Carbon materials and their applications
A composite carbon material with a controlled carbonaceous coating layer addresses the gas generation issue in electric double layer capacitors, enhancing energy and output density while extending cycle life.
Patent Information
- Application Number
- JP2020094311
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-05-29
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-05-29
AI Technical Summary
The degradation of electric double layer capacitors due to gas generation caused by functional groups reacting with the electrolyte, leading to increased internal resistance and reduced cycle life, is addressed by developing a composite carbon material with controlled surface characteristics to minimize residual hydrogen, carbon monoxide, and water content.
A composite carbon material is formulated with a carbonaceous coating layer that satisfies specific gas desorption limits and Raman spectroscopy criteria, ensuring low residual gas content and uniform coating, enhancing capacitance retention and durability.
The composite carbon material achieves high energy and output density with improved cycle life by suppressing gas generation and capacitance decay during charging and discharging.
Smart Images

Figure 0007581660000004 
Figure 0007581660000001 
Figure 0007581660000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a carbon material and its use. [Background technology]
[0002] In recent years, from the perspective of protecting the global environment and effectively utilizing energy with the aim of saving resources, late-night power storage systems, distributed home energy storage systems based on solar power generation technology, energy storage systems for electric vehicles, and the like have been attracting attention.
[0003] Among these, electric double-layer capacitors have characteristics that batteries do not have, such as the ability to be charged and discharged quickly, resistance to overcharging and discharging, a long life because they do not involve chemical reactions, usability over a wide temperature range, and environmental friendliness because they do not contain heavy metals, and research into them is currently underway.
[0004] Carbon materials have been attracting attention as positive or negative electrode materials for electric double layer capacitors, and various improvements have been made to increase power density, improve charge / discharge efficiency, and extend life. In particular, various studies have been conducted on the modification of the surface state.
[0005] Patent Document 1 discloses a microporous material having quinone or acid anhydride as a functional group at the edge portion of the carbon material. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent Publication 2014-107361 Summary of the Invention [Problem to be solved by the invention]
[0007] As a result of intensive research, the present inventors have found that the main factor that causes a decrease in the electrostatic capacitance of the negative electrode during high-voltage charging in a capacitor using a carbon material as the negative electrode active material is that functional groups (hydrogen terminals, or oxygen-containing functional groups such as carboxyl groups, acid anhydrides, epoxy groups, hydroxyl groups, lactone groups, and phenolic hydroxyl groups) present on the surface of the carbon material react with the electrolyte, causing gasification, deterioration of the electrolyte, and interference with contact between the carbon and the electrolyte due to the generation of this gas. The gas has an adverse effect on other components such as the electrolyte, causing problems such as a decrease in cycle life in an electric double layer capacitor, or the formation of a non-electrically conductive film that increases internal resistance and causes malfunction.
[0008] In view of the above-mentioned current situation, an object of the present invention is to provide a composite carbon material that achieves high energy density, high power density, and long life in an electric double layer capacitor. [Means for solving the problem]
[0009] The present invention includes the following inventions [1] to
[14] . [1] A composite carbon material comprising a carbon material (A) and a carbonaceous coating layer (B) coating the surface of the carbon material, wherein the composite carbon material satisfies formula 1. Equation 1: C / E≦7.5 C is the amount of hydrogen molecules (H2) (μmol / g) desorbed from the composite carbon material, as measured by thermal desorption spectroscopy (TDS) at a temperature increase from 80°C to 1400°C, E is the amount of carbon monoxide molecules (CO) (μmol / g) desorbed from the composite carbon material, as measured by thermal desorption spectroscopy (TDS) at a temperature increase from 500°C to 800°C. [2] The composite carbon material according to [1], characterized in that formula 2 is satisfied. Equation 2: C / D≦2.3 D is the amount of carbon dioxide molecules (CO2) (μmol / g) desorbed from the composite carbon material, as measured by thermal desorption spectroscopy (TDS) at a temperature increase from 80°C to 400°C. [3] The composite carbon material according to [1] or [2], characterized in that formula 3 is satisfied. Equation 3: C / F≦6.0 F is the amount of water molecules (H2O) (μmol / g) desorbed from the composite carbon material, as measured by thermal desorption spectroscopy (TDS) at a temperature increase from 80°C to 400°C. [4] The composite carbon material according to any one of [1] to [3], wherein C is 100 μmol / g or more and 1000 μmol / g or less. [5] The composite carbon material according to any one of [1] to [4], wherein E is 100 μmol / g or less. [6] The R value (1350cm) obtained from the Raman spectrum by micro-Raman spectroscopy -1 The peak intensity (I D ) and 1580cm -1 The peak intensity (I G ) ratio (I D / I G )) has a coefficient of variation of 0.60 or less. [7] R value (1350cm) obtained from Raman spectrum by micro-Raman spectroscopy -1 The peak intensity (I D ) and 1580cm -1 The peak intensity (I G ) ratio (I D / I G )) is 0.30 or more and 1.50 or less. [8] The 50% particle size (D50) in the volume-based cumulative particle size distribution by laser diffraction method is 2 to 30 μm, and the 400 tapping density is 0.05 g / cm 3 More than 1.50g / cm 3 The composite carbon material according to any one of the following [1] to [7]. [9] BET specific surface area is 700m2 / g or more 2500m 2 The composite carbon material according to any one of [1] to [8], wherein the value is 0.01 to 0.1 / g or less.
[10] The composite carbon material according to any one of [1] to [9], wherein (BET specific surface area of the composite carbon material) / (BET specific surface area of the carbon material (A)) is 0.50 or more and 1.00 or less.
[11] The R values (1350 cm) obtained from the Raman spectra of carbon material (A) and composite carbon material by micro-Raman spectroscopy -1 The peak intensity (I D ) and 1580cm -1 The peak intensity (I G ) ratio (I D / I G )), wherein (R value of the composite carbon material) / (R value of the carbon material (A)) is 0.50 or more and 1.50 or less.
