Method for improving yield of titanium-rich material for boiling chlorination, and use thereof
Through the pre-acid leaching and pressurized acid leaching process of titanium slag and acid solution, the oxidant is used to remove impurities in the titanium slag, which solves the high energy consumption and complex process problems in the preparation of titanium-rich materials in the boiling chlorination method, and achieves high efficiency and low cost. The titanium yield is increased and is suitable for titanium slag with low titanium slag grade and high impurity content.
Patent Information
- Application Number
- PCT/CN2023/110304
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2023-07-31
- Publication Date
- 2024-10-03
AI Technical Summary
The existing technology in the preparation of titanium-rich materials in the boiling chlorination method has problems such as high energy consumption, complex process flow, high equipment requirements, and incomplete removal of impurities. It is especially suitable for titanium slag with low grade and high impurity content that is difficult to achieve efficient upgrading. .
By pre-acid leaching the titanium slag with an acid solution, and then adding an oxidant for pressurized acid leaching, the oxidant is used to dissolve impurity elements such as calcium and magnesium to achieve the preparation of titanium-rich materials. The process is simplified, energy consumption is reduced, and the scope of application is wide.
It achieves efficient removal of impurities in titanium slag, increases titanium yield, simplifies the process, and reduces costs. It is suitable for titanium slag with low grade and high impurity content, has a wider scope of application, and has low equipment requirements.
Smart Images

Figure CN2023110304_03102024_PF_FP_ABST
Abstract
Description
A method for improving the yield of titanium-rich material for boiling chlorination and its application
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This disclosure claims priority to Chinese patent application number CN202310317209X, filed with the Patent Office of China on March 28, 2023, entitled “A method for improving the yield of titanium-rich material for boiling chlorination and its application,” the entire contents of which are incorporated by reference into this disclosure. Technical Field
[0003] The present disclosure relates to the field of metallurgy technology, and in particular to a method for improving the yield of titanium-rich material for boiling chlorination and an application thereof. Background Art
[0004] The titanium industry chain consists of two distinct branches: the titanium materials industry and the titanium dioxide industry. The titanium materials industry, starting with the mining and processing of ilmenite and rutile, produces titanium sponge, which is then made into titanium alloys. Titanium is widely used in aerospace, chemical engineering, shipbuilding, and other fields. Known as a "modern metal" and a "strategic metal," titanium is an essential raw material for modern industry and cutting-edge technology. The titanium dioxide industry, starting with the mining and processing of ilmenite and rutile, produces the chemical intermediate titanium dioxide through physical and chemical methods. It is widely used in essential industries such as coatings, plastics, papermaking, inks, and chemical fibers.
[0005] Within the titanium industry chain, titanium tetrachloride is an intermediate product in the production of titanium sponge and chloride-process titanium dioxide. Industrial methods for producing titanium tetrachloride by the chloride process include the shaft furnace chlorination process, the molten salt chlorination process, and the boiling chlorination process. The boiling chlorination process uses a mixture of titanium-rich material and petroleum coke in a fluidized furnace with chlorine gas to produce titanium tetrachloride. The boiling chlorination process has rapidly developed and has become the preferred chlorination technology for chloride-process titanium dioxide production. Advantages of the boiling chlorination process include the lack of agglomeration, simple operation, high production capacity, continuous production, and the absence of significant waste, waste, and other issues. However, the boiling chlorination method has very stringent requirements on raw materials. The calcium chloride and magnesium chloride produced are in a molten state and easily adhere to the material and the bed. When they accumulate to a certain level, they will destroy the normal fluidized state, thereby making the chlorination process impossible. Therefore, the boiling chlorination method has extremely stringent requirements on the raw material titanium-rich material, requiring a titanium grade greater than 85wt.% and a low impurity content (CaO≤0.15wt.%, CaO+MgO≤1.5wt.%). There is an urgent need to break through the preparation technology of titanium-rich materials for boiling chlorination.
[0006] my country's Panxi region boasts abundant titanium ore resources, but these are high in gangue and poor in selectivity, requiring deep grinding and selection. The resulting concentrate is low-grade, high in impurities, particularly calcium and magnesium, and fine in particle size. While direct acid leaching or pretreatment plus acid leaching of titanium concentrate can yield titanium-rich materials with the composition required for boiling chlorination, the particle size falls far short of the required level. Using titanium slag as a raw material to prepare titanium-rich materials for chlorination can address this fine particle size issue.
[0007] A great deal of research has been conducted on upgrading titanium slag to high-quality chlorinated titanium-rich materials. For example, patent CN108358238A discloses a "method for producing a modifier for rutile using titanium-containing blast furnace slag and a method for producing artificial rutile using titanium-containing blast furnace slag." However, this method still requires heating to maintain the furnace temperature during the oxygenation process, resulting in high energy consumption and unsuitable for industrial production.
[0008] Patent CN107758729B discloses a "process for modifying high-calcium-magnesium titanium slag." This involves adding a certain amount of fluoride to a boiling chlorination system to prevent the formation of calcium chloride and magnesium chloride, ensuring a smooth chlorination reaction. However, this method is operationally hazardous, as the amount of fluoride added is difficult to control. Furthermore, the content of calcium fluoride and magnesium fluoride in solid slag, furnace slag, and dust collection slag increases, increasing the burden on solid waste disposal.
[0009] Patent CN109399706A discloses "a method for upgrading UGS slag with high calcium magnesium titanium slag", but this method requires boiling and refluxing in a 12-30wt% concentration NaOH solution for 3-6 hours, which is time-consuming and has high requirements for equipment. At the same time, high-temperature reduction and sodium roasting are also required in the later stage, and industrial implementation has high requirements for equipment.
[0010] Patent CN107399758A discloses "a method for preparing artificial rutile from high-titanium slag". This method uses microwaves as a heat source and is difficult to implement industrially. In addition, this method requires the titanium slag grade to be above 85wt.% and the SiO2 content to be below 4wt.%. It has high requirements for raw materials and is not suitable for high-calcium-magnesium titanium slag.
