Transparent Conductive Film
The transparent conductive film with a metal nanowire layer on a base material addresses conductivity loss in flexible applications by optimizing nanowire amount and conductivity, achieving high conductivity and transparency through a controlled manufacturing process.
Patent Information
- Application Number
- JP2021003466
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-13
- Publication Date
- 2024-09-19
- Estimated Expiration
- 2041-01-13
AI Technical Summary
Conventional transparent conductive films with metal oxide layers lose conductivity when bent, making them unsuitable for flexible applications, and existing metal nanowire films require improvements in conductivity.
A transparent conductive film comprising a base material with a transparent conductive layer containing metal nanowires, where the amount of metal nanowires and electrical conductivity are related by the formula y=a×x, with a being 0.77 or more, and the film having a haze value of 20% or less and a surface resistance of 0.1Ω/□ to 1000Ω/□.
The film achieves excellent conductivity and transparency with a balanced haze value, allowing for high flexibility and durability, achieved through a manufacturing process that adjusts the flow of metal nanowires in the coating layer.
Smart Images

Figure 0007554122000002 
Figure 0007554122000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a transparent conductive film. [Background technology]
[0002] Conventionally, in image display devices having touch sensors, transparent conductive films obtained by forming a metal oxide layer such as ITO (indium tin oxide) on a transparent resin film have been widely used as electrodes for the touch sensors. However, transparent conductive films having such metal oxide layers tend to lose conductivity when bent, making them difficult to use in flexible displays and other applications. However, there is a problem that it is difficult to use in applications where high flexibility is required.
[0003] On the other hand, transparent conductive films containing metal nanowires are known as transparent conductive films with high flexibility. Metal nanowires are wire-shaped conductive materials with a diameter of nanometer size. In transparent conductive films made of metal nanowires, the metal nanowires are in a mesh shape, so that a good electrical conduction path is formed with a small amount of metal nanowires, and openings are formed in the gaps of the mesh, thereby achieving high light transmittance. In transparent conductive films containing such metal nanowires, improvement of the conductivity essentially required for conductive films is also being considered. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Special Publication No. 2009-505358 [Patent Document 2] Patent No. 6199034 Summary of the Invention [Problem to be solved by the invention]
[0005] The present invention has been made to solve the above problems, and an object of the present invention is to provide a transparent conductive film that contains metal nanowires and has excellent conductivity and transparency. [Means for solving the problem]
[0006] The transparent conductive film of the present invention is a transparent conductive film comprising a substrate and a transparent conductive layer disposed on one side of the substrate, the transparent conductive layer containing metal nanowires, and an amount of the metal nanowires in the transparent conductive layer x (g / m 2 ) and the electrical conductivity y (1 / Ω) of the transparent conductive film satisfy the following formula (1). y = a × x (1) In formula (1), a is 0.77 or more. In one embodiment, the transparent conductive film has a haze value of 20% or less. In one embodiment, the transparent conductive film has a surface resistance value of 0.1 Ω / □ to 1000 Ω / □. In one embodiment, the amount of metal nanowires in the transparent conductive layer is x (g / m 2 ) is 0.005g / m 2 ~0.05g / m 2 It is. Effect of the Invention
[0007] According to the present invention, it is possible to provide a transparent conductive film that contains metal nanowires and has excellent conductivity and transparency. [Brief description of the drawings]
[0008] [Figure 1] 1 is a schematic cross-sectional view of a transparent conductive film obtained by a production method according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] A. Transparent conductive film 1 is a schematic cross-sectional view of a transparent conductive film obtained by a manufacturing method according to one embodiment of the present invention. The transparent conductive film 100 includes a substrate 10 and a transparent conductive layer 20 disposed on one side of the substrate 10. The transparent conductive layer 20 includes metal nanowires (not shown).
[0010] The surface resistance of the transparent conductive film is preferably 0.1 Ω / □ to 1000 Ω / □, more preferably 0.5 Ω / □ to 300 Ω / □, even more preferably 1 Ω / □ to 200 Ω / □, particularly preferably 1 Ω / □ to 150 Ω / □, and most preferably 20 Ω / □ to 100 Ω / □. The surface resistance can be measured using Mitsubishi Chemical Analytech's "Automatic Resistivity Measurement System MCP-S620 / MCP-S521."
