Setting accelerator for trowelled finishing, concrete composition, and hardened body
The use of a setting accelerator with organic acid calcium salt and inorganic sulfate in a specific ratio addresses the issue of fluidity loss in concrete, allowing for earlier trowel finishing and improved workability, resulting in efficient and high-quality concrete finishes.
Patent Information
- Application Number
- PCT/JP2024/011645
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-07-14
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-03
AI Technical Summary
Current setting accelerators for trowel finishing in concrete work reduce fluidity, leading to poor workability and increased risk of construction defects due to prolonged waiting times before trowel finishing can commence, as they impair the concrete's fluidity and workability.
A setting accelerator containing an organic acid calcium salt and an inorganic sulfate in a specific mass ratio, with the organic acid calcium salt being calcium carboxylate and the inorganic sulfate including aluminum sulfate, sodium thiosulfate, or potassium alum, ensures that at least 95% of both pass through a 0.6 mm sieve, maintaining fluidity and shortening the time to trowel finishing.
The solution maintains concrete fluidity and significantly reduces the time from pouring to trowel finishing, resulting in improved work efficiency and a smoother, defect-free finish, while also controlling bleeding and enhancing the strength of the hardened concrete product.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Setting accelerator for trowel finishing, concrete composition, and hardened product
[0001] The present invention relates to a trowel-finishing set accelerator, a concrete composition, and a hardened concrete product, which are primarily used in the construction and civil engineering industries. The concrete composition of the present invention is a general term for cement paste, mortar, and concrete.
[0002] In concrete construction, the concrete surface is often finished with a trowel after it has been poured. The quality of this trowel finish can affect the cracking and strength of the concrete surface, and ultimately the durability of the concrete structure.
[0003] In this trowel finishing work, the best time to start the final trowel finishing work is when the bleeding begins to subside. Because the bleeding begins to subside just before the concrete begins to set, the current situation is that plasterers have to wait for several hours, and this waiting time reduces work efficiency.
[0004] Therefore, in order to accelerate the setting of concrete, for example, Patent Document 1 below discloses adding a setting accelerator to concrete.
[0005] Japanese Patent Application Publication No. 08-48553
[0006] However, in concrete to which a setting accelerator has been added, the addition of the setting accelerator causes the concrete to lose its fluidity, which significantly reduces workability during pouring, making construction less successful and potentially resulting in construction defects.
[0007] The present invention has been made in view of the above circumstances, and aims to provide a set accelerator for trowel finishing that can maintain the fluidity of concrete and shorten the time from concrete pouring until trowel finishing is possible. It also aims to provide a concrete composition containing this set accelerator for trowel finishing, and a hardened concrete product made from this concrete composition.
[0008] As a result of intensive research into solving the above-mentioned problems, the present inventors have found that the above problems can be solved by a setting accelerator for trowel finishing containing an organic acid calcium salt and an inorganic sulfate in a predetermined ratio, and have arrived at the present invention.
[0009] [1] A set accelerator for trowel finishing, comprising an organic acid calcium salt and an inorganic sulfate, wherein the mass ratio of the organic acid calcium salt to the inorganic sulfate (organic acid calcium salt / inorganic sulfate) is 20 / 80 to 95 / 5. [2] The set accelerator for trowel finishing according to [1], wherein the organic acid calcium salt is calcium carboxylate. [3] The set accelerator for trowel finishing according to [1] or [2], wherein the inorganic sulfate comprises at least one selected from aluminum sulfate, sodium thiosulfate, and potassium alum. [4] The set accelerator for trowel finishing according to any one of [1] to [3], wherein 95% or more of the organic acid calcium salt and the inorganic sulfate pass through a 0.6 mm sieve by mass. [5] A concrete composition comprising the set accelerator for trowel finishing according to any one of [1] to [4] and cement. [6] A concrete composition comprising the set accelerator for trowel finishing according to any one of [1] to [4] and cement. [7] A concrete composition comprising the set accelerator for trowel finishing, wherein the mass ratio of the set accelerator for trowel finishing is 1 / 200 to 1 / 400. 3 [7] The concrete composition according to [5] or [6], further comprising an expansive additive. [8] A hardened body obtained by hardening the concrete composition according to any one of [5] to [7].
