Silicon nitride powder and resin composition using same

By controlling the Rsp value and other properties of silicon nitride powder, the moisture content in resin compositions is reduced, addressing the risk of water leakage and enhancing the thermal and mechanical properties for electronic components.

WO2024202736A1PCT designated stage expired Publication Date: 2024-10-03SUMITOMO CHEM CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/006305
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-02-21
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing resin compositions used for heat dissipation in electronic components often have high moisture content, which can deteriorate semiconductor performance and pose a risk of water leakage, as the moisture content of silicon nitride powders used as fillers is not adequately controlled.

Method used

A silicon nitride powder with a low moisture content is developed by controlling the Rsp value relative to ethanol, surface roughness, specific surface area, apparent density, and aspect ratio, which improves dispersibility and reduces water adsorption, and is used as a filler in a resin composition.

Benefits of technology

The controlled silicon nitride powder effectively reduces the water content in the resin composition, enhancing its suitability for electronic components by improving thermal conductivity and mechanical strength while minimizing moisture-related issues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

This silicon nitride powder contains multiple silicon nitride particles, and has an Rsp value with respect to ethanol of less than 105.6.
Need to check novelty before this filing date? Find Prior Art

Description

Silicon nitride powder and resin composition using same

[0001] The present disclosure relates to a silicon nitride powder and a resin composition using the same.

[0002] Heat generated by passing current through an electronic component is dissipated via a heat sink. To improve heat dissipation efficiency, a technique for filling the space between the electronic component and the heat sink with a heat dissipation material is known. One heat dissipation material is a resin composition containing a resin and inorganic particles, and it is known that silicon nitride powder can be used as the inorganic particles (see, for example, Patent Document 1).

[0003] Patent Document 1 discloses a low-aluminum spherical β-silicon nitride powder for use as a filler in electronic packaging materials. The silicon nitride powder is characterized by a sphericity of 0.5 to 0.99, an Al impurity content of less than 500 ppm, and a particle size range of 0.5 μm to 50 μm.

[0004] Patent Document 2 discloses a method for producing silicon nitride powder suitable for producing silicon nitride sintered bodies, and silicon nitride powder obtained by said method. The silicon nitride powder has an average particle size of 1 to 50 μm, a metal oxide content of 0 to 10 wt %, and an impurity content of less than 1 wt %, preferably the metal oxide content in the silicon nitride powder is less than 1 wt %, and the sintered body has a thermal conductivity of 90 W / mK or more and a bending strength of 700 MPa or more, and preferably the sintering conditions for the sintered body are as follows: the silicon nitride powder is mixed with MgO, Y 2 O 3 The powder is mixed with the above powder, polished, and the powder is dry-press molded, and the powder is gas-pressure sintered at 1900°C and a nitrogen gas pressure of 1 MPa for 8 hours.

[0005] Patent Document 3 discloses a silicon nitride powder suitable for producing a highly thermally conductive silicon nitride sintered body. The silicon nitride powder is characterized by having a β fraction of 30 to 100%, an oxygen content of less than 0.5 wt%, an average particle size of 0.2 to 10 μm, an aspect ratio of 10 or less, and containing columnar particles with grooves formed in the long axis direction of the particle.

[0006] JP 2022-522814 A JP 2022-541208 A JP 2004-262756 A

[0007] The performance of semiconductor components contained in electronic components may be deteriorated by moisture. If a resin composition used as a heat dissipation material contains a large amount of moisture, the moisture may leach out of the resin composition and reach the electronic components. In order to reduce the moisture content of the resin composition as much as possible, it is desirable to use silicon nitride powder with a low moisture content as a filler.

[0008] Patent Document 1 does not consider the moisture content of silicon nitride particles used as a filler. Patent Documents 2 and 3 disclose silicon nitride powders for use in silicon nitride sintered bodies, and therefore do not consider mixing them with resins to form resin compositions, nor do they consider silicon nitride powders suitable as fillers for resin compositions. Patent Documents 2 and 3 also do not consider the moisture content of silicon nitride particles.

[0009] In view of these circumstances, one embodiment of the present invention aims to provide a silicon nitride powder used as a filler for resin compositions, the silicon nitride powder having a low water content. Furthermore, another embodiment of the present invention aims to provide a resin composition using the silicon nitride powder according to one embodiment.

[0010] A first aspect of the present invention is a silicon nitride powder comprising a plurality of silicon nitride particles, the silicon nitride powder having an Rsp value to ethanol of less than 105.6.

[0011] A second aspect of the present invention is the silicon nitride powder according to the first aspect, having a surface roughness Ra of less than 0.97 nm.

[0012] A third aspect of the present invention is the silicon nitride powder according to the first or second aspect, wherein the silicon nitride particles have a diameter equivalent to the specific surface area of ​​more than 0.71 μm.

[0013] In the fourth aspect of the present invention, the specific surface area is 2.66 m 2 4. The silicon nitride powder according to any one of Aspects 1 to 3, wherein the silicon nitride powder has a surface roughness of less than 1 / g.

[0014] Aspect 5 of the present invention is a granular ... 3 The silicon nitride powder according to any one of Aspects 1 to 4, wherein the silicon nitride powder has a molecular weight of 1000 or more.

