Polishing composition, substrate manufacturing method and polishing method

A polishing composition with silica particles of defined size and aspect ratio, combined with an acid and oxidizing agent, addresses the challenge of achieving high workability and low micro waviness in magnetic disk substrate polishing, enhancing both efficiency and surface quality.

JP7587954B2Active Publication Date: 2024-11-21FUJIMI INCORPORATED
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020165691
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-30
Publication Date
2024-11-21
Estimated Expiration
2040-09-30

AI Technical Summary

Technical Problem

In polishing magnetic disk substrates, it is challenging to achieve high workability while suppressing micro waviness, as using silica abrasive grains leads to difficulty in maintaining processing power and results in increased minute waviness.

Method used

A polishing composition containing silica particles with specific size and aspect ratio ranges, along with an acid and an oxidizing agent, is used to enhance workability while minimizing micro waviness.

Benefits of technology

The composition achieves high polishing rates while effectively reducing micro waviness, resulting in improved substrate surface quality and productivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587954000001
    Figure 0007587954000001
Patent Text Reader

Abstract

To provide a polishing composition which offers high processability while suppressing fine waviness to a given level when polishing a magnetic disk substrate.SOLUTION: A composition for polishing magnetic disk substrates is provided. The polishing composition contains silica particles as abrasive grains, an acid, an oxidizing agent, and water. The silica particles have a particle diameter (D1) in a range of 20 to 70 nm, inclusive, as converted from specific surface area measured by the BET method. An average aspect ratio of a particle group having particle diameters of D1 or less is in a range of 1.10 to 1.50 according to SEM image analysis. A ratio (D2 / D1) of an average particle diameter (D2) on the volume basis by SEM image analysis to D1 is in a range of 2.0 to 5.5, inclusive.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polishing composition used for polishing a magnetic disk substrate, a method for producing the substrate, and a method for polishing the substrate. [Background technology]

[0002] Conventionally, the manufacturing process of magnetic disk substrates, which require a highly accurate surface, includes a step of polishing the substrate, which is the raw material of the substrate, using a polishing liquid. For example, in the manufacture of nickel-phosphorus-plated disk substrates (hereinafter also referred to as Ni-P substrates), polishing that places emphasis on polishing efficiency (primary polishing) and final polishing (finish polishing) to finish the surface of the final product are generally performed. Patent documents 1 and 2 are cited as technical documents related to polishing compositions used for polishing magnetic disk substrates. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2017-102990 A [Patent Document 2] JP 2019-029044 A Summary of the Invention [Problem to be solved by the invention]

[0004] In the polishing of magnetic disk substrates, efforts to improve the quality of the substrate surface are continuously made in order to increase the recording capacity. In recent years, in order to improve the quality of the substrate surface after the finish polishing, silica abrasive grains are used instead of alumina abrasive grains from the stage of primary polishing. Compared with polishing using alumina abrasive grains, polishing using silica abrasive grains does not pierce the substrate with abrasive grains, is excellent in reducing defects such as scratches, and is easy to obtain high surface quality. On the other hand, polishing using silica abrasive grains is difficult to obtain a processing force like that of a slurry containing alumina abrasive grains, and maintaining and improving the processing force is an issue. In addition to maintaining and improving such processing force, micro-waviness on the substrate after polishing is also an issue. In the above-mentioned polishing, high processability and maintaining low micro-waviness are in a contradictory relationship in which trying to improve one will deteriorate the other, and it is not easy to achieve both.

[0005] The present invention has been created in view of the above circumstances, and aims to provide a polishing composition that can suppress the increase in microwaviness and exhibit high processability when polishing a magnetic disk substrate. Another related object is to provide a method for manufacturing a substrate and a method for polishing the substrate using the polishing composition. [Means for solving the problem]

[0006] According to the present specification, a magnetic disk substrate polishing composition is provided. This polishing composition contains silica particles as abrasive grains, an acid, an oxidizing agent, and water. The silica particles have a particle diameter (D1) calculated from the specific surface area measured by the BET method of 20 nm to 70 nm, and the average aspect ratio of the particle group having a particle diameter of D1 or less by SEM image analysis is 1.10 to 1.50, and the ratio (D2 / D1) of the volume-based average particle diameter (D2) by SEM image analysis to D1 is 2.0 to 5.5. The polishing composition can achieve high processability while suppressing the increase in microwaviness in polishing a magnetic disk substrate. In addition, suppressing an increase in microwaviness includes not only reducing the microwaviness but also suppressing the microwaviness in relation to an increase in processability. Therefore, exhibiting high processability while suppressing an increase in microwaviness includes, for example, improving the ratio of the polishing rate as processability to the microwaviness, i.e., the "polishing rate / microwaviness" ratio.

[0007] In some preferred embodiments, D2 is less than 180 nm. With such a configuration, the effects of the technology disclosed herein are preferably realized.

[0008] The present specification also provides a method for producing a magnetic disk substrate. The method includes step (1) of polishing a substrate to be polished using any of the polishing compositions disclosed herein. This method allows a magnetic disk substrate having a high-quality surface to be produced with good productivity. In some embodiments, the method for producing the substrate further includes step (2) of polishing the substrate to be polished using a finish polishing composition after step (1). The finish polishing composition preferably contains colloidal silica. By carrying out step (2) after step (1), a magnetic disk substrate having a higher quality surface can be produced with good productivity.

[0009] The present specification also provides a method for polishing a substrate. The polishing method includes step (1) of supplying any one of the polishing compositions disclosed herein to a substrate to be polished and polishing the substrate. Such a polishing method can efficiently improve the surface quality of the polished object. In some embodiments, the method for polishing a substrate further includes step (2) of supplying a finish polishing composition to the substrate to be polished after step (1) and polishing the substrate to be polished. The finish polishing composition preferably contains colloidal silica. By carrying out step (2) after step (1), a substrate surface of higher quality can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Preferred embodiments of the present invention will be described below. Note that matters other than those specifically mentioned in this specification that are necessary for carrying out the present invention can be understood as design matters for a person skilled in the art based on the prior art in the relevant field. The present invention can be carried out based on the contents disclosed in this specification and the technical common sense in the relevant field.

[0011] <Polishing composition> (Silica particles) The polishing composition disclosed herein contains silica particles as abrasive grains. The silica particles have a particle diameter (D1) calculated from the specific surface area measured by the BET method in the range of 20 nm to 70 nm. The silica particles have an average aspect ratio (D1 or less particle aspect ratio) of 1.10 to 1.50 of a particle group having a particle diameter of D1 or less as determined by SEM image analysis. The silica particles have a ratio (D2 / D1) of the volume-based average particle diameter (D2) to D1 as determined by SEM image analysis in the range of 2.0 to 5.5. The polishing composition containing the silica particles can suppress microwaviness to a predetermined level and achieve high processability in polishing a magnetic disk substrate.

