Method for producing sintered compact, sintered compact, and molding die

The method addresses the challenge of removing unbound particles from complex shapes and hollow structures in binder jetting by deforming the precursor on an inclined mold, ensuring efficient particle removal and high accuracy in the sintered body.

WO2024202446A1PCT designated stage expired Publication Date: 2024-10-03HITACHI LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/001698
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-01-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Binder jetting additive manufacturing faces challenges in removing unbound material particles from complex shapes with hollow structures or narrow gaps, as existing methods can damage the precursor and fail to reach closed cavities or narrow spaces effectively.

Method used

A method involving a precursor with open cavities and gaps that are deformed onto an inclined mold surface, allowing unbound particles to be easily removed before heat treatment, which then sinter the parts together without external force, ensuring high shape accuracy and preventing particle sintering within the structure.

Benefits of technology

Enables efficient removal of unbound particles from complex shapes and hollow structures, reducing damage and ensuring high shape accuracy of the sintered body by using an inclined mold surface to close cavities and gaps during heat treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024001698_03102024_PF_FP_ABST
    Figure JP2024001698_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a method for producing a sintered compact with which it is possible to easily remove unnecessary material particles adhering to the inside of a cavity or a gap in the sintered compact, a sintered compact obtained using said method, and a molding die used in said method. This method for producing a sintered compact comprises a molding step for molding a precursor (10), and a heat treatment step for heat-treating the precursor (10) in a molding die (20) to form a sintered compact. The sintered compact has a hollow structure provided with an internal cavity or a complex structure that has a gap opening towards the outside. The precursor (10) is molded to a shape in which portions forming the cavity are separated from each other to open the cavity to the exterior, or a shape in which the gap between portions forming the gap is open. The molding die (20) has inclined surfaces (21) on the upper surface thereof. The precursor (10) is placed on the molding die (20), deformed to a shape in which the portions forming the cavity are in contact with each other to close the cavity or deformed to a shape in which the spacing between the portions forming the gap is reduced, and then heat-treated and sintered.
Need to check novelty before this filing date? Find Prior Art

Description

Method for manufacturing sintered body, sintered body and molding mold

[0001] The present invention relates to a method for producing a sintered body in which a molding material containing material particles and a binder is molded and heat-treated to produce a sintered body in which the material particles are sintered together, a sintered body using this method, and a molding mold used for this method.

[0002] One method for producing sintered bodies is binder jetting additive manufacturing, a type of additive manufacturing that produces objects by layering materials together, and is used for the production of core aftermarket parts and rapid prototyping of molds and specialized machine parts.

[0003] In binder jetting additive manufacturing, a binder is sprayed onto a powder bed formed of material particles to form a bond layer with a predetermined pattern. By repeating the formation of such bond layers in the stacking direction, a shaped object with a predetermined three-dimensional shape is formed. When metal particles or the like are used as the material particles, the shaped object is typically heat-treated to degrease the binder and sinter the material particles together.

[0004] Patent Document 1 describes a sintered body produced by metal injection molding (MIM) and a method for producing the same. In this production method, an injection-molded body formed by injecting a molding material containing a mixture of metal powder and a binder into an injection mold, or an intermediate molded body obtained by degreasing the injection-molded body, is placed in a transfer mold and subjected to gravity molding, which involves deformation due to gravity, and then sintered after gravity molding. Gravity molding is said to enable the mass production of sintered bodies having complex shapes without requiring excessive manual labor during secondary molding.

[0005] Japanese Patent Application Laid-Open No. 2017-186613

[0006] In binder jetting additive manufacturing, a binder is sprayed onto a predetermined build area to form a bonded layer with a predetermined pattern. As a result, there are areas around the build area where the binder is not sprayed, leaving unbound material particles that are not bound by the binder. The unbound material particles remain on the surface of the build object and must be removed after the build. Generally, unbound material particles that have adhered to the build object are removed by sweeping with a brush or by spraying compressed air.

[0007] When using binder jetting additive manufacturing to produce hollow sintered bodies with internal cavities or complex sintered bodies with narrow gaps, there is a problem in that it is difficult to remove unbound material particles that adhere to the precursor of the sintered body. Binder jetting additive manufacturing, a type of additive manufacturing, has the advantage of being able to form complex shapes. However, this advantage is currently limited by the difficulty in removing unbound material particles.

[0008] For example, if the sintered body has a hollow structure with a cavity inside, unbound material particles will remain in the closed cavity, and in order to remove the unbound material particles, it will be necessary to modify the structure of the sintered body. To make it easier for a brush or compressed air to reach the cavity, it will be necessary to provide an opening that connects to the cavity or to provide a dividing structure that opens the cavity.

[0009] Furthermore, when the sintered body has a complex structure with narrow gaps, it is difficult to remove the unbound material particles remaining in the gaps. Precursors in which material particles are bound together tend to have low mechanical strength because their shape is maintained by the binder. When unbound material particles remain in narrow gaps, such as in comb-shaped or groove-shaped areas, attempting to remove them with a brush or compressed air places a heavy load on the precursor, easily damaging it.

[0010] In Patent Document 1, injection-molded bodies and intermediate molded bodies obtained after degreasing of the injection-molded bodies are deformed by gravity. However, the injection-molded bodies must be molded into a shape without undercuts that allows them to be removed by dividing the injection mold. The technology in Patent Document 1 is difficult to apply to shapes with undercuts. On the other hand, when binder jetting-based additive manufacturing is used, problems arise with the removal of unbound material particles.

[0011] Therefore, the present invention aims to provide a method for manufacturing a sintered body that can easily remove unnecessary material particles that adhere to the cavities and gaps of the sintered body, a sintered body made using this method, and a molding mold to be used for this sintered body.

[0012] In order to solve the above-mentioned problems, the method for producing a sintered body according to the present invention is a method for producing a sintered body in which material particles are sintered together, and includes a molding step of molding a precursor using a molding material containing material particles and a binder, and a heat treatment step of heat-treating the precursor on a molding mold to form a sintered body, wherein the sintered body has a hollow structure with an internal cavity or a complex structure with gaps that are open to the outside, and the precursor is molded into a shape in which the portions that form the cavity are separated from each other and the cavity is open, or a shape in which the portions that form the gaps are spaced apart, and the molding mold has an inclined surface on its upper surface, and in the heat treatment step, the precursor is placed on the molding mold and deformed into a shape in which the portions that form the cavity are in contact with each other and the cavity is closed, or into a shape in which the portions that form the gaps are reduced, and then the precursor is heat-treated to be sintered.

[0013] Furthermore, the sintered body according to the present invention is a sintered body formed by sintering material particles together, and the sintered body has a hollow structure with a cavity inside, and the parts forming the cavity are in contact with each other, thereby closing the cavity, or has a complex structure with gaps that are open to the outside, and the distance between the parts forming the gaps is smaller than before sintering, and the lower surface of the sintered body has a ridge shape in which homologous shapes protrude downward along one axial direction, and the ridge shape has an inclined surface that slopes upward from the center of the lower surface toward the outside in a cross-sectional view of the sintered body, and the unsintered material particles in the cavity or the unsintered material particles in the gaps have been removed.

