Method for preparing raw materials for boiling chlorination from titanium slag

By performing low-temperature pretreatment and acid leaching treatment on water-quenched titanium slag, the problems of poor quality and fine particle size in the preparation of titanium slag are solved, efficient preparation of boiling chlorination raw materials is achieved, the yield and grade of TiO2 are improved, and the process is simplified process and reduce costs.

WO2024198212A1PCT designated stage expired Publication Date: 2024-10-03LOMON BILLIONS GRP CO LTD +2

Patent Information

Application Number
PCT/CN2023/114445
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2023-08-23
Publication Date
2024-10-03

Smart Images

  • Figure CN2023114445_03102024_PF_FP_ABST
    Figure CN2023114445_03102024_PF_FP_ABST
Patent Text Reader

Abstract

A method for preparing raw materials for boiling chlorination from titanium slag, comprising the following steps: S1, pretreating water-quenched titanium slag at 150-550℃ to obtain pretreated titanium slag; and S2, successively subjecting the pretreated titanium slag to pre-leaching treatment and acid leaching treatment to obtain raw materials for boiling chlorination. Adding the low-temperature pretreatment step before leaching of the water-quenched titanium slag reduces titanium loss, effectively avoids pulverization of products during the subsequent leaching process so as to ensure the leaching effect of other impurity elements while improving titanium yield, and reduces the amount of fine powder in products, thus improving the grade of TiO2, and satisfying the requirements for raw materials for boiling chlorination. The present disclosure involves a short process flow and simple steps, and achieves high yield of TiO2.
Need to check novelty before this filing date? Find Prior Art

Description

A method for preparing boiling chlorination raw material from titanium slag

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This disclosure claims priority to Chinese patent application No. 2023103172189, filed with the Patent Office of China on March 28, 2023, entitled “A method for preparing boiling chlorination raw materials from titanium slag,” the entire contents of which are incorporated herein by reference. Technical Field

[0003] The present disclosure relates to the technical fields of metallurgy and chemical engineering, and in particular to a method for preparing boiling chlorination raw materials from titanium slag. Background Art

[0004] Titanium dioxide is one of the highest-performing white pigments currently available and is widely used in industries such as coatings, plastics, papermaking, printing inks, chemical fibers, rubber, and cosmetics. Industrial production methods for titanium dioxide include the sulfuric acid process and the chlorination process. The sulfuric acid process has a lengthy production process, poor product quality, and is prone to pollution. The chlorination process is environmentally friendly, but it is very demanding on raw materials and requires a high TiO2 content. This is because the impurities CaO and MgO generate low-melting, high-boiling-point chlorides during the chlorination process, which degrade the fluidity of the fluidized chlorination furnace bed.

[0005] Currently, there are three industrial production methods for titanium-rich materials for large-scale boiling chlorination: the electric furnace method, acid leaching, and reduction corrosion. These methods require high-quality raw materials, primarily high-quality placer resources with low impurity content. However, high-quality ilmenite placer resources are relatively scarce, while ilmenite rock resources are relatively abundant. Therefore, it is of great significance to improve the utilization value of low-quality titanium resources and process them into high-quality titanium-rich materials for large-scale boiling chlorination.

[0006] Methods for utilizing low-quality titanium resources primarily focus on two approaches: the combined process of electric furnace smelting of titanium concentrate and titanium slag upgrading, and the direct upgrading of titanium concentrate to synthetic rutile. While the direct upgrading of titanium concentrate to synthetic rutile is relatively simple, it suffers from the problem of severely substandard product particle size. The combined process of electric furnace smelting and titanium slag upgrading effectively addresses the problem of fine product size, but it also presents significant process complexity and high costs.

[0007] The use of low-quality titanium resources to produce titanium-rich materials presents the following challenges: poor product quality, fine particle size, and significant pulverization. A low percentage of the resulting material can be directly used for boiling chlorination, requiring further granulation to meet boiling chlorination requirements. Furthermore, significant titanium loss and low yields result from the production process. The process is long and complex, resulting in poor economic efficiency, secondary pollution, and high production costs.

[0008] Summary of the Invention

[0009] The present disclosure provides a method for preparing a boiling chlorination raw material from titanium slag, comprising the following steps:

[0010] S1, pre-treating water-quenched titanium slag at 150-550° C. to obtain pre-treated titanium slag;

[0011] S2. The pretreated titanium slag is sequentially subjected to pre-leaching treatment and acid leaching treatment to obtain a boiling chlorination raw material.

[0012] Optionally, in step S1, the content of TiO2 in the water-quenched titanium slag is 70wt.% to 85wt.%, the content of CaO is ≥0.2wt.%, and the content of MgO is ≥2wt.%.

[0013] Optionally, in step S1, the particle size of the water-quenched titanium slag is 20-160 mesh.

[0014] Optionally, in step S1, the pretreatment includes oxidative roasting.

[0015] Optionally, in step S1, the pretreatment time is 0.5 to 4 hours.

