Sulfur-based and alkali-based solid waste stirring, granulating and foaming one-step-forming sintering-free high-strength lightweight aggregate, and preparation method therefor and use thereof
Through a one-time molding process of sulfur-based solid waste mixing, granulation and foaming, combined with sulfur-aluminum-iron cementitious materials and foaming agents, high-strength lightweight aggregates are formed, which solves the problems of low solid waste utilization rate and high energy consumption. It achieves efficient resource utilization and low-cost production, and is suitable for a variety of building material applications.
Patent Information
- Application Number
- PCT/CN2023/098961
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2023-06-07
- Publication Date
- 2024-10-03
AI Technical Summary
The existing lightweight aggregate preparation process has problems such as low solid waste utilization rate, raw materials need to be pre-treated before granulation, poor product quality controllability, high energy consumption, large CO2 emissions and high cost. In addition, the traditional sintering method consumes high energy and It has large carbon emissions and is difficult to apply in load-bearing structures.
The sulfur-based solid waste is used to stir, granulate and foam in one step to form a burn-free high-strength light aggregate. Through the combination of sulfur-based solid waste, alkaline solid waste, auxiliary gelling materials, sulfur-aluminum-iron cementitious materials and foaming agents , realize solid waste resource utilization and high-value utilization, adopt the integrated mixing and granulation process to avoid high-temperature sintering and steam curing, use H2O2 as the foaming agent to form C(N)-A-S-H gel and ettringite, and improve the lightness Aggregate strength and properties.
It achieves efficient resource utilization of solid waste, low production costs, and saves natural resources. The product has high strength, low bulk density, and mechanical strength superior to high-temperature sintered ceramsite lightweight aggregate. It is suitable for ready-mixed lightweight aggregate concrete and lightweight aggregates. Products such as concrete blocks solve the problem of solid waste storage and reduce energy consumption and CO2 emissions.
Smart Images

Figure 000001 
Figure 000002 
Figure 000003
Abstract
Description
Sulfur-based and alkali-based solid waste mixing, granulation and foaming in one step to form unburned high-strength lightweight aggregate and its preparation method and application
[0001] The present invention claims priority to the Chinese patent application filed with the Patent Office of China on March 27, 2023, with application number 202310301719.8 and invention name “Sulfur-based and alkali-based solid waste mixing, granulation and foaming, one-time molding, fire-free high-strength lightweight aggregate and its preparation method and application”, the entire contents of which are incorporated by reference into the present invention. Technical Field
[0002] The present invention relates to the technical field of building materials, realizing the resource conversion and high-value utilization of sulfur-based solid waste and alkali-based solid waste, and specifically relates to a one-step molding, fire-free high-strength lightweight aggregate through stirring, granulating and foaming of sulfur-based and alkali solid waste, as well as a preparation method and application thereof. Background Art
[0003] my country has a large annual production and inventory of sulfur-based solid wastes such as desulfurized gypsum, phosphogypsum, and titanium gypsum, as well as alkaline waste residues such as red mud and steel slag. However, their high-value resource utilization rate is low. The development of multifunctional green building materials with lightweight, high-strength, energy-saving, and thermal insulation properties has become a key focus in the industry. Unlike traditional sand and gravel aggregates, lightweight aggregates, with their high strength and excellent workability, can replace natural aggregates in construction and transportation applications.
[0004] Currently, most lightweight aggregates are produced by burning natural raw materials such as shale, resulting in high energy consumption, large carbon emissions, and high natural resource consumption. Some use solid waste to burn lightweight aggregate, which presents a series of problems, including difficulty in homogenizing the properties of the solid waste, large fluctuations in the firing schedule, poor product performance stability, and difficulty in using it in load-bearing structures. In recent years, some scholars have explored the use of non-burning methods to produce non-burning lightweight aggregates, which offer advantages over traditional sintering methods, such as energy conservation, environmental protection, and low cost. However, existing non-burning lightweight aggregate production processes often use rollers and pelletizing discs for secondary granulation, and all raw materials must be pre-treated before granulation, resulting in complex processes and poor controllability of product quality. The binder used is mostly ordinary Portland cement, which has high energy consumption and high CO2 emissions. To improve the strength of lightweight aggregate, various admixtures are often added, resulting in high production costs.
