Granulated material manufacturing method and optical film manufacturing method
By granulating optical films using frictional heat below the resin's glass transition temperature, the method addresses bulkiness and thermal issues, enhancing handling and reducing contamination, thus improving the production efficiency and quality of optical films.
Patent Information
- Application Number
- JP2022572070
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-12-25
- Filing Date
- 2021-12-06
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-12-06
AI Technical Summary
Optical films containing cycloolefin and (meth)acrylic resins face challenges with bulkiness, handling difficulties, thermal deterioration, and contamination due to high-temperature granulation, leading to poor transport and storage, and adherence to piping surfaces.
A method involving the use of frictional heat to melt and granulate crushed optical films at temperatures below the resin's glass transition temperature, adjusting bulk density and aspect ratio to enhance handling and reduce thermal deterioration and contamination.
The method produces granules with improved handling properties, reduced thermal degradation, and minimized foreign matter contamination, facilitating efficient production and use in optical films.
Smart Images

Figure 0007593416000006 
Figure 0007593416000007 
Figure 0007593416000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a granulated material and a method for producing an optical film. [Background technology]
[0002] Polarizing plates are commonly used in displays such as liquid crystal displays (LCDs), organic light-emitting diode displays (OLEDs), and μLEDs. Polarizing plates include a polarizer and an optical film that has the functions of protecting the polarizer and providing optical compensation.
[0003] In the manufacturing process of such optical films, there are cases where edges are slit, non-standard products, etc. From the viewpoint of effectively utilizing these materials and reducing waste to increase the manufacturing efficiency of optical films, the reuse of the edges slit during film manufacturing and non-standard films (returned materials) is being considered.
[0004] However, crushed materials such as films have a low bulk density (apparent specific gravity) and are therefore difficult to handle. Therefore, crushed materials are sometimes pelletized before use.
[0005] Known methods for pelletization include a method of melting the crushed material at a high temperature of about 250°C, similar to the manufacturing method for new pellets, and a method of granulating the crushed material by frictional heat. Patent Document 1 proposes a method of granulating (or melting) the crushed material of recycled materials such as film by frictional heat to obtain granules with a bulk density reduced to the same level as that of new pellets (see Patent Document 1). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 54-45365 Summary of the Invention [Problem to be solved by the invention]
[0007] Meanwhile, optical films are required to have high optical stability (humidity dependence of retardation) and dimensional stability (humidity dependence of dimensions). Films containing cycloolefin resins or (meth)acrylic resins are becoming more widely used because they have better humidity dependence of retardation and humidity dependence of dimensions than conventional films containing cellulose ester resins.
[0008] However, crushed films containing these resins have a problem that they are bulky and difficult to handle (transport and store) compared to crushed films containing conventional cellulose ester resins. In addition, when crushed films are granulated under the conditions shown in Patent Document 1 (granulation by generating high-temperature frictional heat of about 200°C), the resin in the granulated material is prone to thermal degradation.
[0009] In addition, if the bulk density of the granulated material is high due to a small aspect ratio of the granulated material obtained, or if sufficient granulation cannot be performed due to insufficient melting, the granulated material is likely to adhere to the inner wall surface of the pipe during pneumatic conveyance. If a film is produced using different types of materials using such a pipe, there is also a problem that the granulated material and its components adhering to the inner wall surface of the pipe are likely to be mixed in as foreign matter.
[0010] The present invention has been made in consideration of the above circumstances, and aims to provide a method for producing a granulated material that is easy to handle while suppressing deterioration of materials due to heat and the inclusion of foreign matter, and a method for producing an optical film using the same. [Means for solving the problem]
[0011] The present invention relates to the following method for producing a granule and a method for producing an optical film using the same.
[0012] The method for producing a granulated product of the present invention comprises producing a granulated product having a bulk density of 0.01 to 0.25 g / cm3, the bulk density of which is ... and the bulk density of which is 0.01 to 0.25 g / 3 and fusing the crushed material by frictional heat at a temperature of (50 to Tg) °C (Tg is the glass transition temperature of the resin) to produce a resin having a bulk density of 0.26 to 0.45 g / cm. 3 and obtaining a granulated product comprising the compound.
[0013] The method for producing an optical film of the present invention includes a step of obtaining a granulated material by the method for producing a granulated material of the present invention, and a step of melting the granulated material or dissolving the granulated material in a solvent to obtain a film-like material. Effect of the Invention
[0014] According to the present invention, it is possible to provide a method for producing a granulated material that is excellent in handleability while suppressing deterioration of materials due to heat and inclusion of foreign matter, and a method for producing an optical film using the same. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a cross-sectional view showing the configuration of a crushing and granulating device. [Diagram 2] FIG. 2 is an enlarged view of a main portion of FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] As described above, films containing cycloolefin resins or (meth)acrylic resins are more difficult to cut (shatter) than films containing cellulose ester resins, and shattered products tend to be bulky. The reason for this is unclear, but it is believed to be due to the fact that cycloolefin resins and (meth)acrylic resins have higher toughness than cellulose ester resins and are less polar, which makes them more susceptible to static electricity.
[0017] To address this issue, we discovered that by 1) melting and granulating the crushed film material using frictional heat while keeping the temperature at or below a certain level, and 2) further adjusting the melting and granulation conditions so that the bulk density of the resulting granules does not become too low, it is possible to suppress thermal degradation of the resin in the granules and the introduction of foreign matter when changing product types.
[0018] The reason for this is not clear, but is thought to be as follows. Granulation by frictional heat is different from granulation by general melting, in that heat is applied locally to the contact points between the crushed materials, so that the crushed materials as a whole do not easily become hot. Furthermore, by appropriately lowering the melting temperature by frictional heat (below the Tg of the resin), the heat applied to the crushed materials can be kept to the minimum required for granulation. This makes it possible to suppress the decrease in molecular weight and coloring of the resin caused by thermal degradation. In addition, by making the bulk density of the granulated material higher than before, it is less likely to adhere to the inner wall surface of the pipe during empty transport, etc., and therefore it is possible to suppress the inclusion of foreign matter due to the inclusion of granulated material adhered to the inner wall surface of the pipe during product switching. Incidentally, melting by frictional heat means bringing the material into a semi-molten state, preferably at a temperature lower than the melting point.