[0016] Optionally, in step S1, the content of low-valent titanium in the pretreated titanium slag is ≤0.5 wt.%.

[0017] Optionally, in step S1, the method for preparing water-quenched titanium slag includes: mixing molten titanium slag with a water quenching liquid, and performing water quenching to obtain water-quenched titanium slag.

[0018] Optionally, the water quenching pressure is 1 kg·f / cm 2 ~40kg·f / cm 2 .

[0019] Optionally, in step S2, the preleaching treatment includes acid leaching a mixture of the pretreated titanium slag and the first acid solution to obtain leached slag.

[0020] Optionally, in step S2, the prepreg treatment temperature is 20-100°C, and the prepreg treatment time is 20-120 minutes.

[0021] Optionally, in step S2, the mass ratio of the first acid solution to the pretreated titanium slag is (0.5-2):1.

[0022] Optionally, in step S2, the mass concentration of the first acid solution is 5% to 30%.

[0023] Optionally, in step S2, the acid leaching treatment includes pressurizing the mixture of the leached residue and the second acid solution to acid leach.

[0024] Optionally, in step S2, the temperature of the acid leaching treatment is 130-175° C., and the time of the acid leaching treatment is 0.5-6 hours.

[0025] Optionally, in step S2, the pressure of the acid leaching treatment is 0.2 to 0.9 MPa.

[0026] Optionally, in step S2, the mass ratio of the second acid solution to the leached residue is (1-5):1.

[0027] Optionally, in step S2, the mass concentration of the second acid solution is 13% to 30%.

[0028] Optionally, in step S2, the first acid solution and the second acid solution independently include at least one of hydrochloric acid, nitric acid, acetic acid, sulfuric acid and hydrofluoric acid.

[0029] The present disclosure also provides a boiling chlorination raw material, characterized in that the boiling chlorination raw material is prepared by any of the methods described above.

[0030] Optionally, the fine powder rate of the boiling chlorination raw material is ≤5%.

[0031] Optionally, in the boiling chlorination raw material, the TiO2 content is ≥85wt.%, the CaO content is ≤0.1wt.%, and the total content of CaO and MgO is ≤1.5wt.%;

[0032] Optionally, the TiO2 content in the boiling chlorination raw material is ≥90wt.%. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the specific embodiments of the present disclosure or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the specific embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present disclosure. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0034] FIG1 is an XRD diagram of water-quenched titanium slag after pretreatment at different temperatures according to the present disclosure.

[0035] FIG2 shows the effect of the pretreatment temperature on the TiO2 yield and CaO / MgO content after pressure acid leaching in the present disclosure. DETAILED DESCRIPTION

[0036] The technical solutions of the present disclosure will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but those skilled in the art will understand that the embodiments described below are part of the embodiments of the present disclosure, rather than all of the embodiments, and are only used to illustrate the present disclosure, and should not be considered as limiting the scope of the present disclosure. Based on the embodiments in the present disclosure, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present disclosure. If specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0037] The following is a detailed description of the preparation of boiling chlorination raw materials using titanium slag according to the present disclosure.

[0038] In some embodiments of the present disclosure, a method for preparing a boiling chlorination raw material from titanium slag is provided, comprising the following steps:

[0039] S1, pretreating water-quenched titanium slag at 150-550° C. to obtain pretreated titanium slag;

[0040] S2. Pre-treating the titanium slag: performing pre-leaching treatment and acid leaching treatment in sequence to obtain a boiling chlorination raw material.

[0041] The present invention adds a low-temperature pretreatment step to the water-quenched titanium slag before the leaching process, which not only destroys the black titanium structure in the water-quenched titanium slag, but also oxidizes low-valent titanium to tetravalent titanium, ensuring that no trivalent titanium enters the mother liquor during the subsequent leaching process, reducing titanium losses, and improving the titanium yield while also ensuring the leaching effect of other impurity elements. The low-temperature pretreatment step strengthens the skeleton structure of the water-quenched titanium slag and significantly eliminates the low-valent titanium in the water-quenched titanium slag, effectively avoiding product pulverization during the subsequent leaching process.

[0042] Compared with other process routes for removing impurities such as calcium and magnesium (such as oxidation-reduction-acid leaching, etc.), the process disclosed in the present invention has a short process flow, low cost, and wider adaptability to raw materials. Impurity elements such as calcium and magnesium can be removed from water-quenched titanium slag through pretreatment and leaching processes.

[0043] The present invention discloses a method for preparing a boiling chlorination raw material by using titanium slag as a raw material, comprising sequentially performing pretreatment, preleaching treatment and acid leaching treatment on the water-quenched titanium slag.

