Method for producing colloidal silica and colloidal silica

A method for producing colloidal silica without amine stabilizers ensures stability and purity by using specific hydrolysis catalysts and cation exchange, addressing contamination and odor issues, and enhancing polishing performance.

JP7588019B2Active Publication Date: 2024-11-21TAMA KAGAKU IND
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021055121
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-29
Publication Date
2024-11-21
Estimated Expiration
2041-03-29

AI Technical Summary

Technical Problem

Existing methods for producing colloidal silica involve post-treatments like acid treatment and ion exchange, leading to contamination and limitations in removing metal impurities, and the use of amine compounds as stabilizers can affect polishing rates and cause odor issues.

Method used

A method that produces colloidal silica without amine stabilizers by using a hydrolysis catalyst with quaternary ammoniums, amino alcohols, or morpholines, adjusting the zeta potential to 4 mV or more through cation exchange, and removing the hydrolysis catalyst to ensure stability and purity.

Benefits of technology

The method achieves stable colloidal silica with high polishing rates and low impurity content, suitable for industrial applications such as CMP and ceramic binders, without the drawbacks of amine compounds.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588019000004
    Figure 0007588019000004
  • Figure 0007588019000005
    Figure 0007588019000005
  • Figure 0007588019000006
    Figure 0007588019000006
Patent Text Reader

Abstract

To provide a method of producing colloidal silica good in dispersion stability without having an amine-based stabilizer, and particularly favorable for mechano-chemical polishing.SOLUTION: A method of producing colloidal silica excellent in dispersion stability having substantially no amine-based stabilizer comprises: reacting easily hydrolyzable organosilicate in the presence of a hydrolysis catalyst composed of a mixture of one or two or more selected from the group consisting of a quaternary ammoniums, amino alcohols, morpholines, and piperazines; thereafter removing alcohol generated from the easily hydrolyzable organosilicate; then obtaining a reaction concentration product stabilized in dispersion by an acid; and bringing the reaction concentration product into contact with a cation exchange resin to remove the hydrolysis catalyst, where the colloidal silica has an absolute value of zeta potential of 4 mV or higher.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing colloidal silica suitable for various applications, such as mirror polishing of silicon wafers in the manufacturing process of semiconductor devices, binders to be mixed with organic solvents in hard coating agent applications such as titanium oxide photocatalysts, binders used in ceramic applications such as ceramic furnace materials and ceramic fibers, chromate-based metal surface treatment agents, and ground improvement grouting agents. [Background technology]

[0002] As methods for industrially producing high-purity colloidal silica, a method of ion-exchanging an aqueous sodium silicate solution, a method of thermally decomposing silicon tetrachloride, a method of hydrolyzing an organosilicate in a water-alcohol mixed solvent in the presence of an acid catalyst or an alkali catalyst, and the like have been proposed and put into practice. However, the method of hydrolyzing an organosilicate allows the use of high-purity organosilicates, catalysts, solvents, etc., for the reaction, and therefore the amount of impurities derived from these raw materials, etc. is extremely small, and is therefore suitable as a method for producing high-purity colloidal silica with a particularly small content of metal impurities, and several methods for the hydrolysis of organosilicates have been proposed so far.

[0003] Regarding colloidal silica used for various applications, particularly colloidal silica used in the field of polishing agents for semiconductor wafers, various types of metal wiring, oxide films, and the like are present on a single wafer with the increasing integration density of today's LSIs, and each semiconductor wafer requires its own appropriate polishing performance, resulting in a demand for colloidal silica with various slightly different compositions and properties.

[0004] Furthermore, for colloidal silica used in applications where even slight alkali metal impurities should not be contained, such as binders for hard coating agents and ceramics, chromate-based metal surface treatment agents, and ground improvement grout, acidic colloidal silica is required, and several proposals for methods for producing such acidic colloidal silica are known.

[0005] For example, Patent Document 1 discloses a method for producing an acidic silica sol by first preparing an alkaline silica sol containing an aluminum compound, and then treating this aluminum compound-containing alkaline silica sol with a cation exchange resin to remove the alkali, and Patent Document 2 discloses a method for producing a stable acidic silica sol having a pH of 2 to 5 and a particle size of 4 to 30 by adding an aqueous alkali aluminate solution to a silica sol having a particle size of 4 to 30 and a pH of 2 to 9 so that the Al2O3 / SiO2 molar ratio is 0.0006 to 0.004, and then contacting the silica sol with an ion exchange resin.

[0006] Furthermore, Patent Document 3 discloses a method for producing high-purity modified colloidal silica with an extremely low metal impurity content, which is produced by modifying colloidal silica obtained by hydrolyzing and condensing a hydrolyzable silicon compound with a modifying agent such as a silane coupling agent, and which does not cause aggregation or gelation even in an acidic dispersion medium, can be stably dispersed for a long period of time, and has an extremely low metal impurity content.

[0007] However, in the methods described in Patent Documents 1 and 2, it is necessary to prepare an aluminum compound-containing alkaline silica sol first, and then to treat it with an ion exchange resin to dealkalize it, which increases the production cost and also poses problems such as contamination by the ion exchange resin itself and limitations in ion removal during ion exchange. In addition, in the method described in Patent Document 3, the surface of the obtained colloidal silica is modified with a modifying agent, which may make it unsuitable for the desired application, and also poses problems such as contamination from the modifying agent.

[0008] In order to solve such problems, the present inventors have investigated a method for easily producing colloidal silica having predetermined properties, such as spherical colloidal silica, which does not require special post-treatment such as acid treatment, ion exchange treatment, or further modification treatment, has an extremely low content of metal impurities including alkali metals, and has an average particle size in the range of 5 to 500 nm, a standard deviation of 20 or less, and a polydispersity index of 0.15 or less, as determined by particle size distribution analysis using an electron microscope, for example. As a result, they have proposed that neutral colloidal silica with a pH of 5 to 8 can be easily produced without special post-treatment such as acid treatment or ion exchange treatment by using an easily hydrolyzable organosilicate with a high hydrolysis rate and a specific hydrolysis catalyst as a hydrolysis catalyst, and adding and reacting this hydrolysis catalyst so that at least the ratio of the hydrolysis catalyst (A) to the silica (B) in the reaction mixture at the end of the reaction {catalyst remaining molar ratio (A / B)} is a predetermined value or less (Patent Document 4).