[0011] Patent CN111733331B discloses a method for preparing upgraded titanium slag from hot slag discharged from a furnace. However, this method still requires an oxidation-reduction process after the titanium slag is cooled.
[0012] Patent CN113957271A discloses “a method for reducing calcium oxide content in titanium slag and titanium dioxide”, but the method does not involve the removal of MgO.
[0013] Patent CN113862494A discloses a "method for preparing titanium-rich material and titanium tetrachloride". However, the disadvantage of this method is that the process is relatively long. The water-quenched slag needs to be acid-leached to remove calcium, redox acid-leached to remove magnesium, and then calcined to obtain the titanium-rich material product.
[0014] In view of the above research deficiencies, it is very necessary to develop a low-cost, short-process method for producing boiling chlorination raw materials using high calcium magnesium titanium slag.
[0015] Summary of the Invention
[0016] The present disclosure provides a method for improving the yield of titanium-rich material for boiling chlorination, comprising the following steps:
[0017] The titanium slag is mixed with an acid solution for pre-acid leaching to dissolve metallic iron in the titanium slag, and a pre-acid leaching mixture is obtained after the pre-acid leaching is completed;
[0018] adding an oxidant to the mixture after pre-acid leaching and performing pressurized acid leaching to dissolve impurity elements in the mixture after pre-acid leaching, and then performing solid-liquid separation to obtain the titanium-rich material for boiling chlorination; wherein the impurity elements include at least one of calcium, magnesium, aluminum and manganese;
[0019] Wherein, the oxidant comprises at least one of a gaseous oxidant, an active metal compound oxidant and a non-metal compound oxidant;
[0020] The mass fraction of CaO in the titanium-rich material for boiling chlorination is ≤0.1%, and the sum of the mass fractions of CaO and MgO is ≤1.5%.
[0021] Optionally, the gaseous oxidant comprises a gaseous elemental oxidant.
[0022] Optionally, the gaseous oxidant includes at least one of Cl2, Br2, O2 and O3.
[0023] Optionally, the active metal compound oxidant includes at least one of NaClO, NaClO3, KClO and KClO3.
[0024] Optionally, the non-metal compound oxidant includes at least one of H2O2 and HClO.
[0025] Optionally, the oxidant is added in an amount such that the sum of the mass concentrations of trivalent titanium ions and tetravalent titanium ions in the mixed material is ≤5 g / L.
[0026] Optionally, the mass fraction of TiO2 in the titanium slag is ≥70.0%.
[0027] Optionally, the mass fraction of CaO in the titanium slag is ≥0.3%, and the mass fraction of MgO is ≥3.0%.
[0028] Optionally, the titanium slag includes water-quenched titanium slag obtained by smelting and water quenching titanium concentrate.
[0029] Optionally, the temperature of the pre-acid leaching is 20°C to 105°C.
[0030] Optionally, the pre-acid leaching time is 5 minutes to 300 minutes.
[0031] Optionally, the mass of the titanium slag is 15% to 80% of the total mass of the titanium slag and the acid solution.
[0032] Optionally, the temperature of the pressurized acid leaching is 130°C to 175°C.
[0033] Optionally, the pressurized acid leaching time is ≥0.2h, more preferably 0.5h to 5h.
[0034] Optionally, the pressure of the pressurized acid leaching is 0.3 MPa to 0.9 MPa.
[0035] The present disclosure also provides a titanium-rich material for boiling chlorination, which is prepared by any of the above methods for improving the yield of the titanium-rich material for boiling chlorination.
[0036] Optionally, the mass fraction of TiO2 in the titanium-rich material for boiling chlorination is ≥85%, and the TiO2 yield is ≥90%.
[0037] The present disclosure also provides a method for preparing a titanium-rich material for producing titanium tetrachloride by a boiling chlorination process, comprising the method for improving the yield of the titanium-rich material for boiling chlorination as described above;
[0038] Wherein, in the titanium-rich material used for producing titanium tetrachloride by boiling chlorination method, the mass fraction of CaO is ≤0.1%, and the sum of the mass fractions of CaO and MgO is ≤1.5%.
[0039] The present disclosure further provides a method for preparing titanium tetrachloride, including the method for preparing the titanium-rich material used for producing titanium tetrachloride by the boiling chlorination process as described above.
[0040] The present disclosure also provides a titanium-containing material, which is mainly prepared from titanium tetrachloride prepared by the above-mentioned method for preparing titanium tetrachloride;
[0041] Wherein, the titanium-containing material includes at least one of sponge titanium, titanium alloy, chloride titanium dioxide and pearlescent pigment. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] In order to more clearly illustrate the specific embodiments of the present disclosure or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the specific embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present disclosure. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0043] FIG1 is a SEM image of high calcium and magnesium water-quenched titanium slag provided in Example 4 of the present disclosure;
[0044] FIG2 is a SEM image of a titanium-rich material for boiling chlorination provided in Example 4 of the present disclosure;
[0045] FIG3 is a partially enlarged SEM image of FIG2 . DETAILED DESCRIPTION
[0046] The technical solutions of the present disclosure will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but those skilled in the art will understand that the embodiments described below are part of the embodiments of the present disclosure, rather than all of the embodiments, and are only used to illustrate the present disclosure, and should not be considered as limiting the scope of the present disclosure. Based on the embodiments in the present disclosure, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present disclosure. If specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0047] The present disclosure provides a method for improving the yield of titanium-rich material for boiling chlorination, comprising the following steps:
[0048] The titanium slag is mixed with an acid solution for pre-acid leaching to dissolve the metallic iron in the titanium slag, and a pre-acid leached mixture is obtained after the pre-acid leaching is completed.
[0049] The present invention dissolves metallic iron (i.e., elemental iron) through pre-acid leaching, wherein hydrogen generated during the dissolution of metallic iron in acid will escape, thereby preventing the hydrogen released by the reaction of elemental iron with acid from affecting the efficiency of subsequent pressurized acid leaching.
