Composition for polishing

The polishing composition addresses the challenge of achieving high-quality surface finishes on semiconductor substrates by combining abrasive grains, polyvinyl alcohol polymer, and polyvalent organic acid (salt) to reduce haze and improve wettability, resulting in enhanced surface quality.

JP7588066B2Active Publication Date: 2024-11-21FUJIMI INCORPORATED
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021509368
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-26
Filing Date
2020-03-23
Publication Date
2024-11-21
Estimated Expiration
2040-03-23

Smart Images

  • Figure 0007588066000001
    Figure 0007588066000001
  • Figure 0007588066000002
    Figure 0007588066000002
Patent Text Reader

Abstract

A polishing composition provided by the present invention comprises abrasive grains, a poly(vinyl alcohol)-based polymer as a water-soluble polymer, a basic compound, and water and further contains a polyvalent organic acid (salt) having a valence of 3 or higher.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polishing composition. This application claims priority based on Japanese Patent Application No. 2019-058620, filed on March 26, 2019, the entire contents of which are incorporated herein by reference. [Background technology]

[0002] Precision polishing using a polishing composition is performed on the surfaces of materials such as metals, semi-metals, non-metals, and oxides thereof. For example, the surface of a silicon wafer used as a component of a semiconductor device is generally finished into a high-quality mirror surface through a lapping process (rough polishing process) and a polishing process (precision polishing process). The polishing process typically includes a preliminary polishing process (preliminary polishing process) and a finish polishing process (final polishing process). Patent documents 1 to 4 are technical documents related to polishing compositions mainly used for polishing semiconductor substrates such as silicon wafers. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 11-140427 [Patent Document 2] Japanese Patent No. 5474400 [Patent Document 3] Japanese Patent No. 6029895 [Patent Document 4] Japanese Patent No. 6050125 Summary of the Invention [Problem to be solved by the invention]

[0004] Polishing compositions used in finish polishing processes (particularly finish polishing processes for semiconductor substrates such as silicon wafers and other substrates) are required to have the ability to realize high-quality surfaces after polishing. Many polishing compositions for such applications contain, in addition to abrasive grains and water, water-soluble polymers for the purposes of protecting the surface of the object to be polished and improving wettability.

[0005] By using polyvinyl alcohol-based polymer as water-soluble polymer, the wettability of the surface after polishing can be improved. Meanwhile, in recent years, the demand for surface quality after polishing has become higher. Therefore, the present invention aims to provide a polishing composition that contains polyvinyl alcohol-based polymer as water-soluble polymer and can improve the surface quality of the polishing object after polishing. [Means for solving the problem]

[0006] The polishing composition provided by this specification contains abrasive grains, a polyvinyl alcohol-based polymer as a water-soluble polymer, a basic compound, and water. The polishing composition further contains a polyvalent organic acid (salt) having a valence of 3 or more. The use of the polyvalent organic acid (salt) can improve the surface quality of the object to be polished after polishing with the polishing composition containing the polyvinyl alcohol-based polymer. For example, the haze can be improved.

[0007] In this specification, the term "acid (salt)" refers to an acid and its salt in a comprehensive sense, and may also be written as "acid and / or its salt." For example, the polishing composition disclosed herein containing a trivalent or higher polyvalent organic acid (salt) means that the composition contains at least one selected from the group consisting of trivalent or higher polyvalent organic acids and their salts.

[0008] A preferred embodiment of the polishing composition contains a trivalent or higher polyvalent carboxylic acid (salt) as the polyvalent organic acid (salt). In such an embodiment, the haze improving effect can be suitably exhibited.

[0009] A polishing composition according to another preferred embodiment contains an ammonium salt of a trivalent or higher polyvalent organic acid as the polyvalent organic acid (salt). The ammonium salt of a polyvalent organic acid can effectively improve haze even when used in a small amount.

[0010] In some embodiments of the polishing composition disclosed herein, the polishing composition has the following formula: Dispersity [nm]=(d 84 -d 16 ) / 2; It is preferable that the dispersity calculated by the above formula is less than 10.8 nm. 84 is the particle diameter [nm] at the point where the cumulative curve of the particle size distribution is 84%, and d 16 is the particle diameter [nm] at the point where the cumulative curve of the particle size distribution is 16%. According to such a polishing composition, in a configuration containing a polyvinyl alcohol-based polymer, the haze on the surface of the object to be polished after polishing can be effectively improved.

[0011] In some embodiments of the polishing composition disclosed herein, the polishing composition further contains a water-soluble polymer other than the polyvinyl alcohol-based polymer (hereinafter, also referred to as "other water-soluble polymer"). The polishing composition further contains a water-soluble polymer represented by the following formula: Dispersity [nm]=(d 84 -d 16 ) / 2; It is preferable that the dispersion calculated by the above formula is less than 14.2 nm. 84 and d 16 According to such a polishing composition, in a configuration containing a combination of a polyvinyl alcohol-based polymer and another water-soluble polymer, the haze on the surface of an object to be polished after polishing can be effectively improved.

[0012] In some embodiments of the polishing composition disclosed herein, the polishing composition contains the organic acid (salt) such that the increase ratio of electrical conductivity is not more than 3. This makes it possible to realize a polishing composition that effectively improves haze.

[0013] In a preferred embodiment of the polishing composition disclosed herein, the pH is 8 to 12. In polishing using a polishing composition having such a pH, haze can be more suitably improved.

[0014] The polyvinyl alcohol polymer has a weight average molecular weight (Mw) of 10×10 4 The following can be preferably used: By using a polyvinyl alcohol-based polymer having such Mw in combination with a polyvalent organic acid (salt), the effect of improving haze can be more suitably exhibited.

[0015] As the abrasive grains, silica grains are preferably used. The effect of improving haze by using a combination of a polyvinyl alcohol-based polymer and a polyvalent organic acid (salt) is preferably exhibited in polishing using silica grains as the abrasive grains.

[0016] The polishing composition disclosed herein can be preferably used in the finish polishing process of silicon wafers. By performing finish polishing using the polishing composition, haze can be improved and a high-quality silicon wafer surface can be preferably realized. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Preferred embodiments of the present invention will be described below. Note that matters other than those specifically mentioned in this specification that are necessary for carrying out the present invention can be understood as design matters for a person skilled in the art based on the prior art in the relevant field. The present invention can be carried out based on the contents disclosed in this specification and the technical common sense in the relevant field.

[0018] The polishing composition disclosed herein contains abrasive grains, a polyvinyl alcohol-based polymer as a water-soluble polymer, a polyvalent organic acid (salt), a basic compound, and water. The contents of the polishing composition disclosed herein are described below.

[0019] <Abrasive grain> The polishing composition disclosed herein includes abrasive grains. The abrasive grains function to mechanically polish the surface of the object to be polished. The material and properties of the abrasive grains are not particularly limited, and can be appropriately selected according to the purpose and mode of use of the polishing composition. Examples of the abrasive grains include inorganic particles, organic particles, and organic-inorganic composite particles. Specific examples of inorganic particles include oxide particles such as silica particles, alumina particles, cerium oxide particles, chromium oxide particles, titanium dioxide particles, zirconium oxide particles, magnesium oxide particles, manganese dioxide particles, zinc oxide particles, and red iron oxide particles; nitride particles such as silicon nitride particles and boron nitride particles; carbide particles such as silicon carbide particles and boron carbide particles; diamond particles; carbonates such as calcium carbonate and barium carbonate, and the like. Specific examples of organic particles include polymethylmethacrylate (PMMA) particles, poly(meth)acrylic acid particles (here, (meth)acrylic acid refers to acrylic acid and methacrylic acid in a comprehensive sense), polyacrylonitrile particles, and the like. Such abrasive grains may be used alone or in combination of two or more kinds.

[0020] The abrasive grains are preferably inorganic particles, and among them, particles made of metal or semimetal oxides are preferred, and silica particles are particularly preferred. In a polishing composition that can be used for polishing (e.g., finish polishing) an object to be polished having a surface made of silicon, such as a silicon wafer described below, it is particularly meaningful to employ silica particles as the abrasive grains. The technology disclosed herein can be preferably implemented, for example, in an embodiment in which the abrasive grains are substantially made of silica particles. Here, "substantially" means that 95% by weight or more (preferably 98% by weight or more, more preferably 99% by weight or more, and may be 100% by weight) of the particles constituting the abrasive grains are silica particles.

[0021] Specific examples of silica particles include colloidal silica, fumed silica, precipitated silica, etc. The silica particles can be used alone or in combination of two or more. The use of colloidal silica is particularly preferred because it is easy to obtain a polished surface with excellent surface quality after polishing. As the colloidal silica, for example, colloidal silica produced by an ion exchange method using water glass (sodium silicate) as a raw material, or alkoxide method colloidal silica (colloidal silica produced by hydrolysis and condensation reaction of alkoxysilane) can be preferably used. The colloidal silica can be used alone or in combination of two or more.

[0022] The true specific gravity of the abrasive grain constituent material (e.g., silica constituting silica grains) is preferably 1.5 or more, more preferably 1.6 or more, and even more preferably 1.7 or more. The upper limit of the true specific gravity of silica is not particularly limited, but is typically 2.3 or less, for example, 2.2 or less. The true specific gravity of the abrasive grains (e.g., silica grains) can be measured by a liquid substitution method using ethanol as a substitution liquid.

[0023] The BET diameter (average primary particle diameter) of the abrasive grains (typically silica particles) is not particularly limited, but from the viewpoint of polishing efficiency, etc., it is preferably 5 nm or more, more preferably 10 nm or more. From the viewpoint of obtaining a higher polishing effect (for example, the effect of reducing haze, removing defects, etc.), the BET diameter is preferably 15 nm or more, more preferably 20 nm or more (for example, more than 20 nm). In addition, from the viewpoint of preventing scratches, etc., the BET diameter of the abrasive grains is preferably 100 nm or less, more preferably 50 nm or less, and even more preferably 40 nm or less. From the viewpoint of easily obtaining a surface with a lower haze, in some embodiments, the BET diameter of the abrasive grains may be 35 nm or less, may be less than 32 nm, or may be less than 30 nm.

