Method for producing magnetic material, method for producing rubber latex composition, and method for producing molded body
Vacuum freeze-drying of magnetic functional fluids before mixing with rubber latex addresses high water content and concentration limitations, achieving improved blending and magnetic properties in conductive rubber compositions.
Patent Information
- Application Number
- JP2020128312
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-29
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2040-07-29
AI Technical Summary
Existing methods for producing conductive rubber compositions face challenges with high water content and limited concentration of functional materials, leading to inefficiencies and moisture residues in molded products.
A method involving vacuum freeze-drying of a polar solvent-based magnetic functional fluid to remove the dispersion medium before mixing with rubber latex, ensuring compatibility and high concentration of magnetic particles in the composition.
This approach results in a rubber latex composition with enhanced blending concentration and magnetic properties, eliminating moisture residues in molded articles.
Smart Images

Figure 0007583544000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a magnetic material, a method for producing a rubber latex composition using the magnetic material, and a method for producing a molded article using the rubber latex composition. [Background technology]
[0002] Conductive rubber obtained by dispersing conductive powder in a rubber material that is considered an insulator has insulating properties when no pressure is applied, but exhibits so-called pressure-sensitive conductivity, that is, becomes conductive when a pressure stimulus is applied, and is therefore widely used as a switch or sensor in electric and electronic devices. For example, Patent Document 1 describes that when a rubber composition is produced, a function-imparting agent is blended in the form of a liquid (water dispersion) to impart conductivity to a molded product (final product) of the rubber composition, and the function-imparting agent-dispersed rubber latex mixture is mixed with the rubber latex to prepare the function-imparting agent-dispersed rubber latex mixture, and that constant temperature drying is a preferable method for removing water from the material to be dried. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2013-101080 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, when the function-imparting agent is mixed with the rubber latex in the form of a liquid (aqueous dispersion) as in Patent Document 1, the amount of water in the mixture becomes greater than necessary, and a lot of time must be spent on the task of removing the water, which is not practical.In addition, in the technology of Patent Document 1, since the function-imparting agent is mixed with the rubber latex in the form of a liquid (aqueous dispersion), there is a technical limit to how high the concentration of the function-imparting agent in the mixture can be increased (the upper limit of the concentration is low).
[0005] Incidentally, there is currently no technology that can disperse and mix a magnetic material recovered from a magnetic fluid in which magnetic particles, as an example of a functional material, are dispersed in a polar liquid solvent, typically water, with an aqueous dispersion such as rubber latex.
[0006] An object of the present invention is to provide a method for producing a magnetic material, which is capable of producing a magnetic material that has good compatibility with a mixture with rubber latex and whose blending concentration in a composition consisting of the mixture can be increased, a method for producing a rubber latex composition using the magnetic material produced by the method, and a method for producing a molded article using the rubber latex composition produced by the method. [Means for solving the problem]
[0007] In order to achieve the above object, the method for producing a magnetic material according to the present invention is a method for producing a magnetic material for use in the production of a rubber latex composition, which comprises the steps of: preparing a polar solvent-based magnetic functional fluid in which magnetic particles are dispersed using a polar liquid as a solvent as a material to be dried; removing the polar liquid from the material to be dried to obtain a recovered material; and performing the steps by vacuum freeze drying. The polar liquid can be water or a mixture of water and a water-soluble organic solvent.
[0008] The present invention also provides a method for producing a rubber latex composition, which includes a step of mixing the recovered material (magnetic material) after vacuum freeze-drying with rubber latex to obtain a mixture of the recovered material and rubber latex, and a method for producing a molded product, which includes a step of molding the obtained mixture. The material recovered after vacuum freeze-drying may be mixed with rubber latex, and then other components including a crosslinking agent may be added to form a mixture.
[0009] In the present invention, the reasons for using a "polar solvent-based magnetic functional fluid" as the material to be dried, using "vacuum freeze drying" as the method for removing the dispersion medium, and using "before mixing with rubber latex" as the timing for removing the dispersion medium will be explained using "magnetic fluid," a type of magnetic functional fluid, as an example. Magnetic functional fluids are classified into magnetic fluids and magnetorheological fluids, and both have in common the fact that they contain magnetic particles, dispersants, and dispersion mediums.
[0010] (To be dried) First, regarding the material to be dried, there are polar solvent-based magnetic fluids (simply referred to as "water-based" here) that use polar liquids, such as water, as a solvent, which have a fixed electric dipole inside the molecule, as well as non-polar solvent-based magnetic fluids (simply referred to as "oil-based" here) that use non-polar liquids, such as oils, such as benzene, hexane, and straight-chain hydrocarbons, as a solvent, which have an electric dipole moment of zero or close to zero. It is known that water-based magnetic fluids have a different structure of colloidal particles, which are the units of dispersion in the fluid, compared to oil-based magnetic fluids (non-patent literature: Joint Conference of Magnetic Fluids, Proceedings of Lectures 2019-12 / Considerations on the dispersion stability and aging phenomenon of polar solvent-based (water-based) magnetic fluids and non-polar solvent-based (oil-based) magnetic fluids / Published on December 5, 2019).
