Water-absorbent resin and its manufacturing method
By incorporating a hydrogel of recovered water-absorbing resin treated with polyvalent metal ions into the production process, the method enhances water absorption capacity and maintains resin properties, addressing inefficiencies and costs in existing recycling methods.
Patent Information
- Application Number
- JP2021002386
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-08
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2041-01-08
AI Technical Summary
Existing methods for recycling water-absorbing resins are inefficient, costly, and result in significant deterioration of physical properties, particularly when using decomposing agents or polyvalent metal salts, leading to low water-absorbing capacity.
A method involving the use of a hydrogel of recovered water-absorbing resin treated with polyvalent metal ions, which is added to various stages of the water-absorbing resin production process to remove absorbed water effectively, maintaining high productivity and minimizing property loss.
The method allows for the reuse of water-absorbing resins with improved water absorption capacity and reduced physical deterioration, achieved through simple and cost-effective processing without the need for decomposing agents.
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a water-absorbent resin, which reuses a water-absorbent resin attached to a production apparatus for the water-absorbent resin, or a water-absorbent resin recovered from a mixture containing the water-absorbent resin. [Background technology]
[0002] Water-absorbent resins are water-swellable, water-insoluble polymer gelling agents, and are used for various purposes, such as absorbent articles such as disposable diapers and sanitary napkins, soil water retention agents for agricultural and horticultural use, and industrial water-stopping agents. Partially neutralized salts of crosslinked polyacrylic acid are generally used as water-absorbent resins. Water-absorbent resins are produced through a process that includes a polymerization process of an aqueous solution of a monomer such as acrylic acid, an optional gel crushing process, a drying process, an optional crushing process and a classification process, an optional fine powder recovery process, a surface crosslinking process, an optional additive addition process, and the like, and aqueous solution polymerization or reversed-phase suspension polymerization is used as the polymerization method (Non-Patent Document 1).
[0003] Since water-absorbent resins tend to become sticky even with a small amount of moisture and can cause problems by adhering to equipment used in the production of the water-absorbent resins, it is known that the production equipment is washed with water (Patent Documents 1 to 3). During this process, the water-absorbent resin absorbs a large amount of water and forms a swollen gel.
[0004] As another example of generating swollen gel, a technique is known in which constituent materials are separated and collected by type from a complex containing a water-absorbent resin using water, and this technique is used in combination with a technique for reducing or eliminating the absorption power of the water-absorbent resin so as not to generate excessive swollen gel. Specifically, a method has been proposed in which the water-absorbent resin is solubilized with an acidic aqueous solution and an oxidizing agent such as ozone, or the water-absorbent resin is shrunk and solidified with a polyvalent metal salt such as a water-soluble calcium compound or an aqueous solution thereof, and materials other than the water-absorbent resin contained in the absorbent article are separated and collected (Patent Documents 4 to 10). Furthermore, a technique has been proposed in which the water-absorbent resin is decomposed and reused in the manufacturing process of the water-absorbent resin (Patent Document 11).
[0005] On the other hand, there are known techniques for recovering and reusing water-absorbent resin materials other than swollen gels. Specifically, there are known techniques for recovering and reusing fine powder of water-absorbent resin that is out of the desired size (Non-Patent Document 1, Patent Documents 12 to 20), undried coarse polymer gel that could not be dried as desired in the drying process (Patent Document 21), and the like. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2006-199862 A [Patent Document 2] International Publication No. 2020 / 038742 Brochure [Patent Document 3] JP 2013-076073 A [Patent Document 4] JP 2019-084470 A [Patent Document 5] JP 2017-128840 A [Patent Document 6] JP 2018-165423 A [Patent Document 7] JP 2019-076902 A [Patent Document 8] JP 2019-108639 A [Patent Document 9] JP 2019-108640 A [Patent Document 10] Japanese Patent Application Publication No. 04-317784 [Patent Document 11] International Publication No. 2020 / 213298 Brochure [Patent Document 12] Japanese Patent Application Publication No. 04-041532 [Patent Document 13] Japanese Patent Application Publication No. 04-227934 [Patent Document 14] Japanese Patent Application Publication No. 03-152104 [Patent Document 15] Japanese Patent Application Publication No. 11-106514 [Patent Document 16] Japanese Patent Application Publication No. 11-140194 [Patent Document 17] Japanese Patent Application Publication No. 11-254429 [Patent Document 18] Japanese Patent Application Publication No. 11-240959 [Patent Document 19] International Publication No. 2006 / 098271 Brochure [Patent Document 20] JP 2006-299234 A [Patent Document 21] Japanese Patent Application Publication No. 11-292919 [Non-patent literature]
[0007] [Non-Patent Document 1] Modern Superabsorbent Polymer Technology(1998)p69-103 Summary of the Invention [Problem to be solved by the invention]
[0008] When solubilizing water-absorbent resins, the effects of the decomposition agent used can make it difficult to treat wastewater containing the water-absorbent resin or to reuse the water-absorbent resin. In addition, when treating water-absorbent resins with acid, a large amount of costly organic acid is used. On the other hand, hydrogels produced by shrinking and solidifying water-absorbent resins with an aqueous solution of polyvalent metal salts such as water-soluble calcium compounds have a very low water absorption capacity and cannot easily recover their water-absorption performance, so there has been no method for reusing them.
[0009] Therefore, there is a demand for a simple method for reusing water-absorbent resins that have absorbed a large amount of water, which is inexpensive, highly productive, and causes little deterioration in the physical properties.
[0010] An object of one aspect of the present invention is to provide a method for producing a water-absorbent resin, which reuses a water-absorbent resin that has absorbed a large amount of water by a simple method that is inexpensive, has high productivity, and causes little deterioration in physical properties. [Means for solving the problem]
[0011] Means for Solving the Problems The present inventors have conducted intensive studies to solve the above problems, and as a result have found that, by adding a hydrogel of a recovered water absorbent resin treated with a polyvalent metal ion to a material to be treated in a production process of a water absorbent resin, a water absorbent resin that has absorbed a large amount of water can be reused by a simple method that is inexpensive, has high productivity, and is less susceptible to deterioration in physical properties.
[0012] That is, the method for producing a water absorbent resin according to one embodiment of the present invention is a method for producing a water absorbent resin, comprising a step of adding a hydrogel of a recovered water absorbent resin to a material to be treated in a production step of the water absorbent resin, and the hydrogel contains a polyvalent metal ion and has a solids-corrected CRC of 5 g / g or less.
[0013] Preferably, in the method for producing a water-absorbent resin according to one embodiment of the present invention, the hydrogel is added to a material to be treated in at least one of the following steps (1) to (6) included in the production process of the water-absorbent resin.
[0014] (1) Preparation of monomer aqueous solution (2) Polymerization process (3) Gel crushing step during or after polymerization (4) Drying process (5) Particle size adjustment process, fine powder recovery process, or fine powder granulation process after the drying process (6) Additive addition process or surface cross-linking process after the particle size adjustment process Preferably, in the method for producing a water-absorbing resin according to one embodiment of the present invention, the hydrogel is prepared by dispersing a mixture containing the recovered water-absorbing resin in water, and shrinking the swollen gel formed by swelling the recovered water-absorbing resin with a polyvalent metal ion.
[0015] Preferably, in the method for producing a water absorbent resin according to one embodiment of the present invention, the hydrogel is obtained by washing an apparatus used in a production step of the water absorbent resin with water, and shrinking the swollen gel with a polyvalent metal ion.
[0016] Preferably, in the method for producing a water-absorbent resin according to one embodiment of the present invention, the hydrogel is a dried product obtained by shrinking the swollen gel with a polyvalent metal ion and drying the gel.
[0017] Preferably, in the method for producing a water-absorbent resin according to one embodiment of the present invention, the hydrogel has a mass median particle size of 10 μm to 600 μm.
[0018] Preferably, in the method for producing a water-absorbent resin according to one embodiment of the present invention, a mass ratio of a solid content of the hydrogel to a solid content of a monomer used in a production step of the water-absorbent resin is 0.01-50:99.99-50.
[0019] Preferably, in the method for producing a water-absorbent resin according to one embodiment of the present invention, the hydrogel has a yellowness index (YI) of 20 or less.
[0020] Preferably, in the method for producing a water-absorbent resin according to an embodiment of the present invention, the hydrogel does not contain at least one or more polymer decomposing agents selected from an oxidizing agent and a reducing agent, or when the hydrogel contains the polymer decomposing agent, the content of the polymer decomposing agent is 1000 ppm or less.
[0021] Preferably, in the method for producing a water absorbent resin according to one embodiment of the present invention, the polymer decomposer is at least one selected from the group consisting of L-ascorbic acid (salt), sulfite (hydrogen) salt, chlorite, hypochlorite, and hydrogen peroxide.
[0022] Preferably, in the method for producing a water-absorbent resin according to one embodiment of the present invention, a coloring inhibitor is added in at least one step of the production process of the water-absorbent resin.
[0023] The water-absorbent resin according to one embodiment of the present invention is a water-absorbent resin obtained by adding a hydrogel of a recovered water-absorbent resin to a material to be treated in a production process of an aqueous resin, and the hydrogel contains polyvalent metal ions and has a solids-corrected CRC of 5 g / g or less.
[0024] Preferably, the water-absorbent resin according to one embodiment of the present invention comprises a fine powder granule containing a water-absorbent resin fine powder and the hydrogel.
