How lithium-ion batteries are manufactured
By attaching specific metals to both surfaces of the negative electrode active material in lithium ion batteries, with controlled potentials and void formation, SEI growth is inhibited, leading to reduced battery resistance.
Patent Information
- Application Number
- JP2021201517
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-12-13
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2041-12-13
AI Technical Summary
The growth of the Solid Electrolyte Interface (SEI) film between the negative electrode active material and the electrolyte in lithium ion batteries increases battery resistance, and existing methods to inhibit this growth are inadequate.
Attaching specific metals to both the external and internal surfaces of the negative electrode active material, with dissolution and deposition potentials set to prevent SEI growth, using metals like Fe, Cr, and Ni, and forming voids within the negative electrode active material to allow metal ion penetration.
Inhibits SEI growth on both external and internal surfaces, reducing battery resistance effectively.
Smart Images

Figure 0007552568000003 
Figure 0007552568000002 
Figure 0007552568000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to lithium-ion batteries and methods for making the same. [Background technology]
[0002] Japanese Patent Laid-Open Publication No. 2013-246992 (Patent Document 1) discloses that the surface of the negative electrode active material contains at least one selected from the group consisting of Mo, W, Al, Zr, Mg, Ti, and Zn. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2013-246992 A Summary of the Invention [Problem to be solved by the invention]
[0004] It is known that in lithium ion batteries (hereinafter, abbreviated as "batteries"), a coating is formed at the interface between the negative electrode active material and the electrolyte. This coating is called SEI (Solid Electrolyte Interface). When the SEI grows thick, the battery resistance increases.
[0005] It has been proposed to attach a metal to the outer surface of the negative electrode active material in order to inhibit the growth of the SEI. It is expected that the inhibition of the growth of the SEI will reduce the battery resistance. However, there is still room for improvement.
[0006] An object of the present disclosure is to reduce battery resistance. [Means for solving the problem]
[0007] The technical configuration and effects of the present disclosure will be described below. However, the mechanism of action in this specification includes assumptions. The mechanism of action does not limit the technical scope of the present disclosure.
[0008] 1. A lithium ion battery includes a positive electrode, a negative electrode, and an electrolyte. The positive electrode includes a positive electrode active material. The negative electrode includes a negative electrode active material and a specific metal. Voids are formed inside the negative electrode active material. The specific metal is attached to the outer surface and the inner surface of the negative electrode active material. The specific metal has a dissolution potential and a deposition potential. The dissolution potential is lower than the potential at which the positive electrode active material releases lithium (Li) ions. The deposition potential is higher than the potential at which the negative electrode active material absorbs Li ions.
[0009] A "specific metal" has a specific dissolution potential and deposition potential. The dissolution potential is lower than the potential at which the positive electrode active material releases Li ions. The deposition potential is higher than the potential at which the negative electrode active material absorbs Li ions.
[0010] Conventionally, it has been avoided to mix specific metals into batteries. This is because the specific metal dissolves at the positive electrode and deposits at the negative electrode, which may cause, for example, a micro-short circuit. According to the new findings of the present disclosure, the specific metal has the advantage of being able to inhibit the growth of the SEI. The specific metal is attached to the outer surface of the negative electrode active material, which is expected to reduce the battery resistance.
[0011] However, there are cases where voids are formed inside the negative electrode active material. That is, the negative electrode active material may have not only an external surface but also an internal surface. The internal surface is the surface that contacts the internal voids. The internal surface is not exposed to the outside. The SEI may grow on both the external and internal surfaces. Even if a specific metal is attached only to the external surface, the SEI may grow on the internal surface.
[0012] In the present disclosure, the specific metal is attached to both the external surface and the internal surface. Therefore, the growth of the SEI can be inhibited on both the external surface and the internal surface. By inhibiting the growth of the SEI on the internal surface as well, a further reduction in the battery resistance is expected.
[0013] 2. The specific metal may include at least one selected from the group consisting of potassium (K), rubidium (Rb), barium (Ba), strontium (Sr), calcium (Ca), sodium (Na), magnesium (Mg), aluminum (Al), uranium (U), titanium (Ti), zirconium (Zr), manganese (Mn), zinc (Zn), chromium (Cr), iron (Fe), cadmium (Cd), cobalt (Co), nickel (Ni), tin (Sn), lead (Pb), copper (Cu), mercury (Hg), and silver (Ag).