[0014] Furthermore, the molding mold of the present invention is a molding mold used to mold a sintered body in which material particles are sintered together, and the molding mold has an inclined surface on the upper surface on which the precursor is placed, and the sintered body has a hollow structure with a cavity inside, or a complex structure with gaps that are open to the outside, and the precursor is molded into a shape in which the parts that form the cavity are separated at the upper side and the cavity is open toward the top, or a shape in which the spaces between the parts that form the gaps are open toward the top, and is placed on the inclined surface.

[0015] According to the present invention, it is possible to provide a method for manufacturing a sintered body that can easily remove unnecessary material particles that adhere to the cavities and gaps of the sintered body, a sintered body made using this method, and a molding mold used for this sintered body.

[0016] FIG. 1 is a flowchart showing a method for manufacturing a sintered body according to an embodiment of the present invention. FIG. 1 is a cross-sectional view showing a main part of a binder jetting type additive manufacturing apparatus. FIG. 1 is a cross-sectional view showing a main part of a binder jetting type additive manufacturing apparatus. FIG. 1 is a cross-sectional view showing a main part of a binder jetting type additive manufacturing apparatus. FIG. 1 is a cross-sectional view showing a main part of a binder jetting type additive manufacturing apparatus. FIG. 1 is a cross-sectional view showing a main part of a binder jetting type additive manufacturing apparatus. FIG. 1 is a cross-sectional view showing a main part of a binder jetting type additive manufacturing apparatus. FIG. 1 is a cross-sectional view showing a main part of a binder jetting type additive manufacturing apparatus. FIG. 1 is a cross-sectional view showing a main part of a binder jetting type additive manufacturing apparatus. 1 is a diagram showing a manufacturing method for manufacturing a sintered body having a complex structure with gaps, and FIG 2 is a diagram showing a manufacturing method for manufacturing a sintered body having a complex structure with gaps.

[0017] Hereinafter, a method for producing a sintered body according to one embodiment of the present invention, a sintered body using the same, and a molding mold used therefor will be described with reference to the drawings. In the following drawings, common components are designated by the same reference numerals, and duplicated explanations will be omitted.

[0018] The method for producing a sintered body according to this embodiment relates to a method for producing a sintered body in which material particles are sintered together. In this method, material particles are bound with a binder to form a precursor of the sintered body, which has a shape with open cavities and gaps. The precursor is then deformed in a mold to form a shape with closed cavities and gaps, and then sintered by heat treatment. The precursor can be formed by additive manufacturing using a binder jetting method.

[0019] Generally, when material particles are bound together with a binder to form a shape, unbound material particles remain around the periphery of the object. In binder jetting additive manufacturing, the material particles are supplied as a powder bed, and then the binder is sprayed onto the material particles within the building area to form a bonded layer in which the material particles are bound together. On the other hand, the binder is not sprayed onto particles outside the building area, so the unbound material particles remain as powder.

[0020] Unbound material particles that are not bound by the binder remain attached to the surface of the sintered body, and therefore must be removed from the surface of the sintered body. A sintered body in which material particles are bound together may be subjected to heat treatment to remove the binder and sinter the material particles together. When a sintered body is heat-treated, if unbound material particles adhere to the surface, the unbound material particles will also be sintered. Sintering of unnecessary material particles will affect the shape of the sintered body, so they must be removed before heat treatment.

[0021] When producing sintered bodies with hollow structures or complex structures with narrow gaps, it is difficult to remove unbound material particles remaining in the cavities or gaps. To remove material particles from the cavities, it is necessary to create openings in the precursor or to provide the precursor with a divided structure. Furthermore, when removing material particles from the gaps, a large load is applied to the surface of the precursor due to contact with a removal tool such as a brush or the use of compressed air. Because precursors bound by a binder have low strength, they may be damaged when removing unbound material particles.

[0022] Therefore, in the method for producing a sintered body according to this embodiment, a precursor of the sintered body is formed as a precursor of a predetermined shape, which has an open three-dimensional shape with a surface widely exposed to the outside and which is deformed in a molding die to become the target shape of the sintered body. Furthermore, a molding die of a predetermined shape with a slope formed therein for deforming the precursor is used as the molding die. This precursor is deformed in the molding die into a closed three-dimensional shape, and then sintered to produce a sintered body.

[0023] Fig. 1 is a flowchart showing a method for producing a sintered body according to an embodiment of the present invention. As shown in Fig. 1, the method for producing a sintered body according to this embodiment includes a molding step S10, a removing step S11, and a heat treatment step S12. The removing step S11 can be performed after the molding step S10 and before the heat treatment step S12, as necessary.

[0024] The method for producing a sintered body according to this embodiment produces a sintered body with a hollow structure having cavities inside, or a sintered body with a complex structure having narrow gaps on the surface or inside. The sintered body may have only cavities, only gaps, or both. The cavities and gaps may or may not be connected to each other. There are no particular limitations on the shape, number, and size of the cavities or the shape, number, and size of the gaps.

[0025] The cavity may be a space that is closed to the outside, or a space that is partially open to the outside. The gap may be a bottomed structure that does not penetrate the part, or a through-hole structure that penetrates the part. The gap may have any shape, such as a groove shape, a depression shape, a slit shape, a through-window shape, a comb shape, or a gap shape, or may be any structure formed between parts of any three-dimensional shape.

[0026] The molding step S10 is a step of molding a precursor of a sintered body that will have a desired target shape after deformation on a molding die using a molding material containing material particles and a binder. The precursor can be molded by additive manufacturing using a binder jetting method, or by three-dimensional molding in which a molding material containing material particles and a binder is patterned into a predetermined three-dimensional shape.

[0027] In the molding step S10, when a sintered body having a hollow structure with an internal cavity is produced, a precursor having an open cavity shape with the portions forming the cavity spaced apart from each other is molded. When a sintered body having a complex structure with narrow gaps is produced, a precursor having an open cavity shape with the portions forming the gaps spaced apart from each other is molded.

[0028] From the viewpoint of utilizing deformation of the precursor due to its own weight, the cavity or gap is preferably formed in a shape that is open toward the top of the precursor. The cavity or gap is preferably formed in an open shape that allows at least unbound material particles remaining in the cavity or gap to be discharged, and more preferably is formed in a shape that is open enough to allow the insertion of a removal tool used to remove the unbound material particles.

[0029] Examples of shapes in which the portions forming the cavity are separated from each other to form an open cavity include a shape such as a split in which, in a cross-sectional view of the precursor, at least a portion of the outer periphery of the cavity penetrates toward the outside, and a gap formed between the portions connects the inside of the cavity to the outside of the precursor. Examples of shapes in which the portions forming the gap are spaced apart include a shape in which the distance between the tip ends of the portions forming the gap is larger than the distance between the base ends, and the distance between the portions is open at an arbitrary angle.

[0030] The material particles may be metal particles, ceramic particles, or the like. A sintering aid or a lubricant such as metal soap may be added to the material particles. The particle size of the material particles is not particularly limited, but from the viewpoints of the packing property of the material particles, the molding accuracy and sinterability of the precursor, etc., it is preferably 1 μm or more and 300 μm or less, more preferably 10 μm or more and 150 μm or less, and even more preferably 20 μm or more and 100 μm or less.

