Electrode catalyst, composition for forming gas diffusion electrode, gas diffusion electrode, membrane-electrode assembly, and fuel cell stack

The PtNi/C catalyst with optimized particle distribution inside hollow carbon mesopores addresses the high cost of platinum in PEFCs by enhancing catalytic activity and reducing platinum dissolution, contributing to cost-effective PEFC performance.

JP7555716B2Active Publication Date: 2024-09-25N E CHEMCAT
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020051422
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-23
Publication Date
2024-09-25
Estimated Expiration
2040-03-23

AI Technical Summary

Technical Problem

Existing electrode catalysts for polymer electrolyte fuel cells (PEFC) are costly due to the high proportion of noble metals like platinum, and there is a need to reduce the amount of platinum used while maintaining or improving catalytic activity.

Method used

A PtNi/C catalyst is developed with a structure where a large proportion of PtNi alloy particles are supported inside the mesopores of a hollow carbon carrier, optimized through three-dimensional reconstructed images from electron tomography, ensuring at least 50% of the catalyst particles are inside the mesopores, reducing direct contact with polymer electrolyte and minimizing platinum dissolution.

Benefits of technology

The catalyst exhibits enhanced catalytic activity, leading to reduced platinum usage and lower material costs, with improved durability and performance in PEFCs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555716000003
    Figure 0007555716000003
  • Figure 0007555716000004
    Figure 0007555716000004
  • Figure 0007555716000005
    Figure 0007555716000005
Patent Text Reader

Abstract

To provide an electrode catalyst having an excellent catalytic activity which can be contributed to a low cost of a PEFC.SOLUTION: An electrode catalyst contains: a hollow carbon carrier having a meso hole of which a pore size is 2 to 50nm; and a plurality of catalyst particles carried on the carrier. The catalyst particles are held on both of an inner part and an outer part of the meso hole of the carrier, and contain a PtNi alloy. When executing an analysis of a particle diameter distribution of each catalyst particle using a three-dimentional reconstruction image obtained by an electron beam tomography measurement using a STEM, a rate of the catalyst particles carried in the inner part of the meso hole is 50% or larger.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to an electrode catalyst having a core-shell structure, more particularly to an electrode catalyst suitable for use in a gas diffusion electrode, and more particularly to an electrode catalyst suitable for use in a gas diffusion electrode of a fuel cell. The present invention also relates to a composition for forming a gas diffusion electrode, a membrane-electrode assembly, and a fuel cell stack, each of which contains the electrode catalyst particles. [Background technology]

[0002] 2. Description of the Related Art Polymer electrolyte fuel cells (hereinafter referred to as "PEFC" as necessary) are being researched and developed as power sources for fuel cell vehicles and home cogeneration systems. The catalyst used in the gas diffusion electrode of a PEFC is a precious metal catalyst made of precious metal particles of a platinum group element such as platinum (Pt).

[0003] For example, a typical conventional catalyst is a "Pt-supported carbon catalyst" (hereinafter referred to as "Pt / C catalyst" as necessary), which is a powder of catalyst particles in which Pt fine particles are supported on conductive carbon powder. The cost of precious metal catalysts such as Pt accounts for a large proportion of the manufacturing cost of PEFCs, and this is a challenge to reducing the cost of PEFCs and promoting their widespread use. In the course of these research and development efforts, in order to reduce the amount of platinum used, powders (hereinafter referred to as "core-shell catalysts" as needed) of catalyst particles having a core-shell structure (hereinafter referred to as "core-shell catalyst particles" as needed) formed from a core portion made of a non-platinum element and a shell portion made of Pt have been studied, and many reports have been published.

[0004] For example, Patent Document 1 discloses a particle composite (corresponding to a core-shell catalyst particle) having a configuration in which palladium (Pd) or a Pd alloy (corresponding to a core portion) is coated with an atomically thin layer of Pt atoms (corresponding to a shell portion). Furthermore, Patent Document 1 describes, as an example, a core-shell catalyst particle having a configuration in which the core portion is a Pd particle and the shell portion is a layer made of Pt. On the other hand, there are two types of supports for electrode catalysts: hollow carbon, which has many internal pores, and solid carbon, which has fewer internal pores than hollow carbon. Studies are being conducted to improve performance by taking advantage of the characteristics of each.

[0005] For example, Patent Document 2 discloses a study example in which hollow carbon is used as a carrier, and Patent Document 3 discloses a study example in which solid carbon is used as a carrier. For example, Patent Document 2 discloses the configuration of an electrode catalyst 200 in which, as shown in FIG. 10, the pore volume and mode diameter of the pore distribution of pores (primary pores, mesopores) P220 with a pore diameter of 4 to 20 nm in a porous support (hollow carbon) 220 with an average particle diameter of 20 to 100 nm are controlled within predetermined ranges, and catalyst particles 230 are supported in the primary pores (mesopores) P220 of the support 220. Patent Document 2 mentions that this prevents the polymer electrolyte from being adsorbed onto the surface of the catalyst particles 230 present in the primary pores (mesopores) P220, making it possible to prevent a decrease in the effective reaction surface area of ​​the catalyst while ensuring sufficient gas transportability. Furthermore, it mentions that as a result, the activity per catalyst weight is improved, and a fuel cell catalyst layer that exhibits excellent power generation performance can be provided even when the catalyst amount is reduced.

[0006] Furthermore, for example, Patent Document 3 discloses an electrode catalyst (PtCo / C catalyst) for fuel cells that has a solid carbon support and catalyst particles containing an alloy of platinum and cobalt supported on the support. This electrode catalyst has a platinum to cobalt molar ratio of 4 to 11:1 in the alloy, and is acid-treated at 70 to 90°C. In Patent Document 3, when a PtCo alloy is supported on a hollow carbon support, a portion of the PtCo alloy is contained inside the hollow carbon support, and even if an acid treatment is performed to suppress the elution of Co, it is difficult to sufficiently treat the PtCo alloy present inside the support, and as a result, it is considered a problem that Co is easily eluted from the PtCo alloy present inside the support. Therefore, Patent Document 3 mentions that by using a solid carbon support instead of a hollow carbon support, it is possible to prevent the PtCo alloy from being contained within the support. Furthermore, it discloses that this allows the PtCo alloy to be sufficiently acid-treated, thereby suppressing the elution of Co. It also mentions that as a result, it is possible to achieve both good initial performance and durability of the fuel cell.

[0007] Here, Patent Document 3 defines solid carbon as follows: That is, Patent Document 3 states that solid carbon is carbon with fewer voids inside it compared to hollow carbon, and specifically, it is carbon for which the ratio (t-Pot surface area / BET surface area) of the BET surface area determined by N2 adsorption to the external surface area determined by t-Pot (the surface area of ​​the outside of a particle calculated from the particle size) is 40% or more. The "t-Pot surface area" described in Patent Document 3 is understood to refer to the "t-plot surface area" described, for example, in the technical report "Analysis of Micropore Surface Area Using the t-plot Method" published online by MC Evatec Co., Ltd. on February 1, 2019. Analysis of micropore surface area using the t-plot method is one method of analysis based on nitrogen adsorption isotherms (adsorption temperature: 77 K). This method compares and converts adsorption isotherm data with standard isotherms to plot a graph of the relationship between the adsorption layer thickness t and the amount of adsorption. In addition to being able to separate and quantify the specific surface area into the inside and outside of the pores, the shape of the graph also allows for understanding the pore trends. Furthermore, examples of solid carbon include the carbon described in Japanese Patent No. 4362116, and it is disclosed that specific examples include Denka Black (registered trademark) manufactured by Denki Kagaku Kogyo Kabushiki Kaisha.

[0008] Furthermore, Patent Document 4 discloses an electrode catalyst (core-shell catalyst) in which catalyst particles are supported both inside and outside the mesopores of a hollow carbon support. This electrode catalyst has a configuration in which the proportion of catalyst particles supported inside the mesopores is 50% or more when the particle size distribution of the catalyst particles is analyzed using three-dimensional reconstructed images obtained by electron tomography measurement using a STEM (scanning transmission electron microscope). The following Non-Patent Documents 1 and 2 disclose examples in which the proportion of catalyst particles supported inside pores and the proportion of catalyst particles supported outside pores of catalyst particles supported on a hollow carbon support are analyzed using a method different from that used in Patent Document 4. More specifically, in Non-Patent Document 1, a group of Strasser et al. at the Technical University of Berlin reported that a commercially available hollow carbon (product name: "ketjenblack EC-300J", manufactured by Akzo Nobel, specific surface area: about 839 m) 2 g -1 They reported the results of simultaneously capturing SEM (Scanning Electron Microscopy) and TSEM (Transmission SEM) images of specific Pt / C catalyst particles of interest in the same measurement area for a Pt / C catalyst in which Pt particles are highly dispersed on a substrate. See, for example, Table 1, Figure 2, and the right column on page 79 of Non-Patent Document 1.