[0014] 3. The specific metal may include, for example, at least one selected from the group consisting of Fe, Cr, and Ni.
[0015] 4. The ratio of the mass of the specific metal to the mass of the negative electrode active material may be 0.192 to 0.384.
[0016] Hereinafter, the "ratio of the mass of the specific metal to the mass of the negative electrode active material" may be abbreviated as "mass ratio". When the mass ratio is 0.192 or more, it is expected that the resistance reduction effect will be increased. When the mass ratio is 0.384 or less, the occurrence rate of micro-short circuit can be reduced.
[0017] 5. A method for producing a lithium ion battery includes the following steps (a) to (e): (a) A positive electrode including a positive electrode active material is prepared. (b) preparing a negative electrode containing a negative electrode active material; (c) Assembling a lithium ion battery including a positive electrode, a negative electrode, an electrolyte, and the specific metal. (d) subjecting the lithium ion battery to a first charge. (e) After the first charge, the lithium ion battery is subjected to a second charge. Possibilities are formed inside the negative electrode active material. The specific metal has a dissolution potential and a deposition potential. The dissolution potential is lower than the potential at which the positive electrode active material releases Li ions. The deposition potential is higher than the potential at which the negative electrode active material absorbs Li ions. In the above (c), the specific metal is disposed so as to be in electrical contact with the positive electrode. The first charge involves constant voltage charging of the lithium ion battery at a battery voltage where the positive electrode potential is greater than the dissolution potential and the negative electrode potential is greater than the deposition potential. In the second charge, the negative electrode potential is equal to or less than the deposition potential.
[0018] The battery of "1" above can be manufactured by, for example, the manufacturing method of "5" above. In the first charge, the specific metal is oxidized and dissolved on the positive electrode side, so that specific metal ions can be generated. The specific metal ions diffuse to the negative electrode side. In the first charge, the specific metal is difficult to precipitate because the negative electrode potential is higher than the precipitation potential of the specific metal. Therefore, the specific metal ions can diffuse into the voids of the negative electrode active material. After the specific metal ions diffuse into the voids of the negative electrode active material, the second charge is performed so that the negative electrode potential becomes equal to or lower than the precipitation potential. This allows the specific metal to precipitate on both the outer surface and the inner surface of the negative electrode active material.
[0019] Hereinafter, an embodiment of the present disclosure (hereinafter may be abbreviated as "the present embodiment") and an example of the present disclosure (hereinafter may be abbreviated as "the present embodiment") will be described. However, the present embodiment and the example do not limit the technical scope of the present disclosure. [Brief description of the drawings]
[0020] [Figure 1] FIG. 1 is a schematic diagram of a lithium ion battery according to the present embodiment. [Diagram 2] FIG. 2 is a schematic diagram of an electrode assembly. [Diagram 3] FIG. 3 is a schematic flowchart of the method for producing a lithium ion battery in this embodiment. [Figure 4] FIG. 4 is a graph showing an example of the first charge. [Diagram 5] FIG. 5 is a graph showing the battery resistance. [Figure 6] FIG. 6 shows cross-sectional SEM images of negative electrodes No. 2 and 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] <Definitions of terms, etc.> In this specification, the words "comprise," "include," "have," and variations thereof (e.g., "consisting of") are open-ended. The open-ended form may or may not include additional elements in addition to the required elements. The word "consisting of" is closed-ended. However, even in the closed form, additional elements that are normally associated impurities or unrelated to the disclosed technology are not excluded. The word "consisting essentially of..." is semi-closed. In the semi-closed form, the addition of elements that do not substantially affect the basic and novel characteristics of the disclosed technology is permitted.
[0022] In this specification, expressions such as "may" and "can" are used in the permissive sense of "possibly" rather than in the obligatory sense of "must".
[0023] In this specification, a numerical range such as "m to n%" includes an upper limit and a lower limit unless otherwise specified. That is, "m to n%" indicates a numerical range of "m% or more and n% or less". Furthermore, "m% or more and n% or less" includes "more than m% and less than n%". Furthermore, a numerical value arbitrarily selected from within the numerical range may be set as a new upper limit or lower limit. For example, a new numerical range may be set by arbitrarily combining a numerical value within the numerical range with a numerical value described in another part of this specification, in a table, in a figure, or the like.
