Nickel clad plate and method for manufacturing same
The nickel clad plate manufacturing process enhances scratch resistance by increasing the surface hardness of the nickel layer through hot and cold rolling, and bright annealing, addressing the softness and exposure issues in conventional methods.
Patent Information
- Application Number
- PCT/JP2023/038089
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2023-10-20
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional nickel clad plates face challenges in achieving scratch resistance on the surface of the nickel material layer due to the softness of nickel, which can lead to exposure of the inner base metal layer during bending, and existing surface hardening methods like carburizing or nitrogen absorption are ineffective for nickel.
A nickel clad plate configuration with a metal base material layer and a nickel material layer where the surface nickel layer has a higher Vickers hardness than the internal layer, achieved through a manufacturing process involving hot rolling, cold rolling, and bright annealing in a non-oxidizing atmosphere, with the nickel oxide scale remaining attached to enhance surface hardness.
The process results in a nickel clad plate with improved scratch resistance on the surface nickel layer, maintaining the structural integrity and corrosion resistance while preventing exposure of the inner base metal layer.
Smart Images

Figure JP2023038089_03102024_PF_FP_ABST
Abstract
Description
Nickel clad plate and its manufacturing method
[0001] The present disclosure relates to a nickel clad plate and a method for manufacturing the same.
[0002] Clad plates, which are made by joining different types of metals (hereinafter referred to as "dissimilar metals") together using methods such as rolling or pressure welding, combine the excellent properties of each of the constituent dissimilar metals in a highly balanced manner, thereby providing new properties that cannot be achieved with single metals or alloys.
[0003] Nickel has long been used as a cathode material for brine electrolysis equipment used in caustic soda manufacturing plants, for example, due to its high corrosion resistance in environments immersed in strong alkaline solutions. In recent years, its use has also expanded as a component material for infrastructure equipment supporting a hydrogen society, such as electrodes for alkaline water electrolysis equipment and electrodes for secondary batteries. Nickel used as a component for such electrolysis equipment has traditionally been in the form of plate material made solely of nickel. However, nickel is expensive, and its bullion price tends to fluctuate dramatically due to changes in the global supply and demand balance of nickel ore. In particular, a sharp increase in demand toward the realization of a carbon-neutral society is expected to lead to supply shortages and a sharp rise in nickel bullion prices in the near future.
[0004] As mentioned above, nickel is a metal that has extremely high corrosion resistance in a strong alkaline environment, so that thinning due to alkaline corrosion during use is hardly an issue, and as long as its mechanical strength is maintained, it can withstand long-term practical use. In other words, the inner layer of the plate material used as an electrode, excluding the outer layer, does not utilize the characteristics of nickel, and rather, since nickel is soft and easily deformed, which is a characteristic of nickel, it can be considered to be disadvantageous in terms of maintaining mechanical strength.
[0005] From this perspective, it is conceivable to use a composite material as an electrode material, in which an inexpensive, general-purpose metal is used as the material constituting the inner layer of the sheet material and nickel is disposed only in the outer layer portion. One example of this is nickel plating on the surface of ordinary steel, an inexpensive, general-purpose metal. Nickel plating can be achieved by electrolytic plating or electroless plating using a catalyst. However, achieving a thick, uniform nickel plating layer that can withstand bending is difficult, and the cost of thick plating is high. Furthermore, to obtain a nickel plating layer with excellent adhesion, nickel alloy plating containing alloying elements such as Si is often used. In this case, there is a risk that the corrosion resistance in a strongly alkaline environment, which is the original purpose, will be impaired, and secondary workability such as bending may also be adversely affected.
[0006] An example of a composite material that does not require plating is a nickel-clad plate, in which nickel is integrally bonded to the surface of a substrate made of an inexpensive, commodity metal. In this case, selecting a material with strength characteristics or deformation behavior similar to nickel for the base layer is advantageous both in the manufacturing process and in the forming process during actual use, and typically, carbon steel or stainless steel can be selected. Because the carbon steel or stainless steel used as the base material and the nickel used as the cladding material have a high affinity in the hot-rolling temperature range, interdiffusion easily occurs at the interface during hot-roll bonding, allowing for the production of a nickel-clad steel plate. Furthermore, for example, carbon steel and austenitic stainless steel have the same FCC structure as nickel in the hot-rolling temperature range and comparable hot strength, resulting in similar deformation behavior and being advantageous for the production of nickel-clad steel plates. Furthermore, the thickness of clad plates manufactured by rolling can be controlled uniformly because the thickness of the outer nickel layer is determined by the mechanical gap between the rolling rolls. Such nickel-clad plates can be used as composite materials with a thick and uniform outer nickel layer that can withstand bending.
[0007] For example, Patent Document 1 discloses "a method for manufacturing a clad product, the method comprising the steps of: preparing a welded assembly including a clad material disposed on a substrate, both the substrate and the clad material being individually selected from alloys, wherein at least a first edge of the clad material does not extend to a first edge of the substrate and provides a margin between the first edges, and wherein a material adjacent the first edge of the clad material within the margin is an alloy having a higher hot strength than the clad material; and hot rolling the welded assembly to provide a hot-rolled strip, wherein the material within the margin prevents the clad material from extending beyond the edge of the substrate during hot rolling." Patent Document 1 also discloses that "the substrate is stainless steel and the clad is nickel or a nickel alloy."
[0008] Furthermore, Patent Document 2 discloses "a metal plate having nickel disposed on its surface, wherein the concentration of nickel hydroxide among chemical species detected on the surface by X-ray photoelectron spectroscopy is more than 0 atomic % and not more than 14 atomic %."
[0009] Furthermore, Patent Document 3 discloses "a nickel-based alloy clad steel having a base material made of a nickel-based alloy consisting of, in mass %, C: 0.02% or less, Cr: 14 to 25%, Mo: 5 to 18%, W: 0 to 5% or less, Fe: 6% or less, and the balance being substantially Ni and unavoidable impurities, and characterized in that the hardness (Vickers hardness under a load of 500 g) within 0.1 mm from the surface on the back side of the base material is 180 or less."