[0009] Incidentally, as in the method described in Patent Document 4, it has been known that amine-based compounds such as hydrolysis catalysts contained in colloidal silica dispersions (hereinafter, these may be referred to as "amine-based stabilizers" or the like) contribute partially to the dispersibility and stability of colloidal silica (see, for example, Patent Document 5 and Non-Patent Document 1), and there has been concern that the dispersibility of colloidal silica may become unstable or that aggregation or gelation may occur if such amine-based compounds are not contained. On the other hand, such amine-based compounds are generally used as polishing accelerators for silicon wafers (see, for example, Non-Patent Document 2), and are known to affect the polishing rate and etching rate depending on the type and application, and in some cases, there is concern that they may cause unnecessary polishing rate or deterioration of the surface condition due to etching. In addition, when colloidal silica is used as a binder for ceramic applications, there has been concern that the inclusion of amine-based compounds may cause unpleasant amine odors and blackening due to residual carbon during and after drying and firing.

[0010] Thus, although it is believed that the amine-based compound such as a hydrolysis catalyst used (residual) in the production of a colloidal silica dispersion contributes to a certain extent to the stability of the dispersion, it has been found that there are cases in which it is desirable to exclude such a compound depending on the application, etc. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] Special Publication No. 4-55126 [Patent Document 2] Japanese Patent Application Publication No. 6-199515 [Patent Document 3] JP 2005-162533 A [Patent Document 4] JP 2007-153732 A [Patent Document 5] Japanese Patent Application Publication No. 08-302394 [Non-patent literature]

[0012] [Non-Patent Document 1] Masahiro Izumi and Shinsuke Miyabe, "Introduction of silica products under development", Nippon Chemical Industry Co., Ltd. Technical Report (CREATIVE) No. 8, p62-71 (2007) [Non-Patent Document 2] Shuhei Matsuda et al., Nitta Haas Corporation, "Relationship between Alkali Species in Slurry and Polishing Performance in Silicon Wafer Polishing", 170th Workshop of the Japan Society of Precision Engineering, Planarization CMP and Its Application Technology Special Committee (2018 / 12 / 21) Summary of the Invention [Problem to be solved by the invention]

[0013] Therefore, the present inventors conducted extensive research into a method for producing a colloidal silica dispersion that does not impair dispersion stability and does not cause aggregation or gelation even when an amine compound (amine stabilizer) such as a hydrolysis catalyst that has been conventionally used (remained) is removed, and as a result, they discovered that the above-mentioned problems can be solved by contacting a dispersion-stabilized reaction product (reaction concentrate) with a cation exchange resin and optimizing the zeta potential of the reaction concentrate after contact with the cation exchange resin within a certain range, thereby completing the present invention.

[0014] Therefore, an object of the present invention is to provide a method for producing colloidal silica which has good dispersion stability and is free from aggregation and gelation even if it is substantially free of an amine compound (amine stabilizer), and which can be suitably applied to, for example, an abrasive for chemical mechanical polishing (CMP) or a binder for ceramic applications. [Means for solving the problem]

[0015] That is, the present invention provides a method for producing colloidal silica having excellent dispersion stability substantially free of an amine-based stabilizer, comprising the steps of: This method for producing colloidal silica is characterized by reacting an easily hydrolyzable organosilicate in the presence of a hydrolysis catalyst consisting of one or a mixture of two or more selected from quaternary ammoniums, aminoalcohols, morpholines, and piperazines, removing the alcohol produced from the easily hydrolyzable organosilicate, and then obtaining a reaction concentrate that has been dispersed and stabilized with an acid. The reaction concentrate is then contacted with a cation exchange resin to remove the hydrolysis catalyst, thereby producing colloidal silica having an absolute value of a zeta potential of 4 millivolts (mV) or more. Effect of the Invention

[0016] According to the method for producing colloidal silica of the present invention, it is possible to produce colloidal silica that has good dispersion stability even without containing an amine-based stabilizer and can therefore be suitably used, for example, as an abrasive for CMP, a binder for ceramics, and the like.

[0017] Furthermore, according to the method for producing colloidal silica of the present invention, it is possible to obtain colloidal silica which has a large BET specific surface area for its large SEM average particle diameter, a high particle density (true specific gravity), and an excellent removal rate, making it suitable as a polishing agent for CMP, and which is substantially free of amine compounds. [Brief description of the drawings]

[0018] [Figure 1] FIG. 1 shows an SEM photograph (300,000 times magnification) of the reaction concentrate (colloidal silica) before contact with the cation exchange resin in Example 1. [Diagram 2] FIG. 2 shows an SEM photograph (300,000 times magnification) of the colloidal silica after contact with the cation exchange resin in Example 1. [Diagram 3] FIG. 3 shows an SEM photograph (300,000 times magnification) of the reaction concentrate (colloidal silica) before contact with the cation exchange resin in Example 2. [Figure 4] FIG. 4 shows an SEM photograph (300,000 times magnification) of the colloidal silica after contact with the cation exchange resin in Example 2. [Diagram 5] FIG. 5 shows an SEM photograph (300,000 times magnification) of the reaction concentrate (colloidal silica) before contact with the cation exchange resin in Example 3. [Figure 6] FIG. 6 shows an SEM photograph (300,000 times magnification) of the colloidal silica after contact with the cation exchange resin in Example 3. [Figure 7] FIG. 7 shows an SEM photograph (300,000 times magnification) of the reaction concentrate (colloidal silica) before contact with the cation exchange resin in Example 4. [Figure 8]FIG. 8 shows an SEM photograph (300,000 times magnification) of the colloidal silica after contact with the cation exchange resin in Example 4. [Figure 9] Figure 9 is a general schematic diagram for understanding the relative mass [50%] particle size. In this figure, the vertical axis indicates the relative mass [50%] and the horizontal axis indicates the particle size [μm]. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] As described above, the gist of the production method of the present invention is characterized in that an easily hydrolyzable organosilicate is reacted in the presence of a specific hydrolysis catalyst, an alcohol produced from the easily hydrolyzable organosilicate is removed, and then a reaction concentrate is obtained that has been dispersed and stabilized with an acid. The reaction concentrate is then brought into contact with a cation exchange resin to remove the hydrolysis catalyst, thereby producing a dispersion of colloidal silica having an absolute value of a zeta potential of 4 mV or more.