[0015] A sixth aspect of the present invention is the silicon nitride powder according to any one of the first to fifth aspects, wherein the ratio (L2 / L1) of the total length L2 of the internal boundary lines to the length L1 of the outer edge is 1% or less, and the maximum particle size of the silicon nitride particles is 6.8 μm or more.

[0016] A seventh aspect of the present invention is a resin composition comprising a resin and the silicon nitride powder according to any one of the first to sixth aspects.

[0017] By using the silicon nitride powder according to one embodiment of the present invention as a filler, a resin composition with a low water content can be obtained.

[0018] [Silicon nitride powder] The present inventors have investigated methods for reducing the moisture content of resin compositions because moisture contained in resin compositions can adversely affect electronic components, and have come to the conclusion that it is important to control the moisture content of silicon nitride powder used as a filler in resin compositions. As a result of extensive research, the inventors have discovered for the first time that the Rsp value, which can be determined from pulse MNR measurement, particularly the Rsp value relative to ethanol, is an appropriate indicator of the moisture content of silicon nitride powder, and have completed the present invention.

[0019] In addition, it seems appropriate to use the Rsp value for water as an indicator for controlling the moisture content of silicon nitride powder. However, the inventors considered using a dispersion medium other than water because measuring the Rsp value for water is difficult due to the difficulty in sample preparation and the possibility that an accurate value is difficult to obtain. As a result, they found that the Rsp value for ethanol is relatively easy to prepare a sample for measurement, easy to obtain an accurate value, and also suitable as an indicator for controlling the moisture content of silicon nitride powder.

[0020] (Rsp value for ethanol is less than 105.6) The Rsp value for ethanol is an index related to the mobility of the dispersion medium molecules (ethanol molecules) adsorbed on the surface of the silicon nitride powder. The silicon nitride powder dispersed in the silicon nitride slurry is dispersed in the silicon nitride slurry with the dispersion medium molecules constrained to its surface. Here, as the number of dispersion medium molecules constrained to the surface of the silicon nitride powder increases, the transverse relaxation time (T2) becomes shorter, and therefore the Rsp value increases. Furthermore, as the number of dispersion medium molecules constrained to the surface of the silicon nitride powder increases, the dispersed state in the dispersion medium becomes stable, thereby improving the dispersibility of the silicon nitride powder. For these reasons, as the Rsp value increases, the dispersibility of the silicon nitride powder tends to improve. Therefore, the Rsp value is sometimes used as an index of dispersibility.

[0021] In this embodiment, the Rsp value is used as an index for determining the amount of dispersion medium molecules (ethanol molecules) bound to the surface. Silicon nitride powder with a high Rsp value for ethanol has a high affinity for ethanol molecules and is easily adsorbed to the surface. Because ethanol molecules are hydrophilic polar molecules, the inventors speculated that silicon nitride powder with a high affinity for ethanol molecules would also have a high affinity for water molecules, and conducted extensive research. As a result, it was confirmed that the Rsp value of silicon nitride powder with respect to ethanol is related to the amount of moisture that the silicon nitride powder can adsorb, and that by setting the Rsp value to less than 105.6, the amount of moisture that the silicon nitride powder can adsorb can be reduced to a moisture level suitable for use as a filler in a resin composition. In other words, by controlling the Rsp value of silicon nitride powder with respect to ethanol to less than 105.6, a silicon nitride powder with a low moisture content can be obtained, and by using this silicon nitride powder, a resin composition with a low moisture content can be produced.

[0022] The Rsp value of the silicon nitride powder with respect to ethanol is less than 105.6, preferably 90.0 or less, more preferably 80.0 or less, even more preferably 70.0 or less, and particularly preferably 65.0 or less. The lower limit of the Rsp value is not particularly limited, but may be, for example, 0.5 or more, or 1.0 or more.

[0023] To determine the Rsp value, first, a silicon nitride slurry in which silicon nitride powder is dispersed in a dispersion medium (ethanol) and the dispersion medium alone (blank liquid) are measured by pulse NMR. 1 The relaxation time of the H nuclei (the time it takes for the pulse-excited magnetization to return to its original thermal equilibrium) is measured. Using the obtained measurement results, the Rsp value is calculated using the following formula (1): Rsp value = (Rav - Rb) / Rb (1) Here, Rav is the reciprocal of the transverse relaxation time when a silicon nitride slurry (e.g., volume X (ml)) in which silicon nitride powder is dispersed in a dispersion medium is measured by pulse NMR. Furthermore, Rb is the reciprocal of the transverse relaxation time when only the dispersion medium of the silicon nitride slurry (e.g., volume X (ml)) is measured by pulse NMR. Note that a liquid consisting only of the dispersion medium (ethanol) is sometimes referred to as a "blank liquid." Typically, the volume of the blank liquid is the same as the volume of the silicon nitride slurry during pulse NMR measurement.

[0024] Pulse NMR measurement of the silicon nitride slurry can be performed using, for example, a pulse NMR device "The Minispec MQ20" manufactured by Bruker. The measurement conditions are, for example, a measurement frequency of 20 MHz, a measurement nucleus of 1 H NMR, measurement method: T2 (transverse relaxation time), sample amount: 0.3 ml, temperature: 25°C.

