RHO ZEOLITE AND METHOD FOR PRODUCING RHO ZEOLITE

A novel production method for RHO type zeolite using sodium, cesium, and silicon sources with seed crystals achieves desired XRD peak intensities and molar ratios, enhancing separation membrane performance.

JP7588665B2Active Publication Date: 2024-11-22NGK CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2022581309
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-02-10
Filing Date
2022-01-27
Publication Date
2024-11-22
Estimated Expiration
2042-01-27

AI Technical Summary

Technical Problem

Existing methods for producing RHO type zeolite do not yield zeolites with desired properties, such as specific X-ray diffraction peak intensities and molar ratios, which are crucial for applications like separation membranes.

Method used

A novel method involving mixing sodium, cesium, and silicon sources with seed crystals in water, followed by hydrothermal synthesis, to produce RHO type zeolite with controlled molar ratios and peak intensities, eliminating the need for organic structure-directing agents.

Benefits of technology

The method produces RHO type zeolite with unique XRD peak intensities and molar ratios, enabling the formation of high-permeation-rate separation membranes with improved stability and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588665000008
    Figure 0007588665000008
  • Figure 0007588665000009
    Figure 0007588665000009
  • Figure 0007588665000010
    Figure 0007588665000010
Patent Text Reader

Abstract

In this RHO zeolite, when a peak at a lattice spacing of 9.96-11.25 Å as measured by powder X-ray diffraction is designated as a reference peak and the intensity of the reference peak is designated as 100, the relative intensity of a peak at a lattice spacing of 4.59-4.85 Å is 150-300, the relative intensity of a peak at a lattice spacing of 3.55-3.64 Å is 200-500, and the relative intensity of a peak at a lattice spacing of 2.98-3.06 Å is 100-200.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an RHO type zeolite and a method for producing an RHO type zeolite. [Reference to Related Applications] This application claims the benefit of priority from Japanese patent application JP2021-19690, filed on February 10, 2021, the entire disclosure of which is incorporated herein by reference. [Background technology]

[0002] Zeolites with various structures are known, one of which is the RHO type. For example, Japanese Patent Publication No. 6631663 (Document 1) and Japanese Patent Publication No. 2020-66564 (Document 2) disclose a method for producing RHO type zeolite. Specifically, in the production method of Document 1, a crown ether, an alkali, and water are mixed to prepare a crown ether-alkali aqueous solution. Next, the aqueous solution is added to an aluminum atom raw material solution, mixed uniformly, and then a silicon atom raw material-containing liquid is dropped to prepare an aqueous gel. Then, a zeolite having an RHO type structure is obtained by hydrothermally synthesizing the aqueous gel. In addition, in the example of Document 2, aluminum isopropoxide is mixed and stirred in a predetermined aqueous solution, and then cesium fluoride and tetraethyl orthosilicate are mixed in the aqueous solution. After stirring the aqueous solution, hydrogen fluoride is mixed to obtain a raw material composition. Then, an RHO type zeolite is obtained using the raw material composition.

[0003] Meanwhile, zeolites are being considered or put to practical use in various applications, such as separation of specific gases, adsorption of molecules, etc. Therefore, novel zeolites are constantly being sought to broaden the options for zeolites having desired properties. Summary of the Invention

[0004] The present invention is directed to RHO zeolites, and has an object to provide novel RHO zeolites.

[0005] In the RHO zeolite according to a preferred embodiment of the present invention, when a peak at a lattice spacing of 9.96 to 11.25 Å is used as a reference peak and the intensity of the reference peak is taken as 100, the relative intensity of the peak at a lattice spacing of 4.59 to 4.85 Å is 150 to 300, the relative intensity of the peak at a lattice spacing of 3.55 to 3.64 Å is 200 to 500, and the relative intensity of the peak at a lattice spacing of 2.98 to 3.06 Å is 100 to 200, in measurement by powder X-ray diffraction method. The molar ratio of sodium to aluminum is 0.1 to 1. do.

[0006] According to the present invention, a novel RHO-type zeolite can be provided.

[0007] Preferably, the molar ratio of silicon / aluminum in the RHO zeolite is 1-10.

[0009] Preferably, the RHO type zeolite is a powder having an average particle size of 0.01 to 1 μm.

