Reflective mask blank, method for producing reflective mask blank, reflective mask, and method for producing reflective mask

The reflective mask blank configuration with a ruthenium-based hard mask film and protective film composition addresses the challenge of forming fine patterns and maintaining reflective properties, ensuring efficient pattern transfer and minimizing reflective characteristic deterioration.

WO2024204068A1PCT designated stage expired Publication Date: 2024-10-03AGC INC

Patent Information

Application Number
PCT/JP2024/011707
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-25
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing reflective mask blanks struggle to form fine mask patterns and maintain the reflective properties of multilayer reflective films during the manufacturing process of semiconductor devices, leading to deteriorated reflective characteristics.

Method used

A reflective mask blank configuration with a substrate, a multilayer reflective film, a protective film containing more than 50 atomic percent of Rh, Pd, or Ir, and a hard mask film made of ruthenium, along with an intermediate film and an absorber film, where the hard mask film has a specific dry etching ratio and chemical resistance to prevent deterioration of the reflective properties.

Benefits of technology

Enables the easy formation of fine mask patterns while maintaining the reflective properties of the multilayer reflective film, allowing for precise pattern transfer and reducing the risk of reflective characteristic deterioration during the manufacturing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011707_03102024_PF_FP_ABST
    Figure JP2024011707_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention addresses the problem of providing a reflective mask blank which makes it possible to easily form a fine mask pattern when producing a reflective mask, and which is not prone to degradation of reflection properties of a multilayer reflective film. A reflective mask blank (10) comprises a substrate (12), a multilayer reflective film (14) that reflects EUV light, a protective film (16), an absorbent body film (18), and a hard mask film (20) in this order, wherein the protective film (16) contains more than 50 at% of at least one element selected from the group consisting of rhodium, palladium, iridium, and platinum, and the hard mask film (20) contains ruthenium.
Need to check novelty before this filing date? Find Prior Art

Description

Reflective mask blank, manufacturing method of reflective mask blank, reflective mask, and manufacturing method of reflective mask

[0001] The present invention relates to a reflective mask used in EUV (Extreme Ultra Violet) exposure used in the exposure process of semiconductor manufacturing, a method for manufacturing the same, a reflective mask blank that is an original plate for the reflective mask, and a method for manufacturing the same.

[0002] In recent years, in order to further miniaturize semiconductor devices, EUV lithography using EUV light with a central wavelength of around 13.5 nm as a light source has been considered.

[0003] Due to the characteristics of EUV light, EUV exposure uses a reflective optical system and a reflective mask. A reflective mask has a multilayer reflective film that reflects EUV light formed on a substrate, and an absorber film that absorbs EUV light is patterned on the multilayer reflective film.

[0004] The EUV light incident on the reflective mask from the illumination optical system of the exposure tool is reflected by the areas without an absorber film (openings) and absorbed by the areas with an absorber film (non-openings). As a result, the mask pattern is transferred as a resist pattern onto the wafer through the reduced projection optical system of the exposure tool, and subsequent processing is carried out.

[0005] In a reflective mask blank, a hard mask film may be provided on the side of the absorber film of the reflective mask blank opposite the multilayer reflective film side in order to further refine the line width. Typically, dry etching is often used to etch the absorber film, but if the reflective mask blank has a hard mask film, the hard mask film functions as a mask when dry etching the absorber film. In this way, since the photoresist does not need to function as a dry etching mask in the manufacturing process of the reflective mask, the thickness of the photoresist for forming a pattern corresponding to the absorber film pattern can be made thinner, making it possible to form a finer absorber film pattern. If a finer absorber film pattern can be formed, a finer resist pattern can be formed on the wafer.

[0006] As an example of a reflective mask blank having such a hard mask film, Patent Document 1 discloses a reflective mask blank having a hard mask film containing chromium, nitrogen, and hydrogen.

[0007] International Publication No. 2012 / 105508

[0008] Recently, there has been a demand for even finer patterns formed using reflective masks, and a demand has arisen for a reflective mask blank capable of forming a reflective mask having a finer absorber film pattern. Hereinafter, the absorber film pattern in a reflective mask will also be simply referred to as a "mask pattern." When the present inventors investigated the technology described in Patent Document 1, they found that it was difficult to form the fine mask patterns currently required. Furthermore, when manufacturing a reflective mask, the reflective characteristics of the resulting reflective mask were often degraded.

[0009] The present invention has been made in view of the above-mentioned problems, and aims to provide a reflective mask blank that allows for easy formation of a fine mask pattern and is less likely to cause deterioration in the reflective properties of the multilayer reflective film when manufacturing a reflective mask. Another aim of the present invention is to provide a method for manufacturing the reflective mask blank, as well as a reflective mask and a method for manufacturing a reflective mask.

[0010] As a result of intensive research into the above-mentioned problems, the inventors discovered that the chemical resistance of the hard mask film and adjustment of the dry etching ratio between the protective film and the hard mask film are important, and arrived at the present invention. That is, the inventors found that the above-mentioned problems can be solved by the following configuration. [1] A reflective mask blank having, in this order, a substrate, a multilayer reflective film that reflects EUV light, a protective film, an absorber film, and a hard mask film, wherein the protective film contains more than 50 atomic % of one or more elements selected from the group consisting of rhodium, palladium, iridium, and platinum, and the hard mask film contains ruthenium. [2] The reflective mask blank according to [1], wherein the hard mask film consists solely of ruthenium, or wherein the hard mask film contains ruthenium and one or more elements selected from the group consisting of boron, carbon, nitrogen, oxygen, titanium, chromium, zirconium, niobium, molybdenum, palladium, tantalum, and iridium. [3] The reflective mask blank according to [1] or [2], wherein the hard mask film contains 50 to 100 atomic % of ruthenium. [4] The reflective mask blank according to any of [1] to [3], wherein the hard mask film has a thickness of 0.3 to 30 nm. [5] The reflective mask blank according to any of [1] to [4], wherein the protective film further contains one or more elements selected from the group consisting of boron, carbon, nitrogen, oxygen, titanium, zirconium, niobium, molybdenum, and tantalum. [6] The reflective mask blank according to any one of [1] to [5], further comprising an intermediate film between the protective film and the multilayer reflective film, the intermediate film consisting of only ruthenium, or the intermediate film containing ruthenium and one or more elements selected from the group consisting of boron, carbon, nitrogen, oxygen, silicon, titanium, chromium, zirconium, niobium, molybdenum, palladium, and tantalum. [7] The reflective mask blank according to any one of [1] to [6], wherein the absorber film contains one or more metals selected from the group consisting of Ta, Ti, Sn, Ir, Re, Nb, Mo, and Cr. [8] The reflective mask blank according to any one of [1] to [6], further comprising an intermediate film between the protective film and the multilayer reflective film, the intermediate film consisting of ruthenium and one or more elements selected from the group consisting of boron, carbon, nitrogen, oxygen, silicon, titanium, chromium, zirconium, niobium, molybdenum, palladium, and tantalum. [9] The reflective mask blank according to any one of [1] to [6], wherein the absorber film contains one or more metals selected from the group consisting of Ta, Ti, Sn, Ir, Re, Nb, Mo, and Cr.