[0025] (Surface roughness Ra) The surface roughness Ra (arithmetic mean roughness) of the silicon nitride powder is preferably less than 0.97 nm. If the surface roughness Ra is less than 0.97 nm, the surface area of ​​the silicon nitride particles can be reduced, thereby reducing the amount of moisture adsorbed on the surface of the silicon nitride particles. The surface roughness Ra is preferably less than 0.97 nm, more preferably 0.95 nm or less, even more preferably less than 0.93 nm, even more preferably 0.90 nm or less, even more preferably 0.80 nm or less, and particularly preferably 0.70 nm or less.

[0026] To measure the surface roughness Ra, a 100 nm x 100 nm measurement area on the surface of any silicon nitride particle is observed using a scanning probe microscope (SPM). The surface roughness Ra is calculated from the obtained shape image. The surface roughness Ra is measured for four silicon nitride particles, and the average value is taken as the surface roughness Ra of the silicon nitride powder.

[0027] (Specific surface area equivalent diameter of silicon nitride particles) The specific surface area equivalent diameter (DBET) of the silicon nitride particles is preferably greater than 0.71 μm. If the specific surface area equivalent diameter is greater than 0.71 μm, the number of silicon nitride particles contained in the silicon nitride powder per unit mass can be reduced, thereby reducing the amount of water adsorbed to the silicon nitride powder. DBET is preferably greater than 0.71 μm, more preferably 1.10 μm or more, even more preferably 1.40 μm or more, even more preferably 3.00 μm or more, and particularly preferably 8.00 μm or more. The upper limit of DBET is not particularly limited, but may be, for example, 50 μm or less, 40 μm or less, or even 30 μm or less.

[0028] The specific surface area diameter (DBET) of silicon nitride particles is calculated from the following formula (2), which is a general formula showing the relationship between the particle diameter and the specific surface area of ​​spherical particles: DBET (μm) = 6 / (S × ρ) (2), where S is the specific surface area (m 2 / g), and ρ: apparent density of silicon nitride particles (g / cm 3 )

[0029] S and ρ for determining DBET are determined as follows: S (specific surface area of ​​silicon nitride particles) is substantially the same as the specific surface area of ​​silicon nitride powder, so the measurement result of the specific surface area of ​​silicon nitride powder measured by the method described below is used. ρ (apparent density of silicon nitride particles) is substantially the same as the apparent density of silicon nitride powder, so the measurement result of the apparent density of silicon nitride powder measured by the method described below is used.

[0030] (Specific Surface Area) The specific surface area of ​​the silicon nitride powder according to the embodiment is a BET specific surface area measured by a krypton adsorption method based on JIS Z 8830:2013. The specific surface area of ​​the silicon nitride powder is 2.66 m 2 The specific surface area of ​​the silicon nitride powder is preferably less than 2.00 m / g, which can reduce the amount of water adsorbed on the surface. 2 / g or less, and more preferably 1.50m 2 / g or less, and even more preferably 1.36 m 2 / g, more preferably less than 0.50 m 2 / g or less, and particularly preferably 0.24 m 2 The lower limit of the specific surface area is not particularly limited, but for example, it is 0.01 m 2 / g or more, and 2 / g or more.

[0031] (Apparent density) The apparent density of silicon nitride powder is 3.17 g / cm 3 It is preferable that the density is greater than 3.18 g / cm 3 This results in a silicon nitride powder containing many silicon nitride particles with a small amount of internal voids, that is, a silicon nitride powder with a small amount of moisture that can be retained inside. The upper limit of the apparent density is, for example, 3.44 g / cm 3 In addition, if the apparent density is not too high, it is expected that the powder will be less likely to settle when mixed with a resin and will be easier to disperse. In order to achieve such an effect, the apparent density of the silicon nitride powder should be 3.30 g / cm 3 It is preferable that the density is 3.25 g / cm or less, and more preferably 3.25 g / cm 3 The following is the result.

[0032] The apparent density of silicon nitride particles is measured by the pycnometer method in accordance with JIS R 1620:1995. The measurement is carried out five or more times, and the average value is taken as the apparent density of the silicon nitride powder. For the measurement, for example, an Accupyc 1330 (Micromeritics) can be used.

[0033] (Average aspect ratio of silicon nitride particles) The average aspect ratio of the minor axis to the major axis of the silicon nitride particles contained in the silicon nitride powder is preferably more than 0.50, more preferably more than 0.60, even more preferably 0.65 or more, and even more preferably 0.67 or more. On the other hand, the average aspect ratio of the silicon nitride particles is preferably less than 0.87, more preferably 0.85 or less.

[0034] The average aspect ratio of silicon nitride particles is measured as follows. SEM images of silicon nitride particles contained in silicon nitride powder are analyzed using image processing software (e.g., Image J (manufactured by the National Institute of Health)). The maximum particle size of the silicon nitride particles (referred to as the "major axis") is identified, and the particle size in the direction perpendicular to the major axis is referred to as the "minor axis". The major and minor axes are measured for 20 random silicon nitride particles, and the ratio of the minor axis to the major axis (minor axis / major axis) is determined for each particle. The arithmetic mean value of these ratios is taken as the average aspect ratio of the silicon nitride particles.