[0019] The melting temperature caused by frictional heat can be adjusted by any method. For example, the melting temperature can be adjusted by the width or length of the flow path (the gap between the screw and the cylinder inner wall surface) of the melting zone caused by frictional heat (compression section B or transfer section C) of the crushing / granulating device 10 in Fig. 1 described later, the cooling process (during melting), the supply speed (processing speed) of the crushed material, etc. The bulk density of the granulated material can be adjusted by, for example, the melting temperature caused by frictional heat or the aspect ratio of the granulated material.
[0020] The present invention relates to a method for producing a granulated material by using such recycled resin film. First, the resin film (recycled resin film) that is the raw material for the granulated material will be described.
[0021] 1. About returned materials Returned materials are scraps and non-standard products that are cut off during the manufacturing process of resin films such as optical films. In the manufacturing process of optical films, defective products may be generated due to cut-off edges or irregular winding. Although these do not become products, there is no problem with the material and they can be reused.
[0022] The optical film contains a cycloolefin resin or a (meth)acrylic resin.
[0023] (Cycloolefin resin) Cycloolefin resins are polymers containing structural units derived from norbornene monomers, which are represented by the following formula (1). [ka]
[0024] R in Equation (1) 1 ~R 4 each represents a hydrogen atom, a halogen atom, a hydrocarbon group, or a polar group.
[0025] Examples of the halogen atom include a fluorine atom, a chlorine atom, and the like.
[0026] The hydrocarbon group has 1 to 10 carbon atoms, preferably 1 to 4 carbon atoms, and more preferably 1 or 2 carbon atoms. Examples of the hydrocarbon group include alkyl groups such as a methyl group, an ethyl group, a propyl group, and a butyl group. The hydrocarbon group may further have a divalent linking group containing an oxygen atom, a nitrogen atom, a sulfur atom, or a silicon atom (for example, a carbonyl group, an imino group, an ether bond, a silyl ether bond, a thioether bond, etc.).
[0027] Examples of polar groups include carboxy groups, hydroxy groups, alkoxy groups, alkoxycarbonyl groups, aryloxycarbonyl groups, amino groups, amide groups, and linking groups such as methylene groups (-(CH2) n and n is an integer of 1 or more). Among these, an alkoxycarbonyl group and an aryloxycarbonyl group are preferred, and an alkoxycarbonyl group is more preferred.
[0028] Among them, R 1 ~R 4At least one of the above is preferably a polar group. Cycloolefin resins containing structural units derived from norbornene monomers having polar groups are easily dissolved in a solvent when forming a film by, for example, a solution casting method, and the glass transition temperature of the resulting film is easily increased. On the other hand, in the melt film forming method, the cycloolefin resin may not contain structural units derived from norbornene monomers having polar groups.
[0029] Also, R 1 ~R 4 Of these, R 1 and R 2 Both (or R 3 and R 4 Both of these may be hydrogen atoms.
[0030] In the formula (1), p represents an integer of 0 to 2. From the viewpoint of improving the heat resistance of the optical film, p is preferably 1 or 2.
[0031] Among the norbornene-based monomers represented by formula (1), examples of the norbornene-based monomer having a polar group include the following.
[0032] [ka]
[0033] Examples of norbornene monomers without a polar group include the following: [ka]
[0034] The content of the structural units derived from norbornene-based monomers can be 50 to 100 mol % based on all structural units constituting the cycloolefin-based resin.
[0035] The cycloolefin resin may further contain a structural unit derived from another monomer copolymerizable with the structural unit derived from the norbornene monomer. Examples of the copolymerizable other monomer include a norbornene monomer having no polar group (when the norbornene monomer has a polar group) and a cycloolefin monomer having no norbornene skeleton, such as cyclobutene, cyclopentene, cycloheptene, and dicyclopentadiene.
[0036] The weight average molecular weight Mw of the cycloolefin resin is not particularly limited, but is preferably from 20,000 to 300,000, more preferably from 30,000 to 250,000, and even more preferably from 40,000 to 200,000. When the Mw of the cycloolefin resin is within the above range, the mechanical properties of the film can be improved without impairing the moldability.
[0037] The Mw of the cycloolefin resin can be measured by gel permeation chromatography (GPC). Specifically, it can be measured under the following conditions using HLC8220GPC manufactured by Tosoh Corporation. (Measurement conditions) Eluent:THF Column: Tosoh TSKgel GMHXL x 2 Flow rate: 1.0mL / min Sample concentration: 0.1% by mass Injection volume: 100μL Detector: RI Calibration curve: Standard polystyrene Column temperature: 40℃
[0038] The glass transition temperature Tg of the cycloolefin resin is usually preferably 110° C. or higher, more preferably 110 to 350° C., and even more preferably 120 to 250° C. When the cycloolefin resin has a Tg of 110° C. or higher, sufficient heat resistance is easily obtained, and when the Tg is 350° C. or lower, thermal degradation of the cycloolefin resin during molding can be suppressed.
[0039] Tg can be measured using DSC (Differential Scanning Colorimetry) according to a method in accordance with JIS K 7121-2012 or ASTM D 3418-82.
[0040] ((Meth)acrylic resin) The (meth)acrylic resin is preferably a polymer containing a structural unit derived from methyl methacrylate. The polymer may further contain a structural unit derived from a monomer copolymerizable with methyl methacrylate.
