Method for manufacturing composite particles and electrode for electrochemical element

The method of forming composite particles using a granulation tank with multiple stirring blades addresses the issues of electrode flexibility and cracking, enhancing the performance of electrochemical devices by uniformly dispersing components and optimizing particle size distribution.

WO2024204433A1PCT designated stage expired Publication Date: 2024-10-03ZEON CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012439
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-27
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional methods for producing composite particles for electrochemical devices fail to adequately improve the flexibility and cycle characteristics of electrodes, leading to cracking and reduced performance in electrochemical devices.

Method used

A method involving a granulation tank with multiple stirring blades, where the electrode active material is stirred before adding a composition containing a binder, conductive aid, and solvent, using a specific order and technique to form composite particles that enhance electrode flexibility and suppress cracking.

Benefits of technology

The method effectively increases electrode flexibility, reduces cracking, and improves the cycle characteristics of electrochemical devices by uniformly dispersing components and optimizing particle size distribution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012439_03102024_PF_FP_ABST
    Figure JP2024012439_03102024_PF_FP_ABST
Patent Text Reader

Abstract

In a granulation tank comprising two or more agitation blades having different agitation axes, the following steps are performed in this order: (i) a powder material containing an electrode active material is agitated and brought into an agitation state; and (ii) a composition containing a binder, an electrically conductive assistant, and a solvent is added to the powder material in the agitation state to form composite particles.
Need to check novelty before this filing date? Find Prior Art

Description

Method for producing composite particles and electrodes for electrochemical devices

[0001] The present invention relates to a method for producing composite particles and an electrode for an electrochemical device.

[0002] Electrochemical devices such as lithium-ion secondary batteries are small, lightweight, have high energy density, and can be repeatedly charged and discharged, and are therefore used in a wide range of applications.

[0003] In order to improve the performance of electrochemical devices, various improvements have been made to the materials that form electrodes for electrochemical devices. Electrodes for electrochemical devices have a structure in which an electrode mixture layer is disposed on an electrode substrate, the electrode mixture layer containing an electrode active material as a main component and, as necessary, other components such as a conductive additive and a binder to impart specific functions such as conductivity, adhesion, and flexibility to the electrode. From the viewpoint of improving the performance of electrochemical devices, it is preferable that the electrode active material and other components are uniformly dispersed in the electrode mixture layer.

[0004] As methods for forming an electrode mixture layer, various methods have been considered in the past, including a method of applying a slurry composition containing an electrode active material, a conductive additive, a binder, and a solvent onto an electrode substrate and drying the slurry composition to form an electrode mixture layer, and a method of spray-drying a slurry composition containing an electrode active material, a conductive additive, a binder, and a solvent to obtain composite particles, and then pressure-molding the obtained composite particles onto an electrode substrate to form an electrode mixture layer.

[0005] As methods for producing composite particles, the following have been considered: a method of spray-drying a slurry composition as described above (see, for example, Patent Document 1); a fluidized bed granulation method in which powder is granulated in a state where it is suspended in a fluid such as an air current blown up from below (see, for example, Patent Document 2); and a granulation method which includes stirring an electrode active material and a binder and then crushing the mixture (see, for example, Patent Document 3).

[0006] International Publication No. 2005 / 124801 Japanese Patent Application Laid-Open No. 2006-060193 International Publication No. 2015 / 029829

[0007] However, conventional methods for producing granulated particles leave room for further improvement in the properties of electrodes formed using the resulting granulated particles and electrochemical devices equipped with such electrodes.

[0008] Therefore, an object of the present invention is to provide a method for producing composite particles that can increase the flexibility of an electrode, suppress cracking of the electrode active material in the electrode, and further improve the cycle characteristics of an electrochemical device equipped with such an electrode. Another object of the present invention is to provide a method for producing an electrode for an electrochemical device using the composite particles obtained according to the production method of the present invention.

[0009] The present inventors have conducted extensive research to solve the above problems, and have newly discovered that by forming composite particles by adding a composition containing a binder, a conductive additive, and a solvent under stirring conditions, it is possible to produce composite particles that can improve the properties of the resulting electrodes and electrochemical devices, as described above, and have completed the present invention.

[0010] That is, the present invention aims to advantageously solve the above-mentioned problems. [1] A method for producing composite particles, characterized by carrying out the following steps in this order in a granulation tank equipped with two or more agitation blades having different agitation shafts: (i) agitating a powder material containing an electrode active material to create an agitated state; and (ii) adding a composition containing a binder, a conductive additive, and a solvent to the powder material in the agitated state to form composite particles. By carrying out the above steps (i) to (ii) in this order in a granulation tank equipped with two or more agitation blades having different agitation shafts, it is possible to provide composite particles that increase the flexibility of an electrode, suppress cracking of the electrode active material in the electrode, and further improve the cycle characteristics of an electrochemical device equipped with such an electrode.

[0011] [2] Here, in the method for producing composite particles described in the above [1], it is preferable that the means for adding the composition in the step (ii) is a spray nozzle. By spraying and supplying the composition using a spray nozzle when adding the composition in the step (ii), the properties of the obtained composite particles can be further improved.

[0012] [3] In addition, in the method for producing composite particles described in [1] or [2] above, after the step (ii), a step (iii) of sizing the composite particles by stirring them after the addition of the composition is completed can be carried out.

[0013] [4] In the method for producing composite particles according to the above [3], it is preferable to add a conductive additive in the step (iii). By adding a conductive additive in the step (iii), the properties of the obtained composite particles can be further improved.

[0014] [5] In the method for producing composite particles according to any one of the above [1] to [4], the powder material in step (i) preferably contains a conductive additive. By carrying out step (ii) after stirring the conductive additive together with the electrode active material in step (i), the properties of the resulting composite particles can be further improved.

[0015] [6] In the method for producing composite particles of the present invention described in any one of [1] to [5] above, the solvent contained in the composition is preferably a non-aqueous solvent having a boiling point of 95° C. or less at 1 atm. If a composition containing a solvent that satisfies such conditions is used in the above operation (ii), composite particles can be produced efficiently.

[0016] [7] The present invention also aims to advantageously solve the above-mentioned problems, and provides a method for producing an electrode for an electrochemical device, comprising: producing composite particles according to the method for producing composite particles described in any one of [1] to [6] above; and press-molding the produced composite particles on an electrode substrate to form an electrode mixture layer. An electrode comprising an electrode mixture layer formed using composite particles obtained according to any one of the above-mentioned methods for producing composite particles has excellent flexibility and is less susceptible to cracking of the electrode active material contained therein. Furthermore, the cycle characteristics of an electrochemical device comprising such an electrode can be improved.

[0017] According to the present invention, it is possible to provide a method for producing composite particles that can increase the flexibility of an electrode, suppress cracking of the electrode active material in the electrode, and further improve the cycle characteristics of an electrochemical device equipped with such an electrode. Furthermore, according to the present invention, it is possible to provide a method for producing an electrode for an electrochemical device using the composite particles obtained according to the production method of the present invention.

[0018] 1 is a top view of an example of a granulation tank;

[0019] Hereinafter, embodiments of the present invention will be described in detail. Here, according to the method for producing composite particles of the present invention, it is possible to efficiently provide composite particles that can be advantageously used as a compounding component of an electrode mixture layer provided in an electrode of an electrochemical device such as a secondary battery. Furthermore, the method for producing an electrode for an electrochemical device of the present invention includes pressure-molding the composite particles obtained according to the production method of the present invention.

[0020] (Method for Producing Composite Particles) The method for producing composite particles of the present invention is characterized by carrying out the following steps in this order in a granulation tank equipped with two or more agitation blades having different agitation shafts: (i) a step of agitating a powder material containing an electrode active material to produce an agitated state; and (ii) a step of adding a composition containing a binder, a conductive additive, and a solvent to the agitated powder material to produce composite particles. By carrying out the above steps (i) to (ii) in this order in a granulation tank equipped with two or more agitation blades having different agitation shafts, it is possible to provide composite particles that can increase the flexibility of an electrode, suppress cracking of the electrode active material in the electrode, and further improve the cycle characteristics of an electrochemical device equipped with such an electrode. Furthermore, optionally, following the above step (ii), a step (iii) of sizing the composite particles by stirring them after the addition of the composition is complete may be carried out.

[0021] <Granulation Tank> The granulation tank needs to be equipped with two or more stirring blades with different stirring shafts. Providing two or more stirring blades with different stirring shafts increases the uniformity of the composition of the obtained composite particles, and as a result, the cycle characteristics of an electrochemical device equipped with an electrode formed using such composite particles can be improved. An example of a granulation tank will be described with reference to FIGS. 1 and 2. FIG. 1 is a top view of the granulation tank 1, and FIG. 2 is a cross-sectional view taken along the line A-A in FIG. 1. The granulation tank 1 includes a main stirring blade 2 and a sub-stirring blade 3 with a stirring shaft different from that of the main stirring blade 2. The number of stirring blades is not particularly limited as long as there are two or more. Providing two or more stirring blades increases the uniformity of the composition of the composite particles, thereby improving the cycle characteristics of an electrochemical device equipped with an electrode formed using such composite particles.

[0022] Furthermore, although not shown, the granulation tank 1 is equipped with at least one supply means capable of supplying a liquid composition. Examples of such supply means include a spray nozzle configured to supply a mist of liquid and a dropping funnel. The number of supply means is not particularly limited, but multiple supply means may be arranged discretely depending on the size of the granulation tank. Furthermore, although not shown, the granulation tank 1 may be equipped with a supply port for the powder material and a discharge port configured to discharge the formed composite particles.

