Holding pad, manufacturing method thereof, and manufacturing method of polished product

The holding pad with controlled adsorption force and water retention properties addresses the issue of flatness and edge shape in polishing, enhancing the polishing process by facilitating easier rotation and improved surface quality.

JP7553256B2Active Publication Date: 2024-09-18FUJIBO HLDG
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020049551
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-19
Publication Date
2024-09-18
Estimated Expiration
2040-03-19

AI Technical Summary

Technical Problem

Conventional polishing pads and methods fail to achieve adequate flatness and edge shape in polished objects due to insufficient consideration of the adsorption force between the object and the holding pad, leading to uneven pressure application and suppressed rotation, which deteriorates the shape and flatness of the polished surface.

Method used

A holding pad with a resin sheet having air bubbles, specific pore dimensions, and water retention properties, allowing for controlled adsorption force and improved water retention, enabling easier rotation and enhanced flatness and edge shape during polishing.

Benefits of technology

The holding pad improves the flatness and edge shape of polished objects by maintaining a suitable adsorption force and reducing dynamic friction, resulting in better polishing outcomes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007553256000002
    Figure 0007553256000002
  • Figure 0007553256000003
    Figure 0007553256000003
  • Figure 0007553256000001
    Figure 0007553256000001
Patent Text Reader

Abstract

To provide a holding pad which can impart good flatness and end shape to a polished product after polishing.SOLUTION: A holding pad has a resin sheet having a holding surface for holding a polished object, in which the resin sheet has air bubbles therein, a wall ratio W100 of the resin at a depth of 100 μm from the holding surface is 20.0% or more and 40.0% or less, the holding surface has an aperture having an average opening diameter of 20 μm or more and 50 μm or less, an aperture rate of the holding surface is 20% or more and 40% or less, and water penetration time when water of 1.0 μL is dropped onto the holding surface is 500 seconds or longer and 1,500 seconds or shorter.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a holding pad, a manufacturing method thereof, and a manufacturing method of a polished product. [Background technology]

[0002] Conventionally, polishing using a polishing pad has been performed on materials such as semiconductor devices and electronic components, particularly materials that require good edge shape and / or flatness, such as Si substrates (silicon wafers), GaAs (gallium arsenide) substrates, glass, and LCD (liquid crystal display) substrates. In order to improve the flatness and surface quality of the object to be polished, various polishing pads and polishing methods have been proposed.

[0003] For example, Patent Document 1 discloses a polishing body for wafer polishing (polishing pad) characterized in that, in a polishing body consisting of a polishing cloth or a polishing plate that polishes a wafer (object to be polished) while sliding against the wafer with a relative speed difference, grooves are provided at predetermined intervals on the wafer sliding surface of the polishing body, and the groove density in the part where the peripheral speed of the polishing body is high is increased compared to the groove density in the part where the peripheral speed is low. Patent Document 1 discloses that by using such a polishing pad, the wafer or wafer holding jig rotates stably, improving the flatness of the polished wafer. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 11-285963 Summary of the Invention [Problem to be solved by the invention]

[0005] However, after the inventors conducted a detailed study of conventional polishing pads and polishing methods, including that described in Patent Document 1 above, they found that with conventional polishing pads and polishing methods, at least one of the flatness and end shape of the resulting polished object was insufficient.

[0006] For example, the method described in Patent Document 1 adjusts the groove density of the polishing cloth so that the polished object rotates on its own axis, but such rotation is affected by the adhesive force between the polished object and the holding pad that holds it. However, Patent Document 1 does not specifically consider the adhesive force between the polished object and the holding pad. In this regard, if the adhesive force between the polished object and the holding pad for holding the polished object is low, it is difficult to apply pressure evenly to the polished object, which causes the flatness of the polished object to decrease and the edge shape to deteriorate. Conversely, if the adhesive force between the polished object and the holding pad for holding the polished object is increased, the rotation of the polished object is suppressed, which causes the flatness of the polished object to decrease. Therefore, a holding pad that can impart good flatness and edge shape to the polished object regardless of the level of adhesive force between the polished object and the holding pad for holding the polished object is required.

[0007] The present invention has been made in consideration of the above problems, and aims to provide a holding pad that can impart good flatness and end shape to a polished object after polishing, a manufacturing method thereof, and a manufacturing method for a polished product. [Means for solving the problem]

[0008] The inventors of the present invention have conducted extensive research to solve the above problems, and have found that when an object to be polished is polished using a holding pad whose holding surface has a certain amount of pores, is highly water absorbent, and has a certain range of wall thickness between bubbles near the surface, the object to be polished can rotate easily while maintaining the adhesive force between the object to be polished and the holding pad within a suitable range. As a result, the inventors have found that the flatness of the object to be polished is improved and the end shape is improved, and have completed the present invention.