[0005] Summary of the Invention
[0006] In view of the shortcomings of the existing technology, one of the purposes of the present invention is to provide a sulfur-based alkali solid waste stirring granulation foaming one-time molding fire-free high-strength lightweight aggregate, which has high strength, easy to obtain raw materials, and a simple and easy preparation process, without the need for high-temperature sintering and steam curing. At the same time, it overcomes the defects of the existing technology such as low solid waste utilization rate, the need for pretreatment of raw materials before granulation, poor product quality controllability, high energy consumption, large CO2 emissions and high cost.
[0007] To achieve this object, the present invention adopts the following technical solutions: In a first aspect, the present invention provides a sulfur-based and alkaline solid waste stirred, granulated and foamed one-step forming non-fired high-strength lightweight aggregate, comprising sulfur-based solid waste, alkaline solid waste, auxiliary gelling material, sulfur-aluminum-iron based gelling material, water, and a foaming agent; based on the total solid mass as 100%, the mass percentages of the sulfur-based solid waste, alkaline solid waste, auxiliary gelling material, and sulfur-aluminum-iron based gelling material are as follows: 80%-90% of the total of the sulfur-based solid waste, alkaline solid waste and auxiliary gelling material, and 10%-20% of the sulfur-aluminum-iron based gelling material; the mass ratio of water to total solids is 15-20:80-85; and the foaming agent is 0.3%-0.7% of the total solid mass;
[0008] The mass ratio of sulfur-based solid waste: alkali-based solid waste: auxiliary gelling material is 27-33: 27-33: 18-25.
[0009] The total solid mass is the total mass of sulfur-based solid waste, alkaline solid waste, auxiliary gelling materials, and sulfur-aluminum-iron gelling materials.
[0010] The present invention provides a way to efficiently utilize sulfur-based solid waste and alkali-based solid waste. The method uses sulfur-based and alkali-based solid waste as main raw materials, utilizes the synergistic complementarity of alkali-based and sulfur-based solid waste, and cooperates with aluminum-iron based gelling materials and foaming agents to realize resource-based and high-value utilization of solid waste. It better solves the problem of long-term storage of large amounts of difficult-to-treat solid waste and environmental impact, while greatly improving its excellent performance as a lightweight aggregate. The stacking density is low, and the mechanical strength is better than that of high-temperature sintered ceramsite lightweight aggregate. The method can be widely used in products such as premixed lightweight aggregate concrete, lightweight concrete blocks, and wallboard products.
[0011] More specifically, the present invention uses alkaline solid waste (such as red mud, steel slag, alkaline slag, etc.) and sulfur-based solid waste (such as phosphogypsum, desulfurized gypsum, etc.) as raw materials. The alkali in the alkaline solid waste can dissolve the active Si-Al structure in the auxiliary cementitious material and the cementitious material. The active Si-Al structure is in the Ca 2+ / Na + With the participation of , it can be hydrated to form C(N)-ASH gel. Phosphogypsum can dissolve a large amount of Ca 2+ and SO4 2- , under alkaline conditions, SO4 2- It can stimulate the hydration of auxiliary cementitious materials and cementitious materials to form ettringite. Therefore, based on the synergistic effect of the two solid wastes, the hydration of minerals can be achieved. The hydration-generated C(N)-ASH gel and ettringite jointly improve the strength performance of the unburned lightweight aggregate.
