 300 seconds.

[0092] Referring to FIG. 5d, after the electrolyte membrane 110 is separated from the support substrate 190, the electrolyte membrane 110 is turned over so that the second surface 112 of the electrolyte membrane 110 faces upward.

[0093] Referring to FIG. 5 e , a second electrode 122 is formed on the second surface 112 of the electrolyte membrane 110 .

[0094] The second electrode 122 may be formed in the same manner as the first electrode 121. According to an embodiment of the present invention, the second electrode 122 may be formed by a coating method or a transfer method. When the first electrode 121 is an oxidizing electrode, the second electrode 122 becomes a reducing electrode, and when the first electrode 121 is a reducing electrode, the second electrode 122 becomes an oxidizing electrode. The material of the second electrode 122 may be at least one of a reducing electrode material or an oxidizing electrode material known in the art.

[0095] Referring to FIG. 5 f , a second protective layer 212 is disposed over the second electrode 122 .

[0096] The second protective layer 212 protects the second electrode 122. After coating for forming the second subgasket 132, the second protective layer 212 is removed. Therefore, the second protective layer 212 is formed of a material that can minimize damage to the second electrode 122 during the peeling process.

[0097] The second protective layer 212 is made of the same material as the first protective layer 211 .

[0098] For example, at least one of polyethylene terephthalate (PET), polyimide (PI), tetrafluoroethylene, polyethylene (PE), rubber, and silicone can be used as the second protective layer 212. The first protective layer 211 has a thickness of 1 to 50 μm.

[0099] 5f, the second protective layer 212 has an area smaller than that of the second electrode 122 and is disposed within the region of the second electrode 122. More specifically, the second protective layer 212 is disposed inside the edge of the second electrode 122. Thus, the second subgasket 132 can also be disposed on the peripheral edge of the second electrode 122.

[0100] Referring to FIG. 5g, a second subgasket 132 is formed on the second surface 112 of the electrolyte membrane 110 by coating with a second liquid material.

[0101] The second liquid material for forming the second subgasket 132 may be the same as or different from the first liquid material for forming the first subgasket 131 .

[0102] According to an embodiment of the present invention, the first liquid material and the second liquid material may have the same composition.

[0103] Meanwhile, depending on the application site or use, different additives may be added to the first liquid material and the second liquid material to change their compositions, so that the first subgasket 131 and the second subgasket 132 may have different functions.

[0104] The second liquid material for forming the second subgasket 132 is made of a crosslinkable or curable elastic material.

[0105] Specifically, the second sub-gasket 132 may include at least one of polyethylene terephthalate (PET), polyamide, tetrafluoroethylene / hexafluoropropene (FEP), fluororubber, silicone rubber, hydrocarbon-based elastomer (EPDM, EPR, etc.), and polyurethane. Thus, the second liquid material is a material in which any one of polyethylene terephthalate (PET), polyamide, tetrafluoroethylene / hexafluoropropene (FEP), fluororubber, silicone rubber, hydrocarbon-based elastomer (EPDM, EPR, etc.), and polyurethane is dissolved or dispersed in a solvent. Thus, the second liquid material may include a polymer component. According to an embodiment of the present invention, the second sub-gasket 132 may be formed by a direct coating method using a liquid material.

[0106] Specifically, the coating for forming the second subgasket 132 may be performed by any one of spray coating, comma coating, and slot die coating using a liquid material. For example, the second subgasket 132 may be formed by spray coating.

[0107] 5g, a method of forming the second subgasket 132 by spray coating is shown. As described above, according to one embodiment of the present invention, a direct coating method using a liquid material can be applied to form the second subgasket 132, and typically spray coating can be applied.

[0108] After coating, the second liquid material dries and crosslinks or hardens to form the second subgasket 132 .

[0109] In the step of forming the second subgasket 132, after coating, the second subgasket 132 may be left for 10 to 600 seconds, so that the second liquid material used to form the second subgasket 132 dries and crosslinking or hardening of the polymer component contained in the second liquid material proceeds.

[0110] Furthermore, in the step of forming the second subgasket 132, after coating with the second liquid material, the second subgasket 132 may be heated to a temperature of 40 to 150° C. Such heating promotes thermal crosslinking or thermal curing of the polymer component contained in the second liquid material, thereby completing the second subgasket 132.