[0023] In Figure 2, the agitation shaft of the main agitator blade 2 is shown by a dashed line as a first agitation shaft RA1, and the agitation shaft of the sub-agitator blade is shown by a dashed line as a second agitation shaft RA2. In Figure 2, the angle θ formed by the first agitation shaft RA1 and the second agitation shaft RA2 is approximately 90 degrees. The angle formed by the first agitation shaft RA1 and the second agitation shaft RA2 refers to the acute angle of the angles formed by these two axes. Here, in this specification, "different agitation shafts" means that the angle θ formed by the agitation shafts is 20° or more and 90° or less. The angle θ formed by the agitation shafts is preferably 30° or more, more preferably 45° or more, and even more preferably 85° or more. When the angle θ between the stirring shafts is within the above range, the powder material can be effectively stirred, and the particle size and coefficient of variation of the resulting composite particles can be well controlled. As a result, the flexibility of the electrode formed using such composite particles and cracking of the electrode active material in the electrode can be suppressed, and the cycle characteristics of the resulting electrochemical device can be improved. The "coefficient of variation" refers to the coefficient of variation of the area-equivalent diameter of the composite particles and is an index representing the breadth of the particle size distribution. The coefficient of variation of the area-equivalent diameter can be calculated as a percentage by dividing the standard deviation of the area-equivalent diameter of the composite particles by the average area-equivalent diameter, according to the method described in the Examples of this specification.

[0024] The shape of the granulation vessel is not particularly limited as long as it can accommodate the powder material containing the electrode active material therein for a predetermined period of time and can be stirred by at least two stirring blades. For example, the shape of the granulation vessel may be cylindrical, with circular bottom and top surfaces and a tapered upper portion in the height direction, as shown in granulation vessel 1 in FIGS. 1 and 2. When the granulation vessel has a predetermined cylindrical shape as shown in FIGS. 1 and 2, one of the at least two stirring shafts may coincide with the central axis of the cylinder, and the other stirring shaft may coincide with a direction perpendicular to the central axis. Furthermore, when the granulation vessel has a predetermined cylindrical shape as shown in FIGS. 1 and 2, the value obtained by dividing the diameter of the bottom by the height (diameter / height) is preferably 0.1 or more, more preferably 0.3 or more, even more preferably 0.5 or more, preferably 2.5 or less, more preferably 2.0 or less, and even more preferably 1.5 or less. This is because the powder material can be effectively stirred.

[0025] The main agitating blade 2 has three main blades 21. The shape and number of the main blades 21 are not particularly limited. The auxiliary agitating blade 3 has two auxiliary blades 31. The auxiliary blades 31 are illustrated as anchor blades in FIGS. 1 and 2, but are not limited to this. The number of auxiliary blades 31 is also not limited to the illustrated form and may be one, or three or more. Furthermore, the granulation tank 1 may be equipped with a ventilation mechanism (not shown) configured to ventilate air and thereby prevent powder material from being mixed into the drive parts of the main agitating blade 2 and the auxiliary agitating blade 3.

[0026] Examples of granulation vessels that satisfy the above conditions include a high-speed mixer manufactured by EarthTechnica Co., Ltd., a Henschel mixer manufactured by Mitsui Mining Co., Ltd. (now an FM mixer manufactured by Nippon Coke Company), a vertical granulator manufactured by Powrex Corporation, a CF granulator manufactured by Freund Corporation, a high-speed stirring and mixing granulator manufactured by Nara Machinery Works, Ltd., an SP granulator manufactured by Dalton Corporation, and a balance granulator manufactured by Freund Corporation.

[0027] Various operations carried out in the granulation tank will be described below.

[0028] <(i) Pre-stirring operation> In the pre-stirring operation, the powder material is stirred to bring it into a stirred state. Here, the powder material needs to contain an electrode active material, and may optionally contain a conductive additive. By performing the pre-stirring operation, it is possible to improve the cycle characteristics of an electrochemical device equipped with an electrode formed using the obtained composite particles.

[0029] The positive electrode active material is not particularly limited, and examples thereof include lithium-containing cobalt oxide (lithium cobalt oxide, LiCoO 2 ), lithium manganese oxide (LiMn 2 O 4 ), lithium-containing nickel oxide (LiNiO 2 ), Co—Ni—Mn lithium-containing composite oxide (Li(Co Mn Ni)O 2 ), lithium-containing composite oxide of Ni-Mn-Al, lithium-containing composite oxide of Ni-Co-Al, olivine-type lithium iron phosphate (LiFePO 4 ), olivine-type lithium manganese phosphate (LiMnPO 4 ), Li 2 MnO 3 -LiNiO 2 system solid solution, Li 1+x Mn 2-x O 4 (0<X<2) Lithium-excess spinel compound represented by Li[Ni 0.17 Li 0.2 Co 0.07 Mn 0.56 ]O 2 , LiNi 0.5 Mn 1.5 O 4 Examples of known positive electrode active materials include: carbon-based negative electrode active materials, metal-based negative electrode active materials, and negative electrode active materials that are combinations of these.

[0030] The particle diameter of the electrode active material is preferably 0.03 μm or more, more preferably 0.1 μm or more, even more preferably 0.5 μm or more, and preferably 500 μm or less, more preferably 200 μm or less, and even more preferably 30 μm or less. The particle diameter of the electrode active material can be measured by laser diffraction. More specifically, in the particle size distribution (volume basis) measured using a laser diffraction particle size distribution measurement device, the particle diameter D50 at which the cumulative volume calculated from the smallest diameter side is 50% is defined as the volume average particle diameter, and this value preferably falls within the above particle diameter range. If the particle diameter of the electrode active material is not more than the above upper limit, the composition within the composite particle can be made more homogeneous. Furthermore, if the particle diameter of the electrode active material is not more than the above upper limit, the electrode density of the obtained electrode can be increased, and the specific surface area of ​​the electrode active material is sufficiently large, thereby optimizing the electrochemical reaction when forming an electrochemical element. When the particle size of the electrode active material is equal to or greater than the above-mentioned lower limit, the handling of the powder material as a material for producing the composite particles is improved, and the productivity of the composite particles is improved. Furthermore, when the particle size of the electrode active material is equal to or greater than the above-mentioned lower limit, deterioration of the electrode active material during repeated charging and discharging of the electrochemical device can be effectively suppressed.

[0031] The conductive additive is not particularly limited, and examples thereof include carbon black (e.g., acetylene black, Ketjen Black (registered trademark), furnace black, etc.), single-walled or multi-walled carbon nanotubes (multi-walled carbon nanotubes include cup-stacked types), carbon nanohorns, vapor-grown carbon fibers, milled carbon fibers obtained by calcining and then crushing polymer fibers, single-walled or multi-walled graphene, etc. These may be used alone or in combination.

[0032] When the electrode active material and the conductive additive are used in combination, the blending ratio of these is not particularly limited, and may be a general blending ratio of these contained in an electrode for an electrochemical element.

[0033] It is preferable not to add any liquid components during the preliminary mixing operation. A small amount of liquid components may inevitably be contained in the powder material due to the influence of moisture that may adhere during production and storage. In other words, the solid content of the powder material at the start of the preliminary mixing operation is likely to be less than 100% by mass. From the viewpoint of improving the properties of the resulting composite particles and the production efficiency of composite particles, it is preferable to increase the solid content of the powder material by performing the preliminary mixing operation. Specifically, the solid content of the powder material at the end of the preliminary mixing operation is preferably 95% by mass or more, more preferably 97% by mass or more, and even more preferably 98% by mass or more. The solid content of the powder material can be measured by the method described in the Examples.

[0034] The peripheral speed of the main stirring blade and the auxiliary stirring blade during the preliminary stirring operation is preferably 1 m / s or more and 20 m / s or less. If the peripheral speed is within this range, the homogeneity of the composition of the obtained composite particles can be improved, thereby suppressing cracking of the electrode active material in the obtained electrode and ultimately improving the cycle characteristics of an electrochemical device equipped with such an electrode. Here, the peripheral speeds of the main stirring blade and the auxiliary stirring blade during the preliminary stirring operation may be the same or different, and may be different, but if they are different, it is preferable that the peripheral speed of the auxiliary stirring blade be faster than the peripheral speed of the main stirring blade.

[0035] The aeration rate during the preliminary mixing operation is preferably 0.1 / min to 100 / min, calculated by dividing the flow rate of air flowing into the granulation tank by the volume of the granulation tank (flow rate / volume). If the aeration rate is within this range, the solids concentration of the powder material can be effectively increased during the preliminary mixing operation. The aeration rate may be the aeration rate provided by the ventilation mechanism for preventing the powder material from entering the drive parts of the main and sub-stirring blades. Furthermore, the temperature of the aerated air is preferably less than 50°C, more preferably 45°C or less, even more preferably 40°C or less, and particularly preferably 30°C or less.

[0036] The time for which the pre-stirring operation is performed (pre-stirring time) is not particularly limited. For example, the pre-stirring time is preferably a time that allows the solids concentration to be equal to or higher than the above-mentioned preferred threshold. For example, the pre-stirring time may be 5 minutes or more and 60 minutes or less.

