Carbon electrode materials and redox batteries
A carbon electrode material with specific properties reduces cell resistance and improves energy efficiency in redox batteries by using small carbon particles and fibers bound with a carbonaceous material, enhancing performance in redox batteries and related systems.
Patent Information
- Application Number
- JP2023132717
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-13
- Filing Date
- 2023-08-16
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-03-12
AI Technical Summary
Existing redox batteries require further reduction in cell resistance and the use of cheaper electrode materials to enhance battery energy efficiency.
A carbon electrode material composed of carbon particles with small particle size and low crystallinity, carbon fibers, and a binding carbonaceous material, satisfying specific conditions such as particle size, crystallinity ratios, and oxygen content, is used for the negative electrode to reduce cell resistance and improve battery efficiency.
The carbon electrode material achieves lower cell resistance and enhances battery energy efficiency, suitable for redox batteries, lithium capacitors, and fuel cell systems.
Smart Images

Figure 0007552813000009 
Figure 0007552813000008 
Figure 0007552813000007
Abstract
Description
[Technical field]
[0001] The present invention relates to a carbon electrode material used in the negative electrode of a redox battery, and more particularly to a carbon electrode material which provides excellent energy efficiency for the entire redox battery. [Background technology]
[0002] A redox battery is a battery that utilizes the oxidation-reduction of redox ions in an aqueous solution. Because the reaction is mild and occurs only in the liquid phase, it is an extremely safe, large-capacity storage battery.
[0003] As shown in Figure 1, the main components of a redox battery are external tanks 6, 7 that store electrolytes (positive electrode electrolyte, negative electrode electrolyte), and an electrolytic cell EC. In the electrolytic cell EC, an ion exchange membrane 3 is disposed between opposing current collectors 1, 1. In the redox battery, electrochemical energy conversion, i.e., charging and discharging, takes place on an electrode 5 incorporated in the electrolytic cell EC while pumps 8, 9 send electrolyte containing active materials from the external tanks 6, 7 to the electrolytic cell EC. The electrode 5 is made of a carbon material that is chemically resistant, electrically conductive, and liquid permeable.
[0004] The electrolyte used in redox batteries is typically an aqueous solution containing metal ions whose valence changes due to oxidation and reduction. The electrolyte has changed from a type that used an aqueous solution of iron hydrochloric acid for the positive electrode and an aqueous solution of chromium hydrochloric acid for the negative electrode to a type that uses an aqueous solution of vanadium sulfuric acid, which has a high electromotive force, for both electrodes, resulting in a higher energy density.
[0005] In the case of a redox battery that uses an acidic aqueous solution of vanadium oxysulfate as the positive electrode electrolyte and vanadium sulfate as the negative electrode electrolyte, V 2+ The electrolyte containing V is supplied to the negative electrode side liquid passage, and V is supplied to the positive electrode side liquid passage. 5+ The electrolyte containing oxygen (actually ions) is supplied. In the negative electrode side, the electrolyte is V 2+ releases electrons and V 3+The emitted electrons pass through an external circuit and reach the positive electrode side of the three-dimensional electrode, V 5+ V 4+ (Actually, ions containing oxygen) are reduced to SO4 in the negative electrolyte. 2- In the positive electrode electrolyte, SO4 2- becomes excessive, so it passes through the ion exchange membrane and 2- moves from the positive electrode to the negative electrode, maintaining the charge balance. Or, H + The charge balance can also be maintained by the transfer of charge from the negative electrode to the positive electrode through the ion exchange membrane. During charging, the reverse reaction to the discharge occurs.
[0006] The electrode material for a redox battery is particularly required to have the following properties:
[0007] 1) No side reactions other than the target reaction occur (high reaction selectivity), specifically, current efficiency (η I ) is high. 2) High electrode reaction activity, specifically, low cell resistance (R). In other words, low voltage efficiency (η V ) is high. 3) Battery energy efficiency (η E ) is high. η E = η I ×η V 4) Little deterioration with repeated use (long life), specifically, battery energy efficiency (η E ) decrease is small.
[0008] The development of electrolytes for use in redox batteries has been actively promoted, and as an electrolyte that has an even higher electromotive force than vanadium-based electrolytes and can be stably and inexpensively supplied, for example, Patent Document 1 proposes one that uses manganese in the positive electrode and chromium, vanadium, and titanium in the negative electrode (for example, a manganese-titanium-based electrolyte). [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Japanese Patent Publication No. 2012-204135 Summary of the Invention [Problem to be solved by the invention]
[0010] In order to promote the widespread use of redox batteries, there is a demand for electrode materials with even lower resistance and at lower cost.
[0011] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a carbon electrode material to be used in the negative electrode of a redox battery, which can reduce the cell resistance during initial charge and discharge and improve the battery energy efficiency. [Means for solving the problem]
[0012] The present inventors have conducted research to solve the above problems, and have found that a low-resistance electrode material can be obtained by using carbon particles (excluding graphite) with small particle size and low crystallinity, and a carbonaceous material (C) with high crystallinity for carbonaceous fibers (A) under specified conditions, and have completed the present invention.
[0013] The present invention is configured as follows.
[0014] 1. A carbon electrode material used in the negative electrode of a redox battery, The carbon electrode material comprises carbonaceous fibers (A), carbon particles other than graphite particles (B), and a carbonaceous material (C) that binds them together; A carbon electrode material for a redox battery, characterized by satisfying the following requirements: (1) The particle size of carbon particles (B) other than graphite particles is 1 μm or less, (2) In carbon particles (B) other than graphite particles, when the size of the crystallite in the c-axis direction determined by X-ray diffraction is Lc(B), Lc(B) is 10 nm or less; (3) In the carbonaceous fiber (A) and the carbonaceous material (C), the sizes of the crystallites in the c-axis direction determined by X-ray diffraction are Lc(A) and Lc(C), respectively, and Lc(C) / Lc(A) is 1.0 to 5.0. (4) The mesopore specific surface area determined by the nitrogen gas adsorption method is 30 m 2 / g or less, (5) The number of bonded oxygen atoms on the surface of the carbon electrode material is 1% or more of the total number of carbon atoms on the surface of the carbon electrode material. 2. The mass ratio of the carbonaceous material (C) to the carbon particles (B) is 0.2 to 10. 1. The carbon electrode material according to claim 1. 3. The BET specific surface area calculated from the amount of nitrogen adsorption is 50m 2 3. The carbon electrode material according to claim 1 or 2, wherein the carbon electrode material has a viscosity of less than 1 / g. 4. The carbon electrode material according to any one of 1 to 3 above, wherein a water drop passes through the material at a rate of 0.5 mm / sec or more. 5. A redox flow battery comprising the carbon electrode material according to any one of 1 to 4 above as a negative electrode. 6. A method for producing a carbon electrode material according to any one of 1 to 4 above, A step of attaching carbon particles (B) other than the graphite particles and a carbonaceous material (C) before carbonization to the carbonaceous fibers (A); a carbonization step of heating the product after the impregnation in an inert gas atmosphere at a temperature of 500°C or more and less than 2000°C; A primary oxidation process in which oxidation is performed at a temperature of 500 to 900°C under dry conditions; A graphitization process in which the material is heated at a temperature of 1300 to 2300°C under an inert gas atmosphere; A secondary oxidation process in which oxidation is performed at a temperature of 500 to 900 ° C under dry conditions; A method for producing a carbon electrode material, comprising the steps of: Effect of the Invention
[0015] According to the present invention, a carbon electrode material for use in the negative electrode of a redox battery can be obtained, which has excellent battery energy efficiency by reducing the cell resistance during initial charging and discharging. The carbon electrode material of the present invention is suitably used in flow-type and non-flow-type redox batteries, or redox batteries combined with a lithium, capacitor, or fuel cell system. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a schematic diagram of a redox battery. [Diagram 2] FIG. 2 is an exploded perspective view of a liquid flow-type electrolytic cell having three-dimensional electrodes that is preferably used in the present invention. [Diagram 3] FIG. 3 is an SEM photograph (magnification: 100 times) of No. 5 in Table 3A (an example satisfying the requirements of the present invention) in Example 1 described later. [Figure 4] FIG. 4 is an SEM photograph (magnification: 100 times) of No. 10 (a comparative example not satisfying the requirements of the present invention) in Table 3A in Example 1 described later. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] In order to provide a carbon electrode material with reduced cell resistance during initial charge and discharge, the inventors have investigated the use of carbon particles other than graphite particles, and have found that the use of carbon particles with small particle size and low crystallinity increases the reaction surface area, making it easier to provide oxygen functional groups, increasing reaction activity, and providing low resistance.