[0044] Among them, pretreatment: Due to the poor crystallinity of water-quenched titanium slag, it forms more pores, which makes it have good acid solubility. Although direct acid leaching can effectively remove harmful impurities such as calcium, magnesium, and aluminum in the slag, there is a problem of large titanium loss. Through low-temperature pretreatment, the low-valent titanium in the water-quenched titanium slag is oxidized to TiO2, which significantly reduces the acid solubility of this part of titanium. At the same time, in order to ensure the leaching of impurity elements, it is necessary to control the Fe content in the slag.2+ Oxidation of Fe 2+ Oxidized to Fe 3+ This then forms Fe2TiO5 with poor acid solubility in the titanium phase, resulting in low leaching rates for subsequent impurities such as calcium and magnesium. Heat pretreatment also affects the leaching rate of Ca. The higher the heat pretreatment temperature, the lower the Ca leaching rate. This is mainly because amorphous CaSi2O5 is converted into crystalline CaSi2O5 with poor acid solubility after heating.

[0045] Pre-impregnation treatment: After pre-treatment, a small amount of metallic iron still exists in the water-quenched titanium slag. During the acid leaching process, the metallic iron reacts with the acid to generate free hydrogen. This free hydrogen can reduce the tetravalent titanium in the titanium slag to trivalent titanium. During the acid leaching process, the acid concentration of the reaction system is relatively high. Under high acidity, trivalent titanium cannot be hydrolyzed and precipitated, which will cause titanium to be lost in the solution, resulting in a low TiO2 yield. To avoid the influence of this part of metallic iron, the reaction system needs to be pre-impregnated before acid leaching.

[0046] Acid leaching treatment: During the acid leaching process, the black titanium structure in the titanium slag can be further destroyed, so as to remove the impurities such as calcium and magnesium, and selectively dissolve the impurities such as calcium and magnesium. One of the main chemical reactions during the acid leaching process is as follows: CaSi2O5+2H + →Ca 2+ +H2Si2O5.

[0047] In the method for preparing a boiling chlorination raw material from titanium slag, Ca in the water-quenched slag mainly exists in the form of CaSi2O5, and CaSi2O5 and glass are mutually included to form a complex. Both CaSi2O5 and glass are easily acid-soluble substances. Magnesium mainly exists in the magnesia tantalum structure. The tantalum structure can be further removed by destroying it through low-temperature pretreatment, pre-leaching treatment and acid leaching treatment. Titanium mainly exists in the tantalum or rutile phase and is not easily leached, thereby ensuring a high TiO2 yield.

[0048] In some embodiments of the present disclosure, in step S1, the boiling chlorination raw material refers to a titanium-rich material used in a boiling chlorination process.

[0049] In some embodiments of the present disclosure, in step S1, the method for preparing water-quenched titanium slag includes: mixing molten titanium slag with a water quenching liquid, and performing water quenching to obtain water-quenched titanium slag.

[0050] In some embodiments of the present disclosure, in step S1, the water quenching liquid includes at least one of water, an acidic solution, and an alkaline solution; water may be selected; and the pressure of the water quenching liquid is 1 kg·f / cm 2 ~40kg·f / cm 2 .

[0051] In some embodiments of the present disclosure, in step S1, the molten titanium slag is mainly obtained by smelting a mixture of ilmenite concentrate and a reducing agent.

[0052] Water-quenched titanium slag is produced by subjecting molten titanium slag to high-pressure water quenching. Rapidly cooling the high-temperature molten titanium slag by high-velocity water causes the atoms and ions in the slag to solidify before they have time to form regularly arranged crystalline materials, resulting in poor crystallinity. Furthermore, the rapid cooling causes changes in the slag's physical structure, with some pyroclastic structures undergoing rutile formation and a greater amount of glassy material. Due to the combined effects of high-pressure water shock and internal cooling stress on the molten titanium slag, numerous pores form within the slag. This facilitates acid diffusion during acid leaching, facilitating the leaching of impurity elements. Furthermore, it was found that calcium in the slag primarily exists as CaSi2O5, which is incorporated into the glassy material to form a complex. The pyroclastic material and the complex are interlocked and evenly dispersed. CaSi2O5 is highly acid-soluble and can be easily removed during acid leaching.

[0053] In some embodiments of the present disclosure, in step S1, the content of TiO2 in the water-quenched titanium slag is 70 wt.% to 85 wt.%, for example, it can be 72 wt.% to 82 wt.%, 75 wt.% to 80 wt.% or 76 wt.% to 78 wt.%, such as 71 wt.%, 73 wt.%, 75 wt.%, 77 wt.%, 79 wt.%, 81 wt.%, 83 wt.%, 84 wt.% or 85 wt.%, or a range between any two endpoint values;

[0054] The CaO content is ≥0.2 wt.%, for example, ≥0.4 wt.%, ≥0.6 wt.%, ≥0.8 wt.%, or ≥1.0 wt.%, etc.;

[0055] The content of MgO is ≥ 2 wt.%, for example, ≥ 3 wt.%, 5 wt.%, 7 wt.%, or 9 wt.%.