[0024] In this specification, all numerical values are modified by the term "about". The term "about" may mean, for example, ±5%, ±3%, ±1%, etc. All numerical values may be approximations that may vary depending on the application of the disclosed technology. All numerical values may be expressed in significant figures. Measurements may be average values of multiple measurements. The number of measurements may be three or more, five or more, or ten or more. In general, the more measurements are made, the more reliable the average value is expected to be. Measurements may be rounded off based on the number of significant figures. Measurements may include errors associated with, for example, the detection limit of a measuring device.
[0025] In this specification, when a compound is expressed by a stoichiometric composition formula (e.g., "LiCoO2", etc.), the stoichiometric composition formula is merely a representative example of the compound. The compound may have a non-stoichiometric composition. For example, when lithium cobalt oxide is expressed as "LiCoO2", unless otherwise specified, the lithium cobalt oxide is not limited to the composition ratio of "Li / Co / O=1 / 1 / 2" and may contain Li, Co, and O in any composition ratio. Furthermore, doping, substitution, etc. with trace elements may be allowed.
[0026] In this specification, the order of execution of multiple steps, operations, and the like included in various methods is not limited to the order described unless otherwise specified. For example, multiple steps may proceed simultaneously. For example, multiple steps may be performed in sequence.
[0027] In this specification, "D50" refers to the particle size at which the cumulative frequency from the smaller particle size reaches 50% in the volume-based particle size distribution.
[0028] The "porosity" in this specification can be measured in a cross-sectional image of the negative electrode active material. The cross-sectional image can be obtained by a scanning electron microscope (SEM). The cross-sectional image is binarized to distinguish between solid parts and void parts. In the cross-sectional image, the area of the solid parts and the area of the void parts are measured. The porosity is calculated by the following formula (I).
[0029] φ=S2÷(S1+S2)×100 …(I) φ indicates the porosity (%). S1 indicates the area of the substantial part. S2 indicates the area of the void portion.
[0030] As used herein, an "external surface" refers to the outer surface of an object. An "internal surface" refers to the surface that contacts the interior void of the object.
[0031] As used herein, "electrically in contact" refers to two objects having the same electric potential as a result of the two objects being in direct or indirect contact with each other.
[0032] In this specification, the magnitude of the time rate of current is sometimes represented by the symbol "C." A current of 1 C will discharge the rated capacity of a battery in 1 hour.
[0033] In this specification, "SOC (State Of Charge)" refers to the percentage of the charge capacity at that point in time relative to the fully charged capacity.
[0034] In this specification, the term "ambient temperature" refers to the temperature of the atmosphere around an object. For example, when a battery (object) is placed in a thermostatic chamber, the set temperature of the thermostatic chamber can be considered as the ambient temperature.
[0035] <Lithium-ion battery> FIG. 1 is a schematic diagram of a lithium ion battery according to the present embodiment. Hereinafter, the "lithium ion battery according to the present embodiment" may be abbreviated as "the present battery." The present battery 100 includes a case 90. The case 90 may be made of metal, for example. The case 90 may have any shape. The case 90 may be, for example, rectangular (flattened rectangular parallelepiped) or cylindrical. The case 90 may be, for example, a pouch made of an Al laminate film. The case 90 may be provided with a positive terminal 91 and a negative terminal 92.
[0036] The case 90 houses the electrode assembly 50 and an electrolyte. The electrolyte is impregnated into the electrode assembly 50. A portion of the electrolyte may be stored in the bottom of the case 90. The electrode assembly 50 is connected to a positive electrode terminal 91 and a negative electrode terminal 92.
[0037] FIG. 2 is a schematic diagram of an electrode body. The electrode body 50 includes a positive electrode 10, a separator 30, and a negative electrode 20. The electrode body 50 may have any structure. The electrode body 50 may be, for example, a wound type. The electrode body 50 may include, for example, a laminate 40. The laminate 40 is formed by laminating a positive electrode 10, a separator 30 (first sheet), a negative electrode 20, and a separator 30 (second sheet) in this order. The laminate 40 is wound in a spiral shape to form the electrode body 50. After winding, the electrode body 50 may be formed into a flat shape.