[0037] The preliminary stirring operation may be performed in multiple stages. In this case, it is preferable to perform a preliminary stirring operation using a stirring device (hereinafter also referred to as "stirring device A") different from the granulation tank equipped with the stirring blades described above prior to the preliminary stirring operation in the granulation tank equipped with the stirring blades described above. The stirring device A is not particularly limited as long as it is a stirring device different from the granulation tank equipped with the stirring blades described above, and examples thereof include dry mixing devices and wet mixing devices. Examples of dry mixing devices that can be used include the Miracle KCK manufactured by Asada Iron Works Co., Ltd. and the Hybridization System manufactured by Nara Machinery Co., Ltd. Examples of wet mixing devices that can be used include the Planetary Despa manufactured by Asada Iron Works Co., Ltd. Performing such a preliminary stirring operation using the stirring device A before the preliminary stirring operation using the granulation tank equipped with the stirring blades described above can improve the rate characteristics of the resulting electrochemical device. This is thought to be because the volume resistivity of the resulting composite particles can be reduced by performing the preliminary stirring operation using the stirring device A.

[0038] <(ii) Composite Particle Formation Operation> In the composite particle formation operation, a composition containing a binder, a conductive additive, and a solvent is added to a powder material in a stirred state to form composite particles. The binder is not particularly limited, and binders known to be formulated for electrodes for electrochemical devices can be used. Furthermore, the manner of addition of the composition containing the binder, the conductive additive, and the solvent to the powder material in the composite particle formation operation is not particularly limited as long as it is added in a manner other than all at once. Examples include continuous addition throughout the composite particle formation operation and intermittent addition with one or more addition pauses during the composite particle formation operation. Of these, continuous addition is preferred. During the composite particle formation operation, i.e., in an atmosphere in which the powder material, the solvent, the conductive additive, and the binder are all stirred together, composite particles of the powder material and the binder are gradually formed, and particle size adjustment can occur due to collisions between the particles and between the particles and the solvent. In other words, the composite particle formation and size regulation can proceed simultaneously in the presence of a solvent during the composite particle formation operation. In this way, composite particles can be formed while their size is being regulated during the composite particle formation operation.

[0039] As described above, examples of means for adding a composition containing a binder, a conductive additive, and a solvent to a powder material include a spray nozzle and a dropping funnel. Among these, from the viewpoint of efficiency, it is preferable to use a spray nozzle. When using a two-fluid spray nozzle having a mechanism for pulverizing and atomizing a liquid by a gas flow and spraying it, the gas-liquid ratio (gas volume / liquid volume) is preferably 1.30 or more, more preferably 1.40 or more, even more preferably 1.45 or more, preferably 1.80 or less, more preferably 1.70 or less, and even more preferably 1.60 or less. If the gas-liquid ratio is equal to or greater than the lower limit, it is possible to prevent the particle size of the composite particles from becoming too large. Furthermore, if the gas-liquid ratio is equal to or less than the upper limit, it is possible to prevent the particle size of the composite particles from becoming too small. Furthermore, the spray surface density (g / mm ), which is a value corresponding to the amount of composition sprayed per unit area on a stationary surface, is preferably 1.30 or more, more preferably 1.40 or more, even more preferably 1.45 or more, and even more preferably 1.80 or less, more preferably 1.70 or less, and even more preferably 1.60 or less.2 / min) is 0.20 (g / mm 2 / min) or more, and 0.25 (g / mm 2 / min) or more, and 0.38 (g / mm 2 / min) or more, and 0.60 (g / mm 2 / min) or less, and 0.50 (g / mm 2 / min) or less, and more preferably 0.41 (g / mm 2 / min) or less. 2 When the value of the spray rate (g / min) is equal to or greater than the lower limit, the particle size of the composite particles can be prevented from becoming excessively small. That is, by controlling the gas-liquid ratio and / or the spray surface density within an appropriate range, the particle size of the obtained composite particles can be well controlled.

[0040] [Binder] Examples of binders that can be used include conjugated diene polymers, acrylic polymers, aromatic vinyl block polymers, fluorine-containing polymers, cellulose polymers, cyclic olefin polymers, etc. One type of binder may be used alone, or two or more types may be used in combination.

[0041] The conjugated diene polymer refers to a polymer containing a conjugated diene monomer unit. Specific examples of the conjugated diene polymer include, but are not limited to, a copolymer containing an aromatic vinyl monomer unit and an aliphatic conjugated diene monomer unit, such as styrene-butadiene copolymer (SBR), butadiene rubber (BR), acrylic rubber (NBR) (a copolymer containing an acrylonitrile unit and a butadiene unit), and hydrogenated products thereof.

[0042] The acrylic polymer is not particularly limited, and examples thereof include a polymer containing a crosslinkable monomer unit, a (meth)acrylic acid ester monomer unit, and an acidic group-containing monomer unit. The proportion of the (meth)acrylic acid ester monomer unit in the acrylic polymer is preferably 50% by mass or more, more preferably 55% by mass or more, and even more preferably 58% by mass or more, and is preferably 98% by mass or less, more preferably 97% by mass or less, and even more preferably 96% by mass or less.

[0043] Examples of aromatic vinyl block polymers include block polymers containing block regions composed of aromatic vinyl monomer units. Examples of aromatic vinyl monomers include styrene, styrene sulfonic acid and its salts, α-methylstyrene, p-t-butylstyrene, butoxystyrene, vinyltoluene, chlorostyrene, and vinylnaphthalene, with styrene being preferred. Examples of aromatic vinyl block polymers include styrene-isoprene-styrene block copolymers, styrene-butadiene-styrene copolymers, and hydrogenated versions of these.

[0044] The term "fluorine-containing polymer" refers to a polymer that contains fluorine-containing monomer units and may further contain fluorine-free monomer units (fluorine-free monomers). Examples of fluorine-containing monomers include, but are not limited to, vinylidene fluoride, tetrafluoroethylene, hexafluoropropylene, vinyl trifluoride, vinyl fluoride, trifluoroethylene, trifluorochloroethylene, 2,3,3,3-tetrafluoropropene, and perfluoroalkyl vinyl ether. Examples of fluorine-containing polymers include, but are not limited to, polytetrafluoroethylene, polychlorotrifluoroethylene, polyvinylidene fluoride, polyvinyl fluoride, perfluoroalkoxy fluororesin, tetrafluoroethylene-hexafluoropropylene copolymer, ethylene-tetrafluoroethylene copolymer, ethylene-chlorotrifluoroethylene copolymer, and vinylidene fluoride-hexafluoropropylene copolymer (vinylidene fluoride-hexafluoropropylene copolymer).

[0045] The cellulose-based polymer is not particularly limited, and examples thereof include cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan, and carboxymethyl cellulose.

[0046] The cyclic olefin polymer is not particularly limited, and examples thereof include a polymer (addition polymer or ring-opening polymer) synthesized using a cyclic olefin compound as a monomer and its hydrogenated product, and a hydrogenated polymer using an aromatic vinyl compound as a monomer. Among them, a hydrogenated ring-opening polymer using a cyclic olefin compound as a monomer and a hydrogenated polymer using an aromatic vinyl compound as a monomer are preferred because the electrolyte swelling degree and glass transition temperature can be easily adjusted to appropriate levels.

[0047] The cyclic olefin compound is not particularly limited, and examples thereof include: norbornene, 5-methylnorbornene, 5-ethylnorbornene, 5-butylnorbornene, 5-hexylnorbornene, 5-decylnorbornene, 5-cyclohexylnorbornene, 5-cyclopentylnorbornene, and other unsubstituted or alkyl group-containing norbornenes; norbornenes having an alkenyl group, such as 5-ethylidenenorbornene, 5-vinylnorbornene, 5-propenylnorbornene, 5-cyclohexenylnorbornene, and 5-cyclopentenylnorbornene; norbornenes having an aromatic ring, such as 5-phenylnorbornene; Norbornenes having a polar group containing an oxygen atom, such as 5-methoxycarbonylnorbornene, 5-ethoxycarbonylnorbornene, 5-methyl-5-methoxycarbonylnorbornene, 5-methyl-5-ethoxycarbonylnorbornene, norbornenyl-2-methylpropionate, norbornenyl-2-methyloctanonate, 5-hydroxymethylnorbornene, 5,6-di(hydroxymethyl)norbornene, 5,5-di(hydroxymethyl)norbornene, 5-hydroxy-i-propylnorbornene, 5,6-dicarboxynorbornene, and 5-methoxycarbonyl-6-carboxynorbornene; norbornenes having a polar group containing a nitrogen atom, such as 5-cyanonorbornene; Polycyclic norbornenes having three or more rings that do not contain an aromatic ring structure, such as dicyclopentadiene, methyldicyclopentadiene, and tricyclo[5.2.1.02,6]dec-8-ene; Polycyclic norbornenes having three or more rings that have an aromatic ring, such as tetracyclo[9.2.1.02,10.03,8]tetradeca-3,5,7,12-tetraene (also known as 1,4-methano-1,4,4a,9a-tetrahydro-9H-fluorene) and tetracyclo[10.2.1.02,11.04,9]pentadeca-4,6,8,13-tetraene (also known as 1,4-methano-1,4,4a,9,9a,10-hexahydroanthracene);unsubstituted or alkyl group-containing tetracyclododecenes such as tetracyclododecene, 8-methyltetracyclododecene, 8-ethyltetracyclododecene, 8-cyclohexyltetracyclododecene, 8-cyclopentyltetracyclododecene, 8-methoxycarbonyl-8-methyltetracyclo[4.4.0.12,5.17,10]-3-dodecene; tetracyclododecenes having an exocyclic double bond such as 8-methylidenetetracyclododecene, 8-ethylidenetetracyclododecene, 8-vinyltetracyclododecene, 8-propenyltetracyclododecene, 8-cyclohexenyltetracyclododecene, 8-cyclopentenyltetracyclododecene; tetracyclododecenes having an aromatic ring such as 8-phenyltetracyclododecene; Tetracyclododecenes having a substituent containing an oxygen atom, such as 8-methoxycarbonyltetracyclododecene, 8-methyl-8-methoxycarbonyltetracyclododecene, 8-hydroxymethyltetracyclododecene, 8-carboxytetracyclododecene, tetracyclododecene-8,9-dicarboxylic acid, and tetracyclododecene-8,9-dicarboxylic anhydride; tetracyclododecenes having a substituent containing a nitrogen atom, such as 8-cyanotetracyclododecene and tetracyclododecene-8,9-dicarboxylic imide; tetracyclododecenes having a substituent containing a halogen atom, such as 8-chlorotetracyclododecene; tetracyclododecenes having a substituent containing a silicon atom, such as 8-trimethoxysilyltetracyclododecene; hexacycloheptadecenes such as Diels-Alder adducts of the above-mentioned tetracyclododecenes and cyclopentadiene; and the like.