[10] The reflective mask blank according to any one of [1] to [6], further comprising an intermediate film between the protective film and the multilayer reflective film, the intermediate film consisting of ruthenium and one or more elements selected from the group consisting of boron, carbon, nitrogen, oxygen, silicon, titanium, chromium, zirconium, niobium, molybdenum, palladium, and tantalum. HM) to the dry etching rate (ER ABS ) ratio (ER ABS / ER HM [9] The reflective mask blank according to any one of [1] to [7], wherein the dry etching rate (ER CAP ) to the dry etching rate (ER HM ) ratio (ER HM / ER CAP ) is 30 or more and 500 or less.

[10] A reflective mask having an absorber film pattern formed by patterning the absorber film of the reflective mask blank according to any one of [1] to [9].

[11] A method for manufacturing a reflective mask, comprising a step of patterning the absorber film of the reflective mask blank according to any one of [1] to [9].

[12] A method for manufacturing a reflective mask blank, comprising forming, on a substrate, in this order: a multilayer reflective film that reflects EUV light; an intermediate film; a protective film; an absorber film; and a hard mask film, wherein the protective film contains more than 50 atomic % of one or more elements selected from the group consisting of rhodium, palladium, platinum, and iridium; and the hard mask film contains ruthenium, and the formation is carried out continuously from the start of formation of the multilayer reflective film to the end of formation of the protective film without exposure to the atmosphere.

[0011] According to the present invention, it is possible to provide a reflective mask blank that allows for easy formation of a fine mask pattern when manufacturing a reflective mask and that is less likely to cause deterioration in the reflective properties of the multilayer reflective film. Furthermore, according to the present invention, it is possible to provide a method for manufacturing a reflective mask blank, a reflective mask, and a method for manufacturing a reflective mask.

[0012] 1A and 1B are schematic diagrams showing an example of an embodiment of a reflective mask blank of the present invention, and FIG. 1C are schematic diagrams showing an example of a manufacturing process of a reflective mask using the reflective mask blank of the present invention.

[0013] The present invention will be described in detail below. The following description of the components may be based on representative embodiments of the present invention, but the present invention is not limited to such embodiments.

[0014] The meaning of each description in this specification is shown below. In this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​written before and after "to" as the lower and upper limits. In this specification, elements such as boron, carbon, nitrogen, oxygen, silicon, titanium, chromium, zirconium, niobium, molybdenum, ruthenium, rhodium, palladium, tantalum, rhenium, iridium, and platinum may be represented by their corresponding element symbols (B, C, N, O, Si, Ti, Cr, Zr, Nb, Mo, Ru, Rh, Pd, Ta, Re, Ir, and Pt, etc.).

[0015] <Reflective Mask Blank> The reflective mask blank of the present invention is a reflective mask blank having, in this order, a substrate, a multilayer reflective film that reflects EUV light, a protective film, an absorber film, and a hard mask film, wherein the protective film contains more than 50 atomic % of one or more elements selected from the group consisting of Rh, Pd, Ir, and Pt, and the hard mask film contains Ru. The reflective mask blank of the present invention will be described with reference to the drawings.

[0016] FIG. 1 is a cross-sectional view showing an example of an embodiment of the reflective mask blank of the present invention. The reflective mask blank 10 shown in FIG. 1 has a substrate 12, a multilayer reflective film 14, a protective film 16, an absorber film 18, and a hard mask film 20, in this order. The protective film 16 contains more than 50 atomic % of one or more elements selected from the group consisting of Rh, Pd, Ir, and Pt. The hard mask film 20 contains Ru. Although not shown in FIG. 1 , the reflective mask blank 10 may have a backside conductive film (described later) on the side of the substrate 12 opposite the hard mask film side. The reflective mask blank 10 may also have an intermediate film (described later) between the protective film 16 and the multilayer reflective film 14.

[0017] Although the mechanism by which the reflective mask blank of the present invention facilitates the formation of fine mask patterns and prevents deterioration of the reflective properties of the multilayer reflective film when manufacturing a reflective mask is not entirely clear, the inventors speculate as follows. The reflective mask blank of the present invention has excellent chemical resistance because the hard mask film contains Ru. When the hard mask film has excellent chemical resistance, the film thickness of the hard mask film is less likely to be reduced by chemicals used to strip the resist pattern formed on the hard mask film, allowing the hard mask film to be thin. This also allows the film thickness of the resist pattern that functions as a mask when patterning the hard mask film to be thin. A thin resist pattern facilitates the formation of a high-resolution resist pattern, which is thought to facilitate the formation of a fine mask pattern. Furthermore, when manufacturing a reflective mask, the absorber film is often dry-etched in a pattern using the hard mask film pattern as a mask until the protective film is exposed. After the absorber film is dry-etched in a pattern, the hard mask film is removed. The removal of the hard mask film is often accomplished by dry etching, and the hard mask film and the protective film are exposed to the dry etching. A protective film containing more than 50 atomic % of one or more elements selected from the group consisting of Rh, Pd, Ir, and Pt is less susceptible to dry etching than a hard mask film containing Ru, and the hard mask film containing Ru is more likely to be selectively removed. This allows the protective film to remain at a predetermined thickness and exert its protective function on the multilayer reflective film, which is thought to reduce the deterioration of the reflective properties of the multilayer reflective film.

[0018] The structure of the reflective mask blank of the present invention will be described below.

[0019] [Substrate] The substrate of the reflective mask blank of the present invention preferably has a small thermal expansion coefficient. A substrate with a small thermal expansion coefficient can suppress distortion of the absorber film pattern due to heat during exposure to EUV light. The thermal expansion coefficient of the substrate is 0±1.0×10 at 20° C. -7 / °C, and 0±0.3×10 -7 / °C is more preferable. Examples of materials with a small thermal expansion coefficient include SiO 2 -TiO 2 However, the present invention is not limited to this, and substrates made of crystallized glass in which β-quartz solid solution is precipitated, quartz glass, metallic silicon, metal, and the like can also be used. 2 -TiO 2 The SiO-based glass 2 90 to 95 mass% of TiO 2 It is preferable to use quartz glass containing 5 to 10 mass % of TiO 2 When the content of SiO is 5 to 10 mass %, the linear expansion coefficient is approximately zero at around room temperature, and there is almost no change in dimension at around room temperature. 2 -TiO 2 The SiO-based glass 2 and TiO 2 It may contain other minor components.