[0038] 《Positive electrode》 The positive electrode 10 may be, for example, a strip-shaped sheet. The positive electrode 10 may include a positive electrode collector and a positive electrode active material layer. The positive electrode collector may include, for example, Al foil or the like. The positive electrode active material layer may be disposed on the surface of the positive electrode collector. The positive electrode active material layer may be disposed on only one side of the positive electrode collector, or may be disposed on both the front and back sides. The positive electrode active material layer includes a positive electrode active material. The positive electrode active material layer may further include, for example, a conductive material, a binder, and the like.
[0039] The positive electrode active material may be, for example, in a particulate form. The positive electrode active material may have a D50 of, for example, 1 to 30 μm.
[0040] The positive electrode active material can release Li ions at a release potential. The release potential is also called a reaction potential. The release potential is, for example, 3.0 V vs. Li / Li + More than 3.2V vs. Li / Li + More than 3.4V vs. Li / Li + The emission potential may be, for example, 3.5 to 4.5 V vs. Li / Li + It is also possible to use "V vs. Li / Li + " indicates the potential with the redox potential of Li as the reference (zero).
[0041] The positive electrode active material may contain at least one selected from the group consisting of, for example, LiCoO2, LiNiO2, LiMnO2, LiMn2O4, Li(NiCoMn)O2, Li(NiCoAl)O2, and LiFePO4. For example, "(NiCoMn)" in "Li(NiCoMn)O2" indicates that the sum of the composition ratios in parentheses is 1. As long as the sum is 1, the amount of each component is arbitrary. Li(NiCoMn)O2 is, for example, Li(Ni 1 / 3 Co 1 / 3 Mn 1 / 3 )O2, Li(Ni 0.5 Co 0.2 Mn 0.3 )O2, Li(Ni 0.8 Co 0.1 Mn 0.1 ) O2, etc.
[0042] The conductive material may include, for example, carbon black. The amount of the conductive material may be, for example, 0.1 to 10 parts by mass with respect to 100 parts by mass of the positive electrode active material. The binder may include, for example, polyvinylidene fluoride (PVDF). The amount of the binder may be, for example, 0.1 to 10 parts by mass with respect to 100 parts by mass of the positive electrode active material.
[0043] 《Negative electrode》 The negative electrode 20 may be, for example, a strip-shaped sheet. The negative electrode 20 may include a negative electrode current collector and a negative electrode active material layer. The negative electrode current collector may include, for example, Cu foil or the like. The negative electrode active material layer may be disposed on the surface of the negative electrode current collector. The negative electrode active material layer may be disposed on only one side of the negative electrode current collector, or may be disposed on both the front and back sides. The negative electrode active material layer includes a negative electrode active material and a specific metal. The negative electrode active material layer may further include, for example, a conductive material, a binder, or the like.
[0044] The negative electrode active material may be, for example, in a particulate form. The negative electrode active material may have a D50 of, for example, 1 to 30 μm.
[0045] The negative electrode active material absorbs Li ions at an absorption potential. The absorption potential is also called a reaction potential. The absorption potential is, for example, 2.0 V vs. Li / Li + It may be less than 1.0V vs.Li / Li + It may be less than 0.5V vs.Li / Li + The absorption potential may be, for example, 0 to 0.3 V vs. Li / Li + may be also possible.
[0046] Examples of the negative electrode active material include graphite, soft carbon, hard carbon, silicon (Si), silicon oxide, silicon-based alloys, Sn, tin oxide, tin-based alloys, and Li4Ti5O 12 may contain at least one selected from the group consisting of:
[0047] A void is formed inside the negative electrode active material. The negative electrode active material may be, for example, hollow particles. The negative electrode active material may be, for example, secondary particles. The secondary particles include a plurality of primary particles. A void may be formed between the primary particles. The negative electrode active material may include, for example, spheroidized graphite. The spheroidized graphite is a secondary particle. The spheroidized graphite includes a plurality of flakes (primary particles). A void may be formed between the flakes. The negative electrode active material may have a porosity of, for example, 5 to 70%, or a porosity of 10 to 50%.