[0010] The present invention is also directed to a method for producing RHO type zeolite. A method for producing RHO type zeolite according to a preferred embodiment of the present invention includes the steps of: a) mixing a sodium source, a cesium source, and a silicon source in water and stirring for a predetermined time; b) mixing RHO type zeolite powder as seed crystals into the solution obtained in the step a) and stirring for a predetermined time; c) mixing an aluminum source into the solution obtained in the step b) to obtain a raw material solution; and d) producing RHO type zeolite powder by hydrothermal synthesis using the raw material solution. In the raw material solution, the molar ratio of silicon / aluminum is 2 to 30, the molar ratio of sodium / aluminum is 3 to 100, the molar ratio of cesium / aluminum is 0.4 to 3, and the molar ratio of water / aluminum is 50 to 5000.

[0011] Preferably, the molar ratio of silicon / aluminum is 4-30, the molar ratio of sodium / aluminum is 3-15, the molar ratio of cesium / aluminum is 0.4-2, and the molar ratio of water / aluminum is 160-420.

[0012] The above and other objects, features, aspects and advantages will become apparent from the following detailed description of the invention which proceeds with reference to the accompanying drawings. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a diagram showing a flow of production of RHO-type zeolite. [Diagram 2] FIG. 1 shows an XRD pattern of RHO-type zeolite. [Diagram 3] FIG. 1 shows an XRD pattern of RHO-type zeolite. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The X-ray diffraction (XRD) pattern obtained by measuring the zeolite according to the present invention by the powder X-ray diffraction method has peak positions that match those of the XRD pattern expected from the structure of a zeolite whose structure code is "RHO" defined by the International Zeolite Society. Therefore, the zeolite according to the present invention is an RHO-type zeolite. In the measurement in this embodiment, CuKα radiation is used as the radiation source of the X-ray diffraction device, but other types of radiation sources may be used.

[0015] In the RHO type zeolite according to the present invention (hereinafter also referred to as "the present RHO type zeolite"), when a peak at a lattice spacing of 9.96 to 11.25 Å (angstroms) is used as a reference peak and the intensity of the reference peak is set to 100, the relative value of the intensity of the peak at a lattice spacing of 4.59 to 4.85 Å (the relative value of the intensity when the intensity of the reference peak is set to 100 is hereinafter simply referred to as "relative intensity") is 150 to 300. In addition, the relative intensity of the peak at a lattice spacing of 3.55 to 3.64 Å is 200 to 500, and the relative intensity of the peak at a lattice spacing of 2.98 to 3.06 Å is 100 to 200.

[0016] The relative intensity of the peak at a lattice spacing of 4.59 to 4.85 Å is more preferably 155 to 280, and further preferably 160 to 250. The relative intensity of the peak at a lattice spacing of 3.55 to 3.64 Å is more preferably 220 to 480, and further preferably 250 to 450. The relative intensity of the peak at a lattice spacing of 2.98 to 3.06 Å is more preferably 110 to 190, and further preferably 120 to 190.

[0017] [Table 1]

[0018] The RHO-type zeolite has, for example, X-ray diffraction (XRD) peaks shown in Table 1. Table 1 also shows the range of the relative intensity of the peak at the lattice spacing other than the above-mentioned lattice spacing. Specifically, the relative intensity of the peak at the lattice spacing of 5.89 to 6.32 Å is 10 to 55, and the relative intensity of the peak at the lattice spacing of 5.13 to 5.44 Å is 10 to 80. In addition, the relative intensity of the peak at the lattice spacing of 3.90 to 4.10 Å is 30 to 90, and the relative intensity of the peak at the lattice spacing of 3.27 to 3.46 Å is 100 to 250. The relative intensity of the peak is the height of the bottom line in the XRD pattern, that is, excluding the background noise component. The bottom line in the XRD pattern is obtained, for example, by the Sonneveld-Visser method or the spline interpolation method.

[0019] The XRD pattern of the present RHO-type zeolite produced by the manufacturing method described later is different from the XRD pattern of the RHO-type zeolite shown in Japanese Patent No. 6631663 (above-mentioned document 1) and the XRD pattern of the RHO-type zeolite shown in Japanese Patent Application Laid-Open No. 2020-66564 (above-mentioned document 2). For example, the present RHO-type zeolite differs from the RHO-type zeolite of documents 1 and 2 in that the relative intensity of the peak at the lattice spacing of 4.59 to 4.85 Å is 150 to 300, the relative intensity of the peak at the lattice spacing of 3.55 to 3.64 Å is 200 to 500, and the relative intensity of the peak at the lattice spacing of 2.98 to 3.06 Å is 100 to 200. Therefore, the present RHO-type zeolite can be said to be a novel RHO-type zeolite whose crystal shape is different from that of the RHO-type zeolite of documents 1 and 2. The present RHO type zeolite may include peaks other than those listed in Table 1. When a separation membrane is formed using the novel zeolite of the present invention, an RHO type zeolite membrane with excellent orientation can be formed. That is, the novel zeolite of the present invention is suitable for use in obtaining a separation membrane having a high permeation amount and good separation performance, for example.