[0041] Examples of other monomers copolymerizable with methyl methacrylate include alkyl (meth)acrylates having 1 to 18 carbon atoms other than methyl methacrylate, such as 2-ethylhexyl (meth)acrylate; α,β-unsaturated acids such as (meth)acrylic acid; unsaturated dicarboxylic acids such as maleic acid, fumaric acid, and itaconic acid; styrenes such as styrene and α-methylstyrene; maleic anhydride; maleimides such as maleimide and N-phenylmaleimide; glutaric anhydride, and the like.
[0042] The content of structural units derived from methyl methacrylate is preferably 50% by mass or more, and more preferably 70% by mass or more, based on all structural units constituting the polymer.
[0043] The Tg of the (meth)acrylic resin is preferably 90° C. or higher, and more preferably 100 to 150° C. When the Tg of the (meth)acrylic resin is within the above range, the heat resistance of the optical film is easily improved. The Tg of the (meth)acrylic resin can be measured by the same method as described above.
[0044] The Mw of the (meth)acrylic resin is preferably 400,000 to 3,000,000, and more preferably 500,000 to 2,000,000. When the Mw of the (meth)acrylic resin is in the above range, sufficient mechanical strength can be imparted to the film. The Mw of the (meth)acrylic resin can be measured by the same method as described above.
[0045] The content of the cycloolefin resin or the (meth)acrylic resin is preferably 50% by mass or more, and more preferably 70 to 99% by mass, based on the optical film.
[0046] (Other ingredients) The optical film may further contain other components as necessary. Examples of the other components include rubber particles, matting agents, antioxidants, and ultraviolet absorbing agents.
[0047] The rubber particles can impart flexibility to the film. The rubber particles are graft copolymers containing a rubber-like polymer (crosslinked polymer). Examples of the rubber-like polymer include butadiene-based crosslinked polymers, (meth)acrylic crosslinked polymers, and organosiloxane crosslinked polymers. Among them, (meth)acrylic crosslinked polymers are preferred, and acrylic crosslinked polymers (acrylic rubber-like polymers) are more preferred, from the viewpoint of a small difference in refractive index from methacrylic resins and less loss of transparency of the optical film.
[0048] The matting agent can form unevenness on the surface of the optical film and provide slipperiness. The matting agent can be inorganic particles or resin particles. Examples of inorganic particles include fine particles of silicon dioxide, titanium dioxide, aluminum oxide, zirconium oxide, calcium carbonate, etc., and preferably silicon dioxide particles.
[0049] The antioxidant is not particularly limited, but for example, a hindered phenol-based antioxidant can be used.
[0050] (Thickness) The thickness of the optical film is not particularly limited, but is, for example, about 5 to 100 μm, and preferably about 5 to 40 μm.
[0051] Next, a method for producing a granulated material using the above recycled material will be described.
[0052] 2. Manufacturing method of granulated material The method for producing a granulated material of the present invention includes the steps of: 1) preparing a crushed material containing the resin; and 2) melting the crushed material by frictional heat to obtain a granulated material.
[0053] Regarding step 1) In this step, a crushed material containing the resin is prepared.
[0054] As described above, the resin-containing crushed material is preferably crushed material of recycled resin films such as optical films. The thickness of the recycled material is the same as that of the optical film.
[0055] The resin film is preferably crushed under conditions that minimize the heat generated during crushing and that the crushed material is subjected to, that is, under conditions that result in the bulk density of the resulting film pieces being appropriately low.
[0056] Specifically, the bulk density of the crushed material obtained is 0.01 to 0.25 g / cm 3 It is preferable that the bulk density of the crushed material obtained is 0.25 g / cm 3 If the bulk density of the crushed material is less than 0.01 g / cm3 (i.e., if the crushed material is large), the load during crushing and the heat generated by the crushing are reduced, and deterioration of the crushed material due to the heat during crushing and the resulting coloring are easily suppressed. 3 From the above viewpoint, the crushed material is not too large and can be easily granulated. The bulk density of the crushed material obtained is 0.07 to 0.18 g / cm 3 It is more preferable that the amount is about 100%.
[0057] The bulk density of the crushed material can be measured by the following method. Fill a 100mL container with crushed material until it is completely filled, and measure the mass of the crushed material (or granulated material). This measurement is carried out 10 times, and the average bulk density is calculated in relation to the volume. Note that no tapping is performed when filling the container.
[0058] The size of the crushed material is not particularly limited as long as the bulk density satisfies the above range, but is preferably an approximately square with a side length of about 2 to 8 mm (or a rectangle with the same area). If the side length of the crushed material is 2 mm or more, the bulk density of the crushed material is easily reduced, and the bulk density is easily adjusted to the above range. If the side length of the crushed material is 8 mm or less, the crushed material is not too large, and subsequent melting by frictional heat is easy. From the above viewpoint, it is more preferable that the size of the crushed material is an approximately square with a side length of about 3 to 7 mm (or a rectangle with the same area).
[0059] The fraction (%) of the crushed material separated when sieved for 2 minutes using a mesh with an average opening of 1 mm (fractionation rate) is not particularly limited, but may be, for example, 10% by mass or less relative to the total amount of crushed material before sieving. Crushed material with a fractionation rate of 10% by mass or less is crushed under gentle conditions and the load during crushing is appropriately small, making it easier to suppress thermal deterioration of the resin due to heat generated during crushing. From the above viewpoint, it is more preferable that the fractionation rate (%) of the crushed material is 5% by mass or less relative to the total amount of crushed material before sieving.
[0060] The bulk density, size and fractionation rate of the crushed material can be adjusted by the crushing conditions. In order to make the bulk density, size and fractionation rate of the crushed material within the above range, it is preferable to reduce the heat generated during crushing (reduce the heat that the returned material receives during crushing), specifically, to reduce the load during crushing or remove heat to reduce the heat generated during crushing.
[0061] The resin film can be crushed by any method, for example, by pinching the recycled material between a fixed blade and a rotary blade.
[0062] Regarding step 2) Next, frictional heat is generated in the crushed material, and the crushed material is melted or fused by the heat.