[0048] The specific metal is attached to the external and internal surfaces of the negative electrode active material. The specific metal can inhibit the growth of the SEI. The specific metal has a dissolution potential and a deposition potential. The specific metal can dissolve in the electrolyte at the dissolution potential. The specific metal dissolved in the electrolyte can deposit at the deposition potential. The dissolution potential is lower than the release potential (reaction potential) of the positive electrode active material. The deposition potential is higher than the absorption potential (reaction potential) of the negative electrode active material.
[0049] The difference between the dissolution potential of the specific metal and the release potential of the positive electrode active material may be, for example, 0.01 V or more, or 0.1 V or more. The difference between the dissolution potential and the release potential of the positive electrode active material may be, for example, 0.3 V or less.
[0050] The difference between the deposition potential of the specific metal and the storage potential of the negative electrode active material may be, for example, 0.01 V or more, or 0.1 V or more. The difference between the deposition potential of the specific metal and the storage potential of the negative electrode active material may be, for example, 0.3 V or less.
[0051] The specific metal may penetrate deep into the negative electrode active material. For example, the maximum diameter (d) of the negative electrode active material (particle) is measured in a cross-sectional image of the negative electrode active material. The specific metal may be attached to the inner surface that is 1 / 5d or more away from the surface of the particle toward the center of the particle on the line segment that forms the maximum diameter. The specific metal may be attached to the inner surface that is 2 / 5d or more away from the surface of the particle toward the center of the particle on the line segment that forms the maximum diameter.
[0052] The specific metal may cover 10 to 100% of the internal surface, may cover 30 to 100%, may cover 50 to 100%, or may cover 70 to 100% of the internal surface. The coverage of the internal surface can be measured by the following procedure. In a cross-sectional image of the negative electrode active material, the total length of the contour line of the void is measured. In the same cross-sectional image, the total length of the specific metal (curve) attached to the internal surface is measured. The coverage of the internal surface is calculated by the following formula (II).
[0053] θ = σ2 ÷ σ1 × 100 … (II) θ denotes the coverage (%) of the inner surface. σ1 denotes the total length of the contour of the void. σ2 indicates the total length of the specific metal. Note that the length of the specific metal indicates the length of the specific metal in contact with the void.
[0054] The specific metal may, for example, form a compound. The specific metal may, for example, form a solid solution. The specific metal may, for example, form an intermetallic compound. The specific metal may, for example, form an oxide. The specific metal may, for example, be an alloy. The specific metal may, for example, be an elemental metal. By using the specific metal as an elemental metal, an alloy, or an intermetallic compound, it is expected that the resistance reduction effect will be increased.
[0055] The specific metal may include, for example, at least one selected from the group consisting of K, Rb, Ba, Sr, Ca, Na, Mg, Al, U, Ti, Zr, Mn, Zn, Cr, Fe, Cd, Co, Ni, Sn, Pb, Cu, Hg, and Ag.
[0056] The specific metal may include at least one selected from the group consisting of Fe, Cr, and Ni. Fe, Cr, and Ni are constituent elements of SUS304. SUS304 is often used in battery manufacturing equipment. It has been believed that, for example, small pieces of SUS304 mixed into a battery due to wear of the manufacturing equipment can cause micro-short circuits. For this reason, batteries are usually manufactured so that small pieces of SUS304, Fe, Cr, and Ni, etc. are not mixed into the battery. According to the new findings of the present disclosure, Fe, Cr, and Ni have the advantage of being able to inhibit the growth of SEI. The dissolution potential of SUS304 is 3.5 V vs. Li / Li + The deposition potential of SUS304 is 1.9V vs. Li / Li + It could be.
[0057] The ratio of the mass of the specific metal to the mass of the negative electrode active material (mass ratio) may be, for example, 0.192 to 0.384. When the mass ratio is 0.192 or more, it is expected that the resistance reduction effect is increased. When the mass ratio is 0.384 or less, the occurrence rate of micro-short circuit can be reduced. For example, the mass fraction of the negative electrode active material and the mass fraction of the specific metal can be measured by performing EDX (Energy dispersive X-ray spectroscopy) on a cross-sectional SEM image of the negative electrode active material layer. The mass ratio is obtained by dividing the mass fraction of the specific metal by the mass fraction of the negative electrode active material.
