Hot-rolling equipment and hot-rolling method
The hot rolling method and equipment address the issue of red heat embrittlement cracking by removing the Cu-enriched layer after heating and managing surface temperature, ensuring effective suppression of embrittlement and improved steel quality, which enhances the environmental sustainability of steel production.
Patent Information
- Application Number
- PCT/JP2024/012447
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-03
AI Technical Summary
The use of iron scrap containing copper (Cu) in steel manufacturing leads to surface defects and red heat embrittlement cracking during the hot rolling process, limiting the environmental benefits of increased Cu usage due to inadequate removal of Cu-enriched surface layers.
A hot rolling method and equipment that includes a heating furnace, a removal device to cut off the Cu-enriched surface layer, and a descaling device using cooling water to manage surface temperature, preventing re-embrittlement cracking by maintaining the surface temperature below 1100°C and ensuring the Cu-enriched layer is removed before rolling.
Effectively suppresses red heat embrittlement cracking and improves the surface quality of steel materials by removing the Cu-enriched layer after heating, preventing its re-formation during the rolling process, thus enhancing the environmental sustainability of steel production.
Smart Images

Figure JP2024012447_03102024_PF_FP_ABST
Abstract
Description
Hot rolling equipment and hot rolling method
[0001] The present disclosure relates to hot rolling equipment and hot rolling methods.
[0002] International Publication No. 2008 / 146891 describes a method for treating the surface layer of a hot slab, in which part or all of the surface layer of a steel material (e.g., a slab) after continuous casting is removed from the surface of the steel material by 1 mm or more using a milling-type surface layer removing device consisting of an electric rotary cutting tool with multiple cutting blades.
[0003] Furthermore, Japanese Patent Laid-Open Publication No. 6-198304 describes a hot rolling method in which the surface layer of a continuously cast steel material (for example, a slab) is removed by a cutting device or a grinding device, and then the steel material is hot rolled.
[0004] In recent years, in order to reduce carbon dioxide emissions in the steel manufacturing process, iron sources other than iron ore have been used. For example, increasing the proportion of scrap iron used as the iron source has been considered.
[0005] However, when scrap iron is used as an iron source, surface defects due to copper (Cu) contained in the scrap iron may occur during the steel production process. For example, during the hot rolling process, red embrittlement cracking may occur due to the concentration of Cu in the surface layer of the steel, resulting in a deterioration in the surface quality of the steel. For this reason, it is difficult to increase the proportion of scrap iron containing Cu used as an iron source, making it difficult to realize an environmentally friendly steel production process.
[0006] In the technique described in WO 2008 / 146891, the surface layer of the steel material after continuous casting is removed by a milling-type surface layer cutting device, so there is room for improvement in terms of suppressing red embrittlement cracking.
[0007] On the other hand, in the technique described in JP-A-6-198304, continuously cast steel material is heated in a heating furnace, and then the surface layer of the steel material is removed by a slag-cutting device or a grinding device. As a result, a Cu-enriched layer formed on the surface layer of the steel material when the steel material is heated in the heating furnace is removed by the slag-cutting device or the like. Therefore, red-hot embrittlement cracking on the surface of the steel material is suppressed.
[0008] However, the technology described in JP-A-6-198304 does not take into consideration the influence that removal of the surface layer of the steel material by a scouring device or the like has on the subsequent rolling of the steel material, and there is room for improvement in terms of the rolling quality of the steel material.
[0009] Therefore, an object of the present disclosure is to provide a hot rolling method and hot rolling equipment that can suppress red embrittlement cracking of steel while suppressing deterioration in the rolling quality of the steel.
[0010] The hot rolling equipment according to the first aspect is hot rolling equipment for hot rolling a steel material containing Cu, and includes: a heating furnace that heats the steel material after casting to a predetermined temperature; a rolling device that rolls the steel material heated in the heating furnace; a removal device that is provided downstream of the heating furnace and upstream of the rolling device in the conveying direction of the steel material, and that removes a target region from the steel material heated in the heating furnace, the target region including a Cu-enriched layer that is present on the surface side of the steel material and has a higher concentration of Cu components than in the base material of the steel material; and a post-removal descaling device that is provided downstream of the removal device and upstream of the rolling device in the conveying direction of the steel material, and that removes scales from the steel material using cooling water.
[0011] A hot rolling facility according to a second aspect is the hot rolling facility according to the first aspect, wherein the post-removal descaling device cools the steel material so that the temperature of the surface of the steel material becomes less than 1100°C.
[0012] The hot rolling equipment according to the third aspect is the hot rolling equipment according to the first or second aspect, and includes a width reduction device that is provided downstream of the heating furnace and upstream of the removal device in the conveying direction of the steel material, and that reduces the steel material in the width direction of the steel material.
[0013] The hot rolling equipment of the fourth aspect is the hot rolling equipment of any one of the first to third aspects, and includes a pre-removal descaling device that is provided downstream of the heating furnace and upstream of the removal device in the conveying direction of the steel material, and that removes scale from the steel material using cooling water.
[0014] A hot rolling facility according to a fifth aspect is the hot rolling facility according to any one of the first to fourth aspects, wherein the rolling device is a rough rolling device that performs rough rolling on the steel material, or a finish rolling device that performs finish rolling on the steel material.
[0015] A hot rolling facility according to a sixth aspect is the hot rolling facility according to any one of the first to fifth aspects, wherein the target area is an area that is 2 mm or less from the surface of the steel material in the thickness direction of the steel material.
[0016] A hot rolling facility according to a seventh aspect is the hot rolling facility according to any one of the second to sixth aspects, wherein the removal device removes the target area from the steel material by laser cutting, or removes the target area from the steel material by mechanical removal.
[0017] A hot rolling facility according to an eighth aspect is the hot rolling facility according to any one of the first to seventh aspects, wherein the heating furnace is provided separately from a production line of a casting machine that casts the steel material.
[0018] A hot rolling facility according to a ninth aspect is the hot rolling facility according to any one of the first to seventh aspects, wherein the heating furnace is provided on a production line of a casting machine that casts the steel material.
[0019] The hot rolling method according to the tenth aspect is a hot rolling method for hot rolling a steel material containing Cu, and includes: a heating step in which the steel material after casting is heated to a predetermined temperature; a removal step in which the steel material heated in the heating step is treated to remove a target region that is present on the surface side of the steel material and includes a Cu-enriched layer having a higher concentration of Cu components than in the base material of the steel material; a post-removal descaling step in which, after the removal step, the steel material is descaled using cooling water; and a rolling step in which the steel material is rolled after the post-removal descaling step.
[0020] A hot rolling method according to an eleventh aspect is the hot rolling method according to the tenth aspect, wherein in the post-removal descaling step, the steel material is cooled so that the temperature of the surface of the steel material becomes less than 1100°C.
[0021] A hot rolling method according to a twelfth aspect is the hot rolling method according to the tenth or eleventh aspect, further including a width reduction step of reducing the steel material in a width direction of the steel material after the heating step and before the removing step.