[0020] The surface of the substrate on which the multilayer reflective film is laminated (hereinafter also referred to as the "first principal surface") preferably has high surface smoothness. The surface smoothness of the first principal surface can be evaluated by surface roughness. The surface roughness of the first principal surface is preferably 0.15 nm or less in terms of root-mean-square roughness Rq. Note that the surface roughness can be measured using an atomic force microscope, and the surface roughness is described as the root-mean-square roughness Rq based on JIS-B0601. The first principal surface is preferably surface-processed to achieve a predetermined flatness, in order to improve the pattern transfer accuracy and positional accuracy of a reflective mask obtained using the reflective mask blank. In a predetermined region of the first principal surface (e.g., a 132 mm × 132 mm region), the substrate preferably has a flatness of 100 nm or less, more preferably 50 nm or less, and even more preferably 30 nm or less. The flatness can be measured using a flatness measuring instrument manufactured by Fujinon Corporation. The size and thickness of the substrate are determined appropriately based on the design values ​​of the mask, etc. For example, the outer dimensions may be 6 inches (152 mm) square and the thickness may be 0.25 inches (6.3 mm). Furthermore, the substrate preferably has high rigidity in order to prevent deformation due to film stress of films (multilayer reflective film, absorber film, etc.) formed on the substrate. For example, the Young's modulus of the substrate is preferably 65 GPa or more.

[0021] [Multilayer reflective film] The multilayer reflective film of the reflective mask blank of the present invention is not particularly limited as long as it has the desired properties as a reflective film for an EUV mask blank. The multilayer reflective film preferably has a high reflectivity for EUV light. Specifically, when EUV light is incident on the surface of the multilayer reflective film at an incident angle of 6°, the maximum reflectivity for EUV light with a wavelength of around 13.5 nm is preferably 60% or more, more preferably 65% ​​or more. Similarly, even when a protective film is laminated on the multilayer reflective film, the maximum reflectivity for EUV light with a wavelength of around 13.5 nm is preferably 60% or more, more preferably 65% ​​or more.

[0022] Since multilayer reflective films can achieve high reflectivity for EUV light, they are typically formed by alternately stacking multiple high-refractive index layers, which exhibit a high refractive index for EUV light, and multiple low-refractive index layers, which exhibit a low refractive index for EUV light. The multilayer reflective film may be formed by stacking multiple cycles of a stack structure in which high-refractive index layers and low-refractive index layers are stacked in this order from the substrate side, or multiple cycles of a stack structure in which low-refractive index layers and high-refractive index layers are stacked in this order. The high-refractive index layer may be a layer containing Si. Examples of materials containing Si include elemental Si and Si compounds containing one or more elements selected from the group consisting of B, C, N, and O. The use of a high-refractive index layer containing Si results in a reflective mask with excellent reflectivity for EUV light. The low-refractive index layer may be a layer containing a metal selected from the group consisting of Mo, Ru, Rh, and Pt, or an alloy thereof. Si is commonly used for the high-refractive index layer, and Mo is commonly used for the low-refractive index layer. That is, Mo / Si multilayer reflective films are most common, but the multilayer reflective films are not limited to this, and Ru / Si multilayer reflective films, Mo / Be multilayer reflective films, Mo compound / Si compound multilayer reflective films, Si / Mo / Ru multilayer reflective films, Si / Mo / Ru / Mo multilayer reflective films, and Si / Ru / Mo / Ru multilayer reflective films can also be used.

[0023] The thickness of each layer constituting the multilayer reflective film and the number of repeating units of the layer can be appropriately selected depending on the film material used and the reflectivity of the reflective layer required for EUV light. Taking a Mo / Si multilayer reflective film as an example, to obtain a multilayer reflective film with a maximum reflectivity of 60% or more for EUV light, it is sufficient to laminate a Mo film with a thickness of 2.3±0.1 nm and a Si film with a thickness of 4.5±0.1 nm so that the number of repeating units is 30 to 60.

[0024] Each layer constituting the multilayer reflective film can be formed to a desired thickness using a known film formation method, such as magnetron sputtering or ion beam sputtering. For example, when forming a multilayer reflective film using ion beam sputtering, ion particles are supplied from an ion source to a target of a high refractive index material and a target of a low refractive index material. When the multilayer reflective film is a Mo / Si multilayer reflective film, for example, a Si layer having a predetermined thickness is first formed on a substrate using an ion beam sputtering method, followed by a Mo layer having a predetermined thickness using an Mo target. This Si layer and Mo layer constitute one cycle, and 30 to 60 cycles are stacked to form the Mo / Si multilayer reflective film.

[0025] [Protective Film] The protective film of the reflective mask blank of the present invention contains more than 50 atomic % of one or more elements selected from the group consisting of Rh, Pd, Ir, and Pt (hereinafter also referred to as "first specified element"). The protective film serves to protect the multilayer reflective film from damage during etching (usually a dry etching process) to form a pattern on the absorber film. It also serves to protect the multilayer reflective film during removal of the hard mask film. Note that "containing more than 50 atomic % of the first specified element" means that when one element is contained as the first specified element, the content of that element is more than 50 atomic % of all atoms in the protective film. Furthermore, when two or more elements are contained as the first specified element, the total content of those elements is more than 50 atomic % of all atoms in the protective film.

[0026] The protective film is not particularly limited as long as it contains more than 50 atomic % of the first specified element, but it preferably contains at least Rh, and more preferably more than 50 atomic % Rh, in order to prevent deterioration of the reflection characteristics of the multilayer reflective film. The protective film may consist solely of the first specified element, or may contain other elements. Examples of other elements include one or more elements selected from the group consisting of Si, Ti, Nb, Mo, Ru, Ta, and Zr. The protective film may also contain one or more elements selected from the group consisting of B, C, N, and O.

[0027] The content of the first specific element is more than 50 atomic %, but is preferably 60 atomic % or more, more preferably 80 atomic % or more, and even more preferably 90 atomic % or more, in that deterioration of the reflective properties of the multilayer reflective film is less likely to occur. The protective film may consist solely of the first specific element. The type and content of elements contained in the protective film are obtained by X-ray photoelectron spectroscopy (XPS). When measuring the type and content of elements contained in the protective film by XPS, the layer present on the opposite side of the protective film from the substrate is removed by sputtering or the like before the measurement is performed.

[0028] The thickness of the protective film is not particularly limited as long as it can function as a protective film. In order to maintain the reflectivity of EUV light reflected by the multilayer reflective film, the thickness of the protective film is preferably 1 to 10 nm, more preferably 1.5 to 6 nm, and even more preferably 2 to 5 nm. The thickness of the protective film can be measured by X-ray reflectometry (XRR).

[0029] The protective film can be formed by a known film formation method such as magnetron sputtering, ion beam sputtering, etc. When forming a Rh film by magnetron sputtering, it is preferable to use a Rh target as the target and Ar gas as the sputtering gas.

[0030] [Interlayer film] The reflective mask blank of the present invention may have an intermediate film between the protective film and the multilayer reflective film. The intermediate film is a layer separate from the protective film and is composed of a material with a different composition from that of the protective film. As a material for the intermediate film, a material containing one or more elements selected from the group consisting of Ru, Rh, Pd, Ir, and Pt (hereinafter also referred to as "second specific element") is preferred. Among these, a material containing one or more elements selected from the group consisting of Ru and Rh is preferred, and a material containing Ru is preferred.

[0031] The interlayer film may consist solely of the second specified element, or may contain other elements. Examples of the other elements include one or more elements selected from the group consisting of Si, Ti, Cr, Zr, Nb, Mo, Pd, and Ta. The other elements may also include at least one of B, C, N, and O. When the interlayer film contains the second specified element, the content of the second specified element is preferably more than 50 atomic %, more preferably 60 atomic % or more, even more preferably 80 atomic % or more, and particularly preferably 90 atomic % or more. The interlayer film may consist solely of the second specified element.