[0024] In this specification, the BET diameter is calculated from the specific surface area (BET value) measured by the BET method, as follows: BET diameter (nm) = 6000 / (true density (g / cm 3 ) × BET value (m 2 / g) For example, in the case of silica particles, BET diameter (nm) = 2727 / BET value (m 2 The BET diameter can be calculated from the specific surface area (ratio of specific surface area to specific surface area) of the powder. The specific surface area can be measured using, for example, a surface area measuring device manufactured by Micromeritics, Inc., under the trade name "Flow Sorb II 2300".

[0025] The shape (outer shape) of the abrasive grains may be spherical or non-spherical. Specific examples of non-spherical particles include peanut-shaped (i.e., peanut shell-shaped), cocoon-shaped, confetti-shaped, and rugby ball-shaped. For example, abrasive grains in which most of the particles are peanut-shaped or cocoon-shaped can be preferably used.

[0026] Although not particularly limited, the average value of the long axis / short axis ratio (average aspect ratio) of the abrasive grains is in principle 1.0 or more, preferably 1.05 or more, and more preferably 1.1 or more. By increasing the average aspect ratio, higher polishing efficiency can be realized. Moreover, from the viewpoint of reducing scratches, etc., the average aspect ratio of the abrasive grains is preferably 3.0 or less, more preferably 2.0 or less, and even more preferably 1.5 or less.

[0027] The shape (outer shape) and average aspect ratio of the abrasive grains can be grasped, for example, by observation with an electron microscope. As a specific procedure for grasping the average aspect ratio, for example, a scanning electron microscope (SEM) is used to draw the smallest rectangle circumscribing each particle image for a predetermined number (for example, 200) of abrasive grains whose individual particle shapes can be recognized. Then, for the rectangle drawn for each particle image, the long side length (long axis value) is divided by the short side length (short axis value) to calculate the long axis / short axis ratio (aspect ratio). The average aspect ratio can be obtained by arithmetically averaging the aspect ratios of the above-mentioned predetermined number of particles.

[0028] <Water-soluble polymer> The polishing composition disclosed herein contains a water-soluble polymer, which can be useful for protecting the surface of the object to be polished and for improving the wettability of the surface of the object to be polished after polishing.

[0029] (Polyvinyl alcohol polymer) The polishing composition disclosed herein contains a polyvinyl alcohol-based polymer as a water-soluble polymer. As the polyvinyl alcohol-based polymer, a water-soluble organic material (typically a water-soluble polymer) containing a vinyl alcohol unit as its repeating unit is used. Here, the vinyl alcohol unit (hereinafter also referred to as "VA unit") is a structural portion represented by the following chemical formula: -CH2-CH(OH)-;. The polyvinyl alcohol-based polymer may contain only VA units as repeating units, or may contain repeating units other than VA units (hereinafter also referred to as "non-VA units") in addition to VA units. The polyvinyl alcohol-based polymer may be a random copolymer containing VA units and non-VA units, or may be a block copolymer or a graft copolymer. The polyvinyl alcohol-based polymer may contain only one type of non-VA unit, or may contain two or more types of non-VA units.

[0030] The polyvinyl alcohol-based polymer used in the polishing composition disclosed herein may be unmodified polyvinyl alcohol (unmodified PVA) or modified polyvinyl alcohol (modified PVA). Here, unmodified PVA refers to a polyvinyl alcohol-based polymer that is produced by hydrolysis (saponification) of polyvinyl acetate and does not substantially contain repeating units other than repeating units (-CH2-CH(OCOCH3)-) and VA units that are vinyl polymerized from vinyl acetate. The saponification degree of the unmodified PVA may be, for example, 60% or more, and from the viewpoint of water solubility, may be 70% or more, 80% or more, or 90% or more. In some embodiments, unmodified PVA with a saponification degree of 95% or more or 98% or more may be preferably adopted as a water-soluble polymer compound.

[0031] Examples of non-VA units that may be contained in the modified PVA include, but are not limited to, repeating units derived from N-vinyl monomers or N-(meth)acryloyl monomers described below, repeating units derived from ethylene, repeating units derived from alkyl vinyl ethers, and repeating units derived from vinyl esters of monocarboxylic acids having 3 or more carbon atoms. A suitable example of the N-vinyl monomer is N-vinylpyrrolidone. A suitable example of the N-(meth)acryloyl monomer is N-(meth)acryloylmorpholine. The alkyl vinyl ether may be, for example, a vinyl ether having an alkyl group having 1 to 10 carbon atoms, such as propyl vinyl ether, butyl vinyl ether, or 2-ethylhexyl vinyl ether. The vinyl ester of a monocarboxylic acid having 3 or more carbon atoms may be, for example, a vinyl ester of a monocarboxylic acid having 3 to 7 carbon atoms, such as vinyl propanoate, vinyl butanoate, vinyl pentanoate, or vinyl hexanoate.

[0032] The polyvinyl alcohol-based polymer may be a modified PVA containing VA units and non-VA units having at least one structure selected from oxyalkylene groups, carboxy groups, sulfo groups, amino groups, hydroxyl groups, amide groups, imide groups, nitrile groups, ether groups, ester groups, and salts thereof. The polyvinyl alcohol-based polymer may also be a modified PVA in which a part of the VA units contained in the polyvinyl alcohol-based polymer is acetalized with an aldehyde. As the aldehyde, for example, an alkyl aldehyde can be preferably used, and an alkyl aldehyde having an alkyl group having 1 to 7 carbon atoms is preferable, and n-butyl aldehyde is particularly preferable. As the polyvinyl alcohol-based polymer, a cation-modified polyvinyl alcohol in which a cationic group such as a quaternary ammonium structure is introduced may be used. As the cation-modified polyvinyl alcohol, for example, one in which a cationic group derived from a monomer having a cationic group such as diallyldialkylammonium salt or N-(meth)acryloylaminoalkyl-N,N,N-trialkylammonium salt is introduced is exemplified.

[0033] The ratio of the number of moles of VA units to the number of moles of all repeating units constituting the polyvinyl alcohol-based polymer may be, for example, 5% or more, 10% or more, 20% or more, or 30% or more. Although not particularly limited, in some embodiments, the ratio of the number of moles of VA units may be 50% or more, 65% or more, 75% or more, 80% or more, or 90% or more (for example, 95% or more, or 98% or more). Substantially 100% of the repeating units constituting the polyvinyl alcohol-based polymer may be VA units. Here, "substantially 100%" means that the polyvinyl alcohol-based polymer does not contain non-VA units at least intentionally, and typically the ratio of the number of moles of non-VA units to the number of moles of all repeating units is less than 2% (for example, less than 1%), including the case of 0%. In some other embodiments, the ratio of the number of moles of VA units to the number of moles of all repeating units constituting the polyvinyl alcohol-based polymer may be, for example, 95% or less, 90% or less, 80% or less, or 70% or less.

[0034] The content of VA units in the polyvinyl alcohol-based polymer (content based on weight) may be, for example, 5% by weight or more, 10% by weight or more, 20% by weight or more, or 30% by weight or more. Although not particularly limited, in some embodiments, the content of the VA units may be 50% by weight or more (e.g., more than 50% by weight), 70% by weight or more, or 80% by weight or more (e.g., 90% by weight or more, 95% by weight or more, or 98% by weight or more). Substantially 100% by weight of the repeating units constituting the polyvinyl alcohol-based polymer may be VA units. Here, "substantially 100% by weight" means that non-VA units are not contained as repeating units constituting the polyvinyl alcohol-based polymer at least intentionally, and typically means that the content of non-VA units in the polyvinyl alcohol-based polymer is less than 2% by weight (e.g., less than 1% by weight). In some other embodiments, the content of VA units in the polyvinyl alcohol-based polymer may be, for example, 95% by weight or less, 90% by weight or less, 80% by weight or less, or 70% by weight or less.

[0035] A polyvinyl alcohol-based polymer may contain multiple polymer chains with different VA unit contents in the same molecule. Here, the polymer chain refers to a portion (segment) that constitutes a part of a single polymer molecule. For example, a polyvinyl alcohol-based polymer may contain a polymer chain A with a VA unit content of more than 50% by weight and a polymer chain B with a VA unit content of less than 50% by weight (i.e., a non-VA unit content of more than 50% by weight) in the same molecule.

[0036] The polymer chain A may contain only VA units as repeat units, or may contain non-VA units in addition to VA units. The content of VA units in the polymer chain A may be 60% by weight or more, 70% by weight or more, 80% by weight or more, or 90% by weight or more. In some embodiments, the content of VA units in the polymer chain A may be 95% by weight or more, or 98% by weight or more. Substantially 100% by weight of the repeat units constituting the polymer chain A may be VA units.

[0037] The polymer chain B may contain only non-VA units as repeat units, or may contain VA units in addition to non-VA units. The content of non-VA units in the polymer chain B may be 60% by weight or more, 70% by weight or more, 80% by weight or more, or 90% by weight or more. In some embodiments, the content of non-VA units in the polymer chain B may be 95% by weight or more, or 98% by weight or more. Substantially 100% by weight of the repeat units constituting the polymer chain B may be non-VA units.

[0038] Examples of polyvinyl alcohol-based polymers containing polymer chain A and polymer chain B in the same molecule include block copolymers and graft copolymers containing these polymer chains. The graft copolymer may be a graft copolymer having a structure in which polymer chain B (side chain) is grafted to polymer chain A (main chain), or a graft copolymer having a structure in which polymer chain A (side chain) is grafted to polymer chain B (main chain). In one embodiment, a polyvinyl alcohol-based polymer having a structure in which polymer chain B is grafted to polymer chain A can be used.

[0039] Examples of the polymer chain B include a polymer chain having a repeating unit derived from an N-vinyl type monomer as a main repeating unit, a polymer chain having a repeating unit derived from an N-(meth)acryloyl type monomer as a main repeating unit, a polymer chain having an oxyalkylene unit as a main repeating unit, etc. In this specification, the main repeating unit refers to a repeating unit contained in an amount of more than 50% by weight, unless otherwise specified.