[0025] Preferably, the water absorbent resin according to one embodiment of the present invention does not contain at least one or more polymer decomposing agents selected from an oxidizing agent and a reducing agent, or when the water absorbent resin contains the polymer decomposing agent, the content of the polymer decomposing agent is 100 ppm or less.
[0026] Preferably, in the water absorbent resin according to one embodiment of the present invention, the polymer decomposer is at least one selected from the group consisting of L-ascorbic acid (salt), sulfite (hydrogen) salt, chlorite, hypochlorite, and hydrogen peroxide. Effect of the Invention
[0027] According to the present invention, it is possible to provide a method for producing a water-absorbent resin, which allows the water-absorbent resin that has absorbed a large amount of water to be reused by a simple method that is inexpensive, has high productivity, and causes little deterioration in physical properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] Hereinafter, a method for producing a water-absorbent resin according to one embodiment of the present invention will be described in detail, but the scope of the present invention is not limited to these descriptions, and other than the following examples, the present invention may be modified and embodied as appropriate within the scope of the present invention. Specifically, the present invention is not limited to the following embodiments, and various modifications are possible within the scope of the claims, and embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention.
[0029] [1] Definitions of terms (1-1) Water-absorbing resin In the present invention, the term "water-absorbent resin" refers to a water-swellable, water-insoluble polymer gelling agent, which is generally in powder form. "Water-swellable" means that the absorption capacity without load (hereinafter, sometimes referred to as "Centrifuge Retention Capacity (CRC)") defined in WSP241.3(10) is 5 g / g or more. "Water-insoluble" means that the soluble content (hereinafter, sometimes referred to as "Extr") defined in WSP (Worldwide Strategic Partners) 270.3(10) is 50 mass% or less.
[0030] The "water absorbent resin" is preferably a hydrophilic crosslinked polymer obtained by crosslinking and polymerizing an unsaturated monomer having a carboxyl group, but the entire amount, i.e., 100% by mass, does not need to be a crosslinked polymer, and additives and the like can be contained within a range that satisfies the required performance such as the CRC and Extr.
[0031] (1-2) Acrylic acid (salt) monomers, polyacrylic acid (salt) water-absorbing resins In this specification, "acrylic acid (salt)" means acrylic acid and / or its salt, and "acrylic acid (salt)-based monomer" means a monomer containing 50 mol% or more of acrylic acid (salt) with respect to the total monomers excluding crosslinking agents. In this specification, "polyacrylic acid (salt)-based water absorbent resin" means a polymer made from acrylic acid (salt). In other words, "polyacrylic acid (salt)-based water absorbent resin" is a polymer having a structural unit derived from acrylic acid (salt) and having a graft component as an optional component.
[0032] Specifically, the polyacrylic acid (salt)-based water absorbent resin is a polymer containing preferably 50 mol % or more, more preferably 70 mol % or more, even more preferably 90 mol % or more, and preferably 100 mol % or less, particularly preferably substantially 100 mol % of acrylic acid (salt) relative to the portion of monomers participating in the polymerization reaction excluding an internal crosslinking agent.
[0033] (1-3) "EDANA" and "WSP" "EDANA" is an abbreviation for European Disposables and Nonwovens Associations. "WSP" is an abbreviation for Worldwide Strategic Partners, and indicates the global standard measurement method for water-absorbent resins provided by EDANA. In this specification, the physical properties of water-absorbent resins are measured in accordance with the original WSP (revised in 2010). In this specification, unless otherwise specified, the measurement methods in the following examples are followed.
[0034] (1-4) "CRC" (WSP241.3(10)) "CRC" is an abbreviation of Centrifuge Retention Capacity, and means the absorption capacity of a water-absorbent resin under no pressure. Specifically, 0.2 g of the water-absorbent resin is placed in a nonwoven bag, and then immersed in a large excess of 0.9% by mass sodium chloride aqueous solution for 30 minutes to allow the water-absorbent resin to freely swell, and then dehydrated using a centrifuge (centrifugal force: 250 G), and the absorption capacity (unit: g / g) is calculated by the following formula. CRC[g / g]=(m wi -m b -m si ) / m si m wi : Mass of the bag containing the water-absorbent resin after the test [g] m b : Mass of the bag after testing without using water-absorbent resin [g] m si : Mass of water-absorbent resin before test [g] In the present invention, the hydrogel is also si The CRC was measured after changing m to 1 g. The "solid content corrected CRC" is a theoretical value of the CRC measured for a water absorbent resin with a solid content of 100% by mass, calculated from the CRC of the water absorbent resin containing water. si Calculate by substituting the sample solid content [g], calculated as (sample mass [g]) x (solid content [mass %]), into the formula.
[0035] Furthermore, the "Solid content corrected CRC (6hr)" was obtained by changing the immersion time from 30 minutes to 6 hours in the above "Solid content corrected CRC".
[0036] (1-5) "Extr" (WSP270.3(10)) "Extr" is an abbreviation of Extractables, and means the water-soluble portion of the water-absorbent resin, i.e., the amount of water-soluble components. Specifically, it means the amount of dissolved polymer (unit: mass%) after adding 1.0 g of water-absorbent resin to 200 ml of 0.9 mass% sodium chloride aqueous solution and stirring at 250 rpm for 1 hour or 16 hours. The amount of dissolved polymer is measured by pH titration.
[0037] (1-6) "Moisture Content" (WSP230.3(10)) "Moisture Content" means the moisture content of the water-absorbent resin. Specifically, it means a value (unit: mass%) calculated from the drying loss when 4.0 g of the water-absorbent resin is dried at 105°C for 3 hours. In the present invention, the measurement was performed by changing the amount of water-absorbent resin to 1.0 g and the drying temperature to 180°C. The measurement was also performed for hydrogels as well as water-absorbent resins. The solid content [mass%] is calculated by 100-(moisture content [mass%]).
[0038] (1-7) [Mass average particle size and logarithmic standard deviation] The mass-average particle diameter (D50, unit: μm) of the water absorbent resin and the logarithmic standard deviation (σζ) indicating the narrowness of the particle size distribution of the water absorbent resin particles were measured in accordance with the measurement method of "(3) Mass-Average Particle Diameter (D50) and Logarithmic Standard Deviation (σζ) of Particle Diameter Distribution" described in U.S. Patent No. 7638570. For the measurement of fine powder of the water absorbent resin or hydrogel, a sieve with a small mesh size is appropriately added for measurement.
[0039] (1-8) "Yellowness (YI)" "Yellowness index (YI)" is an abbreviation for Yellow Index, and refers to an index of the degree of coloration, particularly the degree of yellowing, of a water-absorbent resin. More specifically, it is a value measured by the method described in European Patent Nos. 942014 and 1108745.
[0040] [2] Manufacturing method of water-absorbent resin The method for producing a water-absorbent resin of the present invention is a method for producing a water-absorbent resin comprising a step of adding a hydrogel of a recovered water-absorbent resin to a material to be treated in a water-absorbent resin production process, and the hydrogel comprises polyvalent metal ions and has a solids-corrected CRC of 5 g / g or less. Here, the "recovered water-absorbent resin" is not particularly limited as long as it is a water-absorbent resin to be reused, but may be, for example, a water-absorbent resin attached to a water-absorbent resin production device or a water-absorbent resin recovered from a mixture containing a water-absorbent resin. The "water-absorbent resin" in the "recovered water-absorbent resin" means a water-swellable, water-insoluble polymer gelling agent, as in the "water-absorbent resin" produced by the method for producing a water-absorbent resin comprising a step of adding a hydrogel of the recovered water-absorbent resin, and may be as defined in the above-mentioned "Definition of Terms". The "water-absorbent resin" in the "recovered water-absorbent resin" may comprise a polyacrylic acid (salt)-based water-absorbent resin. The manufacturing method is not particularly limited, and may be a method of polymerizing the same monomer as the water absorbent resin obtained by the manufacturing method of the water absorbent resin including the step of adding the hydrogel of the recovered water absorbent resin in the presence of the same internal crosslinking agent. The "water absorbent resin" in the "recovered water absorbent resin" and the water absorbent resin to which the hydrogel of the recovered water absorbent resin is added may be the same or different. In the present invention, the "hydrogel of the recovered water absorbent resin" includes the recovered water absorbent resin in a gel state that has absorbed water, or a dried body obtained by drying the recovered water absorbent resin in a gel state to a desired solid content. The hydrogel may contain a polyvalent metal ion. The embodiment in which the hydrogel contains a polyvalent metal ion is not particularly limited, and may be, for example, a hydrogel obtained by shrinking the water absorbent resin that has absorbed water with a polyvalent metal ion. The hydrogel has a solid content corrected CRC of 5 g / g or less.
[0041] In addition, the object to be treated in the manufacturing process of the water-absorbent resin refers to an object being treated at the time of adding the hydrogel in the manufacturing process. More specifically, in the following process (1), for example, it is a monomer aqueous solution, in the following process (2), for example, it is a reaction mixture during polymerization, in the following process (3), for example, it is a reaction mixture during polymerization or a hydrogel-like crosslinked polymer, in the following process (4), for example, a particulate hydrogel-like crosslinked polymer, in the following process (5), for example, a dried polymer, and in the following process (6), for example, a water-absorbent resin powder or a surface-crosslinked water-absorbent resin powder.