[12] An electrode material comprising the composite carbon material according to any one of [1] to
[11] .
[13] An electrode for an electric double layer capacitor, comprising the electrode material according to
[12] .
[14] An electric double layer capacitor having electrodes immersed in an electrolyte, at least one of the electrodes being the electrode according to
[13] . Effect of the Invention
[0010] According to the present invention, by forming a thin film coating layer on the surface or inside of a carbon material, it is possible to provide a composite carbon material that achieves high energy density, high power density, and long life in an electric double layer capacitor. [Brief description of the drawings]
[0011] [Figure 1] FIG. 2 is a cross-sectional view of an electric double layer capacitor evaluation cell. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, embodiments of the present invention will be described in detail. In the description, "peak intensity" refers to the height of a peak.
[0013] [1] Composite carbon materials The composite carbon material in one embodiment of the present invention is a composite carbon material comprising a carbon material (A) and a carbonaceous coating layer (B) coating the surface of the carbon material (A), and is characterized in that formula 1 is satisfied. Equation 1: C / E≦7.5 In formula 1, C is the amount (μmol / g) of hydrogen molecules (H2) desorbed from the composite carbon material, measured by thermal desorption spectrometry (TDS) when the temperature of the composite carbon material is increased from 80° C. to 1400° C., and E is the amount (μmol / g) of carbon monoxide molecules (CO) desorbed from the composite carbon material, measured by thermal desorption spectrometry (TDS) when the temperature of the composite carbon material is increased from 500° C. to 800° C. In other words, C is the total amount (μmol) of hydrogen molecules generated between 80° C. and 1400° C. per 1 g of the composite carbon material. The same applies to D and E.
[0014] When the C / E is 7.5 or less, the carbon material has a characteristic that hydrogen derived from the residual functional group is very small when used in a capacitor. In other words, such a carbon material is a carbon material with very few residual functional groups, and an electric double layer capacitor made using these carbon materials is excellent in cycle characteristics because gas generation and capacitance decay during charging and discharging are suppressed. From the same viewpoint, the C / E is preferably 6.5 or less, and more preferably 6.0 or less. The C / E is preferably 0.1 or more.
[0015] In the composite carbon material according to one embodiment of the present invention, it is preferable that formula 2 is further satisfied. Equation 2: C / D≦2.3 In formula 2, D is the amount (μmol / g) of carbon dioxide molecules (CO2) desorbed from the composite carbon material, measured by thermal desorption spectrometry (TDS) at a temperature rise from 80°C to 400°C. If formula 2 is satisfied, when used in a capacitor, there is very little hydrogen derived from the remaining functional groups, so gas generation during charging and discharging and capacitance decay are suppressed, resulting in excellent cycle characteristics. From the same viewpoint, C / D is preferably 2.1 or less, more preferably 1.9 or less. C / D is preferably 0.1 or more.
[0016] In the composite carbon material according to one embodiment of the present invention, it is preferable that formula 3 is further satisfied. Equation 3: C / F≦6.0 In formula 3, F is the amount of water molecules (H2O) (μmol / g) desorbed from the composite carbon material, measured by thermal desorption spectrometry (TDS) at a temperature rise from 80°C to 400°C. If formula 3 is satisfied, when used in a capacitor, there is very little hydrogen derived from the remaining functional groups, so gas generation during charging and discharging and attenuation of capacitance are suppressed, resulting in excellent cycle characteristics. From the same viewpoint, C / F is preferably 5.5 or less, more preferably 5.0 or less. C / F is preferably 0.1 or more.
[0017] In the composite carbon material according to one embodiment of the present invention, since C is correlated with the amount of oxygen-based functional groups, it is preferable that C is 100 μmol / g or more and 1000 μmol / g or less. When C is 100 μmol / g or more, the capacitance is sufficiently secured and the energy density is excellent. When C is 1000 μmol / g or less, gas generation during charging and discharging and attenuation of the capacitance are suppressed, so that durability is excellent. From the same viewpoint, C is more preferably 200 μmol / g or more and 500 μmol / g or less.
[0018] In the composite carbon material according to one embodiment of the present invention, since it is correlated with the amount of oxygen-based functional groups, the above E is preferably 100 μmol / g or less. If it is 100 μmol / g or less, gas generation during charging and discharging and attenuation of capacitance are suppressed, so durability is excellent. From the same viewpoint, E is more preferably 80 μmol / g or less, and even more preferably 60 μmol / g or less. The above E is preferably 14 μmol / g or more.
[0019] Carbon materials have a Raman spectrum with a 1350 cm peak due to amorphous carbon. -1 There is a peak (D band) near the I D In addition, the 1580 cm -1 There is a peak (G band) near the I G The ratio of the D band peak intensity to the G band peak intensity (I D / I G ) is taken as the R value (hereinafter sometimes referred to as the "Raman R value"), and the state of the surface of the composite carbon material can be evaluated. The smaller the R value, the higher the crystallinity of the surface of the composite carbon material.
[0020] The composite carbon material according to one embodiment of the present invention has an R value (1350 cm) obtained from a Raman spectrum by microscopic Raman spectroscopy. -1 The peak intensity (I D ) and 1580cm -1 The peak intensity (I G ) ratio (I D / I G The coefficient of variation of R is preferably 0.60 or less, more preferably 0.55 or less, and even more preferably 0.50 or less. When the coefficient of variation of R is 0.60 or less, gas generation and capacitance decay during charging and discharging are suppressed, and durability is improved. The coefficient of variation of R is preferably 0.10 or more.
[0021] The coefficient of variation of the R value is calculated by measuring the R value at multiple points using microscopic Raman spectroscopy and dividing the standard deviation by the average R value. The coefficient of variation can be used to evaluate the variation in the coating condition. The larger the coefficient of variation, the lower the uniformity of the R value and the greater the variation in the coating condition.
