Spherical activated carbon and its manufacturing method
A simple method using an organic binder with a glass transition temperature of 30°C or higher enables the production of spherical activated carbon with small particle size and high sphericity, addressing production complexity and cost issues while improving filter performance.
Patent Information
- Application Number
- JP2020052080
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-24
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2040-03-24
AI Technical Summary
Existing methods for producing spherical activated carbon face challenges in achieving small particle sizes and high sphericity, often requiring complex processes and high-temperature treatments, which increase production costs and limit the material's versatility in applications like cabin and cigarette filters.
A method involving the granulation of activated carbon with an organic binder having a glass transition temperature of 30°C or higher, followed by shaping and heat-treating, results in spherical activated carbon with a small particle size and high sphericity, using binders like polyethylene and polypropylene to maintain the spherical shape during granulation.
The method allows for the production of spherical activated carbon with a particle size of 0.3 to 0.6 mm and sphericity of 1.10 or less, enhancing its durability and reducing fine powder generation, making it suitable for filters with improved air permeability and abrasion resistance.
Smart Images

Figure 0007588469000002 
Figure 0007588469000003 
Figure 0007588469000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a spherical activated carbon and a method for producing the same. [Background technology]
[0002] In the chemical industry, activated carbon is used in a wide range of applications, including separation processes, purification, catalysts, solvent recovery, wastewater treatment related to global environmental pollution issues, pollution control, and medical applications.
[0003] Small particle size activated carbon is often used as a filter by inserting it between layers of fiber sheets, cloth, etc. In this case, ensuring breathability is important, and activated carbon that can reduce pressure loss, has good abrasion resistance, and generates little fine powder is preferred.
[0004] In such cases, the activated carbon used should be spherical rather than crushed, as this will reduce the amount of fine powder produced during use. For this reason, there is a demand for activated carbon with a small particle size and low sphericity (close to a perfect sphere).
[0005] For example, patent documents 1 and 2 propose spherical activated carbon and its manufacturing method. Patent document 1 provides spherical activated carbon with a diameter of 1.5 mm or more and 4.0 mm or less, and patent document 2 relates to spherical activated carbon with an average particle diameter in the range of 0.6 mm to 10 mm. Patent document 3 states that spherical activated carbon with an average particle diameter of 0.1 mm to 1.5 mm is available. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2018 / 116947 [Patent Document 2] JP 2006-083052 A [Patent Document 3] JP 2005-119947 A Summary of the Invention [Problem to be solved by the invention]
[0007] The method of Patent Document 1 produces activated carbon with an aspect ratio of 0.7 or more. However, the activated carbon produced has an average particle size of 1.5 mm or more and 4.0 mm or less, and further reduction in particle size is required. Also, in Patent Document 2, the activated carbon produced has an average particle size of 0.6 to 10 mm, and further reduction in particle size is required.
[0008] Furthermore, in the method of Patent Document 3, an isotropic porous spherical pitch obtained by a mild process using heavy hydrocarbon oils such as petroleum tar, coal tar, and ethylene bottom oil as raw materials is infusible, and then carbonized and activated to obtain spherical activated carbon with good properties, but it is necessary to undergo high-temperature treatment (about 430 to 600°C) in the above-mentioned multiple steps, which is complicated and also poses production cost issues. In addition, since the starting raw materials are limited, even if the activation degree is changed, the pore distribution becomes uniform to a certain extent, and when considering various gas phase and liquid phase adsorption issues and application development, it is not possible to respond and is limited.
[0009] The present invention is intended to solve these problems, and has an object to provide spherical activated carbon having a small particle size and high sphericity by a simple method. [Means for solving the problem]
[0010] The present inventors conducted intensive research to solve the above problems and found that it is possible to provide spherical activated carbon with a small particle size and high sphericity in a simple manner by granulating an activated carbon composition containing activated carbon and an organic binder having a glass transition temperature of 30° C. or higher. Based on this finding, the present inventors conducted further research and completed the present invention. That is, the present invention includes the following configurations.
[0011] Item 1. Spherical activated carbon comprising a granulated activated carbon composition containing activated carbon and an organic binder having a glass transition temperature of 30°C or higher.
[0012] Item 2. The spherical activated carbon according to Item 1, having an average particle size of 0.3 mm or more and less than 0.6 mm.
[0013] Item 3. The spherical activated carbon according to item 1 or 2, having a sphericity of 1.10 or less.
