Preparation method for active layer, narrow-band near-infrared photodiode and preparation method therefor

The bulk heterojunction active layer is prepared by the liquid surface molecular self-assembly method, which solves the problem of poor interface quality between the active layer and the functional layer in photodiodes, improves carrier transmission and photocurrent, and improves the performance of narrow-band near-infrared photodiodes. performance.

WO2024198351A1PCT designated stage expired Publication Date: 2024-10-03PEKING UNIV SHENZHEN GRADUATE SCHOOL

Patent Information

Application Number
PCT/CN2023/128851
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2023-10-31
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

In the existing photodiode preparation methods, the interface quality between the active layer and the functional layer is poor, which leads to obstruction of carrier transmission, increases dark current, reduces photocurrent, and affects device performance.

Method used

The bulk heterojunction active layer is prepared using the liquid surface molecular self-assembly method. A thin film is formed through self-assembly on the water surface, and then transferred to the substrate to be prepared for the active layer and annealed to ensure interface quality and thin film uniformity.

Benefits of technology

It achieves high-quality active layer preparation, improves carrier transport, reduces dark current density, and improves the performance and detection of narrow-band near-infrared photodiodes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023128851_03102024_PF_FP_ABST
    Figure CN2023128851_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present invention are a preparation method for an active layer, a narrow-band near-infrared photodiode and a preparation method therefor. The preparation method for an active layer comprises the steps of: adding a donor material and an acceptor material into a first solvent immiscible with water to form a first mixed solution, the boiling point of the first solvent being less than or equal to 180℃; and applying the first mixed solution to a first water surface for liquid surface molecular self-assembly, transferring a formed first thin film to a substrate on which an active layer is to be prepared, and performing first annealing to obtain a bulk heterojunction active layer. The present invention uses the liquid surface molecular self-assembly method to prepare the high-quality active layer. The first mixed solution is applied to the first water surface, and the first mixed solution diffuses around on the first water surface because of surface tension; simultaneously, the first solvent volatilizes; and when the diffusion and volatilization are both completed, self-assembly is finished so as to form the first thin film. In the present invention, the active layer prepared by means of the liquid surface molecular self-assembly method has good crystallinity and high quality, and will not damage the substrate on which the active layer is to be prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Active layer preparation method, narrow-band near-infrared photodiode and preparation method thereof Technical Field

[0001] The present invention relates to the technical field of photodiodes, and in particular to a method for preparing an active layer, a narrow-band near-infrared photodiode and a preparation method thereof. Background Art

[0002] Optoelectronic devices require an active layer to be fabricated on top of some functional layer. The quality of the active layer and its interface is crucial. Defects can trap carriers, increasing dark current and reducing photocurrent, thereby affecting device performance (e.g., the detectivity of a photodetector). Currently, the most common method for preparing active layers is the orthogonal solvent method. When preparing the active layer on a functional layer (e.g., a filter layer), a solvent orthogonal to the functional layer is selected. Common orthogonal solvent combinations include chlorobenzene and chloroform. However, the orthogonal solvent method does not mean that the functional layer will be completely insoluble in the active layer solvent. Dissolution will still occur to varying degrees at the interface, increasing surface roughness and creating a high density of defect sites, hindering carrier transport. Furthermore, this method is not universally applicable; not all active layer-functional layer combinations can be matched with a suitable orthogonal solvent. Some researchers have proposed adding a crosslinker to the functional layer (e.g., the filter layer) for further protection, building on the orthogonal solvent method. However, the additional insulating crosslinker can reduce carrier transport within the functional layer (e.g., the filter layer), affecting its mobility.

[0003] Therefore, the existing technology still needs to be improved and developed.

[0004] Summary of the Invention

[0005] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a method for preparing an active layer, a narrow-band near-infrared photodiode and a method for preparing the same, aiming to solve the problems of poor quality of the active layer prepared by the existing preparation method and poor interface quality between the prepared active layer and the functional layer.

[0006] The technical solutions of the present invention are as follows:

[0007] A first aspect of the present invention provides a method for preparing a bulk heterojunction active layer, comprising the steps of:

[0008] Providing a donor material, an acceptor material, a first solvent immiscible with water, a first water surface, and a substrate on which an active layer is to be prepared, wherein the boiling point of the first solvent immiscible with water is less than or equal to 180° C.;

[0009] adding the donor material and the acceptor material into a first solvent immiscible with water to form a first mixed solution;

[0010] applying the first mixed liquid onto the first water surface to perform surface molecular self-assembly to form a first thin film;

[0011] The first film is transferred onto the substrate on which the active layer is to be prepared, and is subjected to a first annealing to obtain the bulk heterojunction active layer.

[0012] A second aspect of the present invention provides a method for preparing a narrow-band near-infrared photodiode, comprising the steps of:

[0013] providing a substrate;

[0014] forming a hole transport layer on the substrate;

[0015] forming a filter layer on the hole transport layer;

[0016] forming an intermediate layer on the filter layer;

[0017] Adopting the preparation method of the present invention as described above, forming a bulk heterojunction active layer on the intermediate layer;

[0018] A top electrode is formed on the bulk heterojunction active layer.

[0019] A third aspect of the present invention provides a narrow-band near-infrared photodiode, which is prepared using the preparation method of the present invention as described above.

[0020] Beneficial Effects: The present invention utilizes a liquid surface molecular self-assembly method to prepare a high-quality active layer. The first mixed liquid is applied to the first water surface. Due to surface tension, the first mixed liquid diffuses in all directions on the first water surface, while the first solvent evaporates. When both diffusion and volatilization are complete, self-assembly ends, resulting in a first thin film. The first thin film is then transferred to the substrate on which the active layer is to be prepared. After a first annealing step, the bulk heterojunction active layer is obtained. The present invention utilizes a liquid surface molecular self-assembly method to prepare an active layer. The prepared thin film is of high quality, good uniformity, and good crystallinity. The phase distribution of the bulk heterojunction system is more uniform, and the substrate on which the active layer is to be prepared is not damaged. The interface between the two is of good quality. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] FIG1a is a schematic diagram of a liquid surface molecular self-assembly method according to an embodiment of the present invention, and FIG1b is a physical picture of a thin film prepared by the method described in FIG1a and transferred onto quartz.

[0022] FIG2 is a schematic structural diagram of a narrow-band near-infrared photodiode prepared in an embodiment of the present invention.

[0023] FIG3 is a current-voltage characteristic curve of the narrow-band near-infrared photodiode prepared in Example 2 of the present invention under irradiation of 600 nm, 760 nm, and 900 nm light, respectively.

[0024] FIG4 is a spectrum showing the variation of external quantum efficiency of the narrow-band near-infrared photodiode prepared in Example 2 of the present invention with the wavelength of incident light at bias voltages of 0V, -1.5V, -3V, and -5V.

[0025] FIG5 is a spectrum showing the variation of the responsivity of the narrow-band near-infrared photodiode prepared in Example 2 of the present invention with the wavelength of the incident light at a bias voltage of -3V to -5V.

[0026] FIG6 is a spectrum showing the variation of the specific detectivity of the narrow-band near-infrared photodiode prepared in Example 2 of the present invention with the wavelength of the incident light at bias voltages of 0V, -1.5V, -3V, and -5V.

[0027] FIG7 is a linear dynamic range diagram of the narrow-band near-infrared photodiode prepared in Example 2 of the present invention.

[0028] FIG8 is a noise spectrum of the narrow-band near-infrared photodiode prepared in Example 2 of the present invention under a bias voltage of -5V.