[0011] The haze value of the transparent conductive film is preferably 20% or less, more preferably 10% or less, further preferably 0.1% to 5%, further preferably 0.1% to 3%, and particularly preferably 0.1% to 1%.
[0012] The total light transmittance of the transparent conductive film is preferably 30% or more, more preferably 35% or more, and particularly preferably 40% or more.
[0013] (Transparent conductive layer) As described above, the transparent conductive layer includes metal nanowires.
[0014] The amount of metal nanowires in the transparent conductive layer x (g / m 2 The relationship between the capacitance and the conductivity y (1 / Ω) of the transparent conductive film is expressed by the following formula (1): y = a × x (1) In formula (1), a is 0.77 or more. In the present invention, the amount of metal nanowires x (g / m 2) and the electrical conductivity y (1 / Ω) are in the above-mentioned relationship, a transparent conductive film with remarkably excellent electrical conductivity can be obtained. The transparent conductive film of the present invention has high electrical conductivity while using a relatively small amount of metal nanowires. Such a transparent conductive film is very advantageous in that it can achieve both high electrical conductivity and transparency (low haze). As described below, such a transparent conductive film can be obtained by applying a composition for forming a transparent conductive layer to form a coating layer, leaving the coating layer for a predetermined time, and then performing the next step of blowing air. It is believed that leaving the coating layer for a predetermined time allows the flow of the metal nanowires in the coating layer to be favorably adjusted, and the number of contact points between the metal nanowires increases, thereby achieving the above-mentioned effects.
[0015] In the above formula (1), a is preferably 0.79 or more, more preferably 0.8 or more, even more preferably 0.85 or more, particularly preferably 0.88 or more, and even more preferably 0.9 or more. Within such a range, the above effects become more pronounced. The larger the above a, the more preferable it is, and the upper limit is, for example, 2.0. The greater the amount of silver, the higher the conductivity, but the haze increases accordingly, and transparency is impaired. The amount of metal nanowires x (g / m 2 ) is a transparent conductive layer of 1m 2 The surface resistance is the weight of the metal nanowires present per unit area. The electrical conductivity is the reciprocal of the surface resistance.
[0016] The amount of metal nanowires in the transparent conductive layer x (g / m 2 ) is preferably 0.005 g / m 2 ~0.05g / m 2 , more preferably 0.008 g / m 2 ~0.03g / m 2 and even more preferably 0.01 g / m 2 ~0.025g / m 2 and particularly preferably 0.01 g / m 2 ~0.02g / m 2 It is.
[0017] In one embodiment, the transparent conductive layer further includes a polymer matrix. In this embodiment, the metal nanowires are present in the polymer matrix. In the transparent conductive layer made of a polymer matrix, the metal nanowires are protected by the polymer matrix. As a result, corrosion of the metal nanowires is prevented, and a transparent conductive film with excellent durability can be obtained.
[0018] The thickness of the transparent conductive layer is preferably 2 μm to 10 μm, more preferably 3 μm to 9 μm, and further preferably 4 μm to 8 μm.
[0019] The content of the metal nanowires in the transparent conductive layer is preferably 0.1 to 50 parts by weight, more preferably 0.1 to 30 parts by weight, relative to 100 parts by weight of the binder resin constituting the transparent conductive layer. Within this range, a transparent conductive film having excellent electrical conductivity and light transmittance can be obtained.
[0020] The total light transmittance of the transparent conductive layer is preferably 85% or more, more preferably 90% or more, and even more preferably 95% or more.
[0021] Metal nanowires are conductive materials made of metal, shaped like needles or threads, and with a diameter of nanometers. Metal nanowires may be straight or curved. By using a transparent conductive layer made of metal nanowires, the metal nanowires can be in a mesh shape, so that even a small amount of metal nanowires can form a good electrical conduction path, and a transparent conductive film with low electrical resistance can be obtained. Furthermore, by forming the metal nanowires in a mesh shape, openings can be formed in the gaps of the mesh, and a transparent conductive film with high light transmittance can be obtained.
