Recycled carbon fiber reinforced polyolefin composition and its uses

The recycled carbon fiber-reinforced polyolefin composition addresses the adhesion and dispersion issues of recycled fibers by using modified polyolefin with a carbodiimide group, achieving comparable mechanical strength to virgin fibers and reducing costs.

JP7581481B2Active Publication Date: 2024-11-12MITSUI CHEMICALS INC
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2023505271
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-03-09
Filing Date
2022-02-22
Publication Date
2024-11-12
Estimated Expiration
2042-02-22

AI Technical Summary

Technical Problem

Recycled carbon fibers from used CFRP materials exhibit poor adhesion and dispersion due to thermal decomposition of sizing agents, leading to insufficient mechanical properties in polyolefin composites, making them unsuitable as a cost-effective alternative to virgin carbon fibers.

Method used

A recycled carbon fiber-reinforced polyolefin composition is developed using modified polyolefin containing a group that reacts with a carbodiimide group, combined with recycled carbon fibers, to enhance adhesion and dispersion, achieving mechanical strength comparable to virgin carbon fiber composites.

Benefits of technology

The composition achieves mechanical strength comparable to virgin carbon fiber composites, reducing costs and environmental impact while maintaining high mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581481000001
    Figure 0007581481000001
  • Figure 0007581481000002
    Figure 0007581481000002
Patent Text Reader

Abstract

The purpose of the present invention is to obtain: a recycled carbon fiber-reinforced polyolefin composition which contains recycled carbon fibers and still has a mechanical strength that is just as good as the mechanical strength of a composition which contains unused carbon fibers; and a molded body of this recycled carbon fiber-reinforced polyolefin composition. The present invention relates to a recycled carbon fiber-reinforced polyolefin composition which contains from 0.01 part by mass to 50 parts by mass of (A) a modified polyolefin, from 50 parts by mass to 99 parts by mass of (B) a polyolefin, and from 1 part by mass to 80 parts by mass of (C) recycled carbon fibers (provided that the total of the components (A), (B) and (C) is 100 parts by mass), wherein the modified polyolefin (A) is obtained by reacting (D) a modified polyolefin having a group that is reactive with a carbodiimide group and (E) a carbodiimide group-containing compound with each other.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a recycled carbon fiber reinforced polyolefin composition containing recycled carbon fibers that has mechanical strength comparable to that of a composition containing virgin carbon fibers, and uses thereof. [Background technology]

[0002] Polyolefins (olefin polymers) such as polypropylene and polyethylene are molded by various methods and are used in a wide range of applications. However, polyolefins such as polypropylene are inferior in mechanical properties such as heat resistance, rigidity, and tensile strength compared to engineering plastics (engineering plastics) such as polyamide and polycarbonate, so inorganic fillers such as talc, and heat-resistant fibers such as glass fiber and carbon fiber are mixed (added) as reinforcing materials depending on the application.

[0003] However, in many cases, the reinforcing effect of the reinforcing material is insufficient due to insufficient dispersion of the reinforcing material or poor adhesion between the reinforcing material and the polyolefin. It is known that the mechanical properties of the resulting molded article can be improved by improving the adhesion between the reinforcing material and the polyolefin by adding maleic anhydride-modified polypropylene or the like as a method for improving the adhesion between the polyolefin and the reinforcing material.

[0004] For example, Patent Document 1 discloses a carbon fiber resin composition in which carbon fibers treated with a sizing agent are treated with maleic anhydride modified polypropylene. Patent Document 2 discloses a carbon fiber resin composition in which the adhesive compound is delocalized at the carbon fiber interface to control the ratio of the adhesive compound around the carbon fibers, thereby improving impact resistance.

[0005] In recent years, carbon fiber reinforced plastics (CFRP) containing carbon fibers have been used in parts for aircraft, automobiles, etc. because of their high strength, high rigidity, and the advantage of being lightweight. On the other hand, since carbon fibers are expensive, a method has been proposed in which carbon fibers contained in used CFRP are extracted to produce recycled carbon fibers (for example, Patent Document 3).

[0006] If a carbon fiber composite material having high strength and elasticity could be produced using inexpensive recycled carbon fibers instead of expensive virgin carbon fibers (hereinafter referred to as "carbon fibers"), it would be preferable from the viewpoint of economic efficiency and reducing the burden on the environment. However, in the case of recycled carbon fibers produced from used CFRP, the sizing agent attached to the surface is generally pyrolyzed compared to virgin carbon fibers due to the influence of the manufacturing process, resulting in carbon fibers with an extremely small amount of functional groups on the fiber surface. Therefore, simply adding an acid-modified polyolefin, which is a general compatibilizer, as a compatibilizer results in poor adhesion to the carbon fiber surface, resulting in poor compatibility between the carbon fibers and the matrix resin, poor dispersion of the carbon fibers, and a problem in which a molded product having sufficient mechanical properties cannot be obtained. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2003-277525 A [Patent Document 2] JP 2015-110749 A [Patent Document 3] JP 2017-82037 A Summary of the Invention [Problem to be solved by the invention]

[0008] An object of the present invention is to obtain a recycled carbon fiber reinforced polyolefin composition containing recycled carbon fibers that has mechanical strength comparable to that of a composition containing virgin carbon fibers, and a molded article thereof. [Means for solving the problem]

[0009] The present invention relates to a recycled carbon fiber reinforced polyolefin composition comprising 0.01 to 50 parts by mass of modified polyolefin (A), 50 to 99 parts by mass of polyolefin (B), and 1 to 80 parts by mass of recycled carbon fiber (C) (wherein the total of (A), (B), and (C) is 100 parts by mass), The present invention relates to a recycled carbon fiber-reinforced polyolefin composition, in which the modified polyolefin (A) is a modified polyolefin obtained by reacting a modified polyolefin (D) having a group reactive with a carbodiimide group with a carbodiimide group-containing compound (E). Effect of the Invention

[0010] The recycled carbon fiber reinforced polyolefin composition of the present invention has mechanical strength comparable to that of a composition containing virgin carbon fiber, and therefore can be used as a raw material for a molded article in which a composition containing virgin carbon fiber is used, thereby reducing costs. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] <Modified polyolefin (D) having a group reactive with a carbodiimide group> The modified polyolefin (D) having a group reactive with a carbodiimide group according to the present invention (hereinafter, may be referred to as "modified polyolefin (D)") is a modified polyolefin in which a compound (d) having a group reactive with a carbodiimide group (hereinafter, may be referred to as "compound (d)") has been introduced into a polyolefin.

