Selective tungsten deposition at low temperatures
Low-temperature tungsten deposition using hydrogen and tungsten precursor flows addresses the challenges of high stress and impurities in tungsten films, enabling reliable formation of small semiconductor features with reduced roughness and improved structural integrity.
Patent Information
- Application Number
- JP2022542965
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-06-30
- Filing Date
- 2021-06-30
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2041-06-30
AI Technical Summary
Reliably forming features smaller than 100 nm in semiconductor devices is challenging due to high stress, roughness, and impurities in tungsten films deposited by chemical vapor deposition, which cause issues like wafer warpage, structural deformation, voids, and fluorine attack damage, especially at high temperatures.
A method of depositing tungsten at low temperatures (about 350°C or less) using a hydrogen gas flow and tungsten precursor, with a ratio of hydrogen gas flow to tungsten precursor flow of 500:1 or greater, to reduce roughness, stress, and impurities, and selectively depositing tungsten on different surfaces with a thickness ratio of 200:1 or greater.
The method results in tungsten films with reduced roughness, stress, and impurities, facilitating the formation of high-density semiconductor structures with improved reliability and reduced manufacturing costs.
Smart Images

Figure 0007552984000002 
Figure 0007552984000007 
Figure 0007552984000006
Abstract
Description
[Technical field]
[0001] SUMMARY OF THE DISCLOSURE Embodiments of the present disclosure generally relate to improved methods of forming interconnects. Additional embodiments of the present disclosure relate to methods of forming tungsten at low temperatures. [Background technology]
[0002] Reliable formation of features smaller than 100 nm is one of the key technological challenges for the next generation of very large scale integration (VLSI) and ultra large scale integration (ULSI) of semiconductor devices. However, as the limits of circuit technology are pushed, the shrinking dimensions of VLSI and ULSI technologies have placed additional demands on processing power. Reliable formation of gate structures on substrates is critical to the success of VLSI and ULSI, as well as to the continuing effort to increase circuit density and quality of individual substrates and dies.
[0003] As the circuit density of next generation devices increases, the width of interconnects such as vias, trenches, contacts, gate structures and other features as well as the width of the dielectric material between them decrease below 45 nm and 32 nm dimensions, while the thickness of the dielectric layers remains substantially constant, resulting in an increase in the aspect ratio of the features. To enable the fabrication of next generation devices and structures, three-dimensional (3D) stacking of semiconductor chips is often utilized to improve the performance of transistors. By arranging transistors in three dimensions instead of the traditional two dimensions, a large number of transistors can be placed very close to each other in an integrated circuit (IC). 3D stacking of semiconductor chips shortens the wiring length and keeps wiring delays low. In the fabrication of 3D stacking of semiconductor chips, a stepped structure is often utilized to enable a large number of interconnect structures to be placed on top of it to form a high density vertical transistor device.
[0004] Thus, there is a continuing need for improved methods of forming interconnects to reduce manufacturing costs, memory cell size and power consumption of integrated circuits.
[0005] Tungsten films deposited by chemical vapor deposition (CVD) are known to have relatively high stress values and roughness. Furthermore, tungsten films deposited using tungsten hexafluoride are known to have relatively high levels of fluorine impurities. This relatively high level of stress, roughness and fluorine impurities often causes problems, including but not limited to wafer warpage, structure deformation, voids and seams in gap filling, and fluorine attack damage at interfaces.
[0006] Some of the methods developed to solve these problems rely on atomic layer deposition (ALD). However, ALD processes are typically performed at relatively high temperatures, usually above 400° C. Summary of the Invention [Problem to be solved by the invention]
[0007] Therefore, there is a need for a method of depositing tungsten that results in low roughness, low stress and fewer impurities, as well as being performed at lower temperatures. [Means for solving the problem]
[0008] One or more embodiments of the present disclosure are directed to a method of depositing tungsten, the method including exposing a substrate to a flow of hydrogen gas, and exposing the substrate to a flow of a tungsten precursor while exposing the substrate to the flow of hydrogen gas to deposit a tungsten layer on the substrate. The substrate is maintained at a temperature of about 350° C. or less.