[0029] FIG9 is a time response curve diagram of the narrow-band near-infrared photodiode prepared in Example 2 of the present invention under a bias voltage of -5V.

[0030] FIG10 is an image of the letters “PKU” formed by integrating the narrow-band near-infrared photodiode array prepared in Example 2 of the present invention onto a thin-film transistor backplane.

[0031] In Figure 11, (a) is a spectrum of the normalized external quantum efficiency of the narrow-band near-infrared photodiodes prepared in Examples 1 and 2 of the present invention as a function of the wavelength of the incident light, (b) is a spectrum of the normalized external quantum efficiency of the narrow-band near-infrared photodiodes prepared in Examples 3 and 6 of the present invention as a function of the wavelength of the incident light, and (c) is a spectrum of the normalized external quantum efficiency of the narrow-band near-infrared photodiodes prepared in Examples 4 and 5 of the present invention as a function of the wavelength of the incident light. DETAILED DESCRIPTION

[0032] The present invention provides a method for preparing an active layer, a narrow-band near-infrared photodiode, and a method for preparing the same. To clarify the objectives, technical solutions, and effects of the present invention, the present invention is described in further detail below. It should be understood that the specific embodiments described herein are intended only to illustrate the present invention and are not intended to limit the present invention.

[0033] Unless otherwise defined, all technical terms and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0034] An embodiment of the present invention provides a method for preparing a bulk heterojunction active layer, which includes the following steps:

[0035] S11, providing a donor material, an acceptor material, a first solvent immiscible with water, a first water surface, and a substrate on which an active layer is to be prepared, wherein the boiling point of the first solvent immiscible with water is less than or equal to 180° C.;

[0036] S12, adding the donor material and the acceptor material into a first solvent immiscible with water to form a first mixed solution;

[0037] S13, applying the first mixed liquid onto the first water surface to perform surface molecular self-assembly to form a first thin film;

[0038] S14, transferring the first thin film onto the substrate on which the active layer is to be prepared, and performing a first annealing to obtain the bulk heterojunction active layer.

[0039] As shown in Figure 1a, the present invention utilizes a liquid surface molecular self-assembly method to prepare a high-quality active layer. The first mixed liquid is applied to the first water surface. Due to surface tension, the first mixed liquid diffuses in all directions on the first water surface. Simultaneously, the first solvent evaporates (the boiling point of the first solvent is less than or equal to 180°C and is volatile). When both diffusion and volatilization are complete, self-assembly ends, forming a first thin film. The first thin film is then transferred to the substrate on which the active layer is to be prepared. After a first annealing step, the bulk heterojunction active layer is obtained. The present invention utilizes a liquid surface molecular self-assembly method to prepare the active layer. The resulting thin film is high in quality, uniform, and crystalline. The phase distribution of the bulk heterojunction system is more uniform, and the substrate on which the active layer is to be prepared is not damaged. The interface between the two is of good quality. That is to say, the present invention first prepares a first thin film by a liquid surface molecular self-assembly method, and then transfers the first thin film to the substrate of the active layer to be prepared, which will not have a bad impact on the substrate of the active layer to be prepared and the interface between the two. It effectively solves the problem of the prior art that the substrate of the active layer to be prepared (such as the filter layer, etc.) is dissolved to varying degrees by an orthogonal solvent method, thereby increasing the surface roughness, generating high-density defect sites, and hindering carrier transmission.

[0040] In step S11, in some embodiments, the substrate for preparing the active layer includes a photoelectric device for preparing the active layer, such as a photodiode for preparing the passive layer. When the substrate for preparing the active layer is quartz, the actual image of the active layer on its surface is shown in Figure 1b.

[0041] In step S12, in some embodiments, the total concentration of the donor material and the acceptor material in the first mixed solution is 20-30 mg·mL -1, for example, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29 or 30 mg·mL -1 wait.

[0042] In some embodiments, in the first mixed solution, the mass ratio of the donor material to the acceptor material is 1:0.8-1:1.2, for example, 1:0.8, 1:0.9, 1:1, 1:1.1 or 1:1.2.

[0043] In some embodiments, the donor material includes but is not limited to 3-hexylthiophene (P3HT), poly{[4,8-bis[(2-ethylhexyl)oxy]-benzo[1,2-B:4,5-B']dithiophene-2,6-diyl][3-fluoro-2-[(2-ethylhexyl)carbonyl]thiophene[3,4-B]thiophene} (PTB7), poly[(2,6-(4,8-bis(5-(2-ethylhexyl-3-fluoro)thiophene-2-yl)-benzo[1,2-B:4,5-B']dithiophene])-ALT-(5,5-(1',3'-di-2-thiophene-5',7'-bis(2-ethylhexyl)benzo[1',2'-C:4 ',5'-C']dithiophene-4,8-dione) (PM6), diketopyrrolopyrrole (DPP), polydithiophene diketopyrrolopyrrole-thiophene (PDPPBTT), poly {2,2'-[(2,5-bis(2-octyldodecyl)-3,6-dioxo-2,3,5,6-tetrahydropyrrolo[3,4-c]pyrrole-1,4-diyl)]dithiophene-5,5'-diyl salt thieno[3,2-b]thiophene-2,5-diyl} (PDBT-co-TT), poly (2,5-bis(3-tetradecylthiophene-2-yl)thieno[3,2-b]thiophene) (PBTTT-C14), but is not limited thereto.

[0044] The acceptor material includes but is not limited to 12,13-bis(2-ethylhexyl)-3,9-diundecyl-12,13-dihydro-[1,2,5]thiadiazolo[3,4-e]thieno[2",3":4',5']thieno[2',3':4,5]pyrrolo[3,2-g]thieno[2',3':4,5]thieno[3,2-b]indole-2,10-bis(5,6-difluoro- -3-(dicyanomethylene)indene-1-one)(Y6), 2,2'-[[[6,6,12,12-tetrakis(4-hexylphenyl)-6,12-dihydrodithio[2,3-D:2',3'-D']-S-indolol[1,2-B:5,6-B']dithiophene-2,8-diyl]bis[methylene(3-oxo-1H-indene-2,1(3H)-dimethylene)]]bis[propylamine]( ITIC), 3,9-bis(2-methylene-((3-(1,1-dicyanomethylene)-6,7-difluoro)-indanone))-5,5,11,11-tetrakis(4-hexylphenyl)-dithieno[2,3-D:2,3-D]-S-indacenyl[1,2-B:5,6-B]dithiophene (IT4F), 2,2'-((2Z,2'Z)-((5,5'-(4,4,9,9- Tetrakis(4-hexylphenyl)-4,9-dihydro-S-benzodiindeno[1,2-B:5,6-B']dithiophene-2,7-diyl)bis(4-((2-ethylhexyl)oxy)thiophene-5,2-diyl))bis(methylenediyl))bis(5,6-difluoro-3-oxo-2,3-dihydro-1H-indene-2,1-diylidene))dimalononitrile (IEICO) at least one, but not limited thereto.

[0045] In some embodiments, the first solvent that is immiscible with water includes, but is not limited to, at least one of chlorobenzene, chloroform, and dichloromethane, but is not limited thereto.

[0046] In step S13, the area of ​​the first water surface is larger than the area of ​​the formed first thin film. The first water surface can be formed by adding water to an open container, and the first water surface is a horizontal liquid surface. In some embodiments, the amount of the first mixed solution applied is 10-20 μL. For example, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, or 20 μL of the first mixed solution is applied.

[0047] In step S14, in some embodiments, the atmosphere of the first annealing is an inert gas atmosphere (e.g., a nitrogen atmosphere), the temperature of the first annealing is 80-120° C., for example, 80, 90, 100, 110, or 120° C., etc.; the time of the first annealing is 5-20 min, for example, 5, 6, 7, 8, 9, 10, 12, 15, 18, or 20 min, etc.