[0012] The modified polyolefin (D) according to the present invention has a compound (d) content in the range of usually 0.1 to 10 mass %, preferably 0.1 to 3.0 mass %, and more preferably 0.1 to 2.0 mass %.

[0013] When the content of compound (d) exceeds the above range and becomes excessive, it may be difficult to produce a recycled carbon fiber-reinforced polyolefin composition because compound (d) is crosslinked by the carbodiimide group-containing compound (E) described below. On the other hand, when it is below the above range, although it is possible to produce a recycled carbon fiber-reinforced polyolefin composition, the bonding portion between the carbodiimide group-containing compound (E) that forms the backbone of the modified polyolefin (D) and the modified polyolefin (D) becomes small, so that the reinforcing property and dispersibility of the recycled carbon fiber in the recycled carbon fiber-reinforced polyolefin composition cannot be sufficiently improved.

[0014] In order to prevent crosslinking, it is preferable that the lower the number average molecular weight of the modified polyolefin (D) and the smaller the molar ratio of (the number of moles of compound (d)) / (the number of moles of modified polyolefin (D)). That is, when there is not a plurality of compound (d) but a state close to a single one on the molecular chain of the modified polyolefin (D), it means that when the carbodiimide group (N = C = N) of the carbodiimide group-containing compound (E) reacts with compound (d), it can be bonded without crosslinking or gelation.

[0015] In the present invention, by controlling the number average molecular weight (Mn) of the modified polyolefin (D) and the content of the compound (d), it is possible to prevent crosslinking from occurring in the production of the modified polyolefin (A) and the production stability from decreasing, and when a recycled carbon fiber-reinforced polyolefin composition is prepared using the modified polyolefin (A), the reinforcing property and dispersibility of the recycled carbon fiber can be sufficiently improved. That is, in the present invention, it is preferable that the modified polyolefin (D) satisfies the following formula (1).

[0016] 0.1 < Mn / [(100 - M)×f / M] < 6 Formula (1) (In the formula, f: Molecular weight of compound (d) (g / mol) M: Content of compound (d) (wt%) Mn: Number average molecular weight of the modified polyolefin (D).) Furthermore, from the viewpoint of production stability without crosslinking, it is more preferably in the range satisfying the following formula (2), and most preferably in the range satisfying formula (3).

[0017] 0.3 < Mn / [(100 - M)×f / M] < 6 Formula (2) 0.5 < Mn / [(100 - M)×f / M] < 6 Formula (3) When the relationship between the number average molecular weight (Mn) of the modified polyolefin (D) and the compound (d) is within the above range, when producing the modified polyolefin (A), it is possible to stably produce it without crosslinking.

[0018] In the present invention, when the modified polyolefin (D) is obtained by graft polymerization, if the polyolefin serving as the graft main chain is a polyolefin having a high ethylene content such as linear low-density polyethylene, it tends to be more easily crosslinked during production compared to a polyolefin having a high α-olefin copolymerization amount such as an ethylene-1-butene copolymer. Therefore, in order to use a polyolefin having a high ethylene content as the graft main chain and suppress crosslinking during production, it is preferable to adjust the compound (d) having a group reactive with the carbodiimide group to be present in a number close to a single number on the molecular chain of the modified polyolefin (D).

[0019] In addition, when the polyolefin serving as the graft main chain is a polyolefin that is easily degraded into low molecular weight by thermal decomposition such as polypropylene, the phenomenon of increased viscosity due to crosslinking hardly occurs. Therefore, when using a polyolefin that is easily thermally decomposed as the graft main chain, even if the compound (d) is plural on the molecular chain of the modified polyolefin (D), it may be possible to produce the modified polyolefin (A) without increasing the viscosity.

[0020] Incidentally, the number average molecular weight can be determined by general molecular weight measurement methods for polymers such as the GPC method, light scattering method, low-angle light scattering photometry method, vapor pressure osmometry method, and membrane osmometry method. The melt flow rate (MFR) of the modified polyolefin (D) according to the present invention is usually 0.01 to 500 g / 10 min, preferably 0.05 to 300 g / 10 min, at 230° C. under a load of 2.16 kg according to ASTM D1238. When it is within the above range, a modified polyolefin (A) excellent in improving the reinforcing property and dispersibility of the recycled carbon fibers (C) can be obtained.

[0021] The density of the modified polyolefin (D) is usually 0.8 to 1.1 g / cm 3 , preferably is 0.8~1.05g / cm 3 , more preferably 0.8 to 1.0 g / cm 3 It is. <Compound (d) Having a Group Reactive with a Carbodiimide Group> The compound (d) having a group reactive with a carbodiimide group according to the present invention (hereinafter, sometimes referred to as "compound (d)") includes a compound having a group having active hydrogen reactive with a carbodiimide group, specifically, a compound having a group derived from a carboxylic acid, an amine, an alcohol, a thiol, or the like. Among these, a compound having a group derived from a carboxylic acid is preferably used, and among these, an unsaturated carboxylic acid and / or a derivative thereof is particularly preferred. In addition to the compound having a group having an active hydrogen, a compound having a group that is easily converted into a group having active hydrogen by water or the like can also be preferably used, specifically, a compound having an epoxy group or a glycidyl group can be mentioned. In the present invention, the compound (d) may be used alone or in combination of two or more kinds.

[0022] When an unsaturated carboxylic acid and / or a derivative thereof is used as the compound (d) according to the present invention, examples of the compound include an unsaturated compound having one or more carboxylic acid groups, an unsaturated compound having one or more carboxylic acid anhydride groups, and a derivative thereof, and examples of the unsaturated group include a vinyl group, a vinylene group, and an unsaturated cyclic hydrocarbon group.