[0009] Additional embodiments of the present disclosure are directed to a method of depositing tungsten, the method including exposing a substrate to a flow of hydrogen gas, and exposing the substrate to a flow of tungsten precursor while exposing the substrate to the flow of hydrogen gas, the ratio of the flow of hydrogen gas to the flow of tungsten precursor being about 500:1 or greater.
[0010] Additional embodiments of the present disclosure are directed to a method of selectively depositing tungsten, the method including exposing a substrate including a first material side and a second material side to a flow of hydrogen gas, and exposing the substrate to a flow of tungsten precursor while exposing the substrate to the flow of hydrogen gas to deposit a first thickness of tungsten on the first material side and a second thickness of tungsten on the second material side, the ratio of the first thickness to the second thickness being about 200:1 or greater.
[0011] So that the above-listed features of the present disclosure can be understood in detail, the disclosure briefly outlined above may be more particularly described by reference to embodiments, some of which are illustrated in the accompanying drawings. It should be noted, however, that the accompanying drawings illustrate only typical embodiments of the present disclosure and therefore should not be considered as limiting the scope of the present disclosure, since the present disclosure may embrace other embodiments that are equally effective. [Brief description of the drawings]
[0012] [Figure 1] 1 illustrates a method of forming an interconnect in accordance with one or more embodiments. [Figure 2A] 2A-2D are cross-sectional side views of interconnects formed on a substrate at different stages of the method of FIG. 1 according to one or more embodiments. [Figure 2B] 2A-2D are cross-sectional side views of interconnects formed on a substrate at different stages of the method of FIG. 1 according to one or more embodiments. [Figure 2C] 2A-2D are cross-sectional side views of interconnects formed on a substrate at different stages of the method of FIG. 1 according to one or more embodiments. [Figure 2D] 2A-2D are cross-sectional side views of interconnects formed on a substrate at different stages of the method of FIG. 1 according to one or more embodiments. [Figure 2E] 2A-2D are cross-sectional side views of interconnects formed on a substrate at different stages of the method of FIG. 1 according to one or more embodiments. [Figure 2F] 2A-2D are cross-sectional side views of interconnects formed on a substrate at different stages of the method of FIG. 1 according to one or more embodiments. [Figure 2G] 2A-2D are cross-sectional side views of interconnects formed on a substrate at different stages of the method of FIG. 1 according to one or more embodiments. [Diagram 3] FIG. 2 illustrates a multi-chamber processing system capable of performing the method of FIG. 1 in accordance with one or more embodiments. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] For ease of understanding, the same reference numerals have been used, where possible, to designate identical elements common to the figures, and it is contemplated that elements and features of one embodiment may be beneficially incorporated in other embodiments unless specifically stated otherwise.
[0014] It should be noted, however, that the attached drawings depict only exemplary embodiments of the invention and therefore should not be considered as limiting the scope of the invention, since the invention may embrace other embodiments that are equally effective.
[0015] Before proceeding to describe some exemplary embodiments of the present disclosure, it should be understood that the present disclosure is not limited to the details of structure or process steps set forth in the following description, as the present disclosure may include other embodiments and may be practiced or carried out in various ways.
[0016] As used herein and in the appended claims, the term "substrate" refers to a surface or portion of a surface on which a process is performed. Furthermore, unless otherwise clear from the context, one skilled in the art will understand that a reference to a substrate may also be a reference to only a portion of the substrate. Furthermore, a reference to deposition on a substrate may refer to both a bare substrate and a substrate having one or more films or features deposited or formed thereon.
