Titanium material and method for manufacturing titanium material
By aligning titanium oxide crystals through titanium nitride formation and controlled anodic oxidation, the method ensures uniform oxide film thickness and high color saturation in titanium materials, addressing the dullness issue and reducing equipment complexity.
Patent Information
- Application Number
- JP2021017671
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-05
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2041-02-05
AI Technical Summary
Existing methods for coloring titanium materials result in dull colors when the oxide film thickness exceeds 80 nm due to variations in oxide film thickness and crystal orientation, requiring large-scale capital investments for precise control.
The method involves aligning the crystals of anatase-type and rutile-type titanium oxide in one direction by forming titanium nitride on the titanium base material, followed by anodic oxidation with controlled nitrogen concentration and voltage application, ensuring uniform oxide film thickness and high saturation.
Achieves highly saturated colors even with thick oxide films, reducing the need for precise control equipment and capital investment while maintaining excellent color development.
Smart Images

Figure 0007575677000006 
Figure 0007575677000001 
Figure 0007575677000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a titanium material and a method for producing the titanium material. [Background technology]
[0002] In recent years, titanium has been increasingly recognized as an aesthetic material, thanks to its distinctive, subdued texture and coloring properties resulting from the interference effect of the thin oxide film that forms on its surface.
[0003] Patent Document 1 discloses a method for coloring metallic titanium, which is characterized by nitriding titanium or a titanium alloy to form a titanium nitride film on the surface, and then oxidizing the titanium or titanium alloy, in order to efficiently produce colored titanium in a wide variety of colors.
[0004] One method for forming an oxide film is, for example, an anodization method. The anodization method is a method in which an oxide film is formed on the surface of titanium by passing an electric current through titanium as the anode in an electrolyte solution. Anodization is highly valued as an easy coloring method because the thickness of the oxide film, i.e., the color tone, can be controlled by the applied voltage.
[0005] As a method for forming an oxide film on a titanium material by anodization, for example, Patent Document 2 discloses a method for producing a crystalline titanium oxide film, which includes the following steps (a-1) and (b). (a-1) A step of forming titanium nitride on the surface of titanium or a titanium alloy by carrying out a heat treatment of the titanium or titanium alloy under any one of the conditions described in (1) to (3) below. (1) In a nitrogen and / or ammonia gas atmosphere, in the presence of an oxygen trapping agent, (2) In an atmosphere filled with nitrogen and / or ammonia gas after reducing the pressure and evacuating the atmospheric gas; and (3) In an atmosphere filled with nitrogen and / or ammonia gas after reducing the pressure and evacuating the atmospheric gas, in the presence of an oxygen trapping agent; and (b) A step of immersing the titanium or titanium alloy obtained in the above step (a-1) in an electrolyte containing an inorganic acid and / or an organic acid, and applying a voltage to perform anodization.
[0006] Patent Document 3 discloses a method for producing a surface-treated metallic titanium material or titanium alloy material, comprising the steps of: (1) forming titanium nitride on the surface of a metallic titanium material or titanium alloy material by one treatment method selected from the group consisting of heat treatment in an ammonia gas atmosphere and heat treatment in a nitrogen gas atmosphere, and the heating temperature being 750°C or higher; (2) anodizing the metallic titanium material or titanium alloy material having titanium nitride formed on its surface obtained in step (1) by applying a voltage of 10 V or more in an electrolyte that does not have an etching effect on titanium, thereby forming a titanium oxide film; and (3) heat treating the metallic titanium material or titanium alloy material having a titanium oxide film formed on its surface obtained in step (2) at a temperature of 400°C or higher in an atmosphere selected from the group consisting of an air oxidizing atmosphere, an atmosphere containing a mixture of oxygen gas and nitrogen gas, and an oxygen gas atmosphere.
[0007] Patent Document 4 discloses a method for producing a titanium material having a highly wear-resistant interference color coating, which is characterized in that titanium or a titanium alloy is subjected to a gas nitriding treatment, and then anodized to develop an interference color.
[0008] Patent Document 5 discloses a method for coloring titanium by applying a voltage in an electrolyte to electrolytically oxidize the surface, which is characterized by inserting the application of a low voltage lower than the main voltage while maintaining the application of a main voltage corresponding to the desired color, and dividing the application of the main voltage into multiple stages with the application of the inserted low voltage in between.
[0009] Patent document 6 discloses a method for forming an oxide film on the surface of a workpiece mainly composed of a valve metal by anodization, the method comprising a first anodization step in which anodization is performed at a low current density and a second anodization step in which anodization is performed at a high current density. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] Japanese Patent Application Publication No. 9-263929 [Patent Document 2] International Publication No. 2007 / 23543 [Patent Document 3] International Publication No. 2014 / 132874 [Patent Document 4] JP 2006-63406 A [Patent Document 5] JP 2006-219735 A [Patent Document 6] JP 2005-320623 A Summary of the Invention [Problem to be solved by the invention]
[0011] However, in the techniques disclosed in Patent Documents 1 to 4, when the applied voltage in anodizing was 50 V or more, the saturation of the titanium material surface was low and the color was sometimes perceived as dull. When the applied voltage was 50 V or more, the thickness of the oxide film could be made 80 nm or more, but in the techniques disclosed in Patent Documents 1 to 4, when the thickness of the oxide film was 80 nm or more, the color of the titanium material was sometimes perceived as dull.
[0012] In addition, the technology disclosed in Patent Document 5 is a method in which application of a low voltage lower than the main voltage is inserted in the middle of maintaining the application of the main voltage, and the application of the main voltage is divided into multiple stages sandwiched between the inserted low voltage applications, so that a large capital investment is required.
[0013] In addition, the technology disclosed in Patent Document 6 is a method comprising a first anodizing process in which anodizing is performed at a low current density and a second anodizing process in which anodizing is performed at a high current density, and this method allows precise control of the current density, but requires a large capital investment.
