Separation flotation method for carbonaceous copper-molybdenum ore

By using the synergistic effect of copper-molybdenum collector and carbonaceous substance inhibitor in the separation process of copper-molybdenum mixed concentrate, the problems of low molybdenum recovery rate and high separation cost in the existing technology are solved, and efficient molybdenum resource recovery is achieved and copper-molybdenum separation effect.

CN118768080APending Publication Date: 2024-10-15LIANGSHAN MINING CO LTD +1

Patent Information

Application Number
CN202411137325.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The existing copper-molybdenum mixed concentrate separation technology has problems such as low molybdenum recovery rate and high separation cost. In particular, due to the influence of easily floating carbonaceous matter, it is difficult to achieve a molybdenum concentrate grade of more than 35%.

Method used

A method of separation and flotation of carbonaceous copper-molybdenum ores is adopted. By adding copper-molybdenum collector, foaming agent, copper inhibitor and carbonaceous inhibitor to the slurry, multiple separation and concentration processes are carried out, combined with The copper-molybdenum separation process reduces the concentration of carbonaceous matter in molybdenum concentrate and improves the grade of molybdenum concentrate.

Benefits of technology

It improves the grade of molybdenum concentrate, achieves efficient and comprehensive recovery of molybdenum resources, simplifies the process, reduces energy and steel consumption, improves the copper-molybdenum separation effect, and the grade of molybdenum concentrate can be increased to more than 40%.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of mineral processing, and particularly provides a carbonaceous substance copper-molybdenum ore separation flotation method which comprises the following steps: (1) grinding carbonaceous substance copper-molybdenum ore raw ore to a certain fineness to prepare ore pulp meeting the flotation concentration requirement; (2) a copper-molybdenum collecting agent and a foaming agent are sequentially added into the ore pulp, then roughing, scavenging, concentration, dehydration and reagent removal are conducted, a copper inhibitor and a carbonaceous substance inhibitor are added after concentration is conducted, copper concentrate and molybdenum concentrate are obtained through the copper-molybdenum separation technological process of copper-molybdenum separation roughing, scavenging, concentration and middling sequential returning, and then copper concentrate and molybdenum concentrate are obtained; the method can reduce enrichment of carbonaceous substances in the molybdenum concentrate, improve the grade of the molybdenum concentrate and realize efficient comprehensive recovery of molybdenum resources.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of mineral processing, and in particular to a method for separating and flotating carbonaceous copper-molybdenum ores. Background Art

[0002] Molybdenum is a silvery-white transition metal. It is a precious and rare metal that was discovered relatively late and is non-renewable. Currently, about 50% of the world's molybdenum resources come from copper-molybdenum ores. The main characteristics of copper-molybdenum sulfide ores are large reserves, low copper-molybdenum grades, fine embedded particle size, complex components, and difficulty in separation. As the depth of underground mining increases, the mineral composition changes, the molybdenum grade decreases, and it contains easily floating carbonaceous materials, which has a great impact on the separation of copper and molybdenum. The molybdenum index is significantly reduced, and the molybdenum concentrate grade is difficult to reach more than 35%.

[0003] In order to achieve effective separation of molybdenum and copper in copper-molybdenum mixed concentrate, in the prior art, the residual reagents and other impurities on the surface of the mixed concentrate are generally destroyed or removed first. The commonly used method is to re-grind and wash the copper-molybdenum mixed concentrate. This method has two disadvantages: First, although the re-grinding and washing method can effectively reduce the residual reagents on the surface of the copper-molybdenum mixed concentrate, it will inevitably produce a fine grinding effect on the mixed concentrate, increase the content of fine particles in the mixed concentrate, and cause over-grinding, which brings difficulties to the subsequent molybdenum-copper separation flotation and reduces the molybdenum recovery rate; second, the process is complicated, the steel consumption (grinding steel ball consumption) is high, and the energy consumption is high, which is not conducive to cost reduction and efficiency improvement of enterprises.

[0004] Therefore, in the existing technology, when separating copper-molybdenum mixed concentrate, there are problems such as low molybdenum recovery rate and high copper-molybdenum separation cost, which has always been a bottleneck that is difficult to break through in the copper-molybdenum mixed concentrate separation technology. Summary of the invention

[0005] The object of the present invention is to provide a method for separating and flotating carbonaceous copper-molybdenum ores, which can reduce the enrichment of carbonaceous materials in molybdenum concentrate, improve the grade of molybdenum concentrate, and realize efficient and comprehensive recovery of molybdenum resources.