[0032] The thickness of the intermediate film is preferably 0.3 to 10 nm, more preferably 0.5 to 6 nm, and even more preferably 1 to 5 nm. It is also preferable to adjust the total thickness of the intermediate film and the protective film so that it falls within the above-mentioned preferred range of the protective film thickness.

[0033] The types and contents of elements contained in the interlayer film can be measured by the same method as for the protective film, and the film thickness of the interlayer film can be measured by the same method as for the protective film.

[0034] [Absorber Film] The absorber film of the reflective mask blank of the present invention is required to have a high contrast between the EUV light reflected by the multilayer reflective film and the EUV light at the absorber film when the absorber film is patterned. The patterned absorber film (absorber film pattern) may function as a binary mask by absorbing EUV light, or may function as a phase shift mask that reflects EUV light and interferes with the EUV light from the multilayer reflective film to generate contrast.

[0035] When the absorber film pattern is used as a binary mask, the absorber film must absorb EUV light and have low reflectance for EUV light. Specifically, when EUV light is irradiated onto the surface of the absorber film, the maximum reflectance of EUV light at a wavelength of around 13.5 nm is preferably 2% or less. The absorber film may contain one or more metals selected from the group consisting of Ta, Ti, Sn, Ir, Re, Nb, Mo, and Cr, as well as one or more components selected from the group consisting of O, N, B, Hf, and H. Among these, the absorber film preferably contains Ta and N or B. By containing N or B, the crystalline state of the absorber film can be made amorphous or microcrystalline. The crystalline state of the absorber film is preferably amorphous. This improves the smoothness and flatness of the absorber film. Furthermore, when the smoothness and flatness of the absorber film are increased, the edge roughness of the absorber film pattern is reduced, and the dimensional accuracy of the absorber film pattern can be increased. When the absorber film pattern is used as a binary mask, the film thickness of the absorber film is preferably 40 to 70 nm, and more preferably 50 to 65 nm.

[0036] When the absorber film pattern is used as a phase shift mask, the absorber film preferably has a reflectance of 2% or more to EUV light. To obtain a sufficient phase shift effect, the reflectance of the absorber film is preferably 9 to 15%. Using the absorber film as a phase shift mask improves the contrast of the optical image on the wafer and increases the exposure margin. Examples of materials for forming the phase shift mask include an alloy of Ta and Nb, an alloy of Ta and Re, an alloy of Ta and Mo, a TaRu alloy containing Ta and 0.1 to 10 atomic % of Ru relative to the total atoms, an oxide containing Ta or a TaNb alloy and oxygen, a nitride containing Ta or a Ta alloy and nitrogen, and an oxynitride containing Ta or a Ta alloy, oxygen, and nitrogen. Among these, a material containing Ta is more preferred, and a nitride of Ta or a Ta alloy is even more preferred. When the absorber film pattern is used as a phase shift mask, the thickness of the absorber film is preferably 30 to 75 nm, more preferably 35 to 55 nm.

[0037] The absorber film may be a single layer film or a multilayer film made up of multiple films. When the absorber film is a single layer film, the number of steps in manufacturing the mask blank can be reduced, thereby improving production efficiency. When the absorber film is a multilayer film, the layer disposed on the side opposite to the protective film side of the absorber film may be an anti-reflection film used when inspecting the absorber film pattern using inspection light (e.g., wavelength 193 to 248 nm). Examples of materials that form the anti-reflection film include materials containing Ta and O.

[0038] The absorber film can be formed by a known film formation method such as magnetron sputtering, ion beam sputtering, etc. For example, when a Ta nitride film is formed as the absorber film by magnetron sputtering, the absorber film can be formed by sputtering using a Ta target and supplying a gas containing Ar gas and nitrogen gas.

[0039] [Hard Mask Film] The hard mask film of the reflective mask blank of the present invention contains Ru. The hard mask film is not particularly limited as long as it contains Ru. However, the Ru content is preferably 30 atomic % or more, more preferably 50 atomic % or more, and even more preferably 70 atomic % or more, in order to facilitate the formation of fine mask patterns and to prevent deterioration of the reflective properties of the multilayer reflective film. The hard mask film may consist solely of Ru, and the upper limit of the Ru content is 100 atomic % or less. "Consisting solely of Ru" refers to a Ru content of 99 to 100 atomic %. The hard mask film may contain elements other than Ru. Examples of elements other than Ru contained in the hard mask film include one or more elements selected from the group consisting of B, C, N, O, Ti, Cr, Zr, Nb, Mo, Pd, Ta, and Ir. The elements other than Ru contained in the hard mask film are preferably one or more elements selected from the group consisting of B, C, N, and O, since these elements tend to reduce the crystallinity of the hard mask film, and more preferably one or more elements selected from the group consisting of N and O. The types and contents of elements contained in the hard mask film can be measured by the same method as for the protective film.

[0040] The material of the hard mask film is preferably selected so as to be resistant to dry etching by the material constituting the absorber film. By selecting the above-mentioned preferable material, the hard mask film is likely to be resistant to dry etching by the material constituting the absorber film. The dry etching rate of the hard mask film is expressed as the dry etching rate (ER) of the hard mask film. HM ) to the dry etching rate (ER ABS ), i.e., ER ABS / ER HM is preferably 50 or more, more preferably 100 or more, and even more preferably 150 or more. There is no particular upper limit, but it is preferably 1000 or less, more preferably 800 or less, still more preferably 500 or less, and particularly preferably 300 or less. The dry etching rate of the hard mask film and the dry etching rate of the absorber film are the etching rates under the gas and conditions used in dry etching of the absorber film. Detailed conditions are as described in the examples.

[0041] It is preferable to select a material for the protective film so that it is difficult to be dry-etched by the material constituting the hard mask film. When the above-mentioned preferable material is selected, the protective film is difficult to be dry-etched by the material constituting the hard mask film. The dry etching rate (ER) of the protective film is CAP ) to the dry etching rate (ER HM ), i.e., ER HM / ER CAP is preferably 30 or more, more preferably 40 or more, even more preferably 50 or more, particularly preferably 60 or more, and most preferably 70 or more. HM / ER CAPWhen the R is 30 or more, the hard mask film containing Ru is less susceptible to dry etching, and the hard mask film containing Ru is easily selectively removed. There is no particular upper limit, but it is preferably 500 or less, more preferably 300 or less, even more preferably 200 or less, and particularly preferably 150 or less. The dry etching rates of the hard mask film and the absorber film are the etching rates under the gas and conditions used in dry etching of the absorber film. Detailed conditions are as described in the examples.