[0014] The present invention has been made in consideration of the above problems, and an object of the present invention is to provide a titanium material and a method for manufacturing a titanium material that have excellent color development properties even when the oxide film is thick. [Means for solving the problem]
[0015] In titanium materials with low chroma, each crystal grain has a different color, and the naked eye perceives the color as a mixture of these colors (juxtaposition mixture), resulting in a dull color. It is believed that titanium materials with low chroma have variations in the thickness of the oxide film. The inventors of the present invention have conducted detailed studies on the anodizing conditions and the coloring properties of titanium materials, and have found that the thickness of the oxide film formed by anodizing is determined by the magnitude of the applied voltage and the electrical resistivity of the amorphous titanium oxide, anatase titanium oxide, or rutile titanium oxide formed.
[0016] Anodic oxidation with an applied voltage of less than 50V can produce highly saturated colors. Anodic oxidation with an applied voltage of less than 50V mainly produces amorphous titanium oxide. Amorphous titanium oxide has no anisotropy in electrical resistivity, so it is believed that the thickness of the oxide film formed is likely to be consistent. On the other hand, it was found that anodization with an applied voltage of 50V or more results in a difference in the thickness of the oxide film depending on the crystal unit of the titanium substrate, resulting in a decrease in saturation. This is believed to be because the crystal orientation of anatase-type titanium oxide or rutile-type titanium oxide formed by anodization differs for each crystal orientation of the titanium substrate and changes due to the introduced strain, and the crystals of anatase-type titanium oxide and rutile-type titanium oxide have anisotropy and anisotropy in electrical resistivity.
[0017] The inventors of the present invention have come up with the idea of aligning the crystals of anatase-type titanium oxide and rutile-type titanium oxide in one direction as much as possible to obtain a titanium material with excellent color development properties, thereby achieving electrical resistivity with small anisotropy. The inventors have further investigated the matter and have come up with the present invention.
[0018] The gist of the present invention, which has been completed based on the above findings, is as follows. [1] On the surface of titanium substrate Anodized Film Equipped with the titanium substrate comprises titanium nitride; The titanium substrate Anodized Film When the surface on which the titanium nitride is formed is analyzed by X-ray photoelectron spectroscopy, the maximum concentration of nitrogen forming the titanium nitride is 2 to 10 atomic %, L * a * b * Saturation C in the color system * ab is 20 or more the law of nature , The thickness of the anodized film is 80 nm or more. Titanium material. [2] The position where the nitrogen forming the titanium nitride has a maximum concentration is the position where the titanium substrate and the Anodized Film The titanium material according to [1], wherein the interface is located within a range of 300 nm in the direction of the titanium substrate from the interface with the 。 [3 ] The method for producing a titanium material according to the above [1] or [2], A method for producing a titanium material, comprising the steps of: nitriding a titanium material under any one of the following conditions (i) to (iii) in a nitriding process; and then performing an anodizing process. Condition (i): In an atmosphere having a nitrogen partial pressure of 1 Pa or more and less than 10 Pa, the titanium material is held at a temperature of 600° C. or more and 800° C. or less for 1 minute to 5 hours, and then cooled in an atmosphere having a nitrogen partial pressure of 1 Pa or more and less than 10 Pa. Condition (ii) The titanium material is held at a temperature of 250° C. or more and 600° C. or less for 40 seconds or more and 5 minutes or less in an air atmosphere, and then cooled in the air atmosphere. Condition (iii) In a vacuum atmosphere, the titanium material is maintained at a temperature of 200°C or higher, and, after the temperature is maintained, when the temperature of the titanium material reaches any temperature between 200°C or higher and 500°C or lower, pure nitrogen gas is blown onto the titanium material to cool it; or, in a vacuum atmosphere, the titanium material is maintained at a temperature of 300°C or higher, and, after the temperature is maintained, when the temperature of the titanium material reaches any temperature between 300°C or higher and less than 800°C, air is blown onto the titanium material to cool it. Effect of the Invention
[0019] As described above, according to the present invention, it is possible to provide a titanium material and a method for manufacturing a titanium material that have excellent color development properties even when the oxide film is thick. [Brief description of the drawings]
[0020] [Figure 1] FIG. 2 is a diagram showing an example of the analysis results of a titanium material after anodization using X-ray photoelectron spectroscopy. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] Preferred embodiments of the present invention will now be described in detail.
[0022] <Titanium material manufacturing method> The titanium material according to the present embodiment is provided with an oxide film on the surface of a titanium base material, the titanium base material having titanium nitride, and when the surface of the titanium base material on which the oxide film is disposed is analyzed by X-ray photoelectron spectroscopy, the maximum concentration of nitrogen forming the titanium nitride is 2 to 10 atomic %, and L * a * b * Saturation C in the color system * ab is equal to or greater than 20. The details are explained below.
[0023] (Titanium substrate) The titanium substrate for use in the titanium material according to the present embodiment is not particularly limited and may be either pure titanium or a titanium alloy. The titanium substrate is, for example, pure titanium or a titanium alloy having a Ti content of 70 mass% or more.
[0024] Pure titanium includes, for example, commercially pure titanium as specified by JIS standard (JIS H 4600:2012) types 1 to 4 and the corresponding ASTM standard Grades 1 to 4. That is, the commercially pure titanium targeted in the present invention contains, by mass%, C: 0.1% or less, H: 0.015% or less, O: 0.4% or less, N: 0.07% or less, Fe: 0.5% or less, with the balance being Ti and impurities.
[0025] The titanium alloy may be an α-type titanium alloy, an α+β-type titanium alloy, or a β-type titanium alloy.