[0009] That is, the present invention is as follows. [1] A holding pad including a resin sheet having a holding surface for holding an object to be polished, The resin sheet has air bubbles therein, The resin wall ratio W at a depth of 100 μm from the holding surface 100 is between 20.0% and 40.0%, The support surface has pores with an average pore size of 20 μm or more and 50 μm or less, The porosity of the holding surface is 20% or more and 40% or less, When 1.0 μL of water is dropped onto the support surface, the penetration time of the water is 500 seconds or more and 1500 seconds or less. Holding pad. [2] The holding pad according to [1], wherein the 100% modulus at 23±2° C. of the resin constituting the resin sheet is 5.0 MPa or more and 20.0 MPa or less. [3] The holding pad according to [1] or [2], wherein the kinetic friction force of the resin sheet in a water-immersed state is 3.0 kgf or more and 5.5 kgf or less. [4] The holding pad according to any one of [1] to [3], further comprising an adhesive sheet on the side of the resin sheet opposite to the holding surface. [5] A step of applying a resin solution containing a resin dissolved in an organic solvent onto a film-forming substrate and coagulating the resin solution in a water-based coagulation liquid to obtain a resin sheet; and stretching the obtained resin sheet. A method for manufacturing a holding pad. [6] A holding step of holding an object to be polished on the holding pad according to any one of [1] to [4]; A polishing step of polishing the held object to be polished with a polishing pad. Manufacturing method of polished products. Effect of the Invention

[0010] According to the present invention, it is possible to provide a holding pad capable of imparting good flatness and edge shape to an object to be polished after polishing, a method for manufacturing the same, and a method for manufacturing a polished product. [Brief description of the drawings]

[0011] [Figure 1] 4 is a schematic cross-sectional view of a resin sheet in the holding pad of the present embodiment. FIG. [Diagram 2] 3A to 3C are schematic diagrams illustrating a method of polishing an object to be polished using the holding pad of the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, an embodiment of the present invention (hereinafter referred to as "the present embodiment") will be described in detail with reference to the drawings as necessary, but the present invention is not limited to this, and various modifications are possible without departing from the gist of the present invention. In the drawings, the same elements are given the same symbols, and duplicated explanations will be omitted. Furthermore, unless otherwise specified, positional relationships such as up, down, left, and right are based on the positional relationships shown in the drawings. Furthermore, the dimensional ratios of the drawings are not limited to those shown in the drawings.

[0013] [Retention pad] The holding pad of this embodiment is a holding pad including a resin sheet having a holding surface for holding an object to be polished, the resin sheet has air bubbles inside, and a resin wall ratio W at a depth of 100 μm from the holding surface is 100 is 20.0% or more and 40.0% or less, the holding surface has pores with an average pore size of 20 μm or more and 50 μm or less, the porosity of the holding surface is 20% or more and 40% or less, and the penetration time of water when 1.0 μL of water is dropped on the holding surface is 500 seconds or more and 1500 seconds or less.

[0014] When an object to be polished is held by the above-mentioned holding pad and then polished, the flatness of the resulting object to be polished is improved and the end shape is also improved, and the reasons for this are thought to be as follows, although the reasons are not limited to those mentioned below.

[0015] When the holding surface of the resin sheet has pores with an average pore size of 20 μm or more and 50 μm or less, and the porosity is 20% or more and 40% or less, the holding surface is more likely to hold water. In addition, when the penetration time of water when 1.0 μL of water is dropped on the holding surface is 500 seconds or more and 1500 seconds or less, the resin sheet becomes hydrophilic and the water retention of the resin sheet is improved. Furthermore, the wall ratio W of the resin at a depth of 100 μm from the holding surface is 100 However, when the ratio is 20.0% or more and 40.0% or less, the proportion of air bubbles in the vicinity of the holding surface of the resin sheet increases, and the water retention in the vicinity of the holding surface is further improved.

[0016] In this way, the holding pad having the above configuration is more likely to hold water on the holding surface during polishing, so the amount of water intervening between the holding pad and the object to be polished during polishing increases. As a result, water functions as a lubricant between the holding pad and the object to be polished, so the dynamic friction force on the holding surface decreases, the object to be polished is more likely to rotate, the flatness of the object to be polished is improved, and the end shape is improved. It is also considered that the polishing rate is improved because the object to be polished is more likely to rotate. Furthermore, when the amount of water intervening between the holding pad and the object to be polished during polishing increases, the force of the holding pad to adsorb the object to be polished (hereinafter also referred to as the "adsorption force of the holding pad") increases due to the surface tension of water, so the adsorption force of the holding pad can be set to a suitable range. As a result, the tracking ability of the holding pad to the object to be polished is more improved, the flatness of the object to be polished is more improved, and the end shape is improved.

[0017] In this embodiment, "the flatness of the workpiece is improved" means that the polished surface of the workpiece is flatter overall. This can also be said to have good global flatness. Furthermore, "the end shape is improved" means that the end of the polished surface of the workpiece is flatter. This means, for example, that the sagging shape (also called "roll-off") and the jumping shape (also called "ski-jump shape") that occur on the outer periphery of the workpiece are suppressed.

[0018] [Resin sheet] A schematic cross-sectional view of a resin sheet is shown in Fig. 1. As shown in Fig. 1, a resin sheet 1 of this embodiment has a holding surface 2 for holding an object to be polished, and has air bubbles 3 inside.

[0019] By soaking the holding surface 2 of the resin sheet with an appropriate amount of water 4 and pressing the workpiece W against it, the workpiece W can be held by the interaction between the holding surface 2 and the surface of the workpiece W. The holding surface may be designed to be larger than the workpiece W so that it can easily hold the workpiece, or may be configured to hold multiple works simultaneously.