[0020] One example of this RHO-type zeolite is the oxygen tetrahedron (TO 4 The atom (T atom) located at the center of the RHO zeolite is composed of silicon (Si) and aluminum (Al). A part of the T atoms may be substituted with other elements (gallium, titanium, vanadium, iron, zinc, tin, etc.). This makes it possible to change the pore size and adsorption characteristics. The molar ratio of silicon / aluminum in the present RHO zeolite (a value obtained by dividing the number of moles of silicon atoms by the number of moles of aluminum atoms; the same applies below) is preferably 1 to 10, and more preferably 1.5 to 4.5. This makes it possible to improve the hydrophilicity of the RHO zeolite. The molar ratio of silicon / aluminum can be measured by EDS (energy dispersive X-ray spectroscopy) analysis. The silicon / aluminum ratio in the RHO zeolite can be adjusted by adjusting the blending ratio of the silicon source and the aluminum source in the raw material solution described later, and the like (the same applies to the ratios of other elements).

[0021] Typically, the present RHO type zeolite contains sodium (Na). The molar ratio of sodium / aluminum in the RHO type zeolite is preferably 0.1 to 1, and more preferably 0.2 to 0.8. This makes the structure of the RHO type zeolite stable (such as suppressing crystal collapse). It is preferable that the RHO type zeolite further contains cesium (Cs). The molar ratio of cesium / aluminum in the RHO type zeolite is preferably 0.1 to 0.9, and more preferably 0.15 to 0.85. The RHO type zeolite may contain other alkali metals such as potassium (K) and rubidium (Rb). In addition, some or all of the cations may be converted to protons (H + ) and ammonium ion (NH 4 + ) and the like.

[0022] One example of the present RHO type zeolite is produced without using an organic substance called a structure-directing agent (hereinafter also referred to as "SDA"). In this case, the RHO type zeolite does not contain an SDA. In an RHO type zeolite that does not contain an SDA, the pores are properly secured. Another example of the present RHO type zeolite is produced using an SDA. In this case, it is preferable that the SDA is almost or completely removed after the formation of the RHO type zeolite. As the SDA, for example, 18-crown-6-ether or the like can be used.

[0023] The present RHO type zeolite is produced as a powder. The average particle size of the RHO type zeolite powder is, for example, 0.01 to 1 μm, and preferably 0.1 to 0.5 μm. This makes the structure of the RHO type zeolite stable (such as suppressing crystal collapse). The average particle size of the powder is, for example, the median diameter (D50) in the particle size distribution determined by a laser scattering method.

[0024] FIG. 1 is a diagram showing the flow of production of the present RHO-type zeolite. In this production example, first, the sodium source and cesium source, which are alkali sources, are mixed and dissolved in water. The sodium source and cesium source are also cation sources. The sodium source is, for example, sodium hydroxide, sodium chloride, sodium bromide, etc. The cesium source is, for example, cesium hydroxide, cesium chloride, etc. SDA may be mixed into the solution. The materials already exemplified as SDA can be used. The silicon source is further mixed into the solution, and then stirred for a predetermined time (step S11). The silicon source is, for example, colloidal silica, fumed silica, water glass, etc. The stirring time after mixing the alkali source and silicon source into water is, for example, 5 hours or more, preferably 12 hours or more, and more preferably 24 hours or more. As a result, the silicon source is sufficiently dissolved in the solution. The stirring time is, for example, 72 hours or less.