[0010] According to the present invention, it is possible to provide a trowel-finishing set accelerator that can maintain the fluidity of concrete and shorten the time from pouring concrete until it can be trowel-finished, a concrete composition containing this trowel-finishing set accelerator, and a hardened concrete body made from this concrete composition.
[0011] The setting accelerator for trowel finishing, the concrete composition, and the hardened concrete product of the present invention will be described in detail below, but the present invention is not limited to these embodiments. In this specification, "%" is based on mass unless otherwise specified. Furthermore, a numerical range specified using the symbol "to" includes the numerical values at both ends (upper and lower limits) of "to".
[0012] [Set accelerator for trowel finishing] The set accelerator for trowel finishing of the present invention (hereinafter also simply referred to as "set accelerator") contains an organic acid calcium salt and an inorganic sulfate, and the mass ratio of the organic acid calcium salt to the inorganic sulfate (organic acid calcium salt / inorganic sulfate) is 20 / 80 to 95 / 5.
[0013] The total of the organic acid calcium salt and inorganic sulfate in the setting accelerator is preferably 80% by mass or more, and more preferably 90% by mass or more, from the viewpoint of ensuring the retention of concrete fluidity and shortening the time from concrete pouring until trowel finishing is possible (hereinafter also referred to as "trowel finishing time").
[0014] (Organic Acid Calcium Salt) The setting accelerator of the present invention contains an organic acid calcium salt. By containing an organic acid calcium salt, the time until trowel finishing can be shortened. As the organic acid calcium salt, a carboxylic acid calcium salt can be used, and for example, calcium formate, calcium acetate, and calcium lactate can be used. Only one type of organic acid calcium can be used, or two or more types can be used. In this embodiment, it is preferable to use calcium formate from the viewpoint of shortening the time until trowel finishing.
[0015] In this embodiment, the content of the organic acid calcium salt in the set accelerator is preferably 20% by mass or more and 95% by mass or less, more preferably 30% by mass or more and 90% by mass or less, and even more preferably 40% by mass or more and 85% by mass or less. By making the content of the organic acid calcium salt 20% by mass or more, the time until trowel finishing can be shortened. Furthermore, by making the content 95% by mass or less, the fluidity of the concrete can be appropriately reduced.
[0016] Furthermore, the organic acid calcium used in the setting accelerator of the present invention is preferably in powder form, and preferably has a content passing through a 0.6 mm sieve of 95% or more. By making the organic acid calcium powder so that 95% or more of the content passing through a 0.6 mm sieve, good trowel finishability can be achieved. Good trowel finishability means that the concrete surface after trowel finish is smooth and free of pockmarks, bubbles, and uneven finish. Furthermore, bleeding after trowel finish can be easily suppressed.
[0017] (Inorganic sulfate) The setting accelerator of the present invention contains an inorganic sulfate. By containing an inorganic sulfate, the fluidity retention of concrete can be improved. As the inorganic sulfate, for example, aluminum sulfate and alkali metal sulfates such as sodium sulfate, sodium thiosulfate, and potassium alum are preferred, and aluminum sulfate, sodium thiosulfate, and potassium alum are more preferred. Among them, aluminum sulfate is particularly effective in maintaining the fluidity of the concrete to be produced and reducing the total alkali content (R 2 The inorganic sulfates may be used alone or in combination of two or more.
[0018] In this embodiment, the content of inorganic sulfate in the setting accelerator is preferably 5% by mass or more and 80% by mass or less, more preferably 10% by mass or more and 60% by mass or less, and even more preferably 15% by mass or more and 50% by mass or less. By setting the content of inorganic sulfate to 5% by mass or more, the fluidity of concrete can be appropriately reduced. Furthermore, by setting the content to 80% by mass or less, the time until trowel finishing can be shortened.