[0022] A hot rolling method according to a thirteenth aspect is the hot rolling method according to any one of the tenth to twelfth aspects, further including a pre-removal descaling step of removing scales from the steel material using cooling water after the heating step and before the removing step.
[0023] A hot rolling method according to a fourteenth aspect is the hot rolling method according to any one of the tenth to thirteenth aspects, wherein the rolling step includes performing rough rolling on the steel material.
[0024] A hot rolling method according to a fifteenth aspect is the hot rolling method according to any one of the tenth to fourteenth aspects, wherein the target region is a region that is 2 mm or less from the surface of the steel material in the thickness direction of the steel material.
[0025] A hot rolling method according to a sixteenth aspect is the hot rolling method according to any one of the tenth to fifteenth aspects, wherein in the removing step, the target area is removed from the steel material by laser cutting, or the target area is removed from the steel material by mechanical removal.
[0026] A hot rolling method according to a seventeenth aspect is the hot rolling method according to any one of the tenth to sixteenth aspects, wherein the steel material contains 0.15 mass % or more of Cu.
[0027] As described above, according to the present disclosure, there are provided a hot rolling method and hot rolling equipment that can suppress red embrittlement cracking of steel material while suppressing deterioration in the rolling quality of the steel material.
[0028] FIG. 1 is a schematic diagram showing an example of a schematic configuration of a hot rolling facility according to a first embodiment of the present disclosure; FIG. 2 is a schematic diagram showing an example of a thermal history of a steel material in a hot rolling facility according to a first embodiment of the present disclosure; FIG. 3 is a cross-sectional view showing a steel material to be laser-cut by the laser-cutting device according to the first embodiment of the present disclosure; FIG. 4 is a schematic diagram showing an example of a schematic configuration of a laser-cutting device according to the first embodiment of the present disclosure; FIG. 5 is a schematic diagram showing an example of a schematic configuration of a target region according to the first embodiment of the present disclosure; FIG. 6 is a flowchart showing an example of a hot rolling process according to the first embodiment of the present disclosure; FIG. 7 is a schematic diagram showing an example of a schematic configuration of a hot rolling facility according to a first modified example; FIG. 8 is a schematic diagram showing an example of a schematic configuration of a hot rolling facility according to a second modified example; FIG. 9 is a schematic diagram showing an example of a schematic configuration of a cutting device according to a second embodiment of the present disclosure; FIG. 10 is a schematic diagram showing an example of a schematic configuration of a hot rolling facility according to a third embodiment of the present disclosure; 1 is a schematic diagram showing an example of a schematic configuration of a hot rolling apparatus according to a second modification. 2 is a schematic diagram showing an example of a thermal history of a steel material in a hot rolling facility according to a second modification. 3 is a graph showing the relationship between the number ratio of Cu-enriched portions and the depth of scarification according to an example of the present disclosure.
[0029] Preferred embodiments of the present disclosure will be described in detail below with reference to the accompanying drawings. In this specification and the drawings, components having substantially the same functional configurations are designated by the same reference numerals, and redundant description will be omitted. Furthermore, unless otherwise specified, each component is not limited to one, and may be present in multiple numbers.
[0030] First Embodiment First, a schematic configuration of a hot rolling facility 10 according to a first embodiment of the present disclosure will be described with reference to Fig. 1. Fig. 1 is a diagram showing a schematic configuration of the hot rolling facility 10.
[0031] As an example, as shown in Figure 1, hot rolling equipment 10 is equipment for hot rolling steel material 1. As an example, this hot rolling equipment 10 is provided separately from a production line of a continuous casting machine 11 that continuously casts the steel material 1. The hot rolling equipment 10 includes a heating furnace 20, a laser cutting device 30, a width reduction device 23, a descaling device 40, a roughing rolling device 50, and a finishing rolling device 60. Note that the steel material 1 is not limited to being continuously cast, and may also be cast individually.
[0032] The heating furnace 20 heats the steel material 1 (for example, a slab 1A) obtained by cutting the steel material 1 discharged from the continuous casting machine 11 to a predetermined length, to a predetermined temperature. The "predetermined temperature" here is, for example, 1100°C or higher. The slab 1A is heated by the heating furnace 20 while being transported by the transport rolls 22. Here, the slab 1A is used as an example of the steel material 1, but this is merely an example, and the steel material 1 may also be a billet.
[0033] The steel material 1 is a steel material containing Cu, for example, a steel material containing 0.15 wt% (mass%) or more of Cu, particularly a steel material containing 0.25 wt% or more of Cu. Note that the Cu content here refers to the average Cu content in the base material of the steel material 1, which will be described later, or the average Cu content in the molten steel that becomes the steel material 1. The Cu content of the steel material 1 is, for example, 5.6 wt% or less.
[0034] The slag cutting device 30 performs slag cutting on the slab 1A discharged from the heating furnace 20 to remove a surface portion (surface layer) of the slab 1A. Details of the slag cutting device 30 will be described later. The slag cutting device 30 is located downstream of the heating furnace 20 in the conveying direction of the slab 1A. The slag cutting device 30 is also located upstream of the width reduction device 23 and the descaling device 40 in the conveying direction of the slab 1A. More specifically, the slag cutting device 30 is located downstream of the heating furnace 20 and upstream of the width reduction device 23 in the conveying direction of the slab 1A. The width reduction device 23 is a device that adjusts the width of the slab 1A by reducing (pressing) the slab 1A heated in the heating furnace 20 in the width direction of the slab 1A. The width reduction device 23 has a pair of vertical rolls 24 arranged on both sides of the slab 1A in the width direction. The pair of vertical rolls 24 is arranged along the thickness direction of the slab 1A. This pair of vertical rolls 24 presses down (presses) both surfaces (side end faces) of the slab 1A in the width direction toward the center of the slab 1A in the width direction, thereby adjusting the width of the slab 1A. In this specification, "removal" does not necessarily mean complete removal, but also refers to insufficient removal within a range generally acceptable in the technical field to which this disclosure pertains, and includes cases where there is insufficient removal to a degree that does not contradict the intent of this disclosure. The scalding device 30 is an example of a removal device.
[0035] The descaling device 40 removes scale (i.e., oxide film) formed on both surfaces of the slab 1A in the thickness direction and both surfaces (side end faces) of the slab 1A in the width direction before rough rolling by the roughing rolling device 50. The descaling device 40 removes scale from the surface of the slab 1A by spraying a fluid (e.g., cooling water) from a nozzle 42 onto the surface of the slab 1A. The descaling device 40 also cools the slab 1A by spraying the fluid from the nozzle 42 onto the slab 1A. This suppresses the generation of scale. The descaling device 40 sprays cooling water W, which is supplied from a cooling water tank (not shown) and adjusted to a predetermined water pressure using a pump (not shown), onto the slab 1A from the nozzle 42. The descaling device 40 removes scale from the slab 1A, and the surface temperature of the slab 1A is cooled to less than 1100°C by heat removal by the cooling water W. Here, the temperature of the surface of the slab 1A (for example, the surface in the width direction of the slab 1A) after the scale has been removed by the descaling device 40 is measured by a radiation thermometer. The descaling device 40 is an example of a post-removal descaling device.
