Composition and method for cleaning adhesive polymers

A composition of quaternary alkylammonium fluoride, N-substituted amide, and dipropylene glycol dimethyl ether addresses the challenge of achieving high etching rates on adhesive surfaces with varying polarities, enhancing cleaning efficiency and reducing costs.

JP7574798B2Active Publication Date: 2024-10-29RESONAC CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021542667
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-08-27
Filing Date
2020-07-30
Publication Date
2024-10-29
Estimated Expiration
2040-07-30

AI Technical Summary

Technical Problem

Existing cleaning agents struggle to achieve high etching rates on adhesive surfaces with varying polarities, particularly those containing polyorganosiloxane compounds, due to insufficient affinity and reactivity.

Method used

A composition comprising quaternary alkylammonium fluoride, an N-substituted amide compound, and dipropylene glycol dimethyl ether, with specific isomer proportions, enhances affinity and etching rates by utilizing the reaction activity of fluoride ions.

Benefits of technology

The composition achieves high etching rates with a low fluorine compound concentration, improving performance and reducing costs while effectively decomposing adhesive polymers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007574798000017
    Figure 0007574798000017
  • Figure 0007574798000018
    Figure 0007574798000018
  • Figure 0007574798000019
    Figure 0007574798000019
Patent Text Reader

Abstract

Provided is a composition which has an excellent affinity with the surface of an adhesive agent and can achieve a high etching rate. The composition according to one embodiment comprises: a quaternary alkylammonium fluoride or a hydrate of a quaternary alkylammonium fluoride; and, as an aprotic solvent, (A) an N-substituted amide compound having no active hydrogen on a nitrogen atom, and (B) a dipropylene glycol dimethyl ether, wherein (B) the dipropylene glycol dimethyl ether has the percentage of a structural isomer represented by formula (1) of at least 50 mass% with respect to the total amount of (B) the dipropylene glycol dimethyl ether.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a composition and a method for cleaning an adhesive polymer, and in particular to a composition that can be used for decomposing and cleaning an adhesive that contains an adhesive polymer used for temporarily bonding a device wafer to a support wafer (carrier wafer) and that remains on the device wafer during a semiconductor wafer thinning process, and a method for cleaning an adhesive polymer using the composition. [Background technology]

[0002] In three-dimensional packaging technology for increasing the density of semiconductors, the thickness of each semiconductor wafer is reduced, and multiple semiconductor wafers connected by through-silicon vias (TSVs) are stacked. Specifically, the surface (backside) of a device wafer on which semiconductor devices are formed is polished to make it thinner, and then electrodes including TSVs are formed on the backside.

[0003] In the polishing process of the back surface of the device wafer, a support wafer also called a carrier wafer is temporarily bonded to the semiconductor device forming surface of the device wafer using an adhesive in order to impart mechanical strength to the device wafer. For example, a glass wafer or a silicon wafer is used as the support wafer. After the polishing process, metal wiring or electrode pads containing Al, Cu, Ni, Au, etc., inorganic films such as oxide films and nitride films, or resin layers containing polyimide, etc. are formed on the polished surface (back surface) of the device wafer as necessary. Thereafter, the back surface of the device wafer is bonded to a tape having an acrylic adhesive layer fixed by a ring frame, so that the device wafer is fixed to the tape. Thereafter, the device wafer is separated from the support wafer (debonding), the adhesive on the device wafer is peeled off, and the adhesive residue on the device wafer is washed away using a cleaning agent.

[0004] For the temporary bonding of device wafers, adhesives containing polyorganosiloxane compounds with good heat resistance as adhesive polymers are used. In particular, when the adhesive is a crosslinked polyorganosiloxane compound, the cleaning agent is required to have two functions: cleavage of Si-O bonds and dissolution of decomposition products by a solvent. Examples of such cleaning agents include those in which a fluorine-based compound such as tetrabutylammonium fluoride (TBAF) is dissolved in a polar aprotic solvent. The fluoride ions of TBAF are involved in cleavage of Si-O bonds via the formation of Si-F bonds, and therefore can impart etching performance to the cleaning agent. Polar aprotic solvents can dissolve TBAF and do not form solvations with fluoride ions via hydrogen bonds, and therefore can increase the reactivity of fluoride ions.

[0005] Patent Document 1 (JP 2014-133855 A) describes a cleaning liquid for siloxane resins in which tetraalkylammonium hydroxide is dissolved in a polar aprotic solvent.