[0050] An oxidizing agent is then added to the pre-acid leaching mixture, and pressure acid leaching is performed to dissolve impurity elements in the pre-acid leaching mixture. After the pressure acid leaching is completed, solid-liquid separation is performed to obtain the titanium-rich material for boiling chlorination. The impurity elements include at least one of calcium, magnesium, aluminum, and manganese, but are not limited thereto.
[0051] Among them, the titanium-rich material for boiling chlorination refers to the titanium-rich raw material that can be used for boiling chlorination method.
[0052] In some embodiments of the present disclosure, after the solid-liquid separation, the steps of water washing and drying are also included.
[0053] The mass fraction of CaO in the titanium-rich material for boiling chlorination is ≤0.1%, for example, the mass fraction of CaO is ≤0.08%, ≤0.05% or ≤0.03%, etc., including but not limited to any one of 0.09%, 0.08%, 0.07%, 0.06%, 0.05%, 0.04%, 0.03%, 0.01% or the range between any two of them.
[0054] The sum of the mass fractions of CaO and MgO in the titanium-rich material for boiling chlorination is ≤1.5%, for example, the sum of the mass fractions of CaO and MgO is ≤1.2%, ≤1.0% or ≤0.8%, etc. The sum of the mass fractions of CaO and MgO is ≤0.8%, including but not limited to any one of 1.45%, 1.4%, 1.35%, 1.3%, 1.25%, 1.2%, 1.1%, 1.0%, 0.9%, 0.8%, 0.7%, 0.6%, 0.5% or the range value between any two of them.
[0055] The present disclosure performs pressurized acid leaching on the mixture after pre-acid leaching, which has a good leaching effect on impurity elements, especially magnesium, and can significantly reduce the magnesium oxide content in the titanium-rich material.
[0056] The oxidant includes at least one of a gaseous oxidant, an active metal compound oxidant and a non-metal compound oxidant.
[0057] In some embodiments of the present disclosure, the gaseous oxidant includes a gaseous elemental oxidant, that is, the gaseous oxidant is an elemental substance rather than a compound.
[0058] The main components of titanium ore include TiO2 and FeO, with the remainder consisting of SiO2, CaO, MgO, Al2O3, and V2O5. During the high-temperature smelting process, the titanium ore is heated and melted, and the iron oxides in the titanium ore are reduced to metallic iron and precipitated. Titanium dioxide, along with impurities such as calcium oxide, magnesium oxide, aluminum oxide, and silicon dioxide, enters the slag phase and is eventually separated from the iron. After high-temperature smelting, most of the iron is removed, and titanium is enriched. The main phases of the molten titanium slag obtained after smelting are: tarnite, takisite, and siliceous glass. Calcium is mainly present in the siliceous glass, and magnesium is present in the tarnite.
[0059] After smelting, titanium slag will produce 10% to 30% (mass fraction) of low-valent titanium (Ti2O3), which will form trivalent titanium ions during the pressurized acid leaching process.
[0060] The present invention adds a specific type of oxidant to the pressurized acid leaching system, so that low-valent titanium ions (trivalent titanium ions) are oxidized into tetravalent titanium ions and undergo in-situ hydrolysis, which not only increases the titanium yield but also reduces the fine powder rate (if the fine powder rate is too high, the utilization rate of the product will be low when used). Among them, the ferrous ions dissolved in the pre-acid leaching process will be oxidized into trivalent ferrous ions after the addition of the oxidant, and then enter the internal pores of the titanium slag with the leachate, and fully contact the surface and interior of the titanium slag. When low-valent titanium is dissolved, the oxidant will oxidize it into tetravalent titanium at the first time. At the same time as the low-valent titanium is dissolved, impurity ions such as calcium and magnesium are also dissolved. The dissolution process consumes H + , which reduces the surrounding instantaneous acidity, thereby promoting the in-situ hydrolysis of tetravalent titanium ions on the particles in the titanium slag (surface and internal pores), generating metatitanic acid. The metatitanic acid in-situ hydrolyzed inside the titanium slag particles will no longer flow out with the acid due to the increase in particle size and intermolecular forces. Therefore, most of the fine powder metatitanic acid generated by hydrolysis will remain inside the particles (see Figures 2 and 3), reducing the fine powder of the product while increasing the titanium yield. When tetravalent titanium is in-situ hydrolyzed, a certain amount of H + , the generated H + (Acid) is used for pressurized pickling reaction, which can reduce the amount of acid used in the pickling process.
[0061] The ferrous ions dissolved during the pre-acid leaching process of the present invention serve as an oxidation carrier (iron source). In the initial stage of adding the oxidant, the oxidant first oxidizes the ferrous ions to trivalent ferrous ions, and then returns to the ferrous state with the oxidation of trivalent titanium (i.e., the trivalent ferrous ions and trivalent titanium ions react to generate divalent ferrous ions and tetravalent titanium ions), thus achieving a cycle. During the entire acid leaching process, the iron ions also act as salt ions to increase the activity of the reaction acid. This avoids the high cost caused by the additional addition of trivalent iron and the high iron impurity content in the obtained titanium-rich material.
[0062] To achieve resistance to strong acids and bases, pressurized equipment used in pressurized acid leaching reactions often contains zirconium or titanium components. However, these materials are easily dissolved by acid in a reducing atmosphere, causing corrosion of the zirconium or titanium components. The present disclosure, however, effectively addresses the corrosion problem of zirconium and / or titanium components by adding an oxidizing agent during the acid leaching process to maintain an oxidizing system.
[0063] In addition, the method provided by the present disclosure for improving the yield of titanium-rich material for boiling chlorination has the advantages of simple operation, short process flow and low cost. By using this method to treat high-calcium-magnesium-titanium slag, impurity elements such as calcium and magnesium can be removed quickly and efficiently, thereby obtaining titanium-rich raw materials that can be used for boiling chlorination method.
[0064] Compared with patent CN108358238A, the present application does not need to maintain the high-temperature molten titanium slag at high temperature for oxygen supplementation oxidation, and the process flow is simpler, the equipment requirements are low, the energy consumption is low, and it is easy to industrialize.
[0065] Compared with patent CN107758729B, the boiling chlorination raw material prepared in this application fully meets the requirements before entering the chlorination furnace, has a high safety factor for continuous production, and produces less solid waste during the chlorination process.