[0040] A preferred example of the polymer chain B is a polymer chain having an N-vinyl type monomer as a main repeating unit, i.e., an N-vinyl polymer chain. The content of the repeating unit derived from the N-vinyl type monomer in the N-vinyl polymer chain is typically more than 50% by weight, and may be 70% by weight or more, 85% by weight or more, or 95% by weight or more. Substantially all of the polymer chain B may be a repeating unit derived from an N-vinyl type monomer.

[0041] In this specification, examples of N-vinyl type monomers include monomers having a nitrogen-containing heterocycle (e.g., lactam ring) and N-vinyl chain amides. Specific examples of N-vinyl lactam type monomers include N-vinyl pyrrolidone, N-vinyl piperidone, N-vinyl morpholinone, N-vinyl caprolactam, N-vinyl-1,3-oxazin-2-one, N-vinyl-3,5-morpholinedione, and the like. Specific examples of N-vinyl chain amides include N-vinyl acetamide, N-vinyl propionic acid amide, N-vinyl butyric acid amide, and the like. The polymer chain B may be, for example, an N-vinyl polymer chain in which more than 50% by weight (e.g., 70% by weight or more, 85% by weight or more, or 95% by weight or more) of its repeating units are N-vinyl pyrrolidone units. Substantially all of the repeating units constituting the polymer chain B may be N-vinyl pyrrolidone units.

[0042] Another example of the polymer chain B is a polymer chain having a repeating unit derived from an N-(meth)acryloyl type monomer as a main repeating unit, i.e., an N-(meth)acryloyl-based polymer chain. The content of the repeating unit derived from an N-(meth)acryloyl type monomer in the N-(meth)acryloyl-based polymer chain is typically more than 50% by weight, and may be 70% by weight or more, 85% by weight or more, or 95% by weight or more. Substantially all of the polymer chain B may be a repeating unit derived from an N-(meth)acryloyl type monomer.

[0043] In this specification, examples of N-(meth)acryloyl type monomers include chain amides having an N-(meth)acryloyl group and cyclic amides having an N-(meth)acryloyl group. Examples of chain amides having an N-(meth)acryloyl group include (meth)acrylamide; N-alkyl(meth)acrylamides such as N-methyl(meth)acrylamide, N-ethyl(meth)acrylamide, N-propyl(meth)acrylamide, N-isopropyl(meth)acrylamide, and Nn-butyl(meth)acrylamide; and N,N-dialkyl(meth)acrylamides such as N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-dipropyl(meth)acrylamide, N,N-diisopropyl(meth)acrylamide, and N,N-di(n-butyl)(meth)acrylamide. Examples of cyclic amides having an N-(meth)acryloyl group include N-(meth)acryloylmorpholine and N-(meth)acryloylpyrrolidine.

[0044] Another example of the polymer chain B is a polymer chain containing an oxyalkylene unit as a main repeating unit, i.e., an oxyalkylene-based polymer chain. The content of the oxyalkylene unit in the oxyalkylene-based polymer chain is typically more than 50% by weight, and may be 70% by weight or more, 85% by weight or more, or 95% by weight or more. Substantially all of the repeating units contained in the polymer chain B may be oxyalkylene units.

[0045] Examples of oxyalkylene units include oxyethylene units, oxypropylene units, oxybutylene units, etc. Such oxyalkylene units may be repeating units derived from the corresponding alkylene oxides. The oxyalkylene units contained in the oxyalkylene polymer chain may be one type or two or more types. For example, the oxyalkylene polymer chain may contain a combination of oxyethylene units and oxypropylene units. In the oxyalkylene polymer chain containing two or more types of oxyalkylene units, the oxyalkylene units may be random copolymers of the corresponding alkylene oxides, or may be block copolymers or graft copolymers.

[0046] Further examples of polymer chain B include polymer chains containing a repeating unit derived from an alkyl vinyl ether (e.g., a vinyl ether having an alkyl group having from 1 to 10 carbon atoms), a polymer chain containing a repeating unit derived from a monocarboxylic acid vinyl ester (e.g., a vinyl ester of a monocarboxylic acid having from 3 or more carbon atoms), a polymer chain in which a part of the VA units has been acetalized with an aldehyde (e.g., an alkyl aldehyde having an alkyl group having from 1 to 7 carbon atoms), and a polymer chain into which a cationic group (e.g., a cationic group having a quaternary ammonium structure) has been introduced.

[0047] As the polyvinyl alcohol-based polymer in the polishing composition disclosed herein, non-modified PVA may be used, modified PVA may be used, or non-modified PVA and modified PVA may be used in combination.In the embodiment of using non-modified PVA and modified PVA in combination, the amount of modified PVA used relative to the total amount of polyvinyl alcohol-based polymer contained in the polishing composition may be, for example, less than 95% by weight, 90% by weight or less, 75% by weight or less, 50% by weight or less, 30% by weight or less, 10% by weight or less, 5% by weight or less, or 1% by weight or less.The polishing composition disclosed herein may be preferably implemented, for example, in the embodiment of using only one or more non-modified PVA as the polyvinyl alcohol-based polymer.

[0048] The weight average molecular weight (Mw) of the polyvinyl alcohol-based polymer used in the polishing composition disclosed herein is not particularly limited. The Mw of the polyvinyl alcohol-based polymer is usually 100×10 4 The following is appropriate: 30 x 10 4 Less than or equal to 20×10 is preferred 4 The smaller the Mw of the polyvinyl alcohol-based polymer, the more the dispersion stability of the polyvinyl alcohol-based polymer tends to improve. From this viewpoint, in some embodiments, the Mw of the polyvinyl alcohol-based polymer may be 15×10 4 Less than 10 x 10 is fine. 4 The Mw of the polyvinyl alcohol polymer is usually 2×10 3 It is appropriate that the value is 5×10 or more. 3 May be greater than or equal to 1 x 10 4 As the Mw of the polyvinyl alcohol-based polymer increases, the effect of protecting the object to be polished and improving the wettability tends to increase. From this viewpoint, the Mw of the polyvinyl alcohol-based polymer used in the polishing composition disclosed herein may be 5×10 3 It is preferable that the concentration is 1×10 or more. 4 That is 2 x 10 4 More than 5×10 is fine. 4More than 6×10 is fine. 4 More than 6.5×10 is fine. 4 More than that is fine.

[0049] In this specification, the weight average molecular weight (Mw) of the water-soluble polymer and the surfactant described later can be a value based on aqueous gel permeation chromatography (GPC) (aqueous, polyethylene oxide equivalent). As the GPC measuring device, it is recommended to use a model named "HLC-8320GPC" manufactured by Tosoh Corporation. The measurement can be performed, for example, under the following conditions. The same method is also used in the examples described later. [GPC measurement conditions] Sample concentration: 0.1% by weight Column: TSKgel GMPWXL Detector: Differential refractometer Eluent: 100mM sodium nitrate aqueous solution / acetonitrile = 10~8 / 0~2 Flow rate: 1mL / min Measurement temperature: 40℃ Sample injection volume: 200 μL

[0050] The content of polyvinyl alcohol-based polymer in the polishing composition (the total amount when two or more kinds of polyvinyl alcohol-based polymers are included) is not particularly limited. From the viewpoint of polishing performance and surface quality improvement, in some embodiments, the content may be, for example, 0.0001% by weight or more, and is usually appropriate to be 0.00025% by weight or more, preferably 0.0004% by weight or more, for example 0.0005% by weight or more. The upper limit of the content of polyvinyl alcohol-based polymer is not particularly limited, and can be, for example, 0.05% by weight or less. From the viewpoint of stability, polishing rate, cleanability, etc. at the concentrated liquid stage, in some embodiments, the content of polyvinyl alcohol-based polymer is preferably 0.035% by weight or less, more preferably 0.025% by weight or less, even more preferably 0.02% by weight or less, particularly preferably 0.015% by weight or less, for example 0.0125% by weight or less, typically 0.01% by weight or less. The polishing composition disclosed herein can also be preferably implemented in an embodiment in which the content of the polyvinyl alcohol-based polymer is 0.008% by weight or less, 0.006% by weight or less, or 0.004% by weight or less, for example.

[0051] The content of the polyvinyl alcohol-based polymer (the total amount when two or more kinds of polyvinyl alcohol-based polymers are included) can also be specified by the relative relationship with the abrasive grain. Although not particularly limited, in some embodiments, the content of the polyvinyl alcohol-based polymer relative to 100 parts by weight of the abrasive grain can be, for example, 0.01 parts by weight or more, and from the viewpoint of haze reduction, etc., it is appropriate to set it to 0.1 parts by weight or more, preferably 0.5 parts by weight or more, more preferably 1 part by weight or more, and even more preferably 3 parts by weight or more. In addition, the content of the polyvinyl alcohol-based polymer relative to 100 parts by weight of the abrasive grain may be, for example, 50 parts by weight or less, or may be 30 parts by weight or less. From the viewpoint of dispersion stability of the polishing composition, etc., in some embodiments, the content of the polyvinyl alcohol-based polymer relative to 100 parts by weight of the abrasive grain is appropriate to be 15 parts by weight or less, preferably 10 parts by weight or less, more preferably 8 parts by weight or less, and may be 7 parts by weight or less. The polishing composition disclosed herein can also be preferably implemented in an embodiment in which the content of the polyvinyl alcohol-based polymer per 100 parts by weight of abrasive grains is less than 5 parts by weight, less than 3 parts by weight, or less than 2 parts by weight.

[0052] (Other water-soluble polymers) The polishing composition disclosed herein may further contain other water-soluble polymers, i.e., water-soluble polymers other than polyvinyl alcohol-based polymers, as necessary, within the range that does not significantly impair the effect of the present invention.Other water-soluble polymers can be appropriately selected from water-soluble polymers known in the field of polishing compositions.Examples of other water-soluble polymers include synthetic polymers such as polymers containing oxyalkylene units and polymers containing nitrogen atoms; polymers derived from natural products such as cellulose derivatives and starch derivatives; etc.

