Water-absorbent resin particles, absorbent body, absorbent article, method for measuring liquid permeability maintenance rate of water-absorbent resin particles, and method for producing water-absorbent resin particles

Water-absorbing resin particles with a defined liquid permeation retention rate address the issue of tearing in absorbent articles by ensuring uniform liquid distribution, thereby maintaining structural integrity and performance.

JP7588579B2Active Publication Date: 2024-11-22SUMITOMO SEIKA CHEM CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021505000
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-08
Filing Date
2020-03-05
Publication Date
2024-11-22
Estimated Expiration
2040-03-05

AI Technical Summary

Technical Problem

Absorbent articles, such as diapers, tend to tear internally when the proportion of fibrous materials is low, leading to reduced absorbent performance due to applied shear forces from body weight, especially after liquid absorption.

Method used

Development of water-absorbing resin particles with a specific liquid permeation retention rate, measured by a defined method, to enhance liquid diffusion and prevent tearing by ensuring a minimum 10% liquid permeation retention rate, achieved through controlled polymerization and crosslinking processes.

Benefits of technology

The water-absorbing resin particles effectively suppress tearing in absorbent articles by uniformly diffusing liquids, maintaining structural integrity and enhancing absorbent performance even under load.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588579000002
    Figure 0007588579000002
  • Figure 0007588579000003
    Figure 0007588579000003
  • Figure 0007588579000004
    Figure 0007588579000004
Patent Text Reader

Abstract

Provided is a water absorbent particle having at least 10% of a permeation retention rate which is represented by the following formula (Permeation retention rate (%)=(Swollen gel liquid passing speed / Dry powder liquid passing speed)×100), using a dry powder liquid passing speed measured by a method including steps (A), (B) and (C) in this order and a swollen gel liquid passing speed measured by a method including steps (A), (B), (D), and (E) in this order.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to water-absorbent resin particles, an absorbent body, an absorbent article, a method for measuring a liquid permeability maintenance rate of water-absorbent resin particles, and a method for producing water-absorbent resin particles. [Background technology]

[0002] Water-absorbent resins are used in the field of sanitary products, specifically as materials for absorbents contained in absorbent articles such as diapers (for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Special Publication No. 2014-515987 Summary of the Invention [Problem to be solved by the invention]

[0004] Absorbent articles such as diapers include an absorbent body that absorbs and retains bodily fluids such as urine and menstrual blood. The absorbent body generally contains water-absorbent resin particles and fibrous material such as pulp, and the fibrous material is entangled with itself or with the water-absorbent resin particles. In recent years, there has been a trend toward thinner absorbent articles, and therefore there is a tendency to prefer absorbents with a low ratio of fibrous material in the absorbent body. When the ratio of fibrous material in the absorbent body is low, for example, when a shear force is applied to the absorbent body after absorbing liquid due to the load of the body weight while wearing the absorbent article, the absorbent body may be deformed, such as being torn inside. An absorbent body that has been torn cannot fully exhibit its absorption performance.

[0005] An object of the present invention is to provide water-absorbent resin particles capable of suppressing the occurrence of breakage in an absorbent body after liquid absorption. [Means for solving the problem]

[0006] The water-absorbent resin particle of the present invention has a liquid permeability maintenance rate of 10% or more, which is represented by the following formula using a dry powder liquid permeability measured by a method including the following steps (A), (B), and (C) in this order, and a swollen gel liquid permeability measured by a method including the following steps (A), (B), (D), and (E) in this order. Liquid permeability maintenance rate (%) = (liquid permeability rate of swollen gel / liquid permeability rate of dry powder) x 100 (A) 0.3 g of water-absorbent resin particles are uniformly dispersed in a cylindrical container having an inner diameter of 26 mm and equipped with a mesh-like bottom. (B) A small cylindrical container with an outer diameter of 25 mm and an inner diameter of 19 mm and equipped with a mesh-like bottom is inserted into the cylindrical container to form a measurement section. (C) Saline is poured into the cylindrical small container of the measurement section at a constant rate of 60 ml / min, and the amount of saline flowing out of the bottom of the measurement section within one minute from the start of the pouring is measured to determine the dry powder flow rate (g / min) of saline. (D) The bottom side of the measurement section is immersed in 40 g of physiological saline in a container for 30 minutes, thereby causing the water-absorbent resin particles in the measurement section to swell. (E) 20 g of saline is poured into the small cylindrical container of the measurement section at once, and the amount of saline flowing out of the bottom of the measurement section within 1 minute from the start of the pouring is measured to determine the saline permeation rate through the swollen gel (g / min).

[0007] The water-absorbent resin particles preferably have a swollen gel liquid permeation rate of 2.5 g / min or more. When the water-absorbent resin particles have a swollen gel liquid permeation rate in the above range, the occurrence of breakage after the absorbent body absorbs liquid can be further suppressed.

[0008] The present invention also provides an absorbent body containing the above-mentioned water-absorbent resin particles. When the absorbent body contains the above-mentioned water-absorbent resin particles, the occurrence of breakage can be suppressed.

[0009] The present invention also provides an absorbent article comprising the above-mentioned absorbent body.

[0010] The absorbent article may be a diaper.

[0011] The present invention also provides a method for measuring a liquid permeability maintenance rate of a water-absorbent resin particle represented by the following formula, comprising measuring a dry powder liquid permeability rate by a method comprising the following steps (A), (B), and (C) in this order, and measuring a swollen gel liquid permeability rate by a method comprising the following steps (A), (B), (D), and (E) in this order. Liquid permeability maintenance rate (%) = (liquid permeability rate of swollen gel / liquid permeability rate of dry powder) x 100

[0012] (A) 0.3 g of water-absorbent resin particles are uniformly dispersed in a cylindrical container having an inner diameter of 26 mm and equipped with a mesh-like bottom. (B) A small cylindrical container with an outer diameter of 25 mm and an inner diameter of 19 mm and equipped with a mesh-like bottom is inserted into the cylindrical container to form a measurement section. (C) Saline is poured into the cylindrical small container of the measurement section at a constant rate of 60 ml / min, and the amount of saline flowing out of the bottom of the measurement section within one minute from the start of the pouring is measured to determine the dry powder flow rate (g / min) of saline. (D) The bottom side of the measurement section is immersed in 40 g of physiological saline in a container for 30 minutes, thereby causing the water-absorbent resin particles in the measurement section to swell. (E) 20 g of saline is poured into the small cylindrical container of the measurement section at once, and the amount of saline flowing out of the bottom of the measurement section within 1 minute from the start of the pouring is measured to determine the saline permeation rate through the swollen gel (g / min). The above-mentioned measurement method makes it possible to evaluate the diffusibility of the water-absorbent resin particles, which is involved in the tear resistance of the absorbent body.

[0013] The present invention also provides a method for producing water-absorbent resin particles, comprising selecting water-absorbent resin particles having a liquid permeability maintenance rate of 10% or more measured by the above-mentioned method, which can provide water-absorbent resin particles having excellent liquid diffusibility and suppressed breakage after absorbing liquid when used in an absorbent material.

[0014] The present invention also provides a method for suppressing the occurrence of breakage of an absorbent body containing the above-mentioned water-absorbent resin particles after absorbing liquid, the method comprising increasing a liquid permeability maintenance rate of the water-absorbent resin particles measured by the above-mentioned method. Effect of the Invention

[0015] According to the present invention, water-absorbent resin particles capable of suppressing the occurrence of breakage in an absorbent body after absorbing liquid are obtained. [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is a cross-sectional view showing an example of an absorbent article. [Diagram 2] FIG. 2 is a plan view showing the general shape of the stirring blade (flat blade having slits in the flat plate portion) used in the examples. [Diagram 3] FIG. 2 is a schematic cross-sectional view showing a method for measuring a liquid permeability maintenance rate. [Figure 4] FIG. 1 is a schematic diagram showing a method for measuring non-pressure DW. [Diagram 5] FIG. 2 is a schematic cross-sectional view showing a method for measuring the rupture time of an absorbent body. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Preferred embodiments of the present invention will be described in detail below, however, the present invention is not limited to the following embodiments.

[0018] In this specification, "acrylic" and "methacrylic" are collectively referred to as "(meth)acrylic". "Acrylate" and "methacrylate" are similarly referred to as "(meth)acrylate". "(Poly)" refers to both the case where the "poly" prefix is ​​present and the case where it is not present. In the numerical ranges described in stages in this specification, the upper limit or lower limit of a certain numerical range can be arbitrarily combined with the upper limit or lower limit of the numerical range of another stage. In the numerical ranges described in this specification, the upper limit or lower limit of the numerical range may be replaced with a value shown in the Examples. "Water-soluble" refers to a solubility of 5% by mass or more in water at 25°C. The materials exemplified in this specification may be used alone or in combination of two or more. When a plurality of substances corresponding to each component are present in the composition, the content of each component in the composition means the total amount of the plurality of substances present in the composition, unless otherwise specified. In this specification, physiological saline refers to an aqueous solution of NaCl with a concentration of 0.9% by mass, unless otherwise specified.

[0019] The water-absorbent resin particles according to the present embodiment have a liquid permeability maintenance rate represented by the following formula of 10% or more. The present inventors have found that the occurrence of breakage in the absorbent body after absorbing liquid is suppressed as the ratio of the swollen gel liquid permeability, which is the liquid permeability speed of the water-absorbent resin particles in a swollen state after absorbing liquid, to the dry powder liquid permeability, which is the liquid permeability speed of the water-absorbent resin particles in a dry state, is higher. Liquid permeability maintenance rate (%) = (liquid permeability rate of swollen gel / liquid permeability rate of dry powder) x 100

[0020] According to the present inventor's speculation, the water-absorbent resin particles of the present invention are believed to be able to diffuse liquid more uniformly inside the absorbent when the liquid permeability maintenance rate is 10% or more. If the liquid is not uniformly diffused inside the absorbent, there will be scattered parts that are extremely resistant to breakage (parts that have absorbed almost no liquid) and parts that are extremely prone to tear (parts that have absorbed a large amount of liquid). When a load such as body weight is applied to the absorbent while wearing the absorbent article, the absorbent is likely to tear from the parts that are extremely prone to tear. It is believed that the water-absorbent resin particles of the present invention can diffuse liquid uniformly inside the absorbent, making it difficult for parts that are extremely prone to tear to occur, and as a result, it is believed that the occurrence of tearing of the absorbent is suppressed.

[0021] The dry powder liquid permeation rate is measured by a method including the following steps (A), (B), and (C) in this order. The swollen gel liquid permeation rate is measured by a method including the following steps (A), (B), (D), and (E) in this order. More specific measurement methods are shown in the examples below. (A) 0.3 g of water-absorbent resin particles are uniformly dispersed in a cylindrical container having an inner diameter of 26 mm and equipped with a mesh-like bottom. (B) A small cylindrical container with an outer diameter of 25 mm and an inner diameter of 19 mm and equipped with a mesh-like bottom is inserted into the cylindrical container to form a measurement section. (C) Saline is poured into the cylindrical small container of the measurement section at a constant rate of 60 ml / min, and the amount of saline flowing out of the bottom of the measurement section within one minute from the start of the pouring is measured to determine the dry powder flow rate (g / min) of saline. (D) The bottom side of the measurement section is immersed in 40 g of physiological saline in a container for 30 minutes, thereby causing the water-absorbent resin particles in the measurement section to swell. (E) 20 g of saline is poured into the small cylindrical container of the measurement section at once, and the amount of saline flowing out of the bottom of the measurement section within 1 minute from the start of the pouring is measured to determine the saline permeation rate through the swollen gel (g / min).