[0006] Patent Document 2 (JP Patent Publication No. 2015-505886) describes a polysiloxane cleaning liquid in which TBAF is dissolved in an ester or ketone.

[0007] Patent Document 3 (JP 2004-000969 A) describes a cleaning liquid in which TBAF is dissolved in propylene glycol alkyl ether alcoholate. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2014-133855 A [Patent Document 2] Special Publication No. 2015-505886 [Patent Document 3] JP 2004-000969 A Summary of the Invention [Problem to be solved by the invention]

[0009] The role of the solvent in cleaning agents that contain fluorine compounds and solvents, such as TBAF, is thought to be to sufficiently dissolve the highly polar fluorine compounds, which are reactive substances, and to provide sufficient affinity with the surface of adhesives, which have low polarity, thereby ensuring the reactivity of the fluoride ions contained in the fluorine compounds and dissolving the decomposition products of the adhesive.

[0010] Substituents may be introduced into the adhesive polymer contained in the adhesive for the purpose of improving heat resistance, peelability, etc., and as a result, the surface of the adhesive may exhibit various polarities. It is desired that the cleaning agent exhibits excellent affinity for the adhesive surface exhibiting such various polarities, thereby achieving a high etching rate.

[0011] The present disclosure provides a composition that has excellent compatibility with adhesive surfaces and can achieve a high etching rate. [Means for solving the problem]

[0012] The present inventors have found that in a composition containing a quaternary alkylammonium fluoride or a hydrate thereof, an N-substituted amide compound having no active hydrogen on a nitrogen atom, and dipropylene glycol dimethyl ether, a high etching rate can be achieved by adjusting the ratio of a specific isomer in dipropylene glycol dimethyl ether.

[0013] That is, the present invention includes the following [1] to

[10] . [1] A composition comprising a quaternary alkylammonium fluoride or a hydrate of a quaternary alkylammonium fluoride, and (A) an N-substituted amide compound having no active hydrogen on a nitrogen atom as an aprotic solvent, and (B) dipropylene glycol dimethyl ether, wherein the (B) dipropylene glycol dimethyl ether is represented by the formula (1): [ka] The proportion of the structural isomer represented by the following formula (B) is 50 mass % or more based on the total amount of dipropylene glycol dimethyl ether. [2] The composition according to [1], wherein the proportion of the structural isomer represented by formula (1) is 60 mass% or more based on the total amount of the (B) dipropylene glycol dimethyl ether. [3] The (A) N-substituted amide compound has the formula (2): [ka] (In formula (2), R 1 represents an alkyl group having 1 to 4 carbon atoms. The composition according to either [1] or [2], wherein the 2-pyrrolidone derivative compound is represented by the following formula: [4] The (A) N-substituted amide compound is represented by the formula (2), 1 The composition according to [3], wherein the compound is a 2-pyrrolidone derivative in which [5] The composition according to any one of [1] to [4], wherein the content of the quaternary alkylammonium fluoride is 0.01 to 10 mass %. [6] The quaternary alkyl ammonium fluoride is R 2 R 3 R 4 R 5 N + F - R is a tetraalkylammonium fluoride represented by the formula 2 ~R 5 are each independently an alkyl group selected from the group consisting of a methyl group, an ethyl group, an n-propyl group, an isopropyl group, and an n-butyl group. [7] The composition according to any one of [1] to [6], wherein the content of the (A) N-substituted amide compound is 50 to 95 mass % and the content of the (B) dipropylene glycol dimethyl ether is 5 to 50 mass % relative to 100 mass % of the aprotic solvent. [8] The composition according to any one of [1] to [7], which is a composition for decomposing and cleaning an adhesive polymer. [9] The composition according to [8], wherein the adhesive polymer is a polyorganosiloxane compound.

[10] A method for cleaning an adhesive polymer on a substrate, using the composition according to any one of [1] to [9]. Effect of the Invention

[0014] The composition of the present disclosure has high affinity with the adhesive surface, and therefore, even when a relatively low concentration of a fluorine compound is used in the composition, a high etching rate can be obtained. This is advantageous for both high performance and low cost of the cleaning agent.