[0063] The melting by frictional heat is preferably carried out at (50 to Tg)°C (Tg is the glass transition temperature of the resin). When the melting temperature by frictional heat is 50°C or higher, the crushed material can be in a semi-molten state, so that a granulated material with reduced bulk density is easily obtained. When the melting temperature is Tg°C or lower, the crushed material does not become too hot, so that thermal deterioration of the resin can be suppressed, so that a decrease in the molecular weight of the resin and coloring of the granulated material can be suppressed. In addition, from the viewpoint of further suppressing yellowing of the recycled film obtained using the granulated material, the melting temperature is more preferably 50 to 100°C, and even more preferably 60 to 100°C.
[0064] The melting temperature can be measured as the ambient temperature during melting due to frictional heat. For example, in a crushing / granulating device 10 shown in Fig. 1 described later, the melting temperature can be measured as the ambient temperature downstream of the melting process due to frictional heat (for granulation) (see Fig. 2 described later).
[0065] The melting temperature can be adjusted by, for example, the magnitude of friction applied to the crushed material, the time for which friction is applied (residence time), cooling treatment, etc. When using the crushing / granulating device 10 described later, the melting temperature can be adjusted by the supply speed of the crushed material, the width and length of the flow path in the compression section B or the transfer section C, the degree of cooling or heat removal by the temperature adjustment section (cooling means), etc. When the melting temperature is to be lowered, for example, it is preferable to make the width of the flow path in the compression section B or the transfer section C of the crushing / granulating device 10 appropriately large and the length appropriately short. It is also preferable to lower the cooling temperature by the temperature adjustment section (cooling means) inside and outside the device, or to reduce the supply speed of the crushed material. In particular, it is preferable to cool the crushed material by the temperature adjustment section (cooling means) so that the melting temperature of the crushed material is within the above range.
[0066] The crushed material melted by frictional heat may be further cut into a predetermined size (or length).
[0067] (Physical properties of granulated material) The bulk density of the granulated material is preferably higher than that of the crushed material. Specifically, the bulk density of the granulated material is preferably higher than that of the crushed material and lower than that of new pellets (not recycled products) (for example, 80% or less of the bulk density of new pellets). Specifically, the bulk density of the granulated material is preferably 0.26 to 0.45 g / cm 3 It is preferable that the bulk density of the granules is 0.26 g / cm 3 If the bulk density of the granulated product is 0.45 g / cm or more, the granulated product can be easily transported and stored, and the handling properties can be improved. 3 If the bulk density is less than 0.35 g / cm, excessive heat is not applied during granulation, so that thermal deterioration of the resin in the granulated material can be suppressed, and the molecular weight reduction and coloring of the resin constituting the granulated material can be suppressed. In addition, a recycled film obtained by using such a granulated material can maintain good mechanical properties and optical properties. From the above viewpoint, the bulk density of the granulated material is 0.35 to 0.45 g / cm. 3 The bulk density of the granulated material can be measured in the same manner as the bulk density of the crushed material.
[0068] The bulk density of the granulated material can be about 150 to 1500% of the bulk density of the crushed material.
[0069] The bulk density of the granulated material can be adjusted by the melting temperature and the aspect ratio of the granulated material. In order to appropriately lower the bulk density of the granulated material, it is preferable to appropriately lower the melting temperature and to appropriately increase the aspect ratio of the granulated material.
[0070] The aspect ratio of the granulated product can be appropriately set so that the bulk density of the granulated product satisfies the above range and in accordance with the required handleability. The aspect ratio of the granulated product is preferably, for example, 4 to 50. When the aspect ratio is 4 or more, for example, the granulated product is less likely to adhere to the inner wall surface of a pipe during air transport, making it easier to suppress the inclusion of foreign matter when switching between different types of products, and when the aspect ratio is 50 or less, the bulk density of the granulated product does not become too high, making it less likely to impair the handleability during transportation and storage. From the above viewpoint, the aspect ratio of the granulated product is more preferably 4 to 20. The aspect ratio of the granulated product refers to the average value (average aspect ratio) of the ratio of the length of the major axis to the length of the minor axis of the granulated product.
[0071] The aspect ratio of the granulated product can be measured by the following method. First, for each of 100 random granules, the lengths of the long and short axes of the granules are measured from an image captured by a camera, and the aspect ratio (long axis length / short axis length) is calculated. The long axis is the line segment connecting the two most distant points on the outline of the granule image in the captured image, and the short axis is the longest line segment among the line segments connecting the intersection points of the outline with a straight line perpendicular to the long axis. The average of the obtained aspect ratios is defined as the "aspect ratio."
[0072] The aspect ratio of the granules can be adjusted by the cut length and diameter of the string-like resin extruded from the crushing / granulating device 10 (or the inner diameter of the extrusion port 22 of the crushing / granulating device 10).
[0073] From the viewpoint of reducing coloration of the resulting film, it is preferable that the YI of the granulated product is small. Specifically, the YI of the granulated product is preferably 1.0 or less, and more preferably 0.6 or less.
[0074] The YI of the granulated product can be measured using a spectrophotometer (for example, a spectrophotometer CM-3700d manufactured by Konica Minolta) at a viewing angle of 10° using D65 (color temperature 6504K) as a light source.
[0075] Granulation by frictional heat can be carried out by any method, for example, by using an extrusion device having a screw.
[0076] The above steps 1) and 2) may be carried out in separate apparatuses, or may be carried out in one continuous apparatus. As a continuous apparatus, for example, an apparatus similar to that described in JP-A-54-45365 may be used. In the following embodiment, an example in which the above steps 1) and 2) are carried out in one continuous apparatus is shown.
[0077] Fig. 1 is a cross-sectional view showing the configuration of a crushing / granulating device 10 in this embodiment. Fig. 2 is an enlarged view of the main part of Fig. 1.