[0020] First, the organosilicate used in the present invention is an easily hydrolyzable organosilicate with a fast hydrolysis rate, and the easily hydrolyzable organosilicate refers to an organosilicate in which 10 g of the organosilicate and 100 g of pure water containing 0.1 ppb or less of impurities are hydrolyzed under stirring at 25° C. and the hydrolysis reaction is completed within 1 hour. Specific examples of such easily hydrolyzable organosilicate include trimethyl silicate (hydrolysis reaction time until hydrolysis reaction is completed: 3 minutes), tetramethyl silicate (hydrolysis reaction time: 5 minutes), triethyl silicate (hydrolysis reaction time: 5 minutes), and methyl trimethyl silicate (hydrolysis reaction time: 7 minutes). Tetraethyl silicate and organosilicates with a larger number of carbon atoms than tetraethyl silicate have a slow hydrolysis rate and are prone to gelation (hydrolysis reaction time: 24 hours or more for both), and are therefore not suitable as organosilicates for use in the method of the present invention.

[0021] In the present invention, examples of the quaternary ammoniums used as hydrolysis catalysts include quaternary ammoniums such as tetramethylammonium hydroxide (TMAH), tetraethylammonium hydroxide (TEAH), trimethylethylammonium hydroxide, trimethylethanolammonium hydroxide (choline), triethylethanolammonium hydroxide, tetrapropylammonium hydroxide, and butylammonium hydroxide, as well as carbonates, bicarbonates, and silicates thereof. Since a relatively high pH is desirable for the hydrolysis reaction, tetramethylammonium hydroxide (TMAH), choline, or tetraethylammonium hydroxide (TEAH) is preferred.

[0022] As for the amino alcohols used as the hydrolysis catalyst, various amino alcohols including ethanolamine derivatives can be used, with ethanolamine derivatives being preferred. Examples of such amino alcohols include monoethanolamine, diethanolamine, triethanolamine, N,N-dimethylethanolamine, N,N-diethylethanolamine, N,N-di-n-butylethanolamine, N-(β-aminoethyl)ethanolamine, N-methylethanolamine, N-methyldiethanolamine, N-ethylethanolamine, Nn-butylethanolamine, Nn-butyldiethanolamine, N-tert-butylethanolamine, and N-tert-butyldiethanolamine.

[0023] Furthermore, for the morpholines used as the hydrolysis catalyst, various morpholine derivatives can be used, with preferred examples including morpholine, N-methylmorpholine, N-ethylmorpholine, etc. Furthermore, for the piperazines used as the hydrolysis catalyst, various piperazine derivatives can be used, with preferred examples including piperazine, hydroxyethylpiperazine, etc.

[0024] The quaternary ammoniums, amino alcohols, morpholines and piperazines used as the hydrolysis catalysts can be used alone or as a mixture of two or more of them if necessary. Note that, amines such as ammonia, primary amines such as monomethylamine, secondary amines such as dimethylamine, and tertiary amines such as trimethylamine, which have been conventionally used in this type of hydrolysis reaction, are highly volatile, and when the hydrolysis reaction is carried out at a temperature of 40°C or higher, the composition in the reaction system is likely to change, making it difficult to produce colloidal silica having the desired particle size, and therefore are generally not suitable as hydrolysis catalysts.

[0025] In the present invention, in the mixture obtained after the reaction of the easily hydrolyzable organosilicate with the hydrolysis catalyst (hereinafter, this may be referred to as the "reaction mixture"), or in the reaction mixture after the treatment of removing alcohol or stabilizing dispersion with an acid as described below (hereinafter, this may be particularly referred to as the "reaction concentrate"), it is preferable to add the hydrolysis catalyst to the reaction system so that the ratio of the hydrolysis catalyst (A) to the silica (B) {catalyst remaining molar ratio (A / B)} is 0.012 or less, more preferably in the range of 0.00035 to 0.012, and even more preferably in the range of 0.0035 to 0.011, to carry out the hydrolysis reaction. This is preferable because the pH of the reaction mixture or reaction concentrate can be optimized and thickening and gelation can be suppressed. The method for achieving such a catalyst remaining molar ratio is not particularly limited, and examples thereof include a method of continuously or intermittently introducing an organosilicate calculated so that the final catalyst remaining molar ratio (A / B) falls within the above-mentioned range into a reaction vessel charged with water and the hydrolysis catalyst (A); a method of continuously or intermittently introducing a hydrolysis catalyst and an organosilicate calculated so that the final catalyst remaining molar ratio falls within the above-mentioned range into a reaction vessel charged with only water; and a method of continuously or intermittently introducing a hydrolysis catalyst and an organosilicate calculated so that the final catalyst remaining molar ratio falls within the above-mentioned range into a reaction vessel charged with water and a small amount of the hydrolysis catalyst (A).

[0026] Alternatively, prior to the hydrolysis reaction of the organosilicate, colloidal silica seeds having particle growth properties may be charged into the reaction system for the hydrolysis reaction, and the organosilicate and hydrolysis catalyst may be gradually added to the reaction system so that the catalyst remaining molar ratio (A / B) falls within the above-mentioned range. This is preferable because it makes it possible to produce colloidal silica having uniform particles.

[0027] Furthermore, in the present invention, the organosilicate, hydrolysis catalyst and water used as raw materials for the hydrolysis reaction are preferably high-purity ones having a metal impurity content of 1 ppm or less, preferably 0.01 ppm or less, whereby a dispersion of high-purity colloidal silica with a low metal impurity content can be easily produced.

[0028] Here, in the present invention, after the reaction between the easily hydrolyzable organosilicate and the hydrolysis catalyst, it is preferable to remove the alcohol generated from the hydrolyzable organosilicate. The method of such alcohol removal treatment is not particularly limited, but for example, a method of distilling alcohol by heating using an apparatus equipped with a distillation tube with a condenser can be mentioned. By carrying out such alcohol removal treatment, it is not necessary to consider the alcohol resistance of the material used in the subsequent process, and since the highly volatile alcohol is eliminated, it is preferable in terms of stabilizing the concentration of colloidal silica, etc.

[0029] Next, it is preferable to stabilize the reaction mixture after the alcohol removal treatment by using an acid. As the dispersion stabilization treatment, a carbon dioxide gas blowing method in which carbon dioxide gas is blown in or an acid solution adding method in which an acid solution is added under stirring is performed. Either the carbon dioxide gas blowing method or the acid solution adding method may be performed, or these methods may be used in combination. In any case, during the dispersion stabilization treatment, it is necessary to maintain the reaction mixture in a stirred state by operations such as bubbling with carbon dioxide gas or stirring.

[0030] When the dispersion stabilization treatment is carried out by a carbon dioxide gas injection method, the carbon dioxide gas injected into the reaction mixture may be 100% by volume carbon dioxide gas, or may be inert gas-diluted carbon dioxide gas diluted to about 0.1% by volume with an inert gas such as nitrogen gas, or may even be air, but is preferably 100% by volume carbon dioxide gas or 1% by volume or more of inert gas-diluted carbon dioxide gas.