[0023] Specific examples of the derivatives include unsaturated carboxylic acids such as acrylic acid, methacrylic acid, maleic acid, fumaric acid, tetrahydrophthalic acid, itaconic acid, citraconic acid, crotonic acid, isocrotonic acid, norbornene dicarboxylic acid, and bicyclo[2,2,1]hept-2-ene-5,6-dicarboxylic acid, as well as acid anhydrides and derivatives thereof (e.g., acid halides, amides, imides, esters, etc.). Specific examples of the compound include malenyl chloride, malenylimide, maleic anhydride, itaconic anhydride, citraconic anhydride, tetrahydrophthalic anhydride, bicyclo[2,2,1]hept-2-ene-5,6-dicarboxylic anhydride, dimethyl maleate, monomethyl maleate, diethyl maleate, diethyl fumarate, dimethyl itaconate, diethyl citraconic acid, dimethyl tetrahydrophthalate, dimethyl bicyclo[2,2,1]hept-2-ene-5,6-dicarboxylate, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, glycidyl (meth)acrylate, aminoethyl methacrylate, and aminopropyl methacrylate.

[0024] When using an unsaturated carboxylic acid and / or its derivative as the compound (d) according to the present invention, one type may be used alone, or two or more types may be used in combination. Among these, maleic anhydride, (meth)acrylic acid, itaconic anhydride, citraconic anhydride, tetrahydrophthalic anhydride, bicyclo[2,2,1]hept-2-ene-5,6-dicarboxylic anhydride, hydroxyethyl (meth)acrylate, glycidyl methacrylate, and aminopropyl methacrylate are preferred. Furthermore, dicarboxylic anhydrides such as maleic anhydride, itaconic anhydride, citraconic anhydride, tetrahydrophthalic anhydride, and bicyclo[2,2,1]hept-2-ene-5,6-dicarboxylic anhydride are particularly preferred.

[0025] As a method for introducing the compound (d) according to the present invention into a polyolefin, a well-known method can be adopted, and examples thereof include a method of graft copolymerizing (graft modifying) the compound (d) onto the polyolefin main chain, and a method of radically copolymerizing an olefin with the compound (d).

[0026] The graft modification method and the radical copolymerization method will be specifically described below. Graft Modification The modified polyolefin (D) according to the present invention can be obtained by grafting a compound (d) onto a polyolefin.

[0027] (Polyolefin) The polyolefin to be graft-modified with the compound (d) is a polymer mainly composed of an olefin, such as a homopolymer of an α-olefin having 2 to 6 carbon atoms, a copolymer of the above α-olefin with another α-olefin (having 2 to 20 carbon atoms), or a copolymer of the above α-olefin with a monomer other than the α-olefin. Examples of the monomer other than the α-olefin include a cyclic olefin, a non-conjugated diene, a vinyl group-containing aromatic hydrocarbon, and a vinyl ester.

[0028] Specific examples of the polyolefin according to the present invention include ethylene-based polymers mainly composed of ethylene, such as ethylene homopolymers and copolymers of ethylene and an α-olefin having 3 or more carbon atoms (ethylene-α-olefin copolymers), propylene-based polymers mainly composed of propylene, such as propylene homopolymers and copolymers of propylene and ethylene and / or an α-olefin having 4 or more carbon atoms (polypropylene), 1-butene-based polymers mainly composed of 1-butene, such as 1-butene homopolymers and copolymers of 1-butene with ethylene, propylene and an α-olefin having 5 or more carbon atoms (poly-1-butene), and homopolymers of 4-methyl-1-pentene and copolymers of 4-methyl-1-pentene with other α-olefins (poly-4-methyl-1-pentene).

[0029] In addition, these polyolefins may have either an isotactic structure or a syndiotactic structure, and there is no particular restriction on the stereoregularity. The density of the polyolefin used for graft modification is usually 0.8 to 1.1 g / cm 3 , preferably 0.8 to 1.05 g / cm 3 , more preferably 0.8 to 1.0 g / cm 3 The melt flow rate (MFR) at 230°C under a load of 2.16 kg according to ASTM D 1238 is usually 0.01 to 500 g / 10 min, preferably 0.05 to 300 g / 10 min, and more preferably 0.1 to 100 g / 10 min. If the density and MFR are within this range, the density and MFR of the graft copolymer after modification will also be approximately the same, making it easy to handle.

[0030] The crystallinity of the polyolefin used for graft modification is usually 2% or more, preferably 5% or more, and more preferably 10% or more. If the crystallinity is in this range, the graft copolymer after modification is excellent in handleability.

[0031] The number average molecular weight (Mn) of the polyolefin used for graft modification, as measured by gel permeation chromatography (GPC), is preferably 5,000 to 500,000, and more preferably 10,000 to 100,000. If the number average molecular weight (Mn) is within this range, handling is excellent. The number average molecular weight is calculated in terms of polyethylene when the amount of other α-olefins copolymerized with ethylene is 10 mol % or less, and calculated in terms of ethylene-propylene (based on an ethylene content of 70 mol %) when the amount is 10 mol % or more. In addition, the number average molecular weight of polypropylene can be calculated based on the polypropylene equivalent if the amount of other α-olefins is 10 mol % or less, and based on the polypropylene equivalent if the amount of other α-olefins is 10 mol % or more. For example, it can be determined in terms of propylene-ethylene (based on a propylene content of 70 mol %).

[0032] Such polyolefins can be produced by any conventional method, for example, by polymerization using a titanium catalyst, a vanadium catalyst, a metallocene catalyst, etc. The polyolefins used for graft modification may be in the form of either a resin or an elastomer, and both isotactic and syndiotactic structures can be used, with no particular limitation on stereoregularity. Commercially available resins can also be used as they are.

[0033] (Method of Graft Modification) The compound (d) can be grafted onto the polyolefin by a known method, for example, by dissolving the polyolefin in an organic solvent, adding the compound (d) and a radical initiator to the obtained solution, and reacting at a temperature of preferably 60 to 350°C, more preferably 80 to 190°C, for preferably 0.5 to 15 hours, more preferably 1 to 10 hours.

[0034] Examples of organic solvents that dissolve polyolefins include aromatic hydrocarbon solvents such as benzene, toluene, and xylene, and aliphatic hydrocarbon solvents such as pentane, hexane, and heptane.

[0035] Another example of the graft modification method of polyolefin is a method in which a polyolefin is reacted with a compound (d) using a radical initiator in an extruder in the absence of a solvent, etc. In this case, the reaction temperature is usually higher than the melting point of the olefin polymer, for example, 100 to 350° C., and the reaction time is usually 0.5 to 10 minutes.