[0009] In their method, SEM images provide information on the Pt particles present only on the observed portion (one of the outer surfaces) of the hollow carbon support particles. In other words, information on the number of catalyst particles supported on the exterior of the hollow carbon support particles is obtained. On the other hand, TSEM images (transmission images) provide information on all catalyst particles (Pt particles) supported on the exterior and interior of the observed Pt / C catalyst particles. They then attempted to distinguish between Pt particles supported on the exterior surface and those supported internally, among the Pt particles supported on the hollow carbon support particles, using information from TSEM and SEM images. Here, they did not measure the "opposite back surface" of the observed portion of the outer surface of the hollow carbon support particle ("one side outer surface") in the SEM image. They assumed that the state of the "one side outer surface" and the state of the "opposite back surface" were the same. In other words, they assumed that the number of catalyst particles supported on the "one side outer surface" was the same as the number of catalyst particles supported on the "opposite back surface."

[0010] Next, in Non-Patent Document 2, Uchida and his group at Yamanashi University reported the results of using a STEM (Scanning Transmission Electron Microscope) device capable of taking SEM and TEM (Transmission Electron Microscopy) images of Pt / C catalyst particles to photograph a Pt / C catalyst in which Pt particles were highly dispersed in commercially available hollow carbon (trade name: "Ketjenblack", manufactured by Ketjen Black International, specific surface area: approximately 875 m2 g-1). For example, see Figure 1, Table 2, and the lower right column on page 181 of Non-Patent Document 2. First, they obtained information on the number of all Pt particles supported on hollow carbon support particles from a TEM image of a specific Pt / C catalyst particle of interest. Next, they measured SEM images of the same Pt / C catalyst particle as the TEM image to obtain information on the number of Pt particles present only on the back surface of the hollow carbon support particle. Next, they used a special 3D sample holder to rotate the specific Pt / C catalyst particle of interest (the measurement sample) precisely 180 degrees to measure an SEM image of only the back surface of the same Pt / C catalyst particle. Using this information, they attempted to distinguish between Pt particles supported on the outer surface and those supported internally on hollow carbon support particles. The "internal loading rate" measured by this method = "100 × (number of Pt particles loaded internally) / (total number of Pt particles)" and they reported that it was 62% for a commercially available 30 wt% Pt / C catalyst (trade name: "TEC10E30E", manufactured by Tanaka Metal Industries Co., Ltd., referred to as "c-Pt / CB" in the specification) and over 50% for a commercially available 46 wt% Pt / C catalyst (trade name: "TEC10E50E", manufactured by Tanaka Metal Industries Co., Ltd., referred to as "Pt / CB" in the specification).

[0011] As explained above, the present inventors recognize that the analysis methods of Non-Patent Documents 1 and 2 differ from the analysis method of Patent Document 4 in the following respects: That is, the analysis method using electron tomography measurement of Patent Document 4 is a three-dimensional reconstruction method using an electron microscope, in which electron microscope images of the same field of view of a measurement sample projected from various directions are reconstructed into a three-dimensional image in a computer, and a tomogram is created using the computer. On the other hand, the analysis method of Non-Patent Document 1 uses two-dimensional images, such as SEM images and TSEM images, taken from a specific direction of the measurement sample. Furthermore, the analysis method of Non-Patent Document 2 uses two-dimensional images, such as SEM images taken from two specific directions of the measurement sample (two directions obtained by rotating the sample holder by 180°) and TSEM images taken from a specific direction of the measurement sample. With the analysis methods of Non-Patent Document 1 and Non-Patent Document 2, for example, if the measurement sample (electrode catalyst particles) has irregularities, there is a high possibility that some catalyst particles may exist whose loading position cannot be adequately determined as being inside or outside the hollow carbon support. The analytical method of Patent Document 4 uses a three-dimensional tomogram of the measurement sample, which can be observed from various reports, making it possible to visually confirm and more accurately grasp the support positions on the carrier of the catalyst particles contained in the electrode catalyst particles of the measurement sample. The applicant of the present patent application presents the following publications as publications in which the above-mentioned publicly known inventions are described: [Prior art documents] [Patent documents]

[0012] [Patent Document 1] U.S. Patent Application Publication No. 2007 / 31722 [Patent Document 2] Japanese Patent Application Laid-Open No. 2013-109856 [Patent Document 3] WO2016 / 063968 publication [Patent Document 4] WO2019 / 221168 publication [Non-patent literature]

[0013] [Non-Patent Document 1] Nature Materials Vol 19 (January 2020)77-85 [Non-patent document 2] Journal of Power Sources 315(2016)179-191 Summary of the Invention [Problem to be solved by the invention]

[0014] Toward the widespread use of PEFCs, further improvement in catalytic activity of electrode catalysts is required to reduce the amount of Pt used and material costs. The present inventors analyzed the particle size distribution of catalyst particles in a PtNi / C catalyst, in which PtNi alloy particles are supported on a carbon support, using three-dimensional reconstructed images obtained by electron tomography measurement using a STEM (scanning transmission electron microscope). They found that there have been no reports to date of actually synthesizing an improved product in which catalyst particles are supported in greater numbers inside the mesopores of hollow carbon than outside, and that there is still room for improvement. The present invention has been made in view of the above technical circumstances, and has an object to provide an electrode catalyst (PtNi / C catalyst) having excellent catalytic activity that can contribute to cost reduction of PEFCs. Another object of the present invention is to provide a composition for forming a gas diffusion electrode, a gas diffusion electrode, a membrane electrode assembly (MEA), and a fuel cell stack, each of which contains the electrode catalyst. [Means for solving the problem]

[0015] The present inventors have conducted extensive research into a configuration of an electrode catalyst in which a large number of PtNi / C catalyst particles are supported within the mesopores of hollow carbon, in order to achieve further improvement in catalytic activity. As a result, the inventors have found that supporting catalyst particles on a carrier so as to satisfy the following conditions is effective in improving catalytic activity, and have completed the present invention. More specifically, the present invention comprises the following technical features.

[0016] That is, the present invention provides: The present invention comprises a hollow carbon support having mesopores with a pore diameter of 2 to 50 nm, and a plurality of catalyst particles supported on the support, the catalyst particles contain a PtNi alloy; the catalyst particles are supported both inside and outside the mesopores of the support; When the particle size distribution of the catalyst particles is analyzed using a three-dimensional reconstructed image obtained by electron tomography measurement using a STEM (scanning transmission electron microscope), the proportion of the catalyst particles supported inside the mesopores is 50% or more. An electrode catalyst is provided.

[0017] As described above, by supporting PtNi / C catalyst particles on a hollow carbon support so that the proportion of catalyst particles supported inside the mesopores is 50% or more, the electrode catalyst of the present invention can exhibit excellent catalytic activity that can contribute to cost reduction of PEFCs. The detailed reasons why the electrode catalyst of the present invention has excellent catalytic activity have not been fully elucidated. However, the present inventors believe that, compared to conventional electrode catalysts, a PtNi / C catalyst in which 50% or more of the catalyst particles are supported inside the mesopores has a large number of highly active catalyst particles with relatively small particle diameters present inside the mesopores of the support. The catalyst particles supported inside the mesopores of such a support are supported on the support in a state where they are unlikely to come into direct contact with the polymer electrolyte present in the catalyst layer. Therefore, the electrode catalyst of the present invention is less susceptible to a decrease in catalytic activity due to poisoning of the Pt component, and can exhibit superior catalytic activity when formed into an electrode compared to conventional electrode catalysts. Furthermore, the electrode catalyst of the present invention also reduces dissolution of the Pt component and Ni component. Furthermore, in the electrode catalyst of the present invention, from the viewpoint of more reliably obtaining the effects of the present invention, when the particle size distribution of the catalyst particles is analyzed using a three-dimensional reconstructed image obtained by electron tomography measurement using a STEM (scanning transmission electron microscope), it is preferable that the proportion of the catalyst particles supported inside the mesopores is 60% or more.