[0031] As for the treatment conditions in this carbon dioxide gas injection method, since the injection of carbon dioxide gas itself has a stirring effect, it is appropriate to introduce carbon dioxide gas into the reaction mixture under stirring usually at a speed of 0 rpm or more and 3000 rpm or less, preferably 0 rpm or more and 1000 rpm or less, at a temperature higher than 0°C and less than 100°C, preferably higher than 5°C and lower than 80°C, at a rate preferably exceeding 0 mL / min and not exceeding 100,000 mL / min, more preferably higher than 1 mL / min and not exceeding 10,000 mL / min.

[0032] Furthermore, when the dispersion stabilization treatment is carried out by the acid solution addition method, the acid solution used is preferably an acid aqueous solution having a concentration of 20% by weight or less, and is a mixture of one or more types selected from an aqueous carbonic acid solution, a dilute mineral acid aqueous solution having a concentration of 20% by weight or less, and a dilute organic acid aqueous solution having a concentration of 20% by weight or less, and is preferably a mixture of one or more types selected from a dilute mineral acid aqueous solution having a concentration of 10% by weight or less and a dilute organic acid aqueous solution having a concentration of 10% by weight or less. Specifically, examples of the acid include inorganic acids such as hydrochloric acid, sulfuric acid, nitric acid, hydrofluoric acid, boric acid, carbonic acid, hypophosphorous acid, phosphorous acid, and phosphoric acid, and organic acids such as formic acid, acetic acid, propionic acid, butyric acid, valeric acid, 2-methylbutyric acid, n-hexanoic acid, 3,3-dimethylbutyric acid, 2-ethylbutyric acid, 4-methylpentanoic acid, n-heptanoic acid, 2-methylhexanoic acid, n-octanoic acid, 2-ethylhexanoic acid, benzoic acid, glycolic acid, salicylic acid, glyceric acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, maleic acid, phthalic acid, malic acid, tartaric acid, citric acid, lactic acid, diglycolic acid, 2-furan carboxylic acid, 2,5-furandicarboxylic acid, 3-furan carboxylic acid, 2-tetrahydrofuran carboxylic acid, methoxyacetic acid, methoxyphenylacetic acid, phenoxyacetic acid, methanesulfonic acid, ethanesulfonic acid, and isethionic acid, and are appropriately selected depending on the application.

[0033] The treatment conditions for this aqueous acid solution addition method are as follows: stirring is usually at 1 rpm or more and 3000 rpm or less, and preferably 10 rpm or more and 1000 rpm or less, at a temperature usually at 0°C or more and 100°C or less, and preferably 5°C or more and 80°C or less, and the acid solution is added in an amount of usually 0.0001 mol or more and 10 mol or less, and preferably 0.001 mol or more and 1 mol or less, relative to 1 mol of catalyst in the reaction mixture to be treated.

[0034] The reaction mixture (reaction concentrate) that has been subjected to the dispersion stabilization treatment by the method of the present invention has a silica concentration of 10% by weight or more and 40% by weight or less and a pH value of 6.0 to 8.1 or less, and can almost maintain the pH value before the dispersion stabilization treatment. In addition, excellent dispersion stability is exhibited usually for more than one week, and even for several years, and two-layer separation does not occur.

[0035] Conventionally, the reaction mixture (reaction concentrate) obtained up to this stage is used as a dispersion of colloidal silica, and the obtained colloidal silica has a number of irregular small protrusions on its particle surface as can be seen from the drawings described later, and has a shape like a confetti candy as a whole particle. The SEM average particle diameter measured by measuring the arithmetic mean of particle images observed by SEM is large, but the BET specific surface area is large, and the particle density (true specific gravity) measured by the liquid phase displacement method is high, in other words, the hardness is high. It has an excellent polishing rate and is suitable for a polishing agent for CMP. For example, in the case of colloidal silica used in the field of abrasives for semiconductor wafers, the average particle diameter measured by particle size distribution analysis using an electron microscope is preferably in the range of 5 to 500 nm, more preferably 5 to 300 nm. The shape of colloidal silica particles can be controlled to be monodisperse spherical (spherical product) or to have a shape in which particles are bonded and associated (associated product) depending on the charging composition, etc. For example, by adding a larger amount of catalyst and a silica raw material organosilicate to the reaction field relatively slowly, the organosilicate is hydrolyzed quickly and uniformly and grows mildly, so that the seed particles gradually grow while maintaining their spherical shape, and a spherical product can be obtained. Also, by adding a smaller amount of catalyst and a silica raw material organosilicate to the reaction field relatively quickly, the organosilicate is hydrolyzed non-uniformly, so that it acts like an adhesive between particles, and as a result, an associated product in which the particles are associated can be obtained.

[0036] The present invention is characterized in that the reaction concentrate obtained above is brought into contact (passed through) with a cation exchange resin in order to remove the remaining amine compound (amine stabilizer) which is a hydrolysis catalyst. It is desirable that the characteristics (particularly, dispersion stability) of the reaction concentrate (colloidal silica) before the contact are generally maintained even after such contact with the cation exchange resin, and for this purpose, it has been found that it is important to keep the zeta potential of the colloidal silica dispersion, which is the reaction concentrate, within a specific range even after the contact (passed through). Specifically, it is desirable that the absolute value of the zeta potential of the colloidal silica dispersion (usually having a silica concentration of 10% by weight or more and 40% by weight or more) after contact (liquid passing) is 4 mV or more, preferably 5 mV or more. A larger absolute value of the zeta potential is preferable because the colloidal silica dispersion becomes more stable. By having such a zeta potential, even if the hydrolysis catalyst, which is an amine-based stabilizer, is removed by cation exchange, the colloidal silica dispersion is stable and the occurrence of aggregation is suppressed, and the occurrence of problems such as clogging of the liquid during contact (liquid passing) with the cation exchange, excessive time required for liquid passing, increase in particle size after liquid passing, or gelation can be suppressed as much as possible.

[0037] The type of cation exchange resin used here is not particularly limited as long as it is an H-type cation exchange resin, and from the viewpoints of high purity, long-term stability, and the possibility of repeated regeneration, it is preferable to use a highly crosslinked porous cation exchange resin as a suitable type. As a form of use, a method of passing a liquid through a cation exchange resin packed in a column as is commonly used can be adopted.

[0038] As for the liquid passing conditions, the temperature condition is preferably 0° C. to 30° C., and more preferably 5° C. to 25° C. If the temperature is below 0° C., there is a risk of freezing and making it difficult to pass the liquid through, while if the temperature is above 30° C., the colloidal silica becomes unstable during ion exchange, and may aggregate, making it impossible to pass the liquid through.