[0022] The water-absorbent resin particles according to the present embodiment preferably have a liquid permeability maintenance rate of 12% or more, more preferably 15% or more, 20% or more, 25% or more, or 30% or more, and even more preferably 35% or more, or 40% or more. The water-absorbent resin particles according to the present embodiment may have a liquid permeability maintenance rate of, for example, 80% or less, 70% or less, 60% or less, 58% or less, 55% or less, or 50% or less.

[0023] The water absorbent resin particles according to the present embodiment may have a dry powder liquid permeation rate measured by the above-mentioned method of, for example, 2 g / min or more, 5 g / min or more, 8 g / min or more, 10 g / min or more, 15 g / min or more, 18 g / min or more, or 20 g / min or more. The dry powder liquid permeation rate of the water absorbent resin particles may be, for example, 50 g / min or less, 40 g / min or less, 35 g / min or less, 33 g / min or less, or 30 g / min or less.

[0024] The water-absorbent resin particles according to the present embodiment may have a swollen gel permeation rate measured by the above-mentioned method of, for example, 0.7 g / min or more, 1.0 g / min or more, 1.5 g / min or more, 2.0 g / min or more, 2.5 g / min or more, 3.0 g / min or more, 4.0 g / min or more, 5.0 g / min or more, 6.0 g / min or more, or 8.0 g / min or more. When the swollen gel permeation rate is within the above range, there is a tendency that the occurrence of breakage after the absorbent body absorbs liquid can be more suppressed. The swollen gel permeation rate of the water-absorbent resin particles may be, for example, 30 g / min or less, 25 g / min or less, 20 g / min or less, 18 g / min or less, or 15 g / min or less. From these viewpoints, the swollen gel permeation rate is preferably 1 to 30 g / min, 3 to 25 g / min, or 5 to 20 g / min.

[0025] The water-absorbent resin particles according to the present embodiment can have a high water-absorbing ability for physiological saline. The physiological saline water-retention capacity of the water-absorbent resin particles may be, for example, 20 g / g or more, 23 g / g or more, 25 g / g or more, 28 g / g or more, 30 g / g or more, or 32 g / g or more, and may be 60 g / g or less, 55 g / g or less, 53 g / g or less, 50 g / g or less, 48 ​​g / g or less, 45 g / g or less, 43 g / g or less, or 40 g / g or less. The physiological saline water-retention capacity of the water-absorbent resin particles may be, for example, 20 to 60 g / g, 23 to 55 g / g, 25 to 50 g / g, 28 to 45 g / g, or 30 to 40 g / g. The physiological saline water-retention capacity is measured by the method described in the examples below.

[0026] The water absorbent resin particles according to the present embodiment may have a no-pressure DW3-minute value of, for example, 14 ml / g or more, 16 ml / g or more, 18 ml / g or more, 20 ml / g or more, or 25 ml / g or more. The no-pressure DW3-minute value may be, for example, 55 ml / g or less, 50 ml / g or less, or 40 ml / g or less. The no-pressure DW3-minute value is measured by the method described in the examples below.

[0027] The shape of the water-absorbent resin particles may be substantially spherical, crushed, granular, etc. The median particle size of the water-absorbent resin particles may be 250 to 850 μm, 300 to 700 μm, or 300 to 600 μm. The water-absorbent resin particles according to the present embodiment may have a desired particle size distribution at the time when the polymer particles are obtained by the production method described later, but the particle size distribution may be adjusted by performing an operation such as particle size adjustment using classification with a sieve.

[0028] The water-absorbent resin particles according to the present embodiment may include, for example, a crosslinked polymer formed by polymerization of a monomer including an ethylenically unsaturated monomer. The crosslinked polymer has a monomer unit derived from the ethylenically unsaturated monomer. That is, the water-absorbent resin particles according to the present embodiment may have a structural unit derived from the ethylenically unsaturated monomer.

[0029] The method of polymerizing the monomer includes reversed-phase suspension polymerization, aqueous solution polymerization, bulk polymerization, precipitation polymerization, etc. Among these, the reversed-phase suspension polymerization or aqueous solution polymerization is preferred from the viewpoint of ensuring good water absorption properties of the obtained water absorbent resin particles and easy control of the polymerization reaction. In the following, the reversed-phase suspension polymerization is taken as an example to explain the method of polymerizing the ethylenically unsaturated monomer.

[0030] The ethylenically unsaturated monomer is preferably water-soluble, and examples thereof include (meth)acrylic acid and its salts, 2-(meth)acrylamido-2-methylpropanesulfonic acid and its salts, (meth)acrylamide, N,N-dimethyl(meth)acrylamide, 2-hydroxyethyl(meth)acrylate, N-methylol(meth)acrylamide, polyethylene glycol mono(meth)acrylate, N,N-diethylaminoethyl(meth)acrylate, N,N-diethylaminopropyl(meth)acrylate, and diethylaminopropyl(meth)acrylamide. When the ethylenically unsaturated monomer contains an amino group, the amino group may be quaternized. The functional groups of the above monomers, such as carboxyl groups and amino groups, can function as functional groups capable of crosslinking in the surface crosslinking step described below. These ethylenically unsaturated monomers may be used alone or in combination of two or more.

[0031] Among these, from the viewpoint of industrial availability, the ethylenically unsaturated monomer preferably contains at least one compound selected from the group consisting of (meth)acrylic acid and its salts, acrylamide, methacrylamide, and N,N-dimethylacrylamide, and more preferably contains at least one compound selected from the group consisting of (meth)acrylic acid and its salts, and acrylamide. From the viewpoint of further improving water absorption properties, the ethylenically unsaturated monomer further preferably contains at least one compound selected from the group consisting of (meth)acrylic acid and its salts.

[0032] As the monomer, a monomer other than the above ethylenically unsaturated monomer may be partially used. Such a monomer may be used by mixing with an aqueous solution containing the above ethylenically unsaturated monomer. The amount of the ethylenically unsaturated monomer used may be 70 to 100 mol%, 80 to 100 mol%, 90 to 100 mol%, 95 to 100 mol%, or 100 mol% based on the total amount of monomers (total amount of monomers for obtaining water absorbent resin particles. For example, total amount of monomers that provide structural units of a crosslinked polymer. The same applies below.). Among them, (meth)acrylic acid and salts thereof may be 70 to 100 mol%, 80 to 100 mol%, 90 to 100 mol%, 95 to 100 mol%, or 100 mol% based on the total amount of monomers. "Ratio of (meth)acrylic acid and salts thereof" means the ratio of the total amount of (meth)acrylic acid and salts thereof.

[0033] According to the present embodiment, as an example of the water-absorbent resin particles, it is possible to provide water-absorbent resin particles containing a crosslinked polymer having a structural unit derived from an ethylenically unsaturated monomer, the ethylenically unsaturated monomer containing at least one compound selected from the group consisting of (meth)acrylic acid and salts thereof, and the ratio of the (meth)acrylic acid and the salts thereof is 70 to 100 mol % based on the total amount of monomers for obtaining the water-absorbent resin particles.

[0034] The ethylenically unsaturated monomer is usually preferably used as an aqueous solution. The concentration of the ethylenically unsaturated monomer in the aqueous solution containing the ethylenically unsaturated monomer (hereinafter referred to as the aqueous monomer solution) is usually 20% by mass or more and saturation concentration or less, preferably 25 to 70% by mass, more preferably 30 to 55% by mass. Examples of the water used include tap water, distilled water, and ion-exchanged water.

[0035] When the ethylenically unsaturated monomer used contains an acid group, the aqueous monomer solution may be used after neutralizing the acid group with an alkaline neutralizing agent. The degree of neutralization of the ethylenically unsaturated monomer with the alkaline neutralizing agent is 10 to 100 mol %, preferably 50 to 90 mol %, and more preferably 60 to 80 mol % of the acid group in the ethylenically unsaturated monomer, from the viewpoint of increasing the osmotic pressure of the resulting water-absorbing resin particles and further improving the water-absorbing properties such as water retention. Examples of the alkaline neutralizing agent include alkali metal salts such as sodium hydroxide, sodium carbonate, sodium hydrogen carbonate, potassium hydroxide, and potassium carbonate; and ammonia. These alkaline neutralizing agents may be used in the form of an aqueous solution in order to simplify the neutralization operation. The above-mentioned alkaline neutralizing agents may be used alone or in combination of two or more kinds. The neutralization of the acid group of the ethylenically unsaturated monomer can be carried out, for example, by dropping an aqueous solution of sodium hydroxide, potassium hydroxide, or the like into the above-mentioned aqueous monomer solution and mixing.

[0036] In the reversed phase suspension polymerization method, an aqueous monomer solution is dispersed in a hydrocarbon dispersion medium in the presence of a surfactant, and an ethylenically unsaturated monomer is polymerized using a radical polymerization initiator or the like.

[0037] Examples of the surfactant include nonionic surfactants and anionic surfactants. Examples of the nonionic surfactant include sorbitan fatty acid esters, polyglycerin fatty acid esters, sucrose fatty acid esters, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene glycerin fatty acid esters, sorbitol fatty acid esters, polyoxyethylene sorbitol fatty acid esters, polyoxyethylene alkyl ethers, polyoxyethylene alkylphenyl ethers, polyoxyethylene castor oil, polyoxyethylene hardened castor oil, alkylaryl formaldehyde condensed polyoxyethylene ethers, polyoxyethylene polyoxypropylene block copolymers, polyoxyethylene polyoxypropyl alkyl ethers, and polyethylene glycol fatty acid esters. Examples of the anionic surfactant include fatty acid salts, alkylbenzene sulfonates, alkylmethyl taurate salts, polyoxyethylene alkylphenyl ether sulfates, polyoxyethylene alkyl ether sulfonates, polyoxyethylene alkyl ether phosphates, and polyoxyethylene alkylaryl ether phosphates. Among these, from the viewpoints of obtaining a good W / O type reverse phase suspension state, easily obtaining water absorbent resin particles with a suitable particle size, and being easily available industrially, it is preferable that the surfactant contains at least one compound selected from the group consisting of sorbitan fatty acid esters, polyglycerin fatty acid esters, and sucrose fatty acid esters. Furthermore, from the viewpoint of improving the water absorption properties of the obtained water absorbent resin particles, it is more preferable that the surfactant contains a sucrose fatty acid ester. These surfactants may be used alone or in combination of two or more.

[0038] From the viewpoint of obtaining sufficient effect relative to the amount used and being economical, the amount of the surfactant is preferably 0.05 to 10 parts by mass, more preferably 0.08 to 5 parts by mass, and further preferably 0.1 to 3 parts by mass, relative to 100 parts by mass of the aqueous ethylenically unsaturated monomer solution.

[0039] In addition, a polymeric dispersant may be used together with the above-mentioned surfactant. Examples of the polymeric dispersant include maleic anhydride-modified polyethylene, maleic anhydride-modified polypropylene, maleic anhydride-modified ethylene-propylene copolymer, maleic anhydride-modified EPDM (ethylene-propylene-diene-terpolymer), maleic anhydride-modified polybutadiene, maleic anhydride-ethylene copolymer, maleic anhydride-propylene copolymer, maleic anhydride-ethylene-propylene copolymer, maleic anhydride-butadiene copolymer, polyethylene, polypropylene, ethylene-propylene copolymer, oxidized polyethylene, oxidized polypropylene, oxidized ethylene-propylene copolymer, ethylene-acrylic acid copolymer, ethyl cellulose, and ethylhydroxyethyl cellulose. Among these polymeric dispersants, it is particularly preferable to use maleic anhydride-modified polyethylene, maleic anhydride-modified polypropylene, maleic anhydride-modified ethylene-propylene copolymer, maleic anhydride-ethylene copolymer, maleic anhydride-propylene copolymer, maleic anhydride-ethylene-propylene copolymer, polyethylene, polypropylene, ethylene-propylene copolymer, oxidized polyethylene, oxidized polypropylene, and oxidized ethylene-propylene copolymer, from the viewpoint of dispersion stability of the monomer. These polymeric dispersants may be used alone or in combination of two or more.