[0010] Furthermore, Patent Document 4 discloses a method for manufacturing a lead frame material, which comprises assembling single-sided or double-sided clad plate materials in which the surface material is either Ni, a Ni-Cu alloy, or an Fe-Ni alloy and the base material as the core material is an Fe-based material, an Fe-Ni-based alloy, a Cr-based stainless steel, or a Cr-Ni-based stainless steel, while creating a vacuum at the interface between the materials, hot rolling this assembly to effect clad bonding of the surface material and the base material, and then cold rolling it until the thickness of the surface layer is 5% or less of the total thickness if the surface layer is Ni or Ni-Cu-based.
[0011] Patent Document 1: JP-T-2008-502486A Patent Document 2: JP-A-2017-179441 Patent Document 3: JP-A-2002-194466 Patent Document 4: JP-A-6-275770A
[0012] Here, in the conventional manufacturing process for making nickel-clad plates into plate products, including Patent Documents 1 to 4, the hot-rolled clad plate, which has been bonded in a hot-rolling process, is descaled by pickling or surface cutting, then cold-rolled to a predetermined plate thickness, and then subjected to a finish annealing process to produce the product. The typical product thickness in this case is approximately 0.5 mm to 2.0 mm, and the thickness of the outer nickel material layer is extremely thin, approximately 50 to 200 μm. Nickel is extremely soft and is easily scratched by external forces. While this is not a problem with pure nickel metal plates, scratches on the surface of a nickel-clad plate with a thin outer nickel material layer may expose the inner base material layer to the surface, for example, during subsequent bending. Therefore, it is desirable for the surface of the nickel-clad plate to have excellent scratch resistance. On the other hand, in order to improve the scratch resistance of the surface of, for example, ordinary steel or stainless steel, surface hardening methods such as carburizing and nitrogen absorption are known.
[0013] However, nickel hardly dissolves carbon or nitrogen even at high temperatures, making carburizing or surface hardening treatments by nitrogen absorption inapplicable. On the other hand, nickel, unlike ordinary steel or stainless steel, can dissolve a certain amount of oxygen. However, when the nickel surface comes into contact with oxygen in a heat treatment atmosphere, hydroxides or oxides are formed, forming a protective coating that prevents oxygen from penetrating to the metal base material layer. For this reason, it has been difficult to improve scratch resistance by hardening the surface of the outer nickel material layer, including Patent Documents 1 to 4.
[0014] Therefore, an object of the present disclosure is to provide a nickel clad plate having improved scratch resistance on the surface of the nickel material layer that forms the outer layer, and a method for manufacturing the same.
[0015] Means for solving the above problems include the following aspects. <1> A nickel clad plate comprising: a metal base material layer; and a nickel material layer laminated on one or both sides of the metal base material layer, wherein a difference in Vickers hardness measured from the surface of the nickel material layer with a test force of 0.2 N is greater by 30.0 or more than a difference in Vickers hardness measured from the surface of the nickel material layer with a test force of 9.8 N. <2> The nickel clad plate according to <1>, wherein the oxygen concentration in a surface layer of the nickel material layer is higher than the oxygen concentration in a center part of the layer thickness of the nickel material layer, and is 0.20% or more and 0.55% or less by mass. <3> A hot rolling process in which a laminate obtained by superposing a nickel material to be the nickel material layer on one or both sides of a steel material to be the metal base material layer is hot rolled and bonded to obtain a hot rolled clad plate, wherein the laminate is bonded to the A of the steel material. 3 After heating to a temperature 150°C or more higher than the transformation point, the hot rolling is started, and the A of the steel material is 3A method for producing a nickel clad plate, comprising: a hot rolling step of finishing the hot rolling at a temperature equal to or higher than the transformation point, a cold rolling step of cold rolling the hot rolled clad plate while the oxide scale produced in the hot rolling step remains attached to the nickel material, to obtain a cold rolled clad plate, and a bright annealing step of annealing the cold rolled clad plate in a non-oxidizing atmosphere at a temperature of 700°C or higher. <4> A method for producing a nickel clad plate according to <3>, wherein, in the hot rolling step, four peripheries including the longitudinal end portions and width end portions of the laminate are joined and sealed before the hot rolling.
[0016] According to the present disclosure, it is possible to provide a nickel-clad plate having improved scratch resistance on the surface of the nickel layer that forms the outer layer, and a method for manufacturing the same.
[0017] Fig. 1 is an explanatory diagram showing the overall configuration of an example of a nickel-clad plate according to the present disclosure. Fig. 2 is a graph showing an example of the relationship between Vickers hardness HV and the tip penetration depth h of a Vickers indenter in the nickel-clad plate according to the present disclosure.
[0018] An example of the present disclosure will be described below. In this disclosure, the "%" used to denote the content of each element in a chemical composition means "mass %." When the lower limit of the content of each element in a chemical composition is expressed as "0," this means that the element is an optional component and may not be present. In a numerical range expressed using "to", when the numerical values before and after "to" are not followed by "greater than" or "less than," this means a range that includes these numerical values as the lower and upper limits. Furthermore, when the numerical values before and after "to" are followed by "greater than" or "less than," this means a range that does not include these numerical values as the lower or upper limit. In numerical ranges expressed in stages, the upper limit of a certain numerical range may be replaced by the upper limit of another numerical range described in stages, or may be replaced by a value shown in an example. Furthermore, the lower limit of a certain numerical range may be replaced by the lower limit of another numerical range described in stages, or may be replaced by a value shown in an example. The term "process" includes not only an independent process but also a process that cannot be clearly distinguished from other processes as long as the intended purpose of the process is achieved.
[0019] The nickel-clad plate (hereinafter also referred to simply as "clad plate") of the present disclosure includes a metal base material layer and a nickel material layer laminated on one or both sides of the metal base material layer, and the difference in Vickers hardness measured from the surface of the nickel material layer with a test force of 0.2 N is 30.0 or more compared to the Vickers hardness measured from the surface of the nickel material layer with a test force of 9.8 N. In the nickel-clad plate of the present disclosure, the metal base material layer and the nickel material layer being laminated means that the metal base material layer and the nickel material layer are laminated by metal bonding. Meanwhile, in the present disclosure, the term "laminate" refers to the overlapped materials before becoming a clad.