[0048] Among these, non-polar norbornene-based monomers are preferred as the cyclic olefin compound, and more preferred are unsubstituted or alkyl group-containing norbornenes (e.g., norbornene, 8-ethyltetracyclododecene), alkenyl group-containing norbornenes (e.g., ethylidenetetracyclododecene (8-ethylidenetetracyclododecene)), dicyclopentadiene, aromatic ring-containing norbornene derivatives (e.g., tetracyclo[9.2.1.02,10.03,8]tetradeca-3,5,7,12-tetraene (also referred to as 1,4-methano-1,4,4a,9a-tetrahydro-9H-fluorene)), and unsubstituted or alkyl group-containing tetracyclododecenes (e.g., tetracyclododecene, 8-methoxycarbonyl-8-methyltetracyclo[4.4.0.12,5.17,10]-3-dodecene).

[0049] The polymer using a cyclic olefin compound as a monomer, which can be optionally hydrogenated, may be a polymer using only a cyclic olefin compound as a monomer, or may be a polymer using a cyclic olefin compound and a copolymerizable compound other than a cyclic olefin compound as monomers, but is preferably a polymer using only a cyclic olefin compound as a monomer.

[0050] The polymer using a cyclic olefin compound as a monomer, which can be optionally hydrogenated, is preferably a polymer using tetracyclododecene, dicyclopentadiene, and norbornene as monomers, and more preferably a ring-opening polymer using tetracyclododecene, dicyclopentadiene, and norbornene as monomers.

[0051] [Solvent] The solvent is not particularly limited, and any solvent can be used as long as it can dissolve or disperse the binder described above. For example, organic solvents such as N-methyl-2-pyrrolidone, cyclohexane, n-hexane, acetone, methyl ethyl ketone, ethyl acetate, tetrahydrofuran, methylene chloride, and chloroform, as well as water, can be used as the solvent. Among these, from the viewpoint of efficiently removing the solvent in the granulation tank and reducing the drying energy required to form the composite particles, it is preferable to use a non-aqueous solvent having a boiling point of 95°C or less at 1 atm. Furthermore, from the viewpoint of more effectively achieving the above-mentioned effects, the boiling point of the non-aqueous solvent at 1 atm is more preferably 90°C or less, and even more preferably 85°C or less. The lower limit of the boiling point of the non-aqueous solvent at 1 atm is not particularly limited, but from the viewpoint of improving stability during the formation of the composite particles, it is preferably 50°C or higher. Examples of solvents that satisfy these conditions include cyclohexane, n-hexane, acetone, methyl ethyl ketone, ethyl acetate, tetrahydrofuran, methylene chloride, and chloroform. These may be used alone or in combination of two or more in any ratio.

[0052] [Viscosity index of composition] The viscosity index of the composition containing the binder, conductive aid, and solvent that is continuously added to the granulation tank during the composite particle formation operation is preferably 100 mPa·s or more and 1000 mPa·s or less. By setting the viscosity index of the composition containing the binder, conductive aid, and solvent within the above range, the particle size and coefficient of variation of the obtained composite particles can be well controlled. The viscosity index of the composition is the value obtained by dividing the viscosity of the composition by the solids concentration and multiplying the result by 100, and can be measured and calculated by the method described in the examples.

[0053] [Agitator blade peripheral speed] The peripheral speeds of the main agitator blade and the auxiliary agitator blade in the composite particle formation operation are preferably 1 m / s or more and 20 m / s or less. If the peripheral speed of the main agitator blade is within the above range, the particle size of the obtained composite particles can be well controlled. Furthermore, if the peripheral speed of the auxiliary agitator blade is within the above range, the coefficient of variation of the obtained composite particles can be well controlled. Furthermore, from the viewpoint of enhancing the particle size regulation that occurs during the composite particle formation operation and suppressing gas generation during high-temperature storage of electrodes formed using the composite particles, the lower limit of the peripheral speed of the main agitator blade is preferably 6 m / s or more, and the upper limit is preferably 12 m / s or less.

[0054] [Aeration rate] The aeration rate in the composite particle formation operation, calculated by dividing the flow rate of air flowing into the granulation tank by the volume of the granulation tank (flow rate / volume), is preferably 0.1 / min to 100 / min. If the aeration rate is within this range, the amount of solvent vapor in the granulation tank can be well controlled during the composite particle formation operation, and composite particles can be efficiently formed.

[0055] [Time] The duration of the composite particle formation operation (composite particle formation time) is not particularly limited. For example, the composite particle formation time may be 5 minutes or more and 60 minutes or less.

[0056] <(iii) Sizing Operation> In the sizing operation, the composite particles are sized by stirring after the addition of the composition is completed (i.e., after the composite particle formation operation (ii) is completed). In the sizing operation, a conductive additive may be further added in order to further improve the properties of the composite particles.

[0057] The peripheral speed of the main stirring blade and the auxiliary stirring blade in the sizing operation is preferably 0.1 m / s or more and 10 m / s or less. If the peripheral speed of the main stirring blade is within the above range, the density coefficient and areal circularity of the obtained composite particles can be well controlled. Furthermore, if the peripheral speed of the auxiliary stirring blade is within the above range, the coefficient of variation and circumferential length envelopment of the obtained composite particles can be well controlled. The "circumferential length envelopment" of the composite particles is a value that serves as an index of the roughness of the outer periphery of the particle, and can be measured according to the method described in the examples of this specification.

[0058] The aeration rate in the sizing operation, calculated by dividing the flow rate of air introduced into the granulation tank by the volume of the granulation tank (flow rate / volume), is preferably 0.1 / min to 100 / min. If the aeration rate is within this range, the moist state of the composite particles can be well controlled in the sizing operation, and the composite particles can be efficiently formed.

[0059] When performing a sizing operation, the duration of the sizing operation (sizing time) is not particularly limited. The sizing time may be, for example, 10 seconds or more or 60 minutes or less, preferably 20 minutes or less, preferably 10 minutes or less, and more preferably 3 minutes or less. By setting the sizing operation time to the above upper limit or less, it is possible to reduce the amount of gas generated when an electrode formed using the composite particles is stored under high-temperature conditions.

[0060] <Temperature in Granulation Tank> Throughout the above operations (i) to (iii), the temperature in the granulation tank is preferably less than 50° C., more preferably not more than 45° C., and even more preferably not more than 40° C. By satisfying these temperature conditions, deterioration of the electrode active material contained in the obtained composite particles can be effectively suppressed, and cracking of the electrode active material in an electrode formed using the composite particles can be effectively suppressed.

[0061] (Composite Particles) The composite particles obtained through the above steps (i) to (iii) preferably satisfy the following properties.

[0062] <Particle diameter of composite particles> The particle diameter of the composite particles is preferably 20 μm or more, more preferably 30 μm or more, and even more preferably 40 μm or more, and is preferably 250 μm or less, more preferably 200 μm or less, and even more preferably 150 μm or less. The particle diameter of the composite particles refers to the average particle diameter of the area-equivalent diameter, and can be measured according to the method described in the Examples of this specification. If the particle diameter of the composite particles is equal to or greater than the above-mentioned lower limit, the flexibility of the electrode formed using the composite particles can be increased, and the rate characteristics of the electrochemical device equipped with such an electrode can be improved. Furthermore, if the particle diameter of the composite particles is equal to or less than the above-mentioned upper limit, the cycle characteristics of the resulting electrochemical device can be improved.

[0063] <Coefficient of variation of composite particles> The coefficient of variation of the composite particles is preferably 5% or more, more preferably 7% or more, even more preferably 10% or more, and preferably 50% or less, more preferably 45% or less, and even more preferably 40% or less. If the coefficient of variation is equal to or greater than the lower limit, cracking of the electrode active material in an electrode formed using the composite particles can be effectively suppressed. Furthermore, if the coefficient of variation is equal to or less than the upper limit, the flexibility of the resulting electrode can be improved. In the present application, the coefficient of variation of the composite particles refers to the particle size distribution of the composite particles, and can be calculated as a percentage by dividing the standard deviation of the area-equivalent diameters of the composite particles by the average area-equivalent diameters, according to the method described in the examples of this specification.

[0064] <Bulk Density> The bulk density of the composite particles is preferably 1.0 or more and 4.0 or less. If the bulk density is equal to or more than the lower limit, cracking of the electrode active material in an electrode formed using the composite particles can be suppressed. Furthermore, if the bulk density is equal to or less than the upper limit, the flexibility of the resulting electrode can be increased.