[0012] Preferably, the sulfur-based solid waste includes desulfurized gypsum, phosphogypsum, and titanium gypsum; the sulfur-based solid waste SO3 content is ≥40wt%, and the average particle size of the solid waste is ≤50μm. The sulfur-based solid waste can provide a large amount of SO4 for the hydration of the system. 2- , SO42- It can stimulate the auxiliary cementitious material and cementitious material to generate ettringite, thereby providing the early strength of the unburned lightweight aggregate.
[0013] Preferably, the alkaline solid waste includes red mud, steel slag, and alkali slag; the pH of the leachate of the alkaline solid waste is greater than 10, and the average particle size of the solid waste is ≤50 μm. The alkaline solid waste provides an alkaline environment and alkali metal ions (Na + / Ca 2+ The alkaline environment facilitates the dissolution of active Si-Al structures in the system, where alkali metal ions react with the active Si-Al to form C(N)-ASH gel, which can increase the later strength of the unburned lightweight aggregate.
[0014] Preferably, the auxiliary cementitious material mainly comprises CaO, SiO2 and Al2O3, and includes slag powder, fly ash and silica fume.
[0015] Preferably, the ferroaluminum-sulfur cementitious material has a CaO content of <40wt%, Fe2O3>5wt%, and SO3<15wt%. The ferroaluminum-sulfur cementitious material is hydrated to form ettringite and Fe colloid, and these two minerals provide basic strength for the unburned lightweight aggregate product.
[0016] Preferably, the foaming agent includes H2O2. A suitable foaming agent is selected according to the alkalinity of the system, and the foaming agent is more preferably H2O2.
[0017] A second aspect of the present invention provides a method for preparing the aforementioned sulfur-based and alkaline solid waste stirred, granulated, and foamed one-step forming non-fired high-strength lightweight aggregate, comprising the following steps:
[0018] Step 1: Mix the sulfur-based solid waste, alkali-based solid waste, auxiliary cementitious materials and sulfur-aluminum-iron cementitious materials, add a foaming agent and water, and stir to granulate to obtain lightweight aggregate balls;
[0019] Step 2: The lightweight aggregate balls are cured and then sieved to obtain the unburned high-strength lightweight aggregate based on sulfur-based and alkali-based solid waste.
[0020] Preferably, in step 1, mixing the sulfur-based solid waste, alkali-based solid waste, auxiliary gelling material, and sulfur-aluminum-iron based gelling material is performed in an integrated stirring and granulating machine. The drum and stirring shaft of the integrated stirring and granulating machine can rotate independently or jointly. The stirring shaft has a maximum speed of 150 r / min, corresponding to a torque of 480 Nm, a motor frequency of 50 Hz, and a drum wall linear speed of 0.5 to 1.0 m / s.
[0021] Preferably, in step 1, the first stirring is high-speed stirring, specifically stirring at 50 Hz (corresponding to a torque of 480 N.m) for 1 to 5 minutes; the second stirring is medium-speed stirring, specifically stirring at 25 Hz (corresponding to a torque of 960 N.m) for 5 to 25 minutes.
[0022] Preferably, the particle size of the lightweight aggregate spheres is 1 to 20 mm.
[0023] Preferably, the curing is as follows: curing temperature 25-35°C, humidity 92-98%, curing for 0-5 days; then natural curing for 1-5 days, spraying water regularly and turning over lightly once a day. After curing, the lightweight aggregate is screened and graded and stored in different categories. Among them, after curing for 1 day, the strength of the lightweight aggregate is greater than 4MPa. The bulk density of the lightweight aggregate is 600-1000kg / m3 after 7 days. 3 , strength greater than 10MPa, water absorption less than 10%, softening coefficient ≥0.85.