[0020] Due to the above-mentioned configuration, the nickel clad plate of the present disclosure has a surface of the nickel material layer (i.e., the surface of the nickel material layer opposite to the side joined to the metal base material layer) that is harder than the interior, and therefore the nickel clad plate has an outer layer of the nickel material layer with improved scratch resistance.
[0021] The nickel-clad plate of the present disclosure will be described in detail below. FIG. 1 is an explanatory diagram showing the overall configuration of an example of the nickel-clad plate of the present disclosure. The nickel-clad plate 1 shown in FIG. 1 includes, for example, a nickel material layer 2, a metal base material layer 3, and a nickel material layer 4 laminated in this order. That is, the nickel-clad plate 1 includes a metal base material layer 3 and nickel material layers 2 and 4 laminated on both sides of the metal base material layer 3. However, the nickel material layer 4 is an optional layer provided as needed. That is, the nickel-clad plate 1 may include a metal base material layer 3 and a nickel material layer 2 laminated on one side of the metal base material layer 3. Furthermore, the nickel-clad plate 1 may include, in addition to the nickel material layer 2, the metal base material layer 3, and the nickel material layer 4, a metal base material layer may be laminated on the nickel material layer 4. That is, the nickel-clad plate 1 may include a nickel material layer and a metal base material layer laminated repeatedly. It is preferable that both sides of the nickel-clad plate 1 are made of nickel material layers.
[0022] The elements and characteristics of the nickel-clad plate of the present disclosure will be described in detail below, with the reference numerals omitted.
[0023] (Metal Base Material Layer) Examples of the metal base material layer include a metal base material layer made of ordinary steel and a metal base material layer made of stainless steel. A metal base material layer made of ordinary steel is particularly suitable as the metal base material layer. A nickel-clad plate using a metal base material layer made of ordinary steel has its outer surface covered with a nickel material layer and exhibits excellent corrosion resistance in a high-concentration alkaline environment, which is a characteristic of nickel. Furthermore, if the metal base material layer is made of ordinary steel, an inexpensive, general-purpose metal, the base metal cost of the entire nickel-clad plate can be reduced. Furthermore, when comparing the deformation behavior of ordinary steel and nickel used in the metal base material layer, the strength at which plastic deformation begins due to an external force, i.e., the yield strength of ordinary steel, is greater than the proof strength of nickel. Therefore, a nickel-clad plate using a metal base material layer made of ordinary steel also has excellent structural strength.
[0024] Suitable ordinary steels are those suitable for cold rolling during the manufacturing process, and typical examples include SPCC, SPCD, SPCE, SPCF, and SPCG as specified in JIS G 3141:2017.
[0025] Examples of stainless steel types include ferritic stainless steel, austenitic stainless steel, martensitic stainless steel, austenitic-ferritic duplex stainless steel, and precipitation hardening stainless steel. Specific examples of stainless steel types include SUS304 (austenitic stainless steel), SUS316 (austenitic stainless steel), SUS301 (austenitic stainless steel), SUS302 (austenitic stainless steel), SUS403 (martensitic stainless steel), SUS430 (ferritic stainless steel), SUS329J1 (austenitic-ferritic duplex stainless steel), and SUS821L1 (austenitic-ferritic duplex stainless steel), which are specified in JIS G 4304:2015 or JIS G 4305:2015.
[0026] The metal base material layer may be made of pure aluminum or an aluminum alloy.
[0027] (Nickel Material Layer) The nickel material layer may be a nickel material layer made of pure nickel material containing, by mass %, 98% or more (preferably 99% or more) nickel, with the remainder being impurities. The impurities mainly include elements or impurities necessary for deoxidation in the refining process, and specific examples thereof include carbon, oxygen, silicon, aluminum, magnesium, phosphorus, sulfur, manganese, chromium, cobalt, copper, iron, etc. Representative examples of pure nickel materials include NW2200 and NW2201, which are specified in JIS G 4902:2019. The nickel material layer may also be a nickel material layer made of a nickel alloy material. Examples of nickel alloy materials include alloys containing Fe, Cr, Cu, etc. in addition to nickel. Examples of nickel alloy materials include NCF600, NW4400, etc., which are specified in JIS G 4902:2019, and PC, etc., which are specified in JIS C 2531:1999.
[0028] (Vickers hardness) Both values are measured from the surface of the nickel material layer (i.e., the surface of the nickel material layer opposite the side joined to the metal base material layer), but the Vickers hardness measured with a test force of 0.2 N (hereinafter also referred to as "surface Vickers hardness HV0.02") is greater by 30.0 or more than the Vickers hardness measured with a test force of 9.8 N (hereinafter also referred to as "internal Vickers hardness HV1").
[0029] Here, the fact that the surface layer is harder than the inside of the nickel material layer, which is the outer layer, can be confirmed by investigating how the hardness obtained in a Vickers hardness test standardized in JIS Z 2244: 2009 changes depending on the tip penetration depth of the Vickers indenter. That is, when the test force in the Vickers hardness test is F (N), the Vickers hardness is HV, and the tip penetration depth of the Vickers indenter is h (μm), h is calculated from the relational expression: h = 62.1√(F / HV) [μm], and the hardness of the inside and surface layers of the nickel material layer is compared.
[0030] FIG. 2 shows a graph illustrating an example of the relationship between the Vickers hardness HV and the tip penetration depth h of the Vickers indenter in the nickel-clad plate of the present disclosure. As shown in FIG. 2, the Vickers hardness is approximately the same at a position where h is deeper than 10 μm, so the Vickers hardness in this range can be considered to be equivalent to the hardness of the inside of the nickel material layer in an annealed state. More preferably, the hardness of the inside of the nickel material layer can be evaluated under conditions where h is deeper than 15 μm. Considering that the hardness of the inside of the outer nickel material layer in an annealed state is 80 to 100 HV, the hardness of the inside of the nickel material layer can be evaluated by evaluating the internal Vickers hardness HV1 at a test force of 9.8 N.