[0048] Organic narrowband detection is mainly based on three mechanisms: charge collecting narrowing (CCN), charge injection narrowing (CIN) and exciton dissociation narrowing (EDN). Among them, in the localized Frenkel exciton dissociation device, short-wavelength light is absorbed by the thick filter layer and produces Frenkel excitons, but because the exciton transmission distance in the organic material is only 10-20nm, it cannot reach the donor / acceptor (D / A) interface, so no photocurrent contribution is generated. For long-wavelength light, it may not be absorbed, penetrate the filter layer to reach the active layer, and be absorbed in the active layer to produce Frenkel excitons and dissociate. For the localized Frenkel exciton dissociation device, it is necessary to prepare an active layer on the filter layer, which is a severe challenge for all-solution devices. In a device, the quality of the filter layer, active layer, and their interfaces is crucial. If defects trap carriers, dark current will increase and photocurrent will decrease, thereby reducing device performance (such as detection). Based on this, an embodiment of the present invention also provides a method for preparing a narrow-band near-infrared photodiode, as shown in Figure 2, which includes the following steps:

[0049] S21, providing a substrate 1;

[0050] S22, forming a hole transport layer 2 on the substrate 1;

[0051] S23, forming a filter layer 3 on the hole transport layer 2;

[0052] S24, forming an intermediate layer 4 on the filter layer 3;

[0053] S25, forming a bulk heterojunction active layer 5 on the intermediate layer 4 using the preparation method described above in the embodiment of the present invention;

[0054] S26 , forming a top electrode 6 on the bulk heterojunction active layer 5 .

[0055] The embodiment of the present invention adopts the liquid molecular self-assembly method to prepare the active layer to obtain a high-quality thin film. Moreover, since the thin film is formed first and then transferred to the intermediate layer, it will not affect the filter layer and the intermediate layer. It has a good interface, which provides an important guarantee for higher carrier mobility and charge transfer efficiency, and improves the performance of the narrow-band near-infrared photodiode. At the same time, the provision of the intermediate layer can reduce the surface roughness, improve the interface between the filter layer and the photosensitive layer, and thus promote charge transfer at the interface. The self-powered photodiode provided by the embodiment of the present invention can operate at a high bias voltage of -5V, and the dark current density is only 2.7nA·cm -2, the peak wavelength is 760nm, the half-peak width is 60nm, and the peak responsivity is 0.294A·W -1 , the detection ratio can reach 1×10 13 Jones, with excellent typical narrowband detector performance. The narrowband near-infrared photodiode provided in this embodiment (i.e., exciton dissociation narrowband organic near-infrared photodetector) has wide applications in artificial intelligence, fiber optic communications, biological monitoring and other fields.

[0056] As shown in FIG2 , the narrow-band near-infrared photodiode prepared by the preparation method of an embodiment of the present invention includes a substrate 1, a hole transport layer 2, a filter layer 3, an intermediate layer 4, a bulk heterojunction active layer 5 and a top electrode 6 stacked in sequence.

[0057] In step S21, the substrate includes but is not limited to indium tin oxide (ITO) glass.

[0058] In step S22, in some embodiments, the step of forming a hole transport layer on the substrate specifically includes:

[0059] S221, providing a hole transport material;

[0060] S222, adding the hole transport material to a third solvent to obtain a third mixed solution;

[0061] S223 , applying the third mixed solution to the substrate and performing a first spin coating, and then performing a third annealing to form a hole transport layer on the substrate.

[0062] In step S222, in some embodiments, the mass concentration of the hole transport material in the third mixed solution is 1-3 wt%, for example, 1, 1.5, 2, 2.5 or 3 wt%.

[0063] In some embodiments, the third mixed solution is applied in an amount of 20-50 μL per square centimeter of substrate, for example, 20, 30, 40, or 50 μL per square centimeter of substrate.

[0064] In some embodiments, the hole transport material includes at least one of nickel oxide, poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid) (PEDOT:PSS), and 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene (Spiro-OMeTAD), but is not limited thereto.

[0065] In some embodiments, the third solvent includes at least one of water, ethanol, and chlorobenzene, but is not limited thereto.

[0066] In step S223, in some embodiments, the rotation speed of the first spin coating is 2000-5000 rpm; for example, it can be 2000, 2500, 3000, 3500, 4000, 4500 or 5000 rpm, etc.; the time of the first spin coating is 20-50s, for example, it can be 20, 30, 40 or 50s, etc.

[0067] In some embodiments, the atmosphere of the third annealing is an air atmosphere, and the temperature of the third annealing is 100-200°C; for example, it can be 100, 110, 120, 130, 140, 150, 160, 170, 180, 190 or 200°C; the time of the third annealing is 10-30 minutes, for example, it can be 10, 15, 20, 25 or 30 minutes, etc.

[0068] In step S23, in some embodiments, the step of forming a filter layer on the hole transport layer specifically includes:

[0069] S231, providing filter material;

[0070] S232, adding the filter material to a fourth solvent to obtain a fourth mixed solution;

[0071] S233 , applying the fourth mixed solution to the hole transport layer and performing a second spin coating, and then performing a fourth annealing to form a filter layer on the hole transport layer.

[0072] In steps S231-S232, in some embodiments, the filter material includes but is not limited to 3-hexylthiophene (P3HT), poly{[4,8-bis[(2-ethylhexyl)oxy]-benzo[1,2-B:4,5-B']dithiophene-2,6-diyl][3-fluoro-2-[(2-ethylhexyl)carbonyl]thiophene[3,4-B]thiophene}(PTB7), poly[(2,6-(4,8-bis(5-(2-ethylhexyl-3-fluoro)thiophene-2-yl)-benzo[1,2-B:4,5-B']dithiophene])-ALT-(5,5-(1',3'-di-2-thiophene-5',7'-bis(2-ethylhexyl)benzo[ At least one of poly{2,2'-[(2,5-bis(2-octyldodecyl)-3,6-dioxo-2,3,5,6-tetrahydropyrrolo[3,4-c]pyrrole-1,4-diyl)]dithiophene-5,5'-diyl salt thieno[3,2-b]thiophene-2,5-diyl} (PDBT-co-TT), and poly(2,5-bis(3-tetradecylthiophene-2-yl)thieno[3,2-b]thiophene) (PBTTT-C14).

[0073] In some embodiments, the fourth solvent includes at least one of chlorobenzene, chloroform, and dichloromethane, but is not limited thereto.

[0074] In some embodiments, the concentration of the filter material in the fourth mixture is 60-100 mg·mL -1 , for example, 60, 70, 80, 90 or 100 mg·mL -1 wait.

[0075] In some embodiments, the fourth mixed solution is applied in an amount of 20-50 μL per square centimeter of the hole transport layer, for example, 20, 30, 40, or 50 μL per square centimeter of the hole transport layer.

[0076] S233. In some embodiments, the rotation speed of the second spin coating is 1000-5000 rpm, for example, it can be 1000, 2000, 3000, 4000 or 5000 rpm; the time of the second spin coating is 20-50s, for example, it can be 20, 30, 40 or 50s.

[0077] In some embodiments, the atmosphere of the fourth annealing is an inert gas atmosphere (e.g., nitrogen), the temperature of the fourth annealing is 120-180° C., for example, 120, 130, 140, 150, 160, 170, or 180° C.; the time of the fourth annealing is 15-60 min, for example, 15, 20, 25, 30, 35, 40, 45, 50, 55, or 60 min, etc.