[0017] As used herein, "substrate" refers to any substrate or any material surface formed on a substrate on which a film treatment is performed during a manufacturing process. For example, substrate surfaces on which treatment can be performed include materials such as silicon, silicon oxide, strained silicon, silicon-on-insulator (SOI), carbon-doped silicon oxide, amorphous silicon, doped silicon, germanium, gallium arsenide, glass, sapphire, and any other materials such as metals, metal nitrides, metal alloys, and other conductive materials, depending on the application. Substrates include, but are not limited to, semiconductor wafers. Substrates can be subjected to pretreatment processes to polish, etch, reduce, oxidize, hydroxylate, anneal, UV cure, e-beam cure, and / or bake the substrate surface. In addition to performing film treatment directly on the surface of the substrate itself, the present disclosure also allows any of the disclosed film treatment steps to be performed on an underlying layer formed on the substrate, as disclosed in more detail below, and the term "substrate surface" is intended to include such underlying layers as the context dictates. Thus, for example, if a film / layer or partial film / layer is deposited on a substrate surface, the exposed surface of the newly deposited film / layer becomes the substrate surface.
[0018] Figure 1 is a flow diagram illustrating one embodiment of a method 100 for forming interconnects on a substrate. Figures 2A-2G show cross-sectional views of the substrate prior to and at different stages of the method 100 of Figure 1.
[0019] FIG. 2A illustrates a cross-sectional view of an interconnect 200 prior to beginning the method 100. In general, the interconnect 200 includes multiple film layers that can be utilized to form an interconnect structure, such as a dual damascene structure. A film stack 201 is formed on a substrate 202. The stack 201 includes a dielectric layer 204. The dielectric layer 204 is disposed on the substrate 202 as shown in FIG. 2A, and has a conductive layer 206 formed within and bounding the dielectric layer 204. In one example, the dielectric layer 204 can be formed from one or more insulating materials, such as silicon oxide. In one example, the conductive layer 206 can be formed from a conductive layer, such as copper.
[0020] In block 102, a dielectric barrier layer 208 is deposited on the substrate 202, as shown in FIG. 2B. For example, as shown, the dielectric barrier layer 208 is deposited on both the dielectric layer 204 and the conductive layer 206. Thus, the dielectric barrier layer 208 can form an uninterrupted, uniform layer on the dielectric layer 204 and the conductive layer 206. The dielectric barrier layer 208 can be formed from a low-k material. For example, the dielectric barrier layer 208 can be a silicon layer with carbon (SiC), a silicon layer with carbon doped with nitrogen (SiCN), a silicon nitride layer, a metal nitride, or a metal oxide (e.g., AlN, AlO x , AlON), etc.
[0021] At block 104, a dielectric layer 210 is deposited on the substrate 202, as shown in FIG. 2C. For example, as shown, the dielectric layer 210 is deposited on the dielectric barrier layer 208. The dielectric layer 210 can be substantially similar to the dielectric layer 204. In one embodiment, the dielectric layer 210 can be formed from the same material as the dielectric layer 204. In another embodiment, the dielectric layer 210 can be formed from a different material than the dielectric layer 204 but maintaining the same low-k attributes.
[0022] At block 106, as shown in FIG. 2D , one or more vias 212 are formed in the interconnect 200 to expose the conductive layer 206. For example, the vias 212 may be formed through both the dielectric layer 210 and the dielectric barrier layer 208 to expose the conductive layer 206 underneath. The vias 212 generally have a width W1. In some embodiments, the width of each via 212 is uniform over the entire length of the via 212. In other embodiments, the width of each via 212 may vary gradually from the top of the via 212 to the bottom of the via 212.
[0023] 2E, one or more trenches 214 are formed in the interconnect 200. The one or more trenches 214 may be formed in the dielectric layer 210. The trenches 214 are configured to widen at least a portion of the vias 212. In some embodiments, block 108 may be performed before block 106; that is, the trenches 214 may be formed before the vias 212. In other embodiments, such as the described embodiment, the trenches 214 are formed subsequent to the formation of the vias 212.
[0024] In a traditional manufacturing scheme, a "fill process" is performed to fill the vias 212 and trenches 214 with a metal material to form the interconnect 200. For example, a metal such as copper may be used to fill both the vias 212 and the trenches 214. It has been found that filling both the vias 212 and the trenches 214 with the same material results in a high interconnect resistance, which may lead to RC delays and IR drop in the semiconductor chip.