[0031] To improve scratch resistance, it is effective for the nickel material layer to have a high hardness within a range of several μm deep from the surface. The prototype material shown as a comparative example in FIG. 2 is an example in which no clear effect on scratch resistance was observed, while the prototype material shown as an example of the present invention is a prototype material in which improved scratch resistance was observed. That is, when the Vickers hardness difference from the surface of the nickel material layer to a depth of at least 2 μm is 30.0 or more greater than that of the interior of the nickel material layer, improved scratch resistance is observed. In this case, the hardness of the surface layer of the nickel material layer can be evaluated by evaluating the surface layer Vickers hardness HV0.02 at a test force of 0.2 N.
[0032] In this way, since the surface layer Vickers hardness HV0.02 is larger than the internal Vickers hardness HV1, the surface layer of the nickel material layer is harder than the internal portion, and the scratch resistance of the surface of the nickel material layer, which becomes the outer layer, is improved. Here, since the internal metal structure of the nickel material layer is required to be in an annealed state with ordered crystal grains, it is necessary to avoid increasing the Vickers hardness to the internal portion of the nickel material layer. If the Vickers hardness is increased to the internal portion, there is a concern that the ductility of the entire sheet material will be impaired and formability will be hindered. Therefore, it is necessary to improve the scratch resistance by hardening only the surface layer of the nickel material layer to a depth of at least 2 μm from the surface layer.
[0033] Compared with the internal Vickers hardness HV1, the surface layer Vickers hardness HV0.02 measured from the surface of the nickel material layer with a test force of 0.2 N is preferably 30.0 or more higher, and more preferably 40.0 or more higher. However, from the viewpoint of preventing surface roughening or surface cracking during bending, the difference between the internal Vickers hardness HV1 and the surface layer Vickers hardness HV0.02 is preferably 100 or less.
[0034] From the viewpoint of improving the scratch resistance of the surface of the nickel material layer that becomes the outer layer, the lower limit of the surface layer Vickers hardness HV0.02 is preferably 110, more preferably 115. The upper limit of the surface layer Vickers hardness HV0.02 is preferably 210, more preferably 195. The surface layer Vickers hardness HV0.02 may be 110 to 210, or may be 115 to 195.
[0035] Here, the Vickers hardness is the arithmetic mean value measured at five arbitrary locations on the surface of the nickel layer of the nickel-clad plate to be measured, at the center in the width direction of the clad plate, using the above test forces, according to JIS Z 2244: 2009. However, the arbitrary measurement locations are those separated by a distance of 500 μm or more between the centers of the indentations for the measurement of HV1, and those separated by 80 μm or more for the measurement of HV0.02.
[0036] (Oxygen Concentration) It is preferable that the oxygen concentration of the surface layer of the nickel material layer (i.e., the surface layer of the nickel material layer on the opposite side to the side joined to the metal base material layer) is higher than the oxygen concentration of the central part of the nickel material layer in the thickness direction. Since the oxygen concentration of the surface layer of the nickel material layer is higher than the oxygen concentration of the central part of the nickel material layer in the thickness direction, the surface layer becomes harder than the inside of the nickel material layer. This makes it easier for the Vickers hardness measured from the surface of the nickel material layer with a test force of 9.8 N and the Vickers hardness measured from the surface of the nickel material layer with a test force of 0.2 N to satisfy the above relationship. As a result, the scratch resistance of the surface of the nickel material layer that becomes the outer layer is easily improved. From the viewpoint of improving the scratch resistance of the surface of the nickel material layer that becomes the outer layer, the difference in oxygen concentration between the surface layer of the nickel material layer and the central part of the thickness direction of the nickel material layer is preferably 0.15 to 0.50% by mass, more preferably 0.18 to 0.40%. From the same viewpoint, the oxygen concentration in the surface layer of the nickel material layer is preferably 0.20 to 0.55% by mass, and more preferably 0.23 to 0.45% by mass.
[0037] The surface layer of the nickel material layer refers to a region from the surface of the nickel material layer to a depth of 1 μm to 4 μm. On the other hand, the region where the surface hardness of the nickel material layer is increased is limited to a depth of at most 20 μm from the outer surface. In other words, the nickel at a position 20 μm or deeper from the outer surface has uniform properties with a metal structure adjusted by annealing. Therefore, the central portion of the nickel material layer refers to a position deeper than 20 μm from the outer surface of the nickel material layer. Furthermore, considering that the HV hardness and oxygen concentration are measured from the outer surface layer, the properties of the central portion of the nickel material layer can be measured using the average values in the region from a depth of 20 μm to 40 μm from the surface of the nickel material layer.
[0038] Here, the oxygen concentration is measured as follows. After ultrasonically cleaning the nickel clad plate to be measured with acetone, the surface side of the nickel material layer is sputtered in the depth direction by glow discharge optical emission spectroscopy (quantitative GDS), and the depth direction distribution of the intensity of elements contained in the nickel material layer (O, Ni, Fe, Cr, Mn, Si, Cu, N, C) is measured. Then, the oxygen concentration of the surface layer and the central part of the nickel material layer is obtained from the arithmetic average of the intensity ratio of O (oxygen) to all the elements contained in the nickel material layer in the surface layer and the central part of the plate thickness of the nickel material layer. The measurement conditions are as follows. Measurement equipment: Horiba, Ltd., model number: GD-Profiler 2 Measurement conditions: RF output 35 W, discharge area φ4 mm, argon pressure 600 Pa, measurement depth 50 μm Measurement location: center of clad plate width Sputtering rate: 0.09 μm / sec Measurement timing: every 0.008 (μm) of cutting depth by sputtering
[0039] (Thickness) The total thickness of the clad plate of the present disclosure is preferably 0.3 to 6.0 mm, more preferably 0.5 to 5.0 mm. The ratio of the thickness of the nickel material layer to the total thickness of the clad plate (thickness of the nickel material layer / total thickness of the clad plate) is preferably 5 / 100 to 25 / 100, more preferably 8 / 100 to 20 / 100. The thickness of the nickel material layer is preferably 0.05 to 1.0 mm, more preferably 0.08 to 0.5 mm. By setting the total thickness of the clad plate and the thickness of each layer within the above ranges, the clad plate becomes suitable for use as a cathode material for a sodium chloride electrolysis device, an electrode for an alkaline water electrolysis device, and an electrode for a secondary battery.