[0078] In step S24, in some embodiments, the step of forming an intermediate layer on the filter layer specifically includes:

[0079] S241, providing an intermediate layer material, a second solvent immiscible with water, and a second water surface, wherein the boiling point of the second solvent immiscible with water is less than or equal to 180° C.;

[0080] S242, adding the intermediate layer material to a second solvent immiscible with water to obtain a second mixed solution;

[0081] S243, applying the second mixed liquid onto the second water surface to perform surface molecular self-assembly to form a second thin film;

[0082] S244, transferring the second film onto the filter layer, and performing a second annealing to obtain the intermediate layer.

[0083] This embodiment uses surface molecular self-assembly to form the intermediate layer. The second mixed liquid is applied to the second water surface. Due to surface tension, the second mixed liquid diffuses outward on the second water surface while the second solvent evaporates (the boiling point of the second solvent is less than or equal to 180°C and is highly volatile). When both diffusion and volatilization are complete, self-assembly concludes, forming a second thin film. The second thin film is then transferred to the filter layer and subjected to a second annealing step to obtain the intermediate layer. This invention utilizes surface molecular self-assembly to prepare the intermediate layer without damaging the filter layer, and the resulting thin film exhibits excellent uniformity and crystallinity.

[0084] In steps S241-S242, in some embodiments, the intermediate layer material includes 3-hexylthiophene (P3HT), poly{[4,8-bis[(2-ethylhexyl)oxy]-benzo[1,2-B:4,5-B']dithiophene-2,6-diyl][3-fluoro-2-[(2-ethylhexyl)carbonyl]thiophene[3,4-B]thiophene}(PTB7), poly[(2,6-(4,8-bis(5-(2-ethylhexyl-3-fluoro)thiophene-2-yl)-benzo[1,2-B:4,5-B']dithiophene])-ALT-(5,5-(1',3'-di-2-thiophene-5',7'-bis(2-ethylhexyl)benzo[1',2 '-C:4',5'-C']dithiophene-4,8-dione) (PM6), dione pyrrolopyrrole (DPP), polydithiophene dione pyrrolopyrrole-thiophene (PDPPBTT), poly {2,2'-[(2,5-bis(2-octyldodecyl)-3,6-dioxo-2,3,5,6-tetrahydropyrrolo[3,4-c]pyrrole-1,4-diyl)]dithiophene-5,5'-diyl salt thieno[3,2-b]thiophene-2,5-diyl} (PDBT-co-TT), poly (2,5-bis(3-tetradecylthiophene-2-yl)thieno[3,2-b]thiophene) (PBTTT-C14), but is not limited thereto.

[0085] In some embodiments, the second solvent immiscible with water includes at least one of chlorobenzene, chloroform, and dichloromethane, but is not limited thereto.

[0086] In some embodiments, the concentration of the intermediate layer material in the second mixed solution is 5-15 mg·mL -1 , for example, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14 or 15 mg·mL -1 wait.

[0087] In step S243, the area of ​​the second water surface is larger than the formed second thin film, and the second water surface can be formed by adding water into an open container. Furthermore, the second water surface is a horizontal liquid level.

[0088] In some embodiments, the amount of the second mixed solution applied is 5-15 μL, for example, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14 or 15 μL of the second mixed solution is applied.

[0089] In step S244, in some embodiments, the atmosphere of the second annealing is an inert gas atmosphere (e.g., nitrogen), the temperature of the second annealing is 80-120°C, for example, 80, 90, 100, 110, or 120°C, etc.; the time of the second annealing is 5-20 minutes, for example, 5, 6, 7, 8, 9, 10, 12, 15, 18, or 20 minutes, etc.

[0090] In step S25 , the first thin film formed in step S13 in the above embodiment of the present invention is transferred onto the intermediate layer, and subjected to a first annealing to obtain the bulk heterojunction active layer.

[0091] The ratio and concentration of the donor material and the acceptor material in the first mixed solution are as described above, the amount of the first mixed solution applied is as described above, and the process of the first annealing is as described above, which will not be repeated here.

[0092] The present invention also provides a narrow-band near-infrared photodiode, which is prepared using the preparation method described above. The photodiode provided by the present invention can operate at a high bias voltage of -5V, and the dark current density is only 2.7nA·cm -2 , the peak wavelength is 760nm, the half-peak width is 60nm, and the peak responsivity is 0.294A·W -1 , the detection ratio can reach 1×10 13 Jones, with excellent typical narrowband detector performance.

[0093] The following describes it in detail through specific examples.

[0094] Example 1

[0095] This embodiment provides a method for preparing a narrow-band near-infrared photodiode, comprising the steps of:

[0096] (1) Preparation of hole transport layer by spin coating:

[0097] ITO glass (area 1.5 cm × 1.5 cm) was immersed in acetone and heated at 100 °C for 30 min, ultrasonically treated for 20 min, then ultrasonically treated with isopropyl alcohol and ultrapure water for 20 min in sequence, dried with a nitrogen gun, and treated with ozone UV for 15 min;

[0098] PEDOT:PSS was added to water to prepare a 1.5 wt% PEDOT:PSS aqueous solution;

[0099] 80 μL of PEDOT:PSS aqueous solution was dropped onto the treated ITO glass surface and spin-coated at 1000 rpm for 40 s, followed by annealing at 150 °C for 30 min in an air atmosphere to form a hole transport layer (area of ​​1.5 cm × 1.5 cm) on the ITO glass surface.

[0100] (2) Preparation of filter layer by spin coating:

[0101] P3HT and PTB7 were added to chlorobenzene at a mass ratio of 1:1 to prepare a concentration of 60 mg mL -1 a mixed solution;

[0102] 50 μL of the mixed solution was added dropwise to the hole transport layer prepared in step (1), and spin-coated at a speed of 4000 rpm for 35 s. The mixture was then annealed at 120° C. for 60 min under a nitrogen atmosphere to form a filter layer (with an area of ​​1.5 cm×1.5 cm) on the hole transport layer.

[0103] (3) Preparation of the intermediate layer by liquid surface molecular self-assembly method:

[0104] PBTTT-C14 was added to chlorobenzene to prepare a concentration of 10 mg mL -1 PBTTT-C14 solution;

[0105] 10 μL of PBTTT-C14 solution was dropped onto the second water surface to allow surface molecules to self-assemble. After the solvent evaporated, a second film was formed.

[0106] Use tweezers to clamp both sides of the substrate containing the hole transport layer and the filter layer, and make the filter layer face the second film, move the substrate downward, and when the filter layer is attached to the second film, lift the substrate (at this time the second film is transferred to the filter layer), blow dry with nitrogen, and then anneal at 100°C in a nitrogen atmosphere for 15 minutes to form an intermediate layer (area of ​​1.5cm×1.5cm) on the filter layer.

[0107] (4) Preparation of bulk heterojunction active layer by liquid surface molecular self-assembly method:

[0108] PM6 (donor material) and ITIC (acceptor material) were added to chlorobenzene at a mass ratio of 1:1 to obtain a total concentration of 30 mg mL -1 Bulk heterojunction solution (PM6 and ITIC concentrations were 15 mg mL -1 );

[0109] 20 μL of bulk heterojunction solution is dropped onto the first water surface to allow surface molecules to self-assemble. After the solvent evaporates, a first thin film is formed.

[0110] Use tweezers to clamp both sides of the substrate containing the hole transport layer, the filter layer and the intermediate layer, and make the intermediate layer face the first film, move the substrate downward, and when the intermediate layer is attached to the first film, lift the substrate (at this time the first film is transferred to the intermediate layer), blow dry with nitrogen, and then anneal at 100°C in a nitrogen atmosphere for 15 minutes to form a bulk heterojunction active layer (area of ​​1.5cm×1.5cm) on the intermediate layer.