[0018] Furthermore, in order to more reliably obtain the effects of the present invention, it is preferable that the electrode catalyst of the present invention simultaneously satisfies the conditions of the following formulas (1) and (2) when an analysis of the particle size distribution of the catalyst particles is carried out using a three-dimensional reconstructed image obtained by electron tomography measurement using a STEM (scanning transmission electron microscope). D1 <D2···(1) (N1 / N2)>1.0 (2) In the formulas (1) and (2), D1 represents the equivalent sphere diameter of the catalyst particles that exhibit the highest frequency among the catalyst particles supported inside the mesopores of the support, and D2 represents the equivalent sphere diameter of the catalyst particles that exhibit the highest frequency among the catalyst particles supported outside the mesopores of the support. In addition, in the formulas (1) and (2), N1 represents the frequency of the catalyst particles that exhibits the highest frequency among the catalyst particles supported inside the mesopores of the support, and N2 represents the frequency of the catalyst particles that exhibits the highest frequency among the catalyst particles supported outside the mesopores of the support.

[0019] By supporting catalyst particles of a core-shell catalyst on a hollow carbon support so as to simultaneously satisfy the conditions of the above-mentioned formula (1) and formula (2), the electrode catalyst of the present invention can more reliably exhibit excellent catalytic activity that can contribute to cost reduction of PEFCs. Here, in the present invention, "hollow carbon" refers to carbon that has more voids inside it than the solid carbon described above, and refers to conductive carbon that has mesopores with a pore size defined by IUPAC of 2 to 50 nm.

[0020] Furthermore, in the electrode catalyst of the present invention, at least a portion of the surface of the catalyst particle may be coated with a Pt oxide film to the extent that the catalyst particle can exhibit excellent catalytic activity. In the electrode catalyst of the present invention, at least a part of the surface of the catalyst particle may be coated with a Ni oxide film, as long as the catalyst particle can exhibit excellent catalytic activity. Furthermore, the electrode catalyst of the present invention may contain second catalyst particles made of Pt (zero valence) within the range in which the effects of the present invention can be obtained. The electrode catalyst of the present invention may also contain third catalyst particles made of Ni (zero valent) within the range in which the effects of the present invention can be obtained. Furthermore, from the viewpoint of more reliably obtaining the effects of the present invention, it is preferable that the hollow carbon support in the electrode catalyst of the present invention is Ketjenblack EC300J. In the present invention, the BET specific surface area (nitrogen adsorption specific surface area) of the hollow carbon support (Ketjen Black EC300J) is 750 to 850 m 2 / g is preferred.

[0021] The present invention also provides an electrode catalyst powder containing 10 wt % or more of the above-mentioned electrode catalyst of the present invention. In addition, in the electrode catalyst powder, "components other than the above-mentioned electrode catalyst of the present invention" means "electrode catalysts other than the above-mentioned electrode catalyst of the present invention." In other words, the electrode catalyst powder of the present invention does not include powders that do not function as an electrode catalyst. The electrode catalyst powder of the present invention contains the above-mentioned electrode catalyst of the present invention, and therefore can exhibit excellent catalytic activity that can contribute to reducing the cost of PEFCs. Here, from the viewpoint of more reliably obtaining the effects of the present invention, the content ratio of the above-mentioned electrode catalyst of the present invention in the electrode catalyst powder of the present invention is preferably 30 wt % or more, more preferably 50 wt % or more, even more preferably 70 wt % or more, and most preferably 90 wt % or more. The electrode catalyst powder of the present invention may contain, in addition to the above-mentioned electrode catalyst of the present invention, an electrode catalyst (for convenience, referred to as "electrode catalyst P") having the following configuration.

[0022] That is, the electrode catalyst P includes a hollow carbon support having mesopores with a pore diameter of 2 to 50 nm, and a plurality of catalyst particles supported on the support, the catalyst particles contain a PtNi alloy, the catalyst particles are supported both inside and outside the mesopores of the support; When the particle size distribution of the catalyst particles is analyzed using a three-dimensional reconstructed image obtained by electron tomography measurement using a STEM (scanning transmission electron microscope), the proportion of the catalyst particles supported inside the mesopores is "less than 50%." The electrode catalyst powder of the present invention may be composed of the above-mentioned electrode catalyst of the present invention and the electrode catalyst P. In this case, too, from the viewpoint of more reliably obtaining the effects of the present invention, the content of the above-mentioned electrode catalyst of the present invention in the powder of the electrode catalyst of the present invention is preferably 30 wt % or more, more preferably 50 wt % or more, even more preferably 70 wt % or more, and most preferably 90 wt % or more.

[0023] Furthermore, the present invention provides a gas diffusion electrode forming assembly containing the electrode catalyst of the present invention. The product is provided. The composition for forming a gas diffusion electrode of the present invention contains the electrode catalyst of the present invention, and therefore, It is easy to develop a gas diffusion electrode with excellent catalytic activity (polarization characteristics) that can contribute to cost reduction of C. It can be manufactured.

[0024] The present invention also provides a gas diffusion electrode containing the above-mentioned electrode catalyst of the present invention. The gas diffusion electrode of the present invention is configured to contain the electrode catalyst of the present invention. It is possible to make the structure have excellent catalytic activity (polarization characteristics) that can contribute to cost reduction of EFC. It becomes easier.

[0025] Furthermore, the present invention provides a membrane-electrode assembly (MEA) comprising the gas diffusion electrode of the present invention. A) is provided. The membrane-electrode assembly (MEA) of the present invention includes the gas diffusion electrode of the present invention, and therefore, This makes it easy to create a configuration with battery characteristics that can contribute to reducing the cost of FCs.

[0026] The present invention is also characterized in that it includes the membrane electrode assembly (MEA) of the present invention. The present invention provides a fuel cell stack. According to the fuel cell stack of the present invention, the fuel cell stack includes the membrane electrode assembly (MEA) of the present invention. Therefore, it is easy to create a structure with battery characteristics that can contribute to reducing the cost of PEFC. become. [Effects of the Invention]

[0027] According to the present invention, an electrode catalyst having excellent catalytic activity that can contribute to cost reduction of PEFCs is provided. A medium is provided. According to the present invention, there is also provided a composition for forming a gas diffusion electrode, a gas diffusion electrode, and a method for forming a gas diffusion electrode, each of which contains the electrode catalyst. Dispersed electrodes, membrane electrode assemblies (MEAs), and fuel cell stacks are provided. [Brief explanation of the drawings]

[0028] [Figure 1] FIG. 1 is a schematic cross-sectional view showing a preferred embodiment of an MEA of the present invention. [Figure 2] FIG. 2 is a schematic cross-sectional view showing a preferred embodiment of the electrode catalyst of the present invention contained in at least one of the cathode catalyst layer and the anode catalyst layer of the MEA shown in FIG. [Figure 3] FIG. 3 is an enlarged schematic cross-sectional view showing the schematic configuration of the electrode catalyst shown in FIG. 2. [Figure 4] FIG. 2 is a schematic cross-sectional view showing another preferred embodiment of the MEA of the present invention. [Figure 5] FIG. 1 is a schematic cross-sectional view showing a preferred embodiment of a CCM of the present invention. [Figure 6] FIG. 2 is a schematic cross-sectional view showing another preferred embodiment of the CCM of the present invention. [Figure 7] 1 is a schematic cross-sectional view showing a preferred embodiment of a GDE of the present invention. [Figure 8] FIG. 2 is a schematic cross-sectional view showing another preferred embodiment of the GDE of the present invention. [Figure 9] 1 is a schematic diagram showing a preferred embodiment of a fuel cell stack of the present invention. [Figure 10] FIG. 1 is a schematic cross-sectional view showing a conventional electrode catalyst. [Figure 11] 1 is a STEM image showing the 3D electron tomography measurement conditions (volume size) using a STEM for the electrode catalyst of Example 1. [Figure 12] 1 is a 3D-STEM image (three-dimensional reconstruction image) of the catalyst of Example 1. [Figure 13] 13 is a graph showing the particle size distribution of internal particles among catalyst particles obtained by image analysis of the 3D-STEM image of the catalyst of Example 1 shown in FIG. 12. [Figure 14] 13 is a graph showing the particle size distribution of outer particles among catalyst particles obtained by image analysis of the 3D-STEM image of the catalyst of Example 1 shown in FIG. 12. DETAILED DESCRIPTION OF THE INVENTION

[0029] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings.