[0111] According to an embodiment of the present invention, in the step of forming the second sub-gasket 132, after coating with the second liquid material, the second sub-gasket 132 may be heat-treated with hot air for 3 to 300 seconds.

[0112] The heating of the first subgasket 131 and the heating of the second subgasket 132 can be performed simultaneously or separately.

[0113] However, the embodiment of the present invention is not limited thereto, and heating may or may not be performed depending on the material.

[0114] 5h, the first protective layer 211 and the second protective layer 212 are removed. When the first protective layer 211 and the second protective layer 212 are removed, the coating layer made of the first liquid material and the coating layer made of the second liquid material remaining on the first protective layer 211 and the second protective layer 212 are also removed.

[0115] The first protective layer 211 and the second protective layer 212 are removed to expose the first electrode 121 and the second electrode 122, thereby completing the membrane electrode assembly 100 according to an embodiment of the present invention. Referring to Fig. 5h, the surface of the first electrode 121 opposite the electrolyte membrane 110 is exposed, and the surface of the second electrode 122 opposite the electrolyte membrane 110 is exposed.

[0116] FIG. 6 is a cross-sectional view of a membrane electrode assembly 200 according to another embodiment of the present invention.

[0117] Compared with FIGS. 4 a and 4 b , the membrane electrode assembly 200 shown in FIG. 6 differs in that the entire edge of the electrolyte membrane 110 is surrounded by first and second subgaskets 131 , 132 .

[0118] Compared to the membrane electrode assembly 100 of FIGS. 4a and 4b in which the electrolyte membrane 110 has the same specifications as the first subgasket 131 or the second subgasket 132, the subgasket-integrated membrane electrode assembly 200 of FIG. 6 can protect the edges of the electrolyte membrane 110 more stably and is more economical because it uses less expensive electrolyte membrane 110.

[0119] 7a to 7h are diagrams showing the manufacturing process of a membrane electrode assembly 200 according to another embodiment of the present invention.

[0120] The method for manufacturing the membrane electrode assembly 200 according to another embodiment of the present invention further includes a step of cutting at least a portion of the electrolyte membrane 110 prior to the step of forming the first subgasket 131.

[0121] Hereinafter, a method for manufacturing a membrane electrode assembly 200 according to another embodiment of the present invention will be described with reference to FIGS. 7a to 7h.

[0122] 7a, a first electrode 121 is formed on a first surface 111 of an electrolyte membrane 110. There is no particular limitation on the method of forming the first electrode 121. The first electrode 121 may be formed by a coating method or a transfer method.

[0123] 7b, the edge of the electrolyte membrane 110 is cut. Here, a cutter 260 or a pinnacle die can be used. Thus, the electrolyte membrane 110 has a smaller area than the support substrate 190.

[0124] 7c, a first protective layer 211 is disposed on the first electrode 121. The first protective layer 211 protects the first electrode 121 during a subsequent coating process.

[0125] 7d, a first subgasket 131 is formed on the first surface 111 of the electrolyte membrane 110 by coating with a first liquid material. The first subgasket 131 completely surrounds the first surface 111 and the side surfaces of the electrolyte membrane 110.

[0126] 7d, the first subgasket 131 is formed by spray coating, which is one of the direct coating methods using a liquid material. After coating, the first liquid material may be crosslinked or hardened while drying.

[0127] Referring to FIG. 7e, after the electrolyte membrane 110 is separated from the support substrate 190, the electrolyte membrane 110 is turned over so that the second surface 112 of the electrolyte membrane 110 faces upward.

[0128] 7f, a second electrode 122 is formed on the second surface 112 of the electrolyte membrane 110, and a second protective layer 212 is disposed on the second electrode 122. The second protective layer 212 protects the second electrode 122.

[0129] Referring to FIG. 7g, a second subgasket 132 is formed on the second surface 112 of the electrolyte membrane 110 and the first subgasket 131 by coating with a second liquid material.

[0130] The second liquid material for forming the second subgasket 132 may be the same as or different from the first liquid material for forming the first subgasket 131. Referring to Fig. 7g, the second subgasket 132 is formed by spray coating. Therefore, according to one embodiment of the present invention, the coating for forming the second subgasket 132 may be performed by a direct coating method using a liquid material. For example, it may be performed by spray coating.