[0078] As shown in FIG. 1, the crushing / granulating device 10 includes a cylinder 20, a screw 30 rotatably disposed therein, a cutting section 40, a separating section 50, and a temperature adjusting section 60.
[0079] The cylinder 20 has a supply port 21 through which returned material 70 such as a resin film is supplied, and an extrusion port 22 through which the returned material 70 compressed by the cylinder 20 is extruded.
[0080] The screw 30 has a rotating shaft 31, and a cutter screw 32A, a mixing screw 32B, and a conveyor screw 32C arranged around the rotating shaft 31. That is, the crushing / granulating device 10 has, along the screw 30, in order from the supply port 21 side, a crushing section A (region corresponding to the cutter screw 32A) that crushes the returned material 70, a compression section B (region corresponding to the mixing screw 32B) that compresses the crushed material to generate frictional heat, and a transfer section C (region corresponding to the conveyor screw 32C) that melts and transfers the returned material by frictional heat.
[0081] The cutter screw 32A in the crushing section A may be, for example, a rotary blade formed in a stripe screw shape. On the inner wall surface of the cylinder 20 corresponding to the cutter screw 32A, a plurality of fixed blades 23 are arranged so that the cutting edge is close to the cutter screw 32A. Then, the returned material 70 supplied into the cylinder 20 is cut by the fixed blades 23 and the cutter screw 32A.
[0082] In the compression section B, the cylinder 20 corresponding to the mixing screw 32B is tapered so that its inner diameter becomes smaller in the feed direction. The mixing screw 32B is tapered to match the cylinder 20, and may have, for example, a multi-thread screw. The returned material 70 is compressed in the process of passing through the flow path between the cylinder 20 and the mixing screw 32B, generating frictional heat.
[0083] The conveyor screw 32C in the transfer section C is formed, for example, in a multi-thread screw shape so as to reduce heat generation. A certain propulsive force is applied to the returned material 70 sent from the mixing screw 32B in a semi-molten state, and the returned material 70 is extruded from the extrusion port 22 in a string shape.
[0084] That is, the above step 1) can be carried out in the crushing section A, and the melting by frictional heat in the above step 2) can be carried out in the compression section B and the transfer section C. In the present invention, the melting temperature during melting by frictional heat in the above step 2) is adjusted to the above range, that is, 50 to Tg (°C). In the crushing / granulating device 10 shown in Fig. 1, the melting temperature can be measured by a thermocouple 24 arranged in the vicinity of the extrusion port 22 (see Fig. 2).
[0085] As described above, the melting temperature can be adjusted by, for example, the supply speed of the crushed material (such as the number of revolutions of the screw), the taper angle of the compression section B, the width W1 (or W2) of the flow path between the mixing screw 32B (or the convention screw 32C) and the inner wall surface of the cylinder 20 in the compression section B (or the transfer section C) and the length L1 (or L2) in the feed direction, cooling inside and outside the device, etc. When the melting temperature is to be lowered, for example, it is preferable to reduce the supply speed of the crushed material, it is preferable to reduce the taper angle of the cylinder 20, it is preferable to increase the width C1 (or C2) of the gap between the screw 32B (or 32C) and the inner wall surface of the cylinder 20, and it is preferable to shorten the length L1 (or L2) of the gap in the feed direction. In addition, it is also preferable to adjust (cool) the temperature of the cylinder 20 and the screw 30 by the temperature adjustment section 60 described later.
[0086] The cutting unit 40 is disposed near the extrusion port 22 of the cylinder 20, and cuts the extruded string-like returned material 72 to a predetermined length. The cutting unit 40 has, for example, a cutting blade 41, although there is no particular limitation thereto.
[0087] The separating section 50 separates the re-fused granules obtained by cutting in the cutting section 40. The separating section 50 has, although not particularly limited, a cooling or air blowing means 51 such as a cooling blower, and a rotating disk 52 having fins.
[0088] The temperature adjustment unit 60 may be a cooling device for adjusting the temperature of the cylinder 20 and the screw 30 to appropriate temperatures. The temperature adjustment unit 60 includes, for example, a cooling jacket 61 applied from the outside of the cylinder 20 and a water passage means 62 applied from the inside of the screw 30.
[0089] In the crushing / granulating device 10 configured as described above, returned material 70 such as a resin film is fed from the returned material supplying section 1 into the cylinder 20. The fed returned material 70 is cut into crushed material by the cutter screw 32A (rotary blade) and the fixed blade 23 of the cylinder 20 in the crushing section A, and is sent to the compression section B.
[0090] The returned material 70 (crushed material) sent to the compression section B is mixed in a compressed state by passing through the gap between the tapered cylinder 20 and the mixing screw 32B, and moderate frictional heat is generated. The returned material 70 (crushed material) becomes semi-molten due to the frictional heat, and is sent to the transfer section C.
[0091] The returned material 70 sent to the transfer section C in a semi-molten state is moderately fused as it moves through the gap between the cylinder 20 and the conveyor screw 32C, and is extruded in a semi-fused state from the extrusion port 22 at the tip of the cylinder 20.
[0092] In addition, in the compression section B and the transfer section C, the granulation conditions (the size and length of the gap between the screw and the inner wall surface of the cylinder 20), the supply rate of the return material 70, and cooling by the temperature adjustment section 60 are adjusted so that the melting temperature measured by the thermocouple 24 in the compression section B and the transfer section C falls within the above-mentioned range.
[0093] The return material 70 extruded in a string shape is cut into granules of a predetermined length (aspect ratio) by the cutting section 40 to become granulated material (granular material). The obtained granulated material may be re-fused due to heat, but is separated by applying cooling air in the separation section 50. This allows granulated material with an appropriate bulk density to be continuously collected from the discharge port 53.
[0094] Next, a method for producing an optical film (recycled product) using the obtained granules will be described.