[0011] Colloid particles in water-based magnetic fluids have a structure in which the magnetic particles are coated with three layers (from the side closest to the particle, the first lipophilic coating layer, the second hydrophilic coating layer, and the hydrated fixing layer). Colloid particles in water-based magnetic fluids move through the fluid covered with three coating layers whose total thickness exceeds the radius of the magnetic particle itself, so there is a limit to the amount they can exist in the fluid. As a result, there are many issues, such as the fluid itself becoming magnetically dilute, and the fact that gelation is likely to occur as the dispersion concentration increases, making it difficult to obtain a highly concentrated dispersion system. On the other hand, the colloidal particles of oil-based magnetic fluids have a structure in which the magnetic particles are covered with only one layer (lipophilic coating layer), so they are less likely to have the above problems that colloidal particles of water-based magnetic fluids have. However, because the colloidal particles have lipophilic surfaces, they are poorly compatible with rubber latex, which uses water as a dispersion medium, and separation and aggregation are often observed in mixtures with rubber latex. Therefore, the material to be dried was chosen to be water-based magnetic fluid, as it prioritizes compatibility with rubber latex.
[0012] (Method of Removing Dispersion Medium) Next, as a method for removing the dispersion medium, the coagulation and sedimentation method disclosed in, for example, Patent No. 6309006 (paragraph 0027) was tried. When a polar solvent such as ethanol was used, the magnetic particles did not settle, and when a non-polar solvent such as isooctane was added, the magnetic particles remained separated into two layers, and in either case the magnetic particles did not settle or separate. In addition, when the evaporation method was tried, a recovered material that was compatible with rubber latex could not be obtained, even though a water-based magnetic fluid was used as the material to be dried. This is because separation and coagulation were observed when the recovered material obtained by this method was mixed with rubber latex. This is presumably because the particle structure of the recovered material obtained by the evaporation method was such that, of the three coating layers that cover the central magnetic particles, the hydrophilic first coating layer and the hydrophilic second coating layer were peeled off, and the hydrophilic second coating layer and the hydrated fixing layer were removed (i.e., the magnetic particles were covered only with the hydrophilic first coating layer). It is assumed that the surface of this particle structure is lipophilic and therefore does not mix well with rubber latex, which uses water as a dispersion medium, just like the colloidal particles of the oil-based magnetic fluid described above. On the other hand, it is speculated that when vacuum freeze-drying is used, it is possible to remove only the hydrated fixed layer while leaving the hydrophilic second coating layer on the outermost surface of the core magnetic particles. The particle structure of the recovered material (magnetic material) obtained by vacuum freeze-drying has a hydrophilic surface, so it is speculated that separation and aggregation are not observed in the mixture with rubber latex. The above is the reason why vacuum freeze-drying was adopted as a method for removing the dispersion medium.
[0013] (Timing for removing dispersion medium) Regarding the timing of removing the dispersion medium, if this is done after mixing with the rubber latex, the following inconveniences will occur. First, as mentioned above, the colloidal particles of the water-based magnetic fluid have a structure in which the magnetic particles are covered with a triple coating layer that exceeds the radius of the magnetic particles themselves, so that the amount present in the fluid is small (the concentration is low). Therefore, if the magnetic particles are mixed with rubber latex in the form of a liquid (fluid) and then the dispersion medium is removed (that is, the timing of removing the dispersion medium is after mixing with the rubber latex), the magnetic particle concentration in the composition consisting of the recovered mixture is inevitably low. As a result, it is difficult to impart excellent magnetic properties to the molded body obtained by removing the water from the composition. This is a natural consequence since the fluid itself is magnetically dilute (as mentioned above).
[0014] Secondly, when magnetic particles are mixed with rubber latex in the form of a liquid (fluid), the water content in the mixture becomes too high, and as a result, even if the dispersion medium is subsequently removed, water is likely to remain in the mixture. Therefore, when the obtained composition is molded, it is molded with water remaining. Water may remain as a residue inside the obtained molded product.
[0015] In contrast, if the dispersion medium is removed before mixing with the rubber latex, these inconveniences do not occur, which is the reason why the dispersion medium is removed before mixing with the rubber latex. Effect of the Invention
[0016] In the method for producing a magnetic material according to the present invention, since a water-based magnetic functional fluid is used as a material to be dried, a magnetic material that is easily mixed into a mixture with rubber latex can be obtained. In addition, since the dispersion medium is removed using a specific method before mixing with latex, the blending concentration can be adjusted when mixing with latex, and the blending concentration in the composition consisting of the mixture with rubber latex can be increased. In other words, according to the method for producing a magnetic material of the present invention, it is possible to produce a magnetic material that has good compatibility with a mixture with rubber latex and that can be mixed at an increased concentration in a composition consisting of the mixture.