[0018] Specifically, in the present invention, carbon particles other than graphite particles are adopted that satisfy the following requirements (1) and (2). (1) The particle size of carbon particles (B) other than graphite particles is 1 μm or less, (2) In carbon particles (B) other than graphite particles, when the size of the crystallite in the c-axis direction determined by X-ray diffraction is defined as Lc(B), Lc(B) is 10 nm or less. As mentioned above, the use of small-grained carbon particles increases the reaction surface area, making it possible to reduce the resistance.Furthermore, as mentioned above, the use of low-crystalline carbon particles makes it easier to introduce oxygen functional groups, improving the reaction activity, making it possible to further reduce the resistance.
[0019] Furthermore, in the present invention, the carbonaceous material (C) is a carbonaceous material having adhesive properties that bind both the carbonaceous fibers (A) and the carbon particles (B) other than graphite particles, and is highly crystalline relative to the carbonaceous fibers (A) and satisfies the following requirement (3). (3) When the sizes of crystallites in the c-axis direction of the carbonaceous fiber (A) and the carbonaceous material (C) as determined by X-ray diffraction are Lc(A) and Lc(C), respectively, Lc(C) / Lc(A) is 1.0 to 5. Here, "binding both the carbonaceous fibers (A) and the carbon particles other than graphite particles (B)" (in other words, the carbonaceous material used in the present invention acts as a binder for the carbonaceous fibers and the carbon particles other than graphite particles) means that the carbonaceous material strongly binds the surfaces and interiors of the carbonaceous fibers and the carbon particles other than graphite particles (including between the carbonaceous fibers and between the carbon particles other than graphite particles), so that, when viewed as a whole electrode material, the carbonaceous fibers are covered by the carbonaceous material while the surfaces of the carbon particles other than graphite particles are exposed. However, it is preferable that the carbonaceous material does not become a coating state after binding. Here, "not becoming a coating state" means that the carbonaceous material (C) does not form a web state such as a whole web or a webbed state between the fibers of the carbonaceous fiber (A). If a coating state is formed, the permeability of the electrolyte is deteriorated, and the reaction surface area of the carbon particles cannot be effectively utilized.
[0020] For reference, Fig. 3 shows an SEM photograph showing a state in which both the carbonaceous fiber (A) and the carbon particles (B) other than the graphite particles are bound together. Fig. 3 is an SEM photograph (magnification 100 times) of No. 5 (an example satisfying the requirements of the present invention) in Table 3A in Example 1 described later. Fig. 3 shows that the surfaces and interiors of the carbonaceous fiber (A) and the carbon particles (B) other than the graphite particles are strongly bound together by the carbonaceous material (C), and the carbonaceous fiber (A) is covered by the carbonaceous material (C), while the surfaces of the carbon particles (B) other than the graphite particles are exposed. On the other hand, Fig. 4 is an SEM photograph showing a state in which both the carbonaceous fibers (A) and the carbon particles other than graphite particles (B) are not bonded together. Fig. 4 is an SEM photograph (magnification 100 times) of No. 10 (a comparative example not satisfying the requirements of the present invention) in Table 3A in Example 1 described later.
[0021] In addition, the carbonaceous material strongly bonds between the carbonaceous fibers via carbon particles other than graphite particles, and therefore forms an efficient conductive path between the carbon particles and the carbonaceous fibers. It is necessary to increase the content ratio of the carbonaceous material relative to the total amount of the carbonaceous fibers, carbon particles other than graphite particles, and the carbonaceous material in order to form a conductive path, and therefore in the present invention, the above content is preferably 14.5% or more. In contrast, the content of the carbonaceous material in the examples of the above-mentioned Patent Document 1 is at most 14.4%, which is less than the present invention, and in this respect, the two differ. In the first place, Patent Document 1 is based on the idea that only the parts where the carbonaceous fibers and the carbon fine particles were originally in contact can be fixed (adhered), and the carbonaceous material used is only recognized as being sufficient to act as a partial adhesive. Furthermore, Patent Document 1 does not specifically state the crystallinity of the carbonaceous material to be bonded, but in order to form an excellent conductive path, if a carbonaceous material with high crystallinity is used with respect to the carbonaceous fibers as in the present invention, the electronic conductivity is increased, and more efficient electron transfer is possible.
[0022] Furthermore, the carbon electrode material of the present invention satisfies the following requirements (4) and (5). (4) The mesopore specific surface area determined by the nitrogen gas adsorption method is 30 m 2 / g or less. (5) The number of bonded oxygen atoms on the surface of the carbon electrode material is 1% or more of the total number of carbon atoms on the surface of the carbon electrode material.
[0023] As described in detail later, the mesopore specific surface area defined in the above (4) is a measurement target of the mesopore region having a diameter of 2 to 50 nm, and is generally used as a more effective indicator of the performance of an electrode material than the BET specific surface area which is a measurement target of all pores.
[0024] In addition, the above (5) allows oxygen atoms to be introduced into the edge planes and defect structures of carbon. As a result, the introduced oxygen atoms are generated as reactive groups such as carbonyl groups, quinone groups, lactone groups, and free radical oxides on the surface of the electrode material, and these reactive groups contribute greatly to the electrode reaction, making it possible to obtain sufficiently low resistance.
[0025] Since the electrode material of the present invention is constructed as described above, it is possible to obtain an electrode having high reactivity, low resistance, and low cost.
[0026] Hereinafter, the present invention will be described in detail with reference to FIG.
[0027] FIG. 2 is an exploded perspective view of a liquid flow-type electrolytic cell suitable for use in the present invention. In the electrolytic cell of FIG. 2, an ion exchange membrane 3 is disposed between two opposing current collectors 1, 1, and electrolyte passages 4a, 4b are formed on both sides of the ion exchange membrane 3 along the inner surfaces of the current collectors 1, 1 by spacers 2. An electrode material 5 is disposed in at least one of the liquid passages 4a, 4b. The current collector 1 is provided with a liquid inlet 10 and a liquid outlet 11 for the electrolyte. As shown in FIG. 2, when the electrode is composed of the electrode material 5 and the current collector 1, and the electrolyte passes through the electrode material 5 (three-dimensional electrode structure), the charge / discharge efficiency can be improved by using the entire pore surface of the electrode material 5 as an electrochemical reaction field while the current collector 1 ensures the transport of electrons. As a result, the charge / discharge efficiency of the electrolytic cell is improved.
[0028] As described above, the electrode material 5 of the present invention is an electrode material having carbonaceous fibers (A) as a substrate, in which carbon particles other than graphite particles (A) are supported by highly crystalline carbonaceous material (C), and satisfies the above requirements (1) to (5). Details of each requirement are as follows.
[0029] [Carbon fiber (A)] The carbonaceous fiber used in the present invention is a fiber obtained by subjecting an organic fiber precursor to a heat carbonization treatment (details will be described later), and means a fiber composed of 90% or more by mass of carbon (JIS L 0204-2). As the precursor of the organic fiber that is the raw material of the carbonaceous fiber, acrylic fibers such as polyacrylonitrile; phenol fibers; PBO fibers such as polyparaphenylene benzobisoxazole (PBO); aromatic polyamide fibers; pitch fibers such as isotropic pitch fibers, anisotropic pitch fibers, and mesophase pitch; cellulose fibers; and the like can be used. Among them, from the viewpoint of excellent strength and elastic modulus, etc., as the precursor of the organic fiber, acrylic fibers, phenol fibers, cellulose fibers, isotropic pitch fibers, and anisotropic pitch fibers are preferable, and acrylic fibers are more preferable. The acrylic fiber is not particularly limited as long as it contains acrylonitrile as the main component, but the content of acrylonitrile in the raw material monomer forming the acrylic fiber is preferably 95% by mass or more, and more preferably 98% by mass or more.