[0022] In the microscopic Raman spectroscopy, a microscopic laser Raman spectroscope with high spatial resolution is used to measure the R value at multiple points for the same sample. The number of measurement points for the R value is usually 30 or more, preferably 50 or more, from the viewpoint of measurement accuracy. Typically, the measurement is performed by shifting the laser irradiation position after each measurement so that the location is different each time. If the spatial resolution is too low (i.e., if the overlap of the irradiation positions is too large), the variation between materials is difficult to reflect in the R value, and the accuracy of the evaluation results may decrease.
[0023] The composite carbon material according to one embodiment of the present invention has a Raman R value (I D / I G ) is preferably 0.30 or more, more preferably 0.50 or more, and even more preferably 0.70 or more. When the R value is 0.30 or more, the reaction resistance is sufficiently low, leading to a high output density of the electric double layer capacitor. In addition, the R value is preferably 1.50 or less, more preferably 1.20 or less, and even more preferably 1.15 or less. When the R value is 1.50 or less, gas generation and capacitance decay during charging and discharging are suppressed, and durability is improved.
[0024] In the composite carbon material in one embodiment of the present invention, (Raman R value of composite carbon material) / (Raman R value of carbon material (A)) is preferably 0.50 or more, more preferably 0.60 or more, and particularly preferably 0.65 or more. When it is 0.50 or more, the carbonaceous coating layer (B) is sufficiently formed on the surface of the carbon particle (A), and the active sites in the carbon particle (A) can be sufficiently removed, thereby improving durability. On the other hand, (Raman R value of composite carbon material) / (Raman R value of carbon material (A)) is preferably 1.50 or less, more preferably 1.00 or less, and even more preferably 0.95 or less. When it is 1.50 or less, the formation of an excessive carbonaceous coating layer (B) is suppressed, and therefore the cycle characteristics can be maintained good. The Raman R value of the carbon material (A) is the value of the carbon material used as a raw material.
[0025] In one embodiment of the present invention, the 50% particle size (D50) of the composite carbon material is preferably 2.0 μm or more, more preferably 3.0 μm or more, and most preferably 5.0 μm or more. When D50 is 2.0 μm or more, particle aggregation is suppressed, and it is easy to prepare a slurry for electrode coating. D50 is preferably 30.0 μm or less, more preferably 20.0 μm or less, and even more preferably 15.0 μm or less. When D50 is 30.0 μm or less, the electrical resistance of the electrode is small, and the output density of the electric double layer capacitor is increased. In this specification, the "50% particle size (D50)" means a particle size at 50% of the cumulative particle size distribution on a volume basis determined by a laser diffraction method.
[0026] In one embodiment of the present invention, the composite carbon material has a 400 tapping density of 0.05 g / cm 3 More than 0.10 g / cm is preferable. 3 More preferably, 0.20 g / cm 3 More preferably, the tapping density is 0.05 g / cm 3 If the density is above this level, it is possible to achieve a sufficiently high electrode density during pressing, resulting in a battery with a high energy density. The density after 400 tappings is 1.50 g / cm 3 Less than 1.00 g / cm is preferred. 3 Less than 0.50 g / cm is more preferable.3 More preferably, the tapping density is 1.50 g / cm 3 In the following cases, it is possible to sufficiently increase the electrolyte permeability of the obtained electrode, and a battery with excellent input / output characteristics can be obtained.
[0027] In one embodiment of the present invention, the composite carbon material has a BET specific surface area of 700 m 2 / g or more is preferable, and 1200m 2 / g or more is more preferable, and 1500m 2 / g or more is more preferable. 2 / g or more, the electric double layer capacity becomes large, making it possible to increase the electric capacity of the capacitor. 2 / g or less is preferable, and 2100m 2 / g or less is more preferable, and 1900m 2 / g or less is more preferable. 2 If the capacitance is less than 1.0 μm / g, the electrical capacitance per volume of the electrode (volume density) decreases, and gas generation and capacitance decay during charging and discharging are small, resulting in excellent durability.
[0028] The ratio (BET specific surface area of the composite carbon material) / (BET specific surface area of the carbon material (A)) is preferably 1.00 or less, and more preferably 0.95 or less. This is because gas generation during charging and discharging can be suppressed and the capacitance decay is small, resulting in excellent durability. The ratio is preferably 0.50 or more, more preferably 0.60 or more, and even more preferably 0.70 or more. The BET specific surface area of the carbon material (A) is the value of the carbon material used as the raw material.
[0029] The D50, 400 tapping density and BET specific surface area described in this specification are measured by the method described in the Examples.
[0030] [2] Carbon materials (A) The composite carbon material in one embodiment of the present invention includes a carbon material (A). The carbon material (A) is not limited, and examples thereof include amorphous carbon materials such as soft carbon and hard carbon, carbon fibers, vapor grown carbon fibers, multi-walled carbon nanotubes, single-walled carbon nanotubes, nanowires, and graphite materials. However, amorphous carbon materials or graphite materials are preferred, and amorphous carbon materials are more preferred, because they have high electronic conductivity, are excellent in cycle characteristics, and can increase electrode density.
[0031] The carbon material (A) is preferably a porous carbon material. Examples of porous carbon materials include activated carbon, carbon obtained by pyrolyzing resins or organic substances, molecular sieving carbon, activated carbon fiber, aggregates of vapor-grown carbon fibers, aggregates of CNTs (carbon nanotubes), and inorganic template carbon. Porous carbon materials can be produced by known production methods, for example, the same production methods as activated carbon, or by subjecting polymers to appropriate heat treatment. Here, being porous means a material having a BET specific surface area of 200 m 2 / g or more, preferably 200m 2 / g or more 10000m 2 / g or less.
[0032] The pore distribution of the porous carbon can be examined by, for example, analyzing the adsorption / desorption isotherm by a known method using a gas adsorption method. Although there is no particular limitation on the probe gas, nitrogen gas, carbon dioxide, or argon is usually used.