[0017] In both the methods for producing a rubber latex composition and a molded article according to the present invention, the recovered material (magnetic material) obtained by the method of the present invention is used. Therefore, the blending concentration of the magnetic material in the rubber latex composition can be increased, which can contribute to the production of a molded article having excellent magnetic properties. In addition, since the magnetic material used does not contain moisture, when a molded article is produced from a composition consisting of a mixture of the magnetic material and rubber latex, no moisture residue is generated inside the molded article. That is, according to the method for producing a rubber latex composition of the present invention, it is possible to produce a rubber latex composition having an increased concentration of magnetic material. Also, according to the method for producing a molded article of the present invention, it is possible to produce a molded article that is free of moisture residue and can be imparted with excellent magnetic properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, an embodiment of the present invention will be described. (1.Magnetic materials) The magnetic material according to the present embodiment is a powder made of magnetic particles at least partly coated with a dispersant.
[0019] (2. Manufacturing method of magnetic materials) Such a magnetic material is composed of a material recovered after a vacuum freeze-drying process is performed on a polar solvent-based magnetic functional fluid in which magnetic particles are dispersed in a polar liquid as a solvent, and the material recovered after the vacuum freeze-drying process (hereinafter simply referred to as "recovered material") is useful for mixing with rubber latex constituting a rubber latex composition.
[0020] (Polar Solvent-Based Magnetic Functional Fluid) Polar solvent-based magnetic functional fluids include polar solvent-based magnetic fluids and polar solvent-based magnetorheological fluids. A polar solvent-based magnetic fluid is a colloidal solution in which magnetic particles, at least part of whose surface is coated with a dispersant, are dispersed in a polar liquid as a solvent. This polar solvent-based magnetic fluid has very good dispersibility, so it does not cause solid-liquid separation such as precipitation or separation due to gravity, magnetic field, etc., and can be considered as a homogeneous liquid that is magnetic in itself. A polar solvent-based magnetorheological fluid is a liquid in which magnetic particles, at least part of whose surface is coated with a dispersant, are dispersed in a polar liquid as a solvent, and refers to a fluid that reversibly changes from a highly fluid state to a gel state with a large yield stress depending on the strength of a magnetic field applied from the outside. Polar solvent-based magnetic functional fluids (hereinafter sometimes referred to as magnetic functional fluids) are classified into polar solvent-based magnetic fluids (hereinafter sometimes referred to as magnetic fluids) and polar solvent-based magnetorheological fluids (hereinafter sometimes referred to as magnetorheological fluids), and contain at least (A) magnetic particles, (B) a dispersant, and (C) a polar liquid.
[0021] (A) Magnetic particles The magnetic particles contained in the magnetic fluid are magnetic bodies (having a relative magnetic permeability of, for example, 1.5 or more), and examples of the magnetic bodies include ferromagnetic oxides, ferromagnetic metals, and metal nitrides. Examples of the ferromagnetic oxides include magnetite, γ-iron oxide, manganese ferrite, cobalt ferrite, and composite ferrites of these with zinc or nickel, and barium ferrite. Examples of the ferromagnetic metals include iron, cobalt, and rare earth elements. Among these, magnetite is preferred from the viewpoint of mass production. The magnetic particles contained in the magnetic fluid are not particularly limited as long as they have an average particle size within the range in which they exhibit superparamagnetism, that is, the critical particle size or less. For example, in the case of magnetite or γ-iron oxide, the average particle size is preferably 50 nm or less, particularly preferably 40 nm or less, and preferably 10 nm or more. The average particle size of the magnetic particles contained in the magnetic fluid is the average primary particle size measured by a transmission electron microscope (TEM). The content of the magnetic particles in the magnetic fluid is preferably 10% by mass or more, more preferably 15% by mass or more, and preferably 50% by mass or less, and more preferably 40% by mass or less, calculated as solid content, from the viewpoint of preventing sedimentation. The solid content refers to the content of the magnetic particles after recovery relative to the total mass (hereinafter the same).
[0022] Next, examples of magnetic particles contained in the magnetorheological fluid include ferromagnetic oxides, ferromagnetic metals, metal nitrides, and various alloys. Examples of ferromagnetic oxides include magnetite, carbonyl iron, γ-iron oxide, manganese ferrite, cobalt ferrite, and composite ferrites of these with zinc or nickel, and barium ferrite. Examples of ferromagnetic metals include iron, cobalt, and rare earth elements. Examples of various alloys include Sendust (registered trademark), Permalloy (registered trademark), and Supermalloy (registered trademark). Among these, carbonyl iron is preferred. The average particle size of the magnetic particles contained in the magnetorheological fluid is preferably 1 μm or more, more preferably 2 μm or more, particularly preferably 5 μm or more, preferably 100 μm or less, more preferably 60 μm or less, particularly preferably 50 μm or less. The shape of the magnetic particles contained in the magnetorheological fluid is preferably spherical or nearly spherical. The average particle size of the magnetic particles contained in the magnetorheological fluid is the average primary particle size measured by a laser diffraction / scattering type particle size distribution measuring device. From the viewpoint of mass productivity, the content of magnetic particles in the magnetorheological fluid is preferably 20% by mass or more, more preferably 30% by mass or more, and preferably 85% by mass or less, more preferably 70% by mass or less, calculated as solid content.