[0012] The reason why the above-mentioned configuration achieves the effect of the technology disclosed herein is considered to be the following, although it is not particularly limited to the above. That is, the above ratio (D2 / D1) represents the degree of association of silica particles. When the above ratio (D2 / D1) is within the range of 2.0 to 5.5, the associated particles are in an associated state with appropriate size and strength, and it is considered that the loss of processing energy due to the destruction of the associated state during polishing is small, and good processability is exhibited. Furthermore, when D1 of the silica particles is within the range of 20 to 70 nm, the coarsening of secondary particles formed by the association of primary particles is suppressed, and as a result, local pressure concentration is unlikely to occur during polishing, and the increase of microwaviness is suppressed. It has also been found that particles produced by conventional methods contain small particles with low aspect ratios and large particles that have a higher aspect ratio and larger particle diameter than the small particles as a result of association. As a result, during polishing, pressure concentration occurs due to the suppression of rolling of the large particles with high aspect ratios and large particle diameters, resulting in high processability, but high micro-waviness after polishing. It is believed that the small particles contained in conventional particles do not contribute to improved processability in terms of size and shape. In the particles used in the present disclosure, both the associated large particles and small particles (particles of D1 or less) have a high aspect ratio in the range of 1.10 to 1.50. It has been found that this suppresses the rolling of the small particles and improves the processing power. In addition, by using an associated particle group containing small particles with such a high aspect ratio, the increase in microwaviness is suppressed and the processability is improved. Note that the above explanation is the inventor's consideration based on experimental results, and the technology disclosed herein should not be interpreted as being limited to the above mechanism.

[0013] From the viewpoint of maintaining low microwaviness, D1 of the silica particles is preferably about 65 nm or less, more preferably about 60 nm or less, even more preferably about 50 nm or less, and particularly preferably about 40 nm or less (for example, about 35 nm or less). By using silica particles whose particle diameter is controlled to a relatively small predetermined range in this way, microwaviness can be suppressed to a predetermined level. Moreover, from the viewpoint of processability, the above D1 is preferably about 24 nm or more, more preferably 27 nm or more, and may be about 30 nm or more. According to the technology disclosed herein, a high processing power can be exhibited in an embodiment using silica particles having D1 limited as described above.

[0014] Moreover, from the viewpoint of achieving both high processability and low microwaviness, the above-mentioned D1 or less particle aspect ratio is preferably 1.13 or more, more preferably 1.15 or more, and may be 1.20 or more, or may be 1.25 or more. Moreover, the above-mentioned D1 or less particle aspect ratio is suitably 1.40 or less, may be 1.35 or less, or may be 1.30 or less. According to the technology disclosed herein, even in an embodiment in which the above-mentioned D1 or less particle aspect ratio is 1.25 or less, or even 1.20 or less, it is possible to preferably achieve both high processability and low microwaviness.

[0015] From the viewpoint of achieving both high processability and low microwaviness, the ratio (D2 / D1) is preferably 5.0 or less, more preferably 4.5 or less, and even more preferably 4.2 or less, and may be 4.0 or less (e.g., 3.8 or less). The ratio (D2 / D1) may be, for example, more than 2.0, preferably 2.5 or more, more preferably 2.8 or more, and from the viewpoint of improving processability, it may be more than 3.0, 3.5 or more, or 4.0 or more.

[0016] D2 of the silica particles (average particle diameter on a volume basis by SEM image analysis) is appropriately set based on the range of the above D1 and the above ratio (D2 / D1), and is not limited to a specific range. D2 of the silica particles is about 40 nm or more, and is appropriately about 70 nm or more, preferably 90 nm or more, more preferably 95 nm or more, and may be, for example, 100 nm or more, or may be 110 nm or more. Also, D2 of the silica particles is about 385 nm or less, and is appropriately 300 nm or less. In some preferred embodiments, D2 of the silica particles is 155 nm or less. By using such silica particles, it is possible to preferably achieve both high processability and low microwaviness. The above D2 is more preferably 150 nm or less, even more preferably 130 nm or less, and particularly preferably 120 nm or less.

[0017] Although not particularly limited, the average aspect ratio of the silica particles (which may be in the form of primary particles or secondary particles) used in the technology disclosed herein is preferably about 1.10 or more, more preferably about 1.15 or more, and even more preferably about 1.20 or more, from the viewpoint of maintaining or improving processability. In addition, from the viewpoint of efficiently improving surface quality, in some embodiments, the average aspect ratio is suitably 2.50 or less, preferably 2.0 or less, more preferably 1.70 or less, even more preferably 1.50 or less, and may be 1.35 or less. In silica particles having an average aspect ratio in such a range, the effects of setting D1, D1 particle aspect ratio, and ratio (D2 / D1) to a predetermined range are preferably exhibited.

[0018] In the technology disclosed herein, the particle diameter (D1) of the silica particles is calculated from the specific surface area (BET value) measured by the BET method as follows: Particle diameter (D1) nm = 6000 / (true density (g / cm 3 ) × BET value (m 2 The specific surface area is the particle size (BET particle size) calculated by the formula: (1 / g). The specific surface area can be measured, for example, by using a surface area measuring device manufactured by Mountech Co., Ltd. under the trade name "Macsorb". The same applies to the examples described later.

[0019] The particle aspect ratios D2, D1 and below and the average aspect ratio of silica particles are determined by the following method. That is, using a scanning electron microscope (SEM), 1000 or more particles contained in a dispersion of silica particles to be measured (which may be one type of silica particles or a mixture of two or more types of silica particles) are observed in an SEM image containing 50 or more particles in one field of view. The observation magnification is 20,000 to 50,000 times. Then, for the smallest rectangle circumscribing each particle image, the value obtained by dividing the length of its long side (long axis value) by the length of its short side (short axis value) is calculated as the long axis / short axis ratio (aspect ratio) of each particle. In addition, 4πr from the radius r of an ideal circle (true circle) having an area equal to the projected area of ​​each particle image is calculated. 3The value obtained by / 3 is calculated as the volume of each particle. Here, the aspect ratio and volume are calculated by counting particles dispersed independently in the silica particle dispersion as one particle, regardless of whether they are primary particles or secondary particles. D2 is calculated as the average particle diameter calculated from the volume-based particle size distribution obtained from the volume of the predetermined number of particles. In addition, the particle aspect ratio of D1 or less is calculated by the following method. That is, the particle diameter (volume basis) of each particle is obtained from the volume of each particle obtained by the above measurement, and particles (particle group) whose particle diameter is smaller than D1 (BET specific surface area converted particle diameter) [nm] calculated for the silica particles to be measured are extracted. Then, the aspect ratios obtained for each particle of the extracted particle group are arithmetically averaged to obtain the number-average aspect ratio (particle aspect ratio of D1 or less) of the particle group having a particle diameter of D1 or less. The average aspect ratio of silica particles is the average aspect ratio based on the number of all silica particles (number-average aspect ratio), and can be obtained by arithmetically averaging the aspect ratios of all particles by SEM image analysis. The above D2, D1 and below particle aspect ratios and average aspect ratios can be obtained using a general SEM and image analysis software. For example, a scanning electron microscope "SU8000" manufactured by Hitachi High-Technologies Corporation and image analysis type particle size distribution measurement software "Mac-View" manufactured by Mountec Co., Ltd. are used. The same applies to the examples described below.