[0066] Compared with patent CN109399706A, this application omits the processes of alkali leaching, oxidation roasting, reduction sodium roasting, calcination, etc., and can realize the upgrading of high calcium magnesium titanium slag to UGS slag, which greatly saves the process. In addition, this application does not need to boil and reflux the material under high alkali concentration, has low equipment requirements, short process and low production cost.
[0067] Compared with patent CN107399758A, it is difficult to implement in industry because it requires microwaves as a heat source, while the present invention can use traditional industrial electric furnaces for smelting, and has low equipment requirements; at the same time, the patent requires that the titanium slag grade is above 85wt.% and the SiO2 content is below 4wt.%, which has high requirements for raw materials and is not suitable for Panzhihua titanium ore. The method provided by the present invention has lower requirements for raw materials and a wider range of applications.
[0068] Compared with patent CN111733331B, the present application omits the oxidation process, and can remove impurity elements such as calcium and magnesium in the titanium slag by one high-pressure acid leaching. In addition, the present application does not require oxygen injection treatment when the molten titanium slag is discharged from the furnace, thereby improving production safety.
[0069] Compared with patent CN113957271A, the present disclosure can effectively reduce the content of magnesium oxide, which is an effect that cannot be achieved by the patent.
[0070] Compared with patent CN113862494A, the method provided by the present disclosure is simpler and has shorter steps. Calcium and magnesium impurities can be removed by direct pressurized acid leaching reaction. In addition, the present disclosure effectively reduces the fine powder rate of the product and improves the titanium yield by adding a specific oxidant.
[0071] In order to further comprehensively consider the comprehensive performance of oxidizability, cost, safety performance and yield of titanium-rich material products, this application optimizes the type and dosage of the oxidant.
[0072] Optionally, the gaseous oxidant includes at least one of Cl2, Br2, O2 and O3.
[0073] It is understood that the gaseous oxidant is not limited to substances that are gaseous at room temperature and pressure, but also includes substances that can be converted to gaseous state by heating. For example, Br2 is liquid at room temperature and pressure. When using Br2 in the present disclosure, it is heated to convert it into gaseous bromine vapor.
[0074] Optionally, the active metal compound oxidant includes at least one of NaClO, NaClO3, KClO and KClO3.
[0075] Optionally, the non-metal compound oxidant includes at least one of H2O2 and HClO.
[0076] In some embodiments of the present disclosure, the oxidant may be an oxidant that is not easily decomposed by heat, such as a gaseous oxidant, to improve the leaching efficiency.
[0077] Optionally, the amount of the oxidant added is such that the sum of the mass concentrations of trivalent titanium ions and tetravalent titanium ions in the mixed material is ≤5 g / L, for example ≤4 g / L, ≤3 g / L or ≤3 g / L, etc., including but not limited to any one of 4 g / L, 3 g / L, 2 g / L, 1 g / L, 0.5 g / L, 0.1 g / L or a range value between any two of them.
[0078] In some embodiments of the present disclosure, the oxidant can be added before pressurization or during pressurization. Alternatively, the gaseous oxidant is added during pressurization.
[0079] Optionally, at least one of the active metal compound oxidant and the non-metal compound oxidant is added before pressurization and / or during pressurization.
[0080] Optionally, the mass fraction of TiO2 in the titanium slag is ≥70.0%, for example, ≥75.0%, ≥80.0%, ≥85.0% or ≥90.0%, etc.; including but not limited to any point value of 71%, 72%, 73%, 74%, 75%, 78%, 80%, 83%, 85%, 88%, 90% or the range value between any two of them.
[0081] Optionally, the mass fraction of CaO in the titanium slag is ≥0.3%, for example ≥0.6%, ≥1.0%, ≥2.0%, ≥4.0%, ≥6.0% or ≥8.0%, etc., including but not limited to any point value of 0.5%, 0.8%, 1.0%, 1.3%, 1.5%, 1.8%, 2.0%, 2.5%, 3%, 4%, 5%, 6%, 8%, 10% or any range value between two of them; the mass fraction of MgO is ≥3.0%, for example ≥5.0%, ≥7.0% or ≥9.0%, etc., including but not limited to any point value of 3.5%, 4%, 5%, 6%, 7%, 8%, 9%, 10% or any range value between two of them.
[0082] The method provided by the present invention for improving the yield of titanium-rich material for boiling chlorination has low requirements for raw materials and a wide range of applications. It is applicable even to high-calcium-magnesium-titanium slag obtained from smelting low-grade and high-impurity titanium concentrate, such as titanium slag obtained from smelting Panxi ore.
[0083] Optionally, the titanium slag includes but is not limited to water-quenched titanium slag obtained by smelting and water quenching titanium concentrate, and more optionally, water-quenched titanium slag obtained by smelting and water quenching titanium concentrate.
[0084] The molten titanium slag after smelting (melting) is cooled and crushed by water quenching. The high-temperature molten titanium slag is rapidly cooled by a large amount of high-pressure water quenching liquid. Due to the dual effects of the high-pressure water quenching liquid and the internal stress of the cooling, the high-temperature molten titanium slag will explode into small particles of water-quenched slag. At the same time, the rapid cooling will cause the phase of the water-quenched slag to change. The black titanium in the titanium slag is converted into rutile phase, which deteriorates the acid solubility of titanium and converts calcium into CaSi2O with good acid solubility. 10 At the same time, it contains more glass that has not had time to form a regular arrangement due to rapid cooling.
[0085] Optionally, the pre-acid leaching temperature is 20°C to 105°C, for example, 25°C to 95°C, 35°C to 85°C or 45°C to 75°C, including but not limited to any one of 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 103°C or a range between any two of them.
[0086] In some embodiments of the present disclosure, the acid solution used in the pre-acid leaching process can be any conventional acid, including, but not limited to, at least one of hydrochloric acid solution, nitric acid solution, acetic acid solution, sulfuric acid solution, and hydrofluoric acid solution. Optionally, the mass fraction of the acid solution is 10% to 30%, such as 14% to 26%, 17% to 27%, or 19% to 24%, including but not limited to any one of 12%, 15%, 18%, 20%, 23%, 25%, and 28%, or any range therebetween.