[0015] The above description should not be considered as a disclosure of all embodiments of the present invention and all advantages associated with the present invention. [Brief description of the drawings]

[0016] [Figure 1] 1 is a graph showing the change in film thickness (mm) versus cleaning time (minutes) for NMP:DPGDME=0.764:0.236 (mass ratio) in cleaning test 1. [Diagram 2] 1 is a graph showing the change in film thickness (mm) versus cleaning time (minutes) for NMP:DPGDME=0.764:0.236 (mass ratio) in cleaning test 2. [Diagram 3] 1 is a graph showing the change in film thickness (mm) versus cleaning time (min) for NMP:DPGDME=0.600:0.400 (mass ratio) in cleaning test 1. [Figure 4]1 is a graph showing the change in film thickness (mm) versus cleaning time (min) for NMP:DPGDME=0.600:0.400 (mass ratio) in cleaning test 2. [Diagram 5] 1 is a graph showing the change in film thickness (mm) versus cleaning time (min) for NMP:DPGDME=0.900:0.100 (mass ratio) in cleaning test 1. [Figure 6] 1 is a graph showing the change in film thickness (mm) versus cleaning time (min) for NMP:DPGDME=0.900:0.100 (mass ratio) in cleaning test 2. [Figure 7] 1 is a graph showing the change in film thickness (mm) versus cleaning time (minutes) for NEP:DPGDME=0.764:0.236 (mass ratio) in cleaning test 2. [Figure 8] 1 is a graph showing the change in film thickness (mm) versus cleaning time (min) for NEP:DPGDME=0.600:0.400 (mass ratio) in cleaning test 2. [Figure 9] 1 is a graph showing the change in film thickness (mm) versus cleaning time (min) for NEP:DPGDME=0.900:0.100 (mass ratio) in cleaning test 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The present invention will now be described in further detail.

[0018] [Composition] The composition of one embodiment contains a quaternary alkylammonium fluoride or a hydrate of a quaternary alkylammonium fluoride, and, as an aprotic solvent, (A) an N-substituted amide compound having no active hydrogen on a nitrogen atom, and (B) dipropylene glycol dimethyl ether (DPGDME).

[0019] <Quaternary alkyl ammonium fluoride or its hydrate> Quaternary alkyl ammonium fluoride or its hydrate releases fluoride ions that are involved in the cleavage of Si-O bonds. The quaternary alkyl ammonium moiety can dissolve the salt of quaternary alkyl ammonium fluoride in an aprotic solvent. As the quaternary alkyl ammonium fluoride, various compounds can be used without particular limitation. Hydrates of quaternary alkyl ammonium fluoride include, for example, trihydrate, tetrahydrate, and pentahydrate. The quaternary alkyl ammonium fluoride may be one type or a combination of two or more types.

[0020] In one embodiment, the quaternary alkyl ammonium fluoride is R 2 R 3 R 4 R 5 N + F - R is a tetraalkylammonium fluoride represented by the formula 2 ~R 5 are each independently an alkyl group selected from the group consisting of a methyl group, an ethyl group, an n-propyl group, an isopropyl group, and an n-butyl group. Examples of such quaternary alkyl ammonium fluorides include tetramethylammonium fluoride, tetraethylammonium fluoride, tetrapropylammonium fluoride, and tetrabutylammonium fluoride. From the standpoints of decomposition and cleaning performance, availability, price, and the like, the quaternary alkyl ammonium fluoride is preferably tetrabutylammonium fluoride (TBAF).

[0021] The content of the quaternary alkyl ammonium fluoride in the composition is preferably 0.01 to 10 mass %. Here, the "content of the quaternary alkyl ammonium fluoride" refers to the hydrate of the quaternary alkyl ammonium fluoride in the case where the composition contains the hydrate. waterThe value is calculated as the mass of only the quaternary alkyl ammonium fluoride, excluding the mass of the quaternary alkyl ammonium fluoride. The content of the quaternary alkyl ammonium fluoride in the composition is more preferably 1 to 10 mass%, further preferably 3 to 7 mass%, and particularly preferably 4 to 6 mass%. By making the content of the quaternary alkyl ammonium fluoride 0.01 mass% or more, the adhesive polymer can be effectively decomposed and washed, and by making it 10 mass% or less, corrosion of the metal part included in the device formation surface of the device wafer can be prevented or suppressed.

[0022] <Aprotic Solvents> The composition contains, as an aprotic solvent, (A) an N-substituted amide compound having no active hydrogen on a nitrogen atom, and (B) dipropylene glycol dimethyl ether.

[0023] The content of the aprotic solvent in the composition is preferably from 80 to 99.99 mass %, more preferably from 85 to 99.95 mass %, and even more preferably from 90 to 99.9 mass %.