[0025] Next, a powder of RHO type zeolite prepared separately is mixed into the solution as seed crystals, and the solution is stirred for a predetermined time (step S12). The powder of RHO type zeolite as the seed crystals is produced by a known manufacturing method. In the XRD pattern of the RHO type zeolite, for example, the relative intensity of the peak at the lattice spacing of 4.59 to 4.85 Å is less than 150, the relative intensity of the peak at the lattice spacing of 3.55 to 3.64 Å is less than 200, and the relative intensity of the peak at the lattice spacing of 2.98 to 3.06 Å is less than 100. That is, the RHO type zeolite as the seed crystals is different from the present RHO type zeolite. The stirring time after mixing the seed crystals into the solution is, for example, 1 hour or more, preferably 3 hours or more, and more preferably 5 hours or more. The stirring time is, for example, 24 hours or less.

[0026] Then, an aluminum source is mixed into the solution to obtain a raw material solution (step S13). The aluminum source is, for example, aluminum hydroxide, sodium aluminate, aluminum sulfate, etc. In the raw material solution, a sodium source, a cesium source, a silicon source, a seed crystal, and an aluminum source are dissolved or dispersed in water. In the raw material solution, the molar ratio of silicon / aluminum is 2 to 30, preferably 4 to 30. The molar ratio of sodium / aluminum is 3 to 100, preferably 3 to 15. The molar ratio of cesium / aluminum is 0.4 to 3, preferably 0.4 to 2. The molar ratio of water / aluminum is 50 to 5000, preferably 160 to 420. The mass ratio of the seed crystal in the raw material solution is, for example, 0.0001 to 0.1, preferably 0.001 to 0.05, and more preferably 0.005 to 0.01.

[0027] Next, the raw material solution is subjected to hydrothermal synthesis to generate RHO type zeolite powder (step S14). The temperature during the hydrothermal synthesis is, for example, 60 to 120°C. The hydrothermal synthesis time is, for example, 1 to 60 hours. When the hydrothermal synthesis is completed, the obtained crystals are washed with pure water. Then, the washed crystals are dried to obtain the present RHO type zeolite powder. When the raw material solution contains SDA, the powder is heat-treated under an oxidizing gas atmosphere to burn and remove the SDA in the powder. Preferably, the SDA is almost completely removed. The heating temperature in removing the SDA is, for example, 350 to 700°C. The heating time is, for example, 1 to 100 hours. The oxidizing gas atmosphere is an atmosphere containing oxygen, for example, air.

[0028] As described above, the manufacturing method of FIG. 1 includes a step of mixing a sodium source, a cesium source, and a silicon source in water and stirring for a predetermined time (step S11), a step of mixing RHO type zeolite powder as seed crystals into the solution obtained by step S11 and stirring for a predetermined time (step S12), a step of mixing an aluminum source into the solution obtained by step S12 to obtain a raw material solution (step S13), and a step of producing RHO type zeolite powder by hydrothermal synthesis using the raw material solution (step S14). In the raw material solution, the molar ratio of silicon / aluminum is 2 to 30, the molar ratio of sodium / aluminum is 3 to 100, the molar ratio of cesium / aluminum is 0.4 to 3, and the molar ratio of water / aluminum is 50 to 5000. This makes it possible to easily produce a novel RHO type zeolite.

[0029] Here, the manufacturing method of the comparative example will be described. In the manufacturing method of the comparative example, as in the above-mentioned document 1, an aluminum source is mixed with a solution of an alkali source, and then a silicon source is mixed to prepare a raw material solution. In this case, the silicon source is difficult to dissolve in the raw material solution. The same applies to the case where an alkali source and a silicon source are mixed with a solution of an aluminum source to prepare a raw material solution as in the above-mentioned document 2.

[0030] In contrast, in the manufacturing method of FIG. 1, the silicon source and seed crystals are mixed into an aqueous solution of an alkali source without mixing an aluminum source, and sufficient stirring (aging) is performed. Then, the aluminum source is mixed to prepare a raw material solution. In this case, the alkali source makes it easier to dissolve the silicon source and the seed crystals. As a result, it is presumed that nuclei of RHO-type zeolite are more easily generated in the hydrothermal synthesis, making it possible to produce the present RHO-type zeolite having a unique XRD peak intensity.

[0031] Next, examples of the production of the present RHO-type zeolite will be described. Table 2 shows the compositions (compositions in terms of oxides) of the raw material solutions prepared in Examples 1 to 7 and Comparative Examples 1 and 2. Table 2 also shows the Si / Al ratio, Na / Al ratio, average particle size, synthesis temperature, and synthesis time, which will be described later.