[0030] <Membrane-electrode assembly (MEA)> FIG. 1 is a schematic cross-sectional view showing a preferred embodiment of the MEA of the present invention. The MEA 10 shown in FIG. 1 has a configuration including two flat gas diffusion electrodes (cathode 1 and anode 2) arranged facing each other, and a polymer electrolyte membrane (hereinafter referred to as "PEM" as necessary) 3 arranged between the cathode 1 and the anode 2. In the case of this MEA 10, at least one of the cathode 1 and the anode 2 has a configuration in which a core-shell catalyst, which will be described later, is contained. The MEA 10 can be manufactured by stacking the cathode 1, anode 2, and PEM 3 as shown in FIG. 1, and then pressing them together.

[0031] <Gas diffusion electrode (GDE)> The cathode 1, which is a gas diffusion electrode, includes a gas diffusion layer 1gd and a catalyst layer 1c formed on the surface of the gas diffusion layer 1gd facing the PEM 3. The cathode 1 further includes a water-repellent layer (Micro Porous Layer, hereinafter referred to as "MPL" as necessary) 1m disposed between the gas diffusion layer 1gd and the catalyst layer 1c. Similar to the cathode 1, the anode 2, which is a gas diffusion electrode, has a configuration including a gas diffusion layer 2gd, a catalyst layer 2c formed on the PEM 3 side of the gas diffusion layer 2gd, and an MPL 2m disposed between the gas diffusion layer 2gd and the catalyst layer 2c.

[0032] (Catalyst layer (CL)) In the cathode 1, the catalyst layer 1c is a layer where a reaction proceeds between air (oxygen gas) sent from the gas diffusion layer 1gd and hydrogen ions moving through the PEM 3 from the anode 2 to produce water. In the anode 2, the catalyst layer 2c is a layer where a reaction proceeds to generate hydrogen ions and electrons from the hydrogen gas sent from the gas diffusion layer 2gd. At least one of the catalyst layer 1c of the cathode 1 and the catalyst layer 2c of the anode 2 contains a core-shell catalyst according to the electrode catalyst of the present invention.

[0033] (A preferred embodiment of the electrode catalyst of the present invention) A preferred embodiment of the electrode catalyst of the present invention will be described below with reference to FIG. Fig. 2 is a schematic cross-sectional view showing a preferred embodiment of an electrode catalyst (PtNi / C catalyst) contained in at least one of the cathode catalyst layer 1c and the anode catalyst layer 2c of the MEA 10 shown in Fig. 1. Fig. 3 is an enlarged schematic cross-sectional view showing the general configuration of the electrode catalyst 20 shown in Fig. 2. As shown in FIGS. 2 and 3, the electrode catalyst 20 includes a support 22 which is a hollow carbon support, and catalyst particles 23 which are supported on the support 22 and contain a PtNi alloy.

[0034] Moreover, the electrode catalyst 20 shown in FIGS. 2 and 3 preferably satisfies the following conditions in order to more reliably obtain the effects of the present invention. Here, the catalyst particles 23 contain a PtNi alloy, and are preferably made of a PtNi alloy, although a Pt oxide layer or a Ni oxide layer may be formed on the surface of the catalyst particles as long as the effects of the present invention can be obtained. The electrode catalyst 20 preferably has an average crystallite size of 3 to 16.0 nm as measured by powder X-ray diffraction (XRD). The electrode catalyst 20 preferably has a Pt loading rate of 10.0 to 40.0 wt %, and a Ni loading rate of 1.0 to 25.0 wt %.

[0035] The support 22 is not particularly limited as long as it is a hollow carbon support having mesopores (mesopores as defined by IUPAC) with a pore diameter of 2 to 50 nm, capable of supporting a composite consisting of a core portion 24 and a shell portion 26 (or shell portion 26a), and having a relatively large surface area. Furthermore, the support 22 is preferably a hollow carbon support that has good dispersibility in the composition for forming a gas diffusion electrode containing the core-shell catalyst 20 (or 20A) and has excellent electrical conductivity.

[0036] Examples of hollow carbon supports include Ketjenblack EC300J and Ketjenblack EC600JD. Commercially available products include those under the trade names "Carbon EPC" and "Carbon EPC600JD" (manufactured by Lion Chemical Corporation, etc.). Detailed characteristics of Ketjenblack EC300J and Ketjenblack EC600JD are described, for example, in a document published online by the Functional Carbon Filler Research Group entitled "Characteristics and Applications of the Conductive Carbon Black 'Ketjenblack EC'."

[0037] Other examples of hollow carbon supports include those under the trade name "MCND (Mesoporous Carbon Nano-Dendrite)" (manufactured by Nippon Steel & Sumikin Chemical Co., Ltd.), the trade name "CNovel" (manufactured by Toyo Tanso Co., Ltd.), and the trade name "Black pearls 2000" (manufactured by Cabot Corporation). Here, from the viewpoint of more reliably obtaining the effects of the present invention, the hollow carbon support is preferably one of Ketjenblack EC300J, Ketjenblack EC600JD, and CNovel. In the case of Ketjenblack EC300J, from the same viewpoint, the BET specific surface area (nitrogen adsorption specific surface area) of the hollow carbon support measured using nitrogen is 750 to 850 m 2 In the case of CNovel, from the same viewpoint, the BET specific surface area (nitrogen adsorption specific surface area) of the hollow carbon support measured using nitrogen is preferably 750 to 1300 m 2 / g is preferred.

[0038] As shown in FIG. 2, the catalyst particles 23 are supported both inside the mesopores P22 of the support 22 and outside the mesopores P22. The electrode catalyst 20 simultaneously satisfies the conditions of the following formulas (1) and (2) when measured by electron beam tomography using a 3D-STEM: Catalyst for electrodes. D1 <D2···(1) (N1 / N2)>1.0 (2)

[0039] Here, in formulas (1) and (2), D1 represents the equivalent sphere diameter (nm) of the particles that exhibit the highest frequency among the catalyst particles 23 (or 23a) supported inside the mesopores P22 of the support 22. In addition, in formulas (1) and (2), D2 represents the equivalent particle diameter of the catalyst particles 23 (or 23a) that are supported outside the mesopores P22 of the support 22 and that exhibit the greatest frequency. Furthermore, in formulas (1) and (2), N1 represents the frequency (number of particles) of the particles showing the maximum frequency among the catalyst particles 23 (or 23a) supported inside the mesopores P22 of the support 22. In addition, in formulas (1) and (2), N2 represents the frequency (number of particles) of the particles showing the maximum frequency among the catalyst particles 23 (or 23a) supported outside the mesopores P22 of the support 22.

[0040] Compared to conventional electrode catalysts, an electrode catalyst 20 that simultaneously satisfies the conditions of formula (1) and formula (2) has a large number of highly active catalyst particles 23 with relatively small particle diameters present inside the mesopores P22 of the support 22. Such catalyst particles 23 (or 23a) with a core-shell structure supported inside the mesopores P22 of the support 22 exhibit superior catalytic activity when formed into an electrode compared to conventional electrode catalysts. In addition, the catalyst particles are supported on the support 22 in a state that makes them less likely to come into direct contact with the polymer electrolyte, such as Nafion, contained in the catalyst, thereby reducing dissolution of the Pt and Ni components.

[0041] The method for producing the electrode catalyst 20 is not particularly limited, and the electrode catalyst 20 can be produced by a known method, except that it includes a "Pt salt solution preparation step," a "carrier addition step," a "Ni salt solution dropping step," a "washing step," a "drying step," and a "reduction step" to satisfy the conditions of formula (1) and formula (2).

[0042] In the "Pt salt solution preparation step," an aqueous solution of water-soluble Pt salt dissolved in ultrapure water is prepared at room temperature. The "ultrapure water" used to prepare the aqueous solution in this Pt salt solution preparation step is water with a resistivity R (the reciprocal of electrical conductivity measured by the JIS standard test method (JIS K0552)) of 3.0 MΩ cm or higher, as expressed by the following formula (3). Furthermore, it is preferable that the "ultrapure water" has a water quality equivalent to or higher than "A3" as specified in JIS K0557 "Water used in testing water and wastewater."

[0043] There are no particular limitations on the ultrapure water, as long as it has an electrical conductivity that satisfies the relationship expressed by the following formula (3): For example, the ultrapure water can be produced using an ultrapure water production system such as the "Milli-Q Series" (manufactured by Merck Ltd.) or the "Elix UV Series" (manufactured by Nihon Millipore K.K.). R=1 / ρ (3) In the above formula (3), R represents the resistivity, and ρ represents the electrical conductivity measured according to the JIS standard test method (JIS K0552).