[0036] Examples of the radical initiator include known radical initiators such as dicumyl peroxide, di-t-butyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne-3,2,5-dimethyl-2,5-di(t-butylperoxy)hexane, and 1,4-bis(t-butylperoxyisopropyl)benzene. The radical initiator is preferably used in a ratio of 0.001 to 1 part by mass relative to 100 parts by mass of the olefin polymer before modification.

[0037] Radical copolymerization The modified polyolefin (D) according to the present invention can also be obtained by radical copolymerization of an olefin with a compound (d). The olefin may be the same as the olefin forming the polyolefin, and the compound (d) is also as described above.

[0038] The method for copolymerizing an olefin with a compound having a group reactive with a carbodiimide group is not particularly limited, and any conventionally known radical copolymerization method can be used. <Carbodiimide Group-Containing Compound (E)> The carbodiimide group-containing compound (E) according to the present invention is a polycarbodiimide having a repeating unit represented by the following general formula (4).

[0039] -N=C=N-R1- Formula (4) [In the formula, R1 represents a divalent organic group] The method for synthesizing the carbodiimide group-containing compound (E) according to the present invention is not particularly limited. For example, a polycarbodiimide can be synthesized by reacting an organic polyisocyanate in the presence of a catalyst that promotes the carbodiimidization reaction of an isocyanate group.

[0040] The carbodiimide group-containing compound (E) according to the present invention has a polystyrene-equivalent number average molecular weight (Mn) determined by gel permeation chromatography (GPC) of usually 400 to 500,000, preferably 1,000 to 10,000, and more preferably 1,500 to 4,000. When the number average molecular weight (Mn) is within this range, it is preferable because a modified polyolefin (A) having excellent effects of improving the reinforcing property and dispersibility of the recycled carbon fibers (C) can be obtained.

[0041] The carbodiimide group-containing compound (E) according to the present invention may contain a monocarbodiimide in a polycarbodiimide, and it is also possible to use a single carbodiimide group-containing compound or a mixture of a plurality of carbodiimide group-containing compounds.

[0042] It is also possible to use a commercially available carbodiimide group-containing compound as it is. Examples of commercially available carbodiimide group-containing compounds include Carbodilite HMV-15CA, LA1, and HMV-5CA-LC (all trade names) manufactured by Nisshinbo Industries, Inc.

[0043] The carbodiimide group content in the carbodiimide group-containing compound (E) and the resulting modified polyolefin (A) is 13 It can be measured by C-NMR, IR, titration, etc., and can be understood as the carbodiimide equivalent. 13 130 to 142 ppm for C-NMR and 2130 to 2140 cm for IR -1 It is possible to observe a peak at

[0044] 13 C-NMR measurement is carried out, for example, as follows. That is, 0.35 g of a sample is heated and dissolved in 2.0 ml of hexachlorobutadiene. After filtering this solution through a glass filter (G2), 0.5 ml of deuterated benzene is added and the solution is placed in an NMR tube with an inner diameter of 10 mm. Then, using a JEOL GX-500 NMR measurement device, the sample is heated to 120°C. 13 C-NMR measurement is performed. The number of measurements is set to 10,000 or more.

[0045] The IR measurement is carried out, for example, as follows. After preparing a heat-pressed sheet from the sample at 250°C for 3 minutes, the infrared absorption spectrum is measured by the transmission method using an infrared spectrophotometer (manufactured by JASCO, FT-IR 410 model). The measurement conditions are a resolution of 2 cm -1 The number of accumulations is 32.

[0046] <Modified polyolefin (A)> The modified polyolefin (A), which is one of the components contained in the recycled carbon fiber reinforced polyolefin composition of the present invention, is a modified polyolefin obtained by reacting the modified polyolefin (D) having a group reactive with the above-mentioned carbodiimide group with the above-mentioned carbodiimide group-containing compound (E).

[0047] The method for reacting the modified polyolefin (D) with the carbodiimide group-containing compound (E) can be, specifically, melt-kneading to obtain a melt modification, but is not limited to this method.

[0048] As a method for melt-modifying by melt kneading, for example, when melt-kneading a modified polyolefin (D) having a group reactive with a carbodiimide group and a carbodiimide group-containing compound (E), the modified polyolefin (D) and the carbodiimide group-containing compound (E) are mixed simultaneously or successively using, for example, a Henschel mixer, a V-type blender, a tumbler blender, a ribbon blender, etc., or are not mixed, and are fed into a kneading device such as a single-screw extruder, a multi-screw extruder, a kneader, a Banbury mixer, etc., and melt-kneaded to obtain the modified polyolefin (A) in which the modified polyolefin (D) and the carbodiimide group-containing compound (E) are more uniformly dispersed and reacted, and thus the modified polyolefin (A) can be obtained.

[0049] The modified polyolefin (D) and the carbodiimide group-containing compound (E) can be mixed in advance and then fed from the inlet of the kneading device, or a portion of the components can be fed from the inlet and the other components can be fed from a feed port installed anywhere between the vicinity of the inlet and the tip of the extruder.

[0050] The temperature at which the modified polyolefin (D) and the carbodiimide group-containing compound (E) are melt-kneaded can be equal to or higher than the highest melting point of each of the components to be mixed. Specifically, the melt-kneading is usually performed at a temperature in the range of 150 to 300°C, preferably 200 to 280°C, and more preferably 230 to 270°C.

[0051] The modified polyolefin (A) according to the present invention has excellent fluidity at 230° C. The melt flow rate (MFR) of the modified polyolefin (A) at 230° C. under a load of 2.16 kg is usually in the range of 0.01 to 400 g / 10 min, preferably 0.1 to 300 g / 10 min, and more preferably 1 to 200 g / 10 min. If it is in such a range, the reinforcing property and dispersibility of the filler are excellent, which is preferable.

[0052] In producing the modified polyolefin (A) according to the present invention, it is preferable to set the ratio of the number of moles of the compound (d) having a group reactive with a carbodiimide group in the modified polyolefin (D) to the number of moles of the carbodiimide group-containing compound (E) so as to satisfy the following formula, since this provides a modified polyolefin (A) having high reaction efficiency between the compound (d) and the carbodiimide group-containing compound (E) and excellent fluidity.