[0058] The conductive material may include, for example, carbon nanotubes (CNTs) and the like. The amount of the conductive material may be, for example, 0.1 to 10 parts by mass with respect to 100 parts by mass of the negative electrode active material. The binder may include, for example, carboxymethyl cellulose (CMC), styrene butadiene rubber (SBR), and the like. The amount of the binder may be, for example, 0.1 to 10 parts by mass with respect to 100 parts by mass of the negative electrode active material.
[0059] <Separator> The separator 30 may be, for example, a strip-shaped film. The separator 30 is porous. The separator 30 is permeable to an electrolyte. The separator 30 separates the positive electrode 10 and the negative electrode 20. The separator 30 is electrically insulating. The separator 30 may contain, for example, a polyolefin resin. The polyolefin resin may contain, for example, at least one selected from the group consisting of polyethylene (PE) and polypropylene (PP). The separator 30 may have, for example, a single-layer structure. The separator 30 may be, for example, substantially composed of a PE layer. The separator 30 may have, for example, a multi-layer structure. The separator may be formed by laminating, for example, a PP layer, a PE layer, and a PP layer in this order. For example, a heat-resistant layer (ceramic particle layer) or the like may be formed on the surface of the separator 30.
[0060] 《Electrolyte》 The electrolyte includes a solvent and a Li salt. The solvent is aprotic. The solvent may include any component. The solvent may include at least one selected from the group consisting of ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), 1,2-dimethoxyethane (DME), methyl formate (MF), methyl acetate (MA), methyl propionate (MP), and γ-butyrolactone (GBL).
[0061] The Li salt is a supporting electrolyte. The Li salt is dissolved in a solvent. The Li salt may include at least one selected from the group consisting of LiPF6, LiBF4, and LiN(FSO2)2. The Li salt may have a molar concentration of, for example, 0.5 to 2.0 mol / L, or 0.8 to 1.2 mol / L.
[0062] The electrolytic solution may further contain any additive in addition to the solvent and the Li salt. For example, the electrolytic solution may contain 0.01 to 5% by mass of the additive. The additive may contain at least one selected from the group consisting of vinylene carbonate (VC), vinyl ethylene carbonate (VEC), and the like.
[0063] <Lithium-ion battery manufacturing method> 3 is a schematic flow chart of the method for producing a lithium ion battery in this embodiment. Hereinafter, the "method for producing a lithium ion battery in this embodiment" may be abbreviated as "this production method". This production method includes "(a) preparation of a positive electrode", "(b) preparation of a negative electrode", "(c) assembly", "(d) first charging", and "(e) second charging". This production method may further include, for example, "(f) aging" or the like.
[0064] (a) Preparation of the positive electrode The manufacturing method includes preparing a positive electrode 10 including a positive electrode active material. For example, a positive electrode active material layer may be formed by applying a slurry including the positive electrode active material to the surface of a positive electrode current collector.
[0065] In this manufacturing method, the specific metal is disposed so as to be in electrical contact with the positive electrode 10. The specific metal may be added to the positive electrode 10 in advance. For example, a powder of the specific metal may be added to the slurry. For example, small pieces of the specific metal may be placed on the surface of the positive electrode active material layer.
[0066] (b) Preparation of the negative electrode The manufacturing method includes preparing a negative electrode 20 including a negative electrode active material. For example, a slurry including the negative electrode active material may be applied to a surface of a negative electrode current collector to form a negative electrode active material layer.
[0067] (c) Assembly The manufacturing method includes assembling a battery 100 including a positive electrode 10, a negative electrode 20, an electrolyte, and a specific metal. For example, an electrode assembly 50 may be formed including a positive electrode 10, a separator 30, and a negative electrode 20. The specific metal may be disposed at a position where it contacts the positive electrode 10 when the electrode assembly 50 is assembled.
[0068] The electrode body 50 is housed in the case 90. An electrolyte is poured into the case 90. The case 90 may be sealed at this point, for example. The case 90 may be sealed after "(d) first charging" or after "(e) second charging", for example. This is because gas may be generated during the initial charging.
[0069] 《(d) First charging》 This manufacturing method includes subjecting the battery 100 to a first charge. In the first charge, constant voltage (CV) charging is performed. Hereinafter, the battery voltage during CV charging is also referred to as "CV voltage". For example, CC charging may be performed until the battery voltage reaches the CV voltage. In other words, the first charge may include CCCV charging. Hereinafter, the current during CC charging is also referred to as "CC current". The CC current in the first charge may be, for example, 0.1 to 1 C, or 0.3 to 0.7 C.