[0024] As a preferred technical solution of the present invention, the method for preparing a high-strength lightweight aggregate by stirring, granulating and foaming sulfur-based solid waste in one step and forming it into a non-fired high-strength lightweight aggregate comprises the following steps:
[0025] Step 1: Add sulfur-based solid waste, alkali-based solid waste, auxiliary gelling material and sulfur-aluminum-iron gelling material in proportion to a stirring and granulating machine, stir at 50 Hz (corresponding to a torque of 480 N.m) for 1 to 5 minutes to mix, add a foaming agent and water, stir at 25 Hz (corresponding to a torque of 960 N.m) for 5 to 25 minutes to granulate to obtain lightweight aggregate balls with a particle size of 1 to 20 mm;
[0026] Step 2: Curing the lightweight aggregate balls at a curing temperature of 25-35°C and a humidity of 92-98% for 0-5 days; then naturally curing for 1-5 days, spraying water regularly and turning over lightly once a day, and screening after curing to obtain sulfur-based alkali solid waste mixing, granulation and foaming one-time molding and fire-free high-strength lightweight aggregate.
[0027] The unfired high-strength lightweight aggregate of the present invention has the advantages of light weight and high strength, and can be widely used in prefabricated components such as building exterior walls, floor slabs, and stairs, on-site cast-in-place building beams and columns, and road pavements. Therefore, a third aspect of the present invention provides the use of the above-mentioned sulfur-based and alkaline solid waste stirred, granulated, and foamed one-step unfired high-strength lightweight aggregate in building materials.
[0028] The beneficial effects achieved by one or more embodiments of the present invention are as follows:
[0029] This invention uses sulfur- and alkali-based solid waste as raw materials to produce unburned high-strength lightweight aggregate, achieving synergistic, complementary, resource-based, and high-value utilization of solid waste. This method has high resource utilization efficiency and low production costs, better resolving the environmental impact of long-term storage of large quantities of difficult-to-treat solid waste and saving natural resource consumption.
[0030] The present invention integrates strong stirring, continuous granulation and foaming of sulfur-based and alkali-based solid wastes to prepare lightweight aggregate without burning, so that the lightweight aggregate components are uniform, the product performance is stable, the process is few, the flow is simple and efficient, energy-saving and carbon-reducing.
[0031] The non-burning high-strength lightweight aggregate based on sulfur-based and alkali-based solid waste prepared by the present invention has a low bulk density of 600-1000kg / m 3 ; High strength, ≥10MPa; Water absorption <10%; Softening coefficient ≥0.85. The product performance is far superior to the indicators of lightweight aggregate product performance standards (GB / T 17431.1-2010 Lightweight aggregate and its test methods Part 1: Lightweight aggregate). DETAILED DESCRIPTION
[0032] To facilitate understanding of the present invention, the present invention is illustrated below with examples. Those skilled in the art should understand that the examples are only used to help understand the present invention and should not be considered as specific limitations of the present invention.
[0033] In the following examples and comparative examples, the SO2 content in the sulfur-based solid waste used is 42.67%, and the average particle size of the solid waste is ≤50μm; the pH of the alkali-based solid waste leachate is 11.5, and the average particle size of the solid waste is ≤50μm; the sulfur-aluminum-iron based cementitious material is a phosphogypsum-based cementitious material, in which the CaO content is 34.79%, the Fe2O3 content is 9.32%, and the SO3 content is 13.60%; and the foaming agent is H2O2.
[0034] In the following examples, the obtained sulfur-based alkali solid waste stirring granulation foaming one-time molding non-fired high-strength lightweight aggregate has a 28d cylinder compressive strength of ≥10MPa and a bulk density of <1000kg / m 3 The lightweight aggregate obtained in the comparative example cannot simultaneously meet the requirements of 28d cylinder compressive strength ≥ 10MPa and bulk density < 1000kg / m 3 .
[0035] Example 1
[0036] The method for preparing a high-strength lightweight aggregate by stirring, granulating and foaming sulfur-based solid waste in one step and forming it into a non-fired high-strength lightweight aggregate comprises the following steps:
[0037] Step 1: 82 wt% of phosphogypsum, red mud, and slag powder in a mass ratio of 30:30:22 and 18 wt% of phosphogypsum-based cementitious material are used as raw materials and pre-mixed at high speed (50 Hz) for 3 minutes.