[0019] The inorganic sulfate used in the setting accelerator of the present invention is preferably in powder form, and preferably has a content of 95% or more passing through a 0.6 mm sieve. By making the content of the inorganic sulfate powder 95% or more passing through a 0.6 mm sieve, the finishability with a trowel can be improved. Furthermore, bleeding after trowel finishing can be easily suppressed.
[0020] The set accelerator of the present invention has a mass ratio of organic acid calcium salt to inorganic sulfate (organic acid calcium salt / inorganic sulfate) of 20 / 80 to 95 / 5. If the mass ratio of organic acid calcium salt to inorganic sulfate is less than 20 / 80, the time until troweling is possible is shortened, but the fluidity retention of the concrete is poor. If it exceeds 95 / 5, the fluidity of the concrete is improved, and the slump range is exceeded. The organic acid calcium salt / inorganic sulfate ratio is preferably 30 / 70 to 90 / 10, and more preferably 40 / 60 to 80 / 20.
[0021] In addition, the setting accelerator of this embodiment can use one or more of concrete expansion additives and shrinkage reducing agents in addition to the above-mentioned organic acid calcium salts and inorganic sulfates, within a range that does not substantially impair the object of the present invention.
[0022] [Method for manufacturing the setting accelerator] The setting accelerator of this embodiment is manufactured by mixing the respective materials. The mixing method is not particularly limited, and an existing mixing device can be used.
[0023] [Concrete Composition] The concrete composition according to this embodiment contains a set accelerator and cement.
[0024] The cement is not particularly limited, and examples include various Portland cements such as normal, early-strength, ultra-early-strength, low-heat, and moderate-heat; various blended cements obtained by mixing these Portland cements with blast furnace slag, fly ash, silica fume, etc.; environmentally friendly cements (ecocements) produced using municipal waste incineration ash or sewage sludge incineration ash as raw materials; commercially available fine particle cements; and white cements. Various cements can also be finely powdered and used. Also, cements prepared by increasing or decreasing the amount of components (e.g., gypsum) normally used in cements can be used. Furthermore, combinations of two or more of these can also be used.
[0025] The setting accelerator of the present invention is 3 The content of the setting accelerator is preferably 0.5 to 8 kg per 1 m of concrete composition, more preferably 2.5 to 5 kg, and even more preferably 3 to 4 kg.3 By setting the weight to 0.5 to 8 kg per unit weight, the effect of shortening the time required for finishing with a trowel can be easily obtained, and the fluidity retention of the concrete can be improved.
[0026] The set accelerator is preferably contained in an amount of 0.10 to 2 parts by mass, more preferably 0.45 to 1.7 parts by mass, and even more preferably 0.55 to 1.4 parts by mass, per 100 parts by mass of cement. By containing the set accelerator in an amount of 0.10 to 2 parts by mass per 100 parts by mass of cement, it becomes easier to shorten the time until trowel finishing is possible, and the fluidity retention of the concrete can be improved.
[0027] The concrete composition preferably contains aggregate. The aggregate used may be the same fine aggregate or coarse aggregate as that used in ordinary cement mortar or concrete. Specifically, river sand, river gravel, mountain sand, mountain gravel, crushed stone, crushed sand, limestone aggregate, lime sand, silica sand, colored sand, artificial aggregate, blast furnace slag aggregate, sea sand, sea gravel, artificial lightweight aggregate, heavy aggregate, etc., or a combination of these may be used.
[0028] The concrete composition may contain a water-reducing agent. When the concrete composition contains a water-reducing agent, the fluidity retention is easily improved. Examples of the water-reducing agent include polyol derivatives, lignin sulfonates and their derivatives, and high-performance water-reducing agents, and one or more of these may be used in combination. Among these, high-performance water-reducing agents are preferred from the viewpoint of fluidity retention.
[0029] Examples of high-performance water-reducing agents include formalin condensates of alkylarylsulfonates, formalin condensates of naphthalenesulfonates, formalin condensates of melamine sulfonates, and polycarboxylic acid polymer compounds, and these may be used alone or in combination of two or more. Among these, polycarboxylic acid polymer compounds are preferred because of their significant effect in retaining fluidity.