[0022] The ratio of the thickness d to the length L of the metal nanowire (aspect ratio: L / d) is preferably 10 to 100,000, more preferably 50 to 100,000, and particularly preferably 100 to 10,000. By using metal nanowires with such a large aspect ratio, the metal nanowires can be well crossed, and a small amount of metal nanowires can exhibit high conductivity. As a result, a transparent conductive film with high light transmittance can be obtained. In this specification, the "thickness of the metal nanowire" means the diameter when the cross section of the metal nanowire is circular, means the minor axis when the cross section is elliptical, and means the longest diagonal when the cross section is polygonal. The thickness and length of the metal nanowire can be confirmed by a scanning electron microscope or a transmission electron microscope.
[0023] The thickness of the metal nanowires is preferably less than 500 nm, more preferably less than 200 nm, particularly preferably 10 to 100 nm, and most preferably 10 to 50 nm. Within such a range, a transparent conductive layer with high light transmittance can be formed.
[0024] The length of the metal nanowires is preferably 1 μm to 1000 μm, more preferably 10 μm to 500 μm, and particularly preferably 10 μm to 100 μm. If the length is within this range, a transparent conductive film with high conductivity can be obtained.
[0025] As the metal constituting the metal nanowire, any suitable metal can be used as long as it is a conductive metal. Examples of the metal constituting the metal nanowire include silver, gold, copper, nickel, and the like. Materials obtained by plating these metals (e.g., gold plating) may also be used. Among these, silver, copper, or gold are preferred from the viewpoint of conductivity, and silver is more preferred.
[0026] Any suitable method may be adopted as the method for producing the metal nanowires. For example, a method of reducing silver nitrate in a solution, a method of applying a voltage or current from the tip of a probe to the surface of a precursor, drawing out the metal nanowire at the tip of the probe, and continuously forming the metal nanowire may be mentioned. In the method of reducing silver nitrate in a solution, silver nanowires may be synthesized by reducing a silver salt such as silver nitrate in the liquid phase in the presence of a polyol such as ethylene glycol and polyvinylpyrrolidone. Silver nanowires of uniform size can be mass-produced according to the methods described in, for example, Xia, Y.etal., Chem.Mater.(2002), 14, 4736-4745, and Xia, Y.etal., Nano letters(2003)3(7), 955-960.
[0027] (base material) Any suitable material may be used as the material constituting the substrate. Specifically, for example, a polymer substrate such as a film or a plastic substrate is preferably used. This is because the substrate has excellent smoothness and wettability with respect to the composition for forming a transparent conductive layer, and the productivity can be significantly improved by continuous production using a roll.
[0028] The material constituting the substrate is typically a polymer film mainly composed of a thermoplastic resin. Examples of the thermoplastic resin include polyester resins; cycloolefin resins such as polynorbornene; acrylic resins; polycarbonate resins; and cellulose resins. Among them, polyester resins, cycloolefin resins, and acrylic resins are preferred. These resins are excellent in transparency, mechanical strength, thermal stability, and moisture shielding properties. The thermoplastic resins may be used alone or in combination of two or more. In addition, optical films such as those used in polarizing plates, such as low retardation substrates, high retardation substrates, retardation plates, and brightness-improving films, can also be used as substrates.
[0029] The thickness of the substrate is preferably 20 μm to 200 μm, and more preferably 30 μm to 150 μm.
[0030] The total light transmittance of the above-mentioned substrate is preferably 30% or more, more preferably 35% or more, and further preferably 40% or more.
[0031] B. Manufacturing method of transparent conductive film In one embodiment, the method for producing a transparent conductive film of the present invention includes a coating step of coating a substrate with a transparent conductive layer-forming composition containing metal nanowires to form a coating layer, a leaving step of leaving the coating layer for a predetermined time, and a blowing step of blowing air onto the coating layer after the leaving step. According to this manufacturing method, the transparent conductive film is obtained, that is, a transparent conductive film including a substrate and a transparent conductive layer disposed on one side of the substrate. The manufacturing method may include any other appropriate steps in addition to the coating step and the blowing step. In one embodiment, the manufacturing method may further include a drying step of drying the coating layer after the blowing step. In another embodiment, the blowing step is a step that can dry the coating layer, and the transparent conductive layer is formed through the blowing step.