[0020] Silica particles having the above D1, particle aspect ratio below D1, and ratio (D2 / D1) can be adjusted by selecting the type of silica particles used, selecting or adjusting the silica manufacturing method, mixing two or more types of silica particles having different particle shapes, etc. For example, based on the description of this specification and taking into consideration common general knowledge, one type of particle group having a specific particle size and aspect ratio, or two or more types of particle groups, and mixing them in an appropriate ratio, can be used to obtain the silica particles disclosed herein. Also, based on the description of this specification and taking into consideration common general knowledge, it is possible to adopt, for example, a method of crushing porous silica gel under appropriate conditions to obtain irregularly shaped particles, or a method of growing the obtained irregularly shaped particles by adding a predetermined amount of silicate under appropriate conditions (pH, temperature conditions, etc.) to obtain irregularly shaped particles having a desired particle size. By mixing one type of particle obtained in this way alone or with other silica particles having different particle properties, the silica particles disclosed herein can be obtained.

[0021] The silica particles are not particularly limited as long as they satisfy the predetermined D1, particle aspect ratio below D1, and ratio (D2 / D1), and various silica particles mainly composed of silica can be used. Here, silica particles mainly composed of silica refer to particles in which 90% by weight or more, for example 95% by weight or more, typically 98% by weight or more of the particles are silica. Examples of silica particles that can be used are not particularly limited, and include colloidal silica, agglomerated silica, precipitated silica (also called precipitated silica), sodium silicate silica, alkoxide silica, fumed silica, dried silica, and detonation silica. Furthermore, silica particles obtained using the above silica particles as raw materials can also be used. Examples of such silica particles include silica particles obtained by applying one or more treatments selected from heat treatments such as heating, drying, and firing, pressure treatments such as autoclaving, mechanical treatments such as crushing and grinding, and surface modification to the above raw silica particles (hereinafter also called "raw silica"). Examples of surface modification include chemical modification such as introduction of functional groups and metal modification. The silica particles in the technology disclosed herein may contain one type of silica particles as described above, either alone or in combination of two or more types.

[0022] In the technology disclosed herein, the silica particles may be in the form of secondary particles formed by agglomeration of a plurality of primary particles, or in the form of secondary particles formed by association of a plurality of primary particles. Furthermore, silica particles in the form of primary particles and silica particles in the form of secondary particles may be mixed.

[0023] The content of silica particles in the polishing composition is not particularly limited, and is, for example, 0.1% by weight or more, preferably 0.5% by weight or more, more preferably 1% by weight or more, even more preferably 3% by weight or more, and particularly preferably 5% by weight or more. When multiple types of silica particles are contained, the above content is the total content thereof. By increasing the content of silica particles, higher processability tends to be obtained. From the viewpoint of the surface smoothness of the substrate after polishing and the stability of polishing, the above content is appropriately 30% by weight or less, preferably 25% by weight or less, more preferably 15% by weight or less, and even more preferably 10% by weight or less.

[0024] In the polishing composition disclosed herein, the content of silica particles in the solid content contained in the polishing composition is preferably 90% by weight or more of the total solid content, more preferably 95% by weight or more, even more preferably 98% by weight or more, for example 99% by weight or more, from the viewpoint of better exerting the effects of the technology disclosed herein. Note that, in this specification, the solid content contained in the polishing composition refers to the residual content, i.e., the non-volatile content, after evaporating water from the polishing composition at a temperature at which bound water is not removed, for example, 60°C.

[0025] The polishing composition disclosed herein can be preferably implemented in an embodiment that does not substantially contain alumina particles. Examples of the alumina particles include α-alumina particles. Such a polishing composition prevents quality degradation caused by the use of alumina particles. Examples of quality degradation include the occurrence of scratches and dents, alumina residue, and puncture defects. In this specification, "substantially does not contain alumina particles" means that the proportion of alumina particles in the total solid content contained in the polishing composition is 1% by weight or less, more preferably 0.5% by weight or less, and typically 0.1% by weight or less. A polishing composition with a proportion of alumina particles of 0% by weight, that is, a polishing composition that does not contain alumina particles, is particularly preferred. In addition, the polishing composition disclosed herein can be preferably implemented in an embodiment that does not substantially contain α-alumina particles.

[0026] The polishing composition disclosed herein can also be preferably implemented in an embodiment that does not substantially contain particles other than silica particles, i.e., non-silica particles.Here, "does not substantially contain non-silica particles" means that the proportion of non-silica particles in the total solid content contained in the polishing composition is 1% by weight or less, more preferably 0.5% by weight or less, typically 0.1% by weight or less.In such an embodiment, the application effect of the technology disclosed herein can be preferably exhibited.

[0027] (acid) The polishing composition disclosed herein contains an acid as a polishing accelerator. The acid may be either an inorganic acid or an organic acid. Examples of the organic acid include organic carboxylic acids, organic sulfonic acids, and amino acids having about 1 to 18 carbon atoms, typically about 1 to 10 carbon atoms. The acid may be used alone or in combination of two or more.

[0028] Specific examples of inorganic acids include phosphoric acid (orthophosphoric acid), nitric acid, sulfuric acid, hydrochloric acid, boric acid, sulfamic acid, phosphinic acid, phosphonic acid, pyrophosphoric acid, tripolyphosphoric acid, tetrapolyphosphoric acid, hexametaphosphoric acid, carbonic acid, hydrofluoric acid, sulfurous acid, thiosulfuric acid, chloric acid, perchloric acid, chlorous acid, hydroiodic acid, periodic acid, iodic acid, hydrobromic acid, perbromic acid, bromic acid, chromic acid, and nitrous acid.