[0030] The amount of high-range water-reducing agent used is preferably 0.05 to 3 parts by mass, more preferably 0.1 to 2 parts by mass, per 100 parts by mass of cement. When the amount is 0.05 to 3 parts by mass, sufficient fluidity retention effect is easily obtained. While liquid or powdered high-range water-reducing agents can be used, it is preferable to premix a powdered water-reducing agent with the concrete composition of the present invention in order to reduce workability and fluctuations in physical properties during on-site use.
[0031] The concrete composition can contain an expansive additive. By using the set accelerator of the present invention in a concrete composition containing an expansive additive, it is possible to improve the fluidity of the concrete and shorten the time from pouring to troweling, while imparting a predetermined expansive property and reducing subsequent shrinkage and cracking. Furthermore, a shrinkage-reducing agent can be used instead of or in addition to the expansive additive.
[0032] The expansive agent is not particularly limited, and any agent that has the effect of generating expansion hydrates and expanding concrete or mortar can be used. As the expansive agent, those containing free lime, free magnesia, calcium ferrite, ettringite, lime, ettringite-lime composite, and hauyne are preferred, because they inhibit shrinkage and are more likely to exhibit their expansive agent effect when combined with the organic acid calcium salt and inorganic sulfate contained in the setting accelerator.
[0033] The particle size of the expansive material is 2000 to 9000 cm in terms of Blaine specific surface area. 2 / g, and 3000 to 8000 cm 2 / g. 2 / g or more, the hydration reaction proceeds well, and 2 / g or less, the hydration reaction does not proceed too quickly, making it easier to obtain the desired expansion. In this specification, the Blaine specific surface area can be determined in accordance with JIS R 5201.
[0034] The amount of expansive agent used is 1 m of concrete composition. 3 5 to 30 kg / m3 It is preferable that the density is 10 to 25 kg / m 3 It is more preferable that the load is about 5 kg / m. 3 This makes it easier to obtain the shrinkage compensation effect, and 3 By keeping the value below this, it is possible to prevent the expansion amount from becoming too large and the strength from decreasing.
[0035] The concrete composition may contain an alkali metal carbonate. When the concrete composition contains an alkali metal carbonate, the fluidity retention is easily improved. Examples of the alkali metal carbonate include sodium carbonate, potassium carbonate, lithium carbonate, sodium bicarbonate, potassium bicarbonate, and lithium bicarbonate, and these may also be combined.
[0036] The concrete composition may contain a siliceous fine powder. When the concrete composition contains the siliceous fine powder, it is easy to improve the fluidity retention. Examples of the siliceous fine powder include latent hydraulic substances such as ground granulated blast furnace slag, fly ash, and pozzolanic substances such as silica fume, and among these, silica fume is preferred. The type of silica fume is not limited, but from the viewpoint of fluidity, it is preferable to use silica fume containing ZrO as an impurity. 2 It is more preferable to use silica fume containing 10% or less of the above-mentioned compound or acidic silica fume. Acidic silica fume is a silica fume that, when 1 g of silica fume is added to 100 cc of pure water and stirred, the supernatant liquid has an acidic pH of 5.0 or less.
[0037] The concrete composition may contain an antifoaming agent to the extent that it does not adversely affect performance. Antifoaming agents are used to reduce the amount of air entrained during mixing. The type of antifoaming agent is not particularly limited as long as it does not significantly adversely affect the strength properties of the hardened mortar, and both liquid and powder forms can be used. Examples include polyether-based antifoaming agents, polyhydric alcohol-based antifoaming agents such as polyhydric alcohol esters and alkyl ethers, alkyl phosphate-based antifoaming agents, and silicone-based antifoaming agents.