[0033] [3] Carbonaceous coating layer (B) The carbonaceous coating layer (B) is a layer that covers the surface of the carbon material (A). The carbonaceous coating layer (B) may cover the entire surface of the composite carbon material (A), or may cover only a part of it. The carbonaceous coating layer (B) is obtained by carbonizing an organic compound by heat treatment. The structure of the carbonaceous coating layer (B) is not particularly limited, but it is preferable that the carbonaceous coating layer (B) contains amorphous carbon or graphene in order to improve the electrical conductivity of the surface of the composite carbon material (A). Graphene is a structure in which carbon atoms are continuous as a honeycomb-like surface. When the carbonaceous coating layer (B) contains graphene, the carbonaceous coating layer (B) may contain one single graphene layer, or may contain a multi-layer graphene layer in which multiple graphene layers are overlapped. The graphene layer may contain graphene oxide to which an oxygen-based functional group is added on the surface. The structure of the carbonaceous coating layer (B) can be confirmed by analysis such as FFT (Fast Fourier Transform).
[0034] The carbonaceous coating layer (B) more preferably contains a graphene structure formed along the surface of the carbon material. The graphene structure formed along the surface of the carbon material is a structure in which a honeycomb-shaped surface is formed along the surface of the carbon material. This is because the electrical conductivity of the composite material surface is increased, and the chemical stability and mechanical strength of the carbonaceous coating layer are increased.
[0035] The average thickness of the carbonaceous coating layer (B) is preferably 0.1 nm or more. 0.1 nm corresponds to the thickness of a single layer of graphene. From the viewpoint of providing a certain level of electrical conductivity, chemical stability, and mechanical strength, the average thickness of the carbonaceous coating layer (B) is more preferably 1.0 nm or more, and even more preferably 2.0 nm or more. The average thickness of the carbonaceous coating layer (B) is preferably 30.0 nm or less. When the average thickness of the carbonaceous coating layer (B) is 30.0 nm or less, the formation of an excess of the carbonaceous coating layer (B) is suppressed, and the initial coulombic efficiency and the discharge capacity retention rate can be improved. From the same viewpoint, the average thickness is more preferably 20.0 nm or less, even more preferably 10.0 nm or less, and most preferably 5.0 nm or less.
[0036] The thickness of the carbonaceous coating layer (B) is measured by observation with a transmission electron microscope (TEM). Specifically, it can be measured by the method described in the Examples.
[0037] [4] Manufacturing methods for composite carbon materials A method for producing a composite carbon material in one embodiment of the present invention includes a mixing step of mixing a carbon material (A) with a carbonaceous coating layer raw material, which is a raw material for the carbonaceous coating layer (B), to obtain a mixture, and a heat treatment step of heat treating the mixture obtained in the mixing step at 500°C or more and 2000°C or less.
[0038] [4-1]Mixing process In the mixing step, the carbon material (A) and the carbonaceous coating layer raw material are mixed to obtain a mixture. At this time, carbon fine particles (B2) may be further mixed. The carbon fine particles (B2) are preferably amorphous carbon particles such as coal fine powder, vapor-phase carbon powder, carbon black, ketjen black, and acetylene black. Among these, carbon black is more preferable. When the carbon fine particles (B2) are mixed to obtain a carbonaceous coating layer containing carbon fine particles, the input / output characteristics tend to be improved. When the carbon fine particles (B2) are mixed, the amount of the carbon fine particles (B2) is preferably 0.01 to 10.00 parts by mass, more preferably 0.10 to 5.00 parts by mass, relative to 100 parts by mass of the composite material (A). When the amount of the carbon fine particles (B2) is within the above range, the input / output characteristics can be improved while maintaining the initial coulombic efficiency.
[0039] In the mixing step when carbon fine particles (B2) are used, the carbon material (A) and the carbonaceous coating layer raw material may be mixed first, and then the mixture may be mixed with the carbon fine particles (B2); the carbon material (A) and the carbon fine particles (B2) may be mixed first, and then the mixture may be mixed with the carbonaceous coating layer raw material; the carbonaceous coating layer raw material and the carbon fine particles (B2) may be mixed first, and then the mixture may be mixed with the carbon material (A); or the carbon material (A), the carbonaceous coating layer raw material, and the carbon fine particles (B2) may be mixed simultaneously.
[0040] The mixture obtained in the mixing step may contain materials other than the carbon material (A), the carbonaceous coating layer raw material, and the carbon fine particles (B2), but the mixture is preferably composed of only the carbon material (A), the carbonaceous coating layer raw material, and the optional carbon fine particles (B2). Furthermore, the mixture may be composed of only the carbon material (A) and the carbonaceous coating layer raw material. It is preferable to use the carbonaceous coating layer raw material in a powder state. The mixing method is preferably dry mixing, and commercially available mixers and stirrers can be used. Specific examples include mixers such as ribbon mixers, V-type mixers, W-type mixers, one-blade mixers, and Nauta mixers.
[0041] The carbonaceous coating layer raw material is not limited as long as it is a material containing carbon that adheres to and coats the surface of the carbon material (A), and can be, for example, petroleum pitch, coal pitch, resin, organic compound, etc. Among these, carboxylic acid compounds are preferred, and polycarboxylic acid compounds having no hydroxyl group and two or more carboxyl groups in one molecule (also simply called "polycarboxylic acid compounds") and hydroxycarboxylic acid compounds having one or more carboxyl groups and one or more hydroxyl groups in one molecule (also simply called "hydroxycarboxylic acid compounds") are more preferred. When the carbonaceous coating layer is formed using these compounds, a graphene layer with chemical stability and mechanical strength can be formed, and a battery with high cycle characteristics can be obtained.