[0006] The embodiments of the present invention are implemented by the following technical solutions:

[0007] A method for separating and flotating carbonaceous copper-molybdenum ore, comprising the following steps:

[0008] (1) grinding the carbonaceous copper-molybdenum ore to a certain fineness to obtain a pulp that meets the flotation concentration requirements;

[0009] (2) copper-molybdenum collectors and frothers are added to the ore pulp in sequence, and then roughing, scavenging, concentrating, dehydrating, removing drugs, and concentrating are performed, and then copper inhibitors and carbonaceous inhibitors are added. Then, copper-molybdenum separation roughing, scavenging, concentrating, and intermediate ore are sequentially returned to obtain copper concentrate and molybdenum concentrate through the copper-molybdenum separation process to obtain copper concentrate and molybdenum concentrate.

[0010] More specifically, the carbonaceous copper-molybdenum ore separation flotation method comprises the following steps:

[0011] (1) grinding the carbonaceous copper-molybdenum ore, with a grinding fineness of -0.075 mm accounting for 60%-65%, and adjusting the pulp concentration to 25%-35% after grinding;

[0012] (2) Adding lime, copper-molybdenum collector and frother to the slurry for copper-molybdenum mixed roughing to separate a1 and b; wherein: lime 500-1000g / t, copper-molybdenum collector 20-50g / t, frother 20-40g / t;

[0013] (3) b obtained in step (2) enters scavenging I, and 10-20 g / t of copper-molybdenum collector and 5-10 g / t of foaming agent are added to separate a2 and c;

[0014] (4) The c obtained in step (3) is sent to scavenging II, and 5-10 g / t of copper-molybdenum collector and 0-5 g / t of frother are added to separate a3 and tailings. In addition, a3 can be returned to step (3) for further processing, and the tailings are discarded;

[0015] (5) a1 obtained in step (1) is subjected to copper-molybdenum mixed selection, and 0-10 g / t of copper-molybdenum collector is added to select a4 and d, and a2 and d are returned to step (2) for further processing;

[0016] (6) dehydrating and removing the drug from a4 obtained in step (5), adding 150-250 g / t of sodium sulfide, stirring for 5-10 minutes and concentrating to obtain a concentrated solution;

[0017] (7) The concentrated solution obtained in step (6) is adjusted to a concentration of 20%-30%, and copper inhibitor and carbonaceous inhibitor are added to perform copper-molybdenum separation and roughing. After two scavenging processes, the molybdenum rough concentrate obtained by the separation and roughing is re-ground to a fineness of -0.038 mm, accounting for 93%-96%. After re-grinding, four molybdenum concentrations are performed, and the closed-loop process of sequentially returning the intermediate ore obtains copper concentrate and molybdenum concentrate, wherein the copper concentrate has a copper grade of 25.40% and a molybdenum content of 0.025%; the molybdenum concentrate has a molybdenum grade of 43.25% and a copper content of 0.77%.

[0018] Further, the copper-molybdenum collector is an emulsified product of an ester agent and a hydrocarbon oil mixed in a molar ratio of 2-5:5-8. Specifically, the ester agent can be propylene xanthate and propionitrile, and the hydrocarbon oil is an aromatic hydrocarbon with a C of 5-10; the foaming agent is an alcohol foaming agent, such as methyl isobutyl carbinol and sulfide ether alcohol, and the molar ratio of the two is 3-5:5-7. The copper-molybdenum collector of the present invention utilizes ester agents and hydrocarbon oils to efficiently capture copper-molybdenum sulfide minerals. The hydrocarbon oil can increase the diffusion area on the surface of molybdenite, and the electrostatic charge on the membrane is less, thereby enhancing the contact between molybdenum and bubbles, so that the copper-molybdenum capture effect is better and the recovery rate of molybdenum is improved.

[0019] Furthermore, the copper inhibitor is a mixture of sodium sulfide and D117, and the mass ratio of the two is 3-6:4-7; the copper inhibitor of the present invention utilizes sodium sulfide and D117 to cooperate with each other, and utilizes the interaction between xanthate ions and the surface of copper minerals to form CuX, so that the surface of the copper mineral is hydrophobic, and the addition of D117 can reduce the solubility of CuX, thereby strengthening the inhibitory effect of copper, while reducing the amount of sodium sulfide used and reducing the cost of the agent.

[0020] Furthermore, the carbonaceous material inhibitor is a sodium ion or iron ion complex, and / or a small molecule polysaccharide. If the carbonaceous material inhibitor is a mixture of the two, the mass ratio of the two is 5-8:2-5; wherein the small molecule polysaccharide is a broken chain polymer sugar formed by 4-7 glycosidic bonds, and specifically, oligosaccharides can be obtained by extracting starch substances; the sodium ion or iron ion complex can be sodium humate, sodium hexametaphosphate, sodium lignin sulfonate, and iron pyrophosphate.