[0044] The next step after the "Pt salt solution preparation step" is the "carrier addition step." In this "carrier addition step," the carrier 22 is added to the Pt salt solution obtained through the "Pt salt solution preparation step" at room temperature. The dispersion in which the carrier is dispersed is then stirred and maintained at a temperature of 80 to 99°C, preferably 90 to 99°C, for a predetermined time (but without boiling), and then cooled to room temperature. Next, a pH adjuster is added to the obtained dispersion to prepare a dispersion with a pH adjusted to 9 to 13. Furthermore, this dispersion is stirred and maintained at a predetermined temperature of 40°C or higher for a predetermined time (but without boiling), and then cooled to room temperature. This removes gas from the mesopores P22 of the support 22, allowing the Pt salt aqueous solution to sufficiently penetrate into the mesopores P22. As a result, a large number of catalyst particle precursors are supported in the mesopores P22 of the support 22.

[0045] The next step after the "carrier addition step" is the "Ni salt solution dropping step." In the "Ni salt solution dropping step," an aqueous solution of water-soluble Ni salt dissolved in ultrapure water is added at room temperature to the dispersion obtained through the "carrier addition step." Next, a pH adjuster is added to the obtained dispersion to prepare a dispersion with a pH adjusted to 9 to 13. Furthermore, this dispersion is stirred while being maintained at a predetermined temperature of 40°C or higher for a predetermined time (however, it is maintained in a state where it does not boil). Thereafter, the dispersion is cooled to room temperature.

[0046] The next step after the "Ni salt solution dropping step" is the "washing step." In this "washing step," the solid components in the liquid obtained through the "Ni salt solution dropping step" are separated from the liquid components, and the solid components (a mixture of the PtNi / C catalyst precursor and other impurities) are washed. For example, the solid components in the liquid obtained through the "Ni salt solution dropping step" may be separated from the liquid components using a filtration method such as filter paper or filter cloth. The solid components may be washed using the above-mentioned ultrapure water, pure water (resistivity R expressed by the above-mentioned formula (3) is 0.1 MΩ·cm or more and less than 3.0 MΩ·cm), or pure hot water (pure water at a temperature of 40 to 80°C). For example, when pure hot water is used, washing is repeated until the electrical conductivity of the filtrate after washing is less than 20 μS / cm. The next step after the "washing step" is the "drying step." In this "drying step," water is separated from the solid component (a mixture of PtNi / C catalyst precursor and water) obtained after the "washing step." First, the solid component is air-dried, and then it is dried in a dryer at a specified temperature for a specified time. The process following the "drying process" is the "reduction process." In this "pulverization process," the solid component (the precursor of the PtNi / C catalyst) obtained in the "drying process" is reduced. The reduction treatment method uses a reduction furnace to reduce the solid component (the precursor of the PtNi / C catalyst) using hydrogen gas at a predetermined temperature of 800°C or higher.

[0047] The polymer electrolyte contained in catalyst layer 1c and catalyst layer 2c is not particularly limited as long as it has hydrogen ion conductivity, and known polymer electrolytes can be used. For example, known perfluorocarbon resins having sulfonic acid groups and carboxylic acid groups can be exemplified as polymer electrolytes. Preferred examples of readily available polymer electrolytes having hydrogen ion conductivity include Nafion (registered trademark, manufactured by DuPont), Aciplex (registered trademark, manufactured by Asahi Kasei Corporation), and Flemion (registered trademark, manufactured by Asahi Glass Co., Ltd.). In at least one of the catalyst layer 1c of the cathode 1 and the catalyst layer 2c of the anode 2 shown in FIG. 1, the mass ratio N / C of the mass C of the carrier 22 to the mass N of the polymer electrolyte is set to 0.5 to 1.2, and more preferably, the mass ratio N / C is set to 0.7 to 1.0.

[0048] (Gas Diffusion Layer (GDL)) 1, the gas diffusion layer 1gd is provided to supply an oxidant gas (e.g., oxygen gas or air) to the catalyst layer 1c, and also serves to support the catalyst layer 1c. The gas diffusion layer 2gd provided in the anode 2 is a layer provided to supply a reducing agent gas (for example, hydrogen gas) to the catalyst layer 2c and also serves to support the catalyst layer 2c.

[0049] The gas diffusion layer (1gd) shown in Fig. 1 has a function and structure that allows hydrogen gas or air (oxygen gas) to pass through smoothly and reach the catalyst layer. For this reason, the gas diffusion layer preferably has water repellency. For example, the gas diffusion layer contains a water repellent component such as polyethylene terephthalate (PTFE). The material that can be used for the gas diffusion layer (1gd) is not particularly limited, and known materials can be used. For example, preferred examples include carbon paper and carbon paper that is the main raw material and is coated with a secondary raw material that includes optional components such as carbon powder, ion-exchanged water, and polyethylene terephthalate dispersion as a binder.

[0050] (Water-repellent layer (MPL)) As shown in Fig. 1, the cathode 1 has a water-repellent layer (MPL) 1m disposed between the gas diffusion layer 1gd and the catalyst layer 1c. The water-repellent layer 1m has electronic conductivity, water repellency, and gas diffusivity, and is provided to promote the diffusion of oxidant gas into the catalyst layer 1gd and the discharge of reaction product water generated in the catalyst layer 1gd. The configuration of the water-repellent layer 1m is not particularly limited, and any known configuration can be adopted.

[0051] (Polymer electrolyte membrane (PEM)) The polymer electrolyte membrane (PEM) 3 shown in FIG. 1 is not particularly limited as long as it has hydrogen ion conductivity, and a known one conventionally used in a PEFC can be adopted. For example, a membrane containing, as a constituent, those exemplified as the polymer electrolyte contained in the catalyst layer 1c and the catalyst layer 2c described above may be used.

[0052] <Modified forms of MEA> As described above, the preferred embodiments of the MEA of the present invention (and the catalyst layer of the present invention, the gas diffusion electrode of the present invention) have been described. However, the MEA of the present invention is not limited to the configuration of the MEA10 shown in FIG. 1. For example, the MEA of the present invention may have the configuration of the MEA11 shown in FIG. 4. FIG. 4 is a schematic cross-sectional view showing another preferred form of the MEA of the present invention. The MEA11 shown in FIG. 4 has a configuration in which a gas diffusion electrode (GDE) 1A having the same configuration as the cathode 1 in the MEA10 shown in FIG. 1 is disposed only on one side of the polymer electrolyte membrane (PEM) 3. However, the catalyst layer 1c of the gas diffusion electrode (GDE) 1A has the configuration of the catalyst layer of the present invention. That is, in the catalyst layer 1c of the GDE1A, the mass ratio N / C of the mass C of the carrier of the electrode catalyst and the mass N of the polymer electrolyte is 0.5 to 1.2, more preferably 0.7 to 1.0.

[0053] <Membrane electrode assembly (CCM)> Next, the preferred embodiments of the membrane electrode assembly (CCM) of the present invention will be described. FIG. 5 is a schematic cross-sectional view showing a preferred form of the CCM of the present invention. The CCM12 shown in FIG. 5 has a configuration in which a polymer electrolyte membrane (PEM) 3 is disposed between a cathode catalyst layer 1c and an anode catalyst layer 2c. And at least one of the cathode catalyst layer 1c and the anode catalyst layer 2c has the configuration of the catalyst layer of the present invention. That is, in at least one of the cathode catalyst layer 1c and the anode catalyst layer 2c, the mass ratio N / C of the mass C of the carrier of the electrode catalyst and the mass N of the polymer electrolyte is 0.5 to 1.2, more preferably 0.7 to 1.0.

[0054] <Modified forms of membrane electrode assembly (CCM)> Although a preferred embodiment of the CCM of the present invention has been described above, the CCM of the present invention is not limited to the configuration of the CCM 12 shown in FIG. For example, the CCM of the present invention may have the configuration of the CCM 13 shown in FIG. Fig. 7 is a schematic cross-sectional view showing another preferred embodiment of the CCM of the present invention. The CCM 13 shown in Fig. 6 has a configuration in which a catalyst layer 1c having a configuration similar to that of the cathode 1 in the CCM 12 shown in Fig. 5 is disposed on only one side of a polymer electrolyte membrane (PEM) 3. However, the catalyst layer 1c of the gas diffusion electrode (GDE) 1A has the configuration of the catalyst layer of the present invention. That is, the catalyst layer 1c of the CCM 13 has a mass ratio N / C of the mass C of the electrode catalyst support to the mass N of the polymer electrolyte of 0.5 to 1.2, more preferably 0.7 to 1.0.