[0031] Metal particles are not particularly limited, but include particles formed of iron, cobalt, nickel, copper, titanium, aluminum, tungsten, molybdenum, tantalum, and alloys thereof. Iron alloys include carbon steel, alloy steel, stainless steel, and iron-nickel alloys. Cobalt alloys include cobalt-chromium alloys. Nickel alloys include nickel-iron alloys, nickel-chromium alloys, nickel-chromium-iron alloys, and nickel-copper alloys.

[0032] The ceramic particles are not particularly limited, but examples thereof include oxides such as aluminum oxide, zirconium oxide, cerium oxide, silicon oxide, tin oxide, titanium oxide, vanadium oxide, chromium oxide, zinc oxide, and niobium oxide, nitrides such as silicon nitride, aluminum nitride, and boron nitride, carbides such as silicon carbide, boron carbide, and tungsten carbide, and particles formed from glass materials.

[0033] Examples of binders that can be used include resin-based binders such as polyvinyl alcohol, polyvinylpyrrolidone, polyethylene, polypropylene, polystyrene, polyvinyl chloride, polyvinylidene chloride, polyester, acrylic resin, and polyacetal resin, and wax-based binders such as paraffin wax, polyethylene wax, carnauba wax, microcrystalline wax, and fatty acid ester.

[0034] The removal step S11 is a step of removing unbound material particles that are attached to the precursor of the sintered body but are not bound by a binder. The unbound material particles can be removed by an appropriate method, such as sweeping with a brush or the like, spraying with high-pressure gas such as compressed air using an air gun or the like, or suction using a vacuum gun or the like.

[0035] In the removal step S11, for a precursor formed into a shape in which portions forming cavities are separated from each other and the cavities are open, it is preferable to remove at least unbound material particles remaining in the cavities, such as material particles adhering to the inner surfaces of the portions forming the cavities. Also, for a precursor formed into a shape in which portions forming gaps are spaced from each other, it is preferable to remove at least unbound material particles remaining in the gaps, such as material particles adhering to the inner surfaces of the portions forming the gaps.

[0036] The heat treatment step S12 is a step of heat treating the precursor of the sintered body on a mold to form a sintered body. The heat treatment of the precursor is performed by placing the precursor formed into a predetermined shape on a predetermined mold having an inclined surface on its upper surface. The heat treatment of the precursor can be performed by placing the mold on which the precursor is placed in an appropriate heat treatment furnace, such as a batch heating furnace such as an electric furnace, a continuous heating furnace, or the like.

[0037] In the heat treatment step S12, when a sintered body having a hollow structure with an internal cavity is produced, a precursor having a shape in which the portions forming the cavity are separated and the cavity is open is placed on the inclined surface of the mold, and the precursor is deformed into a shape in which the portions forming the cavity are in contact and the cavity is closed, and then sintered. Also, when a sintered body having a complex structure with narrow gaps is produced, a precursor having a shape in which the portions forming the gaps are spaced apart is placed on the inclined surface of the mold, and the precursor is deformed into a shape in which the spaces between the portions forming the gaps are narrowed, and then sintered.

[0038] The precursor is preferably deformed by its own weight using the inclined surface formed on the mold. It is preferable that a large external force is not applied to the precursor. When the precursor is deformed by its own weight, an external force is not required to deform the precursor into a shape that closes cavities and gaps, so that a situation in which a large load is applied to the precursor can be avoided. Even if the precursor has low strength, damage during deformation can be reduced, and a sintered body with high shape precision can be produced.

[0039] The molding mold can be formed from an appropriate heat-resistant material, such as metal materials such as stainless steel, carbon tool steel, alloy tool steel, high-speed tool steel, iron, nickel, tantalum, etc., or ceramic materials such as silicon nitride, boron carbide, alumina, zirconia, quartz, etc. As the molding mold, a molding mold that has been plated with nickel plating, chrome plating, etc., or a molding mold that has been coated with heat-resistant ceramics, etc., may be used.

[0040] The heat treatment of the precursor may be performed in a single stage or in multiple stages. The heat treatment of the precursor may be performed, for example, by combining a degreasing treatment for degreasing the binder and a firing treatment for firing the degreasing precursor. The temperature, time, atmosphere, etc. of the heat treatment may be set as appropriate depending on the type of material particles, etc. The molding mold may be coated with a lubricant such as metal soap or fatty acid ester, a solid mold release agent such as boron nitride or graphite, or a fluid mold release agent such as wax or silicone, as needed.

[0041] The use of the sintered body is not particularly limited. Examples of uses of the sintered body include parts for mobile bodies such as automobiles, motorcycles, railway vehicles, ships, and aircraft, parts for electrical equipment such as vacuum cleaners, washing machines, air conditioners, televisions, personal computers, telephones, mobile phones, and tablets, parts for industrial machinery, parts for power equipment such as generators, power supply units, and power conversion units, parts for plant equipment, and the manufacture of prototypes by rapid prototyping.

[0042] 2 to 9 are cross-sectional views showing the main parts of a binder jetting additive manufacturing apparatus. The molding step S10 can be performed using such a binder jetting additive manufacturing apparatus.

[0043] Fig. 2 shows the state before the start of modeling. Fig. 3 shows the state where the material particles are being spread. Fig. 4 shows the state where a powder bed has been formed. Fig. 5 shows the state where a binder is being sprayed to form a bond layer. Fig. 6 shows the state where the material particles of the next layer are being spread. Fig. 7 shows the state where a powder bed of the next layer is being formed. Fig. 8 shows the state where a binder is being sprayed to form a bond layer of the next layer. Fig. 9 shows the state where the precursor has been modeled.

[0044] 2 to 9, in binder jetting additive manufacturing, a binder is sprayed onto a powder bed formed of material particles to form a bonded layer in which the material particles are bonded together by the binder. By repeating the formation of the powder bed and the formation of the bonded layer by spraying the binder in the stacking direction, a precursor in which the material particles are bonded together in a predetermined three-dimensional shape is molded.

[0045] 2 to 9, the additive manufacturing apparatus includes a material supply unit 110, an additive manufacturing unit 120, a recovery unit 130, a material supply stage 111, a recoater 112, an additive manufacturing stage 121, and a spraying means 122. The material supply unit 110, the additive manufacturing unit 120, and the recovery unit 130 are housed in a chamber (not shown). A continuous work plane is formed at the upper ends of the material supply unit 110, the additive manufacturing unit 120, and the recovery unit 130 for performing an operation to form a bonding layer.

[0046] The material supply unit 110 is a portion that supplies material particles 100 to the additive manufacturing unit 120, and includes a material supply stage 111. The material supply stage 111 is housed in a shaft space that extends downward from the work plane as its upper end. The material supply stage 111 is provided so as to be movable up and down within the shaft space. The periphery of the material supply stage 111 is surrounded by walls that form the shaft space.

[0047] The additive manufacturing unit 120 is a part where additive manufacturing is performed by injecting a binder onto the material particles 100, and is equipped with an additive manufacturing stage 121 and an injection means 122. The additive manufacturing stage 121 is housed in a shaft space that extends downward from the work plane as its upper end. The additive manufacturing stage 121 is provided so as to be movable up and down within the shaft space. The additive manufacturing stage 121 is surrounded by walls that form the shaft space.