[0036] The roughing rolling device 50 performs rough rolling (hot rough rolling) on the slab 1A to thin the slab 1A to a predetermined thickness. Specifically, the roughing rolling device 50 rolls the slab 1A, which has been rolled down in the width direction by the width reduction device 23 (vertical rolls 24), from the top and bottom to form a rough bar 1B. In the example shown in FIG. 1, the roughing rolling device 50 includes four rolling mills 51, 52, 53, and 54. Each of the rolling mills 51 to 54 has multiple rolls that sandwich the slab 1A from both sides in the thickness direction. The roughing rolling device 50 continuously rolls the slab 1A using the rolling mills 51 to 54. In the roughing rolling device 50, the slab 1A is thinned to a plate thickness of, for example, about 25 to 50 mm and formed into a rough bar 1B. Note that, here, an example in which the roughing rolling device 50 is equipped with four rolling mills 51 to 54 is shown, but this example is merely one example, and for example, the roughing rolling device 50 may be equipped with two rolling mills. In this case, in the roughing rolling device 50, reciprocating rolling is performed between the two rolling mills. Note that the roughing rolling device 50 is an example of a rolling device.
[0037] The finish rolling device 60 further hot finish rolls the rough bar 1B to a predetermined thickness. Specifically, the finish rolling device 60 finish rolls the rough bar 1B, which has been reheated by the rough bar heating device 62, to a thickness of about several mm (e.g., 1 to 2 mm). The finish rolling device 60 has multiple groups of finish rolling rolls 64 across 6 to 7 stands. Each group of finish rolling rolls 64 has multiple rolls aligned vertically. The finish rolling device 60 gradually reduces the rough bar 1B by passing it through the gaps between the multiple groups of finish rolling rolls 64. The steel strip 1C obtained by finish rolling the rough bar 1B to a predetermined thickness by the finish rolling device 60 is sent to a cooling device 70. Note that, although an example in which the finishing rolling apparatus 60 has six to seven stands of finishing rolls 64 is shown here, this example is merely one example, and the finishing rolling apparatus 60 may have, for example, five stands of finishing rolls 64. Note that the finishing rolling apparatus 60 is an example of a rolling apparatus.
[0038] The cooling device 70 cools the steel strip 1C after finish rolling with cooling water W. The cooling device 70 is, for example, a pipe laminar nozzle type cooling device. The steel strip 1C cooled by the cooling device 70 is wound into a coil by a winding device 80 and transported as a hot-rolled coil 1D from the hot rolling facility 10 to the next process.
[0039] Figure 2 shows an example of the thermal history of the steel material 1 in a series of processes including continuous casting, hot rolling, and cold rolling. As shown in Figure 2, at the start of continuous casting, the temperature of the steel material 1 is about 1500°C, and scale is generated on the surface of the steel material 1. This is because, when the temperature of the steel material 1 reaches 1100°C or higher, the surface of the steel material 1 is heated to 2Fe+O 2This is because the reaction of ZnO = 2FeO mainly proceeds, forming iron oxide (i.e., FeO) on the surface of the steel material 1 and turning into scale. In this temperature range, when the base material of the steel material 1 contains a relatively large amount of Cu (for example, when the average concentration of the Cu component in the base material is 0.15 wt % (mass %) or more), the iron oxide formed on the surface of the steel material 1 also contains Cu. Because the Cu in the iron oxide exists in a liquid phase without being oxidized, it infiltrates from the iron oxide into the surface layer of the bare metal part of the steel material 1. The Cu that infiltrates from the iron oxide into the surface layer of the bare metal part of the steel material 1 mainly precipitates and concentrates at the grain boundaries of the surface layer. In this way, a region (hereinafter referred to as a "Cu-enriched layer") where the concentration of the Cu component is higher than the average concentration of the Cu component in the base material of the steel material 1 is formed in the surface layer (surface side) of the bare metal part of the steel material 1 (i.e., a Cu concentration phenomenon occurs).
[0040] The Cu-enriched layer refers to a region in the unoxidized base metal of a steel material where, when a scale formed on the surface of the steel material due to oxidation, the concentration of Cu is higher than the average concentration of Cu in the base material of the steel material. In other words, the Cu-enriched layer refers to the region extending from the interface between the scale formed on the surface of the steel material and the base metal of the steel material, i.e., the surface of the unoxidized base metal of the steel material, toward the center of the thickness direction of the steel material, until the Cu component enriched at the grain boundaries is no longer observed. Here, the "region where the Cu component enriched at the grain boundaries is not observed" refers to a region where the concentration of Cu component present at the grain boundaries is equal to or less than the average concentration of the steel material + 1%. The base material of the steel material refers to the portion of the steel material excluding the Cu-enriched layer.
[0041] When Cu is present at the grain boundaries in a liquid phase (for example, at 1100°C or higher), the ductility of the grain boundaries decreases. Therefore, when a Cu-enriched layer is formed in the steel material 1, the steel material 1 exhibits red embrittlement, and red embrittlement cracks occur on the surface of the steel material 1. The cracks that occur on the surface of the steel material 1 become quality defects and therefore need to be removed. In particular, in high-quality steel materials and automotive steel sheets, for which surface quality is important, it is necessary to remove the surface cracks of the steel material 1.
[0042] In conventional surface treatment methods, surface defects such as iron oxide formed on the surface of the slab 1A, inclusions and casting powder embedded in the surface layer of the slab 1A during casting, or traces of bubbles on the surface layer of the slab 1A are removed using a grinder or the like. The removal of these surface defects is performed before the heating step (i.e., heating in the heating furnace 20) in the hot rolling process. That is, the surface defects are removed from the slab 1A before the hot rolling process. However, in the heating step in the hot rolling process, the slab 1A is heated again to 1100°C or higher (e.g., approximately 1400°C), and scale is re-formed on the surface of the slab 1A. As a result, the Cu concentration phenomenon recurs in the slab 1A, and red embrittlement cracking also recurs.
[0043] Therefore, as a result of intensive research, the inventors have come up with the idea of removing the Cu-enriched layer on the surface of the slab 1A after heating the slab 1A in the heating furnace 20 in the hot rolling process. That is, in the thermal history of the steel material 1 shown in FIG. 2 , after the steel material 1 leaves the heating furnace 20, it is not heated to 1000°C or less in the rough rolling process, and then is not heated to 1100°C or more again. That is, no scale is generated in the steel material 1 in processes subsequent to the heating process of the steel material 1 in the heating furnace 20. Therefore, the Cu-enriched phenomenon does not occur in the steel material 1, and no red-hot embrittlement cracking occurs in the steel material 1 in processes subsequent to the heating process of the steel material 1 in the heating furnace 20.