[0053] Examples of polymers containing oxyalkylene units include polyethylene oxide (PEO), block copolymers of ethylene oxide (EO) and propylene oxide (PO) or butylene oxide (BO), and random copolymers of EO and PO or BO. Among these, block copolymers of EO and PO or random copolymers of EO and PO are preferred. The block copolymers of EO and PO may be diblock copolymers or triblock copolymers containing a PEO block and a polypropylene oxide (PPO) block. Examples of the triblock copolymers include PEO-PPO-PEO type triblock copolymers and PPO-PEO-PPO type triblock copolymers. Among these, PEO-PPO-PEO type triblock copolymers are more preferred. In a block or random copolymer of EO and PO, the molar ratio of EO to PO (EO / PO) constituting the copolymer is preferably greater than 1, more preferably 2 or more, and even more preferably 3 or more (e.g., 5 or more), from the viewpoints of solubility in water, washability, etc.

[0054] Non-limiting examples of polymers containing nitrogen atoms include polymers containing N-vinyl type monomer units; imine derivatives; polymers containing N-(meth)acryloyl type monomer units; and the like.

[0055] Examples of polymers containing N-vinyl monomer units include polymers containing repeating units derived from monomers having nitrogen-containing heterocycles (e.g., lactam rings). Examples of such polymers include homopolymers and copolymers of N-vinyl lactam monomers (e.g., copolymers having a copolymerization ratio of N-vinyl lactam monomers exceeding 50% by weight), homopolymers and copolymers of N-vinyl linear amides (e.g., copolymers having a copolymerization ratio of N-vinyl linear amides exceeding 50% by weight), and the like.

[0056] Specific examples of N-vinyl lactam type monomers (i.e., compounds having a lactam structure and an N-vinyl group in one molecule) include N-vinyl pyrrolidone (VP), N-vinyl piperidone, N-vinyl morpholinone, N-vinyl caprolactam (VC), N-vinyl-1,3-oxazin-2-one, N-vinyl-3,5-morpholinedione, etc. Specific examples of polymers containing N-vinyl lactam type monomer units include polyvinyl pyrrolidone, polyvinyl caprolactam, random copolymers of VP and VC, random copolymers of one or both of VP and VC with other vinyl monomers (e.g., acrylic monomers, vinyl ester monomers, etc.), block copolymers and graft copolymers containing polymer chains containing one or both of VP and VC, etc. Specific examples of the N-vinyl chain amide include N-vinyl acetamide, N-vinyl propionic acid amide, and N-vinyl butyric acid amide.

[0057] Examples of polymers containing N-(meth)acryloyl type monomer units include homopolymers and copolymers of N-(meth)acryloyl type monomers (typically copolymers in which the copolymerization ratio of N-(meth)acryloyl type monomers exceeds 50% by weight). Examples of N-(meth)acryloyl type monomers include linear amides having an N-(meth)acryloyl group and cyclic amides having an N-(meth)acryloyl group.

[0058] Examples of chain amides having an N-(meth)acryloyl group include (meth)acrylamide; N-alkyl (meth)acrylamides such as N-methyl (meth)acrylamide, N-ethyl (meth)acrylamide, N-propyl (meth)acrylamide, N-isopropyl (meth)acrylamide, and Nn-butyl (meth)acrylamide; and N,N-dialkyl (meth)acrylamides such as N,N-dimethyl (meth)acrylamide, N,N-diethyl (meth)acrylamide, N,N-dipropyl (meth)acrylamide, N,N-diisopropyl (meth)acrylamide, and N,N-di(n-butyl) (meth)acrylamide. Examples of polymers containing chain amides having an N-(meth)acryloyl group as monomer units include homopolymers of N-isopropylacrylamide and copolymers of N-isopropylacrylamide (for example, copolymers in which the copolymerization ratio of N-isopropylacrylamide exceeds 50% by weight).

[0059] Examples of cyclic amides having an N-(meth)acryloyl group include N-acryloylmorpholine, N-acryloylthiomorpholine, N-acryloylpiperidine, N-acryloylpyrrolidine, N-methacryloylmorpholine, N-methacryloylpiperidine, and N-methacryloylpyrrolidine. Examples of polymers containing cyclic amides having an N-(meth)acryloyl group as monomer units include acryloylmorpholine-based polymers (PACMO). Typical examples of acryloylmorpholine-based polymers include homopolymers of N-acryloylmorpholine (ACMO) and copolymers of ACMO (e.g., copolymers in which the copolymerization ratio of ACMO exceeds 50% by weight). In acryloylmorpholine-based polymers, the ratio of the number of moles of ACMO units to the number of moles of all repeating units is usually 50% or more, and is suitably 80% or more (e.g., 90% or more, typically 95% or more). All repeat units of the water-soluble polymer may be substantially composed of ACMO units.

[0060] Other examples of polymers containing nitrogen atoms include homopolymers and copolymers of N-acylalkyleneimine type monomers. Specific examples of N-acylalkyleneimine type monomers include N-acetylethyleneimine, N-propionylethyleneimine, and the like.

[0061] Cellulose derivatives are polymers containing β-glucose units as the main repeating unit, such as methyl cellulose, ethyl cellulose, hydroxyethyl cellulose (HEC), methylhydroxyethyl cellulose, etc. Starch derivatives are polymers containing α-glucose units as the main repeating unit, such as pregelatinized starch, pullulan, carboxymethyl starch, cyclodextrin, etc.

[0062] In the technology disclosed herein, the molecular weight of the other water-soluble polymer is not particularly limited. The weight average molecular weight (Mw) of the other water-soluble polymer is, for example, 100×10 4 From the viewpoint of washability, etc., it is usually 60 × 10 4 The following is appropriate: 50 x 10 4 It may be less than 40 x 10 4 In some embodiments, the Mw of the other water-soluble polymer is preferably 20×10 4 For example, 10×10 4 or less or 8×10 4 From the viewpoint of protecting the object to be polished, the Mw of the other water-soluble polymer may be, for example, 2000 or more, and is usually preferably 5000 or more. In some embodiments, the Mw is 1.0×10 4 More than 1.5×10 is appropriate. 4 More preferably, 2×10 4 More preferably, 3×10 4 Or more, for example, 4×10 4 Or more, typically 5×10 4 That's it, 10 x 10 4 More than 20 x 10 is fine. 4 More than 30 x 10 is fine. 4More than that is fine.

[0063] The other water-soluble polymers can be used alone or in combination of two or more. Although not particularly limited, the weight ratio of the polyvinyl alcohol polymer to the other water-soluble polymers may be, for example, 5:95 to 95:5, 10:90 to 90:10, or 25:75 to 75:25. In some embodiments, the weight ratio (polyvinyl alcohol-based polymer: other water-soluble polymer) may be, for example, 50:50 to 100:0, 80:20 to 100:0, or 90:10 to 100:0. In some other embodiments, the weight ratio of polyvinyl alcohol-based polymer:other water-soluble polymer may be, for example, 5:95 to 70:30, 15:85 to 50:50, or 20:80 to 40:60. The above-mentioned effects of using a trivalent or higher polyvalent organic acid (salt) can also be suitably exhibited in an embodiment that includes a combination of a polyvinyl alcohol-based polymer and another water-soluble polymer (e.g., a synthetic polymer such as a polymer containing an oxyalkylene unit or a polymer containing a nitrogen atom).

[0064] From the viewpoint of reducing aggregates and improving cleaning properties, etc., nonionic polymers can be preferably used as the other water-soluble polymers. Also, from the viewpoint of easy control of chemical structure and purity, synthetic polymers can be preferably used as the other water-soluble polymers. The polishing composition disclosed herein can be preferably implemented in an embodiment in which a polymer derived from a natural product is not substantially used as the other water-soluble polymers. Here, "substantially not used" means that the amount used relative to 100 parts by weight of polyvinyl alcohol-based polymer is typically 3 parts by weight or less, preferably 1 part by weight or less, including 0 parts by weight or less than detection limit.

[0065] (Water-soluble polymer content) The content of the water-soluble polymer in the polishing composition (the total amount when two or more kinds are included) is not particularly limited. From the viewpoint of polishing performance and surface quality improvement, in some embodiments, the content may be, for example, 0.0005% by weight or more, and is usually appropriate to be 0.0025% by weight or more, and is preferably 0.005% by weight or more, for example, 0.0075% by weight or more. The upper limit of the content of the water-soluble polymer is not particularly limited, and can be, for example, 0.05% by weight or less. From the viewpoint of stability, polishing rate, cleanability, etc. at the concentrated liquid stage, in some embodiments, the content of the water-soluble polymer is preferably 0.035% by weight or less, more preferably 0.025% by weight or less, even more preferably 0.02% by weight or less, particularly preferably 0.015% by weight or less, for example 0.0125% by weight or less, typically 0.01% by weight or less.

[0066] The content of the water-soluble polymer (the total amount when two or more kinds are included) can also be specified by the relative relationship with the abrasive grain. Although not particularly limited, in some embodiments, the content of the water-soluble polymer relative to 100 parts by weight of the abrasive grain can be, for example, 0.01 parts by weight or more, and from the viewpoint of haze reduction, etc., it is appropriate to set it to 0.1 parts by weight or more, preferably 0.5 parts by weight or more, more preferably 1 part by weight or more, and even more preferably 3 parts by weight or more. In addition, the content of the water-soluble polymer relative to 100 parts by weight of the abrasive grain may be, for example, 50 parts by weight or less, or may be 30 parts by weight or less. From the viewpoint of dispersion stability of the polishing composition, etc., in some embodiments, the content of the water-soluble polymer relative to 100 parts by weight of the abrasive grain is appropriate to be 20 parts by weight or less, preferably 15 parts by weight or less, more preferably 13 parts by weight or less, and may be 12 parts by weight or less.