[0087] In some embodiments of the present disclosure, the acid leaching method of the pre-acid leaching may adopt any conventional acid leaching method, such as stirring leaching, column leaching or heap leaching, but is not limited thereto.
[0088] In some embodiments of the present disclosure, the pre-acid leaching time is 5 min to 300 min, for example, 20 min to 180 min, 40 min to 140 min or 80 min to 110 min, including but not limited to any one of 10 min, 15 min, 20 min, 30 min, 50 min, 60 min, 90 min, 120 min, 150 min, 180 min, 210 min, 240 min, 270 min or a range value between any two of them; it can be optionally 20 min to 120 min.
[0089] In some embodiments of the present disclosure, during the pre-acid leaching process, the mass of the titanium slag is 15% to 80% of the total mass of the titanium slag and the acid solution, for example, 25% to 75%, 35% to 65% or 45% to 55%, including but not limited to any point value of 20%, 30%, 40%, 50%, 60%, 70% or the range value between any two of them, that is, the mass of the titanium slag accounts for 15% to 80% of the total mass of the titanium slag and the acid solution.
[0090] In order to further comprehensively consider the comprehensive performance of pressure acid leaching efficiency, yield of titanium-rich material products and production cost, this application optimizes the parameters in the pressure acid leaching process including temperature, pressure, time, etc.
[0091] Optionally, the temperature of the pressurized acid leaching is 130°C to 175°C, for example, 134°C to 172°C, 146°C to 165°C or 156°C to 160°C; including but not limited to any one of 135°C, 140°C, 145°C, 150°C, 155°C, 160°C, 165°C, 170°C or a range between any two of them.
[0092] Optionally, the time of the pressurized acid leaching is ≥0.2h, such as ≥0.5h, ≥1h or ≥3h, including but not limited to any point value of 0.3h, 0.5h, 0.8h, 1h, 2h, 3h, 4h or a range value between any two of them; it can be optionally 0.5-5h.
[0093] Optionally, the pressure of the pressurized acid leaching is 0.3 MPa to 0.9 MPa, such as 0.35 to 0.85 MPa, 0.45 to 0.75 MPa or 0.55 to 0.65 MPa, including but not limited to any one of 0.4 MPa, 0.5 MPa, 0.6 MPa, 0.7 MPa, 0.8 MPa or a range between any two of them.
[0094] In some embodiments of the present disclosure, the acid leaching method of pressure acid leaching includes stirring leaching.
[0095] In some embodiments of the present disclosure, the pressurized acid leaching is performed in a pressurized apparatus, such as, but not limited to, a pressure vessel (autoclave). Optionally, the pressurized apparatus is provided with a gas hole and / or a feed inlet, wherein the gas hole is used to introduce gas, and the feed inlet is used to input a solid oxidant and / or a liquid oxidant.
[0096] The present disclosure also provides a method for preparing a titanium-rich material for producing titanium tetrachloride by a boiling chlorination process, including the method for improving the yield of the titanium-rich material for boiling chlorination as described above.
[0097] Among them, in the titanium-rich material used for producing titanium tetrachloride by boiling chlorination method, the mass fraction of CaO is ≤0.1%, and can be optionally ≤0.082%. For example, the mass fraction of CaO can be 0.09%, 0.08%, 0.07%, 0.06%, 0.05%, 0.04%, 0.03%, 0.02% or 0.01%, etc.; the sum of the mass fractions of CaO and MgO is ≤1.5%, and can be optionally ≤1.43%. For example, the sum of the mass fractions of CaO and MgO can be 1.4%, 1.3%, 1.2%, 1.1%, 1.0%, etc.
[0098] The preparation method of the titanium-rich material provided by the present disclosure can produce a titanium-rich material that meets the requirements, and can then be used as a raw material for producing titanium tetrachloride by the boiling chlorination method.
[0099] The present disclosure provides a method for preparing titanium tetrachloride, including the method for preparing the titanium-rich material used for producing titanium tetrachloride by the boiling chlorination process as described above.
[0100] The present disclosure provides a titanium-containing material, which is mainly prepared from titanium tetrachloride prepared by the above-mentioned method for preparing titanium tetrachloride;
[0101] Wherein, the titanium-containing material includes at least one of sponge titanium, titanium alloy, chloride titanium dioxide and pearlescent pigment.
[0102] The method provided by the present disclosure for improving the yield of titanium-rich material for boiling chlorination is to add a specific type of oxidant to a pressurized acid leaching system, so that low-valent titanium ions are oxidized into tetravalent titanium ions and undergo in-situ hydrolysis, thereby not only increasing the titanium yield but also reducing the fine powder rate.
[0103] The method provided in the present disclosure improves the yield of titanium-rich materials for boiling chlorination. By adding a specific type of oxidant, low-valent titanium ions are oxidized into tetravalent titanium ions and hydrolyzed. The hydrogen ions generated during the hydrolysis process increase the acidity of the system, thereby reducing the amount of acid used.
[0104] The method for improving the yield of titanium-rich material for boiling chlorination provided by the present disclosure can effectively avoid the corrosion problem of zirconium and / or titanium parts in the pressurized equipment by adding an oxidant during the acid leaching process to maintain the oxidation system.
[0105] The method for improving the yield of titanium-rich material for boiling chlorination provided by the present disclosure has high impurity removal efficiency, simple operation, short process flow, low cost and low equipment requirements.
[0106] The method provided by the present invention for improving the yield of titanium-rich material for boiling chlorination has low requirements for raw materials and a wide range of applications. It is applicable even to high-calcium-magnesium-titanium slag obtained from smelting low-grade and high-impurity titanium concentrate, such as titanium slag obtained from smelting Panxi ore.
[0107] The method for improving the yield of titanium-rich material for boiling chlorination provided by the present disclosure solves the shortcomings of the existing technology. The method can improve the titanium yield and has the advantages of simple operation, short process flow, low cost and low equipment requirements.