[0014] Item 4. The spherical activated carbon according to any one of Items 1 to 3, having an MS hardness of 70.0% or more.
[0015] Item 5. A method for producing a spherical activated carbon according to any one of items 1 to 4, A production method comprising a step of granulating an activated carbon composition comprising activated carbon and an organic binder having a glass transition temperature of 30°C or higher.
[0016] Item 6. The method according to Item 5, wherein the granulation temperature is 0°C or higher and lower than 30°C.
[0017] Item 7. The method according to item 5 or 6, wherein the organic binder has an average particle size of 10 to 300 nm.
[0018] Item 8. The method according to any one of Items 5 to 7, wherein the organic binder has a viscosity of 1 to 20 mPa / s.
[0019] Item 9. The method according to any one of Items 5 to 8, wherein the granulation step is a step of spraying water onto the activated carbon composition, forming the composition into a spherical activated carbon shape, and then heat-treating the resulting product.
[0020] Item 10. A cabin filter using the spherical activated carbon according to any one of items 1 to 4.
[0021] Item 11. A cigarette filter using the spherical activated carbon according to any one of items 1 to 4.
[0022] Item 12. A cigarette comprising the cigarette filter according to item 11. Effect of the Invention
[0023] According to the present invention, it is possible to provide spherical activated carbon having a small particle size and high sphericity by a simple method. [Brief description of the drawings]
[0024] [Figure 1] 1 is a photograph showing the appearance of the spherical activated carbon obtained in Example 1. [Diagram 2] 1 is a photograph showing the appearance of the spherical activated carbon obtained in Comparative Example 1. [Diagram 3] 1 is a photograph showing the appearance of a container used in measuring MS hardness. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] In this specification, "containing" is a concept that encompasses all of "comprise," "consist essentially of," and "consist only of." In addition, in this specification, when a numerical range is shown as "A to B," it means A or more and B or less.
[0026] The spherical activated carbon of the present invention is made of a granulated product of an activated carbon composition containing activated carbon and an organic binder having a glass transition temperature of 30° C. or higher. Specifically, it is obtained by a production method including a step of granulating an activated carbon composition containing activated carbon and an organic binder having a glass transition temperature of 30° C. or higher.
[0027] Since the spherical activated carbon of the present invention is obtained as a small-sized spherical activated carbon, the sphericity is greatly influenced by the fusion state of the organic binder present between the activated carbon particles. By controlling this fusion state by the glass transition temperature of the organic binder, it is possible to obtain a small-sized spherical activated carbon with high sphericity.
[0028] There are no particular limitations on the activated carbon as long as it is in powder form. forActivated carbon obtained from various raw materials such as coal, coconut shell, wood, and lignin can be used, and activated carbon products such as steam activated products, carbon dioxide activated products, and chemically activated products using phosphoric acid, zinc chloride, alkali metals, etc. can be used. These activated carbons can be used alone or in combination of two or more types.
[0029] The activated carbon applicable to the present invention may be in any form, such as powder, granules, or crushed carbon, but a powder having fine pores (activated carbon powder) is preferred because the particles are easily rearranged and easily bound by a binder.
[0030] The average particle size of the activated carbon powder is not particularly limited, and from the viewpoint of the average particle size and sphericity of the obtained spherical activated carbon, it is, for example, preferably 1 μm to 10 mm, more preferably 5 μm to 1 mm, and even more preferably 10 to 100 μm. The average particle size of the activated carbon powder is measured by a laser diffraction particle size distribution measuring device (Microtrac MT3300EXII, manufactured by Microtrac-Bell Co., Ltd.), and the particle size at 50% cumulative volume is defined as the average particle size.
[0031] The specific surface area of the activated carbon is not particularly limited, and is, for example, 500 to 2600 m from the viewpoint of the average particle size and sphericity of the obtained spherical activated carbon. 2 / g is preferable, and 600 to 2400m 2 / g is more preferable, and 800 to 2000m 2 The specific surface area of the activated carbon is measured by the Cranston-Inkley (CI) method.