[0042] In one embodiment of the present invention, the manufacturing process of the water-absorbent resin is not particularly limited, and various steps in the manufacturing method of the water-absorbent resin described in Non-Patent Document 1 and the like can be applied. In addition, the polymerization form of the water-absorbent resin is not particularly limited, and the water-absorbent resin may be manufactured by various polymerization forms such as aqueous solution polymerization, reversed-phase suspension polymerization, gas-phase droplet polymerization, and liquid-phase droplet polymerization, and may be continuous polymerization or batch polymerization. In the present invention, the hydrogel containing polyvalent metal ions and having a solid content corrected CRC of 5 g / g or less is added in any of the steps included in the manufacturing process of the water-absorbent resin, and the hydrogel obtained by treating the water-absorbent resin that has absorbed a large amount of water with a polyvalent metal salt is used as a part of the raw material of the water-absorbent resin.
[0043] In one embodiment of the present invention, the hydrogel containing polyvalent metal ions and having a solids-corrected CRC of 5 g / g or less is added to a material to be treated in at least one of the following steps (1) to (6) and another step (7) included in a production process of a water absorbent resin.
[0044] (1) Preparation of monomer aqueous solution (2) Polymerization process (3) Gel crushing step during or after polymerization (4) Drying process (5) Particle size adjustment process, fine powder recovery process, or fine powder granulation process after the drying process (6) Additive addition process or surface cross-linking process after the particle size adjustment process (7) Other processes Each step will be described in turn below.
[0045] (2-1) Preparation of an aqueous monomer solution and adding the hydrogel to the solution This step is a step of preparing an aqueous monomer solution containing a monomer and at least one kind of internal cross-linking agent. Although a slurry liquid of the monomer can be used within a range that does not affect the water absorption performance of the water absorbing agent obtained as a final product, for the sake of convenience, the aqueous monomer solution in this specification also includes the slurry liquid of the monomer.
[0046] (monomer) Examples of the monomer used in the present invention include unsaturated monomers including acrylic acid, 2-(meth)acrylamido-2-methylpropanesulfonic acid, 2-(meth)acryloylethanesulfonic acid, (meth)acrylamide, etc. The monomer also includes water-soluble or hydrophobic unsaturated monomers. Among them, acrylic acid (salt) is preferred. Acrylic acid (salt) may be used in combination with other monomers. In this case, the amount of acrylic acid (salt) used is preferably 50 mol% or more, more preferably 70 mol% or more, even more preferably 90 mol% or more, and particularly preferably substantially 100 mol% based on the total monomers excluding the crosslinking agent.
[0047] In the present invention, when acrylic acid (salt) is used, the neutralization rate is preferably 10 mol% or more, more preferably 40 mol% or more, even more preferably 50 mol% or more, and particularly preferably 60 mol% or more, and is preferably 90 mol% or less, more preferably 85 mol% or less, even more preferably 80 mol% or less, and particularly preferably 75 mol% or less, based on the acid group of the monomer. By setting the neutralization rate within the range, the deterioration of the water absorption performance of the water absorbent resin can be suppressed. Neutralization may be performed at any time before, during, or after polymerization. The neutralization rate is applied to any of the neutralizations before, during, and after polymerization described above. The same is also applied to the water absorbent as a final product.
[0048] (Internal crosslinking agent) In the preferred manufacturing method of the present invention, an internal crosslinking agent is used. Specific examples of the internal crosslinking agent include N,N'-methylenebis(meth)acrylamide, (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, trimethylolpropane di(meth)acrylate, trimethylolpropane tri(meth)acrylate, glycerin tri(meth)acrylate, poly(meth)allyloxyalkane, (poly)ethylene glycol diglycidyl ether, and glycerol diglycidyl ether. At least one type of internal crosslinking agent is selected from these internal crosslinking agents in consideration of reactivity and the like. In the present invention, from the viewpoint of the water absorption performance of the water-absorbing resin, an internal crosslinking agent having two or more polymerizable unsaturated groups is preferably selected, and an internal crosslinking agent having two or more polymerizable unsaturated groups having a (poly)alkylene glycol structure is more preferably selected. Specific examples of the polymerizable unsaturated group include an allyl group and a (meth)acrylate group. Among these, a (meth)acrylate group is preferred. The amount of the internal crosslinking agent used is preferably 0.0001 mol % or more, more preferably 0.001 mol % or more, and even more preferably 0.01 mol % or more, and is preferably 10 mol % or less, more preferably 5 mol % or less, and even more preferably 1 mol % or less, based on the monomers excluding the internal crosslinking agent.
[0049] (Substance added to the monomer aqueous solution (third component)) In the step of preparing the aqueous monomer solution, a substance (third component) other than the monomer and the crosslinking agent can be added to the aqueous monomer solution from the viewpoint of improving the physical properties of the water absorbent resin. As the third component, a water-soluble polymer such as starch or polyvinyl alcohol, a chain transfer agent, a chelating agent, etc. can be added, but in a preferred embodiment of the present invention, the hydrogel can be added to the aqueous monomer solution as the third component.
[0050] By adding the hydrogel in the preparation process of the aqueous monomer solution, the viscosity of the aqueous monomer solution is increased, and foaming polymerization can be promoted in the subsequent polymerization process. In addition, the hydrogel can be uniformly fixed inside the water absorbent resin, and the water absorption performance of the hydrogel that has been reduced or lost can be restored.
[0051] The amount of the third component, such as the hydrogel, added is preferably 50% by mass or less in total, more preferably 20% by mass or less, even more preferably 10% by mass or less, particularly preferably 5% by mass or less, and is preferably 0% by mass or more, more preferably more than 0% by mass, relative to the aqueous monomer solution.
[0052] The amount of the hydrogel added is the solid content, and the lower limit is preferably 0.01% by mass, more preferably 0.1% by mass, even more preferably 0.2% by mass, particularly preferably 0.5% by mass, and most preferably 1% by mass, based on the total mass of the solid content of the monomer excluding the internal crosslinking agent. The upper limit is preferably 50% by mass, more preferably 40% by mass, even more preferably 30% by mass, particularly preferably 20% by mass, and most preferably 1% by mass. The amount of the hydrogel added in each of the subsequent steps is the same.
[0053] (Monomer component concentration) The above-mentioned substances and components (including the monomer, the internal crosslinking agent, and the third component; hereinafter, these may be referred to as "monomer components") are selected according to the purpose, and the amounts of each are specified so as to satisfy the above-mentioned ranges, and then mixed together to prepare an aqueous monomer solution. In the present invention, the monomer can be made into an aqueous solution, or a mixed solution of water and a hydrophilic solvent can be used.
[0054] In addition, the total concentration of the monomer components in the aqueous monomer solution is, from the viewpoint of the physical properties of the water absorbent resin, preferably 10 mass % or more, more preferably 20 mass % or more, even more preferably 30 mass % or more, and is preferably 80 mass % or less, more preferably 75 mass % or less, even more preferably 70 mass % or less.
[0055] (2-2) Polymerization step and addition of the hydrogel to the step (polymerization form) Examples of the polymerization form applicable to the present invention include aqueous solution polymerization, reversed-phase suspension polymerization, spray polymerization, droplet polymerization, bulk polymerization, precipitation polymerization, etc. Among them, from the viewpoint of ease of control of polymerization and water absorption performance of the water absorbent resin, preferably aqueous solution polymerization or reversed-phase suspension polymerization, more preferably aqueous solution polymerization, and further preferably continuous aqueous solution polymerization is selected.
[0056] Preferred forms of the continuous aqueous solution polymerization include high-temperature initiation polymerization, high-concentration polymerization, and foaming polymerization. "High-temperature initiation polymerization" refers to a polymerization form in which the temperature of the aqueous monomer solution at the start of polymerization is preferably 35°C or higher, more preferably 40°C or higher, even more preferably 45°C or higher, and particularly preferably 50°C or higher, and is preferably below the boiling point of the aqueous monomer solution. "High-concentration polymerization" refers to a polymerization form in which the monomer concentration at the start of polymerization is preferably 30% by mass or higher, more preferably 35% by mass or higher, even more preferably 40% by mass or higher, and particularly preferably 45% by mass or higher, and is preferably below the saturation concentration of the aqueous monomer solution. "Foaming polymerization" refers to a polymerization form in which the aqueous monomer solution containing a foaming agent or bubbles is polymerized. These polymerization forms may be carried out alone, or two or more of them may be used in combination.
[0057] (Polymerization initiator) The polymerization initiator used in the present invention can be selected from one or more of those used in the production of ordinary water-absorbing resins according to the type of monomer to be polymerized and the polymerization conditions. Examples of the polymerization initiator include a thermal decomposition initiator and a photodecomposition initiator. The amount of the polymerization initiator used is preferably 0.001 mol% or more, more preferably 0.01 mol% or more, and preferably 1 mol% or less, more preferably 0.5 mol% or less, and even more preferably 0.1 mol% or less, based on the monomer excluding the internal crosslinking agent. In the present invention, the polymerization reaction may be initiated by irradiation with active energy rays such as radiation, electron beams, and ultraviolet rays. In addition, irradiation with active energy rays and the polymerization initiator may be used in combination.
[0058] (Addition of the third component during polymerization) In one embodiment of the present invention, the third component other than the monomer and the crosslinking agent can be added at any stage of a polymerization rate of 0 to 100% in the polymerization step.
[0059] In a preferred embodiment of the present invention, the hydrogel can be added as a third component to the aqueous monomer solution (polymerization rate: 0%) immediately before the start of the polymerization reaction, or to the aqueous monomer solution and / or polymer gel (polymerization rate: more than 0% and less than 100%) in which the polymerization reaction is proceeding in a polymerization apparatus. When the hydrogel is added to the aqueous monomer solution (polymerization rate: 0%) in the polymerization apparatus, there is no substantial difference from the addition to the monomer preparation step. Even when the hydrogel is added to the aqueous monomer solution or polymer gel (polymerization rate: more than 0% and less than 100%) in which polymerization is proceeding, the hydrogel can be regenerated and uniformly fixed inside the water absorbent resin. Preferably, the hydrogel is added to the polymerization apparatus when the polymerization rate is 50% or more, further 60% or more, or 70% or more.