[0026] Examples of α-type titanium alloys include highly corrosion-resistant alloys (titanium alloys specified in the above JIS standards of 11 to 13, 17, and 19 to 22, and ASTM standards of Grades 7, 11, 13, 14, 17, 30, and 31, as well as titanium alloys containing small amounts of various elements), Ti-0.5Cu, Ti-1.0Cu, Ti-1.0Cu-0.5Nb, Ti-1.0Cu-1.0Sn-0.3Si-0.25Nb, Ti-0.5Al-0.45Si, Ti-0.9Al-0.35Si, Ti-3Al-2.5V, Ti-5Al-2.5Sn, Ti-6Al-2Sn-4Zr-2Mo, Ti-6Al-2.75Sn-4Zr-0.4Mo-0.45Si, and the like.
[0027] Examples of α+β type titanium alloys include Ti-6Al-4V, Ti-6Al-6V-2Sn, Ti-6Al-7V, Ti-3Al-5V, Ti-5Al-2Sn-2Zr-4Mo-4Cr, Ti-6Al-2Sn-4Zr-6Mo, and Ti-1Fe-0. 35O, Ti-1.5Fe-0.5O, Ti-5Al-1Fe, Ti-5Al-1Fe-0.3Si, Ti-5Al-2Fe, Ti-5Al-2Fe-0.3Si, Ti-5Al-2Fe-3Mo, Ti-4.5Al-2Fe-2V-3Mo, etc.
[0028] Furthermore, examples of β-type titanium alloys include Ti-11.5Mo-6Zr-4.5Sn, Ti-8V-3Al-6Cr-4Mo-4Zr, Ti-10V-2Fe-3Mo, Ti-13V-11Cr-3Al, Ti-15V-3Al-3Cr-3Sn, Ti-6.8Mo-4.5Fe-1.5Al, Ti-20V-4Al-1Sn, and Ti-22V-4Al.
[0029] The titanium substrate has finely dispersed titanium nitride near the interface with the oxide film. When a titanium substrate having finely dispersed titanium nitride at least on the surface layer is anodized, the thickness of the oxide film formed by the anodization becomes uniform, and a highly saturated color is obtained. The reason for this is not entirely clear, but the present inventors speculate as follows. That is, the finely dispersed titanium nitride becomes the nucleus of the titanium oxide crystals formed by the anodization, and the crystal orientation of the titanium oxide crystallized from the titanium nitride is accumulated in the same direction. As a result, the crystal orientation of the titanium substrate is less likely to affect the crystal orientation of the titanium oxide, and the thickness of the oxide film becomes uniform.
[0030] In the titanium material according to this embodiment, when the surface of the titanium base material on which the oxide film is disposed is analyzed by X-ray photoelectron spectroscopy (XPS), the maximum concentration of nitrogen forming titanium nitride is 2 to 10 atomic %.
[0031] The concentration of nitrogen, oxygen, etc. forming titanium nitride is measured by the following method using JPS-9200 manufactured by JEOL Ltd. The analysis conditions are X-ray source: MgKα (hν: 1200.0 eV), beam diameter: 1 mmΦ (≒ analysis area), take-in angle: 56°, sputtering conditions: Ar +The sputtering rate is 2.9 nm / min. (SiO2 equivalent). The SiO2 equivalent is the sputtering rate when a SiO2 film whose thickness has been measured in advance using an ellipsometer is used and the same measurement conditions are used. The peak of the spectrum appearing at a binding energy position of about 393 to 402 eV is taken as the N1s peak, and N derived from organic matter is separated as about 399 to 401 eV, and N derived from titanium nitride is separated as about 397 ± 1 eV. The peak of the spectrum appearing at a binding energy position of about 280 to 295 eV is measured as the C1s peak, and C derived from organic matter is separated as about 284 to 289 eV, and C derived from titanium carbide is separated as about 281.5 ± 1 eV. The peak of the spectrum appearing at a binding energy position of about 525 to 540 eV is measured as the O1s peak, and O derived from titanium oxide is separated as 455.1 to 459.1 eV. Note that O derived from organic matter is around 399-401 eV, and is not included in the measurement region. The spectrum peak appearing at a binding energy of 450-470 eV is measured as the Ti2p peak. Titanium element is detected at 454.0 eV, Ti oxide at 455.0-459.1 eV, and Ti nitride at 455.7 eV. The spectrum peak appearing at a binding energy of 700-720 eV is measured as the Fe2p peak. Fe element is detected at 706.9 eV, Fe carbide at 708.1 eV, and Fe oxide at 709.6-710.9 eV. The bond energies of the above substances are general values and may change depending on the charge of the measurement sample, etc. When correcting the bond energy, the correction is made based on the peak position of 284 eV of the C-C bond in C derived from organic matter.
[0032] Using these peaks, the analysis software SpecSurf (Analysis) is used to analyze the element concentration and the concentration by chemical state. The concentration in mass % obtained by XPS is converted to the concentration in atomic % by SpecSurf (Analysis). Specifically, the background is corrected based on the Shirley method. Next, the peaks are fitted by chemical state for each element by Gauss-Lorents function for compounds and by Asymmetric function for metals. Then, the concentration (atomic %) by chemical state is calculated by multiplying the area ratio of the peak from each chemical state by the concentration (atomic %) of the element. The concentration of the above elements is calculated by calculating the peak area including all peaks related to each element (without separation) for each element detected by XPS, and dividing it by the sensitivity coefficient for each element to obtain a percentage. The concentration (atomic %) of each element by analysis depth is shown as a graph as shown in FIG. 1. Note that FIG. 1 shows the concentration of N, O, and Ti by analysis depth, and the concentration of other elements by analysis depth is omitted.