[0032] The pore volume of the activated carbon is not particularly limited, and is preferably, for example, 0.10 to 1.70 mL / g, more preferably 0.20 to 1.50 mL / g, and even more preferably 0.30 to 1.00 mL / g, from the viewpoint of the average particle size and sphericity of the obtained spherical activated carbon. The pore volume of the activated carbon with a diameter of 30 nm or less is measured using a specific surface area / pore distribution measuring device (Belsorp miniII, manufactured by Microtrack-Bell Co., Ltd.), and a nitrogen adsorption isotherm of the activated carbon at liquid nitrogen temperature is prepared and calculated by the CI method.
[0033] From the viewpoint of appropriately adjusting the binding strength of the organic binder to improve sphericity and hardness, the amount of activated carbon added in the activated carbon composition is preferably 70 to 97 mass%, more preferably 80 to 96 mass%, and even more preferably 85 to 95 mass%, relative to 100 mass% of the total solid content of the activated carbon composition.
[0034] The glass transition temperature is the temperature at which the molecular backbone starts or stops rotating or vibrating (micro-Brownian motion) while the relative positions of the polymer molecules do not change. It is called the glass transition temperature because below this temperature the polymer freezes into a glassy state.
[0035] It is generally known that polymers form a continuous film at temperatures above their glass transition temperature, and that the glass transition temperature and the minimum film formation temperature are almost the same. Since molding is also affected by the fusion state of the organic binder present between activated carbon particles, the sphericity depends on the glass transition temperature of the organic polymer.
[0036] In other words, if an organic binder with a glass transition temperature above the granulation temperature is used, it will be in a glassy state in the usage environment and will tend to exist as dots between activated carbon particles without fusing together. This allows the particles to compact while maintaining their spherical shape during the granulation process, facilitating particle growth.
[0037] From the above, it is preferable to adjust the glass transition temperature of the organic binder to be equal to or higher than the granulation temperature in terms of the average particle size and sphericity of the resulting spherical activated carbon. Specifically, the glass transition temperature of the organic binder is 30° C. or higher, preferably 30 to 100° C., and more preferably 30 to 70° C. The glass transition temperature of the organic binder is measured using a DSC7020 (differential scanning calorimeter, manufactured by Seiko Instruments Inc.). Note that organic binders that do not have a glass transition temperature are outside the scope of the present invention.
[0038] The organic binder is not particularly limited, but by having a suitable viscosity, it is easy to prevent the shape of the obtained spherical activated carbon from becoming distorted. Therefore, from the viewpoint of the average particle size and sphericity of the obtained spherical activated carbon, the viscosity of the organic binder is, for example, preferably 1 to 20 mPa / s, more preferably 3 to 19 mPa / s, and even more preferably 5 to 18 mPa / s. The average particle size of the organic binder is measured by a BL type viscometer at 25°C, one minute after stirring.
[0039] The average particle size of the organic binder is not particularly limited, and from the viewpoint of the average particle size and sphericity of the obtained spherical activated carbon, it is, for example, preferably 10 to 300 nm, more preferably 15 to 270 nm, and even more preferably 20 to 250 nm. The average particle size of the organic binder is measured by nanoSAQLA (multi-analyte nanoparticle measurement system, manufactured by Otsuka Electronics Co., Ltd.).
[0040] The organic binder (resin) that can be used in the present invention having the above conditions may be a thermoplastic resin or a thermosetting resin. Examples of such organic binders include polyethylene, polypropylene, acrylonitrile-styrene copolymer (AS) resin, acrylonitrile-butadiene-styrene copolymer (ABS) resin, polycarbonate, methacrylic resin, polyethylene terephthalate (PET), polystyrene, polyacetal, modified polyphenylene ether, polyvinyl chloride, polyvinyl acetate, ethylene-vinyl acetate resin, vinylidene chloride resin, polyester resin, polyamide, polyphenylene sulfide (PPS) resin, acrylic resin, fluorine resin, thermoplastic elastomer, polymethylpentene, polyimide resin, acrylonitrile-butadiene latex, styrene-butadiene latex, acrylate latex, phenol resin, urea resin, epoxy resin, cyanate resin, diallyl phthalate resin, silicone resin, bismaleimide resin, benzoxazine resin, unsaturated polyester resin, melamine resin, polyurethane, etc. These organic binders can be used alone or in combination of two or more. The organic binder is not limited to being in a solid state, but can also be used in a form containing a solvent, such as a solution, a dispersion, or a suspension.