[0038] In addition, the concrete composition may contain one or more of the following additives, within a range that does not adversely affect performance: shrinkage-reducing agents, gas foaming substances, air-entraining agents, rust inhibitors, water repellents, antibacterial agents, colorants, antifreeze agents, limestone fine powder, slowly cooled blast furnace slag fine powder, sewage sludge incineration ash and its molten slag, municipal waste incineration ash and its molten slag, and pulp sludge incineration ash; thickeners; shrinkage-reducing agents; polymers; clay minerals such as bentonite and sepiolite; and anion exchangers such as hydrotalcite.
[0039] [Hardened body] The hardened body according to this embodiment is obtained by hardening a concrete composition and water. The hardened body is usually formed by kneading the concrete composition with water, causing a hydration reaction in the cement, which is a hydraulic material, and hardening the concrete. The amount of water used for mixing is not particularly limited, but is preferably 10 to 70 parts by mass, more preferably 14 to 65 parts by mass, and even more preferably 16 to 60 parts by mass, per 100 parts by mass of the concrete composition. By keeping the amount of water used for mixing within the above range, the fluidity retention effect can be enhanced.
[0040] The hardened concrete body is produced by mixing the set accelerator, cement, and water to produce a cement composition, and then hardening the concrete composition. The mixing of the materials is not particularly limited; the materials may be mixed at the time of construction, or some or all of the materials may be mixed in advance. For example, when mixing a portion of the materials in advance, the concrete composition other than the set accelerator and water can be mixed at the construction site, and the set accelerator can be mixed at the construction site. Any existing mixer, such as a tilting mixer, omni mixer, Henschel mixer, V-type mixer, Plosser mixer, or Nauta mixer, can be used as the mixer.
[0041] Furthermore, the temperature during hardening of the concrete composition is preferably 20°C or lower, more preferably 18°C or lower, and even more preferably 15°C or lower. By using the set accelerator of the present invention, even if hardening (curing) is carried out at a low temperature of 20°C or lower, the time until trowel finishing can be shortened and the fluidity retention effect can be enhanced. In other words, the set accelerator of the present invention can be used particularly effectively at low temperatures.
[0042] The present invention will be explained in more detail below by way of examples, but the present invention is not limited to these examples.
[0043] <Measurement Method> The concrete compositions prepared in each experimental example were evaluated using the following methods. (Slump) The slump of the base concrete was measured in accordance with JIS A 1150 immediately after mixing (0 minutes), 30 minutes later (immediately after adding the set accelerator), 60 minutes later, and 90 minutes later. A good result was obtained when the slump after 60 minutes was in the range of 15.5 to 20.5 cm when using base concrete of Mixture No. 1, and in the range of 12.5 to 17.5 cm when using base concrete of Mixture No. 2. (Initial Set Time) The initial set time was measured in accordance with JIS A 1147:2019. A good result was obtained when the initial set time was shortened by 60 minutes or more compared to the reference example without the addition of a set accelerator. (Bleeding Pull Time) The bleeding was measured in accordance with the concrete bleeding test method (JIS A 1123), and the time until bleeding was no longer observed was defined as the bleeding pull time.
[0044] <Preparation of base concrete> Base concrete was prepared according to the mix proportions shown in Table 1 below. Two types of base concrete were prepared: Mix No. 1 using a high-range water-reducing agent, and Mix No. 2 using a high-range water-reducing agent. The water-reducing agent was added in an amount of 0.8% cement for Mix No. 1 and 1.0% cement for Mix No. 2. The materials used are listed below. (Materials used) Cement: Ordinary Portland cement (commercially available product) Water: Tap water Fine aggregate: River sand from Himekawa River Coarse aggregate: Crushed stone from Himekawa River Water-reducing agent: Polycarboxylic acid high-range water-reducing agent (manufactured by GCP Chemicals Co., Ltd., product name: Super 100phx) Lignin sulfonic acid-based water-reducing agent (manufactured by GCP Chemicals Co., Ltd., product name: WRDA)
[0045]
[0046] (Experimental Example 1) A set accelerator was prepared in the amounts shown in Table 2 below, and added 30 minutes after the base concrete of Mixture No. 1 was completely mixed, followed by mixing to prepare a concrete composition. The slump and initial slump were measured a predetermined time after the base concrete was completely mixed. The environmental temperature for all tests was 10°C. The results are shown in Table 2.