[0055] <Gas diffusion electrode (GDE)> Next, a preferred embodiment of the gas diffusion electrode (GDE) of the present invention will be described. Fig. 8 is a schematic cross-sectional view showing a preferred embodiment of a GDE of the present invention. The gas diffusion electrode (GDE) 1B shown in Fig. 7 has a configuration similar to that of the cathode 1 mounted on the MEA 10 shown in Fig. 1. However, the catalyst layer 1c of the gas diffusion electrode (GDE) 1B has the configuration of the catalyst layer of the present invention. That is, the catalyst layer 1c of the gas diffusion electrode (GDE) 1B has a mass ratio N / C of the mass C of the electrode catalyst support to the mass N of the polymer electrolyte of 0.5 to 1.2, more preferably 0.7 to 1.0.

[0056] <Modification of Gas Diffusion Electrode (GDE)> Although the preferred embodiment of the GDE of the present invention has been described above, the GDE of the present invention is not limited to the configuration of the GDE 1B shown in FIG. For example, the GDE of the present invention may have the configuration of a GDE1C shown in FIG. Fig. 9 is a schematic cross-sectional view showing another preferred embodiment of the GDE of the present invention. Compared to GDE 1B shown in Fig. 8, GDE 1C shown in Fig. 8 does not have a water-repellent layer (MPL) between the catalyst layer 1c and the gas diffusion layer 1gd.

[0057] <Composition for forming catalyst layer> Next, a preferred embodiment of the catalyst layer-forming composition of the present invention will be described. The composition for forming a catalyst layer of the present embodiment contains an electrode catalyst, a polymer electrolyte, and a main component, and the mass ratio N / C of the mass C of the electrode catalyst support to the mass N of the polymer electrolyte is 0.5 to 1.2, and more preferably 0.7 to 1.0. The composition of the polymer electrolyte-containing liquid is not particularly limited. For example, the polymer electrolyte-containing liquid may contain the above-mentioned polymer electrolyte having hydrogen ion conductivity, water, and alcohol.

[0058] The electrode catalyst, polymer electrolyte, and other components (water, aluminum) contained in the catalyst layer-forming composition The composition ratio of the catalyst (e.g., alcohol) is such that the electrode catalyst is well dispersed in the resulting catalyst layer. and is appropriately set so as to improve the power generation performance of the MEA including the catalyst layer. The catalyst layer-forming composition can be prepared by mixing and stirring a liquid containing an electrode catalyst and a polymer electrolyte. To adjust the coatability, the composition may contain a polyhydric alcohol such as glycerin and / or water. When mixing the liquid containing the electrode catalyst and the polymer electrolyte, a grinding mixer such as a ball mill or ultrasonic disperser may be used. At least one of the catalyst layer 1c of the cathode 1 and the catalyst layer 2c of the anode 2 shown in FIG. 1 can be formed using a preferred embodiment of the composition for forming a catalyst layer of the present invention.

[0059] (Method of manufacturing gas diffusion electrode) Next, an example of a method for manufacturing the gas diffusion electrode of the present invention will be described. The gas diffusion electrode may be formed so as to include the catalyst layer of the present invention, and a known method can be used for the manufacturing method. The use of the composition for forming a catalyst layer of the present invention allows for more reliable manufacturing. For example, the catalyst layer may be produced by applying the catalyst layer-forming composition onto the gas diffusion layer (or onto the water-repellent layer of a laminate in which a water-repellent layer is formed on a gas diffusion layer), followed by drying.

[0060] <Fuel cell stack> FIG. 9 is a schematic diagram showing a preferred embodiment of a fuel cell stack of the present invention. The fuel cell stack 30 shown in Fig. 9 has a configuration in which a plurality of unit cells, each of which is the MEA 10 shown in Fig. 1, are stacked one on top of the other. The fuel cell stack 30 has a configuration in which the MEA 10 is disposed between a separator 4 and a separator 5. The separator 4 and the separator 5 each have a gas flow path formed therein. [Example]

[0061] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples. It is not something that is done.

[0062] (I) Preparation of electrode catalyst for use in the cathode catalyst layer of the MEA

[0063] (1) Preparation of PtNi / C catalyst used in the cathode of the MEA of Example 1 [PtNi alloy particle supported carbon catalyst "PtNi / C catalyst" powder] A PtNi / C catalyst powder (Pt loading rate 28.0 wt%, Ni loading rate 8.0 wt%, product name "SA30ABKN8", manufactured by NECHEMCAT) in which catalyst particles containing a PtNi alloy were supported on carbon black powder was prepared. This PtNi / C catalyst powder was prepared by the following procedure.

[0064] (Step 1 (Pt salt solution preparation step)) An aqueous solution of water-soluble Pt salt was prepared by dissolving it in ultrapure water at room temperature. The "ultrapure water" used in this first step (Pt salt solution preparation step) had a resistivity R (the reciprocal of electrical conductivity measured by the JIS standard test method (JIS K0552)) of 3.0 MΩ cm or higher, as expressed by the following formula (3). This "ultrapure water" also had a water quality equivalent to or better than "A3" as specified in JIS K0557, "Water used in testing water and wastewater." This ultrapure water was produced using ultrapure water production equipment "Milli-Q Series" (manufactured by Merck Ltd.) and "Elix UV Series" (manufactured by Nihon Millipore Co., Ltd.). R=1 / ρ (3) In the above general formula (3), R represents the resistivity, and ρ represents the electrical conductivity measured according to the JIS standard test method (JIS K0552).

[0065] (Second step (carrier addition step)) The carrier 22 was added at room temperature to the Pt salt solution obtained through the "Pt salt solution preparation step." The carrier 22 was a commercially available hollow carbon carrier (manufactured by Lion Corporation, trade name "Carbon ECP" (registered trademark) (Ketjen Black EC300J), specific surface area 750 to 800 m) 2 / g} was used. The dispersion liquid with the carrier dispersed therein was stirred while being maintained at a temperature of 80 to 99°C, preferably 90 to 99°C, for a predetermined time (but without boiling), and then cooled to room temperature. Next, a pH adjuster was added to the obtained dispersion liquid to prepare a dispersion liquid with a pH adjusted to 9 to 13. Furthermore, this dispersion liquid was stirred while being maintained at a predetermined temperature of 40°C or higher for a predetermined time (but without boiling), and then the dispersion liquid was cooled to room temperature.

[0066] (Third step (Ni salt solution dropping step)) To the dispersion obtained through the second step (carrier addition step), an aqueous solution of water-soluble Ni salt dissolved in ultrapure water was added at room temperature. Next, a pH adjuster was added to the obtained dispersion to prepare a dispersion with a pH adjusted to 9 to 13. Furthermore, this dispersion was stirred while being kept at a predetermined temperature of 40°C or higher for a predetermined time (however, it was kept in a state where it was not boiled). Thereafter, the dispersion was cooled to room temperature.

[0067] (Fourth step (cleaning step)) The solid and liquid components in the liquid obtained through the third step (Ni salt solution dropping step) were separated, and the solid component (a mixture of the PtNi / C catalyst precursor and other impurities) was washed. Filter paper was used to separate the solid component from the liquid component obtained through the "Ni salt solution dropping step." The solid component was washed using the above-mentioned ultrapure water, pure water (resistivity R, expressed by the above-mentioned formula (3), is 0.1 MΩ·cm or more and less than 3.0 MΩ·cm), and pure hot water (pure water at a temperature of 40 to 80°C). Washing using pure hot water was repeated until the electrical conductivity of the filtrate after washing was less than 20 μS / cm.

[0068] (5th process (drying process)) Next, the solid component on the filter paper (a mixture of PtNi / C catalyst precursor and water) was air-dried in this state. After air-drying, the solid component on the filter paper was transferred to a porcelain dish and dried in an electric dryer at a predetermined temperature of 60°C or higher for a predetermined time. The dried solid component was then pulverized using a mixer to obtain a powder of PtNi / C catalyst precursor.