[0030] The mass average molecular weight of the organic fiber is not particularly limited, but is preferably from 10,000 to 100,000, more preferably from 15,000 to 80,000, and even more preferably from 20,000 to 50,000. The mass average molecular weight can be measured by a method such as gel permeation chromatography (GPC) or solution viscosity.
[0031] The average fiber diameter of the carbonaceous fibers is preferably 0.5 to 40 μm. If the average fiber diameter is smaller than 0.5 μm, the liquid permeability is deteriorated. On the other hand, if the average fiber diameter is larger than 40 μm, the reaction surface area of the fiber portion is reduced, and the cell resistance is increased. In consideration of the balance between the liquid permeability and the reaction surface area, the average fiber diameter is more preferably 3 to 20 μm.
[0032] In the present invention, it is preferable to use the above carbonaceous fiber structure as a substrate, which improves strength and facilitates handling and processing. Specific examples of the above structure include spun yarn, filament bundle yarn, nonwoven fabric, knitted fabric, woven fabric, special woven fabric described in JP-A-63-200467, etc., which are sheet-like products made of carbonaceous fibers, and paper made of carbon fibers. Among these, nonwoven fabric, knitted fabric, woven fabric, special woven fabric, and paper made of carbon fibers are more preferable in terms of handling, processing, manufacturability, etc.
[0033] When nonwoven fabric, knitted fabric, woven fabric, etc. are used, the average fiber length is preferably 30 to 100 mm. When paper made of carbon fiber is used, the average fiber length is preferably 5 to 30 mm. By keeping the length within the above range, a uniform fiber structure can be obtained.
[0034] As described above, the carbonaceous fiber is obtained by subjecting an organic fiber precursor to a thermal carbonization treatment, and the "thermal carbonization treatment" preferably includes at least a flame-retardant process and a carbonization (calcination) process. However, the carbonization process does not necessarily have to be performed after the flame-retardant process as described above, and the carbonization process may be performed after attaching graphite particles and a carbonaceous material to the flame-retardant fiber as described in the examples below, in which case the carbonization process after the flame-retardant process can be omitted.
[0035] Among these, the flame-retarding step refers to a step of heating an organic fiber precursor in an air atmosphere at a temperature of preferably 180°C or more and 350°C or less to obtain a flame-retarded organic fiber. The heat treatment temperature is more preferably 190°C or more, and even more preferably 200°C or more. Also, it is preferably 330°C or less, and even more preferably 300°C or less. By heating within the above temperature range, the organic fiber does not undergo thermal decomposition, and the nitrogen and hydrogen contents in the organic fiber can be reduced while maintaining the form of the carbonaceous fiber, thereby improving the carbonization rate. During the flame-retarding step, the organic fiber may be thermally shrunk and the molecular orientation may be destroyed, resulting in a decrease in the conductivity of the carbonaceous fiber. Therefore, it is preferable to perform the flame-retarding treatment on the organic fiber under tension or stretching, and it is more preferable to perform the flame-retarding treatment under tension.
[0036] The carbonization step refers to a step of heating the flame-retardant organic fiber obtained as described above in an inert atmosphere (preferably a nitrogen atmosphere) at a temperature of preferably 1000°C or higher and 2000°C or lower to obtain a carbonaceous fiber. The heating temperature is more preferably 1100°C or higher, and even more preferably 1200°C or higher. Also, it is more preferably 1900°C or lower. By carrying out the carbonization step within the above temperature range, the carbonization of the organic fiber progresses, and a carbonaceous fiber having a pseudo-graphite crystal structure can be obtained.
[0037] Since organic fibers have different crystallinity, the heating temperature in the carbonization step can be selected according to the type of organic fiber used as the raw material. For example, when an acrylic resin (preferably polyacrylonitrile) is used as the organic fiber, the heating temperature is preferably 800°C or higher and 2000°C or lower, and more preferably 1000°C or higher and 1800°C or lower.
[0038] The flameproofing step and the carbonization step are preferably carried out continuously, and the temperature rise rate when raising the temperature from the flameproofing temperature to the carbonization temperature is preferably 20° C. / min or less, more preferably 15° C. / min or less. By setting the temperature rise rate within the above range, it is possible to obtain a carbonaceous fiber that retains the shape of the organic fiber and has excellent mechanical properties. In addition, the lower limit of the temperature rise rate is preferably 5° C. / min or more, taking into account the mechanical properties, etc.
[0039] As described in detail in the section on carbonaceous material (C) below, the electrode material of the present invention satisfies Lc(C) / Lc(A) of 1.0 to 5 when the sizes of the crystallites in the c-axis direction in the carbonaceous fiber (A) and the carbonaceous material (C) determined by X-ray diffraction are Lc(A) and Lc(C), respectively, as specified in the above (3). Therefore, in the present invention, Lc(A) in the carbonaceous fiber (A) is not particularly limited as long as the above (3) is satisfied, but Lc(A) is preferably 1 to 6 nm. This effectively exerts the effects of moderate electronic conductivity, oxidation resistance to sulfuric acid solvents, and ease of imparting oxygen functional groups. The measurement method of Lc(A) and Lc(C) will be described in detail in the section on examples below.
[0040] [Carbon particles other than graphite particles (B)] In the present invention, the "carbon particles other than graphite particles" are useful for increasing the reaction surface area and realizing low resistance. In the present invention, in order to reduce resistance, those that satisfy the above (1) and (2) are used.
[0041] First, the particle size of the "carbon particles other than graphite particles" used in the present invention is 1 μm or less, as specified in (1) above, and preferably 0.5 μm or less. If the particle size exceeds 1 μm, the reaction surface area decreases and the resistance increases. Here, "particle size" means the average particle size (D50) at the median 50% diameter in the particle size distribution obtained by dynamic light scattering or the like. The carbon particles other than graphite particles may be commercially available products, in which case the particle size listed in the catalog can be used. The preferred lower limit is 0.005 μm or more.
[0042] The BET specific surface area of the "carbon particles other than graphite particles" used in the present invention, calculated from the nitrogen adsorption amount, is 20 m 2 / g or more is preferable, and 30m 2 / g or more is more preferable, and 40m 2 / g or more is more preferable. 2 When the surface area is less than 1000 m / g, the edge exposure of the carbon particles is reduced, and the contact area with the electrolyte is also reduced, making it impossible to obtain the desired low resistance. Although the upper limit is not particularly limited from the above viewpoint, the viscosity of the dispersion solution is likely to increase in bulky particles with a large surface area, and the processability into sheets and the like is deteriorated. 2 The "BET specific surface area determined from the amount of nitrogen adsorption" means the specific surface area calculated from the amount of gas molecules adsorbed when nitrogen molecules are adsorbed on solid particles.
[0043] Furthermore, the Lc(B) of the "carbon particles other than graphite particles" used in the present invention is 10 nm or less as specified in (2) above. When highly crystalline carbon particles with Lc(B) exceeding 10 nm are used, it is difficult to introduce oxygen functional groups, so the affinity of the carbon particles in the vicinity thereof to the aqueous electrolyte decreases, the reaction activity decreases, and the resistance increases. It is preferably 6 nm or less. The lower limit is not particularly limited from the above viewpoint, but is preferably about 0.5 nm or more in consideration of oxidation resistance to the electrolyte. The method for measuring Lc(B) and La(B) will be described in detail in the Examples section below.
[0044] As the "carbon particles other than graphite particles" used in the present invention, for example, carbon blacks such as acetylene black (acetylene soot), oil black (furnace black, oil soot), ketjen black, and gas black (gas soot) are often used, which have high reactivity and specific surface area and low crystallinity. In addition to the above, carbon nanotubes (CNTs), carbon nanofibers, carbon aerogels, mesoporous carbon, graphene, graphene oxide, N-doped CNTs, boron-doped CNTs, fullerenes, etc. are also included. From the viewpoint of raw material prices, etc., carbon blacks are preferably used.