[0033] In this embodiment, the thickness of the oxide film refers to the thickness from the surface of the titanium material to the position where the oxygen concentration calculated based on XPS is the intermediate concentration between the maximum concentration and the base concentration. Therefore, the interface between the titanium base material and the oxide film is the position where the oxygen concentration measured by XPS is the intermediate concentration between the maximum concentration and the base concentration. The maximum concentration of nitrogen that formed titanium nitride is the maximum concentration of nitrogen on the titanium base material side from that position.
[0034] If the maximum concentration of nitrogen forming titanium nitride is 2 to 10 atomic %, the crystal orientation of titanium oxide crystallized from titanium nitride is easily accumulated in the same direction, and the thickness of the oxide film is uniform. As a result, a titanium material with high chroma is obtained. If the maximum concentration of nitrogen forming titanium nitride is less than 2 atomic %, the crystal orientation of titanium oxide is not accumulated in the same direction sufficiently, and it is difficult to obtain a titanium material with high chroma. In addition, if the amount of titanium nitride is too large, the crystal orientation of the titanium substrate affects the crystal orientation of titanium nitride, and the crystal orientation of this titanium nitride affects the crystal orientation of titanium oxide formed by anodization. If the maximum concentration of nitrogen forming titanium nitride is more than 10 atomic %, the amount of titanium nitride affected by the crystal orientation of the titanium substrate is large, and the crystal orientation of the titanium substrate indirectly affects the crystal orientation of titanium oxide formed by anodization. As a result, the thickness of the oxide film varies for each crystal of the titanium substrate, and the chroma of the titanium material decreases. Therefore, the maximum concentration of nitrogen forming titanium nitride is 10 atomic % or less.
[0035] The position where the concentration of the nitrogen forming the titanium nitride is maximum is preferably located within a range of up to 300 nm from the interface between the titanium substrate and the oxide film in the direction of the titanium substrate. If the position where the concentration of the nitrogen forming the titanium nitride is maximum is located within a range of up to 300 nm from the interface between the titanium substrate and the oxide film in the direction of the titanium substrate, the crystal orientation of the titanium oxide crystallized from the titanium nitride as a starting point is likely to accumulate in the same direction. As a result, it becomes easier to ensure the saturation of the titanium material.
[0036] Because a titanium nitride peak was detected in the XPS measurement of the titanium material according to this embodiment and the nitrogen concentration exceeded the solid solubility limit of nitrogen atoms in titanium, it is presumed that titanium nitrides such as Ti2N and TiN are present in the titanium material according to this embodiment. In addition, because the concentration is below the concentration at which a coating is formed, it is presumed that the titanium nitrides are finely dispersed.
[0037] (Oxide film) The titanium material according to the present embodiment preferably has an oxide film having a thickness of 80 nm or more arranged on the surface of the titanium base material. The thickness of the oxide film refers to the distance from the surface of the titanium material to the position where the oxygen concentration measured by the above-mentioned method is the intermediate concentration between the maximum concentration and the base concentration. In detail, the thickness of the oxide film is determined by multiplying the sputtering rate in terms of SiO2 by the basic sputtering time, which is calculated at the position where the oxygen concentration is the intermediate concentration between the maximum concentration and the base concentration, for the measured oxygen concentration on the oxide film surface.
[0038] Even with conventional color-developing materials, when the thickness of the oxide film is less than 80 nm, relatively high chroma is often obtained. On the other hand, as described above, when the thickness of the oxide film is 80 nm or more with conventional color-developing materials, the chroma is often low and the color is dull. In this embodiment, when the surface of the titanium substrate on which the oxide film is disposed is analyzed by X-ray photoelectron spectroscopy, if the maximum concentration of nitrogen forming titanium nitride is 2 to 10 atomic %, L * a * b * Saturation C in the color system * The titanium material has excellent color development properties because ab is 20 or more. Therefore, in this embodiment, excellent color development properties can be obtained even if the oxide film has a thickness of less than 80 nm, but excellent color development properties can also be achieved even if the oxide film has a thickness of 80 nm or more.
[0039] (Titanium saturation C * ab is 20 or more) In the titanium material according to this embodiment, the saturation C * ab is 20 or more. Saturation C * ab is L * C * h color system saturation, L * a * b * Chromaticity a of color space * and chromaticity b * By C * =((a * )2+(b * )2) 1 / 2 The value is expressed as: L* a * b * The color system is defined by the CIE (International Commission on Illumination) and is also standardized in JIS 8781-4:2013. * C * The h color system is L * a * b * It is a color system devised based on the color system. * If a colorimeter can measure ab, use that colorimeter to measure C. * We can measure the chromaticity ab directly, * and b * If a colorimeter can measure chromaticity a, * and b * , and chroma C * ab can be calculated by calculation. Also, for example, the tristimulus values of the XYZ color system specified by the CIE can be measured or calculated, and then used to calculate L * C * Saturation C of the h color system * Calculate ab, etc., L * a * b * Color system and L * C * By measuring or calculating values expressed in a known color system other than the h color system and converting them, L * C * Saturation C of the h color system * It is also possible to calculate
[0040] Saturation C * If ab is 20 or more, it is possible to produce a coloring material with high chroma as the final product. * ab is preferably 25 or more, more preferably 30 or more.
[0041] The shape of the titanium material according to this embodiment is not particularly limited, and may be a plate, a coil, a strip, etc. So far, the titanium material according to this embodiment has been described.
[0042] <Titanium material manufacturing method> Next, an example of a method for producing a titanium material according to this embodiment will be described. The method for producing a titanium material according to this embodiment is not particularly limited, but the titanium material according to this embodiment can be produced, for example, by the following method. Therefore, the method for producing a titanium material described below is one embodiment of the present invention.