[0038] Step 2: 16 wt % of water containing 0.5 % of H 2 O 2 was evenly added and stirred at a medium speed (25 Hz) for 6 min.
[0039] Step 3: The cylinder of the mixing and granulating machine is turned over to discharge the material into the container.
[0040] Step 4: Screen the output material.
[0041] Step 5: After screening, the lightweight aggregate pellets are sent to the curing room for curing at a temperature of 28°C and a humidity of 98% for one day. Then, they are naturally cured for three days, spraying water and turning the pellets lightly every day.
[0042] The sulfur-based alkali solid waste stirring granulation foaming one-step molding non-fired high-strength lightweight aggregate product prepared in this embodiment has a cylinder pressure strength of 4.2MPa at 1d, 6.0MPa at 7d, and 10.5MPa at 28d; and a bulk density of 780kg / m 3 , water absorption rate 9.5%, softening coefficient 0.86.
[0043] Example 2
[0044] A method for preparing a high-strength lightweight aggregate that is formed into a one-step, non-fired aggregate by stirring, granulating, and foaming sulfur-based and alkaline solid waste, which differs from Example 1 in that phosphogypsum is replaced by desulfurized gypsum.
[0045] The sulfur-based alkali solid waste stirring granulation foaming one-step molding non-fired high-strength lightweight aggregate product prepared in this embodiment has a cylinder compressive strength of 4.5 MPa at 1 day, 6.8 MPa at 7 days, and 11.2 MPa at 28 days; and a bulk density of 950 kg / m 3 , water absorption rate 7.5%, softening coefficient 0.88.
[0046] The strength and bulk density of the unburned lightweight aggregate prepared using desulfurized gypsum in this embodiment are slightly higher than those of the lightweight aggregate prepared using phosphogypsum (i.e., the lightweight aggregate prepared in Example 1). The specific reason may be the effect of the large amount of phosphorus in phosphogypsum.
[0047] Example 3
[0048] A method for preparing a high-strength lightweight aggregate that is formed into a one-step, fire-free form by stirring, granulating, and foaming sulfur-based and alkaline solid waste, which differs from Example 1 in that red mud is replaced with carbide slag.
[0049] The sulfur-based alkali solid waste stirred granulation foaming one-step forming non-fired high-strength lightweight aggregate product prepared in this embodiment,
[0050] Cylinder pressure strength 1d 4.3MPa, 7d 6.5MPa, 28d 10.8MPa; bulk density 930kg / m 3 , water absorption rate 6.5%, softening coefficient 0.89.
[0051] Comparative Example 1
[0052] A method for preparing a high-strength lightweight aggregate that is formed into a one-step, unburned form by stirring, granulating, and foaming sulfur-based and alkaline solid wastes, which differs from Example 1 in that: in step 1, 85 wt% of phosphogypsum, red mud, and slag powder are used as raw materials, and 15 wt% of phosphogypsum-based cementitious material is used, and no foaming agent is added.
[0053] The sulfur-based alkali solid waste stirring granulation foaming one-step molding non-fired high-strength lightweight aggregate product prepared in this embodiment has a cylinder compressive strength of 6.0 MPa at 3d, 9.3 MPa at 7d, and 14.8 MPa at 28d; and a bulk density of 1100 kg / m 3 , water absorption rate 3.8%, softening coefficient 0.96.
[0054] The improvement of its cylinder pressure strength and bulk density is due to the following two reasons: (1) by adding more alkaline solid waste and sulfur-based solid waste, the above-mentioned alkali-sulfur dual excitation effect is increased, making the hydration reaction more thorough, thereby increasing the mineral content in the system and increasing the strength performance; (2) the fire-free lightweight aggregate product prepared without adding foaming agent has no pore structure distribution inside, and the structure is relatively denser, thereby increasing the strength performance and bulk density of the aggregate.