[0032] [Table 2]

[0033] Example 1 Sodium hydroxide and cesium hydroxide, which are cation sources, were dissolved in water. Colloidal silica, which is a silicon source, was added to the solution, and the solution was vigorously stirred for 24 hours with a shaker. 0.3 g of RHO-type zeolite powder, which is a seed crystal, was added to 100 g of the resulting solution, and the solution was vigorously stirred for another 2 hours with a shaker. After that, aluminum hydroxide, which is an aluminum source, was added to the solution, and the composition was 9(SiO 2 ):1(Al 2 O 3 ):7(Na 2 O):2(Cs 2 O: 500 (H 2 A raw material solution of O) was prepared. The obtained solution was heated at 100°C for 20 hours (hydrothermal synthesis) to obtain RHO-type zeolite powder. The obtained crystals were collected and thoroughly washed with pure water, and then dried at 120°C.

[0034] The zeolite thus obtained was subjected to measurement by powder X-ray diffraction method (XRD measurement). An X-ray diffraction apparatus manufactured by Rigaku (apparatus name: MiniFlex600) was used. The powder X-ray diffraction measurement was performed at a tube voltage of 40 kV, a tube current of 15 mA, a scanning speed of 0.5° / min, and a scanning step of 0.02°. The divergence slit was 1.25°, the scattering slit was 1.25°, the receiving slit was 0.3 mm, the incident Soller slit was 5.0°, and the receiving Soller slit was 5.0°. No monochromator was used, and a 0.015 mm thick nickel foil was used as a CuKβ ray filter. Figure 2 shows the XRD pattern obtained by XRD measurement. Table 3 shows the relative intensity of each peak in the XRD pattern.

[0035] [Table 3]

[0036] The leftmost number in Table 3 corresponds to the leftmost number in Table 1 (similarly in Tables 4 to 7 described later). In the RHO-type zeolite of Example 1, the relative intensity of the peak near 2θ=18.7° to the peak near 2θ=8.3°, i.e., the relative intensity of the peak at lattice spacing of 4.59 to 4.85 Å, was in the range of 150 to 300 (see number 4). In addition, the relative intensity of the peak near 2θ=25.1° to the peak near 2θ=8.3°, i.e., the relative intensity of the peak at lattice spacing of 3.55 to 3.64 Å, was in the range of 200 to 500 (see number 6). In addition, the relative intensity of the peak near 2θ=30.3° to the peak near 2θ=8.3°, i.e., the relative intensity of the peak at lattice spacing of 2.98 to 3.06 Å, was in the range of 100 to 200 (see number 8). In fact, the relative intensity of each peak in Table 3 was included in the range of relative intensities shown in Table 1, and the RHO zeolite of Example 1 had the XRD peaks listed in Table 1.

[0037] Table 2 shows the silicon / aluminum molar ratio (Si / Al ratio) and sodium / aluminum molar ratio (Na / Al ratio) of the RHO zeolite measured by EDS analysis. The silicon / aluminum molar ratio of the zeolite in Example 1 was 3.5, and the sodium / aluminum molar ratio was 0.5. Table 2 also shows the average particle size of the RHO zeolite. The average particle size is the median diameter (D50) in the particle size distribution determined by a laser scattering method. The average particle size of the zeolite in Example 1 was 0.40 μm.

[0038] Example 2 Sodium hydroxide, which is a cation source, cesium hydroxide, and 18-crown-6-ether (hereinafter also referred to as "18C6"), which is a structure directing agent, were dissolved in water. Colloidal silica, which is a silicon source, was added to the solution, and the solution was vigorously stirred for 24 hours with a shaker. 0.3 g of RHO-type zeolite powder, which is a seed crystal, was added to 100 g of the resulting solution, and the solution was vigorously stirred for another 2 hours with a shaker. After that, aluminum hydroxide, which is an aluminum source, was added to the solution, and the composition was adjusted to 10(SiO2 ):1(Al 2 O 3 ):3(Na 2 O:0.4(Cs 2 O:2(18C6):500(H 2 A raw material solution of 18-crown-6-ether was prepared. The resulting solution was heated at 110°C for 20 hours to obtain RHO-type zeolite powder. The resulting crystals were collected, thoroughly washed with pure water, and then dried at 120°C. The crystals were then calcined in air at 500°C for 10 hours to remove 18-crown-6-ether.

[0039] The zeolite thus obtained was subjected to XRD measurement, and the XRD pattern shown in Figure 3 was obtained. Table 4 also shows the relative intensity of each peak in the XRD pattern.