[0060] (2-3) A gel crushing step during or after polymerization and addition of the hydrogel to the step This step is a gel crushing step for kneading or crushing the hydrogel crosslinked polymer (hereinafter referred to as "hydrogel") during and / or after the polymerization reaction in the polymerization step, to obtain particulate hydrogel finely granulated to a predetermined size. The gel crusher that can be used in the present invention is not particularly limited, and examples thereof include screw extruders such as kneaders and meat choppers, and cutter mills.
[0061] For uniform and efficient drying, the water content of the particulate hydrogel is preferably 30% by mass or more, more preferably 45% by mass or more, and is preferably 70% by mass or less, more preferably 55% by mass or less.
[0062] In one embodiment of the present invention, the hydrogel can be added during the gel crushing step.
[0063] (2-4) Drying step and adding the hydrogel to the drying step This step is a step of drying the particulate hydrogel obtained directly through the polymerization step (2-2) or the particulate hydrogel obtained through the step (2-3), and is a step of drying the particulate hydrogel (a mixture of the particulate hydrogel and the granulated gel when a granulated gel (fine powder granulated gel) is further added to the particulate hydrogel) to a desired solid content to obtain a dried polymer. The solid content of the dried polymer, calculated from the loss on drying when 1 g of powder or particles of the dried polymer is dried at 180°C for 3 hours, is preferably 80% by mass or more, more preferably 85% by mass or more, even more preferably 90% by mass or more, particularly preferably 92% by mass or more, and is preferably 99% by mass or less, even more preferably 98% by mass or less, particularly preferably 97% by mass or less.
[0064] Examples of the drying method in the drying step include heat drying, hot air drying, reduced pressure drying, fluidized bed drying, infrared drying, microwave drying, drying by azeotropic dehydration with a hydrophobic organic solvent, high humidity drying using high temperature water vapor, and stirring drying in which the material to be dried is moved while being dried. Among these, stirring drying and hot air drying are preferred from the viewpoint of drying efficiency. Examples of stirring drying include a paddle dryer or a rotary drum type dryer. In addition, hot air drying is preferably performed with a ventilation band type dryer that performs hot air drying on a ventilation belt.
[0065] In the present invention, the drying temperature, i.e., the temperature of the hot air, is preferably 120° C. or higher, more preferably 130° C. or higher, and even more preferably 150° C. or higher, and is preferably 250° C. or lower, more preferably 230° C. or lower, and even more preferably 200° C. or lower, taking into consideration the drying efficiency. The drying time is preferably 10 minutes or more, more preferably 20 minutes or more, and even more preferably 30 minutes or more, and is preferably 2 hours or less, more preferably 1.5 hours or less, and even more preferably 1 hour or less.
[0066] In a preferred embodiment of the present invention, the hydrogel can be added in the drying step. The hydrogel can be added in the drying step or a step before that, and then dried at the high temperature, so that the hydrogel can be fixed in the water-absorbent resin.
[0067] (2-5) A particle size adjustment process, a fine powder recovery process or a fine powder granulation process after the drying process, and addition of the hydrogel to the process This step may be unnecessary when the monomer is polymerized in droplet form (several hundred microns or several mm) during polymerization, such as in reverse phase suspension polymerization or gas phase droplet polymerization. However, in most other polymerization forms, including aqueous solution polymerization, it is preferable to carry out a particle size adjustment step, a fine powder recovery step, or a fine powder granulation step after the drying step.
[0068] (Crushing and classification) As the particle size adjustment step, pulverization and / or classification of the dried polymer obtained by drying is applied, and pulverization and / or classification after drying may be performed once, or may be performed again after the surface crosslinking described later. Fine powder generated by pulverization or classification may be granulated or collected.
[0069] Examples of the pulverizer used in the pulverization include high-speed rotary pulverizers such as roll mills, hammer mills, screw mills, and pin mills, as well as vibration mills, knuckle-type pulverizers, and cylindrical mixers. Among these, from the viewpoint of pulverization efficiency, a roll mill is preferably selected. Moreover, a plurality of these pulverizers can be used in combination.
[0070] The particle size adjustment method in the classification step includes sieve classification using a JIS standard sieve (JIS Z8801-1 (2000)) and air flow classification. Among them, sieve classification is preferably selected from the viewpoint of classification efficiency. Note that, from the viewpoint of ease of pulverization, a classification step may be additionally performed before the pulverization step.
[0071] (Preferable particle size) The particle size distribution of the water-absorbent resin is preferably such that the mass median particle diameter (D50) is 300 μm or more and 600 μm or less, and the ratio of particles less than 150 μm is 5 mass% or less. The upper limit of the mass median particle diameter (D50) is more preferably 500 μm, further preferably 450 μm, and particularly preferably 400 μm. The ratio of particles less than 150 μm is more preferably 4 mass% or less, further preferably 3 mass% or less, and particularly preferably 2 mass% or less. The logarithmic standard deviation (σζ), which indicates the narrowness of the particle size distribution, is preferably 0.20 or more, more preferably 0.25 or more, and further preferably 0.27 or more, and is preferably 0.50 or less, more preferably 0.40 or less, and further preferably 0.35 or less. The smaller the logarithmic standard deviation (σζ) of the particle size distribution, the more uniform the particle size becomes, and the less the particles segregate. It is preferable that the mass median particle diameter (D50) and the proportion of particles less than 150 μm are each satisfied, and it is more preferable that the mass median particle diameter (D50), the proportion of particles less than 150 μm, and the logarithmic standard deviation are each satisfied, and these can be appropriately combined within the above-mentioned respective ranges.
[0072] The above-mentioned particle size is applied not only to the water absorbent resin after the pulverization step and the classification step, but also to the water absorbing agent as a final product. Therefore, when surface crosslinking is performed, it is preferable to perform surface crosslinking treatment in the surface crosslinking step so as to maintain the particle size in the above range adjusted in the water absorbent resin before surface crosslinking, and it is more preferable to adjust the particle size by providing a sizing step after the surface crosslinking step.
[0073] (Fine powder collection) In the manufacturing method according to one embodiment of the present invention, it is preferable to include a classification step (including a second classification step after a surface cross-linking step; the same applies below) after the drying step, and after separating the water-absorbent resin fine powder that has passed through a standard sieve with an opening of 150 μm in the classification step, to recover (reuse) the water-absorbent resin fine powder or its water additive in a step before the drying step. The fine powder recovery step refers to a step of separating the water-absorbent resin fine powder (particularly, containing 70 mass % or more of particles with a particle diameter of 150 μm or less; hereinafter, sometimes referred to as "fine powder") generated in the drying step and, if necessary, the pulverization and classification steps, and then recovering the water-absorbent resin fine powder as it is or after hydration or granulation in a step before the drying step, preferably recovering the water-absorbent resin fine powder in a polymerization step, a gel pulverization step, or a drying step.
[0074] By collecting the fine powder, particularly by granulating the fine powder, and further by granulating the fine powder with water, the particle size of the water absorbent resin can be controlled and the water absorption rate of the water absorbent resin obtained by this step can be further improved.
[0075] A suitable fine powder recovery method in the present invention is a method of mixing water-absorbent resin fine powder or its hydrate or granulated material, and inorganic fine particles, etc., as necessary, in a monomer aqueous solution before polymerization, a hydrogel during polymerization, or a dryer in a drying process. A fine powder recovery method in a monomer aqueous solution before polymerization is exemplified in International Publication Nos. 92 / 001008 and 92 / 020723, a fine powder recovery method in a hydrogel during polymerization is exemplified in International Publication Nos. 2007 / 074167, 2009 / 109563, 2009 / 153196, and 2010 / 006937, and a fine powder recovery method in a drying process (dryer) is exemplified in U.S. Patent No. 6,228,930, etc. These fine powder recovery methods are preferably applied as the fine powder recovery method in the present invention.
[0076] (Addition of the hydrogel to the particle size adjustment process, the fine powder recovery process, or the fine powder granulation process) In a preferred embodiment of the present invention, the hydrogel can be added in the particle size adjustment step, the fine powder recovery step or the fine powder granulation step.
[0077] In particular, by adding the hydrogel together with the fine powder in the fine powder recovery process or the fine powder granulation process, the hydrogel can be uniformly fixed inside the water-absorbent resin, and the water-absorbing performance of the hydrogel that has decreased or disappeared can be restored.
[0078] The mass ratio of the fine powder to the hydrogel can be appropriately selected from the range of 100:0 to 1:99, preferably 10:90 to 90:10.
[0079] (2-6) Additive addition step or surface crosslinking step after the particle size adjustment step of the water absorbent resin, and addition of the hydrogel to the step (Surface crosslinking process) The water-absorbent resin particles obtained through the above-mentioned steps are preferably further subjected to a crosslinking treatment on the surface of the water-absorbent resin particles to increase the crosslinking density in the vicinity of the surface and improve various physical properties of the water-absorbent resin. In the present invention, as the surface crosslinking agent used in the surface crosslinking step, from the viewpoint of the handling of the surface crosslinking agent and the water absorption performance of the water-absorbent resin, an organic compound that is preferably a surface crosslinking agent having two or more functional groups that react with a carboxyl group and forms a covalent bond is selected.