[0048] The recovery unit 130 is a portion for recovering excess material particles 100 that were not used in modeling. The recovery unit 130 is formed as a container-like space that opens onto the work plane, with the work plane as its upper end. The recovery unit 130 is provided on the opposite side of the material supply unit 110 with respect to the additive manufacturing unit 120.

[0049] The recoater 112 is a device that spreads the material particles 100. The recoater 112 is provided so as to be movable in both directions on a work plane from the material supply unit 110 to the recovery unit 130 via the additive manufacturing unit 120. The recoater 112 is formed of a roller, a squeegee, or the like. The recoater 112 moves while substantially in contact with the work plane, moving the material particles 100 on the work plane and spreading them into layers.

[0050] The spraying means 122 is composed of a dispenser that sprays a solution containing a binder, an inkjet printer head, or the like. The spraying means 122 is connected via a pipeline to a tank (not shown) in which the solution containing the binder is prepared. The spraying means 122 is provided above the additive manufacturing stage 121 so as to be movable in at least two axial directions parallel to the work plane. The movement of the spraying means 122 above the additive manufacturing stage 121 and the spraying of the binder are controlled according to the three-dimensional shape to be formed.

[0051] As shown in Fig. 2, material particles 100 are fed onto the material supply stage 111. At the start of additive manufacturing, the material supply stage 111 waits so that the upper surface of the material supply stage 111 is at a low position below the work plane. During additive manufacturing, the upper surface of the material supply stage 111 rises stepwise from a low position upward for each individual layering process. Through this operation, the material particles 100 fed onto the material supply stage 111 are supplied onto the work plane for each individual layering process.

[0052] 3, material particles 100 supplied onto the work plane of the material supply unit 110 are carried to the additive manufacturing unit 120 by the movement of the recoater 112. The material particles 100 are spread onto an additive manufacturing stage 121 waiting at a position slightly lower than the work plane.

[0053] 4, material particles 100 are spread onto an additive manufacturing stage 121 to form a powder bed. Excess material particles 100 above the work plane are pushed by a recoater 112 to a recovery section 130 for recovery. After forming a powder bed that will become the raw material for the individual bond layers 101, the recoater 112 is returned to its initial position in the material supply section 110.

[0054] As shown in Figure 5, in the additive manufacturing unit 120 where the powder bed is formed, a binder is sprayed onto the powder bed by a spraying means 122. The spraying means 122 sprays the binder in a predetermined pattern based on slice data corresponding to the target three-dimensional shape of the precursor. The slice data is data for each layer obtained by dividing the target three-dimensional shape to be manufactured in the thickness direction, and indicates the two-dimensional shape of the manufacturing area for each layer. The spraying of the binder forms a bonded layer 101 in which material particles 100 are bonded together.

[0055] As shown in Figures 6 to 8, once a bond layer 101 is formed by each lamination process, the lamination process for the next layer of bond layer 101 is carried out on the already formed bond layer 101 in the same manner as in Figures 3 to 5. In the lamination process for the next layer, the material supply stage 111 is raised in stages, and new material particles 100 are supplied onto the work plane. In addition, the additive manufacturing stage 121 is lowered in stages, and a space for forming the next layer of powder bed is formed between the upper surface of the already formed bond layer 101 and the work plane.

[0056] As shown in Figure 9, repeated lamination of patterned binder layers 101 results in the formation of a precursor 102 of a sintered body having a predetermined three-dimensional shape. A precursor of a predetermined shape, which deforms on a mold and closes into the target shape, can be formed by this binder jetting additive manufacturing method. Because the precursor 102 has unbound material particles 100 adhering thereto, which form a powder bed, it is preferable to subject the precursor 102 to a removal step S11 in which the unbound material particles are removed.

[0057] Binder jetting additive manufacturing can produce shapes with high shape and dimensional accuracy, such as open-cavity shapes where the parts that form cavities are separated from each other, or shapes with gaps between parts that form gaps. Even if these shapes have undercuts or structures where parts are connected by thin bridges, they can be produced in one go with high accuracy without dividing into parts.

[0058] 10 to 14 are diagrams showing an example of a manufacturing method for manufacturing a sintered body with a hollow structure having a cavity inside. FIG. 10 is a cross-sectional view showing an example of the completed form of a precursor of a sintered body. FIG. 11 is a cross-sectional view showing the precursor formed in the forming step S10. FIG. 12 is a cross-sectional view showing the precursor from which unbound material particles have been removed in the removing step S11. FIG. 13 is a cross-sectional view showing the precursor before deformation placed on a mold in the heat treatment step S12. FIG. 14 is a cross-sectional view showing the precursor after deformation placed on a mold in the heat treatment step S12.

[0059] 10 to 14, when producing a sintered body having a hollow structure with an internal cavity, a precursor 10 of the sintered body can be provided so as to have a finished shape in which the cavity 11 is closed at a plurality of portions 10a, 10b. In the following explanation, a process for forming the finished shape of the precursor 10 shown in Fig. 10 will be exemplified. The shape in the cross section shown in Fig. 10 is assumed to be homologous and continuous over a certain length along one axial direction (depth direction in the figure) perpendicular to the cross section.

[0060] 11 , when manufacturing a sintered body having a hollow structure with an internal cavity, in the molding step S10, a precursor 10 is molded in which the portions 10a and 10b forming the cavity are separated from each other and the cavity is open. Such a precursor 10 can be molded by repeatedly forming bonding layers in the stacking direction in additive manufacturing using the binder jetting method.

[0061] The cavity-forming portions 10a and 10b can be formed by stacking layers of material particles bound together by the binder using a molding material containing material particles and a binder. When additive manufacturing is performed, a state is obtained in which unbound material particles 100 that were present in the non-printing region of the powder bed remain between the portions 10a and 10b.

[0062] In Fig. 11, the portions 10a and 10b that form the cavity are provided in a shape that divides the cavity 11 in two in the left-right direction. Compared to the finished shape (see Fig. 10), each of the portions 10a and 10b is formed in a shape that is inclined so that the upper side opens outward, with the vicinity of the center of the lower part as a fulcrum. With this shape, the weight of the precursor 10 can deform in a direction that closes the upper side, with both side edges of the precursor 10 as fulcrums.

[0063] The portions 10a, 10b forming the cavity are formed so as to be spaced apart from each other as they move from the bottom to the top of the precursor 10. The portions 10a, 10b are molded so that their inclined inner surfaces 12 face each other. The portions 10a, 10b can be molded so that the inner surfaces 12 intersect the contour line of the cavity 11 at an appropriate position in a cross-sectional view of the precursor 10. The inner surfaces 12 serve as bonding surfaces for sintering the portions 10a, 10b together after the precursor 10 is deformed. When the portions 10a, 10b are formed so as to be spaced apart on one side, the cavity 11 can be opened to the outside by deformation on the molding mold 20.