[0056] In some embodiments of the present disclosure, in step S1, the particle size of the water-quenched titanium slag is 20 mesh to 160 mesh, for example, 40 mesh to 150 mesh, 50 mesh to 140 mesh or 60 mesh to 120 mesh, such as 20 mesh, 40 mesh, 60 mesh, 80 mesh, 90 mesh, 100 mesh, 110 mesh, 120 mesh, 130 mesh, 140 mesh, 150 mesh, or 155 mesh, or a range between any two endpoint values.

[0057] In some embodiments of the present disclosure, in step S1, the pretreatment includes oxidative roasting.

[0058] In some embodiments of the present disclosure, in step S1, the pretreatment temperature is 150-550°C, and the pretreatment time is 0.5-4 h; typically but not limitatively, for example, the pretreatment temperature is 180-520°C, 250-450°C or 300-400°C, such as 150°C, 200°C, 250°C, 300°C, 350°C, 400°C, 450°C, 500°C, 550°C or a range consisting of any two thereof; the pretreatment time is 1.0-3.5 h, 1.5-3.0 h or 2.0-2.5 h, such as 0.5 h, 1 h, 1.5 h, 2 h, 3.5 h, 4 h or a range consisting of any two thereof.

[0059] In some embodiments of the present disclosure, in step S1, the volume content of oxygen in the furnace during the pretreatment process is ≥ 5%; alternatively, the volume content of oxygen in the furnace during the pretreatment process is 10% to 20%. During the pretreatment process, exhaust gas from combustion of a substance and air, such as gas from combustion of natural gas and air, are introduced into the furnace to control the oxygen content in the furnace.

[0060] In some embodiments of the present disclosure, in step S1, the content of low-valent titanium in the pretreated titanium slag is ≤0.5 wt.%. Low-valent titanium is titanium with a valence of +3.

[0061] In some embodiments of the present disclosure, in step S2, the pre-leaching treatment includes acid leaching a mixture of the pre-treated titanium slag and the first acid solution to obtain leached slag.

[0062] Pre-leaching treatment mainly removes metallic iron from pre-treated titanium slag.

[0063] In some embodiments of the present disclosure, in step S2, the prepreg temperature is 20°C to 100°C, and the prepreg time is 20 min to 120 min; typically but not limitatively, for example, the prepreg temperature is 25°C to 85°C, 35°C to 75°C or 45°C to 65°C, such as 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C or a range consisting of any two thereof; the prepreg time is 35 min to 115 min, 45 min to 95 min or 65 min to 75 min, such as 20 min, 40 min, 60 min, 80 min, 100 min, 120 min or a range consisting of any two thereof; optionally, the prepreg temperature is 50°C to 100°C.

[0064] In some embodiments of the present disclosure, in step S2, the pre-leaching treatment method includes any one of stirring leaching, column leaching and heap leaching.

[0065] In some embodiments of the present disclosure, in step S2, the mass ratio of the first acid solution and the pretreated titanium slag is (0.5~2):1; typically but not limitatively, for example, the mass ratio of the first acid solution and the pretreated titanium slag is 0.5:1, 1:1, 1.5:1, 2:1 or a range consisting of any two of them; optionally, the mass ratio of the first acid solution and the pretreated titanium slag is (1~2):1.

[0066] In some embodiments of the present disclosure, in step S2, the mass concentration of the first acid solution is 5% to 30%; typically but not limiting, for example, the mass concentration of the first acid solution is 6% to 28%, 8% to 24% or 12% to 18%, such as 5%, 10%, 15%, 20%, 25%, 30% or a range consisting of any two thereof; optionally, the mass concentration of the first acid solution is 8% to 15%.

[0067] In some embodiments of the present disclosure, in step S2, the acid leaching treatment includes subjecting the mixture of the leached residue and the second acid solution to pressure acid leaching.

[0068] In some embodiments of the present disclosure, in step S2, the acid leaching temperature is 130-175° C., and the acid leaching time is 0.5-6 h. Typically, but not limiting, for example, the acid leaching temperature is 130° C., 140° C., 150° C., 160° C., 170° C., or a range consisting of any two thereof; the acid leaching time is 0.5 h, 2 h, 3 h, 4 h, 5 h, 6 h, or a range consisting of any two thereof.

[0069] In some embodiments of the present disclosure, in step S2, the pressure of the acid leaching treatment is 0.2-0.9 MPa; typically but not limitatively, for example, the pressure of the acid leaching treatment is 0.2 MPa, 0.4 MPa, 0.6 MPa, 0.8 MPa, 0.9 MPa or a range consisting of any two thereof.

[0070] The acid leaching and impurity removal stage adopts the pressurized acid leaching method, which can achieve efficient leaching of impurities at a pressure higher than that of normal pressure acid leaching.

[0071] In some embodiments of the present disclosure, in step S2, the acid leaching treatment includes stirring leaching.

[0072] In some embodiments of the present disclosure, in step S2, the mass ratio of the second acid solution to the leached residue is (1-5):1; typically but not limitatively, for example, the mass ratio of the second acid solution to the leached residue is 1:1, 2:1, 3:1, 4:1, 5:1 or a range consisting of any two thereof.