[0021] The present invention uses sodium ion or iron ion complex as a carbonaceous material inhibitor, which can form a hydrophilic molecular film layer on the surface of the carbonaceous material, weaken the floating effect of the carbonaceous material, and effectively facilitate the floating of molybdenum minerals and the improvement of molybdenum grade. If it is coordinated with small molecular polysaccharides, its inhibitory effect on carbonaceous materials can be further enhanced.

[0022] Furthermore, in step (7), during the rough separation of copper and molybdenum, the amount of copper inhibitor added is 50-150 g / t, and the amount of carbonaceous inhibitor added is 50-100 g / t.

[0023] Further, in step (7), during the fourth molybdenum concentration, the amount of each substance added is:

[0024] During the first concentration: copper inhibitor 20-50g / t, carbonaceous inhibitor 10-20g / t;

[0025] During the second concentration: copper inhibitor 20-50g / t, carbonaceous inhibitor 10-20g / t;

[0026] During the third concentration: copper inhibitor 10-30g / t, carbonaceous inhibitor 20-50g / t;

[0027] During the fourth concentration: copper inhibitor 10-20g / t, carbonaceous inhibitor 10-20g / t.

[0028] Furthermore, in step (7), during the two sweeps, the amount of each substance added is:

[0029] During the first sweep: copper inhibitor 20-50g / t, carbonaceous inhibitor 0-20g / t.

[0030] During the second sweep: copper inhibitor 0-10g / t, carbonaceous inhibitor 0-10g / t.

[0031] The technical solution of the embodiment of the present invention has at least the following advantages and beneficial effects:

[0032] 1. The present invention adopts copper-molybdenum mixed flotation and uses efficient copper-molybdenum collectors to improve the enrichment ratio of low-grade molybdenum and the recovery rate of molybdenum; and the copper inhibitor and carbonaceous substance inhibitor used for copper-molybdenum separation form a hydrophilic molecular film layer on the surface of the carbonaceous substance, weakening the floating effect of the carbonaceous substance, thereby greatly reducing the enrichment of the carbonaceous substance in the molybdenum concentrate, effectively facilitating the floating of molybdenum minerals and the improvement of molybdenum grade, improving the grade of molybdenum concentrate, and better realizing the efficient and comprehensive recovery of molybdenum resources.

[0033] 2. The flotation method of the present invention has a simple process flow and is easy to operate, and has strong process stability. The regrinding of the coarse concentrate is beneficial to energy saving and consumption reduction, and also utilizes the mineral surface to scrub and dissociate, improves the copper-molybdenum separation effect, and reduces the interference of easily floating carbonaceous materials on the molybdenum concentrate grade. The molybdenum concentrate grade can be increased to more than 40%. DETAILED DESCRIPTION

[0034] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0035] Example 1

[0036] (1) Take the raw ore sample (containing Cu 0.95%, Mo 0.10%, C 1.90%), the first-stage grinding fineness is -0.075mm accounting for 55%, and the pulp concentration after grinding is adjusted to 30%;

[0037] (2) adding lime, copper-molybdenum collector and frother to the pulp for copper-molybdenum mixed roughing, wherein the lime is 1000 g / t, the copper-molybdenum collector is 30 g / t, and the frother is 30 g / t, and a1 and b are separated; specifically, the copper-molybdenum collector is propylene xanthate and aromatic hydrocarbons in a molar ratio of 3:7; the frother is methyl isobutyl carbinol and sulfide ether alcohol in a molar ratio of 4:6;

[0038] (3) The b obtained in step (2) is sent to scavenging I, 20 g / t of copper-molybdenum collector and 10 g / t of foaming agent are added, and a2 and c are separated;

[0039] (4) The c obtained in step (3) enters scavenging II, 10 g / t of copper-molybdenum collector and 5 g / t of frother are added, a3 and tailings are separated, a3 is returned to step (3), and the tailings are discarded;

[0040] (5) a1 in step (1) is subjected to copper-molybdenum mixed selection, 10 g / t of copper-molybdenum collector is added, a4 and d are selected, and a2 and d are returned to step (2);

[0041] (6) a4 of step (5) was dehydrated and drug-free, 170 g / t of sodium sulfide was added, stirred for 5 minutes, and concentrated after stirring;

[0042] (7) The concentrated solution obtained in step (6) is adjusted to a concentration of 20%, and a copper inhibitor and a carbonaceous material inhibitor are added to perform a rough separation of copper and molybdenum. After two scavengings, the rough molybdenum concentrate obtained by the rough separation is re-ground to a fineness of -0.038 mm, accounting for 94%. After re-grinding, four molybdenum concentrations are performed. The closed-loop process of sequentially returning the intermediate ore obtains copper concentrate and molybdenum concentrate. The copper concentrate has a copper grade of 25.40% and contains 0.025% molybdenum. The molybdenum concentrate has a molybdenum grade of 43.25% and contains 0.77% copper. The copper inhibitor is a mixture of sodium sulfide and D117 in a mass ratio of 3:7; the carbonaceous material inhibitor is ferric pyrophosphate.