[0032] In one embodiment, the manufacturing method can be performed while transporting the substrate. Typically, the coating step, the leaving step, and the air blowing step (and other steps such as a drying step, if necessary) are performed while the substrate in a roll state is unwound and transported, to form a long transparent conductive film including the substrate and a transparent conductive layer disposed on one side of the substrate. In one embodiment, the transparent conductive film is wound up after formation.
[0033] Any appropriate method may be adopted as the method for transporting the substrate. For example, transport by a transport roll, transport by a transport belt, a combination of these, etc. The transport speed is, for example, 5 m / min to 50 m / min.
[0034] (coating process) As described above, in the coating step, the composition for forming a transparent conductive layer containing metal nanowires is coated on the substrate by any appropriate method to form a coating layer. In one embodiment, the composition for forming a transparent conductive layer containing metal nanowires is coated on the substrate while the substrate is being transported in a long-sized shape to form a coating layer.
[0035] The composition for forming a transparent conductive layer includes the metal nanowires. In one embodiment, the composition for forming a transparent conductive layer is prepared by dispersing the metal nanowires in any appropriate solvent. Examples of the solvent include water, alcohol-based solvents, ketone-based solvents, ether-based solvents, hydrocarbon-based solvents, and aromatic solvents. The composition for forming a transparent conductive layer may further include additives such as a resin (binder resin), a conductive material other than the metal nanowires (e.g., conductive particles), and a leveling agent. The composition for forming a transparent conductive layer may also include additives such as a plasticizer, a heat stabilizer, a light stabilizer, a lubricant, an antioxidant, an ultraviolet absorber, a flame retardant, a colorant, an antistatic agent, a compatibilizer, a crosslinking agent, a thickener, inorganic particles, a surfactant, and a dispersant.
[0036] The viscosity of the composition for forming a transparent conductive layer is preferably 5 mP·s / 25°C to 300 mP·s / 25°C, and more preferably 10 mP·s / 25°C to 100 mP·s / 25°C. Within such a range, the effects of the present invention are prominent. The viscosity of the composition for forming a transparent conductive layer can be measured using a rheometer (e.g., MCR302 by Anton Paar).
[0037] The dispersion concentration of the metal nanowires in the composition for forming a transparent conductive layer is preferably 0.01% by weight to 5% by weight. If it is in this range, the effects of the present invention become prominent.
[0038] The method for applying the composition for forming a transparent conductive layer may be any appropriate method, such as spray coating, bar coating, roll coating, die coating, inkjet coating, screen coating, dip coating, letterpress printing, intaglio printing, gravure printing, or the like.
[0039] The coating layer preferably has a basis weight of 0.3 g / m 2 ~30g / m 2 and more preferably 1.6 g / m 2 ~16g / m 2 Within such a range, the metal nanowires can be well dispersed by the air blowing in the air blowing step, and a transparent conductive film with smaller conductive anisotropy can be produced.
[0040] The thickness Ts of the coating layer in the coating step is preferably 10 μm to 50 μm, more preferably 13 μm to 40 μm, even more preferably 13 μm to 30 μm, and particularly preferably 13 μm to 20 μm. Within such a range, a transparent conductive film with particularly excellent conductivity can be obtained. The thickness Ts (hereinafter also referred to as the initial thickness Ts of the coating layer) means the thickness (wet thickness) of the coating layer immediately after the coating. The thickness Ts (wet thickness) of the coating layer can be measured by an optical interference type film thickness meter (for example, the "Spectrometer FLAME-S" manufactured by Ocean Insight).
[0041] (Leave process) As described above, the leaving step is a step of leaving the coating layer for a predetermined time. More specifically, it is a step of leaving the laminated structure including the substrate and the coating layer in a windless environment at 25° C. or less (preferably 20° C. to 25° C.). In this specification, the windless state refers to a state in which the wind speed (relative wind speed in the case of transporting the substrate) is less than 0.5 m / s. In addition, in this specification, "leaving" means reducing the thickness of the coating layer in a windless state, and is a concept that also includes an operation of reducing the thickness of the coating layer while transporting the laminated structure including the substrate and the coating layer.