[0095] 3. Manufacturing method of optical film The method for producing an optical film of the present invention includes the steps of: 2-1) obtaining granules by the above-described production method; and 2-2) obtaining a film-like material using the obtained granules.
[0096] 2-1) Process Granules are obtained by the above-mentioned manufacturing method.
[0097] 2-2) Process The resulting granules are used to obtain a film-like material. The film-like material can be obtained by any method, and may be obtained by a melt casting method or a solution casting method.
[0098] (Melt casting method) In the melt casting method, a hot-melt granulated material is cast and then cooled and solidified to obtain a cast membrane. Specifically, the method can be obtained through A1) a step of casting a hot-melt granulated material, then cooling and solidifying it, and, if necessary, A2) a step of stretching the obtained membrane.
[0099] In the step A1), the prepared granules are melt-kneaded in a twin-screw extruder or the like, and then cast from a casting die. The heat melting temperature in the melt casting can be (Tg+30) to (Tg+70)°C, where Tg is the glass transition temperature of the resin.
[0100] In the step A2), the stretching may be performed according to the desired optical properties, and it is preferable to stretch in one or more directions among the width direction (TD), the machine direction (MD), and an oblique direction.
[0101] The stretching ratio is set according to the required optical performance, and can be 1.01 to 1.3 times from the viewpoint of functioning as a film with low retardation, for example. The stretching ratio is defined as (stretching direction size of film after stretching) / (stretching direction size of film before stretching). The stretching temperature (drying temperature during stretching) is preferably (Tg-20) to (Tg+30)°C.
[0102] (Solution casting method) In the solution casting method, a solution (dope) in which the granulated material is dissolved in a solvent is cast and then dried to obtain a cast membrane. Specifically, the method can be produced through the steps of B1) preparing a dope containing the granulated material, B2) casting the obtained dope onto a support, drying and peeling the dope to obtain a membrane, and B3) stretching the obtained membrane, if necessary.
[0103] In the step B1), the granulated material is dissolved in a solvent to prepare a dope. The solvent used contains an organic solvent (good solvent) capable of dissolving at least the cycloolefin resin. Examples of the good solvent include chlorine-based organic solvents such as methylene chloride; and non-chlorine-based organic solvents such as methyl acetate, ethyl acetate, acetone, and tetrahydrofuran, and preferably methylene chloride. The solvent used may further contain a poor solvent such as an aliphatic alcohol having 1 to 4 carbon atoms, such as methanol and ethanol, from the viewpoint of enhancing the peelability of the casting film from the support.
[0104] In the step B2), the obtained dope is extruded from a casting die and cast onto a support, and then the solvent is evaporated from the dope cast onto the support, followed by peeling off to obtain a film.
[0105] In step B3), the obtained film-like material is stretched. The stretching ratio and stretching temperature can be the same as those in step A2).
[0106] The optical film thus obtained can be preferably used as a protective film (including a retardation film, etc.) for a polarizing plate.
[0107] (Optical film properties) The total light transmittance of the optical film is not particularly limited as long as it has sufficient light transmittance, but is preferably 80% or more, more preferably 85% or more, and even more preferably 88% or more. The total light transmittance of the optical film can be measured in accordance with JIS K7361-1:1997.
[0108] The difference in YI before and after recycling of the optical film is preferably less than 0.1, more preferably less than 0.05, and even more preferably less than 0.03. The difference in YI before and after recycling of the optical film can be calculated as the difference (YI1-YI0) between YI0 of the optical film (recycled material) before recycling and YI1 of the optical film after recycling (manufactured using the granulated material). YI can be measured by the same method as above. EXAMPLES
[0109] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these.
[0110] 1. Optical film (return material) materials (1) Resin Cycloolefin resin (COP): Cycloolefin resin containing the following structural units (Tg: 165°C, Mw: 150,000) [ka]
[0111] (Meth)acrylic resin (Acr): MMA / N-phenylmaleimide / 2-ethylhexyl acrylate copolymer (Tg: 120℃, Mw: 2 million)
[0112] The Tg and Mw of the resin were measured by the following method.
[0113] (Tg) The Tg of the resin was measured using DSC (Differential Scanning Colorimetry) in accordance with JIS K 7121-2012.
[0114] (Mw) The Mw of the resin was measured using gel permeation chromatography (HLC8220GPC manufactured by Tosoh Corporation) under the following conditions. (Measurement conditions) Eluent:THF Column: Tosoh TSKgel GMHXL x 2 Flow rate: 1.0mL / min Sample concentration: 0.1% by mass Injection volume: 100μL Detector: RI Calibration curve: Standard polystyrene
[0115] (2) Rubber particles Rubber particles (Kane Ace M210 manufactured by Kaneka Corporation, average primary particle diameter R: 200 nm)
[0116] (3) Additives Irganox 1076 (BASF Japan) (antioxidant)
[0117] 2. Preparation of optical film (return material) <Preparation of Film A-1> (Preparation of additive solution) 95 parts by mass of methylene chloride was placed in a sealed container, and 0.00145 parts by mass of Irganox 1076 (manufactured by BASF Japan) (antioxidant) was added while stirring. The mixture was then stirred and mixed for 50 minutes using a dissolver. The resulting mixture was passed through a high-pressure dispersion device (product name: Ultra High Pressure Homogenizer M110-E / H, manufactured by Microfluidics Corporation) and treated once at 175 MPa, and then filtered through Finemet NF manufactured by Nippon Seisen Co., Ltd. to obtain an additive solution (antioxidant content of 0.0015% by mass).