[0024] <(A) N-substituted amide compound having no active hydrogen on the nitrogen atom> (A) N-substituted amide compounds having no active hydrogen on the nitrogen atom (also referred to simply as "(A) N-substituted amide compounds" in the present disclosure) are relatively highly polar aprotic solvents, and can uniformly dissolve or disperse quaternary alkylammonium fluoride and its hydrate in the composition. In the present disclosure, "(A) N-substituted amide compounds" also include urea compounds (carbamide compounds) having no active hydrogen on the nitrogen atom. As the (A) N-substituted amide compound, various compounds can be used without particular limitation, for example, acyclic N-substituted amides such as N,N-dimethylformamide (DMF), N,N-diethylformamide, N,N-dimethylacetamide, N,N-diethylacetamide, N,N-dimethylpropionamide, N,N-diethylpropionamide, and tetramethylurea; cyclic N-substituted amides such as 2-pyrrolidone derivatives, 2-piperidone derivatives, ε-caprolactam derivatives, 1,3-dimethyl-2-imidazolidinone (DMI), 1-methyl-3-ethyl-2-imidazolidinone, 1,3-diethyl-2-imidazolidinone, and 1,3-dimethyl-3,4,5,6-tetrahydro-2(1H)-pyrimidinone (N,N'-dimethylpropyleneurea). The (A) N-substituted amide compound may be one type or a combination of two or more types.

[0025] In one embodiment, the (A) N-substituted amide compound has the formula (2): [ka] (In formula (2), R 1 represents an alkyl group having 1 to 4 carbon atoms. The 2-pyrrolidone derivative compound represented by formula (2) is represented by the formula (1). Examples of the alkyl group having 1 to 4 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, and a t-butyl group. Examples of the 2-pyrrolidone derivative compound represented by formula (2) include N-methylpyrrolidone (NMP), N-ethylpyrrolidone (NEP), N-propylpyrrolidone, and N-butylpyrrolidone.

[0026] The N-substituted amide compound (A) is represented by the formula (2) R 1 is preferably a 2-pyrrolidone derivative compound in which R 1 More preferably, it is a 2-pyrrolidone derivative compound in which is a methyl group, that is, N-methylpyrrolidone.

[0027] The content of the N-substituted amide compound in the aprotic solvent is preferably 50 to 95 mass%, more preferably 60 to 95 mass%, and even more preferably 70 to 90 mass%, when the aprotic solvent is taken as 100 mass%.

[0028] <(B) Dipropylene glycol dimethyl ether> (B) Dipropylene glycol dimethyl ether (DPGDME) can be combined with (A) N-substituted amide compound to form a mixed solvent system that exhibits high affinity for the adhesive surface. Compositions using such a mixed solvent system can achieve high etching rates by effectively utilizing the reactivity of quaternary alkyl ammonium fluorides.

[0029] Dipropylene glycol dimethyl ether has the following three structural isomers: [ka] [ka] [ka]

[0030] In the composition of the present disclosure, the ratio of the structural isomer of dipropylene glycol dimethyl ether represented by formula (1) is 50% by mass or more, preferably 60% by mass or more, based on the total amount of dipropylene glycol dimethyl ether. The ratio of the structural isomer of dipropylene glycol dimethyl ether represented by formula (1) is preferably 50 to 99% by mass, more preferably 60 to 95% by mass, even more preferably 70 to 95% by mass, and particularly preferably 80 to 90% by mass, based on the total amount of dipropylene glycol dimethyl ether.

[0031] Dipropylene glycol dimethyl ether containing the structural isomer represented by formula (1) can be obtained, for example, from Nippon Nyukazai Co., Ltd. (containing 80% by mass or more of the structural isomer represented by formula (1)) and Dow Chemical Japan, Ltd. (containing 45% by mass or more of the structural isomer represented by formula (1)).

[0032] The content of dipropylene glycol dimethyl ether in the aprotic solvent is preferably 5 to 50 mass%, more preferably 5 to 40 mass%, and further preferably 10 to 30 mass%, when the aprotic solvent is taken as 100 mass%.

[0033] The composition may contain an additional aprotic solvent other than (A) the N-substituted amide compound and (B) dipropylene glycol dimethyl ether. Examples of such additional aprotic solvents include dialkyl ethers of glycols such as ethylene glycol dimethyl ether, propylene glycol dimethyl ether, diethylene glycol dimethyl ether, tripropylene glycol dimethyl ether, tripropylene glycol diethyl ether, tripropylene glycol di-n-butyl ether, tetraethylene glycol dimethyl ether, and tetrapropylene glycol dimethyl ether; dialkyl ethers such as dibutyl ether, dipentyl ether, dihexyl ether, diheptyl ether, dioctyl ether, butylhexyl ether, and butyloctyl ether.