[0044] Therefore, in the hot rolling equipment 10 according to this embodiment, the surface layer of the slab 1A is removed by a scarifying device 30 located downstream of the heating furnace 20 in the conveying direction of the slab 1A. As shown in FIG. 3 as an example, the scarifying device 30 has two scarfer units 31 facing the surfaces on both sides (upper and lower) in the thickness direction of the steel material 1, and two scarfer units 31 facing the surfaces (side end faces) on both sides (left and right) in the width direction of the steel material 1. The four scarfer units 31 have the same configuration. Therefore, the following will describe the scarfer unit 31 facing one (upper) surface in the thickness direction of the steel material 1.
[0045] As shown in Figure 4, the scarfer unit 31 has a scarfer unit 31 arranged to face the surface of the steel material 1. This scarfer unit 31 is equipped with a preheating gas jetting section 34 and a scarfer-cutting oxygen jetting section 36. The preheating gas jetting section 34 jets preheating oxygen 32 and combustible gas 33. The scarfer-cutting oxygen jetting section 36 jets scarfer-cutting oxygen 37. Note that from the bottom of the scarfer-cutting oxygen jetting section 36, a shielding gas 38 consisting of combustible gas is jetted together with the scarfer-cutting oxygen 37. The steel material 1 is configured to be transported in the direction of arrow Y in Figure 4.
[0046] As shown in Figure 4, the jet of cutting oxygen 37 jetted from the cutting oxygen jetting section 36 is jetted further forward in the conveying direction Y of the steel material 1 than the jets of preheating oxygen 32 and combustible gas 33 jetted from the preheating gas jetting section 34.
[0047] In the scalding device 30, first, a preheating step is carried out as shown on the left side of Fig. 4. In the preheating step, preheating oxygen 32 and combustible gas 33 are ejected from a preheating gas ejection portion 34 of the scarfer unit 31 toward the surface of the steel material 1, and the combustible gas 33 is burned. Then, a part of the surface of the steel material 1 is melted by the heat of the burning combustible gas 33, and a basin portion 1E is formed.
[0048] The length of the basin 1E formed on the surface of the steel material 1 along the conveying direction Y is set to, for example, a range of about 20 mm to 30 mm.
[0049] Next, as shown on the right side of Fig. 4, a laser cutting process is carried out. In the laser cutting process, laser cutting oxygen 37 is ejected from the laser cutting oxygen ejection portion 36 of the scarfer unit 31 toward the surface of the steel material 1, and the steel material 1 on which the basin portion 1E has been formed is transported in the transport direction Y. At this time, a shielding gas 38 is ejected from the laser cutting oxygen ejection portion 36 together with the laser cutting oxygen 37, and the laser cutting oxygen 37 is protected by the shielding gas 38. The laser cutting process is an example of a removal process.
[0050] Then, the jet of cutting oxygen 37 jetted from the cutting oxygen jetting portion 36 passes through the basin 1E of the steel material 1 being transported, and an oxidation reaction between the cutting oxygen 37 and iron occurs with the basin 1E as a heat source. The heat of this oxidation reaction melts the surface of the steel material 1, and the surface of the steel material 1 is laser-cut. That is, the heat of the oxidation reaction laser-cuts the surface of the steel material 1 on the rear side of the basin 1E in the transport direction Y. In this way, the laser-cutting device 30 laser-cuts the surface layer of the slab 1A after it has been heated in the heating furnace 20.
[0051] 5, the laser cutting device 30 removes a target region T, which is a region including a Cu-enriched layer R. Here, the target region T is a range of a predetermined distance from the surface of the slab 1A (i.e., the surface of the scale S) in the thickness direction t of the slab 1A. The predetermined distance is, for example, greater than 0 mm and less than or equal to 3 mm (0 < distance ≦ 3 mm), preferably greater than 0 mm and less than or equal to 1 mm (0 < distance ≦ 1 mm), more preferably greater than 0 mm and less than or equal to 2 mm (0 < distance ≦ 2 mm), and even more preferably greater than 1 mm and less than or equal to 2 mm (1 < distance ≦ 2 mm).
[0052] The thickness of the slab 1A is, for example, about 250 mm. Therefore, by removing a region of 1 mm or less from the surface of the slab 1A as the target region T in the thickness direction t of the slab 1A, the reduction in the thickness of the slab 1A is reduced, thereby improving the yield of the slab 1A. Furthermore, by removing a region of 2 mm or less from the surface of the slab 1A as the target region T in the thickness direction t of the slab 1A, the Cu-enriched layer R can be more reliably removed while improving the yield of the slab 1A.
[0053] In the example shown in FIG. 5, the surface of one side in the thickness direction of the steel material 1 is subjected to spalling.
[0054] The target region T including the Cu-enriched layer R is removed from the steel material 1 by thermal cutting (removal), thereby removing the Cu-enriched portion R1 present at the grain boundary GB. As a result, red embrittlement cracking on the surface of the slab 1A is suppressed.
[0055] Next, a hot rolling method according to this embodiment will be described with reference to Fig. 6. Fig. 6 is a flowchart for explaining a part of the manufacturing process of a hot-rolled steel sheet according to this embodiment. As shown in Fig. 6, first, in the heating process of step ST10, the continuously cast slab 1A is heated to a predetermined temperature (for example, about 1300°C) by a heating furnace 20. After the heating process of step ST10 is performed, the manufacturing process proceeds to step ST12.
[0056] In the cutting process (removal process) of step ST12, the surface layer of slab 1A heated in step ST10 is cut by a cutting device 30, thereby removing a target region T including a Cu-enriched layer from slab 1A. After the cutting process of step ST12 is performed, the manufacturing process proceeds to step ST14.
[0057] If the average concentration of the Cu element in the base material of the steel material 1 is less than 0.15 wt%, it is difficult for a Cu-enriched layer to be formed in the steel material 1 (slab 1A), and therefore it is not necessary to perform the laser cutting of the surface layer of the steel material 1 (slab 1A) by the laser cutting device 30. In other words, if the average concentration of the Cu element in the base material of the steel material 1 is less than 0.15 wt%, it is not necessary to perform the laser cutting process (removal process) of step ST12.
[0058] In the descaling process of step ST14, the slab 1A from which the target region T has been removed in step ST12 is descaled using cooling water W by the descaling device 40. As a result of the descaling, the surface temperature of the slab 1A is reduced to, for example, less than 1100°C. After the descaling process of step ST14 is performed, the manufacturing process proceeds to step ST16.
[0059] In this embodiment, a width reduction process is performed after step ST12 (scaling process) and before step ST14 (descaling process). In the width reduction process, the slab 1A that has been scarified in step ST12 is reduced in width by a width reduction device 23, thereby adjusting the width of the slab 1A.
[0060] In the rough rolling process of step ST16, the slab 1A descaled in step ST14 is rough rolled by the rough rolling device 50. As a result, the slab 1A is formed into a rough bar 1B having a predetermined thickness. After the rough rolling process of step ST16 is performed, the manufacturing process proceeds to step ST18.
[0061] In the finish rolling process of step ST18, the rough bar 1B obtained in step ST16 is finish rolled by the finish rolling mill 60. As a result, the rough bar 1B is formed into a steel strip 1C having a predetermined thickness. After the finish rolling process of step ST18 is performed, the manufacturing process proceeds to step ST20.