[0080] More specific examples of the surface crosslinking agent include polyhydric alcohol compounds such as (mono-, di-, tri-, tetra-, poly)ethylene glycol, 1,3-propanediol, propylene glycol, butanediol, pentanediol, and hexanediol; alkylene carbonate compounds such as 1,3-dioxolan-2-one (ethylene carbonate) and 4-methyl-1,3-dioxolan-2-one; (mono-, di-, tri-, poly)ethylene glycol diglycidyl ether, (poly)glycerol polyglycidyl etherate polyhydric glycidyl compounds, oxetane compounds, vinyl ether compounds, and cyclic urea compounds.
[0081]
[0223] The amount of the surface crosslinking agent to be used, or the total amount thereof when a plurality of kinds are used, is preferably 0.01 parts by mass or more, and preferably 10 parts by mass or less, more preferably 5 parts by mass or less, and further preferably 2 parts by mass or less, relative to 100 parts by mass of a water absorbent resin before surface crosslinking.
[0082] The surface crosslinking agent is preferably added as an aqueous solution to the water absorbent resin before surface crosslinking. In this case, the amount of water used is preferably 0.1 parts by mass or more, more preferably 0.3 parts by mass or more, and even more preferably 0.5 parts by mass or more, and is preferably 20 parts by mass or less, more preferably 15 parts by mass or less, and even more preferably 10 parts by mass or less, relative to 100 parts by mass of the water absorbent resin before surface crosslinking. In addition, a hydrophilic organic solvent can be used in combination with the water as necessary to prepare the surface crosslinking agent solution. In this case, the amount of the hydrophilic organic solvent used is preferably 5 parts by mass or less, more preferably 3 parts by mass or less, and even more preferably 1 part by mass or less, relative to 100 parts by mass of the water absorbent resin before surface crosslinking. The temperature of the surface crosslinking agent solution is preferably 0°C to the boiling point, more preferably 5 to 50°C, and even more preferably 10 to 30°C, from the viewpoint of mixability and stability. In addition, the temperature of the water absorbent resin before mixing is preferably in the range of 0 to 80°C, more preferably 40 to 70°C, from the viewpoint of mixability.
[0083] The method of adding the surface cross-linking agent is preferably a method of preliminarily mixing the surface cross-linking agent with water and / or a hydrophilic organic solvent as required, and then spraying or dropping the surface cross-linking agent mixed with water and / or a hydrophilic organic solvent as required onto the water absorbent resin, and more preferably a spraying method. The size of the sprayed droplets is preferably 1 to 300 μm, more preferably 10 to 200 μm on average.
[0084] The water absorbent resin after the addition of the surface cross-linking agent is preferably heat-treated. The heating temperature when the heat treatment is performed is preferably 150° C. or higher, more preferably 170° C. or higher, and even more preferably 180° C. or higher, and is preferably 250° C. or lower, more preferably 230° C. or lower, from the viewpoints of the type and amount of the surface cross-linking agent and the water absorption performance of the water absorbent resin. The heating time is preferably at least 5 minutes, more preferably at least 7 minutes.
[0085] (Additive addition process) This step is a step of adding an additive to a water absorbent resin after surface crosslinking, before surface crosslinking or during surface crosslinking, preferably a water absorbent resin after surface crosslinking, in order to impart various functions to the water absorbent resin, and is composed of one or more steps.
[0086] As the additive, at least one compound selected from the group consisting of liquid permeability improvers, fluidity improvers during moisture absorption, coloring inhibitors, powder flow control agents, polyvalent metal salts, cationic polymers, inorganic fine particles, chelating agents, reducing agents, hydroxycarboxylic acid compounds, surfactants, compounds having phosphorus atoms, oxidizing agents, organic powders such as metal soaps, deodorants, antibacterial agents, pulp and thermoplastic fibers, and aromatic substances such as terpene-based aromatic compounds and phenol-based aromatic compounds can be used, and two or more types can be used in combination as necessary. The amount of the additive added is appropriately set depending on the compound selected. A coloring inhibitor is added in the manufacturing process of the water absorbent resin, When a polyvalent metal salt is used, the polyvalent metal cation of the polyvalent metal salt is preferably divalent or more, more preferably divalent or more and tetravalent or less, and even more preferably trivalent or tetravalent. Examples of polyvalent metals that can be used include aluminum and zirconium.
[0087] When inorganic fine particles are used, examples of the inorganic fine particles include substances described in U.S. Patent No. 7,638,570. Among them, silicon dioxide is preferable from the viewpoint of improving liquid permeability.
[0088] When the inorganic fine particles have a primary particle diameter of less than 20 nm, they may be added in an amount of preferably 0 parts by mass or more, more preferably more than 0 parts by mass, and preferably less than 1.2 parts by mass, more preferably less than 1.0 parts by mass, and even more preferably less than 0.5 parts by mass, relative to 100 parts by mass of the water-absorbent resin. When the inorganic fine particles have a primary particle diameter of 20 nm or more, they may be added in an amount of preferably 0 parts by mass or more, more preferably more than 0 parts by mass, and preferably less than 2.0 parts by mass, more preferably less than 1.5 parts by mass, and even more preferably less than 1.0 parts by mass, relative to 100 parts by mass of the water-absorbent resin.
[0089] When an additive is added to a water-absorbent resin, if the additive is a liquid or a solution in an aqueous medium such as water, it is preferable to spray the liquid or solution onto the water-absorbent resin and apply a sufficient torque to uniformly and reliably mix the water-absorbent resin and the additive. On the other hand, if the additive is a solid such as a powder, it may be dry-blended with the water-absorbent resin, or an aqueous liquid such as water may be used as a binder.
[0090] (mixer) Specific examples of the device used for mixing the surface crosslinking agent, water (particularly granulation water), additives, and the hydrogel include an agitation mixer, a cylindrical mixer, a double-walled cone mixer, a V-shaped mixer, a ribbon mixer, a screw mixer, a flow type rotary disk mixer, an airflow type mixer, a double-arm kneader, an internal mixer, a grinding kneader, a rotary mixer, and a screw extruder. When an agitation mixer is used, the rotation speed is preferably 5 rpm or more, more preferably 10 rpm or more, and is preferably 10,000 rpm or less, more preferably 2,000 rpm or less.
[0091] The mixer can also be used in the fine powder granulation step.
[0092] (Addition of the hydrogel to the additive addition step or surface crosslinking step) In a preferred embodiment of the present invention, the hydrogel can be added to an additive addition step or a surface crosslinking step subsequent to a particle size adjustment step of a water-absorbent resin.
[0093] (2-7) Other processes In one embodiment of the present invention, the manufacturing process of the water absorbent resin may further include, in addition to the above-mentioned steps (1) to (6), at least one step selected from a transporting step, a storing step, a packaging step, a storage step, a foreign matter removing step (e.g., removing foreign matter with an iron remover or a color sorter), etc., as necessary.
[0094] (2-8) Amount of the hydrogel added to the production process of the water-absorbent resin The amount of the hydrogel to be added to a material to be treated in a production process of a water absorbent resin is appropriately selected depending on the purpose, and is a mass ratio to the solid content of a monomer excluding an internal crosslinking agent used in a production process of a water absorbent resin to which the hydrogel is added, of 0.01-50:99.99-50, preferably 0.1-40:99.9-60, further preferably 0.2-30:99.8-70, particularly preferably 0.5-20:99.5-80, or 1-15:99-85.
[0095] (2-9) The hydrogel to be added The hydrogel added to the object to be treated in the manufacturing process of the water absorbent resin in the present invention is not limited thereto, but in one embodiment, the hydrogel may be a contracted product obtained by dispersing a mixture containing the recovered water absorbent resin in water and contracting the swollen gel formed by swelling the recovered water absorbent resin with a polyvalent metal ion. When the mixture is a mixture containing other materials, the hydrogel may be the contracted product separated from the other materials. In such a case, it is preferable to disperse the mixture containing the recovered water absorbent resin and the other materials in water, contract the swollen gel formed by swelling the recovered water absorbent resin with a polyvalent metal ion, and then separate the contracted product obtained from the other materials. Here, examples of the other materials include pulp, adhesive, soil, sand, fertilizer, paper, etc. Water is used to separate the composite containing the other materials into their constituent materials, and a swollen gel is generated at that time. In another embodiment, the hydrogel may be a contracted product obtained by contracting a swollen gel obtained by washing an apparatus used in the manufacturing process of the water absorbent resin with water with a polyvalent metal ion. The device is not limited thereto, but is preferably, for example, a polymerization machine. Specific washing methods include, for example, showering with water or pouring water, and when the device is a container-shaped device, storing water for a certain period of time and then draining it. It is also preferable to drain the water from the swollen gel so that the swollen gel to which the polyvalent metal ions are added is not accompanied by excessive water. It is also preferable to crush the swollen gel so that the polyvalent metal ions and the swollen gel can be easily mixed, or so that the hydrogel can be easily added to the material to be treated in the manufacturing process of the water-absorbent resin. The swollen gel to be subjected to the shrinkage treatment is preferably of a size that can pass through a sieve with a mesh size of 20 mm, more preferably a sieve with a mesh size of 10 mm.