[0043] The titanium material according to this embodiment is produced by a nitriding process in which a titanium material is nitrided under any one of the following conditions (i) to (iii), followed by anodizing. Condition (i) In an atmosphere having a nitrogen partial pressure of 1 Pa or more and less than 100 Pa, the titanium material is held at a temperature of 600°C or more and 800°C or less for 1 minute to 5 hours, and then cooled in an atmosphere having a nitrogen partial pressure of 1 Pa or more and less than 100 Pa. Condition (ii) The titanium material is held at a temperature of 250°C or more and 600°C or less for 40 seconds or more and 5 minutes or less in an air atmosphere, and then cooled in the air atmosphere. Condition (iii): In a vacuum atmosphere, a titanium material is maintained at a temperature of 200°C or higher, and, once the temperature of the titanium material reaches any temperature between 200°C or higher and 500°C or lower, pure nitrogen gas is blown onto the titanium material to cool it; or, in a vacuum atmosphere, a titanium material is maintained at a temperature of 300°C or higher, and, once the temperature of the titanium material reaches any temperature between 300°C or higher and less than 800°C, air is blown onto the titanium material to cool it.
[0044] (Nitriding process) First, the nitriding process will be described. In this process, the titanium material is treated under any of the above conditions (i) to (iii), so that nitrogen in the atmosphere diffuses into the surface layer of the titanium material, and titanium nitride is formed near the surface of the titanium material. Each of the conditions (i) to (iii) will be described below.
[0045] Condition (i) In condition (i), the titanium material is held at a temperature of 600°C or more and 800°C or less for 1 minute or more and 5 hours or less in an atmosphere with a nitrogen partial pressure of 1 Pa or more and less than 100 Pa, and then cooled in an atmosphere with a nitrogen partial pressure of 1 Pa or more and less than 100 Pa. Note that the nitrogen partial pressure in the nitriding treatment atmosphere may be 1 Pa or more and less than 100 Pa, and the total pressure may be atmospheric pressure or less, but when the gas constituting the atmosphere is a mixed gas of nitrogen gas and a gas other than nitrogen, the gas other than nitrogen is an inert gas such as argon or helium with a purity of 99.99% by volume or more.
[0046] If the nitrogen partial pressure while the titanium material is held at the holding temperature and the nitrogen partial pressure during cooling are less than 1 Pa, the diffusion of nitrogen in the atmosphere into the titanium material is insufficient, and the maximum concentration of nitrogen forming titanium nitride cannot be set to 2 to 10 atomic %. On the other hand, if the nitrogen partial pressure while the titanium material is held at the holding temperature and the nitrogen partial pressure during cooling are 100 Pa or more, the diffusion of nitrogen in the atmosphere into the titanium material becomes excessive, and the maximum concentration of nitrogen forming titanium nitride exceeds 10 atomic %. Therefore, the nitrogen partial pressure while the titanium material is held at the holding temperature and the nitrogen partial pressure during cooling are each set to 1 Pa or more and less than 100 Pa.
[0047] If the holding temperature is less than 600°C, the reaction of the oxygen present in the atmosphere in trace amounts will be dominant, resulting in insufficient diffusion of nitrogen in the atmosphere, and the maximum concentration of nitrogen forming titanium nitride will not be 2 to 10 atomic %. On the other hand, if the holding temperature is more than 800°C, the diffusion of nitrogen in the atmosphere into the titanium material will be excessive, resulting in the maximum concentration of nitrogen forming titanium nitride exceeding 10 atomic %. Therefore, the holding temperature is set to 600°C or higher and 800°C or lower.
[0048] If the holding time, which is the time during which the titanium material is held at the holding temperature, is less than 1 minute, the diffusion of nitrogen in the atmosphere into the titanium material is insufficient, and the maximum concentration of nitrogen forming titanium nitride cannot be set to 2 to 10 atomic %. On the other hand, if the holding time exceeds 5 hours, the diffusion of nitrogen in the atmosphere into the titanium material becomes excessive, and the maximum concentration of nitrogen forming titanium nitride exceeds 10 atomic %. Therefore, the holding time is set to be 1 minute or more and 5 hours or less.
[0049] The atmosphere during heating to the holding temperature has a nitrogen partial pressure of 1 Pa or more and less than 100 Pa. The atmosphere during heating to the holding temperature is preferably the same as the atmosphere during holding the titanium material at the holding temperature, since this makes it easier to control the atmosphere.
[0050] The cooling rate is not particularly limited, but can be, for example, 1 to 50° C. / min. The cooling rate is preferably 10° C. / min or more, and more preferably 20° C. / min or more, so as to prevent excessive diffusion of nitrogen in the atmosphere into the titanium material. The cooling rate can be controlled by introducing an atmosphere.
[0051] Cooling in an atmosphere with a nitrogen partial pressure of 1 Pa or more and less than 100 Pa may be carried out, for example, until the titanium material reaches room temperature, or the titanium material may be cooled in the above atmosphere to 100° C. and then replaced with air.
[0052] [Condition (ii)] In condition (ii), the titanium material is held at a temperature of 250° C. or more and 600° C. or less for 40 seconds or more and 5 minutes or less in an air atmosphere, and then cooled in the air atmosphere.
[0053] The atmosphere contains a lot of oxygen and nitrogen. Titanium bonds more strongly with oxygen than nitrogen, and the lower the temperature, the more pronounced this tendency is. For this reason, the holding temperature is set to 250°C or higher to diffuse the nitrogen in the atmosphere and achieve a maximum nitrogen concentration of 2-10 atomic percent. On the other hand, if the holding temperature is too high, not only will the nitrogen diffuse excessively, but a thick oxide scale will form, marring the aesthetic appearance. For this reason, the holding temperature is set to 600°C or lower.
[0054] If the holding time, which is the time during which the titanium material is held at the holding temperature, is less than 40 seconds, the diffusion of nitrogen in the atmosphere into the titanium material is insufficient, and the maximum concentration of nitrogen forming titanium nitride cannot be set to 2 to 10 atomic %. On the other hand, if the holding time exceeds 5 minutes, the diffusion of nitrogen in the atmosphere into the titanium material becomes excessive, and the maximum concentration of nitrogen forming titanium nitride exceeds 10 atomic %. Therefore, the holding time is set to be 40 seconds or more and 5 minutes or less.