[0108] Example
[0109] The following examples describe the embodiments of the present disclosure in detail. However, those skilled in the art will appreciate that the following examples are merely illustrative of the present disclosure and should not be construed as limiting the scope of the present disclosure. Where specific conditions are not specified in the examples, the experiments were conducted under conventional conditions or those recommended by the manufacturer. Reagents or instruments used without manufacturer identification are commercially available conventional products. The titanium slag used in the following examples and comparative examples of the present disclosure is water-quenched titanium slag obtained by smelting and water-quenching titanium concentrate.
[0110] In the following examples and comparative examples of the present disclosure, the TiO2 content, CaO content and MgO content in the titanium slag and the titanium-rich material are all obtained by XRF detection.
[0111] Example 1
[0112] This embodiment provides a method for improving the yield of titanium-rich material for boiling chlorination, comprising the following steps:
[0113] (1) A 20-60 mesh material of high calcium and magnesium water-quenched titanium slag (TiO2 content 79.27wt.%, CaO content 1.98wt.%, MgO content 5.79wt.%) is mixed with an acid solution and pre-acid leaching is performed to dissolve metallic iron by reaction with the acid and then separate it from the titanium slag. The acid solution is a hydrochloric acid solution with a concentration of 18wt.%, the pre-acid leaching time is 20min, the pre-acid leaching temperature is 100°C, the mass of the titanium slag is 15% of the total mass of the titanium slag and the acid solution, and the acid leaching method is stirring leaching. After the pre-acid leaching is completed, a pre-acid leached mixture is obtained.
[0114] (2) The pre-acid leaching mixture obtained in step (1) was transferred to a pressure autoclave for pressure acid leaching, and Cl2 was introduced into the system to dissolve impurities such as calcium and magnesium. The acid leaching method adopted stirring acid leaching, the pressure acid leaching temperature was 145°C, the pressure acid leaching time was 3h, and the pressure of the pressure acid leaching was 0.5MPa. After the acid leaching was completed, the total titanium (referring to the sum of the mass concentrations of trivalent titanium ions and tetravalent titanium ions, the same applies to other embodiments) in the test solution was 5g / L, and the solid material (acid leaching residue) was filtered, and then washed with water and dried to obtain a titanium-rich material for boiling chlorination.
[0115] Example 2
[0116] The method for improving the yield of the titanium-rich material for boiling chlorination provided in this embodiment comprises the following steps:
[0117] (1) A high calcium and magnesium water-quenched titanium slag material of 20 to 60 mesh (TiO2 content 86.82 wt.%, CaO content 0.309 wt.%, MgO content 3.06 wt.%) is mixed with an acid solution and pre-acid leaching is performed to dissolve the metallic iron by reaction with the acid and then separate it from the titanium slag. The acid solution is a hydrochloric acid solution with a concentration of 20 wt.%, the pre-acid leaching time is 40 min, the pre-acid leaching temperature is 80°C, the mass of the titanium slag is 30% of the total mass of the titanium slag and the acid solution, the acid leaching method is column leaching, and after the pre-acid leaching is completed, a pre-acid leached mixture is obtained.
[0118] (2) The pre-acid leaching mixture obtained in step (1) is transferred to a pressure autoclave for pressure acid leaching, and O2 is introduced into the system to dissolve impurities such as calcium and magnesium. The acid leaching method adopts stirring acid leaching, the pressure acid leaching temperature is 140°C, the pressure acid leaching time is 3.5 hours, and the pressure of the pressure acid leaching is 0.4 MPa. After the acid leaching is completed, the total titanium in the solution is tested to be 3 g / L. The solution is filtered, and then the solid material (acid leaching residue) is washed with water and dried to obtain a titanium-rich material for boiling chlorination.
[0119] Example 3
[0120] The method for improving the yield of the titanium-rich material for boiling chlorination provided in this embodiment comprises the following steps:
[0121] (1) A high calcium and magnesium water-quenched titanium slag 20-60 mesh material (TiO2 content 81.13wt.%, CaO content 0.93wt.%, MgO content 3.46wt.%) is mixed with an acid solution and pre-acid leaching is performed to dissolve the metallic iron by reaction with the acid and then separate it from the titanium slag. The acid solution is a hydrochloric acid solution with a concentration of 28wt.%, the pre-acid leaching time is 2h, the pre-acid leaching temperature is 20°C, the mass of the titanium slag is 45% of the total mass of the titanium slag and the acid solution, and the acid leaching method is stirring leaching. After the pre-acid leaching is completed, a pre-acid leached mixture is obtained.
[0122] (2) The pre-acid leaching mixture obtained in step (1) is transferred to a pressure autoclave for pressure acid leaching, and O2 is introduced into the system to dissolve impurities such as calcium and magnesium. The acid leaching method adopts stirring leaching, the pressure acid leaching temperature is 135°C, the pressure acid leaching time is 5 hours, and the pressure of the pressure acid leaching is 0.35 MPa. After the acid leaching is completed, the total titanium in the solution is tested to be 4.6 g / L. The solution is filtered, and then the solid material (acid leaching residue) is washed with water and dried to obtain a titanium-rich material for boiling chlorination.
[0123] Example 4
[0124] The method for improving the yield of the titanium-rich material for boiling chlorination provided in this embodiment comprises the following steps:
[0125] (1) A high calcium and magnesium water-quenched titanium slag 20-60 mesh material (TiO2 content 78.93wt.%, CaO content 1.67wt.%, MgO content 4.71wt.%, XRF) is mixed with an acid solution and pre-acid leaching is performed to dissolve the metallic iron by reaction with the acid and then separate it from the titanium slag. The acid solution is a hydrochloric acid solution with a concentration of 20wt.%. The pre-acid leaching time is 1h and the pre-acid leaching temperature is 70°C. The mass of the titanium slag is 50% of the total mass of the titanium slag and the acid solution. The acid leaching method is heap leaching. After the pre-acid leaching is completed, a pre-acid leached mixture is obtained.