[0111] (5) Preparation of top electrode by vacuum evaporation method:

[0112] A 150nm thick Al top electrode was deposited on the bulk heterojunction active layer by vacuum evaporation.

[0113] Example 2

[0114] This embodiment provides a method for preparing a narrow-band near-infrared photodiode, comprising the steps of:

[0115] (1) Preparation of hole transport layer by spin coating:

[0116] ITO glass (area 1.5 cm × 1.5 cm) was immersed in acetone and heated at 100 °C for 30 min, ultrasonically treated for 30 min, then ultrasonically treated with isopropyl alcohol and ultrapure water for 30 min in sequence, dried with a nitrogen gun, and treated with ozone UV for 15 min;

[0117] PEDOT:PSS was added to water to prepare a 1.5 wt% PEDOT:PSS aqueous solution;

[0118] 80 μL of PEDOT:PSS aqueous solution was dropped onto the treated ITO glass surface, spin-coated at 4000 rpm for 40 seconds, and then annealed at 150°C for 30 minutes in an air atmosphere to form a hole transport layer (area of ​​1.5 cm×1.5 cm) on the ITO glass surface.

[0119] (2) Preparation of filter layer by spin coating:

[0120] P3HT and PTB7 were added to chlorobenzene at a mass ratio of 1:1 to prepare a total concentration of 60 mg mL -1 a mixed solution;

[0121] 50 μL of the mixed solution was added dropwise to the hole transport layer prepared in step (1), and spin-coated at a speed of 4000 rpm for 35 s. The mixture was then annealed at 120° C. for 60 min under a nitrogen atmosphere to form a filter layer (with an area of ​​1.5 cm×1.5 cm) on the hole transport layer.

[0122] (3) Preparation of the intermediate layer by liquid surface molecular self-assembly method:

[0123] PBTTT-C14 was added to chlorobenzene to prepare a concentration of 10 mg mL -1 PBTTT-C14 solution;

[0124] 10 μL of PBTTT-C14 solution was dropped onto the second water surface to allow surface molecules to self-assemble. After the solvent evaporated, a second film was formed.

[0125] The second film was transferred onto the filter layer prepared in step (2) (the detailed steps of the second film transfer were the same as those in Example 1), and annealed at 100°C for 15 minutes in a nitrogen atmosphere to form an intermediate layer (with an area of ​​1.5 cm × 1.5 cm) on the filter layer.

[0126] (4) Preparation of bulk heterojunction active layer by liquid surface molecular self-assembly method:

[0127] PM6 (donor material) and IT4F (acceptor material) were added to chlorobenzene at a mass ratio of 1:1 to obtain a total concentration of 30 mg mL -1 Bulk heterojunction solution (PM6 and IT4F concentrations were 15 mg mL -1 );

[0128] 20 μL of bulk heterojunction solution is dropped onto the first water surface to allow surface molecules to self-assemble. After the solvent evaporates, a first thin film is formed.

[0129] The first film was transferred to the intermediate layer prepared in step (3) (the detailed steps of the first film transfer were the same as those in Example 1), and annealed at 100°C for 15 minutes in a nitrogen atmosphere to form a bulk heterojunction active layer (area of ​​1.5 cm×1.5 cm) on the intermediate layer.

[0130] (5) Preparation of top electrode by vacuum evaporation method:

[0131] A 150nm thick Al top electrode was deposited on the bulk heterojunction active layer by vacuum evaporation.

[0132] Example 3

[0133] This embodiment provides a method for preparing a narrow-band near-infrared photodiode, comprising the steps of:

[0134] (1) Preparation of hole transport layer by spin coating:

[0135] ITO glass (area 1.5 cm × 1.5 cm) was immersed in acetone and heated at 100 °C for 30 min, ultrasonically treated for 30 min, then ultrasonically treated with isopropyl alcohol and ultrapure water for 30 min in sequence, dried with a nitrogen gun, and treated with ozone UV for 15 min;

[0136] PEDOT:PSS was added to water to prepare a 1.5 wt% PEDOT:PSS aqueous solution;

[0137] 80 μL of PEDOT:PSS aqueous solution was dropped onto the treated ITO glass surface, spin-coated at 4000 rpm for 40 seconds, and then annealed at 150°C for 30 minutes in an air atmosphere to form a hole transport layer (area of ​​1.5 cm×1.5 cm) on the ITO glass surface.

[0138] (2) Preparation of filter layer by spin coating:

[0139] P3HT, PTB7, and PDPPBTT were added to chlorobenzene at a mass ratio of 5:2:3 to prepare a total concentration of 80 mg mL -1 a mixed solution;

[0140] 50 μL of the mixed solution was added dropwise to the hole transport layer prepared in step (1), and spin-coated at a speed of 1000 rpm for 35 s. The mixture was then annealed at 120° C. for 60 min under a nitrogen atmosphere to form a filter layer (with an area of ​​1.5 cm×1.5 cm) on the hole transport layer.

[0141] (3) Preparation of the intermediate layer by liquid surface molecular self-assembly method:

[0142] PBTTT-C14 was added to chlorobenzene to prepare a concentration of 10 mg mL -1 PBTTT-C14 solution;

[0143] 10 μL of PBTTT-C14 solution was dropped onto the second water surface to allow surface molecules to self-assemble. After the solvent evaporated, a second film was formed.

[0144] The second film was transferred onto the filter layer prepared in step (2) (the detailed steps of the second film transfer were the same as those in Example 1), and annealed at 100°C for 15 minutes in a nitrogen atmosphere to form an intermediate layer (with an area of ​​1.5 cm × 1.5 cm) on the filter layer.

[0145] (4) Preparation of bulk heterojunction active layer by liquid surface molecular self-assembly method:

[0146] PM6 (donor material) and Y6 (acceptor material) were added to chlorobenzene at a mass ratio of 1:1 to obtain a total concentration of 30 mg mL -1 Bulk heterojunction solution (PM6 and Y6 concentrations were 15 mg mL -1 );

[0147] 20 μL of bulk heterojunction solution is dropped onto the first water surface to allow surface molecules to self-assemble. After the solvent evaporates, a first thin film is formed.

[0148] The first film was transferred to the intermediate layer prepared in step (3) (the detailed steps of the first film transfer were the same as those in Example 1), and annealed at 100°C for 15 minutes in a nitrogen atmosphere to form a bulk heterojunction active layer (area of ​​1.5 cm×1.5 cm) on the intermediate layer.

[0149] (5) Preparation of top electrode by vacuum evaporation method:

[0150] A 150nm thick Al top electrode was deposited on the bulk heterojunction active layer by vacuum evaporation.

[0151] Example 4

[0152] This embodiment provides a method for preparing a narrow-band near-infrared photodiode, comprising the steps of:

[0153] (1) Preparation of hole transport layer by spin coating:

[0154] ITO glass (area 1.5 cm × 1.5 cm) was immersed in acetone and heated at 100 °C for 30 min, ultrasonically treated for 30 min, then ultrasonically treated with isopropyl alcohol and ultrapure water for 30 min in sequence, dried with a nitrogen gun, and treated with ozone UV for 15 min;

[0155] PEDOT:PSS was added to water to prepare a 1.5 wt% PEDOT:PSS aqueous solution;

[0156] 80 μL of PEDOT:PSS aqueous solution was dropped onto the treated ITO glass surface, spin-coated at 4000 rpm for 40 seconds, and then annealed at 150°C for 30 minutes in an air atmosphere to form a hole transport layer (area of ​​1.5 cm×1.5 cm) on the ITO glass surface.