[0023] (B) Dispersant The dispersant is added to the magnetic functional fluid in order to improve the dispersibility of the magnetic particles in the dispersion medium (polar liquid). As the dispersant, a known surfactant, a polymer dispersant, etc. can be appropriately used, among which, from the viewpoint of dispersibility and the performance of the obtained magnetic powder, a surfactant is preferable. By including magnetic particles and a dispersant in the magnetic functional fluid, at least a part of the dispersant adheres to the magnetic particles in the magnetic functional fluid. At least a part of the surface of the magnetic particles is covered with a dispersant (preferably a surfactant). In the present embodiment, examples of surfactants preferably used as a dispersant include anionic surfactants that are hydrocarbon compounds having polar groups such as carboxyl groups, hydroxyl groups, and sulfonic acid groups, such as oleic acid or its salts, petroleum sulfonic acid or its salts, synthetic sulfonic acid or its salts, eicosylnaphthalenesulfonic acid or its salts, polybutenesuccinic acid or its salts, and erucic acid or its salts, or nonionic surfactants such as polyoxyethylene nonylphenyl ether, and amphoteric surfactants having both cationic and anionic moieties in the molecular structure, such as alkyldiaminoethylglycine. Among these, sodium oleate is preferred because it is inexpensive and easily available. Only one type of dispersant may be used, or two or more types may be used in combination.
[0024] The average particle size of the dispersant may be any size that can prevent aggregation of the magnetic particles in the magnetic functional fluid, for example, preferably 1 nm or more, more preferably 2 nm or more, and preferably 25 nm or less, more preferably 20 nm or less for each of the first coating layer and the second coating layer. The content of the dispersant (the total amount when multiple types are included) may be an amount that can prevent aggregation of magnetic particles in the magnetic functional fluid, for example, preferably 5% by mass or more, more preferably 10% by mass or more, preferably 25% by mass or less, more preferably 20% by mass or less, calculated as solid content.
[0025] (C)Polar liquid The polar liquid used as the dispersion medium of the magnetic functional fluid means a liquid that has a fixed electric dipole inside the molecule, and when it is used as a solvent, it is called a polar solvent. A typical example is water, but a mixture of water and a water-soluble organic solvent can also be used. Examples of water-soluble organic solvents include ethanol and methanol. When using water as the polar liquid, it is preferable to use pure water with few impurities, ion-exchanged water, etc. The concentration of each of the above components relative to the polar liquid as the dispersion medium is not particularly limited. From the viewpoint of workability in subsequent steps, the content of the dispersion medium in the magnetorheological fluid is an amount such that the total solids concentration of each of the above components is preferably 15% by mass or more, more preferably 30% by mass or more, and preferably 80% by mass or less, and more preferably 70% by mass or less.
[0026] In the magnetic fluid, the ratio of the total content of magnetic particles (inorganic components) in the solid components to the total content of organic components such as dispersants typified by surfactants is not particularly limited as long as it is within a range that exhibits superparamagnetism. In general, the mass ratio of magnetic particles to dispersants is preferably in the range of 60:40 to 90:10, and more preferably in the range of 70:30 to 85:15.
[0027] (D) Magnetic particles coated with a dispersant and a hydrated fixing layer. When magnetic particles and a dispersant are added to a polar solvent and stirred, the magnetic particles become colloidal particles having a structure in which the magnetic particles are coated with three layers (from the side closest to the particle, the first lipophilic coating layer / the second hydrophilic coating layer / the hydrated fixing layer). In the magnetic fluid, when the magnetic particles are magnetite or γ-iron oxide, the average particle size of the magnetic particles coated with the dispersant and the hydrated fixing layer is preferably 120 nm or less, particularly preferably 100 nm or less, and preferably 12 nm or more, taking into account the average particle size of the magnetic particles described above (preferably 50 nm or less, preferably 10 nm or more). The average particle size of the magnetic particles coated with the dispersant and the hydrated fixing layer is the average primary particle size measured by dynamic light scattering. For example, it can be measured using a nanoparticle analyzer (nano Partica SZ-100 series) manufactured by Horiba, Ltd. In magnetorheological fluids, the size of the magnetic particles themselves (average particle diameter is preferably 1 μm or more, and preferably 100 μm or less) is extremely large compared to the thickness of the three layers described above (approximately several tens of nm), so the average particle diameter of the magnetic particles coated with the dispersant and hydrated fixing layer can be determined taking into account the size of the magnetic particles themselves.
[0028] (Vacuum freeze-drying process) In this embodiment, the material to be dried is a polar solvent-based magnetic functional fluid, which is subjected to a vacuum freeze-drying process to obtain a recovered material. The recovered material after vacuum freeze-drying constitutes the magnetic material according to this embodiment. The recovered material is usually in a smooth powder form (magnetic powder), but it may not be in this form (aggregates). Even if the recovered material is entirely in powder form, or even if some or all of the recovered material is aggregated, the aggregated parts are instantly broken down by the moisture in the latex and dispersed and mixed, so this does not pose a problem in this embodiment. The average particle size of each recovered material is equivalent to the average particle size (above) of the magnetic particles coated with the dispersant and the hydrated fixed layer.