[0064] The interior angle of the inclination formed by the inner surfaces 12 on the inside of each portion 10a, 10b, i.e., the angle α at which the cavity 11 opens outward, can be set to any angle as long as it is compatible with the molding mold 20. From the viewpoints of the ease of removing unbound material particles 100 and the closure of each portion 10a, 10b during deformation, the angle α at which the cavity 11 opens outward is preferably 10 degrees or more and 90 degrees or less, and more preferably 20 degrees or more and 45 degrees or less.

[0065] The lower surfaces 13 of the cavity-forming portions 10a, 10b are preferably formed as the same horizontal surface between the opposing portions 10a, 10b. The horizontally continuous lower surface 13 can be easily formed using a single bonding layer during additive manufacturing. Forming the horizontally continuous lower surface 13 using a single bonding layer increases the smoothness of the lower surface 13. Therefore, when the precursor 10 is deformed on the molding mold 20, misalignment between the cavity-forming portions 10a, 10b can be reduced.

[0066] The portions 10a and 10b forming the cavity may be molded to have a structure in which they are connected to each other, or may be molded to have a structure in which they are not connected to each other, but from the viewpoints of handling the precursor 10 and positioning the portions 10a and 10b relative to each other, it is preferable that they be molded to have a structure in which they are connected to each other.

[0067] The portions 10a, 10b can be connected to each other by forming a bridge portion, for example, at the lower portion where the lower surfaces 13 are connected. The bridge portion can be provided on all or part of each portion 10a, 10b along the center line between the portions 10a, 10b that form the cavity (the center line that is perpendicular to the dashed dotted line in the drawing and extends in the depth direction in the drawing).

[0068] 12 , in the removal step S11, unbound material particles 100 remaining between the portions 10a, 10b forming the cavity are removed. Because the portions 10a, 10b are separated from each other on one side, the unbound material particles 100 adhering to the inner surface of the cavity 11 can be easily removed. This makes it easy to insert a brush, air gun, vacuum gun, etc., and to remove the material particles 100, resulting in a state in which fewer unbound material particles 100 remain in the cavity 11.

[0069] As shown in Fig. 13 , in the heat treatment step S12, the precursor 10 of the sintered body is placed on a mold 20 having a predetermined shape. The mold 20 is provided with an inclined surface 21 on its upper surface. In Fig. 13 , the inclined surface 21 is provided as a linear incline in a cross-sectional view of the mold 20. The inclined surface 21 is formed line-symmetrically with respect to the center of the mold 20, and forms an inverted triangular shape (V-shape) in a cross-sectional view of the mold 20.

[0070] The inclined surfaces 21 are provided so that the center is lower than the outside in a cross-sectional view of the mold 20. The inclined surfaces 21 are preferably provided so that inclinations of this direction face each other. The inclined surfaces 21 are formed so that the shape of the cross-sectional view shown in FIG. 13 continues homologously for a certain length along one axial direction (depth direction in the figure) perpendicular to the cross-section. Such inclined surfaces 21 form groove-shaped recesses for deforming the overall shape of the precursor 10.

[0071] The molding die 20 is provided so that the cross-sectional shape of the groove shape formed by the inclined surfaces 21 matches the cross-sectional shape of the lower surface of the completed precursor 10. The interior angle of the slope formed by the inclined surfaces 21, i.e., the angle β of the bottom surface of the groove shape formed on the upper surface of the molding die 20, can be set to any angle as long as it matches the shape of the lower surface of the precursor 10. The angle β of the bottom surface of the groove shape is preferably 90 degrees or more and 170 degrees or less, and more preferably 135 degrees or more and 160 degrees or less.

[0072] The precursor 10 is placed on the mold 20 so that the center line between the portions 10a, 10b that form the cavity (a center line that is perpendicular to the dashed dotted line in the figure and extends in the depth direction in the figure) coincides in plan view with the center line of the groove shape formed by the inclined surface 21 of the mold 20 (a center line that is perpendicular to the dashed dotted line in the figure and extends in the depth direction in the figure) and is aligned vertically upward and parallel. With this arrangement, the portions 10a, 10b are aligned along the inclined surface 21, and therefore the portions 10a, 10b can be appropriately inclined along the inclined surface 21 to accurately close the cavity 11.

[0073] 14, in the heat treatment step S12, the precursor 10 of the sintered body is placed on a molding die 20, and the entire shape of the precursor 10 is deformed in a direction to close. The portions 10a and 10b forming the cavity are placed on an inclined surface 21, and each portion 10a and 10b is inclined inward along the inclined surface 21, whereby the cavity 11 open to the outside can be deformed into a closed shape. The deformation of the entire shape of the precursor 10 can be achieved by the weight of the precursor 10 itself.

[0074] When the precursor 10 is placed on the mold 20 and deformed, the completed precursor 10 shown in Fig. 10 is obtained. The lower surfaces 13 of the portions 10a, 10b are in contact with the inclined surfaces 21 of the mold 20. The inner surfaces 12 of the portions 10a, 10b are in close contact with each other. The completed precursor 10 is heat-treated to sinter the material particles 100 that form the precursor 10, and to sinter the portions 10a, 10b that form the cavities, with the inner surfaces 12 as bonding surfaces.

[0075] According to this method for manufacturing a sintered body, a sintered body having a hollow structure with an internal cavity and in which unbound material particles remaining in the cavity have been removed is obtained. The sintered body has a shape in which the portions forming the cavity come into contact with each other, closing the cavity. The shape of the lower surface of the sintered body in cross section is homologous to the shape of the bottom surface of the groove shape of the molding mold in cross section, with a homologous protrusion protruding downward along one axial direction. The lower surface of the sintered body has a shape on both sides of the center that slopes upward from the center toward the outside of the lower surface in cross section. Furthermore, the portions forming the cavity are obtained in a state in which they are sintered at the joining surfaces that intersect with the cavity in cross section.

[0076] According to the above-described manufacturing method and mold for a sintered body, even when a sintered body having a hollow structure with an internal cavity is manufactured, a precursor having a shape in which the portions forming the cavity are separated from each other and the cavity is open upward is used, so that unnecessary material particles adhering to the inside of the cavity of the sintered body can be easily removed before the heat treatment to close the cavity. Therefore, damage caused by the removal of material particles is reduced, and a sintered body with high shape precision can be manufactured in which unnecessary material particles are not sintered to the inner surface of the cavity.

[0077] 10 to 14, the gaps that open the cavities are provided on the upper side of the precursor 10, but such gaps may be formed on the side of each bonding layer during additive manufacturing. That is, additive manufacturing may be performed in an orientation such that the shape in cross section shown in FIG. 11 becomes the shape in plan view.

[0078] 10 to 14, the precursor 10 is provided in a polygonal shape having a circular cavity 11 in cross section, but the precursor of the sintered body can be provided in any suitable three-dimensional shape having a cavity of any suitable shape, as long as it is molded into a shape with an open cavity and then deformed into a shape that closes the cavity by the inclined surface provided in the molding die.

[0079] Each portion forming the cavity of the precursor may be provided in a symmetrical shape that divides the cavity line-symmetrically, or in an asymmetrical shape that divides the cavity non-symmetrically. Furthermore, the portion forming the cavity of the precursor may be composed of a single portion or multiple portions in a direction perpendicular to the cross section of the precursor (a direction perpendicular to the dashed dotted line in the drawing and extending in the depth direction in the drawing).