[0042] Examples of polycarboxylic acid compounds include succinic acid (melting point 185°C), glutaric acid (melting point 95°C), maleic acid (melting point 131°C), phthalic acid (melting point 210°C), terephthalic acid (melting point 300°C), oxaloacetic acid (melting point 161°C), and malonic acid (melting point 135°C). Examples of hydroxycarboxylic acid compounds include malic acid (melting point 130°C), citric acid (melting point 153°C), tartaric acid (melting point 168°C (L-form), melting point 151°C (meso-form), melting point 206°C (racemic form)), gallic acid (melting point 250°C), and salicylic acid (melting point 159°C). By using such a carboxylic acid compound, dehydration occurs between molecules in the heat treatment process described below, forming a denser network structure, and the carbon material can be covered more widely, thinly, and firmly.
[0043] Among these, compounds containing two or more carboxyl groups and one or more hydroxyl groups in one molecule are more preferred, and malic acid, citric acid, and tartaric acid (L-form) are particularly preferred.
[0044] The carboxylic acid compound may be one type or may contain two or more types. That is, two or more types of polycarboxylic acid compounds may be used, two or more types of hydroxycarboxylic acid compounds may be used, or a polycarboxylic acid compound and a hydroxycarboxylic acid compound may be used in combination. The carboxylic acid compound may be combined with a compound containing one carboxy group in one molecule.
[0045] That is, the carboxylic acid compound can be used in, for example, the following three embodiments: the first embodiment is an embodiment in which only a hydroxycarboxylic acid compound is used as the carboxylic acid compound, the second embodiment is an embodiment in which only a polycarboxylic acid compound is used as the carboxylic acid compound, and the third embodiment is an embodiment in which a hydroxycarboxylic acid compound and a polycarboxylic acid compound are used as the carboxylic acid compound.
[0046] The melting point of the carboxylic acid compound is preferably 500°C or less. By having a melting point within this range, the thermal decomposition of the carboxylic acid compound is reduced and the covering effect is enhanced. From the same viewpoint, the melting point is more preferably 400°C or less, and even more preferably 300°C or less. The melting point of the carboxylic acid compound is preferably 95°C or more. By having a melting point within this range, the carboxylic acid compound is easy to handle and the yield after the mixing process is high. From the same viewpoint, the melting point is more preferably 110°C or more, and even more preferably 130°C or more.
[0047] The carboxylic acid compound has a lower viscosity than the pitch or polymers used in conventional coatings, and the functional groups of the carboxylic acid compound interact with the functional groups on the carbon particles, making it possible to disperse the carbon particles well. As a result, it is believed that the maximum secondary particle size of the carbon particles is smaller than in the conventional case.
[0048] The blending amount of the carbon material (A) and the carbonaceous coating layer raw material is preferably 50.0 mass% or more and 99.9 mass% or less of the carbon material (A) and 0.1 mass% or more and 50.0 mass% or less of the carbonaceous coating layer raw material with respect to the total mass of the carbon material (A) and the carbonaceous coating layer raw material. The reason for making the blending amount of the carbonaceous coating layer raw material 0.1 mass% or more is to sufficiently coat the carbon material with the carbonaceous coating layer raw material. From this viewpoint, the amount of the carbonaceous coating layer raw material is more preferably 1.0 mass% or more, and even more preferably 3.0 mass% or more. The reason for making the blending amount of the carbonaceous coating layer raw material 50.0 mass% or less is to suppress the formation of an excessive carbonaceous coating layer (B), thereby maintaining good cycle characteristics. From this viewpoint, the amount of the carbonaceous coating layer raw material is more preferably 45.0 mass% or less, and even more preferably 40.0 mass% or less.
[0049] [4-2] Heat treatment process The step of heat treating the mixture is not particularly limited as long as a composite carbon material can be obtained. The heat treating step (heat treatment step) can be performed using a heat treatment device such as a rotary kiln, a roller hearth kiln, or an electric tubular furnace. The heat treatment step can provide a composite carbon material in which the surface of the carbon material (A) is covered with a carbonaceous coating layer (B).
[0050] In order to sufficiently advance the carbonization of the carbonaceous coating layer raw material, suppress residual hydrogen and oxygen, and improve the battery characteristics, the heat treatment temperature in the heat treatment step is preferably 500° C. or higher, more preferably 700° C. or higher, and most preferably 900° C. or higher. In addition, in order to suppress structural changes in the carbon material (A) and maintain a good output density of the electric double layer capacitor, the heat treatment temperature is preferably 1500° C. or lower, more preferably 1350° C. or lower, and most preferably 1100° C. or lower.
[0051] The treatment time is not particularly limited as long as the carbonization has progressed sufficiently, but is preferably 10 minutes or more, more preferably 30 minutes or more, and even more preferably 50 minutes or more. The upper limit of the treatment time is not particularly limited as long as the carbonization has progressed sufficiently, but is preferably 600 minutes or less, more preferably 400 minutes or less, and even more preferably 200 minutes or less.
[0052] The heat treatment step is preferably carried out in an inert gas atmosphere, such as argon gas or nitrogen gas.
[0053] The composite carbon material after the heat treatment may be appropriately subjected to crushing and sieving treatment.
[0054] [5] Electrode material In one embodiment of the present invention, the electrode material comprises the composite carbon material described above.
[0055] The electrode material includes the composite carbon material, but may further include other components. Examples of the other components include other carbon materials and conductive assistants. When the other carbon materials and conductive assistants are included, the composite carbon material may be used with 0.01 to 200 parts by mass, preferably 0.01 to 100 parts by mass, of the other carbon materials and conductive assistants blended with respect to 100 parts by mass of the composite carbon material. By using the other carbon materials and conductive assistants in combination, it is possible to obtain a negative electrode active material that has the excellent properties of the other carbon materials and conductive assistants while maintaining the excellent properties of the composite carbon material.