[0045] The content of the "carbon particles other than graphite particles" used in the present invention is preferably 5% or more, preferably 10% or more, in terms of mass ratio to the total amount of the carbonaceous fiber (A), the carbon particles other than graphite particles (B), and the carbonaceous material (C) described below. As a result, the carbon particles other than graphite particles are bound by the carbonaceous material, and the resistance is reduced. However, if the amount of the carbon particles (B) other than graphite particles is excessive, the binding by the carbonaceous material becomes insufficient, causing particles to fall off, and the liquid permeability is deteriorated due to the improvement of the packing density, so that the desired low resistance cannot be obtained. Therefore, the upper limit is preferably about 90% or less. The content of the carbonaceous fiber (A) used to calculate the above content is the content of the structure when a structure such as a nonwoven fabric is used as the substrate.
[0046] In the present invention, the mass ratio of the carbonaceous material (C) to the carbon particles (B) other than graphite particles is preferably 0.2 to 10, more preferably 0.3 to 7. If the ratio is less than 0.2, many carbon particles other than graphite particles fall off, and the carbon particles are not sufficiently bonded to the carbonaceous material. On the other hand, if the ratio exceeds 10, the carbon edge surface of the carbon particles, which is the reaction field, is covered, and the desired low resistance cannot be obtained.
[0047] [Carbonaceous material (C)] The carbonaceous material used in the present invention is added as a binder to strongly bind the carbonaceous fibers, which cannot be bound by nature, and the carbon particles other than graphite particles. In the present invention, as specified in the above (3), when the sizes of the crystallites in the c-axis direction in the carbonaceous fibers (A) and the carbonaceous material (C) are Lc(A) and Lc(C), respectively, determined by X-ray diffraction, Lc(C) / Lc(A) must satisfy 1.0 to 5. In this way, by using a highly crystalline binding carbonaceous material for the carbonaceous fibers (A), the electronic conduction resistance between the carbon particles (B) and the carbonaceous fibers (A) is reduced, and the electronic conduction path between the carbon particles (B) and the carbonaceous fibers (A) becomes smooth. In addition, since the carbonaceous material strongly binds the carbonaceous fibers together via carbon particles other than graphite particles, an efficient conductive path can be formed, and it has been found that the resistance-reducing effect due to the addition of carbon particles other than graphite particles described above is more effectively exerted.
[0048] If the ratio of Lc(C) / Lc(A) is less than 1.0, the above effect is not effectively exhibited. The above ratio is preferably 1.5 or more, more preferably 3.0 or more. On the other hand, if the ratio exceeds 5, it becomes difficult to impart oxygen functional groups to the carbonaceous material portion. The above ratio is preferably 4.5 or less, more preferably 4.0 or less.
[0049] In the present invention, the range of Lc(C) is not particularly limited as long as the ratio of Lc(C) / Lc(A) satisfies the above range, but from the viewpoint of further reducing the resistance, Lc(C) is preferably 10 nm or less, more preferably 7.5 nm or less. The lower limit of Lc(C) is not particularly limited from the above viewpoint, but is preferably about 3 nm or more in consideration of electronic conductivity, etc.
[0050] The content of the carbonaceous material (C) relative to the total amount of the carbonaceous fiber (A), the carbon particles other than graphite particles (B), and the carbonaceous material (C) [(C) / {(A)+(B)+(C)}] is preferably 14.5% or more, more preferably 15% or more, and even more preferably 17% or more, in terms of mass ratio. By increasing the content of the carbonaceous material in this manner, both the carbonaceous fiber and the carbon particles other than graphite particles can be sufficiently bound, and the binding effect due to the addition of the carbonaceous material is effectively exerted. Note that the upper limit is preferably about 90% or less, taking into consideration the permeability of the electrolyte, etc.
[0051] In addition, the mass ratio [(B)+(C) / {(A)+(B)+(C)}] of the total content of the carbon particles other than graphite particles (B) and the carbonaceous material (C) to the total amount of the above-mentioned carbonaceous fibers (A), the carbon particles other than graphite particles (B), and the carbonaceous material (C) is not particularly limited as long as the above requirements are satisfied, and is, for example, 50 to 70%.
[0052] The type of carbonaceous material (C) used in the present invention may be any material capable of binding carbon particles other than the carbonaceous fiber (A) and the graphite particles (B), and is not particularly limited as long as it exhibits binding properties during carbonization in the preparation of the electrode material of the present invention. Examples of such materials include pitches such as coal tar pitch and coal-based pitch; resins such as phenol resins, benzoxazine resins, epoxide resins, furan resins, vinyl ester resins, melamine-formaldehyde resins, urea-formaldehyde resins, resorcinol-formaldehyde resins, cyanate ester resins, bismaleimide resins, polyurethane resins, and polyacrylonitrile; furfuryl alcohol; and rubbers such as acrylonitrile-butadiene rubber. These may be commercially available products.
[0053] Among these, pitches such as coal tar pitch and coal-based pitch, which are particularly easily crystallizable, are preferred because the desired carbonaceous material (C) can be obtained at a low firing temperature. Phenol resins are also preferably used because their crystallinity does not increase or decrease much depending on the firing temperature, making it easy to control the crystallinity. Polyacrylonitrile resins are also preferably used because the desired carbonaceous material (C) can be obtained by increasing the firing temperature. Pitches are particularly preferred. According to a preferred embodiment of the present invention, since no phenol resin is used, the disadvantages associated with phenol resin (generation of formaldehyde and formaldehyde odor at room temperature) do not occur, and there are advantages such as no odor at room temperature, etc. In contrast, in the above-mentioned Patent Document 4, a phenol resin is used as the adhesive, and in addition to the above disadvantages, there are disadvantages in terms of cost and work, such as the need for separate equipment to control the formaldehyde concentration in the work area to below the controlled concentration.
[0054] Here, particularly preferred pitches are described in detail. The mesophase (liquid crystal) content of the above-mentioned coal tar pitch and coal-based pitch can be controlled by the temperature and time of the infusible treatment. If the mesophase content is low, it melts at a relatively low temperature, or is in a liquid state at room temperature. On the other hand, if the mesophase content is high, it melts at a high temperature, and a high carbonization yield is obtained. When pitches are used as the carbonaceous material (C), it is preferable that the mesophase content is high (i.e., the carbonization rate is high), for example, 30% or more is preferable, and 50% or more is more preferable. This suppresses the fluidity during melting, and the carbonaceous fibers can be bonded together via the carbon particles without excessively covering the surfaces of the carbon particles other than the graphite particles. In addition, the upper limit is preferably, for example, 90% or less, taking into consideration the expression of binding properties.
[0055] From the same viewpoint as above, the melting point of the pitch is preferably 100° C. or higher, more preferably 200° C. or higher. This not only provides the above-mentioned effects, but also suppresses odor during the impregnation process, which is also preferable in terms of processability. The upper limit is preferably, for example, 350° C. or lower, taking into account the expression of binding properties.
[0056] (Characteristics of the electrode material of the present invention) The electrode material of the present invention has a mesopore specific surface area of 30 m2 as determined by the nitrogen gas adsorption method. 2 When the specific surface area of mesopores is high, low resistance can be achieved and an electrode material with excellent battery performance can be obtained, but if it is too high, problems such as particle dropout and a decrease in the strength of the electrode material can occur.
[0057] The present invention is a technology for reducing the total cell resistance, which is expressed in detail as the sum of the reaction resistance and the conductive resistance (total cell resistance = reaction resistance + conductive resistance). In detail, the present invention intends to reduce the total cell resistance by reducing the reaction resistance, and does not aim to reduce the conductive resistance. When the conductive resistance is low, the repulsive force of the material becomes excessively high, increasing the risk of the fibers piercing the ion exchange membrane and causing a short circuit, which results in a problem that the battery efficiency is likely to decrease. In contrast, the present invention reduces the reaction resistance by increasing the specific surface area, so that the effect of reducing the total cell resistance can be obtained without excessively increasing the repulsive force, and as a result, it is thought that stable battery efficiency can be easily obtained.