[0055] The atmosphere during which the titanium material is held at the holding temperature is an air atmosphere. If the atmosphere during which the titanium material is held at the holding temperature is an air atmosphere, the saturation of the titanium material after anodization can be further increased. The reason for this is not necessarily clear, but the inventors speculate that the nitrogen that penetrates due to the air oxidation and the thin oxide film formed on the surface reduce the rate at which oxygen atoms penetrate into the titanium material during anodization, and promote the crystallization of titanium oxide starting from titanium nitride, thereby improving the degree of orientation integration of titanium oxide. In addition, if the atmosphere is an air atmosphere, there is no need to control the atmosphere, so the manufacturing equipment can be simplified and the manufacturing cost can be reduced.
[0056] The atmosphere during heating to the holding temperature is preferably at atmospheric pressure.
[0057] The atmosphere during cooling is air. Since the titanium material is cooled in air, there is no need to control the atmosphere, the manufacturing equipment can be simplified, and the manufacturing cost can be reduced.
[0058] [Condition (iii)] In condition (iii), a titanium material is maintained at a temperature of 200°C or higher in a vacuum atmosphere, and after that, when the temperature of the titanium material reaches any temperature between 200°C or higher and 500°C or lower, pure nitrogen gas is blown onto the titanium material to cool it; alternatively, a titanium material is maintained at a temperature of 300°C or higher in a vacuum atmosphere, and after that, when the temperature of the titanium material reaches any temperature between 300°C and 800°C from the maintained temperature, air is blown onto the titanium material to cool it.
[0059] In condition (iii), when the titanium material is cooled by blowing pure nitrogen gas onto it in the cooling process after the holding, the titanium material is held at a temperature of 200°C or higher in a vacuum atmosphere. If the holding temperature in the vacuum atmosphere is less than 200°C, the diffusion of nitrogen is insufficient, and the maximum concentration of nitrogen forming titanium nitride cannot be set to 2 to 10 atomic %. Therefore, if pure nitrogen gas is blown onto the titanium material in the cooling process after the holding, the holding temperature in the vacuum atmosphere is 200°C or higher. However, if the titanium material is cooled by blowing air onto the titanium material after the holding, the holding temperature in the vacuum atmosphere is 300°C or higher. If the holding temperature in the vacuum atmosphere is less than 300°C when the titanium material is cooled by blowing air onto the titanium material after the holding, the diffusion of nitrogen is insufficient, so the holding temperature in the vacuum atmosphere is 300°C or higher. The upper limit of the temperature maintained in the vacuum atmosphere is not particularly limited, and the temperature maintained in the vacuum atmosphere is, for example, 800° C. or lower.
[0060] The atmosphere during heating up to the holding temperature is a vacuum atmosphere.
[0061] In condition (iii), since nitrogen penetrates into the titanium material from the atmosphere during cooling, there is no particular limit to the holding time of the titanium material, but from the viewpoint of uniform surface temperature, it is preferable to ensure a holding time of at least 1 minute. However, if no temperature distribution occurs in the titanium material, it is not necessary to hold the titanium material at the temperature after heating, and the titanium material may be cooled after being heated to the above temperature. In addition, it is preferable that the holding time at the temperature after heating is 5 hours or less, because there is a concern that the crystal grains will become too coarse and the aesthetic appearance will be impaired, but the holding time may be more than 5 hours if the purpose is to form coarse crystal grains.
[0062] In condition (iii), when the titanium material is held at a temperature of 200°C or higher in a vacuum atmosphere, and once the temperature of the titanium material reaches any temperature between 200°C or higher and 500°C or lower after the holding, pure nitrogen gas is blown onto the titanium material to cool it, or when the titanium material is held at a temperature of 300°C or higher in a vacuum atmosphere, and once the temperature of the titanium material reaches any temperature between 300°C or higher and less than 800°C after the holding, air is blown onto the titanium material to cool it. By cooling in this manner, nitrogen is diffused into the surface layer of the titanium material, and titanium nitride can be formed.
[0063] The cooling rate and the method for controlling the cooling rate are not particularly limited, and can be the same as in the case of condition (i) or condition (ii).
[0064] The vacuum atmosphere referred to here is a vacuum degree of 10 -1 Pa (approx. 10 -3 The term "pure nitrogen gas" used here refers to a nitrogen gas atmosphere with a purity of 99.99% by volume or higher.
[0065] The titanium material to be subjected to the nitriding process may be manufactured by a known method. For example, a pure titanium or titanium alloy ingot having the above-mentioned composition is produced by various melting methods such as a vacuum arc melting method, an electron beam melting method, a hearth melting method such as a plasma melting method, etc., using sponge titanium or a mother alloy for adding alloy elements as a raw material. Next, the obtained ingot is divided and hot forged as necessary to form a slab. The slab is then hot rolled to form a hot-rolled coil of pure titanium or titanium alloy having the above-mentioned composition. The hot-rolled coil is cold rolled, and the titanium material after cold rolling is subjected to the nitriding process. The slab may be subjected to pretreatment such as polishing and cutting as necessary. When the slab is formed into a rectangular shape suitable for hot rolling by the hearth melting method, it may be subjected to hot rolling without blooming, hot forging, etc. The cold rolling conditions are not particularly limited, and the slab may be rolled under conditions that provide the desired thickness, characteristics, etc.