[0041] The amount of the organic binder added in the activated carbon composition is preferably 3 to 30% by mass, more preferably 4 to 20% by mass, and even more preferably 5 to 15% by mass, based on the total amount of solids in the activated carbon composition being 100% by mass, from the viewpoint of appropriately adjusting the binding strength of the organic binder to improve sphericity and hardness. The organic binder can also be used in a form containing a solvent such as a solution, dispersion, or suspension, and in that case, it is preferable to adjust the content of the solids to be within the above range.
[0042] Various additives can also be added to the activated carbon composition. Examples of such additives include polycarboxylic acid as a dispersant, ester wax, fatty acid, and fatty acid amide as a lubricant, and carboxymethylcellulose, hard pitch, soft pitch, pulp waste liquor (main component is lignin sulfonate), and crystalline cellulose as a binder. The content of these additives is preferably within a range that does not impair the effects of the present invention, and is preferably 0 to 10% by mass, more preferably 0.01 to 5% by mass, and even more preferably 0.1 to 3% by mass, based on the total amount of solids in the activated carbon composition being 100% by mass.
[0043] In addition, a small amount of water can be added to the activated carbon composition before it is put into the granulator. This allows the spaces between the activated carbon particles to be filled with water, making it easier for the particles to be thoroughly kneaded together and improving the packing density. The amount of water added can be appropriately set according to the required properties.
[0044] In the present invention, the spherical activated carbon of the present invention can be obtained by subjecting the above-mentioned activated carbon composition to a granulation process.
[0045] The granulator used is not particularly limited, and molding can be performed using a general granulator such as an agitation granulator, compression granulator, spray granulator, rolling granulator, extrusion granulator, or marumerizer.
[0046] The granulation step that can be employed is not particularly limited, but may be, for example, a step of spraying water onto the activated carbon composition, forming it into the shape of spherical activated carbon, and then heat-treating it.
[0047] The spraying of water is not particularly limited, and can be carried out, for example, by a spray, a mister, a sprayer, etc. The total amount of water sprayed can be appropriately set depending on the required properties.
[0048] There is no particular limitation on the method for forming the activated carbon into a spherical shape after spraying with water, and any conventional method can be used.
[0049] From the viewpoints of granulation efficiency, sphericity, average particle size, hardness, etc., the heat treatment temperature after molding is preferably equal to or lower than the thermal decomposition temperature of the organic binder, preferably 50 to 200°C, more preferably 70 to 180°C, and even more preferably 80 to 150°C.
[0050] The heat treatment time after molding can be a time that allows spherical activated carbon to be obtained that has a sufficiently small particle size and high sphericity, and is preferably 10 minutes to 10 hours, more preferably 30 minutes to 5 hours, and even more preferably 1 to 4 hours, from the viewpoints of granulation efficiency, sphericity, average particle size, hardness, etc. In this case, it is preferable to adjust the moisture content of the obtained spherical activated carbon to 10 mass% or less, particularly 5 mass% or less.
[0051] As described above, in the present invention, the spherical activated carbon can be produced by a simple method without sintering, and the production cost can be reduced.
[0052] The spherical activated carbon of the present invention thus obtained can have a small particle size. Specifically, the average particle size of the spherical activated carbon of the present invention is preferably 0.3 mm or more and less than 0.6 mm, more preferably 0.32 to 0.58 mm, and even more preferably 0.35 to 0.55 mm. The average particle size of the spherical activated carbon of the present invention is calculated by sieving using a rotor and a sieve in accordance with JIS K1474 (2014) and calculating the mass average particle size.
[0053] The spherical activated carbon of the present invention thus obtained can have a uniform spherical shape. Specifically, the sphericity of the spherical activated carbon of the present invention is preferably 1.10 or less, more preferably 1.00 to 1.09, and even more preferably 1.02 to 1.08. The sphericity of the spherical activated carbon of the present invention is measured by calculating the longest diameter (a) / shortest diameter (b) from an image taken with a digital microscope.
[0054] The spherical activated carbon of the present invention thus obtained can have a high hardness. Specifically, the MS hardness of the spherical activated carbon of the present invention is preferably 70.0% or more, more preferably 71.0 to 80.0%, and even more preferably 72.0 to 75.0%. The MS hardness of the spherical activated carbon of the present invention is measured by placing the spherical activated carbon together with 10 steel balls in a container shown in FIG. 3, rotating the container at 25 revolutions per minute for 40 minutes, separating the activated carbon from the steel balls, and sieving the activated carbon through a 0.212 mm sieve. [Mass on sieve] x 100 (%) / [Mass on sieve + Mass under sieve] This method is used to determine durability against impact and friction.