[0131] After coating, the second liquid material may crosslink or harden as it dries.

[0132] 7h, the first protective layer 211 and the second protective layer 212 are removed. When the first protective layer 211 and the second protective layer 212 are removed, the coating layer made of the first liquid material and the coating layer made of the second liquid material remaining on the first protective layer 211 and the second protective layer 212 are also removed. With the first protective layer 211 and the second protective layer 212 removed, the first electrode 121 and the second electrode 122 are opened, thereby completing the membrane electrode assembly 200 according to another embodiment of the present invention.

[0133] The thickness of the subgaskets 131, 132 formed by the coating method can be adjusted in various ways, and since they are manufactured by a liquid coating method, the subgaskets 131, 132 can be formed without air gaps that occur due to thickness differences in the electrode layers when laminating an existing film-type subgasket. In addition, the subgaskets 131, 132 can be manufactured flat, which allows for easy workability when assembling the gas diffusion layer (GDL).

[0134] FIG. 8 is a perspective view of a membrane electrode assembly wound into a roll.

[0135] The membrane electrode assembly 100, 200 according to the embodiment of the present invention is wound into a roll as shown in Fig. 8. A cross section taken along II' in Fig. 8 can be shown as Fig. 4a, Fig. 4b or Fig. 6.

[0136] According to an embodiment of the present invention, when the sub-gasket integrated membrane electrode assembly 100, 200 is manufactured by directly coating the electrolyte membrane 110 with the material for forming the sub-gasket, the membrane electrode assembly 100, 200 can be manufactured by a roll-to-roll method, thereby enabling mass production.

[0137] Hereinafter, a method for manufacturing a membrane electrode assembly according to still another embodiment of the present invention will be described with reference to FIGS. 9a to 9f.

[0138] Referring to FIG. 9 a , a first electrode 121 is formed on a first surface 111 of an electrolyte membrane 110 .

[0139] In the step of forming the first electrode 121, the electrolyte membrane 110 is supported by the support substrate 190.

[0140] Referring to FIG. 9b, a first subgasket 131 is formed on the first surface 111 of the electrolyte membrane 110 by coating with a first liquid material.

[0141] The first liquid material for forming the first subgasket 131 is made of a crosslinkable or curable elastic material.

[0142] According to yet another embodiment of the present invention, the first subgasket 131 may be formed by directly coating / printing a first liquid material for forming the first subgasket 131 on the electrolyte membrane 110 around the first electrode 121 without a protective layer. For example, using a 3D printer or partial coating equipment, the first liquid material may be directly coated / printed and crosslinked around the first electrode 121 without a protective layer. Thus, the first subgasket 131 is selectively formed on the electrolyte membrane 110.

[0143] FIG. 9b illustrates the use of a 3D printer 350 for direct coating.

[0144] Referring to FIG. 9c, after coating / printing, the first liquid material crosslinks or hardens as it dries to form a first subgasket 131.

[0145] Referring to FIG. 9d, after separating the electrolyte membrane 110 from the supporting substrate 190, the electrolyte membrane 110 is turned over so that the second surface 112 of the electrolyte membrane 110 faces upward, and a second electrode 122 is formed on the second surface 112 of the electrolyte membrane 110.

[0146] The second electrode 122 may be formed in the same manner as the first electrode 121. According to an embodiment of the present invention, the second electrode 122 may be formed by a coating method or a transfer method. When the first electrode 121 is an oxidizing electrode, the second electrode 122 becomes a reducing electrode, and when the first electrode 121 is a reducing electrode, the second electrode 122 becomes an oxidizing electrode.

[0147] Referring to FIG. 9e, a second subgasket 132 is formed on the second surface 112 of the electrolyte membrane 110 by coating with a second liquid material.

[0148] The second liquid material for forming the second subgasket 132 is made of a crosslinkable or curable elastic material. The second liquid material for forming the second subgasket 132 may be the same as or different from the first liquid material for forming the first subgasket 131.