[0020] Furthermore, the structure of the resin sheet 1 in this embodiment is not particularly limited, but preferably has a film (skin layer) as the support surface 2, and has vertically elongated air bubbles 3 in the thickness direction below the skin layer. The air bubbles 3 may have an open cell structure in which the air bubbles communicate with each other. Examples of the vertically elongated air bubbles 3 include air bubbles having a shape in which the air bubble diameter gradually decreases toward the skin layer along the thickness direction of the resin sheet in this embodiment.

[0021] The shape of the bubbles contained inside the resin sheet is not particularly limited, but examples thereof include an approximately spherical shape, a cone shape, and a spindle shape. In the case of a cone shape or a spindle shape, a cone shape that is long in the thickness direction of the resin sheet and a spindle shape are preferable. When the resin sheet contains bubbles having such a shape, the water retention of the resin sheet is further improved, and the amount of water interposed between the holding pad and the polished object during polishing is further increased. As a result, the flatness of the obtained polished object is further improved, and the end shape is further improved. Furthermore, the polishing rate is also further improved. In addition, when the resin sheet has cone-shaped or spindle-shaped bubbles that are long in the thickness direction of the resin sheet, the wall ratio W 100 Therefore, it becomes easier to configure a resin sheet that satisfies the above requirements.

[0022] Resin wall ratio W at a depth of 100 μm from the holding surface of the resin sheet 100is 20.0% or more and 40.0% or less, and preferably 22.0% or more and 39.0% or less. 100 By being in the above range, the water retention near the holding surface is further improved, so that the amount of water interposed between the holding pad and the workpiece during polishing is further increased. As a result, the flatness of the resulting workpiece is further improved, and the end shape is further improved. Furthermore, the polishing rate is further improved.

[0023] Here, the "wall ratio W" is a value indicating the ratio of resin to bubbles, and is an index of the bubble structure. In this specification, the wall ratio W is defined as the ratio of resin in a cross section at a predetermined depth from the holding surface of the resin sheet, that is, it is defined by the following formula (1). The wall ratio W can be measured by the method described in the examples. Wall ratio W(%)=100×{Ap / (Ap+Ab)} (1) Ap: The area of ​​the resin portion in the cross section of the resin sheet at a given depth Ab: Area of ​​the cross section of the resin sheet at a given depth that is occupied by the air bubble portion

[0024] Therefore, when the wall ratio at a given depth is close to 100%, it indicates that there is a large amount of resin component at that depth, i.e., there are few air bubbles, whereas when the wall ratio is close to 0%, it indicates that there are many air bubbles.

[0025] In addition, the wall ratio W 100 is not particularly limited, but can be controlled, for example, by adjusting the content of an organic solvent in a resin solution, stretching a resin sheet, and adjusting the stretching ratio in the manufacturing method described later. The larger the content of an organic solvent in a resin solution, the larger the bubbles formed tend to be and the smaller the wall ratio tends to be, and the smaller the content of an organic solvent, the larger the wall ratio tends to be. In addition, by stretching a resin sheet, the wall ratio becomes smaller compared to the resin sheet before stretching, and the wall ratio can be adjusted by the stretching ratio.

[0026] The resin sheet has openings on the holding surface. The average opening diameter of the openings is 20 μm or more and 50 μm or less, preferably 25 μm or more and 48 μm or less, and more preferably 30 μm or more and 45 μm or less. When the average opening diameter of the openings on the holding surface is within the above range, the holding surface is more likely to hold water, and the amount of water interposed between the holding pad and the workpiece during polishing is further increased. As a result, the flatness of the obtained workpiece is further improved, and the end shape is further improved. Furthermore, the polishing rate is further improved.

[0027] The porosity of the holding surface is 20% or more and 40% or less, preferably 22% or more and 38% or less, and more preferably 23% or more and 35% or less. When the porosity of the holding surface is in the above range, the holding surface is more likely to hold water, and the amount of water interposed between the holding pad and the workpiece during polishing is further increased. As a result, the flatness of the obtained workpiece is further improved, and the end shape is further improved. Furthermore, the polishing rate is further improved.

[0028] The average diameter of the holes and the hole ratio of the support surface can be measured by the method described in the Examples. The method for controlling the average diameter of the holes and the hole ratio of the support surface is not particularly limited, but for example, the above wall ratio W 100 In addition, the surface of the resin sheet that will become the holding surface can be buffed or sliced ​​to appropriately adjust the thickness.

[0029] In the resin sheet, the penetration time of water when 1.0 μL of water is dropped onto the supporting surface is 500 to 1500 seconds, preferably 600 to 1400 seconds, and more preferably 700 to 1350 seconds.

[0030] By setting the penetration time within the above range, the resin sheet becomes moderately hydrophilic, and the water retention of the resin sheet is further improved. As a result, the amount of water present between the holding pad and the workpiece during polishing is further increased, so that the flatness of the resulting workpiece is further improved, and the end shape is further improved. Furthermore, the polishing rate is further improved.

[0031] The penetration time can be measured by the method described in the Examples. The penetration time can be controlled by appropriately selecting or adjusting the resin components constituting the resin sheet, the average pore size and the pore ratio of the holding surface, and the wall ratio. For example, the penetration time tends to be shorter when a preferred resin, particularly a resin with high hydrophilicity, as described below is used. The penetration time also tends to be shorter when the average pore size and the pore ratio of the holding surface are increased. Furthermore, the penetration time also tends to be shorter when the wall ratio is decreased.