[0067] <Polyvalent organic acids (salts)> The polishing composition disclosed herein contains a trivalent or higher polyvalent organic acid (salt). The present inventors have found that the haze of the polished object after polishing is improved by further containing a trivalent or higher polyvalent organic acid (salt) in a polishing composition using a polyvinyl alcohol-based polymer as a water-soluble polymer. The reason why such an effect is achieved is not particularly limited, but is thought to be, for example, as follows. That is, the inclusion of a polyvinyl alcohol-based polymer in a polishing composition containing abrasive grains can be useful for protecting the polished object and improving the wettability of the polished object surface after polishing, but can also be a factor that leads to partial aggregation of the abrasive grains. When the abrasive grains aggregate, minute polishing unevenness is likely to occur, making it difficult to reduce the haze. The trivalent or higher polyvalent organic acid (salt) exerts an effect of suppressing the aggregation of the abrasive grains and improving dispersibility in a polishing composition containing abrasive grains and a polyvinyl alcohol-based polymer, which is thought to contribute to the improvement of haze.

[0068] The polyvalent organic acid (salt) typically has three or more functional groups selected from the group consisting of acid groups and their salts in one molecule. The acid group may be, for example, a carboxy group, a sulfo group, a phospho group, etc. The functional groups may each be independently selected from the group consisting of a carboxy group, a salt of a carboxy group, a sulfo group and a salt of a sulfo group, and a phospho group and a salt of a phospho group. A suitable example of the polyvalent organic acid (salt) is a polyvalent carboxylic acid (salt) having three or more valences. The number of acid groups (the number of carboxy groups in the case of a polyvalent carboxylic acid) per molecule of the polyvalent organic acid (salt) is three or more, for example, 3, 4 or 5, and preferably 3 or 4. In some embodiments, the polyvalent organic acid (salt) may be a hydroxy polyvalent organic acid (salt) having one or more hydroxyl groups in one molecule. A suitable example of the hydroxy polyvalent organic acid (salt) is a hydroxy polyvalent carboxylic acid (salt) having one or more hydroxyl groups and three or more carboxy groups in one molecule. By using a hydroxy polycarboxylic acid (salt) as the polyvalent organic acid (salt), good abrasive grain dispersibility tends to be stably exhibited, which can more suitably realize improvement in surface quality (e.g., improvement in haze).

[0069] The polyvalent organic acid constituting the polyvalent organic acid (salt) may be, for example, aconitic acid, citric acid, butanetetracarboxylic acid, trimesic acid, trimellitic acid, cyclohexanetricarboxylic acid, pyromellitic acid, mellitic acid, nitrilotris(methylenephosphonic acid) (NTMP), 2-phosphonobutane-1,2,4-tricarboxylic acid (PBTC), etc. Among them, preferred examples include citric acid (salt) and butanetetracarboxylic acid (salt). The salt of the polyvalent organic acid may be, for example, an alkali metal salt such as a sodium salt or a potassium salt, or an ammonium salt. Among them, an ammonium salt is preferred. The polyvalent organic acid (salt) may be used alone or in combination of two or more kinds.

[0070] The content of polyvalent organic acid (salt) is not particularly limited, and can be set so that the effect of use is appropriately exhibited. In some embodiments, the content of polyvalent organic acid (salt) may be, for example, 0.0005% by weight or more, 0.001% by weight or more, 0.005% by weight or more, or 0.01% by weight or more, based on the total weight of the polishing composition. By increasing the content of polyvalent organic acid (salt), the dispersibility of abrasive grains is improved, and the effect of improving haze can be exhibited better. Here, the content of polyvalent organic acid (salt) refers to the total content in an embodiment that contains two or more polyvalent organic acids (salts). In addition, since the effect of improving haze may be reduced if the content of polyvalent organic acid (salt) is excessively high, in some embodiments, the content of polyvalent organic acid (salt) may be, for example, 5% by weight or less, 1% by weight or less, 0.3% by weight or less, 0.1% by weight or less, 0.05% by weight or less, or 0.02% by weight or less. These contents may be preferably applied to the content in the polishing liquid (working slurry) supplied to the polishing object, for example.

[0071] In some embodiments of the polishing composition disclosed herein, the preferred content of polyvalent organic acid (salt) can be specified by the relative relationship with the abrasive grains contained in the polishing composition. Specifically, the content of polyvalent organic acid (salt) in the polishing composition is, for example, about 0.01 parts by weight or more relative to 100 parts by weight of the abrasive grains contained in the polishing composition, preferably about 0.1 parts by weight or more, more preferably about 0.5 parts by weight or more, and may be about 0.7 parts by weight or more. By increasing the content of polyvalent organic acid (salt) relative to the content of abrasive grains, the dispersibility of the abrasive grains can be improved, and the effect of improving haze can be better exhibited. If the content of polyvalent organic acid (salt) relative to the content of abrasive grains is excessively high, the effect of improving haze can be reduced, so in some embodiments, the content of polyvalent organic acid (salt) relative to 100 parts by weight of abrasive grains is usually about 50 parts by weight or less, preferably about 20 parts by weight or less, more preferably about 10 parts by weight or less, and may be about 6 parts by weight or less. The content of the polyvalent organic acid (salt) relative to 100 parts by weight of the abrasive grains can be, for example, 5 parts by weight or less, and can also be 3 parts by weight or less.

[0072] In some embodiments of the polishing composition disclosed herein, the preferred content of the polyvalent organic acid (salt) can be specified by the relative relationship with the polyvinyl alcohol-based polymer contained in the polishing composition. Specifically, the content of the polyvinyl alcohol-based polymer in the polishing composition (A HM ) polyvalent organic acid (salt) content (A OA ) ratio (A OA / A HM ) is suitably set to, for example, about 0.01 or more on a weight basis, and from the viewpoint of obtaining better dispersibility, is preferably about 0.05 or more, more preferably about 0.1 or more. In addition, if the content of the polyvalent organic acid (salt) relative to the content of the polyvinyl alcohol-based polymer is excessively high, the effect of improving haze may decrease, so the above ratio (A OA / A HM The ratio (A) is usually about 10 or less, preferably about 3 or less, more preferably about 2 or less, and may be about 1 or less. OA / AHM ) can be, for example, 0.7 or less.

[0073] The preferred content of the polyvalent organic acid (salt) can also be determined from the relative relationship of the water-soluble polymer contained in the polishing composition (in an embodiment containing a combination of a polyvinyl alcohol-based polymer and another water-soluble polymer, the total amount of them). HT ) polyvalent organic acid (salt) content (A OA ) ratio (A OA / A HT The ratio (A) is preferably about 0.01 or more on a weight basis, and from the viewpoint of obtaining better dispersibility, is preferably about 0.05 or more, more preferably about 0.1 or more. The polishing composition disclosed herein uses, for example, a polyvinyl alcohol-based polymer in combination with another water-soluble polymer, and by appropriately selecting the other water-soluble polymer, the ratio (A OA / A HT ) is preferably about 0.2 or more, about 0.3 or more, about 0.4 or more, or about 0.5 or more. In addition, if the content of the polyvalent organic acid (salt) relative to the content of the water-soluble polymer is excessively high, the effect of improving haze may decrease. Therefore, the above ratio (A OA / A HT ) is usually suitably about 10 or less, preferably about 7 or less, more preferably about 5 or less, and may be about 3 or less.

[0074] In some embodiments of the polishing composition disclosed herein, the preferred content of the polyvalent organic acid (salt) can be specified by the increase ratio of electrical conductivity due to the inclusion of the polyvalent organic acid (salt). The increase ratio of electrical conductivity is expressed by the following formula: electrical conductivity increase ratio=EC1 / EC0;, based on the electrical conductivity EC1 [mS / cm] of the polishing composition disclosed herein and the electrical conductivity EC0 [mS / cm] of the composition obtained by removing the polyvalent organic acid (salt) from the polishing composition. The electrical conductivity increase ratio is usually 1 or more, typically more than 1. From the viewpoint of better exerting the effect of using the polyvalent organic acid (salt), in some embodiments, the electrical conductivity increase ratio may be, for example, 1.3 or more, 1.4 or more, 1.5 or more, or 1.7 or more. In addition, from the viewpoint of the dispersion stability of the polishing composition, the electrical conductivity increase ratio may be, for example, less than 10, and is usually appropriate to be less than 5. In some embodiments, the electrical conductivity increase ratio is preferably 3 or less, and may be, for example, less than 3, less than 2.5, or less than 2. In other embodiments, the electrical conductivity increase ratio may be, for example, more than 1 and less than 10, 1.3 or more and less than 7, 1.5 or more and less than 5, or 2 or more and less than 4. By setting the content of polyvalent organic acid (salt) so as to obtain such an electrical conductivity ratio, a polishing composition that effectively improves haze can be realized. The electrical conductivity can be measured by a conventional method under the condition of a liquid temperature of 25°C. For example, a conductivity meter manufactured by Horiba Ltd., model "DS-12", can be used as a measuring instrument. In the examples described later, the electrical conductivity was measured using the above-mentioned conductivity meter.

[0075] In some embodiments of the polishing composition disclosed herein, the electrical conductivity EC1 [mS / cm] of the polishing composition may be, for example, 0.03 mS / cm or more, 0.05 mS / cm or more, 0.08 mS / cm or more, 0.1 mS / cm or more, 0.11 mS / cm or more, or 0.12 mS / cm, from the viewpoint of the dispersibility of the abrasive grains. In addition, from the viewpoint of the dispersion stability of the polishing composition, the electrical conductivity EC1 [mS / cm] may be, for example, 0.30 mS / cm or less, 0.20 mS / cm or less, or 0.15 mS / cm or less. A polishing composition having an electrical conductivity that satisfies any of the upper and / or lower limits described above can effectively improve the haze on the surface of the polished object after polishing.

[0076] The polishing composition disclosed herein may also be preferably implemented in an embodiment in which the electrical conductivity EC1 [mS / cm] of the polishing composition is less than 0.12 mS / cm, less than 0.11 mS / cm, less than 0.10 mS / cm, or even less than 0.08 mS / cm. In such an embodiment in which the electrical conductivity EC1 is relatively low, it is preferable to use a combination of a polyvinyl alcohol-based polymer and another water-soluble polymer as the water-soluble polymer. In such an embodiment, the electrical conductivity EC1 [mS / cm] may be, for example, more than 0.01 mS / cm, and is advantageously more than 0.02 mS / cm from the viewpoint of the dispersion stability of the polishing composition, and may be more than 0.03 mS / cm or more than 0.04 mS / cm. A polishing composition having an electrical conductivity that satisfies any of the upper and / or lower limits described above can effectively improve the haze on the surface of the polished object after polishing.