[0080] The precursor of the sintered body may also be molded into a three-dimensional shape having an undercut by additive manufacturing. The portion of the precursor that forms the cavity may have an undercut portion in both the cross section of the precursor and the longitudinal section parallel to the direction perpendicular to the cross section. The undercut may be provided in a portion other than the cavity 11 in the cross section or longitudinal section. Examples of undercuts include three-dimensional shapes that are difficult to demold in their original form, such as a convex shape with a protrusion protruding in a direction other than the demolding direction, a concave shape with a recessed portion recessed in that direction, a shape with a bent gap internally, or a shape in which the width of a portion changes along an arbitrary direction so that the portion and the mold interfere in that direction. Such three-dimensional shapes can be molded in one go using additive manufacturing.

[0081] The molding die can be formed in an appropriate shape depending on the shape of the finished shape of the precursor and how the precursor is to be deformed, as long as it has an inclined surface that inclines the portion of the precursor that forms the cavity and deforms it into a shape that closes the cavity. The shape of the molding die can be designed to close the cavity by inclining the precursor using an appropriate moment, depending on the shape, material, etc. of the precursor.

[0082] In Figures 13 and 14, the inclined surface 21 forms an inverted triangular shape when viewed in cross section of the molding mold 20, but it may also be formed into an inverted trapezoidal shape, a partial polygonal shape, a partial arc shape, a partial elliptical arc shape, etc., depending on the shape of the side surfaces on both sides of the precursor 10.

[0083] The inclined surface 21 is formed in line symmetry with respect to the center of the mold 20 and is provided to correspond to both of the portions where the cavities are formed, but the inclined surface that deforms the shape to close the cavities may be provided to correspond to one of the portions where the cavities are formed. A horizontal surface may also be provided as the surface that corresponds to the other portion where the cavities are formed.

[0084] However, it is preferable that the mold has inclined surfaces that deform the cavity into a shape that closes the cavity, and that the inclined surfaces face each other in a direction that makes the center lower than the outside. With such a shape, compared to when the inclined surfaces are asymmetric, uneven deformation of one part of the cavity due to the weight of the other part can be reduced, thereby improving the closure of the cavity and the shape precision of the sintered body. The angle between the inclined surface and the horizontal plane is preferably 5 degrees or more and 45 degrees or less, and more preferably 10 degrees or more and 45 degrees or less.

[0085] The mold may have a combination of multiple inclined surfaces, each with a different angle or direction, as an inclined surface that deforms the cavity into a shape that closes the cavity, in addition to an inclined surface facing the inclined surface. The portions that form the cavity of the precursor may be provided at any number of positions, three or more, in the direction of the cross section or in a direction perpendicular to the cross section (the direction perpendicular to the dashed dotted line in the drawing and extending in the depth direction in the drawing).

[0086] In such cases, the angle and direction of deformation can be changed for each region, and an inclined surface corresponding to each region or an inclined surface opposite the inclined surface can be provided. The precursor can be placed on the mold so that the center lines between the multiple regions forming the cavities are aligned vertically upward and parallel to the tip lines of the inclined surfaces or the center lines between the opposing inclined surfaces in a plan view. The cavities can be closed by folding the multiple regions by deforming them at different angles and directions.

[0087] 15 to 19 are diagrams showing an example of a manufacturing method for manufacturing a sintered body having a complex structure with narrow gaps. FIG. 15 is a cross-sectional view showing an example of the completed form of a precursor of a sintered body. FIG. 16 is a cross-sectional view showing the precursor formed in the forming step S10. FIG. 17 is a cross-sectional view showing the precursor from which unbound material particles have been removed in the removing step S11. FIG. 18 is a cross-sectional view showing the precursor before deformation placed on a mold in the heat treatment step S12. FIG. 19 is a cross-sectional view showing the precursor after deformation placed on a mold in the heat treatment step S12.

[0088] 15 to 19, when producing a sintered body with a complex structure having narrow gaps, the portions 10d forming the gaps 14 can be supported by the portions 10c forming the base, and the portions 10d forming the gaps 14 can be arranged so that they change from an open shape to a closed, completed shape. In the following explanation, the process of forming the completed shape of the precursor 10 shown in FIG. 15 will be exemplified. The shape in the cross-sectional view shown in FIG. 15 is assumed to be homologous and continuous for a certain length along one axial direction (depth direction in the figure) perpendicular to the cross-section.

[0089] 16 , when manufacturing a sintered body with a complex structure having narrow gaps, in the molding step S10, a precursor 10 is molded in a shape in which the portions 10d that form the gaps 14 are spaced apart from one another. Such a precursor 10 can be molded by repeatedly forming bonding layers in the stacking direction in additive manufacturing using the binder jetting method.

[0090] The portions 10d that form the gaps 14 can be formed by stacking layers of material particles bound together by the binder using a molding material containing material particles and a binder. When additive manufacturing is performed, a state is obtained in which unbound material particles 100 that were present in the non-printing region of the powder bed remain between the portions 10d, but are not bound together by the binder.

[0091] 16, the portions 10d forming the gaps 14 are formed in a shape that expands the spacing of the gaps 14 in the completed form. Compared to the completed form (see FIG. 15), each portion 10d is formed in a shape that is inclined so that the upper side opens outward, with the center of the lower part as a fulcrum, in a cross-sectional view of the precursor 10. With this shape, the weight of the precursor 10 can deform in a direction that closes the upper side, with both side edges of the precursor 10 as fulcrums.

[0092] The portions 10d that form the gaps 14 are formed so as to be spaced apart from one another as they move from the bottom to the top of the precursor 10. When the portions 10d are formed so as to be spaced apart from one another at the top, the gaps 14 can be opened to the outside by deformation on the molding die 20. Multiple pairs of the portions 10d that form the gaps 14 are provided, and a shape in which multiple gaps 14 are arranged in parallel is molded. The spacing between each gap 14 can be expanded relative to a central axis (indicated by a dashed line in the figure) located at the center of the multiple portions 10d.

[0093] The interior angle of the inclination formed on the inside of each portion 10d, i.e., the angle γ at which the gap 14 is opened outward, can be set to any angle as long as it is compatible with the molding mold 20. From the viewpoints of the ease of removing unbound material particles 100 and the ability of the portions 10d to close when deforming, the angle γ at which the gap 14 is opened outward is preferably 10 degrees or more and 90 degrees or less, and more preferably 20 degrees or more and 45 degrees or less.

[0094] The lower surface of the base-forming portion 10c is preferably formed as a horizontal surface. A horizontally continuous lower surface can be easily formed using a single adhesive layer during additive manufacturing. Forming a horizontally continuous lower surface using a single adhesive layer increases the smoothness of the lower surface. Therefore, when the precursor 10 is deformed on the molding mold 20, misalignment between the portions 10d that form the gap 14 can be reduced.

[0095] 17 , in the removal step S11, unbound material particles 100 remaining between the portions 10d that form the gap 14 are removed. Because the portions 10d are separated from each other on one side, it is possible to easily remove the unbound material particles 100 that have adhered to the inner surface of the gap 14. This makes it easy to insert a brush, air gun, vacuum gun, etc., and to discharge the material particles 100, resulting in a state in which fewer unbound material particles 100 remain in the gap 14.