[0039] The flow rate is preferably set so that the reaction concentrate (colloidal silica) comes into sufficient contact with the ion exchange resin while passing through the ion exchange resin layer, and generally used conditions can be appropriately adopted as long as the conditions are within a range in which gelation of colloidal silica does not occur. The flow rate is preferably set so that, when the amount of colloidal silica flowing per hour relative to the resin volume is SV, the SV is in the range of 5 to 70, and more preferably, the SV is in the range of 15 to 40. The amount of reaction concentrate (colloidal silica) treated is preferably set so that, when the amount of reaction concentrate (colloidal silica) dropped relative to the resin volume is BV, the BV is preferably up to 50, and more preferably up to 40.

[0040] During the passage, the viscosity of the colloidal silica, which is the reaction concentrate, is preferably 1 to 100 mPa·s, and more preferably 1 to 20 mPa·s. In this case, the BET particle size (nm) of the colloidal silica is preferably 10 nm to 500 nm, more preferably 18 nm to 200 nm. By using colloidal silica having such a BET particle size, the colloidal silica does not gel in the ion exchange resin and can be produced without remaining in the resin, which is preferable. The BET particle size can be determined by the method described later.

[0041] In the colloidal silica dispersion obtained after contact with the cation exchange (liquid passing), the hydrolysis catalyst (amine-based stabilizer) is removed and is not substantially contained, but preferably the amount of the remaining hydrolysis catalyst (amine-based stabilizer) is 100 ppm or less, more preferably 50 ppm or less. In this case, the absolute value of the zeta potential needs to be 4 mV or more as described above, and by doing so, a colloidal silica dispersion with stable dispersion can be obtained, but preferably the storage temperature is 0°C to 30°C, more preferably 5°C to 25°C, as in the above-mentioned liquid passing conditions.

[0042] In addition, when contacting (passing) with such a cation exchange resin, the pH of the reaction concentrate or the colloidal silica dispersion after cation exchange may be adjusted in advance by adding an acid or ammonia before or after the contact. Specifically, the following methods can be mentioned.

[0043] That is, in the reaction concentrate before cation exchange, carbon dioxide gas injection or acid solution addition is performed as the dispersion stabilization treatment as described above. Among these, carbon dioxide gas injection is preferable because impurities other than colloidal silica after ion exchange are carbon dioxide or carbonate ions, and the material with which the colloidal silica comes into contact in the use is relatively less affected. However, since the pH of the liquid is usually about 4 to 9 when carbon dioxide gas is injected, if cation exchange is performed on this, the pH becomes about 4 to 7, and the absolute value of the zeta potential becomes small, so the dispersibility of the colloidal silica becomes unstable and aggregation and gelation are likely to occur. Therefore, it is preferable to add an acid or ammonia to perform dispersion stabilization even after cation exchange. As the acid after cation exchange, the acid used in the acid solution addition as the dispersion stabilization treatment described above can be used. In particular, by performing such stabilization treatment after ion exchange, a colloidal silica dispersion liquid that is stable for more than one year at 0 to 50°C, preferably 5 to 40°C, can be obtained. The dispersion stability can be confirmed by visually checking whether aggregation or gelation occurs, or by checking the change in particle size distribution. As shown in the figure below, the occurrence of aggregation can be confirmed by measuring the particle diameter (unit: μm, nm, etc.) of the high particle diameter shoulder of the particle diameter distribution, which is the relative mass [50%], and checking the change (increase) in the particle diameter before and after ion exchange. In the present invention, the change in particle diameter at the relative mass [50%] thus obtained is preferably 0.2 nm or less (including cases where the change is a negative value), and more preferably 0.1 nm or less. The lower limit of the change in the particle diameter is not limited, but it is usually -1.0 nm or more. The reason why the change is a negative value is not necessarily clear, but it is presumed to be because some of the relatively large particles that pushed up the particle diameter value before ion exchange were captured by the ion exchange resin.

[0044] On the other hand, when the dispersion stabilization treatment before cation exchange is the addition of an acid solution, for example, if a relatively strong acid such as citric acid is added before ion exchange, a strong acid such as citric acid remains as an impurity other than colloidal silica after ion exchange, so that even if the solution is made alkaline, the strong acid ions remain, and there is a concern that the influence on the material with which the colloidal silica comes into contact in the intended use is relatively large. However, when an acid solution such as citric acid is added before cation exchange, the pH of the liquid is usually less than 4, so even after cation exchange is performed, the pH is less than 4 without a separate stabilization operation, the absolute value of the zeta potential is large, and the dispersibility is stable. It is not necessary to add a stabilizer such as acid or ammonia after passing the liquid, which is preferable in that a process can be omitted.

[0045] In the present invention, such cation exchange is newly introduced into the colloidal silica production process to actively remove the amine-based stabilizer, which is a remaining hydrolysis catalyst, and the zeta potential of the resulting colloidal silica dispersion is adjusted to fall within a predetermined range, thereby making it possible to obtain a colloidal silica dispersion that is substantially free of amine-based stabilizers, preferably having a concentration of 100 ppm or less, and further, as described above, it has been confirmed that there is almost no change in properties such as dispersion stability before and after ion exchange. Therefore, according to the method of the present invention, it is possible to obtain a dispersion of colloidal silica that is substantially free of amine-based stabilizers while maintaining the physical properties (protrusions, particle size, etc.) suitable for use as an abrasive for semiconductor wafers as described above. The obtained colloidal silica may be a monodisperse spherical product as described above, or may be an association product (cocoon-shaped, chain-like, branched) having a shape that appears to be formed by a plurality of particles coalescing two-dimensionally or three-dimensionally when observed under an electron microscope. EXAMPLES

