Method for manufacturing a field effect transistor
By forming a stacked body with specific openings and a regrown layer in a field effect transistor manufacturing process, the issue of abnormal semiconductor growth is addressed, resulting in controlled and uniform layer formation.
Patent Information
- Application Number
- JP2020092852
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-05-28
- Publication Date
- 2024-09-19
- Estimated Expiration
- 2040-05-28
AI Technical Summary
The existing manufacturing method for enhancement mode III-nitride HEMT devices causes abnormal growth of semiconductor layers due to local concentration of raw materials during the formation of p-doped GaN layers.
A method involving the formation of a stacked body with multiple Group III nitride semiconductor layers, including a first and second opening, where a regrown layer is formed on the exposed surface, and a gate electrode is placed only in the first opening, while a second opening alleviates local material concentration.
This approach suppresses polycrystalline growth in the regrown layer, improving the manufacturing process by ensuring controlled and uniform growth of semiconductor layers.
Smart Images

Figure 0007553770000005 
Figure 0007553770000004 
Figure 0007553770000009
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a field effect transistor. [Background technology]
[0002] Patent Document 1 describes a method for manufacturing an enhancement mode III-nitride HEMT device, which includes the steps of removing a portion of a passivation layer covering an upper layer of the III-nitride layer to form a recessed gate region, and forming a p-doped GaN layer at least in the recessed gate region. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent Publication No. 2013-123047 Summary of the Invention [Problem to be solved by the invention]
[0004] In the manufacturing method described in Patent Document 1, the passivation layer is removed only from the portion that will become the gate region. However, when forming a semiconductor layer such as a p-doped GaN layer, if the raw material for the semiconductor layer is concentrated locally, this may cause abnormal growth. [Means for solving the problem]
[0005] According to one aspect of the present invention, a method for manufacturing a field effect transistor includes the steps of forming a stacked body having a plurality of Group III nitride semiconductor layers; forming a patterned film having a first opening and a second opening on an upper surface of the stacked body; forming a regrowth layer made of a Group III nitride semiconductor on an upper surface of the stacked body exposed in the first opening and the second opening; and forming a gate electrode on a portion of the regrowth layer located in the first opening but not in the second opening. Effect of the Invention
[0006] According to the manufacturing method of one aspect of the present invention, polycrystalline growth of the regrown layer can be suppressed. [Brief description of the drawings]
[0007] [Figure 1] 1 is a flowchart showing a method for manufacturing a field effect transistor according to an embodiment of the present invention. [Diagram 2] 1A to 1C are schematic cross-sectional views showing a method for manufacturing a field-effect transistor according to an embodiment of the present invention. [Figure 3A] 1A to 1C are schematic cross-sectional views showing a method for manufacturing a field-effect transistor according to an embodiment of the present invention. [Figure 3B] 1A to 1C are schematic plan views illustrating a method for manufacturing a field effect transistor according to an embodiment of the present invention. [Figure 4] 1A to 1C are schematic cross-sectional views showing a method for manufacturing a field-effect transistor according to an embodiment of the present invention. [Diagram 5] 1A to 1C are schematic cross-sectional views showing a method for manufacturing a field-effect transistor according to an embodiment of the present invention. [Figure 6] 1A to 1C are schematic cross-sectional views showing a method for manufacturing a field-effect transistor according to an embodiment of the present invention. [Figure 7] 1A to 1C are schematic cross-sectional views showing a method for manufacturing a field-effect transistor according to an embodiment of the present invention. [Figure 8] 1A to 1C are schematic cross-sectional views showing a method for manufacturing a field-effect transistor according to an embodiment of the present invention. [Figure 9] 1 is an optical microscope photograph of a regrown layer and its surrounding area in an experimental example. [Figure 10] 13 is an optical microscope photograph of a regrown layer and its surrounding area in a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In the drawings, the same elements are denoted by the same reference numerals.