[0056] Such an electrode material can be obtained by mixing the composite carbon material with other carbon materials and conductive additives. When mixing, the mixing materials can be appropriately selected and the mixing amounts can be determined according to the required capacitor characteristics.
[0057] As the conductive assistant, carbon fine particles such as carbon fiber and carbon black can be used. Examples of carbon fiber include organic carbon fibers such as PAN-based carbon fiber, pitch-based carbon fiber, and rayon-based carbon fiber, and vapor-grown carbon fiber. Among these, vapor-grown carbon fiber is preferred because of its high crystallinity and high thermal conductivity.
[0058] As a device for mixing the composite carbon material with other materials, a commercially available mixer or stirrer can be used. Specific examples include mixers such as ribbon mixers, V-type mixers, W-type mixers, one-blade mixers, and Nauta mixers. Mixing by a device that simultaneously applies mechanical energy such as shear force, impact, and compression is preferable. For example, a high-speed stirrer that applies shear force and impact to the powder by a high-speed swirling flow, or a dry mixer having a structure in which the gap between the mixing blade and the inner wall of the container is narrow and the powder is pressed against the inner wall of the container, etc., are preferable. Examples of such mixers include Mechanofusion (registered trademark, manufactured by Hosokawa Micron Corporation), Nobilta (registered trademark, manufactured by Hosokawa Micron Corporation), Composite (registered trademark, manufactured by Nippon Coke & Engineering Co., Ltd.), Multipurpose Mixer (manufactured by Nippon Coke & Engineering Co., Ltd.), and Hybridization System (registered trademark, manufactured by Nara Machinery Co., Ltd.).
[0059] [6] Electrodes for electric double layer capacitors An electrode for an electric double layer capacitor in one embodiment of the present invention contains the above electrode material. The method for producing the electrode is not limited, but for example, a binder such as polyethylene, polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), polyvinylidene chloride (PVDC), or carboxymethyl cellulose (CMC) can be added to the electrode material, and the material can be pressure roll molded into a sheet or plate shape to form an electrode. The amount of binder used is not particularly limited, but is preferably 0.5 to 15 mass%, more preferably 1 to 10 mass%, relative to 100 parts by mass of the electrode material. At this time, it is also possible to add a carbon material such as graphite powder, carbon black such as acetylene black, or vapor-grown carbon fiber as a conductive assistant. The conductive assistant is blended to improve the conductivity of the electrode, and is preferably 0.5 to 15 mass%, more preferably 1 to 10 mass%, relative to 100 parts by mass of the electrode material. The current collector is not particularly limited as long as it is made of a conductive material, and examples of the current collector include those made of conductive metals and conductive resins. In particular, those made of aluminum, aluminum alloys, and platinum are preferred. The shape of the current collector is also not particularly limited, and sheet-like or mesh-like ones are preferred.
[0060] [7] Electric double layer capacitor An electric double layer capacitor according to one embodiment of the present invention has electrodes immersed in an electrolyte, at least one of which is an electrode for an electric double layer capacitor that contains the composite carbon material.
[0061] As the electrolyte for the electric double layer capacitor in one embodiment of the present invention, a non-aqueous electrolyte in the form of an electrolyte salt dissolved in a non-aqueous solvent is preferably used. It is known that the non-aqueous electrolyte can increase the amount of stored energy per volume of the capacitor, and is advantageous from the viewpoint of increasing the density of energy per volume.
[0062] Examples of non-aqueous solvents include propylene carbonate, dimethyl carbonate, diethyl carbonate, ethylene carbonate, butylene carbonate, ethyl methyl carbonate, methyl propyl carbonate, γ-butyrolactone, dimethyl sulfoxide, dimethylformamide, acetonitrile, tetrahydrofuran, 1,2-dimethoxyethane, and ethylisopropyl sulfone (EiPS), or organic cations such as 1-ethyl-3-methylimidazolium (EMI) and 1-butyl-3-methylimidazolium (BMI) and BF4 - , PF6 - Ionic liquids consisting of anions such as the above can be used. Propylene carbonate and acetonitrile are more preferable in terms of electrochemical stability and chemical stability. These non-aqueous solvents can also be used as a mixed solvent of two or more kinds.
[0063] In addition, the electrolyte is R 1 R 2 R 3 R 4 The cation represented by N (R1 , R 2 , R 3 , R 4 are each independently an alkyl group or an aryl group having 1 to 10 carbon atoms, and R 1 and R 2 may be bonded to form a ring, R 3 and R 4 An electrolyte consisting of R may be used. 1 R 2 R 3 R 4 Examples of the cation represented by N include tetraethylammonium ion, tetrabutylammonium ion, and spirobipyrrolidinium ion. Examples of the anion include ClO4 - , BF4 - , PF4 - , PF6 - , AsF6 - etc.
[0064] Specific examples of the electrolyte include tetraethylammonium tetrafluoroborate (Et4NBF4), spirobipyrrolidinium tetrafluoroborate, and Bu4NClO4.
[0065] The electrolyte concentration in the non-aqueous electrolytic solution is not particularly limited, but in order to fully utilize the characteristics of the electric double layer capacitor, it is preferably 0.3 to 2.0 M, and more preferably 0.7 to 1.5 M. Within the above range, high electrical conductivity can be obtained.
[0066] Specific examples of the electrolyte include an electrolyte solution in which tetraethylammonium tetrafluoroborate (Et4NBF4) is dissolved in propylene glycol, an electrolyte solution in which tetraethylammonium tetrafluoroborate is dissolved in acetonitrile, and an electrolyte solution in which spirobipyrrolidinium tetrafluoroborate (SBP-BF4) is dissolved in ethylisopropylsulfone (EiPS).
[0067] As the separator, various types of separators can be used, and for example, a polyethylene separator, a nylon nonwoven fabric separator, a polypropylene nonwoven fabric separator, etc. can be suitably used.