[0073] In some embodiments of the present disclosure, in step S2, the mass concentration of the second acid solution is 13% to 30%, for example, 15% to 28%, 18% to 25% or 13% to 30%; optionally, the mass concentration of the second acid solution is 15% to 25%.

[0074] In some embodiments of the present disclosure, in step S2, the first acid solution and the second acid solution each independently include at least one of hydrochloric acid, nitric acid, acetic acid, sulfuric acid and hydrofluoric acid; optionally, in step S2, the first acid solution and the second acid solution are hydrochloric acid solutions.

[0075] The mother liquor after acid leaching disclosed in the present invention can be used as supplementary acid for the next acid leaching, thereby improving the utilization rate of the acid used for acid leaching and effectively reducing the subsequent acid reprocessing.

[0076] In some embodiments of the present disclosure, in step S2, after the acid leaching treatment, solid-liquid separation, washing and drying are also included.

[0077] In some embodiments of the present disclosure, the fine powder rate of the boiling chlorination raw material is ≤5%, for example, ≤4%, ≤3%, or ≤2%.

[0078] In some embodiments of the present disclosure, the TiO2 content in the boiling chlorination raw material is ≥85 wt.%, such as ≥90 wt.%, ≥95 wt.%, or ≥97 wt.%, etc.;

[0079] CaO content ≤ 0.1 wt.%, for example ≤ 0.08 wt.%, ≤ 0.05 wt.%, or ≤ 0.04 wt.%, etc.;

[0080] Total content of CaO and MgO ≤ 1.5wt.%;

[0081] Optionally, the TiO2 content in the boiling chlorination raw material is ≥90wt.%, such as ≥93wt.%, ≥96wt.% or ≥98wt.%.

[0082] In the method for preparing boiling chlorination raw material from titanium slag disclosed in the present invention, the yield of TiO2 is ≥90%; optionally, the yield of TiO2 is ≥95%.

[0083] The present disclosure provides a method for preparing a boiling chlorination raw material from titanium slag, which can reduce the impurity content in the titanium slag and the amount of fine powder in the product, and improve the grade of TiO2, thereby meeting the requirements of the boiling chlorination raw material; moreover, the preparation method has a short process flow, simple steps, and a high TiO2 yield.

[0084] The method for preparing a boiling chlorination raw material from titanium slag disclosed in the present invention reduces the amount of fine powder in the product on the basis of reducing the impurity content in the titanium slag, thereby improving the grade of TiO2 and meeting the requirements of the boiling chlorination raw material. A boiling chlorination raw material with a fine powder rate of ≤5%, a TiO2 content of ≥85wt.%, a CaO content of ≤0.1wt.%, and a total content of CaO and MgO of ≤1.5wt.% can be obtained.

[0085] The preparation method disclosed in the present invention reduces titanium loss, and the yield of TiO2 is ≥90%. In addition, the process flow is short, the cost is low, and the adaptability to raw materials is wider.

[0086] The present invention significantly reduces the content of low-valent titanium in water-quenched titanium slag by adding a low-temperature (150-550°C) pretreatment step before leaching, ensuring that no trivalent titanium enters the mother liquor during the subsequent leaching process, thereby reducing titanium loss; strengthens the skeleton structure of the water-quenched titanium slag, and at the same time significantly eliminates the low-valent titanium in the water-quenched titanium slag, effectively avoiding pulverization of the product during the subsequent leaching process.

[0087] Example

[0088] The particle size of the water-quenched titanium slag in the embodiments and comparative examples of the present disclosure is both 20-160 meshes, and both are obtained by water quenching the molten titanium slag.

[0089] Example 1

[0090] The method for preparing a boiling chlorination raw material from titanium slag provided in this embodiment comprises the following steps:

[0091] S1, pretreating water-quenched titanium slag at 150° C. for 4 h with an oxygen content of 15% by volume in the furnace to obtain pretreated titanium slag, wherein the low-valent titanium content in the pretreated titanium slag is 0.45 wt.%;

[0092] S2. Heap leaching was performed by mixing a 27 wt.% hydrochloric acid solution with the pretreated titanium slag in a mass ratio of 0.5:1 at 80° C. for 20 min, and filtering to obtain leached slag;

[0093] S3. Place the mixture of the leached residue and the hydrochloric acid solution in a pressure reactor and heat it to 130° C., pressurize and leach for 6 hours at a pressure of 0.25 MPa, adjust the liquid-solid ratio of the mixture to 1 g:1 g, and the concentration of the hydrochloric acid solution to 30 wt.%. After the leaching is completed, perform solid-liquid separation, washing, and drying in sequence to obtain the acid leaching residue, which is the boiling chlorination raw material.