[0042] When the absorber film has an anti-reflection film, it is preferable to select a material for the hard mask film so that it is difficult to be dry-etched by the material constituting the anti-reflection film. When the above-mentioned preferable material is selected, the hard mask film is difficult to be dry-etched by the material constituting the anti-reflection film. The dry etching rate of the hard mask film is expressed as the dry etching rate (ER) of the hard mask film. HM ) to the dry etching rate (ER ARC ), i.e., ER ARC / ER HM is preferably 5 or more, more preferably 7 or more. There is no particular upper limit, but an example is 500 or less. The dry etching rates of the hard mask film and the antireflective film are the etching rates using the gas and conditions used in dry etching of the antireflective film. Detailed conditions are as described in the Examples.

[0043] The material of the hard mask film is preferably selected so as to be easily dry-etched relative to the material constituting the protective film, in order to prevent deterioration of the reflective properties of the multilayer reflective film. By selecting the above-mentioned preferable material, the hard mask film is easily dry-etched relative to the material constituting the protective film. The dry etching rate of the hard mask film is determined by the dry etching rate (ER) of the protective film. CAP ) to the dry etching rate (ER HM ), i.e., ER HM / ER CAPis preferably 10 or more, and more preferably 30 or more. There is no particular upper limit, but an example is 1000. The dry etching rates of the hard mask film and the protective film are the etching rates under the gas and conditions used in dry etching of the hard mask film. Detailed conditions are as described in the Examples.

[0044] Furthermore, it is preferable that the hard mask film has high resistance to chemical solutions. Specifically, it is preferable that the hard mask film has high resistance to sulfuric acid-hydrogen peroxide aqueous solution (SPM). More specifically, it is preferable that the hard mask film does not lose thickness or only loses a small amount of thickness when it comes into contact with SPM. Details of the measurement method are as described in the Examples.

[0045] The thickness of the hard mask film is preferably 0.3 to 30 nm, more preferably 0.5 to 20 nm, even more preferably 1 to 10 nm, and particularly preferably 1 to 5 nm, in that it allows for easier formation of a fine mask pattern. The thickness of the hard mask film can be measured in the same manner as for the protective film. The thickness of the hard mask film can be set according to the above-mentioned etching rate ratio.

[0046] The crystallinity of the hard mask film is preferably low, and more preferably amorphous. The crystallinity of the hard mask film refers to a small crystallite diameter calculated using a diffraction chart obtained by X-ray diffraction (XRD). If no clear diffraction peaks are observed in the diffraction chart, the hard mask film can be said to be amorphous. Detailed methods for evaluating the crystallinity of the hard mask film are as described in the Examples. When the crystallinity of the hard mask film is low, unevenness is less likely to occur at the boundary between the etched region and the non-etched region when the hard mask film is etched, allowing for the formation of a finer mask pattern. The degree of unevenness occurring at the boundary is also called edge roughness.

[0047] The hard mask film can be formed by a known film formation method such as magnetron sputtering, ion beam sputtering, etc. For example, when a Ru film is formed as the hard mask film by ion beam sputtering, the hard mask film can be formed by using a Ru target and irradiating the Ru target with an Ar ion beam to perform sputtering.

[0048] [Back Surface Conductive Film] The reflective mask blank of the present invention may have a back surface conductive film on the surface (second main surface) opposite to the first main surface of the substrate. Providing a back surface conductive film enables the reflective mask blank to be handled using an electrostatic chuck. The back surface conductive film preferably has a low sheet resistance. The sheet resistance of the back surface conductive film is preferably, for example, 200 Ω / sq. or less, more preferably 100 Ω / sq. or less. The constituent material of the back surface conductive film can be selected from a wide range of materials described in known literature. For example, a high-dielectric-constant coating described in JP-A-2003-501823, specifically a coating made of Si, Mo, Cr, CrON, or TaSi, can be applied. Furthermore, the constituent material of the back surface conductive film may be a Cr compound containing Cr and one or more elements selected from the group consisting of B, N, O, and C, or a Ta compound containing Ta and one or more elements selected from the group consisting of B, N, O, and C. The thickness of the back surface conductive film is preferably 10 to 1,000 nm, more preferably 10 to 400 nm. The back surface conductive film may also have a function of adjusting stress on the second main surface side of the reflective mask blank. That is, the back surface conductive film can be adjusted to balance the stress from various films formed on the first main surface side and flatten the reflective mask blank. The back surface conductive film can be formed using a known film formation method, for example, a sputtering method such as magnetron sputtering or ion beam sputtering, a CVD method, a vacuum deposition method, or an electrolytic plating method.

[0049] <Method for Manufacturing a Reflective Mask Blank> The method for forming each film contained in the reflective mask blank is as described above. The reflective mask blank of the present invention can be manufactured by sequentially forming each of the above films on a substrate. Specifically, the method for manufacturing a reflective mask blank of the present invention includes a method of forming a multilayer reflective film on a substrate, forming a protective film on the multilayer reflective film, forming an absorber film on the protective film, and forming a hard mask film on the absorber film. The method for manufacturing a reflective mask blank of the present invention may also include a film manufacturing procedure other than the above. For example, after forming a multilayer reflective film, the intermediate film may be formed on the multilayer reflective film, and the protective film may be formed on the intermediate film. As described above, the protective film contains more than 50 atomic % of one or more elements selected from the group consisting of Rh, Pd, Ir, and Pt, and the hard mask film contains Ru. Here, when the intermediate film is formed on the multilayer reflective film after forming the multilayer reflective film, and then the protective film is formed on the intermediate film, it is preferable to perform the formation continuously without exposure to the atmosphere from the start of the formation of the intermediate film to the end of the formation of the protective film. By continuously forming the films without exposing them to the atmosphere, it is possible to suppress the formation of oxides that may cause a decrease in reflectance. Furthermore, it is also preferable to continuously form the multilayer reflective film from the start of the formation to the end of the formation of the protective film without exposing them to the atmosphere.

[0050] <Method for manufacturing a reflective mask and a reflective mask> The reflective mask of the present invention is obtained by patterning the absorber film of the reflective mask blank of the present invention. One example of the method for manufacturing a reflective mask will be described with reference to FIG.

[0051] FIG. 2A shows a state in which a resist pattern 40 is formed on a reflective mask blank having a substrate 12, a multilayer reflective film 14, a protective film 16, an absorber film 18, and a hard mask film 20 in this order. The resist pattern 40 can be formed by a known method, for example, by applying a resist to the hard mask film 20 of the reflective mask blank, followed by exposure and development to form the resist pattern 40. The resist pattern 40 corresponds to a pattern to be formed on a wafer using a reflective mask. The hard mask film 20 is then etched using the resist pattern 40 in FIG. 2A as a mask, and the hard mask film is patterned into a shape corresponding to the resist pattern 40. The resist pattern 40 is then removed to obtain the laminate shown in FIG. 2B. The hard mask film 20 can be etched by a known method, such as dry etching using an oxygen-containing gas. The resist pattern 40 can also be removed by a known method, such as removal with a cleaning solution. Examples of cleaning solutions include sulfuric acid-hydrogen peroxide solution (SPM), sulfuric acid, ammonia water, ammonia-hydrogen peroxide solution (APM), OH radical cleaning water, ozone water, etc. In the present invention, the hard mask film 20 has high resistance to chemical solutions and is less likely to have a reduced thickness due to the cleaning solutions.