[0055] Comparative Example 2
[0056] A method for preparing a high-strength lightweight aggregate that is formed into a one-step, fire-free form by stirring, granulating, and foaming sulfur-based solid waste, which differs from Example 1 in that all red mud components are replaced by phosphogypsum.
[0057] The sulfur-based solid waste stirred granulation foaming one-step molding non-fired high-strength lightweight aggregate product prepared in this embodiment has a cylinder compressive strength of 3.5 MPa at 3d, 4.8 MPa at 7d, and 8.5 MPa at 28d; and a bulk density of 830 kg / m 3 , water absorption rate 6.9%, softening coefficient 0.83.
[0058] Comparative Example 3
[0059] A method for preparing a high-strength lightweight aggregate that is formed into a one-step, unburned shape by stirring, granulating, and foaming alkaline solid waste, which differs from Example 1 in that the phosphogypsum component is completely replaced by red mud.
[0060] The alkali-based solid waste stirring granulation foaming one-step molding non-fired high-strength lightweight aggregate product prepared in this embodiment has a cylinder pressure strength of 9.1MPa and a bulk density of 890kg / m 3 , water absorption rate 10.9%, softening coefficient 0.83.
[0061] Comparative Example 4
[0062] A method for preparing a sulfur-based, base-based, solid, and unfired high-strength lightweight aggregate is different from Example 1 in that a ball-forming disk is used for ball formation instead of an integrated stirring and granulation process.
[0063] The sulfur-based alkali solid waste unburned high-strength lightweight aggregate product prepared in this embodiment has a cylinder compressive strength of 3.1 MPa at 3d, 4.9 MPa at 7d, and 7.6 MPa at 28d; and a bulk density of 900 kg / m 3 , water absorption rate 10.3%, softening coefficient 0.80.
[0064] The applicant declares that the present invention uses the above-described embodiments to illustrate the detailed process equipment and process flow of the present invention. However, the present invention is not limited to the above-described detailed process equipment and process flow, and does not necessarily rely on the above-described detailed process equipment and process flow in order to be implemented. Those skilled in the art should understand that any improvements to the present invention, equivalent replacements for the raw materials of the present invention's products, additions of auxiliary ingredients, and selection of specific methods, etc., fall within the scope of protection and disclosure of the present invention.
Claims
1. A sulfur-based alkali solid waste stirring granulation foaming one-time forming non-fired high-strength lightweight aggregate, characterized in that: Including sulfur-based solid waste, alkaline solid waste, auxiliary cementitious materials, sulfur-aluminum-iron cementitious materials, water, and foaming agent; Taking the total solid mass as 100%, the mass percentages of sulfur-based solid waste, alkaline solid waste, auxiliary cementitious materials, and sulfur-aluminum-iron cementitious materials are as follows: sulfur-based solid waste, alkaline solid waste and auxiliary cementitious materials total 80%-90%, and sulfur-aluminum-iron cementitious materials 10%-20%; The mass ratio of water to total solids is 15-20:80-85; The foaming agent is 0.3%-0.7% of the total solid mass; The mass ratio of sulfur-based solid waste: alkali-based solid waste: auxiliary gelling material is 27-33: 27-33: 18-25; The method for preparing the sulfur-based alkali solid waste stirring granulation foaming one-step forming non-fired high-strength lightweight aggregate comprises the following steps: Step 1: Mix the sulfur-based solid waste, alkali-based solid waste, auxiliary cementitious materials and sulfur-aluminum-iron cementitious materials, add a foaming agent and water, and stir and granulate to obtain lightweight aggregate balls; the mixing of the sulfur-based solid waste, alkali-based solid waste, auxiliary cementitious materials and sulfur-aluminum-iron cementitious materials is carried out in a stirring and granulating integrated machine; the first stirring is high-speed stirring, stirring at 50 Hz for 1 to 5 minutes; the second stirring is medium-speed stirring, stirring at 25 Hz for 5 to 25 minutes; Step 2: Curing the lightweight aggregate balls, and then screening them to obtain the unburned high-strength lightweight aggregate based on sulfur-based and alkali-based solid waste; The 28d cylinder compressive strength of the sulfur-based alkali solid waste stirring granulation foaming one-time molding non-fired high-strength lightweight aggregate is ≥10MPa, and the bulk density is <1000kg / m3.