[0025] Interconnect resistance on a chip impacts chip speed as a result of power management due to RC delay and IR drop. As design rules continue to shrink, reducing interconnect resistance becomes an increasingly important priority. In particular, via (e.g., via 212) resistance accounts for a significant portion of the total resistance due to short interconnect lines, smaller via dimensions below 40 nm, and multiple layer routing with via stacks. That is, the resistance of the via is larger than the resistance of the interconnect line. Therefore, reducing the via resistance becomes increasingly important to achieve chip performance.
[0026] Conventional via formation leads to high resistance due to materials used in process integration. After block 108, conventional methods complete the via filling with metal barrier, liner and bulk fill metal. Metal barrier and liner are used for reliability and gap filling robustness. However, materials used for barrier and liner layers can lead to high via resistance when deposited at the bottom of the via as a result of their high resistivity. As an example, a conventional dual damascene copper fill may consist of a TaN barrier layer (deposited by a physical vapor deposition (PVD) process), a Ta metal liner layer (e.g., PVD or chemical vapor deposition (CVD) process) deposited on the barrier layer, and a Cu seed / plating layer deposited on the metal liner layer. The weight of the barrier and liner may account for about 50% to more than 90% of the total via resistance, depending on the via dimensions. Therefore, removing the metal barrier and liner layers may help reduce the via resistance. However, at the same time, potential risks may arise as a result of eliminating the barrier and liner layers. For example, the interconnects would still need to meet reliability concerns including avoiding dielectric breakdown and metal electromigration. Furthermore, proper metal fill process integration within the dual damascene structure may be required to improve both via resistance and line resistance.
[0027] Therefore, the following discussion proposes a selective filling technique (e.g., W filling technique) that exhibits smaller via resistance while meeting integration and reliability requirements. An interface treatment (discussed below in conjunction with at least block 110) and a filling process (discussed below in conjunction with at least block 118) are developed to selectively grow metal material (e.g., W) from the bottom of the via without damaging the underlying metal layer (e.g., Cu, W, Co, etc.) and the surrounding dielectric (e.g., low-k dielectric, oxide, etc.). As a result, the following discussion provides one or more techniques for reducing the via resistance. A damascene fill is performed following the via fill. This damascene fill helps to form an equivalent line resistance.
[0028] The improved method 100 includes using selective metal via fill to reduce resistance and meet reliability requirements (interaction with sidewall dielectric 204 and exposed conductive layer 206) and line resistance requirements. At block 110, one or more pre-treatment processes are performed on the interconnect 200 to prepare the interconnect 200 for receiving the selective metal via 212 fill. For example, block 110 may include sub-blocks 112-116.
[0029] At sub-block 112, the interconnect 200 is subjected to a first treatment process on the exposed portion of the conductive layer 206 in the via 212. For example, a first pre-treatment process is used to prepare the exposed portion of the conductive layer 206 for bottom-up growth when a first metal is deposited in the via 212. A remote plasma cleaning process can be used to pre-treat the interconnect. The interconnect 200 can be transferred to a pre-treatment chamber where the interconnect 200 is subjected to a cleaning process. For example, the interconnect can be subjected to a cleaning process using a H2 / Ar mixture at a temperature between about 250-350°C and a pressure of about 1-10 Torr. In other embodiments, a slight bias energy can be applied to facilitate oxide knock-off without metal sputtering. For example, an energy of 0-200 W can be applied to the pre-treatment chamber.
[0030] At sub-block 114, the interconnect 200 is subjected to a second pre-treatment process. This second treatment process is used to passivate the sidewalls 216 of the vias to minimize undesired sidewall growth. As mentioned above, the dielectric layer 204 may be formed from a low-k material. As such, this second pre-treatment process helps seal surface pores of the dielectric layer 204 and protect the dielectric layer 204 from soaking precursors. In one embodiment, this second pre-treatment process may be a thermal precursor soak at high temperature (e.g., 200-400° C.). In some examples, precursors that may be used are tetramethylsilane (TMS), dimethylaminotrimethylsilane (DMATMS), and the like. In one embodiment, the second pre-treatment process at sub-block 114 may further include adding UV energy to the precursor soak process by subjecting the interconnect 200 to an ultraviolet (UV) bake process.