[0029] Specific examples of organic acids include citric acid, maleic acid, malic acid, glycolic acid, succinic acid, itaconic acid, malonic acid, iminodiacetic acid, gluconic acid, lactic acid, mandelic acid, tartaric acid, formic acid, acetic acid, propionic acid, butyric acid, adipic acid, oxalic acid, valeric acid, enanthic acid, caproic acid, caprylic acid, pelargonic acid, capric acid, lauric acid, myristic acid, palmitic acid, margaric acid, stearic acid, cyclohexanecarboxylic acid, phenylacetic acid, benzoic acid, crotonic acid, oleic acid, linoleic acid, linolenic acid, ricinoleic acid, and methacrylic acid. , glutaric acid, fumaric acid, phthalic acid, isophthalic acid, terephthalic acid, tartronic acid, glyceric acid, hydroxybutyric acid, hydroxyacetic acid, hydroxybenzoic acid, salicylic acid, isocitric acid, methylenesuccinic acid, gallic acid, ascorbic acid, nitroacetic acid, oxaloacetic acid, chloroacetic acid, dichloroacetic acid, trichloroacetic acid, and other organic carboxylic acids; glycine, alanine, glutamic acid, aspartic acid, valine, leucine, isoleucine, serine, threonine, cysteine, methionine, phenylalanine, tryptophan, tyrosine, proline, Amino acids such as lysine, cystine, glutamine, asparagine, lysine, and arginine; nicotinic acid; picric acid; picolinic acid; phytic acid; 1-hydroxyethylidene-1,1-diphosphonic acid, aminotri(methylenephosphonic acid), ethylenediaminetetra(methylenephosphonic acid), diethylenetriaminepenta(methylenephosphonic acid), ethane-1,1-diphosphonic acid, ethane-1,1,2-triphosphonic acid, ethane-1-hydroxy-1,1-diphosphonic acid, ethanehydroxy-1,1,2-triphosphonic acid, ethane-1 , organic phosphonic acids such as 2-dicarboxy-1,2-diphosphonic acid, methanehydroxyphosphonic acid, 2-phosphonobutane-1,2-dicarboxylic acid, 1-phosphonobutane-2,3,4-tricarboxylic acid, α-methylphosphonosuccinic acid, and aminopoly(methylenephosphonic acid); and organic sulfonic acids such as methanesulfonic acid, ethanesulfonic acid, aminoethanesulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, 2-naphthalenesulfonic acid, sulfosuccinic acid, 10-camphorsulfonic acid, isethionic acid, and taurine.

[0030] Examples of preferred acids from the viewpoint of polishing efficiency include phosphoric acid, phosphonic acid, maleic acid, hydrochloric acid, nitric acid, sulfuric acid, sulfamic acid, phytic acid, 1-hydroxyethylidene-1,1-diphosphonic acid, methanesulfonic acid, etc. Among these, phosphoric acid, phosphonic acid, maleic acid, hydrochloric acid, nitric acid, and sulfuric acid are preferred.

[0031] The acid may be used in the form of a salt of the acid. Examples of the salt include metal salts, ammonium salts, alkanolamine salts, etc. of the above-mentioned inorganic acids and organic acids. Examples of the metal salts include alkali metal salts such as lithium salts, sodium salts, and potassium salts. Examples of the ammonium salts include quaternary ammonium salts such as tetramethylammonium salts and tetraethylammonium salts. Examples of the alkanolamine salts include monoethanolamine salts, diethanolamine salts, and triethanolamine salts. Specific examples of salts include alkali metal phosphates and alkali metal hydrogen phosphates such as tripotassium phosphate, dipotassium hydrogen phosphate, potassium dihydrogen phosphate, trisodium phosphate, disodium hydrogen phosphate, sodium dihydrogen phosphate, etc.; alkali metal salts of the organic acids exemplified above; and, in addition, alkali metal salts of glutamic acid diacetate, alkali metal salts of diethylenetriaminepentaacetic acid, alkali metal salts of hydroxyethylethylenediaminetriacetic acid, alkali metal salts of triethylenetetraminehexaacetic acid; etc. The alkali metal in these alkali metal salts may be, for example, lithium, sodium, potassium, etc.

[0032] As the salt that can be contained in the polishing composition disclosed herein, a salt of an inorganic acid, for example, an alkali metal salt or an ammonium salt, can be preferably used. For example, potassium chloride, sodium chloride, ammonium chloride, potassium nitrate, sodium nitrate, ammonium nitrate, potassium phosphate, etc. can be preferably used.

[0033] The acid and its salt can be used alone or in combination of two or more (e.g., two or three). In some preferred embodiments, the acid can be used in combination with a salt of an acid different from the acid. The acid is preferably an inorganic acid. The acid salt is preferably an inorganic acid salt.

[0034] The molar concentration of the acid in the polishing composition (when a plurality of kinds of acids are contained, the total molar concentration of the acids) is not particularly limited, and is preferably about 0.001 mol / L or more, more preferably about 0.01 mol / L or more, more preferably about 0.05 mol / L or more, even more preferably about 0.07 mol / L or more, and particularly preferably about 0.09 mol / L or more. By increasing the molar concentration of the acid, higher processability can be realized. From the viewpoint of the surface quality after polishing and the stability of polishing, the molar concentration of the acid is preferably about 1.2 mol / L or less, more preferably about 1 mol / L or less, more preferably about 0.8 mol / L or less, even more preferably about 0.5 mol / L or less, and particularly preferably about 0.3 mol / L or less (for example, 0.2 mol / L or less).

[0035] (Oxidizing agent) The polishing composition disclosed herein contains an oxidizing agent. Examples of the oxidizing agent include, but are not limited to, peroxide, nitric acid or its salt, periodic acid or its salt, peroxo acid or its salt, permanganic acid or its salt, chromic acid or its salt, oxyacid or its salt, metal salts, and sulfuric acid. The oxidizing agent can be used alone or in combination of two or more. Specific examples of the oxidizing agent include hydrogen peroxide, sodium peroxide, barium peroxide, nitric acid, iron nitrate, aluminum nitrate, ammonium nitrate, peroxomonosulfuric acid, ammonium peroxomonosulfate, metal peroxomonosulfate, peroxodisulfate, ammonium peroxodisulfate, metal peroxodisulfate, peroxolinic acid, peroxosulfuric acid, sodium peroxoborate, performic acid, peracetic acid, perbenzoic acid, perphthalic acid, hypobromous acid, hypoiodous acid, chloric acid, bromic acid, iodic acid, periodic acid, perchloric acid, hypochlorous acid, sodium hypochlorite, calcium hypochlorite, potassium permanganate, metal chromate, metal dichromate, iron chloride, iron sulfate, iron citrate, ammonium iron sulfate, etc. Preferred examples of the oxidizing agent include hydrogen peroxide, iron nitrate, periodic acid, peroxomonosulfuric acid, peroxodisulfuric acid, and nitric acid. It preferably contains at least hydrogen peroxide, and more preferably consists of hydrogen peroxide.

[0036] The content of the oxidizing agent in the polishing composition is preferably 0.05 mol / L or more, more preferably 0.1 mol / L or more, even more preferably 0.15 mol / L or more, and particularly preferably 0.3 mol / L or more, in consideration of the speed of oxidizing the object to be polished and therefore the processability. Also, the content of the oxidizing agent in the polishing composition is preferably 1 mol / L or less, more preferably 0.8 mol / L or less, and even more preferably 0.6 mol / L or less, in consideration of maintaining surface accuracy.