[0077] The polishing composition disclosed herein may further contain, as necessary, one or more acids (salts) selected from the group consisting of inorganic acids (salts), monovalent organic acids (salts) and divalent organic acids (salts) in addition to the polyvalent organic acids (salts) as described above, as long as the effects of the present invention are not significantly hindered. The other acids (salts) may be used, for example, for the purpose of adjusting the pH of the polishing composition, adjusting the electrical conductivity, etc. The polishing composition disclosed herein may be preferably implemented in an embodiment that does not substantially contain any acids (salts) other than the polyvalent organic acids (salts) from the viewpoint of simplifying the composition and performance stability, etc. Here, substantially not containing any acids (salts) other than the polyvalent organic acids (salts) means that 95% by weight to 100% by weight (typically 98% by weight to 100% by weight) of the total amount of the content of the polyvalent organic acids (salts) and the content of the other acids (salts) is polyvalent organic acids (salts).

[0078] <Basic compounds> The polishing composition disclosed herein contains a basic compound. In this specification, the basic compound refers to a compound that dissolves in water and has the function of increasing the pH of the aqueous solution. As the basic compound, an organic or inorganic basic compound containing nitrogen, a basic compound containing phosphorus, an alkali metal hydroxide, an alkaline earth metal hydroxide, various carbonates and hydrogen carbonates, etc. can be used. Examples of the basic compound containing nitrogen include quaternary ammonium compounds, ammonia, amines (preferably water-soluble amines), etc. Examples of the basic compound containing phosphorus include quaternary phosphonium compounds. Such basic compounds can be used alone or in combination of two or more.

[0079] Specific examples of hydroxides of alkali metals include potassium hydroxide and sodium hydroxide. Specific examples of carbonates or hydrogen carbonates include ammonium hydrogen carbonate, ammonium carbonate, potassium hydrogen carbonate, potassium carbonate, sodium hydrogen carbonate, and sodium carbonate. Specific examples of amines include methylamine, dimethylamine, trimethylamine, ethylamine, diethylamine, triethylamine, ethylenediamine, monoethanolamine, N-(β-aminoethyl)ethanolamine, hexamethylenediamine, diethylenetriamine, triethylenetetramine, anhydrous piperazine, piperazine hexahydrate, 1-(2-aminoethyl)piperazine, N-methylpiperazine, guanidine, azoles such as imidazole and triazole, and the like. Specific examples of quaternary phosphonium compounds include quaternary phosphonium hydroxides such as tetramethylphosphonium hydroxide and tetraethylphosphonium hydroxide.

[0080] As the quaternary ammonium compound, a quaternary ammonium salt (typically a strong base) such as a tetraalkylammonium salt or a hydroxyalkyltrialkylammonium salt can be preferably used. The anion component in such a quaternary ammonium salt is, for example, OH - , F - , Cl - , Br - , I - , ClO4 - , BH4 - etc. In particular, a preferred example is one in which the anion is OH - Specific examples of quaternary ammonium hydroxides include tetraalkylammonium hydroxides such as tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, tetrapentylammonium hydroxide, and tetrahexylammonium hydroxide; hydroxyalkyltrialkylammonium hydroxides such as 2-hydroxyethyltrimethylammonium hydroxide (also called choline); and the like.

[0081] Among these basic compounds, at least one basic compound selected from, for example, alkali metal hydroxides, quaternary ammonium hydroxides, and ammonia can be preferably used. Among these, tetraalkylammonium hydroxides (e.g., tetramethylammonium hydroxide) and ammonia are more preferable, and ammonia is particularly preferable.

[0082] <Surfactant> The polishing composition disclosed herein may contain a surfactant as necessary. By adding a surfactant to the polishing composition, the haze on the surface of the object to be polished after polishing can be reduced better. Any of anionic, cationic, nonionic, and amphoteric surfactants can be used as the surfactant. Usually, anionic or nonionic surfactants can be preferably used. From the viewpoint of low foaming and ease of pH adjustment, nonionic surfactants are more preferable. For example, nonionic surfactants include oxyalkylene polymers such as polyethylene glycol, polypropylene glycol, and polytetramethylene glycol; polyoxyalkylene derivatives such as polyoxyethylene alkyl ethers, polyoxyethylene alkylphenyl ethers, polyoxyethylene alkylamines, polyoxyethylene fatty acid esters, polyoxyethylene glyceryl ether fatty acid esters, and polyoxyethylene sorbitan fatty acid esters (e.g., polyoxyalkylene adducts); and copolymers of multiple types of oxyalkylenes (e.g., diblock copolymers, triblock copolymers, random copolymers, and alternating copolymers). The surfactants may be used alone or in combination of two or more.

[0083] Specific examples of nonionic surfactants include block copolymers of ethylene oxide (EO) and propylene oxide (PO) (diblock copolymers, PEO (polyethylene oxide)-PPO (polypropylene oxide)-PEO type triblock copolymers, PPO-PEO-PPO type triblock copolymers, etc.), random copolymers of EO and PO, polyoxyethylene glycol, polyoxyethylene propyl ether, polyoxyethylene butyl ether, polyoxyethylene pentyl ether, polyoxyethylene hexyl ether, polyoxyethylene octyl ether, polyoxyethylene-2-ethylhexyl ether, polyoxyethylene nonyl ether, polyoxyethylene decyl ether, polyoxyethylene isodecyl ether, polyoxyethylene tridecyl ether, polyoxyethylene lauryl ether, polyoxyethylene cetyl ether, polyoxyethylene stearyl ether, polyoxyethylene isostearyl ether, polyoxyethylene octyl ... oleyl ether, polyoxyethylene phenyl ether, polyoxyethylene octylphenyl ether, polyoxyethylene nonylphenyl ether, polyoxyethylene dodecyl phenyl ether, polyoxyethylene styrenated phenyl ether, polyoxyethylene laurylamine, polyoxyethylene stearylamine, polyoxyethylene oleylamine, polyoxyethylene monolaurate, polyoxyethylene monostearate, polyoxyethylene distearate, polyoxyethylene monooleate, polyoxyethylene dioleate, polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalminate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan monooleate, polyoxyethylene sorbitan trioleate, polyoxyethylene sorbitan tetraoleate, polyoxyethylene castor oil, polyoxyethylene hydrogenated castor oil, and the like.Among them, preferred surfactants include block copolymers of EO and PO (particularly triblock copolymers of PEO-PPO-PEO type), random copolymers of EO and PO, and polyoxyethylene alkyl ethers (e.g., polyoxyethylene decyl ether).As the polyoxyethylene alkyl ether, those having an EO addition mole number of about 1 to 10 (e.g., about 3 to 8) can be preferably used.

[0084] The weight average molecular weight (Mw) of the surfactant is typically less than 2000, and is preferably 1900 or less (for example, less than 1800) from the viewpoint of filterability, washability, etc. In addition, the Mw of the surfactant is usually appropriate to be 200 or more from the viewpoint of surface activity, etc., and is preferably 250 or more (for example, 300 or more) from the viewpoint of haze reduction effect, etc. The more preferable range of the Mw of the surfactant may vary depending on the type of the surfactant. For example, when a polyoxyethylene alkyl ether is used as the surfactant, its Mw is preferably 1500 or less, and may be 1000 or less (for example, 500 or less). In addition, for example, when a PEO-PPO-PEO type triblock copolymer is used as the surfactant, its Mw may be, for example, 500 or more, may be 1000 or more, or may even be 1200 or more.

[0085] When the polishing composition disclosed herein contains a surfactant, its content is not particularly limited as long as it is within a range that does not significantly impair the effects of the present invention. Usually, from the viewpoint of cleaning properties, etc., it is appropriate to set the content of the surfactant to 20 parts by weight or less relative to 100 parts by weight of abrasive grains, preferably 15 parts by weight or less, and more preferably 10 parts by weight or less (for example, 6 parts by weight or less). From the viewpoint of better exerting the effect of using the surfactant, the content of the surfactant to 100 parts by weight of abrasive grains is appropriate to be 0.001 parts by weight or more, preferably 0.005 parts by weight or more, and may be 0.01 parts by weight or more or 0.05 parts by weight or more. When the polishing composition disclosed herein contains a surfactant, the weight ratio (w1 / w2) of the water-soluble polymer content w1 to the surfactant content w2 is not particularly limited and can be, for example, in the range of 0.01 to 200, usually preferably in the range of 0.05 to 100, and more preferably in the range of 0.1 to 70. Alternatively, from the viewpoint of simplifying the composition, etc., the polishing composition disclosed herein can also be preferably implemented in an embodiment that is substantially free of a surfactant.

[0086] <Water> As the water contained in the polishing composition disclosed herein, ion-exchanged water (deionized water), pure water, ultrapure water, distilled water, etc. can be preferably used. In order to prevent the action of other components contained in the polishing composition from being hindered as much as possible, the water used preferably has a total transition metal ion content of, for example, 100 ppb or less. For example, the purity of the water can be increased by removing impurity ions using an ion exchange resin, removing foreign matter using a filter, distillation, etc.

[0087] <Other ingredients> The polishing composition disclosed herein may further contain, as necessary, known additives that can be used in polishing compositions (typically polishing compositions used in the finish polishing step of silicon wafers), such as preservatives and antifungal agents, to the extent that the effects of the present invention are not significantly hindered. Examples of preservatives and antifungal agents include isothiazolinone compounds, paraoxybenzoic acid esters, phenoxyethanol, etc.

[0088] The polishing composition disclosed herein is preferably substantially free of oxidizing agents. If an oxidizing agent is contained in the polishing composition, for example, in polishing a silicon wafer, the surface of the silicon wafer is oxidized to form an oxide film, which increases the required polishing time. Specific examples of the oxidizing agent include hydrogen peroxide (H2O2), sodium persulfate, ammonium persulfate, and sodium dichloroisocyanurate. The polishing composition being substantially free of oxidizing agents means that the oxidizing agent is not intentionally contained at least. Therefore, a polishing composition that inevitably contains a small amount of oxidizing agent (for example, the molar concentration of the oxidizing agent in the polishing composition is 0.0005 mol / L or less, preferably 0.0001 mol / L or less, more preferably 0.00001 mol / L or less, particularly preferably 0.000001 mol / L or less) due to raw materials, manufacturing method, etc., can be included in the concept of a polishing composition that does not substantially contain an oxidizing agent as described here.