[0031] In some embodiments, block 110 may include sub-block 116. In block 116, interconnect 200 is subjected to an optional post-processing clean. For example, this optional pre-processing clean may be used if oxidation or residue growth occurs at the bottom of via 212. This optional pre-processing clean uses an alkaline pH adjusted chemistry that includes peroxide (e.g., H2O2) to lightly strip away residue.
[0032] Following the pre-treatment process (block 110), in block 118, the via 212 is selectively filled with metal 220 as shown in FIG. 2F. For example, metal 220 material is deposited in the via 212 up to the point 222 where the via 212 meets the trench 214. The metal 220 used can be any suitable metal material such as ruthenium (Ru), tungsten (W), cobalt (Co), aluminum (Al), copper (Cu), etc. The main requirement for the metal 220 is that it is a different material than the subsequent metal deposited in the trench 214. Selectively depositing the metal 220 in the via helps to reduce the via resistance as well as meet reliability and line resistance requirements.
[0033] The metal 220 can be deposited using a chemical vapor deposition (CVD) process. The CVD process can include a H2 pre-soak at high temperature (e.g., 350-500°C). The CVD process can be performed in a very wide H2 ambient environment using a small flow rate (e.g., 2-100 sccm) of a metal-containing precursor (e.g., WF6) at a temperature of about 200-500°C. This combination of flow rate, pressure, and temperature helps reduce the morphology of the metal 220 as deposited. A conventional nucleation layer can be applied prior to depositing the metal 220 material for the first 1-3 nm of nucleation. To uniformly fill the vias 212, the overall growth volume is controlled by process time, pressure, and precursor flow rates.
[0034] At block 120, a second metal 224 is deposited in each trench 214, as shown in FIG. 2G. For example, the second metal 224 is deposited from point 222 to the top of the trench 214. The second metal 224 used can be any suitable metal material, such as ruthenium (Ru), tungsten (W), cobalt (Co), aluminum (Al), copper (Cu), etc. The main requirement of the second metal 224 is that it is a different material than the first metal 220 material deposited in the via 212. The second metal 224 can be deposited using a CVD process. Splitting the conventional metal filling of a single metal material into a two-step process that includes depositing the first metal 220 in the via 212 and depositing the second metal 224 in the trench 214 helps reduce the resistance of the via 212.
[0035] In some embodiments, a barrier seed layer (not shown) may be deposited on the first metal 220 prior to depositing the second metal 224. For example, if the second metal 224 is copper, the barrier seed layer may be a copper barrier seed layer.
[0036] In some embodiments, the method 100 may include an optional block 119 that is performed prior to depositing the second metal 224. In block 119, the interconnect 200 may be subjected to a pretreatment process prior to the second metal 224. This pretreatment process may be used to remove oxide that may have formed on the top surface of the first metal 220. For example, the interconnect 200 may be subjected to a process similar to sub-block 112.
[0037] 3 shows a multi-chamber processing system 300. The processing system 300 can include load lock chambers 302, 304, a robot 306, a transfer chamber 308, processing chambers 310, 312, 314, 316, 318, 328, and a controller 320. The load lock chambers 302, 304 allow for the transfer of substrates (not shown) into and out of the processing system 300. The load lock chambers 302, 304 can pump down substrates introduced into the processing system 300 to maintain a vacuum seal. The robot 306 can transfer substrates between the load lock chambers 302, 304 and the processing chambers 310, 312, 314, 316, 318, and 328. The robot 306 can further transfer substrates between the load lock chambers 302, 304 and the transfer chamber 308.
[0038] Each processing chamber 310, 312, 314, 316, 318, and 328 may be equipped to perform several substrate operations, such as atomic layer deposition (ALD), chemical vapor deposition (CVD), PVD, etching, pre-cleaning, degassing, heating, orientation, or other substrate processes. Additionally, each processing chamber 310, 312, 314, 316, 318, and 328 may be equipped to deposit a dielectric barrier layer, deposit a dielectric layer, form one or more vias and trenches in the stack, perform one or more pre-cleaning processes, deposit a first metal material layer, and deposit a second metal material layer.