[0096] (Shrinkage treatment of swollen gel) In one embodiment of the present invention, the polyvalent metal ion used in the shrinking treatment of the swollen gel is not particularly limited. Specifically, the shrinking treatment of the swollen gel can be performed by mixing various salts of polyvalent metal ions with the swollen gel. Examples of polyvalent metal salts that can be used include aluminum salts, zinc salts, alkaline earth metal salts, and transition metal salts. These may be used alone or in combination of two or more. Examples of alkaline earth metal salts include salts of metals such as beryllium, magnesium, calcium, strontium, and barium. Examples of transition metal salts include salts of metals such as iron, cobalt, nickel, and copper. In a preferred embodiment, the polyvalent metal salt is at least one selected from the group consisting of calcium salts, magnesium salts, and aluminum salts.
[0097] Examples of polyvalent metal salts that can be suitably used in the present invention include aluminum chloride, polyaluminum chloride, aluminum sulfate, aluminum nitrate, potassium aluminum bisulfate, sodium aluminum bisulfate, potassium alum, ammonium alum, sodium alum, sodium aluminate, calcium chloride, calcium nitrate, magnesium chloride, magnesium sulfate, magnesium nitrate, and the like.
[0098] In the shrinkage treatment, the amount of the polyvalent metal salt in the mixture of the polyvalent metal salt and the recovered water absorbent resin is preferably 3 mmol or more, more preferably 4 mmol or more, and even more preferably 5 mmol or more per 1 g of solid content of the swollen gel. The upper limit of the amount of the polyvalent metal salt is not particularly limited, but is preferably 20 mmol or less, more preferably 15 mmol or less, per 1 g of solid content of the swollen gel. In the shrinkage treatment, if the amount of the polyvalent metal salt per 1 g of solid content of the swollen gel is 3 mmol or more, it is preferable because the shrinkage treatment is performed sufficiently. If the amount of the polyvalent metal salt per 1 g of solid content of the swollen gel is 20 mmol or less, there is no risk of the water absorption performance of the water absorbent resin decreasing.
[0099] The shrinkage treatment time from the start to the end of the shrinkage treatment can be appropriately set depending on the degree of dehydration of the recovered water absorbent resin that has absorbed the absorbed liquid. The shrinkage treatment time from the start to the end of the shrinkage treatment refers to the time from when the polyvalent metal ions and the recovered water absorbent resin are contacted to form a mixture thereof to when the soluble substances and the hydrogel are separated by a conventional solid-liquid separation means.
[0100] In order to increase productivity, it is preferable that the shrinkage treatment time is short. In one embodiment of the present invention, the shrinkage treatment time can be set to 120 minutes or less, more preferably 90 minutes or less, and even more preferably 60 minutes or less. In order to obtain a dehydrated water absorbent resin having a high dehydration rate, the dehydration time is preferably 5 minutes or more, more preferably 10 minutes or more, and even more preferably 15 minutes or more.
[0101] The mixture of polyvalent metal ions and recovered water-absorbent resin may be appropriately stirred, thereby increasing the contact opportunity between the polyvalent metal ions and the swollen gel, thereby increasing the shrinkage rate.
[0102] The shrinkage treatment can be carried out at any temperature at which the shrinkage of the swollen gel can proceed. Specifically, the temperature of the mixture of the polyvalent metal ion and the swollen gel may be, for example, 5 to 80°C, preferably 10 to 60°C, and more preferably room temperature (20 to 40°C).
[0103] (Drying the hydrogel) The hydrogel is preferably dried. The hydrogel is preferably dried at a high temperature of 100 to 300°C, more preferably 130 to 230°C, and further preferably 150 to 200°C. By being dried and being able to be handled as a powder, the operation of adding the hydrogel to the material to be treated in the production process of the water absorbent resin becomes easy. For the sake of convenience, the dried product of the hydrogel is also called a hydrogel.
[0104] (2-11) Performance of the hydrogel In one embodiment of the present invention, the mass average particle size of the hydrogel added to the material to be treated in the production process of the water-absorbent resin is preferably 10 to 600 μm, more preferably 50 to 500 μm, and even more preferably 100 to 400 μm.
[0105] In one embodiment of the present invention, the solid content of the hydrogel added to the material to be treated in the production process of the water absorbent resin is preferably 20 mass % or more, more preferably 50 mass % or more, even more preferably 80 mass % or more, and particularly preferably 90 mass % or more.
[0106] In one embodiment of the present invention, the solids-corrected CRC of the hydrogel is 5 g / g or less, preferably 3 g / g or less. If the solids-corrected CRC is more than 5 g / g, the shrinkage treatment is insufficient, and the handling of the hydrogel may deteriorate, or a large amount of energy may be required to dry the hydrogel. On the other hand, the solids-corrected CRC (6 hr) of the hydrogel is preferably 5 g / g or more, more preferably 7 g / g or more. That is, it has been found that the hydrogel shrunk by the polyvalent metal ion does not completely lose its water-absorbing ability, and absorbs water very slowly in the liquid to be absorbed. When such a hydrogel is added to the material to be treated in the manufacturing process of the water-absorbent resin, preferably at the above ratio, the water-absorbent resin as a whole is unlikely to decrease in water-absorption speed. The solids-corrected CRC (6 hr) of the hydrogel is preferably 50 g / g or less, more preferably 30 g / g or less.
[0107] In order to suppress coloration of the water-absorbent resin, the yellowness index (YI) of the hydrogel is preferably 20 or less, 15 or less, and 10 or less, in that order.
[0108] In the present invention, since the swollen gel can be treated without decomposing or solubilizing the swollen gel, there is no need to add a polymer decomposer. Therefore, the influence on the manufacturing process of the water absorbent resin is small in terms of the operation and the physical properties of the obtained water absorbent resin. Examples of the polymer decomposer include oxidizing agents and reducing agents. More specifically, L-ascorbic acid (salt), sulfite (hydrogen) salt, chlorite, hypochlorite, and hydrogen peroxide can be mentioned. When the swollen gel is decomposed and solubilized using a polymer decomposer, a large amount of the polymer decomposer is used in the manufacturing process of the water absorbent resin, which may cause the polymerization to become unstable or the water absorbent resin to deteriorate. On the other hand, the polymer decomposer may be originally contained in the swollen gel as a coloring inhibitor for the water absorbent resin, but the amount is usually controlled to such an extent that the water absorbent resin does not deteriorate. That is, preferably, the hydrogel does not contain at least one or more polymer decomposers selected from oxidizing agents and reducing agents, or when it contains them, the content is 1000 ppm or less. The polymer decomposer may be at least one selected from the group consisting of L-ascorbic acid (salt), sulfite (hydrogen) salt, chlorite, hypochlorite, and hydrogen peroxide. When the polymer decomposer is contained, the content is preferably 500 ppm or less, more preferably 100 ppm or less.
[0109] [4] Water-absorbent resin of the present invention The present invention provides a water-absorbent resin obtained by adding a hydrogel of a recovered water-absorbent resin to a material to be treated in a production process of the water-absorbent resin, the hydrogel containing a polyvalent metal ion and having a solids-corrected CRC of 5 g / g or less.
[0110] When the hydrogel is added to the object to be treated in the steps (1) to (4) included in the production process of the water absorbent resin, the hydrogel is contained inside the water absorbent resin. When the hydrogel is added to the object to be treated in the step (6), the hydrogel is contained on the surface of the water absorbent resin. When the hydrogel is added to the object to be treated in the step (5), the hydrogel is contained inside and / or on the surface of the water absorbent resin. In particular, when the hydrogel is added to the object to be treated in the fine powder granulation step, a water absorbent resin containing fine powder of the water absorbent resin and a fine powder granulated product containing the hydrogel is obtained, which is preferable.
[0111] According to the present invention, since decomposition and solubilization of the swollen gel is not necessary, a water absorbent resin having a low content of polymer decomposers that cause deterioration of the water absorbent resin can be obtained. That is, the water absorbent resin according to one embodiment of the present invention does not contain at least one or more polymer decomposers selected from oxidizing agents and reducing agents, or, when it contains the polymer decomposers, the content of the polymer decomposers is 100 ppm or less. The polymer decomposers may be at least one or more selected from the group consisting of L-ascorbic acid (salt), sulfite (hydrogen) salt, chlorite, hypochlorite, and hydrogen peroxide.
[0112] In the water-absorbent resin according to one embodiment of the present invention, the mass ratio of the solid content of the hydrogel to the solid content of the monomer constituting the water-absorbent resin is preferably 0.01-50:99.99-50.
[0113] The water absorbent resin according to one embodiment of the present invention has a centrifuge retention capacity (CRC) of preferably 10 g / g or more, more preferably 20 g / g or more, even more preferably 25 g / g or more, and particularly preferably 30 g / g or more. The upper limit of the centrifuge retention capacity (CRC) is not particularly limited, but is preferably 50 g / g, more preferably 45 g / g, and even more preferably 40 g / g, from the viewpoint of balance with other physical properties.
[0114] [5] Uses of the water-absorbent resin of the present invention The water-absorbent resin of the present invention can be widely used in absorbent articles, for example, in sanitary products, cables, packaging materials, soil additives, or construction materials. EXAMPLES
[0115] The present invention will be described below with reference to examples, comparative examples, and reference examples, but the present invention should not be construed as being limited by these examples, etc. The physical properties described in the claims and examples of the present invention were calculated under conditions of room temperature (23±2°C) and humidity of 50±10 RH%.