[0040] From the viewpoint of obtaining sufficient effect relative to the amount used and being economical, the amount of the polymer dispersant is preferably 0.05 to 10 parts by mass, more preferably 0.08 to 5 parts by mass, and further preferably 0.1 to 3 parts by mass, relative to 100 parts by mass of the aqueous ethylenically unsaturated monomer solution.

[0041] The radical polymerization initiator is preferably water-soluble, and examples thereof include persulfates such as potassium persulfate, ammonium persulfate, and sodium persulfate; peroxides such as methyl ethyl ketone peroxide, methyl isobutyl ketone peroxide, di-t-butyl peroxide, t-butyl cumyl peroxide, t-butyl peroxyacetate, t-butyl peroxyisobutyrate, t-butyl peroxypivalate, and hydrogen peroxide; 2,2'-azobis(2-amidinopropane) dihydrochloride, 2,2'-azobis[2-(N-phenylamidino)propane] dihydrochloride, 2,2 and azo compounds such as 2,2'-azobis[2-(N-allylamidino)propane] dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride, 2,2'-azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane} dihydrochloride, 2,2'-azobis{2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propionamide}, 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)-propionamide], and 4,4'-azobis(4-cyanovaleric acid). Among these, potassium persulfate, ammonium persulfate, sodium persulfate, 2,2'-azobis(2-amidinopropane) dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride, and 2,2'-azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane} dihydrochloride are preferred. These radical polymerization initiators may be used alone or in combination of two or more.

[0042] The amount of the radical polymerization initiator used may be 0.00005 to 0.01 moles per mole of the ethylenically unsaturated monomer. When the amount of the radical polymerization initiator used is 0.00005 moles or more, the polymerization reaction does not take a long time and is efficient. When the amount used is 0.01 moles or less, the polymerization reaction tends not to occur abruptly.

[0043] The above radical polymerization initiators can also be used as redox polymerization initiators in combination with reducing agents such as sodium sulfite, sodium hydrogen sulfite, ferrous sulfate, and L-ascorbic acid.

[0044] In the polymerization reaction, the aqueous solution of the ethylenically unsaturated monomer used in the polymerization may contain a chain transfer agent. Examples of the chain transfer agent include hypophosphites, thiols, thiolic acids, secondary alcohols, and amines.

[0045] In addition, in order to control the particle size of the water-absorbent resin particles, a thickener may be contained in the ethylenically unsaturated monomer aqueous solution used for polymerization. As the thickener, for example, hydroxyethyl cellulose, hydroxypropyl cellulose, methyl cellulose, carboxymethyl cellulose, polyacrylic acid, polyacrylic acid (partially) neutralized product, polyethylene glycol, polyacrylamide, polyethyleneimine, dextrin, sodium alginate, polyvinyl alcohol, polyvinylpyrrolidone, polyethylene oxide, etc. can be used. Note that, if the stirring speed during polymerization is the same, the higher the viscosity of the ethylenically unsaturated monomer aqueous solution, the larger the median particle size of the obtained particles tends to be.

[0046] Examples of the hydrocarbon dispersion medium include chain aliphatic hydrocarbons such as n-hexane, n-heptane, 2-methylhexane, 3-methylhexane, 2,3-dimethylpentane, 3-ethylpentane, and n-octane; alicyclic hydrocarbons such as cyclohexane, methylcyclohexane, cyclopentane, methylcyclopentane, trans-1,2-dimethylcyclopentane, cis-1,3-dimethylcyclopentane, and trans-1,3-dimethylcyclopentane; and aromatic hydrocarbons such as benzene, toluene, and xylene. These hydrocarbon dispersion media may be used alone or in combination of two or more. The hydrocarbon dispersion medium may contain at least one compound selected from the group consisting of chain aliphatic hydrocarbons having 6 to 8 carbon atoms and alicyclic hydrocarbons having 6 to 8 carbon atoms. From the viewpoint of industrial availability and stable quality, the hydrocarbon dispersion medium may contain n-heptane, cyclohexane, or both of them. From the same viewpoint, for example, commercially available Exxolheptane (manufactured by ExxonMobil Corp.: containing 75 to 85% of n-heptane and isomeric hydrocarbons) may be used as the mixture of the hydrocarbon dispersion medium.

[0047] The amount of the hydrocarbon dispersion medium used is preferably 30 to 1000 parts by mass, more preferably 40 to 500 parts by mass, and even more preferably 50 to 300 parts by mass, relative to 100 parts by mass of the aqueous monomer solution, from the viewpoint of adequately removing the heat of polymerization and making it easy to control the polymerization temperature. When the amount of the hydrocarbon dispersion medium used is 30 parts by mass or more, the polymerization temperature tends to be easily controlled. When the amount of the hydrocarbon dispersion medium used is 1000 parts by mass or less, the polymerization productivity tends to be improved, which is economical.

[0048] Usually, internal crosslinking due to self-crosslinking may occur during polymerization, but the water absorption properties of the water-absorbing resin particles may be controlled by further applying internal crosslinking using an internal crosslinking agent. Examples of the internal crosslinking agent used include di- or tri(meth)acrylic acid esters of polyols such as ethylene glycol, propylene glycol, trimethylolpropane, glycerin, polyoxyethylene glycol, polyoxypropylene glycol, and polyglycerin; unsaturated polyesters obtained by reacting the above polyols with unsaturated acids such as maleic acid and fumaric acid; bis(meth)acrylamides such as N,N'-methylenebis(meth)acrylamide; di- or tri(meth)acrylic acid esters obtained by reacting polyepoxides with (meth)acrylic acid; di(meth)acrylic acid carbamyl esters obtained by reacting polyisocyanates such as tolylene diisocyanate and hexamethylene diisocyanate with hydroxyethyl (meth)acrylate. compounds having two or more polymerizable unsaturated groups, such as allylated starch, allylated cellulose, diallyl phthalate, N,N',N''-triallyl isocyanurate, and divinylbenzene; polyglycidyl compounds, such as (poly)ethylene glycol diglycidyl ether, (poly)propylene glycol diglycidyl ether, (poly)glycerin diglycidyl ether, (poly)glycerin triglycidyl ether, (poly)propylene glycol polyglycidyl ether, and polyglycerol polyglycidyl ether; haloepoxy compounds, such as epichlorohydrin, epibromohydrin, and α-methylepichlorohydrin; and compounds having two or more reactive functional groups, such as isocyanate compounds, such as 2,4-tolylene diisocyanate and hexamethylene diisocyanate. Among these internal crosslinking agents, it is preferable to use a polyglycidyl compound, more preferable to use a diglycidyl ether compound, and particularly preferable to use (poly)ethylene glycol diglycidyl ether, (poly)propylene glycol diglycidyl ether, or (poly)glycerin diglycidyl ether. These crosslinking agents may be used alone or in combination of two or more.

[0049] The amount of the internal crosslinking agent is preferably 0 to 0.03 mol, more preferably 0.00001 to 0.01 mol, and even more preferably 0.00002 to 0.005 mol per mol of the ethylenically unsaturated monomer, from the viewpoint of suppressing the water-soluble property by moderate crosslinking of the obtained polymer and exhibiting a sufficient water absorption amount.

[0050] An aqueous phase containing components such as an ethylenically unsaturated monomer, a radical polymerization initiator, and optionally an internal crosslinking agent is mixed with an oil phase containing components such as a hydrocarbon-based dispersion medium, a surfactant, and optionally a polymer-based dispersant, and the mixture is heated under stirring to perform reverse phase suspension polymerization in a water-in-oil system.

[0051] When performing reversed-phase suspension polymerization, an aqueous monomer solution containing an ethylenically unsaturated monomer is dispersed in a hydrocarbon dispersion medium in the presence of a surfactant and, if necessary, a polymeric dispersant. In this case, the timing of adding the surfactant or polymeric dispersant may be either before or after the addition of the aqueous monomer solution, so long as it is before the start of the polymerization reaction.

[0052] Among them, from the viewpoint of easily reducing the amount of the hydrocarbon dispersion medium remaining in the obtained water absorbent resin, it is preferable to disperse an aqueous monomer solution in a hydrocarbon dispersion medium having a polymeric dispersant dispersed therein, and then further disperse a surfactant therein, and then carry out polymerization.

[0053] Such reverse phase suspension polymerization can be carried out in one stage or in multiple stages of two or more stages, and is preferably carried out in two to three stages from the viewpoint of increasing productivity.

[0054] When performing reversed-phase suspension polymerization in two or more stages, after performing reversed-phase suspension polymerization in the first stage, an ethylenically unsaturated monomer is added to the reaction mixture obtained in the polymerization reaction in the first stage and mixed, and reversed-phase suspension polymerization in the second stage and thereafter may be performed in the same manner as in the first stage. In reversed-phase suspension polymerization in each stage after the second stage, in addition to the ethylenically unsaturated monomer, it is preferable to add the above-mentioned radical polymerization initiator and internal crosslinking agent within the range of the molar ratio of each component to the ethylenically unsaturated monomer as described above, based on the amount of the ethylenically unsaturated monomer added during reversed-phase suspension polymerization in each stage after the second stage, to perform reversed-phase suspension polymerization. Note that, in reversed-phase suspension polymerization in each stage after the second stage, an internal crosslinking agent may be used as necessary. When an internal crosslinking agent is used, it is preferable to add the above-mentioned radical polymerization initiator and internal crosslinking agent within the range of the molar ratio of each component to the ethylenically unsaturated monomer as based on the amount of the ethylenically unsaturated monomer to be used in each stage, to perform reversed-phase suspension polymerization.

[0055] The temperature of the polymerization reaction varies depending on the radical polymerization initiator used, but from the viewpoint of quickly progressing the polymerization and shortening the polymerization time to improve economic efficiency and easily removing the polymerization heat to smoothly carry out the reaction, the temperature is preferably 20 to 150°C, more preferably 40 to 120°C. The reaction time is usually 0.5 to 4 hours. The end of the polymerization reaction can be confirmed, for example, by the cessation of the temperature rise in the reaction system. As a result, the polymer of the ethylenically unsaturated monomer is usually obtained in the form of a hydrogel.

[0056] After the polymerization, a crosslinking agent may be added to the obtained hydrogel polymer and the polymer may be heated to perform post-polymerization crosslinking. By performing post-polymerization crosslinking, the degree of crosslinking of the hydrogel polymer can be increased, and the water absorption properties can be more favorably improved.

[0057] Examples of crosslinking agents for crosslinking after polymerization include polyols such as ethylene glycol, propylene glycol, 1,4-butanediol, trimethylolpropane, glycerin, polyoxyethylene glycol, polyoxypropylene glycol, and polyglycerin; compounds having two or more epoxy groups such as (poly)ethylene glycol diglycidyl ether, (poly)propylene glycol diglycidyl ether, and (poly)glycerin diglycidyl ether; haloepoxy compounds such as epichlorohydrin, epibromohydrin, and α-methylepichlorohydrin; compounds having two or more isocyanate groups such as 2,4-tolylene diisocyanate and hexamethylene diisocyanate; oxazoline compounds such as 1,2-ethylenebisoxazoline; carbonate compounds such as ethylene carbonate; and hydroxyalkylamide compounds such as bis[N,N-di(β-hydroxyethyl)]adipamide. Among these, preferred are polyglycidyl compounds such as (poly)ethylene glycol diglycidyl ether, (poly)glycerin diglycidyl ether, (poly)glycerin triglycidyl ether, (poly)propylene glycol polyglycidyl ether, polyglycerol polyglycidyl ether, etc. These crosslinking agents may be used alone or in combination of two or more.