[0042] The time for leaving the coating layer is, for example, 1 to 300 seconds. The time for leaving the coating layer corresponds to the time from the formation of the coating layer in the previous step to the start of air blowing in the subsequent step.
[0043] In the present invention, a transparent conductive film with excellent conductivity can be obtained by leaving the coating layer for a predetermined time and then performing the next step of blowing air. When comparing the transparent conductive film obtained by the above manufacturing method with a transparent conductive film obtained by drying the coating layer without blowing air, or a transparent conductive film obtained by blowing air on the coating layer immediately after coating, the transparent conductive film obtained by the above manufacturing method has superior conductivity per unit weight of the metal nanowires. According to the manufacturing method of the present invention, by leaving the coating layer for a predetermined time, the flow of the metal nanowires in the coating layer can be favorably adjusted, and the number of contact points between the metal nanowires increases, which is thought to result in the above-mentioned effects.
[0044] The thickness of the coating layer after the leaving step (thickness Tb of the coating layer when air blowing is started in the air blowing step) is preferably more than 1 μm, and more preferably 2 μm or more. In other words, it is preferable to end the leaving step before the thickness of the coating layer becomes 1 μm or less (preferably less than 2 μm). In this way, the flow of the metal nanowires in the coating layer can be favorably adjusted, and more points of contact between the metal nanowires can be created.
[0045] In one embodiment, the standing time is determined based on the thickness Ts of the coating layer in the coating step and the thickness of the coating layer after the standing step (the thickness Tb of the coating layer when air blowing is started in the air blowing step). In one embodiment, the thickness Tb of the coating layer when air blowing is started in the air blowing step is 25% to 90%, more preferably 27% to 89%, and even more preferably 30% to 88% of the thickness Ts of the coating layer in the coating step. Within such a range, the flow of the metal nanowires in the coating layer can be preferably adjusted, and the number of contact points between the metal nanowires increases, making it possible to obtain a transparent conductive film with high conductivity per unit weight of the metal nanowires.
[0046] In one embodiment, the coating layer is preferably left until the thickness of the coating layer becomes 2 μm to 12 μm thinner than the initial thickness Ts of the coating layer, more preferably until the thickness of the coating layer becomes 4 μm to 11 μm thinner than the initial thickness Ts of the coating layer, even more preferably until the thickness of the coating layer becomes 6 μm to 10 μm thinner than the initial thickness Ts of the coating layer, and preferably until the thickness of the coating layer becomes 6 μm to 9 μm thinner than the initial thickness Ts of the coating layer. Within such a range, the flow of the metal nanowires in the coating layer can be preferably adjusted, and the number of contact points between the metal nanowires can be increased.
[0047] In addition, when the initial thickness Ts of the coating layer is 10 μm to 13 μm, it is preferable to leave the coating layer until the thickness Tb of the coating layer becomes 2.5 μm to 9 μm, and it is more preferable to leave the coating layer until the thickness Tb of the coating layer becomes 3 μm to 5 μm. In addition, when the initial thickness Ts of the coating layer is more than 13 μm and less than 16 μm, it is preferable to leave the coating layer until the thickness Tb of the coating layer becomes 4 μm to 12 μm, and it is more preferable to leave the coating layer until the thickness Tb of the coating layer becomes 5 μm to 7 μm. In addition, when the initial thickness Ts of the coating layer exceeds 16 μm (preferably more than 16 μm to 30 μm or less, more preferably more than 16 μm to 20 μm or less), it is preferable to leave the coating layer until the thickness Tb of the coating layer becomes 6 μm to 14 μm, and it is more preferable to leave the coating layer until the thickness Tb of the coating layer becomes 7 μm to 9 μm. Within such a range, the flow of the metal nanowires in the coating layer can be preferably adjusted, and the number of contact points between the metal nanowires can be increased.
[0048] (Blowing process) Air can be blown to the coating layer by any appropriate method. In one embodiment, air can be blown to the coating layer using an air blower arranged above (opposite side to the substrate) and / or to the side of the coating layer. The air blowing direction can be any appropriate direction. For example, the air blowing direction may be set to a predetermined angle (for example, 10° to 170°) with respect to the coating layer surface, or may be blown approximately parallel to the coating layer surface (for example, less than 10° with respect to the coating layer surface). Air blowing in a spiral shape may also be blown. The air blowing direction can be adjusted, for example, by providing a louver on the air blower and adjusting the direction of the louver. In one embodiment, the air blowing direction is determined by the opening direction of the louver. In addition, when blowing a spiral wind, a air blower equipped with a spiral wind direction plate at the air blowing port can be used.