[0029] The vacuum freeze-drying applied to the material to be dried means sublimating substantially all of the liquid components (polar liquid) from the material to be dried, and separating and recovering the magnetic particles at least part of whose surface is coated with a dispersant. The vacuum freeze-drying in this embodiment can be carried out, for example, by a method including a pre-freezing step of freezing and solidifying the material to be dried, and a reduced pressure drying step of sublimating and removing substantially all of the frozen polar liquid from the pre-frozen material to be dried.
[0030] Examples of the preliminary freezing step include an air blast method (air freezing), a liquid method (liquid freezing), a contact method (contact freezing), and a liquefied gas method, with the air blast method or the contact method being preferred.
[0031] In the preliminary freezing step, the material to be dried is frozen from room temperature (25°C) to, for example, -10°C to -80°C. The freezing temperature is preferably -20 to -60°C. The freezing time varies depending on the concentration of the magnetic functional fluid and the freezing temperature, but can be, for example, 12 to 36 hours, preferably 20 to 30 hours. The container may be made of either metal or plastic.
[0032] In the reduced pressure drying process, the atmospheric pressure and temperature around the frozen material to be dried are respectively reduced to a pressure at which sublimation is possible, and increased to a temperature at which sublimation is possible, so that the liquid component (polar liquid) in the frozen material to be dried is almost entirely sublimated. For example, the material is dried until the polar liquid content in the frozen material to be dried is preferably 2% by mass or less, more preferably 0.5% by mass or less. When reducing the atmospheric pressure around the frozen material to be dried, the frozen material to be dried may be placed in a freeze-dryer and the atmospheric pressure may be reduced by reducing the pressure in the vacuum chamber. The pressure (degree of vacuum) during drying is preferably 200 Pa or less, more preferably 133 Pa or less, and particularly preferably 106 Pa or less. The drying temperature (shelf temperature) may be any temperature that is higher than the freezing point of the polar liquid and does not cause the surfactant to degrade, and is, for example, preferably 60° C. or less, more preferably 50° C. or less, and particularly preferably 40° C. or less.
[0033] In this embodiment, the preliminary freezing step and the reduced pressure drying step may be performed using a freeze dryer, or the preliminary freezing step and the reduced pressure drying step may be performed using separate means, for example, a refrigerator and a freeze dryer. However, it is preferable to use a freeze dryer in terms of miniaturization of the freeze drying device. For example, the freeze dryers "RLEII" series and "RL-B" series manufactured by Kyowa Vacuum Engineering Co., Ltd. may be mentioned. In the reduced pressure drying process, in order to raise the atmospheric temperature around the frozen material to be dried from the temperature in the freezing process to the temperature in the reduced pressure drying process, a heater or other configuration used in conventional freeze-drying apparatuses can also be used.
[0034] (Other processing) In this embodiment, the recovered material can be used as it is as a magnetic material, but if it (the recovered material) is aggregated, it is not prevented from being subjected to a crushing process or the like as necessary and re-pulverized. Note that in this embodiment, even if the recovered material is aggregated, when it is added to rubber latex and stirred as described below, it is instantly crushed and dispersed and mixed, so that re-pulverization is usually not required.
[0035] (3. Rubber Latex Composition) The rubber latex composition according to the present embodiment is made of a mixture containing the recycled material obtained by the above-mentioned process and rubber latex.
[0036] (rubber latex) Rubber latex may be any material in which water-insoluble rubber particles are dispersed in water. Examples of rubbers constituting the particles include natural rubber (NR), polyisoprene rubber (IR), styrene-butadiene rubber (SBR), polybutadiene rubber (BR), acrylonitrile-butadiene rubber (NBR), acrylonitrile-styrene-butadiene rubber (ABS), methyl methacrylate-butadiene rubber (MBR), polychloroprene rubber (CR), ethylene-propylene rubber (EPM), silicone rubber, acrylic rubber, urethane rubber, and chlorosulfonated polyethylene rubber. These rubbers may be used alone or in combination of two or more.
[0037] The concentration of the rubber in the rubber latex is preferably 20% by mass or more and 80% by mass or less. If the concentration of the rubber is too low, problems arise in the strength and adhesiveness of the molded article of the rubber latex composition, and if the concentration of the rubber in the rubber latex is too high, the amount of the dispersion medium (water) is relatively reduced, and as a result, when attempting to increase the amount of the recycled material to be blended, mixing may be hindered.
[0038] The rubber is preferably dispersed in the rubber latex in a form in which the dispersed particle diameter is, for example, about 0.01 to 0.5 μm. The rubber having a dispersed particle diameter in the predetermined range (mentioned above) may be, for example, 70% or more, preferably 90% or more, of the rubber present in the rubber latex. This dispersed particle diameter is an index showing the degree of dispersion (degree of dispersion) of the rubber particles in the rubber latex, and the smaller this value, the higher the degree of dispersion. The ratio of rubber particles (aggregated particles, temporary particles) dispersed in the form of dispersed particle diameters in the above-mentioned predetermined range can be calculated by utilizing image analysis using, for example, a transmission electron microscope (TEM) or a scanning electron microscope (SEM).