[0065] <Area circularity> The area circularity of the composite particles is preferably 0.50 or more, more preferably 0.60 or more, even more preferably 0.70 or more, and preferably 0.93 or less, more preferably 0.92 or less, and even more preferably 0.91 or less. If the area circularity of the composite particles is equal to or greater than the lower limit, cracking of the electrode active material in an electrode formed using the composite particles can be suppressed. Furthermore, if the area circularity of the composite particles is equal to or less than the upper limit, the rate characteristics of the resulting electrochemical device can be improved.

[0066] <Perimeter Envelope Ratio> The perimeter envelopment ratio of the composite particles is preferably 0.70 or more, more preferably 0.72 or more, even more preferably 0.75 or more, and is preferably 0.97 or less, more preferably 0.94 or less, and even more preferably 0.92 or less. If the perimeter envelopment ratio of the composite particles is equal to or greater than the lower limit, the flexibility of the electrode formed using the composite particles can be improved. If the perimeter envelopment ratio of the composite particles is equal to or less than the upper limit, the cycle characteristics of the resulting electrochemical device can be improved.

[0067] <Fluidity> The fluidity of the composite particles can be evaluated based on the angle of repose and the angle of collapse measured using a powder tester, or based on the roughness of the surface smoothed with a doctor blade, as described in the examples of the present application. 2 The space volume per 3 Preferably, it is 0.50 μm or less. 3 More preferably, it is 0.30 μm or less. 3 More preferably, it is 0.20 μm or less. 3 The lower limit of the surface roughness is not particularly limited, but is, for example, 0.01 μm or less. 3 If the composite particles have excellent fluidity, the smoothness of the surface of the resulting electrode can be increased, thereby reducing the internal resistance of the electrochemical device and improving the rate characteristics.

[0068] (Method for manufacturing an electrode for electrochemical devices) The method for manufacturing an electrode for electrochemical devices of the present invention includes manufacturing composite particles according to the manufacturing method of the present invention described above, and pressure-molding the manufactured composite particles on an electrode substrate to form an electrode mixture layer (pressure molding operation). The electrode for electrochemical devices obtained according to this manufacturing method has excellent flexibility and is less susceptible to cracking of the contained electrode active material, and further can improve the cycle characteristics of an electrochemical device equipped with such an electrode.

[0069] <Pressure Molding Operation> The pressure molding operation can be carried out according to a known method. For example, the composite particles produced according to the production method of the present invention can be subjected to a roll press and roll-pressed on an electrode substrate to pressure mold the composite particles on the electrode substrate to form an electrode mixture layer. The pressure during pressing can be appropriately set according to the desired electrode density.

[0070] The electrode substrate is made of a material that is conductive and electrochemically durable. Specifically, the electrode substrate may be made of a current collector made of, for example, iron, copper, aluminum, nickel, stainless steel, titanium, tantalum, gold, platinum, etc. One of the above materials may be used alone, or two or more may be used in combination in any ratio.

[0071] (Electrochemical device) The electrochemical device formed using the electrode for electrochemical devices of the present invention is not particularly limited, and may be, for example, a lithium ion secondary battery, an electric double layer capacitor, or a lithium ion capacitor, and preferably a lithium ion secondary battery. The electrochemical device formed using the electrode for electrochemical devices of the present invention has excellent cycle characteristics.

[0072] Hereinafter, a case where the electrochemical element is a lithium ion secondary battery will be described as an example, but the present invention is not limited to the following example. A lithium ion secondary battery as the electrochemical element of the present invention usually comprises electrodes (positive and negative electrodes), an electrolyte, and a separator, and uses the electrochemical element electrode of the present invention for at least one of the positive and negative electrodes.

[0073] <Electrode> Here, the electrode other than the above-described electrode for electrochemical elements of the present invention that can be used in a lithium ion secondary battery as an electrochemical element is not particularly limited, and any known electrode can be used. Specifically, the electrode other than the above-described electrode for electrochemical elements can be an electrode obtained by forming an electrode mixture layer on a current collector using a known manufacturing method.

[0074] <Electrolyte> As the electrolyte, an organic electrolyte solution in which a supporting electrolyte is dissolved in an organic solvent is usually used. As the supporting electrolyte, for example, a lithium salt is used. As the lithium salt, for example, LiPF 6 , LiAsF 6 , LiBF 4 , LiSbF 6 , LiAlCl 4 , LiClO 4 , C.F. 3 SO 3 Li, C 4 F 9 SO 3 Li, CF 3 COOLi, (CF 3 CO) 2 NLi, (CF 3 SO 2 ) 2 NLi, (C 2 F 5 SO 2 Among them, LiPF is particularly preferred because it is easily soluble in solvents and shows a high degree of dissociation. 6 , LiClO 4 , C.F. 3 SO 3 Li is preferred, and LiPF 6 The electrolyte may be used singly or in combination of two or more kinds in any ratio.

[0075] The organic solvent used in the electrolyte is not particularly limited as long as it can dissolve the supporting electrolyte. For example, carbonates such as dimethyl carbonate (DMC), ethylene carbonate (EC), diethyl carbonate (DEC), propylene carbonate (PC), butylene carbonate (BC), and methyl ethyl carbonate (EMC) are preferred. Other suitable solvents include esters such as γ-butyrolactone and methyl formate, ethers such as 1,2-dimethoxyethane and tetrahydrofuran, and sulfur-containing compounds such as sulfolane and dimethyl sulfoxide. Mixtures of these solvents may also be used. The electrolyte concentration in the electrolyte can be adjusted as appropriate. Known additives, such as vinylene carbonate, fluoroethylene carbonate, and ethyl methyl sulfone, may also be added to the electrolyte.

[0076] <Separator> The separator is not particularly limited and known separators can be used. Among them, a microporous film made of a polyolefin resin (polyethylene, polypropylene, polybutene, polyvinyl chloride) is preferred. Furthermore, as the separator, a separator with a functional layer, in which a functional layer (porous membrane layer or adhesive layer) is provided on one or both sides of a separator substrate, may be used.

[0077] <Method for manufacturing lithium-ion secondary battery> A lithium-ion secondary battery can be manufactured, for example, by stacking a positive electrode and a negative electrode with a separator interposed therebetween, rolling or folding the resulting structure as needed according to the battery shape, placing it in a battery container, injecting an electrolyte into the battery container, and sealing it. To prevent internal pressure rise, overcharge / discharge, and the like in the secondary battery, a fuse, an overcurrent prevention element such as a PTC element, an expanded metal, a lead plate, or the like may be provided as needed. The shape of the secondary battery may be any type, such as a coin type, a button type, a sheet type, a cylindrical type, a rectangular type, or a flat type.

[0078] The present invention will be described in detail below based on examples, but the present invention is not limited to these examples. In the following description, "%" and "parts" representing amounts are based on mass unless otherwise specified. Furthermore, in a polymer produced by copolymerizing multiple types of monomers, the proportion of a repeating unit (monomer unit) formed by polymerizing a certain monomer in the polymer usually coincides with the ratio (feed ratio) of that certain monomer to all monomers used in the polymerization of the polymer, unless otherwise specified. In the examples and comparative examples, the measurement and evaluation of various attributes were carried out according to the following methods.

[0079] <Solid content concentration of powder material> Wo [g] of the measurement object was weighed out and placed on an aluminum dish with a mass Wa [g], and heated on a hot plate at 130°C for 1 hour. The mass W [g] after heating was measured, and the solid content concentration Cs [%] of the powder material was calculated using the following formula: Cs = (W - Wa) / Wo × 100 [%]

[0080] <Viscosity index Cη of composition containing binder, conductive aid, and solvent> The viscosity index of a composition containing a binder, conductive aid, and solvent was calculated using the following formula from the viscosity measured by the method shown below and the solid content concentration measured by the method described above. Viscosity measurement: The viscosity η was measured at 25°C and 60 rpm using a B-type viscometer ("TVB-10M" manufactured by Toki Sangyo Co., Ltd.). The rotor used was changed appropriately depending on the viscosity. Calculation of viscosity index: Cη = η / Cs × 100 [mPa s]

[0081] <Particle diameter, coefficient of variation of particle diameter distribution, area circularity, and perimeter envelopment of composite particles> Based on the image analysis method in accordance with JIS Z 8827-1, image analysis processing was performed on the composite particles prepared in the Examples and Comparative Examples, and predetermined physical properties were calculated. Specifically, using Malvern's "Morphologi G3," images of 4,000 composite particles prepared in each Example and Comparative Example were binarized and analyzed, and the following physical properties were determined. The definitions of terms are in accordance with JIS Z 8890, "Evaluation of particle characteristics of powders - Terminology." Particle diameter: average particle diameter D of the area-equivalent diameter of 4,000 analyzed composite particles A(μm) Coefficient of variation of particle size distribution: average value D of the area-equivalent diameters of 4,000 analyzed composite particles A and the value CV calculated from its standard deviation σ: CV = σ / D A × 100 (%) Average area circularity: 4πA / P for 4,000 analyzed particles 2 (A: projected area, P: perimeter) A Average perimeter envelopment: The average value of the perimeter of the convex circumscribing figure (minimum convex hull) of all particles within the observation field divided by the perimeter P

[0082] <Bulk density ρ a Based on the constant volume measurement method described in JIS R 1628-1997, the bulk density (g / cm 3 ) was measured.

[0083] <Flowability (Evaluation by Surface Roughness)> 25 g of the composite particles produced in the Examples and Comparative Examples were placed on a 20 cm square glass plate with a smooth surface so that the diameter was about 20 mm, and the particles were smoothed with a 280 μm doctor blade. The smoothed surface was measured using a laser microscope to obtain a 5.4 mm 2 Space volume per unit (μm 3 ) was measured.