[0039] The controller 320 may be configured to operate all aspects of the processing system 300, such as the method disclosed in FIG. 1. For example, the controller 320 may be configured to control a method of forming interconnects on a substrate. The controller 320 includes a programmable central processing unit (CPU) 322 coupled to various components of the processing system to facilitate control of substrate processing, the programmable CPU 322 operable with memory 324 and mass storage devices, such as power supplies, clocks, cache, input / output (I / O) circuits and liners, input control units, and a display unit (not shown). The controller 320 further includes hardware for monitoring substrate processing by sensors in the processing system 300, including sensors monitoring precursor, process gas, and purge gas flows. Other sensors measuring system parameters, such as substrate temperature, chamber air pressure, etc., may also provide information to the controller 320.
[0040] To facilitate control of the processing system 300 described above, the CPU 322 can be one of any form of general-purpose computer processor for controlling various chambers and sub-processors that can be used in an industrial setting, such as a programmable logic controller (PLC). A memory 324 is coupled to the CPU 322, and is non-transient, and can be one or more of readily available local or remote memories, such as random access memory (RAM), read-only memory (ROM), floppy disk drive, hard disk, or other forms of digital storage. Support circuits 326 are coupled to the CPU 322 for supporting the processor in a conventional manner. The memory 324 typically has charged species generation, heating, and other processes stored therein, typically as software routines. The software routines can also be stored and / or executed by a second CPU (not shown) located remotely from the hardware that the CPU 322 controls.
[0041] The memory 324 takes the form of a computer-readable storage medium that includes instructions that, when executed by the CPU 322, facilitate the operation of the processing system 300. The instructions in the memory 324 take the form of a program product, such as a program implementing the methods of the present disclosure. The program code can be in any one of a number of different programming languages. In one example, the present disclosure can be implemented as a program product stored on a computer-readable storage medium for use with a computer system. The program(s) of the program product define the functions of the embodiments (including the methods described herein). Exemplary computer-readable storage media include, but are not limited to, (i) a non-writable storage medium on which information is permanently stored (e.g., a read-only memory device in a computer, such as a CD-ROM disk readable by a CD-ROM drive, a flash memory, a ROM chip, or any type of solid-state non-volatile semiconductor memory), and (ii) a writable storage medium on which changeable information is stored (e.g., a floppy disk in a diskette drive or a hard disk drive or any type of solid-state random access semiconductor memory). Such computer-readable storage media, when carrying computer-readable instructions that direct the functions of the methods described herein, are embodiments of the present disclosure.
[0042] The methods discussed above are not tied solely to the processing system 300. For example, one or more blocks, such as block 120 or sub-block 114, may be performed in a processing chamber outside the processing system 300.
[0043] One or more embodiments of the present disclosure are directed to a low temperature method for depositing tungsten. Some embodiments of the present disclosure selectively deposit tungsten on a metal surface over a dielectric surface.
[0044] Some embodiments of the present disclosure advantageously provide methods of depositing tungsten that provide films with less roughness, less stress and / or fewer impurities.Some embodiments of the present disclosure provide methods of depositing tungsten that are performed at lower temperatures to facilitate applications requiring small thermal budgets.
[0045] Disclosed herein are methods for depositing tungsten. In some embodiments, the methods disclosed herein correspond to block 118, described above. In some embodiments, the tungsten deposited by the methods disclosed herein corresponds to metal 220, described above.
[0046] An exemplary method includes exposing the substrate to a flow of hydrogen gas (H2) and exposing the substrate to a flow of a tungsten precursor while exposing the substrate to the flow of hydrogen gas.
[0047] In some embodiments, the flow of hydrogen gas and the flow of the tungsten precursor are both continuous flows. It should be understood by those skilled in the art that this continuous flow of both hydrogen gas and the tungsten precursor corresponds to a chemical vapor deposition (CVD) process. In some embodiments, the flow of the tungsten precursor is a pulsed flow and the flow of hydrogen gas is a continuous flow. It should be understood by those skilled in the art that this pulsed flow of the tungsten precursor and the continuous flow of the hydrogen gas corresponds to a pulsed CVD process.