[0062] In the winding process of step ST20, the steel strip 1C that has been finish-rolled in step ST18 is wound by a winding device 80 to be formed into a hot-rolled coil 1D. After the winding process of step ST20 is performed, part of the manufacturing process of the hot-rolled steel sheet according to this embodiment is completed.
[0063] As described above, in the hot rolling equipment 10 according to the first embodiment, after heating in the heating furnace 20, the target region T including the Cu-enriched layer formed in the steel material 1 is removed. When the steel material 1 is heated to a predetermined temperature (e.g., 1300°C) in the heating furnace 20, liquid-phase Cu is concentrated at the grain boundaries GB near the surface (surface layer) of the steel material 1. The portion (surface layer) of the steel material 1 where Cu is concentrated has poor ductility compared to the base metal portion of the steel material 1. For this reason, the occurrence of the Cu-enriched layer is one cause of red embrittlement cracking. In this embodiment, the target region T including the Cu-enriched layer is removed from the steel material 1 after heating in the heating furnace 20. Therefore, according to this embodiment, the occurrence of red embrittlement cracking in the steel material 1 is suppressed.
[0064] For example, it is conceivable to remove the Cu-enriched layer in advance from the steel material 1 after continuous casting. However, in this case, the steel material 1 is heated to a predetermined temperature in the heating furnace 20, and the Cu-enriched layer is re-formed in the steel material 1. For this reason, it is difficult to suppress red embrittlement cracking of the steel material 1. According to the present embodiment, after heating in the heating furnace 20, the target region T including the Cu-enriched layer is removed from the steel material 1. Then, in the hot rolling process, in the process after heating in the heating furnace 20 after continuous casting, the steel material 1 is not heated to a temperature above the temperature at which the Cu-enriched layer is formed (e.g., 1100°C), so the re-generation of the Cu-enriched layer is suppressed. As a result, the occurrence of red embrittlement cracking in the steel material 1 is suppressed.
[0065] In addition, even if the steel material 1 is heated to 1100°C or higher in the rough rolling process or the finish rolling process, the heating of the steel material 1 during rolling is short, so scale that causes a Cu-enriched layer is not formed on the surface of the steel material 1.
[0066] Furthermore, in the hot rolling equipment 10 according to the first embodiment, after the target region T is removed from the steel material 1 by the laser cutting device 30, the steel material 1 is descaled by the descaling device 40. In descaling, cooling water W is sprayed onto the surface of the steel material 1 to remove scale S formed on the surface. This descaling removes the scale S from the surface of the steel material 1 and also reduces the temperature of the surface of the steel material 1. The reduction in the temperature of the surface of the steel material 1 further suppresses the re-occurrence of a Cu-enriched layer. Therefore, according to this embodiment, the occurrence of red embrittlement cracking in the steel material 1 is suppressed.
[0067] Furthermore, in the hot rolling equipment 10 according to the first embodiment, the temperature of the surface of the steel material 1 is cooled to less than 1100°C by the descaling device 40. The decrease in the temperature of the surface of the steel material 1 further suppresses the re-generation of a Cu-enriched layer. Therefore, according to this embodiment, the occurrence of red embrittlement cracking in the steel material 1 is suppressed.
[0068] Furthermore, in the hot rolling equipment 10 according to the first embodiment, after the steel material 1 is descaled by the descaling device 40, the steel material 1 is rough rolled by the rough rolling device 50. The rough rolling reduces the temperature of the surface of the steel material 1, thereby further suppressing the re-occurrence of the Cu-enriched layer. Therefore, according to this embodiment, the occurrence of red embrittlement cracking in the steel material 1 is suppressed.
[0069] Furthermore, in the hot rolling equipment 10 according to the first embodiment, a region of 2 mm or less from the surface of the steel material 1 in the thickness direction t of the steel material 1 is removed by the laser cutting device 30. The Cu-enriched layer is mainly formed in a region of 2 mm or less from the surface of the steel material 1 in the thickness direction t of the steel material 1. Therefore, removing the region of 2 mm or less from the surface of the steel material 1 in the thickness direction t of the steel material 1 contributes to the removal of the Cu-enriched layer. Therefore, according to this embodiment, the occurrence of red embrittlement cracking in the steel material 1 is suppressed.
[0070] Furthermore, in the hot rolling equipment 10 according to the first embodiment, the target region T including the Cu-enriched layer is removed from the steel material 1 by the laser cutting device 30 by laser cutting the steel material 1. Removal of the target region T by laser cutting has higher productivity than removal of the target region T by cutting. Therefore, according to the present embodiment, the productivity of the steel material 1 can be improved.
[0071] Furthermore, the hot rolling equipment 10 according to the first embodiment is provided separately from the production line of the continuous casting machine 11. As a result, for example, depending on the production capacities of the continuous casting machine 11 and the hot rolling equipment 10, the steel material 1 continuously cast by each of the two continuous casting machines 11 can be hot rolled by one (one line) of hot rolling equipment 10. Furthermore, for example, even if the hot rolling equipment 10 is stopped, the continuous casting of the steel material 1 can be continued without stopping the continuous casting machine 11. Furthermore, since the thickness (slab thickness) of the steel material 1 is increased, the removal rate of the Cu-enriched layer relative to the steel material 1 can be made relatively thin.
[0072] (First Modification) In the above-described first embodiment, an example in which the descaling process is not performed before or after (immediately before or immediately after) the laser cutting process (removal process) has been described, but the present disclosure is not limited to this example. In the first modification, a pre-removal descaling process is performed before the laser cutting process (removal process), and a post-removal descaling process is performed after the laser cutting process (removal process).
[0073] 7, a pre-removal descaling device 40A is provided downstream of the heating furnace 20 and upstream of the laser cutting device 30 in the conveying direction of the steel material 1. The basic configuration of this pre-removal descaling device 40A is the same as that of the descaling device 40.
[0074] The pre-removal descaling device 40A removes scale and the like adhering to the surface of the steel material 1 before (just before) the surface of the steel material 1 is laser-cut by the laser-cutting device 30. That is, in the first modified example, the pre-removal descaling process is performed after the rough rolling process and before the laser-cutting process.
[0075] Here, when the surface of the steel material 1 is laser-cut by the laser-cutting device 30, if scale or the like is attached to the surface of the steel material 1, the combustion reaction between the laser-cutting oxygen 37 (see FIG. 4 ) sprayed from the laser-cutting device 30 and the steel material 1 is inhibited, and there is a possibility that the laser-cutting of the steel material 1 will be interrupted. In particular, when the laser-cutting thickness of the steel material 1 by the laser-cutting device 30 is kept to about 1 mm to 2 mm, the laser-cutting of the steel material 1 by the laser-cutting device 30 will be easily interrupted.
[0076] In contrast to this, in the first modified example, as described above, before the steel material 1 is laser-cut by the laser-cutting device 30, the pre-removal descaling device 40A removes scale adhering to the surface of the steel material 1. This makes it easier to stabilize the combustion reaction between the laser-cutting oxygen 37 (see FIG. 4 ) and the like sprayed from the laser-cutting device 30 and the steel material 1. Therefore, interruptions in the laser-cutting of the steel material 1 by the laser-cutting device 30 can be suppressed.