[0126] (2) The pre-acid leaching mixture obtained in step (1) is transferred to a pressure autoclave for pressure acid leaching, and Cl2 is introduced into the system to dissolve impurities such as calcium and magnesium. The acid leaching method adopts stirring leaching, the pressure acid leaching temperature is 150°C, the pressure acid leaching time is 1.5h, and the pressure of the pressure acid leaching is 0.57MPa. After the acid leaching is completed, the total titanium in the solution is tested to be 3.8g / L. The solution is filtered, and then the solid material (acid leaching residue) is washed with water and dried to obtain a titanium-rich material for boiling chlorination.
[0127] The high calcium and magnesium water-quenched titanium slag used in step (2) of this embodiment was subjected to SEM examination. The SEM image is shown in Figure 1, and the EDS spectrum data (4 sampling points, corresponding to 1, 2, 3 and 4 in Figure 1) are shown in Table 1.
[0128] Table 1 Element content of each sampling point of high calcium and magnesium water-quenched titanium slag (wt%)
[0129] The titanium-rich material for boiling chlorination obtained in step (2) of this embodiment was subjected to SEM examination, and the results are shown in Figures 2 and 3, respectively, wherein Figure 3 is a partial enlarged view of Figure 2 (the area within the box in Figure 2 is the enlarged area), the magnification of Figure 2 is 1000 times, and the magnification of Figure 3 is 5000 times.
[0130] It can be seen from FIG2 and FIG3 that the internal voids of the titanium-rich material for boiling chlorination are filled with hydrolyzates (including needle-shaped and block-shaped hydrolyzates), and the size of the needle-shaped hydrolyzates is about 0.3 μm×1.6 μm.
[0131] Example 5
[0132] The method for improving the yield of the titanium-rich material for boiling chlorination provided in this embodiment comprises the following steps:
[0133] (1) A high calcium and magnesium water-quenched titanium slag material of 20 to 60 mesh (TiO2 content 79.1wt.%, CaO content 1.14wt.%, MgO content 5.22wt.%) is mixed with an acid solution and pre-acid leaching is performed to dissolve the metallic iron by reaction with the acid and then separate it from the titanium slag. The acid solution is a hydrochloric acid solution with a concentration of 25wt.%, the pre-acid leaching time is 1.5h, the pre-acid leaching temperature is 50°C, the mass of the titanium slag is 40% of the total mass of the titanium slag and the acid solution, the acid leaching method is column leaching, and after the pre-acid leaching is completed, a pre-acid leached mixture is obtained.
[0134] (2) The pre-acid leaching mixture obtained in step (1) is transferred to a pressure autoclave for pressure acid leaching, and Cl2 is introduced into the system to dissolve impurities such as calcium and magnesium. The acid leaching method adopts stirring leaching, the pressure acid leaching temperature is 155°C, the pressure acid leaching time is 0.5h, and the pressure of the pressure acid leaching is 0.6MPa. After the acid leaching is completed, the total titanium in the solution is tested to be 4.2g / L. The solution is filtered, and then the solid material (acid leaching residue) is washed with water and dried to obtain a titanium-rich material for boiling chlorination.
[0135] Example 6
[0136] The method for improving the yield of titanium-rich material for boiling chlorination provided in this embodiment is basically the same as that in Example 1, except that, in step (2), NaClO is added instead of chlorine gas.
[0137] Example 7
[0138] The method for improving the yield of titanium-rich material for boiling chlorination provided in this embodiment is basically the same as that in Example 1, except that, in step (2), H2O2 is added instead of chlorine gas.
[0139] Comparative Example 1
[0140] The preparation method of the titanium-rich material provided in this comparative example is basically the same as that in Example 1, except that chlorine gas is not introduced in step (2).
[0141] Comparative Example 2
[0142] The preparation method of the titanium-rich material provided in this comparative example is basically the same as that in Example 1, except that, in step (2), acid leaching is performed at normal pressure instead of pressurized acid leaching.
[0143] Experimental Example 1
[0144] The titanium-rich materials prepared in the above examples and comparative examples were tested for the contents of titanium dioxide, calcium oxide, and magnesium oxide, and the yield of titanium dioxide was calculated. The content test results and yield results are shown in Table 2.
[0145] The content of titanium dioxide, calcium oxide, and magnesium oxide was determined as follows: the sample was ground in a mortar and then pressed into a sheet using a 30t pressure in a press (ZHY-401B, produced by Beijing Zhonghe Chuangye Technology Development Co., Ltd.). The elemental content was then analyzed using an X-ray fluorescence spectrometer (Axios Max, PANalytical, the Netherlands).
[0146] The calculation formula of TiO2 yield is:
[0147] Where: m1 refers to the mass of high calcium and magnesium water-quenched slag, g;
[0148] ω1 refers to the TiO2 content in high calcium and magnesium water-quenched slag, %;
[0149] m2 refers to the mass of titanium-rich material, g;
[0150] ω2 refers to the TiO2 content in titanium-rich material, %;
[0151] Table 2 Content test results and yield results
[0152] Experimental Example 2
[0153] The titanium-rich materials prepared in each of the above examples and comparative examples were subjected to particle size distribution testing (using sieves of different mesh sizes, i.e., 20 mesh, 60 mesh, and 160 mesh, to hold the materials, ultrasonically vibrating on a vibrating screening filter for 5 minutes, and weighing the materials of different particle sizes to calculate the particle size distribution. The vibrating screening filter was produced by Henan Yachuang Machinery Equipment Co., Ltd., model 200) and fine powder rate testing. The results are shown in Table 3. Among them, the ratio of the mass of the material under the 160 mesh sieve to the total mass of the titanium-rich material is the fine powder rate.
[0154] Table 3 Particle size distribution results and fine powder rate test results of titanium-rich materials
[0155] Among them, "60 mesh sieve oversize, 20 mesh sieve undersize" in Table 3 refers to titanium-rich materials with a particle size of 20 mesh to 60 mesh (excluding 60 mesh); "60 mesh sieve undersize, 160 mesh sieve oversize" refers to titanium-rich materials with a particle size of 60 mesh to 160 mesh.