[0034] The flash point of the additional aprotic solvent is preferably 21°C or higher. By using an additional aprotic solvent with a flash point of 21°C or higher, i.e., not falling under the category of Class 4 Hazardous Materials, Class 1 Petroleum, the requirements for facilities, working environment, etc. in the production and use of the composition can be reduced. For example, the flash points of diethylene glycol dimethyl ether and dibutyl ether are 51°C and 25°C, respectively. The flash point of dipropylene glycol dimethyl ether is 60°C. The flash point is measured by the tag-closed method (JIS K 2265-1:2007).

[0035] The content of the additional aprotic solvent in the aprotic solvent is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 1% by mass or less, based on 100% by mass of the aprotic solvent. In one embodiment, the aprotic solvent does not contain an additional aprotic solvent, i.e., consists of (A) an N-substituted amide compound and (B) dipropylene glycol dimethyl ether.

[0036] <Additives and other ingredients> The composition may contain additives such as antioxidants, surfactants, preservatives, and antifoaming agents as optional components, as long as the effects of the present invention are not significantly impaired.

[0037] In one embodiment, the composition is substantially free of protic solvent or free of protic solvent.For example, the content of protic solvent in the composition can be 5% by weight or less, 3% by weight or less, or 1% by weight or less.The protic solvent that can be included in the composition can be water derived from quaternary alkyl ammonium fluoride hydrate.

[0038] In one embodiment, the composition is substantially free of aprotic solvents selected from ketones and esters, or free of aprotic solvents selected from ketones and esters.For example, the content of aprotic solvents selected from ketones and esters in the composition can be 1% by mass or less, 0.5% by mass or less, or 0.1% by mass or less.In this embodiment, in the presence of a fluorine compound, the reaction product (aldol self-condensation product) or decomposition product (alcohol and carboxylic acid) generated from ketone or ester is solvated with fluoride ion, which suppresses the deactivation of fluoride ion, and suppresses the decrease in etching rate over time.

[0039] The composition of the present disclosure can be used as a decomposition cleaning composition for adhesive polymers contained in various adhesives. The adhesive polymer is not particularly limited as long as it can be cleaned using the composition of the present disclosure. In addition to the adhesive polymer, the adhesive may contain optional components such as a curing agent, a curing accelerator, a crosslinking agent, a surfactant, a leveling agent, and a filler.

[0040] <Adhesive polymer> In one embodiment, the adhesive polymer contains a Si-O bond. The adhesive polymer is depolymerized or loses its crosslinked structure by cleavage of the Si-O bond by the fluoride ion of the quaternary alkyl ammonium fluoride, and becomes soluble in an aprotic solvent, so that the adhesive polymer can be removed from the surface of a device wafer or the like.

[0041] The adhesive polymer containing Si-O bonds is preferably a polyorganosiloxane compound. Since the polyorganosiloxane compound contains a large number of siloxane bonds (Si-O-Si), it can be effectively decomposed and cleaned using the composition. Examples of the polyorganosiloxane compound include silicone resins such as silicone elastomers, silicone gels, and MQ resins, as well as modified products thereof such as epoxy modified products, acrylic modified products, methacrylic modified products, amino modified products, and mercapto modified products. The polyorganosiloxane compound may be a silicone modified polymer such as a silicone modified polyurethane or a silicone modified acrylic resin.

[0042] In one embodiment, the adhesive polymer is an addition-cured silicone elastomer, silicone gel, or silicone resin that includes an ethylenically unsaturated polyorganosiloxane, such as a vinyl-terminated polydimethylsiloxane or a vinyl-terminated MQ resin, and a polyorganohydrogensiloxane, such as a polymethylhydrogensiloxane, as a crosslinker, and is cured with a hydrosilylation catalyst, such as a platinum catalyst.

[0043] In another embodiment, the adhesive polymer comprises an aralkyl-, epoxy-, or phenyl-containing polydiorganosiloxane, particularly an aralkyl-, epoxy-, or phenyl-containing polydimethylsiloxane. An adhesive comprising such an adhesive polymer may be used for temporary adhesion in combination with an adhesive comprising the addition curing silicone.