[0089] <ph> The pH of the polishing composition disclosed herein is typically 8.0 or more, preferably 8.5 or more, more preferably 9.0 or more. When the pH of the polishing composition is high, the polishing efficiency tends to improve. On the other hand, from the viewpoint of preventing dissolution of abrasive grains (e.g., silica particles) and suppressing the decrease in mechanical polishing action, the pH of the polishing composition is usually appropriate to be 12.0 or less, preferably 11.0 or less, more preferably 10.8 or less, and even more preferably 10.5 or less.

[0090] The pH can be determined by using a pH meter (for example, a glass electrode type hydrogen ion concentration indicator (model number F-23) manufactured by HORIBA, Ltd.) and performing three-point calibration using standard buffer solutions (phthalate pH buffer solution, pH: 4.01 (25° C.), neutral phosphate pH buffer solution, pH: 6.86 (25° C.), carbonate pH buffer solution, pH: 10.01 (25° C.)), then placing the glass electrode in the composition to be measured and measuring the value after stabilization for at least two minutes.

[0091] <Dispersibility> In the art disclosed herein, the degree of dispersibility of abrasive grains contained in the polishing composition can be determined, for example, by the following formula: Dispersity [nm]=(d 84 -d 16 ) / 2; The dispersibility can be calculated as a guideline. 84 is the particle diameter [nm] at the point where the cumulative curve of the particle size distribution is 84%, and d 16 is the particle diameter [nm] at the point where the cumulative curve of the particle size distribution is 16%. d 84 and d 16 can be obtained by measurement based on dynamic light scattering. For example, a dynamic light scattering particle size distribution measuring device manufactured by Microtrack Bell, trade name "Nanotrack UPA-UT151" or its equivalent can be used as the measuring device. The smaller the dispersibility value, the narrower the particle size distribution width. In general, when agglomeration of abrasive grains occurs, the particle size distribution width of the abrasive grains tends to become wider. From this, it can be said that a polishing composition with a smaller dispersibility value has better suppression of agglomeration of abrasive grains.

[0092] In some embodiments of the polishing composition disclosed herein, the above-mentioned dispersibility value is suitable to be less than 50 nm, preferably less than 20 nm, more preferably less than 15 nm, and even more preferably less than 10.8 nm.In a preferred embodiment, the above-mentioned dispersibility value is, for example, 10.5 nm or less.The above-mentioned dispersibility is 0 nm in principle, and from a practical viewpoint, it may be 1 nm or more, 3 nm or more, 5 nm or more, or 8 nm or more. The polishing composition disclosed herein, for example, in an embodiment further comprising another water-soluble polymer, can exhibit a good haze improving effect by having the above-mentioned dispersibility value of less than 14.2 nm. In such an embodiment, the above-mentioned dispersibility value may be, for example, 1 nm or more, 3 nm or more, 5 nm or more, 8 nm or more, 10 nm or more, or even 12 nm or more.

[0093] The above dispersibility value can be preferably applied to a polishing composition using abrasive grains (such as colloidal silica) having a BET diameter of 10 nm or more and 35 nm or less, more preferably 15 nm or more and less than 32 nm.

[0094] <Polishing liquid> The polishing composition disclosed herein is typically supplied to the surface of an object to be polished in the form of a polishing liquid containing the polishing composition, and is used to polish the object to be polished. The polishing liquid may be prepared, for example, by diluting any of the polishing compositions disclosed herein (typically diluting with water). Alternatively, the polishing composition may be used as a polishing liquid as it is. That is, the concept of the polishing composition in the technology disclosed herein includes both the polishing liquid (working slurry) that is supplied to an object to be polished and used to polish the object to be polished, and the concentrated liquid (original polishing liquid) that is diluted and used as a polishing liquid.

[0095] <Concentrate> The polishing composition disclosed herein may be in a concentrated form (i.e., in the form of a concentrated polishing liquid) before being supplied to an object to be polished. Such a concentrated polishing composition is advantageous from the viewpoints of convenience and cost reduction during production, distribution, storage, etc. The concentration ratio is not particularly limited, and can be, for example, about 2 to 100 times in volume conversion, and is usually about 5 to 50 times (for example, about 10 to 40 times). Such a concentrated solution can be used in such a manner that it is diluted at a desired timing to prepare a polishing solution (working slurry) and the polishing solution is supplied to an object to be polished. The dilution can be performed, for example, by adding water to the concentrated solution and mixing it.

[0096] The content of the abrasive grains in the concentrated liquid can be, for example, 25% by weight or less. From the viewpoint of dispersion stability and filterability of the polishing composition, the content is usually preferably 20% by weight or less, more preferably 15% by weight or less. In a preferred embodiment, the content of the abrasive grains may be 10% by weight or less, or may be 5% by weight or less. In addition, from the viewpoint of convenience and cost reduction during production, distribution, storage, etc., the content of the abrasive grains in the concentrated liquid can be, for example, 0.1% by weight or more, preferably 0.5% by weight or more, more preferably 0.7% by weight or more, and even more preferably 1% by weight or more.

[0097] <Preparation of Polishing Composition> The polishing composition used in the technology disclosed herein may be a one-component type or a multi-component type including a two-component type. For example, the polishing composition may be configured to prepare a polishing liquid by mixing a part A containing at least abrasive grains and a part B containing at least a part of the remaining components, and mixing and diluting them at an appropriate timing as necessary.

[0098] The method of preparing the polishing composition is not particularly limited.For example, it is advisable to use a well-known mixing device such as a blade type agitator, an ultrasonic disperser, a homomixer, etc. to mix each component that constitutes the polishing composition.The manner of mixing these components is not particularly limited, and for example, all components may be mixed at once, or may be mixed in a suitably set order.

[0099] <Application> The polishing composition disclosed herein can be applied to polishing objects having various materials and shapes.The material of the object to be polished can be, for example, metals or semimetals such as silicon, aluminum, nickel, tungsten, copper, tantalum, titanium, stainless steel, or alloys thereof; glassy materials such as quartz glass, aluminosilicate glass, and glassy carbon; ceramic materials such as alumina, silica, sapphire, silicon nitride, tantalum nitride, and titanium carbide; compound semiconductor substrate materials such as silicon carbide, gallium nitride, and gallium arsenide; resin materials such as polyimide resin; and the like.The object to be polished can be made of a plurality of these materials.

[0100] The polishing composition disclosed herein can be particularly preferably used for polishing a surface made of silicon (typically, polishing a silicon wafer). A typical example of the silicon wafer referred to here is a silicon single crystal wafer, for example, a silicon single crystal wafer obtained by slicing a silicon single crystal ingot.

[0101] The polishing composition disclosed herein can be preferably applied to a polishing step of an object to be polished (e.g., silicon wafer). The object to be polished may be subjected to a general treatment that can be applied to the object to be polished in a step upstream of the polishing step, such as lapping or etching, before the polishing step with the polishing composition disclosed herein.

[0102] The polishing composition disclosed herein is effective for use in the finishing step of an object to be polished (e.g., silicon wafer) or in the polishing step immediately preceding the finishing step, and is particularly preferably used in the finishing polishing step. Here, the finishing polishing step refers to the final polishing step in the manufacturing process of the object (i.e., a step after which no further polishing is performed).

[0103] <Polishing> The polishing composition disclosed herein can be used for polishing an object to be polished, for example, in an embodiment including the following operations. A preferred embodiment of a method for polishing an object to be polished (e.g., a silicon wafer) using the polishing composition disclosed herein is described below. That is, a polishing liquid containing any one of the polishing compositions disclosed herein is prepared. The preparation of the polishing liquid may include adjusting the concentration (e.g., diluting) of the polishing composition, adjusting the pH, and the like to prepare the polishing liquid. Alternatively, the polishing composition may be used as it is as the polishing liquid.

[0104] Next, the polishing liquid is supplied to the object to be polished, and the object is polished by a conventional method. For example, when performing finish polishing of a silicon wafer, typically, the silicon wafer that has been subjected to the lapping process is set in a general polishing device, and the polishing liquid is supplied to the surface of the silicon wafer to be polished through the polishing pad of the polishing device. Typically, while continuously supplying the polishing liquid, the polishing pad is pressed against the surface of the silicon wafer to be polished, and the two are moved relatively (for example, rotated). Through such a polishing process, polishing of the object to be polished is completed.

[0105] The polishing pad used in the polishing step is not particularly limited. For example, polishing pads of polyurethane foam type, nonwoven fabric type, suede type, etc. can be used. Each polishing pad may contain abrasive grains or may not contain abrasive grains. Usually, a polishing pad that does not contain abrasive grains is preferably used.

[0106] The object to be polished that has been polished using the polishing composition disclosed herein is typically washed. The washing can be performed using an appropriate washing liquid. The washing liquid to be used is not particularly limited, and for example, SC-1 washing liquid (a mixture of ammonium hydroxide (NH4OH), hydrogen peroxide (H2O2), and water (H2O)) that is common in the field of semiconductors, etc., SC-2 washing liquid (a mixture of hydrochloric acid (HCl), H2O2, and H2O), etc. can be used. The temperature of the washing liquid can be, for example, in the range of room temperature (typically about 15°C to 25°C) or higher, up to about 90°C. From the viewpoint of improving the washing effect, a washing liquid of about 50°C to 85°C can be preferably used. EXAMPLES

[0107] Some examples of the present invention will be described below, but it is not intended that the present invention be limited to those shown in these examples. In the following description, "parts" and "%" are by weight unless otherwise specified.