[0096] As shown in Fig. 18 , in the heat treatment step S12, the precursor 10 of the sintered body is placed on a mold 20 having a predetermined shape. The mold 20 is provided with an inclined surface 21 on its upper surface. In Fig. 18 , the inclined surface 21 is provided as a curved inclination in a cross-sectional view of the mold 20. The inclined surface 21 is formed line-symmetrically with respect to the center of the mold 20, and forms a partial elliptical arc in a cross-sectional view of the mold 20.

[0097] The inclined surfaces 21 are provided so that the center is lower than the outside in a cross-sectional view of the mold 20. The inclined surfaces 21 are preferably provided so that inclinations of this direction face each other. The inclined surfaces 21 are formed so that the shape of the cross-sectional view shown in FIG. 18 continues homologously for a certain length along one axial direction (depth direction in the figure) perpendicular to the cross-section. Such inclined surfaces 21 form groove-shaped recesses for deforming the overall shape of the precursor 10.

[0098] The molding die 20 is provided so that the cross-sectional shape of the groove shape formed by the inclined surface 21 matches the cross-sectional shape of the lower surface of the completed precursor 10. The curvature of the slope formed by the inclined surface 21, i.e., the curvature of the bottom surface of the groove shape formed on the upper surface of the molding die 20, can be set to any appropriate curvature as long as it matches the shape of the lower surface of the precursor 10.

[0099] The precursor 10 is placed on the mold 20 so that the center lines between the portions 10d that form the gaps 14 (center lines that are perpendicular to the dashed dotted line in the figure and extend in the depth direction in the figure) coincide in plan view with and are aligned vertically upward and parallel to the center lines of the groove shapes formed by the inclined surfaces 21 of the mold 20 (center lines that are perpendicular to the dashed dotted line in the figure and extend in the depth direction in the figure). With this arrangement, the portions 10c that form the bases are aligned along the inclined surfaces 21, so that each portion 10d can be appropriately inclined and accurately deformed in the direction that closes the gaps 14.

[0100] 19 , in the heat treatment step S12, the sintered body precursor 10 is placed on a molding die 20, and the overall shape of the precursor 10 is deformed in a direction that closes the three-dimensional shape. The base-forming portion 10c is placed on an inclined surface 21, and the base-forming portion 10c is deformed inward along the inclined surface 21, so that each portion 10d is inclined inward, and the precursor 10 can be deformed into a shape in which the distance between the portions 10d that form the gaps 14 is reduced. The overall shape of the precursor 10 can be deformed by the weight of the precursor 10.

[0101] When the precursor 10 is placed on the mold 20 and deformed, the completed precursor 10 shown in Fig. 15 is obtained. The lower surface of the base-forming portion 10c abuts against the inclined surface 21 of the mold 20. The distance between the portions 10d is also reduced compared to when the precursor 10 was molded. The completed precursor 10 is then heat-treated to sinter the material particles 100 that form the precursor 10.

[0102] According to the above-described method for manufacturing a sintered body, a sintered body is obtained that has a complex structure with gaps on the surface or inside that are open to the outside, and in which unbound material particles remaining in the gaps have been removed. The sintered body has a shape in which the distances between the portions that form the gaps are smaller than before sintering. The shape of the lower surface of the sintered body in cross section is homologous to the shape of the bottom surface of the groove shape of the molding mold in cross section, and has a shape in which a homologous protrusion protrudes downward along one axial direction. The lower surface of the sintered body in cross section has a shape that has inclined surfaces on both sides of the center that slope upward as they move outward from the center of the lower surface.

[0103] According to the above-described manufacturing method and mold for a sintered body, even when manufacturing a sintered body with a complex structure having gaps on the surface or inside, a precursor having a shape in which the spaces between the portions forming the gaps open upward is used, so that unnecessary material particles adhering to the gaps of the sintered body can be easily removed before the heat treatment that closes the gaps. Therefore, damage caused by the removal of material particles is reduced, and a sintered body with high shape precision can be manufactured in which unnecessary material particles are not sintered on the inner surface of the gaps.

[0104] 15 to 19, the openings that open the gaps are provided on the upper side of the precursor 10, but such openings may be formed on the side of each bonding layer during additive manufacturing. That is, additive manufacturing may be performed in an orientation such that the shape in cross section shown in FIG. 16 becomes the shape in plan view.

[0105] 15 to 19, the precursor 10 has a shape in which a plurality of gaps 14 are arranged in parallel when viewed in cross section, but a precursor of a sintered body with a complex structure can be formed into any suitable three-dimensional shape having gaps of any suitable shape, as long as it is molded into a shape in which the gaps are open and then deformed into a shape in which the gaps are closed by the inclined surface provided on the molding die.

[0106] Each portion forming the gap in the precursor may be provided in a symmetrical shape that forms the gap in line symmetry, or in an asymmetrical shape that forms the gap in non-line symmetry. Furthermore, the portion forming the gap in the precursor may be composed of a single portion or multiple portions in a direction perpendicular to the cross section of the precursor (a direction perpendicular to the dashed dotted line in the drawing and extending in the depth direction in the drawing).

[0107] The precursor of the sintered body may also be molded into a three-dimensional shape having an undercut by additive manufacturing. The portion of the precursor that forms the gap may have an undercut portion in both the cross section of the precursor and the longitudinal section parallel to the direction perpendicular to the cross section. The undercut may be provided in a portion other than the gap 14 in the cross section or longitudinal section. Examples of undercuts include three-dimensional shapes that are difficult to demold in their original form, such as a convex shape with a protrusion protruding in a direction other than the demolding direction, a concave shape with a recessed portion recessed in that direction, a shape with a bent gap internally, or a shape in which the width of a portion changes along an arbitrary direction so that the portion and the mold interfere in that direction. Such three-dimensional shapes can be molded in one go using additive manufacturing.

[0108] The molding die can be formed in an appropriate shape depending on the shape of the finished shape of the precursor and the way in which the precursor is deformed, as long as it has an inclined surface that inclines the portions that form the gaps in the precursor and deforms them in a direction that closes the gaps. The shape of the molding die can be designed to close the gaps by appropriate deformation of the base depending on the shape, material, etc. of the precursor.

[0109] In Figures 18 and 19, the inclined surface 21 forms a partial elliptical arc shape when viewed in cross section of the molding mold 20, but it may also be formed into a partial circular arc shape, an inverted triangle shape, an inverted trapezoid shape, a partial polygonal shape, etc., depending on the shape of the side surfaces on both sides of the precursor 10, etc.

[0110] The inclined surface 21 is formed symmetrically with respect to the center of the mold 20 and is provided to correspond to both of the portions that form the cavities, but the inclined surface that deforms the mold 20 into a shape that closes the gap may be provided to correspond to one side of the base that supports the portion that forms the gap. A horizontal surface may also be provided as the surface that corresponds to the other side of the base that supports the portion that forms the gap.