[0066] (Anodizing process) In this step, the titanium material after the nitriding step is anodized. The electrolytic solution is not particularly limited, and may be, for example, an aqueous solution of an inorganic acid or an aqueous solution of an organic acid. Examples of inorganic acids include phosphoric acid, sulfuric acid, nitric acid, and hydrochloric acid. Examples of organic acids include oxalic acid, formic acid, citric acid, and trichloroacetic acid. One of these may be used alone or two or more may be used in combination. The electrolytic solution is preferably sulfuric acid or phosphoric acid in view of the vividness of the color. The concentration of the inorganic acid in the electrolytic solution is not particularly limited, and may be, for example, 0.1 to 5.0 mass%.
[0067] The temperature of the electrolytic solution is preferably 5 to 30° C. If the temperature of the electrolytic solution is 5 to 30° C., it becomes relatively easy to control the thickness of the oxide film.
[0068] The applied voltage can be selected arbitrarily to obtain the desired color. In the conventional manufacturing method of color-developing material, when the applied voltage is less than 50V, a titanium material with high chroma is obtained, but when the applied voltage is more than 50V, the titanium material with low chroma is often obtained. On the other hand, in the manufacturing method of titanium material according to the present embodiment, by carrying out the above-mentioned nitriding process, a titanium material with high chroma can be obtained even if the applied voltage is 50V or more. Therefore, the applied voltage can be selected arbitrarily. There is no particular upper limit on the applied voltage, but considering that the appearance is impaired by insulation breakdown, the applied voltage is preferably 130V or less.
[0069] The voltage application time, which is the time for which the voltage is maintained after being increased to a predetermined voltage after application of the voltage, is not particularly limited, and can be, for example, 10 to 600 seconds.
[0070] The current density is set to 1mA / cm from the viewpoints of insulation breakdown, color unevenness, and color development. 2 More than 20mA / cm 2 However, if no dielectric breakdown or color unevenness occurs, the current density is preferably 20 mA / cm 2 It may be more than 40mA / cm 2 If color development is possible, the current density may be 1 mA / cm 2 It may be less than 0.1 mA / cm 2 The current density is a value obtained by dividing the electrolytic current by the area of the surface of the titanium material to be anodized.
[0071] The method for producing a titanium material according to this embodiment has been described above. After anodization, the titanium material may be subjected to a cleaning process using a known method. EXAMPLES
[0072] Hereinafter, the embodiment of the present invention will be described in detail with reference to examples. Note that the examples shown below are merely examples of the present invention, and the present invention is not limited to the following examples.
[0073] The slab was hot rolled and then descaled to produce a hot rolled plate with a thickness of 5 mm. This hot rolled plate was then cold rolled to a thickness of 1 mm to produce a number of titanium materials for use as test materials. The composition of each test material obtained is shown in Table 1. The test materials obtained were equivalent to JIS Class 1 to 4 pure titanium in accordance with JIS H 4600:2012.
[0074] [Table 1]
[0075] The test materials were subjected to nitriding treatment under the conditions shown in Tables 2 and 3. The cooling rate differed depending on the cooling conditions, and was 1 to 3600° C. / min on average. The spraying start temperature in Tables 2 and 3 is the temperature at which spraying of pure nitrogen gas or air began to be started on the test material while the test material was cooling after the test material had been held for the holding time specified in Tables 2 and 3 in the holding atmosphere and holding temperature specified in Tables 2 and 3. In Inventive Example 9, pure nitrogen gas was sprayed onto the test material once the temperature of the test material reached 500°C. In Inventive Example 10, pure nitrogen gas was sprayed onto the test material once the temperature of the test material reached 200°C. In Inventive Examples 11 and 17, immediately after the test material was held in the holding atmosphere, for the holding time and at the holding temperature shown in Table 2, air was started to be blown onto the test material. In Inventive Example 12, air was started to be blown onto the test material when the temperature of the test material reached 500°C. In Inventive Example 13, air was started to be blown onto the test material when the temperature of the test material reached 300°C. In Inventive Example 18, pure nitrogen gas was sprayed onto the test material immediately after the test material was held in the holding atmosphere, for the holding time and at the holding temperature shown in Table 2. In Comparative Examples 7 and 9, pure nitrogen gas was sprayed onto the test material immediately after the test material was held in the holding atmosphere, holding time and holding temperature shown in Table 3. In Comparative Examples 10 and 11, immediately after the test material was held in the holding atmosphere, holding time and holding temperature shown in Table 3, air was started to be blown onto the test material. In Examples 1 to 5, 14 to 16 and Comparative Examples 1, 4, 6 and 8, only the nitrogen partial pressure is recorded for the holding atmosphere and the cooling atmosphere, but the gas constituting the atmosphere in the furnace was a mixed gas of nitrogen and Ar with a purity of 99.99% by volume or more. In Examples 1 to 5, 14 to 16 and Comparative Examples 1, 4, 6 and 8, the cooling atmosphere shown in Tables 2 and 3 was maintained until the temperature of the test material reached room temperature.
[0076] The maximum concentration of nitrogen forming titanium nitride was measured by XPS using the following method. Specifically, the analysis conditions were: X-ray source: mono-AlKα (hν: 1486.6 eV), beam diameter: 200 μmΦ (≒ analysis area), take-in angle: 45°, sputtering conditions: Ar + The sputtering rate was 4.3 nm / min. (SiO2 equivalent value). The peaks appearing at binding energies of about 393 to 408 eV were determined as N1s peaks, the peaks appearing at about 399 to 401 eV were determined as N derived from organic matter, and the peaks appearing at about 397 ± 1 eV were determined as N derived from titanium nitride. The peaks appearing at binding energies of about 280 to 395 eV were determined as C1s peaks, the peaks appearing at about 284 to 289 eV were determined as C derived from organic matter, and the peaks appearing at about 281.5 ± 1 eV were determined as C derived from carbides. The peaks appearing at binding energies of about 525 to 540 eV were determined as O1s peaks, the peaks appearing at about 399 to 401 eV were determined as O derived from organic matter, and the peaks appearing at about 529.5 to 530.5 eV were determined as O derived from metal oxides. The peak appearing at a binding energy of 450-470 eV was determined to be the Ti2p peak. The spectrum peak appearing at a binding energy of 700-720 eV was determined to be the Fe2p peak, the peak appearing at 706.9 eV was determined to be due to Fe simple substance, the peak appearing at 708.1 eV was determined to be due to Fe carbide, and the peak appearing at 709.6-710.9 eV was determined to be due to Fe oxide. Changes in binding energy due to electrostatic charge of the measured sample were corrected based on the peak position of the C-C bond in C derived from organic matter.