[0052] Next, the absorber film 18 is etched and patterned using the patterned hard mask film 20 shown in Fig. 2(b) as a mask to obtain a laminate having an absorber film pattern 18pt shown in Fig. 2(c). In the laminate shown in Fig. 2(c), the protective film 16 is exposed. Examples of dry etching used to form the absorber film pattern 18pt include dry etching using a Cl-based gas and dry etching using an F-based gas.

[0053] Next, the hard mask film 20 is removed from the stacked body shown in Fig. 2(c) to obtain the stacked body shown in Fig. 2(d). The method for removing the hard mask film 20 can be performed by the same method as the above-mentioned etching method for the hard mask film 20. When removing the hard mask film 20, not only the hard mask film 20 but also the protective film 16 is exposed to the removal process of the hard mask film 20. In the present invention, the protective film 16 is less susceptible to etching than the hard mask film 20, so the hard mask film 20 is selectively removed and the multilayer reflective film 14 is less likely to be altered.

[0054] Next, as shown in Fig. 2(e), a resist pattern 41 corresponding to the frame of the exposure region is formed on the laminate of Fig. 2(d), and dry etching is performed using the resist pattern 41 of Fig. 2(e) as a mask. Dry etching is performed until it reaches the substrate 12. After dry etching, the resist pattern 41 is removed to obtain the reflective mask shown in Fig. 2(f).

[0055] A reflective mask obtained by patterning the absorber film of the reflective mask blank of the present invention can be suitably used as a reflective mask for exposure with EUV light.

[0056] The present invention will be described in more detail below based on examples. The materials, amounts used, ratios, treatment details, treatment procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the examples shown below. Examples 1 to 6 described below are examples, and Examples 7 to 9 are comparative examples.

[0057] Example 1 First, the procedure for obtaining the reflective mask blank of Example 1 will be described as a representative example.

[0058] [Substrate] First, as a substrate, SiO 2 -TiO 2 A glass substrate (6-inch (152 mm) square outer diameter, 6.3 mm thick) of this type was prepared. This glass substrate had a thermal expansion coefficient of 0.02×10 at 20° C. -7 / °C, Young's modulus is 67 GPa, Poisson's ratio is 0.17, and specific rigidity is 3.07 × 107 m 2 / s2 The quality assurance area of ​​the first main surface of the substrate was polished to a root mean square (RMS) roughness of 0.15 nm or less and a flatness of 100 nm or less. A 100 nm-thick Cr film was formed on the second main surface of the substrate using magnetron sputtering. The sheet resistance of the Cr film was 100 Ω / sq.

[0059] [Multilayer Reflective Film] Next, a Mo / Si multilayer reflective film was formed on the first main surface of the substrate as a multilayer reflective film. The Mo / Si multilayer reflective film was obtained by repeating the process of forming a Si film (4.5 nm thick) and a Mo film (2.3 nm thick) using an ion beam sputtering method 40 times, and then forming an additional Si film (4.5 nm thick) after the 40th Mo film. The total thickness of the Mo / Si multilayer reflective film was 276.5 nm ((4.5 nm + 2.3 nm) × 40 + 4.5 nm).

[0060] [Protective Film] A Rh film (thickness: 2.5 nm) was formed as a protective film on the multilayer reflective film by ion beam sputtering.

[0061] [Absorber Film and Anti-Reflection Film] An absorber film was formed on the protective film by magnetron sputtering. The absorber film was a TaN film, and Ar, Kr, and N were sputtered using a Ta target. 2 A mixed gas (Ar=67% by volume, Kr=17% by volume, N 2 Magnetron sputtering was performed in an atmosphere of SiO 2 (SiO 2 = 16% by volume). The film formation rate was 7.7 nm / min. The film thickness of the absorber film was 75 nm.

[0062] An anti-reflection film was formed on the absorber film by magnetron sputtering. The low-reflection film was a TaON film, and Ar, O 2 , and N 2 A mixed gas (Ar=60% by volume, O 2 = 30% by volume, N 2 Magnetron sputtering was performed in a SiO 2 (SiO 3 ) atmosphere at a deposition rate of 1.32 nm / min. The thickness of the anti-reflection film was 5 nm.

[0063] [Hard Mask Film] A hard mask film was formed on the anti-reflective film by ion beam sputtering. The hard mask film was a Ru film, and the Ru film deposition conditions were as follows: Target: Ru target, Sputtering gas: Ar gas (Ar: 100% by volume), Voltage: 500 V, Deposition rate: 0.023 nm / sec, Film thickness: 2.5 nm.

[0064] By the above procedure, a reflective mask blank was obtained in Example 1. In Examples 2 to 8, only the differences from the procedure for obtaining the reflective mask blank in Example 1 above will be described.

[0065] Example 2 The reflective mask blank of Example 2 was obtained in the same manner as the reflective mask blank of Example 1, except that the hard mask film was a RuN film and the film formation conditions were changed as follows: Target: Ru target Sputtering gas: Ar and N 2 A mixed gas (Ar: 75% by volume, N 2 : 25% by volume Voltage: 500 V Film formation rate: 0.023 nm / sec Film thickness: 2.5 nm

[0066] Example 3 The reflective mask blank of Example 3 was obtained in the same manner as the reflective mask blank of Example 1, except that the hard mask film was a RuON film and the film formation conditions were changed as follows: Target: Ru target Sputtering gas: Ar, O 2 and N 2 A mixed gas (Ar: 60% by volume, O 2 : 20% by volume, N 2 : 20% by volume) Voltage: 500 V Film formation rate: 0.023 nm / sec Film thickness: 2.5 nm

[0067] Example 4 The reflective mask blank of Example 4 was obtained in the same manner as the reflective mask blank of Example 1, except that an intermediate film was formed on the multilayer reflective film before forming the protective film, and a protective film was formed on the intermediate film. The intermediate film was a Ru film, and the Ru film (film thickness: 0.9 nm) was formed by ion beam sputtering. A Rh film (film thickness: 1.6 nm) was formed on the formed Ru film by ion beam sputtering. Note that the film formation was performed without exposure to the atmosphere from the start of Ru film formation to the end of Rh film formation.

[0068] Example 5 The reflective mask blank of Example 5 was obtained in the same manner as the reflective mask blank of Example 2, except that an intermediate film was formed on the multilayer reflective film before forming the protective film, and a protective film was formed on the intermediate film. The intermediate film was a Ru film, and the Ru film (film thickness: 0.9 nm) was formed by ion beam sputtering. A Rh film (film thickness: 1.6 nm) was formed on the formed Ru film by ion beam sputtering. Note that the film formation was performed without exposure to the atmosphere from the start of Ru film formation to the end of Rh film formation.

[0069] Example 6 The reflective mask blank of Example 5 was obtained in the same manner as the reflective mask blank of Example 3, except that an intermediate film was formed on the multilayer reflective film before forming the protective film, and a protective film was formed on the intermediate film. The intermediate film was a Ru film, and the Ru film (film thickness: 0.9 nm) was formed by ion beam sputtering. A Rh film (film thickness: 1.6 nm) was formed on the formed Ru film by ion beam sputtering. Note that the film formation was performed without exposure to the atmosphere from the start of Ru film formation to the end of Rh film formation.