[0111] However, the mold preferably has inclined surfaces that deform in a direction to close the gap, and the inclined surfaces are arranged facing each other with the center side lower than the outside. The inclined surfaces are preferably formed symmetrically with respect to the center side of the mold. With such a shape, uneven deformation of one part of the gap due to the weight of the other part can be reduced compared to when the inclined surfaces are asymmetric, thereby improving the closure of the gap and the shape precision of the sintered body.

[0112] The mold may have a combination of multiple inclined surfaces, each with a different angle or direction, as an inclined surface that deforms the mold in a direction to close the gap, in addition to an inclined surface facing the inclined surface. The portions that form the gaps in the precursor may be provided at any number of positions in the direction of the cross section or in a direction perpendicular to the cross section (a direction perpendicular to the dashed dotted line in the drawing and extending in the depth direction in the drawing).

[0113] In such cases, the angle and direction of deformation can be changed for each region, and an inclined surface corresponding to each region or an inclined surface opposite the inclined surface can be provided. The precursor can be placed on the mold so that the center lines between the multiple regions forming the gaps are aligned vertically upward and parallel to the leading edge lines of the inclined surfaces or the center lines between the opposing inclined surfaces in a plan view. By deforming the multiple regions with different angles and directions for each region, the gaps can be closed by folding.

[0114] Although the embodiments of the present invention have been described above, the present invention is not limited to the above-described embodiments and includes various modifications without departing from the technical scope. For example, the above-described embodiments are not necessarily limited to those including all of the configurations described above. Furthermore, it is possible to replace part of the configuration of an embodiment with another configuration, or to add another configuration to the configuration of an embodiment. Furthermore, it is also possible to add other configurations to, delete configurations from, or replace configurations with respect to part of the configuration of an embodiment.

[0115] For example, the sintered body may have a hollow structure with an internal cavity, and a complex structure with gaps on the surface or inside that are open to the outside. The cavities and gaps can be provided in any shape, number, and size.

[0116] In such a case, the precursor of the sintered body is formed into a shape in which the portions forming the cavities are separated from each other to open the cavities and the portions forming the gaps are spaced apart. In the heat treatment step S12, the precursor is placed on the inclined surface of the mold and deformed into a shape in which the portions forming the cavities are in contact with each other to close the cavities and a shape in which the spaces between the portions forming the gaps are reduced, and then the precursor is heat treated and sintered.

[0117] In such cases, the molding die can be provided with a combination of multiple inclined surfaces, such as an inclined surface that deforms the cavity into a shape that closes the cavity or an inclined surface that deforms the gap in a direction that closes the gap. The angle and direction of deformation can be changed for each region, and an inclined surface corresponding to each region or an inclined surface facing the inclined surface can be provided. On the top surface of the molding die, a combination of multiple inclined surfaces facing each other with the center side lower than the outside can be used to form a combination of multiple groove shapes with homologous shapes cut out along one axial direction.

[0118] The precursor can be placed on the mold so that the center lines between the multiple regions forming the cavities are aligned vertically upward and parallel to the tip lines of the inclined surfaces and the center lines between the opposing inclined surfaces in a plan view. By deforming the multiple regions, each with a different angle or direction, the cavities and gaps can be closed by folding.

[0119] REFERENCE SIGNS LIST 10 precursor 11 cavity 12 inner surface 13 lower surface 14 gap 20 mold 21 inclined surface 100 material particles

Claims

1. A method for producing a sintered body in which material particles are sintered together, comprising: a molding step of molding a precursor with a molding material containing material particles and a binder; and a heat treatment step of heat-treating the precursor in a molding mold to form a sintered body, wherein the sintered body has a hollow structure with an internal cavity or a complex structure with gaps that are open to the outside, and the precursor is molded into a shape in which the portions forming the cavity are separated from each other to open the cavity, or a shape in which the portions forming the gaps are spaced apart, and the molding mold has an inclined surface on its upper surface, and in the heat treatment step, the precursor is placed on the inclined surface and deformed into a shape in which the portions forming the cavity are in contact with each other to close the cavity, or into a shape in which the portions forming the gaps are reduced, and then the precursor is heat-treated to sinter the precursor.

2. A method for producing a sintered body as described in claim 1, comprising a removal step of removing unbound material particles not bound by the binder after the molding step and before the heat treatment step, in which the material particles remaining in the cavities that are open upward or the material particles remaining in the gaps that are open upward are removed in the removal step.

3. A method for manufacturing a sintered body as described in claim 1, wherein the inclined surfaces form a groove shape by opposing each other with the center side lower than the outside when viewed in cross section of the mold.

4. A method for producing a sintered body as described in claim 3, wherein the inclined surface forms an inverted triangular shape, a partial circular arc shape, or a partial elliptical arc shape when viewed in cross section of the molding mold.

5. A method for producing a sintered body as described in claim 3, wherein the precursor is placed so that the center line between the portions forming the cavity or the center line between the portions forming the gap coincides with the center line of the groove shape in a planar view.

6. A method for producing a sintered body as described in claim 1, wherein when the precursor is placed on the molding die, it is deformed by its own weight into a shape in which the cavity is closed or into a shape in which the distance between the portions forming the gap is reduced.

7. A method for producing a sintered body as described in claim 1, wherein the sintered body has a hollow structure having a cavity inside, the precursor is formed into a shape in which the parts forming the cavity are separated from each other to open the cavity, and in the heat treatment process, the precursor is placed on the inclined surface and deformed into a shape in which the parts forming the cavity come into contact with each other to close the cavity, and then the parts that have come into contact due to the deformation are sintered to join them.

8. A method for producing a sintered body according to claim 1, wherein the precursor is formed into a three-dimensional shape having an undercut by an additive manufacturing method.

9. A sintered body formed by sintering material particles together, wherein the sintered body has a hollow structure having an internal cavity, and the parts forming the cavity are in contact with each other to close the cavity, or has a complex structure having gaps that are open to the outside, and the distance between the parts forming the gaps is smaller than before sintering, and the lower surface of the sintered body has a shape that has an inclined surface that slopes upward from the center of the lower surface to the outside in a cross-sectional view of the sintered body, and the unsintered material particles in the cavity or the unsintered material particles in the gaps have been removed.

10. A sintered body according to claim 9, wherein the inclined surface forms an inverted triangular shape, a partial circular arc shape, or a partial elliptical arc shape in a cross-sectional view of the sintered body.

11. A mold used to shape a sintered body in which material particles are sintered together, the mold having an inclined surface on which the precursor is placed, the sintered body having a hollow structure with an internal cavity or a complex structure with gaps that are open to the outside, the precursor being molded into a shape in which the parts that form the cavity are separated at the upper side and the cavity is open toward the top, or into a shape in which the spaces between the parts that form the gaps are open toward the top, and then the precursor is placed on the inclined surface.

12. A mold according to claim 11, wherein the inclined surfaces, in a cross-sectional view of the mold, face each other in a direction such that the center side is lower than the outside, forming a groove shape.

13. The mold according to claim 11, wherein the inclined surface forms an inverted triangular shape, a partial circular arc shape, or a partial elliptical arc shape in a cross-sectional view of the mold.

Citation Information

Patent Citations

  • Controlling green body object deformation

    US20210402467A1

  • Oriented alumina sintered body and method for producing same

    WO2018008207A1