[0094] The content analysis of water-quenched titanium slag and acid-leached slag is carried out using the following test methods:

[0095] 5 g of sample was mixed and ground in a mortar, then pressed into sheets using a 30 t pressure in a sample press (ZHY-401B, manufactured by Beijing Zhonghe Chuangye Technology Development Co., Ltd.). Chemical composition analysis was then performed using an Axios Max X-ray fluorescence spectrometer (XRF) from PANalytical, the Netherlands. For specific methods, see Section 1.3 Analysis and Standards in the following reference: Zhang Jianbo et al. Comparative Study of Panzhihua Titanium Slag and Titanium Concentrate in Redox Modification-Acid Leaching Process [J], Rare Metals, 2016, 40(4): 385-392.

[0096] The index analysis of water-quenched titanium slag and acid-leached slag is shown in Table 1.

[0097] Table 1

[0098] The TiO2 yield and fine powder rate in the acid leaching residue are shown in Table 2.

[0099] Table 2

[0100] Example 2

[0101] The method for preparing a boiling chlorination raw material from titanium slag provided in this embodiment comprises the following steps:

[0102] S1, pretreating water-quenched titanium slag at 300° C. for 2 h with an oxygen content of 10% by volume in the furnace to obtain pretreated titanium slag, wherein the low-valent titanium content in the pretreated titanium slag is 0.3 wt.%;

[0103] S2. A 15 wt.% hydrochloric acid solution and pretreated titanium slag were mixed in a mass ratio of 1:1, and the mixture was reacted at 50° C. for 90 min, and the leached residue was obtained after filtration;

[0104] S3. Place the mixture of the leached residue and the hydrochloric acid solution in a pressure reactor and heat it to 175° C., pressurize and leach at a pressure of 0.86 MPa for 0.5 h, adjust the liquid-solid ratio of the mixture to 2.4 g:1 g, and the concentration of the hydrochloric acid solution to 21 wt.%. After the leaching is completed, perform solid-liquid separation, washing, and drying in sequence to obtain the acid leaching residue, which is the boiling chlorination raw material.

[0105] The content determination method of water-quenched titanium slag and acid-leached slag is the same as that in Example 1.

[0106] The index analysis of water-quenched titanium slag and acid-leached slag is shown in Table 3.

[0107] Table 3

[0108] The TiO2 yield and fine powder rate in the acid leaching residue are shown in Table 4.

[0109] Table 4

[0110] Example 3

[0111] The method for preparing a boiling chlorination raw material from titanium slag provided in this embodiment comprises the following steps:

[0112] S1, pretreating water-quenched titanium slag at 350° C. for 1.5 h, with the volume content of oxygen in the furnace being 18%, to obtain pretreated titanium slag, wherein the content of low-valent titanium in the pretreated titanium slag is 0.23 wt.%;

[0113] S2. A hydrochloric acid solution with a concentration of 8 wt.% and pretreated titanium slag are stirred and leached at a mass ratio of 2:1 at 100° C. for 120 min, and the leached residue is obtained after filtration;

[0114] S3. Place the mixture of the leached residue and the hydrochloric acid solution in a pressure reactor and heat it to 155° C., pressurize and leach for 6 hours at a pressure of 0.86 MPa, adjust the liquid-to-solid ratio of the mixture to 5 g:1 g, and the concentration of the hydrochloric acid solution to 17 wt.%. After the leaching is completed, perform solid-liquid separation, washing, and drying in sequence to obtain the acid leaching residue, which is the boiling chlorination raw material.

[0115] The content determination method of water-quenched titanium slag and acid-leached slag is the same as that in Example 1.

[0116] The index analysis of water-quenched titanium slag and acid-leached slag is shown in Table 5.

[0117] Table 5

[0118] The TiO2 yield and fine powder rate in the acid leaching residue are shown in Table 6.

[0119] Table 6

[0120] Example 4

[0121] The method for preparing a boiling chlorination raw material from titanium slag provided in this embodiment comprises the following steps:

[0122] S1, pretreating water-quenched titanium slag at 550° C. for 0.5 h with an oxygen content of 20% by volume in the furnace to obtain pretreated titanium slag, wherein the low-valent titanium content in the pretreated titanium slag is 0.1 wt.%;

[0123] S2. A 10 wt.% hydrochloric acid solution and pretreated titanium slag were stirred and leached at a mass ratio of 1.5:1 at 25°C for 120 minutes, and the leached residue was obtained after filtration;

[0124] S3. Place the mixture of the leached residue and the hydrochloric acid solution in a pressure reactor and heat it to 160° C., pressurize and leach for 3 hours at a pressure of 0.6 MPa, adjust the liquid-to-solid ratio of the mixture to 4 g:1 g, and the concentration of the hydrochloric acid solution to 15 wt.%. After the leaching is completed, perform solid-liquid separation, washing, and drying in sequence to obtain the acid leaching residue, which is the boiling chlorination raw material.

[0125] The content determination method of water-quenched titanium slag and acid-leached slag is the same as that in Example 1.

[0126] The index analysis of water-quenched titanium slag and acid-leached slag is shown in Table 7.