[0084] <Electrode Flexibility> The positive electrodes prepared in the Examples and Comparative Examples were wound around rods of different diameters to evaluate whether the positive electrode composite layer cracked. The smaller the diameter of the rod on which the positive electrode composite layer did not crack when wound around the rod, the more flexible the electrode and the better the winding ability. The flexibility of the electrode was evaluated according to the diameter of the thinnest rod on which the positive electrode composite layer did not crack, using the following criteria: A: No crack when wound around a rod with a diameter of 1.50 mm. B: No crack when wound around a rod with a diameter of 1.80 mm. C: No crack when wound around a rod with a diameter of 2.10 mm. D: No crack when wound around a rod with a diameter of 3.00 mm.

[0085] <Presence or absence of cracks in active material> Cross-sectional SEM images of the positive electrodes produced in the examples and comparative examples were observed at 1000x magnification, and the number of cracks observed in the active material was evaluated as follows according to the number of cracks observed in the active material. A: No cracked positive electrode active material was observed. B: The number of cracked positive electrode active material was 1 or more and less than 3. C: The number of cracked positive electrode active material was 3 or more and less than 5. D: The number of cracked positive electrode active material was 5 or more.

[0086] <Cycle Characteristics> After injecting the electrolyte, the lithium ion secondary batteries as electrochemical elements prepared in the Examples and Comparative Examples were left standing at 25°C for 5 hours. Next, the batteries were charged to a cell voltage of 3.65 V at 25°C using a constant current method at 0.2 C, and then aged for 12 hours at 60°C. Then, the batteries were discharged to a cell voltage of 3.00 V using a constant current method at 0.2 C at 25°C. Subsequently, CC-CV charging (upper limit cell voltage 4.20 V) was performed using a constant current method at 0.2 C, and CC discharging was performed to 3.00 V using a constant current method at 0.2 C. This 0.2 C charge-discharge cycle was repeated three times to prepare an evaluation cell. Next, the evaluation cell was subjected to 100 cycles of charge-discharge at a cell voltage of 4.20-3.00 V and a charge-discharge rate of 0.5 C under a temperature of 45°C. At this time, the discharge capacity at the first cycle was defined as X1, and the discharge capacity at the 100th cycle as X2. Using the discharge capacities X1 and X2, the capacity retention rate = (X2 / X1) x 100 (%) was calculated and evaluated according to the following criteria. A larger value of the capacity retention rate indicates that the lithium ion secondary battery has better cycle characteristics. A: Capacity retention rate is 90% or more B: Capacity retention rate is 85% or more but less than 90% C: Capacity retention rate is 80% or more but less than 85% D: Capacity retention rate is less than 80%

[0087] <Amount of gas generated during high-temperature storage> The evaluation cell prepared in the above-mentioned <Cycle characteristics> section was CC-CV charged (upper limit cell voltage 4.20 V) at a temperature of 25°C using a constant current method of 0.2 C, and then stored in a constant temperature environment of 60°C for one week. The cell volume was measured before and after storage, and the increase was taken as the amount of gas generated, which was evaluated according to the following criteria: A: Amount of gas generated is less than 5% B: Amount of gas generated is 5% or more but less than 10% C: Amount of gas generated is 10% or more but less than 20% D: Amount of gas generated is 20% or more

[0088] <Rate Characteristics> After injecting the electrolyte, the lithium ion secondary battery as an electrochemical element prepared in the examples was left standing at 25°C for 5 hours. Next, it was charged to a cell voltage of 3.65 V using a constant current method at 0.2 C at 25°C, and then aged for 12 hours at 60°C. Then, it was discharged to a cell voltage of 3.00 V using a constant current method at 0.2 C at 25°C. Thereafter, it was subjected to CC-CV charging (upper limit cell voltage 4.20 V) using a constant current method at 0.2 C, and CC discharge to 3.00 V using a constant current method at 0.2 C. This 0.2 C charge / discharge cycle was repeated three times. Next, it was charged to 4.2 V using a constant current method at 0.1 C in an environment at 25°C, and then discharged to 3.0 V at 0.1 C, and the 0.1 C discharge capacity was determined. Furthermore, the battery was charged to 4.2 V at 0.1 C and then discharged to 3.0 V at 1 C to determine the 1 C discharge capacity. These measurements were performed on 10 cells of each of the lithium ion secondary batteries used as electrochemical elements fabricated in the Examples and Comparative Examples, and the average values ​​of the measurements were designated as 0.1 C discharge capacity a and 1 C discharge capacity b. The electric capacity ratio = b / a x 100 (%) was then calculated and evaluated according to the following criteria. A larger value of the electric capacity ratio indicates that the lithium ion secondary battery used as an electrochemical element has better rate characteristics. AA: electric capacity ratio of 92 or more A: electric capacity ratio of 90% or more and less than 92 B: electric capacity ratio of 80% or more and less than 90% C: electric capacity ratio of 70% or more and less than 80% D: electric capacity ratio less than 70%

[0089] Example 1 Production of Binder A1 270 parts of dehydrated cyclohexane and 0.53 parts of ethylene glycol dibutyl ether were placed in a reactor equipped with a stirrer and the interior of which had been thoroughly purged with nitrogen, and 0.47 parts of n-butyllithium (15% cyclohexane solution) was further added. While stirring the entire contents at 60°C, 12.5 parts of dehydrated styrene were continuously added to the reactor over a period of 40 minutes. After the addition was completed, the entire contents were stirred for an additional 20 minutes at 60°C. When the reaction solution was measured by gas chromatography, the polymerization conversion rate at this point was 99.5%. Next, 75.0 parts of dehydrated isoprene was continuously added to the reaction solution over a period of 100 minutes, and stirring was continued for 20 minutes after the addition was completed. The polymerization conversion rate at this point was 99.5%. Thereafter, 12.5 parts of dehydrated styrene was continuously added over a period of 60 minutes, and after the addition was completed, the entire contents were stirred for an additional 30 minutes. The polymerization conversion rate at this point was nearly 100%. Here, 0.5 parts of isopropyl alcohol was added to the reaction solution to terminate the reaction. Of all the structural units derived from isoprene in the resulting block copolymer, the proportion of structural units derived from 1,2- and 3,4-addition polymerization was 58%. Next, the polymer solution was transferred to a pressure-resistant reactor equipped with a stirrer, and 7.0 parts of a diatomaceous earth-supported nickel catalyst (manufactured by JGC Catalysts and Chemicals, product name "E22U", nickel loading 60%) as a hydrogenation catalyst and 80 parts of dehydrated cyclohexane were added and mixed. The inside of the reactor was purged with hydrogen gas, and hydrogen was further supplied while stirring the solution, and the hydrogenation reaction was carried out at a temperature of 190°C and a pressure of 4.5 MPa for 6 hours. After completion of the hydrogenation reaction, the reaction solution was filtered to remove the hydrogenation catalyst, and then 1.0 part of a xylene solution containing 0.1 part of pentaerythrityl tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate] (manufactured by Koyo Chemical Research Institute, product name "Songnox 1010"), a phenolic antioxidant, was added to the filtrate and dissolved. Cyclohexane was further added to prepare a binder A1 solution of a predetermined concentration.

[0090] <Evaluation of Binder A1> - Proportion of structural units derived from 1,2- and 3,4-addition polymerization among structural units derived from chain conjugated diene compound in polymer block - The proportion of structural units derived from 1,2- and 3,4-addition polymerization among structural units derived from chain conjugated diene compound in polymer block was 1 From the H-NMR spectrum (in deuterated chloroform), it was found that the carbon-carbon unsaturated bond in the polymer main chain 1 H bonded to the carbon of the carbon-carbon unsaturated bond in the polymer side chain 1 The values ​​are shown above.

[0091] <Preparation of composition containing binder, conductive additive, and solvent> Carbon black (BET specific surface area: 62 m) was used as the conductive additive. 2 / g, bulk density 0.16 g / cm 3 ) and 2 parts of the binder A1 solution obtained above (on a solids basis) were mixed, and cyclohexane was added as a solvent to prepare a mixture of conductive additive, binder, and solvent with a solids concentration of 10% and a total amount of 1 kg. The resulting mixture was then dispersed for 1 hour using a bead mill (LMZ015, manufactured by Ashizawa Finetech) using zirconia beads with a diameter of 0.5 mm at a peripheral speed of 12 m / s to prepare a composition containing conductive additive, binder, and solvent. The resulting composition had a solids concentration of 10% by mass and a viscosity index of 300 mPa·s.