[0149] According to yet another embodiment of the present invention, the second subgasket 132 may be formed by directly coating / printing a second liquid material for forming the second subgasket 132 on the electrolyte membrane 110 around the second electrode 122 without a protective layer. For example, using a 3D printer or partial coating equipment, the second liquid material may be directly coated / printed and crosslinked around the second electrode 122 without a protective layer. Thus, the second subgasket 132 is selectively formed on the electrolyte membrane 110.

[0150] FIG. 9e illustrates a method of using a 3D printer 350 for direct coating.

[0151] 9f, after coating / printing, the second liquid material is cross-linked or cured while drying to complete the second subgasket 132. Thus, a membrane electrode assembly according to yet another embodiment of the present invention is manufactured.

[0152] 10a to 10h are diagrams showing the manufacturing process of the membrane electrode assembly according to Comparative Example 1. FIG.

[0153] The method for manufacturing a membrane electrode assembly according to Comparative Example 1 is different from the embodiment of the present invention in that a CCM (Catalyst Coated Membrane) in which a first electrode 121 and a second electrode 122 are already formed on an electrolyte membrane 110 is used.

[0154] Specifically, referring to FIG. 10A, a catalyst coated membrane (CCM) in which a first electrode 121 and a second electrode 122 are already formed on an electrolyte membrane 110 is disposed on a support substrate 190. As shown in FIG.

[0155] Referring to FIG. 10b, a first protective layer 211 is disposed on the first electrode 121 of the CCM.

[0156] Referring to FIG. 10c, a first subgasket 131 is formed on the first surface 111 of the electrolyte membrane 110 by coating with a first liquid material.

[0157] Referring to FIG. 10d, the first protective layer 211 is removed.

[0158] Referring to FIG. 10e, the electrolyte membrane 110 is turned over so that the second side of the electrolyte membrane 110 and the second electrode 122 face upwards.

[0159] 10f, a second protective layer 212 is disposed on the second electrode 122. The second protective layer 212 protects the second electrode 122 during subsequent coating steps.

[0160] Referring to FIG. 10g, a second subgasket 132 is formed on the second surface of the electrolyte membrane 110 by coating with a second liquid material.

[0161] Referring to FIG. 10h, the second protective layer 212 is removed.

[0162] As shown in Figures 10a to 10h, when a subgasket-integrated membrane electrode assembly is manufactured by spray coating using a catalyst coated membrane (CCM), depending on the thickness of the electrodes 121 and 122, the electrolyte membrane 110 of the CCM, especially the non-active area, may not be sufficiently supported by the support substrate 190, which may cause curling in the membrane electrode assembly.

[0163] 10a to 10d, it can be seen that the non-active region of the electrolyte membrane 110 is separated from the support substrate 190 without being in close contact with the support substrate 190. Due to this separation, curling occurs in the non-active region of the electrolyte membrane 110, and as a result, curling occurs in the membrane electrode assembly.

[0164] The average curl occurrence number and the non-defective rate per sample were calculated for 100 samples of the membrane electrode assembly 100 manufactured by the method of Figures 5a to 5h according to an embodiment of the present invention (Example 1) and 100 samples of the membrane electrode assembly manufactured by the method of Figures 10a to 10h (Comparative Example 1). The results are shown in Table 1.

[0165] The average number of curls per sample means the average number of curls that occurred in 100 samples, and the non-defective rate means the ratio of non-defective products.

[0166] [Table 1]

[0167] Referring to Table 1, it can be seen that when the membrane electrode assembly 100 is manufactured according to an embodiment of the present invention, the defect rate is small and the average number of curls is small.

[0168] FIG. 11 is a cross-sectional view of the membrane electrode assembly according to Comparative Example 2. As shown in FIG.

[0169] Film-like subgaskets 161 and 162 are attached to the membrane electrode assembly in FIG.

[0170] In the case of the film-like subgaskets 161, 162, the thickness of the subgaskets 161, 162 is determined by the thickness of the film, so that it is not easy to adjust the thickness compared to the subgaskets 131, 132 formed by direct coating.

[0171] When film-type subgaskets 161, 162 are used, the subgaskets 161, 162 have steps corresponding to the thickness of the electrodes 121, 122, and such steps may cause air gaps 290 between the subgaskets 161, 162 and the electrodes 121, 122. Fig. 11 illustrates an example of an air gap 290 surrounded by the electrolyte membrane 110, the electrodes 121, 122, and the film-type subgaskets 161, 162. Such air gaps 290 cause gas leakage, degrading the quality of the membrane electrode assembly.