[0043] Specifically, when performing rough separation of copper and molybdenum, the addition amount of each substance is: 100g / t of copper inhibitor and 70g / t of carbonaceous inhibitor;

[0044] During the four molybdenum concentrations, the addition amounts of each substance are as follows:

[0045] During the first concentration: copper depressant 50g / t, carbonaceous depressant 20g / t;

[0046] During the second concentration: inhibitor 30g / t, carbonaceous inhibitor 20g / t;

[0047] During the third concentration: copper depressant 30g / t, carbonaceous depressant 22g / t;

[0048] During the fourth concentration: copper inhibitor 10g / t, carbonaceous inhibitor 10g / t.

[0049] When performing two sweeps, the addition amount of each substance is: during the first sweep: 20 g / t of copper inhibitor and 0 g / t of carbonaceous inhibitor; during the second sweep: 0 g / t of copper inhibitor and 0 g / t of carbonaceous inhibitor.

[0050] Example 2

[0051] (1) Take a raw ore sample (containing Cu 1.05%, Mo 0.12%, C 2.04%), grind the raw ore, and the grinding fineness is -0.075mm, accounting for 65%. After grinding, adjust the pulp concentration to 25%.

[0052] (2) Adding lime, copper-molybdenum collector and frother to the pulp for copper-molybdenum mixed roughing, lime 800g / t, copper-molybdenum collector 40g / t, frother 40g / t, to separate a1 and b; specifically, the copper-molybdenum collector is propylene xanthate and aromatic hydrocarbons in a molar ratio of 4:6; the frother is methyl isobutyl carbinol and sulfide ether alcohol in a molar ratio of 3:7;

[0053] (3) b in step (2) enters scavenging I, adds 10 g / t of copper-molybdenum collector and 10 g / t of frother, and selects a2 and c;

[0054] (4) c in step (3) enters scavenging II, adds 5 g / t of copper-molybdenum collector and 5 g / t of frother, separates a3 and tailings, a3 returns to step (3), and the tailings are discarded;

[0055] (5) a1 in step (1) enters copper-molybdenum mixed selection, adds 5 g / t of copper-molybdenum collector, selects a4 and d, and a2 and d return to step (2);

[0056] (6) a4 of step (5) was dehydrated and drug-free, 200 g / t of sodium sulfide was added, stirred for 8 minutes, and concentrated after stirring;

[0057] (7) In step (6), the concentration of the concentrated underflow is adjusted to 22%, and a copper inhibitor and a carbonaceous material inhibitor are added to perform copper-molybdenum separation and roughing. After two scavengings, the separated roughed molybdenum concentrate is re-ground to a fineness of -0.038 mm accounting for 96%, and then four molybdenum concentrations are performed after re-grinding. The closed-loop process of sequentially returning the intermediate ore obtains copper concentrate and molybdenum concentrate. The copper concentrate has a copper grade of 25.58% and contains 0.030% molybdenum. The molybdenum concentrate has a molybdenum grade of 41.35% and contains 0.92% copper. The copper inhibitor is a mixture of sodium sulfide and D117 in a mass ratio of 4:6; the carbonaceous material inhibitor is sodium hexametaphosphate;

[0058] Specifically, when performing rough separation of copper and molybdenum, the addition amount of each substance is: 150g / t of copper inhibitor and 70g / t of carbonaceous inhibitor;

[0059] During the four molybdenum concentrations, the addition amounts of each substance are as follows:

[0060] During the first concentration: copper depressant 25g / t, carbonaceous depressant 15g / t;

[0061] During the second concentration: copper depressant 20g / t, carbonaceous depressant 12g / t;

[0062] During the third concentration: copper depressant 10g / t, carbonaceous depressant 38g / t;

[0063] During the fourth concentration: copper depressant 18g / t, carbonaceous depressant 16g / t;

[0064] When performing two sweeps, the addition amount of each substance is: 30g / t of copper inhibitor and 10g / t of carbonaceous inhibitor; 5g / t of di-copper inhibitor and 3g / t of carbonaceous inhibitor.