[0092] <Preparation of Composite Particles> A composite particle preparation device was prepared. The device consisted of a cylindrical vessel with an inner diameter of 180 mm and a capacity of 2 L, and two agitating blades, one vertical and one horizontal, with the axis of the cylindrical vessel being the vertical direction (the main agitating blade was the vertical axis and the auxiliary agitating blade was the horizontal axis). The main agitating blade was an inclined paddle with three main blades each 170 mm in diameter, and the auxiliary agitating blade had a V-shaped anchor blade with a diameter of 30 mm. The main and auxiliary agitating blades were sealed by ventilating air to prevent raw materials from being mixed into their drive mechanisms. Using the composite particle preparation device, composite particles were prepared by performing (i) a preliminary agitation operation, (ii) a composite particle formation operation, and (iii) a sizing operation in this order. First, in the (i) preliminary agitation operation, 96 parts by mass (1,344 g) of NMC532 (average particle diameter 6 μm) as a positive electrode active material for lithium-ion batteries was added to the granulation vessel. Next, room temperature air (hereinafter also referred to as "sealing air") for sealing the drive parts of the main and auxiliary stirring blades was circulated at 20 L / min (airflow rate 10 / min), and stirring was carried out for 15 minutes under operating conditions of a main stirring blade peripheral speed of 5 m / s and a auxiliary stirring blade peripheral speed of 6 m / s. The solids concentration of the powder material after stirring was measured and was found to be 99% by mass or more. Next, (ii) as the composite particle formation operation, room temperature sealing air was circulated at 20 L / min (airflow rate 10 / min), and the main stirring blade peripheral speed was 5 m / s and the auxiliary stirring blade peripheral speed was 6 m / s. 4 parts by mass (280 g) of a composition containing binder A1, carbon black as a conductive additive, and a solvent (solids concentration: 10% by mass, viscosity index: 300 mPa·s, solvent: cyclohexane) was continuously added as solids using a dropping funnel over 15 minutes. Next, (iii) as a particle size adjustment operation, room temperature sealing air was circulated at 20 L / min (airflow rate 10 / min), and the main stirring blade was operated at a peripheral speed of 2 m / s, and the auxiliary stirring blade was operated at a peripheral speed of 2 m / s for 10 minutes. The maximum temperature in the system throughout these steps (i) to (iii) was 38°C. Various measurements were carried out on the composite particles produced by carrying out the above operations (i) to (iii) in this order. The results are shown in Table 1.

[0093] <Preparation of Positive Electrode for Lithium-Ion Secondary Battery> The prepared composite particles were supplied to a press roll (roll temperature 100°C, press linear pressure 500 kN / m) of a roll press machine ("Press-Cut Rough Surface Hot Roll" manufactured by Hirano Giken Kogyo Co., Ltd.) using a quantitative feeder ("Nikka Spray K-V" manufactured by Nikka Corporation). An aluminum foil having a thickness of 20 μm was inserted between the press rolls, and the composite particles supplied from the quantitative feeder were adhered to the aluminum foil and press-molded at a molding speed of 1.5 m / min to a basis weight of 30 mg / cm. 2 This positive electrode raw sheet was rolled with a roll press to a density of 3.5 g / cm. 3A sheet-shaped positive electrode was fabricated consisting of a positive electrode mixture layer and aluminum foil. <Fabrication of Negative Electrode> 33 parts of 1,3-butadiene as an aliphatic conjugated diene monomer, 3.5 parts of itaconic acid as an acidic group-containing monomer, 63.5 parts of styrene as an aromatic vinyl monomer, 0.4 parts of sodium dodecylbenzenesulfonate as an emulsifier, 150 parts of ion-exchanged water, and 0.5 parts of potassium persulfate as a polymerization initiator were placed in a 5 MPa pressure vessel equipped with a stirrer, thoroughly stirred, and then heated to 50°C to initiate polymerization. The polymerization reaction was stopped by cooling when the polymerization conversion rate reached 96%, yielding a mixture containing a particulate binder (styrene-butadiene copolymer). A 5% aqueous sodium hydroxide solution was added to this mixture to adjust the pH to 8, and unreacted monomer was removed by heated vacuum distillation. The mixture was then cooled to 30°C or below to obtain an aqueous dispersion containing a negative electrode binder. Next, 48.75 parts of artificial graphite as a negative electrode active material, 48.75 parts of natural graphite, and 1 part of carboxymethyl cellulose as a thickener were added to a planetary mixer. The mixture was then diluted with ion-exchanged water to a solids concentration of 60%, and then kneaded for 60 minutes at a rotation speed of 45 rpm. Then, 1.5 parts of the aqueous dispersion containing the negative electrode binder obtained as described above, equivalent to the solids content, was added, and the mixture was kneaded for 40 minutes at a rotation speed of 40 rpm. Then, ion-exchanged water was added to obtain a viscosity of 3000±500 mPa·s (measured with a Brookfield viscometer at 25°C and 60 rpm), thereby preparing a negative electrode composite layer slurry. Next, a 15 μm thick copper foil was prepared as a current collector. The negative electrode composite layer slurry was applied to the copper foil in a coating amount of 15 mg / cm after drying. 2 The coating was dried at 60°C for 20 minutes and at 120°C for 20 minutes. Thereafter, the coating was heated at 150°C for 2 hours to obtain a negative electrode blank. This negative electrode blank was rolled using a roll press to a density of 1.6 g / cm. 3 A sheet-shaped negative electrode was fabricated consisting of the negative electrode composite layer (both sides) and copper foil. <Fabrication of Lithium-ion Secondary Battery> A single-layer laminate cell (discharge capacity equivalent to 250 mAh) was fabricated using the above-described positive electrode, negative electrode, and separator (made of polyethylene, thickness 12 μm) and placed in an aluminum package. Then, a 1.0 M LiPF 6 electrolyte was placed in the aluminum package. 6A solution (solvent: a mixed solvent of ethylene carbonate (EC) / diethyl carbonate (DEC) = 3 / 7 (volume ratio), additive: containing 2 volume % vinylene carbonate (solvent ratio)) was filled. Furthermore, in order to seal the opening of the aluminum packaging, the aluminum packaging was closed by heat sealing at a temperature of 150°C, and a lithium ion secondary battery was produced. Various evaluations were carried out using this lithium ion secondary battery. The results are shown in Table 1.

[0094] (Example 2) In the (ii) composite particle formation operation in <Preparation of composite particles>, various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that a composition produced using binder A2 (solid content concentration: 10 mass %, binder liquid viscosity: 400 mPa s, solvent: acetone) prepared as follows was used instead of binder A1. The results are shown in Table 1. <Production of Binder A2> A 10-liter reactor was charged with 100 parts of ion-exchanged water, 35 parts of acrylonitrile as a nitrile group-containing monomer, and 65 parts of 1,3-butadiene as an aliphatic conjugated diene monomer. 2 parts of potassium oleate as an emulsifier, 0.1 parts of potassium phosphate as a stabilizer, and 0.4 parts of tert-dodecyl mercaptan (TDM) as a molecular weight modifier were added. Emulsion polymerization was carried out at a temperature of 530°C in the presence of 0.35 parts of potassium persulfate as a polymerization initiator, resulting in copolymerization of acrylonitrile and 1,3-butadiene. When the polymerization conversion reached 95%, 0.2 parts of hydroxylamine sulfate per 100 parts of monomer was added to terminate the polymerization. Subsequently, the mixture was heated and subjected to steam distillation under reduced pressure at approximately 90°C to recover the residual monomer. Then, 0.1 parts of dibutylhydroxytoluene (BHT) as a substituted phenol was added to obtain an aqueous dispersion of the polymer. Calcium chloride (CaCl) was added as a coagulant in an amount of 3 parts per 100 parts of polymer solids in the resulting aqueous dispersion. 2A 25% by mass aqueous solution of 2,4-dichloro- ... 2 After adding 500 ppm of palladium, a hydrogenation reaction was carried out at a temperature of 90°C for 6 hours under a hydrogen pressure of 3.0 MPa to obtain a hydrogenated reaction product. After completion of the hydrogenation reaction, the palladium and silica were filtered off, and acetone was added to obtain a predetermined solid content concentration, thereby obtaining a binder A2 solution.

[0095] (Example 3) Various operations, measurements, and evaluations were performed similarly to those in Example 1, except for the following changes in the <Preparation of Composite Particles> step. The results are shown in Table 1. (i) Preparatory stirring in the <Preparation of Composite Particles> step was performed in two stages. Specifically, the preparatory stirring time in the granulation tank was shortened to 1 minute under the same conditions as in Example 1. Furthermore, prior to this operation, a mixture of 96 parts by mass of NMC532 as a positive electrode active material for lithium ion batteries and 0.5 parts by mass of carbon black as a conductive additive was mixed using a Miracle KCK (registered trademark) (model: M·KCK-L) manufactured by Asada Iron Works, Ltd., under conditions of a rotation speed of 40 rpm, a processing speed of 1 L / h, and a processing time of 10 minutes, and the resulting powder material was subjected to a preparatory stirring operation with a stirring time of 1 minute. In addition, (ii) in the composite particle formation operation, the amount of conductive additive blended into the composition containing the binder, solvent, and conductive additive added to the stirring tank was reduced so that the total blend amount in the composite particles was the same as in Example 1. Furthermore, in (ii) the composite particle formation operation, the main stirring blade was operated at a peripheral speed of 8 m / s, room temperature sealing air was circulated at 10 L / min (airflow rate 5 / min), and the means of adding the predetermined composition was changed to a two-fluid spray. The gas-liquid ratio (gas volume / liquid volume) and spray surface density at this time were as shown in Table 1. Finally, (iii) the operating time of the particle size adjustment operation was shortened to 1 minute. The maximum temperature in the system throughout these steps (i) to (iii) was 40°C.

[0096] Example 4 The same operations, measurements, and evaluations as in Example 1 were carried out, except for the following changes in the <Preparation of Composite Particles> step. The results are shown in Table 1. During the (i) pre-stirring operation in the <Preparation of Composite Particles> step, in addition to the electrode active material, a portion of the conductive additive to be blended was also added. The pre-stirring operation was also carried out in two stages. Specifically, the pre-stirring operation in the granulation tank under the same conditions as in Example 1 was shortened to 1 minute. Prior to this operation, a mixture of NMC532 as a positive electrode active material for lithium ion batteries and carbon black as a conductive additive was mixed using a Miracle KCK (registered trademark) (model: M.KCK-L) manufactured by Asada Iron Works, Ltd., under conditions of a rotation speed of 40 rpm, a processing speed of 1 L / h, and a processing time of 10 minutes. The resulting powder material was subjected to a pre-stirring operation with a stirring time of 1 minute.