[0172] Assuming that the air gap 290 has the shape of an isosceles right triangular prism and occurs around the entire circumference of the rectangular electrodes 121 and 122, the volume that occurs when using film-like subgaskets 161 and 162 can be calculated using the following formula.

[0173] V(cm 3 )=T 2 ×(W+L)

[0174] where V is the volume of the air gap 290, T is the thickness of the electrodes 121, 122, W is the width of the electrodes 121, 122, and L is the length of the electrodes 121, 122.

[0175] Meanwhile, according to the embodiment of the present invention, since the subgaskets 131 and 132 are manufactured by direct coating, the thickness of the subgaskets 131 and 132 can be adjusted in various ways. Also, according to the embodiment of the present invention, since the subgaskets 131 and 132 are manufactured by a coating method using a liquid material, the subgaskets 131 and 132 do not have a step, or even if they have a step, the height is very small, about 0.5 times or less, more preferably 0.2 times or less, of the thicknesses T1 and T2 of the electrodes 121 and 122 (i.e., the upper surface is substantially flat). Therefore, according to the present invention, it is possible to improve the workability of the subsequent process such as the formation / assembly process of the gas diffusion layer (GDL), as well as to prevent or minimize the formation of air gaps that cause gas leakage (about 0.5 times or less, more preferably 0.2 times or less of the air gap volume formed when using a film-type subgasket). can be done.

[0176] That is, according to one embodiment of the present invention, even if there is no air gap between the first subgasket 131 and the first electrode 121 or a first air gap exists between the first subgasket 131 and the first electrode 121, the volume of the first air gap satisfies the following formula 1, and even if there is no air gap between the second subgasket 132 and the second electrode 122 or a second air gap exists between the second subgasket 132 and the second electrode 122, the volume of the second air gap satisfies the following formula 2.

[0177] Formula 1: V1≦0.5×T1 2 ×(W1+L1)

[0178] Formula 2: V2≦0.5×T2 2 ×(W2+L2)

[0179] Here, V1 and V2 are the volumes of the first and second air gaps, respectively, T1 and T2 are the thicknesses of the first and second electrodes 121, 122, respectively, W1 and W2 are the widths of the first and second electrodes 121, 122, respectively, and L1 and L2 are the lengths of the first and second electrodes 121, 122, respectively.

[0180] 12a to 12c are photographs of the membrane electrode assembly. Specifically, Figure 12a is a photograph of a membrane electrode assembly 100 manufactured by the method shown in Figures 5a to 5h, Figure 12b is a photograph of a membrane electrode assembly manufactured by the method shown in Figures 10a to 10h (Comparative Example 1), and Figure 12c is a photograph of a membrane electrode assembly to which a film-shaped subgasket is attached (Comparative Example 2).

[0181] Referring to FIG. 12b, it can be seen that a large number of curls were generated in the membrane electrode assembly according to Comparative Example 1.

[0182] An air gap was generated inside the membrane electrode assembly of FIG. 12c manufactured according to Comparative Example 2.

[0183] On the other hand, no curl or air gap was found in the membrane electrode assembly of FIG. 12a manufactured according to the embodiment of the present invention.

[0184] FIG. 13 is a cross-sectional view of a fuel cell 300 according to one embodiment of the present invention.

[0185] A fuel cell 300 according to an embodiment of the present invention includes the above-described membrane electrode assembly 100 of the present invention, a gas diffusion layer 140 on the membrane electrode assembly 100 , and a separator 150 on the gas diffusion layer 140 .

[0186] The membrane electrode assembly 100 includes an electrolyte membrane 110 , a first electrode 121 and a first subgasket 131 on a first surface of the electrolyte membrane 110 , and a second electrode 122 and a second subgasket 132 on a second surface of the electrolyte membrane 110 .

[0187] A gas diffusion layer 140 and a separator 150 may be disposed on each side of the membrane electrode assembly 100. The gas diffusion layer 140 and the separator 150 have been described above, so a detailed description thereof will be omitted.