[0053] The number of moles of (d):the number of moles of (E)=1:0.2-1.6, preferably 1:0.4-1.3, and more preferably 1:0.7-1.1. The amount of the carbodiimide group-containing compound (E) is usually 1 to 200 mmol, preferably 2 to 150 mmol, and more preferably 4 to 100 mmol, of the carbodiimide group per 100 grams of the modified polyolefin (A) obtained by reacting the modified polyolefin (D) with the carbodiimide group-containing compound (E). If the carbodiimide group content is too low, the reinforcing effect and dispersibility of the recycled carbon fibers (C) cannot be expressed, and if the content is too high, the molding processability of the resulting recycled carbon fiber-reinforced polyolefin composition decreases, and the reinforcing effect and dispersibility of the recycled carbon fibers (C) are not significantly improved, making it uneconomical.

[0054] Furthermore, in the modified polyolefin (A) according to the present invention, it is important to control the reaction between the compound (d) in the modified polyolefin (D) and the carbodiimide group in the carbodiimide group-containing compound (E). The progress of the reaction between the compound (d) in the modified polyolefin (D) and the carbodiimide group-containing compound (E) can be investigated, for example, by the following method.

[0055] After preparing heat-pressed sheets of the modified polyolefin (D) and the modified polyolefin (A) obtained by reacting the modified polyolefin (D) with the carbodiimide group-containing compound (E), respectively, infrared absorption was measured using an infrared absorption analyzer. From the obtained chart, the absorption bands due to the peak intensities of the compound (d) having a group reactive with the carbodiimide group in the modified polyolefin (D) and the modified polyolefin (A) (1790 cm when maleic anhydride is used) were identified. -1 The absorbance of the compound (E) before and after the reaction with the carbodiimide group-containing compound (A) is compared, and the reaction rate can be calculated using the following formula.

[0056] Response rate (%) = (X / Y) x 100 X = difference in strength between the carbodiimide group and the reactive group (before reaction (D) - after reaction (A)) Y = strength of the group reacting with the carbodiimide group of (D) before reaction The reaction rate of the modified polyolefin (A) according to the present invention, as determined by the above method, is usually in the range of 40 to 100%, preferably 50 to 100%, and more preferably 60 to 100%.

[0057] Some of the carbodiimide groups are converted to urea groups by absorbing water, and the urea groups are further thermally decomposed to generate amino groups. However, even the urea groups and amino groups are highly reactive with the modified polyolefin (D) and the like. Therefore, the recycled carbon fiber reinforced polyolefin composition of the present invention may contain polyolefins in which some of the carbodiimide groups have been converted to urea groups or amino groups by, for example, water in the air, which is one of the preferred embodiments of the present invention.

[0058] The modified polyolefin (A) according to the present invention is produced by reacting the carbodiimide group (N=C=N) of the carbodiimide group-containing compound (E) with the compound (d) having a group reactive with the carbodiimide group as described above. During the reaction, a certain amount of the carbodiimide group is consumed, and the residue of the carbodiimide group connected to the polyolefin as the same molecular chain interacts with the filler, contributing to reinforcement and dispersibility. The amount of the carbodiimide residue is measured by IR measurement at 2130 to 2140 cm. -1 This is due to the contraction vibration of the N=C=N group in the molecule and can be seen as the size of the peak.

[0059] The modified polyolefin (A) according to the present invention may contain two or more modified polyolefins (D) having groups reactive with carbodiimide groups, and may contain two or more carbodiimide group-containing compounds (E).

[0060] <Polyolefin (B)> Polyolefin (B), one of the components contained in the recycled carbon fiber reinforced polyolefin composition of the present invention, is a polymer mainly composed of olefins, such as homopolymers of α-olefins having 2 to 6 carbon atoms in the same category as the polyolefins used to obtain the modified polyolefin (D) of the present invention, copolymers of the above-mentioned α-olefins with other α-olefins (having 2 to 20 carbon atoms), and copolymers of the above-mentioned α-olefins with monomers other than α-olefins. Examples of monomers other than α-olefins include cyclic olefins, non-conjugated dienes, vinyl group-containing aromatic hydrocarbons, and vinyl esters.

[0061] Specific examples of the polyolefin (B) according to the present invention include ethylene-based polymers mainly composed of ethylene, such as ethylene homopolymers and copolymers of ethylene and an α-olefin having 3 or more carbon atoms (ethylene-α-olefin copolymers) [polyethylene: PE], propylene-based polymers mainly composed of propylene, such as propylene homopolymers and copolymers of propylene and ethylene and / or an α-olefin having 4 or more carbon atoms [polypropylene: PP], 1-butene-based polymers mainly composed of 1-butene, such as 1-butene homopolymers and copolymers of 1-butene with ethylene, propylene and an α-olefin having 5 or more carbon atoms [poly-1-butene: PB], and homopolymers of 4-methyl-1-pentene and copolymers of 4-methyl-1-pentene with other α-olefins [poly-4-methyl-1-pentene].

[0062] In addition, both isotactic and syndiotactic structures of these polyolefins (B) can be used, and there is no particular limitation on the stereoregularity. The density of the polyolefin (B) according to the present invention is usually 0.8 to 1.1 g / cm 3 , preferably 0.8 to 1.05 g / cm 3 , more preferably 0.8 to 1.0 g / cm 3The melt flow rate (MFR) at 230°C under a load of 2.16 kg according to ASTM D 1238 is usually 0.01 to 500 g / 10 min, preferably 0.05 to 300 g / 10 min, and more preferably 0.1 to 100 g / 10 min. If the density and MFR are within these ranges, the recycled carbon fiber reinforced polyolefin composition obtained by using the polyolefin (B) has good molding processability.

[0063] Among these polyolefins (B), polypropylene, which has excellent heat resistance and rigidity, is preferred. <Recycled Carbon Fiber (C)> The recycled carbon fiber (C), which is one of the components contained in the recycled carbon fiber reinforced polyolefin composition of the present invention, is a carbon fiber obtained by incinerating or treating with heated steam a waste carbon fiber reinforced plastic (CFRP). Usually, the carbon fiber used in CFRP is treated with a sizing agent, which is a measure to suppress the carbon fibers from becoming strands and to prevent the carbon fibers from scattering when dispersed in resin. In addition, the sizing agent improves compatibility with resin, so that the impact strength of CFRP is higher than that when untreated carbon fibers are used.