[0009] Fig. 1 is a flow chart showing a method for manufacturing a field effect transistor of this embodiment. As shown in Fig. 1, the method for manufacturing a field effect transistor of this embodiment includes a step S101 for forming a laminate, a step S102 for forming a patterned film, a step S103 for forming a regrown layer, and a step S104 for forming a gate electrode. Figs. 2 to 8 are schematic cross-sectional views and schematic plan views showing the method for manufacturing a field effect transistor of this embodiment.
[0010] First, as shown in FIG. 2, a stacked body 20 having a plurality of group III nitride semiconductor layers is formed (step S101). The stacked body 20 can be formed on a substrate 10. The substrate 10 is, for example, a sapphire substrate. The stacked body 20 can be composed of a plurality of group III nitride semiconductor layers. Examples of group III nitride semiconductors constituting the group III nitride semiconductor layers include GaN, InGaN, AlGaN, and AlN. The step of forming the stacked body 20 can include a step of forming a first semiconductor layer 21 on the substrate 10, and a step of forming a second semiconductor layer 22 on the first semiconductor layer 21. The first semiconductor layer 21 is, for example, composed of GaN. The second semiconductor layer 22 has a larger band gap energy than the first semiconductor layer 21. The second semiconductor layer 22 is, for example, composed of AlGaN. An AlN layer that is thinner than the AlGaN layer may be provided below the AlGaN layer. A channel is formed in the first semiconductor layer 21 near the surface on the second semiconductor layer 22 side. The channel is, for example, a two-dimensional electron gas layer. The laminate 20 can be formed by, for example, metal-organic chemical vapor deposition (MOCVD).
[0011] Next, as shown in FIG. 3A, a patterned film 30 is formed on the upper surface of the laminate 20 (step S102). The patterned film can be obtained, for example, by forming a film that covers the entire upper surface of the laminate 20, and then removing a part of it using a resist or the like. The patterned film 30 may have only the first opening 30a as an opening, but it is preferable that the patterned film 30 has the first opening 30a and the second opening 30b. This can reduce local concentration of the raw material of the regrown layer 40 in the first opening 30a, as described later. The first opening 30a is disposed at a position where a gate electrode 51, which will be described later, is to be provided. The second opening 30b is different from the first opening 30a and is disposed in an area other than the position where the gate electrode 51 is to be provided. The first opening 30a may be disposed in a portion having an element function of a field effect transistor, and the second opening 30b may be disposed in a portion not having an element function of a field effect transistor. The first opening 30a and the second opening 30b do not necessarily have to be completely surrounded by the inner side surface of the patterned film 30. The patterned film 30 may have a plurality of first openings 30a, and may have a plurality of second openings 30b.
[0012] 3B is a schematic plan view corresponding to FIG. 3A. The first direction length L of the first opening 30a in the first direction X along the gate length of the field effect transistor. 1a In the case where a gate electrode 51 is formed on the upper surface of the regrown layer 40 formed in the first opening 30a as described later, the first direction length L 1a is substantially equal to the gate length. The gate width is, for example, greater than the gate length. Correspondingly, the second direction length L of the first opening 30a in the second direction Y perpendicular to the first direction X is 2a is the first direction length L 1a The shorter the distance between the first opening 30a and the second opening 30b, the easier it is to alleviate the concentration of the raw material of the regrowth layer 40, which will be described later, in the first opening 30a. For this reason, it is preferable that the shortest distance D between the first opening 30a and the second opening 30b is 30 μm or less. The shortest distance D between the first opening 30a and the second opening 30b is greater than 0 μm, and can be, for example, the first direction length L of the first opening 30a. 1a The length L of the second opening 30b in the first direction is larger than1b is the length L of the first opening 30a in the first direction. 1a This makes it possible to further reduce the concentration of the raw material of the regrowth layer 40, which will be described later, in the first opening 30a. 1b The length L of the second opening 30b in the second direction can be set to 30 μm or more. 2b is the length L of the first opening 30a in the second direction. 2a It can be equal to or longer than that.
[0013] The patterned film 30 may be composed of a single film, or may be composed of a multi-layer film. It is preferable to form the patterned film 30 by forming a first film 31 in contact with the laminate 20 and a second film 32 disposed on the first film 31 and made of a material different from that of the first film 31. This allows the first film 31 and the second film 32 to be formed to have different functions, so that the patterned film 30 can provide a plurality of effects.