[0035] (β-phase ratio) The β-phase ratio of the silicon nitride powder is preferably 65% ​​or more, more preferably 70% or more, even more preferably 80% or more, still more preferably 85% or more, and particularly preferably 90% or more.

[0036] In this specification, the "β-phase ratio" refers to the content (volume %) of β-type silicon nitride relative to all silicon nitrides contained in the silicon nitride powder.

[0037] In calculating the β-phase ratio, the silicon nitride powder was measured by powder X-ray diffraction, and the diffraction pattern was analyzed by the Gazzara & Messier method (G.P. Gazzara and D.P. Messier, "Determination of Phase Content of Si 3 N 4 The β-phase ratio is calculated by analyzing the β-phase by X-ray Diffraction Analysis, Am. Ceram. Soc. Bull., 56[9]777-80 (1977)).

[0038] (The maximum particle size of silicon nitride particles having a ratio (L2 / L1) of the total length L2 of the internal boundaries to the outer edge length L1 of 1% or less is 6.8 μm or more.) The fewer grain boundaries and cavities there are inside a silicon nitride particle, the less moisture can be retained inside. Therefore, the ratio (L2 / L1) of the total length L2 of the boundaries to the outer edge length L1 is introduced as an indicator of the content of grain boundaries inside a silicon nitride particle. L1 and L2 are determined by observing the cross section of the silicon nitride particle. Note that the terms "grain boundary" and "boundary line" used here refer to boundaries where the crystal orientation misorientation (oblique angle) exceeds 15° as a result of EBSD analysis (also called high-angle grain boundaries).

[0039] When the length of the outer edge of one silicon nitride particle is L1 and the total length of the boundary lines of that silicon nitride particle is L2, silicon nitride particles with a small value of L2 / L1 can be said to have a low content of boundary lines. In this embodiment, silicon nitride particles with an L2 / L1 ratio of 1% or less are considered to be silicon nitride particles consisting of a single crystal (these are referred to as "single crystal particles").

[0040] In this embodiment, the maximum particle size of silicon nitride particles having an L2 / L1 ratio of 1% or less (i.e., single crystal) is preferably 6.8 μm or more, more preferably 10.0 μm or more, even more preferably 20.0 μm or more, even more preferably 40 μm or more, and particularly preferably 60 μm or more.

[0041] (Particle diameter D50 of the cumulative 50% from the fine particle side of the cumulative particle size distribution on a volume basis) The silicon nitride powder preferably has a particle diameter D50 of the cumulative 50% from the fine particle side of the cumulative particle size distribution on a volume basis (hereinafter simply referred to as "D50") of 1.5 μm or more, more preferably 2.0 μm or more, even more preferably 5.0 μm or more, still more preferably 10.0 μm or more, and particularly preferably 30 μm or more. The upper limit is not particularly limited, but is, for example, preferably 500.0 μm or less, more preferably 300.0 μm or less, and even more preferably 200.0 μm or less.

[0042] The D50 of silicon nitride powder is measured by laser diffraction. Specifically, the powder is dispersed in water and irradiated with a laser beam, and the diffraction is measured to determine the particle size. A measuring device such as the 1090L manufactured by CILAS can be used.

[0043] [Method for Producing Silicon Nitride Powder] A method for producing silicon nitride powder according to an embodiment of the present invention will be described. The method for producing silicon nitride powder includes the steps of: (1) synthesizing silicon nitride synthetic crystals by combustion synthesis in a nitrogen atmosphere using raw materials containing Si; (2) crushing the silicon nitride synthetic crystals to obtain coarsely pulverized silicon nitride powder; and (3) finely pulverizing the coarsely pulverized silicon nitride powder to obtain finely pulverized silicon nitride powder. Optionally, the method may further include the step of: (4) heat-treating the finely pulverized silicon nitride powder.

[0044] Step (1): Synthesizing silicon nitride composite crystals. For example, Si powder is used as the raw material containing Si. The average particle diameter D50 of the raw material is, for example, within the range of 2 to 10 μm. This allows the amount of oxygen impurities to be suppressed, and the combustion rate to be increased, allowing for a higher synthesis temperature, resulting in good crystal growth. As an example, the average particle diameter D50 of Si is 5 μm.

[0045] The diluent is used to adjust the amount of Si in the raw material. A separately prepared silicon nitride powder is used as the diluent. The diluent may be either α-type silicon nitride powder or β-type silicon nitride powder, or a mixture of these. The average particle diameter D50 of the diluent is preferably in the range of 0.5 to 2.0 μm. For example, the average particle diameter D50 of the diluent is 1.0 μm. The amount of diluent added is less than 10 mass% of the total raw material (including the diluent). For example, the diluent is added in an amount of 5 to 8 mass% of the total raw material. By adding the amount of diluent within the above range, a predetermined amount of silicon nitride particles having an Rsp value for ethanol of less than 105.6 can be produced.