[0037] (water) The polishing composition disclosed herein typically contains water to disperse the abrasive grains in addition to the above-mentioned abrasive grains. As the water, ion-exchanged water, pure water, ultrapure water, distilled water, etc. can be preferably used. The ion-exchanged water can typically be deionized water.

[0038] The polishing composition disclosed herein can be preferably implemented in a form in which the solid content is, for example, 0.5% by weight to 30.0% by weight. The solid content is more preferably 1.0% by weight to 20.0% by weight. The polishing composition can typically be a slurry-like composition.

[0039] (Other Ingredients) The polishing composition disclosed herein may further contain, as necessary, known additives that can be used in polishing compositions, such as surfactants, water-soluble polymers, dispersants, chelating agents, preservatives, antifungal agents, basic compounds, etc., to the extent that the effects of the present invention are not significantly impeded.

[0040] The surfactant is not particularly limited, and any of anionic surfactants, nonionic surfactants, cationic surfactants, and amphoteric surfactants can be used. The use of a surfactant can improve the dispersion stability of the polishing composition. The surfactant can be used alone or in combination of two or more. The surfactant typically has a molecular weight of 1×10 6 The water-soluble organic compound may be less than 1000 mg / kg. Specific examples of anionic surfactants include polyoxyethylene alkyl ether acetates, polyoxyethylene alkyl sulfates, alkyl sulfates, polyoxyethylene alkyl sulfates, alkyl sulfates, alkyl benzene sulfonates, alkyl phosphates, polyoxyethylene alkyl phosphates, polyoxyethylene sulfosuccinates, alkyl sulfosuccinates, alkyl naphthalene sulfonates, alkyl diphenyl ether disulfonic acids, polyacrylic acids, sodium lauryl sulfate, ammonium lauryl sulfate, sodium dodecylbenzene sulfonate, polyoxyethylene alkyl ether sodium sulfate, polyoxyethylene alkyl phenyl ether ammonium sulfate, polyoxyethylene alkyl phenyl ether sodium sulfate, and salts thereof. Other specific examples of anionic surfactants include polyalkylarylsulfonic acid compounds such as naphthalenesulfonic acid formaldehyde condensate, methylnaphthalenesulfonic acid formaldehyde condensate, anthracenesulfonic acid formaldehyde condensate, and benzenesulfonic acid formaldehyde condensate; melamine formalin resin sulfonic acid compounds such as melaminesulfonic acid formaldehyde condensate; ligninsulfonic acid compounds such as ligninsulfonic acid and modified ligninsulfonic acid; aromatic aminosulfonic acid compounds such as aminoarylsulfonic acid-phenol-formaldehyde condensate; polyisoprene sulfonic acid, polyvinylsulfonic acid, polyallylsulfonic acid, polyisoamylenesulfonic acid, polystyrenesulfonic acid; and salts thereof. As the salt, alkali metal salts such as sodium salts and potassium salts are preferred. Specific examples of nonionic surfactants include polyoxyethylene alkyl ethers, polyoxyalkylene alkyl ethers, sorbitan fatty acid esters, glycerin fatty acid esters, polyoxyethylene fatty acid esters, polyoxyethylene alkyl amines, and alkyl alkanolamides. Specific examples of the cationic surfactant include alkyltrimethylammonium salts, alkyldimethylammonium salts, alkylbenzyldimethylammonium salts, and alkylamine salts. Specific examples of amphoteric surfactants include alkyl betaine type, fatty acid amidopropyl betaine type, alkyl imidazole type, amino acid type, and alkyl amine oxide type.

[0041] In the polishing composition of the embodiment containing a surfactant, the content of the surfactant is suitably, for example, 0.0005% by weight or more. From the viewpoint of the smoothness of the surface after polishing, the content is preferably 0.001% by weight or more, more preferably 0.002% by weight or more. From the viewpoint of processability, the content is suitably, for example, 3.0% by weight or less, preferably 0.5% by weight or less, for example, 0.1% by weight or less.

[0042] The polishing composition disclosed herein may contain a water-soluble polymer. By containing a water-soluble polymer, the surface quality after polishing can be improved. Examples of water-soluble polymers include polyalkylarylsulfonic acid compounds such as naphthalenesulfonic acid formaldehyde condensates, methylnaphthalenesulfonic acid formaldehyde condensates, and anthracenesulfonic acid formaldehyde; melamine formalin resin sulfonic acid compounds such as melaminesulfonic acid formaldehyde condensates; ligninsulfonic acid compounds such as ligninsulfonic acid and modified ligninsulfonic acid; aromatic aminosulfonic acid compounds such as aminoarylsulfonic acid-phenol-formaldehyde condensates; and others, such as polyisoprene sulfonic acid, polyvinyl sulfonic acid, polyarylsulf ... Examples of the water-soluble polymer include sulfonic acid, polyisoamylenesulfonic acid, polystyrenesulfonate, polyacrylate, polyvinyl acetate, polymaleic acid, polyitaconic acid, polyvinyl alcohol, polyglycerin, polyvinylpyrrolidone, copolymer of isoprene sulfonic acid and acrylic acid, polyvinylpyrrolidone-polyacrylic acid copolymer, polyvinylpyrrolidone-vinyl acetate copolymer, diallylamine hydrochloride sulfur dioxide copolymer, carboxymethylcellulose, salt of carboxymethylcellulose, hydroxyethylcellulose, hydroxypropylcellulose, pullulan, chitosan, chitosan salts, etc. The water-soluble polymer may be used alone or in combination of two or more.

[0043] In the polishing composition of the embodiment containing a water-soluble polymer, the content of the water-soluble polymer in the polishing composition is, for example, 0.001 wt% or more. In the embodiment containing a plurality of water-soluble polymers, the content is the total content thereof. From the viewpoint of surface smoothness of the polished object after polishing, the content is preferably 0.003 wt% or more, more preferably 0.005 wt% or more, and even more preferably 0.007 wt% or more. From the viewpoint of processability, the content is preferably 1.0 wt% or less, preferably 0.5 wt% or less, for example 0.1 wt% or less. Note that, the technology disclosed herein can also be preferably implemented in the embodiment in which the polishing composition does not substantially contain a water-soluble polymer from the viewpoint of processability.

[0044] Examples of the dispersant include polycarboxylic acid-based dispersants such as sodium polycarboxylate and ammonium polycarboxylate; naphthalenesulfonic acid-based dispersants such as sodium naphthalenesulfonate and ammonium naphthalenesulfonate; alkylsulfonic acid-based dispersants; polyphosphoric acid-based dispersants; polyalkylenepolyamine-based dispersants; quaternary ammonium-based dispersants; alkylpolyamine-based dispersants; alkylene oxide-based dispersants; polyhydric alcohol ester-based dispersants; etc. The dispersants can be used alone or in combination of two or more.