[0058] In the present invention, the mesopore region with a pore diameter of 2 nm or more and less than 40 nm is the object of measurement, and the mesopore specific surface area is measured based on the adsorption curve when nitrogen gas is adsorbed onto the electrode material. The detailed method for measuring the mesopore specific surface area will be described in detail in the Examples section.
[0059] Furthermore, the electrode material of the present invention has a BET specific surface area of 50 m2 calculated from the amount of nitrogen adsorption. 2 / g is preferable, and 40m 2 / g is more preferable. 2 / g or more, problems such as particle dropout and a decrease in the strength of the electrode material occur due to a decrease in the binding strength of the carbon particles (B) other than the graphite particles. The lower limit of the BET specific surface area is not particularly limited from the above viewpoint, but considering the exposure of the edge surface and the contact area with the electrolyte, it is generally set to about 20 m 2 It is preferable that the molecular weight is 1 / g or more.
[0060] Furthermore, in the electrode material of the present invention, the number of bonded oxygen atoms on the surface of the carbon electrode material satisfies 1% or more of the total number of carbon atoms on the surface of the carbon electrode material. Hereinafter, the ratio of the number of bonded oxygen atoms to the total number of carbon atoms may be abbreviated as O / C. O / C can be measured by surface analysis such as X-ray photoelectron spectroscopy (XPS) or X-ray fluorescence analysis.
[0061] By using an electrode material with an O / C of 1% or more, the electrode reaction rate can be significantly increased, resulting in low resistance. Furthermore, hydrophilicity can be increased by controlling the O / C, and the water flow rate (preferably 0.5 mm / sec or more) of the electrode material described below can be ensured. In contrast, when an electrode material with a low oxygen concentration, that is, an O / C of less than 1%, is used, the electrode reaction rate during discharge is reduced, and the electrode reaction activity cannot be increased. As a result, the resistance increases. Although the details of the reason why the electrode reaction activity (in other words, the voltage efficiency) is increased by using an electrode material with many oxygen atoms bonded to the surface of the electrode material are not clear, it is considered that the oxygen atoms present in large numbers on the surface are effective in the affinity between the carbonaceous material (C) and the electrolyte, the transfer of electrons, the detachment of complex ions from the carbonaceous material, and the complex exchange reaction.
[0062] The electrode material of the present invention has excellent hydrophilicity. The hydrophilicity can be confirmed by the water flow rate when a drop of water is dropped on the electrode material after the electrode material is subjected to a dry oxidation treatment. The water flow rate of the electrode material according to the present invention is preferably 0.5 mm / sec or more. This allows it to be determined that the electrode material has sufficient affinity for the electrolyte. The water flow rate of the electrode material is preferably as high as possible, more preferably 1 mm / sec or more, even more preferably 5 mm / sec or more, and even more preferably 10 mm / sec or more.
[0063] The weight of the electrode material of the present invention is 50 to 500 g / m2 when the thickness of the spacer 2 sandwiched between the current collector 1 and the ion exchange membrane 3 (hereinafter referred to as the "spacer thickness") is 0.3 to 3 mm. 2 is preferable, and 100 to 400 g / m 2 is more preferable. By controlling the basis weight within the above range, it is possible to prevent damage to the ion exchange membrane 3 while ensuring liquid permeability. In particular, in recent years, the thickness of the ion exchange membrane 3 has tended to become thinner from the viewpoint of reducing resistance, and treatment and usage methods for reducing damage to the ion exchange membrane 3 are extremely important. From the above viewpoint, it is also more preferable to use a nonwoven fabric or paper with one side flattened as the substrate for the electrode material of the present invention. Any known method can be applied as the flattening method, and examples of the method include a method in which a slurry is applied to one side of a carbonaceous fiber and dried; and a method in which a slurry is impregnated on a smooth film such as PET and dried.
[0064] The thickness of the electrode material of the present invention is preferably at least greater than the spacer thickness. For example, when a low-density carbonaceous fiber such as a nonwoven fabric is used and carbon particles other than the graphite particles used in the electrode material of the present invention or a carbonaceous material with binding properties are supported on the carbonaceous fiber, the thickness is preferably 1.5 to 6.0 times the spacer thickness. However, if the thickness is too large, the ion exchange membrane 3 may be broken by the compressive stress of the sheet-like material, so that the compressive stress of the electrode material of the present invention is preferably 9.8 N / cm. 2 The following are preferably used. In order to adjust the compressive stress, etc., according to the basis weight and thickness of the electrode material of the present invention, it is also possible to use the electrode material of the present invention by laminating two or three layers. Alternatively, it is also possible to combine it with an electrode material of another form.
[0065] The electrode material of the present invention is used for the negative electrode of a redox battery. On the other hand, the type of electrode material used for the positive electrode of a redox battery is not particularly limited as long as it is one that is commonly used in the technical field, and carbon fiber paper used in fuel cells may be used, or the electrode material of the present invention may be used as it is for the positive electrode. For example, in short-term use (for example, when the total time of the charge / discharge test is 3 hours as in the examples described later), it has been confirmed that the electrode material of the present invention can be used for the positive electrode and the cell resistance during initial charge / discharge can be reduced (see the examples described later). In the examples described later, the same sample was used for the positive electrode and the negative electrode, but the present invention is not limited to this, and different compositions may be used as long as they satisfy the requirements of the present invention.
[0066] (Method of manufacturing electrode material according to the present invention) Next, a method for producing the electrode material of the present invention will be described. The electrode material of the present invention can be produced by attaching carbon particles other than graphite particles and a precursor of the carbonaceous material (before carbonization) to a carbonaceous fiber (substrate), and then carrying out a carbonization step, a primary oxidation step, a graphitization step, and a secondary oxidation step. The present invention is characterized in that the carbonization step and the graphitization step are carried out under predetermined conditions, and that two oxidation treatments are carried out before and after the graphitization step, and in particular, the greatest characteristic is that the oxidation treatment is carried out twice. Here, the "primary oxidation step" refers to the first oxidation step, and the "secondary oxidation step" refers to the second oxidation step.
[0067] Each step will be described below.
[0068] (A process for attaching carbon particles other than graphite particles and a precursor of a carbonaceous material to carbonaceous fibers) First, carbon particles other than graphite particles and a precursor of a carbonaceous material are attached to the carbonaceous fiber. In order to attach carbon particles other than graphite particles and a precursor of a carbonaceous material to the carbonaceous fiber, any known method can be adopted. For example, the above-mentioned carbonaceous material precursor is heated and melted, carbon particles other than graphite particles are dispersed in the obtained molten liquid, and the carbonaceous fiber is immersed in this molten dispersion liquid, and then cooled to room temperature. Alternatively, as shown in the examples described later, the above-mentioned carbonaceous material precursor and carbon particles other than graphite particles are dispersed in a solvent such as water or alcohol to which a binder (temporary adhesive) that disappears during carbonization such as polyvinyl alcohol is added, and the carbonaceous fiber is immersed in this dispersion liquid, and then heated and dried. Here, the excess liquid in the above-mentioned molten dispersion liquid or the dispersion liquid in which the carbonaceous fiber is immersed can be removed by passing the molten dispersion liquid or the dispersion liquid through a nip roller having a predetermined clearance to squeeze out the excess dispersion liquid when immersed in the dispersion liquid, or by scraping off the surface of the excess dispersion liquid when immersed in the dispersion liquid with a doctor blade or the like.
[0069] Thereafter, the mixture is dried in an air atmosphere at, for example, 80 to 150°C.
[0070] (Carbonization process) The carbonization step is carried out to sinter the product obtained after the impregnation step. This allows the carbonaceous fibers to be bonded together via carbon particles other than graphite particles. In the carbonization step, it is preferable to thoroughly remove decomposition gases generated during carbonization, and for example, the fibers are heated at a temperature of 500°C or higher and lower than 2000°C in an inert atmosphere (preferably a nitrogen atmosphere). The heating temperature is preferably 600°C or higher, more preferably 800°C or higher, even more preferably 1000°C or higher, even more preferably 1200°C or higher; more preferably 1400°C or lower, and even more preferably 1300°C or lower. The heating time in the inert atmosphere is preferably, for example, 1 to 2 hours. This short treatment time sufficiently promotes bonding between the carbonaceous fibers and removal of decomposition gases during carbonization.