[0040] <Method for manufacturing nickel-clad plate> Next, an example of a method for manufacturing a nickel-clad plate according to the present disclosure will be described. Note that this example of the method for manufacturing a nickel-clad plate according to the present disclosure is an example in which a steel material is used as the metal material that becomes the metal base material layer (i.e., a metal base material layer made of steel is used as the metal base material layer).
[0041] The method for manufacturing a nickel clad plate according to the present disclosure includes a hot rolling step of hot rolling a laminate in which a nickel material to be a nickel material layer is superimposed on one or both sides of a steel material to be a metal base material layer, and bonding the laminate to obtain a hot rolled clad plate, the hot rolling step being performed by bonding the laminate to the A of the steel material.3 After heating to a temperature 150°C or more higher than the transformation point, the hot rolling is started, and the A of the steel material is 3 The method includes a hot rolling step in which the hot rolling is completed at a temperature equal to or higher than the transformation point; a cold rolling step in which the hot-rolled clad plate is cold-rolled while the oxide scale formed in the hot rolling step remains attached to the nickel material to obtain a cold-rolled clad plate; and a bright annealing step in which the cold-rolled clad plate is annealed in a non-oxidizing atmosphere at a temperature of 700°C or higher.
[0042] In a conventional method for manufacturing a nickel-clad plate, the hot-rolled clad plate is air-annealed after hot rolling, and then the surface oxide scale is removed by pickling or surface grinding before cold rolling. This is because if the oxide scale is fractured during cold rolling, it can cause scratches or roughness on the surface of the clad plate. On the other hand, if a hot-rolled clad plate that has been hot-rolled and not air-annealed is cold-rolled with the oxide scale left, the oxide scale on the surface of the nickel material that becomes the nickel material layer is ductile during cold rolling and remains without fracture. The oxide scale after hot rolling (hot-rolled scale) and the oxide scale after annealing (annealed scale) have different properties: annealed scale is easily fractured during cold rolling, while hot-rolled scale is ductile and easily stretched.
[0043] Furthermore, compared with nickel-clad sheets that are cold-rolled after removing the oxide scale after hot rolling, as in conventional manufacturing methods, nickel-clad sheets that are cold-rolled and bright-annealed while the oxide scale after hot rolling remains attached exhibit increased hardness in the surface layer of the nickel material layer. This is because cold-rolling while leaving the oxide scale after hot rolling disperses nickel oxide in the surface layer of the nickel material layer, and some of the oxygen liberated by reduction of the nickel oxide during the final bright annealing process dissolves in metallic nickel, forming an oxygen-enriched layer on the surface layer of the nickel material layer and hardening it. It should be noted that the outer nickel material layer that constitutes the surface of a nickel-clad steel sheet is difficult to harden using conventional surface hardening treatments such as nitriding or carburizing. Furthermore, when attempting to introduce oxygen into the surface of the nickel material layer by ion implantation or the like, a nickel hydroxide coating forms on the surface, making it difficult to introduce oxygen.
[0044] From the above, the nickel clad plate method of the present disclosure can obtain a nickel clad plate that satisfies the relationship between the Vickers hardness at the surface of the nickel material layer at each of the above test forces and the oxygen concentration at the surface layer and the center of the plate thickness of the nickel material layer.
[0045] Furthermore, in conventional nickel-clad plate manufacturing methods, when removing the surface oxide scale, the thickness of the metal portion of the nickel material is also reduced to a certain extent, and the thickness ratio of the nickel material layer to the metal base material layer changes from the state immediately after hot rolling. On the other hand, if cold rolling is performed without performing deoxidation scaling, a portion of the nickel material that will become the nickel material layer does not need to be removed by pickling or cutting. As a result, the thickness ratio of the nickel material layer to the metal base material layer can be maintained as it was immediately after bonding by hot rolling during cold rolling. As a result, it is possible to produce a nickel-clad plate as a product while maintaining the nickel material layer at a constant and uniform thickness.
[0046] In addition, in cold rolling, when a soft nickel material is brought into contact with a rolling roll under high pressure, the nickel material adheres to the rolling roll, causing deterioration of surface quality and rolling defects. However, by proceeding with cold rolling with an oxide scale attached to the surface of the nickel material, it is possible to prevent deterioration of surface quality and rolling defects due to adhesion of the nickel material.
[0047] Hereinafter, each step of an example of a method for manufacturing a nickel-clad plate according to the present disclosure will be described.
[0048] (Hot rolling step) In the hot rolling step, a laminate in which a nickel material to be the nickel material layer is superimposed on one or both sides of a steel material to be the metal base material layer is hot rolled to bond and roll to obtain a hot rolled clad plate. Specifically, for example, the process is as follows.
[0049] In the hot rolling process, first, for example, a slab or a thick plate is prepared as the steel material and the nickel material. The slab or the thick plate should have a uniform thickness and be free from irregularities, defects, and stains.
[0050] Next, for example, a steel material is laminated on one or both sides of the steel material with a nickel material as a cladding material. Before hot rolling, the laminated body is sealed around all four sides, including the longitudinal and widthwise ends, to form a tightly sealed structure. This prevents oxide scale from forming between the steel material and the nickel material during hot rolling, achieving a good bond.
[0051] Next, the stacked laminate is hot rolled to be bonded. 3 The process starts after heating to a temperature 150°C or higher than the transformation point (i.e., the temperature before hot rolling), and the A of the steel material 3 The rolling is finished at a temperature equal to or higher than the transformation point (i.e., hot rolling finishing temperature). The temperature indicates the surface temperature of the laminate.