[0127] Table 7

[0128] The TiO2 yield and fine powder rate in the acid leaching residue are shown in Table 8.

[0129] Table 8

[0130] Comparative Example 1

[0131] The method for preparing boiling chlorination raw material from titanium slag provided in this comparative example comprises the following steps:

[0132] The mixture of the water-quenched titanium slag and the hydrochloric acid solution in Example 4 was placed in a pressure reactor and heated to 160°C. The mixture was pressurized and leached at a pressure of 0.6 MPa for 3 hours. The liquid-to-solid ratio of the mixture was adjusted to 4g:1g, and the concentration of the hydrochloric acid solution was 15wt.%. After the leaching was completed, the mixture was subjected to solid-liquid separation, washing, and drying in sequence to obtain the acid leaching residue, which was the boiling chlorination raw material.

[0133] The content determination method of water-quenched titanium slag and acid-leached slag is the same as that in Example 1.

[0134] The index analysis of water-quenched titanium slag and acid-leached slag is shown in Table 9.

[0135] Table 9

[0136] The TiO2 yield and fine powder rate in the acid leaching residue are shown in Table 10.

[0137] Table 10

[0138] Comparative Example 2

[0139] The method for preparing boiling chlorination raw material from titanium slag provided in this comparative example refers to Example 4, except that, in step S1, the pretreatment temperature is 800°C.

[0140] The content determination method of water-quenched titanium slag and acid-leached slag is the same as that in Example 1.

[0141] The index analysis of water-quenched titanium slag and acid-leached slag is shown in Table 11.

[0142] Table 11

[0143] The TiO2 yield and fine powder rate in the acid leaching residue are shown in Table 12.

[0144] Table 12

[0145] Test Example 1

[0146] XRD analysis of the phase structure of water-quenched titanium slag after pretreatment at different temperatures clearly shows the structural changes of water-quenched titanium slag at different temperatures, and the results are shown in Figure 1.

[0147] The water-quenched titanium slag is the same as that in Example 4, the pretreatment time is 1 hour, and the volume content of oxygen in the furnace is 10%.

[0148] As can be seen from Figure 1, after the water-quenched slag is heated and pretreated, the diffraction peak intensity at 2Theta (18°, 25.3°, 32.5°) gradually weakens, while the peak intensity at 2Theta (27.5°, 36.1°, 41.2°, 54.3° and 56.6°) gradually increases, indicating that the phase structure of the water-quenched slag undergoes obvious changes during the heating and pretreatment process.

[0149] Using the water-quenched titanium slag in Example 4 as raw material, the relationship between the TiO2 yield and the impurity content in the acid leaching residue after acid leaching at different pretreatment temperatures was investigated. The results are shown in Figure 2.

[0150] Among them, the preparation method of acid leaching residue using water-quenched titanium slag as raw material includes the following steps: S1, pretreating the water-quenched titanium slag of Example 4 at different temperatures for 2 hours, and the oxygen volume content in the furnace is 15% to obtain pretreated titanium slag; S2, mixing the pretreated titanium slag and a hydrochloric acid solution with a concentration of 20wt.%, the liquid-solid ratio of the mixture is 1g:1g, and stirring and leaching is carried out at 100°C for 60 minutes, and the leached residue is obtained after filtration; S3, placing the mixture of the leaching residue and the hydrochloric acid solution in a pressure reactor and heating it to 150°C, pressurizing and leaching for 4 hours at a pressure of 0.45MPa, adjusting the liquid-solid ratio of the mixture to 2.5g:1g, and the concentration of the hydrochloric acid solution to 22wt.%. After the leaching is completed, the acid leaching residue is obtained by solid-liquid separation, washing and drying.

[0151] As can be seen from Figure 2, the higher the pretreatment temperature, the higher the TiO2 yield, and the leaching rates of CaO and MgO are almost unaffected by the pretreatment temperature when the pretreatment temperature is lower than 550°C. However, when the pretreatment temperature is higher than 550°C, the leaching rates of CaO and MgO decrease as the pretreatment temperature increases, which is also reflected in the increase in the CaO and MgO content in the leached residue. Increasing the pretreatment temperature causes the leached residue to be unable to meet the requirements of boiling chlorination raw materials. The preparation method disclosed in the present invention has a high TiO2 yield and a high leaching rate of impurities such as CaO and MgO, and the content of impurities such as CaO and MgO in the acid leaching residue is low. Figure 2 uses the effect of different temperature pretreatments on the CaO and MgO content and TiO2 yield in the acid leaching residue as an example to further describe the advantages of the disclosed patent. The relationship between the pretreatment temperature and the content of other impurities in the acid leaching residue and the TiO2 yield will not be repeated.