[0046] In this embodiment, a diluent is mixed with the raw materials and then filled into an insulated heat-resistant container. This insulated heat-resistant container has a thermal conductivity of 1 W / mK or less, and although alumina or zirconia can be used as the material, carbon is preferred to prevent impurities from being mixed in. After the raw materials are filled, the container is covered with a lid made of the same material as the insulated heat-resistant container. Furthermore, to increase the temperature inside the composite during combustion, the thickness of the mixed raw materials is set to more than 100 mm, preferably more than 100 mm and 150 mm or less. Combustion synthesis is performed in a nitrogen atmosphere in the range of 0.5 to 1 MPa (e.g., 0.9 MPa). Adjusting the pressure range within this range enables efficient synthesis while suppressing increases in equipment costs.

[0047] When the mixed raw material is filled into the crucible, a layer of powder (silicon nitride) having a thickness of 1 mm to 80 mm is spread on the bottom and sides of the crucible, the mixed raw material is then filled, and the top surface is further covered with a layer of powder having a thickness of 1 mm to 80 mm. By covering the entire surface with the powder, the mixed raw material can be kept warm, and a predetermined amount of silicon nitride particles having an Rsp value to ethanol of less than 105.6 can be produced.

[0048] To promote crystal growth more effectively, a catalyst may be used, for example, Y 2 O 3 , Fe 2 O 3 , CaO, Ni, Co, C, etc. are added in an amount of about 0.01 to 0.1 mass %. In addition, external auxiliary heating is performed in the range of 500°C to 1700°C (for example, 1500°C), and the combustion temperature is also increased in the combustion synthesis method by self-ignition.

[0049] Step (2): Obtaining a coarsely pulverized silicon nitride powder. The silicon nitride composite crystal is in the form of an agglomeration of multiple silicon nitride particles. In step (2), the silicon nitride composite crystal is crushed to obtain a coarsely pulverized silicon nitride powder. For example, the composite is crushed using a common crushing device such as a hammer mill or a disk mill until it passes through a sieve with a specified mesh size (for example, a sieve with mesh sizes in the range of 400 μm to 500 μm).

[0050] Step (3): Step of Obtaining Finely Pulverized Silicon Nitride Powder The coarsely pulverized silicon nitride powder is further pulverized to obtain a finely pulverized silicon nitride powder. The pulverization is carried out using a pulverizing device such as a jet mill or a ball mill. If necessary, the resulting finely pulverized powder may be classified. Classification may be carried out by sieving, wet classification, or the like. The resulting finely pulverized powder may be used as is as the silicon nitride powder, or may be subjected to a heat treatment step (step (4) described below) before use as the silicon nitride powder.

[0051] Step (4): Heat-treating the finely pulverized silicon nitride powder. Optionally, the finely pulverized silicon nitride powder may be heat-treated. Heat treatment forms an oxide film on the surface of the silicon nitride particles, which has the effect of chemically stabilizing the silicon nitride particles. The heat treatment is carried out, for example, in air at a temperature of 500°C or higher and 1200°C or lower. The heat treatment time can be adjusted appropriately according to the heat treatment temperature. The heat treatment time is, for example, 5 hours.

[0052] In the method for producing silicon nitride powder, silicon nitride synthetic crystals are synthesized using the heat generated by combustion synthesis, and then the silicon nitride powder according to this embodiment can be produced by crushing, classifying, and pulverizing the synthesized crystals.

[0053] [Resin Composition] The silicon nitride powder according to the embodiment of the present invention is suitable as a filler for a resin composition. The resin composition contains a resin and the silicon nitride powder according to the embodiment of the present invention.

[0054] The compounding ratio of the silicon nitride powder to the resin according to the embodiment of the present invention can be determined appropriately depending on the purpose and application. As an example, the resin may be 5 to 75 volume % and the silicon nitride powder may be 95 to 25 volume % relative to the resin composition (composite). The filling rate of the silicon nitride powder in the resin composition refers to the content (vol %) of the silicon nitride powder when the volume of the resin composition (including the silicon nitride powder) is taken as 100 volume %.

[0055] A method for producing a resin composition will be described. A resin composition can be obtained by mixing silicon nitride powder and a resin using a commonly used known method. For example, when the resin is liquid (e.g., liquid epoxy resin), the resin composition can be obtained by mixing the liquid resin, silicon nitride powder, and a curing agent, and then curing the mixture with heat or ultraviolet light. Known curing agents, mixing methods, and curing methods can be used. On the other hand, when the resin is solid, the desired resin composition can be obtained by mixing the silicon nitride powder and the resin, and then kneading the mixture using a known method such as melt kneading.

[0056] The resin used in the resin composition can be a known resin such as an epoxy resin. The type of resin can be selected from thermoplastic resins, thermoplastic elastomers, and thermosetting resins. The resins can be used alone or in combination of two or more.

[0057] Furthermore, these resin compositions may contain, as needed, known additives such as plasticizers, curing accelerators, coupling agents, fillers, pigments, flame retardants, antioxidants, surfactants, compatibilizers, weather resistance agents, antiblocking agents, antistatic agents, leveling agents, and release agents, either singly or in combination, within the scope of the invention.

[0058] Hereinafter, the embodiments of the present invention will be described in detail with reference to examples carried out to clarify the effects of the embodiments of the present invention. However, the embodiments of the present invention are not limited to the following examples.