[0048] As discussed above, in some embodiments, the method may begin with thermally soaking the substrate in a hydrogen (H2) environment. In some embodiments, the thermally soaking in the hydrogen environment may be performed after depositing tungsten. In some embodiments, the method includes depositing a first amount of tungsten, performing a thermal soak, and depositing a second amount of tungsten. In some embodiments, the thermal soak is performed at a temperature in the range of about 250° C. to about 600° C., in the range of about 300° C. to about 500° C., in the range of about 300° C. to about 400° C., or in the range of about 400° C. to about 500° C.
[0049] In some embodiments, the methods disclosed herein are carried out at relatively low temperatures. As explained above, in some embodiments, the substrate is maintained at a temperature in the range of about 200° C. to about 500° C. In some embodiments, the substrate is maintained at a temperature in the range of about 200° C. to about 400° C., about 250° C. to about 375° C., about 300° C. to about 350° C., or about 250° C. to about 350° C. In some embodiments, the substrate is maintained at a temperature of about 400° C. or less, about 375° C. or less, about 350° C. or less, about 325° C. or less, or about 300° C. or less.
[0050] In some embodiments, the flow rate of the hydrogen gas and / or the tungsten precursor is controlled. In some embodiments, the flow rate of the hydrogen gas is in the range of about 2000 sccm to about 20000 sccm, in the range of about 2000 sccm to about 18000 sccm, in the range of about 5000 sccm to about 20000 sccm, or in the range of about 10000 sccm to about 20000 sccm. In some embodiments, the flow rate of the tungsten precursor is about 500 sccm or less, about 200 sccm or less, about 100 sccm or less, or about 50 sccm or less.
[0051] In some embodiments, the ratio between the flow rate of hydrogen gas and the flow rate of the tungsten precursor is controlled. In some embodiments, the ratio between the flow rate of hydrogen gas and the flow rate of the tungsten precursor is about 100:1 or more, about 200:1 or more, about 500:1 or more, or about 1,000:1 or more, about 5,000:1 or more, or about 10,000:1 or more. Without being bound by theory, it is believed that the beneficial results in the tungsten film (such as reduced roughness and reduced stress) are due to the presence of excess hydrogen in the processing chamber.
[0052] In some embodiments, the pressure of the process chamber is controlled. In some embodiments, the chamber pressure is maintained in the range of about 5 Torr to about 50 Torr, in the range of about 10 Torr to about 50 Torr, in the range of about 20 Torr to about 50 Torr, in the range of about 5 Torr to about 20 Torr, or in the range of about 5 Torr to about 10 Torr. In some embodiments, the chamber pressure is maintained at about 50 Torr or less.
[0053] The tungsten precursor can be any precursor suitable for depositing a tungsten film. In some embodiments, the tungsten precursor comprises a reactive tungsten species and a carrier gas. In some embodiments, the tungsten precursor comprises a reactive tungsten complex and a carrier gas. In some embodiments, the tungsten precursor comprises WF6, W x Cl 5x , WCl6 or W(CO)6.
[0054] In some embodiments, the tungsten precursor comprises or consists essentially of WF. As used in this regard, a tungsten precursor consists essentially of WF when, on a molar basis excluding carrier gas, about 95% or more, about 98% or more, about 99% or more, or about 99.5% or more of the reactive tungsten species is WF.
[0055] In some embodiments, the tungsten deposited by the disclosed methods has a relatively low level of impurities. In embodiments in which the tungsten precursor comprises WF6, the deposited tungsten has a relatively low level of impurities. 20 atoms / cm 3 Below, approximately 5×10 19 atoms / cm 3 Below, about 10 19 atoms / cm 3 Below, approximately 5×10 18 atoms / cm 3 Less than or equal to 10 18 atoms / cm 3 It has the following fluorine content:
[0056] In some embodiments, the deposited tungsten has a relatively low surface roughness, hi some embodiments, the root mean squared roughness of the deposited tungsten is about 2 nm or less, about 1.5 nm or less, about 1 nm or less, or about 0.5 nm or less.