[0152] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present disclosure, rather than to limit them. Although the present disclosure has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present disclosure. Industrial Applicability

[0153] The present disclosure provides a method for preparing a boiling chlorination raw material from titanium slag. By adding a low-temperature pretreatment step before leaching the water-quenched titanium slag, the loss of titanium is reduced, and the pulverization of the product in the subsequent leaching process is effectively avoided. While improving the titanium yield, the leaching effect of other impurity elements is ensured, and the amount of fine powder in the product is reduced, thereby improving the grade of TiO2 and meeting the requirements of the boiling chlorination raw material. In addition, the preparation method disclosed in the present disclosure has a short process flow, simple steps, and a high TiO2 yield, and therefore has excellent practical performance.

Claims

1. A method for preparing boiling chlorination raw material from titanium slag, characterized in that: The steps include: S1, pretreating the water-quenched titanium slag at 150° C. to 550° C. to obtain pretreated titanium slag; S2. The pretreated titanium slag is sequentially subjected to pre-leaching treatment and acid leaching treatment to obtain a boiling chlorination raw material.

2. The method for preparing boiling chlorination raw material from titanium slag according to claim 1, characterized in that: In step S1, the water-quenched titanium slag has a TiO2 content of 70wt.% to 85wt.%, a CaO content of ≥0.2wt.%, and a MgO content of ≥2wt.%; Preferably, the particle size of the water-quenched titanium slag is 20 mesh to 160 mesh.

3. The method for preparing boiling chlorination raw material from titanium slag according to claim 1 or 2, characterized in that: In step S1, the pretreatment includes oxidative roasting; Preferably, the pretreatment time is 0.5h to 4h.

4. The method for preparing boiling chlorination raw material from titanium slag according to any one of claims 1 to 3, characterized in that: In step S1, the content of low-valent titanium in the pretreated titanium slag is ≤0.5wt.%.

5. The method for preparing boiling chlorination raw material from titanium slag according to any one of claims 1 to 4, characterized in that: In step S1, the method for preparing water-quenched titanium slag includes: mixing molten titanium slag with a water quenching liquid, and performing water quenching to obtain water-quenched titanium slag; Preferably, the water quenching pressure is 1 kg·f / cm 2 ~40kg·f / cm 2 .

6. The method for preparing boiling chlorination raw material from titanium slag according to any one of claims 1 to 5, characterized in that: In step S2, the pre-leaching treatment includes acid leaching a mixture of the pre-treated titanium slag and the first acid solution to obtain leached slag; Preferably, the prepreg treatment temperature is 20° C. to 100° C., and the prepreg treatment time is 20 min to 120 min.

7. The method for preparing boiling chlorination raw material from titanium slag according to claim 6, characterized in that: In step S2, the mass ratio of the first acid solution to the pretreated titanium slag is (0.5-2):1; Preferably, the mass concentration of the first acid solution is 5% to 30%.

8. The method for preparing boiling chlorination raw material from titanium slag according to claim 6, characterized in that: In step S2, the acid leaching treatment includes pressurizing the mixture of the leached residue and the second acid solution to acid leach.

9. The method for preparing boiling chlorination raw material from titanium slag according to claim 8, characterized in that: In step S2, the temperature of the acid leaching treatment is 130°C to 175°C, and the time of the acid leaching treatment is 0.5h to 6h; Preferably, the pressure of the acid leaching treatment is 0.2 MPa to 0.9 MPa.

10. The method for preparing boiling chlorination raw material from titanium slag according to claim 8, characterized in that: In step S2, the mass ratio of the second acid solution to the leached residue is (1-5):1; Preferably, the mass concentration of the second acid solution is 13% to 30%.

11. The method for preparing boiling chlorination raw material from titanium slag according to claim 10, characterized in that: In step S2, the first acid solution and the second acid solution independently include at least one of hydrochloric acid, nitric acid, acetic acid, sulfuric acid and hydrofluoric acid.

12. A boiling chlorination raw material, characterized in that: The boiling chlorination raw material is prepared by the method according to any one of claims 1-11.

13. The chlorinated raw material according to claim 12, characterized in that The fine powder rate of the boiling chlorination raw material is ≤5%.

14. The chlorinated raw material according to claim 12 or 13, characterized in that In the boiling chlorination raw material, the TiO2 content is ≥85wt.%, the CaO content is ≤0.1wt.%, and the total content of CaO and MgO is ≤1.5wt.%; Optionally, the TiO2 content in the boiling chlorination raw material is ≥90wt.%.

Citation Information

Patent Citations

  • Method for preparing artificial rutile by titanium slags

    CN102745743A

  • Method for preparing titanium-rich material from Panxi titanium concentrate

    CN111534706A

  • Preparation method of titanium-rich material and preparation method of titanium tetrachloride

    CN113862494A

  • Method for reducing content of calcium oxide in titanium slag and titanium dioxide

    CN113957271A

  • Method for preparing boiling chlorination furnace burden by upgrading titanium slag

    CN114752772A

Cited By

  • Method for enhancing impurity removal of high-calcium-magnesium titanium slag

    CN119753368A

  • Melt separation titanium slag modification treatment method and system

    CN121380608A