[0032] The kinetic friction force of the resin sheet in the water-immersed state is 3.0 kgf or more and 5.5 kgf or less, preferably 3.2 kgf or more and 5.0 kgf or less. When the kinetic friction force in the water-immersed state is in the above range, the polished object rotates more easily, so that the flatness of the polished object obtained is further improved, and the edge shape is further improved. Furthermore, the polishing rate is further improved.

[0033] The term "submerged state" refers to a state in which the resin sheet is immersed in ion-exchanged water for 15 minutes and then the water on the surface is wiped off. The kinetic friction force in the submerged state is measured by the method described in the Examples.

[0034] The kinetic friction force in a water-submerged state tends to be reduced by increasing the water content of the resin sheet. 100 The dynamic frictional force in the water-soaked state tends to be lower when the average pore size and the pore ratio of the holding surface are increased, or the permeation time is shortened. In addition, the dynamic frictional force in the water-soaked state tends to be lower when a preferred resin, particularly a resin with high hydrophilicity or a resin with a small dynamic friction coefficient, is used, as described below.

[0035] To more effectively and reliably achieve the effects of the present invention, the average thickness of the resin sheet is preferably 0.30 mm or more and 3.0 mm or less, more preferably 0.35 mm or more and 2.0 mm or less, and even more preferably 0.35 mm or more and 1.5 mm or less.

[0036] (resin) The resin constituting the resin sheet is not particularly limited, and examples thereof include polyurethane resin, polysulfone resin, polyimide resin, and other resins used in the resin sheet portion of conventional polishing pads. From the viewpoint of more effectively and reliably achieving the effects of the present invention, the resin constituting the resin sheet preferably includes a resin having high hydrophilicity or a resin having a small dynamic friction coefficient. Examples of highly hydrophilic resins include polyurethane resins. The resin constituting the resin sheet may be used alone or in combination of two or more.

[0037] The polyurethane resin is not particularly limited, but examples thereof include polyester-based polyurethane resins, polyether-based polyurethane resins, polyester-ether-based polyurethane resins, and polycarbonate-based polyurethane resins. The polyurethane resins may be used alone or in combination of two or more.

[0038] The resin sheet may contain other additives. The other additives are not particularly limited as long as they can be used in the resin sheet in the holding pad, and examples thereof include pigments such as carbon black, film formation stabilizers such as nonionic surfactants, and foaming regulators such as anionic surfactants. From the viewpoint of reducing the kinetic frictional force of the resin sheet in a water-soaked state, the resin sheet preferably contains a film formation stabilizer such as a nonionic surfactant and / or a foaming regulator such as an anionic surfactant.

[0039] The 100% modulus of the resin constituting the resin sheet at 23±2° C. is preferably 5.0 MPa or more and 20.0 MPa or less, more preferably 5.5 MPa or more and 10.0 MPa or less, and even more preferably 6.0 MPa or more and 9.0 MPa or less. By having the 100% modulus in the above range, the polished object can be more appropriately sunk into the holding pad, and the flatness of the obtained polished object is further improved, and the end shape is further improved.

[0040] The "100% modulus" is the value obtained by dividing the tensile force when a sheet made of the resin is stretched 100%, i.e., when stretched to twice its original length, by the initial cross-sectional area of ​​the test piece. The 100% modulus of the resin at 23±2°C can be measured by the method described in the Examples.

[0041] [Adhesive sheet] The holding pad of this embodiment may further include an adhesive sheet on the side opposite to the holding surface of the resin sheet, which allows the holding pad to be fixed to the polishing apparatus.

[0042] The adhesive contained in the adhesive sheet is not particularly limited, but examples thereof include polyamide-based adhesives, polyester-based adhesives, ethylene-vinyl acetate-based adhesives, acrylic-based adhesives, olefin-based adhesives, epoxy-based adhesives, cyanoacrylate-based adhesives, polyurethane-based adhesives, and silicone-based adhesives.

[0043] The adhesive sheet is not particularly limited as long as it can bond the polishing device and the holding pad, but examples thereof include a substrate having the above-mentioned adhesive applied to both sides thereof. Examples of such substrates include, but are not particularly limited to, substrates made of aromatic ester resins and substrates made of PET resins.

[0044] The method for manufacturing the holding pad of this embodiment is not particularly limited as long as it is a method that can manufacture a holding pad having the above-mentioned configuration, but for example, the method for manufacturing the holding pad described below can be suitably used.

[0045] [Manufacturing method of holding pad] The manufacturing method of the retaining pad of this embodiment includes a solidification process in which a resin solution containing a resin dissolved in an organic solvent is applied onto a film-forming substrate and the resin solution is solidified in a water-based coagulation liquid to obtain a resin sheet, and a stretching process in which the obtained resin sheet is stretched.