[0157] (2) Preparation of filter layer by spin coating:

[0158] P3HT, PTB7, and PDBT-co-TT were added to chlorobenzene at a mass ratio of 3:2:5 to prepare a total concentration of 60 mg mL -1 a mixed solution;

[0159] 50 μL of the mixed solution was added dropwise to the hole transport layer prepared in step (1), and spin-coated at a speed of 1000 rpm for 35 s. The mixture was then annealed at 120° C. for 60 min under a nitrogen atmosphere to form a filter layer (with an area of ​​1.5 cm×1.5 cm) on the hole transport layer.

[0160] (3) Preparation of the intermediate layer by liquid surface molecular self-assembly method:

[0161] PBTTT-C14 was added to chlorobenzene to prepare a concentration of 10 mg mL -1 PBTTT-C14 solution;

[0162] 10 μL of PBTTT-C14 solution was dropped onto the second water surface to allow surface molecules to self-assemble. After the solvent evaporated, a second film was formed.

[0163] The second film was transferred onto the filter layer prepared in step (2) (the detailed steps of the second film transfer were the same as those in Example 1), and annealed at 100°C for 15 minutes in a nitrogen atmosphere to form an intermediate layer (with an area of ​​1.5 cm × 1.5 cm) on the filter layer.

[0164] (4) Preparation of bulk heterojunction active layer by liquid surface molecular self-assembly method:

[0165] PM6 (donor material) and Y6 (acceptor material) were added to chlorobenzene at a mass ratio of 1:1 to obtain a total concentration of 30 mg mL -1 Bulk heterojunction solution (PM6 and Y6 concentrations were 15 mg mL -1 );

[0166] 20 μL of bulk heterojunction solution is dropped onto the first water surface to allow surface molecules to self-assemble. After the solvent evaporates, a first thin film is formed.

[0167] The first film was transferred to the intermediate layer prepared in step (3) (the detailed steps of the first film transfer were the same as those in Example 1), and annealed at 100°C for 15 minutes in a nitrogen atmosphere to form a bulk heterojunction active layer (area of ​​1.5 cm×1.5 cm) on the intermediate layer.

[0168] (5) Preparation of top electrode by vacuum evaporation method:

[0169] A 150nm thick Al top electrode was deposited on the bulk heterojunction active layer by vacuum evaporation.

[0170] Example 5

[0171] This embodiment provides a method for preparing a narrow-band near-infrared photodiode, comprising the steps of:

[0172] (1) Preparation of hole transport layer by spin coating:

[0173] ITO glass (area 1.5 cm × 1.5 cm) was immersed in acetone and heated at 100 °C for 30 min, ultrasonically treated for 30 min, then ultrasonically treated with isopropyl alcohol and ultrapure water for 30 min in sequence, dried with a nitrogen gun, and treated with ozone UV for 15 min;

[0174] PEDOT:PSS was added to water to prepare a 1.5 wt% PEDOT:PSS aqueous solution;

[0175] 80 μL of PEDOT:PSS aqueous solution was dropped onto the treated ITO glass surface, spin-coated at 4000 rpm for 40 seconds, and then annealed at 150°C for 30 minutes in an air atmosphere to form a hole transport layer (area of ​​1.5 cm×1.5 cm) on the ITO glass surface.

[0176] (2) Preparation of filter layer by spin coating:

[0177] P3HT, PTB7, and PDBT-co-TT were added to chlorobenzene at a mass ratio of 3:2:5 to prepare a total concentration of 60 mg mL -1 a mixed solution;

[0178] 50 μL of the mixed solution was added dropwise to the hole transport layer prepared in step (1), and spin-coated at a speed of 1000 rpm for 35 s. The mixture was then annealed at 120° C. for 60 min under a nitrogen atmosphere to form a filter layer (with an area of ​​1.5 cm×1.5 cm) on the hole transport layer.

[0179] (3) Preparation of the intermediate layer by liquid surface molecular self-assembly method:

[0180] PBTTT-C14 was added to chlorobenzene to prepare a concentration of 10 mg mL -1 PBTTT-C14 solution;

[0181] 10 μL of PBTTT-C14 solution was dropped onto the second water surface to allow surface molecules to self-assemble. After the solvent evaporated, a second film was formed.

[0182] The second film was transferred onto the filter layer prepared in step (2) (the detailed steps of the second film transfer were the same as those in Example 1), and annealed at 100°C for 15 minutes in a nitrogen atmosphere to form an intermediate layer (with an area of ​​1.5 cm × 1.5 cm) on the filter layer.

[0183] (4) Preparation of bulk heterojunction active layer by liquid surface molecular self-assembly method:

[0184] PM6 (donor material) and IEICO (acceptor material) were added to chlorobenzene at a mass ratio of 1:1 to obtain a total concentration of 30 mg mL -1 Bulk heterojunction solution (PM6 and IEICO concentrations were both 15 mg mL -1 );

[0185] 20 μL of bulk heterojunction solution is dropped onto the first water surface to allow surface molecules to self-assemble. After the solvent evaporates, a first thin film is formed.

[0186] The first film was transferred onto the intermediate layer prepared in step (3) (the detailed steps of the first film transfer were the same as those in Example 1), and liquid surface molecular self-assembly was performed. After the solvent evaporated, the film was annealed at 100°C for 15 minutes in a nitrogen atmosphere to form a bulk heterojunction active layer (with an area of ​​1.5 cm × 1.5 cm) on the intermediate layer.

[0187] (5) Preparation of top electrode by vacuum evaporation method:

[0188] A 150nm thick Al top electrode was deposited on the bulk heterojunction active layer by vacuum evaporation.

[0189] Example 6

[0190] This embodiment provides a method for preparing a narrow-band near-infrared photodiode, comprising the steps of:

[0191] (1) Preparation of hole transport layer by spin coating:

[0192] ITO glass (area 1.5 cm × 1.5 cm) was immersed in acetone and heated at 100 °C for 30 min, ultrasonically treated for 30 min, then ultrasonically treated with isopropyl alcohol and ultrapure water for 30 min in sequence, dried with a nitrogen gun, and treated with ozone UV for 15 min;

[0193] PEDOT:PSS was added to water to prepare a 1.5 wt% PEDOT:PSS aqueous solution;

[0194] 80 μL of PEDOT:PSS aqueous solution was dropped onto the treated ITO glass surface, spin-coated at 4000 rpm for 40 seconds, and then annealed at 150°C for 30 minutes in an air atmosphere to form a hole transport layer (area of ​​1.5 cm×1.5 cm) on the ITO glass surface.

[0195] (2) Preparation of filter layer by spin coating:

[0196] PTB7 and PDPPBTT were added to chlorobenzene at a mass ratio of 1:1 to prepare a total concentration of 60 mg mL -1 a mixed solution;

[0197] 50 μL of the mixed solution was added dropwise to the hole transport layer prepared in step (1), and spin-coated at a speed of 1000 rpm for 35 s. The mixture was then annealed at 120° C. for 60 min under a nitrogen atmosphere to form a filter layer (with an area of ​​1.5 cm×1.5 cm) on the hole transport layer.

[0198] (3) Preparation of the intermediate layer by liquid surface molecular self-assembly method:

[0199] PBTTT-C14 was added to chlorobenzene to prepare a concentration of 10 mg mL -1 PBTTT-C14 solution;

[0200] 10 μL of PBTTT-C14 solution was dropped onto the second water surface to allow surface molecules to self-assemble. After the solvent evaporated, a second film was formed.