[0057] In some embodiments, the stress of the deposited tungsten is relatively low, ie, the stress of the deposited tungsten is about 2000 MPa or less, about 1500 MPa or less, about 1200 MPa or less, about 1000 MPa or less, about 800 MPa or less, about 500 MPa or less, or about 200 MPa or less.
[0058] In some embodiments, the substrate includes multiple exposed materials. In some embodiments, the substrate includes a first material surface and a second material surface. As identified above, the first material surface can include a metal or metal alloy. In some embodiments, the metal is selected from one or more of copper, tungsten, cobalt, or ruthenium. Additionally, the second material surface can include one or more of a low-k dielectric, an oxide, silicon nitride, silicon oxynitride, and the like.
[0059] In some embodiments, the methods described herein selectively deposit tungsten on a first material surface over a second material surface. Stated another way, in some embodiments, a first thickness of tungsten is deposited on the first material surface and a second thickness of tungsten is deposited on the second material surface. The first thickness is greater than the second thickness. In some embodiments, the ratio of the first thickness to the second thickness is about 100:1 or greater, about 200:1 or greater, about 250:1 or greater, about 500:1 or greater, about 700:1 or greater, or about 1,000:1 or greater.
[0060] While the forgoing is directed to embodiments of the present invention, other and additional embodiments of the invention may be devised without departing from the basic scope thereof, the scope of the invention being determined by the appended claims.
[0061] Throughout this specification, reference to "one embodiment," "certain embodiments," "one or more embodiments," or "an embodiment" means that a particular feature, structure, material, or characteristic described with respect to that embodiment is included in at least one embodiment of the disclosure. Thus, the appearance of phrases such as "in one or more embodiments," "in certain embodiments," "in one embodiment," or "in an embodiment" in various places throughout this specification do not necessarily refer to the same embodiment of the disclosure. Furthermore, the particular features, structures, materials, or characteristics may be combined in any suitable manner in one or more embodiments.
[0062] Although the present disclosure has been described herein with reference to specific embodiments, those skilled in the art will recognize that the described embodiments are merely illustrative of the principles and applications of the present disclosure. It will be apparent to those skilled in the art that various modifications and variations can be made to the disclosed method and apparatus without departing from the spirit and scope of the present disclosure. Thus, the present disclosure may include modifications and variations that come within the scope of the appended claims and their equivalents.
Claims
1. 1. A method for selectively depositing tungsten, the method comprising: exposing a substrate including a first material surface including a metal and a second material surface including a low-k dielectric to a continuous flow of hydrogen gas; exposing the substrate to a pulsed flow of a tungsten precursor while exposing the substrate to the continuous flow of hydrogen gas to deposit a tungsten layer on the substrate, depositing a first thickness of tungsten on the first material side and a second thickness of tungsten on the second material side. a ratio of the first thickness to the second thickness of about 200:1 or greater; The tungsten precursor comprises a reactive tungsten species and a carrier gas, or a reactive tungsten complex and a carrier gas; method.
2. The method of claim 1 , wherein the substrate is maintained at a temperature of about 350° C. or less.
3. 10. The method of claim 1 , wherein the ratio of the flow of hydrogen gas to the flow of the tungsten precursor is about 500:1 or greater.
4. The method of claim 1, wherein the tungsten layer has a root mean square roughness of about 1 nm or less.
5. The method of claim 1, wherein the stress of the tungsten layer is less than about 1000 MPa.
6. The method of claim 1, wherein the tungsten precursor comprises WF 6 .
7. The method of claim 4, wherein the tungsten layer has a fluorine concentration of about 10 19 atoms / cm 3 or less.
Citation Information
Patent Citations
Vapor growth method
JP1988065076A
Laminated tungsten film and formation thereof
JP1994196392A
Method of manufacturing semiconductor device
JP2011029554A
Low fluorine tungsten deposition by subsequent CVD process
JP2017008412A
Method for manufacturing semiconductor device, apparatus for processing substrate, gas-supply system and program