[0039] In addition to rubber particles and a dispersion medium (water), from the viewpoint of improving and stabilizing the quality, for example, surfactants, emulsifiers, antioxidants, preservatives, antibacterial agents, dispersants, etc. may be appropriately selected and blended into the rubber latex.
[0040] (Other ingredients) In addition to the recycled materials and rubber latex, various components can be blended into the rubber latex composition depending on the purpose, such as a crosslinking agent (vulcanizing agent), a crosslinking accelerator (vulcanization accelerator), a pH adjuster, a thickener, an antiaging agent, a dispersant, a pigment, and a filler. The crosslinking agent is not particularly limited, and any agent capable of crosslinking (vulcanizing) with the rubber particles in the rubber latex can be used as appropriate. Examples include sulfur, sulfur-based compounds, organic peroxides, and phenolic compounds. The content of the crosslinking agent when used is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, and preferably 5% by mass or less, and more preferably 3% by mass or less, based on the rubber particles in the rubber latex. The crosslinking agent may be used alone or in combination of two or more kinds.
[0041] The crosslinking accelerator (vulcanization accelerator) is not particularly limited, and examples thereof include dithiocarbamic acids such as diethyldithiocarbamic acid, dibutyldithiocarbamic acid, di-2-ethylhexyldithiocarbamic acid, dicyclohexyldithiocarbamic acid, diphenyldithiocarbamic acid, and dibenzyldithiocarbamic acid, and zinc salts thereof; 2-mercaptobenzothiazole, 2-mercaptobenzothiazole zinc, 2-mercaptothiazole zinc salt, and the like. Examples of the crosslinking accelerator include phosphorus, dibenzothiazyl disulfide, 2-(2,4-dinitrophenylthio)benzothiazole, 2-(N,N-diethylthio carbylthio)benzothiazole, 2-(2,6-dimethyl-4-morpholinothio)benzothiazole, 2-(4'-morpholino dithio)benzothiazole, 4-morpholinyl-2-benzothiazyl disulfide, and 1,3-bis(2-benzothiazyl mercaptomethyl)urea. When a crosslinking accelerator is used, the content is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and more preferably 10% by mass or less, and more preferably 5% by mass or less, based on the rubber particles in the rubber latex. The crosslinking accelerator may be used alone or in combination of two or more kinds.
[0042] Examples of the filler include metals such as aluminum, copper, and nickel, fused silica, crystalline silica, alumina, metal hydroxides such as aluminum hydroxide, calcium carbonate, calcium silicate, mica, talc, clay, titanium white, silicon nitride, boron nitride, silicon carbide, etc. The filler may be used alone or in combination of two or more.
[0043] In the mixture containing the recycled material and rubber latex, the compounding ratio of the recycled material to the rubber particles is preferably, for example, from 100% by mass to 400% by mass for the former and from 25% by mass to 100% by mass for the latter. The proportion of the recovered material in the mixture is, based on the total solid content (100 parts by mass) of the mixture, for example, 50 parts by mass or more, preferably 60 parts by mass or more, for example, 80 parts by mass or less, preferably 70 parts by mass or less. The proportion of rubber particles in the mixture is, based on the total solid content (100 parts by mass) of the mixture, for example, 20 parts by mass or more, preferably 30 parts by mass or more, and for example, 50 parts by mass or less, preferably 40 parts by mass or less.
[0044] (4. Method for Producing Rubber Latex Composition) In the present embodiment, the recycled material obtained by the above-mentioned process is mixed with rubber latex to obtain a mixture, thereby obtaining a rubber latex composition according to the present embodiment. The obtained rubber latex composition is useful for producing a molded article having excellent magnetic properties because the recycled material is uniformly dispersed and mixed in the rubber latex composition.
[0045] The mixture is prepared by adding the recovered material to the rubber latex and stirring. Regardless of the form of the recovered material to be added to the rubber latex (free-flowing powder or aggregates), when it is added to the rubber latex and stirred, the recovered material is instantly disintegrated and dispersed by the moisture in the rubber latex. The temperature and time during mixing are not particularly limited.
[0046] In this embodiment, since the magnetic particles are mixed with the rubber latex in a solid (powdered) form, the ratio (concentration) of the magnetic particles in the mixture can be increased compared to the case where the magnetic particles are mixed with the rubber latex in a liquid (magnetic functional fluid) form. Specifically, the ratio of the magnetic particles in the mixture based on the total amount of solids in the mixture (100 parts by mass) can be set to, for example, 50 parts by mass or more (preferably 60 parts by mass or more).
[0047] (5. Molded body and its manufacturing method) The molded article according to the present embodiment is made of a crosslinked product of the molding material when the molding material contains a crosslinking agent. The molding material is made of the rubber latex composition according to the present embodiment obtained by the above-mentioned process. In the present embodiment, the rubber latex composition obtained by the above-mentioned process is subjected to a desired molding process (molding processing) according to the rubber particles in the latex used in the production of the composition, to obtain a molded article according to the present embodiment. The obtained molded article can be used for various applications (for example, in the medical field) according to the purpose.