[0097] (Example 5) The same operations, measurements, and evaluations as in Example 1 were carried out, except that the <Preparation of Composite Particles> step was changed as follows. The results are shown in Table 1. In (ii) the composite particle formation operation in <Preparation of Composite Particles>, the main stirring blade was operated at a peripheral speed of 8 m / s, and room temperature sealing air was circulated at 10 L / min (airflow rate 5 / min). Then, (iii) the operation time for the particle size adjustment operation was shortened to 1 minute. The maximum temperature in the system throughout these steps (i) to (iii) was 40°C.

[0098] Example 6 The same operations, measurements, and evaluations as in Example 1 were performed, except for the following changes in the <Preparation of Composite Particles> step. The results are shown in Table 1. In the (i) preliminary stirring operation in the <Preparation of Composite Particles> step, in addition to the electrode active material, a portion of the conductive additive was also added. Specifically, a mixture of 96 parts by mass of NMC532 as a positive electrode active material for lithium ion batteries and 0.5 parts by mass of carbon black as a conductive additive was used as a powder material for the preliminary diffusion operation. Furthermore, in the (ii) composite particle formation operation, the amount of conductive additive added to the composition containing the binder, solvent, and conductive additive added to the stirring vessel was reduced so that the total amount in the composite particles was the same as in Example 1. Furthermore, in the (ii) composite particle formation operation, the means of adding the predetermined composition was changed to a two-fluid spray. The gas-liquid ratio (gas volume / liquid volume) and spray surface density were as shown in Table 1. The maximum temperature in the system throughout these steps (i) to (iii) was 40°C.

[0099] (Example 7) Various operations, measurements, and evaluations were carried out in the same manner as in Example 6, except for the following changes in the <preparation of composite particles> step. The results are shown in Table 1. (ii) In the composite particle formation operation, when a predetermined composition was added by two-fluid spray, the gas-liquid ratio (gas volume / liquid volume) and spray surface density were set as shown in Table 1. The maximum temperature in the system throughout steps (i) to (iii) was 36°C.

[0100] (Example 8) Various operations, measurements, and evaluations were carried out in the same manner as in Example 6, except for the following changes in the <composite particle production> step. The results are shown in Table 1. (ii) In the composite particle formation operation, the main stirring blade was operated at a peripheral speed of 15 m / s, the auxiliary stirring blade was operated at a peripheral speed of 2 m / s, and the means of adding the predetermined composition was changed to a two-fluid spray. The gas-liquid ratio (gas volume / liquid volume) and spray surface density at this time were as shown in Table 1. (iii) In the particle size adjustment operation, the auxiliary stirring blade was operated at a peripheral speed of 10 m / s. The maximum temperature in the system throughout steps (i) to (iii) was 42°C.

[0101] (Example 9) Various operations, measurements, and evaluations were carried out in the same manner as in Example 6, except for the following changes in the <preparation of composite particles> step. The results are shown in Table 1. (ii) In the composite particle formation operation, the main stirring blade was operated at a peripheral speed of 3 m / s, the auxiliary stirring blade was operated at a peripheral speed of 10 m / s, and the means for adding the predetermined composition was changed to a two-fluid spray. The gas-liquid ratio (gas volume / liquid volume) and spray surface density at this time were as shown in Table 1. The maximum temperature in the system throughout steps (i) to (iii) was 34°C.

[0102] (Example 10) Various operations, measurements, and evaluations were carried out in the same manner as in Example 6, except for the following changes in the <preparation of composite particles> step. The results are shown in Table 1. (ii) In the composite particle formation operation, the main stirring blade was operated at a peripheral speed of 8 m / s, the sub-stirring blade was operated at a peripheral speed of 6 m / s, and the means of adding the predetermined composition was changed to a two-fluid spray. The gas-liquid ratio (gas volume / liquid volume) and spray surface density at this time were as shown in Table 1. (iii) In the particle size adjustment operation, the main stirring blade was operated at a peripheral speed of 0.4 m / s. The maximum temperature in the system throughout steps (i) to (iii) was 38°C.

[0103] (Example 11) Various operations, measurements, and evaluations were carried out in the same manner as in Example 6, except for the following changes in the <preparation of composite particles> step. The results are shown in Table 1. (ii) In the composite particle formation operation, the main stirring blade was operated at a peripheral speed of 5 m / s, the sub-stirring blade was operated at a peripheral speed of 10 m / s, and the means of adding the predetermined composition was changed to a two-fluid spray. The gas-liquid ratio (gas volume / liquid volume) and spray surface density at this time were as shown in Table 1. (iii) In the particle size adjustment operation, the main stirring blade was operated at a peripheral speed of 6 m / s. The maximum temperature in the system throughout steps (i) to (iii) was 38°C.

[0104] Comparative Example 1 Except for using a granulation vessel without a sub-stirring blade, the same operations, measurements, and evaluations (except for rate characteristics) as in Example 1 were carried out. The results are shown in Table 2.

[0105] Comparative Example 2 A granulation vessel was used in which the rotation axis of the auxiliary stirring blade was in the vertical direction, and the peripheral speeds of both the diffusion blades in (ii) the composite particle formation operation and (iii) the sizing operation were the same, except that the same operations, measurements, and evaluations (except for rate characteristics) were carried out as in Example 1. The results are shown in Table 2.

[0106] (Comparative Example 3) The same operations, measurements, and evaluations (except for rate characteristics) as in Example 1 were carried out, except that (i) no preliminary stirring operation was carried out, (ii) the electrode active material and the conductive additive were charged into the granulation tank when the composite particle formation operation was started, and further, (ii) the conductive additive was not blended into the composition added in the composite particle formation operation. The results are shown in Table 2.

[0107] (Comparative Example 4) (ii) The composite particle formation operation was not performed, and (i) in the preliminary stirring operation, an electrode active material, a conductive additive, and a composition containing a binder and a solvent were all added to a granulation tank and stirred, and then (iii) a particle size adjustment operation was performed. The same operations, measurements, and evaluations (except for rate characteristics) as in Example 1 were performed. The results are shown in Table 2. The maximum temperature in the system throughout these steps was 52°C.

[0108] (Comparative Example 5) (ii) In the composite particle formation operation, a composition not containing a conductive additive or a binder, i.e., only the solvent, was added to the granulation tank. Specifically, (ii) in the composite particle formation operation, sealing air was circulated at 20 L / min (airflow rate 10 / min), the main stirring blade was rotated at a peripheral speed of 5 m / s, and the auxiliary stirring blade was rotated at a peripheral speed of 6 m / s, and 280 g of cyclohexane as a solvent was continuously added to the granulation tank over 15 minutes. Other than this, the same operations, measurements, and evaluations (except for rate characteristics) as in Example 1 were performed. The results are shown in Table 2.

[0109]

[0110]

[0111] As can be seen from Tables 1 and 2, in Examples 1 to 11, in which the following steps were carried out in this order in a granulation tank equipped with two or more stirring blades having different stirring shafts: (i) stirring a powder material containing an electrode active material to create a stirred state; and (ii) adding a composition containing a binder, a conductive additive, and a solvent to the powder material in the stirred state to form composite particles, it was possible to produce composite particles that increased the flexibility of the electrode, suppressed cracking of the electrode active material in the electrode, and further improved the cycle characteristics of an electrochemical device equipped with such an electrode.

[0112] According to the present invention, it is possible to provide a method for producing composite particles that can increase the flexibility of an electrode, suppress cracking of the electrode active material in the electrode, and further improve the cycle characteristics of an electrochemical device equipped with such an electrode. Furthermore, according to the present invention, it is possible to provide a method for producing an electrode for an electrochemical device using the composite particles obtained according to the production method of the present invention.

[0113] REFERENCE SIGNS LIST 1 Granulation tank 2 Main stirring blade 21 Main blade 3 Sub-stirring blade 31 Sub-blade RA1 First stirring shaft RA2 Second stirring shaft

Claims

1. A method for producing composite particles, comprising the steps of: (i) stirring a powder material containing an electrode active material to produce a stirred state in a granulation tank equipped with two or more stirring blades having different stirring shafts; and (ii) adding a composition containing a binder, a conductive additive, and a solvent to the powder material in the stirred state to produce composite particles, in this order.

2. The method for producing composite particles according to claim 1, wherein in step (ii), the means for adding the composition is a spray nozzle.

3. The method for producing composite particles according to claim 1, further comprising the step of (iii) regulating the size of the composite particles by stirring the particles after completion of the addition of the composition, after the step (ii).

4. The method for producing composite particles according to claim 3, wherein a conductive assistant is added in step (iii).

5. The method for producing composite particles according to claim 1, wherein the powder material in step (i) contains a conductive assistant.

6. The method for producing composite particles according to claim 1, wherein the solvent contained in the composition is a non-aqueous solvent having a boiling point of 95° C. or lower at 1 atm.

7. A method for producing an electrode for an electrochemical element, comprising: producing composite particles according to the production method according to any one of claims 1 to 6; and press-molding the produced composite particles on an electrode substrate to form an electrode mixture layer.

Citation Information

Patent Citations

  • Manufacturing method of positive electrode for lithium secondary battery, positive electrode for lithium secondary battery, and agglomerated material

    JP2015170550A

  • Method of manufacturing positive electrode for nonaqueous electrolytic solution secondary battery

    JP2016149242A

  • Method for manufacturing nonaqueous electrolyte secondary battery

    JP2017054637A

  • Production method for composite particles and electrode for electrochemical element

    WO2023053651A1