[0046] By having the above-mentioned solidification process and stretching process, it is easy to have air bubbles inside and the wall ratio W of the resin at a depth of 100 μm from the holding surface 100 is 20.0% or more and 40.0% or less, the holding surface has pores with an average pore size of 20 μm or more and 50 μm or less, the porosity of the holding surface is 20% or more and 40% or less, and the penetration time of water when 1.0 μL of water is dropped on the holding surface is 500 seconds or more and 1500 seconds or less. Hereinafter, the resin sheet obtained by the solidification step is also referred to as the "resin sheet before stretching", and the resin sheet obtained by the stretching step is also referred to as the "resin sheet after stretching".

[0047] (solidification process) The solidification step is a step in which a resin solution containing a resin dissolved in an organic solvent is applied onto a film-forming substrate, and the resin solution is solidified in a water-based solidification liquid to obtain a resin sheet before stretching.

[0048] Generally, a wet film-forming method and a dry molding method (also called a molding method) are known as methods for forming a resin sheet, but the wet film-forming method is adopted in this embodiment. In the wet film-forming method, a resin solution in which a resin is dissolved in a water-miscible organic solvent is continuously applied to a film-forming substrate, and the resin is coagulated and regenerated in a sheet shape by immersing the substrate in a water-based coagulating liquid. The inside of the sheet obtained in this manner contains a large number of bubbles generated by the coagulation and regeneration of the resin. Then, the sheet is washed and dried to obtain a long resin sheet. Each step of the wet film-forming method will be described in detail below.

[0049] In general, the wet film-forming method includes a preparation step, a coating step, and a solidification / regeneration step, and may include a cleaning / drying step and a grinding / removal step for flattening the surface of the resin sheet before stretching, as necessary.

[0050] In the preparation step, the resin is dissolved in an organic solvent that is capable of dissolving the resin and is miscible with water, and then additives are added as necessary, and the mixture is mixed uniformly to prepare a resin solution. The resin solution is preferably filtered to remove aggregates and the like, and then degassed under vacuum.

[0051] The resin may be any of the resins exemplified for the holding pad. The organic solvent is not particularly limited, but may be, for example, a polar solvent such as N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), tetrahydrofuran (THF), dimethylsulfoxide (DMSO), N-methylpyrrolidone (NMP), or methyl ethyl ketone (MEK). The above solvents are capable of dissolving polyurethane and are miscible with water.

[0052] In addition, the resin concentration in the resin solution is not limited, but can be, for example, 10% by mass or more and 50% by mass or less with respect to the entire resin solution. From the viewpoint of more easily obtaining the above-mentioned resin sheet, the resin concentration in the resin solution is preferably 15% by mass or more and 45% by mass or less with respect to the entire resin solution. From the same viewpoint, the resin concentration in the resin solution is more preferably 20% by mass or more and 40% by mass or less, and even more preferably 20% by mass or more and 35% by mass or less with respect to the entire resin solution. Note that the lower the resin concentration in the resin solution, the larger the bubbles formed and the smaller the wall ratio tends to be.

[0053] Furthermore, additives such as a foaming regulator for controlling foaming, a film-forming stabilizer for stabilizing the solidification and regeneration of polyurethane, and carbon black for stabilizing foam formation may be added to the resin solution.

[0054] The film-forming stabilizer is not particularly limited, but may be, for example, a nonionic surfactant.Specific examples include compounds having an alkyl chain with 3 or more carbon atoms added thereto, such as polyoxyethylene alkyl ether, polyoxypropylene alkyl ether, polyoxyethylene polyoxypropylene alkyl ether, perfluoroalkyl ethylene oxide adduct, glycerin fatty acid ester, and propylene glycol fatty acid ester.

[0055] The foaming regulator is not particularly limited, but may be, for example, an anionic surfactant, specifically, for example, sodium lauryl sulfate, carboxylates, sulfonates, sulfates, and phosphates.

[0056] In the coating process, the resin solution prepared in the preparation process is applied substantially uniformly to a strip-shaped film-forming substrate at room temperature using a knife coater or the like to form a coating film. At this time, the coating thickness (coating amount) of the resin solution can be adjusted by adjusting the gap (clearance) between the knife coater and the film-forming substrate.

[0057] As the film-forming substrate, a flexible film, a nonwoven fabric, a woven fabric, etc. can be used. When a nonwoven fabric or a woven fabric is used as the film-forming substrate, it is preferable to perform a pretreatment (sealing) by immersing the substrate in water or an organic solvent aqueous solution (such as a mixture of DMF and water) in advance in order to prevent the polyurethane solution from penetrating into the film-forming substrate when the polyurethane solution is applied. When the resin sheet is peeled off from the film-forming substrate, it is more preferable to use a flexible film.

[0058] In the solidification and regeneration process, the coating film obtained in the coating process (the film-forming substrate coated with the resin solution) is immersed in an aqueous solidification liquid (e.g., water or a solvent mainly composed of water) which is a poor solvent for the resin, and the coating film of the resin solution is solidified and regenerated into a sheet-like film having numerous bubbles inside.

[0059] In the aqueous coagulation liquid, generally, first, a skin layer with a thickness of about several μm in which micropores are formed is formed on the surface of the applied resin solution, and then, as the organic solvent in the polyurethane solution is replaced with the coagulation liquid, the resin is coagulated and regenerated in a sheet shape on one side of the film-forming substrate. At this time, typically, the organic solvent is removed from the resin solution, and the organic solvent is replaced with the coagulation liquid, forming a foam layer on the lower side (film-forming substrate side) of the skin layer, which has a larger pore size than the micropores formed in the skin layer, and in which rounded bubbles with a cross section of approximately triangular shape are distributed approximately evenly in the thickness direction of the sheet, but the bubble structure is not limited to this.