[0048] As the molding process, various molding methods can be adopted depending on the characteristics of the rubber constituting the particles in the latex used in the production of the above-mentioned crosslinkable composition. Examples of the molding method include cast molding, dipping molding, LIM molding, etc. The shape of the molded product obtained by such a molding method is not particularly specified.
[0049] The mechanism by which the molded article according to the present embodiment exhibits excellent magnetic properties is not clear, but is believed to be as follows. First, when fine magnetic particles are dispersed in a rubber matrix, aggregation is likely to occur. In this case, the magnetic properties of the fine magnetic particles cannot be expressed. In contrast, according to the present invention, a polar solvent-based magnetic functional fluid is prepared, and the dispersion medium (polar liquid) in this magnetic functional fluid is removed by a specific processing operation (vacuum freeze-drying) and recovered. The recovered material is in the form of a smooth powder, and at least a part of the magnetic particle surface is coated with a dispersant (preferably a surfactant) contained in the magnetic functional fluid. In other words, since at least a part of the magnetic particle surface of the recovered material is coated with a dispersant (preferably a surfactant), oxidation in the atmosphere as a powder is suppressed. Secondly, taking magnetic fluid as an example, the magnetic particles in the magnetic fluid exist as superparamagnetic materials, and when this magnetic fluid is used as the starting material (material to be dried) and turned into a magnetic powder by vacuum freeze-drying, even if the recovered material appears to be an aggregate, it will not re-aggregate at the nano-order level and will be turned into powder while maintaining its superparamagnetic state. Thirdly, even if the recovered material after vacuum freeze-drying appears to be aggregated, it is instantly broken down, dispersed and mixed by the moisture in the rubber latex. For these reasons, when a molded body is produced using the rubber latex composition according to the present embodiment, which is a mixture of recycled materials and rubber latex, under processing conditions suitable for the rubber particles in the rubber latex, the obtained molded body is presumed to have magnetic properties similar to those of the magnetic functional fluid (e.g., magnetic hysteresis is not observed in the magnetic fluid). EXAMPLES
[0050] The present invention will be specifically described below based on experimental examples (including examples and comparative examples), but the present invention is not limited to these examples. In the following description, "%" indicates "% by mass".
[0051] (1. Raw materials) The following raw materials (materials to be dried) were prepared: "Magnetic fluid 1": Water-based magnetic fluid (solid content 22.4%, product name "EXP.14005", Ferrotec Corporation, solid content: magnetite particles (magnetic particles) coated with sodium oleate (dispersant) with an average particle size of 40 nm, dispersion medium (polar liquid): water) "Magnetic fluid 2": Oil-based magnetic fluid (solid content 80%, product name "EXP.12038", Ferrotec Corporation, solid content: magnetite particles (magnetic particles) coated with sodium oleate (dispersant) with an average particle size of 15 nm, dispersion medium (non-polar liquid): isoparaffin)
[0052] (2. Recovered items) The raw materials described in the above (1. Raw materials) were subjected to the following treatment to obtain recovered materials 1 to 3 in Experimental Examples 1 to 3 (Experimental Examples 4 and 5 were untreated).
[0053] "Vacuum freeze-drying method": 2 liters of magnetic fluid 1 was dispensed into an aluminum container and placed on a shelf in a freeze-dryer (RLEII-103 model, manufactured by Kyowa Vacuum Engineering Co., Ltd.). Next, reduced pressure drying was performed at -56°C under 133 Pa (shelf temperature: 40°C) for 24 hours. After that, the container was removed from the freeze-dryer, and recovered material 1 of Experimental Example 1 was obtained. "Evaporation method": 100 ml of magnetic fluid 1 was placed in a beaker and dried at a drying temperature of 80° C. under atmospheric pressure for 8 hours to obtain recovered material 2 of Experimental Example 2. "Coagulation and Sedimentation Method": 50 ml of magnetic fluid 2 was taken, 50 ml of ethanol (85% aqueous solution) was added, and the mixture was thoroughly stirred to cause the magnetic particles to coagulate and settle. The settling time was 24 hours. After that, the ethanol was filtered off to obtain the recovered material 3 of Experimental Example 3.
[0054] (3. Evaluation of Recovered Items 1) The state of each of the recovered materials 1 to 3 obtained in Experimental Examples 1 to 3 was visually observed. As a result, recovered material 1 in Experimental Example 1 was in the form of a smooth powder. Recovered materials 2 and 3 in Experimental Examples 2 and 3 were both in the form of a rough crystalline powder (no recovered material was obtained in Experimental Examples 4 and 5).
[0055] (4. Mixing with rubber latex) 20 g of natural rubber latex (60% solids, product name "Halatex", manufactured by Resitex Corporation) was added and mixed with 20 g of each of the recovered materials from Experimental Examples 1, 2, and 3, 89.3 g of magnetic fluid 1 from Experimental Example 4, and 25 g of magnetic fluid 2 from Experimental Example 5 to obtain the rubber latex compositions of Experimental Examples 1 to 5.