[0045] Examples of the chelating agent include aminocarboxylic acid chelating agents and organic phosphonic acid chelating agents. Examples of the aminocarboxylic acid chelating agent include ethylenediaminetetraacetic acid, sodium ethylenediaminetetraacetate, nitrilotriacetic acid, sodium nitrilotriacetate, ammonium nitrilotriacetate, hydroxyethylethylenediaminetriacetic acid, sodium hydroxyethylethylenediaminetriacetate, diethylenetriaminepentaacetic acid, sodium diethylenetriaminepentaacetate, triethylenetetraminehexaacetic acid, and sodium triethylenetetraminehexaacetate. Examples of organic phosphonic acid chelating agents include 2-aminoethylphosphonic acid, 1-hydroxyethylidene-1,1-diphosphonic acid, aminotri(methylenephosphonic acid), ethylenediaminetetrakis(methylenephosphonic acid), diethylenetriaminepenta(methylenephosphonic acid), ethane-1,1-diphosphonic acid, ethane-1,1,2-triphosphonic acid, ethane-1-hydroxy-1,1-diphosphonic acid, ethane-1-hydroxy-1,1,2-triphosphonic acid, ethane-1,2-dicarboxy-1,2-diphosphonic acid, methanehydroxyphosphonic acid, 2-phosphonobutane-1,2-dicarboxylic acid, 1-phosphonobutane-2,3,4-tricarboxylic acid, and α-methylphosphonosuccinic acid. Among these, organic phosphonic acid chelating agents are more preferred, and among them, ethylenediaminetetrakis(methylenephosphonic acid) and diethylenetriaminepenta(methylenephosphonic acid) are preferred. Particularly preferred chelating agents include ethylenediaminetetrakis(methylenephosphonic acid). The chelating agents can be used alone or in combination of two or more.

[0046] Examples of the preservatives and antifungal agents include isothiazoline preservatives such as 2-methyl-4-isothiazolin-3-one and 5-chloro-2-methyl-4-isothiazolin-3-one, paraoxybenzoic acid esters, phenoxyethanol, and the like.

[0047] The polishing composition may contain a basic compound as required. Here, the basic compound refers to a compound that has the function of increasing the pH of the polishing composition by being added to the composition. Examples of basic compounds include alkali metal hydroxides, carbonates and hydrogen carbonates, quaternary ammonium or its salts, ammonia, amines, phosphates and hydrogen phosphates, organic acid salts, etc. The basic compounds may be used alone or in combination of two or more.

[0048] (pH) The pH of the polishing composition disclosed herein is not particularly limited. The pH of the polishing composition may be, for example, 12.0 or less, typically 0.5 to 12.0, or 10.0 or less, typically 0.5 to 10.0. From the viewpoint of processability, surface quality, etc., the pH of the polishing composition may be 7.0 or less, for example 0.5 to 7.0, more preferably 5.0 or less, typically 1.0 to 5.0, and even more preferably 4.0 or less, for example 1.0 to 4.0. The pH of the polishing composition may be, for example, 3.0 or less, typically 1.0 to 3.0, preferably 1.0 to 2.0, more preferably 1.0 to 1.8. In order to realize the above pH in the polishing liquid, a pH adjuster such as an organic acid, an inorganic acid, or a basic compound may be contained as necessary. The above pH may be preferably applied to a polishing composition for a magnetic disk substrate such as a nickel phosphorus substrate. In particular, it may be preferably applied to a polishing composition for primary polishing.

[0049] (polishing liquid) The polishing composition disclosed herein is typically supplied to an object to be polished in the form of a polishing liquid containing the polishing composition, and used to polish the object to be polished. The polishing liquid may be prepared, for example, by diluting the polishing composition. Here, dilution typically refers to dilution with water. Alternatively, the polishing composition may be used as a polishing liquid as it is. That is, the concept of the polishing composition in the technology disclosed herein includes both a polishing liquid (working slurry) that is supplied to an object to be polished and used to polish the object to be polished, and a concentrated liquid that is diluted and used as a polishing liquid. Such a polishing composition in the form of a concentrated liquid is advantageous from the viewpoint of convenience and cost reduction during production, distribution, storage, etc. The concentration ratio can be, for example, about 1.5 to 50 times. From the viewpoint of storage stability of the concentrated liquid, a concentration ratio of, for example, 2 to 20 times, typically about 2 to 10 times, is appropriate.

[0050] (Multi-component polishing composition) The polishing composition disclosed herein may be a one-component type or a multi-component type including a two-component type. For example, the polishing composition may be configured so that a part A containing some of the components, typically components other than water, and a part B containing the remaining components are mixed and used to polish an object to be polished. Some preferred embodiments of the multi-component polishing composition are composed of a part A containing abrasive grains and a part B containing components other than abrasive grains. The part A containing abrasive grains may further contain a dispersant. Examples of components other than abrasive grains contained in part B include acids. Part B may also contain water-soluble polymers and other additives. During mixing, an oxidizing agent such as hydrogen peroxide may be further mixed. For example, when the oxidizing agent is supplied in the form of an aqueous solution, the aqueous solution may be part C constituting the multi-component polishing composition.

[0051] The polishing composition disclosed herein can be preferably applied to polishing magnetic disk substrates such as nickel phosphorus substrates, glass substrates, and carbon substrates. In addition, the plating material may be a disk substrate having a metal layer or a metal compound layer other than a nickel phosphorus plating layer on the surface of a substrate disk. In particular, it is suitable as a polishing composition for a nickel phosphorus plated substrate having a nickel phosphorus plating layer on an aluminum alloy substrate disk. In such applications, it is particularly meaningful to apply the technology disclosed herein.

[0052] The polishing composition disclosed herein can be used particularly effectively in applications requiring high polishing efficiency, such as the preliminary polishing step in the manufacturing process of a magnetic disk substrate, which requires a highly accurate surface after the final polishing step. When there are multiple preliminary polishing steps as a step before the final polishing step, the polishing composition can be used in any of the preliminary polishing steps, and the same or different polishing compositions can be used in these preliminary polishing steps. The polishing composition disclosed herein is suitable, for example, as a polishing composition used in the primary polishing step, i.e., the first polishing step, of a magnetic disk substrate. In particular, it can be preferably used in the first polishing step, i.e., the first polishing step, after nickel phosphorus plating in the manufacturing process of a nickel phosphorus substrate.

[0053] The polishing composition disclosed herein is suitable for use in polishing a magnetic disk substrate having a surface roughness of about 20 Å to 300 Å as measured by a laser scanning surface roughness meter "TMS-3000WRC" manufactured by Schmitt Measurement System Inc., and adjusting the surface roughness of the magnetic disk substrate to 10 Å or less. In such applications, it is particularly meaningful to apply the technology disclosed herein. The surface roughness referred to here means the arithmetic mean roughness (Ra).