[0014] The first film 31 is preferably a film that functions as a passivation film on the surface of the laminate 20. By providing such a first film 31 in contact with the laminate 20, the characteristics of the channel formed in the laminate 20 can be improved. Specifically, it is possible to improve the carrier mobility and / or carrier concentration in the channel. Examples of the first film 31 that can be used as a passivation film include a film containing silicon and nitrogen (e.g., a SiN film), a film containing silicon and oxygen (e.g., a SiO2 film), or a film containing aluminum and oxygen (e.g., an Al2O3 film). When the second film 32 is provided on the first film 31, the first film 31 is preferably a film containing silicon and nitrogen or a film containing silicon and oxygen. This makes it easy to selectively remove the second film 32 in a later process. The first film 31 can be formed using a sputtering device such as an ECR (Electron Cyclotron Resonance) sputtering device.
[0015] The second film 32 is preferably a film to which the material of the regrown layer to be formed later is more easily attached than the first film 31. When it is desired to attach the material of the regrown layer to the second film 32, the second film 32 is disposed at the top of the patterned film 30. The second film 32 may be a film containing aluminum and nitrogen (for example, an AlN film). The second film 32 may be a film containing gallium and nitrogen (for example, a GaN film). The second film 32 can be formed, for example, by using a sputtering device. The second film 32 is preferably a polycrystalline film. This makes it easy to selectively remove the second film 32. The polycrystalline second film 32 can be obtained, for example, by forming the second film 32 on the surface of the first film 31 made of the above-mentioned material using a sputtering device. The first film 31 is, for example, a polycrystalline film, and if the second film 32 is formed thereon, the polycrystalline second film 32 can be easily obtained.
[0016] Next, as shown in FIG. 4, a regrowth layer 40 made of a group III nitride semiconductor is formed on the upper surface of the stack 20 exposed in the first opening 30a and the second opening 30b (step S103). By providing not only the first opening 30a but also the second opening 30b, localized concentration of the raw material of the regrowth layer 40 in the first opening 30a can be alleviated. In addition, the material of the regrowth layer 40 adheres to the upper surface of the second film 32, and an adhesion layer 41 made of an adhesion such as a polycrystalline layer is formed. Therefore, the provision of the second film 32 can also alleviate localized concentration of the raw material of the regrowth layer 40 in the first opening 30a. By providing at least one of these concentration alleviation structures, and preferably by providing both, the polycrystalline growth of the regrowth layer 40 can be suppressed.
[0017] FIG. 9 is an optical microscope photograph of an experimental example in which a regrowth layer is formed by providing a first opening and a second opening, and providing a first film and a second film as a patterned film. FIG. 10 is an optical microscope photograph of a comparative example in which a regrowth layer is formed without providing a second opening or a second film. Both were photographed from above the regrowth layer after it was formed. In FIG. 10, it is observed that the regrowth layer formed in the first opening cannot grow into a single crystal and has grown into a granular polycrystalline layer. This is presumably due to an oversupply of raw material. On the other hand, in FIG. 9, no granular growth as in FIG. 10 is observed in the regrowth layer. From this, it can be seen that by providing the second opening and by providing the second film, it is possible to alleviate the concentration of raw material in the first opening and to suppress the polycrystalline growth of the regrowth layer.
[0018] The adhesion layer 41 may be formed on the entire upper surface of the second film 32, or may be formed partially. The upper surface of the second film 32 is preferably a surface on which the regrowth layer 40 is less likely to grow than the upper surface of the stack 20. This can prevent the raw material of the regrowth layer 40 from being insufficient in the first opening 30a. For example, the upper surface of the stack 20 can be substantially made of single crystal, and the upper surface of the second film 32 can be substantially made of polycrystal. Since the upper surface of the second film 32 is a surface on which the regrowth layer 40 is less likely to grow, the adhesion layer 41 is formed, for example, as a polycrystalline layer. The adhesion layer 41 may be a layer having poorer crystallinity and / or a thinner film thickness than the regrowth layer 40. The thickness of the regrowth layer 40 is preferably thinner than the thickness of the patterned film 30. This can separate the adhesion layer 41 formed on the upper surface of the patterned film 30 from the regrowth layer 40, making it easy to remove the adhesion layer 41 together with the second film 32 in a later step. When removing the second film 32, it is preferable that the upper surface of the regrown layer 40 is located lower than the lower surface of the second film 32. This makes it possible to remove the second film 32 more easily.