[0044] [How to clean adhesive polymers] The adhesive polymer on a substrate such as a silicon wafer can be cleaned by a variety of conventional methods using the composition. Examples of methods for cleaning the adhesive polymer include discharging the composition onto the substrate so as to come into contact with the adhesive polymer while rotating the substrate at a predetermined speed using a spin coater or the like (spin etch), spraying the composition onto the adhesive polymer on the substrate (spray), and immersing the substrate having the adhesive polymer in a tank containing the composition (dipping). The temperature of the decomposition cleaning may vary depending on the type and amount of adhesion of the adhesive polymer on the substrate, and is generally 20°C to 90°C, preferably 40°C to 60°C. The time of the decomposition cleaning may vary depending on the type and amount of adhesion of the adhesive polymer on the substrate, and is generally 5 seconds to 10 hours, preferably 10 seconds to 2 hours. During the decomposition cleaning, ultrasonic waves may be applied to the bath of the composition or the substrate.

[0045] After disassembly and cleaning, the substrate may be rinsed with alcohol such as isopropyl alcohol (IPA) or deionized water (DIW), and the substrate may be dried by spraying with nitrogen gas or air, or by heating under normal or reduced pressure.

[0046] [Device wafer manufacturing method] In one embodiment, a method for producing a device wafer includes cleaning an adhesive polymer on the device wafer with the composition. After cleaning, the device wafer may be optionally rinsed or dried.

[0047] The method for manufacturing a device wafer may further include the following steps: forming a semiconductor device on a substrate such as a silicon wafer to obtain a device wafer, placing a semiconductor device-forming surface of the device wafer opposite a support wafer and temporarily bonding the device wafer and the support wafer via an adhesive containing an adhesive polymer, thinning the device wafer by polishing the surface (back surface) of the device wafer opposite to the device-forming surface, and separating the support wafer from the device wafer. The formation of the semiconductor device, the temporary bonding of the device wafer and the support wafer, the polishing of the back surface of the device wafer, and the separation of the device wafer from the support wafer may be performed by a conventionally known method and are not particularly limited.

[0048] [Support wafer regeneration method] The composition can be used to regenerate a support wafer used in the manufacture of a device wafer. In one embodiment, a method for regenerating a support wafer includes cleaning an adhesive polymer on the support wafer with the composition. After cleaning, the support wafer may be rinsed or dried as required. EXAMPLES

[0049] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples.

[0050] Dipropylene glycol dimethyl ether (DPGDME), which is a mixture of structural isomers, having different ratios of the structural isomer represented by formula (1) was prepared by the following procedure. 1. Ratio of structural isomer represented by formula (1): 86.41% by mass DPGDME obtained from Nippon Nyukazai Co., Ltd. was used. 2. Proportion of structural isomer represented by formula (1): 73.71% by mass DPGDME obtained from Nippon Nyukazai Co., Ltd. and DPGDME obtained from Dow Chemical Japan Co., Ltd. were mixed in a ratio of 2:1. 3. Proportion of structural isomer represented by formula (1): 61.41% by mass DPGDME obtained from Nippon Nyukazai Co., Ltd. and DPGDME obtained from Dow Chemical Japan Co., Ltd. were mixed in a ratio of 1:2. 4. Proportion of structural isomer represented by formula (1) 49.12% by mass DPGDME obtained from Dow Chemical Japan Co., Ltd. was used.

[0051] Preparation of composition (5% by mass TBAF / mixed solvent) Example 1 In a 125mL polyethylene container, 1.167g of tetrabutylammonium fluoride trihydrate (TBAF·3H2O) (Kanto Chemical Co., Ltd., 97% special grade) was added, followed by 13.572g of N-methyl-pyrrolidone (NMP) and 4.197g of DPGDME (Nippon Nyukazai Co., Ltd.), which were then mixed to dissolve the TBAF·3H2O. In this way, a 5% by mass TBAF mixed solvent composition was prepared in which the proportion of the structural isomer represented by formula (1) in DPGDME was 86.41% by mass and the mass ratio of NMP:DPGDME was 0.764:0.236.

[0052] Examples 2 to 3 and Comparative Example 1 Using a procedure similar to that of Example 1, compositions were prepared using DPGDME having a ratio of the structural isomer represented by formula (1) of 73.71 mass%, 61.41 mass%, or 49.12 mass%, in which the ratio of the structural isomer represented by formula (1) in DPGDME was 73.71 mass% (Example 2), 61.41 mass% (Example 3), or 49.12 mass% (Comparative Example 1), and the mass ratio of NMP:DPGDME was 0.764:0.236, respectively, of 5 mass% TBAF mixed solvent.