[0077] Furthermore, the pre-removal descaling device 40A removes scale adhering to the surface of the steel material 1 by spraying cooling water W onto the surface of the steel material 1. At this time, the surface of the steel material 1 is cooled by the cooling water W, which further suppresses the re-generation of a Cu-enriched layer on the steel material 1. Furthermore, in the fourth modified example, the pre-removal descaling device 40A cools the surface of the steel material 1 to less than 1100°C. Therefore, the re-generation of a Cu-enriched layer on the steel material 1 is further suppressed.
[0078] In addition, a post-removal descaling device 40B is provided downstream of the laser cutting device 30 and upstream of the width reduction device 23 in the conveying direction of the steel material 1. The basic configuration of this post-removal descaling device 40B is the same as that of the descaling device 40.
[0079] The post-removal descaling device 40B removes scale and the like formed on the surface of the steel material 1 after the steel material 1 has been laser-cut by the laser-cutting device 30. That is, in the first modified example, the post-removal descaling process is performed after the laser-cutting process and before the width reduction process.
[0080] By removing scales and the like formed on the surface of the steel material 1 using the post-removal descaling device 40B in this way, the quality of width adjustment of the steel material 1 by the width reduction device 23 can be improved.
[0081] Furthermore, when the steel material 1 is laser-cut by the laser-cutting device 30, the temperature of the surface of the steel material 1 rises (for example, to about 50°C). In response to this, the post-removal descaling device 40B removes scale adhering to the surface of the steel material 1 by spraying cooling water W onto the surface of the steel material 1. At this time, the surface of the steel material 1 is cooled by the cooling water W, which further suppresses the re-generation of a Cu-enriched layer in the steel material 1. Furthermore, in the first modified example, the post-removal descaling device 40B cools the surface of the steel material 1 to less than 1100°C. Therefore, the re-generation of a Cu-enriched layer in the steel material 1 is further suppressed. Therefore, the occurrence of red embrittlement cracking in the steel material 1 is suppressed.
[0082] Fig. 8 shows an example of the thermal history of the steel material 1 in a series of processes of continuous casting, hot rolling, and cold rolling in the first modified example. As shown in Fig. 8, at the start of continuous casting, the temperature of the steel material 1 is about 1500°C. Therefore, scale is generated on the surface of the steel material 1. On the other hand, after leaving the heating furnace 20, the steel material 1 is cooled to 1000°C or less during the rough rolling process, and is not heated to 1100°C or more thereafter. Therefore, in the first modified example, the same effects as those of the first embodiment can be obtained.
[0083] In the first modified example, a pre-removal descaling step is performed before the laser cutting step (removal step), and a post-removal descaling step is performed after the laser cutting step (removal step). However, at least one of the pre-removal descaling step and the post-removal descaling step can be omitted.
[0084] (Second Modification) In the above-described first embodiment, an example in which a laser cutting process (removal process) is performed before the width reduction process has been described, but the present disclosure is not limited to this example. In a second modification, the laser cutting process (removal process) is performed after the width reduction process and before the rough rolling process. Furthermore, in the second modification, a pre-removal descaling process is performed after the width reduction process and before the laser cutting process, and a post-removal descaling process is performed after the laser cutting process and before the rough rolling process.
[0085] 9, the laser cutting device 30 is provided downstream of the width reduction device 23 and upstream of the rough rolling device 50 in the conveying direction of the steel material 1. A pre-removal descaling device 40A is provided downstream of the width reduction device 23 and upstream of the laser cutting device 30 in the conveying direction of the steel material 1. Furthermore, a post-removal descaling device 40B is provided downstream of the laser cutting device 30 and upstream of the rough rolling device 50 in the conveying direction of the steel material 1.
[0086] The laser cutting device 30 laser cuts the surface of the steel material 1 that has been reduced in the width direction by the width reduction device 23. That is, in the second modified example, the laser cutting process is performed after the width reduction process and before the rough rolling process.
[0087] Here, when the steel material 1 is reduced in the width direction by the width reduction device 23, there is a possibility that red embrittlement cracking due to a Cu-enriched layer may occur, for example, on both surfaces (side end faces) in the width direction of the steel material 1. In contrast, in the second modified example, after the steel material 1 is reduced in the width direction by the width reduction device 23, the surfaces on both sides in the thickness direction of the steel material 1 and the surfaces on both sides in the width direction (side end faces) of the steel material 1 are laser-cut by the laser-cutting device 30. This makes it possible to remove red embrittlement cracking formed on both surfaces (side end faces) in the width direction of the steel material 1. Therefore, quality defects in the surface of the steel material 1 can be suppressed.
[0088] In the second modification, the pre-removal descaling step is performed before the laser cutting step, and the post-removal descaling step is performed after the laser cutting step. Therefore, the second modification can achieve the same effects as the first modification.
[0089] Second Embodiment In the above-described first embodiment, an example has been described in which the target region T including the Cu-enriched layer is removed from the steel material 1 by the laser cutting device 30, but the present disclosure is not limited to this example. In a second embodiment, the target region T is removed from the steel material 1 by a cutting device 90 instead of the laser cutting device 30. The cutting device 90 is an example of a removal device.
[0090] As an example, as shown in FIG. 10 , a hot rolling facility 10 includes a cutting device 90 instead of the slag cutting device 30. The cutting device 90 performs cutting on the slab 1A discharged from the heating furnace 20 to remove a surface portion of the slab 1A. Details of the cutting device 90 will be described later. The cutting device 90 is located downstream of the heating furnace 20 in the conveying direction of the slab 1A. The cutting device 90 is also located upstream of the width reduction device 23 and the descaling device 40 in the conveying direction of the slab 1A. More specifically, the cutting device 90 is located downstream of the heating furnace 20 and upstream of the width reduction device 23 (vertical rolls 24) in the conveying direction of the slab 1A.
[0091] As an example, as shown in Figure 11, the cutting device 90 includes a rotary cutting tool 92. The rotary cutting tool 92 has a holder 94 and a number of cutting blades 96 attached to the outer periphery of the holder 94. The rotary cutting tool 92 receives power from a power source (not shown) and rotates. The rotating cutting blades 96 come into contact with the surface of the steel material 1, thereby cutting the surface of the steel material 1. In this way, the cutting device 90 cuts the surface of the steel material 1, thereby removing a target area T on the surface of the steel material 1 after it has been heated in the heating furnace 20.
[0092] Although an example in which the cutting device 90 has one rotary cutting tool 92 has been given here, the present disclosure is not limited to this example. For example, one surface of the steel material 1 may be cut by a plurality of rotary cutting tools 92. Furthermore, the cutting device 90 may be provided with rotary cutting tools 92 at positions facing both surfaces of the steel material 1 in the thickness direction and both surfaces (side end faces) of the steel material 1 in the width direction.