[0077] Using the analysis software SpecSurf (Analysis), the concentration was analyzed based on these peaks. Specifically, the background was corrected based on the Shirley method. Next, the peaks of each element were fitted by chemical state using the Gauss-Lorents function for compounds and the Asymmetric function for metals. The concentration (atomic %) of each chemical state was calculated by multiplying the area ratio of the peak from each chemical state by the concentration (atomic %) of the element. The concentration of the above elements was calculated by calculating the peak area including all peaks related to the element (without separating them) for each element detected by XPS, and dividing it by the sensitivity coefficient for each element to obtain a percentage.
[0078] The thickness of the oxide film was determined from the surface of the titanium material after the nitriding process to a position where the oxygen concentration measured by XPS was the intermediate concentration between the maximum concentration and the base concentration.
[0079] Tables 2 and 3 show the maximum nitrogen concentration of the titanium material after the nitriding process, the presence or absence of titanium nitride, and the oxide film thickness.
[0080] [Table 2]
[0081] [Table 3]
[0082] The titanium material after the nitriding process was subjected to anodizing. The applied voltage, application time, and electrolytic solution used are shown in Table 3. The temperature of the electrolytic solution was 20°C, and the electrolytic current density was 4mA / cm. 2 It was.
[0083] The oxide film thickness of the titanium material after the anodizing process, the presence or absence of titanium nitride in the titanium substrate, the maximum nitrogen concentration in the titanium substrate, and the depth from the titanium material surface at which the maximum nitrogen concentration was observed are shown in Tables 4 and 5. The oxide film thickness, the maximum nitrogen concentration, and the depth from the titanium material surface at which the maximum nitrogen concentration was observed were calculated in the same manner as above.
[0084] Saturation C * The measurement of ab was carried out using a Minolta Co., Ltd. color difference meter CR-200b under light source C.
[0085] Saturation C * If ab is 20 or more, the color development is deemed to be good and the product is considered to pass. * When ab is less than 20, the color development is deemed to be poor and the sample is deemed to be unacceptable. * The evaluation results of ab are shown in Tables 4 and 5.
[0086] [Table 4]
[0087] [Table 5]
[0088] As shown in Tables 1 to 5, when the surface of the titanium substrate on which the oxide film was formed was analyzed by X-ray photoelectron spectroscopy, the maximum concentration of nitrogen forming titanium nitride was 2 to 10 atomic %. * a * b * Saturation C in the color system * When ab was 20 or more, the color development was excellent.
[0089] Although the preferred embodiment of the present invention has been described in detail above, the present invention is not limited to such an example. It is clear that a person having ordinary knowledge in the technical field to which the present invention pertains can conceive of various modified or amended examples within the scope of the technical ideas described in the claims, and it is understood that these also naturally fall within the technical scope of the present invention.
Claims
1. The surface of the titanium base material is provided with an anodized film. the titanium substrate comprises titanium nitride; when the surface of the titanium base material on which the anodized coating is disposed is analyzed by X-ray photoelectron spectroscopy, the maximum concentration of nitrogen forming the titanium nitride is 2 to 10 atomic %; L * a * b * Saturation C in color system * ab is 20 or more, The thickness of the anodic oxide film is 80 nm or more.
2. 2. The titanium material according to claim 1, wherein the position at which the nitrogen forming the titanium nitride has a maximum concentration is located within a range of up to 300 nm in the direction of the titanium substrate from the interface between the titanium substrate and the anodized film.
3. A method for producing a titanium material according to claim 1 or 2, comprising the steps of: A method for producing a titanium material, comprising the steps of: nitriding a titanium material under any one of the following conditions (i) to (iii) and then performing an anodizing process: Condition (i): In an atmosphere having a nitrogen partial pressure of 1 Pa or more and less than 100 Pa, the titanium material is held at a temperature of 600° C. or more and 800° C. or less for 1 minute to 5 hours, and then cooled in an atmosphere having a nitrogen partial pressure of 1 Pa or more and less than 100 Pa. Condition (ii) The titanium material is held at a temperature of 250° C. or more and 600° C. or less for 40 seconds or more and 5 minutes or less in an air atmosphere, and then cooled in the air atmosphere. Condition (iii) In a vacuum atmosphere, the titanium material is maintained at a temperature of 200°C or higher, and, after the temperature is maintained, when the temperature of the titanium material reaches any temperature between 200°C or higher and 500°C or lower, pure nitrogen gas is blown onto the titanium material to cool it; or, in a vacuum atmosphere, the titanium material is maintained at a temperature of 300°C or higher, and, after the temperature is maintained, when the temperature of the titanium material reaches any temperature between 300°C or higher and less than 800°C, air is blown onto the titanium material to cool it.
Citation Information
Patent Citations
Titanium material or titanium alloy material allowed to develop color by anodic oxidation and having high lightness and low saturation color tone
JP1996049095A
Method for coloring metallic titanium
JP1997263929A
Production method for anatase type titanium oxide film by anodic electrolytic oxidation treatment
JP2005240139A
Method for forming oxide film
JP2005320623A
Method for manufacturing titanium material having highly abrasion-resistant film with interference color
JP2006063406A