[0019] The regrown layer 40 can function as a gate contact layer provided between the stack 20 and a gate electrode described later. Examples of III-nitride semiconductors constituting the regrown layer 40 include GaN, InGaN, and AlGaN. The regrown layer 40 may contain n-type or p-type impurities in at least a part thereof. When the channel formed in the stack 20 is a two-dimensional electron gas layer, the regrown layer 40 preferably contains p-type impurities. The regrown layer 40 is, for example, a GaN layer containing p-type impurities. The regrown layer 40 may be composed of only one layer or may be composed of multiple layers. The regrown layer 40 can be formed, for example, by MOCVD. The regrown layer 40 can be formed, for example, by using a III-group source gas (e.g., trimethylgallium (TMG) gas), a nitrogen source gas (e.g., ammonia gas), and a carrier gas (e.g., nitrogen gas).
[0020] Next, as shown in FIG. 5, the second film 32 may be removed while leaving the first film 31. If there is an adhesion layer 41 on the upper surface of the second film 32 that was attached when forming the regrowth layer 40, it is preferable to remove at least a part of the second film 32 including the upper surface. As described above, the adhesion layer 41 is a layer that is likely to have an uneven thickness and shape like a polycrystalline layer, and it is preferable that the gate electrode described below is not formed on the adhesion layer 41. By removing the adhesion layer 41, the shape of the gate electrode can be formed more stably. Although a part of the second film 32 may be left, in order for the first film 31 to fully function as a passivation film for the surface of the laminate 20, it is preferable to remove the rest of the patterned film 30 while leaving only the first film 31.
[0021] As described above, the first film 31 can contribute to improving the characteristics of the channel as a passivation film, so it is preferable to leave it without removing it. By using a removal method in which the removal rate of the first film 31 is slower than that of the second film 32, the second film 32 can be selectively removed, which is preferable. As an example of such a removal method, there is a method in which the second film 32 is removed by wet etching using a tetramethylammonium hydroxide (TMAH) solution. Wet etching using a TMAH solution is particularly suitable when the first film 31 is a film containing silicon and nitrogen, such as SiN, and the second film 32 is a film containing aluminum and nitrogen, such as an AlN film.
[0022] Next, as shown in FIG. 6, a gate electrode 51 is formed on a portion of the regrown layer 40 located in the first opening 30a (step S104). Even if the regrown layer 40 is also formed in the second opening 30b, the gate electrode 51 is formed on a portion of the regrown layer 40 located in the first opening 30a, not on a portion of the regrown layer 40 located in the second opening 30b. That is, the gate electrode 51 is not formed on a portion of the regrown layer 40 located in the second opening 30b. The gate electrode 51 can be formed in contact with the upper surface of the regrown layer 40 located in the first opening 30a. A part of the gate electrode 51 may be formed on the patterned film 30. The gate electrode 51 is formed so as not to come into contact with the regrown layer 40 located in the second opening 30b. For example, if an insulating film covering the regrown layer 40 located in the second opening 30b is formed before the gate electrode 51 is formed, a part of the gate electrode 51 may be disposed above the regrown layer 40 located in the second opening 30b. In order to further reduce the possibility of contact between the gate electrode 51 and the regrown layer 40 located in the second opening 30b, even if such an insulating film is provided, it is preferable that the gate electrode 51 is not disposed above the second opening 30b. The gate electrode 51 is composed of, for example, a structure in which Ni / Au / Pt are laminated in this order from the stacked body 20 side, a structure in which Ti / Al are laminated, or a Ni single film. The gate electrode 51 can be patterned by, for example, a lift-off method.