[0093] As described above, in the hot rolling equipment 10 according to the second embodiment, the target region T including the Cu-enriched layer is removed from the steel material 1 by the cutting device 90. Mechanical removal such as cutting is less likely to cause deterioration in the surface quality of the steel material 1 (e.g., surface roughness) compared to removal by surface cutting. Therefore, according to this embodiment, deterioration in the surface quality of the steel material 1 in the hot rolling process can be suppressed.
[0094] In the second embodiment, an example in which the steel material 1 is cut by the cutting device 90 has been described, but the present disclosure is not limited to this example. The removal device is not limited to the cutting device 90, and may be, for example, a mechanical removal method such as grinding using a grinding wheel device.
[0095] <Third embodiment> In the above-described first embodiment, an example has been described in which the heating furnace 20 is provided separately from the production line of the continuous casting machine 11 that continuously casts the steel material 1. However, the present disclosure is not limited to this example. In a third embodiment, a heating furnace 102 is provided on the production line of the continuous casting machine that continuously casts the steel material 1.
[0096] As shown in FIG. 12 as an example, a continuous casting machine 11 continuously casts a slab 1A that is thinner (e.g., 50 mm to 100 mm) than the continuous casting machine 11 of the first embodiment. A hot rolling facility 100 is provided on the production line of the continuous casting machine 11. That is, the production line of the hot rolling facility 100 is continuous with the production line of the continuous casting machine 11. The hot rolling facility 100 includes a heating furnace 102, a pre-removal descaling device 40A, a laser cutting device 30, a post-removal descaling device 40B, a roughing rolling device 50, a rough bar heating furnace 104, and a finish rolling device 60. Note that the hot rolling facility 100 of the third embodiment does not include the width reduction device 23 (see FIG. 1) of the first embodiment. Furthermore, the roughing rolling facility 50 of the third embodiment includes, as an example, two rolling mills 51 and 52.
[0097] The heating furnace 102 is, for example, a table heating furnace. The heating furnace 102 is provided upstream of the roughing rolling device 50 in the conveying direction of the steel material 1. The heating furnace 102 heats the steel material 1 (for example, a slab 1A) obtained by cutting the steel material 1 discharged from the continuous casting machine 11 to a predetermined length, to a predetermined temperature (1100°C or higher).
[0098] The rough bar heating furnace 104 is, for example, a table heating furnace. The heating furnace 102 is provided downstream of the rough rolling device 50 and upstream of the finish rolling device 60 in the conveying direction of the steel material 1. The heating furnace 102 heats the steel material 1 that has been rough rolled by the rough rolling device 50 to a predetermined temperature (less than 1100°C).
[0099] Fig. 13 shows an example of the thermal history of the steel material 1 in a series of processes of continuous casting, hot rolling, and cold rolling in the third embodiment. As shown in Fig. 13, at the start of continuous casting, the temperature of the steel material 1 is about 1500°C. Therefore, scale is generated on the surface of the steel material 1. On the other hand, after leaving the heating furnace 102, the steel material 1 is cooled to 1000°C or less during the rough rolling process, and is not heated to 1100°C or more thereafter. Therefore, the third embodiment can achieve the same effects as the first embodiment.
[0100] Furthermore, in the third embodiment, a hot rolling facility 100 is provided on the production line of the continuous casting machine 11. This reduces heat loss between the continuous casting machine 11 and the hot rolling facility 100, thereby improving energy efficiency. In addition, since the steel material 1 is thin and the rolling load in the hot rolling facility 100 is small, the hot rolling facility 100 can be made smaller in size.
[0101] (Third Modification) In the third embodiment, the hot rolling facility 100 includes the roughing mill 50. However, the present disclosure is not limited to this embodiment. For example, in the third modification, the hot rolling facility 110 does not include the roughing mill 50.
[0102] As an example, as shown in FIG. 14, a hot rolling facility 110 includes a heating furnace 102, a pre-removal descaling device 40A, a surface cutting device 30, a post-removal descaling device 40B, a rough bar heating device 62, and a finish rolling device 60, but does not include a rough rolling device 50.
[0103] In this way, when the slab 1A continuously cast by the continuous casting machine 11 is thin, the roughing rolling device 50 may be omitted. In addition, in the third modified example, the hot rolling equipment 110 includes the rough bar heating device 62, but the hot rolling equipment 110 does not necessarily have to include the rough bar heating device 62.
[0104] Fig. 15 shows an example of the thermal history of the steel material 1 in a series of processes of continuous casting, hot rolling, and cold rolling in the third modified example. As shown in Fig. 15, at the start of continuous casting, the temperature of the steel material 1 is about 1500°C. Therefore, scale is generated on the surface of the steel material 1. On the other hand, after leaving the heating furnace 102, the steel material 1 is cooled to 1000°C or less during the rough rolling process, and is not heated to 1100°C or more thereafter. Therefore, the third embodiment can achieve the same effects as the first embodiment.
[0105] In order to evaluate the performance of the hot rolling equipment 10 and the hot rolling method according to the present disclosure, an evaluation was made of the relationship between the thickness of the steel material 1 that was scarcely machined and the number of Cu-enriched portions in the steel material 1 .
[0106] Specifically, in Example 1, the composition of steel material 1 was adjusted to C: 0.0027 wt%, Si: 0.039 wt%, Mn: 0.2 wt%, P: 0.02 wt%, S: 0.011 wt%, Cu: 0.45 wt%, and the balance Fe. In Example 1, three steel materials 1 adjusted in this manner were heated in the heating furnace 20 of the hot rolling equipment 10 for 120 minutes, and each steel material 1 was heated to 1250°C. Then, the surfaces of the three steel materials 1 were respectively subjected to laser cutting to different laser cutting thicknesses. Furthermore, after descaling the surface of each steel material 1, the temperature of each steel material 1 was lowered to approximately 1000°C, which corresponds to the rough rolling start temperature, and then rapidly cooled.
[0107] The composition of the steel material 1 in Example 2 was the same as that of the steel material 1 in Example 1, except that the Cu content was 0.98 wt%. In Example 2, the four steel materials 1 prepared in this manner were subjected to heating, laser cutting, descaling, and cooling in the same manner as in Example 1. Note that the seven steel materials 1 in Examples 1 and 2 each had a different laser cutting thickness. Each of the steel materials 1 in Examples 1 and 2 manufactured in this manner was cut. Then, the cut surface near the surface of each steel material 1 was observed, and the number of grain boundaries reaching the surface of the steel material 1 where Cu enrichment was observed was counted within a range of 1 cm in the sheet passing direction (conveyance direction) or width direction of the steel material 1.
[0108] FIG. 16 shows the results of counting the number of Cu-enriched portions for each steel material 1 in Example 1 and Example 2. The vertical axis of FIG. 16 (proportion of the number of Cu-enriched portions) indicates the proportion of the measurement result for each steel material 1 to the maximum value (100%) of the measurement result (number of Cu-enriched portions) for each steel material 1. As shown in FIG. 16 as an example, in Example 1, the proportion of the number of Cu-enriched portions in each steel material 1 was significantly reduced after the steel material 1 was spalled. For example, in Example 1, the proportion of the number of Cu-enriched portions in each steel material 1 was 70 to 90% before spalling each steel material 1 (before spalling), but after spalling each steel material 1 to a spalling thickness of about 1 mm (after spalling), the proportion was reduced to 30% or less.