[0059] <Preparation of Silicon Nitride Powder> (Samples No. 1-3, 9) Si powder (particle diameter = 5 μm) and silicon nitride powder (particle diameter = 1 μm) prepared separately as a diluent were mixed in a tumbling ball mill. The amount of diluent added was 5-8 mass% of the total raw material (including diluent). The mixed powder was packed into a carbonaceous, heat-resistant container with a layer of powder 1 mm to 80 mm thick on the bottom and sides, so that the raw material layer was thicker than 100 mm and not more than 150 mm. The raw material layer was then covered with a layer of powder 1 mm to 80 mm thick. A lid made of a carbonaceous, heat-resistant material was then placed in the container, and synthesis was carried out under a nitrogen atmosphere at 0.9 MPa. After synthesis, the mixture was coarsely crushed (disintegrated) in a mortar until it passed through a sieve with the specified mesh size. The mesh size of the sieve for each sample is shown in Table 1.

[0060] The obtained coarsely pulverized powder was further finely pulverized using a nanojetmizer (manufactured by Aisin Nano Technologies Co., Ltd.). The nanojetmizer with the model number listed in Table 1 was used for the fine pulverization. The obtained finely pulverized powder was classified using the method listed in Table 1. Note that classification was not performed for Sample No. 2. The obtained classified powders (Samples No. 1, 3, and 9) and the finely pulverized powder (Sample No. 2) were then placed in an alumina crucible and heat-treated in an air atmosphere using a small-scale powder programmable electric furnace (MMF series, manufactured by AS ONE) under the conditions (heat treatment temperature, heat treatment time) listed in Table 1 to obtain silicon nitride powders (Samples Nos. 1 to 3 and 9).

[0061] (Samples Nos. 5 to 7) Coarsely pulverized powders were prepared in the same manner as in "Samples Nos. 1 to 3, 9" above. The sieve used during coarse pulverization (disintegration) had a mesh size of 500 μm. The obtained coarsely pulverized powder was then finely pulverized in a ball mill. The obtained finely pulverized powder was subjected to sieve classification using a vibrating sieve according to the following procedure, and then further wet classification was carried out to obtain silicon nitride powders (Samples Nos. 5 to 7) having the desired D50. - Sample No. 5: Silicon nitride particles remaining on a sieve with a mesh size of 150 μm (D50 was 192.0 μm). - Sample No. Sample No. 6: When sieving using a 106 μm sieve, the powder remaining below the sieve was further sieved using a 75 μm sieve, and the silicon nitride particles remaining on the sieve (D50 is 83.0 μm). Sample No. 7: When sieving using a 63 μm sieve, the silicon nitride particles remaining below the sieve (D50 is 22.0 μm).

[0062] (Sample No. 8) The silicon nitride particles (Sample No. 6) described above were placed in an alumina crucible and heat-treated in an air atmosphere using a small powder programmable electric furnace (MMF series manufactured by AS ONE) at a heat treatment temperature of 900°C for 5 hours to obtain silicon nitride powder (Sample No. 8).

[0063]

[0064] Various measurements were carried out on the obtained Samples Nos. 1 to 3 and 5 to 9 (Examples) and, as a comparative example, a commercially available silicon nitride powder (manufactured by Aldrich, silicon nitride (predominantly β-phase, ≦10 micron primary particle size, product code 248622); hereinafter referred to as "Sample No. 4").

[0065] (1) Measurement of the β-phase ratio of silicon nitride powder A diffraction pattern of the sample (silicon nitride powder) was obtained using a powder X-ray diffractometer (manufactured by Rigaku Denki). The measurement conditions were as follows: X-ray source: CuKα radiation X-ray output: 45 kV, 200 mA Graphite monochromator Diffraction angle (2θ): Step scan in 0.02° increments over the range of 2 to 90° Scanning speed: 21.7 deg / min

[0066] When a sample contained components other than silicon nitride, the peaks of those components were compared with the corresponding peaks of standard samples of those components to determine the proportions of those components. For Samples No. 1 to 9, the powder X-ray diffraction patterns obtained confirmed that the samples were composed solely of α-type silicon nitride and β-type silicon nitride. The proportion of β-type silicon nitride in the sample (β-conversion ratio) was then calculated using the Gazzara & Messier method.

[0067] (2) Maximum particle size of silicon nitride particles with an L2 / L1 ratio of 1% or less (maximum particle size of single-crystal particles) A ​​sample for cross-sectional observation was prepared using the sample (silicon nitride particles). To prepare the sample for cross-sectional observation, the silicon nitride particles were embedded in resin, and then the resin and silicon nitride particles were cut using a diamond cutter. Subsequently, a protective film of platinum was vapor-deposited on the cross-section, and the cross-section was prepared by Ar ion milling. The sample was then fixed to the SEM sample stage with Cu double-sided tape, and SEM-EBSD measurement was performed without vapor deposition. The observation position was determined so that two or more silicon nitride particles were completely contained within the observation region (i.e., two or more silicon nitride particles did not come into contact with the frame of the observation region). Measurements were performed using β-type silicon nitride particles.