[0053] Examples 4 to 9 and Comparative Examples 2 to 3 Using the same procedures as in Examples 1 to 3 and Comparative Example 1, compositions of 5 mass% TBAF mixed solvent with an NMP:DPGDME mass ratio of 0.600:0.400 (Examples 4 to 6 and Comparative Example 2) or 0.900:0.100 (Examples 7 to 9 and Comparative Example 3) were prepared.

[0054] Examples 10 to 18 and Comparative Examples 4 to 6 Compositions of 5 mass% TBAF mixed solvent with a mass ratio of NEP:DPGDME of 0.764:0.236 (Examples 10-12 and Comparative Example 4), 0.600:0.400 (Examples 13-15 and Comparative Example 5), or 0.900:0.100 (Examples 16-18 and Comparative Example 6) were prepared in the same manner as in Examples 1-3 and Comparative Example 1, except that N-ethyl-pyrrolidone (NEP) was used instead of N-methyl-pyrrolidone (NMP).

[0055] The compositions of the examples and comparative examples are shown in Tables 1-1 and 1-2.

[0056] [Table 1-1]

[0057] [Table 1-2]

[0058] Cleaning test 1 Silicone resin was applied onto a 12-inch (300 mm) silicon wafer (thickness 770 μm) so that the dry film thickness was 110 μm. Then, the wafer was heated on a hot plate at 140° C. for 15 minutes and at 190° C. for 10 minutes to form an adhesive layer on the silicon wafer. The silicon wafer with the adhesive layer was divided into test pieces measuring 1 cm×1 cm, and the thickness of the center of the test piece was measured using a micrometer.

[0059] A screw cap with a volume of 50 cc was placed on a magnetic stirrer. 15.0 mL of the composition immediately after preparation (within 30 minutes after preparation) and a stirrer were placed in the screw cap. One test piece was immersed in the composition, and the stirrer was rotated at 900 rpm for 1 minute at room temperature (25 ° C.). After immersion, the test piece was removed with tweezers and thoroughly rinsed using a wash bottle of isopropyl alcohol (IPA). Then, the test piece was thoroughly rinsed in the same manner using a wash bottle of ion-exchanged water (DIW). Nitrogen gas was sprayed onto the test piece to dry the adhering water, and the thickness of the center of the test piece was measured using a micrometer. The same test was performed with cleaning times of 2 minutes, 3 minutes, and 5 minutes. The difference in thickness of the test piece before and after immersion for each stirring time, i.e., the change in the film thickness of the silicone resin, was calculated, and the slope of the approximation line (intercept is 0) was taken as the etching rate (ER) of the composition.

[0060] Cleaning test 2 A 12-inch (300 mm) silicon wafer (770 μm thick) was divided into pieces measuring 1.5 cm x 1.5 cm. An adhesive consisting of 2.339 g of SYLGARD (registered trademark) 184 (manufactured by Dow Corning Toray Co., Ltd.) base agent and 0.2388 g of hardener was drawn up with a Pasteur pipette and dropped onto the divided silicon wafer in one drop. The mixture was then heated in a dryer (125°C) for 20 minutes to form an adhesive layer on the silicon wafer. This was used as a test piece, and the thickness of the center of the test piece was measured using a micrometer.

[0061] A screw cap with a volume of 50 cc was placed on a magnetic stirrer. 15.0 mL of the composition immediately after preparation (within 30 minutes after preparation) and a stirrer were placed in the screw cap. One test piece was immersed in the composition, and the stirrer was rotated at 900 rpm for 1 minute at room temperature (25 ° C.). After immersion, the test piece was removed with tweezers and thoroughly rinsed using a wash bottle of isopropyl alcohol (IPA). Then, the test piece was similarly thoroughly rinsed using a wash bottle of ion-exchanged water (DIW). Nitrogen gas was sprayed onto the test piece to dry the adhering water, and the thickness of the center of the test piece was measured using a micrometer. The same test was performed with a cleaning time of 3 minutes and 5 minutes. The difference in thickness of the test piece before and after immersion for each stirring time, i.e., the change in the film thickness of the silicone resin, was calculated, and the slope of the approximation line (intercept is 0) was taken as the etching rate (ER) of the composition.