[0052] Here, when cold rolling is performed on the hot-rolled bonded body after hot rolling, the thickness ratio between the steel material that will become the metal base material layer and the nickel material that will become the nickel material layer (i.e., the composite material) is substantially unchanged before and after cold rolling. Therefore, it is preferable to adjust the thickness ratio between the steel material that will become the metal base material layer and the nickel material that will become the nickel material layer (i.e., the composite material) to a desired ratio immediately after hot rolling. However, if the hot rolling conditions are not appropriate, the deformation amounts of each material due to hot rolling will not be constant, making it difficult to achieve the desired thickness ratio. Such uneven deformation amounts mainly occur when the high-temperature deformation resistances of the steel material that will become the metal base material layer and the nickel material that will become the nickel material layer are not the same in the heating temperature range of hot rolling.
[0053] If the high-temperature deformation resistances of the steel material forming the metal base layer and the nickel material forming the nickel material layer differ, the amount of thickness reduction in the two materials during hot rolling will differ, resulting in different amounts of elongation in the longitudinal or width direction. When the difference in deformation resistance between the two materials is small within a certain range, the difference in thickness reduction is absorbed as a deviation in the amount of elongation in the width direction, and hot rolling is unlikely to be affected. However, when the difference in deformation resistance between the two materials exceeds a certain range, the difference in thickness reduction manifests as a deviation in not only the width direction but also the amount of elongation in the longitudinal direction. This causes misalignment of the weld seal in the longitudinal direction. If the nickel material used as a cladding material is too long, out-of-plane deformation occurs, changing the thickness ratio. If the nickel material is too short, excessive thickness reduction can occur, leading to fracture and chipping. If the weld fractures, this can interfere with joining by hot rolling.
[0054] To prevent such a situation, hot rolling is carried out under the above temperature conditions.
[0055] In order to sufficiently form an oxide scale on the surface of the nickel material layer of the hot-rolled joined body after the hot rolling, when preheating the laminate before the hot rolling, it is preferable to heat the laminate using a burner-type heat source using a combustion gas such as natural gas, and then perform the hot rolling.
[0056] (Cold Rolling Process) In the cold rolling process, the hot-rolled clad plate is cold-rolled while the oxide scale formed in the hot rolling process remains attached to the nickel material to obtain a cold-rolled clad plate. Specifically, the hot-rolled clad plate after the hot rolling process is cold-rolled without air annealing and while the oxide scale remains attached to the nickel material. This prevents the formation of new oxide scale with voids by not performing air annealing, and the oxide scale, which is a continuous body compressed and integrated in the hot rolling process, has ductility, allowing cold rolling to be performed without crushing. Nickel oxide is then dispersed in the surface layer of the nickel material layer.
[0057] However, if deoxidation treatment such as pickling or surface grinding is performed to remove the oxide scale, not only the oxide scale but also a considerable amount of the nickel material is removed. As a result, the thickness ratio of the nickel material layer in the nickel clad plate changes from the state immediately after hot rolling. In this respect, there is an advantage to not performing deoxidation treatment.
[0058] The cold rolling conditions are not particularly limited and can be well-known conditions. Annealing in a non-oxidizing atmosphere or an atmosphere with a reduced oxygen concentration may be performed between the hot rolling and the cold rolling. Furthermore, if a sufficient amount of oxide scale is attached to the nickel material, a descaling treatment may be performed to remove a portion of the oxide scale.
[0059] (Bright annealing process) In the bright annealing process, the cold-rolled clad sheet is bright annealed. Bright annealing is performed under conditions that prevent the formation of new oxide scale and the thinning of the nickel material layer due to deoxidation scaling. Therefore, bright annealing is performed in a non-oxidizing atmosphere. Examples of non-oxidizing atmospheres include a mixed gas of nitrogen and hydrogen, nitrogen gas, hydrogen gas, and argon gas, as well as a vacuum atmosphere.
[0060] Bright annealing is performed under conditions in which at least a portion of the nickel oxide present on the surface of the nickel material layer of the cold-rolled clad sheet after cold rolling is reduced, and the liberated oxygen dissolves in the nickel. Therefore, the bright annealing temperature is set to 700°C or higher. The bright annealing temperature is more preferably 800°C or higher. However, from the viewpoint of preventing excessive grain growth, the bright annealing temperature is preferably 1000°C or lower. The dew point of the bright annealing atmosphere is preferably -75°C or higher and lower than -30°C, and more preferably -75°C or higher and lower than -40°C.
[0061] (Temper Rolling) When it is desired to increase the structural strength of a component manufactured using the nickel-clad plate of the present disclosure, temper rolling can be performed following bright annealing in order to increase the material strength of the nickel-clad plate in advance. The reduction ratio of the temper rolling can be appropriately set according to the desired material strength, but an excessively large reduction ratio will impair the ductility of the material, so the reduction ratio of the temper rolling is preferably in the range of 0.5% to 10.0%, more preferably in the range of 1.0% to 5.0%. A general temper rolling mill can be used for this rolling, and rolling with or without a rolling lubricant can be applied. However, in order to accurately achieve a small reduction ratio and perform temper rolling while maintaining good plate flatness, it is desirable to perform temper rolling using large-diameter work rolls with a diameter of 250 mm to 1000 mm, more preferably 400 mm to 1000 mm.
[0062] Through the above steps, the nickel clad plate of the present disclosure is obtained.
[0063] The effects of the present disclosure will be explained below using examples, but the present disclosure is not limited to the conditions used in the following examples.