[0064] However, during the incineration or heated steam treatment process, the sizing agent is lost and the surface of the recycled carbon fiber remains in a pristine state, which means that it has poor dispersibility and compatibility with resin. As a result, recycled carbon fiber that could not be kneaded into the resin during extrusion processing accumulates at the tip of the extruder, making the strands unstable and creating problems with CFRP productivity. It is also difficult to obtain CFRP molded products with sufficient impact strength.

[0065] The recycled carbon fiber (C) according to the present invention is not particularly limited as long as it has an average fiber length in the range of 0.05 to 15.0 mm, and recycled carbon fibers obtained by incinerating or subjecting CFRP waste to heated steam treatment can be used. By having the average fiber length in this range, the flying Scatter The fibers are less likely to break during processing, and the reinforced polyolefin composition containing the recycled carbon fibers has good productivity for moldings, and the obtained moldings have excellent mechanical properties.

[0066] The recycled carbon fibers (C) according to the present invention preferably have an average fiber length of 0.1 to 5.0 mm. The fiber length of the recycled carbon fiber (C) can be calculated by observing the fiber length of 50 carbon fibers observed in a 100x magnification field using an optical microscope such as the "Digital Microscope VHX-100" (manufactured by Keyence Corporation) and averaging the fiber lengths of the 50 carbon fibers observed in the field.

[0067] Specific examples of the recycled carbon fiber (C) according to the present invention include the CARBISO MF series (average fiber length: 0.08 to 0.1 mm), CARBISO C series (average fiber length: 3 to 10 mm), and CARBISO CT series (average fiber length: 6 to 12 mm) manufactured by ELG Carbon Fiber Co., Ltd., and pyrolyzed products manufactured by Carbon Fiber Recycle Industry Co., Ltd.

[0068] Carbon fibers are usually treated with a surface sizing agent, and the surface oxygen concentration ratio (O / C), which is the ratio of the number of oxygen (O) and carbon (C) atoms on the fiber surface measured by X-ray photoelectron spectroscopy (XPS), is usually 0.05 or more. The higher the surface oxygen concentration ratio (O / C), the more functional groups there are on the carbon fiber surface, and the lower the surface oxygen concentration ratio (O / C), the fewer functional groups there are on the carbon fiber surface.

[0069] On the other hand, recycled carbon fiber (C) is incinerated or treated with heated steam, which causes even the surface sizing agent to be thermally decomposed. As a result, the amount of functional groups on the fiber surface is extremely small, and the surface oxygen concentration ratio (O / C) is a low value of less than 0.05.

[0070] The surface oxygen concentration ratio (O / C) of carbon fibers can be determined by X-ray photoelectron spectroscopy according to the following procedure. First, the carbon fibers are cut and spread out on a copper sample support. Then, the photoelectron escape angle is set to 90°, and an AlKα X-ray source is used. The sample chamber is filled with 1×10 -8Torr. The kinetic energy (KE) of the main C1S peak is adjusted to 969 eV to correct for peaks associated with charging during measurement. The C1S peak area is determined by drawing a straight baseline in the KE range of 958-972 eV. The O1S peak area is determined by drawing a straight baseline in the KE range of 714-726 eV. The surface oxygen concentration ratio (O / C) is calculated as an atomic ratio from the ratio of the O1S peak area to the C1S peak area using a sensitivity correction value specific to the device.

[0071] The means for controlling the surface oxygen concentration ratio (O / C) is not particularly limited, but may be, for example, electrolytic oxidation treatment, chemical oxidation treatment, or gas phase oxidation treatment, and among these, electrolytic oxidation treatment is preferred.

[0072] <Recycled carbon fiber reinforced polyolefin composition> The recycled carbon fiber reinforced polyolefin composition of the present invention is a recycled carbon fiber reinforced polyolefin composition containing 0.01 to 50 parts by mass, preferably 0.1 to 30 parts by mass, of the modified polyolefin (A), 50 to 99 parts by mass, preferably 60 to 90 parts by mass, of the polyolefin (B), and 1 to 80 parts by mass, preferably 5 to 50 parts by mass of the recycled carbon fiber (C) (wherein the total of (A), (B) and (C) is 100 parts by mass).

[0073] The content of the modified polyolefin (A) can be, for example, 4.5 to 50 parts by mass, 4.5 to 30 parts by mass, 5.5 to 30 parts by mass, 6.5 to 30 parts by mass, 7.5 to 30 parts by mass, 8.5 to 30 parts by mass, or 9.5 to 30 parts by mass. The content of the recycled carbon fibers (C) can be, for example, 10 to 80 parts by mass, 10 to 50 parts by mass, or 15 to 50 parts by mass.

[0074] The recycled carbon fiber reinforced polyolefin composition of the present invention contains modified polyolefin (A) in the above range, so that the dispersibility of polyolefin (B) and recycled carbon fiber (C) is good and the adhesion between recycled carbon fiber (C) and modified polyolefin (A) and polyolefin (B) is excellent, making it possible to obtain molded articles with excellent heat resistance and mechanical properties such as rigidity and impact strength. If the content of the recycled carbon fibers (C) is less than the above range, the effect of reinforcing the resin by the fibers cannot be obtained, whereas if the content exceeds the above range, toughness may be lost.

[0075] In the recycled carbon fiber reinforced polyolefin composition of the present invention, the content of carbodiimide groups contained in the polyolefin component in the recycled carbon fiber reinforced polyolefin resin composition is preferably 0.0001 to 140 mmol per 100 g of the polyolefin component, more preferably 0.01 to 10 mmol / 100 g.

[0076] When the content of the carbodiimide group is within the above range, the dispersibility of the filler can be improved, and the desired structure can be easily and economically produced. If the content of the carbodiimide group is too low, the dispersibility of the filler cannot be expressed, and if the content is too high, the molding processability decreases, and the effect of improving the dispersibility of the filler is not so high, making it uneconomical.

[0077] The recycled carbon fiber reinforced polyolefin composition of the present invention may contain known softeners, tackifiers, antioxidants, processing aids, adhesion promoters, heat stabilizers, weather stabilizers, antistatic agents, colorants, lubricants, flame retardants, anti-blooming agents, etc., as long as the object of the present invention is not impaired.

[0078] <Molded body> The recycled carbon fiber reinforced polyolefin composition of the present invention can be used to produce molded articles by various known molding methods, specifically injection molding, blow molding, press molding, calendar molding, extrusion molding, stamping molding, and the like.