[0070] FIG. 4 is a graph showing an example of the first charge. The vertical axis of the graph is the electrode potential [unit: V vs. Li / Li + ] or battery voltage [unit: V]. The horizontal axis of the graph indicates charging time [unit: h]. If the dissolution potential of a specific metal is 3.5V vs. Li / Li + The deposition potential of a specific metal is 1.9V vs. Li / Li + For example, the CV voltage is set to 1.5 V. During CV charging, the positive electrode potential is the dissolution potential (3.5 V vs. Li / Li + ). Therefore, it is considered that the specific metal in electrical contact with the positive electrode 10 is oxidized and dissolved. The specific metal ions are generated by the oxidization and dissolution of the specific metal. The specific metal ions are attracted to the negative electrode 20, which has a lower potential. During CV charging, the negative electrode potential is higher than the deposition potential (1.9 V vs. Li / Li + ) is higher. Therefore, it is considered that the specific metal ions that reach the negative electrode 20 are unlikely to precipitate. It is considered that the specific metal ions can penetrate into the inside (voids) of the negative electrode active material without being precipitated.
[0071] The CV voltage may be, for example, 1.1 to 1.8V, or 1.2 to 1.5V.
[0072] The CV charging may be carried out for, for example, 1 to 48 hours, or 8 to 24 hours.
[0073] During the first charge, the battery 100 may be heated. Heating may, for example, promote the diffusion of specific metal ions. The ambient temperature during the first charge may be, for example, 40 to 70°C, or 55 to 65°C.
[0074] 《(e) Second charging》 The present manufacturing method includes subjecting the battery 100 to a second charge after the first charge. In the second charge, the battery 100 is charged so that the negative electrode potential becomes equal to or lower than the deposition potential. This causes the specific metal to deposit on the negative electrode 20. Since the specific metal ions have penetrated into the negative electrode active material in the first charge, the specific metal can deposit on both the outer and inner surfaces of the negative electrode active material.
[0075] The ambient temperature during the second charging may be, for example, room temperature (25±10° C.). The second charging may include, for example, CCCV charging. The CC current may be, for example, 0.1 to 10 C, or 0.5 to 5 C. During the second charging, the battery 100 may be charged to, for example, 50 to 100% SOC, 70 to 100% SOC, or 80 to 90% SOC.
[0076] (f) Aging The present manufacturing method may include aging after the second charge. For example, the present battery 100 may be stored in a high temperature environment. The ambient temperature during aging may be, for example, 40 to 70° C., or 55 to 65° C. The storage time (aging time) may be, for example, 1 to 48 hours, or 18 to 24 hours. EXAMPLES
[0077] <Production of test batteries> Test batteries No. 1 to 3 were produced as follows. Hereinafter, for example, "test battery No. 1" may be abbreviated as "No. 1."
[0078] No.1 "(a) Preparation of the positive electrode" and "(b) Preparation of the negative electrode" were carried out (see Figure 3). In "(c) Assembly", the test battery was assembled in a way that did not allow specific metals to be mixed inside.
[0079] “(e) Second charging” was performed up to 90% SOC under the following conditions: Ambient temperature: 25℃ Charging mode: CCCV CC current: 5C Cut-off current: 0.2C
[0080] After the second charge, “(f) Aging” was carried out under the following conditions. Ambient temperature: 60℃ Aging time: 22 hours
[0081] As a result of the above, No. 1 was manufactured. It is believed that No. 1 does not contain specific metals. In the manufacturing process of No. 1, "(d) the first charging" was not carried out (see Figure 3).
[0082] No.2 As the specific metal, a small piece of SUS304 was prepared. SUS304 contains Fe, Cr, and Ni.
[0083] A small piece of a specific metal was placed on the surface of the positive electrode. After the specific metal was placed, an electrode body was formed. Except for this, "(c) Assembly" was carried out in the same way as No.1.
[0084] After assembling the test battery, "(e) the second charging" and "(f) aging" were carried out in the same manner as for No.1. From the above, No.2 was manufactured. In the manufacturing process of No.2, "(d) the first charging" was not carried out (see Figure 3).