[0046] Hereinafter, preferred embodiments of the present invention will be described in detail based on examples and comparative examples. [Example 1] In a 5-liter (L) glass vessel equipped with a stirrer, a thermometer, a distillation tube with a condenser, and an organosilicate inlet tube, 3368 g of pure water with a metal impurity content of 0.1 ppb or less and 3.60 g of triethanolamine (bp: 361°C) with a metal impurity content of 10 ppb or less were charged, and while keeping the liquid temperature in the reaction vessel at 70°C using a mantle heater, 1470 g of tetramethyl silicate (manufactured by Tama Chemicals Co., Ltd.) with a metal impurity content of 10 ppb or less was continuously fed with stirring over a period of 3 hours. The feeding of tetramethyl silicate into the reaction vessel was then completed. The obtained colloidal silica having a silica concentration of 12.6% by weight was charged into the reaction vessel, followed by 1,108 g of pure water having a metal impurity content of 0.1 ppb or less, and 8.00 g of triethanolamine having a metal impurity content of 10 ppb or less. While maintaining the liquid temperature in the reaction vessel at 80°C using a mantle heater, 1,111 g of tetramethyl silicate having a metal impurity content of 10 ppb or less (manufactured by Tama Chemicals Co., Ltd.) was continuously fed into the reaction vessel with stirring over a period of 3 hours. After the supply of tetramethylsilicate to the reaction vessel was stopped, the temperature in the reaction vessel was lowered to 40°C, the pressure in the system was reduced by a vacuum pump, and then heating was resumed. The reaction mixture in the reaction vessel was further heated to 52-68°C, and the methanol produced was distilled from the distillation tube with a condenser at a distillation temperature of 32-67°C. 833g of pure water was further added while distilling off water and methanol, and the reaction mixture (colloidal silica) produced in the reaction vessel was concentrated to 2850g. Carbon dioxide gas was blown in at 40mL / min for 16 minutes while stirring the reaction concentrate at 55rpm, and dispersion stabilization treatment was performed. After that, it was confirmed by SEM observation that the particles were spherical particles with protrusions with a particle diameter of 30nm as shown in Figure 1.

[0047] Next, 2,200 g of the obtained reaction concentrate (colloidal silica) was passed through an ion exchange column packed with 50 mL of cation exchange resin (PK228L manufactured by Mitsubishi Chemical Corporation) at a flow rate of 18.6 g / min while maintaining the liquid temperature at 15°C to 20°C, to remove triethanolamine, an alkaline stabilizer used in the reaction. After the cation exchange, the colloidal silica was diluted with pure water to a concentration of 20.20-20.40%, and then an aqueous ammonia solution (28% special grade) was added to make the ammonia concentration 120 ppm. The colloidal silica was then stirred at 55 rpm while carbon dioxide gas was blown in at 40 mL / min for 2 minutes to perform a dispersion stabilization treatment. Various analyses were performed on the stabilized product, and the results are shown in Tables 1-3. In addition, by observing with an SEM as shown in Figure 2, it was confirmed that the shape of the particles did not change before and after the ion exchange.

[0048] [Example 2] In a 5-liter (L) glass vessel equipped with a stirrer, a thermometer, a distillation tube with a condenser, and an organosilicate inlet tube, 3233 g of pure water with a metal impurity content of 0.1 ppb or less and 3.46 g of triethanolamine (bp: 361°C) with a metal impurity content of 10 ppb or less were charged, and while keeping the liquid temperature in the reaction vessel at 70°C using a mantle heater, 1411 g of tetramethyl silicate (manufactured by Tama Chemicals Co., Ltd.) with a metal impurity content of 10 ppb or less was continuously fed with stirring over a period of 3 hours. The feeding of tetramethyl silicate into the reaction vessel was then completed. 457 g of the obtained colloidal silica having a silica concentration of 12.6% by weight, 2916 g of pure water having a metal impurity content of 0.1 ppb or less, and 8.12 g of triethanolamine having a metal impurity content of 10 ppb or less were charged, and while maintaining the liquid temperature in the reaction vessel at 80°C using a mantle heater, 1264 g of tetramethyl silicate having a metal impurity content of 10 ppb or less (manufactured by Tama Chemicals Co., Ltd.) was continuously fed with stirring over a period of 3 hours. After the supply of tetramethylsilicate to the reaction vessel was stopped, the temperature in the reaction vessel was lowered to 40°C, the pressure in the system was reduced by a vacuum pump, and then heating was resumed. The reaction mixture in the reaction vessel was further heated to 52-68°C, and the generated methanol was distilled from the distillation tube with a condenser at a distillation temperature of 32-67°C. 833g of pure water was further added while distilling off water and methanol, and the reaction mixture (colloidal silica) generated in the reaction vessel was concentrated to 2850g. While stirring the reaction mixture at 55 rpm, carbon dioxide gas was blown in at 40mL / min for 16 minutes to perform a dispersion stabilization treatment, and it was confirmed by SEM observation that the particles were spherical with protrusions with a particle diameter of 50nm as shown in Figure 3. 2200 g of the resulting reaction concentrate (colloidal silica) was subjected to ion exchange treatment, ammonia stabilization, and dispersion stabilization in the same manner as in Example 1. The stabilized product was subjected to various analyses, and the results are shown in the table. In addition, by observing with an SEM as shown in Figure 4, it was confirmed that the shape of the particles did not change before and after ion exchange.

[0049] [Example 3] In a 5L glass reaction vessel equipped with a stirrer, a thermometer, a distillation tube with a condenser, and an organosilicate inlet tube, 3457g of pure water with a metal impurity content of 0.1ppb or less and 7.51g of a 25wt%-TMAH aqueous solution with a metal impurity content of 10ppb or less were charged, and while keeping the liquid temperature in the reaction vessel at 70°C using a mantle heater, 1134g of tetramethylsilicate (manufactured by Tama Chemicals Co., Ltd.) with a metal impurity content of 10ppb or less was continuously fed under stirring over 1.87 hours. In addition, 10 minutes after the completion of the feeding of tetramethylsilicate, 8.372g of 100% triethanolamine was added as an alkali stabilizer. The obtained colloidal silica was an association-type colloidal silica having a silica concentration of 10.18% by weight, a transmittance of 97.2%, a secondary particle diameter (DLS diameter) measured by dynamic light scattering method of 30.9 nm, a particle diameter converted into specific surface area (BET diameter) of 11.0 nm, and a degree of association (an index showing how many single spherical particles are connected: DLS diameter / BET diameter) of 2.80. In the same reaction vessel as the above reaction, 1097g of colloidal silica obtained in the above reaction, 2358g of pure water with a metal impurity content of 0.1 ppb or less, and 29.87g of a 25wt%-TMAH aqueous solution with a metal impurity content of 10 ppb or less were charged, and while maintaining the liquid temperature in the reaction vessel at 80°C using a mantle heater, 1115g of tetramethyl silicate (manufactured by Tama Chemicals Co., Ltd.) with a metal impurity content of 10 ppb or less was continuously fed under stirring for 6 hours. In addition, 10 minutes after the completion of the feeding of tetramethyl silicate, 6.375g of 100% triethanolamine was added as an alkali stabilizer. After the addition, the reaction mixture was cooled with water until the liquid temperature was 40°C or less. After cooling with water, the pressure in the reaction vessel was reduced to 0.03 MPa, and the reaction mixture was further heated to 50°C to 70°C to distill the produced methanol together with water from a distillation tube equipped with a condenser at a distillation temperature of 50°C to 70°C. The reaction mixture (colloidal silica) produced in this reaction vessel was concentrated to 2300 g. Next, this reaction mixture was stirred at 55 rpm and carbon dioxide gas was blown in at 40 mL / min for 13 minutes to perform a dispersion stabilization treatment. After that, SEM observation confirmed that the particles were associated particles with few protrusions and a minor axis of 30 nm, as shown in Figure 5. 2200 g of the resulting reaction concentrate (colloidal silica) was subjected to ion exchange treatment, ammonia stabilization, and dispersion stabilization in the same manner as in Example 1. The stabilized product was subjected to various analyses, and the results are shown in the table. In addition, by observing with an SEM as shown in Figure 6, it was confirmed that the shape of the particles did not change before and after ion exchange.