[0064] (Example A: Invention Examples 1-2, Comparative Examples 3-6) Small-scale prototypes of nickel-clad plates were conducted as follows. A cast slab equivalent to ordinary steel (SPCE as specified in JIS G 3141:2017) was prepared, hot-rolled, and then cut to a predetermined width and length. Both surfaces of the hot-rolled plate were machined. As a result, a 30 mm thick, 500 mm wide, and 1000 mm long SPCE thick plate was obtained as the steel material for the metal base layer. A hot coil of NW2201 as specified in JIS G 4902:2019 was prepared. A nickel plate drawn from the hot coil was flattened with a leveler, and then the surface of the nickel plate was belt-polished and washed before being fine-cut. As a result, a 5 mm thick, 480 mm wide, and 980 mm long NW2201 plate was obtained as the nickel material (clad material) for the nickel material layer. The joining surfaces of both the steel and nickel materials were cut or polished until a metallic luster appeared and the metal surface was exposed. NW2201 plates were stacked on both sides of the SPCE thick plate to obtain a laminate, and the four peripheries of the laminate, including the longitudinal and widthwise ends, were sealed by TIG welding using a welding rod. The welded and sealed laminate was uniformly heated to the temperature shown in Table 1 (temperature before hot rolling), and subjected to a total of four passes of hot rolling using a reversible two-high hot rolling mill to produce a 5 mm thick hot-rolled clad plate. The hot rolling completion temperature was the temperature shown in Table 1. Furthermore, the A of SPCE 3 The transformation point is 910°C.
[0065] Next, the hot-rolled clad plate was cold-rolled to a total thickness shown in Table 1 without annealing or deoxidation scaling. However, in some examples, the deoxidation scaling shown in Table 1 was performed. Here, the thickness of each of the first layer (nickel material layer), second layer (steel base material layer), and third layer (nickel material layer) in the cold-rolled clad plate after cold rolling is shown in Table 1. The total thickness of the hot-rolled joined body and the thickness of each of the first layer (nickel material layer), second layer (steel base material layer), and third layer (nickel material layer) correspond to the total thickness of the obtained nickel-clad plate and the thickness of each of the first layer (nickel material layer), second layer (steel base material layer), and third layer (nickel material layer).
[0066] Next, the cold-rolled clad plate was bright annealed in a non-oxidizing atmosphere using the atmospheric gas and annealing temperature shown in Table 1, with a dew point of -60°C and a bright annealing time of 1.5 to 6.0 minutes. Here, the bright annealing time was set according to the total thickness of the cold-rolled clad plate as follows: Total thickness of cold-rolled clad plate 0.5 mm: Bright annealing time 1.5 minutes Total thickness of cold-rolled clad plate 0.8 mm: Bright annealing time 2.4 minutes Total thickness of cold-rolled clad plate 1.0 mm: Bright annealing time 3.0 minutes Total thickness of cold-rolled clad plate 2.0 mm: Bright annealing time 6.0 minutes
[0067] A nickel clad plate was obtained through the above steps, as shown in Table 1. The Vickers hardness and oxygen concentration of the nickel material layer shown in Table 1 indicate the Vickers hardness and oxygen concentration of one of the nickel material layers (first layer).
[0068] The scratch resistance of the obtained nickel-clad plate was then evaluated. Specifically, the evaluation was as follows. The scratch resistance was evaluated by a pin-on-disk sliding test without lubrication. The evaluation sample was a φ80 mm disk taken from a prototype plate sample. A φ5 mm round bar made of tool steel SUJ2 was used as the processing pin, and the outer periphery of the flat tip surface was chamfered to give an effective area of φ4 mm. The pin tip was contacted at a position 30 mm from the center of the disk sample and pressed with a force of 300 gf in a direction perpendicular to the disk, while the disk sample was rotated at a rotation speed of 60 rpm. After 300 rotations (sliding distance 56 m), the disk surface condition was evaluated according to the following evaluation criteria: A: No scratches were observed B: Minor surface roughness that was not a problem was observed C: Scratches with a maximum depth of 2 μm or more were observed D: Scratches with a maximum depth of 5 μm or more were observed
[0069] Examples No. 1 and No. 2 are examples that fall within the scope of the present disclosure. In these examples, joining by hot rolling and cold rolling could be performed without any problems. Furthermore, the difference between the surface Vickers hardness HV0.02 and the internal Vickers hardness HV1 was large, at 30.0 or more. Furthermore, the oxygen concentration in the surface layer of the nickel material layer (i.e., the surface layer of the nickel material layer on the side opposite to the side joined to the metal base material layer) was higher than the oxygen concentration in the central portion of the nickel material layer. Therefore, the scratch resistance was evaluated as good.
[0070] Examples No. 3 and No. 4 are comparative examples. In these examples, deoxidation scaling was performed by pickling or cutting after hot rolling, so the difference between the surface Vickers hardness HV0.02 and the internal Vickers hardness HV1 was small, less than 30.0. Therefore, the evaluation of scratch resistance was also poor. Example No. 5 is a comparative example. In this example, the bright annealing temperature was low at 680°C, so the difference between the surface Vickers hardness HV0.02 and the internal Vickers hardness HV1 was small, less than 30.0. This is thought to be because the oxide scale remaining on the surface of the cold-rolled clad sheet remained as it was, and an oxygen-enriched layer was not formed on the surface of the nickel material layer. Therefore, the evaluation of scratch resistance was also poor. Example No. In No. 6 and No. 7, the temperature of hot roll joining was low, and the deformation amounts of the SPEC material and the nickel material were inconsistent during hot rolling, resulting in a deviation in the thickness of the nickel material, which led to fracture during cold rolling or hot rolling.
[0071] (Example B: Invention Examples 8 to 13) Nickel-clad steel plates were manufactured using a production line as follows. A cast slab equivalent to ordinary steel (SPCE as specified in JIS G 3141:2017) was prepared. The dimensions of the cast slab were 250 mm thick and 1600 mm wide. Both sides of the cast slab were machined to a smooth finish. As a result, an SPCE slab with a thickness of 245 mm and a width of 1600 mm was obtained as the steel material for the metal base layer. A thick plate of NW2201 specified in JIS G 4902:2019 was prepared. Both sides of the thick plate were machined to a smooth finish and further fine-cut. As a result, an NW2201 plate with a thickness of 40 mm and a width of 1550 mm was obtained as the nickel material (clad material) for the nickel material layer. NW2201 plates were stacked on both sides of the SPCE slab to obtain a laminate, and the four peripheries including the longitudinal and widthwise ends were sealed by TIG welding using a welding rod.