[0085] No.3 Similar to No. 2, a test battery containing specific metals was constructed.
[0086] “(d) The first charging” was carried out under the following conditions: Ambient temperature: 60℃ Charging mode: CCCV CC current: 0.5C CV voltage: 1.5V Cutting time: 24 hours
[0087] After the first charge, "(e) the second charge" and "(f) aging" were carried out in the same way as for No. 1 and No. 2. From the above, No. 3 was manufactured.
[0088] <Evaluation> The SOC of the test battery was adjusted to 10%. The test battery was discharged at a current of 5C at an ambient temperature of 25°C. The voltage drop 10 seconds after the start of discharge was measured. The battery resistance (DC-IR) was calculated from the current and the voltage drop.
[0089] FIG. 5 is a graph showing battery resistance. The vertical axis of the graph shows battery resistance. The battery resistance in FIG. 5 is a relative value with the battery resistance of No. 1 set at 100%. No. 2 had a battery resistance reduced by 4.3% compared to No. 1. No. 3 had a battery resistance reduced by 7.8% compared to No. 1.
[0090] Figure 6 shows cross-sectional SEM images of negative electrodes No. 2 and 3. Differences in brightness within the images indicate differences in composition. The black areas are thought to represent voids. The gray areas are thought to represent negative electrode active material 2 (graphite). The white areas are thought to represent specific metals 3 (Fe, Cr, Ni).
[0091] In No. 2, the specific metal 3 was attached to the outer surface of the negative electrode active material 2. It is believed that the growth of the SEI on the outer surface was inhibited by covering the outer surface with the specific metal 3, resulting in a 4.3% reduction in battery resistance. In No. 2, the specific metal 3 was not attached to the inner surface of the negative electrode active material 2.
[0092] In No. 3, the specific metal 3 was attached to both the external and internal surfaces of the negative electrode active material 2. In No. 3, it is believed that the specific metal ions penetrated into the inside of the negative electrode active material 2 due to the first charge. It is believed that the growth of SEI was inhibited on both the external and internal surfaces by covering both the external and internal surfaces with the specific metal 3, resulting in a 7.8% reduction in battery resistance.
[0093] The present embodiment and the present embodiment are illustrative in all respects. The present embodiment and the present embodiment are not restrictive. The technical scope of the present disclosure includes all modifications within the meaning and scope equivalent to the description of the claims. For example, it is also intended from the beginning that any configuration may be extracted from the present embodiment and the present embodiment, and that they may be arbitrarily combined. [Explanation of symbols]
[0094] 2 negative electrode active material, 3 specific metal, 10 positive electrode, 20 negative electrode, 30 separator, 40 laminate, 50 electrode body, 90 case, 91 positive electrode terminal, 92 negative electrode terminal, 100 lithium ion battery.
Claims
[Claim 1] (a) providing a positive electrode comprising a positive electrode active material; (b) providing a negative electrode comprising a negative electrode active material; (c) assembling a lithium ion battery including the positive electrode, the negative electrode, an electrolyte, and a specific metal; (d) subjecting the lithium ion battery to a first charge; and (e) subjecting the lithium ion battery to a second charge after the first charge. Including, A void is formed inside the negative electrode active material, The specific metal has a dissolution potential and a deposition potential, the dissolution potential is lower than a potential at which the positive electrode active material releases lithium ions, the deposition potential is higher than a potential at which the negative electrode active material absorbs lithium ions, In the (c), the specific metal is disposed so as to be in electrical contact with the positive electrode; The first charging includes subjecting the lithium ion battery to constant voltage charging at a battery voltage at which a positive electrode potential is higher than the dissolution potential and a negative electrode potential is higher than the precipitation potential, In the second charge, the negative electrode potential becomes equal to or lower than the deposition potential. How lithium-ion batteries are manufactured.
Citation Information
Patent Citations
Manufacturing method of non-aqueous electrolyte secondary battery
JP2005243537A
Anode, and secondary battery
JP2010147005A
Negative electrode active material for nonaqueous secondary battery and nonaqueous secondary battery
JP2012094364A
Lithium ion secondary battery
JP2013246992A
Lithium ion secondary battery
JP2014082084A