[0071] As described above, the treatment corresponding to the carbonization step may be performed after the fiber is flame-retarded, but the carbonization treatment performed after the fiber is flame-retarded may be omitted. That is, the method for producing the electrode material of the present invention is roughly divided into the following method 1 and method 2. Method 1: Fiber flame retardancy → fiber carbonization → impregnation of carbon particles other than graphite particles and carbonaceous materials → carbonization → primary oxidation → graphitization → secondary oxidation Method 2: Fiber flame retardation → impregnation of carbon particles other than graphite particles and carbonaceous materials → carbonization → primary oxidation → graphitization → secondary oxidation According to the above method 1, although the processing cost increases because the carbonization is performed twice, the sheet used as the electrode material is less susceptible to the effects of differences in the volumetric shrinkage ratio, and therefore the obtained sheet is less likely to deform (warp). On the other hand, according to the above method 2, the carbonization step is only performed once, so the processing cost can be reduced, but the obtained sheet is more likely to deform due to the difference in the volumetric shrinkage ratio during carbonization of each material. It is sufficient to decide whether to adopt the above method 1 or 2, taking these factors into consideration.
[0072] (Primary oxidation process) In the present invention, it is important to carry out a first oxidation treatment under a dry condition after the carbonization step and before the graphitization step described below. This activates the carbonaceous fibers and exposes the surfaces of carbon particles other than graphite particles by removing the carbonaceous material. As a result, reactivity is improved and low resistance is obtained.
[0073] Generally, the oxidation treatment can be performed by either dry or wet method, for example, wet chemical oxidation, electrolytic oxidation, dry oxidation, etc., but in the present invention, dry oxidation treatment is performed from the viewpoint of workability and manufacturing cost. The oxidation treatment is preferably performed in an air atmosphere. The heating temperature is controlled in the range of 500°C or more and 900°C or less. This introduces oxygen functional groups to the surface of the electrode material, and the above-mentioned effects are effectively exhibited. The heating temperature is more preferably 550°C or more. Also, 800°C or less is more preferable, and 750°C or less is even more preferable. The primary oxidation treatment is preferably carried out for, for example, 5 minutes to 1 hour. If the primary oxidation treatment solution is used for less than 5 minutes, the entire carbon electrode material may not be oxidized uniformly. On the other hand, if the primary oxidation treatment solution is used for more than 1 hour, the strength of the carbon electrode material may be reduced, and the working efficiency may be reduced.
[0074] Here, in the above primary oxidation step, from the two viewpoints of increasing the specific surface area of the electrode material and maintaining the mechanical strength, it is preferable to adjust the mass yield of the electrode material before and after the primary oxidation step (i.e., the ratio of the mass of the electrode material after the primary oxidation treatment solution to the mass of the electrode material before the primary oxidation treatment) to a range of, for example, 85% or more and 95% or less. The above mass yield can be adjusted, for example, by appropriately adjusting the treatment time and heating temperature during dry air oxidation.
[0075] (Graphitization process) The graphitization step is a step carried out to sufficiently increase the crystallinity of the carbonaceous material, improve electronic conductivity, and improve oxidation resistance against sulfuric acid solution in the electrolyte. After the primary oxidation step, the carbonaceous material is preferably heated in an inert atmosphere (preferably in a nitrogen atmosphere) at a temperature of 1300°C or higher, which is higher than the heating temperature in the carbonization step, and more preferably at 1500°C or higher. In addition, the upper limit is preferably 2000°C or lower, in consideration of imparting high electrolyte affinity to the carbonaceous material.
[0076] (Secondary oxidation process) After the graphitization process, a secondary oxidation process is performed to introduce oxygen functional groups such as hydroxyl groups, carbonyl groups, quinone groups, lactone groups, and free radical oxides onto the surface of the electrode material. As a result, the aforementioned O / C ratio of ≥ 1% can be achieved. These oxygen functional groups contribute greatly to the electrode reaction, resulting in a sufficiently low resistance. The water flow rate is also increased.
[0077] The secondary oxidation treatment step can be various treatment steps such as wet chemical oxidation, electrolytic oxidation, and dry oxidation, but in the present invention, dry oxidation treatment is performed from the viewpoint of workability and manufacturing costs. The oxidation treatment is preferably performed in an air atmosphere. The heating temperature is controlled in the range of 500°C or more and 900°C or less. This introduces oxygen functional groups to the surface of the electrode material, and the above-mentioned effects are effectively exhibited. The heating temperature is preferably 600°C or more, more preferably 650°C or more. Also, it is preferably 800°C or less, more preferably 750°C or less. Similarly to the above-mentioned primary oxidation treatment, the secondary oxidation treatment is preferably carried out for, for example, 5 minutes to 1 hour. If the primary oxidation treatment solution is used for less than 5 minutes, there is a risk that the entire carbon electrode material will not be oxidized uniformly. On the other hand, if the primary oxidation treatment solution is used for more than 1 hour, there is a risk that the strength of the carbon electrode material will be reduced and the working efficiency will decrease.
[0078] Here, the conditions for the first and second oxidation treatments described above may be the same or different as long as the above conditions are satisfied, but it is preferable that the heating temperature in the second oxidation treatment (secondary oxidation treatment) is higher than that in the first oxidation treatment (primary oxidation treatment). In the primary oxidation treatment, graphitization treatment for improving crystallinity has not yet been carried out, and it is considered that oxidation proceeds quickly, so the heating temperature is controlled to be lower than that in the secondary oxidation treatment.
[0079] Furthermore, in the secondary dry oxidation treatment step, from the viewpoint of maintaining the mechanical strength of the electrode material, it is preferable to adjust the mass yield of the electrode material before and after the oxidation treatment (i.e., the ratio of the mass of the electrode material after the secondary oxidation treatment solution to the mass of the electrode material before the secondary oxidation treatment) to 90% or more and 96% or less. The above mass yield can be adjusted, for example, by appropriately adjusting the treatment time and heating temperature of the dry air oxidation. EXAMPLES
[0080] The present invention will be described in more detail below with reference to examples and comparative examples. Note that the present invention is not limited to the following examples. In the following, % means "mass %" unless otherwise specified.
[0081] In this example, the following items were measured. The details of the measurement method are as follows.
[0082] (1) Measurement of the crystallite size (Lc) along the c-axis by X-ray diffraction In detail, Lc(A) of carbonaceous fiber, Lc(B) and La(B) of carbon particles other than graphite particles, and Lc(C) of carbonaceous material were measured as follows. The carbonaceous fibers, carbon particles other than graphite particles, and carbonaceous materials (single substances) used in this example were sequentially subjected to the same heat treatment as in Example 1, and the final treated samples were used for measurement. Basically, carbon crystallinity is dominated by the influence of the thermal energy given to the sample, and it is considered that the thermal history of the highest temperature given to the sample determines the crystallinity of Lc, but depending on the degree of the subsequent oxidation treatment, it is possible that the graphene stacking structure formed during the graphitization process is disturbed, resulting in a decrease in crystallinity due to the generation of defective structures. Therefore, the final treated samples were used.
[0083] Each of the single samples collected as described above was crushed in an agate mortar until the particle size was about 10 μm. Approximately 5% by mass of high-purity silicon powder for X-ray standard was mixed with the crushed sample as an internal standard substance, and the mixture was packed into a sample cell. Wide-angle X-rays were measured by the diffractometer method using CuKα radiation as the radiation source.