[0201] The second film was transferred onto the filter layer prepared in step (2) (the detailed steps of the second film transfer were the same as those in Example 1), and annealed at 100°C for 15 minutes in a nitrogen atmosphere to form an intermediate layer (with an area of ​​1.5 cm × 1.5 cm) on the filter layer.

[0202] (4) Preparation of bulk heterojunction active layer by liquid surface molecular self-assembly method:

[0203] PDBT-co-TT (donor material) and ITIC (acceptor material) were added to chlorobenzene at a mass ratio of 1:1 to obtain a total concentration of 30 mg mL -1 The bulk heterojunction solution (the concentrations of PDBT-co-TT and ITIC were both 15 mg mL -1 );

[0204] 20 μL of bulk heterojunction solution is dropped onto the first water surface to allow surface molecules to self-assemble. After the solvent evaporates, a first thin film is formed.

[0205] The first film was transferred to the intermediate layer prepared in step (3) (the detailed steps of the first film transfer were the same as those in Example 1), and annealed at 100°C for 15 minutes in a nitrogen atmosphere to form a bulk heterojunction active layer (area of ​​1.5 cm×1.5 cm) on the intermediate layer.

[0206] (5) Preparation of top electrode by vacuum evaporation method:

[0207] A 150nm thick Al top electrode was deposited on the bulk heterojunction active layer by vacuum evaporation.

[0208] test:

[0209] The current-voltage characteristic curves of the narrow-band near-infrared photodiode prepared in Example 2 under 600nm, 760nm, and 900nm light irradiation are shown in Figure 3, where the solid line is the photocurrent and the dotted line is the dark current. It can be seen from Figure 3 that the narrow-band near-infrared photodiode provided in this example has a low dark current. The narrow-band near-infrared photodiode can operate at a bias voltage of -5V, and the dark current is only 2.7nA·cm -2, and has typical narrowband response performance.

[0210] Figure 4 shows the external quantum efficiency (EQE) spectra of the narrow-band near-infrared photodiode prepared in Example 2 as a function of incident light wavelength at bias voltages of 0V, -1.5V, -3V, and -5V. This demonstrates that the narrow-band near-infrared photodiode provided in this example exhibits typical narrowband response performance and an extremely high EQE. The peak wavelength of the narrow-band near-infrared photodiode at a bias voltage of -5V is 760nm, and the half-width at half maximum is 60nm.

[0211] The responsivity (R) of the narrow-band near-infrared photodiode prepared in Example 2 varies with the incident light wavelength under a bias voltage of -3V to -5V as shown in FIG5 . It can be seen that the narrow-band near-infrared photodiode provided in this example has typical narrow-band response performance and high responsivity. The peak responsivity at 760nm under a bias voltage of -5V reaches 0.294A·W. -1 .

[0212] The narrow-band near-infrared photodiode prepared in Example 2 has a specific detectivity (D*) spectrum varying with the wavelength of incident light at bias voltages of 0V, -1.5V, -3V, and -5V, as shown in FIG6 . It can be seen that the narrow-band near-infrared photodiode provided in this example has a typical narrow-band response performance and high detectivity. At a bias voltage of -5V, the specific detectivity at the peak of 760nm reaches 1×10 13 Jones.

[0213] The linear dynamic range (LDR) diagram of the narrow-band near-infrared photodiode prepared in Example 2 is shown in FIG7 . It can be seen that the narrow-band near-infrared photodiode provided in this example has a large linear dynamic range (96 dB).

[0214] The noise spectrum of the narrow-band near-infrared photodiode prepared in Example 2 under a bias voltage of -5 V is shown in FIG8 . It can be seen that the actual noise level of the narrow-band near-infrared photodiode provided in this example is low, which confirms its high specific detection.

[0215] The time response curve of the narrow-band near-infrared photodiode prepared in Example 2 under a bias voltage of -5 V is shown in FIG9 . It can be seen that the response time of the narrow-band near-infrared photodiode provided in this example is only 6 ms.

[0216] The narrow-band near-infrared photodiode array prepared in Example 2 is integrated on the thin-film transistor backplane to form an image of the letters "PKU", as shown in FIG10 , where the pixel size is 200 μm×200 μm. It can be seen that the narrow-band near-infrared photodiode provided in this example can perform high-resolution imaging.

[0217] The normalized external quantum efficiency (EQE) of the narrow-band near-infrared photodiodes prepared in Examples 1 and 2 as a function of the incident light wavelength is shown in Figure 11(a). The normalized external quantum efficiency (EQE) of the narrow-band near-infrared photodiodes prepared in Examples 3 and 6 as a function of the incident light wavelength is shown in Figure 11(b). The normalized external quantum efficiency (EQE) of the narrow-band near-infrared photodiodes prepared in Examples 4 and 5 as a function of the incident light wavelength is shown in Figure 11(c). This shows that the preparation method provided by the present invention is universal and can be used to prepare a series of narrow-band near-infrared photodiodes.

[0218] It should be understood that the application of the present invention is not limited to the above examples. For those skilled in the art, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.

Claims

1. A method for preparing a bulk heterojunction active layer, characterized in that: Includes steps: Providing a donor material, an acceptor material, a first solvent immiscible with water, a first water surface, and a substrate on which an active layer is to be prepared, wherein the boiling point of the first solvent immiscible with water is less than or equal to 180° C.; Adding the donor material and the acceptor material into a first solvent that is immiscible with water to form a first mixed solution; applying the first mixed liquid onto the first water surface to perform surface molecular self-assembly to form a first thin film; The first film is transferred to the substrate of the active layer to be prepared, and after a first annealing, the bulk heterojunction active layer is obtained.

2. The preparation method according to claim 1, characterized in that: In the first mixed solution, the total concentration of the donor material and the acceptor material is 20-30 mg·mL -1 ; In the first mixed solution, the mass ratio of the donor material to the acceptor material is 1:0.8-1:1.2; The amount of the first mixed solution applied is 10-20 μL.

3. The preparation method according to claim 1, characterized in that: The donor material includes 3-hexylthiophene, poly{[4,8-bis[(2-ethylhexyl)oxy]-benzo[1,2-B:4,5-B']dithiophene-2,6-diyl][3-fluoro-2-[(2-ethylhexyl)carbonyl]thiophene[3,4-B]thiophene}, poly[(2,6-(4,8-bis(5-(2-ethylhexyl-3-fluoro)thiophene-2-yl)-benzo[1,2-B:4,5-B']dithiophene])-ALT-(5,5-(1',3'-di-2-thiophene-5',7'-bis(2-ethylhexyl) at least one of dithiophene-4,8-dione, dionepyrrolopyrrole, polydithiophene dionepyrrolopyrrole-thiophene, poly{2,2'-[(2,5-bis(2-octyldodecyl)-3,6-dioxo-2,3,5,6-tetrahydropyrrolo[3,4-c]pyrrole-1,4-diyl)]dithiophene-5,5'-diyl salt thieno[3,2-b]thiophene-2,5-diyl}, poly(2,5-bis(3-tetradecylthiophene-2-yl)thieno[3,2-b]thiophene); The acceptor material includes 12,13-di(2-ethylhexyl)-3,9-diundecyl-12,13-dihydro-[1,2,5]thiadiazo[3,4-e]thieno[2",3":4',5']thieno[2',3':4,5]pyrrolo[3,2-g]thieno[2',3':4,5]thieno[3,2-b]indole-2,10-di(5 ,6-difluoro-3-(dicyanomethylidene)inden-1-one), 2,2'-[[[6,6,12,12-tetrakis(4-hexylphenyl)-6,12-dihydrodithio[2,3-D:2',3'-D']-S-indolol[1,2-B:5,6-B']dithiophene-2,8-diyl]bis[methylene(3-oxo-1H-indene-2,1(3H)-dimethylene )]]bis[propylamine], 3,9-bis(2-methylene-((3-(1,1-dicyanomethylene)-6,7-difluoro)-indanone))-5,5,11,11-tetra(4-hexylphenyl)-dithieno[2,3-D:2,3-D]-S-indacen[1,2-B:5,6-B]dithiophene, 2,2'-((2Z,2'Z)-((5,5'-(4,4 ,9,9-tetrakis(4-hexylphenyl)-4,9-dihydro-S-benzodiindeno[1,2-B:5,6-B']dithiophene-2,7-diyl)bis(4-((2-ethylhexyl)oxy)thiophene-5,2-diyl))bis(methylenediyl))bis(5,6-difluoro-3-oxo-2,3-dihydro-1H-indene-2,1-diylidene))dimalononitrile; The first solvent immiscible with water comprises at least one of chlorobenzene, chloroform and dichloromethane; The atmosphere of the first annealing is an inert gas atmosphere, the temperature of the first annealing is 80-120° C., and the time of the first annealing is 5-20 min.