[0047]
[0048] (Raw materials used) Calcium formate: manufactured by Asahi Chemical Industry Co., Ltd., 98% passing through a 0.6 mm sieve Anhydrous aluminum sulfate: manufactured by Taimei Chemical Industry Co., Ltd., 100% passing through a 0.6 mm sieve Powdered aluminum sulfate 14-hydrate: manufactured by Taimei Chemical Industry Co., Ltd., 98% passing through a 0.6 mm sieve (pulverized product used) Potassium alum: manufactured by Taimei Chemical Industry Co., Ltd., 100% passing through a 0.6 mm sieve Sodium thiosulfate: manufactured by Air Water Performance Chemicals Inc., 98% passing through a 0.6 mm sieve
[0049] As shown in Table 2, in Examples No. 1-2 to 1-5 of the present invention, the initial set time could be shortened, and the slump could be set to a value equivalent to that in the case where no setting accelerator was added.
[0050] (Experimental Example 2) A set accelerator was prepared in the amounts shown in Table 3 below, and added 30 minutes after the base concrete of Mixture No. 1 was completely mixed, followed by mixing to prepare a concrete composition. The slump, initial bleeding time, and bleeding time were measured a predetermined time after the base concrete was completely mixed. The results are shown in Table 3.
[0051]
[0052] As shown in Table 3, Test Nos. 2-2 to 2-10, which are examples of the present invention, achieved favorable results. In particular, Test Nos. 2-2 to 2-4, which used aluminum sulfate, had a setting acceleration effect and were able to moderately reduce fluidity. Test Nos. 2-11 to 2-16, in which the ratio of organic acid calcium salt to inorganic sulfate was outside the range of the present invention, and Test Nos. 2-17 to 2-20, in which only one of the components was used, were unable to maintain slump.
[0053] (Experimental Example 3) A set accelerator was prepared in the amounts shown in Table 4 below, and added 30 minutes after the base concrete of Mixture No. 2 was completely mixed, followed by mixing to prepare a concrete composition. The slump, initial bleeding time, and bleeding time were measured a predetermined time after the base concrete was completely mixed. The results are shown in Table 4.
[0054]
[0055] As shown in Table 4, even when a lignin sulfonic acid-based water-reducing agent is used as the water-reducing agent, it was confirmed that the use of the setting accelerator of the present invention can improve slump retention, shorten the initial settling time, and shorten the bleeding time.
[0056] (Experimental Example 4) A set accelerator was prepared using calcium formate and calcium acetate as organic acid calcium in the amounts shown in Table 5 below. Thirty minutes after the base concrete of Mixture No. 1 was completely mixed, the accelerator was added and mixed to prepare a concrete composition. The slump, initial bleeding time, and bleeding time were measured after a predetermined time had elapsed since the base concrete was completely mixed. The results are shown in Table 5.
[0057]
[0058] (Raw materials used) Calcium acetate: manufactured by Yoneyama Chemical Industry Co., Ltd., 98% passing through a 0.6 mm sieve (coarse particles removed)
[0059] Good results were also obtained when calcium acetate was used as the organic acid calcium.
[0060] (Experimental Example 5) A set accelerator was prepared using 80% by mass of calcium formate as an organic acid calcium salt and 20% by mass of aluminum sulfate as an inorganic sulfate. The set accelerator was added in the amounts shown in Table 5 30 minutes after the base concrete of Mix No. 1 was mixed, and the concrete was mixed to prepare a concrete composition. The slump, initial bleeding time, and bleeding time were measured after a predetermined time had elapsed since the base concrete was mixed. The results are shown in Table 6.
[0061]
[0062] As shown in Table 6, when the amount of setting accelerator added was small, the initial set time was long, and when the amount added was large, the decrease in slump was suppressed.