[0058] The amount of the crosslinking agent used in the post-polymerization crosslinking is preferably 0 to 0.03 mol, more preferably 0 to 0.01 mol, and even more preferably 0.00001 to 0.005 mol, per 1 mol of the ethylenically unsaturated monomer, from the viewpoint of allowing the resulting hydrous gel polymer to be appropriately crosslinked and thereby exhibiting favorable water absorption properties.

[0059] The timing of adding the post-polymerization crosslinking agent may be after the polymerization of the ethylenically unsaturated monomer used in the polymerization, and in the case of multi-stage polymerization, it is preferable to add it after the multi-stage polymerization. In addition, taking into consideration heat generation during and after polymerization, retention due to process delay, opening of the system when the crosslinking agent is added, and fluctuation in moisture due to addition of water accompanying the addition of the crosslinking agent, the crosslinking agent for post-polymerization crosslinking is preferably added in the region of [moisture content immediately after polymerization ±3% by mass] from the viewpoint of moisture content (described later).

[0060] Subsequently, the obtained hydrogel polymer is dried to remove water. By drying, polymer particles containing a polymer of an ethylenically unsaturated monomer are obtained. Examples of the drying method include (a) a method in which the hydrogel polymer is dispersed in a hydrocarbon dispersion medium and azeotropic distilled by heating from the outside, and the hydrocarbon dispersion medium is refluxed to remove water, (b) a method in which the hydrogel polymer is taken out by decantation and dried under reduced pressure, and (c) a method in which the hydrogel polymer is filtered through a filter and dried under reduced pressure. Among them, the method (a) is preferably used because of the simplicity of the production process.

[0061] The particle size of the water-absorbent resin particles can be controlled, for example, by adjusting the rotation speed of the agitator during the polymerization reaction, or by adding a powdered inorganic flocculant to the system after the polymerization reaction or at the beginning of drying. By adding the flocculant, the particle size of the obtained water-absorbent resin particles can be increased. Examples of the powdered inorganic flocculant include silica, zeolite, bentonite, aluminum oxide, talc, titanium dioxide, kaolin, clay, hydrotalcite, etc., and among them, silica, aluminum oxide, talc, or kaolin are preferred from the viewpoint of flocculation effect.

[0062] In the reversed-phase suspension polymerization, the method of adding the powdered inorganic flocculant is preferably a method in which the powdered inorganic flocculant is previously dispersed in the same type of hydrocarbon dispersion medium or water as that used in the polymerization, and then mixed into the hydrocarbon dispersion medium containing the hydrous gel under stirring.

[0063] In the production of the water-absorbent resin particles according to the present embodiment, it is preferable to crosslink (surface crosslink) the surface portion of the hydrogel polymer using a crosslinking agent in the drying step or any of the steps thereafter. The surface crosslinking is preferably performed at a timing when the hydrogel polymer has a specific water content. The timing of the surface crosslinking is preferably when the water content of the hydrogel polymer is 5 to 50% by mass, more preferably when it is 10 to 40% by mass, and even more preferably when it is 15 to 35% by mass.

[0064] The water content (mass%) of the hydrous gel polymer is calculated by the following formula. Moisture content=[Ww / (Ww+Ws)]×100 Ww: The water content of the hydrous gel polymer, calculated by subtracting the water content discharged outside the system in the drying process from the water content contained in the aqueous liquid before polymerization in all polymerization processes, plus the water content used as necessary when mixing a powdered inorganic flocculant, a surface crosslinking agent, etc. Ws: The solid content calculated from the amounts of the ethylenically unsaturated monomer, crosslinking agent, initiator, and other materials that constitute the hydrous gel polymer.

[0065] Examples of the surface cross-linking agent for performing surface cross-linking include compounds having two or more reactive functional groups. Examples of the surface cross-linking agent include polyols such as ethylene glycol, propylene glycol, 1,4-butanediol, trimethylolpropane, glycerin, polyoxyethylene glycol, polyoxypropylene glycol, and polyglycerin; polyglycidyl compounds such as (poly)ethylene glycol diglycidyl ether, (poly)glycerin diglycidyl ether, (poly)glycerin triglycidyl ether, trimethylolpropane triglycidyl ether, (poly)propylene glycol polyglycidyl ether, and (poly)glycerol polyglycidyl ether; epichlorohydrin, epibromohydrin, α-methylepichlorohydrin, Examples of the epoxy compounds include haloepoxy compounds such as 2,4-tolylene diisocyanate and hexamethylene diisocyanate; oxetane compounds such as 3-methyl-3-oxetane methanol, 3-ethyl-3-oxetane methanol, 3-butyl-3-oxetane methanol, 3-methyl-3-oxetane ethanol, 3-ethyl-3-oxetane ethanol, and 3-butyl-3-oxetane ethanol; oxazoline compounds such as 1,2-ethylenebisoxazoline; carbonate compounds such as ethylene carbonate; and hydroxyalkylamide compounds such as bis[N,N-di(β-hydroxyethyl)]adipamide. Among these, polyglycidyl compounds such as (poly)ethylene glycol diglycidyl ether, (poly)glycerin diglycidyl ether, (poly)glycerin triglycidyl ether, (poly)propylene glycol polyglycidyl ether, and polyglycerol polyglycidyl ether are more preferred. These surface cross-linking agents may be used alone or in combination of two or more kinds.

[0066] The amount of the surface crosslinking agent is usually 0.00001 to 0.02 mol, preferably 0.00005 to 0.01 mol, and more preferably 0.0001 to 0.005 mol, relative to 1 mol of the ethylenically unsaturated monomer used in the polymerization, from the viewpoint of allowing the resulting hydrogel polymer to be appropriately crosslinked and thus exhibiting suitable water absorption properties.

[0067] From the viewpoint of sufficiently increasing the crosslinking density in the surface portion of the polymer particle and increasing the gel strength of the water-absorbent resin particle, the amount of the surface crosslinking agent used is preferably 0.00001 mol or more, and from the viewpoint of increasing the water retention capacity of the water-absorbent resin particle, the amount is preferably 0.02 mol or less.

[0068] After the surface cross-linking reaction, the water and the hydrocarbon dispersion medium are distilled off by a known method to obtain polymer particles which are a surface-cross-linked, dry product.

[0069] The polymerization reaction can be carried out using various stirrers having stirring blades. As the stirring blades, flat blades, lattice blades, paddle blades, propeller blades, anchor blades, turbine blades, Pfaudle blades, ribbon blades, full zone blades, Max Blend blades, etc. can be used. The flat blades have a shaft (stirring shaft) and a flat plate part (stirring part) arranged around the shaft. The flat plate part may have slits, etc. When flat blades are used as the stirring blades, the crosslinking reaction in the polymer particles is easily carried out uniformly, and the liquid passing maintenance rate is easily adjusted to a range suitable for the present invention while maintaining water absorption properties such as water retention.

[0070] The water-absorbent resin particles according to the present embodiment may be composed of only polymer particles, but may further contain various additional components selected from, for example, inorganic powders, surfactants, oxidizing agents, reducing agents, metal chelating agents, radical chain inhibitors, antioxidants, antibacterial agents, deodorants, gel stabilizers, flow improvers (lubricants), etc. The additional components may be disposed inside the polymer particles, on the surfaces of the polymer particles, or both.

[0071] The water-absorbent resin particles according to the present embodiment preferably contain inorganic particles. Examples of inorganic particles include silica particles such as amorphous silica. The amorphous silica may be hydrophilic amorphous silica. For example, the inorganic particles can be arranged on the surface of the polymer particles by mixing the polymer particles with the inorganic particles. The inorganic particles here usually have a minute size compared to the size of the polymer particles. For example, the average particle size of the inorganic particles may be 0.1 to 50 μm, 0.5 to 30 μm, or 1 to 20 μm. The average particle size here can be a value measured by a dynamic light scattering method or a laser diffraction / scattering method. When the amount of inorganic particles added is within the above range, water-absorbent resin particles having good water absorption properties can be easily obtained.

[0072] For example, the fluidity of the water-absorbent resin particles can be improved by adding 0.05 to 5 parts by mass of amorphous silica as inorganic particles to 100 parts by mass of the polymer particles. When the water-absorbent resin particles contain inorganic particles, the ratio of the inorganic particles to the mass of the polymer particles may be 0.05% by mass or more, 0.1% by mass or more, 0.2% by mass or more, 0.5% by mass or more, 1.0% by mass or more, or 1.5% by mass or more, or 5.0% by mass or less, 3.5% by mass or less, 1.5% by mass or less, 1.0% by mass or less, 0.8% by mass or less, 0.5% by mass or less, or 0.3% by mass or less.

[0073] The method for producing water-absorbent resin particles according to the present embodiment may include a step of selecting water-absorbent resin particles having a liquid-permeability maintenance rate of 10% or more measured by the above-mentioned method. The above-mentioned production method may include a step of measuring the liquid-permeability maintenance rate of the water-absorbent resin particles. The properties of the water-absorbent resin particles to be selected may satisfy the above-mentioned aspects of the water-absorbent resin particles (for example, a specific range of physiological saline water retention capacity, a specific range of unpressurized DW 3-minute value, etc.).

[0074] The water-absorbent resin particles according to the present embodiment have excellent absorbency of body fluids such as urine and blood, and can be applied to, for example, fields such as sanitary products such as paper diapers, sanitary napkins, and tampons, pet sheets, and animal excrement treatment materials such as dog or cat litter mixtures, and the like.

[0075] The water-absorbent resin particles according to the present embodiment can be suitably used in an absorbent body. The absorbent body according to the present embodiment contains water-absorbent resin particles. The content of the water-absorbent resin particles in the absorbent body is set to 100 to 1000 g per square meter of the absorbent body (i.e., 100 to 1000 g / m2) from the viewpoint of obtaining sufficient liquid absorption performance when the absorbent body is used in an absorbent article. 2 ), and more preferably 150 to 800 g / m 2 , and more preferably 200 to 700 g / m 2 In order to ensure that the absorbent article exhibits sufficient liquid absorption performance and, in particular, to suppress liquid leakage, the content is set to 100 g / m 2 From the viewpoints of suppressing the occurrence of the gel blocking phenomenon, exhibiting the liquid diffusion performance as an absorbent article, and further improving the liquid permeation rate, the above content is preferably 1000 g / m 2 It is preferable that:

[0076] The absorbent may further include, for example, a fibrous material in addition to the water-absorbent resin particles. The absorbent may be, for example, a mixture containing water-absorbent resin particles and fibrous materials. The mass ratio of the water-absorbent resin particles in the absorbent may be 2% by mass to 100% by mass, preferably 10% by mass to 80% by mass, and more preferably 20% by mass to 70% by mass, based on the total of the water-absorbent resin particles and fibrous materials. The absorbent may be configured, for example, in a form in which the water-absorbent resin particles and fibrous materials are uniformly mixed, in a form in which the water-absorbent resin particles are sandwiched between fibrous materials formed in a sheet or layer, or in other forms.

[0077] Examples of fibrous materials include pulverized wood pulp, cellulosic fibers such as cotton, cotton linters, rayon, cellulose acetate, etc., and synthetic fibers such as polyamides, polyesters, polyolefins, etc. The fibrous materials may also be mixtures of the above-mentioned fibers.

[0078] In order to further improve the shape retention of the absorbent before and during use, an adhesive binder may be added to the fibrous material to bond the fibers together. Examples of the adhesive binder include heat-fusible synthetic fibers, hot melt adhesives, adhesive emulsions, etc. The water-absorbent resin particles according to the present embodiment have excellent shape retention when used in an absorbent, so that the amount of adhesive binder used can be reduced.