[0050] [Example 4] In a 5-liter (L) glass vessel equipped with a stirrer, a thermometer, a distillation tube with a condenser, and an organosilicate inlet tube, 3233 g of pure water with a metal impurity content of 0.1 ppb or less and 3.46 g of triethanolamine (bp: 361°C) with a metal impurity content of 10 ppb or less were charged, and while keeping the liquid temperature in the reaction vessel at 70°C using a mantle heater, 1411 g of tetramethyl silicate (manufactured by Tama Chemicals Co., Ltd.) with a metal impurity content of 10 ppb or less was continuously fed with stirring over a period of 3 hours. The feeding of tetramethyl silicate into the reaction vessel was then completed. 457 g of the obtained colloidal silica having a silica concentration of 12.6% by weight, 2916 g of pure water having a metal impurity content of 0.1 ppb or less, and 8.12 g of triethanolamine having a metal impurity content of 10 ppb or less were charged, and while maintaining the liquid temperature in the reaction vessel at 80°C using a mantle heater, 1264 g of tetramethyl silicate having a metal impurity content of 10 ppb or less (manufactured by Tama Chemicals Co., Ltd.) was continuously fed with stirring over a period of 3 hours. After the supply of tetramethylsilicate into the reaction vessel was completed, the temperature inside the reaction vessel was temporarily lowered to 40°C, the pressure inside the system was reduced by a vacuum pump, and then heating was resumed. The reaction mixture inside the reaction vessel was further heated to 52 to 68°C, and the generated methanol was distilled from the distillation tube equipped with a condenser at a distillation temperature of 32 to 67°C. Furthermore, 833 g of pure water was added while distilling off the water and methanol, and the reaction mixture (colloidal silica) generated in this reaction vessel was concentrated to 2850 g. 3 g of citric acid powder (Kanto Chemical Co., Ltd., special grade) was added to this reaction mixture, and after dispersion stabilization treatment, SEM observation confirmed that the particles were spherical with protrusions and a particle diameter of 50 nm, as shown in Figure 7. 2200 g of the resulting reaction concentrate (colloidal silica) was subjected to ion exchange treatment in the same manner as in Example 1. Various analyses were performed, and the results are shown in Table 1. In addition, by observing with an SEM as shown in Figure 8, it was confirmed that the shape of the particles did not change before and after the ion exchange.

[0051] [Comparative Example 1] Into a 5-liter (L) glass vessel equipped with a stirrer, a thermometer, a distillation tube with a condenser, and an organosilicate inlet tube, 37,974 g of pure water with a metal impurity content of 0.1 ppb or less and 1.31 g of triethanolamine (bp: 361°C) with a metal impurity content of 10 ppb or less were charged, and while maintaining the liquid temperature inside the reaction vessel at 70°C using a mantle heater, 681.4 g of tetramethylsilicate (manufactured by Tama Chemicals Co., Ltd.) with a metal impurity content of 10 ppb or less was continuously fed with stirring over a period of 3 hours. After the supply of tetramethylsilicate into the reaction vessel was completed, the temperature inside the reaction vessel was temporarily lowered to 40°C, the pressure inside the system was reduced by a vacuum pump, and then heating was resumed. The reaction mixture inside the reaction vessel was further heated to 52 to 68°C, and the generated methanol was distilled from the distillation tube equipped with a condenser at a distillation temperature of 32 to 67°C. Furthermore, 1840 g of pure water was added while distilling off the water and methanol, and the reaction mixture (colloidal silica) generated in this reaction vessel was concentrated to 2600 g. Next, this reaction mixture was stirred at 55 rpm, and carbon dioxide gas was blown in at 40 mL / min for 13 minutes to carry out a dispersion stabilization treatment. 2200 g of the resulting reaction concentrate (colloidal silica) was subjected to ion exchange treatment in the same manner as in Example 1, but the zeta potential was −1.98 mV, and the liquid passing time gradually became slower during the ion exchange. The obtained colloidal silica was confirmed to have undergone silica aggregation after ion exchange and before the addition of an alkaline stabilizer (ammonia).

[0052] [Comparative Example 2] In a 5L glass reactor equipped with a stirrer, a thermometer, a distillation tube with a condenser, and an organosilicate inlet tube, 3404g of pure water with a metal impurity content of 0.1ppb or less and 2.76g of a 25wt%-TMAH aqueous solution with a metal impurity content of 10ppb or less were charged, and while keeping the liquid temperature in the reactor at 80°C using a mantle heater, 1196g of tetramethylsilicate with a metal impurity content of 10ppb or less (manufactured by Tama Chemicals Co., Ltd.) was continuously fed with stirring over 2.25 hours. 10 minutes after the completion of the feeding of tetramethylsilicate, 8.372g of 100% triethanolamine was added as an alkali stabilizer. The resulting colloidal silica was an association-type colloidal silica having a silica concentration of 10.89% by weight and a transmittance of 89.9%. After cooling with water, the pressure in the reaction vessel was reduced to 0.03 MPa, and the reaction mixture was further heated to 50°C to 70°C to distill the produced methanol together with water from a distillation tube equipped with a condenser at a distillation temperature of 50°C to 70°C, and the reaction mixture (colloidal silica) produced in this reaction vessel was concentrated to 2300 g. Next, this reaction mixture was stirred at 55 rpm, and carbon dioxide gas was blown in at 40 mL / min for 13 minutes to carry out a dispersion stabilization treatment. 2200 g of the resulting reaction concentrate (colloidal silica) was subjected to ion exchange treatment in the same manner as in Example 1, but the zeta potential was −2.53 mV, and the liquid passing time gradually became slower during the ion exchange. The obtained colloidal silica was confirmed to have undergone silica aggregation after ion exchange and before the addition of an alkaline stabilizer (ammonia).