[0063] (Experimental Example 6) A setting accelerator was prepared using 80% by mass of calcium formate as the organic calcium salt and 20% by mass of aluminum sulfate as the inorganic sulfate. The calcium formate and aluminum sulfate were raw materials whose 0.6 mm sieve passing ratios are shown in Table 7. The prepared setting accelerator was measured for slump, initial bleeding time, and bleeding time after a predetermined time had elapsed since the base concrete was mixed. The results are shown in Table 7.
[0064]
[0065] (Experimental Example 7) Using a concrete composition containing an expansive additive, the effect of adding a set accelerator on the expansion rate was confirmed. The slump and initial set time were also confirmed. The composition of the base concrete containing the expansive additive used in Experimental Example 7 is shown in Table 8. The expansive additive used was an ettringite-lime composite (Denka Power CSA) or a lime-based (Pacific Materials Hyperexpan). The binder in Table 8 is the total amount of C (cement) and expansive additive.
[0066]
[0067] The setting accelerators used were those listed in Table 9. As a comparative example, a setting accelerator consisting of aluminum sulfate, a water-reducing agent, and a retarder was used. The water-reducing agent and retarder used in Test No. 7-2 were as follows: Water-reducing agent: Lignin sulfonic acid type Retarder: Tartaric acid
[0068] The set accelerator was prepared in the amounts shown in Table 9 below, and 30 minutes after the base concrete containing the expansive additive of Mix No. 3 was completely mixed, the set accelerator was added and mixed to prepare a concrete composition. The expansion rate was measured a predetermined number of days after the base concrete containing the expansive additive was completely mixed. The results are shown in Table 9. The expansion rate was measured based on the test method for expansive additives for concrete of JIS A 6202.
[0069]
[0070] As shown in Table 9, in Test Nos. 7-3 to 7-5, which are examples of the present invention, no difference in expansion coefficient was observed compared to Test No. 7-1, in which no set accelerator was added. In Test No. 7-2, which did not contain an organic acid (calcium formate), the expansion coefficient was reduced to about one-third of that of Test No. 7-1, in which no set accelerator was added. Even when added to a concrete composition containing an expansive additive, the set accelerator of the present invention can achieve an expansion coefficient equivalent to that of a concrete composition to which no set accelerator is added, or can suppress a decrease in the expansion coefficient.
[0071] By using the setting accelerator for trowel finishing of the present invention, the fluidity of concrete can be maintained and the time from concrete pouring to trowel finishing can be shortened, so that it can be widely applied in the fields of civil engineering and construction.
Claims
1. A setting accelerator for trowel finishing, comprising an organic acid calcium salt and an inorganic sulfate, wherein the mass ratio of the organic acid calcium salt to the inorganic sulfate (organic acid calcium salt / inorganic sulfate) is 20 / 80 to 95 / 5.
2. The setting accelerator for trowel finishing according to claim 1, wherein the organic acid calcium salt is a calcium carboxylate.
3. The setting accelerator for trowel finishing according to claim 1 or 2, wherein the inorganic sulfate comprises at least one selected from aluminum sulfate, sodium thiosulfate, and potassium alum.
4. A setting accelerator for trowel finishing according to claim 1 or 2, wherein the organic acid calcium salt and the inorganic sulfate have a mass ratio of 95% or more passing through a 0.6 mm sieve.
5. A concrete composition containing the setting accelerator for trowel finishing according to claim 1 or 2 and cement.
6. The content of the trowel finishing setting accelerator is 1 m of the concrete composition. 3 The concrete composition according to claim 5, wherein the weight of the concrete composition is 0.5 to 8 kg per unit weight.
7. The concrete composition of claim 5, further comprising an expansive material.
8. A hardened body obtained by hardening the concrete composition according to claim 5.
Citation Information
Patent Citations
Manufacture of concrete product
JP1999090918A
Cement hardening accelerator and cement hardening acceleratig method
JP2001213646A
Trowelled finishing agent and usage thereof
WO2019142906A1
Method for feeding hardening accelerator for concrete surface finish
WO2019244601A1