[0065] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for separating and flotating carbonaceous copper-molybdenum ore, characterized in that: The following steps are involved: S1. Grinding the carbonaceous copper-molybdenum ore to a certain fineness to obtain a slurry that meets the flotation concentration requirements; S2. Add copper-molybdenum collector and frother to the ore pulp in sequence, and then carry out roughing, scavenging, concentrating, dehydrating and removing drugs, and adding copper inhibitor and carbonaceous inhibitor after concentration, and then obtain copper concentrate and molybdenum concentrate through the copper-molybdenum separation process of roughing, scavenging, concentrating and returning the intermediate ore in sequence to obtain copper concentrate and molybdenum concentrate.

2. The method for separating and flotating carbonaceous copper-molybdenum ore according to claim 1, characterized in that: S1 includes: The carbonaceous copper-molybdenum ore is ground to a grinding fineness of -0.075mm accounting for 60%-65%. After grinding, the pulp concentration is adjusted to 25%-35%.

3. The method for separating and flotating carbonaceous copper-molybdenum ore according to claim 1, characterized in that: S2 includes the following steps: S21. Add lime, copper-molybdenum collector and frother to the slurry for mixed roughing of copper-molybdenum to separate a1 and b; S22. The b obtained in S21 is sent to scavenging selection Ⅰ, and copper-molybdenum collector and frother are added to select a2 and c; S23. The c obtained in S22 enters the scavenging II, and copper-molybdenum collector and frother are added to separate a3 and tailings; S24. The a1 obtained in S21 is subjected to copper-molybdenum mixed selection, and a copper-molybdenum collector is added to select a4 and d; S25. The a4 obtained in S24 was dehydrated and demedicated, and sodium sulfide was added, stirred for a period of time and concentrated to obtain a concentrate; S26. The concentration of the concentrated liquid obtained in S25 is adjusted to 20%-30%, and copper inhibitors and carbonaceous inhibitors are added to perform rough separation of copper and molybdenum. After two sweeping selections, the rough molybdenum concentrate obtained by the separation and rough selection is ground again, and after grinding, multiple molybdenum concentrations are performed to obtain copper concentrate and molybdenum concentrate.

4. The method for separating and flotating carbonaceous copper-molybdenum ore according to claim 3, characterized in that: In S21, the addition amount of each substance is as follows: lime 500-1000g / t, copper-molybdenum collector 20-50g / t, foaming agent 20-40g / t.

5. The method for separating and flotating carbonaceous copper-molybdenum ore according to claim 3, characterized in that: In S23, the obtained a3 is returned to step S22 for further processing.

6. The method for separating and flotating carbonaceous copper-molybdenum ore according to claim 3, characterized in that: In S24, the obtained a2 and d are returned to step S21 for further processing.

7. The method for separating and flotating carbonaceous copper-molybdenum ore according to claim 1 or 3, characterized in that: The copper-molybdenum collector is an emulsified product of an ester agent and a hydrocarbon oil in a molar ratio of 2-5:5-8.

8. The method for separating and flotating carbonaceous copper-molybdenum ore according to claim 7, characterized in that: The ester agent is propylene xanthate and / or propionitrile, and the hydrocarbon oil is an aromatic hydrocarbon with a C content of 5-10.

9. The method for separating and flotating carbonaceous copper-molybdenum ore according to claim 1 or 3, characterized in that: The foaming agent is an alcohol foaming agent.

10. The method for separating and flotating carbonaceous copper-molybdenum ore according to claim 1 or 3, characterized in that: The copper inhibitor is a mixture of sodium sulfide and D117 in a ratio of 3 to 6:4 to 7; the carbonaceous material inhibitor is any one or more of sodium humate, sodium hexametaphosphate, sodium lignin sulfonate, and ferric pyrophosphate.

Citation Information

Patent Citations

  • Carbonaceous mineral inhibitor and method for flotation of multi-metal sulfide ores

    CN103861741A

  • Method for copper-molybdenum bulk concentrate floatation

    CN103934116A

  • Beneficiation method for low-grade mixed copper ore containing molybdenum

    CN105435953A

  • Low-grade associated molybdenum-copper-sulfur ore flotation composite collecting agent and flotation method

    CN113996445A

  • Copper-molybdenum ore flotation separation method

    CN116651619A

Cited By

  • Flotation method for porphyry type copper-molybdenum ore

    CN122273688A

  • A method of flotation of a porphyry copper-molybdenum ore

    CN122273688B

  • Method for flotation separation of copper and molybdenum in copper-molybdenum mixed concentrate

    NL4000110A

  • Beneficiation method for improving grade of molybdenum by means of staged intensified carbon depression

    WO2026207929A1