[0049] The wind speed of the wind is preferably 0.5 m / s to 10 m / s, more preferably 1 m / s to 5 m / s. Within such a range, the metal nanowires are well dispersed, and a transparent conductive film having excellent conductivity can be produced. In addition, a transparent conductive film having excellent surface smoothness and thickness uniformity can be obtained. The wind speed can be appropriately set depending on the solvent contained in the transparent conductive layer forming composition. When a transparent conductive layer forming composition prepared with water is used, the wind speed is preferably 0.5 m / s to 10 m / s, more preferably 1 m / s to 5 m / s. In this specification, the wind speed means the wind speed at the time when it reaches the coating layer.
[0050] The temperature of the air is preferably 10° C. to 50° C., and more preferably 15° C. to 30° C. The air speed can be appropriately set depending on the solvent contained in the composition for forming a transparent conductive layer, etc. When a composition for forming a transparent conductive layer prepared with water is used, the temperature of the air is preferably 10° C. to 50° C., and more preferably 15° C. to 30° C. In this specification, the temperature of the air means the temperature of the air at the time when it reaches the coating layer.
[0051] The air blowing time is preferably 1 to 10 minutes, and more preferably 2 to 5 minutes. Within this range, the metal nanowires are well dispersed, and a transparent conductive film with smaller conductive anisotropy can be produced. Specifically, if the air blowing area is determined so that the air blowing time falls within the above range, the metal nanowires can be appropriately dispersed throughout the coating layer. In addition, a transparent conductive film with excellent surface smoothness and thickness uniformity can be obtained.
[0052] In the air blowing step, air may be blown in multiple stages. For example, air may be blown in stages into zones having different wind directions, wind speeds, temperatures, etc.
[0053] After the air blowing step, any appropriate treatment may be performed. For example, when a transparent conductive layer forming composition containing a binder resin is used, a curing treatment such as ultraviolet irradiation may be performed. In addition, after the delivery step, a drying step may be performed. Examples of the drying method include oven heating and natural drying. EXAMPLES
[0054] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The evaluation methods in the examples are as follows. The thickness was measured using an optical interference type film thickness meter ("Spectrometer FLAME-S" manufactured by Ocean Insight).
[0055] (1) Surface resistance, conductivity The surface resistance values (MD and TD surface resistance values) of the transparent conductive film were measured by an eddy current method using a non-contact surface resistance meter (product name "EC-80") manufactured by Napson Co., Ltd. The measurement temperature was 23°C. The reciprocal of the surface resistance value was calculated to obtain the conductivity. Also, {conductivity y(1 / Ω) / 1m 2 Amount of metal nanowires per unit x (g / m 2 )}, a(m 2 / Ω·g) was calculated.
[0056] (2) Haze value The haze value of the transparent conductive film was measured by the method defined in JIS 7136 using a haze meter (manufactured by Murakami Color Science Laboratory, product name "HN-150").
[0057] [Production Example 1] Preparation of composition for forming transparent conductive layer Silver nanowires were synthesized based on the method described in Chem. Mater. 2002, 14, 4736-4745. The silver nanowires obtained above were dispersed in pure water to a concentration of 0.2% by weight, and dodecyl-pentaethylene glycol was dispersed to a concentration of 0.1% by weight, to obtain a composition for forming a transparent conductive layer.