[0084] The carbonaceous fiber (A) and carbon particles other than graphite particles (B) used in the electrode material of the present invention, as well as the carbonaceous material (C) binding them, were subjected to peak separation from the chart obtained by the wide-angle X-ray measurement, and the Lc value of each was calculated. Specifically, the peak with an apex in the range of 26.4° to 26.6° of the diffraction angle θ (2θ) was determined as the carbonaceous particle (B) other than graphite particles, and the peak with an apex in the range of 25.3° to 25.7° was determined as the carbonaceous material (C). After determining the peak shape as a sine wave from each peak top, the peak shape as a sine wave was determined from the foot part seen in the vicinity of 24.0° to 25.0°, and this was determined as the carbonaceous fiber (A). From the three peaks separated by the above method, the Lc of each was calculated by the following method.
[0085] The curves were corrected using the following simple method, without correction for the so-called Lorentz factor, polarization factor, absorption factor, atomic scattering factor, etc. <002> The actual intensity of the peaks corresponding to the diffraction is plotted from the baseline. <002> A corrected intensity curve was obtained. The length of the line segment (half-width β) where a line parallel to the angle axis drawn at half the height of this peak intersects with the corrected intensity curve was used to calculate the crystallite size Lc in the c-axis direction using the following formula.
[0086] Lc=(k λ) / (β cosθ) Here, the structure factor k = 0.9, the wavelength λ = 1.5418 Å, and β is <002> The half-width of the diffraction peak, θ, is <002> The diffraction angles are indicated.
[0087] (2) Measurement of the specific surface area of the electrode material (2-1) Mesopore specific surface area with pore diameter of 2 nm or more and less than 40 nm (S2-40 nm:m 2 / g) Approximately 50 mg of the sample was weighed out and vacuum dried at 130° C. for 24 hours. The amount of nitrogen adsorption was measured for the dried sample using an automatic specific surface area measurement device (Shimadzu Corporation, GEMINI VII) by a gas adsorption method using nitrogen gas, and the nitrogen adsorption isotherm during the adsorption process was analyzed by the BJH method to determine the specific surface area (m2) of mesopores with pore diameters of 2 nm or more and less than 40 nm. 2 / g) was calculated.
[0088] (2-2)BET specific surface area (BET:m 2 / g) Approximately 50 mg of a sample was weighed out and dried in vacuum at 130° C. for 24 hours. The amount of nitrogen adsorption was measured for the dried sample using an automatic specific surface area measuring device (Shimadzu Corporation, GEMINI VII) by a gas adsorption method using nitrogen gas, and the BET specific surface area (m 2 / g) was determined.
[0089] (3) Measurement of O / C by XPS surface analysis For the measurement by X-ray photoelectron spectroscopy, abbreviated as ESCA or XPS, an ULVAC-PHI 5801MC instrument was used. First, the sample was fixed on a sample holder with a Mo plate, and after sufficient evacuation in the preliminary evacuation chamber, it was placed in the chamber of the measurement room. The monochromatic AlKα ray was used as the radiation source, the output was 14 kV, 12 mA, and the degree of vacuum inside the device was 10 -8 torr. A full elemental scan was performed to investigate the composition of surface elements, and narrow scans were performed on detected and predicted elements to evaluate their abundance ratios. The ratio of the number of surface-bound oxygen atoms to the total number of surface carbon atoms was calculated as a percentage (%) to calculate O / C.
[0090] (4) Charge / discharge test (4-1) Measurement of total cell resistance (total cell resistance at SOC50%) The electrode material obtained by the method described below was cut into a size of 2.7 cm in the vertical direction (flow direction), 3.3 cm in the width direction, and 8.91 cm in electrode area. 2 The total charge / discharge time in this test was short, so even if the electrode material of the present invention was used on the positive electrode side, no adverse effects due to oxidative decomposition of manganese would occur, and therefore the same sample was used for the positive and negative electrodes. 2 The number of sheets was adjusted so that the cell shown in Figure 1 was assembled. The ion exchange membrane used was Nafion 211 membrane, and the spacer thickness was 0.4 mm. 144 mA / cm2 From the voltage curve after 10 cycles in the voltage range of 1.55 to 1.00 V, the total cell resistance (SOC50% total cell resistance, Ω cm 2 ) was calculated. The electrolyte for both the positive and negative electrodes was a 5.0 mol / L aqueous sulfuric acid solution containing 1.0 mol / L each of titanium oxysulfate and manganese oxysulfate. The amount of electrolyte was in large excess relative to the cell and piping. The liquid flow rate was 10 mL per minute, and measurements were performed at 35°C.
[0091] Total cell resistance = (V C50 -V D50 ) / (2×I) [Ω cm 2 ] Where: V C50 is the charging voltage for the amount of electricity when the charging rate is 50% obtained from the electrode curve, V D50 is the discharge voltage for the amount of electricity when the charge rate is 50% calculated from the electrode curve, I=current density (mA / cm 2 ) It is.
[0092] (4-2) Measurement of reaction resistance In this example, the resistance components were separated and the reaction resistance was also measured. As described above, total cell resistance = reaction resistance + conductive resistance, and the present invention aims to reduce the total cell resistance by reducing the reaction resistance.
[0093] In detail, the current density is 144mA / cm to achieve a state of charge (SOC) of 50%. 2 After charging for 5 minutes, the AC impedance was measured in the frequency range of 20 kHz to 0.01 Hz. The intersection point of the obtained Nyquist plot with the real axis was taken as the conductive resistance (Ω cm 2 ), the sum of the diameter of the semicircular part and the straight part of the low frequency region is the reaction resistance (Ω cm 2 ) was decided.
[0094] (5) Water flow test A drop of ion-exchanged water was dropped onto the electrode from a 3 mm diameter pipette at a point 5 cm above the electrode, and the time it took for the drop to penetrate was measured, and the water flow rate was calculated using the following formula. Water flow rate (mm / sec) = electrode material thickness (mm) ÷ time it takes for the water droplet to penetrate (sec)
[0095] Example 1 In this example, carbon particles (B) other than graphite particles were carbon blacks A and B shown in Table 1, graphite particles D shown in Table 1 for comparison, carbonaceous materials (C) were a (Osaka Kasei Co., Ltd. TGP-3500 pitches) and b (DIC Corporation TD-4304 phenolic resin, solid content 40%) shown in Table 2, and carbonaceous fibers (A) were polyacrylonitrile fibers shown in Table 2. An electrode material made of a carbonaceous sheet was produced as follows, and various items were measured. A, B, and D are all commercially available products, and the average particle diameters shown in Table 1 are values listed in the catalog.
[0096] (No.1) First, a dispersion was prepared by adding 2.0% Kao Corporation Rheodol TW-L120 (nonionic surfactant), 2.0% polyvinyl alcohol (temporary adhesive), 6.7% of the above carbonaceous material a, and 7.0% of A in Table 1 as carbon particles other than graphite to ion-exchanged water. Into the dispersion thus obtained, carbon paper (CB0-030TP6, manufactured by Orivest Co., Ltd., basis weight 30 g / m) made of carbonized polyacrylonitrile fiber (average fiber length 6 mm) was added as a substrate (fiber structure). 2 After immersion, the film was passed through nip rollers to remove excess dispersion liquid. Next, it was dried at 120°C for 20 minutes in an air atmosphere. Thereafter, the temperature was increased to 1000°C at a rate of 5°C / min in nitrogen gas, and carbonized (calcined) by holding at this temperature for 1 hour, and then oxidized at 550°C for 25 minutes in an air atmosphere (first oxidation treatment). After the above oxidation treatment, it was cooled, and further increased to 1500°C at a rate of 5°C / min in nitrogen gas, and graphitized by holding at this temperature for 1 hour, and then oxidized at 650°C for 5 minutes in an air atmosphere (second oxidation treatment) to obtain No. 1 electrode material (thickness 0.43 mm, basis weight 77 g / m 2 ) was obtained.
[0097] (No.2) An electrode material No. 2 (thickness: 0.45 mm, basis weight: 71 g / m) was prepared in the same manner as No. 1 above, except that a dispersion was prepared by adding 2.0% of Kao Corporation's Rheodol TW-L120 (nonionic surfactant), 2.0% of polyvinyl alcohol (temporary adhesive), 6.7% of the carbonaceous material a, and 7.0% of B in Table 1 as carbon particles other than graphite to ion-exchanged water. 2 ) was obtained.