[0116] (Reference Example 1) Production of water-absorbent resin A sodium acrylate aqueous solution containing 0.07 mol% (relative to monomer) of a crosslinking agent polyethylene glycol diacrylate (average number of ethylene oxide units: n=9) was prepared with a neutralization rate of 75 mol% and a concentration of 39% by mass (monomer aqueous solution preparation step). Next, 0.12 g of sodium persulfate per mol of monomer was added to the obtained sodium acrylate aqueous solution, and the monomer was polymerized in aqueous solution to obtain a hydrogel-like crosslinked polymer (1) (polymerization step). Next, the hydrogel-like crosslinked polymer (1) was cut into several centimeters at 60°C, and then further granulated to 1 mm or less with a meat chopper to obtain a particulate hydrogel-like crosslinked polymer (1) (gel crushing step). The particulate hydrogel-like crosslinked polymer (1) was layered to a thickness of several centimeters and dried for 20 minutes in a hot air dryer at an air temperature of 180°C to a solid content of 95% to obtain a block-like dried polymer (1) (drying step).
[0117] The block-shaped dry polymer (1) was pulverized by a roll mill and further classified by JIS standard sieves with mesh sizes of 850 μm and 150 μm. Fine powders of less than 150 μm (about 10% by mass based on the total amount of the block-shaped dry polymer (1)) were collected, and particles of more than 850 μm were re-pulverized by a roll mill to obtain a water absorbent resin powder (A) of 850 to 150 μm and a water absorbent resin fine powder (B) of less than 150 μm (particle size adjustment step).
[0118] To the obtained water absorbent resin powder (A) of 850 to 150 μm, a surface cross-linking agent aqueous solution consisting of 2 mass% water and 0.5 mass% ethylene carbonate as a surface cross-linking agent was sprayed and added in a Loedige mixer, and then heat-treated at 180° C. for 30 minutes. The water absorbent resin powder (A) after the heat treatment was sized using JIS standard sieves with openings of 850 μm and 150 μm to obtain a surface cross-linked water absorbent resin powder (1) (surface cross-linking step). Here, the 150 μm passing material (fine powder of less than 150 μm) was taken as a surface cross-linked water absorbent resin fine powder (b).
[0119] (Reference Example 2) Granulation of water-absorbent resin powder The water-absorbent resin fine powder (B) of less than 150 μm obtained in Reference Example 1 and the surface-crosslinked water-absorbent resin fine powder (b) of less than 150 μm were mixed. 100 parts by mass of the obtained fine powder mixture was mixed with 100 parts by mass of hot water at 80 to 90 ° C. under stirring to obtain a fine powder granulated gel (solid content rate about 50%) having a particle size of several mm. Thereafter, the obtained fine powder granulated gel was dried for 30 minutes in a hot air dryer at 190 ° C. The fine powder granulated gel after drying was granulated to a particle size of several mm, which was further pulverized with a roll mill and further classified with JIS standard sieves with mesh openings of 850 μm and 150 μm to obtain a fine powder granulated product (1) having a particle size of 850 to 150 μm (fine powder granulation process). The water absorption capacity CRC of the fine powder granulated product (1) was 27.9 g / g.
[0120] (Reference Example 3) Separation and recovery of water-absorbent resin from paper diapers (shrinkage treatment with polyvalent metal salts) After cutting a commercially available paper diaper into pieces of several centimeters, a large amount of water was added to the cut pieces and stirred to obtain an aqueous dispersion containing pulp, nonwoven fabric, thermoplastic binder, and swollen gel particles of water-absorbent resin. Next, in order to separate and settle the swollen gel particles from the water, calcium chloride was added to the aqueous dispersion to cause the swollen gel particles of water-absorbent resin (partially neutralized sodium polyacrylate crosslinked body) to shrink and settle, and then the pulp, nonwoven fabric, and thermoplastic binder were removed.
[0121] By adding calcium chloride, the swollen gel particles of the water-absorbent resin shrunk and settled to a particle size of approximately 1 mm or less. The shrunk and settled swollen gel particles were separated by filtration and then dried to obtain hydrogel (1) (water-absorbent resin cross-linked with calcium chloride. The main component is cross-linked calcium polyacrylate. Particle size after drying is approximately 300 μm or less) from a commercially available paper diaper. The solid content of the obtained hydrogel (1) was 99 mass%, the solid content-corrected CRC was 1.0 g / g, and the solid content-corrected CRC (6 hr) was 6.4 g / g.
[0122] The water-absorbent resin (partially neutralized sodium polyacrylate crosslinked body) in commercially available paper diapers usually has a water-absorbent capacity CRC of 30 to 40 g / g. In contrast, the water-absorbent resin of the hydrogel obtained in the process of recovering the components (pulp, etc.) from the commercially available paper diapers is shrunk with calcium chloride in the process of recovering the components (pulp, etc.), and therefore the water-absorbent capacity CRC is significantly reduced, and the hydrogel is not suitable for practical use as a water-absorbent resin.
[0123] (Reference Example 4) The polymerization vessel used in Reference Example 1 was washed with deionized water, and a swollen gel was obtained. This was crushed in a juicer to obtain swollen gel particles. By adding calcium chloride to this, the swollen gel particles of the water absorbent resin shrunk and settled so that the particle diameter became about 1 mm or less. The shrunk and settled swollen gel particles were separated by filtration and then dried to obtain a hydrogel (2). The solid content of the obtained hydrogel (2) was 98 mass%, the solid content-corrected CRC was 0.8 g / g, and the solid content-corrected CRC (6 hr) was 7.3 g / g.
[0124] Example 1: Addition of the hydrogel to the fine powder granulation process The hydrogel (1) (water-absorbent resin cross-linked with calcium chloride, CRC=1.0 g / g) obtained from the paper diaper in Reference Example 3 was classified using a JIS standard sieve with a mesh size of 150 μm to obtain a 150 μm pass-through material. The CRC of the 150 μm pass-through material was 1.0 g / g.
[0125] Next, in the fine powder granulation of Reference Example 2, instead of 100 parts by mass of a fine powder mixture obtained by mixing the water absorbent resin fine powder (B) of less than 150 μm and the surface cross-linked water absorbent resin fine powder (b) of less than 150 μm, a mixture obtained by adding 10 parts by mass of the 150 μm passing hydrogel (1) obtained from paper diapers in Reference Example 3 to 90 parts by mass of the fine powder mixture was used, and fine powder granulation was performed in the same manner as in Reference Example 2.
[0126] Specifically, 90 parts by mass of a fine powder mixture obtained by mixing a water absorbent resin fine powder (B) of less than 150 μm and a surface cross-linked water absorbent resin fine powder (b) of less than 150 μm, and 10 parts by mass of a 150 μm passing through hydrogel (1) were mixed with 100 parts by mass of hot water at 80 to 90 ° C. under stirring in the same manner as in the fine powder granulation of Reference Example 2 to obtain a fine powder granulated gel (solid content rate of about 50%), and then dried. The fine powder granulated gel after drying was granulated to a particle size of several mm in the same manner as in Reference Example 2, and was further pulverized with a roll mill and further classified with JIS standard sieves with mesh openings of 850 μm and 150 μm to obtain a fine powder granulated product (2) (hereinafter, water absorbent resin (1)) having a particle size of 850 to 150 μm (fine powder granulation process).
[0127] The water absorption capacity (CRC) of the water-absorbent resin (1) containing 10% by mass of the 150 μm filtrate (solid content corrected CRC=1.0 g / g) of the hydrogel (1) was 27.3 g / g.
[0128] Here, the CRC of the fine powder granulated material (1) is 27.9 g / g, and the solid content corrected CRC of the 150 μm passing hydrogel (1) is 1.0 g / g. The theoretical CRC of the water absorbent resin (1) calculated from the mixing ratio of the fine powder mixture obtained by mixing the water absorbent resin fine powder (B) of less than 150 μm and the surface cross-linked water absorbent resin fine powder (b) of less than 150 μm in Example 1 and the 150 μm passing hydrogel (1) is 25.2 g / g (= 27.9 * 0.9 + 1.0 * 0.1) =, the CRC of the water absorbent resin (1) actually measured is 27.3 g / g, and an improvement in the water absorption capacity of 2.1 g / g compared to the theoretical CRC was confirmed. This corresponds to a significant recovery of the solid content corrected CRC of the hydrogel (1) from 1.0 g / g to 21.9 g / g.
[0129] (Comparative Example 1) Fine powder granulation using only hydrogel In the fine powder granulation of Reference Example 2, instead of 100 parts by mass of the mixture of the water absorbent resin fine powder (B) less than 150 μm and the surface cross-linked water absorbent resin fine powder (b) less than 150 μm, fine powder granulation was similarly performed only with the 150 μm passing material of the hydrogel (1) (solid content corrected CRC is 1.0 g / g). However, granulation was not possible due to the low water absorption performance.
[0130] (Comparative Example 2) Conventional Hydrogel Treatment Hydrogel (1) (solid content corrected CRC was 1.0 g / g) was subjected to a CRC recovery treatment by removing calcium chloride according to JP 2013-198862 A. However, the CRC was only restored to about 1 to 2 g / g.
[0131] (Example 2) Change in the amount of hydrogel added in Example 1 In the addition of the hydrogel to the fine powder granulation step of Example 1, the mixing ratio of the fine powder mixture obtained by mixing the water absorbent resin fine powder (B) of less than 150 μm and the surface cross-linked water absorbent resin fine powder (b) of less than 150 μm and the 150 μm passing material of the hydrogel (1) was changed from 90:10 to 80:20, that is, the mixture of the water absorbent resin fine powder (B) of less than 150 μm and the surface cross-linked water absorbent resin fine powder (b) of less than 150 μm was changed to 80 parts by mass, and the 150 μm passing material of the hydrogel (1) obtained from the paper diaper in Reference Example 3 was changed to 20 parts by mass. By performing fine powder granulation in the same manner as in Example 1, a fine powder granulated product (3) (hereinafter, water absorbent resin (2)) was obtained.