[0068] The electric double layer capacitor according to one embodiment of the present invention has a configuration in which a separator is disposed between a pair of polarizable electrodes immersed in an electrolytic solution, and may be of any configuration, such as a coin type in which the pair of polarizable electrodes are housed in a metal case together with the electrolytic solution via the separator, a wound type in which a pair of electrodes are wound via a separator, or a laminated type in which a plurality of separators and electrodes are stacked. The electric double layer capacitor is preferably sealed with a stainless steel or aluminum container. In addition, from the viewpoint of preventing the electrolytic solution from volatilizing even when heat is generated and for the purpose of ensuring the high-temperature stability of the electric double layer capacitor, it is preferable to use a highly heat-resistant insulating material for the seal part of the container, and in particular, it is preferable to use at least one selected from the group consisting of polyphenylene sulfide resin, polyether ketone resin, polyether ether ketone resin, polyethylene terephthalate resin, polybutylene terephthalate resin, and glass. EXAMPLES
[0069] The present invention will be specifically described below with reference to examples. Note that these are merely illustrative examples and are not intended to limit the present invention.
[0070] [1] Evaluation of composite carbon materials [1-1] Thermal Desorption Spectroscopy (TDS) Using an EMD-WA1000S / W model thermal desorption gas analyzer manufactured by Electron Science Corporation, the number of moles (μmol / g) of hydrogen molecules desorbed from the composite carbon materials obtained in the Examples or Comparative Examples was measured as the temperature was increased from 80° C. to 1400° C., from 80° C. to 400° C. for carbon dioxide molecules and water molecules, and from 500° C. to 800° C. for carbon monoxide molecules. C, D, E, and F were calculated by integrating these values within each range.
[0071] The sample stage and sample plate used to measure the composite carbon material were both made of quartz. The heating rate was 60°C / min in a vacuum atmosphere. The sample weight was 0.5 mg, and was corrected based on the actual measured weight. A quadrupole mass spectrometer was used for detection. The mass numbers [M / z] used to analyze the measured values were 2 for H2, 18 for H2O, 28 for CO, and 44 for CO2, and the gases corresponding to the above mass numbers were all determined to be the above substances.
[0072] [1-2] Tapping density (tap density) Using Autotap manufactured by Quantachrome as a tap density measuring device, 50 g of each carbon composite material obtained in the examples and comparative examples was placed in a 250 mL glass cylinder, and the density was measured after 400 taps. This is a measuring method based on ASTM B527 and JIS K5101-12-2, and the drop height of the Autotap was set to 5 mm.
[0073] [1-3]BET specific surface area A Quantachrome NOVA2200e was used as a BET specific surface area measurement device, and 0.1 g of each carbon composite material obtained in the examples or comparative examples was placed in a sample cell (9 mm x 135 mm), dried at 300°C under vacuum conditions for 1 hour, and then measured by the BET three-point method at relative pressures of 0.1, 0.2, and 0.3. N2 was used as the gas for measuring the BET specific surface area.
[0074] [1-4]50% particle size (D50) A Malvern Mastersizer 2000 (Mastersizer; registered trademark) was used as a laser diffraction particle size distribution measurement device. A 5 mg sample of each carbon composite material obtained in the Examples or Comparative Examples was placed in a container, 10 g of water containing 0.04 mass % of a surfactant was added, and ultrasonic treatment was performed for 5 minutes. Then, measurement was performed to obtain the 50% particle size (D50) in the cumulative particle size distribution based on volume.
[0075] [1-5] R-value and coefficient of variation of R-value The measurement was performed using a JASCO NRS-5100 laser Raman microscope at an excitation wavelength of 532.36 nm under the following measurement conditions: Exposure time: 5 seconds Number of times: 2 Diffraction grating: 300 lines / mm (600 nm) 1350cm in Raman spectrum -1 The peak intensity (I D ) and 1580cm -1 The peak intensity (I G ) is the R value (I D / I G )
[0076] Microscopic laser Raman spectroscopic imaging was performed on the composite carbon material in the following regions: Measurement points: 22 x 28 locations Measurement step: 0.32μm Measurement area: 7.0 x 9.0 μm
[0077] Of the above measurements, 100 points were randomly selected from the region corresponding to the composite carbon material, and the standard deviation of the obtained R values was divided by the average R value to obtain the coefficient of variation. The average value of the R values was taken as the R value of the composite carbon material.
[0078] [2] Preparation of electrodes 80 parts by mass of composite carbon material with an average particle size of 10 μm were mixed with 10 parts by mass of PTFE (polytetrafluoroethylene) and 10 parts by mass of carbon black, kneaded, and rolled into a sheet with a thickness of 0.5 mm on an aluminum current collector. This sheet was punched into a disk with a diameter of 20 mm, vacuum dried at 200°C for one day, and used as a polarizable electrode.
[0079] [3] Assembly of electric double layer capacitor The electrodes were assembled into an evaluation cell as shown in Fig. 1 in a glove box in which high-purity argon was circulated, and used for evaluation. In Fig. 1, 1 is an aluminum top cover, 2 is a fluororubber O-ring, 3 is an aluminum current collector, 4 is an insulating material made of Teflon (registered trademark), 5 is an aluminum container, 6 is an aluminum leaf spring, 7 is a polarizable electrode, and 8 is a 1 mm thick separator made of glass fiber. The electrolyte used was LIPASTE-P / TEMAF14N (1 mol / liter) manufactured by Toyama Pharmaceutical Co., Ltd., which uses PC (propylene carbonate) as a solvent and (CH3)(C2H5)3NBF4 as an electrolyte.
[0080] The charge and discharge measurements were carried out using a charge and discharge tester HJ-101SM6 manufactured by Hokuto Denko Corporation, with charging and discharging performed at 1.59 mA from 0 to 2.5 V. The capacitance per mass (F / g) and capacitance per volume (F / ml) of the activated carbon at both electrodes of the electric double layer capacitor were calculated from the discharge curve obtained by the second constant current discharge. The durability was evaluated based on the capacity retention rate (capacity after cycle test / capacity after the second charge / discharge) of the electric capacity after 200 charge / discharge cycle tests.