[0079] Examples of heat-fusible synthetic fibers include fully melted binders such as polyethylene, polypropylene, and ethylene-propylene copolymers, and non-fully melted binders consisting of a side-by-side or core-sheath structure of polypropylene and polyethylene. In the above-mentioned non-fully melted binders, only the polyethylene portion is heat-fused. Examples of hot melt adhesives include blends of base polymers such as ethylene-vinyl acetate copolymer, styrene-isoprene-styrene block copolymer, styrene-butadiene-styrene block copolymer, styrene-ethylene-butylene-styrene block copolymer, styrene-ethylene-propylene-styrene block copolymer, and amorphous polypropylene with tackifiers, plasticizers, antioxidants, and the like.

[0080] The adhesive emulsion may be, for example, a polymer of at least one monomer selected from the group consisting of methyl methacrylate, styrene, acrylonitrile, 2-ethylhexyl acrylate, butyl acrylate, butadiene, ethylene, and vinyl acetate. These adhesive binders may be used alone or in combination of two or more.

[0081] The absorbent according to the present embodiment may further contain additives such as inorganic powder (e.g., amorphous silica), deodorant, pigment, dye, antibacterial agent, fragrance, adhesive, etc. These additives can impart various functions to the absorbent. When the water-absorbent resin particles contain inorganic particles, the absorbent may contain inorganic powder in addition to the inorganic particles in the water-absorbent resin particles. Examples of inorganic powder include silicon dioxide, zeolite, kaolin, clay, etc.

[0082] The shape of the absorbent body according to this embodiment is not particularly limited, and may be, for example, a sheet-like shape. The thickness of the absorbent body (for example, the thickness of a sheet-like absorbent body) may be, for example, 0.1 to 20 mm, or 0.3 to 15 mm.

[0083] The absorbent article according to the present embodiment may include, in addition to the absorbent body, a core wrap, a liquid-permeable top sheet, and a liquid-impermeable back sheet. The core wrap maintains the shape of the absorbent body. The liquid-permeable top sheet is disposed on the outermost side of the side into which the liquid to be absorbed penetrates. The liquid-impermeable back sheet is disposed on the outermost side of the side opposite to the side into which the liquid to be absorbed penetrates.

[0084] Examples of absorbent articles include diapers (e.g., paper diapers), toilet training pants, incontinence pads, sanitary products (sanitary napkins, tampons, etc.), sweat pads, pet sheets, parts for simple toilets, and animal waste treatment materials.

[0085] Fig. 1 is a cross-sectional view showing an example of an absorbent article. The absorbent article 100 shown in Fig. 1 includes an absorbent body 10, core wraps 20a and 20b, a liquid-permeable top sheet 30, and a liquid-impermeable back sheet 40. In the absorbent article 100, the liquid-impermeable back sheet 40, the core wrap 20b, the absorbent body 10, the core wrap 20a, and the liquid-permeable top sheet 30 are laminated in this order. In Fig. 1, there are some parts shown as having gaps between the members, but the members may be in close contact with each other without the presence of such gaps.

[0086] The absorbent body 10 includes water-absorbent resin particles 10a and a fiber layer 10b containing fibrous material. The water-absorbent resin particles 10a are dispersed in the fiber layer 10b.

[0087] The core wrap 20a is disposed on one side of the absorbent body 10 (the upper side of the absorbent body 10 in FIG. 1) in contact with the absorbent body 10. The core wrap 20b is disposed on the other side of the absorbent body 10 (the lower side of the absorbent body 10 in FIG. 1) in contact with the absorbent body 10. The absorbent body 10 is disposed between the core wrap 20a and the core wrap 20b.

[0088] The core wrap 20a and the core wrap 20b have, for example, a main surface of the same size as the absorbent 10. By using the core wrap, the shape retention of the absorbent can be maintained and the water-absorbent resin particles constituting the absorbent can be prevented from falling off or flowing. Examples of the core wrap include nonwoven fabric, woven fabric, tissue, synthetic resin film having liquid-permeable holes, and net-like sheet having mesh, and from the viewpoint of economy, tissue obtained by wet molding pulp is preferably used.

[0089] The liquid permeable top sheet 30 is disposed on the outermost side of the absorbent article 100, on the side into which the liquid to be absorbed penetrates. The liquid permeable top sheet 30 is disposed on the core wrap 20a in contact with the core wrap 20a. The liquid impermeable back sheet 40 is disposed on the outermost side of the absorbent article 100, on the side opposite the liquid permeable top sheet 30. The liquid impermeable back sheet 40 is disposed below the core wrap 20b in contact with the core wrap 20b. The liquid permeable top sheet 30 and the liquid impermeable back sheet 40 have, for example, a main surface that is wider than the main surface of the absorbent body 10, and the outer edges of the liquid permeable top sheet 30 and the liquid impermeable back sheet 40 extend around the absorbent body 10 and the core wraps 20a and 20b.

[0090] Examples of the liquid-permeable top sheet 30 include nonwoven fabrics and porous sheets. Examples of nonwoven fabrics include thermal bonded nonwoven fabrics, air-through nonwoven fabrics, resin bonded nonwoven fabrics, spunbonded nonwoven fabrics, melt-blown nonwoven fabrics, spunbonded / melt-blown / spunbonded nonwoven fabrics, air-laid nonwoven fabrics, spunlace nonwoven fabrics, and point-bonded nonwoven fabrics. Of these, thermal bonded nonwoven fabrics, air-through nonwoven fabrics, spunbonded nonwoven fabrics, and spunbonded / melt-blown / spunbonded nonwoven fabrics are preferably used.

[0091] The material of the liquid permeable top sheet 30 may be a resin or fiber known in the art, and may include polyolefins such as polyethylene (PE) and polypropylene (PP), polyesters such as polyethylene terephthalate (PET), polytrimethylene terephthalate (PTT), and polyethylene naphthalate (PEN), polyamides such as nylon, rayon, other synthetic resins or fibers, cotton, silk, hemp, and pulp (cellulose) fibers, from the viewpoint of increasing the strength of the liquid permeable top sheet 30. As the material of the liquid permeable top sheet 30, synthetic fibers are preferably used, and polyolefins and polyesters are particularly preferable. These materials may be used alone or in combination of two or more materials.

[0092] From the viewpoint of improving the liquid absorption performance of the absorbent article, it is desirable that the nonwoven fabric used in the liquid permeable top sheet 30 has a suitable hydrophilicity. From this viewpoint, the hydrophilicity measured according to "Hydrophilicity of Nonwoven Fabrics" (based on Paper Pulp Test Method No. 68 (2000)) described in WO 2011 / 086843 is preferably 5 to 200, and more preferably 10 to 150. Such a hydrophilic nonwoven fabric may be one of the above-mentioned nonwoven fabrics that uses a material that itself exhibits a suitable hydrophilicity, such as rayon fiber, or one that uses hydrophobic chemical fibers, such as polyolefin fibers and polyester fibers, that have been hydrophilized by a known method to impart a suitable hydrophilicity.

[0093] Examples of methods for hydrophilizing chemical fibers include a method of mixing hydrophobic chemical fibers with a hydrophilizing agent and then subjecting the mixture to a spunbonding process to obtain a nonwoven fabric, a method of adding a hydrophilizing agent when preparing a spunbonded nonwoven fabric from hydrophobic chemical fibers, or a method of impregnating a spunbonded nonwoven fabric from hydrophobic chemical fibers with a hydrophilizing agent after obtaining the nonwoven fabric from hydrophobic chemical fibers. Examples of hydrophilizing agents include anionic surfactants such as aliphatic sulfonates and higher alcohol sulfate salts, cationic surfactants such as quaternary ammonium salts, nonionic surfactants such as polyethylene glycol fatty acid esters, polyglycerin fatty acid esters, and sorbitan fatty acid esters, silicone surfactants such as polyoxyalkylene-modified silicones, and stain release agents made of polyester, polyamide, acrylic, and urethane resins.

[0094] The nonwoven fabric used in the liquid-permeable top sheet 30 is preferably appropriately bulky and has a large basis weight, from the viewpoints of imparting good liquid permeability, flexibility, strength, and cushioning properties to the absorbent article, and of increasing the liquid permeation rate of the absorbent article. The basis weight of the nonwoven fabric is preferably 5 to 200 g / m 2 and more preferably 8 to 150 g / m 2 and more preferably 10 to 100 g / m 2 The thickness of the nonwoven fabric is preferably from 20 to 1400 μm, more preferably from 50 to 1200 μm, and further preferably from 80 to 1000 μm.

[0095] The liquid-impermeable back sheet 40 prevents the liquid absorbed in the absorber 10 from leaking out from the back sheet 40 side to the outside. For the liquid-impermeable back sheet 40, a liquid-impermeable film mainly made of polyolefin resin such as polyethylene (PE) or polypropylene (PP), a breathable resin film, a composite film in which a breathable resin film is bonded to a nonwoven fabric such as spunbond or spunlace, or a spunbond / meltblown / spunbond (SMS) nonwoven fabric in which a water-resistant meltblown nonwoven fabric is sandwiched between high-strength spunbond nonwoven fabrics can be used. From the viewpoint of ensuring flexibility so as not to impair the wearing comfort of the absorbent article, the back sheet 40 is mainly made of low-density polyethylene (LDPE) resin and has a basis weight of 10 to 50 g / m 2 In addition, when a breathable material is used, stuffiness during wearing is reduced, and discomfort to the wearer can be alleviated.

[0096] The size relationship between the absorbent body 10, the core wraps 20a, 20b, the liquid permeable top sheet 30, and the liquid impermeable back sheet 40 is not particularly limited and is adjusted appropriately depending on the application of the absorbent article, etc. Furthermore, the method of maintaining the shape of the absorbent body 10 using the core wraps 20a, 20b is not particularly limited, and the absorbent body may be sandwiched between multiple core wraps as shown in Figure 1, or the absorbent body may be covered by one core wrap.

[0097] The absorbent 10 may be bonded to the liquid-permeable top sheet 30. By bonding the absorbent 10 and the liquid-permeable top sheet 30, the liquid is more smoothly guided to the absorbent, and an absorbent article with better liquid leakage prevention is easily obtained. When the absorbent 10 is sandwiched or covered by a core wrap, it is preferable that at least the core wrap and the liquid-permeable top sheet 30 are bonded, and it is more preferable that the core wrap and the absorbent 10 are bonded. Examples of bonding methods include a method of applying a hot melt adhesive to the liquid-permeable top sheet 30 in a longitudinal stripe shape, a spiral shape, or the like at a predetermined interval in the width direction, and a method of bonding using a water-soluble binder selected from starch, carboxymethyl cellulose, polyvinyl alcohol, polyvinylpyrrolidone, and other water-soluble polymers. In addition, when the absorbent 10 contains heat-fusible synthetic fibers, a method of bonding by heat fusion may be adopted.

[0098] The present invention also provides a method for measuring a liquid permeability retention rate of water-absorbent resin particles, which is represented by the following formula: Liquid permeability maintenance rate (%) = (liquid permeability rate of swollen gel / liquid permeability rate of dry powder) x 100

[0099] The dry powder liquid permeation rate is measured by a method including the following steps (A), (B) and (C) in this order. (A) 0.3 g of water-absorbent resin particles are uniformly dispersed in a cylindrical container having an inner diameter of 26 mm and equipped with a mesh-like bottom. (B) A small cylindrical container with an outer diameter of 25 mm and an inner diameter of 19 mm and equipped with a mesh-like bottom is inserted into the cylindrical container to form a measurement section. (C) Saline is poured into the cylindrical small container of the measurement section at a constant rate of 60 ml / min, and the amount of saline flowing out of the bottom of the measurement section within one minute from the start of the pouring is measured to determine the dry powder flow rate (g / min) of saline.