4. A method for preparing a narrow-band near-infrared photodiode, characterized in that: Includes steps: providing a substrate; forming a hole transport layer on the substrate; forming a filter layer on the hole transport layer; forming an intermediate layer on the filter layer; Adopting the preparation method according to any one of claims 1 to 3, forming a bulk heterojunction active layer on the intermediate layer; A top electrode is formed on the bulk heterojunction active layer.

5. The preparation method according to claim 4, characterized in that: The step of forming an intermediate layer on the filter layer specifically includes: Providing an intermediate layer material, a second solvent immiscible with water, and a second water surface, wherein the boiling point of the second solvent immiscible with water is less than or equal to 180° C.; adding the intermediate layer material into a second solvent that is immiscible with water to obtain a second mixed solution; applying the second mixed liquid onto the second water surface to perform surface molecular self-assembly to form a second film; The second film is transferred to the filter layer and annealed for the second time to obtain the intermediate layer.

6. The preparation method according to claim 5, characterized in that: The concentration of the intermediate layer material in the second mixed solution is 5-15 mg·mL -1 ; The amount of the second mixed solution applied is 5-15 μL; The intermediate layer material includes 3-hexylthiophene, poly{[4,8-bis[(2-ethylhexyl)oxy]-benzo[1,2-B:4,5-B']dithiophene-2,6-diyl][3-fluoro-2-[(2-ethylhexyl)carbonyl]thiophene[3,4-B]thiophene}, poly[(2,6-(4,8-bis(5-(2-ethylhexyl-3-fluoro)thiophene-2-yl)-benzo[1,2-B:4,5-B']dithiophene])-ALT-(5,5-(1',3'-di-2-thiophene-5',7'-bis(2-ethylhexyl) At least one of benzo[1',2'-C:4',5'-C']dithiophene-4,8-dione), dionepyrrolopyrrole, polydithiophene dionepyrrolopyrrole-thiophene, poly{2,2'-[(2,5-bis(2-octyldodecyl)-3,6-dioxo-2,3,5,6-tetrahydropyrrolo[3,4-c]pyrrole-1,4-diyl)]dithiophene-5,5'-diyl salt thieno[3,2-b]thiophene-2,5-diyl}, poly(2,5-bis(3-tetradecylthiophene-2-yl)thieno[3,2-b]thiophene); The second solvent immiscible with water comprises at least one of chlorobenzene, chloroform and dichloromethane; The atmosphere of the second annealing is an inert gas atmosphere, the temperature of the second annealing is 80-120° C., and the time of the second annealing is 5-20 min.

7. The preparation method according to claim 4, characterized in that: forming a hole transport layer on the substrate; The step of forming a filter layer on the hole transport layer specifically includes: Providing hole transport materials and light filtering materials; Adding the hole transport material to a third solvent to obtain a third mixed solution; adding the filter material to a fourth solvent to obtain a fourth mixed solution; Applying the third mixed solution to the substrate and performing a first spin coating, and then performing a third annealing to form a hole transport layer on the substrate; The fourth mixed solution is applied to the hole transport layer and spin-coated for a second time, and then annealed for a fourth time to form a filter layer on the hole transport layer.

8. The preparation method according to claim 7, characterized in that: The mass concentration of the hole transport material in the third mixed solution is 1-3wt%; The application amount of the third mixed liquid is: 20-50 μL of the third mixed liquid is applied per square centimeter of substrate; The hole transport material comprises at least one of nickel oxide, poly(3,4-ethylenedioxythiophene):poly(styrene sulfonic acid), and 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene; The third solvent includes at least one of water, ethanol and chlorobenzene; The first spin coating is performed at a speed of 2000-5000 rpm and a time of 20-50 s. The atmosphere of the third annealing is air atmosphere, the temperature of the third annealing is 100-200° C., and the time of the third annealing is 10-30 minutes.

9. The preparation method according to claim 7, characterized in that: The concentration of the filter material in the fourth mixture is 60-100 mg·mL -1 ; The application amount of the fourth mixed liquid is: 20-50 μL of the fourth mixed liquid is applied per square centimeter of the hole transport layer; The filter material includes 3-hexylthiophene, poly{[4,8-bis[(2-ethylhexyl)oxy]-benzo[1,2-B:4,5-B']dithiophene-2,6-diyl][3-fluoro-2-[(2-ethylhexyl)carbonyl]thiophene[3,4-B]thiophene}, poly[(2,6-(4,8-bis(5-(2-ethylhexyl-3-fluoro)thiophene-2-yl)-benzo[1,2-B:4,5-B']dithiophene])-ALT-(5,5-(1',3'-di-2-thiophene-5',7'-bis(2-ethylhexyl) at least one of dithiophene-4,8-dione, dionepyrrolopyrrole, polydithiophene dionepyrrolopyrrole-thiophene, poly{2,2'-[(2,5-bis(2-octyldodecyl)-3,6-dioxo-2,3,5,6-tetrahydropyrrolo[3,4-c]pyrrole-1,4-diyl)]dithiophene-5,5'-diyl salt thieno[3,2-b]thiophene-2,5-diyl}, poly(2,5-bis(3-tetradecylthiophene-2-yl)thieno[3,2-b]thiophene); The fourth solvent includes at least one of chlorobenzene, chloroform and dichloromethane; The second spin coating is performed at a speed of 1000-5000 rpm and a time of 20-50 s. The atmosphere of the fourth annealing is an inert gas atmosphere, the temperature of the fourth annealing is 120-180° C., and the time of the fourth annealing is 15-60 min.

10. A narrow-band near-infrared photodiode, characterized in that: The preparation method is described in any one of claims 4 to 9.

Citation Information

Patent Citations

  • Photomultiplier organic light detector with spectral selectivity and preparation method of photomultiplier organic light detector

    CN106025070A

  • Visible blind near-infrared narrow-band organic photoelectric detector

    CN112635676A

  • Organic solar cell produced by spontaneous orientation film forming method and production method thereof

    CN113644202A

  • Preparation method of active layer, narrow-band near-infrared photodiode and preparation method of narrow-band near-infrared photodiode

    CN116528638A

  • Ultra-fast method for preparing organic / inorganic thin film by using self-diffusion effects

    US20180212148A1

Cited By

  • Organic photovoltaic heterojunction passive multi-parameter gas sensor as well as preparation method and application thereof

    CN121656348A