[0068] The following equipment was used for sample pretreatment and EBSD measurement: Equipment used Ion milling equipment: E-3500 (manufactured by Hitachi High-Tech Corporation) Ion sputtering equipment: E-1030 (manufactured by Hitachi, Ltd.) Schottky scanning electron microscope: SU5000 (manufactured by Hitachi High-Tech Corporation) Backscattered electron diffraction equipment: Velocity (manufactured by METEK Corporation)

[0069] The conditions for the EBSD measurement were as follows: Measurement area: 500.0 μm×400.0 μm Acceleration voltage: 15.0 kV Magnification: ×500 Vacuum degree: 30 Pa

[0070] In the obtained EBSD image, two or more silicon nitride particles that were not in contact with the frame of the observation area were selected, and the average of the outer edge length L1 of each silicon nitride particle was calculated using image processing software Image J (manufactured by the National Institute of Health). The total length L2 of the boundary lines was also calculated. The "total length L2 of the boundary lines" is the sum of the boundary lines contained within the silicon nitride particle and does not include the outer edge of the silicon nitride particle. The total length L2 of the boundary lines was calculated by adding the total length of the grain boundaries within the silicon nitride particle and the total length of the inner walls of the cavities (if any) within the silicon nitride particle.

[0071] This measurement was carried out once for 20 random silicon nitride particles, and silicon nitride particles with an L2 / L1 ratio of 1% or less were considered to be single crystal particles, and the length of their major axis was measured and recorded as the "maximum particle size of the single crystal particles." If the 20 silicon nitride particles measured contained multiple single crystal particles, the arithmetic average of their maximum particle sizes was calculated.

[0072] (3) Specific surface area diameter (DBET) of silicon nitride particles The specific surface area diameter of silicon nitride particles was calculated from the following formula (2): DBET (μm) = 6 / (S × ρ) (2) The specific surface area (m 2 Since the apparent density (g / cm) of the silicon nitride particles is substantially equal to the specific surface area of ​​the silicon nitride powder, the specific surface area measured in "(5) Specific Surface Area" below was substituted for S in formula (2). 3 ) substantially coincides with the apparent density of the silicon nitride powder, so the apparent density measured in "(8) Apparent density of silicon nitride powder" described later was substituted for ρ in formula (2).

[0073] (4) Average aspect ratio of silicon nitride particles SEM images of the sample (silicon nitride powder) were taken. The following equipment was used for taking the images. Equipment used: Scanning electron microscope: JSM-IT200 (manufactured by JEOL Ltd.) The imaging conditions were as follows: Acceleration voltage: 5.0 kV Signal: SED Probe current: Std. -PC55 Magnification: 1000x

[0074] The SEM images were processed using image processing software Image J (manufactured by the National Institute of Health), and the aspect ratios of 20 randomly selected silicon nitride particles in the SEM images were determined. The maximum diameter of the silicon nitride particles was taken as the major axis, and the particle size in the direction perpendicular to the major axis was taken as the minor axis. The major and minor axes of 20 randomly selected silicon nitride particles were measured, and the ratio of the minor axis to the major axis (minor axis / major axis) was determined for each particle. The arithmetic mean value of these ratios was taken as the average aspect ratio of the silicon nitride particles (referred to as "aspect ratio" in the table).

[0075] (5) Specific Surface Area The specific surface area of ​​the sample (silicon nitride powder) was measured. The specific surface area of ​​powder (solid) was measured by gas adsorption in accordance with JIS Z 8830:2013, using krypton as the adsorption gas. In the measurement, 1 g of silicon nitride powder was placed in a sample tube, and an adsorption / desorption isotherm was obtained. The specific surface area (m 2 / g) was calculated.

[0076] (6) Measurement of surface roughness Ra A scanning probe microscope SPA300HV manufactured by Seiko Instruments Inc. was used to measure the surface roughness Ra. The measurement conditions were as follows: Probe station / unit SPI4000 / SPA300HV Cantilever: SI-DF20 Scanner: 20 μm Data type: Topographic image Observation mode: DFM (Dynamic Force Mode Microscope) Scanning area: 100 nm x 100 nm Scanning frequency: 0.25 Hz Analysis software: (attached to the measuring device)

[0077] Five silicon nitride particles were randomly selected from the image, and a measurement area of ​​100 nm × 100 nm on the surface of each particle was observed using a scanning probe microscope (SPM). The surface roughness Ra of each particle was calculated from the obtained shape image, and the average value was taken as the surface roughness Ra of the silicon nitride powder.

[0078] (7) Measurement of the Rsp value of silicon nitride powder in ethanol 0.2 g of sample (silicon nitride powder) was mixed with 0.3 mL of dispersion medium (ethanol) to prepare a test solution. The transverse relaxation time (T2) of this test solution was measured using a pulsed NMR device "The Minispec mq20" manufactured by Bruker. The measurement conditions were: resonance frequency: 20 MHz, measurement nucleus: 1H NMR, measurement method: T2, sample amount: 0.3 ml, temperature 25 ° C. The transverse relaxation time (T2) of a blank solution using pure water was also measured under the same measurement conditions. The reciprocal of the transverse relaxation time (T2) of the silicon nitride slurry was Rav, and the reciprocal of the transverse relaxation time (T2) of the blank solution was Rb, and Rsp was calculated from the following formula (1). Rsp value = (Rav - Rb) / Rb (1)