[0188] Referring to FIG. 13, a fuel cell 300 according to another embodiment of the present invention may include a first gasket 171 and a second gasket 172 .

[0189] The first gasket 171 and the second gasket 172 are disposed between the membrane electrode assembly 100 and the separator 150, respectively, to seal the space between the electrolyte membrane 110 and the separator 150. Referring to FIG. 13, the gas diffusion layer 140 may be disposed in the space defined by the first subgasket 131 and the first gasket 171, and in the space defined by the second subgasket 132 and the second gasket 172.

[0190] Although FIG. 13 illustrates an example of the gas diffusion layer 140 being formed only on the exposed portions of the first and second electrodes 121, 122, the present invention is not limited thereto, and the gas diffusion layer 140 may extend to cover at least a portion of each of the first and second subgaskets 131, 132.

[0191] The above-described embodiments are provided to aid in the understanding of the present invention, and are not intended to limit the scope of the present invention, which is defined by the claims.

Claims

1. forming a first electrode on a first surface of the electrolyte membrane; forming a first subgasket on a first surface of the electrolyte membrane by coating with a first liquid material; forming a second electrode on a second surface of the electrolyte membrane; forming a second subgasket on a second surface of the electrolyte membrane by coating with a second liquid material, The production method comprises the steps of: prior to forming the first subgasket, disposing a first protective layer on the first electrode; and disposing a second protective layer on the second electrode prior to forming the second subgasket. A method for producing a membrane electrode assembly.

2. The method for manufacturing a membrane electrode assembly according to claim 1 , further comprising removing at least one of the first protective layer and the second protective layer.

3. The method for producing a membrane electrode assembly according to claim 1 , wherein the first electrode is formed by coating or transferring.

4. The method of claim 1 , wherein in the forming of the first electrode, the electrolyte membrane is supported by a support substrate.

5. 2. The method for manufacturing a membrane electrode assembly according to claim 1, wherein the coating for forming the first subgasket and the coating for forming the second subgasket are each performed by one of spray coating, comma coating, and slot die coating using a liquid material.

6. The method for manufacturing a membrane electrode assembly according to claim 1 , wherein at least one of a 3D printer and a partial coating facility is used in forming the first subgasket and the second subgasket.

7. The method for producing a membrane electrode assembly according to claim 1 , wherein the first liquid material and the second liquid material are each a crosslinkable or curable elastic material.

8. The method for manufacturing a membrane electrode assembly according to claim 1 , wherein the first liquid material and the second liquid material are the same.

9. The method for manufacturing a membrane electrode assembly according to claim 1 , wherein the first liquid material and the second liquid material are different from each other.

10. 2. The method for producing a membrane electrode assembly according to claim 1, wherein the first subgasket and the second subgasket contain at least one of polyethylene terephthalate (PET), polyamide, tetrafluoroethylene / hexafluoropropene (FEP), fluororubber, silicone rubber, a hydrocarbon-based elastomer, and polyurethane.

11. 2. The method for producing a membrane electrode assembly according to claim 1, wherein in at least one of the steps of forming the first subgasket and forming the second subgasket, the first subgasket or the second subgasket is left for 10 seconds to 600 seconds after the coating.

12. 2. The method for producing a membrane electrode assembly according to claim 1, wherein in at least one of the steps of forming the first subgasket and forming the second subgasket, the first subgasket or the second subgasket is heated to a temperature of 40 to 150° C. after the coating.

13. 2. The method for producing a membrane electrode assembly according to claim 1, wherein in at least one of the steps of forming the first subgasket and forming the second subgasket, after the coating, the first subgasket or the second subgasket is heat-treated with hot air for 3 seconds to 300 seconds.

14. 2. The method for producing a membrane electrode assembly according to claim 1, wherein the first protective layer and the second protective layer each contain at least one of polyethylene terephthalate (PET), polyimide (PI), tetrafluoroethylene, polyethylene (PE), rubber, and silicone.

15. 2. The method of claim 1, further comprising the step of cutting at least a portion of the electrolyte membrane prior to the step of forming the first subgasket.

Citation Information

Patent Citations

  • Manufacturing method of solid polymer fuel cell, and solid polymer fuel cell manufactured by the method

    JP2010073562A