[0070] Example 7 A reflective mask blank of Example 7 was obtained in the same manner as the reflective mask blank of Example 1, except that the protective film was a Ru film and the hard mask film was a CrO film. Specifically, in the reflective mask blank of Example 7, a Ru film (film thickness 2.5 nm) was formed as a protective film on the multilayer reflective film by ion beam sputtering. The hard mask film was formed under the following conditions: Target: Cr target Sputtering gas: Ar and O 2 Mixed gas (Ar: 35% by volume, O 2 : 65% by volume, gas pressure 1.5 × 10 -1 Pa) Input power density per target area: 4.1 W / cm 2 Film formation rate: 0.250 nm / sec Distance between target and substrate: 300 mm Film thickness: 10 nm

[0071] Example 8 The reflective mask blank of Example 8 was obtained in the same manner as the reflective mask blank of Example 7, except that the hard mask film was a Ru film and the film formation conditions were changed as follows: Target: Ru target Sputtering gas: Ar gas (gas pressure 2.0 × 10 -2 Pa) Voltage: 500 V Film formation rate: 0.023 nm / sec Film thickness: 2.5 nm

[0072] Example 9 The reflective mask blank of Example 9 was obtained in the same manner as the reflective mask blank of Example 7, except that an intermediate film was formed on the multilayer reflective film before forming the protective film, and a protective film was formed on the intermediate film. The intermediate film was a Ru film, and the Ru film (film thickness: 0.9 nm) was formed by ion beam sputtering. A Rh film (film thickness: 1.6 nm) was formed on the formed Ru film by ion beam sputtering. Note that the film formation was performed without exposure to the atmosphere from the start of Ru film formation to the end of Rh film formation.

[0073] <Evaluation Method and Evaluation Criteria> [Chemical Solution Resistance] The chemical solution resistance of the reflective mask blank was evaluated using the following procedure. First, the reflective mask blank was immersed in a chemical solution under the following conditions, and then the change in film thickness of the hard mask film was measured by XRR. The conditions for immersion in the chemical solution were as follows: Chemical solution: sulfuric acid-hydrogen peroxide aqueous solution (75% concentrated sulfuric acid by volume, 25% hydrogen peroxide solution by volume) Concentrated sulfuric acid: 96% sulfuric acid by volume, 4% water by volume Hydrogen peroxide solution: 30-35% hydrogen peroxide by volume, 65-70% water by volume Etching solution temperature: 100°C Immersion time: 20 minutes If the reduction in the film thickness of the hard mask film after immersion in the chemical solution compared to before immersion (film thickness before immersion - film thickness after immersion) was less than 0.1 nm, it was rated as "A," and if it was more than 0.1 nm, it was rated as "B." The film thickness of the hard mask film was measured using a Smart Lab manufactured by RIGAKU Corporation. In the measurement of the dry etching rate below, the film thickness of the hard mask film or the like is measured in the same manner.

[0074] [Dry Etching Rate Ratio (Absorber Film / Hard Mask Film)] The dry etching rate (ER HM1 ) and the dry etching rate (ER ABS) and the ratio of the dry etching rate of the absorber film to the dry etching rate of the hard mask film (ER ABS / ER HM1 Specifically, dry etching was performed on the hard mask film and absorber film formed as model films on the substrate under the following conditions, and the etching rates (dry etching rates) were calculated from the film thickness of the hard mask film and the film thickness change of the absorber film. From the obtained etching rates, the dry etching rate ratio (ER ABS / ER HM1 Dry etching was performed using an inductively coupled plasma (ICP) etching device under the following conditions: ICP antenna bias output: 500 W, substrate bias output: 15 W, etching gas: Cl 2 Gas Cl 2 Gas flow rate: 60 sccm Etching pressure: 6.6×10 -1 Pa Note that "sccm" is an abbreviation for "Standard Cubic Centimeter per Minute" and is the gas flow rate (cm) per minute converted into a volume value at 1 atmosphere (1013.25 hPa) and 0°C. 3 / min). ABS / ER HM1 If the value is 50 or more, it is rated as "A", and if it is less than 50, it is rated as "B".

[0075] [Dry Etching Rate Ratio (Anti-Reflective Film / Hard Mask Film)] The dry etching rate (ER HM2 ) and the dry etching rate (ER ARC ) and the ratio of the dry etching rate of the absorber film to the dry etching rate of the hard mask film (ER ARC / ER HM2Specifically, dry etching was performed on the hard mask film and the anti-reflective film formed as model films on the substrate under the following conditions, and the etching speed (dry etching rate) was calculated from the film thickness of the hard mask film and the film thickness change of the anti-reflective film. From the obtained etching speeds, the dry etching rate ratio (ER ARC / ER HM2 Dry etching was performed using an ICP etching device under the following conditions: ICP antenna bias output: 1200 W, substrate bias output: 50 W, etching gas: CF 4 Gas CF 4 Gas flow rate: 60 sccm Etching pressure: 4.0×10 -1 Pa ER ARC / ER HM2 When the value was 5 or more, it was rated as "A", and when it was less than 5, it was rated as "B".

[0076] [Dry Etching Rate Ratio (Hard Mask Film / Protective Film)] The dry etching rate of the protective film (ER CAP ) and the dry etching rate (ER HM3 ) was calculated, and the ratio of the dry etching rate of the hard mask film to the dry etching rate of the protective film (ER HM3 / ER CAP Specifically, dry etching was performed on the hard mask film and the protective film formed as model films on the substrate under the following conditions, and the etching speed (dry etching rate) was calculated from the film thickness of the hard mask film and the change in film thickness of the protective film. From the obtained etching speeds, the dry etching rate ratio (ER HM3 / ER CAP Dry etching was performed using an ICP etching device under the following conditions: ICP antenna bias output: 700 W, substrate bias output: 10 W, etching gas: Cl 2 Gas and O 2 Gas mixture Cl 2 Gas flow rate: 72 sccm O 2 Gas flow rate: 18 sccm Etching pressure: 1.0×10 0Pa ER HM3 / ER CAP When the value was 10 or more, it was rated as "A", and when it was less than 10, it was rated as "B".

[0077] [Crystallinity of Hard Mask Film] The crystallinity of the hard mask film was evaluated by obtaining a diffraction chart using an X-ray diffraction analyzer (MiniFlex II) manufactured by Rigaku Corporation. The FWHM shown in Table 1 is the full width at half maximum (FWHM) of the peak with the highest intensity in the 2θ range of 35° to 60°. The crystallite size was calculated from the FWHM and other data using Scherrer's equation. In the table below, FWHM (half width) of 3.0 or more is designated "A," FWHM of 0.5 or more but less than 3.0 is designated "B," and FWHM of less than 0.5 is designated "C."

[0078] <Results> The configuration of each reflective mask blank, the measurement results, and the evaluation results are shown in the table.