[0060] In the washing and drying process, the resin sheet regenerated in the coagulation and regeneration process is peeled off from the film-forming substrate and washed in a washing liquid such as water to remove the organic solvent remaining in the resin. After washing, the obtained resin sheet is dried in a cylinder dryer or the like as necessary.

[0061] The cylinder dryer is a dryer equipped with a cylinder having an internal heat source, and the resin sheet is dried by passing along the circumferential surface of the cylinder. After drying, the resin sheet is wound up into a roll.

[0062] (Stretching process) The resin sheet before stretching wound up as described above is stretched at a predetermined stretch ratio by the stretching process. As a result, the resin sheet before stretching is stretched and the wall ratio changes. The stretch ratio of the resin sheet is 105% or more and 300% or less, and more preferably 110% or more and 250% or less. Although it varies depending on the type of resin constituting the resin sheet, a stretch ratio of 105% or more tends to make it easier to make the resin sheet after stretching have a predetermined wall ratio, and a stretch ratio of 300% or less tends to prevent breakage or excessive thinning of the resin sheet after stretching. Note that "stretch ratio is 105%" means that the resin sheet is stretched to a length 1.05 times the length of the resin sheet before stretching.

[0063] In the stretching step, the stretching mode is not particularly limited, but may be, for example, uniaxial stretching or biaxial stretching. From the viewpoint of more easily obtaining a resin sheet having a desired wall ratio, the stretching step is preferably uniaxial stretching. In the case of uniaxial stretching, the stretching direction is not particularly limited, and may be stretched in the longitudinal direction or the transverse direction.

[0064] The manufacturing method of the holding pad of this embodiment may further include a grinding / removal step. The grinding / removal step is a step of grinding and / or partially removing at least one of both sides of the resin sheet after stretching by buffing or slicing. The thickness of the resin sheet can be made uniform by buffing or slicing, and the surface of the resin sheet can be made flatter. As a result, the holding force for the polished object can be made more uniform, the flatness of the polished object can be further improved, and the end shape can be further improved. In addition, the above-mentioned resin sheet can be obtained more easily by appropriately adjusting the amount of buffing or slicing on the surface of the resin sheet after stretching.

[0065] The resin sheet in this embodiment can be manufactured from two types of thermoplastic polyurethanes with different 100% modulus not only by the above-mentioned wet film formation method but also by other methods, such as the supercritical gas foaming method disclosed in Japanese Patent No. 4624781.

[0066] [Method of manufacturing polished products] The manufacturing method of the polished product includes a holding step of holding the object to be polished on the holding pad, and a polishing step of polishing the held object to be polished using the polishing pad. FIG. 2 shows a schematic cross-sectional view of the manufacturing method of the polished product. In FIG. 2, first, the holding pad 10 is fixed on the holding platen 21 of the polishing machine to hold the object to be polished W. Next, while the object to be polished W is held on the holding surface of the holding pad 10, a polishing slurry 22 is supplied to the opposite surface (surface to be polished) of the object to be polished W, and the polishing pad 24 attached to the polishing platen 23 of the polishing device is pressed against the object to be polished W and rotated, thereby polishing the object to be polished W. Each step will be described below.

[0067] The holding step is not particularly limited as long as it is a step that can hold the object to be polished on the holding pad, but for example, an aqueous solution is interposed between the holding surface of the holding pad and the object to be polished, and the object to be polished is held on the holding pad by the surface tension of the water. An example of such an aqueous solution is pure water. Alternatively, the holding step may be to hold the object to be polished on the holding pad by sucking the object to be polished through the holding pad.

[0068] The object to be polished is not particularly limited, but examples thereof include materials such as semiconductor devices and electronic components, in particular materials that require good edge shape and / or flatness, such as Si substrates (silicon wafers), GaAs (gallium arsenide) substrates, glass, and LCD (liquid crystal display) substrates.

[0069] The polishing step is a step of polishing the held object to be polished using a polishing pad. As the polishing pad, various conventionally known polishing pads can be used. The polishing step may be a primary polishing (rough polishing), a secondary polishing (finish polishing), or a step that combines both of these polishing steps.

[0070] In the polishing process, the workpiece is pressed against the polishing pad by the holding platen, while the holding platen and the polishing platen are rotated relative to each other, so that the processed surface of the workpiece is polished by the polishing pad. The holding platen and the polishing platen may rotate in the same direction at different rotation speeds, or may rotate in different directions.

[0071] In the polishing process, a polishing slurry may be used as an abrasive. Such a polishing slurry is not particularly limited, but may include, for example, a polishing slurry containing water, chemical components such as an oxidizing agent represented by hydrogen peroxide, additives, abrasive grains (polishing particles; for example, SiC, SiO2, Al2O3, CeO2), etc. EXAMPLES

[0072] The present invention will be described in more detail below using examples and comparative examples, but the present invention is not limited to the following examples. [Example 1] A resin solution was obtained by mixing and stirring 100 parts by mass of a solution in which 30% polyester-based polyurethane resin having a 100% modulus of 9.0 MPa at 25°C was dissolved in dimethylformamide (DMF), 7.9 parts by mass of a 20% carbon black dispersion in DMF, 4.0 parts by mass of a film-forming stabilizer (nonionic surfactant), 1.2 parts by mass of a foaming adjuster (anionic surfactant), 8 parts by mass of water, and 55 parts by mass of DMF.