2. The sulfur-based alkali solid waste stirring granulation foaming one-step forming non-fired high-strength lightweight aggregate as claimed in claim 1, characterized in that: The sulfur-based solid waste includes desulfurized gypsum, phosphogypsum, and titanium gypsum; The sulfur-based solid waste has a SO3 content of ≥40wt% and an average particle size of ≤50μm.
3. The sulfur-based alkali solid waste stirring granulation foaming one-step forming non-fired high-strength lightweight aggregate as claimed in claim 1, characterized in that: The alkaline solid waste includes red mud, steel slag and alkaline slag; The pH of the leaching solution of the alkali solid waste is greater than 10, and the average particle size of the solid waste is ≤50 μm.
4. The sulfur-based alkali solid waste stirring granulation foaming one-step forming non-fired high-strength lightweight aggregate as claimed in claim 1, characterized in that: The auxiliary cementitious materials include slag powder, fly ash and silica fume; Or, the sulphur-aluminum-iron based cementitious material comprises a phosphogypsum-based cementitious material, wherein the content of CaO in the sulphur-aluminum-iron based cementitious material is <40wt%, the content of Fe2O3>5wt%, and the content of SO3<15wt%.
5. The sulfur-based alkali solid waste stirring granulation foaming one-step forming non-fired high-strength lightweight aggregate as claimed in claim 1, characterized in that: The foaming agent includes H2O2 and aluminum powder.
6. The method for preparing a non-fired high-strength lightweight aggregate by stirring, granulating and foaming sulfur-based solid waste as described in any one of claims 1 to 5, characterized in that: The steps include: Step 1: Mix the sulfur-based solid waste, alkali-based solid waste, auxiliary cementitious materials and sulfur-aluminum-iron cementitious materials, add a foaming agent and water, and stir and granulate to obtain lightweight aggregate balls; the mixing of the sulfur-based solid waste, alkali-based solid waste, auxiliary cementitious materials and sulfur-aluminum-iron cementitious materials is carried out in a stirring and granulating integrated machine; the first stirring is high-speed stirring, stirring at 50 Hz for 1 to 5 minutes; the second stirring is medium-speed stirring, stirring at 25 Hz for 5 to 25 minutes; Step 2: The lightweight aggregate balls are cured and sieved after curing to obtain the unburned high-strength lightweight aggregate based on sulfur-based and alkali-based solid waste.
7. The preparation method according to claim 6, characterized in that: The particle size of the lightweight aggregate spheres is 1 to 20 mm.
8. The preparation method according to claim 6, characterized in that: In step 2, the curing is as follows: curing temperature is 25-35° C., humidity is 92-98%, curing is 0-5 days; then natural curing is performed for 1-5 days, and water is sprayed regularly and the soil is gently turned over once a day.
9. Use of the sulfur-based alkali solid waste stirring granulation foaming one-time forming non-fired high-strength lightweight aggregate as described in any one of claims 1 to 5 in building materials.
Citation Information
Patent Citations
Method for preparing unbaked ceremsite from solid waste-based sulphoaluminate cementing material
CN109020418A
Red mud-based cementing material, red mud-based lightweight aggregate, red mud-based lightweight aggregate concrete and preparation method thereof
CN112723764A
Multi-element solid waste recycled aggregate and preparation process thereof
CN113149586A
Alkali-sulfur double-excited multi-shell high-strength baking-free lightweight aggregate as well as preparation method and application thereof
CN115140959A
Multi-solid-waste non-sintered ceramsite based on phosphogypsum and preparation method of multi-solid-waste non-sintered ceramsite
CN115368041A
Cited By
High-toughness foamed ceramic as well as preparation method and application thereof