[0055] The spherical activated carbon of the present invention as described above has excellent properties such as a small particle size, high sphericity, and high hardness, and can be inserted between layers of a fiber sheet, cloth, etc. and used as a filter. In particular, the spherical activated carbon of the present invention has a small size and high sphericity, so that even if friction occurs, there are few angular parts and therefore it is difficult for fine powder to be generated. For this reason, it is useful for cigarette filters and cabin filters. EXAMPLES
[0056] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the embodiments of the examples.
[0057] In the following examples and comparative examples, the glass transition temperature of the organic binder was measured using a DSC7020 (differential scanning calorimeter, manufactured by Seiko Instruments Inc.), the viscosity was measured at 25°C using a BL viscometer, and the average particle size was measured using a nanoSAQLA (multi-analyte nanoparticle measurement system, manufactured by Otsuka Electronics Co., Ltd.), and the particle size at 50% cumulative volume was defined as the average particle size.
[0058] Example 1 The coconut shell activated carbon was adjusted to an average particle size of 40 μm (166 mesh pass, 98% by mass). The specific surface area of the activated carbon calculated by the CI method was 1086 m 2 / g, and the pore volume was 0.47 mL / g.
[0059] While operating a granulator (manufactured in-house), the organic binder, the activated carbon, and an appropriate amount of water were mixed in advance. At this time, as the organic binder in the mixture, a vinyl chloride emulsion (Vinyblan 700 manufactured by Nissin Chemical Industry Co., Ltd., solid content concentration 30 mass%) was blended in such an amount that it was 6.0 mass% based on the total solid content of the mixture being 100 mass%, and the activated carbon was blended in such an amount that it was 94.0 mass% based on the total solid content of the mixture being 100 mass%.
[0060] Thereafter, the crushed mixture was placed in a granulator and granulated at 26° C. while spraying an appropriate amount of water. The water spray rate was 20 mL / min.
[0061] The mixture was then molded into spherical activated carbon and dried at 115°C for 3 hours or more to reduce the moisture content of the molded product to less than 5% by mass. The molded product was then sieved using a sieve selected according to its size. A photograph of the appearance of the obtained spherical activated carbon is shown in Figure 1.
[0062] Example 2 A spherical activated carbon of Example 2 was obtained in the same manner as in Example 1, except that an ethylene-vinyl chloride copolymer resin emulsion (Sumielite 1320 manufactured by Sumika Chemtex Co., Ltd., solid content concentration 51.8% by mass) was used as the organic binder.
[0063] Comparative Example 1 A spherical activated carbon of Comparative Example 1 was obtained in the same manner as in Example 1, except that a vinyl chloride emulsion (Vinyblan 715S manufactured by Nissin Chemical Industry Co., Ltd., solid content concentration 23.8 mass%) was used as the organic binder. A photograph of the appearance of the obtained spherical activated carbon is shown in FIG.
[0064] Comparative Example 2 A spherical activated carbon of Comparative Example 2 was obtained in the same manner as in Example 1, except that polyvinyl alcohol (Gohsenol N300, manufactured by Nippon Synthetic Chemical Industry Co., Ltd., solid content concentration 7.0 mass %) was used as the organic binder.
[0065] Comparative Example 3 A spherical activated carbon of Comparative Example 3 was obtained in the same manner as in Example 1, except that sodium carboxymethyl cellulose (Sunrose F30MC, manufactured by Nippon Paper Industries Co., Ltd.) was used as the organic binder.
[0066] Comparative Example 4 A spherical activated carbon of Comparative Example 4 was obtained in the same manner as in Example 1, except that an ethylene-vinyl acetate resin (EVA Tex #100 manufactured by Denka Co., Ltd., solid content concentration 55.0 mass %) was used as the organic binder.
[0067] Comparative Example 5 A spherical activated carbon of Comparative Example 5 was obtained in the same manner as in Example 1, except that an acrylate-based latex (Nipol LX851C manufactured by Zeon Corporation, solid content concentration 45% by mass) was used as the organic binder.
[0068] Test Example 1: Average particle size of spherical activated carbon The average particle size of the obtained spherical activated carbon was measured in accordance with JIS K 1474 (2014) and calculated as the mass average particle size. In the examples, sieves with openings of 0.3 mm to 0.71 mm were used for evaluation, and in the comparative examples, the openings of the sieves were changed depending on the molded product.