[0081] [4] Raw materials [Carbon material (A)] BET specific surface area 1800m 2 Commercially available activated carbon (amorphous carbon material) with a particle size of 1 / g, D50 of 10 μm, and Raman R value of 1.24 was used.
[0082] [Carbon coating layer raw material] The carbonaceous coating layer materials shown in Table 1 were used.
[0083] <Examples 1-5, Comparative Examples 1-2> In each of the Examples and Comparative Examples, the raw materials and ratios shown in Table 1 were charged into a multipurpose mixer (manufactured by Nippon Coke and Engineering Co., Ltd.) and dry mixed at room temperature for 10 minutes.
[0084] [Table 1]
[0085] The resulting mixture was heat-treated in an electric tube furnace for 1 hour at the temperature shown in Table 2 under a nitrogen gas atmosphere. , multiple A composite carbon material or carbon material was obtained. Various physical properties were measured for the obtained composite carbon material. The results are shown in Table 2. In Table 2, "none" in the heat treatment step column means that the corresponding heat treatment step was not performed.
[0086] [Table 2]
[0087] In addition, an electric double layer capacitor was fabricated using the obtained composite carbon material and evaluated. The results are shown in Table 3.
[0088] [Table 3] [Explanation of symbols]
[0089] 1: Upper lid 2: O-ring 3: Current collector 4: Insulator 5: Container 6: Leaf spring 7: Electrode 8: Separator
Claims
1. A composite carbon material comprising a carbon material (A) and a carbonaceous coating layer (B) coating the surface of the carbon material, the composite carbon material being characterized in that formula 1 is satisfied. Formula 1: C / E≦7.5 C is the hydrogen molecule (H) desorbed from the composite carbon material, as measured by thermal desorption spectroscopy (TDS) at a temperature increase from 80° C. to 1400° C. 2 ) amount (μmol / g), E is the amount of carbon monoxide molecules (CO) (μmol / g) desorbed from the composite carbon material, as measured by thermal desorption spectroscopy (TDS) at a temperature increase from 500° C. to 800° C. Here, laser Raman spectroscopic imaging was performed using the Raman spectrum of the composite carbon material by microscopic Raman spectroscopic analysis with an excitation wavelength of 532.36 nm, and the R value (1350 cm ) obtained from 100 points randomly extracted from the region corresponding to the composite carbon material was -1 The peak intensity (I D ) and 1580 cm -1 The peak intensity (I G ) ratio (I D / I G ) is 0.50 or more and 1.50 or less (wherein the peak intensity indicates the height of the peak).
2. The composite carbon material according to claim 1, characterized in that it satisfies formula 2. Formula 2: C / D≦2.3 D is the number of carbon dioxide molecules (CO) desorbed from the composite carbon material, as measured by thermal desorption spectroscopy (TDS) at a temperature increase from 80° C. to 400° C. 2 ) amount (μmol / g).
3. 3. The composite carbon material according to claim 1 or 2, wherein formula 3 is satisfied. Formula 3: C / F≦6.0 F is the water molecule (H) desorbed from the composite carbon material, measured by thermal desorption spectroscopy (TDS) at a temperature increase from 80° C. to 400° C. 2 O) amount (μmol / g).
4. The composite carbon material according to any one of claims 1 to 3, wherein the C is 100 µmol / g or more and 1000 µmol / g or less.
5. The composite carbon material according to any one of claims 1 to 4, wherein E is 100 µmol / g or less.
6. Using the Raman spectrum of the composite carbon material by microscopic Raman spectroscopy with an excitation wavelength of 532.36 nm, laser Raman spectroscopic imaging was performed, and the R value (1350 cm) obtained from 100 points randomly extracted from the area corresponding to the composite carbon material was -1 The peak intensity (I D ) and 1580 cm -1 The peak intensity (I G ) ratio (I D / I G 6. The composite carbon material according to claim 1 , wherein the coefficient of variation of the peak intensity (peak intensity) is 0.60 or less.
7. The 50% particle size (D50) in the volume-based cumulative particle size distribution by the laser diffraction method is 2 to 30 μm, and the 400 tapping density is 0.05 g / cm 3 1.50g / cm or more 3 The composite carbon material according to any one of claims 1 to 6, wherein:
8. BET specific surface area is 700m 2 / g or more 2500m 2 The composite carbon material according to any one of claims 1 to 7, wherein the molecular weight is 1 / g or less.
9. 9. The composite carbon material according to claim 1, wherein (BET specific surface area of the composite carbon material) / (BET specific surface area of the carbon material (A)) is 0.50 or more and 1.00 or less.
10. The R value (1350 cm) obtained from the Raman spectrum of the carbon material (A) and the composite carbon material by micro-Raman spectroscopy -1 The peak intensity (I D ) and 1580 cm -1 The peak intensity (I G ) ratio (I D / I G 10. The composite carbon material according to claim 1, wherein (R value of the composite carbon material) / (R value of the carbon material (A)) is 0.50 or more and 1.50 or less.
11. An electrode material comprising the composite carbon material according to any one of claims 1 to 10.
12. An electrode for an electric double layer capacitor, comprising the electrode material according to claim 11.
13. 13. An electric double layer capacitor having electrodes immersed in an electrolyte, at least one of the electrodes being the electrode according to claim 12.
Citation Information
Patent Citations
Preparation method of graphene-modified activated carbon applicable to supercapacitor
CN103723720A
Multilayer electrode and supercapacitor including the electrode
JP2012114396A
Electrode for electrochemical capacitor and manufacturing method therefor
JP2014107361A
Methods for producing carbon material-graphene composite films
WO2018073691A1
Carbonaceous material and method for producing same
WO2018074303A1