[0132] The CRC of the water-absorbent resin (2) containing 20 mass% of the hydrogel (1) (solids-corrected CRC = 1.0 g / g) was 24.3 g / g.
[0133] Here, the theoretical CRC of the water absorbent resin (2) calculated from the mixture ratio of the fine powder mixture obtained by mixing the water absorbent resin fine powder (B) of less than 150 μm and the surface cross-linked water absorbent resin fine powder (b) of less than 150 μm in Example 2 and the 150 μm passing material of the hydrogel (1) of 8:2 was 22.5 g / g (= 27.9 * 0.8 + 1.0 * 0.2), whereas the CRC of the water absorbent resin (2) actually measured was 24.3 g / g, and an improvement in the water absorption capacity CRC of 1.6 g / g was confirmed compared to the theoretical CRC. This corresponds to the CRC of the hydrogel (1) being greatly restored from 1.0 g / g to 9.9 g / g.
[0134] Example 3: Addition of the hydrogel to the polymerization process In the polymerization step of the water absorbent resin of Reference Example 1, 5% by mass [relative to (hydrogel (1) + monomer solid content)] of hydrogel (1) (solid content corrected CRC = 1.0 g / g; passing through a JIS standard sieve with an opening of 150 μm) was added to the monomer aqueous solution to carry out polymerization. Thereafter, in the same manner as in Reference Example 1, gel crushing, drying, particle size adjustment, and surface crosslinking were carried out, and the particles were sized using JIS standard sieves with openings of 850 μm and 150 μm to obtain a surface crosslinked water absorbent resin powder (2) (hereinafter, water absorbent resin (3)). In the obtained water absorbent resin (3), the hydrogel (1) (150 μm or less) was entirely incorporated inside, and no residual hydrogel (1) was present.
[0135] Example 4: Addition of the hydrogel to the gel grinding process In the gel crushing step of the water absorbent resin in Reference Example 1, 5% by mass of hydrogel (1) (solid content corrected CRC=1.0 g / g) [relative to (hydrogel (1) + monomer solid content)] was added to the hydrogel-like crosslinked polymer to perform gel crushing. Thereafter, in the same manner as in Reference Example 1, drying, particle size adjustment, and surface crosslinking were performed, and the particles were sized using JIS standard sieves with mesh sizes of 850 μm and 150 μm to obtain a surface crosslinked water absorbent resin powder (3) (hereinafter, water absorbent resin (4)). The hydrogel (1) (150 μm or less) was entirely contained inside the water absorbent resin (4), and no residual hydrogel (1) was present.
[0136] Example 5 A water-absorbent resin (5) was obtained in the same manner as in Example 1, except that the hydrogel (2) was used instead of the hydrogel (1) in Example 1. The solid content-corrected CRC of the 150 μm filtrate of the hydrogel (2) was 0.7 g / g, and the CRC of the water-absorbent resin (5) was 27.1 g / g.
[0137] (summary) Comparing the above-mentioned Examples 1 and 2 with the Comparative Examples 1 and 2, it is found that by adding a hydrogel obtained by shrinking a swollen gel with a polyvalent metal ion to a production process (fine powder granulation process) of a water absorbent resin at a usage ratio of 10 mass % or 20 mass % relative to the water absorbent resin, the water absorption capacity (CRC) is improved to be higher than the theoretical value calculated from the mixing ratio, i.e., the water absorption performance of the hydrogel is restored.
[0138] Moreover, it is evident from Examples 3 and 4 that the hydrogel can also be used as a raw material for water-absorbent resins in each step of the production process for other water-absorbent resins.
[0139] Furthermore, it is understood from Example 5 that the present invention can be applied to the swollen gel that is generated when cleaning a water-absorbent resin production device. [Industrial Applicability]
[0140] It is possible to provide a method for producing a water-absorbing resin that is useful for reducing resources and energy consumption, based on the perspectives of reducing the burden on the global environment, resource conservation, carbon neutrality, SDGs (Sustainable Development Goals), etc.
Claims
1. A method for producing a water-absorbent resin, comprising the step of adding a hydrogel of a recovered water-absorbent resin to a material to be treated in a production step of the water-absorbent resin, The water-absorbing resin is a polyacrylic acid (salt)-based water-absorbing resin, The hydrogel contains polyvalent metal ions and has a solids-corrected CRC of 5 g / g or less; The solid content corrected CRC is a value theoretically obtained from the CRC of a water absorbent resin containing water, when the CRC is measured for a water absorbent resin having a solid content of 100 mass%, In the measurement of CRC in accordance with WSP241.3(10), m si is changed to 1 g, CRC is measured, and the CRC is calculated by substituting the sample solid content [g] calculated by (sample mass [g]) × (solid content rate [mass %]) for m si in the following formula for calculating CRC. CRC [g / g] = (m wi - m b - m si ) / m si mwi: Mass of the bag containing the water-absorbent resin after the test [g] m b : Mass of the bag after testing without using the water-absorbent resin [g] m si : mass of the water-absorbent resin before the test [g].
2. The method for producing a water-absorbent resin according to claim 1, wherein the hydrogel is added to a material to be treated in at least one of the following steps (1) to (6) included in the production process of the water-absorbent resin: (1) Preparation of an aqueous monomer solution (2) Polymerization process (3) Gel crushing step during or after polymerization (4) Drying process (5) Particle size adjustment process, fine powder recovery process, or fine powder granulation process after the drying process (6) Additive addition step or surface cross-linking step following the particle size adjustment step
3. 3. The method for producing a water absorbent resin according to claim 1, wherein the hydrogel is produced by dispersing a mixture containing the recovered water absorbent resin in water, and shrinking the swollen gel formed by swelling the recovered water absorbent resin with a polyvalent metal ion.
4. 3. The method for producing a water-absorbent resin according to claim 1 or 2, wherein the hydrogel is obtained by washing an apparatus used in a production step of the water-absorbent resin with water to obtain a swollen gel, and then shrinking the swollen gel with a polyvalent metal ion.
5. 5. The method for producing a water-absorbent resin according to claim 3, wherein the hydrogel is a dried product obtained by shrinking the swollen gel with a polyvalent metal ion and drying the gel.
6. The method for producing a water-absorbent resin according to claim 5, wherein the hydrogel has a mass average particle size of 10 μm to 600 μm.
7. The method for producing a water-absorbent resin according to any one of claims 1 to 6, wherein a mass ratio of a solid content of the hydrogel to a solid content of a monomer used in the production process of the water-absorbent resin is 0.01 to 50:99.99 to 50.
8. The method for producing a water-absorbing resin according to any one of claims 1 to 7, wherein the hydrogel has a yellowness index (YI) of 20 or less.
9. The hydrogel does not contain at least one or more polymer decomposing agents selected from an oxidizing agent and a reducing agent, or, when the hydrogel contains the polymer decomposing agent, the content of the polymer decomposing agent is 1000 ppm or less. The method for producing a water-absorbing resin according to any one of claims 1 to 8.
10. The method for producing a water absorbent resin according to claim 9, wherein the polymer decomposing agent is at least one selected from the group consisting of L-ascorbic acid (salt), sulfite (hydrogen) salt, chlorite, hypochlorite, and hydrogen peroxide.
11. The method for producing a water-absorbing resin according to any one of claims 1 to 10, wherein a coloring inhibitor is added in at least one step of the production process of the water-absorbing resin.
12. A water-absorbent resin obtained by adding a hydrogel of a recovered water-absorbent resin to a material to be treated in a production process of the water-absorbent resin, the water-absorbent resin being a polyacrylic acid (salt)-based water-absorbent resin, the hydrogel containing a polyvalent metal ion and having a solids-corrected CRC of 5 g / g or less, the solids-corrected CRC being a theoretically calculated value of CRC when measured for a water-absorbent resin having a solids content of 100% by mass, from the CRC of the water-absorbent resin containing water, In the measurement of CRC in accordance with WSP241.3 (10), m si was changed to 1 g, CRC was measured, and the CRC was calculated by substituting the sample solid content [g] calculated by (sample mass [g]) × (solid content rate [mass %]) for m si in the following formula for calculating CRC: CRC [g / g] = (m wi - m b - m si ) / m si mwi: Mass of the bag containing the water-absorbent resin after the test [g] m b : Mass of the bag after testing without using the water-absorbent resin [g] m si : mass of the water-absorbent resin before the test [g].
13. The water-absorbent resin according to claim 12, comprising a fine powder granule comprising a fine water-absorbent resin powder and said hydrogel.
14. The water absorbent resin according to claim 12 or 13, which does not contain at least one polymer decomposing agent selected from an oxidizing agent and a reducing agent, or when the water absorbent resin contains the polymer decomposing agent, the content of the polymer decomposing agent is 100 ppm or less.
15. The polymer decomposing agent is at least one selected from the group consisting of L-ascorbic acid (salt), sulfite (hydrogen) salt, chlorite, hypochlorite, and hydrogen peroxide. The water absorbent resin according to claim 14.
Citation Information
Patent Citations
Method and device for recirculating aqueous fluid absorbing particles
JP1991152104A
Reclamation of fine powder of super-absorptive polymer
JP1992041532A
Method for forming coarse particle from fine particle of ultra-absorbent
JP1992227934A
Disposal of water absorbable polymer
JP1992317784A
Production of granulated water-absorbing resin
JP1999106514A