[0098] (No.3) No. 3 is an example that does not use any carbon particles or carbonaceous materials other than graphite particles, but is made only of carbonaceous fibers. In detail, the carbon paper was directly subjected to the same heat treatment as No. 1, and the electrode material of No. 3 (thickness 0.33 mm, basis weight 27 g / m2) was obtained. 2 ) was obtained.
[0099] (No.4) A dispersion was prepared by adding 2.0% Rheodol TW-L120 (nonionic surfactant) manufactured by Kao Corporation, 2.0% polyvinyl alcohol (temporary adhesive), 14.0% of the above carbonaceous material a, and 9.8% of graphite particles D in Table 1 (an example not satisfying the requirements of the present invention) to ion-exchanged water.
[0100] The same process as for No. 1 was carried out except that the dispersion liquid prepared above was used, and electrode material No. 4 (thickness 0.46 mm, basis weight 129 g / m) was obtained. 2 ) was obtained.
[0101] (No.5) A dispersion was prepared by adding 2.0% Kao Corporation's Rheodol TW-L120 (nonionic surfactant), 2.0% polyvinyl alcohol (temporary adhesive), 5.7% of b (solid content 40%) in Table 2 as a carbonaceous material, and 4.0% of A in Table 1 as carbon particles other than graphite particles to ion-exchanged water.
[0102] The same process as No. 1 was carried out except that the dispersion liquid prepared above was used, and electrode material No. 5 (thickness 0.38 mm, basis weight 70 g / m) was obtained. 2 ) was obtained.
[0103] (No.6) Carbon paper was immersed in the dispersion liquid in the same manner as in No. 1 above, and then carbonization and graphitization were carried out in the same manner as in No. 6 above, but the subsequent oxidation treatment in an air atmosphere was not carried out. 2 ) was obtained.
[0104] (No.7) A dispersion was prepared by adding 2.0% Kao Corporation's Rheodol TW-L120 (nonionic surfactant), 2.0% polyvinyl alcohol (temporary adhesive), 3.8% carbonaceous material b (solid content 40%) from Table 2, and 1.5% carbon particles other than graphite particles B' from Table 1 to ion-exchanged water.
[0105] The same process as No. 1 was carried out except that the dispersion liquid prepared above was used, and electrode material No. 7 (thickness 0.35 mm, basis weight 55 g / m) was obtained. 2 ) was obtained.
[0106] Table 2 shows the types of carbonaceous materials used, and Tables 3A, 3B and 4 show the measurement results for the above Nos. 1 to 7.
[0107] [Table 1]
[0108] [Table 2]
[0109] [Table 3A]
[0110] [Table 3B]
[0111] [Table 4]
[0112] Nos. 1 and 2 are electrode materials that satisfy the requirements of the present invention, and low-resistance electrode materials were obtained. This is thought to be because, in particular, A to B in Table 1, which have small particle diameters, were used as carbon particles other than graphite, and the electrode materials were produced under specified conditions, so that the reaction surface area was increased, and the electrode activity was improved by activating the carbonaceous fibers and exposing the surfaces of carbon particles other than graphite particles by removing the carbonaceous material.
[0113] In contrast, No. 3 is an example that does not use any carbon particles or carbonaceous materials other than graphite particles, but is composed only of carbonaceous fibers, and the resistance significantly increased due to an insufficient reaction surface area.
[0114] In No. 4, the total cell resistance increased because carbon particles D in Table 1, which has a large particle size and a large Lc(B), were used. This is thought to be because the use of carbon particles with a large particle size results in a smaller reaction surface area than in the examples of the present invention, and because the use of carbon particles with high carbon crystallinity makes it difficult to impart oxygen functional groups, which reduces the affinity of the carbon particles to the aqueous electrolyte and prevents the reaction activity from improving.
[0115] No. 5 is an example with a small ratio of Lc(C) / Lc(A), and the resistance increased. This is thought to be because the carbon crystallinity of the carbonaceous material was lower than that of the present invention examples, which resulted in a high electronic conduction resistance between the carbon particles and the carbonaceous fiber, and the reactivity of the carbon particles could not be utilized efficiently.
[0116] No. 6 is an example with a small O / C ratio, and the resistance increased and water did not pass through. This is thought to be because the amount of oxygen functional groups was small, which reduced the affinity with the electrolyte compared to the examples of the present invention, and reduced the reaction activity.
[0117] No. 7 is an example in which the Lc(C) / Lc(A) ratio is small and the mesopore specific surface area is large, and the resistance increased. This is thought to be because the carbon crystallinity of the carbonaceous material was lower than that of the present invention examples, resulting in high electronic conduction resistance between the carbon particles and the carbonaceous fiber, and the reactivity of the carbon particles could not be utilized efficiently. [Industrial Applicability]
[0118] According to the present invention, a carbon electrode material that can reduce cell resistance during initial charge and discharge and has excellent battery energy efficiency can be provided, and is therefore useful as a carbon electrode material used in the negative electrode of a redox battery. The carbon electrode material of the present invention is suitably used in flow-type and non-flow-type redox batteries, redox batteries combined with lithium, capacitors, and fuel cell systems, and the like. [Explanation of symbols]
[0119] 1 Current collector plate 2 Spacers 3. Ion exchange membrane 4a,4b Liquid passage 5 Electrode material 6 Positive Electrolyte Tank 7. Negative Electrolyte Tank 8,9 Pump 10 Liquid inlet 11 Liquid outlet 12,13 External flow path
Claims
1. A carbon electrode material used in a negative electrode of a redox battery, The carbon electrode material is obtained by carbonizing a product including carbonaceous fibers (A), carbon particles other than graphite particles (B), and a carbonaceous material (C) binding the carbonaceous fibers and the carbon particles together, A carbon electrode material for a redox battery, characterized by satisfying the following requirements: (1) the particle size of the carbon particles (B) other than the graphite particles before carbonization is 1 μm or less; (2) In the carbon particles (B) other than the graphite particles, when the size of the crystallite in the c-axis direction determined by X-ray diffraction is Lc(B), Lc(B) is 10 nm or less; (3) When the sizes of crystallites in the c-axis direction in the carbonaceous fiber (A) and the carbonaceous material (C) determined by X-ray diffraction are Lc(A) and Lc(C), respectively, Lc(C) / Lc(A) is 1.0 to 5.0; (4) When a drop of water is dropped, the water flow rate is 1.0 mm / sec or more; (5) The number of bonded oxygen atoms on the surface of the carbon electrode material is 1% or more of the total number of carbon atoms on the surface of the carbon electrode material.
2. 2. The carbon electrode material according to claim 1, wherein a mass ratio of the carbonaceous material (C) to the carbon particles (B) is 0.2 to 10.
3. The BET specific surface area calculated from the nitrogen adsorption amount is 50 m 2 The carbon electrode material according to claim 1 or 2, wherein the carbon electrode material has a molecular weight of less than 10000 / g.
4. A redox flow battery comprising the carbon electrode material according to any one of claims 1 to 3 as a negative electrode.
5. A method for producing the carbon electrode material according to any one of claims 1 to 3, comprising the steps of: A step of attaching carbon particles (B) other than the graphite particles and a carbonaceous material (C) before carbonization to the carbonaceous fibers (A); a carbonization step of heating the product after the impregnation in an inert gas atmosphere at a temperature of 500° C. or more and less than 2000° C.; A primary oxidation step of performing oxidation treatment at a temperature of 500 to 900°C under dry conditions; a graphitization step of heating at a temperature of 1300 to 2300°C under an inert gas atmosphere; A secondary oxidation process in which oxidation treatment is performed at a temperature of 500 to 900 ° C. under dry conditions; A method for producing a carbon electrode material, comprising the steps of:
Citation Information
Patent Citations
Electrode material
JP1984101776A
Manufacture of carbon fiber porous body
JP1988222080A
Redox flow battery, and operation method thereof
JP2012204135A
Gas diffusion electrode base material and production method therefor