[0040] [Table 4]

[0041] In the RHO zeolite of Example 2, the relative intensity of the peak at the lattice spacing of 4.59 to 4.85 Å was in the range of 150 to 300 (see number 4). In addition, the relative intensity of the peak at the lattice spacing of 3.55 to 3.64 Å was in the range of 200 to 500 (see number 6), and the relative intensity of the peak at the lattice spacing of 2.98 to 3.06 Å was in the range of 100 to 200 (see number 8). In fact, the relative intensity of each peak in Table 4 was included in the range of relative intensity shown in Table 1, and the RHO zeolite of Example 2 had the XRD peaks listed in Table 1. As shown in Table 2, the molar ratio of silicon / aluminum of the zeolite was 4.2, and the molar ratio of sodium / aluminum was 0.6. The average particle size was 0.35 μm.

[0042] (Examples 3 to 7) Examples 3 to 7 are similar to Example 1, except that the composition of the raw material solution was changed as shown in Table 2. Table 5 shows the relative intensity of each peak in the XRD pattern of the obtained zeolite. The numbers in Table 5 correspond to the numbers on the left side in Table 1. Table 5 also shows the relative intensity of each peak of the zeolites of Examples 1 and 2 and Comparative Examples 1 and 2.

[0043] [Table 5]

[0044] In the RHO zeolites of Examples 3 to 7, the relative intensity of the peak at the lattice spacing of 4.59 to 4.85 Å was in the range of 150 to 300 (see number 4). In addition, the relative intensity of the peak at the lattice spacing of 3.55 to 3.64 Å was in the range of 200 to 500 (see number 6), and the relative intensity of the peak at the lattice spacing of 2.98 to 3.06 Å was in the range of 100 to 200 (see number 8). In fact, in all of the RHO zeolites of Examples 3 to 7, the relative intensity of each peak was included in the range of relative intensity shown in Table 1, and the RHO zeolites of Examples 3 to 7 had the XRD peaks shown in Table 1. In addition, as shown in Table 2, the molar ratio of silicon / aluminum of the zeolites of Examples 3 to 7 was 3.5 to 4.0, and the molar ratio of sodium / aluminum was 0.2 to 0.3. The average particle size was 0.35 to 0.42 μm.

[0045] Comparative Example 1 Sodium hydroxide and cesium hydroxide, which are cation sources, were added to water, and then aluminum hydroxide, which is an aluminum source, and colloidal silica, which is a silicon source, were added, and the mixture was vigorously stirred for 24 hours with a shaker. As a result, the composition of the mixture was 9(SiO 2 ):1(Al 2 O 3 ):7(Na 2 O):2(Cs 2 O: 500 (H 2A raw material solution of O) was prepared. 0.3 g of RHO type zeolite powder as seed crystals was added to 100 g of the obtained solution, and the mixture was heated at 100° C. for 20 hours to obtain an RHO type zeolite powder.

[0046] The XRD of the zeolite thus obtained was measured, giving the relative intensities of the XRD peaks shown in Table 6.

[0047] [Table 6]

[0048] In the RHO zeolite of Comparative Example 1, the relative intensity of the peak at the lattice spacing of 4.59 to 4.85 Å was less than 150 (see No. 4), the relative intensity of the peak at the lattice spacing of 3.55 to 3.64 Å was less than 200 (see No. 6), and the relative intensity of the peak at the lattice spacing of 2.98 to 3.06 Å was less than 100 (see No. 8). Thus, the relative intensities of some of the peaks in Table 6 were not included in the range of relative intensities shown in Table 1, and the RHO zeolite of Comparative Example 1 did not have the XRD peaks listed in Table 1. As shown in Table 2, the molar ratio of silicon / aluminum of the zeolite was 3.0, and the molar ratio of sodium / aluminum was 0.4. The average particle size was 0.45 μm.

[0049] Comparative Example 2 Sodium hydroxide and cesium hydroxide, which are cation sources, were added to water, followed by 18-crown-6-ether, which is a structure directing agent, and then aluminum hydroxide, which is an aluminum source, and colloidal silica, which is a silicon source, were added, and the mixture was vigorously stirred for 24 hours with a shaker. As a result, the composition was 10(SiO 2 ):1(Al 2 O 3 ):0.4(Na 2 O:0.1(Cs 2 O):0.1(18C6):10(H 2A raw material solution of 18-crown-6-ether was prepared. 0.3 g of RHO-type zeolite powder as seed crystals was added to 100 g of the obtained solution, and the solution was heated at 110°C for 20 hours to obtain RHO-type zeolite powder. The solution was then calcined in air at 500°C for 10 hours to remove 18-crown-6-ether.