[0108] <Experimental Example 1> <Preparation of Polishing Composition> (Examples 1 to 3) Abrasive grains, water-soluble polymer, acid (salt), basic compound, surfactant and deionized water were mixed to prepare a polishing composition according to each example. Colloidal silica (average primary particle size: 25 nm) was used as the abrasive grains, and its content was 0.175%. Polyvinyl alcohol (non-modified PVA) with a weight average molecular weight (Mw) of about 70000 and a saponification degree of 98% or more was used as the water-soluble polymer, and its content was 0.00875%. Ammonia was used as the basic compound, and its content was 0.005%. Polyoxyethylene decyl ether (C10EO5) with 5 moles of ethylene oxide added was used as the surfactant, and its content was 0.00015%. Triammonium citrate was used as the acid (salt) in the amount shown in Table 1.

[0109] Example 4 In this example, triammonium citrate was replaced with citric acid in the amount shown in Table 1. In other respects, the polishing composition of this example was prepared in the same manner as in Example 1.

[0110] Example 5 In this example, triammonium citrate was replaced with butanetetracarboxylic acid in the amount shown in Table 1. In other respects, the polishing composition of this example was prepared in the same manner as in Example 1.

[0111] Comparative Example 1 A polishing composition according to this example was prepared in the same manner as in Example 1, except that triammonium citrate was omitted from the composition of Example 1.

[0112] (Comparative Examples 2 to 5) Polishing compositions according to Comparative Examples 2 to 5 were prepared in the same manner as in Example 1, except that the types and amounts of acids (salts) shown in Table 1 were used instead of triammonium citrate.

[0113] <Dispersion measurement> The particle size distribution of the prepared polishing composition was measured using a dynamic light scattering particle size distribution measuring device manufactured by Microtrac-Bell, product name "Nanotrac UPA-UT151". The particle diameter (nm) at the point where the cumulative curve is 84% ​​was defined as d 84 The particle size (nm) at the point where the cumulative curve is 16% is d 16 Then, the following formula: Dispersity [nm]=(d 84 -d 16 ) / 2; The dispersibility was calculated by the above method. The results are shown in Table 1. Table 1 also shows the electrical conductivity measured by the above method. The polishing composition of Comparative Example 1 had a pH of 10.0, and the polishing compositions of the other examples all had a pH in the range of 9.0 to 9.9.

[0114] <Silicon wafer polishing> The polishing target was a commercially available silicon single crystal wafer with a diameter of 200 mm (conductivity type: P type, crystal orientation: <100> Silicon wafers (free of crystal originated particles (COP)) were prepared by pre-polishing under the following polishing condition 1. Pre-polishing was performed using a polishing solution containing 1.0% abrasive grains (colloidal silica with a BET diameter of 35 nm) and 0.068% potassium hydroxide in deionized water.

[0115] [Polishing conditions 1] Polishing device: Single-wafer polishing device model "PNX-322" manufactured by Okamoto Machine Tool Works, Ltd. Polishing load: 15kPa Rotation speed of the platen: 30 rpm Head (carrier) rotation speed: 30 rpm Polishing pad: Fujibo Ehime Co., Ltd. Product name "FP55" Pre-polishing liquid supply rate: 550mL / min Temperature of pre-polishing solution: 20℃ Plate cooling water temperature: 20℃ Polishing time: 3min

[0116] The polishing compositions according to the respective examples prepared above were used as polishing liquids to polish the silicon wafers after the pre-polishing under the following polishing conditions 2.

[0117] [Polishing conditions 2] Polishing device: Single-wafer polishing device model "PNX-322" manufactured by Okamoto Machine Tool Works, Ltd. Polishing load: 15kPa Rotation speed of the platen: 30 rpm Head (carrier) rotation speed: 30 rpm Polishing pad: Fujibo Ehime Co., Ltd. Product name "POLYPAS27NX" Polishing fluid supply rate: 400mL / min Polishing solution temperature: 20℃ Plate cooling water temperature: 20℃ Polishing time: 4 min

[0118] The polished silicon wafer was removed from the polishing apparatus and washed with a cleaning solution of NH4OH (29%):H2O2 (31%):deionized water (DIW) = 1:1:12 (volume ratio) (SC-1 washing). Specifically, first and second washing tanks were prepared, and the above-mentioned cleaning solution was contained in each of these washing tanks and maintained at 60°C. The polished silicon wafer was immersed in the first washing tank for 5 minutes, passed through a rinse tank in which it was immersed in ultrapure water and subjected to ultrasonic waves, immersed in the second washing tank for 5 minutes, passed through a rinse tank in which it was immersed in ultrapure water and subjected to ultrasonic waves, and then dried using a spin dryer.

[0119] <Haze measurement> After cleaning, the silicon wafer surface was inspected using a wafer inspection device manufactured by KLA Tencor, called "Surfscan SP2 XP The haze (ppm) was measured in DWO mode using a 350 psi meter. The results were converted into relative values ​​(haze ratios) with the haze value for Comparative Example 1 taken as 100%, and are shown in Table 1. If the haze ratio is less than 100%, it can be said that the haze improvement effect can be significantly confirmed.

[0120] [Table 1]

[0121] As shown in Table 1, in Examples 1 to 5 in which a polyvalent organic acid (salt) was used, a significant haze improvement effect was confirmed compared to Comparative Example 1. In these Examples, the dispersibility (nm) value of the polishing composition was clearly lower than in Comparative Example 1, which is considered to have contributed to the improvement in haze. On the other hand, in Comparative Examples 2 to 5 in which a monovalent or divalent acid (salt) was used, no effect of improving haze was observed compared to Comparative Example 1.

[0122] The dispersibility of the polishing composition of Reference Example 1, which was prepared in the same manner as in Example 1 except that polyvinyl alcohol was changed to hydroxyethyl cellulose (HEC), was 51.2 nm, and the dispersibility of the polishing composition of Reference Example 2, which was prepared in the same manner as in Reference Example 1 except that triammonium citrate was not used, was 23.3 nm. That is, in the polishing composition in which HEC was used alone as the water-soluble polymer, unlike the results shown in Table 1, no improvement in dispersibility due to the polyvalent organic acid (salt) was observed.

[0123] <Experimental Example 2> <Preparation of Polishing Composition> Example 6 As the water-soluble polymer, polyvinyl alcohol (non-modified PVA) having a weight average molecular weight (Mw) of about 70000 and a saponification degree of 98% or more and polyacryloylmorpholine (PACMO) having a weight average molecular weight (Mw) of about 350,000 were used. The content of the polyvinyl alcohol was 0.00263%, and the content of the polyacryloylmorpholine was 0.00560%. The content of C10EO5 was 0.00007%, and the content of triammonium citrate was 0.0042%. The polishing composition according to this example was prepared in the same manner as in Example 1.

[0124] Comparative Example 6 A polishing composition according to this example was prepared in the same manner as in Example 6, except that triammonium citrate was omitted from the composition of Example 6.

[0125] <Evaluation> The prepared polishing composition was subjected to dispersibility measurement, silicon wafer polishing, and haze measurement in the same manner as in the above-mentioned Experimental Example 1. The results are shown in Table 2. The haze value obtained for Example 6 was converted into a relative value (haze ratio) with the haze value for Comparative Example 6 taken as 100%. The results are shown in Table 2.

[0126] [Table 2]

[0127] As shown in Table 2, in comparison between Example 6, which is a polishing composition containing a combination of a polyvinyl alcohol-based polymer and other water-soluble polymers, and Comparative Example 6, a clear haze improvement effect was confirmed by adding a polyvalent organic acid (salt) to the composition of Comparative Example 6.

[0128] Although the specific examples of the present invention have been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and changes of the specific examples exemplified above.< / ph>

Claims

1. A polishing composition for use in a finish polishing step of a silicon wafer, comprising: The polishing agent includes an abrasive grain, a polyvinyl alcohol-based polymer as a water-soluble polymer, a basic compound, and water, Further containing a trivalent or higher polyvalent organic acid (salt), The polishing composition, wherein a ratio (A OA / A HM ) of the content (A OA ) of the polyvalent organic acid (salt) to the content (A HM ) of the polyvinyl alcohol-based polymer is 0.01 or more and 10 or less on a weight basis.

2. The polishing composition according to claim 1 , wherein the polyvalent organic acid (salt) comprises a trivalent or higher polyvalent carboxylic acid (salt).

3. The polishing composition according to claim 1 or 2, wherein the polyvalent organic acid (salt) comprises an ammonium salt of a trivalent or higher polyvalent organic acid.

4. The following formula: Dispersity [nm] = (d 84 -d 16 ) / 2 (wherein d in the formula 84 represents the particle diameter [nm] at the point where the cumulative curve of the particle size distribution is 84%, and d 16 represents the particle diameter [nm] at the point where the cumulative curve of the particle size distribution is 16%; The polishing composition according to claim 1 , wherein the dispersibility is less than 10.8 nm.

5. The water-soluble polymer further includes a water-soluble polymer other than the polyvinyl alcohol-based polymer, The following formula: Dispersity [nm] = (d 84 -d 16 ) / 2 (wherein d in the formula 84 represents the particle diameter [nm] at the point where the cumulative curve of the particle size distribution is 84%, and d 16 represents the particle diameter [nm] at the point where the cumulative curve of the particle size distribution is 16%; The polishing composition according to claim 1 , wherein the dispersibility is less than 14.2 nm.

6. The polishing composition according to claim 1 , wherein an increase ratio of electrical conductivity due to the inclusion of the polyvalent organic acid (salt) is 3 or less.

7. The polishing composition according to any one of claims 1 to 6, having a pH of 8 to 12.

8. The weight average molecular weight of the polyvinyl alcohol-based polymer is 10×10 4 The polishing composition according to claim 1 , wherein:

9. The polishing composition according to claim 1 , further comprising a surfactant.

10. The polishing composition according to claim 1 , wherein the abrasive grains are silica grains.

Citation Information

Patent Citations

  • Barium titanate chemico-mechanical polishing aqueous composition and its application

    CN102786879A

  • Aluminum oxide polishing solution used for polishing sapphire and preparation method thereof

    CN108239484A

  • Device for automatically controlling operatorless lighthouse

    JP1979074400A

  • Article transfer detector

    JP1985029895A

  • Pretreatment of starting material for sintering

    JP1985050125A