[0069] (Sixth Step (Reduction Step)) The solid component (precursor of PtNi / C catalyst) obtained from the "drying step" was subjected to reduction treatment. The solid component (precursor of the PtNi / C catalyst) was placed in a baking dish and placed in a reduction furnace. Next, nitrogen gas was passed through the reduction furnace at a specified flow rate to purge any remaining oxygen. Next, hydrogen gas was introduced into the reduction furnace and reduction treatment was carried out at a specified temperature of 800°C or higher for a specified time. After that, the temperature inside the reduction furnace was lowered and the solid component after reduction treatment was subjected to a gradual oxidation treatment. This yielded a PtNi / C catalyst.

[0070] <Measurement of loading rate (ICP analysis)> For this core-shell catalyst A, the Pt loading rate (wt%) and the Ni loading rate (wt%) were measured by the following methods. The PtNi / C catalyst was immersed in aqua regia to dissolve the metal. Next, the insoluble carbon was removed from the aqua regia. The carbon-free aqua regia was then subjected to ICP analysis. As a result of ICP analysis, the PtNi / C catalyst had a Pt loading rate of 28.0 wt% and a Ni loading rate of 8.0 wt%.

[0071] <Surface and structural observation of electrode catalysts> To observe the three-dimensional structure of this PtNi / C catalyst, electron warfare tomography measurements using STEM were carried out under the following conditions. ·STEM equipment: JEOL JEM-ARM200F atomic resolution analytical electron microscope Data analysis software: System In Frontier's 3D reconstruction software Composer, 3D data visualization software Visualizer-kai, and image analysis software Colorist Measurement conditions Accelerating voltage: 60 kV Magnification: 800,000 to 1,000,000 times Measurement sample tilt angle: -80° to +80° Tilt step angle of measurement sample: 2° Number of pixels: 512 × 512 pixels 512 × 512 pixels Pixel size: 0.350 nm / pixel ~ 0.500 nm / pixel Volume size: shown in Figure 11.

[0072] For the PtNi / C catalyst, three-dimensional reconstructed images (3D-STEM images) obtained by electron tomography measurement using a STEM (scanning transmission electron microscope) were analyzed to separate the PtNi / C catalyst particles present inside the carbon support (hereinafter referred to as internal particles) and the PtNi / C catalyst particles present on the surface of the carbon support (hereinafter referred to as external particles), and the particle size distribution of the PtNi / C catalyst particles in each region was calculated. A three-dimensional reconstruction image (3D-STEM image) of core-shell catalyst A is shown in Figure 12. The particle size analysis results of the internal and external particles obtained by image analysis are shown in Figs. 13 and 14. The 3D-STEM image was obtained by reconstructing multiple 2D STEM images obtained by tilting the sample stage stepwise under the above measurement conditions.

[0073] Image analysis (particle size analysis) of the three-dimensional reconstructed image (3D-STEM image) was performed as follows. First, the catalyst particle region was selected from the three-dimensional reconstructed image, and each catalyst particle was labeled (not shown). Next, the sphere-equivalent diameter was calculated from the volume of the labeled Pt particles, and the particle size distribution (Figures 13 and 14) was obtained. Here, the sphere-equivalent diameter was calculated in units of nm, with decimal values ​​(values ​​less than 1 nm) rounded off. For the PtNi / C catalyst, the ratio of catalyst particles supported inside the mesopores of the support and the ratio of catalyst particles supported outside the mesopores of the support were determined. The values ​​of D1, D2, N1, and N2 were also determined. The results are shown in Tables 1 and 2. Furthermore, the average particle size of the PtNi / C catalyst measured from the STEM image was 5.5 nm.

[0074] (2) Preparation of Pt / C catalyst powder for use in the cathode of the MEA of Comparative Example 1 A Pt / C catalyst with a Pt loading rate of 50 wt% manufactured by NECHEMCAT (product name: "SA50BK") was prepared as the Pt / C catalyst. The support for this Pt / C catalyst was a commercially available hollow carbon support (manufactured by Lion Corporation, product name "Carbon ECP" (registered trademark) (Ketjenblack EC300J), specific surface area 750 to 800 m). 2 / g} was used. XRD analysis of this Pt / C catalyst revealed that the average crystallite size was 2.6 nm.

[0075] (II) Preparation of P / C catalyst used in the anode of MEAs in Example 1 and Comparative Example 1 The same Pt / C catalyst as Pt / C catalyst B used in the cathode of the MEA of Comparative Example 1 was used as the Pt / C catalyst for the anode of the MEA of Example 1 and Comparative Example 1.

[0076] Example 1 An MEA having a configuration similar to that of the MEA 10 shown in FIG. 1 was fabricated by the following procedure.

[0077] (1) Creating the cathode Cathode GDL Carbon paper (manufactured by Toray Industries, Inc., product name "TGP-H-60") was prepared as the GDL. Ink for forming cathode MPL 1.5 g of carbon powder (trade name "Denka Black" manufactured by Denki Kagaku Kogyo Kabushiki Kaisha), 1.1 g of ion-exchanged water, and 6.0 g of surfactant (trade name "Triton" (35 wt % aqueous solution) manufactured by Dow Chemical Company) were placed in a Teflon (registered trademark) ball mill container containing Teflon (registered trademark) balls and mixed. Next, 1.75 g of polytetrafluoroethylene (PTFE) dispersion (manufactured by DuPont-Mitsui Fluorochemicals, product name "31-JR") was added to the ball mill container and mixed, thereby producing an ink for forming the MPL of the cathode. Cathode MPL The cathode MPL ink was applied to one side of the GDL using a bar coder to form a coating film, which was then thoroughly dried in a dryer and further subjected to a heat-pressing process to form a laminate with the MPL formed on the GDL. Ink for forming the cathode catalyst layer The above-mentioned PtNi / C catalyst, ion-exchanged water, 10 wt% Nafion aqueous dispersion (manufactured by DuPont under the trade name "DE1021CS"), and glycerin were mixed in a Teflon ball mill container containing Teflon balls to prepare an ink for forming a cathode catalyst layer. The N / C ratio for this ink was 0.7. The ratio of carbon:ion-exchanged water:glycerin in the core-shell catalyst A was 1:10:0.8 (mass ratio). Cathode catalyst layer (CL) The ink for forming the cathode catalyst layer was applied to the surface of the MPL of the laminate formed by the MPL on the GDL by bar coating to form a coating film. This coating film was dried at room temperature for 30 minutes, and then dried at 60 ° C for 1.0 hour to form a catalyst layer. In this way, a cathode, which is a gas diffusion electrode, was prepared. The Pt loading of the cathode catalyst layer was adjusted to the values ​​shown in Table 1.

[0078] (2) Creating the anode Anode GDL The GDL was the same carbon paper as the cathode. Ink for forming anode MPL 1.5 g of carbon powder (trade name "Denka Black" manufactured by Denki Kagaku Kogyo Kabushiki Kaisha), 1.0 g of ion-exchanged water, and 6.0 g of surfactant (trade name "Triton" (35 wt % aqueous solution) manufactured by Dow Chemical Company) were placed in a Teflon (registered trademark) ball mill container containing Teflon (registered trademark) balls and mixed. Next, 2.5 g of polytetrafluoroethylene (PTFE) dispersion (manufactured by DuPont-Mitsui Fluorochemicals, product name "31-JR") was added to the ball mill container and mixed, thereby preparing an ink for forming the MPL for the anode. Anode MPL The ink for forming the anode MPL was applied to one side of the GDL using a bar coder to form a coating film. The coating film was then thoroughly dried in a dryer and further subjected to a heat-pressing process to create a laminate with the MPL formed on the GDL. Ink for forming the anode catalyst layer SA50BK (Pt loading: 50 wt%), ion-exchanged water, a 5 wt% Nafion alcohol dispersion (manufactured by SIGMA-ALDRICH under the trade name "Nafion 5 wt.% dispersion", product number "274704"), and glycerin were mixed in a Teflon ball mill container containing Teflon balls to prepare an ink for forming the anode catalyst layer. The N / C ratio for this ink was 1.2. The mass ratio of carbon in the SA50BK to ion-exchanged water to glycerin was 1:6:4. Anode catalyst layer (CL) The ink for forming the anode catalyst layer was applied to the surface of the MPL of the laminate formed by the above-mentioned GDL and MPL by bar coating to form a coating film. This coating film was dried at room temperature for 30 minutes, and then dried at 60°C for 1.0 hour to form a catalyst layer. In this way, an anode, which is a gas diffusion electrode, was produced. The Pt loading in the anode catalyst layer was 0.3 mg / cm. 2 It was decided.