[0100] The swollen gel liquid permeation rate is measured by a method including the above steps (A) and (B) as well as the following steps (D) and (E) in this order. (D) The bottom side of the measurement section is immersed in 40 g of physiological saline in a container for 30 minutes, thereby causing the water-absorbent resin particles in the measurement section to swell. (E) 20 g of saline is poured into the small cylindrical container of the measurement section at once, and the amount of saline flowing out of the bottom of the measurement section within 1 minute from the start of the pouring is measured to determine the saline permeation rate through the swollen gel (g / min).

[0101] The higher the liquid permeability retention rate of the water-absorbent resin particles used in the absorbent body, the more likely it is that the occurrence of breakage after the absorbent body absorbs liquid can be suppressed. Therefore, the present invention can also be understood as a method for suppressing the occurrence of breakage after the absorbent body containing the water-absorbent resin particles absorbs liquid, including increasing the liquid permeability retention rate of the water-absorbent resin particles measured by the above-mentioned measurement method. Water-absorbent resin particles with a high liquid permeability retention rate tend to have excellent diffusibility of absorbed liquid, and absorbents containing the water-absorbent resin particles tend to have excellent shape retention. Therefore, the above method can also be understood as a method for improving the diffusibility of the water-absorbent resin particles, or a method for improving the shape retention of the absorbent body. The liquid permeability retention rate of the water-absorbent resin particles can be achieved, for example, by selecting the manufacturing conditions of the water-absorbent resin particles so that the uniformity of crosslinking in the water-absorbent resin particles is high. EXAMPLES

[0102] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0103] <Production of Water-Absorbent Resin Particles> [Example 1] A round-bottomed cylindrical separable flask with an inner diameter of 11 cm and an internal volume of 2 L was prepared, equipped with a reflux condenser, a dropping funnel, a nitrogen gas introduction tube, and a stirrer. A stirring blade (flat blade) 200, the outline of which is shown in FIG. 2, was attached to the stirrer. The stirring blade 200 has a shaft 200a and a flat plate portion 200b. The flat plate portion 200b is welded to the shaft 200a and has a curved tip. The flat plate portion 200b has four slits S extending along the axial direction of the shaft 200a. The four slits S are arranged in the width direction of the flat plate portion 200b, with the width of the two inner slits S being 1 cm and the width of the two outer slits S being 0.5 cm. The length of the flat plate portion 200b is about 10 cm, and the width of the flat plate portion 200b is about 6 cm. Next, 293 g of n-heptane was added to the flask as a hydrocarbon dispersion medium, and 0.736 g of maleic anhydride-modified ethylene-propylene copolymer (Hiwax 1105A, Mitsui Chemicals, Inc.) was added as a polymeric dispersant to obtain a mixture. The mixture was heated to 80°C while stirring to dissolve the dispersant, and then cooled to 50°C.

[0104] On the other hand, 92.0g (1.03 mol) of 80.5% by mass acrylic acid aqueous solution was placed in a 300ml beaker as an ethylenically unsaturated monomer, and 147.7g of 20.9% by mass sodium hydroxide aqueous solution was added dropwise while cooling from the outside to perform 75 mol% neutralization. Then, 0.092g of hydroxyethyl cellulose (Sumitomo Seika Chemicals Co., Ltd., HEC AW-15F) as a thickener, 0.092g (0.339 mmol) of 2,2'-azobis(2-amidinopropane) dihydrochloride as a radical polymerization initiator, and 0.018g (0.067 mmol) of potassium persulfate, and 0.0046g (0.026 mmol) of ethylene glycol diglycidyl ether as an internal crosslinking agent were added and dissolved to prepare the first stage aqueous liquid.

[0105] The prepared aqueous solution was added to the reaction solution in the separable flask and stirred for 10 minutes. Next, 0.736 g of sucrose stearate (Mitsubishi Chemical Foods Corporation, Ryoto Sugar Ester S-370, HLB: 3) was dissolved as a surfactant in 6.62 g of n-heptane under heating to prepare a surfactant solution. The surfactant solution was further added to the reaction solution, and the inside of the system was thoroughly replaced with nitrogen while stirring at a stirrer speed of 425 rpm. Then, the flask was immersed in a water bath at 70°C to raise the temperature, and polymerization was carried out for 60 minutes to obtain a first-stage polymerization slurry.

[0106] On the other hand, 128.8g (1.44 mol) of 80.5% by mass acrylic acid aqueous solution was placed in another 500ml beaker as an ethylenically unsaturated monomer, and 159.0g of 27% by mass sodium hydroxide aqueous solution was added dropwise while cooling from the outside to perform 75 mol% neutralization. After that, 0.129g (0.476 mmol) of 2,2'-azobis(2-amidinopropane) dihydrochloride and 0.026g (0.096 mmol) of potassium persulfate as radical polymerization initiators, and 0.0116g (0.067 mmol) of ethylene glycol diglycidyl ether as an internal crosslinking agent were added and dissolved to prepare the second aqueous solution.

[0107] The separable flask system was cooled to 25° C. while stirring at a stirrer speed of 650 rpm. Then, the entire amount of the second-stage aqueous liquid was added to the first-stage polymerization slurry liquid, and the system was replaced with nitrogen for 30 minutes. Thereafter, the flask was again immersed in a 70° C. water bath to raise the temperature, and a polymerization reaction was carried out for 60 minutes to obtain a hydrous gel polymer.

[0108] 0.589g of 45% by mass of pentasodium diethylenetriamine pentacetate aqueous solution was added to the hydrous gel polymer after the second-stage polymerization under stirring. Then, the flask was immersed in an oil bath set at 125°C, and 207.9g of water was extracted from the system by azeotropic distillation of n-heptane and water while refluxing n-heptane. Then, 4.42g (0.507mmol) of 2% by mass of ethylene glycol diglycidyl ether aqueous solution was added to the flask as a surface crosslinking agent, and the mixture was kept at 83°C for 2 hours.

[0109] Thereafter, n-heptane was evaporated at 125°C to dry the mixture, thereby obtaining polymer particles (dried product). The polymer particles were passed through a sieve with an opening of 850 μm, and 0.2% by mass of amorphous silica (Oriental Silicas Corporation, Toxil NP-S) relative to the mass of the polymer particles was mixed with the polymer particles, thereby obtaining 232.3 g of water-absorbent resin particles containing amorphous silica. The median particle diameter of the water-absorbent resin particles was 361 μm.

[0110] [Example 2] Except for changing the amount of water discharged from the system to 224.3 g, the same procedure as in Example 1 was carried out to obtain 231.0 g of water-absorbent resin particles. The median particle size of the water-absorbent resin particles was 342 μm.

[0111] [Example 3] Except for changing the amount of water discharged from the system to 234.6 g, the same procedure as in Example 1 was carried out to obtain 232.1 g of water-absorbent resin particles. The median particle diameter of the water-absorbent resin particles was 355 μm.

[0112] [Example 4] In the preparation of the first stage aqueous liquid, 2,2'-azobis(2-amidinopropane) dihydrochloride was not used as a radical polymerization initiator, and the amount of potassium persulfate used was changed to 0.0736g (0.272) millimoles, the amount of ethylene glycol diglycidyl ether used as an internal crosslinking agent was changed to 0.010g (0.057 millimoles), the amount of potassium persulfate used was not used as a radical polymerization initiator in the preparation of the second stage aqueous liquid, and the amount of potassium persulfate used was changed to 0.090g (0.333 millimoles), and the amount of water extracted from the system was changed to 247.3g. Except for this, 231.5g of water absorbent resin particles were obtained in the same manner as in Example 1. The median particle diameter of the water absorbent resin particles was 359μm.

[0113] [Example 5] Except for changing the amount of ethylene glycol diglycidyl ether used as an internal crosslinking agent in the preparation of the first-stage aqueous liquid to 0.010 g (0.057 mmol), and changing the amount of water extracted from the system to 238.5 g, the same procedure as in Example 1 was carried out to obtain 222.4 g of water-absorbent resin particles. The median particle diameter of the water-absorbent resin particles was 354 μm.

[0114] [Example 6] In the preparation of the first stage aqueous liquid, 2,2'-azobis(2-amidinopropane) dihydrochloride was not used as a radical polymerization initiator, and the amount of potassium persulfate used was changed to 0.0736g (0.272mmol), the amount of ethylene glycol diglycidyl ether used as an internal crosslinking agent was changed to 0.010g (0.057mmol), the amount of potassium persulfate used was not used as a radical polymerization initiator in the preparation of the second stage aqueous liquid, and the amount of potassium persulfate used was changed to 0.090g (0.334mmol), and the amount of water taken out of the system was changed to 257.6g, except that the procedure was the same as in Example 1 to obtain 229.8g of water-absorbent resin particles. The median particle diameter of the water-absorbent resin particles was 362μm.

[0115] [Example 7] Except for changing the amount of water to be extracted from the system to 201.3 g and changing the amount of 2 mass% ethylene glycol diglycidyl ether aqueous solution used as a surface crosslinking agent to 6.62 g (0.761 mmol), the same procedure as in Example 1 was carried out to obtain 224.0 g of water absorbent resin particles. The median particle diameter of the water absorbent resin particles was 356 μm.

[0116] [Comparative Example 1] A round-bottomed cylindrical separable flask with an inner diameter of 11 cm and a volume of 2 L was prepared, equipped with a reflux condenser, a dropping funnel, a nitrogen gas inlet tube, and a stirring blade with two stages of four inclined paddle blades with a blade diameter of 5 cm. 293 g of n-heptane was placed in the flask as a hydrocarbon dispersion medium, and 0.736 g of maleic anhydride-modified ethylene-propylene copolymer (Hiwax 1105A, Mitsui Chemicals, Inc.) was added as a polymeric dispersant to obtain a mixture. The mixture was heated to 80°C while stirring to dissolve the dispersant, and then cooled to 50°C.

[0117] On the other hand, 92.0g (1.03 mol) of 80.5% by mass acrylic acid aqueous solution was placed in a 300ml beaker as an ethylenically unsaturated monomer, and 147.7g of 20.9% by mass sodium hydroxide aqueous solution was added dropwise while cooling from the outside to neutralize 75% by mole. Then, 0.092g of hydroxyethyl cellulose (Sumitomo Seika Chemicals Co., Ltd., HEC AW-15F) as a thickener, 0.0736g (0.272 mmol) of potassium persulfate as a radical polymerization agent, and 0.010g (0.057 mmol) of ethylene glycol diglycidyl ether as an internal crosslinking agent were added and dissolved to prepare the first aqueous solution.

[0118] The prepared aqueous solution was added to the reaction solution in the separable flask and stirred for 10 minutes. Next, 0.736 g of sucrose stearate (Mitsubishi Chemical Foods Corporation, Ryoto Sugar Ester S-370, HLB: 3) was dissolved as a surfactant in 6.62 g of n-heptane under heating to prepare a surfactant solution. The surfactant solution was further added to the reaction solution, and the inside of the system was thoroughly replaced with nitrogen while stirring at a stirrer speed of 550 rpm. Then, the flask was immersed in a water bath at 70°C to raise the temperature, and polymerization was carried out for 60 minutes to obtain a first-stage polymerization slurry.

[0119] On the other hand, 128.8g (1.44 mol) of 80.5% by mass acrylic acid aqueous solution was placed in another 500ml beaker as an ethylenically unsaturated monomer, and 159.0g of 27% by mass sodium hydroxide aqueous solution was added dropwise while cooling from the outside to carry out 75 mol% neutralization. After that, 0.090g (0.333 mmol) of potassium persulfate was added and dissolved as a radical polymerization initiator to prepare the second stage aqueous solution.