[0079]

[0080] The results shown in Table 1 indicate that in Examples 7 and 8, where the protective film does not contain more than 50 atomic % of one or more elements selected from the group consisting of Rh, Pd, Ir, and Pt, the hard mask film cannot be selectively removed relative to the protective film, and the reflective properties of the multilayer reflective film in the resulting reflective mask are likely to deteriorate. Furthermore, the results shown in Table 1 indicate that in Examples 7 and 9, where the hard mask film does not contain Ru, the hard mask film has low chemical resistance and cannot be thinned. This necessitates thickening the thickness of the resist film formed on the hard mask film in order to etch the hard mask film. A thick resist film makes it difficult to form a high-resolution pattern, thereby making it difficult to form a fine mask pattern. Furthermore, comparison of Examples 1 and 4 with Examples 2, 3, 5, and 6 confirmed that the crystallinity of the hard mask film is reduced when the hard mask film contains one or more elements selected from the group consisting of B, C, N, and O (preferably, one or more elements selected from the group consisting of N and O). When the crystallinity of the hard mask film is low, the above-mentioned edge roughness tends to be small, and it becomes easier to form a finer mask pattern.

[0081] Furthermore, the minimum film thickness of the resist to be formed on the hard mask film was calculated for the reflective mask blanks of Examples 1 to 7. Specifically, the ratio of the etching rate of the absorber film to the etching rate of the hard mask film was used to calculate the film thickness of the hard mask film at which the absorber film was completely etched away and the hard mask film was simultaneously etched away for each reflective mask blank. That is, the minimum film thickness required for the hard mask film to function as an etching mask for the absorber film was calculated. This is shown in the "Minimum Required Hard Mask Film Thickness" column in the "Considering Only Absorber Film" column of Table 2. As described above, to form a hard mask film, a resist pattern is formed on the hard mask film, and dry etching is performed using this resist pattern as a mask to pattern the hard mask film. Therefore, the time required to remove the hard mask film and the film thickness of the resist pattern required to pattern the hard mask film are proportional to each other. This allows the minimum film thickness of the resist to be calculated for the reflective mask blanks of Examples 1 to 7. The time required to remove the hard mask film was calculated from the results shown in Table 1 and the "minimum required hard mask film thickness" calculated above, and is shown in the "Patterning Time" column. The resist film thickness ratio calculated from the "Patterning Time" is shown in the "Resist Film Thickness Ratio" column as a value for Example 7. Similarly, the "minimum required hard mask film thickness" was calculated so that the absorber film and anti-reflective film could be patterned for the "minimum required hard mask film thickness" described above. The results are shown in the "Minimum Required Hard Mask Film Thickness" column under "Considering Absorber Film and Anti-reflective Film" in Table 2. The "Patterning Time" and "Resist Film Thickness Ratio" calculated in the "Considering Absorber Film and Anti-reflective Film" column are also shown. The smaller the "Resist Film Thickness Ratio" value, the smaller the resist film thickness required for the reflective mask blanks of Examples 1 to 7.

[0082]

[0083] The results shown in Table 2 show that in the reflective mask blanks of Examples 1 to 6, the resist film thickness formed on the hard mask film can be made smaller than that of the reflective mask blank of Example 7, making it easier to form a high-definition resist pattern and a finer mask pattern. The entire contents of the specification, claims, drawings and abstract of Japanese Patent Application No. 2023-057859, filed on March 31, 2023, are hereby incorporated by reference as part of the disclosure of the present invention.

[0084] REFERENCE SIGNS LIST 10 Reflective mask blank 12 Substrate 14 Multilayer reflective film 16 Protective film 18 Absorber film 18pt Absorber film pattern 20 Hard mask film 40, 41 Resist pattern

Claims

1. A reflective mask blank having, in this order, a substrate, a multilayer reflective film that reflects EUV light, a protective film, an absorber film, and a hard mask film, wherein the protective film contains more than 50 atomic % of one or more elements selected from the group consisting of rhodium, palladium, iridium, and platinum, and the hard mask film contains ruthenium.

2. The reflective mask blank according to claim 1, wherein the hard mask film consists solely of ruthenium, or the hard mask film contains ruthenium and one or more elements selected from the group consisting of boron, carbon, nitrogen, oxygen, titanium, chromium, zirconium, niobium, molybdenum, palladium, tantalum and iridium.

3. The reflective mask blank according to claim 1, wherein the hard mask film contains 50 to 100 atomic % of ruthenium.

4. The reflective mask blank according to claim 1 or 2, wherein the hard mask film has a thickness of 0.3 to 30 nm.

5. The reflective mask blank according to claim 1 or 2, wherein the protective film further contains one or more elements selected from the group consisting of boron, carbon, nitrogen, oxygen, titanium, zirconium, niobium, molybdenum and tantalum.

6. The reflective mask blank according to claim 1 or 2, further comprising an intermediate film between the protective film and the multilayer reflective film, the intermediate film consisting of only ruthenium, or the intermediate film containing ruthenium and one or more elements selected from the group consisting of boron, carbon, nitrogen, oxygen, silicon, titanium, chromium, zirconium, niobium, molybdenum, palladium and tantalum.

7. A reflective mask blank according to claim 1 or 2, wherein the absorber film contains one or more metals selected from the group consisting of Ta, Ti, Sn, Ir, Re, Nb, Mo and Cr.

8. Dry etching rate (ER) of the hard mask film HM ) to the dry etching rate (ER ABS ) ratio (ER ABS / ER HM 3. The reflective mask blank according to claim 1 , wherein n is 50 or more and 1,000 or less.

9. Dry etching rate (ER) of the protective film CAP ) to the dry etching rate (ER HM ) ratio (ER HM / ER CAP 3. The reflective mask blank according to claim 1 , wherein the n-th order number is 30 or more and 500 or less.

10. A reflective mask having an absorber film pattern formed by patterning the absorber film of the reflective mask blank according to claim 1 or 2.

11. A method for manufacturing a reflective mask, comprising the step of patterning the absorber film of the reflective mask blank according to claim 1 or 2.

12. A method for manufacturing a reflective mask blank, comprising forming on a substrate in this order: a multilayer reflective film that reflects EUV light; an intermediate film; a protective film; an absorber film; and a hard mask film, wherein the protective film contains more than 50 atomic % of one or more elements selected from the group consisting of rhodium, palladium, platinum and iridium; and the hard mask film contains ruthenium, and the formation is carried out continuously from the start of formation of the multilayer reflective film to the end of formation of the protective film without exposure to the atmosphere.

Citation Information

Patent Citations

  • Reflective photomask

    JP2002122981A

  • Reflective mask blank, method of manufacturing reflective mask blank, and method of manufacturing reflective mask

    JP2015142083A

  • Reflective mask blank, method of manufacturing reflective mask, and method of manufacturing semiconductor device

    JP2018173664A

  • Reflection type mask blank, reflection type mask, and method for producing reflection type mask blank

    JP2019219651A

  • Blankmask for Extreme Ultra-Violet Lithography and Photomask using the same

    KR1020150056435A

Cited By

  • Blankmask and photomask for EUV lithography with hard mask film containing chrome and niobium

    EP4738004A1