[0079] (3) Creation of MEA A polymer electrolyte membrane (trade name "Nafion NR212" manufactured by DuPont) was prepared. This polymer electrolyte membrane was placed between a cathode and an anode to form a laminate, which was then thermocompressed using a hot press to form an MEA. The thermocompression conditions were 140°C, 5 KN for 5 minutes, and then 140°C, 25 KN for 3 minutes.

[0080] <Comparative Example 1> Each MEA was prepared under the same conditions and procedures as in Example 1, except that the conditions for the cathode catalyst layer were changed as follows. That is, in the preparation of the ink for forming the cathode catalyst layer, Instead of the PtNi / C catalyst, the P / C catalyst (product name: "SA-50BK") mentioned above was used. was used. Instead of the 10 wt% Nafion aqueous dispersion, a 5 wt% Nafion alcohol dispersion (manufactured by DuPont under the trade name "DE520CS"; containing 48 wt% 1-propanol) was used. The composition of the ink for forming the cathode catalyst layer and the coating conditions for the ink were adjusted so that the Pt loading and N / C would be the values ​​shown in Table 1. The mass ratio of carbon:ion-exchanged water:glycerin in the P / C catalyst (product name: "SA50BH") was 1:10:1.

[0081] <Battery performance evaluation> The cell performance of the MEAs of Example 1 and Comparative Example 1 was evaluated by the following cell performance evaluation method. The MEAs of Example 1 and Comparative Example 1 were placed in a single fuel cell evaluation device. Next, the power generation reaction was allowed to proceed within the MEA under the following conditions. The single cell (MEA) temperature was set to 80°C. Pure hydrogen at 1.0 atmospheres, humidified with saturated steam, was supplied to the anode with the flow rate adjusted to achieve a utilization rate of 70%. Pure oxygen at 1.0 atmospheres, humidified with saturated steam at 80°C, was supplied to the cathode with the flow rate adjusted to achieve a utilization rate of 50%. The evaluation of the single cell (MEA) was carried out by controlling the current using an electronic load device attached to the fuel cell single cell evaluation device, with the current value being 0 to 1.0 A / cm 2 The current-voltage curve obtained by scanning up to 1000 kJ / s was obtained as data. A graph (not shown) was created by plotting the data from the current-voltage curve with the X axis (current density) on a logarithmic scale, and the current density value (current value per unit area of ​​the electrode) at a voltage of 850 mV was obtained.

[0082] The current density value thus obtained was divided by the platinum weight per unit area of ​​the cathode to calculate the activity per unit weight (Mass Act.) of the platinum contained in the cathode, which was used as an index of the oxygen reduction ability of the catalyst contained in the cathode. The results are shown in Table 1. Table 1 shows the results of comparing the Mass. Act. values ​​obtained in other Examples and Comparative Examples as relative values ​​(relative ratios) with the Mass. Act. value obtained in Comparative Example 1 set as the standard (1.0). [Table 1] [Table 2]

[0083] The results shown in Table 1 reveal that the MEA of Example 1 has higher Pt mass activity than the MEA of Comparative Example 1. [Industrial Applicability]

[0084] The electrode catalyst of the present invention exhibits excellent catalytic activity, and the GDE, CCM, MEA, and fuel cell stack that include the catalyst layer of the present invention exhibit excellent cell characteristics that can contribute to cost reduction of PEFCs. Therefore, the present invention can be applied not only to the electrical equipment industry such as fuel cells, fuel cell vehicles, and portable mobile devices, but also to ENE-FARM, cogeneration systems, etc., and contributes to the development of the energy industry and environmental technology. [Explanation of symbols]

[0085] 1···cathode, 1A, 1B, 1C... Gas diffusion electrode (GDE) 1c...Catalyst layer (CL), 1m...Water-repellent layer (MPL), 1gd···Gas diffusion layer (GDL), 2 anode, 2c...Catalyst layer (CL), 2m...Water-repellent layer (MPL), 2gd···Gas diffusion layer (GDL), 3...polymer electrolyte membrane (PEM), 4, 5...Separator 10, 11... Membrane-electrode assembly (MEA), 12, 13... Membrane / catalyst layer assembly (CCM) 20...PtNi / C catalyst, 22... Carrier, 23···Catalytic particles, 30. Fuel cell stack, P22···Mesopores of the support

Claims

1. A catalyst for an electrode comprising: a hollow carbon support having mesopores with a pore size of 2 to 50 nm; and a plurality of PtNi alloy catalyst particles supported on the support, the catalyst particles are supported both inside the mesopores and outside the mesopores of the support, when a particle size distribution analysis is carried out based on a sphere-equivalent diameter calculated from the volume of the catalyst particles using a three-dimensional reconstructed image obtained by electron beam tomography measurement using a STEM (scanning transmission electron microscope), the ratio of the catalyst particles supported inside the mesopores is 50% or more, At least a portion of the surface of the catalyst particle is covered with a Ni oxide coating. Catalyst for electrodes.

2. When a particle size distribution analysis is carried out based on a sphere-equivalent diameter calculated from the volume of the catalyst particles using a three-dimensional reconstructed image obtained by electron beam tomography measurement using a STEM (scanning transmission electron microscope), the ratio of the catalyst particles supported inside the mesopores is 60% or more. The electrode catalyst according to claim 1 .

3. 3. The electrode catalyst according to claim 1 or 2, which simultaneously satisfies the conditions of the following formulas (1) and (2) when an analysis of a particle size distribution of the catalyst particles is carried out using a three-dimensional reconstructed image obtained by electron beam tomography measurement using a STEM (scanning transmission electron microscope). D1<D2...(1) (N1 / N2)>1.0...(2) [In the formula (1) and the formula (2), D1 represents the sphere-equivalent diameter of the particle exhibiting the highest frequency among the catalyst particles supported inside the mesopores of the support, D2 represents the particle equivalent sphere diameter exhibiting the maximum frequency among the catalyst particles supported outside the mesopores of the support, N1 represents the frequency of the particles having the maximum frequency among the catalyst particles supported inside the mesopores of the support, N2 represents the frequency of the particles having the maximum frequency among the catalyst particles supported outside the mesopores of the support.

4. At least a portion of the surface of the catalyst particle is covered with a Pt oxide coating. The electrode catalyst according to any one of claims 1 to 3.

5. Further, a second catalyst particle made of Pt (zero valence) is included. The electrode catalyst according to any one of claims 1 to 4.

6. Further, a third catalyst particle made of Ni (zero valence) is included. The electrode catalyst according to any one of claims 1 to 4.

7. The hollow carbon support has a BET specific surface area (nitrogen adsorption specific surface area) of 750 to 850 m 2 / g, The electrode catalyst according to claim 1 .

8. The electrode catalyst according to any one of claims 1 to 7 is contained in an amount of 10 wt % or more. Electrode catalyst powder.

9. The electrode catalyst according to any one of claims 1 to 7 is contained. A composition for forming a gas diffusion electrode.

10. A gas diffusion electrode comprising the electrode catalyst according to any one of claims 1 to 7.

11. A membrane electrode assembly (MEA) comprising the gas diffusion electrode of claim 10.

12. A fuel cell stack comprising the membrane electrode assembly (MEA) of claim 11.

13. A catalyst for an electrode comprising: a hollow carbon support having mesopores with a pore size of 2 to 50 nm; and a plurality of PtNi alloy catalyst particles supported on the support, the catalyst particles are supported both inside the mesopores and outside the mesopores of the support, when a particle size distribution analysis is carried out based on a sphere-equivalent diameter calculated from the volume of the catalyst particles using a three-dimensional reconstructed image obtained by electron beam tomography measurement using a STEM (scanning transmission electron microscope), the ratio of the catalyst particles supported inside the mesopores is 50% or more, Further, a second catalyst particle made of Pt (zero valence) is included. Catalyst for electrodes.

Citation Information

Patent Citations

  • Carried catalyst for electrode and its manufacturing method, electrode for proton exchange membrane fuel cell and proton exchange membrane fuel cell

    JP2006253145A

  • Alloy catalyst for oxidation-reduction reaction

    JP2011016125A

  • Electrode catalyst layer for fuel cell

    JP2013109856A

  • Oxygen reduction catalyst

    JP2020021610A

  • Catalyst for fuel cell and method of manufacturing the same, and membrane-electrode assmbly and method of manufacturing the same

    KR1020190009584A