[0054] <Polishing method> The polishing composition disclosed herein can be suitably used for polishing a magnetic disk substrate as an object to be polished, for example, in an embodiment including the following operations. A preferred embodiment of a method for polishing an object to be polished using the polishing composition disclosed herein is described below. Hereinafter, the object to be polished is also referred to as a substrate to be polished. That is, prepare a polishing liquid (working slurry) containing any of the polishing compositions disclosed herein. The preparation of the polishing liquid may include adjusting the concentration or pH of the polishing composition to prepare the polishing liquid. The concentration adjustment may be, for example, dilution. Alternatively, the polishing composition may be used as it is as a polishing liquid.

[0055] Next, the polishing liquid is supplied to the object to be polished, and polished in a conventional manner. For example, the object to be polished is set in a general polishing device, and the polishing liquid is supplied to the surface of the object to be polished, i.e., the surface to be polished, through the polishing pad of the polishing device. Typically, the polishing liquid is continuously supplied while the polishing pad is pressed against the surface of the object to be polished, and the two are moved relatively to each other. The movement can be, for example, a rotational movement. Through such a polishing process, the polishing of the object to be polished is completed.

[0056] The polishing pad that can be used is not particularly limited. For example, polishing pads such as hard foam polyurethane type, nonwoven fabric type, suede type, etc. can be used. The suede type may be a buff pad, and typically may be a polishing pad in a non-buff state with no buffing on the surface (so-called non-buff pad). Such suede type polishing pads (typically polyurethane polishing pads) are excellent in processability and easily realize high quality of the substrate surface. The polishing pad used in the technology disclosed herein does not contain abrasive grains.

[0057] After polishing (specifically, after the primary polishing of the magnetic disk substrate), it is preferable to wash the substrate (washing step). The washing step is typically performed using a washing machine. In the washing step, a washing liquid may be used, or washing may be performed using only running water without using a washing liquid. An ultrasonic treatment may be performed in which ultrasonic waves are applied to the substrate immersed in the washing liquid or water. By performing such a washing step, silica remaining on the substrate after polishing can be efficiently removed.

[0058] The polishing machine used in the polishing step may be a double-sided polishing machine that polishes both sides of the object to be polished at the same time, or a single-sided polishing machine that polishes only one side of the object to be polished. When the polishing step is a preliminary polishing step, in some embodiments, a double-sided polishing machine may be preferably used as the polishing machine that performs the polishing step. When a finish polishing step is performed after the primary polishing step, a single-sided polishing machine may be preferably used as the polishing machine that performs the finish polishing step.

[0059] The polishing step as described above may be part of a manufacturing process for a magnetic disk substrate, for example a nickel phosphorus substrate. Therefore, according to this specification, there is provided a manufacturing method and a polishing method for a magnetic disk substrate, which includes the polishing step.

[0060] The polishing composition disclosed herein can be preferably used in a preliminary polishing step of an object to be polished, for example, a primary polishing step. According to this specification, a manufacturing method and a polishing method for a magnetic disk substrate are provided, which include a step of performing preliminary polishing using any of the polishing compositions described above. The above method includes a step (1) of supplying the polishing composition disclosed herein to an object to be polished and polishing the object to be polished. The above method may include a final polishing step after the preliminary polishing step. The polishing composition used in the final polishing step is not particularly limited. Therefore, the matter disclosed by this specification includes a manufacturing method and a polishing method for a magnetic disk substrate, which include, in this order, a step (1) of polishing an object to be polished with a polishing composition containing abrasive grains disclosed herein, and a step (2) of polishing an object to be polished with a polishing composition (e.g., a final polishing composition) different from the polishing composition used in step (1). According to such a manufacturing method, a magnetic disk substrate can be efficiently manufactured.

[0061] The abrasive grains used in step (2) are not particularly limited, and for example, colloidal silica is preferably used. By using colloidal silica, the polished object with high surface accuracy can be efficiently manufactured. The particle shape of colloidal silica is not particularly limited, and for example, it may be spherical or non-spherical, and spherical colloidal silica is preferably used.

[0062] The final polishing composition that can be used in step (2) contains water in addition to the abrasive grains. In addition, the final polishing composition can contain the same components as those in the above-mentioned polishing composition (acid, oxidizing agent, basic compound, various additives, etc.) as necessary. EXAMPLES

[0063] Some examples of the present invention will be described below, but it is not intended that the present invention be limited to those shown in these examples.

[0064] <Examples 1 to 12 and Comparative Examples 1 to 11> [Preparation of polishing composition] A polishing composition according to each example was prepared by mixing silica abrasive grains, phosphoric acid, 31% hydrogen peroxide solution, and deionized water. The pH of the polishing composition was 1.5. As the silica abrasive grains, a plurality of types of silica particles having different particle diameters, particle size distributions, and aspect ratios were prepared, and the silica particles were used alone or in combination to obtain abrasive grains having the particle diameter (D1) converted from the specific surface area measured by the BET method, the average aspect ratio of the particle group having a particle diameter of D1 or less by SEM image analysis (D1 or less particle aspect ratio), and the ratio (D2 / D1) of the volume-based average particle diameter (D2) by SEM image analysis to D1, as shown in Table 1. The D2 and average aspect ratio (average aspect ratio of the particle group of 0 to 100% cumulative volume-based by SEM image analysis) of the silica abrasive grains used are also shown in Table 1. In the polishing composition, the concentration of silica particles was 7 wt %, the concentration of phosphoric acid was 0.1 mol / L, and the concentration of hydrogen peroxide was 0.4 mol / L.

[0065] [Disc grinding] The polishing composition according to each example was used as a polishing liquid as it was, and the polishing object was polished under the following conditions. The polishing object was an aluminum substrate for a hard disk having an electroless nickel phosphorus plating layer on its surface. The diameter of the polishing object (substrate to be polished) was 3.5 inches (a doughnut shape with an outer diameter of about 95 mm and an inner diameter of about 25 mm), the thickness was 1.75 mm, and the surface roughness Ra (the arithmetic mean roughness of the nickel phosphorus plating layer measured by a laser scanning surface roughness meter "TMS-3000WRC" manufactured by Schmitt Measurement System Inc.) before polishing was 130 Å.