[0120] The separable flask system was cooled to 25°C while stirring at a stirrer speed of 1000 rpm. Next, the entire amount of the second stage aqueous liquid was added to the first stage polymerization slurry liquid, and the system was replaced with nitrogen for 30 minutes. Thereafter, the flask was again immersed in a 70°C water bath to raise the temperature, and the polymerization reaction was carried out for 60 minutes. Thereafter, 0.580g (0.067 mmol) of a 2% by mass aqueous solution of ethylene glycol diglycidyl ether was added as a crosslinking agent for post-polymerization crosslinking, and a hydrous gel polymer was obtained.

[0121] 0.265g of 45% by mass of diethylenetriaminepentaacetic acid pentasodium aqueous solution was added to the hydrous gel polymer after the second-stage polymerization under stirring. Then, the flask was immersed in an oil bath set at 125°C, and 259.4g of water was extracted from the system by azeotropic distillation of n-heptane and water while refluxing n-heptane. Then, 6.30g (0.723 mmol) of 2% by mass of ethylene glycol diglycidyl ether aqueous solution was added to the flask as a surface crosslinking agent, and the mixture was kept at 83°C for 2 hours.

[0122] Thereafter, n-heptane was evaporated at 125°C to dry the mixture, thereby obtaining polymer particles (dried product). The polymer particles were passed through a sieve with an opening of 850 μm, and 0.5% by mass of amorphous silica (Toxil NP-S, Oriental Silicas Corporation) relative to the mass of the polymer particles was mixed with the polymer particles, thereby obtaining 230.8 g of water-absorbent resin particles containing amorphous silica. The median particle size of the water-absorbent resin particles was 349 μm.

[0123] [Comparative Example 2] 230.8 g of water-absorbent resin particles were obtained in the same manner as in Comparative Example 1, except that 0.012 g (0.067 mmol) of ethylene glycol diglycidyl ether was added as an internal crosslinking agent in the preparation of the second-stage aqueous liquid, a 2 mass% ethylene glycol diglycidyl ether aqueous solution for post-polymerization crosslinking was not used, the amount of water extracted from the system was changed to 278.9 g, the amount of 2 mass% ethylene glycol diglycidyl ether aqueous solution used as a surface crosslinking agent was changed to 4.42 g (0.507 mmol), and the amount of amorphous silica mixed with respect to the polymer particles was changed to 0.2 mass%. The median particle diameter of the water-absorbent resin particles was 358 μm.

[0124] [Comparative Example 3] The amount of ethylene glycol diglycidyl ether used as an internal crosslinking agent in the preparation of the first-stage aqueous liquid was changed to 0.011 g (0.063 mmol), 0.013 g (0.075 mmol) of ethylene glycol diglycidyl ether was added as an internal crosslinking agent in the preparation of the second-stage aqueous liquid, a crosslinking agent for post-polymerization crosslinking was not used, the amount of water extracted from the system was changed to 262.6 g, the amount of 2 mass% ethylene glycol diglycidyl ether aqueous solution used as a surface crosslinking agent was changed to 9.93 g (1.14 mmol), and amorphous silica was not mixed. Except for this, 230.3 g of water-absorbent resin particles were obtained in the same manner as in Comparative Example 1. The median particle diameter of the water-absorbent resin particles was 349 μm.

[0125] The obtained water-absorbent resin particles were evaluated for the liquid permeability retention rate, saline water retention capacity, median particle size, no-pressure DW 3-minute value, and rupture property of the absorbent body by the following methods. Note that the saline used in this example was a 0.9 mass % NaCl aqueous solution.

[0126] <Measurement of Liquid Flow Maintenance Rate> [Measurement of liquid permeation rate through swollen gel] The measurement of the swollen gel liquid permeation rate was carried out using the device shown in Figure 3. The measurement section 60 has a cylindrical container 61 made of acrylic resin with a 250-mesh nylon mesh sheet 64 at its bottom, and a small cylindrical container 62 made of acrylic resin similarly with a nylon mesh sheet 63 at its bottom, placed inside the cylindrical container 61. The cylindrical container 61 has an inner diameter of 26 mm, an outer diameter of 40 mm, and a height of 140 mm. The small cylindrical container 62 has an inner diameter of 19 mm, an outer diameter of 25 mm, a height of 120 mm, and a mass of 30 g. The small cylindrical container 62 can move up and down inside the cylindrical container 61 without resistance.

[0127] The measurement of the swollen gel liquid permeation rate was carried out as follows: 0.3 g of water-absorbent resin particles 10a were uniformly scattered in a cylindrical container 61, a small cylindrical container 62 was inserted from above, and the water-absorbent resin particles 10a were sandwiched between a nylon mesh sheet 63 and a nylon mesh sheet 64 to form a measurement section 60 having the water-absorbent resin particles 10a in a dry state.

[0128] Separately, a petri dish containing 40±0.1 g of physiological saline was prepared, and the bottom side of the measurement part 60 was immersed in the physiological saline for 30 minutes, causing the water-absorbent resin particles 10a to absorb the physiological saline and swell to saturation, thereby obtaining a measurement part 60 having a swollen gel.

[0129] A wire mesh 67 with a size of 10 cm square and 2 mm mesh size was placed on a petri dish 66 with an inner diameter of about 90 mm, whose empty mass (Wa) had been measured beforehand, and the measurement section 60 containing the above-mentioned swollen gel was placed on the wire mesh 67. 20 g of physiological saline solution 65 was poured into the measurement section 60 at once from the top of the small cylindrical container 62. The mass (Wb) of the petri dish 66 containing the physiological saline solution 65 that had passed through the swollen gel within 1 minute from the start of the pouring was measured, and the liquid passing speed (g / min) was calculated using the following formula. The results are shown in Table 1. Liquid passing rate (g / min)=Wb-Wa

[0130] [Measurement of dry powder permeability] For the measurement of the dry powder liquid permeation rate, dry water absorbent resin particles stored at 25°C and 45% humidity (RH) were used. The liquid permeation rate was measured at 25°C and 45% humidity (RH). As in the measurement of the swollen gel liquid permeation rate, a measurement section 60 having dry water absorbent resin particles 10a was formed. Physiological saline was poured into the measurement section 60 for 1 minute at a constant rate of 60 ml / min using an automatic pump (INTEGRA DOSE IT P910) from the top of the cylindrical small container 62. The liquid that passed through the water absorbent resin particles 10a in the measurement section 60 and flowed out from the bottom of the measurement section 60 was collected in another container, and the mass of the collected liquid was measured to determine the amount of liquid that passed through the dry powder in 1 minute from the start of the pouring (liquid permeation rate (g / min)). The results are shown in Table 1.

[0131] The liquid permeability maintenance rate was calculated from the measured swollen gel liquid permeability rate and dry powder liquid permeability rate. The results are shown in Table 1. Liquid permeability maintenance rate (%) = (liquid permeability rate of swollen gel / liquid permeability rate of dry powder) x 100

[0132] <Measurement of saline water retention> A cotton bag (membrane broad 60, 100 mm wide x 200 mm long) containing 2.0 g of absorbent resin particles was placed in a 500 ml beaker. 500 g of saline was poured into the cotton bag containing the absorbent resin particles at once so as not to cause the bag to swell, the top of the cotton bag was tied with a rubber band, and the bag was left to stand for 30 minutes to swell the absorbent resin particles. After 30 minutes, the cotton bag was dehydrated for 1 minute using a dehydrator (manufactured by Kokusan Co., Ltd., product number: H-122) set to a centrifugal force of 167 G, and the mass Wc (g) of the cotton bag containing the swollen gel after dehydration was measured. The same operation was performed without adding the absorbent resin particles, and the empty mass Wd (g) of the cotton bag when wet was measured, and the saline water retention was calculated from the following formula. The results are shown in Table 1. Saline water retention capacity (g / g) = [Wc-Wd] / 2.0

[0133] <Measurement of median particle size (particle size distribution)> 50 g of water-absorbent resin particles were used for measuring the median particle size (particle size distribution). JIS standard sieves were arranged in the following order from the top: a sieve with an opening of 850 μm, a sieve with an opening of 500 μm, a sieve with an opening of 425 μm, a sieve with an opening of 300 μm, a sieve with an opening of 250 μm, a sieve with an opening of 180 μm, a sieve with an opening of 150 μm, and a tray.

[0134] The water-absorbent resin particles were placed on the top sieve of the combination, and classified in accordance with JIS Z 8815 (1994) using a Rotap type shaker (manufactured by Iida Manufacturing Co., Ltd.). After classification, the mass of the water-absorbent resin particles remaining on each sieve was calculated as a mass percentage relative to the total amount to obtain a particle size distribution. By accumulating the particles on the sieves in order from the largest particle diameter with respect to this particle size distribution, the relationship between the sieve opening and the accumulated value of the mass percentage of the water-absorbent resin particles remaining on the sieves was plotted on a logarithmic probability paper. By connecting the plots on the probability paper with a straight line, the particle size corresponding to an accumulated mass percentage of 50 mass% was determined as the median particle size.

[0135] <Measurement of non-pressure DW> The unpressurized DW of the water-absorbent resin particles was measured using a measuring device shown in Fig. 4. The measurement was carried out five times for one type of water-absorbent resin particle, and the average value of the three measured values ​​excluding the minimum and maximum values ​​was calculated. The measurement device includes a burette unit 1, a conduit 5, a measurement table 13, a nylon mesh sheet 15, a stand 11, and a clamp 3. The burette unit 1 includes a burette tube 21 with a scale, a rubber plug 23 that seals the opening at the top of the burette tube 21, a cock 22 connected to the tip of the bottom of the burette tube 21, and an air introduction tube 25 and a cock 24 connected to the bottom of the burette tube 21. The burette unit 1 is fixed with a clamp 3. The flat measurement table 13 has a through hole 13a with a diameter of 2 mm formed in its center, and is supported by a stand 11 whose height is variable. The through hole 13a of the measurement table 13 and the cock 22 of the burette unit 1 are connected by a conduit 5. The inner diameter of the conduit 5 is 6 mm.

[0136] The measurement was performed in an environment with a temperature of 25°C and a humidity of 60±10%. First, the cocks 22 and 24 of the burette part 1 were closed, and physiological saline solution 50 adjusted to 25°C was poured into the burette tube 21 from the opening at the top of the burette tube 21. The concentration of physiological saline solution (0.9% by mass) is based on the mass of the NaCl aqueous solution. After sealing the opening of the burette tube 21 with a rubber plug 23, the cocks 22 and 24 were opened. The inside of the conduit 5 was filled with 0.9% by mass saline solution 50 so as to prevent air bubbles from entering. The height of the measurement table 13 was adjusted so that the height of the water surface of the physiological saline solution that reached the through hole 13a was the same as the height of the upper surface of the measurement table 13. After the adjustment, the water surface height of the physiological saline solution 50 in the burette tube 21 was read on the scale of the burette tube 21, and that position was set as the zero point (the reading at 0 seconds).

[0137] A nylon mesh sheet 15 (100 mm x 100 mm, 250 mesh, thickness about 50 μm) was laid near the through hole 13a on the measurement table 13, and a cylinder with an inner diameter of 30 mm and a height of 20 mm was placed in the center of the sheet. 1.00 g of water-absorbent resin particles 10a was uniformly spread on the cylinder. After that, the cylinder was carefully removed, and a sample in which the water-absorbent resin particles 10a were circularly dispersed in the center of the nylon mesh sheet 15 was obtained. Next, the nylon mesh sheet 15 on which the water-absorbent resin particles 10a were placed was moved quickly so that the center of the sheet was at the position of the through hole 13a, without dissipating the water-absorbent resin particles 10a, and the measurement was started. The time when air bubbles were first introduced into the burette tube 21 from the air introduction tube 25 was defined as the start of water absorption (0 seconds).