[0073] Next, a PET film was prepared as a film-forming substrate, and the above-mentioned resin solution was applied onto it using a knife coater to obtain a coating film.

[0074] Next, the obtained coating film was immersed together with the film-forming substrate in water, which was a coagulating liquid, to coagulate and regenerate the resin, thereby obtaining a resin sheet. The resin sheet was removed from the coagulating bath, the film-forming substrate was peeled off from the resin sheet, and then the resin sheet was immersed in a cleaning solution consisting of water to remove the solvent DMF. The resin sheet was then wound up while being dried.

[0075] The obtained unstretched resin sheet having a thickness of 0.60 mm was stretched by 140% in the transverse direction, and then the surface of the stretched resin sheet was buffed to obtain a resin sheet having a thickness of 0.40 mm.

[0076] An adhesive sheet including a PET substrate provided with release paper was attached to the surface of the resin sheet obtained above that had not been subjected to buffing, thereby obtaining a holding pad.

[0077] [Example 2] A holding pad was produced in the same manner as in Example 1, except that a polyester-based polyurethane resin having a 100% modulus of 6.3 MPa at 25° C. was used, and the obtained resin sheet before stretching was stretched 110% in the lateral direction.

[0078] [Comparative Example 1] A holding pad was produced in the same manner as in Example 1, except that the resin sheet obtained in the solidification step was not stretched.

[0079] [Comparative Example 2] A supporting pad was produced in the same manner as in Example 1, except that the content of DMF was changed from 55 parts by mass to 30 parts by mass.

[0080] [Wall ratio] A tomographic image at a depth of 100 μm from the holding surface of the resin sheet (the surface opposite to the surface to which the adhesive sheet was attached) was obtained using a three-dimensional measurement X-ray CT device (Yamato Scientific Co., Ltd. TDM1000H-II (2K)). Next, the area Ab occupied by the air bubble part and the area Ap occupied by the resin part were measured using image processing software (Volume Graphics Co., Ltd. VG Studio MAX 3.0) for the obtained tomographic image, and the wall ratio was calculated according to the above formula (1). The results are shown in Table 1.

[0081] [Average pore size and pore ratio of the support surface] Using a microscope (Keyence Corporation, product name "VH-6300"), an area of ​​approximately 1.3 mm square on the holding surface of the resin sheet was photographed at 175 times magnification. The obtained image was binarized using image processing software (Image Analyzer V20LAB Ver. 1.3, Nikon Corporation), and the average diameter of the circle equivalent was calculated from the area of ​​each opening, thereby obtaining the average opening diameter of the holding surface. In addition, the opening rate per unit area was calculated based on the binarized image. The cutoff value (lower limit) of the opening diameter was set to 10 μm, and noise components were excluded. The results are shown in Table 1.

[0082] [Water penetration time to the support surface] The penetration time of water when 1.0 μL of water was dropped on the support surface was measured as follows. That is, under conditions of a temperature of 20° C. and a humidity of 60%, 1.0 μL of ion-exchanged water was dropped on the support surface of the dry resin sheet using a syringe needle. Then, using a solid-liquid interface analyzer (manufactured by Kyowa Interface Science Co., Ltd., product name "DropMaster500") as a contact angle meter, the time from the drop of the water droplet until the contact angle of the water droplet reached 20 degrees was measured. The above test was performed in a closed system. In addition, the "dry state" refers to the state when the resin sheet was held in a constant temperature and humidity chamber at a temperature of 23° C. (±2° C.) and a humidity of 50% (±5%) for 40 hours. The results are shown in Table 1.

[0083] [Kinematic friction force in a flooded state] The resin sheet was immersed in ion-exchanged water at room temperature for 15 minutes, and the surface moisture was wiped off to use as a measurement sample. The sample was attached to the platen of a universal tensile tester (Orientec RTC-1210A), and the adherend, a silicon wafer (10 cm x 10 cm), was placed on top of the sample. Then, while the sample was fixed, the adherend was pulled in the shear direction at a pulling speed of 50 mm / min, and the average value of the tensile force while the adherend was pulled 80 mm was taken as the kinetic friction force. The results are shown in Table 1.