[0109] In Example 2, similar to Example 1, the number ratio of Cu-enriched portions in each steel material 1 decreased after the laser cutting. For example, in the case of a steel material 1 that was laser-cut to a thickness of about 3 mm, the number ratio of Cu-enriched portions was approximately 70% before the laser cutting of the steel material 1, but was 0% after the laser cutting of the steel material 1. In addition, in the case of two steel materials 1 that were laser-cut to a thickness of about 1.5 mm, the number ratio of Cu-enriched portions in each steel material 1 was approximately 100% or 35% before the laser cutting of each steel material 1, but was 0% after the laser cutting of each steel material 1. In addition, in the case of a steel material 1 that was laser-cut to a thickness of about 0.75 mm, the number ratio of Cu-enriched portions in the steel material 1 was approximately 35% before the laser cutting, but was approximately 25% after the laser cutting. In this way, it was confirmed that the Cu-enriched portions were reduced by laser-cutting the steel material 1.
[0110] Although the preferred embodiments of the present disclosure have been described in detail above with reference to the accompanying drawings, the present disclosure is not limited to these embodiments. It is clear that a person skilled in the art of the present disclosure can conceive of various modifications or applications within the scope of the technical ideas described in the claims, and it is understood that these also naturally fall within the technical scope of the present disclosure.
[0111] The disclosure of Japanese Patent Application No. 2023-054364, filed on March 29, 2023, is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards described herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard was specifically and individually indicated to be incorporated by reference.
[0112] In addition to the above-described embodiment, the following supplementary notes are also disclosed.
[0113] (Appendix 1) A hot rolling method for hot rolling a steel material containing Cu, comprising: a heating step of heating the steel material after continuous casting to a predetermined temperature; and a removing step of treating the steel material heated in the heating step, the removing step being a treatment for removing a target region that is present on the surface side of the steel material and includes a Cu-enriched layer having a higher Cu concentration than in the base material. (Appendix 2) The hot rolling method according to Appendix 1, further comprising a descaling step of removing scales from the steel material using cooling water after the removing step. (Appendix 3) The hot rolling method according to Appendix 2, in which the descaling step cools the surface of the steel material to a temperature of 1100°C or less. (Appendix 4) The hot rolling method according to Appendix 2 or Appendix 3, further comprising a rough rolling step of rough rolling the steel material, the rough rolling step being performed after the descaling step. (Supplementary Note 5) The hot rolling method according to any one of Supplementary Notes 1 to 4, wherein the target region is a region 2 mm or less from the surface of the steel material in the thickness direction. (Supplementary Note 6) The hot rolling method according to any one of Supplementary Notes 1 to 5, wherein the removing step removes the target region by dry cutting. (Supplementary Note 7) The hot rolling method according to any one of Supplementary Notes 1 to 5, wherein the removing step removes the target region by mechanical removal.
Claims
1. A hot rolling facility for hot rolling a steel material containing Cu, comprising: a heating furnace for heating the steel material after casting to a predetermined temperature; a rolling device for rolling the steel material heated in the heating furnace; a removal device provided downstream of the heating furnace and upstream of the rolling device in the conveying direction of the steel material, for removing a target area from the steel material heated in the heating furnace, the target area including a Cu-enriched layer that is present on the surface side of the steel material and has a higher concentration of Cu components than in the base material of the steel material; and a post-removal descaling device provided downstream of the removal device and upstream of the rolling device in the conveying direction of the steel material, for removing scales from the steel material using cooling water.
2. The hot rolling facility according to claim 1, wherein the post-removal descaling device cools the steel material so that the temperature of the surface of the steel material is less than 1100°C.
3. The hot rolling equipment according to claim 1 or 2, further comprising a width reduction device that is provided downstream of the heating furnace and upstream of the removal device in the conveying direction of the steel material, and reduces the steel material in the width direction of the steel material.
4. A hot rolling facility as claimed in any one of claims 1 to 3, including a pre-removal descaling device that is provided downstream of the heating furnace and upstream of the removal device in the transport direction of the steel material, and that removes scale from the steel material using cooling water.
5. The hot rolling facility according to any one of claims 1 to 4, wherein the rolling device is a rough rolling device that performs rough rolling on the steel material, or a finish rolling device that performs finish rolling on the steel material.
6. The hot rolling facility according to any one of claims 1 to 5, wherein the target area is an area that is 2 mm or less from the surface of the steel material in the thickness direction of the steel material.
7. The hot rolling facility according to any one of claims 1 to 6, wherein the removal device removes the target area from the steel material by dry cutting, or removes the target area from the steel material by mechanical removal.
8. The hot rolling facility according to any one of claims 1 to 7, wherein the heating furnace is provided separately from a production line of a casting machine that casts the steel material.
9. The hot rolling facility according to any one of claims 1 to 7, wherein the heating furnace is provided on a production line of a casting machine that casts the steel material.
10. A hot rolling method for hot rolling a steel material containing Cu, comprising: a heating step for heating the steel material after casting to a predetermined temperature; a removal step for treating the steel material heated in the heating step, which is a treatment for removing a target area that is present on the surface side of the steel material and includes a Cu-enriched layer having a higher concentration of Cu than in the base material of the steel material; a post-removal descaling step for removing scale from the steel material using cooling water after the removal step; and a rolling step for rolling the steel material after the post-removal descaling step.
11. The hot rolling method according to claim 10, wherein in the post-removal descaling step, the steel material is cooled so that the temperature of the surface of the steel material becomes less than 1100°C.
12. The hot rolling method according to claim 10 or 11, further comprising a width reduction step of reducing the steel material in the width direction of the steel material after the heating step and before the removing step.
13. A hot rolling method according to any one of claims 10 to 12, further comprising a pre-removal descaling step of removing scale from the steel material using cooling water after the heating step and before the removing step.
14. A hot rolling method according to any one of claims 10 to 13, wherein in the rolling step, rough rolling or finish rolling is performed on the steel material.
15. A hot rolling method according to any one of claims 10 to 14, wherein the target region is a region that is 2 mm or less from the surface of the steel material in the thickness direction of the steel material.
16. A hot rolling method according to any one of claims 10 to 15, wherein in the removing step, the target area is removed from the steel material by laser cutting, and the target area is removed from the steel material by mechanical removal.
17. A hot rolling method according to any one of claims 10 to 16, wherein the steel material contains 0.15 mass% or more of Cu.
Citation Information
Patent Citations
Method for rolling steel containing cu or sn
JP1994198304A
Marine Electric Actuators
JP2023054364A
Method of trimming surface layer portion of hot slab and process for producing hot rolled steel
WO2008146891A1
Process for producing copper alloy without surface defect
JP1976126322A
Slag deposition prevention apparatus, and slag deposition prevention method using the same