[0079] (8) Apparent Density of Silicon Nitride Powder The apparent density of the sample (silicon nitride powder) was measured in accordance with JIS R 1620:1995. The measurement method and conditions were as follows: Measurement method: Gas substitution method Sample drying: 200°C, 8 hours or more Apparatus used: Accupyc 1330 (Micromeritics) Measurement conditions Number of purges: 10 Purge filling pressure: 15.0 psig Number of measurements: 5 Measurement filling pressure: 15.0 psig Equilibrium pressure: 0.005 psig / min Measurement with set precision: Yes Allowable error of variation: 0.05% Sample cell size: 10 cm 3

[0080] (9) Measurement of D50 of silicon nitride powder The particle size distribution of the sample (silicon nitride powder) was measured, and the cumulative 50% particle size D50 was determined. The particle size distribution of the silicon nitride powder was measured by laser diffraction. A sample dispersed in water was irradiated with a laser beam, and the diffraction was measured to determine the particle size. The measuring device used was a CILAS 1090L model. The particle size was taken as the circle-equivalent particle size. The circle-equivalent particle size is the particle size of a perfect circle that has the same area as a projected particle image. The particle size was measured by volume.

[0081] (10) Measurement of Moisture Content of Silicon Nitride Powder The moisture content of the sample (silicon nitride powder) was measured by the Karl Fischer method in accordance with JIS K 0068:2001 "Method for measuring moisture content in chemical products."

[0082] (11) Measurement of moisture content of resin composition (composite) Epoxy resin (main agent: room temperature curing potting resin 53 type (manufactured by Sankei Co., Ltd.) 010-8140, curing agent: room temperature curing potting resin 53 type (manufactured by Sankei Co., Ltd.) 010-8143) and a sample (silicon nitride powder) were mixed in a blending ratio (volume ratio) of 50:50, and the mixture was stirred and mixed using a Foam Mixer (manufactured by Thinky Corporation) to obtain an epoxy resin-filler (silicon nitride powder) composite. The filling rate of the silicon nitride powder in the resin composition was 50% by volume.

[0083] A 1 mm thick aluminum plate with a 1 cm x 10 cm rectangular hole was prepared as a mold frame. A PET film (back side film) coated with a release agent was attached to the back side of the mold frame so as to cover the rectangular hole, with the release agent-coated surface facing the mold frame. After the stirred composite was poured into the rectangular hole of the mold frame, a PET film (front side film) coated with a release agent was attached on top of it, with the release agent-coated surface facing the mold frame and resin composition. Furthermore, light pressure was applied from above with a metal roller to fit the composite into the rectangular hole of the mold frame. Another aluminum plate was placed on top of the front side film, and the composite was cured by heating at 100°C for 1 hour. After curing was complete, the aluminum plate was allowed to cool, and when the temperature of the aluminum plate had dropped to approximately room temperature, the aluminum plate was removed. The PET films on the front and back sides of the cured composite were then peeled off, respectively, to obtain a sheet-like sample for measuring the moisture content.

[0084] The moisture content of the obtained sheet-like sample was measured. The moisture content was measured by the Karl Fischer method in accordance with JIS K 0068:2001 "Method for measuring moisture content in chemical products." A resin composition with a moisture content of less than 380 ppm was evaluated as pass (◯), and a resin composition with a moisture content of 380 ppm or more was evaluated as fail (×).

[0085] The measurement results are summarized in Tables 2 and 3.

[0086]

[0087]

[0088] The measurement results are discussed below. The silicon nitride powders of Samples Nos. 1 to 3 and 5 to 9, which satisfied the requirements of this embodiment, had low water contents. Therefore, it was possible to reduce the water contents of resin compositions prepared using these silicon nitride powders. On the other hand, the silicon nitride powder of Sample No. 4, which did not satisfy the requirements of this embodiment, had a high water content. Therefore, the water content of resin compositions prepared using this silicon nitride powder was also high.

[0089] This application claims priority from Japanese Patent Application No. 2023-058739, filed March 31, 2023. Japanese Patent Application No. 2023-058739 is incorporated herein by reference.

Claims

1. A silicon nitride powder comprising a plurality of silicon nitride particles, the silicon nitride powder having an Rsp value to ethanol of less than 105.

6.

2. The silicon nitride powder according to claim 1, having a surface roughness Ra of less than 0.97 nm.

3. The silicon nitride powder according to claim 1, wherein the silicon nitride particles have a specific surface area equivalent diameter of more than 0.71 μm.

4. Specific surface area is 2.66 m 2 2. The silicon nitride powder of claim 1, wherein the silicon nitride powder has a molecular weight of less than 1.0 / g.

5. Apparent density is 3.17 g / cm 3 The silicon nitride powder of claim 1, wherein the silicon nitride powder has a molecular weight of 1.0 or more.

6. The silicon nitride powder according to claim 1, wherein the maximum particle size of silicon nitride particles having a ratio (L2 / L1) of the total length L2 of the internal boundary lines to the length L1 of the outer edge of the silicon nitride particles is 6.8 μm or more.

7. A resin composition comprising a resin and the silicon nitride powder according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Production of silicon nitride powder

    JP1988274604A

  • Silicon nitride filler, resin composite, insulating substrate, and semiconductor sealant

    JP2015081205A

  • Silicon nitride powder, method for producing the same and composition for underfill material using the same

    JP2022135240A

  • Method for manufacturing silicon nitride sintered compact

    WO2021107021A1