[0084] [Polishing test] The release paper was peeled off from the holding pads obtained in the Examples and Comparative Examples, and the holding pads after peeling were attached to the holding platen of a polishing machine with the adhesive sheet side. Then, a silicon wafer (diameter 12 inches × thickness 780 μm) was polished under the polishing conditions shown below. (polishing conditions) Polishing machine: Fujikoshi Corporation MCP-150X Rotation speed: (table) 40 rpm / (top ring) 41 rpm Grinding pressure: 100g / cm 2 Oscillation: 20mm Polishing time: 20 minutes Polishing pad: Fujibo Ehime Co., Ltd. Suede pad #27 Abrasive: Fujimi Incorporated's GLANZOX 1306 (undiluted solution: water = 1:20) Number of samples: 25 for each example

[0085] (flatness) A total of 25 polished objects were evaluated for flatness using an optical interference flatness measuring device (KLA Tencor, product name "Wafersight") as follows. First, the GBIR of the polished object before the polishing test (hereinafter referred to as "GBIR0") and the GBIR of the polished object after the polishing test were measured, and the difference between them was calculated. Then, the average of the ratio (ΔGBIR / GBIR0) of the absolute value of the difference in GBIR (hereinafter referred to as "ΔGBIR") to the GBIR before the polishing test (GBIR0) was calculated for the 25 polished objects. Based on the average value of the obtained ratio (ΔGBIR / GBIR0), the flatness was evaluated according to the following evaluation criteria. The smaller the ratio (ΔGBIR / GBIR0), the higher the flatness of the polished object obtained. The GBIR was measured under the condition of EE (Edge Exclusion) 2 mm. The results are shown in Table 1. (Evaluation Criteria) A: The ratio (ΔGBIR / GBIR0) is 8.5% or less. B: The ratio (ΔGBIR / GBIR0) is greater than 8.5% and less than or equal to 11.5%. C: The ratio (ΔGBIR / GBIR0) exceeds 11.5%.

[0086] (end shape) The edge shape of a total of 25 polished objects that had been subjected to the above polishing process was evaluated using an optical interference flatness measuring device (manufactured by KLA Tencor, product name "Wafersight") as follows. First, the ESFQR of the polished object before the above polishing test (hereinafter referred to as "ESFQR0") and the ESFQR of the polished object after the above polishing test were measured, and the difference between them was calculated. Then, for the 25 polished objects, the average of the ratio (ΔESFQR / ESFQR0) of the absolute value of the difference in ESFQR (hereinafter referred to as "ΔESFQR") to the ESFQR (ESFQR0) before the polishing test was calculated. Based on the average value of the obtained ratio (ΔESFQR / ESFQR0), the edge shape was evaluated according to the following evaluation criteria. The smaller the ratio (ΔESFQR / ESFQR0), the better the edge shape of the polished object obtained. The ESFQR was measured under the condition of EE (Edge Exclusion) 1 mm (angle 5°, length 10 mm). The results are shown in Table 1. (Evaluation Criteria) A: The ratio (ΔESFQR / ESFQR0) is 17.5% or less. B: The ratio (ΔESFQR / ESFQR0) is greater than 17.5% and less than or equal to 22.5%. C: The ratio (ΔESFQR / ESFQR0) exceeds 22.5%.

[0087] [Table 1] [Industrial Applicability]

[0088] The holding pad of the present invention is used to hold an object to be polished when polishing materials such as semiconductor devices and electronic components, particularly materials that require good edge shapes and / or flatness, such as Si substrates (silicon wafers), GaAs (gallium arsenide) substrates, glass, and LCD (liquid crystal display) substrates, and has industrial applicability as a holding pad that is particularly suitable for use in polishing silicon wafers.

Claims

1. A holding pad including a resin sheet having a holding surface for holding an object to be polished, The resin sheet has air bubbles therein, The resin wall ratio W at a depth of 100 μm from the holding surface 100 is 20.0% or more and 40.0% or less, The holding surface has openings with an average opening diameter of 20 μm or more and 50 μm or less, The porosity of the holding surface is 20% or more and 40% or less, When 1.0 μL of water is dropped onto the support surface, the penetration time of the water is 500 seconds or more and 1500 seconds or less. Holding pad.

2. 2. The holding pad according to claim 1, wherein the 100% modulus at 23±2° C. of the resin constituting the resin sheet is 5.0 MPa or more and 20.0 MPa or less.

3. A retaining pad as described in claim 1 or 2, wherein the kinetic friction force of the resin sheet in a submerged state measured by the following measurement method is 3.0 kgf or more and 5.5 kgf or less. (Measurement method) The resin sheet is immersed in ion-exchanged water at room temperature for 15 minutes, and then the moisture on the surface is wiped off to use as a measurement sample. A silicon wafer of 10 cm × 10 cm is placed on the measurement sample, and while the measurement sample is fixed, the silicon wafer is pulled in the shear direction at a tensile speed of 50 mm / min, and the average tensile force while the silicon wafer is pulled 80 mm is defined as the kinetic friction force.

4. The holding pad according to any one of claims 1 to 3, further comprising an adhesive sheet on the side of the resin sheet opposite the holding surface.

5. A method for manufacturing a support pad according to any one of claims 1 to 4, comprising the steps of: A step of applying a resin solution containing a resin dissolved in an organic solvent onto a film-forming substrate and coagulating the resin solution in a water-based coagulation liquid to obtain a resin sheet; and stretching the obtained resin sheet. Manufacturing method.

6. A holding step of holding an object to be polished on the holding pad according to any one of claims 1 to 4; A polishing step of polishing the held object to be polished with a polishing pad. Manufacturing method of polished products.

Citation Information

Patent Citations

  • Sheet-form resilient foam and jig for polishing wafer by using it

    JP1994023664A

  • Polishing body composed of wafer polishing cloth or polishing surface plate and wafer polishing method using same

    JP1999285963A

  • Sheet for holding wafer

    JP2004342651A

  • Holding pad

    JP2009061524A

  • Holding pad

    JP2010240790A