[0058] [Example 1] A PET film (manufactured by Mitsubishi Plastics, product name "S100") was used as the substrate. While this substrate was being transported using a transport roll, the composition for forming a transparent conductive layer prepared in Production Example 1 was applied onto the substrate using a bar coater (manufactured by Daiichi Rika Co., Ltd., product name "Bar Coater No. 6") to form a coating layer having a thickness (initial thickness Ts of the coating layer) of 13 μm (i.e., 1 m 2 Amount of metal nanowires per unit x (g / m 2 )=0.012g / m 2 ). After that, it was left until the thickness of the coating layer (the thickness Tb of the coating layer when the air blowing process starts) became 9.1 μm (i.e., Tb / Ts=0.7) (left-standing process). Next, air was blown from the center of the substrate to both ends in a direction from the inside in the width direction to both outside in the width direction. The angle between the transport direction of the substrate and the air blowing direction (air blowing direction as seen from the coating layer surface side) was 90°, and the angle between the transport direction of the substrate and the air blowing direction (air blowing direction as seen from the side of the coating layer) was 0°. The wind speed was 2 m / s, and the air temperature was 25° C. The air blowing time (drying time) was 2 minutes. The obtained transparent conductive film was subjected to the above evaluations (1) and (2), and the results are shown in Table 1.
[0059] [Examples 2 to 8, Comparative Examples 1 to 2] A transparent conductive film was obtained in the same manner as in Example 1, except that the initial thickness Ts of the coating layer (resulting in the amount x of metal nanowires) and the thickness Tb of the coating layer when air blowing was started in the air blowing step (at the start of air blowing) were set as shown in Table 1. The obtained transparent conductive film was subjected to the above evaluations (1) and (2). The results are shown in Table 1.
[0060] [Comparative Example 3] A PET film (manufactured by Mitsubishi Plastics, product name "S100") was used as the substrate. While this substrate was being transported using a transport roll, the composition for forming a transparent conductive layer prepared in Production Example 1 was applied onto the substrate using a bar coater (manufactured by Daiichi Rika Co., Ltd., product name "Bar Coater No. 6") to form a coating layer having a thickness of 13 μm (i.e., 1 m 2 Amount of metal nanowires per unit x (g / m 2 )=0.012g / m 2 ). The substrate on which the coating layer was formed was then placed in an oven at an oven temperature of 100°C for 2 minutes to obtain a transparent conductive film. The obtained transparent conductive film was subjected to the above evaluations (1) and (2). The results are shown in Table 1.
[0061] [Table 1]
[0062] As is clear from Table 1, according to the present invention, the electrical conductivity y(1 / Ω) / 1m 2 Amount of metal nanowires per unit x (g / m 2 )} of the above "y=a×x (1)" 2 By setting the coefficient of electrical conductivity (Hg) at a specific value or more, it is possible to obtain a transparent conductive film in which high electrical conductivity and low haze value are well-adjusted and well-balanced. Such a transparent conductive film can be obtained by manufacturing the film through a leaving step. Furthermore, the above effect becomes more pronounced by optimizing the thickness of the coating layer at the start of blowing air (optimizing the leaving time) according to the initial thickness of the coating layer. [Explanation of symbols]
[0063] 10 Base material 20 Transparent conductive layer 100 Transparent conductive film
Claims
1. The transparent conductive layer is produced by a production method including a coating step of coating a substrate with a composition for forming a transparent conductive layer, the composition including silver nanowires, to form a coating layer, a leaving step of leaving the coating layer, and a blowing step of blowing air onto the coating layer after the leaving step, A transparent conductive film comprising the substrate and a transparent conductive layer disposed on one side of the substrate, a thickness Tb of the coating layer after the leaving step is 25% to 90% of a thickness Ts of the coating layer in the coating step; the transparent conductive layer comprises silver nanowires; The amount of silver nanowires in the transparent conductive layer x (g / m 2 The relationship between the conductivity y (1 / Ω) of the transparent conductive film and the surface roughness y of the transparent conductive film is expressed by the following formula (1): Transparent conductive film: y=axx...(1) In formula (1), a is 0.77 to 0.
96.
2. The transparent conductive film according to claim 1 , which has a haze value of 20% or less.
3. 3. The transparent conductive film according to claim 1, having a surface resistance of 0.1 Ω / □ to 1000 Ω / □.
4. The amount of silver nanowires in the transparent conductive layer x (g / m 2 ) is 0.005 g / m 2 ~0.05g / m 2 The transparent conductive film according to claim 1 ,
Citation Information
Patent Citations
Steamer
JP1986099034A
Transparent conductors based on nanowires
JP2009505358A
Electroconductive film, sensor, touch panel, and image display device
WO2019172423A1