[0062] The results are shown in Table 2 (Examples 1 to 3, Comparative Example 1), Table 3 (Examples 4 to 6, Comparative Example 2), Table 4 (Examples 7 to 9, Comparative Example 3), Table 5 (Examples 10 to 12, Comparative Example 4), Table 6 (Examples 13 to 15, Comparative Example 5), and Table 7 (Examples 16 to 18, Comparative Example 6). In addition, graphs of the change in film thickness (mm) versus cleaning time (min) are combined with approximation lines to show the results in FIG. 1 (NMP:DPGDME=0.764:0.236, cleaning test 1), FIG. 2 (NMP:DPGDME=0.764:0.236, cleaning test 2), FIG. 3 (NMP:DPGDME=0.600:0.400, cleaning test 1), and FIG. 4 (NMP:DPGDME=0.600:0.400, cleaning test 2). The results are shown in Figure 5 (NMP:DPGDME = 0.900:0.100, cleaning test 1), Figure 6 (NMP:DPGDME = 0.900:0.100, cleaning test 2), Figure 7 (NEP:DPGDME = 0.764:0.236, cleaning test 2), Figure 8 (NEP:DPGDME = 0.600:0.400, cleaning test 2), and Figure 9 (NEP:DPGDME = 0.900:0.100, cleaning test 2). The numbers in the legends of Figures 1 to 9 are the proportions of the structural isomers represented by formula (1) (%, "mass" is omitted).

[0063] [Table 2]

[0064] [Table 3]

[0065] [Table 4]

[0066] [Table 5]

[0067] [Table 6]

[0068] [Table 7] [Industrial Applicability]

[0069] The composition of the present disclosure can be suitably used for removing and cleaning adhesive residues from device wafers, particularly adhesive residues containing a polyorganosiloxane compound as an adhesive polymer, used in the thinning process of semiconductor wafers.

Claims

1. A composition for decomposing and cleaning an adhesive polymer, comprising a quaternary alkylammonium fluoride or a hydrate of a quaternary alkylammonium fluoride, and (A) an N-substituted amide compound having no active hydrogen on a nitrogen atom as an aprotic solvent, and (B) dipropylene glycol dimethyl ether, wherein the dipropylene glycol dimethyl ether (B) is a compound represented by the formula (1): [Formula 1] The composition for decomposition and cleaning of adhesive polymers, wherein the proportion of the structural isomer represented by the following formula (1) is 50 mass % or more based on the total amount of the dipropylene glycol dimethyl ether (B).

2. 2. The composition for decomposing and cleaning an adhesive polymer according to claim 1, wherein the proportion of the structural isomer represented by formula (1) is 60 mass% or more based on the total amount of the dipropylene glycol dimethyl ether (B).

3. The (A) N-substituted amide compound is represented by the formula (2): [Case 2] (In formula (2), R 1 represents an alkyl group having 1 to 4 carbon atoms. The composition for decomposing and cleaning an adhesive polymer according to claim 1 or 2, wherein the 2-pyrrolidone derivative compound is represented by the following formula:

4. The (A) N-substituted amide compound is represented by the formula (2) R 1 The composition for decomposing and cleaning an adhesive polymer according to claim 3, which is a 2-pyrrolidone derivative compound in which R is a methyl group or an ethyl group.

5. The adhesive polymer decomposition cleaning composition according to any one of claims 1 to 4, wherein the content of the quaternary alkyl ammonium fluoride is 0.01 to 10 mass%.

6. The quaternary alkyl ammonium fluoride is R 2 R 3 R 4 R 5 N + F -R is a tetraalkylammonium fluoride represented by the formula: 2 ~R 5 The composition for decomposing and cleaning an adhesive polymer according to any one of claims 1 to 5, wherein each of the alkyl groups is independently selected from the group consisting of a methyl group, an ethyl group, an n-propyl group, an isopropyl group, and an n-butyl group.

7. The adhesive polymer decomposition cleaning composition according to any one of claims 1 to 6, wherein the content of the N-substituted amide compound (A) is 50 to 95 mass% and the content of the dipropylene glycol dimethyl ether (B) is 5 to 50 mass% relative to 100 mass% of the aprotic solvent.

8. The adhesive polymer decomposition cleaning composition according to any one of claims 1 to 7, wherein the adhesive polymer is a polyorganosiloxane compound.

9. A method for cleaning an adhesive polymer on a substrate, using the composition for decomposing and cleaning an adhesive polymer according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Method for removing silicone polymer deposit from electronic component

    JP2004000969A

  • Remover and cleaning agent for semiconductor etching residue

    JP2008252100A

  • Remover of siloxane resin, method for removing siloxane resin using the same, and methods for manufacturing semiconductor substrate product and semiconductor element

    JP2014133855A

  • Silicone solubilizer

    JP2015505886A

  • Detergent composition and method for manufacturing thin substrate

    JP2017199754A