[0072] The welded and sealed laminate was inserted into an atmospheric heating furnace at 1250°C (temperature before hot rolling) and uniformly heated, and then hot-rolled for a total of 19 passes using a reversible four-high hot rolling mill to obtain a hot-rolled clad plate with a thickness of 150 mm. The heat source of the atmospheric heating furnace was a burner system using natural gas as fuel. However, the hot-rolling completion temperature was 1000°C. In addition, the A of SPCE 3 The transformation point is 910°C. The obtained hot-rolled clad plate having a thickness of 150 mm was again inserted into an atmospheric heating furnace at 1250°C (the temperature before hot rolling) and uniformly heated, and then continuously rolled in a tandem hot rolling mill to obtain a hot-rolled clad plate having a thickness of 5 mm. The hot-rolled clad plate was then wound up to obtain a hot-rolled bonded coil. Here, the thicknesses of the first layer (nickel material layer), second layer (steel base material layer), and third layer (nickel material layer) in the cold-rolled clad plate after cold rolling are shown in Table 1. The total thickness of the hot-rolled bonded body and the thicknesses of the first layer (nickel material layer), second layer (steel base material layer), and third layer (nickel material layer) correspond to the total thickness of the obtained nickel-clad plate and the thicknesses of the first layer (nickel material layer), second layer (steel base material layer), and third layer (nickel material layer).
[0073] A hot-rolled clad plate was drawn out from the obtained hot-rolled bonded coil, and the hot-rolled clad plate was cold-rolled as it was in a six-high cold rolling mill without being annealed or deoxidized and scaled, to obtain a cold-rolled clad plate cold-rolled to the total thickness shown in Table 1. The obtained cold-rolled clad plate was then coiled to form a plurality of cold-rolled bonded coils.
[0074] Next, the cold-rolled bonded coil was bright annealed in a non-oxidizing atmosphere using the atmospheric gas shown in Table 1, at an annealing temperature of −60°C, and for a bright annealing time of 1.5 to 6.0 minutes. Here, the bright annealing time was set according to the total thickness of the cold-rolled clad sheet, as in Example A. In the examples using an argon gas atmosphere and an annealing temperature of 750°C, bright annealing was performed in a batch annealing furnace. In the examples using a nitrogen gas atmosphere or a nitrogen and hydrogen gas atmosphere (nitrogen + hydrogen) and an annealing temperature of 850°C, bright annealing was performed by passing the cold-rolled clad sheet through a bright annealing line. Following bright annealing, some coils were subjected to lubrication-free temper rolling using a two-high temper mill with a work roll diameter of 610 mm. The rolling reduction ratios were 2% for Example 12 and 4% for Example 13.
[0075] A nickel clad plate was obtained through the above steps. Details are shown in Table 1. The obtained nickel clad plate was then subjected to the same evaluation of scratch resistance as above. The Vickers hardness and oxygen concentration of the nickel material layer shown in Table 1 indicate the Vickers hardness and oxygen concentration of one of the nickel material layers (first layer). The underlined values indicate values outside the scope of the present disclosure.
[0076] Nos. 8 to 13 are examples that fall within the scope of the present disclosure. In these examples, joining by hot rolling and cold rolling could be performed without any problems. Furthermore, the difference between the surface Vickers hardness HV0.02 and the internal Vickers hardness HV1 was large, at 30.0 or more. Furthermore, the oxygen concentration in the surface layer of the nickel material layer (i.e., the surface layer of the nickel material layer on the side opposite to the side joined to the metal base material layer) was higher than the oxygen concentration in the central portion of the nickel material layer. Therefore, the evaluation of scratch resistance was favorable.
[0077]
[0078] From the above results, it can be seen that the clad plate of the present disclosure has high scratch resistance on the surface of the nickel material layer that forms the outer layer.
[0079] The disclosure of Japanese Patent Application No. 2023-054363, filed on March 29, 2023, is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards mentioned herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard was specifically and individually indicated to be incorporated herein by reference.
[0080] 1 Nickel clad plate 2 Nickel material layer 3 Metal base material layer 4 Nickel material layer
Claims
1. A nickel clad plate comprising: a metal base layer; and a nickel material layer laminated on one or both sides of the metal base layer, wherein the Vickers hardness measured from the surface of the nickel material layer with a test force of 9.8 N is greater than the Vickers hardness measured from the surface of the nickel material layer with a test force of 0.2 N by a difference of 30.0 or more.
2. A nickel clad plate as described in claim 1, wherein the oxygen concentration in the surface layer of the nickel material layer is higher than the oxygen concentration in the central part of the thickness of the nickel material layer, and is 0.20% or more and 0.55% or less in mass percent.
3. A hot rolling process in which a laminate in which a nickel material to be a nickel material layer is laminated on one or both sides of a steel material to be a metal base material layer is hot rolled to bond the laminate to obtain a hot rolled clad plate, 3 After heating to a temperature 150° C. or more higher than the transformation point, the hot rolling is started, and the A of the steel material is 3 A method for producing a nickel clad plate, comprising: a hot rolling step of finishing the hot rolling at a temperature equal to or higher than a transformation point; a cold rolling step of cold rolling the hot rolled clad plate while the oxide scale generated in the hot rolling step remains attached to the nickel material to obtain a cold rolled clad plate; and a bright annealing step of annealing the cold rolled clad plate in a non-oxidizing atmosphere at a temperature of 700°C or higher.
4. A method for producing a nickel clad plate as described in claim 3, wherein in the hot rolling step, all four peripheries of the laminate, including the longitudinal and widthwise ends, are joined and sealed before hot rolling.
Citation Information
Patent Citations
Battery can forming material and manufacture thereof
JP1998092395A
Iron-based parts and manufacturing method therefor
JP2006342409A
Lead material for battery, and manufacturing method thereof
JP2017054775A
Surface-treated steel plate for cell container
WO2017094919A1
Ni-PLATED STEEL SHEET HAVING EXCELLENT POST-PROCESSING CORROSION RESISTANCE AND PRODUCTION METHOD THEREFOR