[0118] (Preparation of dope) Next, a dope having the following composition was prepared. First, methylene chloride and ethanol were added to a pressure dissolving vessel. Next, pellets of cycloolefin resin (COP-1) were added to a pressure dissolving tank while stirring, and then the additive solution prepared above was added and completely dissolved or dispersed while stirring. The obtained solution was filtered using SHP150 manufactured by ROKI TECHNO CO., LTD., to obtain a dope having the following composition. Cycloolefin resin (COP): 100 parts by mass Methylene chloride: 220 parts by mass Ethanol: 35 parts by weight Additive solution: 200 parts by weight
[0119] (Film forming) On the stainless steel belt support, the solvent was evaporated until the residual solvent content in the cast dope was 30% by mass. Then, the dope was peeled off from the stainless steel belt support at a peeling tension of 128 N / m to obtain a film-like material (the residual solvent content of the film-like material at the time of peeling was 30% by mass). While the peeled film was transported by a number of rollers, the obtained film-like material was stretched by 30% in the width direction at (Tg+15) ° C. (140 ° C. in this example) in a tenter. The residual solvent content of the film-like material at the start of stretching was 10% by mass. After that, the film was further dried at (Tg-20) ° C. while being transported by rolls, and a film A-1 (cycloolefin resin film) with a thickness of 40 μm was obtained. The obtained film A-1 was slit by a laser cutter to obtain a return material.
[0120] <Preparation of Film A-2> A film A-2 (cycloolefin resin film) having a thickness of 15 μm was obtained in the same manner as film A-1, except that the casting amount was changed.
[0121] <Preparation of Film A-3> (Preparation of Rubber Particle Dispersion) 11.3 parts by mass of rubber particles R1 and 200 parts by mass of methylene chloride were mixed and stirred in a dissolver for 50 minutes, and then dispersed at 1500 rpm using a Milder disperser (manufactured by Pacific Machinery Works, Ltd.) to obtain a rubber particle dispersion.
[0122] (Preparation of dope) Next, a dope having the following composition was prepared, and a film A-3 (a (meth)acrylic resin film) having a thickness of 40 μm and a remnant thereof were obtained in the same manner as in the film A-1, except that the dope was used. (Meth)acrylic resin: 100 parts by mass Methylene chloride: 220 parts by mass Ethanol: 35 parts by weight Rubber particle dispersion: 200 parts by mass
[0123] 3. Production and evaluation of granules <Test 1> (Crushing of return materials) The resulting recycled material is crushed in the crushing section A of the crushing / granulating device 10 in FIG. 1 to produce pellets with a size of 2 mm square (2 mm × 2 mm) and a bulk density of 0.10 g / cm 3 As a result, film pieces (crushed material) of 1000 g were obtained.
[0124] (Melting and granulation due to frictional heat) The crushed material was melted (granulated) by frictional heat in the compression section B and transfer section C of the crushing / granulating device 10 in Fig. 1. Granulation (melting) was carried out while cooling (cooling by passing water) by the temperature adjustment section 60. The melting temperature by frictional heat was measured by a K-type thermocouple (thermocouple 24) arranged near the extrusion port 22 of the crushing / granulating device 10 in Fig. 1.
[0125] Next, the resin extruded in a string shape from the crushing / granulating device 10 was cut to a predetermined length so that the bulk density of the granulated material would be the value shown in Table 1, thereby obtaining granulated material.
[0126] <Tests 2-6> Granulation was performed in the same manner as in Test 1, except that the cooling temperature (water temperature) by the temperature adjustment unit 60 was changed to change the granulation conditions (melting temperature due to frictional heat) as shown in Table 1.
[0127] <Tests 7 and 8> Granulation was performed in the same manner as in Test 1, except that the granulation conditions (treatment speed) were changed as shown in Table 1.
[0128] <Tests 9, 10 and 12> Granulation was performed in the same manner as in Test 4, except that the cutting length was changed so that the aspect ratio of the granulated product would be the value shown in Table 1.
[0129] <Test 11> Granulation was performed in the same manner as in Test 1, except that the cutting length was changed so that the aspect ratio of the granulated product would be the value shown in Table 1.
[0130] <Test 13> Granulation was performed in the same manner as in Test 4, except that the type of return material (thickness of the film piece) was changed to that shown in Table 1.
[0131] <Test 14> Granulation was performed in the same manner as in Test 4, except that the type of recycled material (type of resin) and the granulation conditions (melting temperature) were changed to the values shown in Table 1. The melting temperature was adjusted by changing the cooling temperature by the temperature adjustment unit 60.
[0132] <Test 15> Granulation was performed in the same manner as in Test 14, except that the granulation conditions (melting temperature) and the aspect ratio of the granulated product were changed as shown in Table 1. The melting temperature was adjusted by changing the cooling temperature by the temperature adjustment unit 60.
[0133] <Evaluation> The bulk density before and after granulation, the aspect ratio of the granules, and the molecular weight of the resin used in Tests 1 to 15, as well as the properties of the films made using the granules (coloration, presence or absence of foreign matter contamination) were evaluated by the following methods.
[0134] (1) Bulk density The crushed material (or granulated material) was filled to the brim in a 100 mL container, and the mass of the crushed material (or granulated material) was measured. This measurement was performed 10 times, and the average bulk density was calculated from the relationship with the volume. Note that no tapping was performed when filling the container.
[0135] (2) Aspect ratio of granulated material The aspect ratio of the granulated product was measured by the following procedure. First, for each of 100 random granules, the lengths of the long and short axes of the granules were measured from an image captured by a camera, and the aspect ratio (long axis length / short axis length) was calculated. The long axis was taken as the line segment connecting the two most distant points on the outline of the granule image in the captured image, and the short axis was taken as the longest line segment among the line segments connecting the intersection of a straight line perpendicular to the long axis and the outline. The average of the obtained aspect ratios was taken as the "aspect ratio."
[0136] (3) Molecular weight of the resin in the granulated product The Mw of the resin after granulation was measured in the same manner as in measuring the Mw of the resin before granulation. And the evaluation was based on the following criteria: ○: The decrease in Mw (relative to Mw before granulation) is less than 20% ×: The decrease in Mw is 20% or more (relative to Mw before granulation)
[0137] (4) Film characteristics (Production of recycled film) A recycled film having a thickness of 40 μm was obtained in the same manner as in the production method of Films A-1 to A-3, except that the obtained granules were used as the resin.