[0138] The amount of reduction in the saline solution 50 in the burette tube 21 (i.e., the amount of saline solution absorbed by the water-absorbent resin particles 10a) was successively read in increments of 0.1 ml, and the amount of reduction in the amount of saline solution 50 We (g) 3 minutes after the start of water absorption by the water-absorbent resin particles 10a was read. From We, the 3-minute value of the no-pressure DW was calculated by the following formula. The no-pressure DW is the amount of water absorbed per 1.00 g of the water-absorbent resin particles 10a. The results are shown in Table 1. 3-minute value of unpressurized DW (ml / g) = We / 1.00

[0139] <Measurement of absorbent tear resistance> [Preparation of absorbent articles for evaluation] Using a pad former manufactured by Autech Co., Ltd., 10 g of water-absorbent resin particles and 6.67 g of crushed pulp were uniformly mixed by air papermaking to produce an absorbent body measuring 40 cm x 12 cm. The size was 42 cm x 14 cm, and the basis weight was 16 g / m. 2 The absorbent body was placed on a tissue paper of 40 cm×12 cm, and 0.4 g of ion-exchanged water was sprayed on it with a spray bottle, and a tissue of 40 cm×12 cm was placed on the absorbent body to produce a laminate. Next, a wire mesh of 62 cm×22 cm with a mesh size of 2 mm was placed on the laminate, and the laminate was pressed at a pressure of 0.141 MPa using a press (small air press, Imoto Manufacturing Co., Ltd.). After pressing, the wire mesh was removed from the laminate.

[0140] After pressing, the laminate was cut with a roll cutter at a distance of 15 cm from the center in the longitudinal direction to a length of 30 cm. 2 The laminate was sandwiched between two 34 cm x 14 cm polyethylene air-through type porous liquid-permeable sheets (hereinafter also referred to as "liquid-permeable sheets"), and the four sides of the two liquid-permeable sheets sandwiching the laminate were pressed together using a heat sealer (Fuji Impulse Sealer, model number: FI-450-5, manufactured by Fuji Impulse) to obtain an absorbent article for evaluation 100'. During pressing, any portions of the tissue protruding from the absorbent body were sandwiched between the liquid-permeable sheets and pressed together.

[0141] [Preparation of test solution] Put an appropriate amount of distilled water into a 10L container, add 100g of sodium chloride, 3.0g of calcium chloride dihydrate, and 6.0g of magnesium chloride hexahydrate, and dissolve them. Next, add 0.25g of polyoxyethylene nonylphenyl ether, and further add distilled water to make the total mass 10kg. Furthermore, by coloring with a small amount of Blue No. 1, the test liquid for measuring the rupture property was prepared.

[0142] [Measurement of absorber rupture time 1] The absorbent rupture time was measured in a room at a temperature of 25±2°C using a U-shaped device 51 (depth 14 cm, made of acrylic) shown in FIG. 5. The opening width w of the U-shaped device 51 was 21 cm, and the depth d was 18.5 cm, and the opening was used so that it was facing upward. A 14 cm×6.5 cm thick paper 52 was placed on the bottom of the U-shape to form a flat bottom part with a width of 6.5 cm×depth of 14 cm. The absorbent article 100′ for evaluation was placed on the U-shaped device 51 with the center of the thick paper 52 aligned and the longitudinal direction of the absorbent article 100′ for evaluation aligned with the curve of the U-shaped device 51. A cylindrical cylinder 53 having an inner diameter of 2 cm, an outer diameter of 3 cm, a height of 6.5 cm, and a mass of 60 g was placed at the center of the absorbent article for evaluation 100', and 80 ml of the above test liquid adjusted to 25±1° C. was poured into the cylinder 53. While the test liquid was being poured, it was continued to be poured so as to maintain the liquid level of the test liquid at about 5 cm from the bottom of the cylinder.

[0143] After the test liquid poured into the cylinder 53 was completely absorbed by the absorbent article for evaluation 100', the cylinder 53 was removed from the top of the absorbent article for evaluation 100'. Three minutes after the start of pouring the test liquid, the cylinder 53 was placed again at the center of the absorbent article for evaluation 100' placed on the U-shaped device 51, and 80 ml of the test liquid (second time) was poured in the same manner as above and absorbed into the absorbent article for evaluation 100'.

[0144] Six minutes after the start of the first test liquid injection, a piece of cardboard (with a basis weight of 3,500 g / m) of the same size as the absorbent article 100′ for evaluation was 2 The absorbent article 100' for evaluation was placed on a cardboard sheet, and both ends in the longitudinal direction were attached with adhesive tape to fix the absorbent article 100' for evaluation to the cardboard. The fixed absorbent article 100' for evaluation was placed in a transparent polyethylene bag with a zipper (40 cm x 28 cm, thickness 0.04 mm, Unipack, manufactured by Nippon Seisakusho Co., Ltd., K-4) with three 1 cm cuts for removing air. When placing the absorbent article 100' for evaluation in the transparent bag, the corners of the bag and the corners of the absorbent article 100' for evaluation were placed so as to match, and the remaining part of the bag was folded back and fixed with adhesive tape, and the bag was filled so that the entire bag was approximately the same size as the absorbent article 100' for evaluation.

[0145] The filled absorbent article for evaluation 100' was centrifuged at a centrifugal force of 27.5 G (rotation speed: 405 r / min) 11 minutes after the start of the first test liquid pouring. The centrifugation was performed by fixing the filled absorbent article for evaluation 100' to a turntable with a diameter of 30 cm with packing tape so that the surface of the absorbent article for evaluation 100' was perpendicular to the rotation axis and the rotation axis was at the center of the absorbent article for evaluation 100'.

[0146] Centrifugation was interrupted every minute from the start of centrifugation until the fourth minute, and every two minutes after four minutes had passed, and the absorbent body was visually checked for any tears after absorption. The total centrifugation time until tears were observed was taken as the tear time. A longer tear time can be considered to indicate better performance. Measurements were performed for up to 20 minutes, and if no tears were observed in the absorbent body during this time, it was evaluated as "20 minutes or more." The results are shown in Table 1.

[0147] [Measurement of absorber rupture time 2] After the second injection of the test liquid, 80 ml of the test liquid (third injection) was injected in the same manner after another 3 minutes, and the subsequent operations were delayed by 3 minutes each, but the same procedure as in Measurement 1 of the absorbent body rupture time was followed to evaluate the rupture properties of the absorbent body obtained in the examples. The results are shown in Table 1.

[0148] [Table 1]

[0149] In the absorbent body using the water-absorbent resin particles of the Examples having a certain or higher liquid permeability maintenance rate, the rupture time was 20 minutes or more in the rupture property measurement in Measurement 1 (test liquid was added twice), and it was confirmed that the occurrence of rupture in the absorbent body after absorbing liquid was suppressed. In the rupture property measurement in Measurement 2 (test liquid was added three times), which is a stricter condition, it was confirmed that the rupture property was further suppressed in Examples 1 to 3 and 7, especially Examples 1 and 7. [Explanation of symbols]

[0150] 1...burette part, 3...clamp, 5...conduit, 10...absorbent body, 10a...water-absorbent resin particles, 10b...fiber layer, 11...frame, 13...measurement table, 13a...through hole, 15, 63, 64...nylon mesh sheet, 20a, 20b...core wrap, 21...burette tube, 22...cock, 23...rubber stopper, 24...cock, 25...air introduction tube, 30...liquid-permeable top sheet, 40...liquid-impermeable back sheet, 50...saline solution, 51...U-shaped device, 52...cardboard, 53...cylindrical cylinder, 60...measurement part, 61...cylindrical container, 62...small cylindrical container, 65...saline solution, 66...petri dish, 67...wire mesh, 100, 100'...absorbent article, 200...stirring blade, 200a...shaft, 200b...flat plate part, S...slit.

Claims

1. The present invention comprises: polymer particles including a crosslinked polymer having monomer units derived from an ethylenically unsaturated monomer including acrylic acid; and a plurality of inorganic particles disposed on the surfaces of the polymer particles; A water-absorbent resin particle having a liquid permeability maintenance rate of 10% or more, which is represented by the following formula using a dry powder liquid permeability rate measured by a method including the following steps (A), (B), and (C) in this order, and a swollen gel liquid permeability rate measured by a method including the following steps (A), (B), (D), and (E) in this order: Liquid permeability maintenance rate (%)=(liquid permeability rate of swollen gel / liquid permeability rate of dry powder)×100 (A) 0.3 g of water-absorbent resin particles are uniformly dispersed in a cylindrical container having an inner diameter of 26 mm and equipped with a mesh-like bottom. (B) A small cylindrical container with an outer diameter of 25 mm and an inner diameter of 19 mm and equipped with a mesh-like bottom is inserted into the cylindrical container to form a measurement section. (C) Physiological saline is poured into the cylindrical small container of the measurement section at a constant rate of 60 ml / min, and the amount of saline flowing out from the bottom of the measurement section within one minute from the start of the pouring is measured to determine the dry powder permeation rate (g / min) of the saline. (D) The bottom side of the measurement section is immersed in 40 g of physiological saline in a container for 30 minutes to swell the water-absorbent resin particles in the measurement section. (E) 20 g of saline is poured into the small cylindrical container of the measurement section at once, and the amount of saline flowing out of the bottom of the measurement section within 1 minute from the start of the pouring is measured to determine the saline permeation rate (g / min) through the swollen gel.

2. 2. The water-absorbent resin particles according to claim 1, wherein the swollen gel liquid permeation rate is 2.5 g / min or more.

3. An absorbent comprising the water-absorbent resin particles according to claim 1 or 2.

4. An absorbent article comprising the absorbent body according to claim 3.

5. 5. The absorbent article of claim 4 which is a diaper.

6. Measuring the dry powder liquid permeation rate by a method including the following steps (A), (B) and (C) in this order; A method for measuring a liquid permeability maintenance rate of a water-absorbent resin particle represented by the following formula, comprising measuring a swollen gel liquid permeability rate by a method including the following steps (A), (B), (D) and (E) in this order: Liquid permeability maintenance rate (%)=(liquid permeability rate of swollen gel / liquid permeability rate of dry powder)×100 (A) 0.3 g of water-absorbent resin particles are uniformly dispersed in a cylindrical container having an inner diameter of 26 mm and equipped with a mesh-like bottom. (B) A small cylindrical container with an outer diameter of 25 mm and an inner diameter of 19 mm and equipped with a mesh-like bottom is inserted into the cylindrical container to form a measurement section. (C) Physiological saline is poured into the cylindrical small container of the measurement section at a constant rate of 60 ml / min, and the amount of saline flowing out from the bottom of the measurement section within one minute from the start of the pouring is measured to determine the dry powder permeation rate (g / min) of the saline. (D) The bottom side of the measurement section is immersed in 40 g of physiological saline in a container for 30 minutes to swell the water-absorbent resin particles in the measurement section. (E) 20 g of saline is poured into the small cylindrical container of the measurement section at once, and the amount of saline flowing out of the bottom of the measurement section within 1 minute from the start of the pouring is measured to determine the saline permeation rate (g / min) through the swollen gel.

Citation Information

Patent Citations

  • Method for preparing porous super absorbent polymer

    EP3412711A1

  • Water-absorbing agent and production method thereof

    JP2005344103A

  • Water absorbent and method for producing the same

    JP2010540207A

  • Absorbent articles having improved absorption properties

    JP2014515987A

  • Absorbent article

    JP2018164732A