[0023] Next, as shown in FIG. 7, the portion of the regrown layer 40 located in the second opening 30b may be removed. This removal may be performed using the patterned film 30 and the gate electrode 51 as a mask. By removing the regrown layer 40 located in the second opening 30b, unintended current leakage through the regrown layer 40 located in the second opening 30b can be prevented. The second opening 30b may be used as a region for forming the source electrode 52 and / or the drain electrode 53. In this case, by removing the regrown layer 40 located in the second opening 30b, the contact resistance of the source electrode 52 and / or the drain electrode 53 can be reduced.
[0024] Next, as shown in FIG. 8, a source electrode 52 and a drain electrode 53 are formed to obtain a field effect transistor. The source electrode 52 and the drain electrode 53 are made of, for example, Ti / Al. The source electrode 52 and the drain electrode 53 are formed, for example, by removing a part of the stack 20 and the patterned film 30, at a position where they contact the channel. In the field effect transistor shown in FIG. 8, the second opening 30b and the patterned film 30 around it are left, but they may be removed. As described above, the second opening 30b is provided in a region other than the region that functions as a field effect transistor, so that the stack 20 directly below the second opening 30b and around it may be removed. The field effect transistor is not limited to the members shown in FIG. 8, and may have other members such as a pad electrode and an insulating film. The field effect transistor is, for example, a high electron mobility transistor (HEMT).
[0025] According to the manufacturing method of the above embodiment, the polycrystalline growth of the regrown layer 40 can be suppressed.
[0026] The above describes the embodiments of the present invention with reference to specific examples. However, the present invention is not limited to these specific examples. All forms that can be implemented by a person skilled in the art through appropriate design modifications based on the above-described embodiments of the present invention also fall within the scope of the present invention as long as they include the gist of the present invention. In addition, within the scope of the concept of the present invention, a person skilled in the art may come up with various modified examples and examples of modifications, and it is understood that these modified examples and examples of modifications also fall within the scope of the present invention. [Explanation of symbols]
[0027] 10 Substrate 20 Laminate 21 first semiconductor layer, 22 second semiconductor layer 30 Patterned Film 30a 1st opening, 30b 2nd opening 31 1st membrane, 32 2nd membrane 40 Regrowth layer 41 Adhesion layer 51 Gate electrode 52 Source electrode 53 Drain electrode
Claims
1. forming a stack having a plurality of Group III nitride semiconductor layers; forming a patterned film having a first opening and a second opening on an upper surface of the laminate; forming a regrowth layer made of a Group III nitride semiconductor on an upper surface of the stack exposed in the first opening and the second opening; forming a gate electrode on a portion of the regrown layer located in the first opening but not on a portion of the regrown layer located in the second opening; Equipped with 13. A method for manufacturing a field effect transistor, comprising the steps of: after the step of forming a gate electrode, removing a portion of the regrown layer located in the second opening by using the patterned film and the gate electrode as a mask.
2. In the step of forming the patterned film, a first film in contact with the laminate and a second film disposed on the first film and made of a material different from that of the first film are formed as the patterned film; 2. The method for manufacturing a field effect transistor according to claim 1, further comprising the step of removing the second film while leaving the first film after the step of forming the regrown layer.
3. The method for manufacturing a field effect transistor according to claim 2 , wherein the first film is a film containing silicon and nitrogen or a film containing silicon and oxygen.
4. The method for manufacturing a field effect transistor according to claim 3 , wherein the second film is a film containing aluminum and nitrogen.
5. 5. The method for manufacturing a field effect transistor according to claim 4, wherein in the step of removing the second film, the second film is removed by wet etching using a tetramethylammonium hydroxide (TMAH) solution.
Citation Information
Patent Citations
Method of fabricating nitride-based transistors with regrown ohmic contact regions and nitride-based transistors with regrown ohmic contact regions
JP2007538402A
Nitride semiconductor device and its manufacturing method
JP2008078526A
Enhancement mode iii-nitride device and method for manufacturing the same
JP2013123047A
Manufacturing method of semiconductor device with schottky diode and high electron mobility transistor
JP2014212316A
Semiconductor device manufacturing method
JP2015073034A