[0138] (evaluation) (4-1)YI The YI0 of the film before recycling (new film) and the YI1 of the film after recycling (recycled film) were measured using a Konica Minolta CM-3700d spectrophotometer, using D65 (color temperature 6504K) as the light source, and a viewing angle of 10°. And the evaluation was based on the following criteria: ◎: YI increase (YI1-YI0) is less than 0.03 〇: The increase in YI (YI1-YI0) is 0.03 or more and less than 0.05. △: The increase in YI (YI1-YI0) is 0.05 or more and less than 0.1. ×: YI increase (YI1-YI0) is 0.1 or more If it was △ or higher, it was considered to be within the acceptable range.
[0139] (4-2) Foreign matter contamination (Preparation of Film B) Film B having a thickness of 40 μm and its return film were obtained in the same manner as Films A-1 to A-3, except that no antioxidant was added.
[0140] (Crushing and granulation of return materials) The resulting recycled material was crushed in the same manner and under the same conditions as in Test 1, and granulated material was obtained in the same manner and under the same conditions as in Test 1, except that the crushed material was melted by frictional heat and granulated.
[0141] (Preparation of recycled film B) (1) Pipe cleaning included Recycled film B-1 was produced in the same manner as recycled film A-1, except that after the inside of the pipe after the granulated material of film A-1 was air-fed, the inside of the pipe was cleaned and then the granulated material of film B was air-fed into the same pipe.
[0142] (2) No pipe cleaning Recycled film B-2 was produced in the same manner as recycled film A-1, except that the inside of the pipe after the granulated material of film A-1 was not cleaned, and the granulated material of film B was fed into the pipe without any cleaning.
[0143] (evaluation) The YI1 of the recycled film B-1 (with pipe cleaning) and the YI2 of the recycled film B-2 (without pipe cleaning) were measured in the same manner as above. The effects of foreign matter contamination were evaluated based on the following criteria. ◎: The increase in YI (YI2-YI1) is less than 0.03 〇: The increase in YI (YI2-YI1) is 0.03 or more and less than 0.05. △: The increase in YI (YI2-YI1) is 0.05 or more and less than 0.1. ×: YI increase (YI2-YI1) is 0.1 or more If it was △ or higher, it was considered to be within the acceptable range.
[0144] The evaluation results of the granules obtained in Tests 1 to 15 are shown in Table 1.
[0145] [Table 1]
[0146] As shown in Table 1, melting by frictional heat at a low temperature below Tg and the bulk density of the granulated material is 0.6 g / cm 3 It can be seen that the granulated materials of Tests 2 to 5, 8 to 10, and 13 to 14, which were adjusted to the following (80% or less of new pellets), can reduce the molecular weight reduction and discoloration of the resin caused by thermal degradation, and can also suppress the introduction of foreign matter when changing types.
[0147] In contrast, melting by frictional heat at a high temperature exceeding Tg and keeping the bulk density of the granulated material at 0.6 g / cm 3 It can be seen that the granules of Tests 1, 11 (Test 11 corresponds to the conditions in Patent Document 1), and 15, which were adjusted to over 90% of the new pellets, not only suffered from a decrease in molecular weight of the resin and discoloration due to thermal degradation, but also suffered from the inclusion of foreign matter when changing the type.
[0148] The reason why foreign matter was mixed in in Test 6 is unclear, but it is thought that the granulation temperature was too low, so some of the crushed material remained in the crushed state before granulation, and this foreign matter adhered to the inner walls of pipes, etc. and became mixed in.
[0149] This application claims priority to Japanese Patent Application No. 2020-216666, filed December 25, 2020. The contents of the specification and drawings of that application are incorporated herein by reference in their entirety. [Explanation of symbols]
[0150] 10 Crushing and granulating equipment 20 cylinders 21 Supply port 22 Extrusion port 23 Fixed blade 24 Thermocouple 30 Screw 31 Rotation axis 32A Cutter screw 32B mixing screw 32C Conveyor screw 40 Cut section 41 Cutting blade 50 Separation part 51 Cooling Blower 52 Rotating disc 60 Temperature adjustment section 61 Cooling jacket 62 Water passage means 70 Return material A Crushing section B Compression section C Transfer section W1, W2 (flow path) width L1, L2 (flow path) length
Claims
1. The composite material contains one or more resins selected from the group consisting of (meth)acrylic resins and cycloolefin resins, and has a bulk density of 0.01 to 0.25 g / cm 3 preparing a crushed material comprising: The crushed material is melted by frictional heat at a temperature of (50 to Tg) ° C. (Tg is the glass transition temperature of the resin) to obtain a bulk density of 0.26 to 0.45 g / cm. 3 and obtaining a granulated product comprising the steps of: A method for producing granulated material.
2. The crushed material is obtained by crushing a recycled film containing the resin. A method for producing the granules according to claim 1.
3. The crushed material is cooled so that the temperature is (50 to Tg) ° C. A method for producing the granules according to claim 1 or 2.
4. The melting by frictional heat is carried out at 50 to 100°C. A method for producing the granules according to any one of claims 1 to 3.
5. The aspect ratio of the granules is 4 to 50. A method for producing the granules according to any one of claims 1 to 4.
6. A step of obtaining a granulated product by the method for producing a granulated product according to any one of claims 1 to 5; The granules are melted or dissolved in a solvent to obtain a membrane-like material. A method for producing an optical film.
7. The step of obtaining the film-like material includes: dissolving the granulated material in a solvent to obtain a dope; and casting the dope on a support, drying the dope and peeling the dope to obtain a film. The method for producing the optical film according to claim 6 .
Citation Information
Patent Citations
Method and apparatus for granulating resin
JP1979045365A
Method of manufacturing optical film
JP2020166194A
Optical film manufacturing method
JP2021016964A