[0156] As can be seen from Tables 2 and 3, compared with Example 1, the fine powder rate in Comparative Example 1 increased significantly, while the titanium yield decreased (trivalent titanium ions generated after the dissolution of the low-valent titanium compound remained in the filtrate). In contrast, the addition of an oxidant to Example 1 significantly reduced the fine powder rate and significantly improved the titanium yield. This indicates that the addition of an oxidant during the pressure acid leaching process can effectively improve the fine powder rate and titanium yield of the product.
[0157] At the same time, compared with Example 1, in Comparative Example 2, acid leaching was carried out at normal pressure, and the impurity element removal efficiency was low, especially the removal rate of magnesium was low (the titanium dioxide yield in Comparative Example 2 was high because the acid leaching in step (2) basically did not leach magnesium oxide).
[0158] Although the present disclosure has been illustrated and described using specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present disclosure, rather than to limit them. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features therein may be replaced by equivalents, without departing from the spirit and scope of the present disclosure. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present disclosure. Therefore, this means that all such replacements and modifications within the scope of the present disclosure are included in the appended claims. Industrial Applicability
[0159] The present disclosure provides a method for improving the yield of titanium-rich material for boiling chlorination and its application. The method not only improves the titanium yield, but also has the advantages of simple operation, short process flow, low cost and low equipment requirements, thus having excellent practical properties.
Claims
1. A method for improving the yield of titanium-rich material for boiling chlorination, characterized in that: The steps include: The titanium slag is mixed with an acid solution for pre-acid leaching to dissolve the metallic iron in the titanium slag, and a pre-acid leaching mixture is obtained after the pre-acid leaching is completed; Adding an oxidant to the pre-acid leaching mixture and performing pressurized acid leaching to dissolve the impurity elements in the pre-acid leaching mixture, and then performing solid-liquid separation to obtain the boiling chlorination titanium-rich material; wherein the impurity elements include at least one of calcium, magnesium, aluminum and manganese; Wherein, the oxidant comprises at least one of a gaseous oxidant, an active metal compound oxidant and a non-metal compound oxidant; The mass fraction of CaO in the titanium-rich material for boiling chlorination is ≤0.1%, and the sum of the mass fractions of CaO and MgO is ≤1.5%.
2. The method for improving the yield of titanium-rich material for boiling chlorination according to claim 1, characterized in that: The gaseous oxidant includes a gaseous elemental oxidant.
3. The method for improving the yield of titanium-rich material for boiling chlorination according to claim 1 or 2, characterized in that: The gaseous oxidant comprises at least one of Cl2, Br2, O2 and O3; Preferably, the active metal compound oxidant comprises at least one of NaClO, NaClO3, KClO and KClO3; Preferably, the non-metal compound oxidant includes at least one of H2O2 and HClO.
4. The method for improving the yield of titanium-rich material for boiling chlorination according to any one of claims 1 to 3, characterized in that: The amount of the oxidant added is such that the sum of the mass concentrations of trivalent titanium ions and tetravalent titanium ions in the mixed material is ≤5 g / L.
5. The method for improving the yield of titanium-rich material for boiling chlorination according to any one of claims 1 to 4, characterized in that: The mass fraction of TiO2 in the titanium slag is ≥70.0%; Preferably, the mass fraction of CaO in the titanium slag is ≥0.3%, and the mass fraction of MgO is ≥3.0%; Preferably, the titanium slag includes water-quenched titanium slag obtained by smelting and water quenching titanium concentrate.
6. The method for improving the yield of titanium-rich material for boiling chlorination according to any one of claims 1 to 5, characterized in that: The pre-acid leaching temperature is 20°C to 105°C; Preferably, the pre-acid leaching time is 5 min to 300 min; Preferably, the mass of the titanium slag is 15% to 80% of the total mass of the titanium slag and the acid solution.
7. The method for improving the yield of titanium-rich material for boiling chlorination according to any one of claims 1 to 6, characterized in that: The temperature of the pressurized acid leaching is 130°C to 175°C; Preferably, the pressurized acid leaching time is ≥ 0.2 h, more preferably 0.5 h to 5 h.
8. The method for improving the yield of titanium-rich material for boiling chlorination according to any one of claims 1 to 7, characterized in that: The pressure of the pressurized acid leaching is 0.3MPa to 0.9MPa.
9. A titanium-rich material for boiling chlorination, prepared by the method for improving the yield of titanium-rich material for boiling chlorination according to any one of claims 1 to 8; Preferably, the mass fraction of TiO2 in the titanium-rich material for boiling chlorination is ≥85%, and the TiO2 yield is ≥90%.
10. A method for preparing a titanium-rich material for producing titanium tetrachloride by boiling chlorination method, characterized in that: A method for improving the yield of titanium-rich material for boiling chlorination as claimed in any one of claims 1 to 8; Wherein, in the titanium-rich material used for producing titanium tetrachloride by boiling chlorination method, the mass fraction of CaO is ≤0.1%, and the sum of the mass fractions of CaO and MgO is ≤1.5%.
11. A method for preparing titanium tetrachloride, characterized in that: The invention comprises the method for preparing the titanium-rich material for producing titanium tetrachloride by boiling chlorination process as claimed in claim 10.
12. A titanium-containing material, characterized in that: Mainly prepared from titanium tetrachloride prepared by the method for preparing titanium tetrachloride as claimed in claim 11; Wherein, the titanium-containing material includes at least one of sponge titanium, titanium alloy, chloride titanium dioxide and pearlescent pigment.
Citation Information
Patent Citations
Method for preparing titanium pigment by using titanium residues obtained by directly reducing titanium-iron oxide
CN102627321A
Method for preparing titanium-rich material for fluidizing chlorination from high-calcium-magnesium low-grade titanium slag
CN110629045A
Production method of titanium-rich material
CN111979413A
Preparation method of titanium-rich material and preparation method of titanium tetrachloride
CN113862494A
Method for improving yield of titanium-rich material for fluidizing chlorination and application thereof
CN116426759A
Cited By
Reconstruction method of anosovite of chlorination process titanium dioxide oxidation unqualified primary product and anosovite
CN121134830A