[0066] (polishing conditions) Polishing equipment: System Seiko double-sided polishing machine, model "9.5B-5P" Polishing pad: FILWEL polyurethane pad, product name "CR200" Number of substrates to be polished: 15 (3 substrates / carrier x 5 carriers) Polishing fluid supply rate: 135mL / min Polishing load: 120g / cm 2 Upper platen rotation speed: 27 rpm Lower surface plate rotation speed: 36rpm Sun gear rotation speed: 8 rpm Amount polished: Total thickness of approximately 2.2 μm on both sides of each substrate The above removal amount was calculated based on the following formula. Polishing amount [μm] = weight loss of substrate due to polishing [g] / (substrate area [cm 2 ] × density of nickel phosphorus plating [g / cm 3 ])×10 4

[0067] [Workability] The polishing rate was calculated for both sides of a substrate to be polished under the above-mentioned polishing conditions using the polishing composition according to each example. The polishing rate was calculated based on the following formula. The results were converted into relative values, with the polishing rate of Comparative Example 1 taken as 100%, and shown in the "polishing rate" column of Table 1. The higher the polishing rate, the higher the processability. Polishing rate [μm / min] = weight loss of substrate due to polishing [g] / (substrate area [cm 2 ] × density of nickel phosphorus plating [g / cm 3 ] × polishing time [min]) × 10 4

[0068] [Micro waviness] After polishing using the polishing composition according to each example, one Ni-P substrate was randomly selected from the Ni-P substrates (substrates after polishing) set in each carrier during the polishing, for a total of three Ni-P substrates. Microwaviness was measured for the front and back surfaces of these three Ni-P substrates, a total of six surfaces, using a non-contact surface profiler "NEWVIEW5032" manufactured by ZYGO Corporation, under the conditions of an objective lens magnification of 2.5 times, an intermediate lens magnification of 0.5 times, and a bandpass filter of 80 to 500 μm. Measurements were performed for each of the six surfaces at four points spaced at 90° intervals at a position 37 mm radially outward from the center of the polished substrate, and the average value of these 24 points was taken as the microwaviness (Å) value. The obtained values ​​were converted into relative values ​​with the value of Comparative Example 1 taken as 100%, and are shown in the "microwaviness" column of Table 1. The smaller the value, the more the microwaviness is reduced.

[0069] The ratio of the polishing rate to the microwaviness was calculated, and the obtained value was converted into a relative value with the value of Comparative Example 1 taken as 100%, and shown in the "polishing rate / microwaviness ratio" column in Table 1. If the "polishing rate / microwaviness ratio" is 110% or more, it is determined that high processability has been achieved while suppressing the microwaviness to a predetermined level.

[0070] [Table 1]

[0071] As shown in Table 1, Examples 1 to 12, which used a polishing composition containing silica abrasive grains in which D1 is 20 nm or more and 70 nm or less, the average aspect ratio of the particle group having a particle diameter of D1 or less (D1 or less particle aspect ratio) is 1.10 to 1.50, and the ratio (D2 / D1) is 2.0 to 5.5 or less, were confirmed to be superior in polishing rate / microwaviness ratio compared to Comparative Examples 1 to 11. Specifically, in Examples 1 to 12, which used silica abrasive grains in which D1 is 20 to 70 nm and the D1 or less particle aspect ratio is 1.10 to 1.50, although D1 was 20 to 70 nm, the polishing rate was improved while suppressing microwaviness within a predetermined range compared to Comparative Example 1, which used silica abrasive grains in which the D1 or less particle aspect ratio is less than 1.10. On the other hand, in Comparative Example 2, in which silica abrasive grains with a particle aspect ratio of D1 or less than 1.10 but D1 exceeding 70 nm were used, the microwaviness increased with respect to the polishing rate. In Comparative Examples 3 to 5, in which D1 exceeds 70 nm and the particle aspect ratio of D1 or less is less than 1.10, a similar tendency, that is, a tendency that the microwaviness increases with respect to the polishing rate, was confirmed. The cause of this is thought to be that the secondary particles formed by the association of large-diameter primary particles are coarse, which may cause local pressure concentration and lead to an increase in microwaviness. In addition, in comparison with Comparative Examples 3 to 5, when the particle aspect ratio of D1 or less is 1.10 or more, the particle group containing such particles with a particle size of D1 or less (which may be in the form of primary particles or secondary particles) is suppressed from rolling during polishing due to its irregularity and surface state, and the processability in the horizontal direction with respect to the polished surface is improved, which is thought to improve the polishing rate. In Comparative Examples 6 to 9, in which D2 / D1 was greater than 5.5, a tendency that the polishing rate is lower was confirmed. The reasons for this are considered to be that the associated particles were broken during polishing, resulting in a loss of processing energy, and that associated particles having a certain aspect ratio rolled in the minor axis direction, resulting in no processing power being exerted. In Comparative Example 10, the degree of association (D2 / D1) was low, but the particle diameter was large, and the polishing rate was improved. However, the microwaviness was significantly worsened. In Comparative Example 10, the particle aspect ratio below D1 was within the range of 1.10 to 1.50, but as in the case of Comparative Example 2, this shows the importance of the D1 size for suppressing microwaviness.In Comparative Example 11, the microwaviness was reduced, but the processability was significantly reduced. This is believed to be because the particle aspect ratio of D1 or less was 1.00, the particle shape was spherical, and the degree of association (D2 / D1) was also small.

[0072] From the above results, it can be seen that a polishing composition containing silica particles as abrasive grains, acid, an oxidizing agent and water, in which the D1 of the silica particles is 20 nm or more and 70 nm or less, the average aspect ratio of a particle group having a particle diameter of D1 or less is 1.10 or more and 1.50 or less, and the ratio (D2 / D1) is 2.0 or more and 5.5 or less, can achieve high processability while suppressing microwaviness to a predetermined level in polishing of magnetic disk substrates.

[0073] Although specific examples of the present invention have been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and changes of the specific examples exemplified above.

Claims

1. A polishing composition for magnetic disk substrates, comprising: The abrasive includes silica particles, an acid, an oxidizing agent, and water. The silica particles are A particle diameter (D1) calculated from a specific surface area measured by a BET method is 20 nm or more and 70 nm or less, The volume-based average particle size (D2) measured by SEM image analysis is less than 180 nm; The average aspect ratio of the particle group having a particle diameter of D1 or less as determined by SEM image analysis is 1.10 to 1.50, and A polishing composition having a ratio of D2 to D1 (D2 / D1) of 2.0 or more and 5.5 or less.

2. A method for producing a magnetic disk substrate, comprising: a step (1) of polishing a substrate to be polished with the polishing composition according to claim 1.

3. 13. A method for polishing a substrate, comprising: a step (1) of supplying the polishing composition according to claim 1 to a substrate to be polished, and polishing the substrate.

Citation Information

Patent Citations

  • Polishing liquid composition for magnetic disk substrate

    JP2017102990A

  • Polishing composition, manufacturing method of substrate and polishing method

    JP2017179217A

  • Polishing liquid composition

    JP2019006935A

  • Silica slurry

    JP2019029044A

  • Polishing composition

    WO2014069043A1