[0050] The XRD of the zeolite thus obtained was measured, giving the relative intensities of the XRD peaks shown in Table 7.

[0051] [Table 7]

[0052] In the RHO zeolite of Comparative Example 2, the relative intensity of the peak at the lattice spacing of 4.59 to 4.85 Å was less than 150 (see No. 4), the relative intensity of the peak at the lattice spacing of 3.55 to 3.64 Å was less than 200 (see No. 6), and the relative intensity of the peak at the lattice spacing of 2.98 to 3.06 Å was less than 100 (see No. 8). Thus, the relative intensities of some of the peaks in Table 7 were not included in the range of relative intensities shown in Table 1, and the RHO zeolite of Comparative Example 2 did not have the XRD peaks listed in Table 1. As shown in Table 2, the molar ratio of silicon / aluminum of the zeolite was 4.5, and the molar ratio of sodium / aluminum was 0.5. The average particle size was 0.33 μm.

[0053] The above-mentioned RHO type zeolite and the method for producing RHO type zeolite can be modified in various ways.

[0054] The present RHO zeolite powder may be produced by a production method other than that shown in FIG.

[0055] The silicon / aluminum molar ratio in the RHO zeolite may be greater than 10. Similarly, the sodium / aluminum molar ratio may be less than 0.1 or greater than 1. The average particle size of the RHO zeolite may be less than 0.01 μm or greater than 1 μm.

[0056] The configurations in the above-described embodiment and each of the modified examples may be combined as appropriate as long as they are not mutually inconsistent.

[0057] Although the invention has been particularly illustrated and described, it is to be understood that the above description is illustrative and not restrictive, and therefore numerous modifications and variations are possible without departing from the scope of the invention. [Industrial Applicability]

[0058] The RHO zeolite of the present invention can be used in various applications in which zeolites are used. [Explanation of symbols]

[0059] S11~S14 steps

Claims

1. An RHO type zeolite, When measured by powder X-ray diffraction method, a peak at a lattice spacing of 9.96 to 11.25 Å is used as a reference peak and the intensity of the reference peak is taken as 100, the relative intensity of the peak at a lattice spacing of 4.59 to 4.85 Å is 150 to 300, the relative intensity of the peak at a lattice spacing of 3.55 to 3.64 Å is 200 to 500, and the relative intensity of the peak at a lattice spacing of 2.98 to 3.06 Å is 100 to 200, An RHO-type zeolite having a sodium / aluminum molar ratio of 0.1 to 1.

2. The RHO zeolite according to claim 1, An RHO-type zeolite having a silicon / aluminum molar ratio of 1-10.

3. 3. The RHO zeolite according to claim 1 or 2, RHO type zeolite is a powder with an average particle size of 0.01 to 1 μm.

4. A method for producing RHO zeolite, comprising the steps of: a) mixing a sodium source, a cesium source, and a silicon source in water and stirring the mixture for a predetermined period of time; b) mixing RHO type zeolite powder as seed crystals into the solution obtained in the a) step and stirring for a predetermined period of time; c) mixing an aluminum source with the solution obtained in the b) step to obtain a raw material solution; d) producing RHO zeolite powder by hydrothermal synthesis using the raw material solution; Equipped with In the raw material solution, a molar ratio of silicon / aluminum is 2 to 30, a molar ratio of sodium / aluminum is 3 to 100, a molar ratio of cesium / aluminum is 0.4 to 3, and a molar ratio of water / aluminum is 50 to 5000.

5. A method for producing the RHO zeolite according to claim 4, A method for producing an RHO-type zeolite, in which the molar ratio of silicon / aluminum is 4-30, the molar ratio of sodium / aluminum is 3-15, the molar ratio of cesium / aluminum is 0.4-2, and the molar ratio of water / aluminum is 160-420.

Citation Information

Patent Citations

  • Zeolite membrane composite for gas separation and production method of the same

    JP2016112563A

  • Porous support-zeolite membrane composite body, method for producing RHO type zeolite and separation method

    JP2018130719A

  • Highly efficient solid-state thermal synthesis of zeolite materials