[0056] (5. Evaluation of Rubber Latex Composition 2) The following evaluation of 5-1 was carried out for each of the rubber latex compositions of Experimental Examples 1 to 5. The results are shown in Table 1.
[0057] (5-1. Mixed state) The state of the recovered matter in each rubber latex composition was visually observed and evaluated according to the following criteria. "〇": Good (no separation or aggregation in the rubber latex composition of the recovered material) "△": Partially defective (10% or more and less than 30% of the collected material is separated and aggregated in the rubber latex composition) "X": Poor (30% or more of the collected material is separated and aggregated in the rubber latex composition)
[0058] (6. Production of Molded Body) The rubber latex compositions of Experimental Examples 1 and 4, which were in a good mixed state, were placed in a 100 ml disposable cup (manufactured by AS ONE Corporation) and dried under conditions of 90°C x 3 hours to prepare molded bodies of Experimental Examples 1 and 4.
[0059] (7. Evaluation of Molded Products 3) The molded articles of Experimental Examples 1 and 4 were evaluated in accordance with the following items 7-1 and 7-2. The results are shown in Table 1.
[0060] (7-1. Shape stability) The shape stability of each molded article taken out of the disposable cup was visually observed and evaluated according to the following criteria. "〇": Good (can be removed from disposable cup and retains shape) "X": Defective (cannot be removed from the disposable cup or the molded body is partially damaged when removed.)
[0061] (7-2. Moisture residue) Each molded article was removed from the disposable cup and evaluated for residual moisture according to the following criteria. "〇": Good (water does not flow out even when the surface of the molded product is pressed with a finger) "X": Defective (water flows out when the surface of the molded product is pressed with a finger)
[0062] [Table 1]
[0063] (8. Discussion) As shown in Table 1, the recovered material 1 of Experimental Example 1, which was obtained by vacuum freeze-drying a water-based magnetic functional fluid, which is an example of a polar solvent-based magnetic functional fluid, had a smooth powdery form (evaluation 1) and was confirmed to have good compatibility with the rubber latex mixture, that is, no separation or aggregation (evaluation 2: ○). In contrast, the recovered material 2 of Experimental Example 2, which was obtained by the evaporation method using a water-based magnetic fluid as the dried material, had a rough crystalline powder form (evaluation 1), and was confirmed to have poor compatibility with the rubber latex mixture (evaluation 2: ×). The recovered material 3 of Experimental Example 3, which was obtained by the coagulation and sedimentation method using an oil-based magnetic fluid as the dried material, also had a rough crystalline powder form (evaluation 1), similar to the recovered material 2, and was confirmed to have poor compatibility with the rubber latex mixture (evaluation 2: ×). The rubber latex composition of Experimental Example 4, obtained by mixing a water-based magnetic fluid with rubber latex without carrying out any treatment to remove the dispersing medium, had a good mixed state (evaluation 2 was O), whereas the rubber latex composition of Experimental Example 5, obtained by mixing an oil-based magnetic fluid with rubber latex without carrying out any treatment to remove the dispersing medium, had a poor mixed state (evaluation 2 was X).
[0064] The molded article of Experimental Example 1, which was produced from the rubber latex composition obtained using the recovered material 1, was confirmed to have good shape stability and water residual property (both in Evaluation 3: ○). In contrast, the molded article of Experimental Example 4, which was produced from the rubber latex composition obtained by mixing the water-based magnetic fluid with rubber latex, had good shape stability (Evaluation 3: shape stability: ○), but was confirmed to have deteriorated water residual property (Evaluation 3: water residual property: ×).
[0065] From the above, the usefulness of the recovered material 1 obtained in Experimental Example 1, the rubber latex composition produced using the recovered material 1, and the molded article produced from the rubber latex composition was confirmed.
Claims
1. A method for producing a rubber latex composition for use in producing a molded article, comprising the steps of: A method for producing a rubber latex composition, comprising the steps of: removing the polar liquid from a polar solvent-based magnetic fluid in which magnetic particles having an average primary particle diameter of 50 nm or less are dispersed using the polar liquid as a solvent, by vacuum freeze-drying to obtain a recovered material; and mixing the recovered material obtained by the above step with rubber latex to obtain a mixture of the recovered material and rubber latex.
2. 2. The method according to claim 1, wherein the polar liquid is water or a mixture of water and a water-soluble organic solvent.
3. The method of claim 1 or 2, further comprising the step of adding other ingredients to the mixture, including a cross-linking agent.
4. A method for producing a molded article, comprising a step of molding using the rubber latex composition produced by the method according to any one of claims 1 to 3.
Citation Information
Patent Citations
Separation of ultrafine particle of magnetic substance
JP1986220719A
Method for concentrating water soluble magnetic fluid
JP1986222591A
Method for producing magnetic rubber material
JP2002127170A
Ferrite magnetic powder and its manufacturing method
JP2004265936A
Magnetic polymer particles for liquid magnetography and developer for liquid magnetography
JP2009103959A