[0053] [Comparative Example 3] In a 5L glass reaction vessel equipped with a stirrer, a thermometer, a distillation tube with a condenser, and an organosilicate inlet tube, 3404g of pure water with a metal impurity content of 0.1ppb or less and 2.76g of a 25wt%-TMAH aqueous solution with a metal impurity content of 10ppb or less were charged, and while the liquid temperature in the reaction vessel was kept at 80°C using a mantle heater, 1196g of tetramethylsilicate (manufactured by Tama Chemicals Co., Ltd.) with a metal impurity content of 10ppb or less was continuously fed under stirring over a period of 6 hours. In addition, 10 minutes after the completion of the feeding of tetramethylsilicate, 8.372g of 100% triethanolamine was added as an alkali stabilizer. After cooling with water, the pressure in the reaction vessel was reduced to 0.03 MPa, and the reaction mixture was further heated to 50°C to 70°C to distill the produced methanol together with water from a distillation tube equipped with a condenser at a distillation temperature of 50°C to 70°C, and the reaction mixture (colloidal silica) produced in this reaction vessel was concentrated to 2300 g. Next, this reaction mixture was stirred at 55 rpm, and carbon dioxide gas was blown in at 40 mL / min for 13 minutes to carry out a dispersion stabilization treatment. 2200 g of the resulting reaction concentrate (colloidal silica) was subjected to ion exchange treatment in the same manner as in Example 1, but the zeta potential was −3.41 mV, and the liquid passing time gradually became slower during the ion exchange. Colloidal silica was confirmed to have aggregated after ion exchange and before the addition of an alkaline stabilizer (ammonia).

[0054] The physical properties of the resulting colloidal silica were evaluated by the following methods. (1) SEM observation: Colloidal silica was diluted with water, placed on a silicon wafer sample stage, and then dried. The sample was then observed using a Hitachi High-Tech ultra-high resolution field emission scanning electron microscope SU9000 (magnification: 300,000 times). (2) BET particle size: Measured using a NOVA4200e manufactured by Yuasa Ionics Co., Ltd. The average particle size of the spherical colloidal silica particles constituting the colloidal silica particles is measured by the nitrogen adsorption method (BET method) and the specific surface area Sm 2 The particle diameter is calculated from the particle diameter by the formula D2 = 2720 / S based on the mass per unit area (g). (3) Zeta potential: Using a ZetaProbe zeta potential meter manufactured by Colloidal Dynamics, it was measured according to the method for measuring the zeta potential in high-concentration colloidal solutions (solutions having silica concentrations shown in Tables 1 to 3) based on the theory of ESA electroacoustic phenomena. (4) Average particle size (nm): The median value of the particle size distribution measured using a disk centrifugal particle size distribution measuring device manufactured by CPS Instruments, USA, was taken as the average particle size (nm). (5) Particle size (nm) of relative mass [50%]: In the evaluation of aggregation, the particle size (nm) of relative mass [50%] (the high particle size shoulder of the particle size distribution) was measured using a disk centrifugal particle size distribution analyzer manufactured by CPS Instruments, USA. A typical schematic diagram is shown in Figure 9. (6) Silica concentration: The residue after evaporation of the water content was taken as the silica concentration. (7) pH, viscosity, and electrical conductivity: Measured at 25°C.

[0055] [Table 1]

[0056]

Table 2

[0057]

Table 3

Claims

1. A method for producing colloidal silica having excellent dispersion stability, comprising the steps of: A method for producing colloidal silica, comprising the steps of reacting trimethyl silicate, tetramethyl silicate, triethyl silicate or methyltrimethyl silicate as an easily hydrolyzable organosilicate in the presence of a hydrolysis catalyst consisting of one or a mixture of two or more selected from quaternary ammoniums, aminoalcohols, morpholines and piperazines, removing an alcohol produced from the easily hydrolyzable organosilicate, and then obtaining a reaction concentrate which has been dispersed and stabilized with an acid. The reaction concentrate is then contacted with a cation exchange resin to remove the hydrolysis catalyst, thereby producing colloidal silica in which the hydrolysis catalyst is 100 ppm or less and the absolute value of the zeta potential is 4 millivolts (mV) or more.

2. 2. The method for producing colloidal silica according to claim 1, wherein the quaternary ammonium is one or a mixture of two or more selected from tetramethylammonium hydroxide (TMAH), choline, tetraethylammonium hydroxide (TEAH), and carbonates, bicarbonates, and silicates thereof.

3. 3. The method for producing colloidal silica according to claim 1, wherein the amino alcohol is an ethanolamine derivative.

4. The method for producing colloidal silica according to any one of claims 1 to 3, characterized in that the viscosity of the reaction concentrate is adjusted to 1 to 100 mPa·s and then the reaction concentrate is brought into contact with a cation exchange resin.

5. The method for producing colloidal silica according to any one of claims 1 to 4, wherein an acid or ammonia is added to the reaction concentrate before or after the contact with the cation exchange resin.

6. The method for producing colloidal silica according to claim 5, wherein an acid is added to the reaction concentrate before the reaction concentrate is contacted with a cation exchange resin to adjust the pH to 4 to 9, and an acid or ammonia is further added to the reaction concentrate after the reaction concentrate is contacted with the cation exchange resin.

7. 6. The method for producing colloidal silica according to claim 5, wherein an acid is added to the reaction concentrate before the reaction concentrate is brought into contact with the cation exchange resin to adjust the pH to less than 4, and no stabilizer containing an acid or ammonia is added to the reaction concentrate after the reaction concentrate is brought into contact with the cation exchange resin.

8. 8. A colloidal silica obtained by the method according to any one of claims 1 to 7, characterized in that the colloidal silica has a plurality of protrusions on its surface, contains 100 ppm or less of a hydrolysis catalyst consisting of one or a mixture of two or more selected from the group consisting of quaternary ammonium compounds, amino alcohols, morpholines, and piperazines, and has an absolute value of a zeta potential of 4 millivolts (mV) or more.

9. The colloidal silica according to claim 8, characterized in that the metal impurity content is 1 ppm or less.

Citation Information

Patent Citations

  • Exhaust pipe supporting device

    JP1992055126A

  • Production of acidic silica sol

    JP1994199515A

  • Production of silica sol

    JP1994316407A

  • Detergent for automotive window glass

    JP1996302394A

  • Method for producing modified colloidal silica

    JP2005162533A