[0079] The molded article made of the recycled carbon fiber reinforced polyolefin composition of the present invention is used in a wide range of applications from household goods to industrial goods. The molded article obtained by such a method includes electric parts, electronic parts, automobile parts, mechanical parts, food containers, films, sheets, fibers, etc., and more specifically, for example, office and office equipment such as printers, personal computers, word processors, keyboards, PDAs (personal digital assistants), telephones, facsimiles, copiers, ECRs (electronic cash registers), calculators, electronic organizers, electronic dictionaries, cards, holders, stationery, etc., home appliances such as washing machines, refrigerators, vacuum cleaners, microwave ovens, lighting equipment, game consoles, irons, kotatsu, etc., AV equipment such as TVs, VTRs, video cameras, radio cassette recorders, tape recorders, minidiscs, CD players, speakers, liquid crystal displays, etc., electrical and electronic parts and communication equipment such as connectors, relays, capacitors, switches, printed circuit boards, coil bobbins, semiconductor sealing materials, electric wires, cables, transformers, deflection yokes, distribution boards, clocks, etc.

[0080] Further examples include seats (padding, outer material, etc.), belts, ceiling coverings, convertible tops, armrests, door trims, rear package trays, carpets, mats, sun visors, wheel covers, tires, mattress covers, airbags, insulation materials, hanging handles, hanging handle straps, electric wire covering materials, electric insulation materials, paints, coating materials, upholstery materials, flooring materials, corner walls, deck panels, covers, plywood, ceiling boards, partition boards, side walls, carpets, wallpaper, wall covering materials, exterior materials, interior materials, roofing materials, soundproofing boards, heat insulating boards, window materials, and other automobile, vehicle, ship, aircraft, and building materials; clothing, curtains, sheets, plywood, synthetic fiber boards, rugs, entrance mats, sheets, buckets, hoses, containers, glasses, bags, cases, goggles, skis, rackets, tents, musical instruments, and other lifestyle and sporting goods. EXAMPLES

[0081] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the following description of the examples, "parts" refers to "parts by mass" unless otherwise specified. (Various measurement methods) In the present examples, measurements were carried out according to the following method. [Melt flow rate (MFR)] The MFR was measured at 230° C. under a load of 2.16 kg according to ASTM D1238.

[0082] [Number average molecular weight (Mn)] The number average molecular weight (Mn) was measured by GPC. Specifically, a gel permeation chromatograph Alliance GPC-2000 manufactured by Waters was used. The separation columns used were two TSKgel GMH6-HT and two TSKgel GMH6-HTL, each with a diameter of 7.5 mm and a length of 300 mm. The column temperature was set to 140°C, and the mobile phase was o-dichlorobenzene (Wako Pure Chemical Industries, Ltd.) containing 0.025% by weight of an antioxidant (butylhydroxytoluene, Takeda Pharmaceutical Co., Ltd.), moved at 1.0 mL / min. The sample concentration was 15 mg / 10 mL. Sample injection The volume was 500 microliters, and a differential refractometer was used as the detector.

[0083] Standard polystyrene has molecular weights of Mw<1000 and Mw>4×10 6 In the case of , the product manufactured by Tosoh Corporation is used, and 1000≦Mw≦4×10 6 In this case, a product manufactured by Pressure Chemical Co. was used.

[0084] In the case of maleic anhydride-modified polypropylene, Mn was calculated based on polypropylene. The modified polyolefins (A) used in the examples and comparative examples are shown below.

[0085] [Modified polyolefin (A)] CDI-PP1 was used as the modified polyolefin (A) produced by the following production method. <Production of Modified Polyolefin (A)> As the modified polyolefin (D), maleic anhydride modified polypropylene PP1 and Carbodilite HMV-15CA manufactured by Nisshinbo Chemical Co., Ltd. were prepared as the carbodiimide group-containing compound (E). PP1 was mixed with 4.4 parts by mass of HMV-15CA per 100 parts by mass, and the mixture was extruded using a twin-screw kneader (Kobe Steel KTX-30) at a cylinder temperature of 270°C, a screw rotation speed of 200 rpm, and a discharge rate of 10 kg / h to obtain CDI-PP1 as the modified polyolefin (A). The carbodiimide group content of the obtained CDI-PP1 was 10.7 mmol / 100 g. The carbodiimide group content was determined by measuring the infrared absorption spectrum by a transmission method using an infrared spectrophotometer (Japan Spectroscopy, FT-IR 410 type) after preparing a heat press sheet from the sample at 250°C for 3 minutes. The measurement conditions were a resolution of 2 cm -1 The number of integration times was set to 32.

[0086] [Modified polyolefin (D)] Maleic anhydride-modified polypropylene PP1 (D-1) was used as modified polyolefin (D). The maleic anhydride content of PP1 was 0.6 mass%, the number average molecular weight Mn determined by GPC was 50,180, and Mn / [(100-M)×f / M] was 3.1.

[0087] [Carbodiimide group-containing compound (E)] As the carbodiimide group-containing compound (E), Carbodilite HMV-15CA (E-1) (trade name, manufactured by Nisshinbo Chemical Inc.) having a carbodiimide equivalent of 262 g / mol was used.

[0088] [Polyolefin (B)] As the polyolefin (B), a homopolypropylene PP2 (J106G, manufactured by Prime Polymer Co., Ltd.) MFR (230° C.): 15 g / 10 min) (B-1) was used.

[0089] [Recycled carbon fiber (C)] As the recycled carbon fiber (C), recycled carbon fiber CF1 (first heating, 3 mm classification and cutting product, fiber surface oxygen concentration ratio O / C = 0.03) (C-1) manufactured by Carbon Fiber Recycle Industry Co., Ltd. was used.

[0090] Example 1 5 parts by mass of the above CDI-PP1 as modified polyolefin (A), 75 parts by mass of the above (B-1) as polyolefin resin (B), and 20 parts by mass of the above (C-1) as recycled carbon fiber (C) were mixed and extruded using a twin-screw kneader (Kobe Steel KTX-30) at a cylinder temperature of 200°C, a screw rotation speed of 200 rpm, and a discharge rate of 10 kg / h to obtain a recycled carbon fiber reinforced polyolefin resin composition (RCFRPP1).