[0069] Test Example 2: MS Hardness 10 mL of activated carbon that had been sieved using a sieve with a particle size range was placed in the container shown in Figure 3 together with 10 steel balls with a diameter of 7.94 mm. After rotating at 25 revolutions per minute for 40 minutes, the activated carbon and steel balls were separated, and the activated carbon was sieved using a 0.212 mm sieve. [Mass on sieve] x 100 (%) / [Mass on sieve + Mass under sieve] This method is used to determine durability against impact and friction.
[0070] Test example 3: Sphericity The spherical activated carbon obtained (N=10) was photographed using a digital microscope (KH-8700, manufactured by Hirox Corporation) and the sphericity was measured by calculating the longest diameter (a) / shortest diameter (b) of the spherical activated carbon.
[0071] The results are shown in Table 1.
[0072] [Table 1]
[0073] Comparing the spherical activated carbons of Example 1 and Comparative Example 1, it can be seen that the sphericity is high in Example 1 (Fig. 1), while the carbon in Comparative Example 1 (Fig. 2) is irregular and crushed. When an organic binder with a glass transition temperature of 20°C or higher is used as in the present invention, granulation is good, and the sphericity was 1.06 in Examples 1 and 2. The closer the sphericity is to 1.00, the closer it is to a sphere with no irregularities.
[0074] The temperature during granulation is less than 30°C (actual measurement was 26°C), and the organic binder, which has a high glass transition temperature, is not fused in Examples 1 and 2. This causes the activated carbon particles to bond together at points, and as a result, it is believed that the particles form a close-packed structure and become spherical during the granulation process.
[0075] On the other hand, in the case of the binders having low glass transition temperatures as seen in Comparative Examples 1, 4, and 5, the binders were fused at the temperature during granulation, and the activated carbon particles themselves were covered with the organic binder, causing extensive bonding between the particles. Once the surfaces of the granulated particles became uneven, the unevenness continued to grow, resulting in irregularly shaped crushed coal.
[0076] As for the MS hardness, as shown in Table 1 for Examples 1 and 2, the MS hardness is 70% or more, whereas the MS hardness is less than 70% in the comparative example. This indicates that the angular parts of the comparative example are easily removed by friction, which makes it easier for fine powder to be generated.
[0077] The PVA and CMC used in Comparative Examples 2 and 3 have good film-forming properties and tend to increase the viscosity of the organic binder itself, which tends to increase the MS hardness of the molded product itself (68% or more and less than 70%), but significantly reduces the granulation properties as spherical activated carbon.
Claims
1. A spherical activated carbon comprising a granulated product of an activated carbon composition containing activated carbon and an organic binder having a glass transition temperature of 30° C. or higher, and having an MS hardness of 70.0% or higher.
2. The spherical activated carbon according to claim 1, having an average particle size of 0.3 mm or more and less than 0.6 mm.
3. The spherical activated carbon according to claim 1 or 2, having a sphericity of 1.10 or less.
4. A method for producing spherical activated carbon according to any one of claims 1 to 3, A step of obtaining the spherical activated carbon by granulating an activated carbon composition containing activated carbon and an organic binder having a glass transition temperature of 30° C. or higher. A manufacturing method comprising:
5. The method according to claim 4, wherein the granulation temperature is 0°C or higher and lower than 30°C.
6. The method according to claim 4 or 5, wherein the organic binder has an average particle size of 10 to 300 nm.
7. The method according to any one of claims 4 to 6, wherein the organic binder has a viscosity of 1 to 20 mPa / s.
8. The method according to any one of claims 4 to 7, wherein the granulation step is a step of spraying water onto the activated carbon composition, forming the composition into a spherical activated carbon shape, and then heat treating the resulting product.
9. A cabin filter using the spherical activated carbon according to any one of claims 1 to 3.
10. A cigarette filter using the spherical activated carbon according to any one of claims 1 to 3.
11. A cigarette comprising the cigarette filter of claim 10.
Citation Information
Patent Citations
Method for manufacturing spherical active carbon
JP2005119947A
Spherical activated carbon and method of manufacturing the same
JP2006083052A
Functional separation material, gas adsorbent and filter for deodorizing tobacco
JP2007111692A
Transpiration fuel gas adsorbent and process for producing the same