[0091] The obtained recycled carbon fiber reinforced polyolefin resin composition (RCFRPP1) was injection molded using an injection molding machine (Meiki Seisakusho, 50T) at a cylinder temperature of 250°C and a mold temperature of 40°C, and the Izod impact strength (IZOD) and flexural strength (FS) of the molded body were measured.

[0092] Izod impact strength was measured in accordance with ASTM D256 using 1 / 8 inch thick injection molded test specimens (machined notch and cut notch) at 23°C. The bending strength was measured by a three-point bending test using an injection-molded test piece having a length of 2.5 inches, a width of 1 / 2 inch, and a thickness of 1 / 8 inch, with a span of 48 mm, a compression speed of 5 mm / min, and an atmosphere of 23°C. The results are shown in Table 1.

[0093] Example 2 The procedure of Example 1 was repeated except that the amount of CDI-PP1 used in Example 1 was changed to 10 parts by mass, to obtain a recycled carbon fiber reinforced polyolefin resin composition (RCFRPP2). The physical properties of the molded body obtained by the same molding method as in Example 1 were measured. The results are shown in Table 1.

[0094] [Examples 3 to 4] The procedure of Example 1 was repeated to obtain a recycled carbon fiber reinforced polyolefin resin composition, except that the amounts of CDI-PP1, (B-1) and (C-1) used in Example 1 were changed as shown in Table 1. The physical properties of the molded body obtained by the same molding method as in Example 1 were measured. The results are shown in Table 1.

[0095] Comparative Example 1 The procedure of Example 1 was repeated except that maleic anhydride modified polypropylene resin PP3 (acid functional group amount = 5.5 mmol, Mn = 14000, Mn / [(100-M) x f / M] is 0.8) was used instead of CDI-PP1 used in Example 1, to obtain a recycled carbon fiber reinforced polyolefin resin composition (RCFRPP3), and its physical properties were measured by the method described in Example 1. The results are shown in Table 2.

[0096] Comparative Example 2 The procedure was repeated in the same manner as in Comparative Example 1, except that the amount of maleic anhydride-modified polypropylene resin PP3 used in Comparative Example 1 was changed to 10 parts by mass, to obtain a recycled carbon fiber reinforced polyolefin resin composition (RCFRPP4). The physical properties of the molded body obtained by the same molding method as in Example 1 were measured. The results are shown in Table 2.

[0097] Comparative Example 3 Instead of using CDI-PP1 used in Example 1, 80 parts by mass of (B-1) and 20 parts by mass of (C-1) were used, and the procedure was carried out in the same manner as in Example 1 to obtain a recycled carbon fiber reinforced polyolefin resin composition (RCFRPP5), and the physical properties of the molded body obtained by the same molding method as in Example 1 were measured. The results are shown in Table 2.

[0098] Comparative Example 4 The same as Comparative Example 1 except that the contents of PP3, PP2 and C-1 were changed as shown in Table 2. Like A recycled carbon fiber reinforced polyolefin resin composition was obtained, and a molded body obtained by the same molding method as in Example 1 was measured for physical properties. The results are shown in Table 2.

[0099] [Reference example 1] As Reference Example 1, the same procedure as in Example 1 was carried out except that the recycled carbon fiber (C) CF1 used in Example 1 was replaced with carbon fiber CF2 (Teijin HTC702, 6 mm chopped product, fiber surface oxygen concentration ratio O / C = 0.20) containing a sizing agent, to obtain a carbon fiber reinforced polyolefin resin composition (RCFRPP6). The physical properties of the molded body obtained by the same molding method as in Example 1 were measured. The results are shown in Table 2.

[0100] [Reference example 2] As Reference Example 2, the same procedure as in Comparative Example 2 was carried out except that the recycled carbon fiber (C) CF1 used in Comparative Example 2 was replaced with carbon fiber CF2 (Teijin HTC702, 6 mm chopped product, fiber surface oxygen concentration ratio O / C = 0.20) containing a sizing agent, to obtain a carbon fiber reinforced polyolefin resin composition (RCFRPP7). The physical properties of the molded body obtained by the same molding method as in Example 1 were measured.

[0101] The results are shown in Table 2.

[0102] [Table 1]

[0103] [Table 2]

Claims

1. 0.01 to 50 parts by mass of modified polyolefin (A), 50 to 99 parts by mass of polyolefin (B), Recycled carbon fiber (C) 1 to 80 parts by mass (wherein the total of (A), (B) and (C) is 100 parts by mass), The modified polyolefin (A) is a modified polyolefin obtained by reacting a modified polyolefin (D) having a group reactive with a carbodiimide group with a carbodiimide group-containing compound (E), The recycled carbon fiber (C) is a recycled carbon fiber-reinforced polyolefin composition having a surface oxygen concentration ratio O / C of less than 0.05 as measured by X-ray photoelectron spectroscopy (XPS).

2. 2. The recycled carbon fiber reinforced polyolefin composition according to claim 1, wherein the modified polyolefin (A) has a carbodiimide group content in the range of 1 to 200 mmol per 100 grams of the modified polyolefin (A).

3. 3. The recycled carbon fiber-reinforced polyolefin composition according to claim 1, wherein the modified polyolefin (D) has a maleic anhydride group.

4. The recycled carbon fiber reinforced polyolefin composition according to any one of claims 1 to 3, wherein the polyolefin (B) and the modified polyolefin (D) are polypropylene.

5. The recycled carbon fiber reinforced polyolefin composition according to any one of claims 1 to 4, wherein the content of the modified polyolefin (A) is 4.5 to 50 parts by mass.

6. The recycled carbon fiber reinforced polyolefin composition according to any one of claims 1 to 5, wherein the content of the recycled carbon fiber (C) is 10 to 80 parts by mass.

7. A molded article obtained by molding the recycled carbon fiber reinforced polyolefin composition according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Recycled chopped carbon fiber-polypropylene composite and preparation method thereof

    CN109486018A

  • Polypropylene-based composite material

    JP2003277525A

  • Short carbon fiber, method for producing the same, short carbon fiber-reinforced resin composition, and short carbon fiber-reinforced cement composition

    JP2013087269A

  • Fiber-reinforced polypropylene-based resin composition

    JP2013166921A

  • Regenerated carbon fiber-reinforced plastic molding and production method thereof

    JP2015081262A